Manufacturing method of welded joint by gas shielded arc welding of steel plate

The gas-shielded arc welding method for thick steel plates addresses the challenges of high strength and low-temperature toughness by using multi-electrode welding with controlled parameters and compositions, resulting in defect-free welds for large structures.

JP7558480B1Active Publication Date: 2024-10-01JFE STEEL CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024536460
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-27
Publication Date
2024-10-01
Estimated Expiration
2044-03-27

Smart Images

  • Figure 0007558480000012
    Figure 0007558480000012
  • Figure 0007558480000013
    Figure 0007558480000013
  • Figure 0007558480000014
    Figure 0007558480000014
Patent Text Reader

Abstract

The present invention provides a method for producing a narrow gap welded joint by gas-shielded arc welding, which is free from welding defects in steel plates with a thickness of 50 mm or more and has high strength and excellent low-temperature impact toughness. The method for producing a welded joint by gas-shielded arc welding of the present invention is a method for producing a welded joint by gas-shielded arc welding, in which the width W of each layer excluding the initial layer and the outermost layer of the weld metal is 5.0 to 0.4T (mm), and the ratio A / p of the cross-sectional area A perpendicular to the weld line to the number of weld layers p is 120.0 mm. 2 / layer or less, the ratio p / T of the number of welding layers p to the plate thickness T is 0.40 layers / mm or less, the gas shielded arc welding is a multi-electrode welding in which the welding wire tips of the first and second electrodes are arranged on different parallel welding lines, one of the first and second electrodes has positive polarity and the other has opposite polarity, the distance a between the welding wire tips of the first and second electrodes is 5 to 16 mm, the angle α of the straight line connecting the welding wire tips of the first and second electrodes with respect to the perpendicular direction to the welding line is 60° or less, and a welding wire containing REM is used for the positive polarity electrode.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a welded joint by gas-shielded arc welding using a steel plate, particularly a steel plate having a plate thickness of 50 to 160 mm. [Background technology]

[0002] With the growth of the energy industry, for example, in order to improve the efficiency of drilling marine resources and the efficiency of power generation, marine structures and offshore wind turbines constructed on the ocean are becoming larger. As a result, as structures and generators become larger, it is necessary to ensure high strength in the foundations of the equipment, and the use of steel plates with a plate thickness of 50 to 160 mm is being considered. In addition, in cold oceans, it is expected that waves and drift ice will collide with the thick plates used in the structures, so excellent toughness at -40°C is also required. When manufacturing marine structures and offshore generator equipment that use thick plates, improving the construction efficiency is an important issue, and in particular, it is required to weld such thick plates with high efficiency.

[0003] Large heat input welding has been proposed as one of the highly efficient welding methods for thick plates. However, when large heat input welding is used, it is often difficult to ensure the toughness of the weld metal and the heat affected zone of the base metal.

[0004] For example, Patent Document 1 discloses a "two-electrode, one-side, one-pass, large heat input submerged arc welding method with excellent toughness of weld metal." The welding method disclosed in Patent Document 1 uses a specific flux and specific welding wires for the first and second electrodes for a specific steel plate when performing one-pass welding on a steel plate having a thickness of 40 mm or more by two-electrode submerged arc welding. The steel plate contains, by mass%, C: 0.02-0.2%, Si: 0.01-1%, Mn: 0.1-2.5%, Al: 0.002-0.1%, N: 0.001-0.015%, P: 0.02% or less, S: 0.01% or less, O: 0.01% or less, and the balance being Fe and unavoidable impurities. The flux contains, by mass%, SiO2: 10-25%, MgO: 5-20%, CaO: 5-15%, CaF2: 1-10%, Al2O3: 5-25%, TiO2: 2-20%, Fe: 10-25%, and B2O3: 0.1-2.5%. The welding wire contains, by mass%, C: 0.02-0.2%, Si: 0.01-1%, Mn: 0.5-2.5%, Al: 0.002-0.1%, Ti: 0.005-0.3%, and N: 0.001-0.015%, with P: 0.02% or less, S: 0.01% or less, and O: 0.01% or less, with the balance being Fe and unavoidable impurities. Furthermore, welding is performed under the conditions that the diameter of the welding wire of the second electrode is 6 to 8 mm, and the ratio of the cross-sectional area of ​​the welding wire of the first electrode to the cross-sectional area of ​​the welding wire of the second electrode is 35 to 75%. Patent Document 1 describes this as a two-electrode, single-side, one-pass, large heat input submerged arc welding method that produces excellent toughness in the weld metal.

[0005] Patent Document 2 discloses a "two-electrode large heat input submerged arc welding method." The welding method described in Patent Document 2 is a two-electrode large heat input submerged arc welding method in which welding is performed using a specific wire and a specific flux. The wire contains, by mass%, C: 0.02-0.18%, Si: 0.02-0.5%, Mn: 1.15-2.2%, Mo: 0.1-1.0%, Ni: 0.1-1.5%, Ti: 0.005-0.05%, P: 0.006% or less, S: 0.003% or less, and the balance being Fe and unavoidable impurities. The flux is composed of SiO2: 13-25%, MgO: 8-20%, CaO: 5-13%, CaF2: 1-7%, Al2O3: 9-23%, TiO2: 3-11%, Fe: 11-25%, B2O3: 0.1-0.6%, Mo: 1-4.3%, and Ni: 1-4.5%. This welding method is said to provide excellent weld metal mechanical performance and good welding workability even in high heat input submerged arc welding with a welding heat input of 500 kJ / cm or more, and to significantly increase the safety of architectural structures while at the same time significantly increasing welding efficiency.

[0006] Narrow-gap welding has also been proposed as a highly efficient welding method for thick plates. By reducing the cross-sectional area of ​​the groove, it is possible to reduce the amount of heat input during welding, and it is possible to ensure the toughness of the weld metal and the heat-affected zone of the base metal. However, when welding thick plates using narrow-gap welding, there is a problem that hot cracks and incomplete fusion are likely to occur.

[0007] For this problem, for example, Patent Document 3 discloses a "narrow gap submerged arc welding method". The welding method disclosed in Patent Document 3 is a narrow gap submerged arc welding method for extra thick steel plates, in which a backing material is abutted against the back side of a narrow gap with a groove angle of 1 to 5° and a root gap of 10 to 14 mm, and steel particles are scattered in the groove to a height of 10 to 15 mm from the back side of the groove. Then, a molten flux containing, in mass % relative to the total mass of the flux, a total of 50 to 70% of Al2O3, TiO2, and CaF2, 10 to 20% of SiO2, and the rest being CaO, MnO, BaO, K2O, Na2O, and unavoidable impurities is used. Then, the method is a narrow gap submerged arc welding method with one layer and one pass multi-layer welding. According to Patent Document 3, a sound welded joint free of welding defects such as hot cracking, slag inclusion, and incomplete fusion can be obtained, the slag is easily removable, the bead shape is good, and welding workability is excellent, and welding can be performed without back chipping. Patent Document 3 claims to be able to provide such a highly efficient narrow gap submerged arc welding method.

[0008] Also, for example, Patent Document 4 discloses a "highly efficient welding method for thick steel plates". According to Patent Document 4, the method includes a processing step of processing an X-shaped groove on a pair of steel materials having a plate thickness of more than 50 mm and less than 100 mm. Furthermore, the method includes a welding step of performing one pass of welding on each of the front and back sides of the pair of steel materials using a flux by multi-electrode submerged arc welding with two or more and six or less electrodes. In the welding step, the welding current of the first electrode is an AC current with a waveform ratio of 60% or more and 90% or less, and the welding current of the other electrodes is an AC current with a waveform ratio of 70% or more or a negative DC current. The flux used here contains Al2O3: 10% or more and 50% or less, and SiO2: 16% or more and 30% or less, in mass ratio with respect to the total mass of the flux. In addition, one or more of MgO, TiO2, CaF2, and MnO are contained in a total amount of 10% or more and 60% or less, with MgO limited to 40% or less, TiO2 limited to 20% or less, CaF2 limited to 30% or less, and MnO limited to 20% or less. By using such a submerged arc welding method, it is possible to obtain a weld metal with excellent toughness even at low temperatures, so it is said that the foundation parts of wind power generation facilities to be installed in cold regions can be efficiently manufactured.

[0009] In the submerged arc welding method, which is a narrow gap welding method for thick steel plates as described above, it is necessary to spray flux in front of the weld before welding and to collect the flux after welding, and these fluxes must be managed separately. Furthermore, after welding, the slag formed in the weld must be removed, which makes the work less efficient. In response to this, a narrow gap gas shielded arc welding method has been proposed that has excellent workability during on-site construction.

[0010] For example, Patent Document 5 discloses a narrow-gap gas-shielded arc welding method for joining thick steel materials by narrow-gap multi-layer welding. In the technology described in Patent Document 5, the first layer welding is performed by multi-electrode welding with two or more electrodes, the first electrode and the second electrode are positioned along a predetermined parallel welding line, and the distance between the welding wire tips of the first electrode and the second electrode is controlled to a range of 5 mm to 16 mm. In addition, the angle of the straight line connecting the welding wire tips of the first electrode and the second electrode with respect to the perpendicular direction of the welding line is controlled to a range of 45° or less. Furthermore, the melting depth perpendicular to the welding line at the bottom of the thick steel material is set to 1.5 mm or more. As a result, even when groove processing such as gas cutting or plasma cutting is performed, there is no defect and the welding construction efficiency is improved. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Patent No. 4673710 [Patent Document 2] JP 2006-212676 A [Patent Document 3] JP 2021-126696 A [Patent Document 4] International Publication No. 2013 / 073565 [Patent Document 5] Patent No. 6137053 Summary of the Invention [Problem to be solved by the invention]

[0012] However, the invention of Patent Document 1, which aims to realize high-efficiency construction by large heat input welding, aims to provide a welding method that can obtain high toughness with 2 mm V-notch Charpy absorbed energy of 70 J or more at 0 ° C. In other words, it is not suitable for use in a cold environment of -40 ° C. In Patent Document 2, the toughness evaluation is also performed at 0 ° C, and use in a cold environment of -40 ° C is not assumed. Furthermore, the invention of Patent Document 3, which aims to realize high-efficiency construction by narrow gap welding, does not mention the mechanical properties of the weld metal and the base metal heat affected zone (hereinafter, the base metal heat affected zone is also called "weld heat affected zone"). Similarly, the invention of Patent Document 4 does not mention the low-temperature toughness value of the weld heat affected zone, and is intended for welding of steel materials with a plate thickness of more than 50 mm and 100 mm or less. Therefore, there is no knowledge about welding of thick plates with a plate thickness of up to 160 mm, such as those used in marine structures and foundation equipment for offshore wind power generators. Furthermore, in the narrow gap gas-shielded arc welding method disclosed in Patent Document 5, when multi-electrode welding using three or more electrodes is performed, hot cracks may occur in the center of the weld metal.

[0013] The present invention aims to solve the problems of the prior art and to provide a method for manufacturing a narrow gap welded joint using steel plate with a thickness of 50 mm or more by gas shielded arc welding, which is free of welding defects, has high strength, and has excellent low-temperature impact toughness.

[0014] In this context, "high strength" refers to a weld metal manufactured in accordance with the provisions of JIS Z 3111 having a room temperature yield strength (0.2% proof stress) of 325 MPa or more, a tensile strength of 520 MPa or more, and a welded joint having a room temperature tensile strength of 520 MPa or more. Also, "excellent low-temperature impact toughness" refers to the absorbed energy (vE -40 This means that the value is 30J or more. [Means for solving the problem]

[0015] [How the present invention was made] In order to achieve the above-mentioned object, the inventors first conducted extensive research into a weld metal shape that can efficiently and soundly weld welded joints of steel plates (hereinafter also referred to as "base metal") having a plate thickness of 50 to 160 mm. The total length of the welds for marine structures and foundations for offshore wind power plants can exceed 1.0 km per structure, and reducing the number of layers of weld metal is effective for highly efficient welding. Here, it was defined that high efficiency is achieved when the ratio [p / T] of the total number of layers of weld metal p to the plate thickness T is 0.40 layers / mm or less. Furthermore, when the deposition area of ​​the weld metal per layer is 120.0 mm in cross-sectional area perpendicular to the weld line, 2 It has been found that if the welding heat input is below this value, the thermal effect on the steel plate is sufficiently small, and excellent low-temperature toughness characteristics of the weld metal can be obtained.

