Method for manufacturing doped electrode and method for manufacturing electric storage device
By employing a flowing dope solution and counter electrode units, the method addresses low doping rates in electrodes, achieving improved alkali metal distribution and device performance.
Patent Information
- Application Number
- JP2021542057
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-30
- Filing Date
- 2020-06-25
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-06-25
AI Technical Summary
Existing methods for pre-doping electrodes in batteries and capacitors suffer from low doping rates, which hinder the efficiency and performance of alkali metal-based energy storage devices.
A method for manufacturing doped electrodes involves contacting the electrode with a flowing dope solution containing alkali metal ions, using a system with counter electrode units and controlled fluidization to enhance the doping process.
The method significantly improves the doping rate, ensuring uniform distribution of alkali metals within the electrode active material, thereby enhancing the performance and efficiency of the energy storage devices.
Smart Images

Figure 0007556864000016 
Figure 0007556864000003 
Figure 0007556864000005
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This international application claims priority based on Japanese Patent Application No. 2019-158839, filed with the Japan Patent Office on August 30, 2019, the entire contents of which are incorporated herein by reference. [Technical field]
[0002] The present disclosure relates to a method for manufacturing a doped electrode, a method for manufacturing an electricity storage device, an electrode manufacturing system, and a doped electrode. [Background technology]
[0003] In recent years, electronic devices have become increasingly smaller and lighter. Accordingly, there is an increasing demand for smaller and lighter batteries to be used as the power source for these electronic devices.
[0004] In order to satisfy such demands for miniaturization and weight reduction, non-aqueous electrolyte secondary batteries, such as lithium ion secondary batteries, have been developed. In addition, lithium ion capacitors are known as power storage devices that can be used in applications that require high energy density and high output. Furthermore, sodium ion batteries and capacitors are also known that use sodium, which is less expensive and more abundant than lithium.
[0005] In such batteries and capacitors, a process of doping an electrode with an alkali metal in advance (generally called pre-doping) is adopted for various purposes. As a method of pre-doping an electrode with an alkali metal, for example, there is a continuous method. In the continuous method, pre-doping is performed while a strip-shaped electrode is transported in a doping solution. The continuous method is disclosed in Patent Documents 1 to 4. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 10-308212 [Patent Document 2] JP 2008-77963 A [Patent Document 3] JP 2012-49543 A [Patent Document 4] JP 2012-49544 A Summary of the Invention [Problem to be solved by the invention]
[0007] It is necessary to improve the doping rate in the pre-doping. In one aspect of the present disclosure, it is preferable to provide a method for manufacturing a doped electrode, a method for manufacturing an electricity storage device, an electrode manufacturing system, and an electricity storage device that can improve the doping rate in the pre-doping. [Means for solving the problem]
[0008] One aspect of the present disclosure is a method for producing a doped electrode including an active material doped with an alkali metal, the method comprising contacting an electrode including a current collector and an active material layer formed on a surface of the current collector and including the active material with a flowing doping solution containing alkali metal ions, thereby doping the alkali metal into the active material.
[0009] A method for producing a doped electrode that is one aspect of the present disclosure can improve the doping rate in pre-doping.
[0010] Another aspect of the present disclosure is a method for manufacturing an electricity storage device including an electrode cell, the method comprising: contacting a negative electrode including a negative electrode current collector and a negative electrode active material layer formed on a surface of the negative electrode current collector and containing an active material with a flowing doping solution containing alkali metal ions to dope the active material with the alkali metal; and after doping the active material with the alkali metal, stacking the negative electrode and an electrode other than the negative electrode to form the electrode cell.
[0011] A method for producing an electricity storage device according to another aspect of the present disclosure can improve the doping rate in pre-doping of the negative electrode.
[0012] Another aspect of the present disclosure is an electrode manufacturing system that manufactures a doped electrode including an active material doped with an alkali metal by performing a process for doping an alkali metal into an electrode including a current collector and an active material layer formed on a surface of the current collector and including an active material.
[0013] The electrode manufacturing system includes a doping tank that contains a doping solution containing alkali metal ions and in which the above-mentioned processing is carried out, and a flow unit that flows the doping solution contained in the doping tank.
[0014] The electrode manufacturing system according to another aspect of the present disclosure can improve the doping rate in the pre-doping step. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a plan view showing the configuration of an electrode. [Diagram 2] 2 is a cross-sectional view showing a cross section taken along line II-II in FIG. [Diagram 3] FIG. 1 is an explanatory diagram illustrating a configuration of an electrode manufacturing system. [Figure 4] FIG. 2 is an explanatory diagram illustrating a configuration of a doping tank. [Diagram 5] FIG. 2 is an explanatory diagram showing the configuration of a counter electrode unit. [Figure 6] FIG. 2 is an explanatory diagram illustrating a configuration of a nozzle. [Figure 7] FIG. 2 is an explanatory diagram showing the arrangement of the nozzles, electrodes, and counter electrode unit when viewed from above. [Figure 8] 13 is an explanatory diagram showing another arrangement of the nozzle, the electrode, and the counter electrode unit when viewed from above. FIG. [Figure 9] FIG. 2 is a plan view showing the configuration of an electrode test piece. [Figure 10] FIG. 2 is a plan view illustrating a configuration of an electrode unit. [Figure 11]FIG. 2 is a plan view showing the configuration of a stainless steel plate. [Figure 12] FIG. 2 is a cross-sectional view showing a configuration of a counter electrode unit. [Figure 13] FIG. 2 is a plan view showing the configuration of a Teflon (registered trademark) plate. [Figure 14] FIG. 4 is a plan view illustrating a configuration of a spacer. [Figure 15] FIG. 2 is a side view showing the configuration of a simple doped electrode manufacturing apparatus. [Figure 16] FIG. 2 is an explanatory diagram showing the configuration of a counter electrode unit and a nozzle. [Figure 17] FIG. 2 is an explanatory diagram showing the configuration of a counter electrode unit and a nozzle. [Explanation of symbols]
[0016] 1...electrode, 3...current collector, 5...active material layer, 6...active material layer forming section, 7...active material layer not formed section, 11...electrode manufacturing system, 15...electrolyte treatment tank, 17, 19, 21...doping tank, 23...cleaning tank, 25, 27, 29, 31, 33, 35, 37, 39, 40, 41, 43, 45, 46, 47, 49, 51, 52, 53, 55, 57, 58, 59, 61, 63, 64, 65, 67, 69, 70, 71, 73, 75, 77, 79, 81, 83, 85, 87, 89, 9 1, 93...conveyor roller, 101...supply roll, 103...winding roll, 105...support stand, 107...circulating filtration unit, 109, 110, 111, 112, 113, 114...power source, 117...tub cleaner, 119...recovery unit, 121...end sensor, 131...upstream tank, 133...downstream tank, 137, 139, 141, 143...counter electrode unit, 149, 151...space, 153...conductive substrate, 155...alkali metal-containing plate, 157...porous insulating member, 161 ...filter, 163...pump, 165...piping, 201...flow unit, 203, 205, 207, 209, 211, 213, 215, 217...nozzle, 219, 221...pump, 223, 225, 227, 229...piping, 231...hole, 301...electrode test piece, 303...main body, 305...projection, 307...lead, 309...Teflon plate, 311...opening, 312...electrode unit, 313...stainless steel plate, 315...recess, 317...screw hole, 319...tube Tube connector, 321... Fluorine rubber tube, 323... Lithium metal plate, 325... Teflon plate, 327... Opening, 329... Main body, 331... Notch, 333... Counter electrode unit, 335... Spacer, 337... Opening, 339... Simple doped electrode manufacturing device, 401... Frame, 403... Bus bar, 405... Conductive spacer, 407... Copper plate, 409... Lithium plate, 411... Mask, 413, 415, 417... Nozzle, 419, 421, 423... Pipe, 431... Hole DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Exemplary embodiments of the present disclosure will now be described with reference to the drawings. First Embodiment 1. Configuration of electrode 1 The structure of the electrode 1 will be described with reference to Figures 1 and 2. The electrode 1 has a strip-like shape. The electrode 1 includes a current collector 3 and an active material layer 5. The current collector 3 has a strip-like shape. The active material layers 5 are formed on both sides of the current collector 3.
[0018] The surface of the electrode 1 includes an active material layer formed portion 6 and an active material layer unformed portion 7. The active material layer formed portion 6 is a portion where an active material layer 5 is formed. The active material layer unformed portion 7 is a portion where an active material layer 5 is not formed. In the active material layer unformed portion 7, the current collector 3 is exposed.
[0019] The portion 7 without the active material layer formed has a band-like shape extending in the longitudinal direction L of the electrode 1. The portion 7 without the active material layer formed is located at an end of the electrode 1 in the width direction W of the electrode 1.
[0020] The current collector 3 is preferably a metal foil such as copper, nickel, or stainless steel. The current collector 3 may be a metal foil on which a conductive layer mainly made of a carbon material is formed. The thickness of the current collector 3 is, for example, 5 to 50 μm.
[0021] The active material layer 5 can be produced, for example, by applying a slurry containing an active material, a binder, and the like onto the current collector 3 and drying it.
