Optical element and method for manufacturing the same
A light-shielding film using epoxy resin and coumaron-indene resin with controlled dye migration addresses the issue of reduced dye concentration on complex optical elements, enhancing optical performance by minimizing internal reflection and ghosting.
Patent Information
- Application Number
- JP2020037250
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-04
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2040-03-04
AI Technical Summary
Existing light-shielding films on optical elements with complex shapes suffer from dye migration during drying, leading to reduced film thickness and dye concentration, which compromises light-shielding performance and increases internal reflection, causing flare and ghosting.
A light-shielding film composed of an epoxy resin, coumaron-indene resin, and a dye, with a specific composition and viscosity range, is applied and cured to maintain dye concentration and reduce internal reflection, using materials that suppress dye migration and enhance film adhesion.
The solution effectively suppresses internal reflection and maintains optical quality by preventing dye migration and ensuring uniform dye distribution, even on optical elements with complicated shapes, thereby reducing flare and ghosting.
Smart Images

Figure 0007557270000004 
Figure 0007557270000007 
Figure 0007557270000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a light-shielding film for use in optical instruments such as cameras, binoculars, and microscopes, an optical element, and a method for manufacturing an optical element. [Background technology]
[0002] The light-shielding film used in optical elements is a coating film that is mainly formed on the surface of glass. The optical element may be a lens, a prism, or other optical glass, but the light-shielding film will be explained below using a lens as an example.
[0003] As shown in FIG. 1, the light-shielding film 1 of the optical element is formed on the outer periphery of the lens 2. When light hits only the lens 2, as in the case of incident light 3, it is transmitted as transmitted light 4. In contrast, when obliquely incident light 5 is incident, the light hits the light-shielding film 1. At this time, if the light-shielding film 1 is not formed (the lower side of the lens in FIG. 1), the light 5 that hits the outer periphery of the lens 2 is internally reflected and goes outside the lens 2 as internally reflected light 6 that is unrelated to the image, causing flare and ghosting and degrading the image quality. If the light-shielding film 1 is provided (the upper side of the lens in FIG. 1), it is possible to reduce the internal reflection of the obliquely incident light 5, thereby reducing the internally reflected light 6 that adversely affects the image and making it possible to prevent flare and ghosting.
[0004] In recent years, as optical devices have become more compact and have higher performance, optical elements having more complex shapes are used in the optical systems, and the light-shielding film is also formed in a complex shape.
[0005] Patent Document 1 discloses a light-shielding film for optical elements that reduces internal reflection by absorbing light with a dye. Patent Document 2 provides an anticorrosive coating composition comprising (A) an epoxy resin, (B) an amine-based curing agent, and (C) a hydroxyl group-containing coumarone resin, the hydroxyl group-containing coumarone resin being contained in an amount of 1 to 500 parts by weight per 100 parts by weight of the epoxy resin. The anticorrosive coating composition is capable of forming a coating film having excellent seawater resistance and a light color such as gray, and can also be used for surface coating of undersea pipelines, etc., and is particularly useful for coating the inside of ships, such as ballast tanks. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2011-186437 A [Patent Document 2] International Publication No. 2007 / 129564 Summary of the Invention [Problem to be solved by the invention]
[0007] In the light-shielding film described in Patent Document 1, for example, when a light-shielding film is formed on an optical element having a complex shape with ridges 12 as shown in Fig. 3(a), a phenomenon 13 occurs in which the light-shielding paint moves during drying, and the film thickness at the ridges decreases as shown in Fig. 3(b). Furthermore, at the ridges, not only does the paint film become thinner, but the concentration of the dye for absorbing light decreases, making it difficult to achieve sufficient light-shielding performance. The dye is relatively small in size among the components in the light-shielding paint and moves at high speed within the paint components, so it selectively moves away from the ridges.
[0008] The present invention has been made in consideration of the above-described background technology, and provides an optical element having good optical characteristics by suppressing internal reflection, even when a light-shielding film is provided on a substrate of the optical element having a complex shape. [Means for solving the problem]
[0009] The optical element of the present invention is an optical element having a light-shielding film provided on a part of the outer periphery of a substrate, and is characterized in that the light-shielding film contains an epoxy resin, a resin having at least coumarone or indene (hereinafter also referred to as a "coumarone-indene-based resin"), and a dye.
