Positive electrode active material, positive electrode and lithium ion battery
A mixed particle structure of nickel-rich first and second particles with a lithium-containing metal oxide interface enhances packing density and cycle characteristics in lithium ion batteries, addressing the limitations of existing active materials.
Patent Information
- Application Number
- JP2022036834
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-03-10
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2042-03-10
AI Technical Summary
Existing positive electrode active materials with aggregated particles have limited packing density and voids that can lead to cracking and decreased capacity retention, hindering the achievement of desired energy density and cycle characteristics in lithium ion batteries.
A positive electrode active material comprising a mixture of first particles with a maximum diameter of 0.5 μm or more and second particles formed by aggregating 50 or more primary particles with a maximum diameter of less than 0.5 μm, containing nickel-rich compounds and a lithium-containing metal oxide at the primary particle interface, with a porosity of 2% to 8% and a mass ratio of 20:80 to 50:50, enhancing durability and packing density.
The solution results in a high packing density of 3.7 g/cm³ or higher, providing lithium ion batteries with excellent cycle characteristics and improved durability.
Smart Images

Figure 0007556905000002 
Figure 0007556905000003 
Figure 0007556905000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode active material, and further to a positive electrode and a lithium ion battery. [Background technology]
[0002] Patent Document 1 (JP 2020-087879 A) proposes the use of a mixed active material that improves the packing density by blending single particles with agglomerated particles whose surfaces are coated with lithium tungstate or lithium borate to make the circularity distribution of the active material bimodal (two-peak distribution). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-087879 A Summary of the Invention [Problem to be solved by the invention]
[0004] Positive electrodes using positive active materials containing aggregated particles with voids have excellent cycle characteristics, but the packing density is 3.7 g / cm 3 If the density is more than this, the particles may crack, and the capacity retention rate after cycling may decrease. Even when agglomerated particles with voids are blended with single particles, the density is 3.65 g / cm 3 In addition, the packing density can be increased only to a certain extent, and the desired energy density may not be obtained. Furthermore, the agglomerated particles described in Patent Document 1 may lose voids due to crystal growth caused by reheating.
[0005] The object of the present invention is to provide a high packing density (e.g., 3.7 g / cm 3 The object of the present invention is to provide a positive electrode active material which can provide a lithium ion battery with excellent cycle characteristics. [Means for solving the problem]
[0006] The present invention provides the following positive electrode active material, positive electrode, and lithium ion battery. [1] A positive electrode active material comprising a first particle group and a second particle group, the first particle group is composed of a plurality of first particles, the first particle comprises 1 to 10 single particles; the single particle has a first maximum dimension of 0.5 μm or more; the first maximum diameter indicates the distance between the two most distant points on the contour line of the single particle, the second particle group is composed of a plurality of second particles, the second particles include aggregated particles, the aggregated particles are formed by agglomeration of 50 or more primary particles, the primary particles have a second maximum dimension of less than 0.5 μm; the second maximum diameter indicates the distance between the two most distant points on the contour line of the primary particle, The single particle has a nickel ratio of 70 mol % or more to metal elements other than lithium, The primary particles have a nickel ratio of 75 mol % or more to metal elements other than lithium, the agglomerated particles contain a lithium-containing metal oxide at the interfaces of the primary particles, The aggregate particles have a porosity of 2% or more and 8% or less, A mass ratio of the first particle group to the second particle group is 20:80 to 50:50. [2] The positive electrode active material according to [1], wherein the monoparticles and the primary particles contain a nickel-, cobalt-, and manganese-containing compound. [3] The positive electrode active material according to [1] or [2], wherein the agglomerated particles have a breaking strength of 150 MPa or more. [4] The positive electrode active material according to any one of [1] to [3], wherein the lithium-containing metal oxide is at least one selected from the group consisting of lithium tungstate, lithium zirconate, lithium titanate, lithium aluminate, and lithium borate. [5] A positive electrode comprising a positive electrode active material layer and a substrate, the positive electrode active material layer comprising the positive electrode active material according to any one of [1] to [4]. [6] A lithium-ion battery comprising the positive electrode according to [5]. Effect of the Invention
[0007] According to the present invention, the packing density is high (e.g., 3.7 g / cm 3 As described above, a positive electrode active material that can provide a lithium ion battery with excellent cycle characteristics can be provided. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a conceptual diagram of aggregated particles in this embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a lithium ion battery according to this embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing an example of an electrode body in this embodiment. [Figure 4] FIG. 4 is a conceptual diagram showing the positive electrode in this embodiment. [Diagram 5] FIG. 5 is a schematic diagram of an agglomerated particle when the porosity is 0%. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present disclosure (hereinafter also referred to as "the present embodiment") will be described. However, the following description does not limit the scope of the claims.
