Optical pressure sensitive adhesive composition and its use
The optical adhesive composition with a specific acrylic polymer formulation addresses the challenge of achieving high adhesive strength and reworkability by using a surfactant or compound with a polyoxyalkylene skeleton, ensuring easy removal and transparency in optical applications.
Patent Information
- Application Number
- JP2019138604
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-07-31
- Filing Date
- 2019-07-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2039-07-29
AI Technical Summary
Existing pressure-sensitive adhesives face challenges in achieving both high adhesive strength and reworkability, particularly in optical applications, where maintaining transparency and avoiding damage to fragile adherends is crucial.
An optical adhesive composition is developed using an acrylic polymer with limited alkoxyalkyl (meth)acrylate and alkoxypolyalkylene glycol (meth)acrylate content, combined with a surfactant or compound having a polyoxyalkylene skeleton, to enhance water releasability and reduce peeling force, ensuring both strong adhesion and easy removal.
The composition achieves sufficient adhesive strength for optical applications while allowing easy reworkability using water, maintaining transparency and preventing damage to adherends.
Smart Images

Figure 0007558649000009 
Figure 0007558649000010 
Figure 0007558649000011
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical pressure-sensitive adhesive composition, a pressure-sensitive adhesive sheet, an optical member with a pressure-sensitive adhesive sheet, and a method for peeling off the pressure-sensitive adhesive sheet. [Background technology]
[0002] In general, adhesives (also called pressure-sensitive adhesives; the same applies below) are in a soft solid (viscoelastic) state in a temperature range near room temperature, and have the property of easily adhering to an adherend by pressure. Taking advantage of such properties, adhesives are widely used in various fields in the form of a supported adhesive sheet having an adhesive layer on a support, or in the form of a support-less adhesive sheet without a support. For example, adhesives are used for the purpose of bonding optical components such as polarizing plates in various optical applications such as optical input devices such as touch panels and display devices such as liquid crystal display devices. Patent documents 1 to 3 are technical documents related to this type of adhesive. Patent document 1 discloses an adhesive used for touch panels. Patent documents 2 and 3 disclose prior art related to adhesives for polarizing plates. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-047295 A [Patent Document 2] JP 2009-516048 A [Patent Document 3] JP 2009-519372 A Summary of the Invention [Problem to be solved by the invention]
[0004] Various properties are required for adhesives depending on the application. Some of these properties are difficult to achieve at a high level, such as when one property is improved, the other property tends to decrease. One example of properties that are difficult to achieve at the same time is adhesion to an adherend and reworkability. The above-mentioned rework refers to peeling the adhesive sheet from the adherend and reattaching it when, for example, a mistake occurs when attaching the adhesive sheet to the adherend (misalignment, generation of wrinkles or air bubbles, inclusion of foreign matter, etc.) or when a defect is found in the adherend after the adhesive sheet is attached. In particular, when the adherend is fragile or thin, it is required to keep the peeling force of the adhesive sheet from the adherend (i.e., the adhesive force to the adherend) low to prevent damage or deformation of the adherend due to rework, so it is not easy to realize an adhesive sheet that combines good reworkability and high adhesion.
[0005] Furthermore, for example, in optical applications, in addition to achieving both the reworkability and adhesive strength, properties such as transparency that do not impair the optical properties of the object to which the adhesive is applied are required, so the restrictions on adhesive design are even stricter. For example, Patent Document 1 deals with improving optical properties such as thermal whitening resistance and thermal foaming resistance using a composition that uses an acrylic polymer in which alkoxyalkyl (meth)acrylate or alkoxypolyalkylene glycol (meth)acrylate is copolymerized at a specified ratio or higher.
[0006] The present invention has been made in view of the above circumstances, and aims to provide an optical pressure-sensitive adhesive composition that can be easily peeled off using an aqueous liquid such as water and has sufficient adhesive strength. Other related objects of the present invention include providing a pressure-sensitive adhesive sheet, an optical member with a pressure-sensitive adhesive sheet, and a method for peeling off the pressure-sensitive adhesive sheet. [Means for solving the problem]
[0007] According to this specification, an optical pressure-sensitive adhesive composition containing an acrylic polymer is provided. In one embodiment of the pressure-sensitive adhesive composition, the monomer components forming the acrylic polymer contain less than 20% by weight of alkoxyalkyl (meth)acrylate and less than 20% by weight of alkoxypolyalkylene glycol (meth)acrylate. The pressure-sensitive adhesive composition further contains at least one compound A selected from a surfactant and a compound having a polyoxyalkylene skeleton.
[0008] The pressure-sensitive adhesive composition can exhibit good adhesive strength by using an acrylic polymer. The acrylic polymer is used with a limited amount of alkoxyalkyl (meth)acrylate or alkoxypolyalkylene glycol (meth)acrylate as a monomer component in order to suppress gelation during the production of the polymer. In addition to the acrylic polymer, the composition contains at least one compound A selected from a surfactant and a compound having a polyoxyalkylene skeleton, so that the peel strength can be effectively reduced by using an aqueous liquid such as water. That is, in a composition suitable for optical applications, sufficient adhesive strength and water peelability leading to reworkability can be achieved at the same time.
[0009] According to this specification, there is provided an optical pressure-sensitive adhesive composition according to another embodiment. The pressure-sensitive adhesive composition includes an acrylic polymer and at least one compound A selected from a surfactant and a compound having a polyoxyalkylene skeleton. The content of the compound A is less than 1 part by weight based on 100 parts by weight of the acrylic polymer.
[0010] The pressure-sensitive adhesive composition can exhibit good adhesive strength by using an acrylic polymer. In addition, by including compound A in addition to the acrylic polymer, peel strength can be reduced by using an aqueous liquid such as water. That is, sufficient adhesive strength and water peelability leading to reworkability can be achieved at the same time. In addition, since the amount of compound A used is limited, transparency required for optical applications can be easily obtained, and the decrease in adhesive strength can be suppressed.
[0011] A pressure-sensitive adhesive composition according to a preferred embodiment of the technology disclosed herein (including an optical pressure-sensitive adhesive composition, a pressure-sensitive adhesive sheet, an optical member with a pressure-sensitive adhesive sheet, and a pressure-sensitive adhesive sheet peeling method; the same applies below) is a solvent-based pressure-sensitive adhesive composition or a solventless pressure-sensitive adhesive composition. In an embodiment using a solvent-based or solventless pressure-sensitive adhesive composition, the effects of the technology disclosed herein are preferably exhibited.
[0012] In a preferred embodiment of the technology disclosed herein, the compound A is a nonionic surfactant. By including a nonionic surfactant in the acrylic polymer-containing pressure-sensitive adhesive layer, water peelability can be favorably expressed. In addition, by using a nonionic surfactant as the compound A, low haze can be easily maintained.
[0013] In a preferred embodiment of the technology disclosed herein, the compound A has an HLB (hydrophile-lipophile balance) of 10 or more. By using a compound (typically a surfactant) having an HLB of 10 or more as compound A, water peelability is preferably exhibited.
[0014] In a preferred embodiment of the technology disclosed herein, the monomer components forming the acrylic polymer include a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 20 carbon atoms at the ester terminal, and a monomer having a nitrogen atom. By using an acrylic polymer having the above monomer composition, optical properties and good adhesive strength can be preferably exhibited. Furthermore, in a configuration using the acrylic polymer, water peelability due to compound A is easily exhibited. The monomer having a nitrogen atom is a compound represented by the general formula (1): [ka] (In general formula (1), R 1 is a divalent organic group. ); and (meth)acrylamide.
[0015] In a preferred embodiment of the technique disclosed herein, the acrylic polymer has a solubility parameter (SP) of 18.0 to 23.0 (MJ / m 3 ) 1 / 2 By incorporating compound A into a pressure-sensitive adhesive containing an acrylic polymer having the above SP value, the effects of the technology disclosed herein are preferably exhibited.
[0016] The pressure-sensitive adhesive composition according to a preferred embodiment of the technology disclosed herein further contains a peel strength increasing agent. By including the peel strength increasing agent, the peel strength (adhesive strength) can be improved. In a more preferred embodiment, the peel strength increasing agent is a compound having an alkoxysilyl group. By using a compound having an alkoxysilyl group as the peel strength increasing agent, the peel strength from the adherend can be effectively improved.
[0017] This specification also provides an optical pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer made of any of the pressure-sensitive adhesive compositions disclosed herein, which can achieve both good adhesive strength and water removability leading to reworkability.
[0018] This specification also provides a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer. This pressure-sensitive adhesive sheet has a normal peel force FN1 of 2 N / cm or more, measured under conditions of a tensile speed of 60 mm / min and a peel angle of 180 degrees after the pressure-sensitive adhesive surface of the pressure-sensitive adhesive sheet is attached to an alkaline glass plate as an adherend and left at 23° C. for 30 minutes. The water-peeling adhesion reduction rate A is 50% or more. Here, the water-peeling adhesion reduction rate A is calculated by the following formula from the water peel force FW1 [N / cm] measured under conditions of a tensile speed of 60 mm / min and a peel angle of 180 degrees using a tensile tester based on JIS Z0237, and the normal peel force FN1 [N / cm], after 30 minutes from attaching the pressure-sensitive adhesive surface of the pressure-sensitive adhesive sheet to an alkaline glass plate as an adherend under a measurement environment of 23° C. and 50% RH, and dropping 10 μL to 40 μL of distilled water onto the adherend and allowing the distilled water to penetrate into one end of the interface between the pressure-sensitive adhesive layer and the adherend: (1-(FW1 / FN1)) x 100; This pressure sensitive adhesive sheet can achieve both good adhesive strength and water peelability leading to reworkability. The normal peel strength FN1 and the water peel strength FW1 are specifically measured by the method described in the Examples below.
[0019] This specification also provides a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer. The pressure-sensitive adhesive sheet has an adhesive strength (normal adhesive strength) N0 of 2.0 N / 10 mm or more after one day at room temperature when the adhesive surface is attached to an adherend of an alkali glass plate produced by the float method, the adherend having a contact angle with distilled water of 5 degrees to 10 degrees. The pressure-sensitive adhesive sheet also has a water-peeling adhesive strength reduction rate B of 40% or more. Here, the water peeling adhesive strength reduction rate B is calculated by the following formula: (1-(N2 / N0))×100; from the water peeling strength N2 [N / 10mm] and adhesive strength (normal adhesive strength) N0 [N / 10mm] measured at a test temperature of 23°C using a tensile tester at a tensile speed of 300mm / min and a peel angle of 180°, after the adhesive surface is attached to a surface of an alkali glass plate prepared by the float method as an adherend, with a contact angle to distilled water of 5° to 10°, at room temperature for 1 day, dropping 20μL of distilled water onto the adherend, and allowing the distilled water to penetrate into one end of the interface between the adhesive layer and the adherend, in accordance with JIS Z0237:2009, 10.4.1, Method 1: 180° peeling adhesive strength against a test plate. This adhesive sheet can achieve both good adhesive strength and water peelability leading to reworkability. The normal adhesive strength N0 and the water peel strength N2 are specifically measured by the method described in the Examples below.
