Germanosilicate CIT-14 / IST and its preparation from germanosilicate CIT-13 / OH
A fluoride-free synthesis of germanosilicate CIT-13 transforms into CIT-14, addressing the inefficiencies of existing methods by producing a high-quality, ultra-large pore zeolite with enhanced catalytic capabilities for larger molecules, suitable for industrial applications.
Patent Information
- Application Number
- JP2022530332
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-12
- Filing Date
- 2020-12-11
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2040-12-11
AI Technical Summary
Existing methods for synthesizing new zeolite frameworks are unpredictable and inefficient, particularly in creating large-pore structures suitable for handling larger feed molecules in oil upgrading processes, and there is a need for new crystalline phases with improved catalytic properties.
The development of a fluoride-free hydrothermal synthesis method for germanosilicate CIT-13, which undergoes inverse sigma transformation to produce CIT-14, a germanosilicate with 12- and 8-membered ring channels, allowing for the creation of ultra-large pore structures without mesoporosity, characterized by specific X-ray diffraction patterns and nuclear magnetic resonance spectroscopy.
The method produces high-quality CIT-14/IST germanosilicate with unique structural and catalytic properties, enabling effective handling of larger molecules and enhancing catalytic performance in industrial applications.
Smart Images

Figure 0007557535000029 
Figure 0007557535000037 
Figure 0007557535000045
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims priority from U.S. Provisional Patent Application No. 62 / 947,434, filed December 12, 2019, the contents of which are incorporated by reference for all purposes.
[0002] (Government Rights) none [Technical field]
[0003] This disclosure relates to germanosilicates designated CIT-13 / OH and CIT-14 and the conversion of the former to the latter by inverse sigma conversion. [Background technology]
[0004] Zeolites play an important role as heterogeneous catalysts and are used in various industrial settings. Initially, these materials were primarily developed to aid the petroleum industry in its quest to create more selective and robust catalysts for making gasoline and other fuels. Now, these solids have emerged as specialized materials with properties based on their structure and chemical composition that make them suitable for certain large-scale applications. Although it takes a great deal of effort to bring new materials from the discovery stage to commercially viable catalysts, there is still room for the discovery of new structures that may emerge as superior to existing materials.
[0005] One goal for discovering new materials is the hope that larger pores that retain some catalytic properties on their interior surfaces might enable them to process larger feed molecules in the oil upgrading sector.
[0006] Therefore, there remains interest in discovering new crystalline phases for use in these applications, and this work aims to address the deficiencies in the technology in this area.
[0007] Synthetic molecular sieves are typically prepared using hydrothermal synthesis involving the use of inorganic (Na+, K+, etc.) and organic structure directing agents (OSDAs), mineralizers (OH- or F-), heteroatoms (Al, B, Ge, Ti, Sn, etc. in addition to elemental Si), etc. The synthesis of crystalline molecular sieves is complex. Although progress has been made in designing the recipes and specific parts of the assembly process, it is difficult to predict the outcome from the approach.
[0008] Topotactic transformation of existing zeolites has served as a method to prepare new zeolitic frameworks that could not be synthesized by conventional hydrothermal methods. A typical example is the assembly-disassembly-organization-reassembly (ADOR) strategy for the transformation of germanosilicates, which exploits the property that germanium sites preferably occupy small compositional building units (CBUs) such as double-4 rings (d4r), and these transformations are shown diagrammatically in Figures 1(A) and 1(B), respectively.
[0009] In the course of investigating the function of imidazolium-derived compounds with benzyl pendant groups as OSDAs, the ultra-large pore structure CIT-13 (*CTH: the asterisk (*) denotes the presence of crystallographic disorder in the structure) with channels of 14 MR and 10 MR was discovered. Also reported are isostructural germanosilicates, NUD-2 and SAZ-1, crystallized from imidazolium-based OSDAs and fluoride-based gels. CIT-13 is a structure in which Si-rich cfi layers are crosslinked with a two-dimensional array of Ge-rich d4r units. The structure of the cfi layers gives the d4r units two crystallographically equivalent positions. This equivalence is revealed by the disorder of the positions of the d4r units in the CIT-13 backbone and the conversion of *CTH to CFI (Figure 1(C)). Most importantly, the structure of CIT-13 resembles that of IM-12, which indicates the rich chemistry of germanosilicate transformation.
[0010] We previously reported the similarity between *CTH and UTL and disclosed two novel frameworks, CIT-14 and CIT-15, with 2D 12 / 8MR and 1D 10MR channel systems, respectively, prepared based on the ADOR transformation. However, ADOR products of sufficient quality for Rietveld refinement from powder X-ray diffraction (PXRD) have never been prepared before. This is likely due to the possible presence of Si-O-Si linkages within the interlayer region, which may cause incomplete exfoliation. reported that a weak base solution, such as ammonium hydroxide, could dissociate the interlayer Si-O-Si bonds that prevent complete exfoliation of the cfi-type layers of CIT-13, resulting in a structure called ECNU-21 (isostructural to CIT-15). We also found that a weak base solution could exfoliate the cfi-type layers from the germanosilicate Ge-CIT-5, which has double zigzag chain (dzc) composition building units instead of d4r units. Very recently, the formation of ECNU-23 (isostructural to CIT-14) by partial degermanation from the d4r unit of CIT-13 and its structure solution (based on electron diffraction) were also reported. The synthesis was similar to the inverse sigma transformation of IM-12. However, due to the unique germanium configuration in the d4r unit of CIT-13, the inverse sigma transformation by leaching the pure Ge-4-ring with strong acid has not been reported so far. Summary of the Invention
[0011] The present disclosure is directed to novel germanosilicates derived from recently reported crystalline microporous germanosilicates with CIT-13 topology prepared by a fluoride-free hydroxide route as described in U.S. Pat. No. 10,828,625. This reference is incorporated herein by reference in its entirety for all purposes, including characterization of materials of CIT-13 topology and methods of making and using. These CIT-13 germanosilicates were prepared hydrothermally using benzylimidazolium organic structure directing agents to form a three-dimensional framework with pores defined by 10- and 14-membered rings. These structures are characterized by the presence of pore sizes of 6.2x4.5Å and 9.1x7.2Å, respectively. These structures are the first known crystalline silicates. These structures have been confirmed by powder X-ray diffraction (PXRD) patterns, unit cell parameters, SEM micrographs, and 29 It was characterized by Si MAS NMR spectroscopy and adsorption / desorption isotherms.
[0012] This disclosure describes a germanium-containing ultra-large pore molecular sieve, CIT-13, synthesized without the use of fluoride. After removal of occluded organic matter, CIT-13 obtained from the fluoride-free preparation shows differences from CIT-13 samples prepared in the presence of fluoride. It was found that CIT-13 made by the fluoride-free method undergoes inverse sigma transformation to produce mesopore-free CIT-14, which is converted to CIT-5 type germanosilicate much faster than Ge-CIT-13 with a similar Si / Ge ratio obtained from the fluoride-containing synthesis. Rietveld refinement of the structure of CIT-14 confirmed that it has 12- and 8-membered ring channels, although the unit call parameters of this material differed slightly from previous reports. 19 F Magic Angle Spinning (MAS) and 1 H- 29 Si cross-polarization (CP) MAS nuclear magnetic resonance (NMR) spectroscopy revealed that CIT-13 crystallized without fluoride has different germanium positions than CIT-13 synthesized in the presence of fluoride.
[0013] The present disclosure is further directed to methods of engineering the structure of these CIT-13 germanosilicates prepared by the fluoride-free hydroxide route, with Si / Ge ratios ranging from 3.8 to 10, by exposure to heat and steam under suitable reaction conditions to effect an inverse sigma transformation. This mechanism of this material was not previously known. The present disclosure is also directed to the germanosilicate CIT-14 product obtained from such manipulation. Previously, the germanosilicate CIT-14 was available by ADOR transformation (assembly-disassembly-organization-reassembly) of a phyllosilicate designated CIT-13P, as described in U.S. Pat. No. 10,293,33, the contents of which are incorporated herein by reference for all purposes or at least for the preparation and characterization of CIT-14.
[0014] Certain embodiments of the present disclosure include those crystalline microporous germanosilicate compositions, designated CIT-14 / IST, having 8- and 12-ring channels. The CIT-14 / IST compositions, in some embodiments, are characterized by powder X-ray diffraction (RD) patterns having at least 5, 7, or 10 characteristic peaks at 7.59±0.5, 8.07±0.5, 12.88±0.5, 19.12±0.5, 19.32±0.5, 20.73±0.5, 22.33±0.5, 24.37±0.5, 27.19±0.5, and 27.69±0.5 degrees 2-θ. The present disclosure further provides a more complete disclosure of the various uncertainties associated with the peaks, the full range of characteristic peaks, and the relative intensities and selection of peaks that characterize these materials.
[0015] CIT-14 / IST compositions, in some embodiments, are characterized in that their Si:Ge ratio is in the range of 12:1 to 20:1 or 14:1 to 18:1 or any subrange within these ranges.
[0016] The CIT-14 / IST composition, in some embodiments, is characterized by claims 1-4, wherein the crystal is of the orthorhombic system. In some embodiments, the CIT-14 / IST crystal has the Cmmm space group or the Cmcm space group or an intracrystalline mixture of the two domains (disorder). In some embodiments, the crystalline microporous germanosilicate CIT-14 / IST composition has the following unit cell parameters:
[0017] [Table 1]
[0018] In some embodiments, the 8-ring channels have pore sizes of CIT-14 / IST compositions of about 3.3 Å×3.9 Å, and the 12-ring channels have pore sizes of about 4.9 Å×6.4 Å. Physical strain (e.g., compression) or the Si:Ge ratio can change these values.
[0019] In some embodiments, the crystalline microporous germanosilicate CIT-14 / IST composition is derived or derivable from the inverse sigma transformation of the crystalline microporous germanosilicate designated CIT-13 / OH. In some embodiments, the crystalline microporous germanosilicate CIT-14 / IST composition is derived or derivable from the crystalline microporous germanosilicate designated CIT-13 / OH by subjecting the CIT-13 / OH germanosilicate to concentrated aqueous mineral or other strong aqueous acid conditions at elevated temperatures for a time sufficient to degermanate the CIT-13 / OH germanosilicate to form the "-CIT-14" composition, and isolating and calcining the as-formed "-CIT-14" germanosilicate to form the crystalline microporous germanosilicate CIT-14 / IST composition. Exemplary conditions for effecting these transformations are described elsewhere in this disclosure.
[0020] The specific morphology, properties and preparation conditions of the crystalline microporous CIT-13 / OH germanosilicates are more clearly defined in the present disclosure, but these compositions require that they are produced without the presence of fluoride ions and within a specific range of Si:Ge ratios. The synthesis of these CIT-13 / OH germanosilicates is conveniently carried out using certain substituted benzylimidazolium organic structure directing agent (OSDA) cations as defined herein. In some preferred embodiments, the precursor CIT-13 / OH germanosilicates are fluoride-free and have d4r units with at least, and preferably more than 4, Ge atoms on average, allowing the presence of Ge-4-rings in the d4r units.
[0021] In another embodiment, the crystalline microporous germanosilicate CIT-14 / IST composition contains micropores comprising at least one alkali metal salt, alkaline earth metal cation salt, transition metal, transition metal oxide, transition metal salt, or combinations thereof.
[0022] In another embodiment, the crystalline microporous germanosilicate CIT-14 / IST in either their acid or metal-containing forms, are used as catalysts or adsorbents in a range of processes described elsewhere herein.
[0023] The present disclosure also includes other embodiments for the preparation of crystalline microporous germanosilicate CIT-14 / IST, including methods that include contacting crystalline microporous germanosilicate CIT-13 / OH germanosilicate with concentrated strong aqueous mineral acid at elevated temperature for a time sufficient to convert the crystalline microporous germanosilicate CIT-13 / OH germanosilicate to the as-formed "-CIT-14" composition. The present disclosure also includes pre-calcined as-formed "-CIT-14" compositions.
[0024] The present disclosure also encompasses embodiments of CIT-13 / OH germanosilicates prepared by the hydroxide route specifically described herein. The present disclosure also encompasses embodiments of CIT-13 / OH germanosilicates characterized as having d4r units containing, on average, at least, and preferably more than 4 Ge atoms per d4r, allowing for the presence of Ge-4-rings in the d4r units. The present disclosure also encompasses embodiments of CIT-13 / OH germanosilicates that exhibit previously unobserved reactivity characteristics that are the result of the novel and unique physical features defined herein.
[0025] The patent or application file contains at least one drawing / photograph executed in color. Copies of this patent or patent application publication with color drawing / photographs will be provided by the U.S. Patent and Trademark Office upon request and payment of the necessary fee.