[0010] <Cathode active material> The positive electrode active material includes a first particle group and a second particle group. The positive electrode active material may be substantially composed of the first particle group and the second particle group. The positive electrode active material may be composed of the first particle group and the second particle group. The first particle group is an aggregate of the first particles. The second particle group is an aggregate of the second particles. The first particles have a particle structure different from that of the second particles. The positive electrode active material of this embodiment can be used for a lithium ion battery. The lithium ion battery will be described in detail later.
[0011] The first particle group is composed of a plurality of first particles. The first particles may have any shape. The first particles may be, for example, spherical, cylindrical, or lumpy. The first particles include 1 to 10 single particles. A single particle is a relatively large grown primary particle. A single particle may form a first particle by itself. A first particle may be formed by agglomeration of 2 to 10 single particles.
[0012] In this embodiment, the "single particle" refers to a particle in which no grain boundary can be visually confirmed in a scanning electron microscope (SEM) image of the particle, and which has a first maximum diameter of 0.5 μm or more. The first maximum diameter indicates the distance between the two most distant points on the contour line of the single particle. In this embodiment, the "contour line of the particle" may be confirmed in a two-dimensional projection image of the particle, or in a cross-sectional image of the particle. The contour line of the particle may be confirmed, for example, in an SEM image of a powder, or in a cross-sectional SEM image of the particle.
[0013] The single particles may have a first maximum dimension of 0.5 μm or more, preferably a first maximum dimension of from 1 μm to 7 μm, more preferably from 2 μm to 5 μm.
[0014] The second particle group is composed of a plurality of second particles. The second particles may have any shape. The second particles may be, for example, spherical, cylindrical, clumpy, etc. The second particles include aggregated particles. The second particles may be, for example, substantially composed of aggregated particles. The second particles may be, for example, composed of aggregated particles. The aggregated particles are formed by agglomeration of 50 or more primary particles.
[0015] The aggregated particles may be formed by aggregating, for example, 100 or more primary particles. There is no upper limit to the number of primary particles in the aggregated particles. The aggregated particles may be formed by aggregating, for example, 10,000 or less primary particles. The aggregated particles may be formed by aggregating, for example, 1,000 or less primary particles. The aggregated particles may have any shape. The aggregated particles may be, for example, spherical, columnar, clumpy, etc.
[0016] A primary particle is a particle in which no grain boundary can be seen in appearance in an SEM image of the particle, and has a second maximum diameter of less than 0.5 μm. The second maximum diameter refers to the distance between the two most distant points on the contour line of the primary particle. The primary particle has a second maximum diameter of 0.05 μm to 0.5 μm, preferably a second maximum diameter of 0.05 μm to 0.3 μm. When 10 or more primary particles randomly sampled from an SEM image of one agglomerate particle have a second maximum diameter of 0.05 μm to 0.3 μm, all of the primary particles contained in the agglomerate particle are considered to have a second maximum diameter of 0.05 μm to 0.3 μm. The primary particle may have a second maximum diameter of, for example, 0.1 μm to 0.3 μm.
[0017] In this specification, the number of single particles contained in the first particle and the number of primary particles contained in the aggregated particle are measured in the SEM image of the first particle and the aggregated particle. The magnification of the SEM image is appropriately adjusted according to the size of the particle. The magnification of the SEM image may be, for example, 10000 times to 30000 times.