[0020] The thickness of the pressure-sensitive adhesive layer may be, for example, from 10 μm to 200 μm. A pressure-sensitive adhesive layer having such a thickness can exhibit a preferable adhesive strength in optical applications.
[0021] Also, according to this specification, there is provided an optical member with a pressure-sensitive adhesive sheet, comprising any one of the pressure-sensitive adhesive sheets disclosed herein and an optical member bonded to one surface of the pressure-sensitive adhesive sheet. Such an optical member with a pressure-sensitive adhesive sheet can have good reworkability, for example, when the pressure-sensitive adhesive sheet is bonded to the optical member. For example, when a defect such as a foreign object being caught during the bonding occurs, the pressure-sensitive adhesive sheet can be easily peeled off from the optical member using an aqueous liquid such as water and re-bonded. Furthermore, the optical member with a pressure-sensitive adhesive sheet can have sufficient adhesion reliability after bonding with the pressure-sensitive adhesive sheet.
[0022] Furthermore, according to this specification, a method for peeling a pressure-sensitive adhesive sheet attached to an adherend from the adherend is provided. The method may include a water peeling step of peeling the pressure-sensitive adhesive sheet from the adherend while advancing the intrusion of the aqueous liquid into the interface in accordance with the movement of the peel front, in a state where an aqueous liquid is present at the interface between the adherend and the pressure-sensitive adhesive sheet at the peel front of the pressure-sensitive adhesive sheet from the adherend. Here, the peel front refers to a location where the pressure-sensitive adhesive sheet starts to separate from the adherend when the peeling of the pressure-sensitive adhesive sheet from the adherend progresses. According to the water peeling step, the aqueous liquid can be effectively used to peel the pressure-sensitive adhesive sheet from the adherend. The pressure-sensitive adhesive sheet peeled by applying the peeling method disclosed herein typically includes an adhesive layer. The pressure-sensitive adhesive sheet may be, for example, any of the pressure-sensitive adhesive sheets disclosed herein.
[0023] In addition, any suitable combination of the above-mentioned elements may also be included within the scope of the invention for which patent protection is sought through this patent application. [Brief description of the drawings]
[0024] [Figure 1] 1 is a cross-sectional view illustrating a schematic configuration of a pressure-sensitive adhesive sheet according to an embodiment. [Diagram 2] FIG. 4 is a cross-sectional view illustrating a schematic configuration of a pressure-sensitive adhesive sheet according to another embodiment. [Diagram 3]1 is a cross-sectional view showing a schematic diagram of an optical member with a pressure-sensitive adhesive sheet in which the pressure-sensitive adhesive sheet according to one embodiment is attached to an optical member. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] A preferred embodiment of the present invention will be described below. Note that matters other than those specifically mentioned in this specification and necessary for carrying out the present invention can be understood by a person skilled in the art based on the teachings on carrying out the invention described in this specification and the common general knowledge at the time of filing. The present invention can be carried out based on the contents disclosed in this specification and the common general knowledge in the field. In addition, in the following drawings, components and parts having the same function may be described by using the same reference numerals, and duplicated descriptions may be omitted or simplified. In addition, the embodiments described in the drawings are schematic in order to clearly explain the present invention, and do not necessarily accurately represent the size or scale of the product actually provided.
[0026] In this specification, "acrylic polymer" refers to a polymer derived from a monomer component containing more than 50% by weight of an acrylic monomer, and is also called an acrylic polymer. The acrylic monomer refers to a monomer derived from a monomer having at least one (meth)acryloyl group in one molecule. In addition, in this specification, "(meth)acryloyl" refers to acryloyl and methacryloyl in a comprehensive sense. Similarly, "(meth)acrylate" refers to acrylate and methacrylate, and "(meth)acrylic" refers to acrylic and methacrylic in a comprehensive sense.
[0027] <Adhesive composition> The pressure-sensitive adhesive composition disclosed herein contains an acrylic polymer. Typically, the pressure-sensitive adhesive composition may be an acrylic pressure-sensitive adhesive composition containing an acrylic polymer as a main component. The acrylic pressure-sensitive adhesive composition has excellent transparency and is preferably used for optical applications.
[0028] The adhesive composition disclosed herein preferably contains, for example, an acrylic polymer as a base polymer, which is composed of monomer components containing 40% by weight or more of (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 20 carbon atoms at the ester terminal. Hereinafter, the (meth)acrylic acid alkyl ester having an alkyl group having a carbon number of X to Y at the ester terminal is referred to as "(meth)acrylic acid C X-Y Since it is easy to balance the properties, (meth)acrylic acid C is preferably used as the monomer component of the acrylic polymer according to one embodiment. 1-20 The proportion of alkyl ester is suitably more than 50% by weight, and may be, for example, 55% by weight or more, 60% by weight or more, or 70% by weight or more. For the same reason, the proportion of (meth)acrylic acid C among the monomer components is preferably 50% by weight or more, and more preferably 55% by weight or more, more preferably 60% by weight or more, or more preferably 70% by weight or more. 1-20 The proportion of alkyl esters may be, for example, 99.9% by weight or less, 99.5% by weight or less, or 99% by weight or less. 1-20 The proportion of the (meth)acrylic acid alkyl ester may be, for example, 98% by weight or less, or from the standpoint of improving the cohesiveness of the adhesive layer, 95% by weight or less, 85% by weight or less (for example, less than 80% by weight), 70% by weight or less, or 60% by weight or less.
[0029] (Meth)acrylic acid C 1-20Non-limiting examples of alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl ... and isopropyl (meth)acrylate. Examples of such acrylates include isooctyl, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.
[0030] Among these, at least (meth)acrylic acid C 4-20 It is preferable to use an alkyl ester, and at least (meth)acrylic acid C 4-18 It is more preferable to use an alkyl ester. For example, it is preferable to include one or both of n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA) as the monomer component, and an acrylic adhesive containing at least 2EHA is particularly preferable. 4-20 Other examples of alkyl esters include isononyl acrylate, n-butyl methacrylate (BMA), 2-ethylhexyl methacrylate (2EHMA), isostearyl acrylate (iSTA), and the like.
[0031] In some embodiments, the monomer component constituting the acrylic polymer is (meth)acrylic acid C 4-18 The monomer component may contain 40% by weight or more of alkyl ester. 4-18The proportion of the alkyl ester may be, for example, 50% by weight or more, 60% by weight or more, or 65% by weight or more. 6-18 The monomer component may include an alkyl ester. In addition, from the viewpoint of enhancing the cohesiveness of the adhesive layer, (meth)acrylic acid C in the monomer components 4-18 The proportion of the alkyl ester is usually 99.5% by weight or less, and may be 95% by weight or less, 85% by weight or less, or 75% by weight or less. 6-18 The monomer component may include an alkyl ester.
[0032] The monomer components constituting the acrylic polymer may contain, as necessary, other monomers (copolymerizable monomers) that are copolymerizable with the (meth)acrylic acid alkyl ester, together with the (meth)acrylic acid alkyl ester. As the copolymerizable monomer, a monomer having a polar group (e.g., a carboxyl group, a hydroxyl group, a nitrogen atom-containing ring, etc.) or a monomer having a relatively high homopolymer glass transition temperature (e.g., 10°C or higher) can be suitably used. The monomer having a polar group can be useful for introducing a crosslinking point into the acrylic polymer or for increasing the cohesive strength of the adhesive. The copolymerizable monomers can be used alone or in combination of two or more.
[0033] Non-limiting examples of copolymerizable monomers include the following: Carboxy group-containing monomers: for example, acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, isocrotonic acid, and the like. Acid anhydride group-containing monomers: for example, maleic anhydride, itaconic anhydride. Hydroxyl group-containing monomers: for example, hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate. Monomers containing a sulfonic acid group or a phosphoric acid group: for example, styrene sulfonic acid, allyl sulfonic acid, sodium vinyl sulfonate, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, (meth)acryloyloxynaphthalenesulfonic acid, 2-hydroxyethyl acryloyl phosphate, etc. Epoxy group-containing monomers: for example, epoxy group-containing acrylates such as glycidyl (meth)acrylate and 2-ethyl glycidyl ether (meth)acrylate, allyl glycidyl ether, and glycidyl ether (meth)acrylate. Cyano group-containing monomers: for example, acrylonitrile, methacrylonitrile, etc. Isocyanate group-containing monomers: for example, 2-isocyanatoethyl (meth)acrylate. Amide group-containing monomers: for example, (meth)acrylamide; N,N-dialkyl(meth)acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, and N,N-di(t-butyl)(meth)acrylamide; N-alkyl(meth)acrylamides such as N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-butyl(meth)acrylamide, and Nn-butyl(meth)acrylamide; N-vinyl carboxylic acid amides such as N-vinylacetamide; monomers having a hydroxyl group and an amide group, for example, N-(2-hydroxyethyl)(meth)acrylamide; N-hydroxyalkyl (meth)acrylamides such as N-(2-hydroxypropyl) (meth)acrylamide, N-(1-hydroxypropyl) (meth)acrylamide, N-(3-hydroxypropyl) (meth)acrylamide, N-(2-hydroxybutyl) (meth)acrylamide, N-(3-hydroxybutyl) (meth)acrylamide, and N-(4-hydroxybutyl) (meth)acrylamide; monomers having an alkoxy group and an amide group, for example, N-alkoxyalkyl (meth)acrylamide such as N-methoxymethyl (meth)acrylamide, N-methoxyethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide; and others, N,N-dimethylaminopropyl (meth)acrylamide, N-(meth)acryloylmorpholine, and the like. Amino group-containing monomers: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, t-butylaminoethyl (meth)acrylate. Monomers having an epoxy group: for example, glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, allyl glycidyl ether. Monomers having a nitrogen atom-containing ring: for example, N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-vinylmorpholine, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, N-vinylpyrazole, N-vinylisoxazole, N-vinylthiazole, N-vinylisothiazole, N-vinylpyridazine, etc. (for example, lactams such as N-vinyl-2-caprolactam). Monomers having a succinimide skeleton: for example, N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, N-(meth)acryloyl-8-oxyhexamethylene succinimide, and the like. Maleimides: for example, N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, N-phenylmaleimide, and the like. Itaconimides: for example, N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, N-laurylitaconimide, and the like. Aminoalkyl (meth)acrylates: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate. Alkoxy group-containing monomers: for example, alkoxyalkyl (meth)acrylates (alkoxyalkyl (meth)acrylates) such as 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, and ethoxypropyl (meth)acrylate; alkoxyalkylene (meth)acrylates (for example, alkoxypolyalkylene glycol (meth)acrylates) such as methoxyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, and methoxypolypropylene glycol (meth)acrylate. Alkoxysilyl group-containing monomers: for example, alkoxysilyl group-containing (meth)acrylates such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane; alkoxysilyl group-containing vinyl compounds such as vinyltrimethoxysilane and vinyltriethoxysilane; and the like. Vinyl esters: for example, vinyl acetate, vinyl propionate, etc. Vinyl ethers: for example, vinyl alkyl ethers such as methyl vinyl ether and ethyl vinyl ether. Aromatic vinyl compounds: for example, styrene, α-methylstyrene, vinyltoluene, etc. Olefins: For example, ethylene, butadiene, isoprene, isobutylene, etc. (Meth)acrylic acid esters having an alicyclic hydrocarbon group: for example, (meth)acrylates containing an alicyclic hydrocarbon group such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and adamantyl (meth)acrylate. (Meth)acrylic acid esters having an aromatic hydrocarbon group: for example, (meth)acrylates containing an aromatic hydrocarbon group such as phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, and benzyl (meth)acrylate. Other examples include heterocyclic ring-containing (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate, halogen atom-containing (meth)acrylates such as vinyl chloride and fluorine atom-containing (meth)acrylates, silicon atom-containing (meth)acrylates such as silicone (meth)acrylate, and (meth)acrylic acid esters obtained from alcohols derived from terpene compounds.
