Metal surface treatment method

The use of a tellurium-based surface treatment solution efficiently colors metal surfaces in a gray tone by eliminating the need for oxide film formation and electrolysis, improving processing efficiency and aesthetic quality.

JP7558537B2Active Publication Date: 2024-10-01NIPPON HYOMEN KAGAKU KK +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023139242
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-08-29
Publication Date
2024-10-01
Estimated Expiration
2039-06-21

AI Technical Summary

Technical Problem

Conventional methods for coloring metal surfaces in a gray tone, such as those using alumite on aluminum or aluminum alloys, are inefficient and require multiple processing steps, including the formation of an oxide film and electrolytic coloring.

Method used

A metal surface treatment method using a solution containing tellurium, tellurium compounds, or their salts, along with inorganic acids, organic sulfur compounds, carboxylic acids, and oxoacids, to directly color metal surfaces in a gray tone without forming an oxide film or electrolysis.

Benefits of technology

The method achieves efficient coloring of metal surfaces in a gray tone with improved adhesion and aesthetic appearance, reducing processing steps and enhancing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558537000001
    Figure 0007558537000001
  • Figure 0007558537000002
    Figure 0007558537000002
  • Figure 0007558537000003
    Figure 0007558537000003
Patent Text Reader

Abstract

To provide a metal surface treatment method that can color a metal surface into a gray-based tone with a preferable treatment efficiency.SOLUTION: A metal surface treatment method includes a step of immersing copper, a copper alloy, zinc or a zinc alloy into a metal surface treatment liquid including tellurium, a tellurium compound, or salts thereof and having pH8-13 for 10 seconds to 10 minutes at 20-80°C to color the copper, copper alloy, zinc or zinc alloy into a gray-based tone.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a metal surface treatment method. [Background technology]

[0002] 2. Description of the Related Art Conventionally, in coloring various metals, particularly aluminum or aluminum alloys, a gray color tone has generally been obtained by anodizing or by adsorbing a dye onto an anodized film.

[0003] For example, Patent Document 1 discloses a method for electrolytic coloring of aluminum and aluminum alloys, which is characterized in that a colored coating formed on the surface of aluminum or aluminum alloy substrate by electrolytic coloring or natural coloring is made into a coating structure capable of electrolytic coloring, and then electrolytic coloring is performed to obtain a coating of a new color tone by superimposing colors. It is described that such a configuration can provide an electrolytic coloring method capable of obtaining various colors including various intermediate colors that cannot be obtained by conventional electrolytic coloring methods. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Publication No. 110895 / 1989 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the past, in order to color a metal surface in a grayish color tone, for example, in the case of aluminum or an aluminum alloy, it was necessary to use anodizing. In other words, in order to color a metal surface in a grayish color tone, it is necessary to use a metal having an oxide film on the surface, which requires many processing steps, and there is a demand for improvement in processing efficiency.

[0006] In view of the above problems, an object of the present invention is to provide a metal surface treatment method capable of coloring a metal surface in a grayish color tone with good treatment efficiency. [Means for solving the problem]

[0007] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have found that it is possible to color a metal surface in a grayish hue with good treatment efficiency by performing treatment with a metal surface treatment solution containing tellurium or a tellurium compound, or a salt thereof.

[0008] One aspect of the present invention, which was completed based on the above findings, is a metal surface treatment solution containing tellurium or a tellurium compound, or a salt thereof.

[0009] In one embodiment of the metal surface treatment liquid of the present invention, the tellurium or tellurium compound, or a salt thereof is tellurium monoxide, tellurium dioxide, tellurium trioxide, tellurous acid, telluric acid, tellurium tetrachloride, dimethyl telluride, or a salt thereof, or a combination thereof.

[0010] In another embodiment of the metal surface treatment liquid of the present invention, the total content of the tellurium or tellurium compound, or a salt thereof is 0.5 to 100 g / L.

[0011] In yet another embodiment, the metal surface treatment liquid of the present invention further contains an inorganic acid or a salt thereof.

[0012] In yet another embodiment of the metal surface treatment liquid of the present invention, the inorganic acid or the salt thereof is sulfuric acid, nitric acid, hydrochloric acid, phosphoric acid, or a salt thereof, or a combination thereof.

[0013] In still another embodiment of the metal surface treatment liquid of the present invention, the total content of the inorganic acid or the salt thereof is 1 to 200 g / L.