[0016] After careful consideration of the groove shape that satisfies the above, it was found that a groove angle of 20° or less and a gap between the base materials of 6 mm or less for one-sided welding and 10 mm or less for double-sided welding, respectively, would be satisfactory.

[0017] On the other hand, it was found that if the gap between the base materials exceeds 6 mm, there is a possibility that poor fusion may occur during welding of the first layer, and further, if the groove angle is less than 4°, poor fusion and hot cracking are likely to occur during welding. In other words, it was found that the groove shape that can weld 50 to 160 mm steel plates soundly and efficiently is preferably a gap between the base materials of 6 mm or less and a groove angle of 4° to 20°, regardless of whether single-sided welding or double-sided welding is used.

[0018] Furthermore, the shape of the weld metal when welding is performed on the above groove shape was studied. As a result, it was found that it is preferable that the weld metal has three or more layers in any cross section perpendicular to the weld line of the weld metal, and that the width W (mm) of the weld metal for each layer, excluding the first layer and the outermost layer, is 5.0 to 0.4T (mm). Here, the width of the first layer is 5.0 mm or less depending on the gap between the base metals, but this does not particularly deteriorate the properties of the weld metal. In addition, the outermost layer may be repaired to make the surface shape of the reinforcement more beautiful, or to improve defects such as a convex bead at the toe of the reinforcement, undercut, or overlap. For these reasons, the weld metal of the first layer and the outermost layer are excluded because they are non-steady parts.

[0019] [Summary of the present invention] The present invention was completed based on these findings and through further investigation, and the gist of the present invention is as follows. [1] In a method for manufacturing a welded joint by gas-shielded arc welding of steel plates, The thickness T (mm) of the steel plate is 50 to 160 mm, The weld metal consists of three or more layers. The width W (mm) of each layer excluding the first layer and the outermost layer of the weld metal is 5.0 or more and 0.4T or less (mm), The cross-sectional area A (mm 2 ) and the number of weld layers p (layers) ratio [A / p] is 120.0 mm 2 / layer or lower, The ratio [p / T] of the number of welded layers p to the plate thickness T is 0.40 layers / mm or less, The gas shielded arc welding is a multi-electrode welding having three or more electrodes, The tips of the welding wires of the first electrode and the second electrode are disposed on different parallel welding lines; One of the first electrode and the second electrode is a wire negative (positive polarity), and the other is a wire positive (reverse polarity), The distance a (mm) between the welding wire tips of the first electrode and the second electrode is 5 to 16 mm, an angle α of a straight line connecting the welding wire tips of the first electrode and the second electrode with respect to a perpendicular direction of the welding line is 60° or less; A welding wire containing 0.015 to 0.100 mass % of REM is used for the electrode that is the negative (positive) wire. A method for manufacturing welded joints by gas-shielded arc welding of steel plates. [2] In the above [1], a tilt angle Φ of a tip of each of the first electrode and the second electrode toward a groove surface side with respect to a perpendicular direction of the weld line is 0° to 15°, A distance d (mm) between a side end portion of each of the welding wire tips of the first electrode and the second electrode and the groove surface is 0.5 to 3.0 mm, Each of the welding wires is a welding wire that is bent in advance to have a radius of curvature in the range of 150 to 300 mm, A third electrode and subsequent electrodes are disposed at the center of the groove behind the first electrode and the second electrode, Use a gas containing 60% or more of CO2 gas as a shielding gas. A method for manufacturing welded joints by gas-shielded arc welding of steel plates. [3] In the above [1] or [2], the chemical composition of the steel plate is, in mass%, C: 0.04 to 0.14%, Si: 0.03 to 0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001 to 0.100%, O: 0.0100% or less, and N: 0.0100% or less The balance is Fe and unavoidable impurities, Ceq and plate thickness (T) defined by the following formula (1) are 0.0004T+0.25≦Ceq≦0.0004T+0.45 The composition satisfies the following: The dislocation density ρ at a position 1 mm below the surface of the steel plate is 4.0×10 14 m -2 is as follows: The average crystal grain size at a position 1 mm below the surface of the steel plate is 15.0 μm or less, and the average crystal grain size at the center of the plate thickness is 20.0 μm or less; A method for manufacturing welded joints by gas-shielded arc welding of steel plates. Ceq=[C]+[Mn] / 6+([Cr]+[Mo]+[V]) / 5+([Cu]+[Ni]) / 15...(1) However, each element symbol in the above formula (1) represents the content (mass%) of the corresponding element, and if the corresponding element is not contained, it is set to 0. [4] In the above [3], the chemical composition of the steel plate further comprises, in mass%, Cu: 2.000% or less, Ni: 2.500% or less, Cr:1.500% or less, Mo: 1.000% or less Ti: 0.100% or less, V: 0.300% or less, B: 0.0100% or less, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less A method for producing a welded joint by gas-shielded arc welding of steel plates, comprising one or more types selected from the group consisting of: [5] In any one of the above [1] to [4], the chemical composition of the weld metal is, in mass%, C: 0.04 to 0.14%, Si: 0.03 to 0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001 to 0.100%, Cu: 0.001 to 2.000%, Ni: 0.001 to 2.500%, Cr: 0.001~1.500%, Mo: 0.001 to 1.000%, Ti: 0.001 to 0.100%, V: 0.001 to 0.300%, B: 0.001 to 0.020%, O: 0.050% or less, and N: 0.010% or less The balance is Fe and unavoidable impurities. A method for manufacturing welded joints by gas-shielded arc welding of steel plates. [6] In the above [5], the chemical composition of the weld metal further comprises, in mass%, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less A method for producing a welded joint by gas-shielded arc welding of steel plates, comprising one or more types selected from the group consisting of: Effect of the Invention

[0020] According to the present invention, a welded joint can be obtained by welding steel plates having a thickness of 50 to 160 mm, and the welded joint has sound weld metal free of welding defects such as high-temperature cracking and insufficient fusion, and is a narrow-gap welded joint that combines high strength with excellent low-temperature impact toughness, and therefore has a significant industrial effect.

[0021] The welded joint of steel plates according to the present invention is not limited to marine structures and offshore wind turbines, but can also be applied to, for example, shipbuilding, line pipes, construction, and the like. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is a schematic cross-sectional view showing the shape of a weld metal of a welded joint according to the present invention. [Diagram 2]FIG. 2 is a schematic cross-sectional view of a weld metal illustrating a welding process for a welded joint according to the present invention. [Diagram 3] FIG. 3 is a partially enlarged schematic cross-sectional view of a weld metal illustrating a welding process using three electrodes. [Figure 4] FIG. 4 is a schematic plan view showing a welding process using three electrodes. [Diagram 5] FIG. 5 is a schematic plan view showing a welding process using four electrodes. [Figure 6] FIG. 6 is a schematic cross-sectional view showing (a) a groove shape in a V groove and (b) a groove shape in an X groove. [Figure 7] FIG. 7 is a side cross-sectional view that illustrates a schematic relationship between a gas supply nozzle and an electrode according to the present invention. [Figure 8] FIG. 8 is a plan view showing a schematic relationship between the gas supply nozzle and the electrodes according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The present invention will be described in detail below. Note that the present invention is not limited to the following embodiments.

[0024] [Cross-sectional shape of welded joint] First, a welded joint of steel plates according to the present invention will be described. The welded joint of steel plates according to the present invention is a butt welded joint of steel plates having a plate thickness T (mm) of 50 to 160 mm, the weld metal is composed of three or more layers, and the width W (mm) of each layer excluding the initial layer and the outermost layer of the weld metal is 5.0 to 0.4T (mm). 2 ) and the number of weld layers p (layers) ratio [A / p] is 120.0 mm 2 / layer or less, and the ratio [p / T] of the number of weld layers p to the plate thickness T is 0.40 layers / mm or less. In the present invention, with the above groove shape, sound and highly efficient welding is possible without being limited to one layer and one pass.

[0025] Here, the thickness T of the steel plate is set to 50 mm or more for application to large structures, etc. There is no particular upper limit for the thickness T, but it is set to 160 mm or less due to manufacturing constraints. Here, the weld line refers to a virtual line when expressing a bead or a welded part as a single line.

[0026] The cross-sectional shape of the above-mentioned welded joint will be described with reference to FIG. In the present invention, the first layer L1 and the outermost layer L P The weld metal excluding the L2 layer, i.e., the L3 layer P-1 As mentioned above, the first layer and the outermost weld metal are excluded because they are non-steady parts. For example, the i-th weld layer (L i ) width W i Then, this width W i represents the width of the weld metal (i.e., the distance between the fusion lines) at the center line between the top and bottom of each layer. The width W (mm) of this weld metal is stipulated to be 5.0 to 0.4T (mm). In other words, the first layer L1 and the outermost layer L P Layer L2 to L excluding P-1 The width W of each layer is determined by cross-sectional macroscopic observation, etc., and each value is limited to be in the range of 5.0 mm or more and 0.4T (mm) or less. If the width W of each layer is less than 5.0 mm, the groove likelihood when placing the steel plate before welding is small, and physical interference between the welding wire and the groove wall is likely to occur during welding, resulting in a decrease in welding efficiency. Furthermore, a pear-shaped weld bead is likely to be formed, the possibility of hot cracking is significantly increased, and poor fusion is also likely to occur. Preferably, the width W is 8.0 mm or more. The upper limit of the width W is set to 0.4T (mm) because the area of ​​the weld metal is affected by the plate thickness T, and in the present invention, which targets steel plates with a plate thickness of 50 to 160 mm, if the width W exceeds 0.4T (mm), the area of ​​the weld metal becomes too large, resulting in a decrease in welding efficiency. The width W is preferably 0.35T mm or less, and more preferably 0.3T mm or less.

[0027] In addition, the cross-sectional area A (mm 2), the welding layers are L1 (first layer) to L p When construction is performed up to the top layer (p), the cross-sectional area per layer [A / p] is 120.0 mm 2 In other words, it is preferable that the deposition area of ​​the weld metal is 120.0 mm per layer or less. 2 If the ratio [A / p] is set to 100.0 mm or less, the amount of welding heat input is not excessive, the thermal effect on the base material is sufficiently small, and excellent low-temperature toughness characteristics of the weld metal and the weld heat-affected zone can be obtained. 2 The lower limit of this ratio [A / p] is not specified, but from the viewpoint of welding efficiency, the ratio [A / p] is preferably 30.0 mm 2 / layer or more, more preferably 45.0 mm 2 / layer or more.

[0028] Furthermore, it is preferable that the ratio [p / T] of the number of weld layers p to the plate thickness T is 0.40 layers / mm or less. If this ratio [p / T] is greater than 0.40 layers / mm, the number of welding passes required to produce a welded joint increases, and the welding efficiency decreases. Therefore, by controlling the ratio [p / T] to 0.40 layers / mm or less, highly efficient welding can be achieved. More preferably, the ratio [p / T] is 0.35 layers / mm or less. There is no particular lower limit for this ratio, but for reasons of resistance to welding defects, the ratio [p / T] is preferably 0.10 layers / mm or more, and more preferably 0.13 layers / mm or more.

[0029] [Chemical composition of steel plate] Next, the steel plate which is the base material of the welded joint of the present invention will be described. First, the steel plate may be a carbon steel or a low alloy steel. Next, the chemical composition will be described. The "%" in the chemical composition described below means "mass %" unless otherwise specified.

[0030] [Basic composition of steel plate] Among the chemical compositions of the steel plates of the welded joint according to the present invention, the basic composition is as follows. It is preferable that the steel sheet has a chemical composition containing C: 0.04 to 0.14%, Si: 0.03 to 0.70%, Mn: 0.30 to 2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001 to 0.100%, O: 0.0100% or less, and N: 0.0100% or less, with the balance being Fe and unavoidable impurities.