[0034] When such a copolymerizable monomer is used, the amount of the copolymerizable monomer is not particularly limited, but is usually appropriate to be 0.01% by weight or more of the total monomer components. From the viewpoint of better exerting the effect of using the copolymerizable monomer, the amount of the copolymerizable monomer may be 0.1% by weight or more of the total monomer components, or may be 0.5% by weight or more. Also, from the viewpoint of easily balancing the adhesive properties, the amount of the copolymerizable monomer is usually appropriate to be 50% by weight or less of the total monomer components, and preferably 40% by weight or less.
[0035] In some embodiments, the monomer component constituting the acrylic polymer may contain a monomer having a nitrogen atom. This can increase the cohesive strength of the adhesive and favorably improve the peel strength after aging. A suitable example of the monomer having a nitrogen atom is a monomer having a nitrogen atom-containing ring. As the monomer having a nitrogen atom-containing ring, those exemplified above can be used, and for example, a monomer represented by the general formula (1): [ka] In the general formula (1), R 1 is a divalent organic group, specifically -(CH2) n -. n is an integer of 2 to 7 (preferably 2, 3 or 4). Among them, N-vinyl-2-pyrrolidone can be preferably used. Another suitable example of the monomer having a nitrogen atom is (meth)acrylamide.
[0036] The amount of the monomer having a nitrogen atom (preferably a monomer having a nitrogen atom-containing ring) used is not particularly limited, and may be, for example, 1% by weight or more, 3% by weight or more, or even 5% by weight or more or 7% by weight or more of the entire monomer components. In one embodiment, the amount of the monomer having a nitrogen atom used may be 10% by weight or more, 15% by weight or more, or 20% by weight or more of the entire monomer components from the viewpoint of improving adhesive strength. In addition, the amount of the monomer having a nitrogen atom used is suitably, for example, 40% by weight or less of the entire monomer components, and may be 35% by weight or less, 30% by weight or less, or 25% by weight or less. In another embodiment, the amount of the monomer having a nitrogen atom used may be, for example, 20% by weight or less, or 15% by weight or less of the entire monomer components.
[0037] In some embodiments, the monomer components constituting the acrylic polymer may include a hydroxyl group-containing monomer. The use of the hydroxyl group-containing monomer may suitably adjust the cohesive strength of the adhesive and the degree of crosslinking (for example, crosslinking by an isocyanate crosslinking agent). The amount of the hydroxyl group-containing monomer used is not particularly limited, and may be, for example, 0.01% by weight or more of the total monomer components, 0.1% by weight or more, 0.5% by weight or more, 1% by weight or more, 5% by weight or more, or 10% by weight or more. In addition, from the viewpoint of suppressing the water absorption of the adhesive layer, in some embodiments, the amount of the hydroxyl group-containing monomer used is suitably, for example, 40% by weight or less of the total monomer components, and may be 30% by weight or less, 25% by weight or less, or 20% by weight or less. In another embodiment, the amount of the hydroxyl group-containing monomer used may be, for example, 15% by weight or less, 10% by weight or less, or 5% by weight or less of the total monomer components.
[0038] In the adhesive composition disclosed herein, the monomer component of the acrylic polymer may or may not contain the alkoxyalkyl(meth)acrylate or alkoxypolyalkylene glycol (meth)acrylate exemplified above. In one embodiment of the technology disclosed herein, the proportion of alkoxyalkyl(meth)acrylate among the monomer components of the acrylic polymer is less than 20% by weight, and the proportion of alkoxypolyalkylene glycol (meth)acrylate is less than 20% by weight. This makes it easy to form the adhesive layer into a sheet without problems such as gelation. By employing the above monomer composition, the solids concentration of the monomer mixture can be maintained within a predetermined range, and a desired high molecular weight substance (for example, a weight average molecular weight (Mw) of 30×10 can be obtained. 4 Over, typically Mw40×10 4 or more) can be preferably polymerized. The proportion of alkoxyalkyl (meth)acrylate in the above monomer component is preferably less than 10% by weight, more preferably less than 3% by weight, and even more preferably less than 1% by weight, and in a particularly preferred embodiment, the above monomer component does not substantially contain alkoxyalkyl (meth)acrylate (content: 0 to 0.3% by weight). Similarly, the proportion of alkoxypolyalkylene glycol (meth)acrylate in the above monomer component is preferably less than 10% by weight, more preferably less than 3% by weight, and even more preferably less than 1% by weight, and in a particularly preferred embodiment, the above monomer component does not substantially contain alkoxypolyalkylene glycol (meth)acrylate (content: 0 to 0.3% by weight).
[0039] In addition, in the monomer component of the acrylic polymer according to a preferred embodiment, the total ratio of alkoxyalkyl (meth)acrylate and alkoxypolyalkylene glycol (meth)acrylate is limited to less than 20% by weight from the viewpoint of suppressing gelation. The total ratio of the alkoxyalkyl (meth)acrylate and alkoxypolyalkylene glycol (meth)acrylate is more preferably less than 10% by weight, even more preferably less than 3% by weight, and particularly preferably less than 1% by weight. In one embodiment, the monomer component does not substantially contain alkoxyalkyl (meth)acrylate and alkoxypolyalkylene glycol (meth)acrylate (content 0 to 0.3% by weight). Similarly, the monomer component of the acrylic polymer disclosed herein may contain less than 20% by weight of an alkoxy group-containing monomer, or may contain no alkoxy group-containing monomer. The amount of the alkoxy group-containing monomer in the monomer component is preferably less than 10% by weight, more preferably less than 3% by weight, and even more preferably less than 1% by weight. In a particularly preferred embodiment, the monomer component is substantially free of an alkoxy group-containing monomer (content of 0 to 0.3% by weight).
[0040] In some embodiments, the ratio of the carboxyl group-containing monomer in the monomer components of the acrylic polymer may be, for example, 2% by weight or less, 1% by weight or less, or 0.5% by weight or less (for example, less than 0.1% by weight). The acrylic polymer may not substantially use a carboxyl group-containing monomer as a monomer component. Here, substantially not using a carboxyl group-containing monomer means that at least intentionally not using a carboxyl group-containing monomer. An acrylic polymer having such a composition is likely to have high water resistance and high reliability, and may have metal corrosion prevention properties for adherends containing metal.
[0041] In a preferred embodiment, the ratio of the hydrophilic monomer in the monomer component of the acrylic polymer is limited. This allows the water peelability of the compound A to be preferably exhibited. Here, the "hydrophilic monomer" in this specification refers to a carboxyl group-containing monomer, an acid anhydride group-containing monomer, a hydroxyl group-containing monomer, a monomer having a nitrogen atom (typically, an amide group-containing monomer such as (meth)acrylamide, a monomer having a nitrogen atom-containing ring such as N-vinyl-2-pyrrolidone), and an alkoxy group-containing monomer (typically, an alkoxyalkyl (meth)acrylate and an alkoxypolyalkylene glycol (meth)acrylate). In this embodiment, the ratio of the hydrophilic monomer in the monomer component of the acrylic polymer is suitably 40% by weight or less (e.g., 35% by weight or less), preferably 32% by weight or less, for example, 30% by weight or less, or 28% by weight or less. Although not particularly limited, the ratio of the hydrophilic monomer in the monomer component of the acrylic polymer may be 1% by weight or more, 10% by weight or more, or 20% by weight or more.
[0042] In some embodiments, the monomer component constituting the acrylic polymer may contain an alicyclic hydrocarbon group-containing (meth)acrylate. This can increase the cohesive strength of the adhesive and improve the peel strength after aging. As the alicyclic hydrocarbon group-containing (meth)acrylate, the above-mentioned examples can be used, and for example, cyclohexyl acrylate and isobornyl acrylate can be preferably used. When an alicyclic hydrocarbon group-containing (meth)acrylate is used, the amount used is not particularly limited, and can be, for example, 1% by weight or more, 3% by weight or more, or 5% by weight or more of the entire monomer component. In one embodiment, the amount used of the alicyclic hydrocarbon group-containing (meth)acrylate may be 10% by weight or more, or 15% by weight or more of the entire monomer component. The upper limit of the amount used of the alicyclic hydrocarbon group-containing (meth)acrylate is suitably about 40% by weight or less, and may be, for example, 30% by weight or less, or 25% by weight or less (for example, 15% by weight or less, or even 10% by weight or less).
[0043] The composition of the monomer components constituting the acrylic polymer may be set so that the glass transition temperature Tg calculated by the Fox formula based on the composition of the monomer components is −75° C. or more and 10° C. or less. In some embodiments, the Tg is suitably 0° C. or less, preferably −10° C. or less, and may be −20° C. or less or −30° C. or less, from the viewpoint of cohesiveness, impact resistance, and the like. The Tg may be, for example, −60° C. or more, −50° C. or more, −45° C. or more, or −40° C. or more.
[0044] Here, the Fox formula is a relational expression between the Tg of a copolymer and the glass transition temperature Tgi of a homopolymer obtained by homopolymerizing each of the monomers constituting the copolymer, as shown below. 1 / Tg=Σ(Wi / Tgi) In the above Fox formula, Tg represents the glass transition temperature (unit: K) of the copolymer, Wi represents the weight fraction of monomer i in the copolymer (copolymerization ratio on a weight basis), and Tgi represents the glass transition temperature (unit: K) of the homopolymer of monomer i.