[0014] In yet another embodiment, the metal surface treatment liquid of the present invention further contains an organic sulfur compound or a salt thereof.

[0015] In yet another embodiment of the metal surface treatment liquid of the present invention, the organic sulfur compound or a salt thereof is thiourea, thiourea dioxide, thiodiglycol, dimethylthiourea, thiomalic acid, dithiodiglycolic acid, dimethylsulfoxide, methanesulfonic acid, p-toluenesulfonic acid, p-phenolsulfonic acid, thiocyanic acid, cysteine, methionine, or a salt thereof, or a combination thereof.

[0016] In still another embodiment of the metal surface treatment liquid of the present invention, the total content of the organic sulfur compounds or salts thereof is 0.1 to 50 g / L.

[0017] In yet another embodiment, the metal surface treatment liquid of the present invention further contains a carboxylic acid or a hydroxycarboxylic acid, or a salt thereof.

[0018] In yet another embodiment of the metal surface treatment liquid of the present invention, the carboxylic acid or hydroxycarboxylic acid, or a salt thereof, is formic acid, acetic acid, propionic acid, lactic acid, malic acid, citric acid, oxalic acid, gluconic acid, malonic acid, succinic acid, benzoic acid, pyruvic acid, glyoxylic acid, nitrilotriacetic acid, ethylenediaminetetraacetic acid, or a salt thereof, or a combination thereof.

[0019] In still another embodiment of the metal surface treatment liquid of the present invention, the total content of the carboxylic acid or hydroxycarboxylic acid, or a salt thereof is 0.5 to 100 g / L.

[0020] In yet another embodiment, the metal surface treatment liquid of the present invention further contains an oxoacid or a salt thereof.

[0021] In yet another embodiment of the metal surface treatment liquid of the present invention, the oxoacid or a salt thereof is perchloric acid, chloric acid, chlorous acid, hypochlorous acid, bromic acid, carbonic acid, boric acid, or a salt thereof, or a combination thereof.

[0022] In still another embodiment of the metal surface treatment liquid of the present invention, the total content of the oxoacid or a salt thereof is 0.5 to 100 g / L.

[0023] In yet another embodiment of the metal surface treatment solution of the present invention, the metal to be treated is at least one selected from the group consisting of aluminum, aluminum alloys, copper, copper alloys, iron, iron alloys, zinc, zinc alloys, nickel, nickel alloys, magnesium, and magnesium alloys.

[0024] In another aspect, the present invention provides a metal surface treatment method including a step of coloring a metal using the metal surface treatment liquid of the present invention.

[0025] In one embodiment of the metal surface treatment method of the present invention, in the step of coloring the metal, the metal is colored by immersing the metal in the metal surface treatment solution at 10° C. to 80° C. for 10 seconds to 20 minutes. Effect of the Invention

[0026] According to the present invention, there can be provided a metal surface treatment method capable of coloring a metal surface in a grayish color tone with good treatment efficiency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Hereinafter, embodiments of the metal surface treatment liquid and metal surface treatment method of the present invention will be described, but the present invention should not be interpreted as being limited thereto, and various changes, modifications, and improvements can be made based on the knowledge of those skilled in the art without departing from the scope of the present invention.

[0028] [Metal surface treatment liquid] The metal surface treatment liquid according to the embodiment of the present invention contains tellurium or a tellurium compound, or a salt thereof. By using the metal surface treatment liquid containing tellurium or a tellurium compound, or a salt thereof, a film (colored film) can be formed on the metal surface by simply immersing the metal to be treated in the metal surface treatment liquid, and thus the metal surface can be colored in a grayish color tone. Therefore, when coloring the metal surface in a grayish color tone, it is not necessary to form an oxide film on the surface of the metal, and it is not necessary to color the metal surface by electrolysis, and the treatment efficiency is improved. In addition, the metal surface treatment liquid according to the embodiment of the present invention also provides good adhesion of the film (colored film) formed on the metal surface.

[0029] (Metal to be treated) The metal to be treated (metal to be treated) whose surface is to be colored with the metal surface treatment liquid according to the embodiment of the present invention may be at least one selected from the group consisting of aluminum, aluminum alloy, copper, copper alloy, iron, iron alloy, zinc, zinc alloy, nickel, nickel alloy, magnesium, and magnesium alloy. The metal to be treated may be the metal itself, or may be, for example, a plating of the metal formed on the surface of a metal substrate such as an iron-based material or an iron-based part.