[0031] The reason why the chemical composition of the steel sheet according to the present invention is specified as above will be explained. [C: 0.04~0.14%] C is an element that can most inexpensively improve the strength of a steel plate, and also contributes to strengthening the austenite grain boundaries. If the C content is less than 0.04%, the grain boundary strength of austenite decreases, and hot cracking of the slab occurs, so that manufacturability is significantly reduced. In addition, there is a possibility that the strength targeted by the present invention cannot be obtained. On the other hand, if the C content exceeds 0.14%, the weldability decreases, and the toughness may also decrease. Therefore, the C content is preferably 0.04 to 0.14%. In addition, the C content is more preferably 0.05 to 0.12%.

[0032] [Si: 0.03~0.70%] Although Si is an effective element for deoxidization, if the Si content is less than 0.03%, it may not be possible to obtain a sufficient effect. On the other hand, if the Si content exceeds 0.70%, the weldability may decrease. Therefore, the Si content is preferably 0.03 to 0.70%. The Si content is more preferably 0.04 to 0.60%.

[0033] [Mn: 0.30~2.50%] Mn is an element that can improve the hardenability and strength of steel at low cost. To obtain this effect, it is preferable to contain 0.30% or more of Mn. On the other hand, if the Mn content exceeds 2.50%, the weldability may decrease. Therefore, the Mn content is preferably 0.30 to 2.50%. The Mn content is more preferably 0.50 to 2.20%.

[0034] [P:0.030% or less] P is an element that has a strong effect of embrittling grain boundaries, and if contained in a large amount, it may reduce the toughness of the steel plate. Therefore, the P content is preferably 0.030% or less. Furthermore, the P content is more preferably 0.025% or less. On the other hand, since the lower the P content, the more preferable it is, the lower limit of the P content is not particularly limited and may be 0%. However, P is an element that is inevitably contained in the steel plate as an impurity, and excessively reducing the P content leads to an increase in refining time and an increase in costs, so the P content is preferably 0.001% or more.

[0035] [S:0.020% or less] Since S may reduce the toughness of the steel plate, the S content is preferably 0.020% or less. Furthermore, the S content is more preferably 0.010% or less. On the other hand, since the lower the S content, the more preferable it is, the lower limit of the S content is not particularly limited and may be 0%. However, S is an element that is inevitably contained in the steel plate as an impurity, and excessive reduction in S content leads to an increase in refining time and an increase in costs, so the S content is preferably 0.0001% or more.

[0036] [Nb: 0.001~0.100%] Nb is an element that has the effect of suppressing recrystallization when strain is applied to the austenite structure through solid solution Nb and finely precipitated NbC, and also raising the non-recrystallization temperature range to the higher temperature side. In order to obtain this effect, the Nb content is preferably 0.001% or more. On the other hand, if the Nb content exceeds 0.100%, there is a possibility that the weldability will deteriorate. Therefore, the Nb content is preferably 0.001 to 0.100%. The Nb content is more preferably 0.005 to 0.075%. Furthermore, the Nb content is particularly preferably 0.005 to 0.050%.

[0037] [Al: 0.001~0.100%] Al is an element that is effective as a deoxidizer and also has the effect of forming nitrides to reduce the austenite grain size. In order to obtain this effect, the Al content is preferably 0.001% or more. On the other hand, if the Al content exceeds 0.100%, the cleanliness of the steel material or steel plate may decrease, and as a result, the ductility and toughness may decrease. Therefore, the Al content is preferably 0.001 to 0.100%. The Al content is more preferably 0.005 to 0.080% or less.

[0038] [O:0.0100% or less] Since O is an element that reduces ductility and toughness, the O content is preferably 0.0100% or less. On the other hand, since the lower the O content, the more preferable it is, the lower limit of the O content is not particularly limited and may be 0%. However, since O is an element that is inevitably contained in steel sheet as an impurity, and excessive reduction in O content leads to an increase in refining time and an increase in costs, the O content is preferably 0.0005% or more.

[0039] [N:0.0100% or less] Since N is an element that reduces ductility and toughness, the N content is preferably 0.0100% or less. On the other hand, since the lower the N content, the better, the lower limit of the N content is not particularly limited and may be 0%. However, since N is an element that is inevitably contained in the weld metal as an impurity, excessive reduction in N content leads to an increase in refining time and an increase in costs. Therefore, the N content is preferably 0.0005% or more.

[0040] [Optional composition of steel plate] The steel plate for the welded joint of the present invention has the above-mentioned basic composition to obtain the characteristics targeted by the present invention. However, in order to further improve the strength and weldability (specifically, the toughness of the welded part, the weldability, etc.), the steel plate may contain the following optional compositions as necessary in addition to the above-mentioned basic composition.

[0041] One or more selected from the group consisting of Cu: 2.000% or less, Ni: 2.500% or less, Cr: 1.500% or less, Mo: 1.000% or less, Ti: 0.100% or less, V: 0.300% or less, B: 0.0100% or less, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less. Since Cu, Ni, Cr, Mo, Ti, V, B, W, Ca, Mg, and REM are chemical compositions that can be contained arbitrarily, the content of these elements may be 0%.

[0042] [Cu:2.000% or less] Cu is an element that can improve the strength of the steel plate without significantly deteriorating the toughness of the steel plate. On the other hand, if the Cu content exceeds 2.000%, hot cracking due to the Cu-enriched layer formed just below the scale may become a problem. Therefore, when Cu is contained, the Cu content is preferably 2.000% or less. More preferably, the Cu content is 0.010 to 1.500%.

[0043] [Ni:2.500% or less] Ni is an element that has the effect of improving the hardenability and toughness of the steel plate. On the other hand, if the Ni content exceeds 2.500%, an increase in manufacturing costs may become a problem. Therefore, when Ni is contained, the Ni content is preferably 2.500% or less. More preferably, the Ni content is 0.010 to 2.000%.

[0044] [Cr:1.500% or less] Cr is an element that can improve the hardenability of a steel sheet, thereby improving the strength of the steel sheet. On the other hand, if the Cr content exceeds 1.500%, the weldability may be reduced. Therefore, when Cr is contained, the Cr content is preferably 1.500% or less. More preferably, the Cr content is 0.010 to 1.200%.

[0045] [Mo: 1.000% or less] Mo is an element that can improve the hardenability of a steel sheet, thereby improving the strength of the steel sheet. On the other hand, if the Mo content exceeds 1.000%, the weldability may be reduced. Therefore, when Mo is contained, the Mo content is preferably 1.000% or less. More preferably, the Mo content is 0.010 to 0.800%.

[0046] [Ti:0.100% or less] Ti is an element that has the effect of pinning the movement of grain boundaries by precipitating as TiN and suppressing grain growth. On the other hand, if the Ti content exceeds 0.100%, the cleanliness of the steel sheet structure may decrease, and as a result, the ductility and toughness may decrease. Therefore, when Ti is contained, the Ti content is preferably 0.100% or less. More preferably, the Ti content is 0.001 to 0.080%.

[0047] [V:0.300% or less] V is an element that can improve the hardenability of a steel sheet and can improve the strength of the steel sheet by forming carbonitrides. On the other hand, if the V content exceeds 0.300%, the weldability may decrease. Therefore, when V is contained, the V content is preferably 0.300% or less. More preferably, the V content is 0.010 to 0.250%.

[0048] [B:0.0100% or less] B is an element that has the effect of improving the hardenability by adding a very small amount, thereby improving the strength of the steel sheet. On the other hand, if the B content exceeds 0.0100%, the weldability may decrease. Therefore, when B is contained, the B content is preferably 0.0100% or less. More preferably, the B content is 0.0001 to 0.0070%.

[0049] [W:0.500% or less] W is an element that can improve the hardenability of steel, thereby improving the strength of the steel plate. On the other hand, if the W content exceeds 0.500%, the weldability may decrease. Therefore, when W is contained, the W content is preferably 0.500% or less. More preferably, the W content is 0.010 to 0.400%.

[0050] [Ca:0.0200% or less] Ca is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the Ca content exceeds 0.0200%, the cleanliness may decrease and the toughness of the steel plate may be impaired. Therefore, when Ca is contained, the Ca content is preferably 0.0200% or less. More preferably, the Ca content is 0.0001 to 0.0180%.

[0051] [Mg:0.0200% or less] Mg is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the Mg content exceeds 0.0200%, the effect of adding Mg becomes saturated and an effect commensurate with the content cannot be expected, which may be economically disadvantageous. Therefore, when Mg is contained, the Mg content is preferably 0.0200% or less. More preferably, the Mg content is 0.0001 to 0.0180%.

[0052] [REM:0.0500% or less] REM (rare earth metal) is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the REM content exceeds 0.0500%, the effect of adding REM becomes saturated and the effect commensurate with the content cannot be expected, which may be economically disadvantageous. Therefore, when REM is contained, the REM content is preferably 0.0500% or less. More preferably, the REM content is 0.0001 to 0.0450%.

[0053] [Remainder of steel plate composition] The steel plate for the welded joint of the present invention has the above chemical composition and the remainder is Fe and inevitable impurities. Examples of inevitable impurities include H, Zn, Re, Co, Sb, Bi, etc., and a total of 0.0100% or less is acceptable. In addition, as long as the basic composition and optional composition are satisfied, elements other than these may be contained, and such embodiments are also included in the technical scope of the present invention.

[0054] [Ceq] Furthermore, it is more preferable that the chemical composition of the above steel sheet satisfies the following conditions. The relationship between Ceq and plate thickness T (mm) is as follows: 0.0004T+0.25≦Ceq≦0.0004T+0.45 It satisfies the above. Here, Ceq is defined by the following formula (1) and is an index of hardenability due to contained elements. Ceq=[C]+[Mn] / 6+([Cr]+[Mo]+[V]) / 5+([Cu]+[Ni]) / 15...(1) In the formula (1), each element symbol represents the content (mass%) of the corresponding element, and if the corresponding element is not contained, it is set to 0.

[0055] In the present invention, in order to obtain a desired high-strength structure, it is necessary to control the cooling rate according to the plate thickness T of a certain steel plate and the amount of alloy added according to the plate thickness T. If Ceq is less than (0.0004T+0.25), the required strength cannot be obtained. On the other hand, if Ceq is greater than (0.0004T+0.45), the strength becomes too high at the surface of the steel plate, where the cooling rate is faster than at the center of the plate thickness, and the low-temperature impact toughness becomes low. For this reason, 0.0004T+0.25≦Ceq≦0.0004T+0.45 It is preferable that the above formula is satisfied. More preferably, the formula is as follows: 0.0004T+0.27≦Ceq≦0.0004T+0.43 It is.

[0056] [Steel plate properties] Here, the characteristics of the steel plate used in the welded joint according to the present invention will be described. Dislocation density ρ(m -2 ) is 4.0×10 14 m -2 The dislocation density ρ(m -2 ) refers to the dislocation length per unit volume present in a metal crystal. The reason for specifying the position 1 mm below the surface of the base material (i.e. "1 mm below the surface of the steel plate") is from the perspective of the bending workability of the steel plate. The bending workability of a steel plate is determined by the ductility of the surface layer structure of the steel plate. If the dislocation density of the surface layer structure increases due to processing strain during hot rolling, the deformation limit of the surface layer structure decreases, and bending workability decreases. For this reason, the dislocation density 1 mm below the surface of the steel plate is set to 4.0 × 10 14 m -2 In addition, since the steel structure usually inevitably contains dislocations, the above dislocation density was set to 1.0 × 10 11 m -2 Therefore, the dislocation density is preferably 1.0×10 11 m -2 More preferably, it is 3.0×10 14 m -2 The following is the result.

[0057] It is also preferable that the average crystal grain size at a position 1 mm below the surface of the base material is 15.0 μm or less, and the average crystal grain size at the center position of the plate thickness of the base material is 20.0 μm or less.