[0022] Examples of the binder include rubber-based binders such as styrene-butadiene rubber (SBR) and NBR; fluorine-based resins such as polytetrafluoroethylene and polyvinylidene fluoride; polypropylene, polyethylene, and fluorine-modified (meth)acrylic binders as disclosed in JP-A-2009-246137.
[0023] The slurry may contain other components in addition to the active material and the binder. Examples of the other components include a conductive agent and a thickener. Examples of the conductive agent include carbon black, graphite, vapor-grown carbon fiber, and metal powder. Examples of the thickener include carboxymethylcellulose, its Na salt or ammonium salt, methylcellulose, hydroxymethylcellulose, ethylcellulose, hydroxypropylcellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, and casein.
[0024] There are no particular limitations on the thickness of the active material layer 5. The thickness of the active material layer 5 is, for example, 5 μm or more and 500 μm or less, preferably 10 μm or more and 200 μm or less, and particularly preferably 10 μm or more and 100 μm or less.
[0025] The active material contained in the active material layer 5 is not particularly limited as long as it is an electrode active material applicable to a battery or capacitor that utilizes the insertion and desorption of alkali metal ions. The active material may be either a negative electrode active material or a positive electrode active material.
[0026] The negative electrode active material is not particularly limited. Examples of the negative electrode active material include carbon materials such as graphite, easily graphitized carbon, hardly graphitized carbon, and composite carbon materials in which graphite particles are coated with pitch or resin carbide; metals such as Si and Sn that can be alloyed with lithium, semimetals, and materials containing oxides of these metals and semimetals.
[0027] Specific examples of the carbon material include the carbon material described in JP 2013-258392 A. Specific examples of the material containing a metal or semimetal capable of being alloyed with lithium or an oxide thereof include the materials described in JP 2005-123175 A and JP 2006-107795 A.
[0028] Examples of the positive electrode active material include transition metal oxides such as cobalt oxide, nickel oxide, manganese oxide, and vanadium oxide, and sulfur-based active materials such as elemental sulfur and metal sulfides. Both the positive electrode active material and the negative electrode active material may be made of a single material or a mixture of two or more materials.
[0029] The active material contained in the active material layer 5 is pre-doped with an alkali metal using an electrode manufacturing system 11 described later. As the alkali metal pre-doped into the active material, lithium or sodium is preferable, and lithium is particularly preferable. When the electrode 1 is used for manufacturing an electrode of a lithium ion secondary battery, the density of the active material layer 5 is preferably 1.30 g / cc or more and 2.00 g / cc or less, and particularly preferably 1.40 g / cc or more and 1.90 g / cc or less. When the electrode 1 is used for manufacturing an electrode of a lithium ion capacitor, the density of the active material layer 5 is preferably 0.50 g / cc or more and 1.50 g / cc or less, and particularly preferably 0.60 g / cc or more and 1.20 g / cc or less.
[0030] 2. Configuration of electrode manufacturing system 11 The configuration of the electrode manufacturing system 11 will be described with reference to Fig. 3 to Fig. 7. As shown in Fig. 3, the electrode manufacturing system 11 includes an electrolyte treatment tank 15, doping tanks 17, 19, and 21, a cleaning tank 23, and conveying rollers 25, 27, 29, 31, 33, 35, 37, 39, 40, 41, 43, 45, 46, 47, 49, 51, 52, 53, 55, 57, 58, 59, 61, 63, 64, 65, 67, 69, 70, 71, 73, 75, 77, 79, The rollers include rollers 81, 83, 85, 87, 89, 91, and 93 (hereinafter, these may be collectively referred to as a conveying roller group), a supply roll 101, a take-up roll 103, a support stand 105, a circulation filtration unit 107, six power sources 109, 110, 111, 112, 113, and 114, a tub cleaner 117, a recovery unit 119, and an end sensor 121. For the sake of convenience, a flow unit 201, which will be described later, is omitted in FIG. 3.
[0031] The electrolyte treatment tank 15 is a rectangular tank that is open at the top. The bottom surface of the electrolyte treatment tank 15 has a substantially U-shaped cross section. The electrolyte treatment tank 15 includes a partition plate 123. The partition plate 123 is supported by a support rod 125 that penetrates its upper end. The support rod 125 is fixed to a wall or the like (not shown). The partition plate 123 extends in the vertical direction, and divides the inside of the electrolyte treatment tank 15 into two spaces.
[0032] The electrolyte treatment tank 15 immerses the electrode 1 in the electrolyte before the electrode 1 reaches the doping tanks 17, 19, and 21. This makes it easier for the electrode 1 to be doped. As a result, it becomes easier to obtain a desired doped electrode.
[0033] The transport roller 33 is attached to the lower end of the partition plate 123. The partition plate 123 and the transport roller 33 are supported by a support rod 127 that penetrates them. The vicinity of the lower end of the partition plate 123 is cut out so as not to come into contact with the transport roller 33. A space exists between the transport roller 33 and the bottom surface of the electrolyte treatment tank 15.
[0034] The configuration of the dope tank 17 will be described with reference to Fig. 4. The dope tank 17 is composed of an upstream tank 131 and a downstream tank 133. The upstream tank 131 is disposed on the side of the supply roll 101 (hereinafter referred to as the upstream side), and the downstream tank 133 is disposed on the side of the take-up roll 103 (hereinafter referred to as the downstream side).
[0035] First, the configuration of the upstream tank 131 will be described. The upstream tank 131 is a rectangular tank that is open at the top. The bottom surface of the upstream tank 131 has a substantially U-shaped cross section. The upstream tank 131 includes a partition plate 135 and four counter electrode units 137, 139, 141, and 143.
[0036] The partition plate 135 is supported by a support rod 145 that passes through its upper end. The support rod 145 is fixed to a wall or the like (not shown). The partition plate 135 extends in the vertical direction and divides the interior of the upstream tank 131 into two spaces. The transport roller 40 is attached to the lower end of the partition plate 135. The partition plate 135 and the transport roller 40 are supported by a support rod 147 that passes through them. The partition plate 135 is cut out near its lower end so as not to come into contact with the transport roller 40. A space exists between the transport roller 40 and the bottom surface of the upstream tank 131.
[0037] The counter electrode unit 137 is disposed on the upstream side of the upstream tank 131. The counter electrode units 139 and 141 are disposed to sandwich the partition plate 135 from both sides. The counter electrode unit 143 is disposed on the downstream side of the upstream tank 131.
[0038] A space 149 exists between the counter electrode units 137 and 139. A space 151 exists between the counter electrode units 141 and 143. The counter electrode units 137, 139, 141, and 143 are connected to one pole of the power source 109. The counter electrode units 137, 139, 141, and 143 have the same configuration. Here, the configuration of the counter electrode units 137 and 139 will be described with reference to FIG. 5.
[0039] The counter electrode units 137 and 139 have a configuration in which a conductive base material 153, an alkali metal-containing plate 155, and a porous insulating member 157 are laminated. Examples of the material of the conductive base material 153 include copper, stainless steel, and nickel. The form of the alkali metal-containing plate 155 is not particularly limited, and examples of the form include an alkali metal plate and an alkali metal alloy plate. Examples of the alkali metal contained in the alkali metal-containing plate 155 include lithium and sodium. The thickness of the alkali metal-containing plate 155 is, for example, 0.03 to 6 mm.
[0040] The porous insulating member 157 has a plate-like shape. The porous insulating member 157 is layered on the alkali metal-containing plate 155. The plate-like shape of the porous insulating member 157 is the shape of the porous insulating member 157 when it is layered on the alkali metal-containing plate 155. The porous insulating member 157 may be a member that maintains a certain shape by itself, or may be a member that is easily deformable, such as a net.
[0041] The porous insulating member 157 is porous. Therefore, a doping solution, which will be described later, can pass through the porous insulating member 157. This allows the alkali metal-containing plate 155 to come into contact with the doping solution.
[0042] The porous insulating member 157 may be, for example, a mesh made of resin. Examples of resin include polyethylene, polypropylene, nylon, polyether ether ketone, and polytetrafluoroethylene. The mesh opening can be set appropriately. The mesh opening is, for example, 0.1 μm to 10 mm, and preferably 0.1 to 5 mm. The mesh thickness can be set appropriately.
[0043] The thickness of the mesh is, for example, 1 μm to 10 mm, and preferably 30 μm to 1 mm. The opening ratio of the mesh can be appropriately set. The opening ratio of the mesh is, for example, 5 to 98%, preferably 5 to 95%, and more preferably 50 to 95%.
[0044] The porous insulating member 157 may be made entirely of an insulating material, or may include an insulating layer in part.
[0045] The downstream tank 133 basically has the same configuration as the upstream tank 131. However, inside the downstream tank 133, a transport roller 46 is present instead of the transport roller 40. In addition, the counter electrode units 137, 139, 141, and 143 provided in the downstream tank 133 are connected to one pole of the power source 110.
[0046] The dope tank 19 basically has the same configuration as the dope tank 17. However, inside the dope tank 19, transport rollers 52 and 58 are present instead of transport rollers 40 and 46. Furthermore, the counter electrode units 137, 139, 141, and 143 of the upstream tank 131 of the dope tank 19 are connected to one pole of a power source 111. Furthermore, the counter electrode units 137, 139, 141, and 143 of the downstream tank 133 of the dope tank 19 are connected to one pole of a power source 112.