[0018] The first particle (single particle) and the second particle (primary particle) contain nickel. The ratio of nickel to the metal elements excluding lithium in the first particle (single particle) and the second particle (primary particle) is 70 mol% or more and 75 mol% or more, respectively, and preferably 70 mol% or more and 75 mol% or more, respectively. Either or both of the first particle (single particle) and the second particle (primary particle) may contain, for example, a nickel, cobalt and manganese-containing compound, and preferably contains nickel-cobalt-manganese composite hydroxide, more preferably lithium-nickel-cobalt-manganese composite oxide. The nickel-cobalt-manganese composite hydroxide may be obtained, for example, by a coprecipitation method or the like. The nickel-cobalt-manganese composite hydroxide is, for example, a compound represented by the general formula: Ni x Co y Mn z It may be a compound represented by (OH)2 (wherein x+y+z=1). The lithium nickel cobalt manganese composite oxide may have a molar ratio of lithium to nickel, cobalt and manganese of, for example, 1.0-1.2:1.0.
[0019] The monoparticle may, for example, comprise a first layered metal oxide. The first layered metal oxide has the formula (1): Li 1-a1 Ni x1 Me 1 1-x1 O2(1) It is represented by: In formula (1), “a1” satisfies the relationship “−0.3≦a1≦0.3”. “x1” satisfies the relationship 0.7≦x1<1.0. "Me 1 ” is Co, Mn, Al, Zr, Ti, V, Cr, Fe, Cu, Zn, Mo, At least one selected from the group consisting of Sn, Ge, Nb, and W is shown.
[0020] The primary particles may, for example, comprise a second layered metal oxide. The second layered metal oxide has the formula (2): Li1-a2 Ni x2 Me 2 1-x2 O2(2) is represented by In formula (2), "a2" satisfies the relationship of "-0.3 ≤ a2 ≤ 0.3". "x2" satisfies the relationship of 0.75 ≤ x2 ≤ 1.0. "Me 2 " represents at least one selected from the group consisting of Co, Mn, Al, Zr, Ti, V, Cr, Fe, Cu, Zn, Mo, Sn, Ge, Nb, and W.
[0021] In formulas (1) and (2), for example, the relationship of "x1 < x2" may be satisfied.
[0022] For example, the single particle may contain at least one selected from the group consisting of LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.7 Co 0.2 Mn 0.1 O2, and LiNi 0.7 Co 0.1 Mn 0.2 O2. For example, the primary particle may contain LiNi 0.8 Co 0.1 Mn 0.1 O2.
[0023] For example, both the single particle and the primary particle may consist essentially of LiNi 0.8 Co 0.1 Mn 0.1 O2.
[0024] The agglomerated particles contain a lithium-containing metal oxide at the interface of the primary particles inside. The agglomerated particles contain a lithium-containing metal oxide at the interface of the primary particles inside, which tends to improve the durability of the battery. The lithium-containing metal oxide is, for example, at least one selected from the group consisting of lithium tungstate, lithium zirconate, lithium titanate, lithium aluminate, and lithium borate. Among them, lithium borate is preferred.
[0025] The aggregated particles may have the entire surface coated with the lithium-containing metal oxide, or the surface of the second particle (primary particle) may be coated with the lithium-containing metal oxide, or the surface of the first particle (single particle) may be coated with the lithium-containing metal oxide.
[0026] The agglomerated particles have a porosity of 2% or more and 8% or less. When the agglomerated particles have a porosity in the above range, the lithium-containing metal oxide tends to be easily contained in the primary particle interface, and a decrease in particle breaking strength tends to be easily suppressed. The porosity of the agglomerated particles is preferably 2% or more and 6% or less. The particle breaking strength of the agglomerated particles may be, for example, 149 MPa or more, and is preferably 150 MPa or more and 154 MPa or less. The porosity and particle breaking strength of the agglomerated particles are determined according to the method described in the Examples section below.
[0027] The agglomerated particles can be obtained, for example, by mixing a lithium source such as lithium hydroxide with a nickel-cobalt-manganese composite hydroxide, calcining the mixture to obtain a lithium-nickel-cobalt-manganese composite oxide having an agglomerated structure, and then adding a metal oxide to the mixture and subjecting it to a heat treatment. The porosity can be adjusted to the above range by adjusting the calcination temperature and heat treatment temperature. The first particles (single particles) can be obtained, for example, by dry-pulverizing and drying the lithium-nickel-cobalt-manganese composite oxide having the agglomerated structure using a jet mill or the like.