[0058] The average grain size refers to the average of all grains at a position 1 mm below the surface of the steel sheet and at the center of the thickness of the sheet, when the region surrounded by the boundary with a crystal orientation difference of 15° or more is regarded as a grain, and can be measured by the method described in the examples described later. The finer the grain size of the surface layer structure of the steel sheet, the more the toughness of the surface layer of the steel sheet is improved. In order to obtain this effect, it is preferable that the average grain size at a position 1 mm below the surface of the steel sheet is 15.0 μm or less. More preferably, the average grain size at a position 1 mm below the surface of the steel sheet is 13.0 μm or less. Furthermore, the finer the grain size of the steel structure at the center of the thickness of the steel sheet, the more the toughness at the center of the thickness of the steel sheet is improved. In order to obtain this effect, it is preferable that the average grain size at the center of the thickness of the sheet is 20.0 μm or less. More preferably, the average grain size at the center of the thickness of the sheet is 15.0 μm or less. Here, in the present invention, "1 mm below the surface of the steel sheet" refers to a depth position of 1 mm in the thickness direction from the surface of the steel sheet. The "plate thickness center position" refers to the 1 / 2 position of the plate thickness.

[0059] [Steel plate manufacturing method] Next, a method for manufacturing the above steel sheet will be described. The steel plate to which the present invention is directed is obtained by heating, hot rolling, and cooling a slab (steel material) having the above-mentioned composition. After the cooling, an optional tempering process can be performed. Various preferable conditions are explained below. However, the manufacturing method is not limited to a specific method, and it is sufficient if it includes the above-mentioned steps.

[0060] In the following description of the manufacturing method, the temperature indicated in "°C" refers to the surface temperature of the slab or steel plate unless otherwise specified. The surface temperature can be measured, for example, by a radiation thermometer.

[0061] In the present invention, the method for producing the slab is not particularly limited, and any of the known methods for producing the slab, such as a converter, an electric furnace, a vacuum melting furnace, etc., is suitable. The slab is produced to the desired dimensions, for example, by a continuous casting method. The molten steel may further be subjected to secondary refining, such as ladle refining.

[0062] ·Heating conditions As described above, it is preferable to heat the manufactured slab to a temperature of 1000 to 1200 ° C. If the heating temperature of the slab is less than 1000 ° C., the coarse NbC precipitated inside the slab during slab casting does not redissolve and remains. As a result, the effect of increasing the temperature of the non-recrystallization temperature range by the dissolved Nb and the fine NbC reprecipitated during hot rolling cannot be obtained. Accordingly, the effect of refining the crystal grains by the controlled rolling is reduced, and the toughness is reduced. On the other hand, if the heating temperature of the slab exceeds 1200 ° C., the grain size at the start of hot rolling becomes coarse due to the grain growth of austenite, and the grain size of the final structure after hot rolling also becomes coarse accordingly, and the toughness is reduced. Therefore, the heating temperature of the slab is preferably 1000 to 1200 ° C. The heating temperature of the slab is more preferably 1030 ° C. or more, and further preferably 1170 ° C. or less.

[0063] Hot rolling conditions Next, the heated slab is preferably hot-rolled. As described above, in the present invention, the dislocation density and average grain size at a position 1 mm below the steel sheet surface, and the average grain size at the center of the sheet thickness are important. In order to obtain various properties, it is preferable to roll the slab under the following hot rolling conditions.

[0064] Here, the temperature range from (8250[Nb]+770°C) to Ar3 temperature at a temperature 1 mm below the surface of the steel plate or at the center of the plate thickness is referred to as the non-recrystallization temperature range. The temperature at the center of the plate thickness of the steel plate can be obtained, for example, by measuring with a thermocouple attached at the center of the plate thickness of the steel plate, or by calculating the temperature distribution in the cross section of the steel plate by heat transfer analysis and correcting the result by the surface temperature of the steel plate. The above-mentioned [Nb] represents the content (mass%) of the element in the chemical composition of the steel plate described above.

[0065] First, the steel plate temperature at 1 mm below the surface is temporarily cooled to Ar3 temperature or lower, and then reheated to exceed Ac3 temperature. Next, reduction is performed at a rolling rate of 25% or more in the temperature range where the steel plate temperature at 1 mm below the surface is from (8250[Nb]+770°C) to Ar3 temperature. After that, reduction is performed at a total rolling rate of 15% or less in the temperature range where the steel plate temperature at 1 mm below the surface is less than Ar3 temperature.

[0066] During hot rolling of a heated slab, the surface layer of the steel sheet is cooled once to below the Ar3 temperature, transforming the austenite into a low-temperature structure such as ferrite. The surface layer of the steel sheet is then heated to above the Ac3 temperature by reheating, retransforming into an austenite structure and turning the surface layer of the steel sheet into fine austenite.

[0067] The cooling in the hot rolling process may be performed by water cooling, air cooling, or the like, and any method may be used as long as the temperature can be controlled to a predetermined level. For example, water cooling is used to cool the steel sheet to a temperature of Ar3 or lower, and the retention time at which the steel sheet is at a temperature of Ar3 or lower at a position 1 mm below the surface is preferably 5 seconds or more, and more preferably 300 seconds or less. Reheating after cooling involves holding the steel sheet in the atmosphere, and the retention time is preferably 30 seconds or more, and more preferably 600 seconds or less.

[0068] Next, a rolling reduction of 25% or more is applied in the temperature range of (8250[Nb]+770°C) to Ar3 temperature, where the surface layer of the steel sheet is in the non-recrystallization temperature range, to introduce processing strain into the austenite in the surface layer of the steel sheet. This acts as a transformation nucleus during final cooling, resulting in a fine structure with good toughness. Preferably, the rolling reduction in this temperature range is 30% or more. From the viewpoint of rolling efficiency, the rolling reduction in this temperature range is preferably 80% or less, and even more preferably 70% or less.

[0069] There is no particular upper limit on the number of passes in this temperature range. In addition, as long as the above-mentioned rolling reduction condition is satisfied, the rolling may be performed, for example, in a plurality of passes.

[0070] If the total reduction exceeds 15% in the temperature range where the temperature of the steel sheet surface layer is below the Ar3 temperature, processing strain is introduced into the ferrite structure and pearlite structure in which transformation is completed in the steel sheet surface layer, resulting in a decrease in ductility and deterioration of bending workability. Therefore, it is preferable to set the total reduction in the temperature range where the temperature of the steel sheet surface layer is below the Ar3 temperature to 15% or less. The total reduction in this temperature range is more preferably set to 6% or less.

[0071] By controlling the structure through the above-mentioned rolling conditions for the steel sheet surface layer, it is possible to give the steel sheet surface layer a structure having a low dislocation density, a small crystal grain size, and excellent bending workability and toughness.

[0072] Next, it is advisable to apply reduction to the center of the plate thickness so that the steel plate temperature at the center of the plate thickness is below (8250[Nb]+770°C) and the total reduction rate in the temperature range above the Ar3 temperature is 25% or more.

[0073] During hot rolling of the heated slab under the above-mentioned rolling conditions of the steel plate surface layer, a reduction of 25% or more is applied in the temperature range of (8250[Nb]+770°C) to Ar3 temperature, which is the non-recrystallization temperature range of the center of the thickness of the steel plate. This introduces processing strain into the austenite at the center of the thickness. This acts as a transformation nucleus during final cooling, resulting in a fine structure with good toughness. Therefore, it is preferable to set the total reduction rate to 25% or more in the temperature range where the center of the thickness of the steel plate is (8250[Nb]+770°C) or less. More preferably, the total reduction rate in this temperature range is 30% or more. From the viewpoint of rolling efficiency, the total reduction rate in this temperature range is preferably 80% or less, and even more preferably 70% or less.

[0074] In addition, if the temperature at the center of the thickness of the steel plate is lower than the Ar3 temperature, processing strain is introduced into the generated ferrite, and the toughness is reduced. Therefore, it is preferable that the temperature at the center of the thickness of the steel plate is Ar3 temperature or higher.

[0075] In the present invention, the temperature ranges may overlap within the above-mentioned rolling conditions in the two types of rolling, "rolling on the steel sheet surface layer" and "rolling on the sheet thickness center position". In this case, the reduction amounts in the overlapping temperature ranges are integrated as the reduction amounts for the "steel sheet surface layer" and the "sheet thickness center position", and the integrated reduction amounts should be within the ranges of the rolling conditions.

[0076] Here, the total reduction ratio at the surface layer and the center of thickness of the steel plate is Total reduction rate = (r0-r1) / r0 x 100 (%) Here, r0 is the thickness at the start of the first rolling, and r1 is the thickness after the final rolling. The Ar3 temperature and Ac3 temperature can be obtained by a Formastor test or the like.

[0077] By controlling the structure through the above-mentioned rolling conditions at the center position of the thickness of the steel plate, the center position of the steel plate can have a structure with small crystal grain size and excellent toughness.

[0078] Cooling conditions After the above-mentioned hot rolling, the obtained steel plate is cooled. In the cooling, the average cooling rate in the temperature range of 700 to 550 °C at the center of the thickness of the steel plate is 2500 × t [mm]. -1.7 The cooling is performed at a rate of 0.4 °C / sec or more. Examples of the cooling method include water cooling in which water is sprayed from a nozzle at a large flow rate. In the present invention, it is preferable to perform the cooling operation (treatment) on both sides of the steel sheet so that both sides of the steel sheet are cooled under the same conditions.

[0079] The average cooling rate between 700 and 550°C at the center of thickness after hot rolling is 2500×t -1.7 If the cooling rate is less than 2500×t / sec, the required strength targeted by the present invention cannot be obtained due to insufficient cooling rate in the temperature range where transformation from austenite to a low-temperature transformation structure occurs. In addition, coarse ferrite is generated, resulting in a decrease in toughness. Therefore, the average cooling rate in the temperature range of 700 to 550°C at the center of the plate thickness is set to 2500×t -1.7 ° C. / sec or more is preferable.

[0080] In the present invention, after the cooling, tempering can be performed as necessary to further improve the strength and toughness. In this case, the steel sheet is tempered at a tempering temperature of 650°C or less after cooling. If the tempering temperature is higher than 650°C, significant softening may occur and the necessary strength may not be ensured. Therefore, it is preferable to set the tempering temperature to 650°C or less. On the other hand, the lower limit of the tempering temperature is not particularly limited, but it is preferable to set it to 200°C or more. The tempering time can be appropriately adjusted. The tempering temperature here refers to the temperature of the steel sheet surface.

[0081] [Chemical composition of weld metal] Next, the chemical composition of the weld metal of the weld joint of the present invention will be described. Note that "%" regarding the chemical composition means "mass %" unless otherwise specified.

[0082] [Basic composition of weld metal] The basic chemical composition of the weld metal of the weld joint according to the present invention is as follows. It is preferable that the weld metal has a chemical composition containing C: 0.04 to 0.14%, Si: 0.03 to 0.70%, Mn: 0.30 to 2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001 to 0.100%, Cu: 0.001 to 2.000%, Ni: 0.001 to 2.500%, Cr: 0.001 to 1.500%, Mo: 0.001 to 1.000%, Ti: 0.001 to 0.100%, V: 0.001 to 0.300%, B: 0.001 to 0.020%, O: 0.050% or less, and N: 0.010% or less, with the balance being Fe and unavoidable impurities.

[0083] The reason why the chemical composition of the weld metal in the present invention is specified as above will now be explained. Each composition can be added (contained) to the weld metal from either the steel plate or the wire, which is the welding material.

[0084] [C: 0.04~0.14%] C is an element that has the effect of increasing the strength of the weld metal by solid solution strengthening, and also contributes to strengthening the austenite grain boundary. If the C content is less than 0.04%, the grain boundary strength of the austenite decreases, and the strength targeted by the present invention may not be obtained. On the other hand, if the C content exceeds 0.14%, the occurrence of weld cracks is promoted, and the low-temperature impact toughness of the weld metal may also decrease. Therefore, the C content is preferably 0.04 to 0.14%. The C content is more preferably 0.05 to 0.12%.

[0085] [Si: 0.03~0.70%] Silicon acts as a deoxidizer and has the effect of increasing the viscosity of the weld metal and stably maintaining the bead shape. To obtain such an effect, the Si content is preferably 0.03% or more. However, if the Si content exceeds 0.70%, there is a possibility that the low-temperature impact toughness of the weld metal may decrease. In addition, silicon segregates during solidification and generates a liquid phase at the solidification cell interface, which may decrease the weld crack resistance. Therefore, the Si content is preferably 0.03 to 0.70%. The Si content is more preferably 0.04 to 0.60%.