[0047] The dope tank 21 basically has the same configuration as the dope tank 17. However, inside the dope tank 21, transport rollers 64 and 70 are present instead of transport rollers 40 and 46. Furthermore, the counter electrode units 137, 139, 141, and 143 of the upstream tank 131 of the dope tank 21 are connected to one pole of the power source 113. Furthermore, the counter electrode units 137, 139, 141, and 143 of the downstream tank 133 of the dope tank 21 are connected to one pole of the power source 114.
[0048] The cleaning tank 23 basically has the same configuration as the electrolyte treatment tank 15. However, inside the cleaning tank 23, there are transport rollers 75 instead of transport rollers 33. The electrolyte carried out from the doping tank 21 adheres to the electrode 1 that has passed through the doping tank 21. In the cleaning tank 23, the electrolyte adhering to the electrode 1 is efficiently removed. This makes it easier to handle the electrode 1 in the next process.
[0049] Among the group of conveying rollers, conveying rollers 37, 39, 43, 45, 49, 51, 55, 57, 61, 63, 67, and 69 are made of a conductive material. The other conveying rollers, except for the bearing parts, are made of elastomer. The group of conveying rollers conveys the electrode 1 along a certain path. The path along which the group of conveying rollers conveys the electrode 1 is a path from the supply roll 101 through the electrolyte treatment tank 15, the dope tank 17, the dope tank 19, the dope tank 21, the cleaning tank 23, the tub cleaner 117, and finally to the take-up roll 103.
[0050] In the portion of the path that passes through the electrolyte treatment tank 15, the material first moves downward via the transport rollers 29 and 31, and then the transport roller 33 changes the direction of movement to an upward direction.
[0051] The portion of the above-mentioned path that passes through the dope tank 17 is as follows. First, the moving direction is changed downward by the conveying roller 37, and the dope tank 17 moves downward through the space 149 of the upstream tank 131. Next, the moving direction is changed upward by the conveying roller 40, and the dope tank 17 moves upward through the space 151 of the upstream tank 131. Next, the moving direction is changed downward by the conveying rollers 41 and 43, and the dope tank 17 moves downward through the space 149 of the downstream tank 133. Next, the moving direction is changed upward by the conveying roller 46, and the dope tank 17 moves upward through the space 151 of the downstream tank 133. Finally, the moving direction is changed horizontally by the conveying roller 47, and the dope tank 19 moves forward.
[0052] The portion of the above-mentioned path that passes through the dope tank 19 is as follows. First, the moving direction is changed downward by the conveying roller 49, and the dope tank 19 moves downward through the space 149 of the upstream tank 131. Next, the moving direction is changed upward by the conveying roller 52, and the dope tank 19 moves upward through the space 151 of the upstream tank 131. Next, the moving direction is changed downward by the conveying rollers 53 and 55, and the dope tank 19 moves downward through the space 149 of the downstream tank 133. Next, the moving direction is changed upward by the conveying roller 58, and the dope tank 21 moves upward through the space 151 of the downstream tank 133. Finally, the moving direction is changed horizontally by the conveying roller 59, and the dope tank 21 moves forward.
[0053] The portion of the above-mentioned path that passes through the dope tank 21 is as follows. First, the moving direction is changed downward by the conveying roller 61, and the roller moves downward through the space 149 of the upstream tank 131. Next, the moving direction is changed upward by the conveying roller 64, and the roller moves upward through the space 151 of the upstream tank 131. Next, the moving direction is changed downward by the conveying rollers 65 and 67, and the roller moves downward through the space 149 of the downstream tank 133. Next, the moving direction is changed upward by the conveying roller 70, and the roller moves upward through the space 151 of the downstream tank 133. Finally, the moving direction is changed horizontally by the conveying roller 71, and the roller moves toward the cleaning tank 23.
[0054] In addition, in the above-mentioned path, the portion that passes through the cleaning tank 23 is a path in which the direction of movement is first changed downward by the conveying roller 73 and moves downward, and then the direction of movement is changed upward by the conveying roller 75.
[0055] The electrode 1 is wound around the supply roll 101. That is, the supply roll 101 holds the electrode 1 in a wound state. The active material in the electrode 1 held by the supply roll 101 has not yet been doped with an alkali metal.
[0056] The group of transport rollers pulls out and transports the electrode 1 held by the supply roll 101. The winding roll 103 winds up and stores the electrode 1 transported by the group of transport rollers. The electrode 1 stored on the winding roll 103 has been pre-doped in the doping tanks 17, 19, and 21. Therefore, the active material in the electrode 1 stored on the winding roll 103 is doped with an alkali metal. The electrode 1 stored on the winding roll 103 corresponds to a doped electrode.
[0057] The support stand 105 supports the electrolytic solution treatment tank 15, the dope tanks 17, 19, 21, and the cleaning tank 23 from below. The height of the support stand 105 can be changed. The circulation filtration units 107 are provided in the dope tanks 17, 19, 21, respectively. The circulation filtration units 107 include a filter 161, a pump 163, and a pipe 165.
[0058] In the circulation filtration unit 107 provided in the dope tank 17, the pipe 165 is a circulation pipe that goes out from the dope tank 17, passes through the pump 163 and the filter 161 in order, and returns to the dope tank 17. The dope solution in the dope tank 17 circulates through the pipe 165 and the filter 161 by the driving force of the pump 163, and returns to the dope tank 17 again. At this time, foreign matter in the dope solution is filtered by the filter 161. Examples of the foreign matter include foreign matter precipitated from the dope solution and foreign matter generated from the electrode 1. The material of the filter 161 is, for example, a resin such as polypropylene or polytetrafluoroethylene. The pore size of the filter 161 can be appropriately set. The pore size of the filter 161 is, for example, 0.2 μm to 50 μm.
[0059] The circulation filtration units 107 provided in the dope tanks 19 and 21 have the same configuration and provide the same effects. For convenience, the dope solution is not shown in FIGS.
[0060] One terminal of the power source 109 is connected to the transport rollers 37 and 39. The other terminal of the power source 109 is connected to the counter electrode units 137, 139, 141, and 143 provided in the upstream tank 131 of the dope tank 17. The electrode 1 contacts the transport rollers 37 and 39. The electrode 1 and the counter electrode units 137, 139, 141, and 143 are in the dope solution, which is an electrolyte. Therefore, in the upstream tank 131 of the dope tank 17, the electrode 1 and the counter electrode units 137, 139, 141, and 143 are electrically connected via the electrolyte.
[0061] One terminal of the power source 110 is connected to the transport rollers 43 and 45. The other terminal of the power source 110 is connected to the counter electrode units 137, 139, 141, and 143 provided in the downstream tank 133 of the dope tank 17. The electrode 1 contacts the transport rollers 43 and 45. The electrode 1 and the counter electrode units 137, 139, 141, and 143 are in the dope solution, which is an electrolyte. Therefore, in the downstream tank 133 of the dope tank 17, the electrode 1 and the counter electrode units 137, 139, 141, and 143 are electrically connected via the electrolyte.
[0062] One terminal of the power source 111 is connected to the transport rollers 49 and 51. The other terminal of the power source 111 is connected to the counter electrode units 137, 139, 141, and 143 provided in the upstream tank 131 of the dope tank 19. The electrode 1 contacts the transport rollers 49 and 51. The electrode 1 and the counter electrode units 137, 139, 141, and 143 are in the dope solution, which is an electrolyte. Therefore, in the upstream tank 131 of the dope tank 19, the electrode 1 and the counter electrode units 137, 139, 141, and 143 are electrically connected via the electrolyte.
[0063] One terminal of the power source 112 is connected to the transport rollers 55 and 57. The other terminal of the power source 112 is connected to the counter electrode units 137, 139, 141, and 143 provided in the downstream tank 133 of the dope tank 19. The electrode 1 contacts the transport rollers 55 and 57. The electrode 1 and the counter electrode units 137, 139, 141, and 143 are in the dope solution, which is an electrolyte. Therefore, in the downstream tank 133 of the dope tank 19, the electrode 1 and the counter electrode units 137, 139, 141, and 143 are electrically connected via the electrolyte.
[0064] One terminal of the power source 113 is connected to the transport rollers 61 and 63. The other terminal of the power source 113 is connected to the counter electrode units 137, 139, 141, and 143 provided in the upstream tank 131 of the dope tank 21. The electrode 1 contacts the transport rollers 61 and 63. The electrode 1 and the counter electrode units 137, 139, 141, and 143 are in the dope solution, which is an electrolyte. Therefore, in the upstream tank 131 of the dope tank 21, the electrode 1 and the counter electrode units 137, 139, 141, and 143 are electrically connected via the electrolyte.
[0065] One terminal of the power source 114 is connected to the transport rollers 67 and 69. The other terminal of the power source 114 is connected to the counter electrode units 137, 139, 141, and 143 provided in the downstream tank 133 of the dope tank 21. The electrode 1 contacts the transport rollers 67 and 69. The electrode 1 and the counter electrode units 137, 139, 141, and 143 are in the dope solution, which is an electrolyte. Therefore, in the downstream tank 133 of the dope tank 21, the electrode 1 and the counter electrode units 137, 139, 141, and 143 are electrically connected via the electrolyte.