[0010] The method for manufacturing an optical element of the present invention is a method for manufacturing an optical element in which a light-shielding film is provided on a part of the outer periphery of a substrate, and is characterized by having a step of applying a light-shielding paint to the outer periphery surface of the substrate, and a step of hardening the applied light-shielding paint to produce a light-shielding film. Effect of the Invention
[0011] According to the present invention, it is possible to provide an optical element having good optical characteristics that suppress flare and ghost even in an optical glass having a complex shape, a light-shielding film made of a light-shielding coating material, and a method for manufacturing the optical element. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a schematic diagram showing the travel of internally reflected light. [Diagram 2] FIG. 2 is a schematic diagram showing a light-shielding film of the optical element of the present invention. [Diagram 3] FIG. 1 is a schematic diagram showing the movement of a light-shielding paint when the paint dries. [Figure 4] FIG. 2 is a schematic diagram showing a method for measuring internal reflection. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Preferred embodiments of the present invention will now be described. The light-shielding film made of the light-shielding coating material used in the optical element of the present invention can provide an optical element having a sufficient internal reflection reducing function even in the case of optical glass having a complex shape.
[0014] The internal reflection of an optical element will be described below. Next, the configuration of the light-shielding film according to the present invention will be described. After that, the light-shielding coating material, the light-shielding film, the optical element, the method for manufacturing the light-shielding film, and the method for manufacturing the optical element according to the present invention will be described.
[0015] [Internal reflection of optical elements] First, transmitted light 10 through an optical element will be described with reference to Figure 2. Internal reflection in an optical element occurs mainly at two interfaces 7 and 8. That is, incident light 3 passes through substrate (lens) 2, and part of it becomes first reflected light 9 at interface 7 between substrate (lens) 2 and light-shielding film 1. Transmitted light 10 that passes through light-shielding film 1 is attenuated by light-shielding film 1, and then becomes second reflected light 11 at interface 8 between light-shielding film 1 and air.
[0016] The first reflected light 9 can be reduced by bringing the refractive indexes of the light-shielding film 1 and the substrate (lens) 2 closer together. The reason that bringing the refractive indexes closer together reduces the internal reflection is that, as shown in the following formula (1), the reflectance R of the interface between the light-shielding film 1 and the lens 2 is determined by the difference between the refractive index n0 of the lens 2 on the incident light 3 side and the refractive index n1 of the light-shielding film 1, and the smaller this difference is, the smaller the reflectance becomes.
number
[0017] The second reflected light 11 can be reduced by absorbing the transmitted light 10 that passes through the light-shielding film. In order to efficiently absorb the transmitted light 10 into the coating film, it is preferable to add a colorant to the light-shielding film 1 to increase the blackness of the film.
[0018] [Features of the light-shielding film of the optical element of the present invention] The light-shielding film 1 of the optical element of the present invention is characterized in that, even when formed on an optical element having ridge lines 12 as shown in Figure 3(a), it is possible to suppress a decrease in dye concentration at the ridge line portion by preventing selective migration of the dye that accompanies migration of the light-shielding paint.
[0019] In order to suppress the decrease in dye concentration even when the light-shielding film 1 according to the present invention is formed on an optical element having a ridge line 12, the light-shielding film 1 is composed of at least an epoxy resin cured by an amine-based curing agent, a dye, and at least one or more kinds of coumarone-indene resins. In this specification, the coumarone-indene resin is a resin having at least coumarone or indene, and is a coumarone and indene resin, a coumarone resin, or an indene resin. The coumarone and indene resin is a resin containing coumarone and indene as main monomer components constituting the skeleton (main chain) of the resin, and examples of monomer components contained in the skeleton other than coumarone and indene include styrene. The coumarone resin is a resin containing coumarone as a main monomer component constituting the skeleton (main chain) of the resin. The indene resin is a resin containing indene as a main monomer component constituting the skeleton (main chain) of the resin. The coumarone and indene resins are preferred because of their ease of availability.
[0020] (Technical coumarone-indene resin effect) In Patent Document 2, coumarone-indene resin is used to impart coating strength and corrosion resistance. However, the present inventors have found that the addition of coumarone-indene resin suppresses the migration of dyes during the drying process of the light-shielding paint. Since coumarone-indene resin is a resin mainly composed of coumarone and indene, which are five-membered and six-membered rings, the molecules are very bulky, and it can be presumed that the migration of dyes, which have a relatively small molecular size, can be suppressed. In addition, since coumarone and indene have good compatibility with dyes, it was found that it is possible to disperse the dyes throughout the light-shielding paint and suppress their migration. Therefore, it is possible to suppress the selective migration of dyes in the parts where the film thickness has decreased due to the movement of the light-shielding paint during painting. As a result, it was found that the concentration of the dye does not decrease even in the parts where the film thickness of the light-shielding film has decreased, and internal reflection can be effectively suppressed.