[0030] (Tellurium or tellurium compounds, or their salts) The tellurium or tellurium compound, or a salt thereof, is preferably tellurium monoxide, tellurium dioxide, tellurium trioxide, tellurous acid, telluric acid, tellurium tetrachloride, dimethyl telluride, or a salt thereof, or a combination thereof. As the salt of tellurium monoxide, tellurium dioxide, tellurium trioxide, tellurous acid, telluric acid, tellurium tetrachloride, or dimethyl telluride, a metal salt or an ammonium salt thereof can be used.

[0031] The total content of tellurium or tellurium compounds or their salts in the metal surface treatment liquid according to the embodiment of the present invention depends on the type of metal to be treated and the degree of grayish color to be colored, but for example, the total content of tellurium or tellurium compounds or their salts can be 0.5 to 100 g / L. Basically, the smaller the total content of tellurium or tellurium compounds or their salts, the more the metal surface can be colored in a light grayish color. Also, the larger the total content of tellurium or tellurium compounds or their salts, the more the metal surface can be colored in a dark grayish color. The total content of tellurium or tellurium compounds or their salts is more preferably 1 to 50 g / L, and more preferably 2 to 20 g / L.

[0032] As described below, the metal surface treatment solution according to the embodiment of the present invention may contain an inorganic acid or a salt thereof, an organic sulfur compound or a salt thereof, a carboxylic acid or a hydroxycarboxylic acid or a salt thereof, an oxoacid or a salt thereof, etc., but in the case of a metal surface treatment solution that does not contain these components, it is possible to color metal surfaces, particularly aluminum and aluminum alloys, in a more aesthetically pleasing grayish tone.

[0033] (Inorganic acid or its salt) The metal surface treatment liquid according to the embodiment of the present invention may further contain an inorganic acid or a salt thereof. Even if the metal surface treatment liquid according to the embodiment of the present invention contains an inorganic acid or a salt thereof, it can color the above-mentioned metal surface to be treated in a grayish color tone with good treatment efficiency. Furthermore, the metal surface treatment liquid according to the embodiment of the present invention contains an inorganic acid or a salt thereof, which promotes metal dissolution and increases the pH of the metal surface, thereby promoting the reaction of forming a colored film, and therefore can color the surface of metals such as copper, copper alloys, iron, iron alloys, zinc, zinc alloys, nickel, nickel alloys, magnesium, and magnesium alloys in a grayish color tone with a more aesthetic appearance.

[0034] The inorganic acid or its salt is preferably sulfuric acid, nitric acid, hydrochloric acid, phosphoric acid, or a salt thereof, or a combination thereof. As the salt of sulfuric acid, nitric acid, hydrochloric acid, or phosphoric acid, a metal salt or an ammonium salt thereof can be used.

[0035] The total content of inorganic acid or its salt in the metal surface treatment liquid according to the embodiment of the present invention can be 1 to 200 g / L. Basically, the smaller the total content of inorganic acid or its salt, the more the metal surface can be colored in a light grayish tone. Also, the larger the total content of inorganic acid or its salt, the more the metal surface can be colored in a dark grayish tone. The total content of inorganic acid or its salt is more preferably 10 to 150 g / L, and more preferably 70 to 120 g / L.

[0036] (Organosulfur compounds or their salts) The metal surface treatment liquid according to the embodiment of the present invention may further contain an organic sulfur compound or a salt thereof. Even if the metal surface treatment liquid according to the embodiment of the present invention contains an organic sulfur compound or a salt thereof, it can color the above-mentioned metal surface to be treated in a grayish color tone with good treatment efficiency. Furthermore, the metal surface treatment liquid according to the embodiment of the present invention contains an organic sulfur compound or a salt thereof, and the organic sulfur compound promotes metal dissolution and increases the pH of the metal surface, thereby promoting the reaction of forming a colored film. Therefore, the surface of metals such as copper, copper alloys, nickel, and nickel alloys can be colored in a grayish color tone with a more aesthetic appearance.