[0045] The glass transition temperature of the homopolymer used to calculate Tg is a value described in a publicly known document. For example, for the monomers listed below, the following values are used as the glass transition temperatures of the homopolymers of the monomers. 2-Ethylhexyl acrylate -70℃ n-Butyl acrylate -55℃ Isostearyl acrylate -18℃ Methyl methacrylate 105℃ Methyl acrylate 8℃ Cyclohexyl acrylate 15℃ N-vinyl-2-pyrrolidone 54℃ 2-Hydroxyethyl acrylate -15℃ 4-Hydroxybutyl acrylate -40℃ Dicyclopentanyl methacrylate 175℃ Isobornyl acrylate 94℃ Acrylic acid 106℃ Methacrylic acid 228℃
[0046] For the glass transition temperatures of homopolymers of monomers other than those listed above, the values given in "Polymer Handbook" (3rd Edition, John Wiley & Sons, Inc., 1989) shall be used. When multiple values are given in this document, the highest value shall be used.
[0047] For monomers for which the glass transition temperature of the homopolymer is not described in the Polymer Handbook, the value obtained by the following measurement method shall be used (see JP 2007-51271 A). Specifically, 100 parts by weight of monomer, 0.2 parts by weight of azobisisobutyronitrile, and 200 parts by weight of ethyl acetate as a polymerization solvent are charged into a reactor equipped with a thermometer, a stirrer, a nitrogen inlet tube, and a reflux condenser, and stirred for 1 hour while passing nitrogen gas through. After removing oxygen from the polymerization system in this way, the temperature is raised to 63°C and reacted for 10 hours. Then, the mixture is cooled to room temperature to obtain a homopolymer solution with a solid concentration of 33% by weight. Then, the homopolymer solution is cast and applied onto a release liner, and dried to prepare a test sample (sheet-shaped homopolymer) with a thickness of about 2 mm. This test sample was punched out into a disk with a diameter of 7.9 mm, sandwiched between parallel plates, and subjected to a shear strain of 1 Hz using a viscoelasticity tester (ARES, Rheometrics Corporation). Viscoelasticity was measured in shear mode at a temperature range of -70 to 150°C and a heating rate of 5°C / min. The peak top temperature of tan δ was taken as the Tg of the homopolymer.
[0048] The acrylic polymer disclosed herein is not particularly limited, but has an SP value of 23.0 (MJ / m 3 ) 1 / 2It is preferable that the SP value is 21.0 (MJ / m or less). By adding the compound A described below to an adhesive containing an acrylic polymer having such an SP value, it is possible to preferably realize an adhesive having sufficient adhesive strength and excellent water peelability. The above SP value is more preferably 21.0 (MJ / m 3 ) 1 / 2 Less than or equal to (e.g. 20.0(MJ / m 3 ) 1 / 2 The lower limit of the SP value is not particularly limited, and is, for example, about 10.0 (MJ / m 3 ) 1 / 2 More than 15.0 (MJ / m 3 ) 1 / 2 It is appropriate that the concentration is equal to or higher than 18.0 (MJ / m 3 ) 1 / 2 That's all.
[0049] The SP value of an acrylic polymer is calculated by the Fedors calculation method [see Polymer Engineering and Science, Vol. 14, No. 2 (1974), pp. 148-154], that is, the formula: SP value δ = (Σ△e / Σ△v) 1 / 2 (where Δe is the vaporization energy Δe of each atom or atomic group at 25° C., and Δv is the molar volume of each atom or atomic group at the same temperature.); The acrylic polymer having the above SP value can be obtained by appropriately determining the monomer composition based on the technical common sense of a person skilled in the art.
[0050] The above-mentioned adhesive composition is an adhesive composition containing the monomer components having the above-mentioned composition in the form of a polymer, an unpolymer (i.e., a form in which the polymerizable functional group is unreacted) or a mixture thereof, and further containing compound A. The above-mentioned adhesive composition may be in various forms, such as a water-dispersed adhesive composition in the form in which an adhesive (adhesive component) is dispersed in water, a solvent-type adhesive composition in the form in which an adhesive is contained in an organic solvent, an active energy ray-curable adhesive composition prepared to be cured by active energy rays such as ultraviolet rays or radiation to form an adhesive, and a hot melt type adhesive composition that is applied in a heated and molten state and forms an adhesive when cooled to around room temperature. A preferred adhesive composition is a solvent-type adhesive composition or a solventless type adhesive composition. Solventless type adhesive compositions include active energy ray-curable adhesive compositions and hot melt type adhesive compositions.
[0051] In the polymerization, a known or commonly used thermal polymerization initiator or photopolymerization initiator may be used depending on the polymerization method, polymerization mode, etc. Such polymerization initiators may be used alone or in appropriate combination of two or more.
[0052] The thermal polymerization initiator is not particularly limited, and examples thereof include azo polymerization initiators, peroxide initiators, redox initiators formed by combining peroxides with reducing agents, and substituted ethane initiators. More specifically, examples thereof include 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2-methylpropionamidine) disulfate, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis(N,N'-dimethyleneisobutylamidine), 2,2'-azobis[N-(2-carboxyethyl)-2- Examples of initiators include, but are not limited to, azo initiators such as methylpropionamidine hydrate; persulfates such as potassium persulfate and ammonium persulfate; peroxide initiators such as benzoyl peroxide, t-butyl hydroperoxide, and hydrogen peroxide; substituted ethane initiators such as phenyl-substituted ethane; redox initiators such as a combination of a persulfate and sodium hydrogen sulfite, and a combination of a peroxide and sodium ascorbate. Thermal polymerization can be preferably carried out at a temperature of, for example, about 20 to 100°C (typically 40 to 80°C).
[0053] The photopolymerization initiator is not particularly limited, but examples of the photopolymerization initiator that can be used include ketal-based photopolymerization initiators, acetophenone-based photopolymerization initiators, benzoin ether-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, α-ketol-based photopolymerization initiators, aromatic sulfonyl chloride-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzyl-based photopolymerization initiators, benzophenone-based photopolymerization initiators, and thioxanthone-based photopolymerization initiators.
[0054] The amount of such a thermal polymerization initiator or photopolymerization initiator used is not particularly limited and may be a normal amount depending on the polymerization method, polymerization mode, etc. For example, about 0.001 to 5 parts by weight (typically about 0.01 to 2 parts by weight, for example about 0.01 to 1 part by weight) of the polymerization initiator can be used relative to 100 parts by weight of the monomer to be polymerized.
[0055] In the above polymerization, various conventionally known chain transfer agents (which may also be understood as molecular weight regulators or polymerization degree regulators) may be used as necessary. As the chain transfer agent, mercaptans such as n-dodecyl mercaptan, t-dodecyl mercaptan, thioglycolic acid, and α-thioglycerol may be used. Alternatively, a chain transfer agent that does not contain a sulfur atom (non-sulfur chain transfer agent) may be used. Specific examples of non-sulfur chain transfer agents include anilines such as N,N-dimethylaniline and N,N-diethylaniline; terpenoids such as α-pinene and terpinolene; styrenes such as α-methylstyrene and α-methylstyrene dimer; compounds having a benzylidenyl group such as dibenzylideneacetone, cinnamyl alcohol, and cinnamylaldehyde; hydroquinones such as hydroquinone and naphthohydroquinone; quinones such as benzoquinone and naphthoquinone; olefins such as 2,3-dimethyl-2-butene and 1,5-cyclooctadiene; alcohols such as phenol, benzyl alcohol, and allyl alcohol; and benzyl hydrogens such as diphenylbenzene and triphenylbenzene. The chain transfer agent can be used alone or in combination of two or more. When using a chain transfer agent, the amount of the agent can be, for example, about 0.01 to 1 part by weight based on 100 parts by weight of the monomer component. The technology disclosed herein can also be preferably implemented in an embodiment in which no chain transfer agent is used.
[0056] The molecular weight of the acrylic polymer obtained by appropriately adopting the above-mentioned various polymerization methods is not particularly limited and can be set in an appropriate range according to the required performance. The weight average molecular weight (Mw) of the acrylic polymer is usually about 10 × 10 4 or more (e.g. 20×10 4 From the viewpoint of achieving a good balance between cohesive strength and adhesive strength, 4 In order to obtain good adhesion reliability even in a high-temperature environment, the acrylic polymer according to one embodiment has a viscosity of preferably 40×10 4 or more (typically about 50×10 4For example, approximately 55 x 10 4 According to a preferred embodiment of the technology disclosed herein, gelation can be suppressed by designing the monomer composition, so that a high molecular weight polymer in the above range can be obtained with good productivity by setting an appropriate solid content concentration. The upper limit of the Mw of the acrylic polymer is usually about 500×10 4 Less than (for example, about 150 x 10 4 The Mw can be about 75×10 4 or less. Here, Mw refers to a value calculated in terms of standard polystyrene obtained by gel permeation chromatography (GPC). As a GPC device, for example, a model named "HLC-8320GPC" (column: TSKgelGMH-H(S), manufactured by Tosoh Corporation) may be used. The same applies to the examples described later. The above Mw may be the Mw of an acrylic polymer in either the pressure-sensitive adhesive composition or the pressure-sensitive adhesive layer.
[0057] The adhesive composition according to some embodiments may be an active energy ray curable adhesive composition containing compound A. In the present specification, the term "active energy ray" refers to an energy ray having energy capable of inducing a chemical reaction such as a polymerization reaction, a crosslinking reaction, or decomposition of an initiator. Examples of the active energy ray include light such as ultraviolet light, visible light, and infrared light, and radiation such as α-rays, β-rays, γ-rays, electron beams, neutron beams, and X-rays. A suitable example of the active energy ray curable adhesive composition is a photocurable adhesive composition. The photocurable adhesive composition has the advantage that even a thick adhesive layer can be easily formed. Among them, an ultraviolet ray curable adhesive composition is preferred.
[0058] Typically, the photocurable pressure-sensitive adhesive composition contains at least a part of the monomer components of the composition (which may be a part of the type of monomer or a part of the amount) in the form of a polymer. The polymerization method for forming the polymer is not particularly limited, and various conventionally known polymerization methods can be appropriately adopted. For example, thermal polymerization such as solution polymerization, emulsion polymerization, and bulk polymerization (typically carried out in the presence of a thermal polymerization initiator); photopolymerization carried out by irradiating with light such as ultraviolet rays (typically carried out in the presence of a photopolymerization initiator); radiation polymerization carried out by irradiating with radiation such as β rays and γ rays; and the like can be appropriately adopted. Among them, photopolymerization is preferred.
[0059] A photocurable pressure-sensitive adhesive composition according to a preferred embodiment includes a partial polymer of a monomer component. Such a partial polymer is typically a mixture of a polymer derived from a monomer component and an unreacted monomer, and is preferably in a syrup state (viscous liquid state). Hereinafter, a partial polymer of such a nature may be referred to as a "monomer syrup" or simply as a "syrup". The polymerization method for partially polymerizing the monomer component is not particularly limited, and various polymerization methods as described above can be appropriately selected and used. From the viewpoint of efficiency and simplicity, a photopolymerization method can be preferably adopted. According to photopolymerization, the polymerization conversion rate of the monomer component (monomer conversion) can be easily controlled by the polymerization conditions such as the amount of light irradiation (light amount).