[0026] This application is better understood when read in conjunction with the accompanying drawings. For the purpose of illustrating the subject matter, the drawings show example embodiments of the subject matter, however, the presently disclosed subject matter is not limited to the particular methods, apparatus and systems disclosed. Additionally, the drawings are not necessarily drawn to scale. In the drawings: [Brief description of the drawings]
[0027] [Figure 1] A schematic illustration of known germanosilicate transformations is provided: Fig. 1(A) shows the inverse sigma transformation, Fig. 1(B) shows the ADOR transformation, and Fig. 1(C) shows the diffusionless rearrangement of the d4r sequence (conversion of *CTH to CFI). *CTH-type frameworks are shown as model matrices. [Diagram 2] FIG. 1 is a schematic diagram of the work carried out and reported herein. [Diagram 3] FIG. 3 illustrates the structure of CIT-14 / ESP (ESP stands for ethoxysilylated pillaring), including its theoretical PXRD data (FIG. 3(A)) and pore channel dimensions (FIG. 3(B)), as described in U.S. Pat. No. 10,293,33. [Figure 4](a) SEM images of CIT-14 / IST samples derived from CIT-13 / OH[3.71] (FIG. 4(A)); and CIT-13 / OH[3.56] (FIG. 4(B)). [Diagram 5] SEM images of CIT-13 / OH samples: CIT-13 / OH[3.71] (Figure 5(A)); CIT-13 / OH[3.56] (Figure 5(A)) and CIT-13 / OH[4.33] (Figure 5(C)). [Figure 6] Figure 1 shows 1H-13C 8 kHz CPMAS spectra of as-prepared versions of CIT-13 / OH[4.33], CIT-13 / F[4.33] and 13C solution spectrum of 1,2-dimethyl-3-(3-methylbenzyl)imidazolium chloride in chloroform-d. [Figure 7] FIG. 14 shows the 1H-29Si 8 kHz CPMAS spectrum of the as-prepared version of CIT-13 / OH[4.33]. [Figure 8] Figure 8: Characterization results of CIT-13. Figure 8(A): Two OSDAs capable of crystallizing CIT-13 without fluoride mineralizer. Figure 8(B-E): PXRD patterns of selected examples of CIT-13 / OH samples: (b) as-prepared and Figure 8(C): calcined CIT-13 / OH[3.88], Figure 8(D): as-prepared and Figure 8(E): calcined CIT-13 / OH[4.33]. Figure 8(F): PXRD profile of reference CIT-13 / F with Si / Ge of about 5. Figure 8(G): Ar adsorption isotherms of CIT-13 / OH[3.56] and CIT-13 / F[4.18] on logarithmic scale. [Figure 9] Figure 9 shows PXRD patterns of as-prepared CIT-13 / OH samples compared to those of reference CIT-13 / F with Si / Ge = approx. 5. Figure 9(A): Reference CIT-13 / F, Figure 9(B): Batch #A, Figure 9(C): Batch #5, Figure 9(D): Batch #7, Figure 9(E): Batch #8, Figure 9(F): Batch #12, Figure 9(G): Batch #13, Figure 9(H): Batch #15, Figure 9(I): Batch #16, Figure 9(J): Batch #17 and Figure 9(K): Batch #18. [Figure 10]FIG. 1 shows the PXRD patterns of the as-prepared CIT-13 / OH sample and its refluorinated version, with the (310) diffraction highlighted. [Figure 11(AE)] Figure 11 shows the structural changes during the conversion of *CTH to CFI observed based on the PXRD profiles. PXRD profiles of calcined CIT-13 / OH[4.33] (Figure 11(AB)) and CIT-13 / OH[3.88] after 10 days of exposure to atmospheric humidity in the ranges (a, c) 4-40° and (b, d) 5-9° (Figure 11(CD)). Change in d200 interlayer distance of CIT-13 / OH[4.33] compared to CIT-13 / F[4.31] (Figure 11(E)). [Figure 12] Figure 2 shows the 29Si 8 kHz MAS spectra of calcined CIT-13 / OH[3.88] and Ge-CIT-5 prepared therefrom. The 29Si MAS NMR is qualitatively similar to that of CIT-14 / ESP germanosilicate prepared by ADOR synthesis as described in U.S. Pat. No. 10,293,33, showing a small amount of Q3 Si species and multiple Q4 Si environments in the chemical shift region of -108 to -120. [Figure 13] Figure 13: Inverse sigma conversion of CIT-13 to CIT-14. Schematic of the inverse sigma conversion of CIT-13 / OH to give CIT-14 / IST (Figure 13(A)); PXRD profiles of parent CIT-13 / OH and the corresponding CIT-14 / IST sample (Figure 13(A)). [Figure 14] FIG. 14 shows the PXRD profiles of the parent CIT-13 sample (black), the material immediately after 12M HCl treatment (fuchsia) and the calcined sample (blue): CIT-13 / F[3.87] (FIG. 14(A)) and CIT-13 / OH[4.33] (FIG. 14(B)). [Figure 15]PXRD profiles of CIT-13 / OH[3.56] (top), CIT-14 / IST from CIT-13 / F[4.33] (middle) and the theoretical model of "disorder-free" CIT-14 optimized based on the GULP algorithm in the ranges (a) 4-40°, (b) 6-10° and (c) 10.0-12.5°. (d) 29Si NMR spectra of CIT-14 / IST and CIT-14 / ESP samples. (29Si MAS spectrum of CIT-14 / ESP taken from U.S. Patent Application Publication No. 20170252729). [Figure 16] Figure 1 shows the effect of elemental composition on the intensity of PXRD peaks of CIT-14. (a) Simulated PXRD profiles of CIT-14 framework with 0% (black), 10% (cyan) and 20% (red) germanium at the seven T sites of CIT-14 and (b) T1, (c) T2, (d) T3, (e) T4, (f) T5, (g) T6 and (h) T7 sites. Peak-1, peak-2 and peak-3 represent (110), (200) and (001) diffraction, respectively. [Figure 17] FIG. 17 shows the experimental design and PXRD patterns in the ranges of 4 to 40° (FIG. 17(B)) and 6 to 9° (FIG. 17(C)) of the obtained CIT-14 / ESP sample. [Figure 18] SEM images of IM-12[3.80] (Figure 18(A)), IM-12[4.79] (Figure 18(B)), COK-14 from IM-12[3.80] (Figure 18(C)), and COK-14 from IM-12[4.79] (Figure 18(D)). [Figure 19] FIG. 1 shows the PXRD profiles of COK-14 from IM-12[3.80] and COK-14 from IM-12[4.79]. [Figure 20] Ar-adsorption and desorption isotherms of parent CIT-13 / OH, CIT-14 / IST and CIT-14 / ESP: in linear scale (FIG. 20(A)) and logarithmic scale (FIG. 20(B)). [Figure 21]Figure 21 shows the results of the structure analysis of CIT-14 / IST. (Figure 21(A)) Observed (top), calculated (middle) and difference (bottom) profiles in the Rietveld refinement of CIT-14. (Figure 21(B)) Projections (3x3x3 unit cell) of CIT-14 along the principal crystal axes
[0001] ,
[0010] and
[0100] . (Figure 21(C)) Two-dimensional 12- / 8-ring channel system in the idealized structure of CIT-14. (Figure 21(D)) Schematic of the disorder of CIT-14. [Figure 22] Figure 22 (B-C) shows the idealized structure of CIT-14 / IST. Silicon, germanium and oxygen atoms are shown in blue, green and red, respectively. Figure 22 (B-C) shows the pore sizes of the 12- and 8-membered rings of CIT-14 / IST, respectively. [Figure 23] Figure 23(B) shows the 19F 12k MAS NMR spectra of as-prepared CIT-13 / F[4.33], fluorinated CIT-13 / OH[4.33] (Figure 23(B)) and fluorinated CIT-13 / OH[3.56] (Figure 23(C)). (The asterisk (*) indicates the rotating sidebands of the fluorinated silica (19F-Si) surface formed as a result of fluorination with ammonium fluoride.) [Figure 24] Figure 1 shows 1H-29Si CPMAS spectra of water-degermanated CIT-13 / OH, CIT-13 / F and IM-12 samples with different germanium contents. The parent germanosilicate sample and its acid leached product are shown on the left and right side of the spectrum, respectively. [Diagram 25] Schematic of possible germanium configurations within a d4r unit: green balls and silver nodes indicate germanium and silicon sites, respectively (not all possibilities are shown). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] The present disclosure is directed to novel compositions of matter comprising crystalline microporous germanosilicates and methods of making and using these compositions.
[0029] Herein, a new method for the synthesis of fluoride-free *CTH-type germanosilicate molecular sieves is disclosed. Removal of fluoride from the synthesis narrows the compositional range previously reported for CIT-13 crystallization and slows down the crystallization time. However, CIT-13 prepared from hydroxide media (referred to as CIT-13 / OH) exhibits interesting properties that are not achievable with CIT-13 synthesized in the presence of fluoride (referred to as CIT-13 / F). After calcination and exposure to environmental humidity, fluoride-free CIT-13 / OH converts to CFI-type germanosilicate (Ge-CIT-5) much faster than conventional CIT-13 / F from fluoride-containing gels with similar Si / Ge ratios. Also, CIT-13 / OH from the fluoride-free route can undergo reverse sigma transformation to another scaffold, CIT-14, with 12MR and 8MR ring channels upon contact with strong acid. CIT-14 from reverse sigma transformation (designated CIT-14 / ist) did not show the mesoporosity present in its isostructural analogue obtained from ADOR-type transformation. Since these transformations are based on the presence and arrangement of germanium sites in the d4r unit, it is concluded that the presence of fluoride anions in the synthesis mixture influences the element (Ge and Si) composition and / or arrangement in the d4r unit of CIT-13. These results also indirectly support the presence of Ge-O-Ge bonds and germanium 4-rings in the d4r unit of CIT-13 / OH synthesized from hydroxide-based gel, similar to that observed in IM-12. Figure 2 summarizes the work reported in this disclosure.
[0030] The present disclosure is now described by reference to the following description taken in conjunction with the accompanying figures and examples. The present disclosure may be more easily understood by referring to the following detailed description, all of which form part of this disclosure. It will be understood that the present disclosure is not limited to the specific products, methods, conditions, or parameters described or shown herein, and that the terms used herein are intended to illustratively describe certain embodiments and are not intended to limit the disclosure of any claims. Similarly, unless specifically stated otherwise, any statements regarding possible mechanisms or modes of action or reasons for improvements are intended to be illustrative only, and the disclosure herein is not bound by the correctness or implied correctness of the mechanisms or modes of action or reasons for improvements. It will be recognized that throughout this text, statements refer to compositions and methods of making and using said compositions. That is, when the present disclosure describes or claims features or embodiments related to compositions or methods of making or using the compositions, it will be understood that such statements or claims are intended to extend those features or embodiments to embodiments in each of these contexts (i.e., compositions, methods of making, and methods of using). Where a processing method is described, unless specifically excluded, additional embodiments provide that the product composition is isolated and optionally post-processed in a manner consistent with molecular sieve or zeolite synthesis.
[0031] The present disclosure encompasses compositions designated "CIT-13 / OH," "-CIT-14," and "CIT-14 / IST," as well as methods for converting the former to the latter.
[0032] (Crystalline Microporous Germanosilicate Compositions Designated CIT-14 / IST and "-CIT-14") Particular embodiments include crystalline microporous germanosilicate compositions having 8- and 12-ring channels, designated CIT-14 / IST, which include compositions derived or derivable from CIT-13 / OH by the use of concentrated strong acids.
[0033] In certain embodiments, the CIT-14 / IST germanosilicate composition comprises a pure germanosilicate. In other independent embodiments, the CIT-14 / IST germanosilicate composition comprises a framework that comprises one or more oxides of aluminum, boron, gallium, hafnium, iron, tin, titanium, vanadium, zinc, or zirconium. These additional oxides may be derived from the precursor CIT-13 / OH used to prepare the CIT-14 / IST germanosilicate composition. Methods for incorporating these oxides into the precursor CIT-13 / OH composition are described elsewhere herein.
[0034] These crystalline microporous germanosilicate CIT-14 / IST compositions can be characterized by a powder X-ray diffraction (XRD) pattern having at least five characteristic peaks at 7.59±0.5, 8.07±0.5, 12.88±0.5, 19.12±0.5, 19.32±0.5, 20.73±0.5, 22.33±0.5, 24.37±0.5, 27.19±0.5, and 27.69±0.5 degrees 2-θ. In certain independent embodiments, the powder X-ray diffraction (XRD) pattern exhibits at least five characteristic peaks at 5, 6, 7, 8, 9, or 10 of these characteristic peaks. In certain independent embodiments, the uncertainty in the peak positions is independently (for each peak) ±0.5 degrees 2-θ, ±0.4 degrees 2-θ, ±0.3 degrees 2-θ, ±0.2 degrees 2-θ, ±0.15 degrees 2-θ, or ±0.15 degrees 2-θ.
[0035] Table 1 provides a list of powder XRD data from samples of crystalline germanosilicate CIT-14 / IST compositions. These data are considered representative of these materials. Various permutations of these data can be used to characterize these compositions, for example, by including multiple peaks selected by their relative intensities. These crystalline microporous germanosilicate CIT-14 / IST compositions can be further characterized by comparison with the powder XRD patterns shown in FIG. 15.
[0036] [Table 2]
[0037] For example, in certain other embodiments, the crystalline microporous germanosilicate CIT-14 / IST composition is characterized by a powder X-ray diffraction (XRD) pattern exhibiting characteristic peaks at 7.59±0.5, 8.07±0.5, 19.12±0.5, 20.73±0.5, and 22.33±0.5 degrees 2-θ, and optionally by at least three characteristic peaks at 12.88±0.5, 19.32±0.5, 24.37±0.5, 27.19±0.5, and 27.69±0.5 degrees 2-θ. The peaks at 7.59 and 8.07 degrees 2-θ correspond to Miller indices of (110 and (200), respectively, and are the most intense peaks in the pattern. Other individual weaker peaks may also be useful in distinguishing it from other materials.
[0038] The observed intensity values in Table 1 are likely based on the completely random orientation of the crystallites, the perfect long-range order in all crystallographic directions, and the ideal interlocking of the CIT-14 / IST framework. However, the crystallite morphology of CIT-14 / IST is very flat and exhibits a high aspect ratio, which indicates that in fact the intensity may be convoluted by the preferred orientation of the sample. Furthermore, as the crystallinity (quality) of the CIT-14 sample increases, the intensity of the first peak (110) (7.67) seems to increase. This is due to the diagonal long-range order of the interlocking units (single 4-ring in CIT-14) contributing to the (110) diffraction. The relatively chemically inert Si-rich layers are attributed to the (200) peak at 8.08° (and therefore generally stronger).
[0039] In certain embodiments, the crystalline microporous germanosilicate CIT-14 / IST compositions prepared from CIT-13 / OH described herein have a Si:Ge ratio in the range of 12:1 to 13:1, 13:1 to 14:1, 14:1 to 15:1, 15:1 to 16:1, 16:1 to 17:1, 17:1 to 18:1, 18:1 to 19:1, 19:1 to 20:1, or any combination of two or more of these aforesaid subranges, such as 14:1 to 18:1. Certain compositions described in the examples are also considered to be within these ranges.
[0040] The crystals of the crystalline microporous germanosilicate CIT-14 / IST are orthorhombic. In some cases, as described in the examples, the crystals may be disordered, including crystals of the Cmmm or Cmcm space groups, or an intracrystalline mixture of the two domains (disordered).
[0041] Within this context, it has been found that the crystals of the crystalline microporous germanosilicate CIT-14 / IST composition exhibit the following unit cell parameters:
[0042] [Table 3]
[0043] The Å values in the right-most column are those actually determined (or estimated) based on Rietveld refinement (see Examples), while those shown in the middle column provide the estimated variance that may occur as a function of a particular composition (e.g., Si:Ge ratio or any metal oxide substitution).
[0044] The channels within these crystalline microporous germanosilicate CIT-14 / IST compositions are also characterized as follows: the 8-ring channels have a pore size of approximately 3.3 Å x 3.9 Å, and the 12-ring channels have a pore size of approximately 4.9 Å x 6.4 Å. The respective pore sizes have been experimentally determined to be 3.26 Å x 3.93 Å and 4.86 Å x 6.44 Å, respectively, although a wider variance is necessary since, for example, physical strain (e.g., compression) or the Si:Ge ratio can alter these values. Additionally, the average metal-oxygen (TO) bond length within the framework is 1.55-1.65 Å, and the average oxygen-metal-oxygen (OTO) bond length is 98-1.55 Å. o ~116 o , the average metal-oxygen-metal (TOT) is 139 o ~180 o where T is Si or Ge.
[0045] Thus far, the crystalline microporous germanosilicate CIT-14 / IST compositions have been characterized by their physical attributes. However, the present disclosure also contemplates embodiments in which these compositions are characterized by the method of their preparation from the reaction of germanosilicate CIT-13 / OH with a concentrated strong acid. Such embodiments include those in which the structure is considered independently of the physical parameters mentioned (i.e., a pure product-by-process description) and those in which the structure is considered simultaneously with one or more of the physical attributes.
[0046] In these embodiments, the crystalline microporous germanosilicate CIT-14 / IST composition is prepared by contacting a crystalline microporous germanosilicate designated CIT-13 / OH with concentrated aqueous mineral acid at elevated temperature for a time sufficient to form the as-formed microporous germanosilicate "-CIT-14". Both the CIT-13 / OH (as described and used herein) and "-CIT-14" compositions The subject matter is described elsewhere herein. The following description also relates to methods of preparing germanosilicate CIT-14 / IST compositions from germanosilicate CIT-13 / OH compositions, and it will be understood that the methods of preparing germanosilicate CIT-14 / IST compositions by these methods constitute independent embodiments. This CIT-13 / OH germanosilicate composition, as well as the composition designated "-CIT-14", are considered independent embodiments of the present disclosure, as is its use in preparing CIT-14 / IST.
[0047] To prepare the CIT-14 / IST composition from the germanosilicate CIT-13 / OH composition, the method includes one or more of the following conditions:
[0048] (1) The CIT-13 / OH composition is conveniently dispersed in a strong aqueous acid solution. The reaction mixture can then be allowed to stand or mixed more efficiently in a moving reactor, e.g., a rotating reactor. As highlighted in the examples, it may be useful to physically disperse the reaction medium at intermediate points.
[0049] (2) Mineral acids are strong acids; i.e., those that dissociate substantially completely in aqueous solution, as distinguished from weak acids, which only partially ionize in aqueous solution. HCl or HNO3 are typical acids used in this capacity, although other strong acids may be used. These strong acids are those that have anions that can be incorporated into the framework lattice (e.g., phosphoric acid), but are not considered when such incorporation is deemed undesirable.
[0050] (3) The use of concentrated acid appears to be important. In a preferred embodiment, the concentration of mineral acid is in the range of 6-12 M. Higher concentrations are preferred (e.g., 10-12 M) as they appear to improve reaction rates and yields.
[0051] (4) The high temperature is a temperature in the range of 80° C. to 120° C., preferably about 95° C. Considering the volatility of water at this temperature, it is necessary to use a closed reactor.
[0052] (5) The time sufficient to effect the conversion ranges from 4 hours to 96 hours, preferably 6 hours to 24 hours. Clearly there is a balance between the time, temperature, and type and concentration of acid required for the reaction to proceed to an adequate yield of product. Conditions equivalent to 95°C for 6 hours using 12M aqueous HCl have been found to be suitable.
