Positive electrode active material, positive electrode and method for producing the same, and lithium ion battery
The positive electrode active material with surface-coated boron- or tungsten-containing compounds addresses the issue of gas generation and particle breakage, enhancing battery performance by improving filling properties and reducing resistance.
Patent Information
- Application Number
- JP2022036836
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-03-10
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2042-03-10
AI Technical Summary
Lithium tungsten compounds segregate at grain boundaries of primary particles due to lattice constant mismatch, increasing specific surface area and leading to gas generation, while aggregated particles are prone to breakage, affecting battery performance.
A positive electrode active material comprising single and aggregated particles with surface-coated boron- or tungsten-containing compounds, achieving a sphericity of 0.91 or more, and a fluidity index of 3.25 or more, with a specific mass ratio, to enhance filling properties and suppress gas generation.
The solution effectively suppresses gas generation during high-temperature storage, improving battery performance by enhancing filling properties and reducing resistance.
Smart Images

Figure 0007556906000006 
Figure 0007556906000007 
Figure 0007556906000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode active material, and further to a positive electrode and a lithium ion battery. [Background technology]
[0002] Patent Document 1 describes that the surfaces of primary particles of a positive electrode active material composed of secondary particles having internal voids are coated with a lithium tungsten compound, WO3. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-084628 A Summary of the Invention [Problem to be solved by the invention]
[0004] In order to reduce the positive electrode resistance of the battery, improve the output characteristics, and achieve a high energy density, it is effective to increase the particle size of the lithium nickel composite oxide particles, increase the voids inside the particles in the cross-sectional area of the lithium nickel composite oxide particles, and use a lithium nickel composite oxide doped with tungsten. However, lithium tungsten compounds tend to segregate at the grain boundaries of primary particles due to a mismatch in lattice constants, which may increase the specific surface area and lead to gas generation. On the other hand, although it has been considered to mix agglomerated particles with single particles as a positive electrode active material in order to improve the packing property, the single particles tend to easily become the starting point for destroying the agglomerated particles.
[0005] An object of the present invention is to provide a non-aqueous electrolyte secondary battery in which gas generation during high-temperature storage is suppressed. [Means for solving the problem]
[0006] The present invention provides the following positive electrode active material, positive electrode and method for producing the same, and lithium ion battery. [1] A positive electrode active material comprising single particles and agglomerated particles formed by agglomeration of primary particles, the single particles containing a boron-containing compound or a tungsten-containing compound on a surface thereof, the single particles having a sphericity of 0.91 or more, a flowability index (FI) of the positive electrode active material measured by a powder bed shear test of 3.25 or more, and a mass ratio of the single particles to the agglomerated particles of 20:80 to 60:40. [2] The positive electrode active material according to [1], wherein the single particles contain a nickel, cobalt, and manganese-containing compound and have a nickel content ratio with respect to the metal elements excluding lithium of 60 mol % or more, and the agglomerated particles contain a nickel, cobalt, and manganese-containing compound and have a nickel content ratio with respect to the metal elements excluding lithium of 70 mol % or more. [3] The positive electrode active material according to [1] or [2], wherein the boron-containing compound is lithium borate and the tungsten-containing compound is lithium tungstate. [4] The positive electrode active material according to any one of [1] to [3], wherein the flowability index (FI) is 3.25 or more and 8.0 or less. [5] A positive electrode comprising a positive electrode active material layer containing the positive electrode active material according to any one of [1] to [4] and a substrate. [6] A lithium-ion battery comprising the positive electrode according to [5]. [7] A method for producing a positive electrode, comprising: preparing a positive electrode slurry containing the positive electrode active material according to [1]; applying the positive electrode slurry to a surface of a positive electrode substrate to form a positive electrode active material layer; and rolling the positive electrode active material layer and the positive electrode substrate to produce a positive electrode. [8] The method for producing a positive electrode according to [7], further comprising coating a surface of a base material with a boron-containing compound or a tungsten-containing compound and adjusting the sphericity to obtain the single particles. Effect of the Invention
[0007] According to the present invention, it is possible to provide a nonaqueous electrolyte secondary battery in which gas generation during high-temperature storage is suppressed. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a first explanatory diagram of the powder bed shear test. [Diagram 2] FIG. 2 is a second explanatory diagram of the powder bed shear test. [Diagram 3] FIG. 3 is a schematic diagram showing an example of a lithium ion battery according to this embodiment. [Figure 4] FIG. 4 is a schematic diagram showing an example of an electrode body in this embodiment. [Diagram 5] FIG. 5 is a conceptual diagram showing the positive electrode in this embodiment. [Figure 6] FIG. 6 is a schematic flowchart of a method for producing a positive electrode in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present disclosure (hereinafter also referred to as "the present embodiment") will be described. However, the following description does not limit the scope of the claims.