[0086] [Mn: 0.30~2.50%] Mn is an element that can improve the hardenability and strength of the weld metal at low cost. To obtain this effect, it is preferable to contain 0.30% or more of Mn. On the other hand, if the Mn content exceeds 2.50%, Mn segregation occurs during solidification, inducing hot cracking, which may result in a decrease in weldability. Therefore, the Mn content is preferably 0.30 to 2.50%. The Mn content is more preferably 0.50 to 2.20%.

[0087] [P:0.030% or less] P is an element that has a large effect of embrittling grain boundaries, and if contained in a large amount, it reduces the low-temperature impact toughness of the weld metal and may segregate at the interface during solidification, inducing hot cracking. Therefore, the P content is preferably 0.030% or less. Furthermore, the P content is more preferably 0.025% or less. On the other hand, since the lower the P content, the more preferable it is, the lower limit of the P content is not particularly limited and may be 0%. However, P is an element that is inevitably contained in the weld metal as an impurity, and excessively reducing the P content leads to an increase in costs, so the P content is preferably 0.001% or more.

[0088] [S:0.020% or less] Since S reduces the low-temperature impact toughness of the weld metal and may segregate at the interface during solidification, inducing hot cracking, the S content is preferably 0.020% or less. Furthermore, the S content is more preferably 0.010% or less. On the other hand, since the lower the S content, the more preferable it is, the lower limit of the S content is not particularly limited and may be 0%. However, S is an element that is inevitably contained in the weld metal as an impurity, and excessively reducing the S content leads to an increase in costs, so the S content is preferably 0.0001% or more.

[0089] [Nb: 0.001~0.100%] Nb is a carbide-forming element, and contributes to improving the strength of the weld metal by precipitating carbides. Nb also contributes to suppressing the occurrence of hot cracks by precipitating carbides at the solidification cell interface of the weld metal. In order to obtain this effect, the Nb content is preferably 0.001% or more. On the other hand, if the Nb content exceeds 0.100%, the carbides are coarsened and become the starting point of fracture, which may lead to a decrease in cryogenic impact toughness. Therefore, the Nb content is preferably 0.001 to 0.100%. The Nb content is more preferably 0.005 to 0.075%. Furthermore, the Nb content is particularly preferably 0.005 to 0.050%.

[0090] [Al: 0.001~0.100%] Al acts as a deoxidizer, increases the viscosity of the molten metal, and has an important effect of stably maintaining the bead shape. In order to obtain this effect, the Al content is preferably 0.001% or more. On the other hand, if the Al content exceeds 0.100%, the cleanliness of the weld metal decreases, and as a result, the ductility and toughness may decrease. Furthermore, if the viscosity of the weld metal becomes too high, the bead may not spread, and defects such as poor fusion may increase. Therefore, the Al content is preferably 0.001 to 0.100%. The Al content is more preferably 0.005 to 0.080%.

[0091] [Cu:0.001~2.000%] Cu is an element that can improve the strength of the weld metal without significantly deteriorating the toughness of the weld metal. To obtain this effect, the Cu content is preferably 0.001% or more. On the other hand, if the Cu content is more than 2.000%, it may segregate during solidification and induce hot cracking. Therefore, when Cu is contained, the Cu content is preferably 2.000% or less. More preferably, the Cu content is 0.005 to 1.500%. The Cu content is still more preferably 0.005 to 1.000%, and further preferably 0.005 to 0.500%.

[0092] [Ni:0.001~2.500%] Ni is an element that has the effect of increasing the hardenability of the weld metal and improving its toughness. In order to obtain this effect, the Ni content is preferably 0.001% or more. However, Ni is an expensive element, and a content of more than 2.500% is economically disadvantageous. Therefore, when Ni is contained, the Ni content is preferably 2.500% or less. More preferably, the Ni content is 0.010 to 2.000%. The Ni content is still more preferably 0.010 to 1.500%, and further preferably 0.010 to 1.000%.

[0093] [Cr:0.001~1.500%] Cr is an element that can improve the hardenability of the weld metal, thereby improving the strength of the weld metal. To obtain this effect, the Cr content is preferably 0.001% or more. On the other hand, if the Cr content exceeds 1.500%, the weldability may decrease. In addition, Cr carbides may be generated, which may lead to a decrease in low-temperature impact toughness. Therefore, when Cr is contained, the Cr content is preferably 1.500% or less. More preferably, the Cr content is 0.010 to 1.200%.

[0094] [Mo:0.001~1.000%] Mo is an element that can improve the hardenability of the weld metal, thereby improving the strength of the weld metal. To obtain this effect, the Mo content is preferably 0.001% or more. On the other hand, if the Mo content exceeds 1.000%, the weldability may decrease. Therefore, when Mo is contained, the Mo content is preferably 1.000% or less. More preferably, the Mo content is 0.010 to 0.800%.

[0095] [Ti: 0.001~0.100%] Ti is an element that can precipitate as fine carbonitrides in the weld metal and improve the strength of the weld metal. To obtain this effect, the Ti content is preferably 0.001% or more. On the other hand, if the Ti content exceeds 0.100%, the cleanliness of the weld metal structure decreases, and as a result, there is a possibility that the ductility and toughness decrease. Therefore, when Ti is contained, the Ti content is preferably 0.100% or less. More preferably, the Ti content is 0.005 to 0.080%.

[0096] [V:0.001~0.300%] V is an element that can improve the hardenability of the weld metal and can improve the strength of the weld metal by forming carbonitrides. To obtain this effect, the V content is preferably 0.001% or more. On the other hand, if the V content exceeds 0.300%, the weldability may decrease. Therefore, when V is contained, the V content is preferably 0.300% or less. The V content is more preferably 0.005 to 0.250%. The V content is still more preferably 0.005 to 0.150%, and further preferably 0.005 to 0.100%.

[0097] [B: 0.001~0.020%] B is an element that has the effect of improving the hardenability by adding a very small amount, thereby improving the strength of the weld metal. In order to obtain this effect, the B content is preferably 0.001% or more. On the other hand, if the B content exceeds 0.020%, the weldability may decrease. Therefore, when B is contained, the B content is preferably 0.020% or less. More preferably, the B content is 0.005 to 0.018%.

[0098] [O:0.050% or less] Since O is an element that reduces ductility and toughness, the O content is preferably 0.050% or less. On the other hand, since the lower the O content, the more preferable it is, the lower limit of the O content is not particularly limited and may be 0%. However, since O is an element that is inevitably contained in the weld metal as an impurity, and excessive reduction in O content leads to an increase in costs, the O content is preferably 0.0005% or more.

[0099] [N:0.010% or less] Since N is an element that reduces ductility and toughness, the N content is preferably 0.010% or less. On the other hand, since the lower the N content, the better, the lower limit of the N content is not particularly limited and may be 0%. However, since N is an element that is inevitably contained in the weld metal as an impurity, excessive reduction in N content leads to an increase in costs, so the N content is preferably 0.0005% or more.

[0100] [Optional composition of weld metal] The weld metal of the present invention can obtain the characteristics targeted by the present invention by using the basic composition described above. However, for the purpose of further improving strength and weldability (specifically, toughness of the welded portion, welding workability, etc.), the weld metal may contain the following optional compositions as necessary in addition to the basic composition described above.

[0101] One or more selected from the group consisting of W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less. W, Ca, Mg, and REM are compositions that can be contained arbitrarily, so the contents of these elements may be 0%.

[0102] [W:0.500% or less] W is an element that can improve the hardenability of the weld metal, thereby improving the strength of the weld metal. On the other hand, if the W content exceeds 0.500%, the weldability may decrease. Therefore, when W is contained, the W content is preferably 0.500% or less. The W content is preferably 0.001% or more. More preferably, the W content is 0.001 to 0.300%.

[0103] [Ca:0.0200% or less] Ca is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the Ca content exceeds 0.0200%, the cleanliness decreases and the toughness of the weld metal may be impaired. Therefore, when Ca is contained, the Ca content is preferably 0.0200% or less. More preferably, the Ca content is 0.0001 to 0.0150%. Even more preferably, the Ca content is 0.0001 to 0.0100%.

[0104] [Mg:0.0200% or less] Mg is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the Mg content exceeds 0.0200%, the effect of adding Mg becomes saturated and an effect commensurate with the content cannot be expected, which may be economically disadvantageous. Therefore, when Mg is contained, the Mg content is preferably 0.0200% or less. More preferably, the Mg content is 0.0001 to 0.0180%. Even more preferably, the Mg content is 0.0001 to 0.0150%.

[0105] [REM:0.0500% or less] REM (rare earth metal) is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the REM content exceeds 0.0500%, the effect of adding REM becomes saturated and an effect commensurate with the content cannot be expected, which may be economically disadvantageous. Therefore, when REM is contained, the REM content is preferably 0.0500% or less. More preferably, the REM content is 0.0001 to 0.0450%.

[0106] [Remainder of weld metal composition] The remainder of the weld metal of the present invention, other than the above chemical composition, is Fe and inevitable impurities. Incidentally, inevitable impurities refer to components that are mixed in from the welding wire, steel sheet, surrounding atmosphere, etc. during the welding process and are not intentionally included. Examples of inevitable impurities include H, Zn, Re, Co, Sb, Bi, etc., and a total of 0.0100% or less is acceptable. In addition, elements other than these may be contained as long as the above basic composition and optional composition are satisfied, and such embodiments are also included in the technical scope of the present invention.

[0107] [Mechanical properties of weld metal] Here, preferred mechanical properties of the welded joint according to the present invention will be described. It is preferable that the weld metal having the above-mentioned chemical composition and produced in accordance with the regulations of JIS Z 3111 has a room temperature yield strength (0.2% proof stress) of 325 MPa or more and a tensile strength of 520 MPa or more in a tensile test.

[0108] The welded joint preferably has a tensile strength of 520 MPa or more at room temperature. In the present invention, "room temperature" refers to 25.0°C.

[0109] In addition, the absorbed energy (vE -40 ) is preferably 30 J or more. If it is less than 30 J, the toughness of the structure including the joint may be reduced and fracture may occur more easily.

[0110] [Manufacturing method for welded joints] Next, a method for manufacturing a welded joint according to the present invention will be described, that is, a method for manufacturing a welded joint formed by gas-shielded arc welding the above-mentioned steel plates will be described.

[0111] First, prepare a steel plate having the above-mentioned chemical composition and a thickness of 50 to 160 mm. Then, perform groove processing so that the prepared steel plates form a predetermined groove shape. The groove shape to be formed does not need to be particularly limited, and examples of the groove shape that can be used for welded structures include normal V grooves, L grooves, X grooves, and K grooves.

[0112] Next, the above-mentioned groove-processed steel plates are welded together to form a multi-layer weld metal of three or more layers, resulting in a welded joint. If welding is performed with one or two layers of weld metal, the heat during welding does not spread uniformly within the groove, inducing welding defects. The number of passes per layer is not particularly limited, and may be two or more passes, not limited to one pass. However, since the welding efficiency is significantly reduced if the number of passes exceeds four, four passes or less is preferable. Furthermore, from the viewpoint of welding efficiency, two passes or less is more preferable.

[0113] [Gas shielded arc welding method] The welding method used in the present invention is a multi-electrode gas-shielded arc welding method that can stably obtain narrow gap welded joints that have weld metal free of welding defects and have high strength and excellent low-temperature impact toughness.

[0114] As the welding conditions for the gas-shielded arc welding method of the present invention, it is necessary to properly control the welding conditions described below with reference to the drawings.