[0053] (6) Following contact of the germanosilicate with acid, the resulting degermanated germanosilicate, designated "-CIT-14", is isolated, conveniently by centrifugation, although other separation methods can be used.
[0054] (7) The isolated "-CIT-14" material is then washed liquid Repeatedly rinse or wash with water (preferably distilled or deionized water) until pH neutral. This "-CIT-14" material is also considered a separate embodiment of this disclosure, and representative features of this material are described in the Examples.
[0055] (8) Preparation of CIT-14 / IST from the as-produced "-CIT-14" material can be carried out by heating the isolated and washed "-CIT-14" material at a temperature ranging from about 450° C. to 650° C. for a time ranging from 2 hours to 12 hours, preferably at 580° C. for 6 hours, or conditions substantially equivalent thereto. In a preferred embodiment, heating is carried out at a temperature ramp rate of 1-5° C. / min, preferably 1° C. / min.
[0056] The conversion of CIT-13 / OH to CIT-14 / IST is accompanied by a decrease in the micropore volume of about 25–30 vol%.
[0057] The above process provides CIT-14 / IST germanosilicate, consistent with a mechanism characterized as an inverse sigma transformation of crystalline microporous CIT-13 / OH germanosilicate, for reasons discussed in the Discussion of Examples section, and therefore the process and product can be characterized using that term.
[0058] (Crystalline Microporous Germanosilicate Composition Designated CIT-13 / OH) Compositions generally defined as CIT-13 and their reactivity under various processing conditions have been previously reported, see, for example, U.S. Patent Nos. 10,293,330 and 10,828,625, and U.S. Patent Application Publication No. 2017-0252729, each of which is incorporated by reference herein for all purposes or at least for information related to the germanosilicate CIT-13.
[0059] US Pat. No. 10,293,330 states that CIT-13 has a three-dimensional framework with pore channels defined by 10- and 14-membered rings and exhibits a powder XRD pattern as shown in Table 2.
[0060] [Table 4]
[0061] The CIT-13 / OH germanosilicate described herein also contains 10-membered rings and 1 They have a three-dimensional framework with pores defined by four-membered rings, but are fluoride-free. Consistent with other CIT-13 germanosilicates, they exhibit powder XRD (X-ray diffraction) patterns with at least five peaks at 6.45±0.2, 7.18±0.2, 12.85±0.2, 20.78±0.2, 26.01±0.2, and 26.68±0.2 degrees 2-θ. See Table 2. These CIT-13 / OH germanosilicates may also be characterized by powder XRD patterns with peaks at 6.45±0.2 and 7.18±0.2 degrees 2-θ, as well as five, six, or seven of the other peaks shown in Table 2.
[0062] As discussed in the Examples, the powder XRD patterns of CIT-13 / OH described herein show some differences from the data shown in Table 2, particularly with respect to the intensity of the (200) peak of the as-produced material. This observation is further elaborated in the Examples. In some embodiments, the peak at 6.45±0.2 degrees 2-θ is reduced in intensity (weaker) compared to the peak at 7.18±0.2 degrees 2-θ, the latter peak being the most intense in the pattern (see Examples). In other embodiments, the powder XRD patterns of CIT-13 / OH germanosilicate show an additional peak at 11.58 degrees ±0.2 degrees 2-θ of moderate to weak intensity due to the (310) index.
[0063] The CIT-13 / OH germanosilicate also matches the spectrum shown in Figure 12 (top). 29 The Si MAS-nmr spectrum is shown and is further explained in the Examples.
[0064] The Si:Ge ratios of these CIT-13 / OH germanosilicates are in the ranges of 3.5-3.6, 3.6-3.7, 3.7-3.8, 3.8-3.9, 3.9-4.0, 4.0-4.1, 4.1-4.2, 4.2-4.3, 4.3-4.4, 4.4-4.5, 4.5-4.6, 4.6-4.7, 4.7-4.8, 4.8-4.9, 4.9-5.0, 5.0-5.2, or a range defined by any two or more of the foregoing ranges, e.g., 3.5-5.2 or 3.5-3.9. These ranges are similar to those previously reported for CIT-13 materials.
[0065] However, unlike those previously reported materials, the present fluoride-free CIT-13 / OH germanosilicates contain d4r structural units with an average of at least four, and preferably more than four, Ge atoms per d4r unit, allowing the presence of Ge-4-rings in the d4r units. This feature allows the unexpected conversion of these materials to the corresponding CIT-5 and "-CIT-14" / CIT-14 / IST materials. Again, these features are further illustrated in the Examples.
[0066] One such method for determining the average number of Ge atoms in the d4r units is described in the Examples and involves the addition of fluoride ions to CIT-13 / OH germanosilicate and the determination of the average number of Ge atoms in the d4r units. 19 This involves measuring the F MAS-nmr spectrum.
[0067] Critical to the final structure of the CIT-13 / OH materials is their preparation in the complete absence of fluoride ions. As described herein, the crystalline microporous germanosilicate CIT-13 / OH compositions are (a) A source of silicon oxide (SiO2); (b) a source of germanium oxide (GeO2); and (c) an optional source of aluminum oxide, boron oxide, gallium oxide, hafnium oxide, iron oxide, tin oxide, titanium oxide, vanadium oxide, zinc oxide, zirconium oxide, or combinations or mixtures thereof; (d) at least one hydroxide salt of a substituted benzylimidazolium organic structure directing agent (OSDA) cation having the structure: [ka] (e) optionally, at least one compositionally matched seed crystal; and (f) water and hydrothermally treating the aqueous composition obtained from the mixture of: under conditions effective to crystallize a crystalline microporous germanosilicate composition designated CIT-13 / OH; wherein the aqueous composition comprises: (a) a molar ratio of Si:Ge ranging from 2 to 4, preferably from 2.5 to 3.0; (b) water with a water:Si molar ratio in the range of 8:1 to 12:1; (c) Water:(SiO2+GeO2) molar ratio in the range of 6:1 to 7:1; (c) Hydroxide ion (OH) with a molar ratio of OH:(SiO2+GeO2) in the range of approximately 0.3:1 to 0.7:1 wherein the aqueous composition is essentially free of fluoride ions.
[0068] These ranges are narrower than those previously reported. These narrower ranges are important for generating Ge-rich d4r units.
[0069] Within this framework, the method includes one or more of the following features.
[0070] (1) The source of silicon oxide can be any source known to be suitable for molecular sieve synthesis, but in preferred embodiments includes silicic acid, silica hydrogel, silicic acid, fumed silica, colloidal silica, tetraalkyl orthosilicate, silica hydroxide, or combinations thereof (or equivalent sources), preferably sodium silicate or tetraalkyl orthosilicate, even more preferably tetraethyl orthosilicate (TEOS).
[0071] (2) The source of germanium oxide can be any source known to be suitable for molecular sieve synthesis, including GeO2 or its hydrated derivatives (or equivalent sources).
[0072] (3) The substituted benzylimidazolium organic structure directing agent (OSDA) cation is present in a molar ratio of OSDA:(SiO2+GeO2) ranging from about 0.3:1 to 0.7:1, preferably from about 0.4:1 to 0.6:1.
[0073] (4) The aqueous composition contains an alkali metal cation, an alkaline earth metal cation, or an alkali metal cation. It is essentially free of thiones or combinations thereof.
[0074] (5) The at least one substituted benzyl imidazolium organic structure directing agent (OSDA) cation preferably has the following structure: [ka]
[0075] (6) The aqueous composition is a suspension or a gel.
[0076] (7) Effective crystallization conditions include exposing the mixture to a temperature of about 140° C. to about 180° C. for about 4 days to about 4 weeks.
[0077] (7) The aqueous composition is hydrothermally treated in a rotary oven.
[0078] (8) The method further comprising isolating the crystalline microporous germanosilicate solid composition.
[0079] The CIT-14 / IST described herein is compositionally distinct from the CIT-14 / ESP (ESP stands for ethoxysilylated pillared) structure previously reported in US Patent Application Publication No. 2017 / 0252729 (hereby incorporated by reference for all purposes or at least for the disclosures thereof). These previously reported CIT-14 / ESPs were prepared by treating a phyllosilicate of CIT-13P topology with a source of silica in the presence of a concentrated aqueous mineral acid (e.g., HCl or preferably HNO3) at one or more temperatures ranging from about 165°C to about 225°C for a time ranging from 12 hours to 48 hours to form an intermediate composition, followed by isolating and calcining the intermediate composition to form a crystalline microporous silicate composition of CIT-14 / ESP topology.
[0080] In particular, CIT-14 / ESP germanosilicates have been formed using CIT-13P phyllosicates having much higher Si:Ge ratios than described by the present method, resulting in CIT-14 / ESP germanosilicates with Si:Ge ratios ranging from about 25 to virtually infinity, including embodiments having Si:Ge ratios from about 25 to about 150, or from about 75 to about 150. The quality of the crystals formed by the ADOR process was lower than reported herein.
[0081] These CIT-14 / ESP germanosilicates exhibited powder X-ray diffraction (XRD) patterns not significantly different from those reported for CIT-14 / IST germanosilicates, with at least five characteristic peaks at 7.7, 8.2, 13.1, 19.5, 21.1, 22.7 and 27.6 degrees 2-θ. Due to the structural disorder of the material, The diffraction peaks observed were broad, and the error assigned to these peaks was ±0.5 degrees 2-θ. In other embodiments, the error associated with these peaks was ±0.3 degrees 2-θ. Consistent with other structures prepared by pillaring and the methods by which they can be made, the structure of this new material was described in terms of a three-dimensional framework with pores defined by 8- and 12-membered rings. Based on the theoretical structure, the dimensions of the 8- and 12-membered rings were calculated to be 4.0x3.4 Å and 6.9x5.4 Å, respectively (see FIG. 3(AB)). The PXRD patterns identified from the isolated products were not identical, but were consistent with the theoretical values associated with this structure (predicted by the General Utility Lattice Program, GULP (Gale, 1997)), i.e., with silica pillars separating the silica-rich cfi layers. Such differences in patterns were believed to be explained by structural disorder and / or imperfect silica pillaring. In this case, the CIT-14 / ESP version can also be described in terms of the crystallographic parameters shown in Figures 3(A) and 3(B).
[0082] [Table 5]
[0083] Other Changes in Microcrystalline Composition In certain embodiments, the crystalline microporous solids described herein, including the CIT-13 / OH germanosilicate and the newly described microcrystalline CIT-14 / IST germanosilicate, are present in their hydrogen form. In other embodiments, the crystalline microporous solids contain at least one metal cation salt or transition metal or salt within their micropores. In other specific embodiments, the metal cation salt is K + , Li + , Rb + , Ca 2+ , Cs + :Co 2+ , Cu 2+ , Mg 2+ , Sr2+ , B.A. 2+ , Ni 2+ , or Fe 2+ where the copper salt may include, for example, Schweizer's reagent (tetraamminediaquacopper dihydroxide, [Cu(NH3)4(H2O)2](OH)2]), copper(II) nitrate or copper(II) carbonate, etc. Such metal cations may be incorporated, for example, using techniques known to be suitable for this purpose (e.g., ion exchange).
[0084] In other embodiments, the micropores may contain a transition metal or transition metal oxide. Addition of such materials may be accomplished, for example, by chemical vapor deposition or chemical precipitation. In certain independent embodiments, the transition metal or transition metal oxide comprises an element of group 6, 7, 8, 9, 10, 11, or 12. In other independent embodiments, the transition metal or transition metal oxide comprises scandium, yttrium, titanium, zirconium, vanadium, manganese, chromium, molybdenum, tungsten, iron, ruthenium, osmium, cobalt, rhodium, iridium, nickel, palladium, platinum, copper, silver, gold, or mixtures. Fe, Ru, Os, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, and mixtures thereof are preferred. In separate embodiments, the aqueous ammonium salt or metal salt or chemically vapor deposited or precipitated material is independently selected from Li, Na, K, Rb, Cs, Be, Mg, Ca, Sr, Be, Al, Ga, In, Zn, Ag, Cd, Ru, Rh, Pd, Pt, Au, Hg, La, Ce, Pr, Nd, Pm, Sm, Eu, or R 4-n N + H n cations (R is alkyl and n=0-4 in at least some of the pores).
[0085] The term "transition metal" is defined elsewhere herein, however, in certain other independent embodiments, the transition metal or transition metal oxide comprises an element of Group 6, 7, 8, 9, 10, 11, or 12. In yet other independent embodiments, the transition metal or transition metal oxide comprises scandium, yttrium, titanium, zirconium, vanadium, manganese, chromium, molybdenum, tungsten, iron, ruthenium, osmium, cobalt, rhodium, iridium, nickel, palladium, platinum, copper, silver, gold, or mixtures. Fe, Ru, Os, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, and mixtures thereof are preferred dopants.
[0086] In other embodiments, the optionally doped crystalline solid is calcined in air at a temperature defined to be in the range of at least one of 400° C. to 500° C., 500° C. to 600° C., 600° C. to 700° C., 700° C. to 800° C., 800° C. to 900° C., 900° C. to 1000° C., 1000° C. to 1200° C., and 500° C. to about 1200° C. Selection of a particular temperature may in some cases be limited by the stability of the particular solid with respect to decomposition or transformation to another crystalline phase.
[0087] Other methods of modifying molecular sieves for use as catalysts will be known to those of skill in the art, and such additional modifications are considered to be within the scope of this disclosure.
[0088] Use of the Compositions of the Invention - Catalytic Conversion / Separation In various embodiments, the crystalline microporous germanosilicate solids as disclosed herein are calcined, doped or treated as described herein to act as catalysts to mediate or catalyze a series of chemical transformations or separations. All such combinations of compositions and catalytic reactions are considered individual embodiments of the present disclosure as if they were individually depicted separately. Use of these germanosilicates for these purposes is also within the scope of the present disclosure. Such conversions / separations include carbonylation of DME (dimethyl ether) with CO at low temperatures, reduction of NOx with methane (e.g., exhaust applications), cracking, hydrocracking, dehydrogenation, conversion of paraffins to aromatics, dewaxing of a hydrocarbon feedstock, MTO (methanol to olefins), isomerization of aromatics (e.g., xylenes), disproportionation of aromatics (e.g., toluene), alkylation of aromatic hydrocarbons, oligomerization of alkenes, amination of lower alcohols, separation and sorption of lower alkanes, hydrocracking of hydrocarbons, dewaxing of a hydrocarbon feedstock, isomerization of olefins, production of higher molecular weight hydrocarbons from lower molecular weight hydrocarbons, hydrocarbon reforming, conversion of lower alcohols or other oxygenated hydrocarbons to olefin products, epoxidation of olefins with hydrogen peroxide, reducing the content of nitrogen oxides in a gas stream in the presence of oxygen, or separation of nitrogen from a nitrogen-containing gas mixture, each of which is subjected to the process described herein under conditions sufficient to affect the specified conversion. and separations carried out by contacting the catalyst with a crystalline microporous solid of any one of the materials described in 1. Particularly attractive applications in which these germanosilicates are expected to be useful include catalytic cracking, hydrocracking, dewaxing, alkylation, and olefin and aromatics forming reactions. Additional applications include gas drying and separations.
[0089] Certain embodiments provide hydrocracking processes, each process comprising contacting a hydrocarbon feedstock under hydrocracking conditions with a catalyst comprising the crystalline microporous solid of the present disclosure, preferably predominantly in hydrogen form.
[0090] Still other embodiments provide processes for dewaxing a hydrocarbon feed, each process comprising contacting the hydrocarbon feed under dewaxing conditions with a catalyst comprising the crystalline microporous solid of the present disclosure. Still other embodiments provide processes for improving the viscosity index of a dewaxed product of a waxy hydrocarbon feed, each process comprising contacting the waxy hydrocarbon feed under isomerization dewaxing conditions with a catalyst comprising the crystalline microporous solid of the present disclosure.
[0091] Additional embodiments include processes for producing C20+ lubricants from a C20+ olefin feedstock, each process comprising isomerizing the olefin feedstock under isomerization conditions over a catalyst comprising at least one transition metal catalyst and a crystalline microporous solid of the present disclosure.