[0021] [Blackout paint] Next, the material composition of the light-shielding paint forming the light-shielding film for the optical element of the present invention will be described. Hereinafter, unless otherwise specified, the content of each material used in the light-shielding paint will be described based on the content of the light-shielding paint including the hardener.
[0022] The light-shielding coating material according to the present invention contains an epoxy resin, a coumarone-indene resin, a dye, and an amine curing agent.
[0023] The viscosity of the light-shielding coating material according to the present invention is preferably 20.0 mPa·s or more and 65.0 mPa·s or less, and more preferably 30.0 mPa·s or more and 50.0 mPa·s or less. If the viscosity of the light-shielding coating material is less than 20 mPa·s, the viscosity becomes too low and the coating material tends to move during drying, resulting in poor coatability. If the viscosity of the light-shielding coating material exceeds 65.0 mPa·s, the leveling property during coating becomes poor, and the resulting light-shielding film will have poor appearance such as streaks and unevenness.
[0024] Next, each material contained in the light-shielding coating material according to the present invention will be described. (Epoxy resin) The epoxy resin contained in the light-shielding coating material according to the present invention can be bisphenol A type, bisphenol F type, multifunctional epoxy resin, flexible epoxy resin, brominated epoxy resin, glycidyl ester type epoxy resin, polymer type epoxy resin, or biphenyl type epoxy resin. One type of epoxy resin may be used alone, or multiple types may be mixed together.
[0025] The content of the epoxy resin contained in the light-shielding coating material according to the present invention is preferably 5.0% by mass or more and 25.0% by mass or less in the light-shielding coating material. If the content of the epoxy resin is less than 5.0% by mass, the resin component in the light-shielding coating material is small, so the solvent resistance is reduced. If the content of the epoxy resin is more than 25.0% by mass, the refractive index is reduced, so the internal reflection is increased.
[0026] (Coumarone-indene resin) The coumarone-indene resin contained in the light-shielding coating material according to the present invention is a polymer using at least one of coumarone and indene, and therefore may be either a coumarone resin alone or an indene resin alone. Coumarone and indene resins are preferred in terms of availability, etc.
[0027] The content of the coumarone-indene resin is preferably 100 parts by mass or more and 300 parts by mass or less relative to 100 parts by mass of the epoxy resin. If the content is less than 100 parts by mass, the effect of suppressing the migration of the dye becomes insufficient, and if it is more than 300 parts by mass, the crosslinking ratio of the epoxy resin becomes small, causing a problem of elution from the light-shielding film.
[0028] (dye) The dye contained in the light-shielding coating material according to the present invention can be at least one type of dye. The dye can be any material that absorbs visible light with a wavelength of 400 nm to 700 nm and can be dissolved in any solvent. The dye can be one type, or several types of dyes such as black, red, yellow, and blue can be mixed.
[0029] The content of the dye is preferably 46 parts by mass or more and 115 parts by mass or less relative to 100 parts by mass of the coumarone-indene resin. If the content of the dye is less than 46 parts by mass, the light-shielding performance becomes insufficient, and if it is more than 115 parts by mass, elution of the dye from the light-shielding film becomes a problem.
[0030] (Pigments) Optical lenses generally have a high refractive index, and it is necessary to increase the refractive index of the light-shielding film in order to reduce the reflection at the interface between the light-shielding film and the optical glass. For this purpose, as described in Patent Document 1, particles with a high refractive index may be introduced as a pigment. For example, titania, zirconia, etc. may be mentioned.
[0031] Furthermore, black particles may be used as the pigment, and carbon black, titanium black, iron oxide, and copper-iron-manganese composite oxide can be used.
[0032] The number-average particle size of the pigment is preferably 5 nm or more and 200 nm or less. If the number-average particle size of the pigment is less than 5 nm, the stability of the light-shielding paint decreases. Also, if the number-average particle size of the pigment is more than 200 nm, the internal reflection increases when the light-shielding film is made.