[0028] Fig. 1 shows a schematic cross-sectional view of an agglomerated particle. Agglomerated particle 10 shown in Fig. 1 is composed of a plurality of primary particles 11. Agglomerated particle 10 is coated with lithium-containing metal oxide 12. Agglomerated particle 10 has voids 13 therein. Agglomerated particle 10 contains lithium-containing metal oxide 12 at the interfaces of primary particles 11 inside.
[0029] The mass ratio of the first particle group to the second particle group is 20:80 to 50:50. By having the mass ratio of the first particle group to the second particle group in the above range, the durability of the battery tends to be easily improved. The mass ratio of the first particle group to the second particle group is preferably 20:80 to 30:70.
[0030] <Lithium-ion battery> Fig. 2 is a schematic diagram showing an example of a lithium ion battery in this embodiment. The battery 100 shown in Fig. 2 is a lithium ion battery. The battery 100 may be an in-vehicle prismatic lithium ion battery such as a main power source or a power source for power assist in an electric vehicle, for example.
[0031] The battery 100 includes an exterior body 90. The exterior body 90 houses an electrode assembly 50 and an electrolyte (not shown). The electrode assembly 50 is connected to a positive electrode terminal 91 by a positive electrode current collecting member 81. The electrode assembly 50 is connected to a negative electrode terminal 92 by a negative electrode current collecting member 82. FIG. 3 is a schematic diagram showing an example of an electrode assembly in this embodiment. The electrode assembly 50 is of a wound type. The electrode assembly 50 includes a positive electrode 20, a separator 40, and a negative electrode 30. That is, the battery 100 includes a positive electrode 20. The positive electrode 20 includes a positive electrode active material layer 22 and a positive electrode substrate 21. The negative electrode 30 includes a negative electrode active material layer 32 and a negative electrode substrate 31.
[0032] <Positive electrode> 4, the positive electrode 20 may have a positive electrode active material layer 22 formed directly on only one side of a positive electrode substrate 21. An intermediate layer (not shown) may be formed between the positive electrode active material layer 22 and the positive electrode substrate 21. The positive electrode active material layer 22 may be formed on both sides of the positive electrode substrate 21. The positive electrode substrate 21 may be a conductive sheet made of, for example, an Al alloy foil, a pure Al foil, or the like.
[0033] The positive electrode active material layer 22 includes a positive electrode active material including first particles 14 and second particles 15. The first particles 14 include single particles. The second particles 15 include aggregated particles. The positive electrode active material layer 22 may further include a conductive material (not shown) and a binder (not shown) in addition to the positive electrode active material.
[0034] The positive electrode active material layer 22 may have a thickness of, for example, 10 μm to 200 μm. The positive electrode active material layer 22 may have a high density. The positive electrode active material layer 22 may have a density of, for example, 3.7 g / cm. 3 It may have a density of 3.8 g / cm or more. 3 It may have a density of 3.9 g / cm or more. 3 The upper limit of the density is arbitrary. The positive electrode active material layer 22 may have a density of, for example, 4.0 g / cm 3 It may have the following densities: EXAMPLES
[0035] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified. The following description does not limit the scope of the claims.
[0036] [Porosity] The porosity Vp was calculated as a volume percentage according to the formula: Vp = (1 - Dp / D0) × 100 (%), using the particle density Dp of the positive electrode active material powder measured based on a constant volume expansion method using an Accupyc II 1340 manufactured by Micromeritics Corporation and the theoretical density D0 calculated from the crystal lattice constant of the same powder.
[0037] [Particle breaking strength] The breaking strength of the agglomerated particles was measured in accordance with JIS Z 8844 using a Shimadzu Corporation micro-compression testing machine MCT-501. While observing under a microscope, a single agglomerated particle of approximately the same size as the average particle diameter D50 (=12 μm) was pressed with a flat indenter of 50 μm diameter, and the ss curve indicating the breaking behavior was measured from the displacement and test force. The particle breaking strength at the time of particle crushing was calculated by calculating the average of 10 measurements.