[0092] The present disclosure also includes processes for isomerization dewaxing a raffinate, each process comprising contacting the raffinate, e.g., bright stock, in the presence of added hydrogen with a catalyst comprising at least one transition metal and a crystalline microporous solid of the present disclosure.
[0093] Another embodiment is about 350 o The present invention provides a method for dewaxing a hydrocarbon oil feedstock boiling above F and containing straight chain and slightly branched chain hydrocarbons, comprising contacting the hydrocarbon oil feedstock with a catalyst comprising at least one transition metal and the crystalline microporous solid of the present disclosure, preferably predominantly in hydrogen form, in the presence of added hydrogen gas at a hydrogen pressure of about 15 to 3000 psi.
[0094] The present disclosure also includes a method for hydrocracking a hydrocarbon feedstock in a hydrocracking zone to obtain an effluent comprising a hydrocracked oil, and a method for producing a hydrocracked oil product comprising the steps of: hydrocracking a hydrocarbon feedstock in a hydrocracking zone to obtain an effluent comprising a hydrocracked oil product; and hydrocracking a hydrocarbon feedstock in a hydrocracking zone to obtain an effluent comprising a hydrocracked oil product in a hydrocracking zone to obtain an effluent comprising a hydrocracked oil product. The method includes the steps of hydrocracking a hydrocarbon feedstock in a hydrocracking zone to obtain an effluent comprising a hydrocracked oil product ... o and catalytically dewaxing said effluent comprising hydrocracked oil at a temperature of from about 15 psig to about 3000 psig.
[0095] The disclosure also includes processes for increasing the octane of a hydrocarbon feedstock to produce products with increased aromatic content, each process comprising contacting a hydrocarbon feedstock comprising linear and slightly branched hydrocarbons having a boiling range above about 40° C. and below about 200° C. under aromatics conversion conditions with a catalyst comprising the crystalline microporous solid of the disclosure. In these embodiments, the crystalline microporous solid is preferably rendered substantially acid free by neutralizing the solid with a basic metal. The disclosure also provides processes in which the crystalline microporous solid comprises a transition metal component.
[0096] Catalytic cracking processes are also provided by the present disclosure, each process comprising contacting a hydrocarbon feedstock with a catalyst comprising a crystalline microporous solid of the present disclosure in a reaction zone under catalytic cracking conditions in the absence of added hydrogen. Also included in the present disclosure are catalytic cracking processes in which the catalyst further comprises a large pore crystalline cracking component.
[0097] The present disclosure further provides isomerization processes for isomerizing C4-C7 hydrocarbons, each process comprising contacting a feed having linear and slightly branched C4-C hydrocarbons with a catalyst comprising a crystalline microporous solid of the present disclosure, preferably predominantly in hydrogen form, under isomerization conditions. The crystalline microporous solid may be impregnated with at least one transition metal, preferably platinum. The catalyst may be calcined at high temperature in a steam / air mixture after impregnation with the transition metal.
[0098] Also provided by the present disclosure are processes for alkylating aromatic hydrocarbons, each process comprising contacting at least a molar excess of an aromatic hydrocarbon with a C2-C20 olefin under alkylation conditions, under at least partial liquid phase conditions, in the presence of a catalyst comprising the crystalline microporous solid of the present disclosure, preferably predominantly in hydrogen form. The olefin may be a C2-C4 olefin, and the aromatic hydrocarbon and olefin may be present in a molar ratio of about 4:1 to about 20:1, respectively. The aromatic hydrocarbon may be selected from the group consisting of benzene, toluene, ethylbenzene, xylene, or mixtures thereof.
[0099] Further provided in accordance with the present disclosure are processes for transalkylating aromatic hydrocarbons, each of which comprises contacting an aromatic hydrocarbon with a polyalkyl aromatic hydrocarbon under transalkylation conditions under at least partial liquid phase conditions in the presence of a catalyst comprising the crystalline microporous solid of the present disclosure, preferably in predominantly hydrogen form. The aromatic hydrocarbon and the polyalkyl aromatic hydrocarbon may be present in a molar ratio of about 1:1 to about 25:1, respectively. The aromatic hydrocarbon may be selected from the group consisting of benzene, toluene, ethylbenzene, xylene or mixtures thereof, and the polyalkyl aromatic hydrocarbon may be a dialkylbenzene.
[0100] Further provided by the present disclosure are processes for converting paraffins to aromatics, each of which comprises contacting paraffins with a catalyst comprising a crystalline microporous solid of the present disclosure under conditions to convert the paraffins to aromatics, said catalyst comprising gallium, zinc, or a compound of gallium or zinc.
[0101] Also provided in accordance with the present disclosure are processes for isomerizing olefins, each process comprising contacting an olefin with a catalyst comprising the crystalline microporous solid of the present disclosure under conditions that cause isomerization of the olefin.
[0102] Further in accordance with the present disclosure, there are provided processes for isomerizing an isomerization feedstock, each of which comprises an aromatic C8 stream of xylene isomers or a mixture of xylene isomers and ethylbenzene, wherein a more equilibrium ratio of ortho, meta and para-xylene is obtained, said processes comprising contacting said feedstock under isomerization conditions with a catalyst comprising the crystalline microporous solid of the present disclosure.
[0103] The present disclosure further provides processes for oligomerizing olefins, each process comprising contacting an olefin feedstock under oligomerization conditions with a catalyst comprising the crystalline microporous solid of the present disclosure.
[0104] The present disclosure also provides processes for converting lower alcohols and other oxygenated hydrocarbons, each process comprising contacting the lower alcohol (e.g., methanol, ethanol, or propanol) or other oxygenated hydrocarbon with a catalyst comprising the crystalline microporous solid of the present disclosure under conditions to produce a liquid product.
[0105] The present disclosure also provides a process for reducing nitrogen oxides in a gas stream in the presence of oxygen. are provided, each process comprising contacting a gas stream with a crystalline microporous solid of the present disclosure. The crystalline microporous solid may comprise a metal or metal ion (such as cobalt, copper or mixtures thereof) capable of catalyzing the reduction of nitrogen oxides, and may be carried out in the presence of a stoichiometric excess of oxygen. In a preferred embodiment, the gas stream is the exhaust stream of an internal combustion engine.
[0106] Also provided is a process for converting synthesis gas, also referred to as syngas, containing hydrogen and carbon monoxide, to liquid hydrocarbon fuels using a catalyst comprising any of the germanosilicates described herein, including those having a CIT-13 framework, and a Fischer-Tropsch catalyst. Such catalysts are described in U.S. Pat. No. 9,278,344, which is incorporated by reference for its teaching of catalysts and methods of using the catalysts. The Fischer-Tropsch component comprises a Group 8-10 transition metal component (i.e., Fe, Ru, Os, Co, Rh, Ir, Ni, Pd, Pt), preferably cobalt, iron and / or ruthenium. The optimum amount of catalytically active metal present will depend, among other things, on the particular catalytically active metal. Typically, the amount of cobalt present in the catalyst may range from 1 to 100 parts by weight per 100 parts by weight of support material, preferably from 10 to 50 parts by weight per 100 parts by weight of support material. In one embodiment, 15 to 45% by weight of cobalt is deposited on the hybrid support as the Fischer-Tropsch component. In another embodiment, 20-45 wt% cobalt is deposited on the hybrid support. The catalytically active Fischer-Tropsch component may be present in the catalyst along with one or more metal promoters or cocatalysts. The promoters may be present as metals or metal oxides, depending on the particular promoter involved. Suitable promoters include oxides of metals or transition metals, including lanthanides and / or actinides or oxides of lanthanides and / or actinides. As an alternative to, or in addition to, a metal oxide promoter, the catalyst may include a metal promoter selected from Group 7 (Mn, Tc, Re) and / or Groups 8-10. In some embodiments, the Fischer-Tropsch component further includes a cobalt reduction promoter selected from the group consisting of platinum, ruthenium, rhenium, silver, and combinations thereof. The methods employed to deposit the Fischer-Tropsch components onto the hybrid supports include impregnation techniques using aqueous or non-aqueous solutions containing a soluble cobalt salt and optionally a soluble promoter metal salt, such as a platinum salt, to achieve the metal loading and distribution required to provide a highly selective and active hybrid syngas conversion catalyst.
[0107] Yet further process embodiments include those for reducing halogen compound concentrations in an initial hydrocarbon product containing undesirable levels of organohalogen compounds, the process comprising contacting at least a portion of the hydrocarbon product with a composition comprising any of the germanosilicate structures described herein, including CIT-13, under organohalogen absorption conditions to reduce the halogen concentration in the hydrocarbon. The initial hydrocarbon product may be produced by a hydrocarbon conversion process using an ionic liquid catalyst comprising a halogen-containing acidic ionic liquid. In some embodiments, the organohalide content in the initial hydrocarbon product ranges from 50 to 4000 ppm, and in other embodiments, the halogen concentration is reduced to provide a product with less than 40 ppm. In other embodiments, the production may achieve a reduction of 85%, 90%, 95%, 97% or more. The initial hydrocarbon stream may comprise an alkylate or gasoline alkylate. Preferably, the hydrocarbon alkylate or alkylate gasoline product is not cracked during contacting. Any of the materials or process conditions described in U.S. Pat. No. 8,105,481 are considered illustrative of the range of materials and process conditions of the present disclosure. No. 8,105,481 is incorporated by reference at least for its teachings regarding the methods and materials used to effect such transformations, both alkylation and halogen reduction.
[0108] Yet further process embodiments include a process for increasing the octane of a hydrocarbon feedstock to produce a product having increased aromatics content, which, under aromatic conversion conditions, comprises: The process involves contacting a hydrocarbon feedstock, which includes linear and slightly branched hydrocarbons having a boiling range above about 40° C. and below about 200° C., with a catalyst.
[0109] The specific conditions for many of these transformations are known to those of skill in the art. Exemplary conditions for such reactions / transformations can also be found in WO / 1999 / 008961, U.S. Patent Nos. 4,544,538, 7,083,714, 6,841,063, and 6,827,843, each of which is incorporated herein by reference in its entirety for at least these purposes.
[0110] Depending on the type of reaction being catalyzed, the microporous solid may be predominantly in hydrogen form, partially acidic, or substantially free of acid. Those skilled in the art will be able to define these conditions without undue effort. As used herein, "predominantly in hydrogen form" refers to the solid after calcination (precalcination of the precalcined material with NH4 + means that at least 80% of the cationic sites are occupied by hydrogen ions and / or rare earth ions.
[0111] The germanosilicates of the present disclosure may also be used as adsorbents for gas separation. For example, these germanosilicates may also be used as hydrocarbon traps, such as cold start hydrocarbon traps in combustion engine pollution control systems. In particular, such germanosilicates are believed to be particularly useful for trapping C3 fragments. Such embodiments may include processes and devices for trapping low molecular weight hydrocarbons from an incoming gas stream, the process comprising passing the gas stream across or through a composition comprising any one of the crystalline microporous germane silicate compositions described herein to provide an outgoing gas stream having a reduced concentration of low molecular weight hydrocarbons compared to the incoming gas stream. In this context, the term "low molecular weight hydrocarbons" refers to C1-C6 hydrocarbons or hydrocarbon fragments.
[0112] The germanosilicates of the present disclosure may also be used in a process for treating a cold-start engine exhaust gas stream containing hydrocarbons and other pollutants, the process comprising or consisting of flowing the engine exhaust gas stream over one of the germanosilicate compositions of the present disclosure that preferentially adsorbs hydrocarbons over water to provide a first exhaust stream, flowing the first exhaust gas stream over a catalyst to convert residual hydrocarbons and other pollutants contained in the first exhaust gas stream into harmless products to provide a treated exhaust stream, and exhausting the treated exhaust stream to the atmosphere.
[0113] The germanosilicates of the present disclosure can also be used to separate gases. For example, they can be used to separate water, carbon dioxide and sulfur dioxide from fluid streams such as low-grade natural gas streams, and carbon dioxide from natural gas. Typically, molecular sieves are used as components of membranes used to separate gases. Examples of such membranes are disclosed in U.S. Pat. No. 6,508,801.
[0114] For each of the above processes described, additional corresponding embodiments include those that include an apparatus or system that includes or contains the materials described for each process. For example, in gas trapping gases, additional embodiments include an apparatus known in the art as a hydrocarbon trap that can be placed in the exhaust gas flow path of a vehicle. In such an apparatus, the hydrocarbons are adsorbed on the trap and stored until the engine and exhaust reach a temperature sufficient for desorption. The apparatus can also include a membrane that includes a germanosilicate composition useful in the described processes.
[0115] (term) In this disclosure, the singular forms "a," "an," and "the" include plural references and a reference to a particular value includes at least that particular value unless the context clearly dictates otherwise. Thus, for example, a reference to a "substance" is a reference to at least one of such substances and / or equivalents thereof known to one of ordinary skill in the art.
[0116] When values are expressed as approximations by use of the descriptor "about", it will be understood that the particular value forms another embodiment. In general, the use of the term "about" indicates an approximation that may vary depending on the desired properties sought to be obtained by the disclosed subject matter and is to be interpreted in the particular context in which it is used based on its function. Those skilled in the art will be able to interpret this as a routine matter. In some cases, the number of significant figures used for a particular value may be one non-limiting way of determining the scope of the word "about". In other cases, the gradations used in a series of values may be used to determine the intended range available to the term "about" for each value. When present, all ranges are inclusive and combinable. That is, reference to values stated within a range includes all values within that range.
[0117] For clarity, it will be understood that certain features of the present disclosure that are described herein in the context of separate embodiments can also be provided in combination in a single embodiment. That is, unless expressly incompatible or expressly excluded, each embodiment is considered to be combinable with any other embodiment, and such combination is considered to be another embodiment. Conversely, for brevity, various features of the present disclosure that are described in the context of a single embodiment can also be provided separately or in any subcombination. Finally, while an embodiment may be described as part of a series of steps or as part of a more general structure, each said step can also be considered to be an independent embodiment in itself and combinable with others.
[0118] The transition terms "comprising," "consisting essentially of," and "consisting of" are intended to connote the generally accepted meaning in patent language, i.e., (i) "comprising," which is synonymous with "included," "containing," or "characterized by," is inclusive or open-ended and does not exclude additional, unrecited elements or method steps; (ii) "consisting of" excludes elements, steps, or ingredients not specified in the claim; and (iii) "consisting essentially of" limits the scope of the claim to certain materials or steps and those that do not "materially affect the basic and novel characteristics" of the claimed disclosure. The embodiments described with respect to the phrase "comprising" (or its equivalent) also provide embodiments described independently with respect to "consisting of" and "consisting essentially of." For the embodiments provided with respect to "consisting essentially of," the basic and novel characteristic is the ease of operation of the method or composition / system to provide germanosilicate compositions in meaningful yields, or the ability of the system to use only the recited ingredients.
[0119] The term "meaningful product yield" is intended to reflect a product yield as described herein, including greater than 20%, although where specified, the term may also refer to a yield of 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80% or 90% or more relative to the amount of original substrate.
[0120] When lists are presented, unless otherwise stated, each individual element of the list, and every combination of the list, is understood to be a separate embodiment. For example, a list of embodiments presented as "A, B, or C" is to be interpreted as including the embodiments "A," "B," "C," "A or B," "A or C," "B or C," or "A, B, or C," as separate embodiments.
[0121] Throughout this specification, words shall be given their ordinary meanings as understood by those of ordinary skill in the art. However, to avoid any doubt, the meaning of certain terms will be specifically defined or clarified.
[0122] As used herein, the term "alkyl" refers to a saturated hydrocarbon group which may, but need not necessarily, contain from 1 to about 6 carbon atoms, and which is typically straight-chained, branched, or cyclic, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, and the like.
[0123] The term "aromatic" refers to cyclic moieties that satisfy the Huckel 4n+2 rule of aromaticity, and includes both aryl (ie, carbocyclic) and heteroaryl structures.
[0124] The term "halide" is used in its conventional sense to refer to chloride, bromide, fluoride, or iodide.
[0125] "Lower alcohol" or lower alkane means an alcohol or alkane, respectively, having 1 to 10 carbon atoms, linear or branched, preferably having 1 to 6 carbon atoms, preferably linear. Methanol, ethanol, propanol, butanol, pentanol, and hexanol are examples of lower alcohols. Methane, ethane, propane, butane, pentane, and hexane are examples of lower alkanes.