[0066] In addition, performing doping while electrode 1 and counter electrode units 137, 139, 141, and 143 are electrically connected via the electrolyte corresponds to electrically doping an alkali metal into the active material using counter electrode units 137, 139, 141, and 143 arranged opposite electrode 1.
[0067] The tub cleaner 117 cleans the portion 7 of the electrode 1 where the active material layer is not formed. The recovery units 119 are disposed in the electrolyte treatment tank 15, the dope tanks 17, 19, 21, and the cleaning tank 23. The recovery units 119 recover the liquid that the electrode 1 takes out of the tanks and return it to the tank.
[0068] The end sensor 121 detects the position of the end of the electrode 1 in the width direction W. The electrode manufacturing system 11 adjusts the positions of the supply roll 101 and the take-up roll 103 in the width direction W based on the detection result of the end sensor 121.
[0069] The electrode manufacturing system 11 includes a fluidizing unit 201 for each of the doping baths 17, 19, and 21. The configuration of the fluidizing unit 201 in the doping bath 17 is shown in Figures 4, 6, and 7. The configuration of the fluidizing unit 201 in the doping baths 19 and 21 is also similar.
[0070] The flow unit 201 includes a number of nozzles 203, 205, 207, 209, 211, 213, 215, and 217, two pumps 219 and 221, and a number of pipes 223, 225, 227, and 229.
[0071] 6, the nozzle 203 has a cylindrical shape. The nozzle 203 includes a plurality of holes 231. The plurality of holes 231 are arranged at predetermined intervals along the axial direction of the nozzle 203. The positions of the plurality of holes 231 in the circumferential direction are the same. Note that the positions of the plurality of holes 231 in the circumferential direction may change periodically as the nozzle 203 progresses in the axial direction. The nozzles 205, 207, 209, 211, 213, 215, and 217 also have a similar configuration to the nozzle 203.
[0072] 4, the nozzle 203 is attached in the upstream tank 131 near the counter electrode unit 137. The nozzle 205 is attached in the upstream tank 131 near the counter electrode unit 139. The nozzle 207 is attached in the upstream tank 131 near the counter electrode unit 141. The nozzle 209 is attached in the upstream tank 131 near the counter electrode unit 143.
[0073] The arrangement of the nozzles 203, 205, 207, and 209 as viewed from above is as shown in Fig. 7. There are two each of the nozzles 203, 205, 207, and 209. The axial directions of the nozzles 203, 205, 207, and 209 are parallel to the longitudinal direction L of the electrode 1. In each of the nozzles 203, 205, 207, and 209, the hole 231 faces the electrode 1 side.
[0074] In the width direction W of the electrode 1, the two nozzles 203 are each located near an end of the electrode 1. In the thickness direction of the electrode 1, the two nozzles 203 are each located between the counter electrode unit 137 and the electrode 1.
[0075] In the width direction W of the electrode 1, the two nozzles 205 are each located near an end of the electrode 1. In the thickness direction of the electrode 1, the two nozzles 205 are each located between the counter electrode unit 139 and the electrode 1.
[0076] In the width direction W of the electrode 1, the two nozzles 207 are each located near an end of the electrode 1. In the thickness direction of the electrode 1, the two nozzles 207 are each located between the counter electrode unit 141 and the electrode 1.
[0077] In the width direction W of the electrode 1, the two nozzles 209 are each located near an end of the electrode 1. In the thickness direction of the electrode 1, the two nozzles 209 are each located between the counter electrode unit 143 and the electrode 1.
[0078] The pump 219 sucks the dope solution from the upstream tank 131 using the pipe 223. The pump 219 sends the sucked dope solution to the nozzles 203, 205, 207, and 209 using the pipe 227. The sent dope solution is sprayed from the holes 231 of the nozzles 203, 205, 207, and 209. The sprayed dope solution flows along a direction F toward the electrode 1. The flow of the dope solution may start before the electrode 1 is set on the conveying roller group, or may start after the electrode 1 is set on the conveying roller group.
[0079] As a result, the doped solution flows between the counter electrode unit 137 of the upstream tank 131 and the electrode 1, between the counter electrode unit 139 of the upstream tank 131 and the electrode 1, between the counter electrode unit 141 of the upstream tank 131 and the electrode 1, and between the counter electrode unit 143 of the upstream tank 131 and the electrode 1. The flow direction of the doped solution is approximately parallel to the surface of the electrode 1. The flow direction of the doped solution is perpendicular to the longitudinal direction L of the electrode 1.
[0080] Here, "substantially parallel" has the following meaning. The center position of the hole 231 is defined as position A. On the surface of the electrode 1, a position that is at the same height as position A and in the center in the width direction W is defined as position B. If the angle formed by a line passing through positions A and B and the surface of the electrode 1 is 45 degrees or less, it is "substantially parallel."
[0081] The flow direction of the dope solution blown out from the hole 231 may be changed by using a plate-shaped tool or the like. For example, the flow direction of the dope solution changed by using a plate-shaped tool or the like is approximately parallel to the surface of the electrode 1.
[0082] 4, the nozzle 211 is attached in the downstream tank 133 near the counter electrode unit 137. The nozzle 213 is attached in the downstream tank 133 near the counter electrode unit 139. The nozzle 215 is attached in the downstream tank 133 near the counter electrode unit 141. The nozzle 217 is attached in the downstream tank 133 near the counter electrode unit 143.
[0083] The arrangement and orientation of the nozzles 211, 213, 215, and 217 are similar to the arrangement and orientation of the nozzles 203, 205, 207, and 209. The axial directions of the nozzles 211, 213, 215, and 217 are parallel to the longitudinal direction L of the electrode 1. In each of the nozzles 211, 213, 215, and 217, the hole 231 faces the electrode 1 side.
[0084] The pump 221 sucks the dope solution from the downstream tank 133 using a pipe 225. The pump 221 sends the sucked dope solution to the nozzles 211, 213, 215, and 217 using a pipe 229. The sent dope solution is blown out from holes 231 of the nozzles 211, 213, 215, and 217. The blown dope solution flows along a direction F toward the electrode 1.
[0085] As a result, the doped solution flows between the counter electrode unit 137 in the downstream tank 133 and the electrode 1, between the counter electrode unit 139 in the downstream tank 133 and the electrode 1, between the counter electrode unit 141 in the downstream tank 133 and the electrode 1, and between the counter electrode unit 143 in the downstream tank 133 and the electrode 1. The flow direction of the doped solution is approximately parallel to the surface of the electrode 1. The flow direction of the doped solution is perpendicular to the longitudinal direction L of the electrode 1.
[0086] As described above, the flow unit 201 causes the dope solution to flow between the electrode 1 and each counter electrode unit. The counter electrode units are the counter electrode units 137, 139, 141, and 143 in the upstream tank 131 and the counter electrode units 137, 139, 141, and 143 in the downstream tank 133. The average flow rate of the dope solution caused by the flow unit 201 is J (cm / sec).
[0087] The average flow velocity J can be defined as follows. A cross section is assumed in the flow path of the dope solution. The cross section is perpendicular to the flow direction of the dope solution. The average volumetric flow rate of the dope solution passing through the cross section per unit time is V (cm 3 / sec). The area of the cross section is S (cm 2 ) The average flow velocity J is V / S (cm / sec).
[0088] 3. Composition of the dope solution When the electrode manufacturing system 11 is used, a dope solution is contained in the electrolyte treatment tank 15 and the dope tanks 17, 19, and 21. The dope solution contains alkali metal ions and a solvent. The dope solution is an electrolyte.
[0089] Examples of the solvent include carbonate-based solvents, ester-based solvents, ether-based solvents, and hydrocarbon-based solvents. Ketone solvents, The solvent may be one or more selected from the group consisting of nitrile solvents, sulfur-containing solvents, and amide solvents.
[0090] Examples of the carbonate-based solvent include ethylene carbonate, 1-fluoroethylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl ethyl carbonate, ethyl methyl carbonate, propylene carbonate, and butylene carbonate.
[0091] Examples of the ester-based solvent include butyl acetate, amyl acetate, propylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl-3-ethoxypropionate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, butyl formate, propyl formate, ethyl lactate, butyl lactate, propyl lactate, γ-butyrolactone, valerolactone, mevalonolactone, and caprolactone.
[0092] Examples of the ether solvent include ethyl ether, i-propyl ether, n-butyl ether, n-hexyl ether, 2-ethylhexyl ether, ethylene oxide, 1,2-propylene oxide, dioxolane, 4-methyldioxolane, dioxane, dimethyldioxane, tetrahydrofuran, 2-methyltetrahydrofuran, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, dipropylene glycol dimethyl ether, and dipropylene glycol diethyl ether.
[0093] Examples of the hydrocarbon solvent include n-pentane, i-pentane, n-hexane, i-hexane, n-heptane, i-heptane, 2,2,4-trimethylpentane, n-octane, i-octane, cyclohexane, methylcyclohexane, benzene, toluene, xylene, ethylbenzene, trimethylbenzene, methylethylbenzene, n-propylbenzene, i-propylbenzene, diethylbenzene, i-butylbenzene, triethylbenzene, di-i-propylbenzene, n-amylnaphthalene, and trimethylbenzene.
[0094] Examples of the ketone solvent include 1-octanone, 2-octanone, 1-nonanone, 2-nonanone, 4-heptanone, 2-hexanone, diisobutyl ketone, cyclohexanone, methylcyclohexanone, phenylacetone, and methyl isobutyl ketone.