[0038] [Preparation of active material A1 with aggregate structure] Obtained by coprecipitation, with the composition Ni 0.8 Co 0.1 Mn 0.1 Nickel-cobalt-manganese composite hydroxide (OH)2 was subjected to a primary heat treatment at 450°C for 5 hours in air to produce an oxide. After cooling, it was mixed with lithium hydroxide to obtain a predetermined Li / Me ratio, and then calcined at 770°C for 10 hours in an oxygen atmosphere to obtain a lithium composite oxide powder (active material A1) with an aggregated particle structure. Active material A1 had no internal voids and had a porosity of 0%. Figure 5 shows a schematic diagram of aggregated particles when the porosity is 0%.
[0039] [Preparation of active material A2 with aggregate structure] A lithium composite oxide powder (active material A1) having an aggregated particle structure was mixed with 1 at % of boric acid and heat-treated at 200° C. for 3 hours to obtain an active material A2 coated with lithium borate.
[0040] [Preparation of active material A3 with aggregate structure] Obtained by coprecipitation, with the composition Ni 0.8 Co 0.1 Mn 0.1 The nickel-cobalt-manganese composite hydroxide (OH)2 was subjected to a primary heat treatment at 450°C for 1 hour in air to produce an oxide, which was then cooled and mixed with lithium hydroxide to obtain a specified Li / Me ratio, and calcined at 750°C for 10 hours in an oxygen atmosphere to obtain a lithium composite oxide with an aggregated particle structure. The porosity of the resulting powder with a secondary particle structure was 5% depending on the primary heat treatment.
[0041] The obtained active material particles having an aggregated particle structure were mixed with 1 at % of boric acid and heat-treated at 300° C. for 3 hours to obtain active material A3 coated with lithium borate.
[0042] [Preparation of active materials A4 to A6 with aggregate structure] Nickel-cobalt-manganese composite hydroxide was heated at 500℃ and 550℃. ,ohLithium composite oxides (A4 to A6) with an aggregated particle structure were obtained in the same manner as in the preparation of active material A3, except that the primary heat treatment was performed at 650° C. and 650° C. The porosities of the obtained powders with secondary particle structure were 2%, 6%, and 12%, respectively.
[0043] [Preparation of active materials A7 and A8 with aggregated structure] Active materials A7 and A8 were prepared by coating the surfaces of the same aggregated particles as in Example 1 with lithium tungstate and lithium aluminate in place of the lithium borate.
[0044] [Preparation of active material B with single particle structure] Obtained by coprecipitation, with the composition Ni 0.8 Co 0.1 Mn 0.1 The nickel-cobalt-manganese composite hydroxide (OH)2 was calcined at 500°C to obtain the nickel-cobalt-manganese composite oxide (Z1).
[0045] Next, lithium hydroxide and nickel-cobalt-manganese composite oxide (Z1) were mixed so that the molar ratio of Li to the total amount of Ni, Co, and Mn was 1.05:1, and the mixture was fired in an oxygen atmosphere at 850°C for 72 hours, then wet-pulverized in a ball mill and dried to form a single particle structure, and again heat-treated in an oxygen atmosphere at 750°C for 10 hours to obtain a lithium composite oxide (B) with a single particle structure. Note that when the particle size distribution of the lithium composite oxide (B) was measured, the particle diameter (D50) was 3.3 μm, and when the structure was observed by SEM, the composite oxide (B) was almost a particle with a single particle structure, and the particle diameter was 2.3 to 3.5 μm.
[0046] <Examples 1 to 6 and Comparative Examples 1 to 4> [Mixture of single particles and agglomerated particles] The active materials A1 to A8 with the aggregated structure and the active material B with the single particle structure were weighed out in a predetermined weight ratio (mixing ratio 80:20) and uniformly mixed in a rocking mixer to obtain the positive electrode active materials C1 to C8. Similarly, the positive electrode active materials C9 to C11 were also produced by mixing the active material A3 with the aggregated structure and the active material B with the single particle structure in ratios of 10:90, 50:50, and 60:40, respectively.