[0126] As used herein, unless otherwise specified, the term "high temperature" typically refers to at least one temperature in the range of about 170°C to about 230°C. The term "calcination" is reserved for higher temperatures. Unless otherwise specified, it refers to one or more temperatures in the range of about 450°C to about 800°C.
[0127] As used herein, the term "metal or metalloid" refers to elements in Groups 4, 5, 8, 13, 14, and 15 of the periodic table, such as in a "source of metal or metalloid" or an "oxide of metal or metalloid". These elements are typically included in the molecular sieve as oxides, and include, for example, aluminum, boron, gallium, hafnium, iron, silicon, tin, titanium, vanadium, zinc, zirconium, or combinations thereof.
[0128] Typical sources of silicon oxide for the reaction mixture include silicon alkoxides, hydroxides or oxides, or combinations thereof. Exemplary compounds also include silicates (including sodium silicate), silica hydrogels, silicic acid, fumed silica, colloidal silica, tetraalkyl orthosilicates, silica hydroxides, or combinations thereof. Sodium silicate or tetraalkyl orthosilicates, such as tetraethyl orthosilicate (TEOS), diethoxydimethylsilane (DEDMS) and / or 1,3-diethoxy-1,1,3,3-tetramethyldisiloxane (DETMDS), are preferred sources.
[0129] Sources of germanium oxide include alkali metal orthogermanates, isolated GeO4 4‐ M4GeO4, GeO(OH)3 containing ions ‐ , GeO2(OH)2 2‐ , [(Ge(OH)4)8(OH)3] 3‐ or a neutral solution of germanium dioxide comprising Ge(OH)4 or its alkoxide or carboxylate derivatives.
[0130] Typical sources of aluminum oxide for the reaction mixture include aluminates, alumina, aluminum colloids, aluminum alkoxides, aluminum oxide coated on silica sol, hydrated alumina gels such as Al(OH)3, and sodium aluminate. Sources of aluminum oxide may also include aluminum alkoxides, hydroxides, or oxides, or combinations thereof. Additionally, sources of alumina may also include other Ligands such as acetylacetonate, carboxylate, and oxalate may also be included; such compounds are well known to be useful in hydrothermal or sol-gel synthesis. Additional sources of aluminum oxide may include aluminum salts such as AlCl3, Al(OH)3, Al(NO3)3, and Al2(SO4)3.
[0131] Sources of boron oxide, gallium oxide, hafnium oxide, iron oxide, tin oxide, titanium oxide, indium oxide, vanadium oxide and / or zirconium oxide can be added in forms corresponding to their aluminum and silicon counterparts.
[0132] As used herein, the term "mineral acid" refers to mineralizing acids conventionally used in molecular sieve zeolite synthesis, such as HCl, HBr, HF, HNO3, or H2SO4. Oxalic acid and other strong organic acids can also be used in place of mineral acids. Generally, HCl and HNO3 are preferred mineral acids. As used throughout this specification, the terms "concentrated" and "dilute" with respect to mineral acids refer to concentrations greater than 0.5M and less than 0.5M, respectively. In some embodiments, the term "concentrated" refers to one or more of the following concentrations: 0.5-0.6, 0.6-0.7, 0.7-0.8, 0.8-0.9, 0.9-1.0, 1.0-1.1, 1.1-1.2, 1.2-1.3, 1.3-1.4, 1.4-1.5, 1.5-1.6, 1.6-1.7, 1.7-1.8, 1.8-1.9, 1.9-2.0, or more. In the experiments and preferred embodiments described herein, concentrated acid refers to one in the composition range of 0.9-1.1 M. Similarly, the term "dilute" refers to one or more of the following concentrations: 0.5-0.4, 0.4-0.3, 0.3-0.2, 0.2-0.15, 0.15-0.1, and 0.1-0.05. In the experiments and preferred embodiments described herein, dilute acid refers to those in the composition range of 0.5-0.15M.
[0133] The term "CIT-13" topology refers to a crystalline microporous composition similar to that described in U.S. Patent No. 10,293,330, having a set of orthogonally oriented 14-membered pores. The term "phyllosilicate" refers to a two-dimensional layered structure of silica-containing oxides, as described in U.S. Patent Application Publication No. 2017 / 0252729.
[0134] The term "oxygenated hydrocarbon" or "oxygenates" as known in the art of hydrocarbon processing refers to components including alcohols, aldehydes, carboxylic acids, ethers and / or ketones that are known to be present in hydrocarbon streams or obtained from other sources in biomass streams (e.g., ethanol from fermented sugars).
[0135] The term "separate" or "separated" has its ordinary meaning as would be understood by one of ordinary skill in the art insofar as it refers to physically dividing or isolating a solid product material from other starting materials or co-products or by-products (impurities) associated with the reaction conditions that produce the material. Thus, one of ordinary skill in the art is presumed to at least recognize the presence of the product and take certain actions to separate or isolate it from the starting materials and / or co-products or by-products. Absolute purity is not required, but is preferred. When these terms are used in the context of gas processing, the term "separate" or "separated" refers to the partitioning of gases by adsorption or by permeation based on size or physical or chemical properties, as would be understood by one of ordinary skill in the art.
[0136] Unless otherwise specified, the term "isolated" means physically separated from other components, at least free of solvent or other impurities, such as starting materials, co-products, or by-products. In some embodiments, isolated crystalline materials can be considered isolated, for example, when separated from the reaction mixture that gave rise to their preparation, from mixed phase co-products, or from both. In some of these embodiments, pure germanosilicates (including structures with or without incorporated OSDA) can be prepared by: The crystal phases may be directly produced from the methods described. In some cases, the crystalline phases may not be able to be separated from one another, in which case the term "isolated" may refer to separation from their source composition.
[0137] According to IUPAC notation, the term "microporous" refers to a material with a pore size of less than 2 nm. Similarly, the term "macroporous" refers to a material with a pore size of more than 50 nm. And the term "mesoporous" refers to a material with a pore size intermediate between microporous and macroporous. In the context of this disclosure, the material properties and applications are determined by the properties of the scaffold, such as pore size and diameter, cage dimensions, and material composition. For this reason, there is often only one scaffold and composition that performs optimally in a desired application.
[0138] "Optional" or "optionally" means that the subsequently described situation may or may not occur, and thus the description includes instances where the situation occurs and instances where it does not occur. For example, the phrase "optionally substituted" means that non-hydrogen substituents may or may not be present on a given atom, and thus the description includes structures where non-hydrogen substituents are present and structures where non-hydrogen substituents are not present.
[0139] The terms "method" and "process" are considered interchangeable within this disclosure.
[0140] As used herein, the terms "crystalline microporous solids" or "crystalline microporous germanosilicates" are crystalline structures with highly regular pore structures of molecular dimensions, i.e., less than 2 nm. The maximum size of species that can enter the pores of crystalline microporous solids is controlled by the dimensions of the channels. These terms may also refer specifically to the CIT-13 composition.
[0141] As used herein, the term "pillaring" generally refers to the process of introducing stable metal oxide structures (so-called "pillars") between substantially parallel crystalline silicate layers. The metal oxide structures maintain the separation of the silicate layers and are created by interlayer spacing of molecular dimensions. The term is generally used in the context of clay chemistry and is well understood by those skilled in the art of clays and zeolites, particularly as applied to catalysis.
[0142] The term "germanosilicate" refers to any composition that contains silicon and germanium oxides in its framework. The terms "pure" and "pure germanosilicate" mean that these compositions contain, as far as practicable, only germania and silica, respectively, with other metal oxides in the framework being present as unavoidable and unintentional impurities. The germanosilicates may be "pure germanosilicates" or may be optionally substituted with other metal oxides or semi-metal oxides. Similarly, the terms aluminosilicate, borosilicate, ferrosilicate, stannosilicate, titanosilicate or zincosilicate structures contain silicon oxide and oxides of aluminum, boron, iron, tin, titanium and zinc, respectively. Where "optionally substituted" is described, each backbone may contain aluminum, boron, gallium, germanium, hafnium, iron, tin, titanium, indium, vanadium, zinc, zirconium or other atoms or oxides substituted with one or more of the atoms or oxides not already included in the parent backbone.
[0143] As used herein, the term "transition metal" refers to any element in the d-block of the periodic table, including groups 3-12 of the periodic table. In fact, the lanthanide and actinide series of the f-block are also considered transition metals and are referred to as "inner transition metals." This definition of transition metal also encompasses elements of groups 3-12. In certain other independent embodiments, the transition metal or transition metal oxide comprises an element of groups 6, 7, 8, 9, 10, 11, or 12. Still other In an independent embodiment, the transition metal or transition metal oxide comprises scandium, yttrium, titanium, zirconium, vanadium, manganese, chromium, molybdenum, tungsten, iron, ruthenium, osmium, cobalt, rhodium, iridium, nickel, palladium, platinum, copper, silver, gold or mixtures. Fe, Ru, Os, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au and mixtures thereof are preferred dopants.
[0144] The following list of embodiments is intended to supplement, not replace or supplant, the preceding discussion.
[0145] (Embodiment 1) A crystalline microporous germanosilicate composition, designated CIT-14 / IST, having 8- and 12-ring channels.
[0146] (Embodiment 2) The crystalline microporous germanous silicate CIT-14 / IST composition of embodiment 1, characterized in that the powder X-ray diffraction (XRD) pattern has at least five characteristic peaks at 7.59±0.5, 8.07±0.5, 12.88±0.5, 19.12±0.5, 19.32±0.5, 20.73±0.5, 22.33±0.5, 24.37±0.5, 27.19±0.5, and 27.69±0.5 degrees 2-θ. In a particular aspect of this embodiment, the CIT-14 / IST germanous silicate composition comprises a pure germanous silicate. In another independent aspect of this embodiment, the CIT-14 / IST germanous silicate composition comprises a framework comprising one or more oxides of aluminum, boron, gallium, hafnium, iron, tin, titanium, vanadium, zinc, or zirconium. In certain independent aspects of this embodiment, the powder X-ray diffraction (XRD) pattern exhibits at least five characteristic peaks at 5, 6, 7, 8, 9, or 10 of these characteristic peaks above. In certain independent aspects of this embodiment, the uncertainty in the peak positions is independently (for each peak) ±0.5 degrees 2-θ, ±0.4 degrees 2-θ, ±0.3 degrees 2-θ, ±0.2 degrees 2-θ, ±0.15 degrees 2-θ, or ±0.15 degrees 2-θ.
[0147] (Embodiment 3) The crystalline microporous germanosilicate CIT-14 / IST composition of embodiment 1 or 2, characterized in that the powder X-ray diffraction (XRD) pattern exhibits at least three characteristic peaks at 7.59±0.5, 8.07±0.5, 19.12±0.5, 20.73±0.5 and 22.33±0.5 degrees 2-θ, and optionally at 12.88±0.5, 19.32±0.5, 24.37±0.5, 27.19±0.5 and 27.69±0.5 degrees 2-θ. The data in Table 1 and the comments above in connection with that table are considered independent aspects of this embodiment.
[0148] (Embodiment 4) The crystalline microporous germanosilicate CIT-14 / IST composition according to any one of the preceding embodiments, having a Si:Ge ratio in the range of 12:1 to 13:1, 13:1 to 14:1, 14:1 to 15:1, 15:1 to 16:1, 16:1 to 17:1, 17:1 to 18:1, 18:1 to 19:1, 19:1 to 20:1, or any combination of two or more of these aforesaid subranges, such as 14:1 to 18:1. Each of these ranges is considered an independent aspect within this embodiment.
[0149] (Embodiment 5) The crystalline microporous germanosilicate CIT-14 / IST composition according to any one of the preceding embodiments, wherein the crystals are orthorhombic and have the Cmmm or Cmcm space group or an intracrystalline mixture (disorder) of the two domains.
[0150] (Embodiment 6) The crystalline microporous germanosilicate CIT-14 / IST composition according to any one of embodiments 1 to 5, having unit cell parameters according to:
[0151] [Table 6]
[0152] (Embodiment 7) The crystalline microporous germanosilicate CIT-14 / IST composition according to any one of the first to sixth embodiments, wherein the 8-ring channels have a pore size of about 3.3 Å×3.9 Å and the 12-ring channels have a pore size of about 4.9 Å×6.4 Å. In a particular aspect of this embodiment, the respective pore sizes are 3.26 Å×3.93 Å and 4.86 Å×6.44 Å. These values may change due to physical strain (e.g., compression) or the Si:Ge ratio. In a particular aspect of this embodiment, the average metal-oxygen (TO) bond length in the framework is in the range of 1.55-1.65 Å, and the average oxygen-metal-oxygen (OTO) bond length in the framework is 98-1.55 Å. o ~116 oThe average metal-oxygen-metal (TOT) ratio in the framework is 139 o ~180 o in the range.]
[0153] (Embodiment 8) The method of any one of embodiments 1 to 7, which is derived or derivable from a reaction characterized as an inverse sigma transformation of a crystalline microporous germanosilicate designated CIT-13 / OH. The specific properties of the crystalline microporous germanosilicate CIT-14 / IST composition according to any one of the preceding claims, CIT-13 / OH, are described in more detail elsewhere herein, and these descriptions are incorporated herein as if physically incorporated.
[0154] (Embodiment 9) A crystalline microporous germanosilicate CIT-14 / IST composition according to any one of embodiments 1 to 8, prepared by contacting a crystalline microporous germanosilicate designated CIT-13 / OH (described elsewhere herein) with a concentrated aqueous mineral acid (e.g., as a dispersion of germanosilicate in aqueous acid) at elevated temperature for a sufficient time to form the as-formed microporous germanosilicate "-CIT-14" (also described elsewhere herein, and these descriptions are incorporated herein).
[0155] In a particular aspect of this embodiment, (a) the mineral acid is aqueous HCl or HNO3 or an equivalent strong acid; (b) the concentration of the mineral acid is in the range of 6-12M; (c) the elevated temperature is in the range of 80°C-120°C, preferably about 95°C; (d) the sufficient time is in the range of 4-96 hours, preferably 4-24 hours; conditions equivalent to 6 hours at 95°C are suitable; (e) following contact with the acid, the resulting degermanized germanosilicate is isolated, which is a material designated "-CIT-14"; (f) the "-CIT-14" material is rinsed with water (preferably distilled or deionized water) until the pH of the wash solution is neutral; (g) the conditions further comprise heating the isolated and washed "-CIT-14" material at a temperature in the range of about 450°C-650°C for a time in the range of 2-12 hours, preferably 580°C for 6 hours, more preferably at a temperature ramp rate of 1°C / min.
[0156] (Embodiment 10) A crystalline microporous germanosilicate designated CIT-13 / OH, which is fluoride-free, has a three-dimensional framework with pores defined by 10- and 14-membered rings, and exhibits a powder X-ray diffraction (XRD) pattern with at least five peaks at 6.45±0.2, 7.18±0.2, 12.85±0.2, 20.78±0.2, 26.01±0.2, and 26.68±0.2 degrees 2-θ. In some aspects of this embodiment, the peak at 6.45±0.2 degrees 2-θ is reduced in intensity (weaker) compared to the peak at 7.18±0.2 degrees 2-θ, the latter peak being the most intense in the pattern (see Examples). In other aspects of this embodiment, the powder XRD pattern exhibits an additional peak at 11.58°±0.2° 2-θ. The data in Table 2 and the associated comments are considered independent aspects of this embodiment.
[0157] This composition of CIT-13 / OH germanosilicate is considered an independent embodiment of the present disclosure, as is its use in the preparation of CIT-14 / IST.