[0095] Examples of the nitrile solvent include acetonitrile, propionitrile, etc. Examples of the sulfur-containing solvent include sulfolane, dimethyl sulfoxide, etc. Examples of the amide solvent include dimethylacetamide, dimethylformamide, N-methylpyrrolidone, etc.
[0096] The solvent may be composed of a single component, or may be a mixed solvent of two or more components.
[0097] The alkali metal ions contained in the dope solution are ions constituting an alkali metal salt. The alkali metal salt is preferably a lithium salt or a sodium salt, and more preferably a lithium salt. The anion moiety constituting the alkali metal salt is, for example, PF6 - , PF3(C2F5)3 - , PF3(CF3)3 - Phosphorus anion with fluoro group such as BF4 - , BF2(CF)2 - , BF3(CF3) - , B(CN)4 - Boron anions with fluoro or cyano groups such as N(FSO2)2 - , N(CF3SO2)2 - , N(C2F5SO2)2 - Sulfonylimide anions with fluoro groups such as CF3SO3 - and the like.
[0098] Examples of lithium salts include LiClO4, LiAsF6, LiBF4, LiPF6, LiN(FSO2)2, LiN(C2F5SO2)2, and LiN(CF3SO2)2.
[0099] The concentration of the alkali metal salt in the doping solution is preferably 0.1 mol / L or more, and more preferably in the range of 0.5 to 1.5 mol / L. When the concentration of the alkali metal salt is within this range, pre-doping of the alkali metal proceeds efficiently.
[0100] The dope solution may further contain additives such as vinylene carbonate, vinyl ethylene carbonate, 1-fluoroethylene carbonate, 1-(trifluoromethyl)ethylene carbonate, succinic anhydride, maleic anhydride, propane sultone, and diethyl sulfone.
[0101] The dope solution may further contain a flame retardant such as a phosphazene compound. The amount of the flame retardant added is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, per 100 parts by mass of the dope solution, from the viewpoint of effectively controlling the thermal runaway reaction when doping with an alkali metal. Also, the amount of the flame retardant added is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less, per 100 parts by mass of the dope solution, from the viewpoint of obtaining a high-quality doped electrode.
[0102] 4. Method for manufacturing doped electrodes using the electrode manufacturing system 11 The manufacturing method for manufacturing the doped electrode is as follows. The electrode 1 before pre-doping is wound around the supply roll 101. Next, the electrode 1 before pre-doping is pulled out from the supply roll 101 and set to the take-up roll 103 along the above-mentioned path. Then, the electrolyte treatment tank 15, the doping tanks 17, 19, 21, and the cleaning tank 23 are raised and set to the fixed positions shown in FIG.
[0103] Next, the dope solution is placed in the electrolyte treatment tank 15 and the dope tanks 17, 19, and 21. The dope solution is as described in "3. Composition of the dope solution". The temperature of the dope solution is 40° C. or higher and 100° C. or lower. The cleaning tank 23 is placed with a cleaning solution. The cleaning solution is an organic solvent.
[0104] Next, the electrode 1 is transported along the above-mentioned path from the supply roll 101 to the take-up roll 103 by a group of transport rollers. The path along which the electrode 1 is transported passes through the doping tanks 17, 19, and 21. The transport direction of the electrode 1 is parallel to the longitudinal direction L. When the electrode 1 passes through the doping tanks 17, 19, and 21, the active material contained in the active material layer 5 is pre-doped with an alkali metal.
[0105] During pre-doping, the dope solution in the dope tanks 17, 19, and 21 is made to flow by the flow unit 201. More specifically, in each of the dope tanks 17, 19, and 21, the dope solution between the electrode 1 and each counter electrode unit is made to flow by the flow unit 201. The electrode 1 comes into contact with the flowing dope solution. Note that the dope solution does not need to be constantly flowing, and it is desirable that the dope solution be flowing when the alkali metal is doped into the electrode 1.
[0106] In each of the doping tanks 17, 19, and 21, the pre-doping is performed in a state in which the electrode 1 and each counter electrode unit are electrically connected via the electrolyte. In each of the doping tanks 17, 19, and 21, the current density per area of the electrode 1 in the pre-doping is I (mA / cm 2 The average flow velocity of the doping solution in each of the doping tanks 17, 19, and 21 is J (cm / sec). The average flow velocity J of the doping solution and the current density I in the pre-doping preferably satisfy the relationship of the following formula (1).
[0107] Formula (1) 0 Also, I / J is preferably 1 or more, more preferably 5 or more, and even more preferably 10 or more. When I / J is 5 or more, lithium doping can be performed more uniformly within the electrode surface, and when I / J is 10 or more, the effect is even more remarkable.
[0108] Also, I / J is preferably 150 or less, more preferably 100 or less, and even more preferably 60 or less. When I / J is 100 or less, lithium precipitation can be suppressed when the doping rate is increased, and when I / J is 60 or less, this effect is even more remarkable.
[0109] The current density I is 5mA / cm 2 It is preferable that the current is 25mA / cm or more. 2 More preferably, it is 45 mA / cm or more. 2 More preferably, it is 60 mA / cm or more. 2 It is more preferable that the current density I is 5 mA / cm or more. 2 When the current density I is 25 mA / cm or more, the doping rate is further improved. 2 When the current density I is 45 mA / cm or more, the above effect is more remarkable. 2 When the current density I is 60 mA / cm or more, the above effect is more remarkable. 2 In the above cases, the above effects are particularly remarkable.
[0110] The current density I is 500mA / cm 2 It is preferable that the current is less than 300mA / cm 2 More preferably, it is 180 mA / cm or less. 2 More preferably, it is 170 mA / cm or less. 2 It is particularly preferable that the current density I is 500 mA / cm or less. 2 When the current density I is 300 mA / cm or less, lithium deposition can be suppressed. 2 When the current density I is 180 mA / cm or less, the deposition of lithium can be further suppressed. 2 When the current density I is 170 mA / cm or less, lithium deposition can be further suppressed. 2 When the average flow velocity J of the doping solution is 0.1 cm / sec or more, the deposition of lithium can be particularly suppressed. cm / secIt is more preferable that the average flow velocity J of the doping solution is 0.1 cm / sec or more, and further preferably 1.0 cm / sec or more. When the average flow velocity J of the doping solution is 0.1 cm / sec or more, the doping speed is further improved. When the average flow velocity J of the doping solution is 0.5 cm / sec or more, the doping speed is further improved. When the average flow velocity J of the doping solution is 1.0 cm / sec or more, the doping speed is particularly improved.
[0111] In addition, the average flow velocity J of the doping solution is preferably 20 cm / sec or less, more preferably 10 cm / sec or less, and even more preferably 5 cm / sec or less. When the average flow velocity J of the doping solution is 20 cm / sec or less, lithium precipitation can be suppressed. When the average flow velocity J of the doping solution is 10 cm / sec or less, lithium precipitation can be further suppressed. When the average flow velocity J of the doping solution is 5 cm / sec or less, lithium precipitation can be particularly suppressed.
[0112] During pre-doping, the electrode 1 is transported along the above-mentioned path by the transport roller group. The transport direction is parallel to the longitudinal direction L of the electrode 1. The transport direction of the electrode 1 corresponds to a predetermined direction. The flow direction of the dope solution is perpendicular to the longitudinal direction L of the electrode 1. Therefore, during pre-doping, the flow direction of the dope solution is perpendicular to the transport direction of the electrode 1.
[0113] Furthermore, the group of transport rollers transports the electrode 1 to the cleaning tank 23. The electrode 1 is cleaned in the cleaning tank 23 while being transported by the group of transport rollers.
[0114] Furthermore, the group of transport rollers continuously transports the electrode 1 to a tub cleaner 117. The tub cleaner 117 cleans a portion 7 of the electrode 1 where an active material layer is not formed.
[0115] The electrode 1 may be a positive electrode or a negative electrode. When manufacturing a positive electrode, the electrode manufacturing system 11 dopes the positive electrode active material with an alkali metal. When manufacturing a negative electrode, the electrode manufacturing system 11 dopes the negative electrode active material with an alkali metal.
[0116] The doping amount of the alkali metal is preferably 70% or more and 95% or less of the theoretical capacity of the negative electrode active material when lithium is absorbed in the negative electrode active material of a lithium ion capacitor. The doping amount of the alkali metal is preferably 10% or more and 30% or less of the theoretical capacity of the negative electrode active material when lithium is absorbed in the negative electrode active material of a lithium ion secondary battery.
[0117] 5. Manufacturing method of electricity storage device Examples of the power storage device include a battery and a capacitor. Examples of the battery include a lithium ion secondary battery. Examples of the capacitor include a lithium ion capacitor. The power storage device includes an electrode cell. The electrode cell has a configuration in which a negative electrode and a positive electrode are stacked.
[0118] In the method for producing an electricity storage device, the negative electrode is produced by the above-mentioned "4. Method for producing doped electrode using electrode production system 11". Next, the negative electrode and the positive electrode are laminated to form an electrode cell.