[0010] <Cathode active material> The positive electrode active material includes single particles and aggregated particles in which primary particles are aggregated. The positive electrode active material may be substantially composed of single particles and aggregated particles. The positive electrode active material of this embodiment may be for a lithium ion battery. The lithium ion battery will be described in detail later.
[0011] The single particles and the aggregated particles may have any size. The average particle size D50 of the single particles may be, for example, 1 μm or more and 20 μm or less, preferably 1 μm or less and 10 μm or less, and more preferably 1 μm or more and 5 μm or less. The average particle sizes D50, D70, and D30 of the aggregated particles may be, for example, 1 μm or less and 40 μm or less, preferably 1 μm or less and 30 μm or less, and more preferably 1 μm or more and 20 μm or less. The average particle sizes D50, D70, and D30 represent particle sizes at which the cumulative particle volume from the small particle size side in the volume-based particle size distribution is 50%, 70%, and 30% of the total particle volume, respectively. The average particle size can be measured by a laser diffraction / scattering method.
[0012] A primary particle refers to a particle in which grain boundaries cannot be visually confirmed in an SEM image of the particle, and has an average primary particle diameter of less than 0.5 μm. The average primary particle diameter refers to the distance between the two most distant points on the contour line of the primary particle. The average primary particle diameter of the primary particles may be, for example, 0.05 μm to 0.2 μm or 0.1 μm to 0.2 μm. When 10 or more primary particles randomly extracted from an SEM image of one agglomerated particle have an average primary particle diameter of 0.05 μm to 0.2 μm, all of the primary particles contained in the agglomerated particle are considered to have an average primary particle diameter of 0.05 μm to 0.2 μm. The primary particles may have an average primary particle diameter of, for example, 0.1 μm to 0.2 μm.
[0013] The single particles and agglomerated particles (primary particles) may contain a nickel, cobalt and manganese-containing compound. The nickel content ratio of the metal elements other than lithium in the single particles and agglomerated particles (primary particles) may be, for example, 60 mol% or more and 70 mol% or more, respectively, and is preferably 70 mol% or more and 80 mol% or more, respectively. The nickel, cobalt and manganese-containing compound preferably contains nickel-cobalt-manganese composite hydroxide, more preferably lithium-nickel-cobalt-manganese composite oxide. The nickel-cobalt-manganese composite hydroxide may be obtained, for example, by a coprecipitation method or the like. The nickel-cobalt-manganese composite hydroxide is, for example, a compound represented by the general formula: Nix Co y Mn z It may be a compound represented by (OH)2 (wherein x+y+z=1). The lithium nickel cobalt manganese composite oxide may have a molar ratio of lithium to nickel, cobalt and manganese, Li:(Ni+Co+Mn), of, for example, 1.0 to 1.2:1.0.
[0014] The monoparticle may, for example, comprise a first layered metal oxide. The first layered metal oxide has the formula (1): Li 1-a1 Ni x1 Me 1 1-x1 O2(1) It is represented by: In formula (1), “a1” satisfies the relationship “−0.3≦a1≦0.3”. “x1” satisfies the relationship 0.6≦x1<1.0. "Me 1 ” is Co, Mn, Al, Zr, Ti, V, Cr, Fe, Cu, Zn, Mo, At least one selected from the group consisting of Sn, Ge, Nb, and W is shown.
[0015] The primary particles may, for example, comprise a second layered metal oxide. The second layered metal oxide has the formula (2): Li 1-a2 Ni x2 Me 2 1-x2 O2(2) It is represented by: In formula (2), “a2” satisfies the relationship “-0.3≦a2≦0.3”. “x2” satisfies the relationship 0.7≦x2≦1.0. "Me 2 ” is Co, Mn, Al, Zr, Ti, V, Cr, Fe, Cu, Zn, Mo, At least one selected from the group consisting of Sn, Ge, Nb, and W is shown.