[0158] (Embodiment 11) The crystalline microporous germanosilicate CIT-14 / IST composition of embodiment 8 or 9 or the crystalline microporous germanosilicate CIT-13 / OH of embodiment 10, wherein the crystalline microporous germanosilicate designated CIT-13 / OH is (a) A source of silicon oxide (SiO2); (b) a source of germanium oxide (GeO2); and (c) an optional source of aluminum oxide, boron oxide, gallium oxide, hafnium oxide, iron oxide, tin oxide, titanium oxide, vanadium oxide, zinc oxide, zirconium oxide, or combinations or mixtures thereof; (d) at least one hydroxide salt of a substituted benzylimidazolium organic structure directing agent (OSDA) cation having the structure: [ka] (e) optionally, at least one compositionally matched seed crystal; and (f) water and hydrothermally treating an aqueous composition resulting from the mixture of: under conditions effective to crystallize a crystalline microporous germanosilicate composition designated CIT-13 / OH, wherein the aqueous composition comprises: (a) a molar ratio of Si:Ge ranging from 2 to 4, preferably from 2.5 to 3.0; (b) water with a water:Si molar ratio in the range of 8:1 to 12:1; (c) Water:(SiO2+GeO2) molar ratio in the range of 6:1 to 7:1; (c) Hydroxide ion (OH) with a molar ratio of OH:(SiO2+GeO2) in the range of approximately 0.3:1 to 0.7:1 wherein the aqueous composition is essentially free of fluoride ions; the crystalline microporous germanosilicate CIT-14 / IST composition of embodiment 8 or 9 or the crystalline microporous germanosilicate CIT-13 / OH of embodiment 10.
[0159] In an independent aspect of this embodiment,
[0160] (1) Sources of silicon oxide include silicic acid, silica hydrogel, silicic acid, fumed silica, colloidal silica, tetraalkyl orthosilicate, silica hydroxide or combinations thereof (or equivalent sources), preferably sodium silicate or tetraalkyl orthosilicate, more preferably tetraethyl orthosilicate (TEOS).
[0161] (2) Sources of germanium oxide include GeO2 or its hydrated derivatives (or equivalent sources).
[0162] (3) The substituted benzylimidazolium organic structure directing agent (OSDA) cation is present in a molar ratio of OSDA:(SiO2+GeO2) ranging from about 0.3:1 to 0.7:1, preferably from about 0.4:1 to 0.6:1.
[0163] (4) The aqueous composition is essentially free of alkali metal cations, alkaline earth metal cations, or dications, or combinations thereof.
[0164] (5) At least one substituted benzyl imidazolium organic structure directing agent (OSDA) cation has the following structure: [ka]
[0165] (6) The aqueous composition is a suspension or a gel.
[0166] (7) Effective crystallization conditions include exposing the mixture to a temperature of about 140° C. to about 180° C. for about 4 days to about 4 weeks.
[0167] (7) The aqueous composition is hydrothermally treated in a rotary oven.
[0168] (8) The method further comprising isolating the crystalline microporous germanosilicate solid composition.
[0169] (Embodiment 12) The crystalline microporous germanosilicate CIT-14 / IST composition of embodiment 8, 9 or 11 or the crystalline microporous germanosilicate CIT-13 / OH of embodiment 10 or 11, wherein the crystalline microporous germanosilicate, designated CIT-13 / OH, is fluoride-free and has d4r units with an average of at least 4, preferably more than 4, Ge atoms per d4r unit, allowing for the presence of Ge4 rings in the d4r units. Methods for determining the average number of Ge atoms in the d4r units are described elsewhere and are incorporated into this embodiment. In some independent aspects of this embodiment, the Si:Ge ratio is in the range of 3.5-3.6, 3.6-3.7, 3.7-3.8, 3.8-3.9, 3.9-4.0, 4.0-4.1, 4.1-4.2, 4.2-4.3, 4.3-4.4, 4.4-4.5, 4.5-4.6, 4.6-4.7, 4.7-4.8, 4.8-4.9, 4.9-5.0, 5.0-5.2, or a range defined by any two or more of the foregoing ranges, e.g., 3.5-3.9. Each of these ranges is considered an independent aspect within this embodiment.
[0170] (Embodiment 13) The crystalline microporous germanosilicate CIT-14 / IST composition of embodiment 8, 9, 11 or 12, or the crystalline microporous germanosilicate CIT-13 / OH of any one of embodiments 10-12, containing micropores that optionally contain an alkali metal cation salt, an alkaline earth metal salt, a transition metal, a transition metal oxide, a transition metal salt, or a combination thereof. The nature of the salt, metal, and metal oxide are discussed elsewhere in this specification and are incorporated into this embodiment. In certain aspects of this embodiment, each germanosilicate is in its hydrogen form. In other aspects of this embodiment, each germanosilicate contains one or more of a salt, a metal, or a metal oxide within its micropores.
[0171] (Embodiment 14) A catalyst comprising the crystalline microporous germanosilicate CIT-14 / IST composition according to any one of embodiments 1 to 9 or 11 to 13, or the crystalline microporous germanosilicate CIT-13 / OH according to any one of embodiments 10 to 13.
[0172] (Embodiment 15) A process for affecting an organic transformation or separating a substance, comprising the steps of: (a) Carbonylation of DME with CO at low temperature; (b) reducing NOx with methane; (c) Cracking, hydrocracking or dehydrogenating hydrocarbons; (d) dewaxing the hydrocarbon feed; (e) converting paraffins to aromatic compounds; (f) isomerizing or heterogenizing an aromatic feedstock; (g) alkylating aromatic hydrocarbons; (h) oligomerizing alkenes; (i) aminating a lower alcohol; (j) separating and sorbing lower alkanes from a hydrocarbon feedstock; (k) isomerizing olefins; (l) Producing higher molecular weight hydrocarbons from lower molecular weight hydrocarbons; (m) reforming hydrocarbons; (n) converting lower alcohols or other oxygenated hydrocarbons to produce olefin products (including MTO); (o) epoxidizing an olefin with hydrogen peroxide; (p) reducing the nitrogen oxide content of a gas stream in the presence of oxygen; (q) Separating nitrogen from a nitrogen-containing gas mixture; or (r) converting synthesis gas containing hydrogen and carbon monoxide into a hydrocarbon stream; or (s) Reducing the concentration of organic halides in the initial hydrocarbon product. 15. A process comprising:
[0173] (Embodiment 16) A method for preparing the crystalline microporous germanosilicate CIT-14 / IST composition of any one of embodiments 1-9 or 11-13 (or any of the compositions referred to as CIT-14 / IST elsewhere herein), comprising contacting at least the crystalline microporous germanosilicate referred to as CIT-13 / OH as described in any one of embodiments 10-12 (or described elsewhere herein) with concentrated aqueous mineral acid (e.g., as a dispersion of germanosilicate in aqueous acid) at elevated temperature for a time sufficient to form the as-formed microporous germanosilicate "-CIT-14" (also described elsewhere herein, and those descriptions are incorporated herein).
[0174] In particular aspects of this embodiment, (a) the mineral acid is aqueous HCl or HNO3 or an equivalent strong acid; (b) the concentration of the mineral acid is in the range of 6-12M; (c) the elevated temperature is in the range of 80°C to 120°C, preferably about 95°C; (d) the sufficient time is in the range of 4-96 hours, preferably 4-24 hours; conditions equivalent to 6 hours at 95°C are suitable; (e) following contact with the acid, the resulting degermanized germanosilicate is isolated, a material designated "-CIT-14"; (f) the "-CIT-14" material is rinsed with water (preferably distilled or deionized) until the pH of the wash solution is neutral.
[0175] (Embodiment 17) The method of embodiment 16, further comprising calcining the as-formed, washed "-CIT-14" composition for a time and at a temperature sufficient to form a crystalline microporous germanosilicate CIT-14 / IST composition. In certain independent aspects, these conditions further comprise heating the isolated and washed "-CIT-14" material at a temperature in the range of about 450° C. to 650° C. for a time in the range of 2 hours to 12 hours, preferably at 580° C. for 6 hours, more preferably at a temperature ramp rate of 1° C. / min.
[0176] The present disclosure also encompasses embodiments of CIT-13 / OH germanosilicates prepared by the hydroxide route specifically described herein. The present disclosure also encompasses embodiments of CIT-13 / OH germanosilicates characterized by having d4r units containing, on average, at least, and preferably more than 4 Ge atoms per d4r, allowing for the presence of Ge-4-rings in the d4r units. The present disclosure also encompasses embodiments of CIT-13 / OH germanosilicates that exhibit previously unobserved reactivity characteristics that are the result of the novel and unique physical features defined herein. EXAMPLES
[0177] The following examples provide the experimental methods used to characterize these novel materials and their transformations, and illustrate some of the concepts described within this disclosure. Each example, both those provided therein and those provided elsewhere in the body of the specification, is considered to provide a specific individual embodiment of the compositions, methods of preparation and uses, but none of the examples should be considered to be limiting of the more general embodiments described herein.
[0178] Unless otherwise specified, powder XRD patterns, nmr-spectra or other representations of structure shown herein for particular compositions are believed to be representative of those ascribed to the general structure with which they are associated.
[0179] In the following examples, efforts have been made to ensure accuracy with respect to numbers used (e.g., amounts, temperatures, etc.), but some experimental error and deviation should be accounted for. Unless otherwise indicated, temperatures are in ° C. and pressures are at or near atmospheric.
[0180] Example 1. Experimental Example 1.1. Preparation of Materials 1,2-Dimethyl-3-(2-methylbenzyl)imidazolium hydroxide (denoted as "orthomethylbenzyl") or 1,2-Dimethyl-3-(3-methylbenzyl)imidazolium hydroxide (denoted as "metamethylbenzyl") was used as the OSDA to crystallize CIT-13 from fluoride-free gels (denoted as CIT-13 / OH), which were the same as those to obtain CIT-13 in fluoride media. The synthesis protocols for the two OSDAs are provided elsewhere. The gel composition ratios are x / (x+1)SiO2:1 / (x+1)GeO2:0.5ROH:yH2O, where x is the Si / Ge ratio of the gel and y is the H2O / (Si+Ge) ratio of the gel. The preferred values of x and y are given below. The detailed procedure and gel composition are as follows: The CIT-13 / OH sample is denoted as CIT-13 / OH[z], where z is the Si / Ge ratio of the CIT-13 crystal measured using energy dispersive spectroscopy (EDS).
[0181] CIT-13 from conventional fluoride-containing gels (denoted as CIT-13 / F) was also prepared for comparative analysis with CIT-13 / OH, based on a previously reported method. As with the CIT-13 / OH samples, the CIT-13 / F samples are denoted as CIT-13 / F[z], where z represents the crystalline Si / Ge ratio measured using EDS.
[0182] IM-12 samples were also prepared according to protocols previously reported in the literature for comparison with CIT-13. Similar to CIT-13, IM-12 samples were designated as IM-12[z] (z = EDS Si / Ge ratio).
[0183] Example 1.2. Detailed synthesis of CIT-13 / OH The dry weights of the liner and stir bar need to be characterized because in the final stages of gel preparation the desired water level needs to be adjusted based on the total weight (liner + stir bar + gel).
[0184] Germanium dioxide (99.999%, Strem) was completely dissolved in the OSDA solution in a 23 mL PTFE liner for Parr steel autoclave. 1,2-Dimethyl-3-(2-methylbenzyl)imidazolium hydroxide and 1,2-Dimethyl-3-(3-methylbenzyl)imidazolium hydroxide were used as the OSDAs for CIT-13 / OH. The methods used for the preparation of these OSDAs are known. The desired amount of TEOS was added to the solution and the mixture was stirred overnight until the TEOS phase was completely hydrolyzed. The excess water and ethanol were evaporated under air flow at room temperature until the gel was thick and viscous. Ethanol, a hydrolysis product of TEOS, appears to have a detrimental effect on both the crystallization rate and the purity of the product. To maximize the extent of ethanol removal, purified water (approximately 10 mL) was added to the viscous gel and evaporated again with stirring until the gel became viscous. This water addition-evaporation process was repeated a total of five times. (Note: If fumed silica was used as the Si source, this ethanol removal step is not necessary). Finally, the desired water content was adjusted based on the total weight (liner + stir bar + gel) above. The final gel composition was x / (x+1)SiO2:1 / (x+1)GeO2:0.5ROH:yH2O, where x is the Si / Ge ratio of the gel and y is the H2O / (Si+Ge) ratio of the gel. The values of x and y are as shown in Table 4. The optimal ranges of x and y are described in the text. CIT-13 seed crystals (5 wt% based on the total weight of SiO2+GeO2) were added as needed. The gel was sealed in a steel autoclave and placed in an oven preheated to the desired temperature.
[0185] After one week of crystallization, the gel was removed. Typically, after the first week of crystallization, the gel turned dark brown and solidified. Using a clean, stiff PTFE rod, the solidified gel was thoroughly crushed into a powder. The crushed gel was placed back into the oven and crystallization resumed. Aliquots were taken every week to monitor the extent of crystallization. The final product was washed repeatedly using distilled water and acetone and dried in a convection oven at 100°C.
[0186] The gel compositions, crystallization conditions and corresponding results are summarized in Table 4.
[0187] [Table 7]
[0188] Example 1.2. Germanosilicate Conversion and CIT-13 / OH to CIT-14 / IS Post-synthetic modification to T) The conversion of CTH to CFI was carried out by exposing the freshly calcined CIT-13 / OH sample to a moisture-bearing atmosphere. Here, only one condition (30% relative humidity (pH2O=7.1 Torr) at 25 °C) was used to ensure consistency with the results from the previous study. The degree of conversion was monitored based on PXRD. CIT-14 / ESP (ESP stands for ethoxysilylated pillaring) and CIT-14 / IST (IST stands for inverse sigma conversion) were prepared based on the weak acid ADOR-type conversion of CIT-13 / F and the inverse sigma-type conversion of CIT-13 / OH, respectively. The inverse sigma conversion of CIT-13 / OH was carried out by treating the freshly calcined CIT-13 / OH with 12 M HCl at 95 °C for 48 h. The resulting solid ("-CIT-14") was collected using a centrifuge and washed repeatedly with distilled water until the pH was neutral. The final product, CIT-14 / IST (IST stands for inverse sigma transformation), is -1The temperature was then increased to 580 °C for 6 h at a temperature ramp rate of 0.01 μm. For comparison, the inverse sigma conversion from UTL to OKO was also performed using the prepared IM-12 sample. The SEM images of the CIT-14 / IST sample are shown in Figure 4 (AB).
[0189] 19 F Magic Angle Spinning (MAS) and 1 H- 29 Degermanization and fluorination of germanosilicates were carried out for Si cross-polarization (CP) MAS NMR studies. Cold water degermanization of calcined germanosilicate was carried out as follows: 100 mg of freshly calcined germanosilicate was immersed in 100 mL of distilled water at room temperature and stirred overnight. The resulting solid was collected using a centrifuge and washed repeatedly with distilled water. The degermanized sample was dried under vacuum at room temperature. Post-synthesis fluorination of germanosilicate crystallized in fluoride-free media was carried out as follows: 100 mg of as-prepared CIT-13 / OH was finely ground with 20–25 mg of ammonium fluoride and heated at 150 °C for 24 h. Excess ammonium fluoride was removed by washing with cold distilled water and the collected solid was dried at 100 °C.
[0190] Example 1.3. Characterization Powder X-ray diffraction (PXRD) profiles were collected using a Rigaku Miniflex II diffractometer (CuKα radiation, λ=1.5418A). High-resolution PXRD data were collected at the 2-1 powder diffraction beamline at the Stanford Synchrotron Radiation Lightsource (SSRL) using a wavelength of 0.9998A. For high-resolution PXRD experiments, calcined CIT-14 powder samples were packed and sealed in 1.0 mm glass capillaries.
[0191] Scanning electron microscope (SEM) images and elemental analysis data from Oxford X-max Collected with a ZEISS 1550VP field emission (FE)-SEM microscope equipped with an SDD EDS system. The Ar-adsorption isotherm was obtained at 87.45 K using a Quantachrome Autosorb iQ analyzer. Solid magic angle spinning (MAS) Nuclear magnetic resonance (NMR) spectra were acquired with a Bruker Avance 500 MHz spectrometer (magnetic field = 11.2 T). The molecular sieve sample was loaded into a 4 mm diameter zirconia rotor with a Kel-FR cap. 1 H- 13 C cross-polarization (CP) MAS spectra, 29 Si MAS spectra and 1 H- 29 Si CPMAS spectra were collected at a MAS rotation speed of 8 kHz, 19 and F MAS spectra were collected at 12 kHz.