[0119] 6. Effects of the manufacturing method of the doped electrode and the manufacturing method of the electricity storage device (1A) In the method for producing a doped electrode of the present disclosure, a flowing doping solution containing alkali metal ions is brought into contact with the electrode 1, thereby doping the active material with the alkali metal. According to the method for producing a doped electrode of the present disclosure, the doping speed in pre-doping can be improved. It is presumed that the reason for the improvement in the doping speed is that the concentration of the solvent component on the surface of the electrode 1 is suppressed by the flow of the doping solution. Examples of the solvent component include ethylene carbonate.
[0120] As a method for suppressing the concentration of the solvent component on the surface of the electrode 1, in addition to the above-mentioned method of flowing the dope solution, a method of irradiating the electrode 1 with ultrasonic waves can also be mentioned.
[0121] (1B) In the method of manufacturing a doped electrode of the present disclosure, for example, an alkali metal is electrically doped into an active material using counter electrode units 137, 139, 141, and 143 provided opposite electrode 1. This can further improve the doping speed in pre-doping.
[0122] (1C) In the method for producing a doped electrode of the present disclosure, for example, an alkali metal is doped into an active material in a state in which a doping solution is flowing between the electrode 1 and the counter electrode units 137, 139, 141, and 143. This can further improve the doping speed in the pre-doping step.
[0123] (1D) In the method for producing a doped electrode according to the present disclosure, for example, the current density I (mA / cm 2 The relationship between the flow rate J (cm / sec) of the dope solution and the flow rate J (cm / sec) satisfies the following formula (1).
[0124] Formula (1) 0 This makes it possible to further improve the doping speed in the pre-doping step.
[0125] (1E) In the method for producing a doped electrode of the present disclosure, for example, the current density I is 25 mA / cm 2 More than 500mA / cm 2 This makes it possible to further improve the doping speed in the pre-doping step.
[0126] (1F) In the method for producing a doped electrode of the present disclosure, for example, when an alkali metal is doped into an active material, the electrode 1 is moved in a predetermined direction in a doping solution, which can further improve the doping speed in the pre-doping step.
[0127] (1G) In the method for producing a doped electrode of the present disclosure, for example, when an alkali metal is doped into an active material, the flow direction of the doping solution is approximately parallel to the surface of the electrode 1. This can further improve the doping speed in the pre-doping step.
[0128] (1H) In the method for producing a doped electrode of the present disclosure, for example, when an alkali metal is doped into an active material, the flow direction of the doping solution is perpendicular to the transport direction of the electrode 1. This can further increase the doping speed in pre-doping.
[0129] (1I) In the method for producing a doped electrode of the present disclosure, for example, when an alkali metal is doped into an active material, the temperature of the doping solution is 40° C. or more and 100° C. or less. This can further improve the doping speed in pre-doping.
[0130] (1J) In the manufacturing method of the doped electrode of the present disclosure, for example, the electrolyte concentration in the doping solution is preferably 0.8 mol / L or more and 5.0 mol / L or less, more preferably 1.3 mol / L or more and 4.0 mol / L or less, so that the doping speed in the pre-doping can be further improved, and the initial coulombic efficiency can be further improved. do.
[0131] (1K) In the manufacturing method of the doped electrode of the present disclosure, for example, the solvent of the doping solution is one or more selected from the group consisting of carbonate-based solvents, ester-based solvents, ether-based solvents, hydrocarbon-based solvents, nitrile-based solvents, sulfur-containing solvents, and amide-based solvents. This can further improve the doping speed in pre-doping.
[0132] (1L) In the method for producing an electricity storage device according to the present disclosure, a negative electrode is produced by the method for producing a doped electrode according to the present disclosure, which makes it possible to further improve the doping speed in pre-doping of the negative electrode.
[0133] (1M) According to the method for producing a doped electrode of the present disclosure, it is possible to achieve a desired doping amount in the pre-doping step while suppressing lithium precipitation.
[0134] (1N) According to the method for producing a doped electrode of the present disclosure, it is possible to produce a doped electrode that has a desired initial Coulombic efficiency when used as an electrode.
[0135] 7. Example 1 (7-1) Preparation of electrode 1 A negative electrode slurry was obtained by thoroughly mixing a composition consisting of 1 part by mass of SiO3, 62 parts by mass of artificial graphite, 4 parts by mass of acetylene black powder, 2 parts by mass of SBR binder, 1 part by mass of carboxymethyl cellulose, and 85 parts by mass of ion-exchanged water using a planetary mixer. Acetylene black corresponds to a conductive agent.
[0136] A current collector 3 was prepared. In Example 1, the current collector 3 was a negative electrode current collector. The size of the current collector 3 was 150 mm in width, 300 mm in length, and 10 μm in thickness. The surface roughness Ra of the current collector 3 was 0.1 μm. The current collector 3 was made of copper foil.
[0137] The negative electrode slurry was applied to both sides of the current collector 3 using a doctor blade comma coater. As a result, as shown in Fig. 2, active material layers 5 were formed on both sides of the current collector 3. In Example 1, the active material layers 5 correspond to the negative electrode active material layers.
[0138] Next, it was dried under reduced pressure for 12 hours at 120° C. Next, the current collector 3 and the active material layer 5 were pressed using a roll press machine to obtain an electrode 1. In Example 1, the electrode 1 corresponds to a negative electrode for an electricity storage device.
[0139] The total weight of the active material layers 5 formed on both sides of the electrode 1 is 120 g / m 2 The total thickness of the active material layers 5 formed on both sides of the electrode 1 was 80 μm. As shown in FIG. 1, the active material layers 5 were formed along the longitudinal direction of the current collector 3. The active material layers 5 were formed in the center of the current collector 3 in the width direction, over a width of 120 mm. The active material layer unformed portions 7 at both ends of the current collector 3 in the width direction each had a length of 15 mm. The active material layer unformed portions 7 are portions where the active material layers 5 are not formed.
[0140] (7-2) Creation of a simple doped electrode manufacturing device 339 An electrode specimen 301 shown in FIG. 9 was cut out from the electrode 1. The electrode specimen 301 had a rectangular main body 303 and a protruding portion 305. The main body 303 was a portion of the electrode 1 that was cut out from the active material layer forming portion 6. The length of the short side of the main body 303 was 26 mm. The length of the long side of the main body 303 was 40 mm.
[0141] Protruding portion 305 was a portion of electrode 1 cut out from portion 7 where no active material layer was formed. Protruding portion 305 was connected to a short side of main body portion 303. Lead 307 was attached to protruding portion 305. Lead 307 had a thickness of 0.1 mm. Lead 307 had a width of 3 mm. Lead 307 had a length of 50 mm. Lead 307 was made of stainless steel SUS316.
[0142] Two Teflon plates 309 shown in Fig. 10 were prepared. The basic shape of the Teflon plates 309 was rectangular. The length of the short side of the Teflon plate 309 was 80 mm. The length of the long side of the Teflon plate 309 was 90 mm. The thickness of the Teflon plate 309 was 1 mm. The material of the Teflon plate 309 was polytetrafluoroethylene.
[0143] The Teflon plate 309 had a rectangular opening 311 in the center. The opening 311 penetrated the Teflon plate 309 in the thickness direction. The length of the short side of the opening 311 was 24 mm. The length of the long side of the opening 311 was 37 mm.
[0144] Two Teflon plates 309 were placed on both sides of electrode test piece 301. As shown in FIG. 10, the outer peripheral portion of main body 303 was sandwiched between two Teflon plates 309. The rest of main body 303 except for the outer peripheral portion was exposed through opening 311. Lead 307 passed through the gap between two Teflon plates 309 and protruded in the outer peripheral direction of two Teflon plates 309. A member constituted by electrode test piece 301, two Teflon plates 309, and lead 307 was used as electrode unit 312.
[0145] A stainless steel plate 313 shown in Figs. 11 and 12 was prepared. The basic shape of the stainless steel plate 313 was rectangular. The length of the short side of the stainless steel plate 313 was 80 mm. The length of the long side of the stainless steel plate 313 was 90 mm. The thickness of the stainless steel plate 313 was 4 mm. The material of the stainless steel plate 313 was stainless steel.
[0146] Stainless steel plate 313 had a recess 315 in the center on one side. When viewed in the thickness direction of stainless steel plate 313, recess 315 had a rectangular shape. The length of the short side of recess 315 was 14 mm. The length of the long side of recess 315 was 37 mm. The depth of recess 315 was 0.3 mm.
[0147] The stainless steel plate 313 had two screw holes 317. The screw holes 317 penetrated the stainless steel plate 313 in the thickness direction. The position of the screw holes 317 was shifted 6 mm from the short side of the recess 315 toward the outer periphery of the stainless steel plate 313. The diameter of the screw holes 317 was 6 mm.
[0148] 12, a Teflon tube connector 319 was attached to the screw hole 317. A fluororubber tube 321 was connected to the tube connector 319. The inner diameter of the fluororubber tube 321 was 3 mm. The fluororubber tube 321 was located on the opposite side to the recessed portion 315 when viewed from the stainless steel plate 313.
[0149] A lithium metal plate 323 shown in Figures 11 and 12 was prepared. The shape of the lithium metal plate 323 was rectangular. The length of the short side of the lithium metal plate 323 was 26 mm. The length of the long side of the lithium metal plate 323 was 40 mm. The thickness of the lithium metal plate 323 was 0.06 mm. As shown in Figures 11 and 12, the lithium metal plate 323 was attached inside the recess 315.