[0016] In formulas (1) and (2), for example, the relationship “x1 < x2” may be satisfied.
[0017] For example, the single particle is LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.7 Co 0.2 Mn 0.1 O2, LiNi 0.7 Co 0.1 Mn 0.2 O2, LiNi 0.6 Co 0.3 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, and LiNi 0.6 Co 0.1 Mn 0.3 O2 and may contain at least one selected from the group consisting of. For example, the primary particle is LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.7 Co 0.2 Mn 0.1 O2, and LiNi 0.7 Co 0.1 Mn 0.2 O2 and may contain at least one selected from the group consisting of.
[0018] For example, both the single particle and the primary particle may consist essentially of LiNi 0.8 Co 0.1 Mn 0.1 O2. For example, both the single particle and the primary particle may consist essentially of LiNi 0.7 Co 0.2 Mn 0.1 O2. For example, the single particle consists essentially of LiNi 0.6 Co 0.2 Mn 0.2 O2, and the primary particle may consist essentially of LiNi 0.7 Co 0.2 Mn 0.1 O2. For example, the single particle consists essentially of LiNi 0.6 Co 0.2Mn 0.2 O2, and the primary particles are essentially LiNi 0.8 Co 0.1 Mn 0.1 It may consist of O2.
[0019] When the agglomerated particles are lithium nickel cobalt manganese composite oxide, for example, a lithium source such as lithium hydroxide and a nickel cobalt manganese composite hydroxide are mixed and fired to obtain a lithium nickel cobalt manganese composite oxide having an agglomerated structure, and then a metal oxide is added thereto and heat-treated to obtain a lithium nickel cobalt manganese composite oxide having an agglomerated structure. The single particles can be obtained, for example, by dry-pulverizing and drying the lithium nickel cobalt manganese composite oxide having the agglomerated structure using a jet mill or the like.
[0020] The single particle contains a boron-containing compound or a tungsten-containing compound on the surface. From the viewpoint of sphericity, the surface of the single particle is preferably coated with a boron-containing compound or a tungsten-containing compound. The boron-containing compound is preferably lithium borate. The tungsten-containing compound is preferably lithium tungstate. The boron-containing compound or the tungsten-containing compound contained on the surface of the single particle may be, for example, 0.1% by mass or more and 2.0% by mass or less, preferably 0.2% by mass or more and 1.0% by mass or less, based on the mass of the single particle.
[0021] Examples of methods for coating the surface of a single particle with a boron-containing compound or a tungsten-containing compound include mechanochemical treatment. Mechanochemical treatment can be, for example, a dry treatment in which a base material (particles made of lithium nickel cobalt manganese composite oxide) and a coating particle (boron or tungstic acid) are rotated at high speed in a container together with media (ZrO2 beads), and the coating particles are crushed and bonded to the surface of the base material to coat them. The ratio of the coating particles to the base material can be, for example, 0.1 at% or more and 2.0 at% or less.
[0022] The sphericity of the single particle is 0.91 or more, preferably 0.92 or more, more preferably 0.93 or more, and may be, for example, 1.00 or less, or may be 0.99 or less. The sphericity of the single particle is determined according to the method described in the Examples section below. When the sphericity of the single particle is within the above range, the packing property tends to be easily improved. The sphericity of the single particle can be adjusted, for example, by adjusting the conditions of the mechanochemical treatment described above.
[0023] The flowability index (FI) of the positive electrode active material measured by a powder bed shear test is 3.25 or more, and from the viewpoint of packing property, it is preferably 3.5 or more, more preferably 4 or more, and may be, for example, 8.0 or less. Methods for making the flowability index (FI) within the above range include, for example, selection of the type of single particles and agglomerated particles, the sphericity of single particles, the average particle size and mixing ratio of single particles and agglomerated particles, and adjustment of mixing conditions. The method for measuring the flowability index (FI) is described below.
[0024] FIG. 1 is a first explanatory diagram of a powder bed shear test. The test apparatus 200 includes a servo cylinder 210, a first load cell 220, a sample cell 230, a second load cell 240, a linear actuator 250, and a third load cell 260. The measurement target is filled into the sample cell 230. This forms a powder bed 201. The sample cell 230 is cylindrical. The sample cell 230 includes an upper cell 231 and a lower cell 232. The sample cell 230 is divided into the upper cell 231 and the lower cell 232. The servo cylinder 210 applies a load in the vertical direction (z-axis direction) to the powder. This generates a vertical stress, and the powder bed 201 is consolidated. The upper cell 231 is fixed. The linear actuator 250 moves the lower cell 232 in the horizontal direction (x-axis direction). This causes the powder bed 201 to collapse by shear.