[0192] (Example 2. Results and Discussion) (Example 2.1 Discussion of Synthesis) By excluding fluoride and further changing other gel compositions from those of the fluoride route of CIT-13, CIT-13 can be crystallized in a hydroxide medium. Unlike CIT-13 / F which can be crystallized in a moderately high range of gel compositions, CIT-13 / OH is obtained in a rather narrow gel composition range. The ranges of the gel Si / Ge ratio and the gel H2O / (Si + Ge) ratio were 2 < Si / Ge < 4 and 6 < H2O / (Si + Ge) < 7, preferably 2.5 < Si / Ge < 3.0 and 6.0 < H2O / (Si + Ge) < 6.5 when OSDA / (Si + Ge) = 0.5. Outside this composition range of the gel composition, amorphous gel germanosilicates or unknown high-density phases were obtained. Crystallization of the pure CIT-13 phase was observed at 160 °C and 175 °C. The details of the synthesis (such as gel composition, etc.) are shown in Table 4. CIT-13 / OH had a plate-like crystal morphology as shown in Figures 5(A - C), similar to CIT-13 obtained from fluorine-containing preparations and its isostructural gel germanosilicates. As-prepared CIT-13 / OH[4.33]'s 1 H- 13C CPMAS spectra and solution phase OSDA 13 C NMR (Figure 6) confirmed that the structure of OSDA was preserved during crystallization of CIT-13 / OH. 1 H- 29 S The CPMAS spectrum also confirmed the presence of connectivity defects that compensate for the absence of fluoride (Figure 7).
[0193] PXRD profiles of as-prepared and calcined CIT-13 / OH[3.88] and CIT-13 / OH[4.33] are displayed in Figure 8(BE). Other PXRD patterns are provided in Figure 9. All PXRD profiles were obtained under ambient conditions. The diffraction peak positions were in good agreement with those of reference CIT-13 / F shown in Figure 8(F). However, differences in peak intensities were observed between CIT-13 / F and CIT-13 / OH. Except for the only CIT-13 / OH[3.88] crystallized with orthomethylbenzyl OSDA (Figures 8(A) and 9(B)), the other as-prepared CIT-13 / OH synthesized from metamethylbenzyl OSDA showed a very weak (200) peak at 2θ=6.44° as shown in Figures 8(D) and 9(A). 9(CK) shows a very weak (200) peak at 2θ=6.44°. These weak (200) peaks from as-prepared CIT-13 / OH became stronger after removing the OSDA by calcination (Figure 8(E)). Moreover, some of the CIT-13 / OH samples show a clearly identifiable (310) peak at 2θ=11.58°, as shown in Figures 9(DG) and 9(IJ). These (310) diffractions are found to be attenuated by the post-synthetic insertion of fluorides using ammonium fluoride. Also, the fluorination of CIT-13 / OH increased the intensity of the (200) peak (Figure 10). Thus, the absence of fluorides and the presence of meta-methylbenzyl OSDA cations in the CIT-13 framework appeared to be responsible for the weak intensity of the (200) peak and the occasional appearance of the (310) peak.
[0194] The argon physical adsorption isotherm of CIT-13 / OH[3.56] obtained at 87.45 K is shown in Fig. 8(G) overlaid with that of CIT-13 / F[4.18] for comparison. The micropore volume of CIT-13 / OH[3.56] was 0.141 cc / g based on the t-plot method (0.202 cc / g from the Saito-Foley method). This microporosity was slightly lower than that of the reference CIT-13 / F[4.18] (de Boer t-plot: 0.172 cc / g; Saito-Foley: 0.223 cc / g). The characteristic two-step adsorption due to the presence of 10MR and 14MR of CIT-13 (↓ mark in Fig. 8(G)) was also observed for CIT-13 / OH as expected.
[0195] Example 2.2. Discussion of the Conversion of CTH to CFI Unlike other d4r-type germanosilicates such as UTL, IWW and ITH, CIT-13-type germanosilicates slowly transformed to CFI-type germanosilicates upon exposure to environmental humidity (*CTH to CFI transformation). This transformation occurred due to the rearrangement of Ge-rich d4r units into dzc units due to the instability of the CIT-13 framework caused by the presence of germanium-rich d4r units and the crystallographic nature of the cfi layer. Interestingly, CIT-13 / OH was transformed to the corresponding germanosilicate CIT-5 much faster than CIT-13 / F with a similar germanium content. CIT-13 / OH[4.33] completed the transformation to CFI within 12 days, whereas CIT-13 / OH[4.33] was transformed to CFI within 12 days. CIT-13 / F[4.31] was completely converted to CFI-type germanosilicate over 85 days. The PXRD profiles of calcined CIT-13 / OH[4.33] after exposure to ambient humidity (pH2O=7.1 torr at 25 °C, 30% relative humidity) for a certain period of time are shown in Figure 11(A) and Figure 11(B). The (400) peak of CIT-13 was initially overlapped with the (002) diffraction at 2θ=13.07°, but after 2 days it shifted to 2θ=13.69° and became separately visible. After 8 days, the three characteristic diffractions of the CFI framework ((301), (002), and (400)) began to appear. The PXRD profile after 10 days of ambient exposure was in good agreement with that of the reference pure silica CIT-5. The time-dependent position of the cfi-cfi interlayer distance, estimated from the position of the (200) diffraction, is shown for CIT-13 / OH[4.33] and CIT-13 / F[4.31] in Figure 11(E), indicating a faster transformation of CIT-13 / OH compared to CIT-13 / F.
[0196] In the case of CIT-13 / F, decreasing the Si / Ge ratio from 4.31 to 3.87 reduced the time required to achieve full conversion from approximately 4 months to 12 days. This acceleration in the conversion rate can be attributed to an increase in germanium sites in the d4r units, which are structural building units that convert to dzc units in the CFI framework. As in the case of CIT-13 / F, decreasing the Si / Ge ratio of CIT-13 / OH further accelerated the conversion of *CTH to CFI. CIT-13 / OH[3.88] converted to the corresponding CIT-5-type germanosilicate within 2 days, as shown in Figures 11(C) and 11(D). This was at least 6 times faster than the similar conversion in CIT-13 / F[3.87]. The calcined CIT-13 / OH[3.88] and the resulting Ge-CIT-5 29Si NMR spectra were acquired to investigate the environment of the Si sites in these germanosilicates (Figure 12). As in the case of CIT-13 / F, CIT-13 / OH showed three groups of signals at -104.2, -109.4, and -113.9 ppm. This spectral shape was consistent with the previously reported CIT-13 (see Figure 3 above) and related materials synthesized in fluoride media. Unlike Ge-CIT-5 derived from CIT-13 / F, which showed a single broad set of signals at -110.61 ppm, Ge-CIT-5 derived from CIT-13 / OH[3.88] showed two separate groups of peaks at approximately -109.0 and -112.2 ppm. The disappearance of the shoulder at -104.2 ppm in the spectrum of CIT-13 can be attributed to the rearrangement of d4r units to dzc bridging units, which was also observed in the transformation of CIT-13 / F. Therefore, both signals can be assigned to the cfi layer Si site since they have the same origin as the signals at −113 ppm and −115 ppm in pure silica CIT-5.
[0197] Based on the fact that the higher germanium content of the parent CIT-13 resulted in a faster conversion of *CTH to CFI, it can be inferred that CIT-13 / OH crystals have more germanium in their d4r units compared to CIT-13 / F crystals with a similar overall Si / Ge ratio. It was also confirmed that the cfi layers have a non-zero germanium occupancy in CIT-13 / F. The formation of d4r units is known to be promoted by the presence of fluoride anions and / or high germanium content, which can stabilize the low framework TOT angle. The formation of the d4r-type CIT-13 framework in the absence of fluoride could result in increased incorporation of germanium in the d4r units. Indeed, the CIT-13 / OH sample with a lower Si / Ge ratio underwent inverse sigma conversion in concentrated acid to produce “-CIT-14”, an analogue of COK-14 derived from IM-12. The ability to undergo this type of transformation strongly suggests not only a high content of clustered germanium sites within the d4r units but also the presence of pure Ge-4 rings.
[0198] (Example 2.3. Consideration of the topotactic conversion of CIT-13 to "-CIT-14" and CIT-14 / IST) Despite the structural similarity between CIT-13 and IM-12, the *CTH type gel produced by strong acid The leaching of Ge-4-rings from germanosilicates has not yet been reported. Unlike IM-12, it has been suggested that the Si-O-Si interlayer cross-linking bonds of *CTH-type germanosilicates are the main obstacle for such transformation. ADOR-type transformation of SAZ-1 to IPC-16 and Pawley refinement of the latter appeared. Very recently, partial removal of the T sites in the d4r units of CIT-13 / F based on weak base treatment to give ECNU-23 was reported. However, the presence of pure Ge-4-rings in the d4r units is essential for true reverse sigma transformation by strong acid, and IM-12 was the only d4r-type germanosilicate with such structural and elemental prerequisites.
[0199] Ge-rich CIT-13 crystallized in hydroxide media can undergo a structural transformation that can be explained by an inverse sigma transformation with the simultaneous removal of the Ge-4-ring from the d4r, as shown diagrammatically in Figure 13(A). Herein, two examples (CIT-13 / OH[3.71] and CIT-13 / OH[3.56]) were demonstrated based on the PXRD profiles shown in Figure 13(B). Following the nomenclature used by Verheyen (Nat. Mater. 2012, 11, 1059), the freshly acid-treated material before calcination is designated as "-CIT-14". Although no Rietveld refinement was performed for "CIT-14", a slight decrease in the unit cell parameters along the interlayer direction (i.e., the a-direction) was observed after calcination of "-CIT-14", similar to the condensation of -COK-14 to COK-14. The presence or absence of fluoride and the germanium content were the two most important synthetic factors for the preparation of CIT-13 germanosilicate, which can generate CIT-14 by inverse sigma conversion. Treatment of calcined CIT-13 / F[3.87] with 12 M HCl did not afford "-CIT-14", despite the high germanium content. Also, a similar treatment of CIT-13 / OH[4.33] afforded a disordered layered material (Figure 14(AB)).
[0200] For comparison, an isostructural material was obtained based on the conventional ADOR conversion of CIT-13, denoted here as CIT-14 / ESP. This conversion was similar to that of SAZ-1 to IPC-16. The PXRD profiles of CIT-14 / IST, prepared by treating calcined CIT-13 / OH[3.56] with 12 M HCl, and CIT-14 / ESP from the ADOR-type conversion of CIT-13 / F[4.33] are shown in Figures 15(A) and 15(B) together with that of the reference CIT-14 model based on the GULP structure optimization algorithm. Obviously, the intensity of the (200) interlayer diffraction of CIT-14 / IST was stronger than that of CIT-14 / ESP. This difference in diffraction intensity may be attributed to the elemental composition of the single four-ring (s4r) bridging unit of CIT-14. The effect of germanium occupancy at each of the seven T sites of CIT-14 on the intensity of the (110) and (200) diffractions was calculated and the results are shown in Figure 16. It was found that the relative intensity of the (110) diffraction in PXRD increases significantly when germanium occupies two T sites (T3 and T7). T7 is an s4r site and T3 is a site directly adjacent to the d4r site. Indeed, in the Rietveld refinement of CIT-14 / IST, the germanium content of T7 is 21%, which accounts for 52% of the total number of germanium in the entire framework (Table 5, see above). For T3, no significant germanium occupancy was detected. Considering the departure of a pure Ge-4 ring from the d4r unit of the parent germanosilicate by inverse sigma transformation, it can be concluded that the d4r unit of CIT-13 / OH has more than four germanium atoms on average. However, the relative intensity of the d4r unit of CIT-14 / IST and CIT-14 / ESP is 1.2 times that of the d4r unit of CIT-13 / OH. 1 H-Decouple 29 No significant differences were observed in the Si MAS spectra (Figure 15(D)). Both CIT-14s show a broad envelope of signals centered at approximately -112 ppm. This spectral similarity is presumably due to the presence of remaining germanium sites in the CIT-14 backbone. Also, only small amounts of Q3-type silanols were detected.
[0201] As mentioned above, CIT-14 / IST contains more germanium than CIT-14 / ESP. The EDS Si / Ge ratios of the two CIT-14 / IST samples obtained from CIT-13 / OH[3.56] and CIT-13 / OH[3.71] were found to be 14.5 and 17.5, respectively. These values were lower than those of the CIT-14 / ESP samples whose preparation procedure involved degermanization exfoliation with a weak acid (0.1 M HCl) (Si / Ge=50-253, depending on the degree of degermanization, see Fig. 17). The Si / Ge ratios of the COK-14 samples prepared here using the same procedure on the two IM-12 samples (Si / Ge=3.80 and 4.79) were 17.5 and 29.2, which are much lower than those reported by Verheyen et al. (Si / Ge=110), probably due to the lower Si / Ge ratio of the parent IM-12.18 (see Figs. 18 and 19). These values are also much lower than those of IPC-2 (reported Si / Ge=97), which was prepared as an ADOR product from IM-12, which similarly underwent weak acid exfoliation as CIT-14 / ESP. These results confirm that the inverse sigma conversion by strong acid leaves extra germanium sites in the d4r units unleached (other than the removal of the Ge-4-ring).
[0202] The microporosity of CIT-14 was investigated using argon adsorption isotherms obtained at 87.45 K (Figure 20). While CIT-14 / IST did not show any adsorption-desorption hysteresis, CIT-14 / ESP showed a desorption curve that clearly deviated from its adsorption curve. Similar hysteresis was observed from IPC-2 formed by the ADOR-type pillaring method. This minor mesoporosity is commonly observed after post-synthesis treatment in nitric acid medium. Also, the specific micropore volume of CIT-14 / IST (0.105 cc / g by t-plot, 0.141 cc / g by Saito-Foley) was larger than that of CIT-14 / ESP (0.065 cc / g by t-plot, 102 cc / g by Saito-Foley). A similar trend was observed in the conversion of UTL to OKO. As can be clearly seen in Figure 20(B), CIT-14 / IST is a 100% ... -4 ) p / p0 = approx. 1 × 10 -4 Argon began to be adsorbed at a low pressure. This adsorption onset pressure was 8MR ring zeolite A (LTA) (p / p0~1×10 -4 ) Therefore, argon adsorption of CIT-14 was initiated by its adsorption into the 8MR pores.
[0203] The reduction in micropore volume associated with the inverse sigma transformation of CIT-13 to “-CIT-14” was investigated theoretically and experimentally. For the theoretical evaluation, the TOTOPOL utility for topology analysis developed by Treacy and Foster was used to estimate the reduction in pore volume. As framework models for the calculations, the crystallographic information (cif) files obtained from the Rietveld refinement of CIT-13 and CIT-14 / IST (this work, see below) were used. The results are summarized in Table 6. The experimentally observed reduction in micropore volume (Saito-Foley: 30.2%; t-plot: 25.5%) was comparable or lower than that estimated using TOTOPOL (30.2%), although TOTOPOL seemed to underestimate the micropore volume of CIT-13 and CIT-14 compared to the experimentally obtained values.
[0204] [Table 8]
[0205] Since the positions of the bridging sites, i.e., the layer sites directly connected to the d4r or s4r units of CIT-13 or CIT-14, respectively, did not change during the inverse sigma transformation, CIT-14 / IST should have directly inherited the disorder pattern from its parent CIT-13. In fact, the (111) and (201) diffraction peaks estimated to be located at 2θ = 11.43° and 11.78°, respectively, by the disorder model based on the GULP algorithm were not observed in the actual PXRD pattern of CIT-14 / IST (Figure 15(C)). These diffractions were also not observed in CIT-14 / ESP, which is consistent with the previously reported ADOR transformation of SAZ-1 to IPC-16. However, in the ADOR transformation, the Ge-rich d4r was completely removed by exfoliation in weak acid, and the bridging s4r was formed by the newly introduced silicon source such as diethoxydimethylsilane. Therefore, the pattern of disorder in CIT-14 / IST may not be identical to that of CIT-14 / ESP and IPC-16.