[0033] (Amine-based hardener) The light-shielding coating material according to the present invention contains an amine-based curing agent to cure the epoxy resin contained in the light-shielding coating material. As the amine-based curing agent, linear aliphatic, polyamide, alicyclic, aromatic, and other dicyandiamide and adipic dihydrazide can be used. In addition, since the amino group of the amine-based curing agent is active, the active amino group may be protected by the structure shown in formula (2). For example, the structure shown in formula (2) becomes an active amino group by hydrolysis in the presence of water. Therefore, when the light-shielding coating material is formed, the amount of amino group is small, so that the reaction with the components in the light-shielding coating material can be suppressed.
number
[0034] The content of the amine-based curing agent contained in the light-shielding coating material according to the present invention is preferably 80 parts by mass or more and 150 parts by mass or less with respect to 100 parts by mass of the epoxy resin. If the content of the amine-based curing agent is less than 80 parts by mass, the degree of curing of the light-shielding film decreases, and the adhesion of the light-shielding film to the substrate decreases. Also, if the content of the amine-based curing agent is more than 150 parts by mass, the optical properties decrease.
[0035] (Organic solvent) The light-shielding coating material according to the present invention preferably contains an organic solvent to adjust the viscosity. The organic solvent used in the light-shielding coating material according to the present invention is not particularly limited as long as it satisfies the solubility of the epoxy resin, the colorant, and the amine-based curing agent, and the dispersibility of the pigment. As the organic solvent, propylene glycol monomethyl ether, propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, methyl isobutyl ketone, 1-butoxy-2-propanol, dipropylene glycol dimethyl ether, diethylene glycol dimethyl ether, 3-methoxybutyl acetate, 4-methoxy-4-methyl-2-pentanone, xylene, toluene, benzyl alcohol, isopropyl alcohol, acetone, and ethanol can be used. These organic solvents may be used alone or in combination.
[0036] (curing catalyst) The light-shielding coating material according to the present invention may contain a curing catalyst in order to increase the crosslink density of the epoxy resin when the light-shielding film is produced and improve the solvent resistance. As the curing catalyst used in the present invention, it is preferable to use a tertiary amine or an imidazole compound. As the tertiary amine, benzyldimethylamine, 2-(dimethylaminomethyl)phenol, 2,4,6-tris(diaminomethyl)phenol, and tri-2-ethylhexyl salt can be used. In addition, as the imidazole compound, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-methylimidazole, and 2,4-diamino-6-[2-methylimidazolyl-(1)]-ethyl S-triazine can be used.
[0037] The content of the curing catalyst contained in the light-shielding coating material according to the present invention is preferably 7.5 parts by mass or more and 35 parts by mass or less. If the content of the curing catalyst is less than 7.5 parts by mass, the solvent resistance of the light-shielding film produced may decrease. If the content of the curing catalyst is more than 35 parts by mass, the crosslink density of the light-shielding film produced may increase, and the toughness of the film may decrease.
[0038] (Coupling Agent) The light-shielding coating material according to the present invention preferably contains a coupling agent in order to improve the adhesion between the resin and the pigment when the light-shielding film is produced. Examples thereof include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2-(aminoethyl)-2-(methylaminoethyl)-1,1-dimethylethyl ... )-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, 3-isocyanatopropyltriethoxysilane.
[0039] (Plasticizer) The light-shielding coating material according to the present invention is preferably added with a plasticizer to improve the flexibility of the light-shielding film when it is produced, thereby making it less likely to crack. As the plasticizer used in the present invention, dioctyl phthalate, diisononyl phthalate, diisodecyl phthalate, dibutyl phthalate, dioctyl adipate, diisononyl adipate, trioctyl trimellitate, polyester, tricresyl phosphate, tributyl acetyl citrate, sebacic acid ester, xylene resin, epoxidized soybean oil, epoxidized linseed oil, azelaic acid ester, maleic acid ester, and benzoic acid ester can be used.
[0040] (Additives) The light-shielding coating material according to the present invention may contain additives within the range that does not impair the original purpose. The additives that can be added include a viscosity modifier, a fungicide, and an antioxidant.
[0041] [Light-shielding film] Next, the light-shielding film according to the present invention will be described. The light-shielding film according to the present invention is produced by applying the light-shielding coating material and then curing it. The light-shielding film has a composition that is the same as the composition of the light-shielding coating material except that the organic solvent is removed. That is, the light-shielding film according to the present invention contains at least an epoxy resin, a coumarone-indene resin, a dye, and an amine-based curing agent, and may contain the materials of the light-shielding coating material in addition to these. The thickness of the light-shielding film is preferably from 0.3 μm to 100 μm, and more preferably from 0.5 μm to 50 μm.