[0037] The organic sulfur compound or its salt is preferably thiourea, thiourea dioxide, thiodiglycol, dimethylthiourea, thiomalic acid, dithiodiglycolic acid, dimethylsulfoxide, methanesulfonic acid, p-toluenesulfonic acid, p-phenolsulfonic acid, thiocyanic acid, cysteine, methionine, or a salt thereof, or a combination thereof. As the salts of thiourea, thiourea dioxide, thiodiglycol, dimethylthiourea, thiomalic acid, dithiodiglycolic acid, dimethylsulfoxide, methanesulfonic acid, p-toluenesulfonic acid, p-phenolsulfonic acid, thiocyanic acid, cysteine, and methionine, metal salts or ammonium salts thereof can be used.

[0038] The total content of the organic sulfur compounds or their salts in the metal surface treatment liquid according to the embodiment of the present invention can be 0.1 to 50 g / L. Basically, the smaller the total content of the organic sulfur compounds or their salts, the more the metal surface can be colored in a light grayish tone. Also, the larger the total content of the organic sulfur compounds or their salts, the more the metal surface can be colored in a dark grayish tone. The total content of the organic sulfur compounds or their salts is more preferably 1 to 30 g / L, and more preferably 5 to 15 g / L.

[0039] (Carboxylic acid or hydroxycarboxylic acid, or their salts) The metal surface treatment liquid according to the embodiment of the present invention may further contain a carboxylic acid or a hydroxycarboxylic acid, or a salt thereof. Even if the metal surface treatment liquid according to the embodiment of the present invention contains a carboxylic acid or a hydroxycarboxylic acid, or a salt thereof, it can color the above-mentioned metal surface to be treated in a grayish color tone with good treatment efficiency. Furthermore, the metal surface treatment liquid according to the embodiment of the present invention contains a carboxylic acid or a hydroxycarboxylic acid, or a salt thereof, and the carboxylic acid or the hydroxycarboxylic acid is chelated with tellurium, thereby suppressing the coloring reaction and facilitating the formation of a dense film. Therefore, it is possible to color the surfaces of metals such as copper, copper alloys, iron, iron alloys, zinc, and zinc alloys in a grayish color tone with a more aesthetic appearance.

[0040] The carboxylic acid or hydroxycarboxylic acid, or a salt thereof, is preferably formic acid, acetic acid, propionic acid, lactic acid, malic acid, citric acid, oxalic acid, gluconic acid, malonic acid, succinic acid, benzoic acid, pyruvic acid, glyoxylic acid, nitrilotriacetic acid, ethylenediaminetetraacetic acid, or a salt thereof, or a combination thereof. As the salt of formic acid, acetic acid, propionic acid, lactic acid, malic acid, citric acid, oxalic acid, gluconic acid, malonic acid, succinic acid, benzoic acid, pyruvic acid, glyoxylic acid, nitrilotriacetic acid, or ethylenediaminetetraacetic acid, a metal salt or an ammonium salt thereof can be used.

[0041] The total content of carboxylic acid or hydroxycarboxylic acid, or a salt thereof in the metal surface treatment liquid according to the embodiment of the present invention can be 0.5 to 100 g / L. Basically, the smaller the total content of carboxylic acid or hydroxycarboxylic acid, or a salt thereof, the darker the grayish color tone of the metal surface can be colored. Also, the larger the total content of carboxylic acid or hydroxycarboxylic acid, or a salt thereof, the lighter the grayish color tone of the metal surface can be colored. The total content of carboxylic acid or hydroxycarboxylic acid, or a salt thereof is more preferably 1 to 50 g / L, and more preferably 10 to 30 g / L.

[0042] (Oxoacid or its salt) The metal surface treatment liquid according to the embodiment of the present invention may further contain an oxoacid or a salt thereof. Even if the metal surface treatment liquid according to the embodiment of the present invention contains an oxoacid or a salt thereof, it can color the above-mentioned metal surface to be treated in a grayish color tone with good treatment efficiency. Furthermore, by containing an oxoacid or a salt thereof, the metal surface treatment liquid according to the embodiment of the present invention can color the surface of metals such as copper, copper alloys, iron, iron alloys, zinc, and zinc alloys in a more aesthetically pleasing grayish color tone.

[0043] The oxoacid or its salt is preferably perchloric acid, chloric acid, chlorous acid, hypochlorous acid, bromic acid, carbonic acid, boric acid, or a salt thereof, or a combination thereof. As the salt of perchloric acid, chloric acid, chlorous acid, hypochlorous acid, bromic acid, carbonic acid, or boric acid, a metal salt or an ammonium salt thereof can be used.