[0115] [Welding conditions (basic conditions and optional conditions)] (1) Basic welding conditions (a) Multi-layer welding is performed using three or more electrodes. (b) The tips of the welding wires of the first electrode and the second electrode are arranged on different parallel welding lines (see FIG. 4). (c) One of the first electrode and the second electrode is set as a wire negative (positive polarity), and the other is set as a wire positive (reverse polarity). (d) The distance a (mm) between the tips of the welding wires of the first electrode and the second electrode is 5 to 16 mm (see FIG. 4). (e) The angle α of the straight line connecting the tips of the welding wires of the first electrode and the second electrode with respect to the perpendicular direction to the welding line is 60° or less (see FIG. 4). (f) A welding wire containing 0.015 to 0.100 mass % of REM is used for the electrode serving as the negative wire (positive polarity). (2) Optional welding conditions (g) The inclination angle Φ of the tip of each of the first and second electrodes toward the groove surface with respect to the perpendicular direction of the weld line is 0° to 15° (see FIG. 3). (h) The distance d (mm) between the side end of the tip of the welding wire of each of the first electrode and the second electrode and the groove surface is 0.5 to 3.0 mm (see Figs. 2 and 3). (i) Each welding wire is curved in advance to have a radius of curvature in the range of 150 to 300 mm. (j) The third and subsequent electrodes are placed in the center of the groove behind the first and second electrodes (see Figures 4 and 5). (k) A gas containing 60% or more of CO2 gas by volume is used as a shielding gas.

[0116] [Individual welding conditions] The above welding conditions will be explained in more detail below.

[0117] (a) Multi-layer welding with three or more electrodes In narrow-gap multi-pass welding, when one pass is performed per layer, heat tends to concentrate at the center of the groove with one electrode, resulting in insufficient melting of the steel material at the groove surface, and defects due to poor fusion (cold lap) and spatter and slag entrapment on the groove surface are likely to occur. In particular, the temperature of the steel material is low in the first layer welding, and the melting depth is small, so defects due to poor fusion are likely to occur. In addition, from the viewpoint of improving welding efficiency, it is advantageous to use multi-electrode welding with three or more electrodes. Note that, from the viewpoint of welding efficiency, four or less electrodes are preferable. Three electrodes are most preferable.

[0118] (b) Electrode placement The welding wire tips of the first electrode and the second electrode are arranged on different parallel welding lines. Fig. 4 shows an example of the arrangement of the welding wire tips in the case of three electrodes, and Fig. 5 shows an example of the arrangement of the welding wire tips in the case of four electrodes. As shown in these figures, the welding wire tip 5c of the first electrode 5 and the welding wire tip 6c of the second electrode 6 are arranged on different parallel welding lines 9. In this way, the arcs emitted from the welding wires of the first electrode and the second electrode spread in the width direction of the weld metal being formed.

[0119] (c) Electrode polarity One of the first electrode and the second electrode is wire negative (positive polarity), and the other is wire positive (negative polarity). If the first electrode and the second electrode are of the same polarity, for example, if both the first electrode and the second electrode are wire positive, the arcs of each electrode will be inward due to the electromagnetic force of attraction, and heat will be concentrated in the center of the groove, and sufficient melting will not be obtained on the groove surface. However, if the first electrode and the second electrode are of different polarities and the tips of the welding wires described in (b) above are arranged on different parallel welding lines, the magnetic fields due to the welding currents of each electrode will generate strong outward electromagnetic forces, and the arcs will repel each other. As a result, it is possible to obtain a sufficient melting depth on the groove surface. From this result, in the present invention, the polarities of the first electrode and the second electrode are one of wire negative (positive polarity) and the other of wire positive (negative polarity).

[0120] (d) Distance between 1st and 2nd electrode tips a: 5~16mm Distance a between the tips of welding wires 5b and 6b supplied from power feed tips 5a and 6a at the tips of the welding torches of first electrode 5 and second electrode 6 (hereinafter simply referred to as "first-second electrode tip distance") needs to be controlled within the range of 5 to 16 mm. Note that distance a between the tips of welding wires 5b and 6b here refers to the distance between the centers of welding wire tips 5c and 6c of each electrode, as shown in FIG. 4.

[0121] If the distance a between the first and second electrode tips is less than 5 mm, the current (electrons) flowing between the electrodes reduces the heat of the arc itself, and sufficient melting of the groove surface is not achieved. On the other hand, if the distance a exceeds 16 mm, the outward electromagnetic force between the electrodes decreases inversely proportional to the distance, and the arc repulsive force sufficient to overcome the inward electromagnetic force generated by the current flowing through the groove surface is not obtained, so the arcs face inward and heat is concentrated in the center of the groove. As a result, sufficient melting of the groove surface is not achieved.

[0122] Furthermore, in narrow gap welding, suppressing welding defects caused by spatter adhesion to the groove surface is an issue, but by controlling the above-mentioned welding conditions (b), (c), and (d), the spatter is absorbed into the molten metal. This suppresses the adhesion of spatter to the groove surface, making it possible to obtain a sound weld.

[0123] From the above, the distance a between the first and second electrode tips is controlled to be in the range of 5 to 16 mm. However, in order to obtain a deeper and more stable melting depth at the groove face by stronger arc repulsion, it is preferable to control the distance a between the first and second electrode tips to be in the range of 5 to 8 mm.

[0124] (e) 1st-2nd electrode tip arrangement angle α: 60° or less In the narrow gap gas shielded arc welding method of the present invention, the melting of the groove surface is ensured by utilizing the repulsion of the arc. Here, in FIG. 4, the angle α of the straight line connecting the welding wire tips 5c and 6c of the first electrode 5 and the second electrode 6 with respect to the perpendicular direction of the welding line 9 (hereinafter, also simply referred to as the "first-second electrode tip arrangement angle") will be described. If this angle α exceeds 60°, a sufficient repulsive force of the arc cannot be obtained, and sufficient melting cannot be obtained at the groove surface. Therefore, the angle α is limited to 60° or less. Preferably, the angle α is 45° or less. The angle α may be 0° (i.e., parallel to the perpendicular direction of the welding line). More preferably, the angle α is 25° or more.

[0125] (f) REM content of the welding wire used for the positive electrode REM (rare earth elements) are effective elements for refining inclusions during steelmaking and casting, and for improving the toughness of weld metal during welding. Furthermore, when welding is performed by supplying a welding wire containing REM to an electrode with a negative (positive) polarity, it is possible to refine droplets and stabilize transfer. This refinement of droplet transfer suppresses the generation of spatters, and enables stable gas shielded arc welding even with a positive polarity. For this reason, in the present invention, a steel wire containing 0.015 to 0.100 mass% of REM (rare earth elements) is supplied to an electrode with a positive polarity. Note that elements other than REM (rare earth elements) are intended to contain appropriate amounts that are normally contained according to the grade (steel type) of the welding wire, as specified in JIS Z 3312. If the content of REM (rare earth elements) is less than 0.015 mass%, the above-mentioned refinement of droplets and stabilization of transfer cannot be achieved. On the other hand, if the REM content exceeds 0.100 mass%, cracks will occur during the wire manufacturing process, making it difficult to manufacture the welding wire. For this reason, the REM (rare earth element) content is limited to the range of 0.015 to 0.100 mass%. The REM content is preferably 0.025 to 0.050 mass%.

[0126] In addition, welding wire for gas shielded arc welding is generally manufactured in a diameter range of 0.6 to 2.0 mm, but when welding with the same current, generally, the thinner the wire diameter, the higher the deposition rate due to Joule heat. Therefore, in order to realize highly efficient welding work, it is preferable to select a relatively thin wire diameter. On the other hand, if the wire diameter is too thin, the wire will soften due to Joule heat, making the welding unstable. Therefore, it is preferable that the diameter of the welding wire used is in the range of 1.0 to 1.6 mm.

[0127] The above welding conditions are the basic welding conditions for gas-shielded arc welding of the present invention, and by performing welding under the above-mentioned conditions, it is possible to produce a narrow gap welded joint that is free of welding defects, has high strength, and has excellent low-temperature impact toughness.

[0128] Furthermore, in the present invention, by satisfying the optional welding conditions described below in addition to the basic welding conditions described above, it becomes possible to more stably obtain narrow gap welded joints that are free of welding defects, have high strength, and have excellent low-temperature impact toughness.

[0129] (g) Tilt angle of power supply tip Φ: 0°~15° The arc has a directivity and tends to point in the direction in which the tip of the welding wire of the electrode points. In order to effectively utilize the directivity of the arc in melting the groove surface, it is advantageous to point the direction of the welding wire tip toward the groove surface, and the direction in which the tip of the welding wire points varies greatly depending on the feed angle of the welding wire supplied from the power feed tip at the tip of the electrode. As shown in FIG. 3, the feed angle of the welding wires 5b and 6b of the first electrode 5 and the second electrode 6 with respect to the bottom of the weld metal 2 is the same as the inclination of the tips of the power feed tips 5a and 6a of the electrodes. Therefore, by adjusting the inclination angle Φ of the tip of the power feed tip toward the groove surface 4 (hereinafter also referred to as the "inclination angle Φ of the power feed tip"), the feed angle of the welding wire supplied from each power feed tip with respect to the bottom of the weld metal can be controlled. Here, the bottom of the weld metal refers to the bottom of each weld layer of the weld metal, and refers to the vicinity of the boundary with the previous weld layer.

[0130] When the inclination angle Φ of the power feed tips of the first and second electrodes is less than 0° (i.e., when the inclination angle Φ is inclined away from the groove surface), the current flows through a path with less resistance. As a result, the arc creeps up the wire electrode (this is called "arc creeping"), making it difficult to maintain the melting at the target groove surface, especially the bottom. On the other hand, when the inclination angle Φ of the power feed tip exceeds 15°, the arc faces too far toward the groove surface, resulting in a convex weld bead shape, and melting by the arc in the first layer and subsequent layers becomes insufficient, making it easy for welding defects to occur. For this reason, the inclination angle Φ of the power feed tip is preferably set in the range of 0° to 15°. More preferably, the inclination angle Φ of the power feed tip is 5° to 12°.

[0131] (h) Distance d between the tip of the welding wire and the groove surface: 0.5 to 3.0 mm In order to obtain a deeper and more stable fusion depth at the bottom of the weld metal, it is preferable that the distance d between the side ends of the welding wire tips 5c and 6c of the first electrode 5 and the second electrode 6 and the groove surface 4 of the steel plate is 0.5 to 3.0 mm, as shown in Figures 2 and 3. If the distance d is less than 0.5 mm, the arc will be generated not between the wire and the bottom of the weld metal but between the wire and the groove surface, and the previous weld layer and the groove surface will not be efficiently fused at the bottom of the weld metal.

[0132] On the other hand, if the distance d exceeds 3.0 mm, the arc will be away from the groove surface, and the groove surface will not be melted efficiently. More preferably, the distance d is in the range of 0.5 to 2.0 mm, and even more preferably, in the range of 0.5 to 1.0 mm. Note that the "side end of the tip of the welding wire" referred to here refers to the side end closest to the groove surface of the steel sheet to be melted by each electrode, and the distance d refers to the shortest distance between the side end and the groove surface 4.

[0133] (i) Curvature radius of the welding wire to be fed: 150 to 300 mm In the present invention, in order to control the feed angle (Φ) of the welding wires 5b, 6b supplied from the power feed tips at the tips of the welding torches of the first electrode 5 and the second electrode 6, power feed tips 5a, 6a with their tips inclined toward the groove surface are used as shown in Fig. 3. At this time, the welding wires 5b, 6b pass through the power feed tips with their tips inclined toward the groove surface, and in order to pass through them more smoothly, it is preferable to curve the supplied welding wire in advance using a so-called three-point roller or the like (not shown).

[0134] The radius of curvature when bending in advance is preferably 150 to 300 mm. If the radius of curvature is less than 150 mm, the wire feed resistance increases, the welding wire cannot be stably fed, and it becomes difficult to maintain an arc. On the other hand, if the radius of curvature of the welding wire exceeds 300 mm, there is no effect in reducing the wire feed resistance when the tip of the power feed tip is bent, so the welding wire cannot be stably fed, and it becomes difficult to maintain an arc. Therefore, the radius of curvature of the welding wire fed to the power feed tips of the first electrode and the second electrode is preferably 150 to 300 mm. More preferably, the radius of curvature of the welding wire is 175 to 275 mm.

[0135] (j) Arrangement of the third and subsequent electrodes To avoid the risk of hot cracking, it is effective to position the welding wire tips (7c and 8c) of the third and subsequent electrodes in the center of the groove behind the welding wire tips (5c and 6c) of the first and second electrodes, as shown in Figures 4 and 5. This also makes it possible to further reduce the number of layers, greatly reducing the risk of stacking defects in multi-layer welding.