[0060] The polymerization conversion rate of the monomer mixture in the partial polymer is not particularly limited. The polymerization conversion rate can be, for example, about 70% by weight or less, and is preferably about 60% by weight or less. From the viewpoint of ease of preparation and coatability of the pressure-sensitive adhesive composition containing the partial polymer, the polymerization conversion rate is usually appropriate to be about 50% by weight or less, and is preferably about 40% by weight or less (for example, about 35% by weight or less). The lower limit of the polymerization conversion rate is not particularly limited, but is typically about 1% by weight or more, and is usually appropriate to be about 5% by weight or more.
[0061] The adhesive composition containing the partial polymer of the monomer component can be obtained, for example, by partially polymerizing a monomer mixture containing the entire amount of the monomer component used in the preparation of the adhesive composition by an appropriate polymerization method (for example, photopolymerization method). The adhesive composition containing the partial polymer of the monomer component may be a mixture of a partial polymer or a complete polymer of a monomer mixture containing a part of the monomer component used in the preparation of the adhesive composition, and the remaining monomer component or a partial polymer thereof. In this specification, the term "complete polymer" refers to a polymerization conversion rate of more than 95% by weight.
[0062] The pressure-sensitive adhesive composition containing the partial polymer may contain, in addition to the peel strength increasing agent, other components used as necessary (e.g., a photopolymerization initiator, a crosslinking agent as described below, a polyfunctional monomer, an acrylic oligomer, a tackifier resin, etc.) The method of blending such other components is not particularly limited, and for example, they may be contained in the monomer mixture in advance, or may be added to the partial polymer.
[0063] The pressure-sensitive adhesive composition according to some embodiments may be a solvent-based pressure-sensitive adhesive composition containing compound A. The solvent-based pressure-sensitive adhesive composition typically contains a solution polymer of a monomer component, compound A, and an additive (e.g., a peel strength increasing agent) that is used as needed. The solvent (polymerization solvent) used in the solution polymerization can be appropriately selected from conventionally known organic solvents. For example, any one solvent selected from aromatic compounds such as toluene (typically aromatic hydrocarbons); esters such as ethyl acetate and butyl acetate; aliphatic or alicyclic hydrocarbons such as hexane and cyclohexane; halogenated alkanes such as 1,2-dichloroethane; lower alcohols such as isopropyl alcohol (e.g., monohydric alcohols having 1 to 4 carbon atoms); ethers such as tert-butyl methyl ether; ketones such as methyl ethyl ketone; and the like, or a mixed solvent of two or more of them can be used. According to the solution polymerization, a polymerization reaction liquid in the form of a polymer of a monomer component dissolved in a polymerization solvent is obtained. The solvent-based pressure-sensitive adhesive composition disclosed herein can be preferably produced using the above-mentioned polymerization reaction liquid.
[0064] The above-mentioned solvent-based pressure-sensitive adhesive composition may contain other components (e.g., a photopolymerization initiator, a crosslinking agent as described below, a polyfunctional monomer, an acrylic oligomer, etc.) that are used as necessary, in addition to the compound A. The above-mentioned solvent-based pressure-sensitive adhesive composition may be provided with photocurability (photocrosslinkability), for example, by adding a polyfunctional monomer and a photopolymerization initiator to the above-mentioned polymerization reaction liquid.
[0065] (Compound A) The adhesive composition disclosed herein may typically be characterized by including at least one compound A selected from a surfactant and a compound having a polyoxyalkylene skeleton. This allows the peeling force to be effectively reduced by utilizing an aqueous liquid such as water. The reason for this is not particularly limited, but it is believed that both the surfactant and the compound having a polyoxyalkylene skeleton have a hydrophilic region, which allows them to be unevenly distributed on the surface of the adhesive layer and effectively reduce the peeling force when they come into contact with water. As the surfactant and the compound having a polyoxyalkylene skeleton, one or more of known surfactants and compounds having a polyoxyalkylene skeleton can be used without any particular restrictions. Typically, it is preferable that the compound A is contained in the adhesive composition (and thus the adhesive layer) in a free form. As the compound A, a compound that is liquid at room temperature (about 25°C) is preferably used from the viewpoint of the preparation of the adhesive composition. It goes without saying that among the above surfactants, there are compounds having a polyoxyalkylene skeleton, and vice versa.
[0066] The HLB of compound A (typically a surfactant) is not particularly limited, and may be, for example, 3 or more, suitably about 6 or more, and may be 8 or more (e.g., 9 or more). In a preferred embodiment, the HLB of compound A is 10 or more. This tends to favorably express water peelability. The above HLB is more preferably 11 or more, even more preferably 12 or more, and particularly preferably 13 or more (e.g., 14 or more, 15 or more, or even 16 or more). Compound A having an HLB in the above range is subjected to a polymerization reaction with an SP value of 23.0 (MJ / m 3 )1 / 2 Less than or equal to (e.g. 18.0 to 23.0 (MJ / m 3 By incorporating the acrylic polymer in the pressure-sensitive adhesive composition (and thus the pressure-sensitive adhesive layer), water peelability can be more effectively exhibited. The upper limit of the HLB is 20 or less, and may be, for example, 18 or less, or 16 or less (for example, 15 or less).
[0067] In this specification, HLB is the hydrophile-lipophile balance according to Griffin, which is a value indicating the degree of affinity of a surfactant to water or oil, and is a ratio of hydrophilicity to lipophilicity expressed as a number between 0 and 20. The definition of HLB is as described in WC Griffin: J. Soc. Cosmetic Chemists, 1, 311 (1949), Takahashi Kotami, Namba Yoshiro, Koike Motoo, and Kobayashi Masao, "Surfactant Handbook", 3rd Edition, Kogaku Toshosha Publishing, November 25, 1972, pp. 179-182, etc. Compound A having the above HLB can be selected based on the technical common sense of a person skilled in the art, by referring to the above reference literature as necessary.
[0068] As the surfactant that can be used as compound A, known nonionic surfactants, anionic surfactants, cationic surfactants, etc. can be used. Among them, nonionic surfactants are preferable. The surfactants can be used alone or in combination of two or more.
[0069] Examples of nonionic surfactants include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, and polyoxyethylene oleyl ether; polyoxyethylene alkyl phenyl ethers such as polyoxyethylene octyl phenyl ether and polyoxyethylene nonyl phenyl ether; sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, and sorbitan monooleate; polyoxyethylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan tristearate, polyoxyethylene sorbitan triisostearate, polyoxyethylene sorbitan monooleate, and polyoxyethylene sorbitan trioleate; polyoxyethylene glyceryl ether fatty acid esters; polyoxyethylene-polyoxypropylene block copolymers; and the like. These nonionic surfactants can be used alone or in combination of two or more.
[0070] Examples of anionic surfactants include alkyl sulfates such as lauryl sulfate and octadecyl sulfate; fatty acid salts; alkyl benzene sulfonates such as nonyl benzene sulfonate and dodecyl benzene sulfonate; naphthalene sulfonates such as dodecyl naphthalene sulfonate; alkyl diphenyl ether disulfonates such as dodecyl diphenyl ether disulfonate; polyoxyethylene alkyl ether sulfates such as polyoxyethylene octadecyl ether sulfate and polyoxyethylene lauryl ether sulfate; polyoxyethylene alkyl phenyl ether sulfates such as polyoxyethylene lauryl phenyl ether sulfate; polyoxyethylene styrenated phenyl ether sulfate; sulfosuccinates such as lauryl sulfosuccinate and polyoxyethylene lauryl sulfosuccinate; polyoxyethylene alkyl ether phosphates; polyoxyethylene alkyl ether acetates; etc. When the anionic surfactant forms a salt, the salt may be, for example, a metal salt (preferably a monovalent metal salt) such as sodium salt, potassium salt, calcium salt, magnesium salt, etc., an ammonium salt, an amine salt, etc. These anionic surfactants can be used alone or in combination of two or more.
[0071] Examples of compounds having a polyoxyalkylene skeleton that can be used as compound A include polyalkylene glycols such as polyethylene glycol (PEG) and polypropylene glycol (PPG); polyethers containing polyoxyethylene units, polyethers containing polyoxypropylene units, compounds containing oxyethylene units and oxypropylene units (these units may be arranged randomly or in blocks); and derivatives thereof. Also, among the above-mentioned surfactants, compounds having a polyoxyalkylene skeleton can be used. These can be used alone or in combination of two or more. Among them, it is preferable to use a compound having a polyoxyethylene skeleton (also called a polyoxyethylene segment), and PEG is more preferable.
[0072] The molecular weight (chemical formula weight) of the compound having a polyoxyalkylene skeleton (e.g., polyethylene glycol) is not particularly limited, and is suitably less than 1000, and from the viewpoint of the preparation of the adhesive composition, is preferably about 600 or less (e.g., 500 or less). The lower limit of the molecular weight of the compound having a polyoxyalkylene skeleton (e.g., polyethylene glycol) is not particularly limited, and those having a molecular weight of about 100 or more (e.g., about 200 or more, further about 300 or more) are preferably used.
[0073] In the pressure-sensitive adhesive composition according to one embodiment, the amount of compound A used can be about 3 parts by weight or less, and is suitably about 2 parts by weight or less, relative to 100 parts by weight of the acrylic polymer (which may be the total amount of monomer components forming the acrylic polymer. The same applies hereinafter unless otherwise specified). From the viewpoint of optical properties such as transparency, the amount is preferably less than 1 part by weight, more preferably less than 0.7 parts by weight, and even more preferably less than 0.3 parts by weight (e.g., less than 0.2 parts by weight). By limiting the amount of compound A used, the adhesive strength tends to be easily maintained. In addition, compound A having an HLB of 10 or more tends to easily exhibit good water peelability even when added in small amounts. In addition, from the viewpoint of exhibiting the effect of adding compound A, the amount of compound A can be 0.001 parts by weight or more, and is suitably, for example, 0.01 parts by weight or more, and is preferably 0.03 parts by weight or more (e.g., 0.1 parts by weight or more) relative to 100 parts by weight of the acrylic polymer. In a composition in which importance is placed on water-removable properties, the amount of compound A relative to 100 parts by weight of the acrylic polymer may be 0.3 parts by weight or more (eg, 0.5 parts by weight or more).
[0074] (peel strength increasing agent) The adhesive composition disclosed herein may contain a peeling force increasing agent. As the peeling force increasing agent, a material capable of increasing the peeling force of the adhesive sheet from the adherend after the surface (adhesive surface) of the adhesive layer formed from the adhesive composition is attached to the adherend can be appropriately selected and used. As the peeling force increasing agent, for example, a known silane coupling agent can be used. The peeling force increasing agent is preferably contained in the adhesive composition (and thus the adhesive layer) in a free form. The peeling force increasing agent is preferably not chemically bonded to other components that may be contained in the adhesive composition (and thus the adhesive layer). The peeling force increasing agent contained in the adhesive composition in such a form can effectively contribute to improving the peeling force.