[0044] The total content of oxoacids or salts thereof in the metal surface treatment solution according to the embodiment of the present invention may be 0.5 to 100 g / L. Basically, the smaller the total content of oxoacids or salts thereof, the more the metal surface can be colored in a lighter grayish tone. Also, the greater the total content of oxoacids or salts thereof, the more the metal surface can be colored in a darker grayish tone. The total content of oxoacids or salts thereof is more preferably 1 to 50 g / L, and more preferably 10 to 30 g / L.

[0045] (aqueous medium) The metal surface treatment liquid according to the embodiment of the present invention may be a mixture of the above-mentioned various components and an aqueous medium. The aqueous medium refers to a medium mainly composed of water. Examples of the aqueous medium include a medium mainly composed of water and containing an organic solvent such as an alcohol miscible with water. The aqueous medium may contain various components that act advantageously to improve some properties of the colored surface of the metal during preparation of the metal surface treatment liquid according to the embodiment of the present invention, during storage of the metal surface treatment liquid, or after coloring the metal surface, or various components that do not substantially inhibit the effects of the present invention, as necessary. For example, pH adjusters, storage stabilizers, etc. are specific examples of such components.

[0046] [Metal surface treatment method] Next, the metal surface treatment method according to the embodiment of the present invention will be described in detail. First, a bath containing the metal surface treatment liquid according to the embodiment of the present invention is prepared. Next, the metal to be treated is immersed in the metal surface treatment liquid while controlling the temperature of the metal surface treatment liquid in the bath. After a predetermined time has elapsed, the metal to be treated is pulled out of the bath to obtain a metal whose surface is colored in a grayish hue. In this way, according to the metal surface treatment method according to the embodiment of the present invention, the metal to be treated can be colored in a grayish hue simply by immersing it in the metal surface treatment liquid. Therefore, when coloring the metal surface in a grayish hue, it is not necessary to form an oxide film on the surface of the metal, and it is not necessary to color the metal by electrolysis, and the treatment efficiency is improved.

[0047] Furthermore, in the metal surface treatment method according to the embodiment of the present invention, other than immersing the metal to be treated in the metal surface treatment liquid, the surface of the metal to be treated may be colored by contacting the metal surface treatment liquid with the surface of the metal to be treated, for example, by a spraying step using the metal surface treatment liquid.

[0048] The treatment temperature with the metal surface treatment liquid is preferably in the range of 10 to 80° C., more preferably in the range of 10 to 60° C., and even more preferably in the range of 30 to 60° C. If the treatment temperature is 10° C. or higher, the reaction rate of the surface treatment increases, and if it is 80° C. or lower, a drop in the liquid level of the metal surface treatment liquid due to evaporation can be suppressed.

[0049] The treatment time with the metal surface treatment liquid is preferably in the range of 10 seconds to 20 minutes, more preferably in the range of 30 seconds to 20 minutes, and even more preferably in the range of 1 minute to 10 minutes. Basically, the shorter the treatment time, the more the metal surface can be colored in a light grayish tone. Also, the longer the treatment time, the more the metal surface can be colored in a dark grayish tone.

[0050] When performing metal surface treatment, it is possible to improve the appearance, corrosion resistance, and reactivity with the metal surface treatment solution of the metal to be treated by first degreasing, activating, and conditioning the surface of the metal to be treated.

[0051] After the metal surface treatment, post-treatment may be performed with a coating agent containing one or more of the group consisting of silicon, resin, and wax. There are no particular limitations on these coating agents as long as they do not affect the desired color tone of the metal surface, and coating agents containing resins such as acrylic resin, olefin resin, alkyd resin, urea resin, epoxy resin, melamine resin, fluororesin, polyethylene, polyvinyl chloride, polystyrene, polypropylene, methacrylic resin, phenolic resin, polyester resin, polyurethane, polyamide, polycarbonate, silicate, colloidal silica, etc. may be used. The resin concentration is preferably 0.01 to 800 g / L, but the appropriate concentration varies depending on the type of resin. Specific examples of coating agents include Cosmo Coat (trade name, Kansai Paint Co., Ltd.), Hi-Seal 272 (trade name, Nippon Hyomen Kagaku Co., Ltd.), Stron JS Coat (trade name, Nippon Hyomen Kagaku Co., Ltd.), Tryner TR-170 (trade name, Nippon Hyomen Kagaku Co., Ltd.), Finigard (trade name, Coventya Co., Ltd.), etc. Specific examples of acrylic resins include Hirotite (trade name, Hitachi Chemical Co., Ltd.) and Aroset (trade name, Nippon Shokubai Co., Ltd.), and examples of olefin resins include Flothane (trade name, Sumitomo Seika Chemicals Co., Ltd.), PES (trade name, Nippon Unicar Co., Ltd.), Chemipearl (trade name, Mitsui Chemicals Inc.), and Sunfine (trade name, Asahi Kasei Corporation).