[0136] The distance b between the welding wire tip 6c of the second electrode and the welding wire tip 7c of the third electrode is preferably in the range of 10 to 100 mm, more preferably 10 to 60 mm, even more preferably 10 to 40 mm, and most preferably 10 to 25 mm. Furthermore, the distance c between the welding wire tip 7c of the third electrode and the welding wire tip 8c of the fourth electrode is also preferably in the range of 10 to 100 mm, more preferably 10 to 60 mm, even more preferably 10 to 40 mm, and most preferably 10 to 25 mm.

[0137] Furthermore, the polarity of the third electrode and thereafter is not particularly limited, and may be either wire negative (positive polarity) or wire positive (negative polarity).

[0138] (k) Shielding gas composition Since the oxygen content in the weld metal is also greatly affected by the shielding gas composition, it is preferable to use a gas containing 60 volume % or more of CO2 gas and the remainder as an inert gas such as Ar as the shielding gas composition, and more preferably a gas containing 100 volume % CO2 gas.

[0139] The nozzles for supplying the shielding gas are preferably arranged as follows.

[0140] In order to ensure good shielding in gas-shielded arc welding, which is the object of the present invention, suppress the inclusion of nitrogen from the atmosphere, and reduce the deterioration of the low-temperature toughness of the weld metal and the occurrence of welding defects, a shielding gas supply nozzle 11 is positioned in front of the welding direction of the first electrode 5 in the groove.

[0141] A detailed description will be given based on Figs. 7 and 8. Fig. 7 is a side cross-sectional view showing a schematic arrangement of the shielding gas supply nozzle and the electrodes, and Fig. 8 is a plan view showing the same arrangement as Fig. 7 from above. These figures show an example of three-electrode welding in which a first electrode 5, a second electrode 6, and a third electrode 7 are arranged. A shielding gas supply nozzle 11 is arranged in front of the first electrode 5 in the welding direction, and a gas discharge port 11a from which the shielding gas is discharged is directed toward the first electrode 5. During welding, the shielding gas supply nozzle 11 moves in conjunction with the three electrodes along the welding direction, and arc welding is performed while supplying the shielding gas.

[0142] The cross-sectional area N of the gas discharge port 11a is 100 mm 2 ~350mm 2 It is preferable that the range is 100%.

[0143] The cross-sectional area N of the gas discharge port 11a is 100 mm 2 If the cross-sectional area N of the gas discharge port 11a is less than 350 mm, the area onto which the gas is blown becomes small, and the shielding performance becomes insufficient. 2 If the cross-sectional area exceeds 100 mm, the gas will disperse to areas other than the bottom of the groove, resulting in insufficient shielding. 2 ~350mm2 More preferably, the cross-sectional area N is 125 mm 2 ~300mm 2 It is.

[0144] Moreover, the supply flow rate Q of the shielding gas is preferably in the range of 35 L / min to 70 L / min.

[0145] If the supply flow rate Q of the shielding gas is less than 35 L / min, the amount of gas supplied to the molten pool 12 becomes insufficient, and the shielding performance deteriorates. On the other hand, if the supply flow rate Q of the shielding gas exceeds 70 L / min, the flow rate of the shielding gas becomes excessive, and the possibility of occurrence of welding defects increases. Therefore, the supply flow rate Q of the shielding gas is preferably 35 L / min to 70 L / min. This supply flow rate Q is more preferably 40 L / min to 65 L / min. Note that the flow rate of the shielding gas changes depending on the combination of the supply flow rate Q of the shielding gas and the cross-sectional area N of the gas outlet, but the flow rate is preferably 2 m / s to 7 m / s.

[0146] The preferred cross-sectional shape of the tip of the gas discharge port is as follows.

[0147] 7 and 8 show only the tip portion of the shielding gas supply nozzle 11, but the cross-sectional shape of the tip portion of the gas discharge port 11a is not particularly limited. However, since a nozzle with a larger cross-sectional area can be inserted into the groove when the cross-sectional shape of the tip portion is rectangular rather than circular, it is preferable that the cross-sectional shape of the tip portion of the gas discharge port be rectangular.

[0148] The angle X between the cross section of the gas discharge port 11a and the bottom of the groove to be welded is preferably 40° to 80° (see FIG. 7).

[0149] If the angle X between the cross section of the gas discharge port 11a and the bottom of the groove to be welded is less than 40°, the shielding gas does not reach the third electrode 7 sufficiently, resulting in insufficient shielding. On the other hand, if the angle X exceeds 80°, the gas is dispersed to areas other than the bottom of the groove, resulting in insufficient shielding. Therefore, the angle X between the cross section of the gas discharge port 11a and the bottom of the groove to be welded is preferably 40° to 80°. This angle X is more preferably 45° to 75°.

[0150] Furthermore, the distance Y between the tip of the gas discharge port 11a and the welding wire tip 5c of the first electrode 5 is preferably 40 mm or less (see Figs. 7 and 8). The distance between the gas discharge port 11a and the electrodes is also effective for shielding. That is, if the distance Y between the tip of the gas discharge port 11a (specifically, the part closest to the electrode) and the welding wire tip 5c of the first electrode 5 exceeds 40 mm, the shielding gas does not reach the entire electrode sufficiently, and the gas is dispersed to areas other than the bottom of the groove, resulting in insufficient shielding. Therefore, the distance Y is preferably 40 mm or less. The distance Y is more preferably 5 mm to 35 mm.

[0151] [Other welding conditions] The welding conditions other than those mentioned above are not particularly specified, but may be, for example, a welding current of 280 to 360 A, a welding voltage of 32 to 37 V, a welding speed of 30 to 90 (cm / min), a wire extension length of 15 to 30 (mm), and a welding heat input per pass of 10 to 50 (kJ / cm).

[0152] In addition, when multi-layer welding is performed using three electrodes, the following welding current conditions are more suitable. First, the current value I1 of the first electrode and the current value I2 of the second electrode are set to a range of 280A to 360A. If the current values ​​I1 and I2 of the first and second electrodes are less than 280A, the groove face cannot be melted sufficiently, and there is a high possibility of incomplete fusion. On the other hand, if the current values ​​I1 and I2 exceed 360A, the height of the weld bead increases and the bead becomes elongated, increasing the risk of hot cracking. Therefore, the range of the current value I1 of the first electrode and the current value I2 of the second electrode is preferably 280A to 360A, and more preferably 280A to 340A.

[0153] Next, the current value I3 of the third electrode is controlled for each layer of the multi-layer welding based on the relationship with the width of the weld bead of each layer, thereby suppressing hot cracks that occur in each weld layer, which is the object of the present invention. i is set to a range that satisfies the following formula (2). I3 i ≦30×G i-1 -10 ···(2) Here, I3 i : Current value of the third electrode of the i-th layer [A], G i-1 is the width [mm] of the weld bead formed by welding the layer before the i-th layer (i.e. the i-1th layer), and i is a natural number greater than or equal to 2.

[0154] Current value I3 of the third electrode i When the weld bead width G becomes larger, the height of the weld bead becomes larger and the bead becomes longer, which increases the risk of hot cracking. i is the width G of the weld bead formed by welding one layer before (i.e., the i-1th layer) i-1 As the number of layers increases, the width of the weld bead also increases due to the influence of the current value of the third electrode. Based on this, the relationship between the width of the weld bead and the current value of the third electrode was examined, and a favorable range was found, from which the above formula (2) was derived. In other words, if the range satisfies formula (2), the formation of a vertically elongated weld bead is suppressed, and the excellent effect of preventing hot cracks can be obtained. EXAMPLES

[0155] The present invention will be further described below with reference to examples. However, the following examples are merely intended to illustrate and explain the present invention in more detail, and are not intended to limit the scope of the present invention.

[0156] First, molten steel having the chemical composition shown in Table 1 was produced, and steel material (slab) was manufactured by continuous casting or the like. This composition in Table 1 becomes the chemical composition of the steel plate that will become the base material. Note that the "-" column in Table 1 indicates that the element is not intentionally added, and includes not only cases where the element is not contained (0%), but also cases where the element is unavoidably contained.

[0157] [Table 1]

[0158] Next, the obtained slab was subjected to the steps of heating, hot rolling, and cooling in order to obtain steel plates having thicknesses T (mm) shown in Tables 2-1 and 2-2. The rolling start temperature in the hot rolling step was in the range of 990 to 1140°C at the surface layer of the steel plate, and the rolling finish temperature was in the range of 670 to 830°C at the surface layer of the steel plate. The above steel plate temperatures were measured by an emissivity thermometer for the surface layer temperature and by attaching a thermocouple to the center of the thickness of the steel plate. Cooling after hot rolling was performed by spraying water at a large flow rate from the front and back sides of the steel plate.

[0159] On the other hand, molten steel was melted in a vacuum melting furnace and cast to obtain a steel ingot, which was heated to 1200°C and then hot and cold worked to produce a 1.2 mmΦ gas shielded arc welding wire. In addition to YGW18, G 59J A 1 was used as the wire steel type (grade).

[0160] Next, the above steel plate was subjected to groove processing to obtain the groove shapes shown in Tables 2-1 and 2-2. Note that the groove shapes V (groove) in Tables 2-1 and 2-2 are the shapes shown in Fig. 6(a), and X (groove) are the shapes shown in Fig. 6(b). Furthermore, gas-shielded arc welding was performed using the welding wire obtained above to form a weld metal in the above-mentioned groove, and a welded joint was obtained.

[0161] [Table 2-1]

[0162] [Table 2-2]

[0163] The specific welding conditions for the gas shielded arc welding were as follows: no preheating, downward welding, welding current: 180-390 A, welding voltage: 22-38 V, welding speed: 40-120 cm / min, interpass temperature: 200° C. or less. The weld metal was three or more layers.

[0164] Tables 3-1 to 3-4 show the welding conditions for each electrode in gas shielded arc welding. The welding electrodes were arranged as shown in Figures 4 and 5. Here, the distance b between the welding wire tips of the second and third electrodes was 18 mm, and the distance c between the welding wire tips of the third and fourth electrodes was 10 mm. In the "Polarity" column of Tables 3-1 and 3-3, "Positive polarity" is written for negative wire, and "Reverse polarity" is written for positive wire.

[0165] [Table 3-1]

[0166] [Table 3-2]

[0167] [Table 3-3]

[0168] [Table 3-4]

[0169] [Evaluation of weld metal shape] Vertical cross-sectional macros were taken and observed at positions 1 / 4D, 2 / 4D, and 3 / 4D in the weld line direction of the welded joint. Here, D above refers to the length from one end of the weld line to the other end. The 1 / 4D position represents a position 1 / 4 of D moved in the welding direction from one end of the weld line, and similarly, the 2 / 4D position is the center position of the weld line, and the 3 / 4D position represents a position 3 / 4 of D moved in the welding direction.

[0170] Then, for each layer of weld metal except for the first and last layers, the width of the weld metal (the distance between the fusion lines) at the center line between the top and bottom was measured to determine the width W (mm) of each layer, and the minimum and maximum values ​​of the width W for the entire weld metal were recorded.

[0171] In addition, the cross-sectional area A (mm 2 ) was measured and the ratio [A / p] obtained by dividing it by the number of weld layers p (layers) was recorded. Similarly, the ratio [p / T] of the number of weld layers p to the steel plate thickness T was recorded.

[0172] [Measurement of dislocation density in steel sheets] Samples were taken from each steel plate at the center in the longitudinal and transverse directions, 1 mm below the surface of the steel plate, to be the evaluation surface. The surfaces of the samples were mirror-polished by mechanical polishing and electrolytic polishing, and the dislocation density ρ(m -2 ) was evaluated. (Reference 1) GKWilliams and WHHall:Acta Metall.,1(1953),22

[0173] [Average grain size] Similarly to the above, samples were taken so that the evaluation surfaces were 1 mm below the surface of the steel plate at the center of the longitudinal and width directions of each steel plate and the longitudinal cross section of the steel plate at the center of the plate thickness. The surfaces of the obtained samples were mirror-polished with a colloidal silica finish and measured by EBSP (electron backscatter diffraction) under the following conditions. The measurement area was 300 μm × 400 μm, and the measurement step size was 1 μm. From the obtained crystal orientation map, the circle equivalent diameter of the structure surrounded by high-angle grain boundaries where the crystal orientation difference with adjacent crystal grains was 15° or more was obtained, and the average value of the circle equivalent diameter in the measurement area was taken as the average crystal grain size. Note that the steel plate surface layer and the plate thickness center of the present invention had a structure mainly composed of bainite and pseudo-polygonal ferrite.