[0047] [Preparation of positive electrode plate] The positive electrode active materials C1 to C11, acetylene black, and polyvinylidene fluoride (PVdF) were mixed in a solid content mass ratio of 96.3:2.5:1.2, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added, followed by kneading to prepare a positive electrode composite slurry. The positive electrode composite slurry was applied to both sides of a 13 μm-thick aluminum foil core No. 1C32, the coating was dried, and then the coating was rolled using a rolling machine until the composite density of the coating became 3.7 g / cm. 3 (3.65 for Example 5 only) and cut to a predetermined electrode size to obtain a positive electrode having a positive electrode mixture layer formed on both sides of the positive electrode core.
[0048] [Making small lithium-ion batteries] The above positive electrode was placed opposite a carbon negative electrode through a separator, and a 1.1MPF6 EC / EMC / DMC(343)+VC2% electrolyte was poured into the battery to prepare a small laminated battery. The initial charge / discharge capacity was confirmed in a thermostatic chamber at 25°C under the conditions of 0.3C rate 4.2V CVCC charge and 2.5V cut discharge, and the battery was charged and discharged 1000 times under the cycle conditions of 0.5C rate 4.2V CVCC charge and 3.0V discharge. The discharge capacity was obtained again from a charge / discharge test at 0.3C rate, and the capacity retention rate was calculated by comparing with the initial capacity value. The results are shown in Table 1.
[0049] [Table 1] [Explanation of symbols]
[0050] 10, 60 agglomerated particles, 11 primary particles, 12 lithium-containing metal oxide, 13 voids, 14 first particles, 15 second particles, 20 positive electrode, 21 positive electrode substrate, 22 positive electrode active material layer, 30 negative electrode, 31 negative electrode substrate, 32 negative electrode active material layer, 40 separator, 50 electrode body, 81 positive electrode current collecting member, 82 negative electrode current collecting member, 90 exterior body, 91 positive electrode terminal, 92 negative electrode terminal, 100 battery (lithium ion battery).
Claims
1. A positive electrode active material including a first particle group and a second particle group, the first particle group is composed of a plurality of first particles, the first particle comprises 1 to 10 single particles; the single particle has a first maximum diameter of 0.5 μm or more; the first maximum diameter indicates the distance between the two most distant points on the contour line of the single particle, the second particle group is composed of a plurality of second particles, the second particles include aggregated particles, the aggregated particles are formed by agglomerating 50 or more primary particles, the primary particles have a second maximum dimension of less than 0.5 μm; the second maximum diameter indicates the distance between the two most distant points on the contour line of the primary particle, The single particle has a nickel ratio of 70 mol % or more to metal elements other than lithium, The primary particles have a nickel ratio of 75 mol % or more to metal elements other than lithium, the agglomerated particles contain a lithium-containing metal oxide at the interfaces of the primary particles, The aggregate particles have a porosity of 2% or more and 8% or less, A mass ratio of the first particle group to the second particle group is 20:80 to 50:
50.
2. 10. The cathode active material of claim 1, wherein the monoparticles and the primary particles comprise a nickel, cobalt and manganese-containing compound.
3. The positive electrode active material according to claim 1 or 2, wherein the agglomerated particles have a breaking strength of 150 MPa or more.
4. The positive electrode active material according to any one of claims 1 to 3, wherein the lithium-containing metal oxide is at least one selected from the group consisting of lithium tungstate, lithium zirconate, lithium titanate, lithium aluminate, and lithium borate.
5. A positive electrode comprising a positive electrode active material layer and a substrate, the positive electrode active material layer comprising the positive electrode active material according to any one of claims 1 to 4.
6. A lithium ion battery comprising the positive electrode of claim 5.
Citation Information
Patent Citations
Positive electrode active material for nonaqueous electrolyte secondary battery, manufacturing method thereof, and nonaqueous electrolyte secondary battery
JP2017084628A
Lithium metal composite oxide powder, positive electrode active material for lithium secondary cell, positive electrode for lithium secondary cell, and lithium secondary cell
JP2018095523A
Lithium metal composite oxide powder, positive electrode active material for lithium secondary battery, positive electrode, and lithium secondary battery
JP2020087879A
Secondary battery active material
WO2021025479A1
Non-aqueous electrolyte secondary battery
WO2021059857A1