[0052] The metal surface treatment liquid according to the embodiment of the present invention can be used for the purpose of coloring a metal surface in a desired color, imparting a desired aesthetic appearance, imparting distinguishability, etc. The form of the metal to be treated can be of any shape, and is not particularly limited, but examples of the metal that can be used include ornaments, fastening members such as buttons and zippers, and in-vehicle parts. In addition, the shape of the metal to be treated is also not limited, and any shape can be used. EXAMPLES

[0053] Examples of the present invention are given below, but these are provided for a better understanding of the present invention and are not intended to limit the present invention.

[0054] [Test Example 1: Coloring test of aluminum and aluminum alloys] (Reference examples 1-35, 92, 93) As test pieces (metal pieces to be treated), JIS A5052 (aluminum-magnesium alloy) and ADC12 (aluminum die-cast) were prepared, and the surfaces of the test pieces were degreased and washed with water in that order. Next, a bath was prepared containing a metal surface treatment solution having the composition shown in Tables 1 to 3 and 8. Pure water was used as the aqueous medium for the metal surface treatment solution. Next, the test pieces were immersed in the metal surface treatment liquid in the bath while controlling the temperature to the values ​​shown in Tables 1 to 3 and 8. After immersion for the time shown in Tables 1 to 3 and 8, the test pieces were taken out. Next, the surfaces of the test pieces were washed with water and then dried.

[0055] In addition, for Reference Examples 92 and 93, the test pieces after forming a film (colored film) by immersion were washed with water, coated, and dried. Stron JS Coat (a coating agent manufactured by Nippon Hyomen Kagaku Co., Ltd.) was used for the coating treatment of Reference Example 92, and TR-170 (a coating agent manufactured by Nippon Hyomen Kagaku Co., Ltd.) was used for the coating treatment of Reference Example 93.

[0056] [Test Example 2: Coloring test of copper and copper alloys] (Examples 36 to 38, 45, and 51, Reference Examples 39 to 44, 46 to 50, and 52 to 55) As test pieces (metal pieces to be treated), JIS C2600P (brass) and C1100P (pure copper) were prepared, and the surfaces of the test pieces were degreased and washed with water in that order. Next, a bath was prepared containing a metal surface treatment solution having the composition shown in Tables 4 and 5. Pure water was used as the aqueous medium for the metal surface treatment solution. Next, the test pieces were immersed in the metal surface treatment solution in the bath, with the temperature controlled to the values ​​shown in Tables 4 to 5. After immersion for the time shown in Tables 4 to 5, the test pieces were removed. Next, the surfaces of the test pieces were washed with water and then dried.

[0057] [Test Example 3: Coloring test of zinc and zinc alloys] (Examples 56 to 59, 65, 69 to 71, 75, Reference Examples 60 to 64, 66 to 68, 72 to 74) JIS ZDC2 (zinc die-cast) and zinc-plated material were prepared as test pieces (metal pieces to be treated), and the surfaces of the test pieces were degreased and washed with water. The zinc-plated material was a JIS SPCC (rolled steel plate) specified by JIS that was used as a base material and was plated with zincate zinc to a thickness of 8 μm. In addition, 9000ABS manufactured by Nippon Hyomen Kagaku Co., Ltd. was used as a brightener for the zincate zinc plating. Next, a bath was prepared containing a metal surface treatment solution having the composition shown in Tables 6 to 7. Pure water was used as the aqueous medium for the metal surface treatment solution. Next, the test pieces were immersed in the metal surface treatment solution in the bath, with the temperature controlled to the values ​​shown in Tables 6 to 7. After immersion for the time shown in Tables 6 to 7, the test pieces were removed. Next, the surfaces of the test pieces were washed with water and then dried.