[0042] [Optical elements] The optical element of the present invention is an optical element having a light-shielding film provided on a part of the outer periphery of a substrate, the light-shielding film being the light-shielding film described above.
[0043] The glass substrate that is an optical element may be a lens or a prism. The refractive index of the glass substrate at d-line is preferably 1.60 or more and 2.00 or less, and more preferably 1.80 or more and 2.00 or less.
[0044] The optical element of the present invention can be used as an element constituting an optical instrument such as a lens, a prism, a reflecting mirror, a diffraction grating, etc. For example, it can be used as an optical element for use in any one of a camera, a binocular, a microscope, or a semiconductor exposure apparatus, and can be used as an optical element having a light-shielding film formed outside the optically effective surface.
[0045] [Method of manufacturing optical elements] The method for manufacturing an optical element of the present invention is a method for manufacturing an optical element having a light-shielding film provided on a part of the outer periphery of a substrate, and includes a step of applying a light-shielding coating to the surface of the outer periphery of the substrate, and a step of curing the applied light-shielding coating. The light-shielding coating used in the method for manufacturing an optical element of the present invention is the above-mentioned light-shielding coating. In the method for manufacturing an optical element of the present invention, the materials and conditions of the above-mentioned optical elements can be used. Each step will be described below.
[0046] (Adjustment of light-blocking paint) The light-shielding coating material used in the method for producing an optical element of the present invention is preferably prepared by mixing and dispersing the above-mentioned light-shielding coating materials. As a mixing and dispersing method, a ball mill, a bead mill, a collision dispersion device, a planetary rotary stirrer, a homogenizer, or a stirrer can be used.
[0047] When a pigment is used, it is preferable to nano-disperse it before use. Specific methods for nano-dispersion include a method of nano-dispersing it using a bead mill or a collision dispersion device. It is also possible to synthesize the pigment by a sol-gel method and nano-disperse it during synthesis, or to use a commercially available product that has already been nano-dispersed.
[0048] (Process of applying light-shielding paint) In the step of applying the light-shielding coating material, the light-shielding coating material of the present invention is applied to a part of the surface of the glass substrate.
[0049] The method for applying the light-shielding coating material can be selected from a variety of methods depending on the desired coating shape, including dipping, spin coating, slit coating, electrostatic coating, and coating methods using coating tools such as a brush, sponge, or bar coater.
[0050] (Process for hardening the light-shielding paint) In the process of curing the light-shielding paint, the applied light-shielding paint is cured. To cure the light-shielding paint, the applied light-shielding paint may be dried or baked. In order to promote the curing reaction between the epoxy resin and the curing agent used in the present invention, it is desirable to perform drying as follows. When drying, it is preferable to dry at a temperature of 20°C or more and 100°C or less, more preferably at a temperature of 40°C or more and 80°C or less, and even more preferably at a temperature of 40°C or more and 60°C or less. The drying time is preferably 10 minutes or more and 24 hours or less, more preferably 30 minutes or more and 24 hours or less, and even more preferably 1 hour or more and 24 hours or less. When baking, the temperature is preferably 40°C or more and 300°C or less, more preferably 40°C or more and 250°C or less, and even more preferably 40°C or more and 200°C or less. The baking time is preferably 10 minutes or more and 10 hours or less, and more preferably 10 minutes or more and 6 hours or less. EXAMPLES
[0051] The present invention will be specifically described below with reference to examples and comparative examples. In the examples and comparative examples, the following measurement and evaluation methods were used. In the following, "parts" refers to "parts by mass."
[0052] <Evaluation of optical properties> The internal reflectance was measured using a spectrophotometer (U-4000; Hitachi High-Tech) as shown in Figure 4. A triangular prism was used as the measurement sample. 14 indicates the prism. The triangular prism 14 has a side length of 30 mm that includes a right angle, a thickness of 10 mm, and is made of S-LaH53 (nd=1.8; manufactured by Ohara).