[0174] [Evaluation of welding defects] In addition, radiographic testing was performed on the obtained welded joints in accordance with JIS Z 3104 to evaluate the presence or absence of weld defects. Weld defects were judged as falling under JIS Z3104 Class 1 with a "○", Class 2 with a "△", and Class 3 or 4 with an "×". Class 1 or 2 was deemed to be pass, and Class 3 or 4 was deemed to be fail.

[0175] [Evaluation of mechanical properties of weld metal] From the welded joints thus obtained, tensile test pieces (parallel diameter 6 mm) and Charpy impact test pieces (V notch) were taken from the welded metal and tensile tests and impact tests were carried out in accordance with the provisions of JIS Z 3111. Tensile tests were carried out on three pieces each at room temperature (normal temperature), and the average values ​​obtained (0.2% proof stress, tensile strength) were regarded as the tensile properties of the welded metal of the welded joint. Charpy impact tests were also carried out on three pieces each in the same way, and the absorbed energy (vE -40 ) was obtained, and the average value was regarded as the cryogenic impact toughness of the weld metal of the welded joint. A value of 30 J or more was evaluated as "○", and a value less than this was evaluated as "×".

[0176] In addition, tensile tests were also conducted on the welded joints at room temperature in accordance with the provisions of JIS Z 3121. The test specimens were taken perpendicular to the weld axis so that the weld axis was in the center of the parallel length of the test specimen, and the thickness was the full thickness of the welded joint, which was a No. 1A test specimen. Yield stress values ​​of 325 MPa or more were evaluated as "○", and values ​​less than this were evaluated as "×". Tensile strength values ​​of 520 MPa or more were evaluated as "○", and values ​​less than this were evaluated as "×".

[0177] Furthermore, Charpy impact tests were also conducted on the heat-affected zones of the welded joints in accordance with the provisions of JIS Z 3128. The V-notch direction of the test specimens was perpendicular to the steel plate surface, and the test specimens were taken from the center of the plate thickness, the center of the weld metal, on the fusion line, and 1 mm from the fusion line. Values ​​of 30 J or more were evaluated as "○", and values ​​less than this were evaluated as "×".

[0178] As described above, the target values ​​in the present invention are a room temperature yield strength (0.2% proof stress) of the weld metal of 325 MPa or more, a tensile strength of the weld metal of 520 MPa or more, and a room temperature tensile strength of the welded joint of 520 MPa or more. Furthermore, the absorbed energy (vE -40 ) is 30J or more.

[0179] [Welding efficiency] The wire diameter (mm) used during welding and the wire feed speed (mm / min) during welding were measured, and the deposition amount (g) divided by the unit welding time (min) was recorded as the deposition efficiency (g / min). If this value was 250g / min or more, it was evaluated as "○", and if it was less than that, it was evaluated as "×".

[0180] Of the above measurement and evaluation results, the results of the chemical composition of the weld metal are shown in Tables 4-1 and 4-2, and the results of the properties of the weld metal and steel plate, the performance of the welded joints, etc. are shown in Tables 5-1 and 5-2.

[0181] [Table 4-1]

[0182] [Table 4-2]

[0183] [Table 5-1]

[0184] [Table 5-2]

[0185] All of the examples of the present invention have sound welded joints with no welding defects such as hot cracks or incomplete fusion. Furthermore, all of the examples of the present invention have a room temperature yield strength (0.2% proof stress) of the weld metal of 325 MPa or more, a tensile strength of 520 MPa or more, and a room temperature tensile strength of the welded joint of 520 MPa or more. In addition, the absorbed energy (vE -40 ) is 30 J or more, and the weld metal has both high strength and excellent low-temperature impact toughness.

[0186] On the other hand, in the examples that are outside the preferred range of the steel plate and welded weld metal of the present invention, hot cracking occurs, lowering hot cracking resistance, or insufficient fusion occurs. In addition, the room temperature yield strength (0.2% proof stress) and tensile strength of the weld metal, the room temperature tensile strength of the welded joint, and the absorbed energy (vE -40 ) and other mechanical properties were at slightly lower levels. [Explanation of symbols]

[0187] 1 steel plate 2. Weld metal 3. Welding Line 4 Bevel surface 5 1st electrode 6 Second electrode 7 Third electrode 8 4th electrode 5a, 6a, 7a, 8a: Power supply chips for the first electrode, the second electrode, the third electrode, and the fourth electrode 5b, 6b, 7b, 8b Welding wires for the first electrode, second electrode, third electrode, and fourth electrode 5c, 6c, 7c, 8c Welding wire tips of the first electrode, second electrode, third electrode, and fourth electrode 9 Welding Lines 10 Backing material 11 Shielding gas supply nozzle 11a Gas outlet 12 Molten pool T plate thickness A Cross-sectional area of ​​the entire weld metal L i Welding layer (i=1~p layer), (L1: first layer, L P : outermost layer) W i Width of weld layer (i=1 to p layers) a) Distance between tip 5c of the welding wire of the first electrode and tip 6c of the welding wire of the second electrode b Distance between tip 6c of the welding wire of the second electrode and tip 7c of the welding wire of the third electrode c) Distance between tip 7c of the welding wire of the third electrode and tip 8c of the welding wire of the fourth electrode d Distance between the tip end 5c or 6c of the welding wire and the groove surface 4 α The angle of the straight line connecting the tips of the welding wires of the first and second electrodes with respect to the perpendicular direction of the welding line θ Bevel angle, θ f Surface bevel angle, θ b Back bevel angle Φ Tilt angle of the tip of the power supply tip G Gap T f Surface thickness, T m Intermediate thickness, T b Back Thickness

Claims

1. In a method for manufacturing a welded joint by gas shielded arc welding of steel plates, The thickness T (mm) of the steel plate is 50 to 160 mm, The weld metal consists of three or more layers, The width W (mm) of each layer excluding the first layer and the outermost layer of the weld metal is 5.0 or more and 0.4T or less (mm), The cross-sectional area A (mm 2 The ratio [A / p] of the number of weld layers p (layers) to the number of layers p (layers) is 120.0 mm 2 Below / layer, The ratio [p / T] of the number of weld layers p to the plate thickness T is 0.40 layers / mm or less, The gas shielded arc welding is a multi-electrode welding having three or more electrodes, The tips of the welding wires of the first electrode and the second electrode are disposed on different parallel welding lines; One of the first electrode and the second electrode is a wire negative (positive polarity), and the other is a wire positive (reverse polarity), The distance a (mm) between the welding wire tips of the first electrode and the second electrode is 5 to 16 mm, an angle α of a straight line connecting the welding wire tips of the first electrode and the second electrode with respect to a perpendicular direction to the welding line is 60° or less; A welding wire containing 0.015 to 0.100 mass % of REM is used for the electrode that is the negative wire (positive polarity). A method for manufacturing welded joints by gas-shielded arc welding of steel plates.

2. The inclination angle Φ of the tip of each of the first electrode and the second electrode toward the groove surface side with respect to the perpendicular direction of the weld line is 0° to 15°, A distance d (mm) between a side end portion of each welding wire tip of the first electrode and the second electrode and the groove surface is 0.5 to 3.0 mm, Each of the welding wires is a welding wire that is bent in advance to have a radius of curvature in the range of 150 to 300 mm, A third electrode and subsequent electrodes are disposed at the center of the groove behind the first electrode and the second electrode, Shielding gas containing 60% or more by volume of CO 2 Using gas containing gas, A method for producing a welded joint by gas shielded arc welding of the steel plate according to claim 1.

3. The chemical composition of the steel sheet is, in mass%, C: 0.04-0.14%, Si: 0.03-0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001-0.100%, O: 0.0100% or less, and N: 0.0100% or less; The balance is Fe and unavoidable impurities, Ceq and plate thickness (T) defined by the following formula (1) 0.0004T+0.25≦Ceq≦0.0004T+0.45 The composition satisfies the following: The dislocation density ρ at a position 1 mm below the surface of the steel plate is 4.0 × 10 14 m -2 is as follows: The average crystal grain size at a position 1 mm below the surface of the steel plate is 15.0 μm or less, and the average crystal grain size at the center of the plate thickness is 20.0 μm or less; A method for producing a welded joint by gas-shielded arc welding of the steel plate according to claim 1 or 2. Ceq=[C]+[Mn] / 6+([Cr]+[Mo]+[V]) / 5+([Cu]+[Ni]) / 15...(1) However, each element symbol in the above formula (1) represents the content (mass%) of the corresponding element, and if the corresponding element is not contained, it is set to 0.

4. The chemical composition of the steel sheet further comprises, in mass%, Cu: 2.000% or less, Ni: 2.500% or less, Cr: 1.500% or less, Mo: 1.000% or less, Ti: 0.100% or less, V: 0.300% or less, B: 0.0100% or less, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less The method for producing a welded joint by gas-shielded arc welding of steel plates according to claim 3, comprising one or more selected from the group consisting of:

5. The chemical composition of the weld metal is, in mass%, C: 0.04-0.14%, Si: 0.03 to 0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001-0.100%, Al: 0.001-0.100%, Cu: 0.001-2.000%, Ni: 0.001 to 2.500%, Cr: 0.001-1.500%, Mo: 0.001 to 1.000%, Ti: 0.001 to 0.100%, V: 0.001 to 0.300%, B: 0.001 to 0.020%, O: 0.050% or less, and N: 0.010% or less; The balance is Fe and inevitable impurities. A method for producing a welded joint by gas-shielded arc welding of the steel plate according to claim 1 or 2.

6. The chemical composition of the weld metal is, in mass%, C: 0.04-0.14%, Si: 0.03 to 0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001-0.100%, Al: 0.001-0.100%, Cu: 0.001-2.000%, Ni: 0.001 to 2.500%, Cr: 0.001-1.500%, Mo: 0.001 to 1.000%, Ti: 0.001 to 0.100%, V: 0.001 to 0.300%, B: 0.001 to 0.020%, O: 0.050% or less, and N: 0.010% or less; The balance is Fe and inevitable impurities. A method for producing a welded joint by gas shielded arc welding of the steel plate according to claim 3.

7. The chemical composition of the weld metal is, in mass%, C: 0.04-0.14%, Si: 0.03 to 0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001-0.100%, Al: 0.001-0.100%, Cu: 0.001-2.000%, Ni: 0.001 to 2.500%, Cr: 0.001-1.500%, Mo: 0.001 to 1.000%, Ti: 0.001 to 0.100%, V: 0.001 to 0.300%, B: 0.001 to 0.020%, O: 0.050% or less, and N: 0.010% or less; The balance is Fe and inevitable impurities. A method for producing a welded joint by gas shielded arc welding of steel plates according to claim 4.

8. The chemical composition of the weld metal further comprises, in mass %, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less The method for producing a welded joint by gas-shielded arc welding of steel plates according to claim 5, comprising one or more selected from the group consisting of:

9. The chemical composition of the weld metal further comprises, in mass %, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less The method for producing a welded joint by gas-shielded arc welding of steel plates according to claim 6, comprising one or more selected from the group consisting of:

10. The chemical composition of the weld metal further comprises, in mass %, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less The method for producing a welded joint by gas-shielded arc welding of steel plates according to claim 7, comprising one or more selected from the group consisting of:

Citation Information

Patent Citations

  • Shallow penetration submerged arc welding method

    JP1980084278A

  • Three electrode two layer submerged arc welding of thick plate

    JP1996257752A

  • Method and apparatus for submerged arc welding

    JP2011200920A

  • Narrow groove gas-shield arc-welding method

    JP2015223605A

  • Thick steel sheet, and method for producing thick steel sheet

    WO2021054344A1