[0058] [Test Example 4: Coloring test of iron and iron alloys] (Reference examples 76~80) A JIS SPCC (rolled steel plate) was prepared as a test piece (metal piece to be treated), and the surface of the test piece was degreased and washed with water in that order. Next, a bath was prepared containing a metal surface treatment solution having the composition shown in Table 7. Pure water was used as the aqueous medium for the metal surface treatment solution. Next, the test piece was immersed in the metal surface treatment solution in the bath, with the temperature controlled to that shown in Table 7. After immersion for the time shown in Table 7, the test piece was taken out. Next, the surface of the test piece was washed with water and then dried.

[0059] [Test Example 5: Coloring test of magnesium and magnesium alloys] (Reference examples 81~86) As test pieces (metal pieces to be treated), JIS AZ31 and JIS AZ91 (magnesium-zinc alloys) were prepared, and the surfaces of the test pieces were degreased and washed with water in that order. Next, a bath was prepared containing a metal surface treatment solution having the composition shown in Table 8. Pure water was used as the aqueous medium for the metal surface treatment solution. Next, the test piece was immersed in the metal surface treatment solution in the bath, with the temperature controlled to that shown in Table 8. After immersion for the time shown in Table 8, the test piece was taken out. Next, the surface of the test piece was washed with water and then dried.

[0060] [Test Example 6: Coloring test of nickel and nickel alloys] (Reference examples 87~91) A JIS Ni200 (pure nickel) test piece (metal piece to be treated) was prepared, and the surface of the test piece was degreased and washed with water in that order. Next, a bath was prepared containing a metal surface treatment solution having the composition shown in Table 8. Pure water was used as the aqueous medium for the metal surface treatment solution. Next, the test piece was immersed in the metal surface treatment solution in the bath, with the temperature controlled to that shown in Table 8. After immersion for the time shown in Table 8, the test piece was taken out. Next, the surface of the test piece was washed with water and then dried.

[0061] [Test Example 7] (Comparative Examples 1 to 10) The metals shown in Table 9 were prepared as test pieces (metal pieces to be treated), and the surfaces of the test pieces were degreased and washed with water in that order. Next, a bath was prepared containing a metal surface treatment solution having the composition shown in Table 9. Pure water was used as the aqueous medium for the metal surface treatment solution. Next, the test piece was immersed in the metal surface treatment solution in the bath, with the temperature controlled to that shown in Table 9. After immersion for the time shown in Table 9, the test piece was taken out. Next, the surface of the test piece was washed with water and then dried.

[0062] [Various evaluations] For the test pieces produced in Examples 36 to 38, 45, 51, 56 to 59, 65, 69 to 71, 75, Reference Examples 1 to 35, 39 to 44, 46 to 50, 52 to 55, 60 to 64, 66 to 68, 72 to 74, 76 to 93 and Comparative Examples 1 to 10, color tone evaluation and adhesion evaluation were performed as follows.

[0063] (Color Tone Evaluation) The surface color tone of the test piece was evaluated visually according to the following criteria: A: Antique gray with a uniform and aesthetically pleasing finish B: Antique gray with a uniform and beautiful finish, darker than A C: Antique gray with a uniform and beautiful finish, lighter than A D: No coloring

[0064] (Adhesion evaluation) The surface of the test piece was cut with a cutter into 10 × 10 squares (100 squares in total), and the number of squares in which the colored film did not come off when Scotch tape (registered trademark) was applied and peeled off was counted. The size of one square was 1 mm x 1 mm in length x width. In each table, the result is shown as (the number of squares where the colored film did not peel off) / 100, and the greater the number of squares where the colored film did not peel off, the higher the adhesion of the colored film.

[0065] Tables 1 to 9 show the test conditions and evaluation results for Examples 36 to 38, 45, 51, 56 to 59, 65, 69 to 71, and 75, Reference Examples 1 to 35, 39 to 44, 46 to 50, 52 to 55, 60 to 64, 66 to 68, 72 to 74, and 76 to 93, and Comparative Examples 1 to 10. In addition, Test Nos. 1 to 35, 39 to 44, 46 to 50, 52 to 55, 60 to 64, 66 to 68, 72 to 74, and 76 to 93 in Tables 1 to 8 are reference examples.