[0053] FIG. 4 is a schematic diagram showing a measurement method when the incident angle b to the triangular prism 14 is 90°. First, the measurement method using a spectrophotometer will be explained with reference to FIG. 4. The light emitted from the spectrophotometer is incident on the triangular prism 14 at an incident angle b=90°. At this time, refraction of the light occurs due to the difference between the refractive index of air and the refractive index (n) of the triangular prism 14. The incident angle after refraction is c=68.13°. The angle e after refraction with respect to the incident angle d was calculated from the following formula (3). The incident angle c was also calculated from e after refraction. n=sin d / sin e Equation (3)
[0054] Next, the light refracted by the triangular prism 14 hits the bottom surface of the triangular prism 14 and is reflected to exit the triangular prism 14. The intensity of this reflected light was detected by a detector in the visible light region of wavelengths from 400 nm to 700 nm. Note that the background was a sample in which nothing was applied to the bottom surface of the triangular prism 14, which had three mirror surfaces: the bottom surface, the incident surface, and the reflecting surface, and the internal reflectance was measured when the light-shielding film 1 was formed on the bottom surface of the triangular prism 14, which had three mirror surfaces: the bottom surface, the incident surface, and the reflecting surface. The internal reflectance was measured by measuring the internal reflection of visible light of wavelengths from 400 nm to 700 nm at 1 nm intervals and recording the average value of the results.
[0055] <Viscosity evaluation of light-shielding paint at 20℃> The viscosity of the light-shielding paint at a temperature of 20°C was evaluated using a tuning-fork vibration viscometer (SV-1H [product name] (manufactured by A&D Co., Ltd.)) at a constant temperature.
[0056] <Evaluation of luminance in the moving area of light-shielding paint> The coating evaluation of the dye concentration for optical elements was carried out by coating a light-shielding coating material on a flat glass (MICRO SLIDGLASS S1126 (manufactured by Matsunami Glass Industry Co., Ltd.)) and allowing the coating material to move during drying.
[0057] Specifically, two pieces of 10mm x 100mm x 0.065mm Kapton tape were attached to each end of a flat glass plate measuring 30mm x 100mm x 1mm, creating a sample with a step (0.130mm) between the flat glass plate and the Kapton tape.
[0058] A light-shielding paint for optical elements was uniformly applied to the coating area (10 mm x 100 mm x 0.196 mm) of the obtained flat plate sample using a slide star, and the brightness of the paint at the coated edge was evaluated after drying for 1 hour.
[0059] The evaluation of the luminance value was carried out by placing the sample coated on the flat glass on a white paper with the coated surface facing up, photographing the upper surface of the coated surface, and then performing image processing to compare the results. From the obtained image, the coated edge was extracted, and the luminance value was binarized to 256 gradations, and the average value was calculated to obtain the luminance value. It was confirmed that there was a linear correlation between the obtained 256 gradations of luminance and the results of internal reflection. The luminance value in Comparative Example 1 was used as a reference value, and the same processing was performed to compare the luminance values of each sample. The effects were evaluated according to the following criteria. A: The luminance value reduction effect is good, being reduced by 10% or more compared to the reference value. B: The reduction in luminance value is less than 10% compared to the reference value, which is insufficient.
[0060] <Appearance evaluation of light-shielding film> The appearance of the light-shielding film for optical elements was evaluated by forming a film having a thickness of 10 μm on a flat glass plate made of S-LaH53 (nd=1.8; manufactured by Ohara Corporation) and evaluating it according to the following criteria. A: There are no visible cracks or peeling of the light-shielding film, and the color is uniform. B: Any one of the following is visually observed: cracks in the light-shielding film, peeling of the light-shielding film, or uneven color.
[0061] Example 1 <Preparation of light-shielding paint> The light-shielding coating was prepared in the following manner. First, 100 parts of epoxy resin (jER828 [product name] (manufactured by Mitsubishi Chemical Co., Ltd.)), 174 parts of coumarone-indene resin (L-20 [product name] (manufactured by Nippon Paint Chemical Co., Ltd.)), 21 parts of dye (1) VALIFAST-BLACK 3810 [product name] (manufactured by Orient Chemical Co., Ltd.), 43 parts of dye (2) VALIFAST-RED 3320 [product name] (manufactured by Orient Chemical Co., Ltd.), 24 parts of dye (3) VALIFAST-YELLOW 3108 [product name] (manufactured by Orient Chemical Co., Ltd.), 43 parts of dye (4) VALIFAST-BLUE 2620 [product name] (manufactured by Orient Chemical Co., Ltd.), 43 parts of titania dispersion (ND139 [product name] (manufactured by Teika Co., Ltd., titania concentrated) The light-shielding paint precursor was prepared in a ratio of 580 parts of PGME dispersion (25% by mass), 135 parts of coupling agent (KBM403 [product name] (Shin-Etsu Silicone)), 300 parts of organic solvent propylene glycol monomethyl ether (PGME) (Kishida Chemical Co., Ltd.), 45 parts of hydrophobic silica (1) (Aerosil R972 [product name] (Nippon Aerosil)), 18 parts of hydrophilic silica (2) (Aerosil 200 [product name] (Nippon Aerosil)), and 7 parts of fungicide Synthol (M-100 [product name] (Sumika Enviroscience Co., Ltd.)) into a stirring container, and the stirring container was set on a roll coater and stirred at 66 rpm for 10 hours. The total amount of solvent is the sum of 75% by mass of PGME345 in the titania dispersion and PGME300 added as an organic solvent. A light-shielding coating material was obtained by mixing 100 parts of the precursor epoxy resin with 110 parts of a curing agent (EH-6019 [product name] (manufactured by ADEKA Corporation)).