[0075] A silane coupling agent is typically a compound containing a functional group X and a functional group Y in one molecule, and the functional group X is an alkoxysilyl group. The alkoxysilyl group is a functional group having at least one alkoxy group on a silicon atom. By supplying a silane coupling agent to the surface of the adhesive layer after pasting to an adherend, the silanol group generated by hydrolysis of the alkoxy group reacts with the hydroxyl group on the adherend surface, thereby increasing the peeling force of the adhesive sheet from the adherend. The alkoxysilyl group is hydrolyzed to generate a silanol group that reacts with the hydroxyl group on the adherend surface. Therefore, the alkoxysilyl group is a precursor of the group that reacts with the hydroxyl group.
[0076] The alkoxy group constituting the above alkoxysilyl group is typically a methoxy group or an ethoxy group. Usually, the methoxy group having higher hydrolysis is preferred. The above alkoxysilyl group may be a trialkoxysilyl group or a dialkoxysilyl group. From the viewpoint of enhancing the effect of increasing the peeling force, in some embodiments, the silane coupling agent having a trialkoxysilyl group can be preferably adopted.
[0077] The functional group Y may be, for example, an epoxy group, an amino group, an isocyanate group (which may be in the form of an isocyanurate), an acetoacetyl group, a (meth)acryloyl group, a mercapto group, a vinyl group, a halogenated alkyl group, etc. Examples of silane coupling agents having such a functional group Y include epoxy group-containing silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino group-containing silane coupling agents such as 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)3-aminopropylmethyldimethoxysilane; isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane and tris(trimethoxysilylpropyl)isocyanurate; Containing silane coupling agents; for example, acetoacetyl group-containing silane coupling agents such as acetoacetyl group-containing trimethoxysilane; (meth)acryloyl group-containing silane coupling agents such as 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane; vinyl group-containing silane coupling agents such as vinyltrimethoxysilane, vinyltriethoxysilane; mercapto group-containing silane coupling agents such as 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane; halogenated alkyl group-containing silane coupling agents such as 3-chloropropyltrimethoxysilane; etc. Among them, epoxy group-containing silane coupling agents such as glycidoxypropyltrialkoxysilane (for example, 3-glycidoxypropyltrimethoxysilane and 3-glycidoxypropyltriethoxysilane) are preferred.
[0078] The silane coupling agent may have a functional group Y that reacts with the functional group y contained in the pressure-sensitive adhesive layer. From the viewpoint of reactivity at room temperature, a combination of a silane coupling agent having a carboxy group as the functional group y and an epoxy group as the functional group Y may be mentioned. Other examples of combinations include a combination of an amino group and an epoxy group, a combination of a hydroxyl group and an epoxy group, a combination of a carboxy group and an amino group, a combination of an isocyanate group and an amino group, and a combination of a sulfo group and an amino group. On the other hand, in some embodiments, the pressure-sensitive adhesive composition may not have a functional group y (e.g., a carboxy group) that reacts with the functional group Y (e.g., an epoxy group) of the silane coupling agent, from the viewpoint of maintaining the release force increasing agent in a free state in the pressure-sensitive adhesive composition and facilitating the transfer of the release force increasing agent to the surface.
[0079] The molecular weight (chemical formula weight) of the silane coupling agent is not particularly limited, and may be, for example, about 120 to 100. In general, from the viewpoint of ease of adjusting the reworkable period and mobility to the adhesive surface, a silane coupling agent having a molecular weight of 180 or more, 200 or more, or 220 or more is generally preferred. For the same reason, a silane coupling agent having a molecular weight of 800 or less, 600 or less, 400 or less, or 300 or less is preferred. In some embodiments, a silane coupling agent having a molecular weight of 200 or more and 300 or less may be preferably used. As the molecular weight value of the silane coupling agent, a value calculated based on the structural formula of the silane coupling agent is used. Alternatively, a manufacturer's nominal value may be used.
[0080] The amount of the peeling force increasing agent (e.g., silane coupling agent) contained in the adhesive composition disclosed herein can be set so as to obtain the desired effect of use, and is not particularly limited. The amount of the peeling force increasing agent can be, for example, 0.005 parts by weight or more per 100 parts by weight of the acrylic polymer contained in the adhesive composition. The content of the peeling force increasing agent per 100 parts by weight of the acrylic polymer is usually appropriate to be 0.05 parts by weight or more, and may be 0.10 parts by weight or more, 0.20 parts by weight or more, or 0.30 parts by weight or more. By increasing the content of the peeling force increasing agent, the effect of increasing the peeling force can be exhibited. In addition, depending on the mode of use, if the period until the peeling force increases over time at room temperature is too short, the period during which rework is possible becomes too short, which may cause inconvenience such as complicated process management. From this viewpoint, in some embodiments, the content of the peel strength increasing agent per 100 parts by weight of the acrylic polymer in the pressure-sensitive adhesive composition may be, for example, 5 parts by weight or less, 3 parts by weight or less, 1 part by weight or less, or 0.7 parts by weight or less (for example, 0.5 parts by weight or less). The technology disclosed herein can be implemented in an embodiment using a pressure-sensitive adhesive composition that does not substantially contain a peel strength increasing agent (for example, a silane coupling agent). By limiting the use of the peel strength increasing agent or not using the peel strength increasing agent, it is possible to suppress the increase in adhesive strength over time, and also to preferably exhibit good water peelability even after heated storage.
[0081] (Crosslinking agent) The adhesive composition disclosed herein may contain a crosslinking agent as necessary, mainly for the purpose of crosslinking within the adhesive layer or crosslinking between the adhesive layer and its adjacent surface. The type of crosslinking agent is not particularly limited, and may be selected from conventionally known crosslinking agents so that the crosslinking agent exerts an appropriate crosslinking function within the adhesive layer, for example, according to the composition of the adhesive composition. Examples of crosslinking agents that can be used include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, carbodiimide-based crosslinking agents, melamine-based crosslinking agents, urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, hydrazine-based crosslinking agents, and amine-based crosslinking agents. These may be used alone or in combination of two or more.
[0082] As the isocyanate-based crosslinking agent, a polyfunctional isocyanate compound having two or more functionalities can be used. For example, aromatic isocyanates such as tolylene diisocyanate, xylene diisocyanate, polymethylene polyphenyl diisocyanate, tris(p-isocyanatophenyl)thiophosphate, diphenylmethane diisocyanate, etc.; alicyclic isocyanates such as isophorone diisocyanate, etc.; aliphatic isocyanates such as hexamethylene diisocyanate, etc. can be mentioned. Examples of commercially available products include isocyanate adducts such as trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, product name "Coronate L"), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, product name "Coronate HL"), and isocyanurate of hexamethylene diisocyanate (manufactured by Tosoh Corporation, product name "Coronate HX"), etc.
[0083] As the epoxy crosslinking agent, those having two or more epoxy groups in one molecule can be used without any particular limitation. An epoxy crosslinking agent having 3 to 5 epoxy groups in one molecule is preferable. Specific examples of the epoxy crosslinking agent include N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, polyethylene glycol diglycidyl ether, polyglycerol polyglycidyl ether, and the like. Commercially available epoxy crosslinking agents include Mitsubishi Gas Chemical Company's product names "TETRAD-X" and "TETRAD-C", DIC Corporation's product name "Epicron CR-5L", Nagase ChemteX Corporation's product name "Denacol EX-512", Nissan Chemical Industries' product name "TEPIC-G", and the like.
[0084] As the oxazoline-based crosslinking agent, any agent having one or more oxazoline groups in one molecule can be used without any particular limitation. Examples of the aziridine crosslinking agent include trimethylolpropane tris[3-(1-aziridinyl)propionate], trimethylolpropane tris[3-(1-(2-methyl)aziridinylpropionate)], and the like. As the carbodiimide crosslinking agent, a low molecular weight compound or a high molecular weight compound having two or more carbodiimide groups can be used.
[0085] In some embodiments, peroxides may be used as crosslinking agents. Examples of peroxides include di(2-ethylhexyl)peroxydicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butylperoxydicarbonate, t-butylperoxyneodecanoate, t-hexylperoxypivalate, t-butylperoxypivalate, dilauroylperoxide, di-n-octanoylperoxide, 1,1,3,3-tetramethylbutylperoxyisobutyrate, and dibenzoylperoxide. Among these, examples of peroxides that are particularly excellent in crosslinking reaction efficiency include di(4-t-butylcyclohexyl)peroxydicarbonate, dilauroylperoxide, and dibenzoylperoxide. In addition, when peroxides are used as the polymerization initiator, it is also possible to use the remaining peroxides that are not used in the polymerization reaction in the crosslinking reaction. In this case, the remaining amount of peroxide is quantified, and if the ratio of peroxide is less than the predetermined amount, peroxide is added as necessary to reach the predetermined amount. The amount of peroxide can be quantified by the method described in Japanese Patent No. 4971517.
[0086] The content of the crosslinking agent (the total amount of the crosslinking agents when two or more kinds of crosslinking agents are included) is not particularly limited. From the viewpoint of realizing an adhesive that exhibits well-balanced adhesive properties such as adhesive strength and cohesive strength, the content of the crosslinking agent is usually about 5 parts by weight or less relative to 100 parts by weight of the acrylic polymer contained in the adhesive composition, preferably about 0.001 to 5 parts by weight, more preferably about 0.001 to 4 parts by weight, and even more preferably about 0.001 to 3 parts by weight. Alternatively, the adhesive composition may be one that does not contain the above-mentioned crosslinking agent. When a photocurable adhesive composition is used as the adhesive composition disclosed herein, the adhesive composition may be one that does not substantially contain a crosslinking agent such as an isocyanate-based crosslinking agent. Here, the adhesive composition does not substantially contain a crosslinking agent (typically an isocyanate-based crosslinking agent) means that the amount of the crosslinking agent relative to 100 parts by weight of the acrylic polymer is less than 0.05 parts by weight (for example, less than 0.01 parts by weight).
[0087] A crosslinking catalyst may be used to promote the crosslinking reaction more effectively. Examples of the crosslinking catalyst include metal-based crosslinking catalysts such as tetra-n-butyl titanate, tetraisopropyl titanate, nursem ferric, butyltin oxide, and dioctyltin dilaurate. Among them, tin-based crosslinking catalysts such as dioctyltin dilaurate are preferred. The amount of the crosslinking catalyst used is not particularly limited. The amount of the crosslinking catalyst used relative to 100 parts by weight of the acrylic polymer in the pressure-sensitive adhesive composition may be, for example, approximately 0.0001 parts by weight or more and 1 part by weight or less, 0.001 parts by weight or more and 0.1 parts by weight or less, or 0.005 parts by weight or more and 0.5 parts by weight or less.