[0066] [Table 1]

[0067] [Table 2]

[0068] [Table 3]

[0069] [Table 4]

[0070] [Table 5]

[0071] [Table 6]

[0072] [Table 7]

[0073] [Table 8]

[0074] [Table 9]

[0075] From the above results, as in Examples 36 to 38, 45, 51, 56 to 59, 65, 69 to 71, 75 and Reference Examples 1 to 35, 39 to 44, 46 to 50, 52 to 55, 60 to 64, 66 to 68, 72 to 74, and 76 to 93, it was confirmed that by using a metal surface treatment solution containing tellurium or a tellurium compound, or a salt thereof, it is possible to color a metal surface in a grayish color tone with good treatment efficiency. On the other hand, it was confirmed that, as in Comparative Examples 1 to 10, if the metal surface treatment solution does not contain tellurium, a tellurium compound, or a salt thereof, it is not possible to color the metal surface in a grayish color tone.

Claims

1. A metal surface treatment method comprising the step of immersing copper, a copper alloy, zinc or a zinc alloy in a metal surface treatment solution containing tellurium or a tellurium compound or a salt thereof, not containing potassium ferricyanide and having a pH of 8 to 13, at 20°C to 80°C for 10 seconds to 10 minutes, thereby coloring the copper, copper alloy, zinc or zinc alloy in a grayish color tone.

2. 2. The metal surface treatment method according to claim 1, wherein the tellurium or tellurium compound, or a salt thereof, is tellurium monoxide, tellurium dioxide, tellurium trioxide, tellurous acid, telluric acid, tellurium tetrachloride, dimethyl telluride, or a salt thereof, or a combination thereof.

3. 3. The method for metal surface treatment according to claim 1, wherein the total content of the tellurium or tellurium compound, or a salt thereof is 0.5 to 100 g / L.

4. The metal surface treatment method according to any one of claims 1 to 3, further comprising a salt of an inorganic acid.

5. 5. The method of claim 4, wherein the salt of an inorganic acid is a salt of sulfuric acid, nitric acid, hydrochloric acid, or phosphoric acid, or a combination thereof.

6. 6. The method for treating a metal surface according to claim 4, wherein the total content of the inorganic acid salts is 1 to 200 g / L.

7. The metal surface treatment method according to any one of claims 1 to 6, further comprising an organic sulfur compound or a salt thereof.

8. 8. The metal surface treatment method according to claim 7, wherein the organic sulfur compound or a salt thereof is thiourea, thiourea dioxide, thiodiglycol, dimethylthiourea, thiomalic acid, dithiodiglycolic acid, dimethylsulfoxide, methanesulfonic acid, p-toluenesulfonic acid, p-phenolsulfonic acid, thiocyanic acid, cysteine, methionine, or a salt thereof, or a combination thereof.

9. 9. The method for treating a metal surface according to claim 7, wherein the total content of the organic sulfur compounds or salts thereof is 0.1 to 50 g / L.

10. The method for treating a metal surface according to any one of claims 1 to 9, further comprising a salt of a carboxylic acid or a salt of a hydroxycarboxylic acid.

11. 11. The metal surface treatment method according to claim 10, wherein the salt of a carboxylic acid or the salt of a hydroxycarboxylic acid is a salt of formic acid, acetic acid, propionic acid, lactic acid, malic acid, citric acid, oxalic acid, gluconic acid, malonic acid, succinic acid, benzoic acid, pyruvic acid, glyoxylic acid, nitrilotriacetic acid or ethylenediaminetetraacetic acid, or a combination thereof.

12. 12. The method for treating a metal surface according to claim 10, wherein the total content of the salt of a carboxylic acid or the salt of a hydroxycarboxylic acid is 0.5 to 100 g / L.

13. 13. The method for treating a metal surface according to claim 1, further comprising a salt of an oxoacid, which is a salt of perchloric acid, chloric acid, chlorous acid, hypochlorous acid, bromic acid, carbonic acid or boric acid, or a combination thereof.

14. 14. The method for treating a metal surface according to claim 13, wherein the total content of the salts of oxoacids is 0.5 to 100 g / L.

Citation Information

Patent Citations

  • Electrolytic coloring method of aluminum and aluminum alloy

    JP1985110895A

  • Improved composition and method for imparting coating to metal surface

    JP1991094074A

  • Improvement for applying tellurium-containing coating film on metal surface using cyclodeoxtrin / Tellurium composition

    JP1993295561A

  • Treatment of zinc surfaces

    US2522474A

  • Method for applying tellurium-containing coatings to metallic surfaces using organic acids

    US5238505A