[0062] Next, the obtained light-shielding coating material was applied to a flat glass (MICRO SLIDGLASS S1126 (manufactured by Matsunami Glass Industry Co., Ltd.)) with a thickness of 130 μm, and dried at room temperature for 60 minutes. After drying, the light-shielding coating material was cured for 2 hours in a thermostatic oven at a temperature of 140° C. to obtain the light-shielding film of Example 1. The brightness of the obtained optical element was evaluated under the above conditions. Next, the obtained light-shielding paint was applied to a flat glass plate made of S-LaH53 (nd=1.8; manufactured by OHARA) with a thickness of 10 μm, and dried at room temperature for 60 minutes. After drying, the light-shielding paint was cured in a thermostatic oven at a temperature of 140° C. for 2 hours to obtain a light-shielding film of Example 1. The appearance of the obtained light-shielding film was evaluated under the above conditions.
[0063] Table 1 shows the main components of the obtained light-shielding film, the evaluation results of the brightness of the obtained optical element, and the evaluation results of the appearance of the film.
[0064] (Examples 2 to 5) A light-shielding coating material, a light-shielding film and an optical element were prepared and evaluated in the same manner as in Example 1, except that the epoxy resin, the curing agent, the coumarone-indene resin and the dye were prepared according to the materials and conditions shown in Table 1. The results of the luminance value evaluation and the appearance evaluation of the obtained optical element are shown in Table 1.
[0065] (Examples 6 to 12) In Examples 6 to 12, except for changing the type of coumarone-indene resin, light-shielding coating materials, light-shielding films, and optical elements were prepared and evaluated in the same manner as in Example 1. The appearance and brightness values of the obtained optical elements, and the coating evaluation results are shown in Table 1. In Example 6, coumarone-indene resin (V-120 [product name] (manufactured by Nippon Paint Chemical Co., Ltd.)) was used, in Example 7, coumarone-indene resin (A-053 [product name] (manufactured by Nippon Paint Chemical Co., Ltd.)) was used, in Example 8, coumarone-indene resin (G-90 [product name] (manufactured by Nippon Paint Chemical Co., Ltd.)) was used, in Example 9, coumarone-indene resin (V-120S [product name] (manufactured by Nippon Paint Chemical Co., Ltd.)) was used, in Example 10, coumarone-indene resin (L-5 [product name] (manufactured by Nippon Paint Chemical Co., Ltd.)) was used, in Example 11, coumarone-indene resin (PS-65 [product name] (manufactured by Nippon Paint Chemical Co., Ltd.)) was used, and in Example 12, coumarone-indene resin (L-80 [product name] (manufactured by Nippon Paint Chemical Co., Ltd.)) was used.
[0066] Example 13 A light-shielding coating material, a light-shielding film, and an optical element were prepared and evaluated in the same manner as in Example 1, except that the type of curing agent was changed to 110 parts of a curing agent (jER Cure(R) H30 [product name] (manufactured by Mitsubishi Chemical Corporation)).
[0067] Comparative Example 1 A light-shielding coating material, a light-shielding film, and an optical element were prepared and evaluated in the same manner as in Example 1, except that the coumarone-indene resin was replaced with a xylene resin (Nikanol Y-50, [product name] (manufactured by Fudow Co., Ltd.)) and the epoxy resin and hardener were used under the materials and conditions shown in Table 1. The results of the internal reflection and coating evaluation of the obtained optical element are shown in Table 1.
[0068] (Comparative Examples 2 to 5) A light-shielding coating material, a light-shielding film and an optical element were prepared and evaluated in the same manner as in Example 1, except that the coumarone-indene resin was prepared from the materials and under the conditions shown in Table 1. The results of the internal reflection and coating evaluation of the obtained optical element are shown in Table 1.