[0025] FIG. 2 is a second explanatory diagram of the powder bed shear test. The uniaxial collapse stress f cand the maximum principal stress σ1 are derived. In the Cartesian coordinate system of FIG. 2, the vertical stress σ is the horizontal axis, and the shear stress τ is the vertical axis. First, the failure envelope YL is drawn. With the vertical stress σ applied to any surface in the powder layer 201, the shear stress τ gradually acts horizontally on that surface. The surface in the powder layer 201 begins to collapse due to the shear stress τ. This is the limit stress state. The vertical stress σ and the shear stress τ in the limit stress state are plotted. This draws the failure envelope YL. Next, the limit state line CSL is drawn. After the shear collapse, the shear stress τ changes linearly, but eventually becomes a constant value. The constant shear stress τ and the vertical stress σ at that time are plotted. This draws the limit state line CSL. The limit state line CSL is a straight line passing through the origin. The intersection of the failure envelope YL and the limit state line CSL is the limit state Cs. A Mohr's stress circle m1 is drawn, passing through the limit state Cs and tangent to the fracture envelope YL. The larger of the intersections of the Mohr's stress circle m1 and the horizontal axis is the maximum principal stress σ1. A Mohr's stress circle m2 is drawn, passing through the origin and tangent to the fracture envelope YL. The intersections of the Mohr's stress circle m2 and the horizontal axis (excluding the origin) are the uniaxial collapse stress f c The liquidity index (FI) is calculated by the formula: c =σ1 / f c ff calculated by c It can be calculated from the value of
[0026] The mass ratio of the single particles to the aggregated particles in the positive electrode active material is 20:80 to 60:40, and preferably 30:70 to 50:50. When the mass ratio of the single particles to the aggregated particles in the positive electrode active material is within the above range, the filling property tends to be easily improved.
[0027] <Lithium-ion battery> Fig. 3 is a schematic diagram showing an example of a lithium ion battery in this embodiment. The battery 100 shown in Fig. 3 may be a lithium ion battery such as a main power source or a power source for power assist of an electric vehicle.
[0028] The battery 100 includes an exterior body 90. The exterior body 90 houses an electrode assembly 50 and an electrolyte (not shown). The electrode assembly 50 is connected to a positive electrode terminal 91 by a positive electrode current collecting member 81. The electrode assembly 50 is connected to a negative electrode terminal 92 by a negative electrode current collecting member 82. FIG. 4 is a schematic diagram showing an example of an electrode assembly in this embodiment. The electrode assembly 50 is of a wound type. The electrode assembly 50 includes a positive electrode 20, a separator 40, and a negative electrode 30. That is, the battery 100 includes a positive electrode 20. The positive electrode 20 includes a positive electrode active material layer 22 and a positive electrode substrate 21. The negative electrode 30 includes a negative electrode active material layer 32 and a negative electrode substrate 31.
[0029] <Positive electrode> 5, the positive electrode 20 may have a positive electrode active material layer 22 formed directly or indirectly on one or both sides of a positive electrode substrate 21. The positive electrode substrate 21 may be, for example, a conductive sheet made of an Al alloy foil, a pure Al foil, or the like. The positive electrode active material layer 22 contains a positive electrode active material including single particles 11 and agglomerated particles 12. The positive electrode active material layer 22 may further contain a conductive material, a binder, and the like.
[0030] The positive electrode active material layer 22 may have a thickness of, for example, 10 μm to 200 μm. The positive electrode active material layer 22 may have a high density. The density of the positive electrode active material layer 22 may be, for example, 3.7 g / cm. 3 or more, 3.8 g / cm 3 or more than 3.9g / cm 3 The positive electrode active material layer 22 may have a density of, for example, 4.0 g / cm 3 It may have the following densities:
[0031] <Manufacturing method of positive electrode> The method for producing the positive electrode 20 in this embodiment includes (A) preparation of a positive electrode slurry, (B) application, and (C) rolling, as shown in FIG.