[0206] The XPD pattern could be indexed with an orthorhombic unit cell (a = 21.90 A, b = 13.74 A, c = 10.11 A) using the program TREOR35 implemented in the software CMPR.36. The initial CIT-14 framework model was derived from the CIT-13 framework structure (assuming all silica)20 by inverse sigma transformation, with no disorder introduced from CIT-13. Furthermore, the geometry was optimized assuming the same space group Cmmm as the parent CIT-13 (*CTH) using the program DLS-7637. Taking this as a starting point, a Rietveld refinement was performed using the program TOPAS. The final structure of CIT-14 / IST was obtained with a match value R F = 0.057, R wp = 0.078 and R exp= 0.053 was obtained based on the Rietveld refinement of the powder pattern (Figure 21(A)).
[0207] Since all symmetry elements are preserved, the inverse sigma transformation satisfies the IUPAC definition of a topotactic transformation. The idealized structure and pore system of CIT-14 / IST are shown in Figure 21(B) and Figure 21(C), respectively. CIT-14 / IST has a two-dimensional channel system separated by 12MR and 8MR pores with critical dimensions of 6.4 x 4.9A and 3.9 x 3.3A, respectively. Similar to ferrierite (FER), CIT-14 / IST has a small cage connected to two adjacent linear main channels through small pore openings, while other two-dimensional 12 / 8MR topologies known as EON and M The OR does not have such a cage structure. Due to the presence of disorder (illustrated in FIG. 21(D)), the 8-MR subchannel is not linear. The unit cell parameter c can also be defined as c'=c / 2=5.0569A for the average structure, but using a smaller unit cell did not improve the refinement (i.e., the changes in the atomic coordinates and the fit of the profile are minimal, but the number of parameters undergoing refinement increases). Detailed crystallographic information of CIT-14 / IST is listed in Tables 5 and 7 and FIG. 22.
[0208] [Table 9-1] [Table 9-2]
[0209] [Table 10]
[0210] (Example 2.4. Consideration of Ge arrangement in d4r unit) The inverse sigma transformation ability of d4r-type germanosilicates can indirectly provide evidence for the presence of pure Ge-4 rings (d4r units) parallel to the layers. As mentioned in the previous section, Ge-rich CIT-13 / OH (Si / Ge ratio < 3.7) underwent inverse sigma transformation similar to IM-12 to give CIT-14 / IST with high crystallinity and a clear pore system. Based on PXRD and structure refinement, the remaining s4r units of CIT-14 were found to have germanium sites. Thus, the elemental composition of the d4r units of CIT-13 / OH was [Si n Ge 8-n ]-d4r (n<4), and it is inferred that the four Ge atoms fully occupy the d4r flanks. Although CIT-13 / F could be converted to CIT-14 / ESP using the ADOR strategy, we were unable to achieve inverse sigma conversion with it. Furthermore, as mentioned above, CIT-13 / OH showed a much higher conversion rate of *CTH to CFI than the CIT-13 / F sample with similar germanium content. These results indicate that the presence or absence of fluoride, which can also direct and stabilize the structure of the d4r unit, plays a major role in the organization of the elemental composition and distribution within the d4r unit of the ultralarge pore germanosilicate CIT-13.
[0211] 19F NMR spectroscopy can be used as a tool to reveal the elemental composition of small ring building units such as d4r units. Germanosilicates that do not incorporate fluoride anions from direct synthesis can be modified post-synthesis by inserting fluoride into the as-produced or degermanated framework. Fluoride-incorporated d4r-type germanosilicates typically show three signals at approximately -8 ppm (broad), -19 ppm (sharp) and -38 ppm (sharp), which are usually assigned to [Si4Ge4]-d4r, [Si7Ge]-d4r and [Si8]-d4r, respectively. There is general agreement on the assignment of the latter two. However, the nature of the former -8 ppm peak, which is usually broad and sometimes accompanied by one or two shoulder signals, still leaves open the possibility of many germanium configurations.
[0212] As-prepared CIT-13 / F and fluorinated CIT-13 / OH samples 19 F NMR spectra are shown in Figure 23(AC). All CIT-13 samples show a broad peak centered around -8 ppm, with no signals at -19 ppm and -38 ppm, indicating that the d4r units of these CIT-13 samples are rich in germanium. In addition, post-synthetic fluorination of CIT-13 / OH revealed a sharp signal with multiple spinning sidebands at -123.7 ppm, which is likely due to surface etching. 19It is presumed to originate from F-Si species. This surface etching did not result in structural degradation, as supported by the PXRD profiles (Figure 10). The -8 ppm signal of the CIT-13 sample was broader than that of IM-12, indicating that the germanium configuration in the d4r units of CIT-13 appears to be less uniform than that of fluorinated IM-12, regardless of the type of mineralizer used. The -8 ppm signal of the CIT-13 sample was deconvoluted into two peaks, line 1 (-7.3 to -8.3 ppm) and line 2 (-11.0 to -11.7 ppm). As shown in Figures 23(A) and (B), CIT-13 / OH[4.33] (16%) gave a stronger line 2 signal than CIT-13 / F[4.33] (1%), despite the similar germanium content. This result indicates that the absence of fluoride in the synthesis of CIT-13 did indeed affect the arrangement of germanium sites in the d4r units. It was shown above that CIT-13 / OH[4.33] converted to the corresponding Ge-CIT-5 faster than CIT-13 / F with a similar Si / Ge ratio, and this *CTH to CFI conversion was caused by hydrolysis of TO-Ge bonds. IM-12 with Ge-O-Ge bonds decayed very quickly (within 1 day) when exposed to environmental conditions. Kasian et al. showed that fluorinated IM-12 exhibited a shoulder peak at -12 ppm next to the main peak at -8 ppm (the shoulder peak at -3 ppm observed in fluorinated IM-12 was not detected in CIT-13). This suggests that the line 2 signature of CIT-13 / OH The origin of the rings may be due to the highly clustered arrangement of germanium sites within d4r units such as the Ge-4-ring.
[0213] The 19F spectrum of CIT-13 / OH[3.56] further increased the contribution of line 2 (23%) and underwent an inverse sigma transformation to CIT-14 / IST (as shown in Figure 23(C)). Others have investigated the 19F NMR spectra of a series of STW-type germanosilicates ranging from pure silica to pure germania and reported that the main 19F signal shifted from -7.5 ppm to -10.5 ppm as the Si / Ge ratio decreased from 5 to 0.42. Still others have reported that the 19F spectrum of the Ge-rich ITQ-21 material 19 They also reported the presence of an upfield signal at −14 ppm in the F NMR spectrum. Based on these results, the inventors believe that upfield signals such as line 2 may be due to the high germanium content in the d4r unit.
[0214] The arrangement of germanium sites within the d4r units of CIT-13 / OH was similar to that of the related germanosilicates degermanated with distilled water. 1 H- 29 Further investigation was carried out based on the Si CPMAS NMR spectrum (Figure 24). It is speculated that using this type of treatment, most of the germanium sites are removed from the d4r units, with the adjacent silicon sites becoming silanol sites. The water-degermanized CIT-13 and IM-12 samples share a strong Q3 signal in addition to the fully connected Q4 signal. The major difference between the samples is the intensity of the Q2 type (geminal) silanol signal. The degermanized IM-12 samples (Si / Ge=4.89 and 4.23) showed the weakest Q2 signal among the degermanized materials studied, which is consistent with previous observations by other researchers. These IM-12 samples were more Ge-rich than IM-12 (Si / Ge=5.3), which was confirmed to undergo inverse sigma transformation. 1 H- 29The trace of Q2 signal in the Si CPMAS spectrum may be due to excessive degermanization. Unlike IM-12, the four CIT-13 samples shown in Fig. 24 gave a moderately intense Q2 signal. Of the four studied CIT-13 samples, only CIT-13 / OH[3.71] underwent inverse sigma conversion to CIT-14 / IST, which showed the weakest Q2 signal among CIT-13. The two CIT-13 / F samples gave stronger Q2 signals than CIT-13 / OH[4.33], regardless of the Si / Ge ratio. These CIT-13 / F samples did not convert to CIT-14 by inverse sigma conversion as shown above. Also, their degermanized forms 1 H- 29 The Si CPMAS spectrum was similar to those of ITH and IWW in terms of its strong Q2 signal, an observation that further supports the premise that the presence or absence of fluoride in the synthesis gel of CIT-13 influenced the placement of germanium within the d4r bridging units.
[0215] Three example types (I, II, and III) of germanium configurations in the [Si4Ge4]-d4r unit as well as two Ge-rich configurations (II-2 and III-2 with 5 and 6 Ge sites, respectively) are shown in Figure 25. Based on their computational results, Corma et al. showed that among the possible [Si4Ge4]-d4r configurations of AST-type germanosilicates, the alternating arrangement of Si and Ge sites in the d4r unit (i.e., type I configuration) is the most energetically favorable. This germanium configuration has also been suggested by Liu et al. to exist in as-prepared CIT-13 / F. Types II and III are the [Si4Ge4]-d4r configurations suggested to exist in ITH / IWW and UTL, respectively, and in the fluorinated and degermanated ITQ-13, ITQ-22, and IM-12 germanosilicates.28 19 F MAS and 1 H- 29Based on the Si CPMAS spectrum, most importantly, the type III configuration can explain the extraction of the Ge-4-ring during the inverse sigma transformation of IM-12 and the resulting high Si / Ge ratio of the COK-14 material.
[0216] It has been pointed out that the presence of Si-O-Si bridges in CIT-13 / F may hinder the complete exfoliation of the cfi-type layered material in acidic media. CIT-13 / F did not convert to CIT-14 by strong acid treatment as described above. This result suggests that the d4r units of the CIT-13 / F sample do not have pure Ge-4-rings. Although very slow, CIT-13 / F converted completely to Ge-CIT-5 upon exposure to environmental humidity. This conversion mechanistically involves hydrolysis of TOT bonds parallel to the main 14MR channel in the d4r unit. Therefore, it is unlikely that CIT-13 / F has Si-O-Si bonds along the main d4r channel direction. Therefore, it is possible that type I or type II-2 (Ge-rich) configurations could explain all the conversion behaviors exhibited by CIT-13 / F. However, DFT-based calculations by Cambrour et al. suggest that highly clustered germanium sites such as type II-2 are not associated with the Ge-CIT-5 structure. 19 This could result in a large contribution of the line 2 signal in the F NMR, which is not observed in CIT-13 / F (Figure 23(A)). Therefore, CIT-13 / F may have type I or other possible configurations that could explain its conversion behavior.
[0217] As shown in Figures 23(B) and 23(C), the fluorinated form of the CIT-13 / OH sample showed a broader -8 ppm signal (line 1) and 16-23% contribution of extra upfield signals (line 2) than those of IM-12,28. These data suggest the presence of highly clustered germanium sites such as type II-2 and type III-2 in the d4r units. Also, the fast *CTH to CFI conversion of CIT-13 / OH can be explained by Ge-O-Ge bonds parallel to the channel direction. The type III-2 configuration is also consistent with the pure Ge-4 ring and high germanium content in the s4r sites of the obtained CIT-14 / IST. Indeed, our refined structure solution obtained from synchrotron PXRD confirmed that the Si / Ge ratio of the bridging s4r units is about 4, which means that there are one or two additional germanium substitutions on the pure Ge-4-ring in the d4r units of CIT-13 / OH. Therefore, we suggest that in the absence of fluoride in the synthesis gel of CIT-13, clustered germanium sites such as type II-2 or type III-2 are obtained.
[0218] As those skilled in the art will appreciate, numerous modifications and variations of the present invention are possible in light of these teachings, all of which are contemplated herein. All references cited herein are incorporated by reference for their teachings at least in the context presented.
Claims
1. A crystalline microporous germanosilicate composition designated CIT-14 / IST, characterized in that the composition has 8 and 12 membered ring channels and a powder X-ray diffraction (XRD) pattern having at least five characteristic peaks at 7.59±0.5, 8.07±0.5, 12.88±0.3, 19.12±0.3, 19.32±0.3, 20.73±0.3, 22.33±0.3, 24.37±0.3, 27.19±0.3 and 27.69±0.3 degrees 2-theta.
2. 2. The crystalline microporous germanosilicate CIT-14 / IST composition of claim 1 having a Si:Ge ratio in the range of 12:1 to 20:
1.
3. The crystalline microporous germanosilicate CIT-14 / IST composition of claim 1, comprising an orthorhombic crystal system.
4. The crystalline microporous germanosilicate CIT-14 / IST composition according to claim 3, characterized by the Cmmm space group or the Cmcm space group or an intracrystalline mixture (disorder) of the two domains.
5. The crystalline microporous germanosilicate CIT-14 / IST composition of claim 3, whose crystals have the following unit cell parameters: [Table 1]
6. 2. The crystalline microporous germanosilicate CIT-14 / IST composition of claim 1, wherein the 8-ring channels have a pore size of about 3.3 Å×3.9 Å and the 12-ring channels have a pore size of about 4.9 Å×6.4 Å.
7. 10. The crystalline microporous germanosilicate CIT-14 / IST composition of claim 1, which is substantially fluoride-free.
8. 2. The crystalline microporous germanosilicate CIT-14 / IST composition of claim 1 having micropores that optionally contain an alkali metal cation salt, an alkaline earth metal salt, a transition metal, a transition metal oxide, a transition metal salt, or a combination thereof.
9. 2. A method for preparing the crystalline microporous germanosilicate CIT-14 / IST composition of claim 1, comprising contacting a crystalline microporous germanosilicate CIT-13 / OH, which is fluoride-free, has a three-dimensional framework with pores defined by 10- and 14-membered rings, and exhibits a powder X-ray diffraction (XRD) pattern with at least five peaks at 6.45±0.2, 7.18±0.2, 12.85±0.2, 20.78±0.2, 26.01±0.2 and 26.68±0.2 degrees 2-theta, with a concentrated strong aqueous mineral acid at an elevated temperature for a time sufficient to form an intermediate microporous germanosilicate "-CIT-14".
10. 10. The method of claim 9, wherein: (a) the concentrated strong aqueous mineral acid is aqueous HCl or HNO 3 (b) the concentration of said concentrated strong aqueous mineral acid is in the range of 6 to 12M; (c) said elevated temperature is in the range of 80° C. to 120° C.; and / or (d) said sufficient time is in the range of 4 to 24 hours.
11. 10. The method of claim 9, further comprising isolating the intermediate microporous germanosilicate "-CIT-14" and washing the intermediate microporous germanosilicate "-CIT-14" with water until the pH of the washing solution is neutral, and then heating the isolated and washed intermediate microporous germanosilicate "-CIT-14" at a temperature in the range of about 450°C to 650°C for a time in the range of 2 hours to 12 hours.
12. Use of the crystalline microporous germanosilicate CIT-14 / IST composition according to claim 8 as a catalyst or vehicle for gas separation.
13. (a) carbonylation of dimethyl ether (DME) with CO at low temperature; (b) reducing NOx with methane; (c) Cracking, hydrocracking or dehydrogenating hydrocarbons; (d) dewaxing the hydrocarbon feed; (e) converting paraffins to aromatics; (f) isomerizing or heterogenizing the aromatic feedstock; (g) alkylating aromatic hydrocarbons; (h) oligomerizing alkenes; (i) aminating a lower alcohol; (j) separating and sorbing lower alkanes from a hydrocarbon feedstock; (k) isomerizing olefins; (l) producing higher molecular weight hydrocarbons from lower molecular weight hydrocarbons; (m) reforming hydrocarbons; (n) converting lower alcohols or other oxygenated hydrocarbons to produce olefin products, including methanol to olefins processes; (o) epoxidizing an olefin with hydrogen peroxide; (p) reducing the nitrogen oxide content of a gas stream in the presence of oxygen; (q) separating nitrogen from a nitrogen-containing gas mixture; or (r) converting a synthesis gas containing hydrogen and carbon monoxide into a hydrocarbon stream; or (s) reducing the concentration of organic halides in the initial hydrocarbon product; The process is carried out by contacting each of the feedstocks with the crystalline microporous germanosilicate CIT-14 / IST composition of claim 8.
Citation Information
Patent Citations
Novel cit-13 phase crystalline germanosilicate material and its preparation method
JP2018521933A
Novel germanosilicate composition and method for producing same
JP2019508351A
Methods of preparing crystalline germanosilicate materials of CIT-13 topology
WO2019231595A1