[0069] [Table 1]
[0070] Evaluation Results In Examples 1 to 13, the effect of reducing the luminance value was good, being reduced by 10% or more compared to the reference value, and the appearance of the coating film was also good, with no peeling or cracking.
[0071] In contrast, in Comparative Examples 1, 2, 3, and 5, the reduction in brightness was less than 10% compared to the reference value, which was insufficient. In Comparative Example 3, cracks occurred. In Comparative Example 4, dissolution of the dye occurred when wiping with a solvent. [Industrial Applicability]
[0072] The optical element of the present invention can be used in optical instruments such as cameras, binoculars, microscopes, and semiconductor exposure devices. [Explanation of symbols]
[0073] 1. Light-shielding film 2 Lenses 3 Incident light 4 Transmitted light 5 Incident light 6 Reflected light 7 Interface 8 Interface 9 Reflected light 10 Transmitted light 11 Reflected light 12 Ridgeline 13. The phenomenon of light-blocking paint moving 14 Triangular Prism
Claims
1. An optical element having a light-shielding film provided on a part of an outer periphery of a substrate, The light-shielding film comprises an epoxy resin, a resin containing at least coumarone or indene, and a dye.
2. 2. The optical element according to claim 1, wherein the resin containing coumarone or indene contains coumarone and indene.
3. 3. The optical element according to claim 1, wherein the content of the dye is 80 parts by mass or more and 200 parts by mass or less with respect to 100 parts by mass of the epoxy resin.
4. 4. The optical element according to claim 1, wherein the content of the resin having coumarone or indene is 100 parts by mass or more and 300 parts by mass or less relative to 100 parts by mass of the epoxy resin, and the content of the dye is 80 parts by mass or more and 200 parts by mass or less relative to 100 parts by mass of the epoxy resin.
5. 5. The optical element according to claim 1, wherein a ratio of the dye to the resin containing coumarone or indene is 0.44 or more.
6. 6. The optical element of claim 5, wherein the ratio of the dye to the coumarone or indene-containing resin is 1.31 or less.
7. 7. The optical element of claim 6, wherein the ratio of the dye to the coumarone or indene-containing resin is 1.15 or less.
8. The optical element according to claim 1 , wherein the light-shielding film contains several types of dyes.
9. The optical element according to claim 8 , wherein the light-shielding film contains a pigment.
10. 3. The optical element according to claim 1, wherein the content of the resin having coumarone or indene is 100 parts by mass or more and 300 parts by mass or less with respect to 100 parts by mass of the epoxy resin.
11. The optical element according to claim 1 , wherein the substrate is a lens or a prism.
12. 12. The optical element according to claim 1, wherein the light-shielding film has a thickness of 0.3 μm or more and 100 μm or less.
13. The optical element according to claim 1 , wherein the optical element is a lens or a prism.
14. 14. The optical element according to claim 1, wherein a content of the dye is 46 parts by mass or more and 115 parts by mass or less with respect to 100 parts by mass of the resin containing coumarone or indene.
15. An optical instrument comprising the optical element according to any one of claims 1 to 14.
16. 16. The optical instrument according to claim 15, which is any one of a camera, binoculars, a microscope, and a semiconductor exposure apparatus.
17. A method for manufacturing an optical element having a light-shielding film provided on a part of an outer periphery of a substrate, comprising the steps of: A step of applying a light-shielding paint to the outer peripheral surface of the substrate; and a step of hardening the applied light-shielding coating material to form a light-shielding film. The light-shielding coating material comprises an epoxy resin, a resin having at least coumarone or indene, a dye, and an amine-based curing agent.
18. 18. The method for producing an optical element according to claim 17, wherein the content of the resin having coumarone or indene is 100 parts by mass or more and 300 parts by mass or less with respect to 100 parts by mass of the epoxy resin.
19. 19. The method for producing an optical element according to claim 17, wherein the content of the dye is 80 parts by mass or more and 200 parts by mass or less with respect to 100 parts by mass of the resin having coumarone or indene.
Citation Information
Patent Citations
Improved mirror
JP1988184702A
Decorative sheet for mirror member, mirror member and method for manufacturing the same
JP2003227911A
Light-shielding film for optical element, and optical element
JP2011186437A
Cemented lens, optical system having the same, optical device, and method of fabricating cemented lens
JP2020024331A
Anticorrosive coating composition
WO2007129564A1