[0150] A Teflon plate 325 shown in Fig. 13 was prepared. The basic shape of the Teflon plate 325 was rectangular. The length of the short side of the Teflon plate 325 was 80 mm. The length of the long side of the Teflon plate 325 was 90 mm. The thickness of the Teflon plate 325 was 1 mm. The material of the Teflon plate 325 was polytetrafluoroethylene.
[0151] Teflon plate 325 had an opening 327 in its center. Opening 327 penetrated Teflon plate 325 in the thickness direction. Opening 327 had a rectangular main body 329 and a notch 331. The length of the short side of main body 329 was 24 mm. The length of the long side of main body 329 was 37 mm. Notch 331 extended from the short side of main body 329 toward the outer periphery of Teflon plate 325.
[0152] 12, Teflon plate 325 was placed on the surface of stainless steel plate 313 on the side where recess 315 was formed. Main body 329 was located so as to overlap lithium metal plate 323 when viewed from the thickness direction. Therefore, lithium metal plate 323 was not covered by Teflon plate 325. Cutout portion 331 was located so as to overlap screw hole 317 when viewed from the thickness direction. Therefore, screw hole 317 was not covered by Teflon plate 325.
[0153] A member constituted by the stainless steel plate 313 , the tube connector 319 , the fluororubber tube 321 , the lithium metal plate 323 , and the Teflon plate 325 was used as a counter electrode unit 333 .
[0154] A spacer 335 shown in Fig. 14 was prepared. The basic shape of the spacer 335 was rectangular. The length of the short side of the spacer 335 was 80 mm. The length of the long side of the spacer 335 was 90 mm. The thickness of the spacer 335 was 4 mm. The material of the spacer 335 was stainless steel.
[0155] The spacer 335 had a rectangular opening 337 in the center. The opening 337 penetrated the spacer 335 in the thickness direction. The length of the short side of the opening 337 was 34 mm. The length of the long side of the opening 337 was 42 mm.
[0156] 15, the electrode unit 312, two spacers 335, and two counter electrode units 333 were stacked and fixed together to obtain a simple doped electrode manufacturing apparatus 339. In the simple doped electrode manufacturing apparatus 339, the counter electrode unit 333 was provided opposite the electrode unit 312.
[0157] (7-3) Fabrication of doped electrodes The dope solution was supplied from the lower fluororubber tube 321 into the simple doped electrode manufacturing apparatus 339, and the same amount of the dope solution was sucked out from the upper fluororubber tube 321, so that the dope solution was made to flow. The flow rate of the dope solution was 0.37 ml / sec. Inside the simple doped electrode manufacturing apparatus 339, the cross-sectional area of the portion where the dope solution flows was 1.84 cm2. 2 The average flow velocity J of the dope solution was 0.2 cm / sec. The average flow velocity J is a value obtained by dividing the flow rate of the dope solution by the cross-sectional area of the portion where the dope solution flows. The temperature of the dope solution was 25° C. The supplied dope solution contacted the electrode test piece 301 while flowing between the counter electrode unit 333 and the electrode test piece 301. The flow direction of the dope solution was approximately parallel to the surface of the electrode test piece 301.
[0158] The doping solution was a solution containing 1.2 M LiPF6. The solvent of the doping solution was a mixed solvent containing ethylene carbonate, 1-fluoroethylene carbonate, and ethyl methyl carbonate in a volume ratio of 1:2:7.
[0159] Next, the electrode unit 312 and the counter electrode unit 333 were connected to a DC power supply equipped with a current / voltage monitor.
[0160] Next, the current density per unit area on both sides of the negative electrode is 20 mA / cm 2A current of 0.42 A was passed so as to dope the electrode with lithium.
[0161] The current flow time was set to the time when the doped ratio of lithium per unit area was 20% of the discharge capacity per unit area of the negative electrode. However, if the voltage exceeded a certain value during the current flow time, the current flow was stopped. The discharge capacity equivalent to the doped ratio of lithium per unit area was set as the target doping amount.
[0162] Through the above steps, the negative electrode active material in active material layer 5 was doped with lithium, and electrode specimen 301 became a doped electrode. In this example and in Examples 2 to 15 and Comparative Examples 1 to 5 described below, the doped electrode was an electricity storage device negative electrode, and was an lithium ion secondary battery negative electrode. (7-4) Evaluation of doped electrodes A rectangular test sample was cut out from the doped electrode. The length of the short side of the test sample was 1.5 cm. The length of the long side of the test sample was 2.0 cm. The area of the test sample was 3.0 cm. 2 It was.
[0163] A counter electrode for the measurement sample was prepared. The shape of the counter electrode was rectangular. The length of the short side of the counter electrode was 1.5 cm. The length of the long side of the counter electrode was 2.0 cm. The area of the counter electrode was 3.0 cm. 2 The thickness of the counter electrode was 200 μm. The material of the counter electrode was metallic lithium.
[0164] A separator was prepared. The thickness of the separator was 50 μm. The material of the separator was a polyethylene nonwoven fabric.
[0165] A coin-shaped cell for evaluating the negative electrode was prepared using the measurement sample, a separator, a reference electrode, and an electrolyte. In the coin-shaped cell, the counter electrodes were arranged on both sides of the measurement sample via a separator. The reference electrode was a metallic lithium plate. The electrolyte contained 1.4M LiPF6. The solvent of the electrolyte was a mixed solution containing ethylene carbonate, 1-fluoroethylene carbonate, and ethyl methyl carbonate in a volume ratio of 1:2:7.
[0166] The obtained coin-type cell was charged to 0 V with a charging current of 4 mA. Next, constant current-constant voltage charging was performed at 0 V until the charging current was reduced to 0.4 mA, and the charge capacity was calculated. Next, constant current discharging was performed with a discharge current of 4 mA until the cell voltage reached 3.0 V, and the discharge capacity was calculated. The value obtained by dividing the discharge capacity by the charge capacity was taken as the initial coulombic efficiency.
[0167] In addition, the actual doping amount was calculated based on the difference between the obtained charge capacity and the discharge capacity of the electrode before doping. Then, the ratio of the actual doping amount to the target doping amount was calculated. The above results are shown in Tables 1 and 2.
[0168] [Table 1]
[0169] [Table 2]
[0170] In Tables 1 and 2, the target doping time is the time required for doping estimated to reach the target doping amount. The target doping time is calculated from the current density and the target doping amount. The "concentration" in Tables 1 and 2 is the concentration of the electrolyte. The unit of concentration is mole / L.
[0171] 8. Examples 2 to 27 and Comparative Examples 1 to 5 Doped electrodes were manufactured and evaluated in the same manner as in Example 1, except that the temperature of the doped solution, the type of electrolyte, the current, the current density, the flow rate of the doped solution, and the average flow rate J were set to the values shown in Tables 1 and 2. In Comparative Examples 1 to 5, after the simple doped electrode manufacturing apparatus 339 was filled with the doped solution, doping was performed without supplying the doped solution. The evaluation results are shown in Tables 1 and 2.
[0172] The evaluations of the target doping time, the ratio of the actual doping amount to the target doping amount, and the initial coulombic efficiency in Tables 1 and 2 were performed based on the following criteria: In addition, the "overall evaluation" of "pass" in Tables 1 and 2 means that the evaluation results of the target doping time and the evaluation results of the ratio of the actual doping amount to the target doping amount are both rated as "○". (Evaluation criteria for target doping time) ○: Less than 100 seconds △: 100sec or more and less than 300sec ×:300sec or more (Evaluation criteria for doping ratio) ○: 70% or more △: 50% or more but less than 70% ×: Less than 50% (Initial Coulombic Efficiency Evaluation Criteria) ○: 90 or more △: 85 or more and less than 90 ×:85 or less As shown in Tables 1 and 2, each Example gave better results than each Comparative Example. It was confirmed that the same effects as each Example were obtained when a doped electrode was produced using the electrode production system 11 described in the embodiment, and the doping rate was improved. It was confirmed that lithium was precipitated in the doped electrodes of Comparative Examples 1 to 3. <Second embodiment> 1. Differences from the first embodiment The second embodiment has a basic configuration similar to that of the first embodiment, and therefore differences will be described below. Note that the same reference numerals as those in the first embodiment indicate the same configuration, and the preceding description will be referred to.
[0173] The counter electrode unit 137 has a configuration shown in Figures 16 and 17. The counter electrode units 139, 141, and 143 also have a similar configuration to the counter electrode unit 137.
[0174] The counter electrode unit 137 includes a frame 401 , a bus bar 403 , a conductive spacer 405 , a copper plate 407 , a lithium plate 409 , and a mask 411 .
[0175] Frame 401 is a box-shaped member that is open on the side of electrode 1. Frame 401 is made of polypropylene. Bus bar 403 is a conductive member. Most of bus bar 403 is housed in frame 401. One end of bus bar 403 protrudes outside frame 401. Bus bar 403 is electrically connected to a power source.
[0176] The conductive spacer 405, the copper plate 407, and the lithium plate 409 are housed in a frame 401. The lithium plate 409 is electrically connected to a power source via the copper plate 407, the conductive spacer 405, and the bus bar 403. As shown in Fig. 17, the mask 411 exposes a portion of the lithium plate 409 that faces the electrode 1, and covers the other portion.