[0088] A polyfunctional monomer may be used in the adhesive composition (and thus in the adhesive layer) as necessary. The polyfunctional monomer may be used in place of the crosslinking agent as described above or in combination with the crosslinking agent, and may be useful for purposes such as adjusting the cohesive strength. For example, the polyfunctional monomer may be preferably used in the adhesive layer formed from the photocurable adhesive composition. Examples of the polyfunctional monomer include ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, butyl diol (meth)acrylate, and hexyl diol di(meth)acrylate. Among them, trimethylolpropane tri(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and dipentaerythritol hexa(meth)acrylate can be preferably used. The polyfunctional monomers can be used alone or in combination of two or more.
[0089] The amount of the polyfunctional monomer used varies depending on its molecular weight, the number of functional groups, etc., but is usually appropriate to be in the range of about 0.01 to 3.0 parts by weight relative to 100 parts by weight of the acrylic polymer. In some embodiments, the amount of the polyfunctional monomer used relative to 100 parts by weight of the acrylic polymer may be, for example, 0.02 parts by weight or more, 0.1 parts by weight or more, 0.5 parts by weight or more, 1.0 parts by weight or more, or 2.0 parts by weight or more. By increasing the amount of the polyfunctional monomer used, there is a tendency to obtain a higher cohesive force. On the other hand, from the viewpoint of avoiding a decrease in the adhesiveness between the pressure-sensitive adhesive layer and the adjacent layer due to an excessive improvement in cohesive force, the amount of the polyfunctional monomer used relative to 100 parts by weight of the acrylic polymer may be, for example, 10 parts by weight or less, 5.0 parts by weight or less, or 3.0 parts by weight or less.
[0090] (Acrylic Oligomer) The adhesive composition (and thus the adhesive layer) disclosed herein may contain an acrylic oligomer from the viewpoints of improving cohesive strength, improving adhesion to a surface adjacent to the adhesive layer (which may be, for example, the surface of a support, etc.), etc. As the acrylic oligomer, it is preferable to use a polymer having a Tg higher than that of the above-mentioned acrylic polymer.
[0091] The Tg of the acrylic oligomer is not particularly limited, and may be, for example, about 20°C or more and 300°C or less. The Tg may be, for example, about 30°C or more, about 40°C or more, about 60°C or more, about 80°C or more, or about 100°C or more. When the Tg of the acrylic oligomer is high, the effect of improving the cohesive force generally tends to be high. In addition, from the viewpoint of anchoring to the support and impact absorption, the Tg of the acrylic oligomer may be, for example, about 250°C or less, about 200°C or less, about 180°C or less, or about 150°C or less. The Tg of the acrylic oligomer is a value calculated based on the Fox formula, like the Tg of the acrylic polymer corresponding to the composition of the monomer components.
[0092] The Mw of the acrylic oligomer can typically be about 1000 or more and less than about 30000, preferably about 1500 or more and less than about 10000, and more preferably about 2000 or more and less than about 5000. When the Mw is within the above range, the effect of improving the cohesiveness and adhesion to adjacent surfaces is easily exhibited. The Mw of the acrylic oligomer can be measured by gel permeation chromatography (GPC) and calculated as a value equivalent to standard polystyrene. Specifically, the measurement is performed using a HPLC8020 manufactured by Tosoh Corporation, two TSKgelGMH-H(20) columns, and a tetrahydrofuran solvent at a flow rate of about 0.5 mL / min.
[0093] As the monomer component constituting the acrylic oligomer, the above-mentioned various (meth)acrylic acids C 1-20Examples of (meth)acrylate monomers include alkyl esters, the various alicyclic hydrocarbon group-containing (meth)acrylates described above, the various aromatic hydrocarbon group-containing (meth)acrylates described above, and (meth)acrylates obtained from alcohols derived from terpene compounds. These can be used alone or in combination of two or more.
[0094] From the viewpoint of improving adhesiveness, it is preferable that the acrylic oligomer contains, as a monomer unit, an acrylic monomer having a relatively bulky structure, such as an alkyl (meth)acrylate having a branched structure such as isobutyl (meth)acrylate or t-butyl (meth)acrylate, an alicyclic hydrocarbon group-containing (meth)acrylate, or an aromatic hydrocarbon group-containing (meth)acrylate, etc. In addition, when ultraviolet light is used in synthesizing the acrylic oligomer or in preparing the adhesive layer, a monomer having a saturated hydrocarbon group at the ester end is preferable in terms of being less likely to cause polymerization inhibition, and for example, an alkyl (meth)acrylate having a branched structure such as an alkyl group or a saturated alicyclic hydrocarbon group-containing (meth)acrylate can be suitably used.
[0095] The proportion of (meth)acrylate monomers in all monomer components constituting the acrylic oligomer is typically more than 50% by weight, preferably 60% by weight or more, more preferably 70% by weight or more (e.g., 80% by weight or more, or even 90% by weight or more). In a preferred embodiment, the acrylic oligomer has a monomer composition substantially consisting of one or more (meth)acrylate monomers. The monomer components are an alicyclic hydrocarbon group-containing (meth)acrylate and (meth)acrylic acid C. 1-20 When an alkyl ester is contained, the weight ratio thereof is not particularly limited and can be, for example, in the range of 10 / 90 to 90 / 10, 20 / 80 to 80 / 20, or 70 / 30 to 30 / 70.
[0096] In addition to the above (meth)acrylate monomer, functional group-containing monomers can be used as monomer components constituting the acrylic oligomer, if necessary. Examples of functional group-containing monomers include monomers having nitrogen atom-containing heterocycles such as N-vinyl-2-pyrrolidone and N-acryloylmorpholine; amino group-containing monomers such as N,N-dimethylaminoethyl (meth)acrylate; amide group-containing monomers such as N,N-diethyl (meth)acrylamide; carboxy group-containing monomers such as AA and MAA; and hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate. These functional group-containing monomers can be used alone or in combination of two or more. When using a functional group-containing monomer, the ratio of the functional group-containing monomer to the total monomer components constituting the acrylic oligomer can be, for example, 1% by weight or more, 2% by weight or more, or 3% by weight or more, and can be, for example, 15% by weight or less, 10% by weight or less, or 7% by weight or less.
[0097] Suitable acrylic oligomers include, for example, homopolymers of dicyclopentanyl methacrylate (DCPMA), cyclohexyl methacrylate (CHMA), isobornyl methacrylate (IBXMA), isobornyl acrylate (IBXA), dicyclopentanyl acrylate (DCPA), 1-adamantyl methacrylate (ADMA), and 1-adamantyl acrylate (ADA), as well as copolymers of DCPMA and MMA, copolymers of DCPMA and IBXMA, copolymers of ADA and methyl methacrylate (MMA), copolymers of CHMA and isobutyl methacrylate (IBMA), copolymers of CHMA and IBXMA, copolymers of CHMA and acryloylmorpholine (ACMO), copolymers of CHMA and diethylacrylamide (DEAA), and copolymers of CHMA and AA.
[0098] The acrylic oligomer can be formed by polymerizing its constituent monomer components. The polymerization method and polymerization mode are not particularly limited, and various conventionally known polymerization methods (e.g., solution polymerization, emulsion polymerization, bulk polymerization, photopolymerization, radiation polymerization, etc.) can be used in an appropriate mode. The type of polymerization initiator (e.g., azo-based polymerization initiator) that can be used as necessary is generally as exemplified for the synthesis of acrylic polymers, and the amount of polymerization initiator and the amount of chain transfer agent (e.g., mercaptans) that is optionally used are appropriately set based on technical common sense so as to obtain a desired molecular weight, so detailed explanations are omitted.
[0099] When the pressure-sensitive adhesive composition contains an acrylic oligomer, the content thereof can be, for example, 0.01 parts by weight or more relative to 100 parts by weight of the acrylic polymer, and from the viewpoint of obtaining a higher effect, it may be 0.05 parts by weight or more, or 0.1 parts by weight or more, or 0.2 parts by weight or more. Also, from the viewpoint of compatibility with the acrylic polymer, the content of the acrylic oligomer is usually appropriate to be less than 50 parts by weight, preferably less than 30 parts by weight, more preferably 25 parts by weight or less, and may be, for example, 10 parts by weight or less, 5 parts by weight or less, or 1 part by weight or less.
[0100] The adhesive composition disclosed herein may contain, as necessary, various additives that are common in the field of adhesive compositions, such as tackifier resins (e.g., rosin-based, petroleum-based, terpene-based, phenol-based, ketone-based, and other tackifier resins), viscosity adjusters (e.g., thickeners), leveling agents, plasticizers, fillers, colorants such as pigments and dyes, stabilizers, preservatives, and antioxidants, as other optional components. As for such various additives, conventionally known ones can be used in the usual manner, and they do not particularly characterize the present invention, so detailed explanations will be omitted. In addition, since the technology disclosed herein can exhibit good adhesive strength without using the above-mentioned tackifier resin, the content of the tackifier resin in the pressure-sensitive adhesive composition can be, for example, less than 10 parts by weight, or even less than 5 parts by weight, relative to 100 parts by weight of the acrylic polymer. The content of the tackifier resin may be less than 1 part by weight (for example, less than 0.5 parts by weight), or less than 0.1 parts by weight (0 parts by weight or more and less than 0.1 parts by weight), and the pressure-sensitive adhesive composition may not contain a tackifier resin.
[0101] The adhesive composition disclosed herein can be used for optical applications, and therefore can have a predetermined optical property (e.g., transparency) even after the adhesive layer is formed. From the viewpoint of such optical property, it is preferable that the amount of components other than acrylic polymers in the adhesive composition is limited. In the technology disclosed herein, the amount of components other than acrylic polymers in the adhesive composition is usually about 30% by weight or less, appropriately about 15% by weight or less, and preferably about 12% by weight or less (e.g., about 10% by weight or less). The amount of components other than acrylic polymers in the adhesive composition according to one embodiment may be about 5% by weight or less, about 3% by weight or less, or about 1.5% by weight or less (e.g., about 1% by weight or less). A composition in which the amount of components other than acrylic polymers is limited in this way can be preferably adopted for a photocurable adhesive composition.
[0102] <Adhesive sheet configuration example> Next, the adhesive sheet disclosed herein will be described. The adhesive sheet in the technology disclosed herein comprises an adhesive layer formed from an adhesive composition. One configuration example of the adhesive sheet disclosed herein is shown in FIG. 1. This adhesive sheet 1 is configured as a single-sided adhesive sheet including an adhesive layer 10, one surface 10A of which is a surface to be attached to an adherend, and a support 20 laminated on the other surface 10B of the adhesive layer 10. The adhesive layer 10 is fixedly bonded to one surface 20A of the support 20. For example, a plastic film such as a polyester film can be used as the support 20. In the example shown in FIG. 1, the adhesive layer 10 has a single layer structure. The adhesive sheet 1 before use (before being attached to an adherend) can be in the form of an adhesive sheet 50 with a release liner, in which the adhesive surface 10A is protected by a release liner 30, at least the adhesive layer side of which is a release surface (release surface), as shown in FIG. 1, for example. Alternatively, the second surface 20B of the support 20 (the surface opposite to the first surface 20A, also called the back surface) may be the release surface, and the adhesive surface 10A may be protected by being wound or laminated so that the adhesive surface 10A abuts against the second surface 20B of the support 20.