[0032] In the preparation of the positive electrode slurry (A), a positive electrode slurry containing the above-mentioned positive electrode active material is prepared. The positive electrode slurry is prepared by dispersing the positive electrode active material in a dispersion medium. The single particles and the aggregated particles can be synthesized independently, for example, by a coprecipitation method. For example, the single particles and the aggregated particles are mixed so that the flowability index (FI) is 3.25 or more. The single particles can be obtained by coating the surface of a base material with a boron-containing compound or a tungsten-containing compound and adjusting the sphericity (sphericity). The sphericity (sphericity) is adjusted as described above.
[0033] In coating (B), the positive electrode slurry is coated on the surface of the positive electrode substrate 11 to form a positive electrode active material layer 12. In rolling (C), the positive electrode active material layer 12 and the positive electrode substrate 11 are rolled to produce a positive electrode 10. A raw sheet of the positive electrode 10 is produced by rolling. The raw sheet can be cut to a predetermined planar size according to the specifications of the battery 100. EXAMPLES
[0034] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified. The following description does not limit the scope of the claims.
[0035] [Preparation of single particles No. 1 to 3] Obtained by coprecipitation, with the composition Ni 0.80 Co 0.10 Mn 0.10 The nickel-cobalt-manganese composite hydroxide (OH)2 was calcined at 500°C to obtain the nickel-cobalt-manganese composite oxide (Z1).
[0036] Next, lithium hydroxide and nickel-cobalt-manganese composite oxide (Z1) were mixed so that the molar ratio of Li to the total amount of Ni, Co, and Mn was 1.05:1, and the mixture was fired at 850°C for 72 hours in an oxygen atmosphere. The mixture was then wet-pulverized in a ball mill and dried to form a single particle structure, and was again heat-treated at 750°C for 10 hours in an oxygen atmosphere to obtain a lithium composite oxide A having a single particle structure.
[0037] When the particle size distribution of lithium composite oxide A was measured, the particle diameter (D50) was 3.3 μm. When the structure of the composite oxide A was observed by SEM, the composite oxide A was found to be composed of particles with a nearly single particle structure, with a particle diameter of 2.3 to 3.5 μm.
[0038] The obtained single-particle active material particles were placed in an agate container together with 1 at% boric acid and Φ20 mm ZrO2 beads, and mechanochemically treated for 2 hours using a planetary ball mill (P5 manufactured by Filecce). The mechanochemical treatment time is shown in Table 1.
[0039] [Preparation of single particle structure No. 4] Single particle No. 4 was obtained in the same manner as in the preparation of single particles Nos. 1 to 3, except that tungstic acid was used for the mechanochemical treatment and the time for the mechanochemical treatment was set to one hour.
[0040] [Sphericity] An arbitrary particle is selected from the SEM photograph of a single particle, and the projected area (A) and perimeter (M) of that particle are measured. If a perfect sphere with the measured perimeter (M) is assumed, its radius (r) is M / 2π, and the area (B) of the assumed perfect sphere is π×(M / 2π)2. From the areas A and B thus measured and calculated, the sphericity (A / B)=A×4π / M2 is calculated. The sphericity of 100 single particles is measured, and the average value is regarded as the sphericity. The sphericity is shown in Table 1.
[0041] [Preparation of aggregated particles] Obtained by coprecipitation, with the composition Ni 0.80 Co 0.10 Mn 0.10 A nickel-cobalt-manganese composite hydroxide of (OH)2 was baked together with lithium hydroxide in an oxygen atmosphere at 800°C for 10 hours, and then crushed in an agate mortar to obtain a lithium composite oxide (B) with an aggregated particle structure.
[0042] The particle size distribution of composite oxide B was D50 12 μm, D70 14 μm, and D30 10 μm. The cross section of composite oxide B after CP processing was observed by SEM, and the average primary particle diameter of composite oxide B was 0.13 μm.
[0043] [Mixing method of single particles and agglomerated particles] The single particles and aggregated particles were weighed out to have the mass ratio shown in Table 1, placed in a tumbling fluidized dryer, and mixed uniformly to obtain a mixed positive electrode active material powder.
[0044] [Liquidity index (FI)] The powder bed shear test was conducted in accordance with "JIS Z8835: Measurement method of critical state line (CSL) and wall yield line (WYL) by direct shear test". c was measured three or more times. The arithmetic mean of the three or more results was the ff of the measured object. c It was considered that. c (Average value) was calculated to the first decimal place, and any fractional part beyond the first decimal place was rounded off.