[0177] Flow unit 201 includes nozzles 413, 415, and 417 instead of nozzles 203, 205, 207, 209, 211, 213, 215, and 217. Nozzles 413, 415, and 417 are disposed in counter electrode units 137, 139, 141, and 143, respectively. Nozzles 413, 415, and 417 are connected to pumps included in flow unit 201 by pipes 419, 421, and 423, respectively.
[0178] As shown in FIG. 16, the nozzles 413, 415, 417 are positioned between the electrode 1 and the counter electrode unit 137. The nozzles 413, 415, 417 are positioned between the lithium plate 409 and the electrode 1. The nozzles 413, 415, 417 are aligned in the vertical direction. The nozzles 413, 415, 417 each have a cylindrical shape. The axial direction of the nozzles 413, 415, 417 is horizontal and parallel to the surface of the electrode 1. As shown in FIG. 17, the nozzles 413, 415, 417, at the portions facing the electrode 1, are not covered by the mask 411.
[0179] The nozzle 413 includes a plurality of holes 431. The plurality of holes 431 are arranged at predetermined intervals along the axial direction of the nozzle 413. The positions of the plurality of holes 431 in the circumferential direction are the same. Since the axial direction of the nozzle 413 is the horizontal direction, the plurality of holes 431 are arranged along the horizontal direction. The nozzle 417 has a similar configuration to the nozzle 413.
[0180] The nozzle 415 includes a plurality of holes 431. The plurality of holes 431 are arranged at predetermined intervals along the axial direction of the nozzle 415. The circumferential positions of the plurality of holes 431 change periodically as the nozzle 415 progresses in the axial direction.
[0181] The hole 431 of the nozzle 413 and the hole 431 of the nozzle 417 suck the dope solution. The hole 431 of the nozzle 415 blows out the dope solution. As a result, the dope solution between the counter electrode unit 137 and the electrode 1 flows. In addition, the dope solution between the counter electrode unit 139 and the electrode 1, the dope solution between the counter electrode unit 141 and the electrode 1, and the dope solution between the counter electrode unit 143 and the electrode 1 also flow.
[0182] 2. Effects of the Second Embodiment According to the second embodiment, in addition to the effects of the first embodiment, the following effects are further achieved.
[0183] (2A) The holes 431 are aligned horizontally. Therefore, the flow of the doping solution is uniform in the width direction W. As a result, it is possible to manufacture a doped electrode with high in-plane uniformity while improving the doping speed in the pre-doping. <Other embodiments> Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments and can be implemented in various modified forms.
[0184] (1) As shown in Fig. 8, the electrode manufacturing system 11 may transport a wide electrode 1. As shown in Fig. 8, the electrode manufacturing system 11 includes three or more nozzles 203, three or more nozzles 205, three or more nozzles 207, and three or more nozzles 209 in an upstream tank 131 of the doping tanks 17, 19, and 21. The three or more nozzles 203 are lined up along the width direction W. The same is true for the three or more nozzles 205, the three or more nozzles 207, and the three or more nozzles 209.
[0185] The electrode manufacturing system 11 includes a plurality of counter electrode units 137, a plurality of counter electrode units 139, a plurality of counter electrode units 141, and a plurality of counter electrode units 143 in an upstream tank 131 of the doping tanks 17, 19, and 21. The plurality of counter electrode units 137 are lined up along the width direction W. The same is true for the plurality of counter electrode units 139, the plurality of counter electrode units 141, and the plurality of counter electrode units 143.
[0186] The electrode manufacturing system 11 has a similar configuration in the downstream tank 133 of the doping tanks 17, 19, and 21. The electrode manufacturing system 11 may have one dual-purpose nozzle instead of the two adjacent nozzles. The dual-purpose nozzle has two holes 231 in the circumferential direction. The dual-purpose nozzle sprays the dope solution in two directions from the two holes 231. The two directions are each toward the electrode 1. After pre-doping, the wide electrode 1 can be cut along a cut surface parallel to the longitudinal direction L to obtain multiple electrodes 1.
[0187] (2) In each of the above embodiments, the flow direction of the dope solution is a direction perpendicular to the transport direction of the electrode 1, but is not limited to this direction and may be the same as or opposite to the transport direction of the electrode 1.
[0188] (3) The function of one component in each of the above embodiments may be shared by multiple components, or the functions of multiple components may be performed by one component. Also, part of the configuration of each of the above embodiments may be omitted. Also, at least part of the configuration of each of the above embodiments may be added to or substituted for the configuration of another of the above embodiments.
[0189] (4) In addition to the above-described methods for manufacturing a doped electrode and a method for manufacturing an electricity storage device, the present disclosure can also be realized in various other forms, such as an electrode manufacturing system and a doping method.
Claims
1. 1. A method for producing a doped electrode including an active material doped with an alkali metal, comprising: a current collector; and an active material layer formed on a surface of the current collector and containing the active material, the active material being electrically doped with an alkali metal using a counter electrode unit provided opposite the electrode in a state in which a flowing dope solution containing alkali metal ions is in contact with the electrode having a strip-like form extending in a longitudinal direction; When the alkali metal is doped into the active material, the electrode is moved in the longitudinal direction in the doping solution; A method for manufacturing a doped electrode, comprising: discharging the doped solution from a nozzle located between the electrode and the counter electrode unit, thereby causing the doped solution to flow.
2. 2. A method for producing a doped electrode according to claim 1, comprising the steps of: The current density I per area of the electrode is 5 mA / cm 2 Above, 500mA / cm 2 A method for producing a doped electrode is as follows:
3. A method for producing a doped electrode according to claim 2, comprising the steps of: The current density I is 75 mA / cm 2 More than 500mA / cm 2 is as follows: A method for manufacturing a doped electrode, in which the relationship of the following formula (1) is satisfied: Formula (1) 10≦I / J≦100 (In equation (1), J is the average flow velocity of the dope solution in cm / sec.)
4. A method for producing a doped electrode according to any one of claims 1 to 3, comprising the steps of: A method for producing a doped electrode, wherein when an alkali metal is doped into the active material, the flow direction of the doping solution is approximately parallel to the surface of the electrode.
5. A method for producing a doped electrode according to claim 4, comprising the steps of: A method for manufacturing a doped electrode, wherein when an alkali metal is doped into the active material, a flow direction of the doping solution is approximately perpendicular to the longitudinal direction.
6. A method for producing a doped electrode according to any one of claims 1 to 5, comprising the steps of: The method for producing a doped electrode, wherein the temperature of the doping solution is 40° C. or higher and 100° C. or lower when the alkali metal is doped into the active material.
7. A method for producing a doped electrode according to any one of claims 1 to 6, comprising the steps of: The method for producing a doped electrode, wherein the electrolyte concentration in the dope solution is 0.8 mol / L or more and 5.0 mol / L or less.
8. A method for producing a doped electrode according to any one of claims 1 to 7, comprising the steps of: The method for producing a doped electrode, wherein the solvent of the dope solution is at least one selected from the group consisting of carbonate-based solvents, ester-based solvents, ether-based solvents, hydrocarbon-based solvents, ketone-based solvents, nitrile-based solvents, sulfur-containing solvents, and amide-based solvents.
9. A method for manufacturing an electricity storage device including an electrode cell, comprising: a negative electrode having a strip-like shape extending in a longitudinal direction, the negative electrode including a negative electrode current collector and a negative electrode active material layer formed on a surface of the negative electrode current collector and containing an active material; a counter electrode unit provided opposite the negative electrode in a state in which a flowing dope solution containing alkali metal ions is in contact with the negative electrode, and the active material is electrically doped with an alkali metal using the counter electrode unit; doping the active material with an alkali metal, and then stacking the negative electrode and an electrode different from the negative electrode to form the electrode cell; When the alkali metal is doped into the active material, the negative electrode is moved in the longitudinal direction in the doping solution; The method for manufacturing an electricity storage device includes discharging the dope solution from a nozzle located between the negative electrode and the counter electrode unit, thereby causing the dope solution to flow.
10. An electrode manufacturing system for manufacturing a doped electrode including an active material doped with an alkali metal, the electrode including a current collector and an active material layer formed on a surface of the current collector and including an active material, the electrode having a strip-like shape extending in a longitudinal direction, by performing a process of electrically doping an alkali metal into the active material using a counter electrode unit provided opposite the electrode, the electrode comprising: a doping tank containing a doping solution containing alkali metal ions and in which the treatment is carried out; a flow unit for flowing the dope solution contained in the dope tank by feeding the dope solution from a nozzle located between the electrode and the counter electrode unit; Equipped with An electrode manufacturing system that moves the electrode in the longitudinal direction in the doping solution as an alkali metal is doped into the active material.
Citation Information
Patent Citations
Step-by-step pre-lithiation method of lithium-ion battery negative plate
CN109742325A
Electrode plate processing device for secondary battery
JP1998308212A
Method and device to store lithium ion in negative electrode precursor for non-aqueous electrolyte secondary battery
JP2008077963A
Doping apparatus for manufacturing electrode of energy storage device, and electrode manufacturing method using the apparatus
JP2012049543A
Doping apparatus for manufacturing electrode of energy storage device, and electrode manufacturing method using the apparatus
JP2012049544A