[0045] [Preparation of positive electrode plate] The mixed positive electrode active material powder, acetylene black, and polyvinylidene fluoride (PVdF) were mixed in a solid content mass ratio of 96.3:2.5:1.2, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added, followed by kneading to prepare a positive electrode composite slurry. The positive electrode composite slurry was applied to both sides of a 13μ thick aluminum foil core of No. 1C32, the coating was dried, and then the coating was rolled using a rolling machine until the composite density of the coating was 3.7g / cm. 3 The positive electrode core was compressed so as to have a diameter of 10 mm and then cut to a predetermined electrode size to obtain a positive electrode having a positive electrode mixture layer formed on both sides of the positive electrode core.
[0046] [Making small lithium-ion batteries] A small laminated battery was produced in combination with a carbon anode, aiming for a design of 650 WH / L. In addition, the particle structure, composition, and mixture ratio of the positive electrode active material were changed to produce batteries of the examples and comparative examples shown in the table, and the amount of gas generated before and after a 30-day storage test at 60°C was measured from the volume change obtained by the Archimedes method. The results are shown in Table 1.
[0047] [Table 1] [Explanation of symbols]
[0048] 14 single particle, 15 agglomerated particle, 20 positive electrode, 21 positive electrode substrate, 22 positive electrode active material layer, 30 negative electrode, 31 negative electrode substrate, 32 negative electrode active material layer, 40 separator, 50 electrode body, 81 positive electrode current collector, 82 negative electrode current collector, 90 exterior body, 91 positive electrode terminal, 92 negative electrode terminal, 100 battery (lithium ion battery), 200 test device, 201 powder bed, 210 servo cylinder, 220 first load cell, 230 sample cell, 231 upper cell, 232 lower cell, 240 second load cell, 250 linear actuator, 260 third load cell, 300 mixing device, 301 powder, 310 container, 320 stirring blade.
Claims
1. A positive electrode active material including single particles and aggregate particles in which the primary particles are aggregated, the single particle comprises a boron-containing compound or a tungsten-containing compound at a surface thereof; The sphericity of the single particle is 0.91 or more, The positive electrode active material has a fluidity index (F.I) of 3.25 or more as measured by a powder bed shear test; A mass ratio of the single particles to the aggregated particles is 20:80 to 60:
40.
2. The single particle contains a nickel, cobalt and manganese-containing compound, and the nickel content ratio with respect to metal elements other than lithium is 60 mol % or more; 2. The positive electrode active material according to claim 1, wherein the agglomerated particles contain a nickel, cobalt and manganese-containing compound, and the nickel content ratio to the metal elements other than lithium is 70 mol % or more.
3. 3. The positive electrode active material according to claim 1, wherein the boron-containing compound is lithium borate and the tungsten-containing compound is lithium tungstate.
4. The positive electrode active material according to any one of claims 1 to 3, wherein the fluidity index (FI) is 3.25 or more and 8.0 or less.
5. A positive electrode comprising a positive electrode active material layer containing the positive electrode active material according to any one of claims 1 to 4 and a substrate.
6. A lithium ion battery comprising the positive electrode of claim 5.
7. A method for producing a positive electrode, comprising the steps of: Preparing a cathode slurry comprising the cathode active material of claim 1; applying the positive electrode slurry to a surface of a positive electrode substrate to form a positive electrode active material layer; and, producing a positive electrode by rolling the positive electrode active material layer and the positive electrode substrate; Including, A method for manufacturing a positive electrode.
8. The method for producing a positive electrode according to claim 7, further comprising: coating a surface of a base material with a boron-containing compound or a tungsten-containing compound to adjust the sphericity to obtain the single particles.
Citation Information
Patent Citations
Positive electrode active material for nonaqueous electrolyte secondary battery, manufacturing method thereof, and nonaqueous electrolyte secondary battery
JP2017084628A
Cathode for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery
JP2021150051A
Positive electrode active material for nonaqueous electrolyte secondary battery, positive electrode and secondary battery
WO2008078784A1
Nonaqueous electrolyte secondary battery
WO2013146054A1
W-containing high-nickel ternary positive electrode material and preparation method therefor
WO2021000868A1