[0103] The release liner is not particularly limited, and may be, for example, a release liner in which the surface of a liner substrate such as a resin film or paper is release-treated, or a release liner made of a low-adhesion material such as a fluorine-based polymer (polytetrafluoroethylene, etc.) or a polyolefin-based resin (polyethylene, polypropylene, etc.). For the release treatment, for example, a silicone-based or long-chain alkyl-based release treating agent may be used. In some embodiments, a release-treated resin film may be preferably used as the release liner.
[0104] The adhesive layer of the adhesive sheet disclosed herein is not limited to a single layer structure as in the above configuration example, and may further comprise one or more adhesive layers (additional adhesive layers) of the same or different composition in addition to the above adhesive layer (typically a compound A-containing adhesive layer). Each layer of such one or more additionally arranged adhesive layers may or may not contain the above-mentioned compound A. When the additional adhesive layer is arranged closer to the support than the above adhesive layer, the additional adhesive layer may or may not contain a peel strength increasing agent from the viewpoint of achieving both good reworkability and high peel strength.
[0105] The adhesive sheet disclosed herein may be in the form of a support-less double-sided adhesive sheet made of an adhesive layer. As shown in FIG. 2, the support-less double-sided adhesive sheet 2 may be in a form in which, before use, each surface 10A, 10B of the adhesive layer 10 is protected by release liners 31, 32 in which at least the adhesive layer side is a releasable surface (release surface). Alternatively, the back surface of the release liner 31 (the surface opposite to the adhesive side) is a release surface, and the release liner 31 may be wound or laminated so that the adhesive surface 10B abuts against the back surface of the release liner 31, thereby protecting the adhesive surfaces 10A, 10B. Such a support-less double-sided adhesive sheet may be used, for example, by bonding a support to one surface of the adhesive layer.
[0106] The adhesive sheet disclosed herein may be a component of an optical member with an adhesive sheet, in which an optical member is bonded to one surface of the adhesive layer. For example, the adhesive sheet 1 shown in FIG. 1 may be a component of an optical member with an adhesive sheet 100, in which an optical member 70 is bonded to one surface 10A of the adhesive layer 10, as shown in FIG. 3. The optical member is preferably one in which the surface to which the adhesive sheet is attached is a non-water-absorbent smooth surface. The optical member with an adhesive sheet having such a configuration can be easily reworked by applying a water peeling method described later as necessary when attaching the adhesive sheet to the optical member. The optical member may be, for example, a glass substrate, a resin film, a metal plate, or the like. In addition, the surface of the member to be attached to the adhesive sheet may be hydrophilized. Examples of hydrophilization treatment include corona treatment, plasma treatment, and treatments that contribute to improving hydrophilicity, such as hydrophilic coating treatment in which a hydrophilic coating layer is provided.
[0107] <Adhesive layer> The adhesive sheet disclosed herein comprises an adhesive layer formed from the adhesive composition disclosed herein. The adhesive layer constituting the adhesive sheet may be a cured layer of the adhesive composition. That is, the adhesive layer may be formed by applying (e.g., coating) the adhesive composition to a suitable surface, followed by a suitable curing treatment. When two or more types of curing treatments (drying, crosslinking, polymerization, etc.) are performed, they may be performed simultaneously or in multiple stages. In the case of a pressure-sensitive adhesive composition using a partial polymer of a monomer component (acrylic polymer syrup), typically, a final copolymerization reaction is carried out as the curing treatment. That is, the partial polymer is subjected to a further copolymerization reaction to form a complete polymer. For example, in the case of a photocurable pressure-sensitive adhesive composition, light irradiation is carried out. If necessary, a curing treatment such as crosslinking or drying may be carried out. For example, in the case of a photocurable pressure-sensitive adhesive composition that needs to be dried (for example, in the case of a photocurable pressure-sensitive adhesive composition in which a partial polymer of a monomer component is dissolved in an organic solvent), it is advisable to carry out photocuring after drying the composition. In the case of a pressure-sensitive adhesive composition using a completely polymerized product, typically, the curing treatment is carried out as necessary, such as drying (heat drying) or crosslinking. In the case of a solvent-based pressure-sensitive adhesive composition to which photocurability (photocrosslinkability) has been imparted by the addition of a polyfunctional monomer, photocuring may be carried out after the composition has been dried. Here, "after the composition has been dried" may refer to after the pressure-sensitive adhesive sheet obtained through the drying is attached to an adherend. The pressure-sensitive adhesive sheet disclosed herein may be used in an embodiment in which the sheet is attached to the adherend by a method including photocuring after being attached to the adherend. A pressure-sensitive adhesive layer having a multi-layer structure of two or more layers can be prepared by laminating pressure-sensitive adhesive layers formed in advance. Alternatively, a pressure-sensitive adhesive composition may be applied onto a first pressure-sensitive adhesive layer formed in advance, and the pressure-sensitive adhesive composition may be cured to form a second pressure-sensitive adhesive layer. When the pressure-sensitive adhesive layer of a pressure-sensitive adhesive sheet used in an attachment mode in which the sheet is photocured after being attached to an adherend has a multi-layer structure, the pressure-sensitive adhesive layer to be photocured may be a part of the layers (e.g., one layer) or all of the layers included in the multi-layer structure.
[0108] The pressure-sensitive adhesive composition can be applied using a conventional coater such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a bar coater, a knife coater, a spray coater, etc. In a pressure-sensitive adhesive sheet having a support, a method for providing a pressure-sensitive adhesive layer on a support may be a direct method in which a pressure-sensitive adhesive composition is directly applied to the support to form a pressure-sensitive adhesive layer, or a transfer method in which a pressure-sensitive adhesive layer formed on a release surface is transferred to a support.
[0109] The thickness of the pressure-sensitive adhesive layer is not particularly limited, and may be, for example, about 3 μm to 2000 μm. From the viewpoint of adhesion to the adherend, such as step conformability, in some embodiments, the thickness of the pressure-sensitive adhesive layer may be, for example, 5 μm or more, appropriately 10 μm or more, preferably 20 μm or more, and more preferably 30 μm or more. The thickness of the pressure-sensitive adhesive layer may be 50 μm or more, may be more than 50 μm, may be 70 μm or more, may be 100 μm or more, or may be 120 μm or more. In addition, from the viewpoint of preventing the occurrence of adhesive residue due to cohesive failure of the pressure-sensitive adhesive layer, in some embodiments, the thickness of the pressure-sensitive adhesive layer may be, for example, 1000 μm or less, may be 700 μm or less, may be 500 μm or less, may be 300 μm or less, or may be 200 μm or less, or may be 170 μm or less. The technology disclosed herein may be suitably implemented in the form of a pressure-sensitive adhesive sheet having a thickness of 130 μm or less, 90 μm or less, or 60 μm or less (e.g., 40 μm or less). In a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer with a multilayer structure of two or more layers, the thickness of the pressure-sensitive adhesive layer refers to the thickness from the adhesive surface attached to the adherend to the surface opposite to the adhesive surface.
[0110] <Support> The pressure-sensitive adhesive sheet according to some embodiments may be in the form of a pressure-sensitive adhesive sheet with a support, which includes a support bonded to the other back surface of the pressure-sensitive adhesive layer. The material of the support is not particularly limited, and can be appropriately selected according to the purpose and mode of use of the pressure-sensitive adhesive sheet. Non-limiting examples of supports that can be used include plastic films such as polyolefin films mainly composed of polyolefins such as polypropylene and ethylene-propylene copolymers, polyester films mainly composed of polyesters such as polyethylene terephthalate and polybutylene terephthalate, and polyvinyl chloride films mainly composed of polyvinyl chloride; foam sheets made of foams such as polyurethane foam, polyethylene foam, and polychloroprene foam; woven fabrics and nonwoven fabrics made by spinning various fibrous materials alone or in combination; papers such as Japanese paper, wood-free paper, craft paper, and crepe paper; metal foils such as aluminum foil and copper foil; and the like. The support may be a composite of these. Examples of such a composite support include a support having a structure in which a metal foil and the above-mentioned plastic film are laminated together, and a plastic sheet reinforced with inorganic fibers such as glass cloth.
[0111] As the support of the adhesive sheet disclosed herein, various films (hereinafter, also referred to as support films) can be preferably used. The support film may be a porous film such as a foam film or a nonwoven sheet, or may be a nonporous film, or may be a film having a structure in which a porous layer and a nonporous layer are laminated. In some embodiments, the support film may preferably be one that includes a resin film that can independently maintain its shape (self-supporting or independent) as a base film. Here, the term "resin film" refers to a resin film that has a nonporous structure and typically does not substantially contain air bubbles (voidless). Therefore, the resin film is a concept that is distinguished from foam films and nonwoven fabrics. The resin film may be a single-layer structure, or may be a multi-layer structure of two or more layers (for example, a three-layer structure).
[0112] Examples of resin materials constituting the resin film include polyester, polyolefin, polycycloolefin derived from a monomer having an aliphatic ring structure such as a norbornene structure, polyamide (PA) such as nylon 6, nylon 66, and partially aromatic polyamide, polyimide (PI), polyamideimide (PAI), polyetheretherketone (PEEK), polyethersulfone (PES), polyphenylene sulfide (PPS), polycarbonate (PC), polyurethane (PU), ethylene-vinyl acetate copolymer (EVA), polystyrene, fluororesins such as polyvinyl chloride, polyvinylidene chloride, and polytetrafluoroethylene (PTFE), acrylic resins such as polymethyl methacrylate, cellulose-based polymers such as diacetyl cellulose and triacetyl cellulose, vinyl butyral-based polymers, arylate-based polymers, polyoxymethylene-based polymers, and epoxy-based polymers. The resin film may be formed using a resin material containing one of these resins alone, or may be formed using a resin material in which two or more of them are blended. The resin film may be unstretched or stretched (for example, uniaxially or biaxially stretched).
[0113] Suitable examples of resin materials constituting the resin film include polyester-based resin, PPS resin, and polyolefin-based resin. Here, polyester-based resin refers to a resin containing more than 50% by weight of polyester. Similarly, PPS resin refers to a resin containing more than 50% by weight of PPS, and polyolefin-based resin refers to a resin containing more than 50% by weight of polyolefin.
[0114] As the polyester-based resin, typically, a polyester-based resin containing, as a main component, a polyester obtained by polycondensation of a dicarboxylic acid and a diol is used. Specific examples of the polyester-based resin include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polybutylene naphthalate, etc.
[0115] As the polyolefin resin, one type of polyolefin can be used alone, or two or more types of polyolefins can be used in combination. The polyolefin can be, for example, a homopolymer of an α-olefin, a copolymer of two or more types of α-olefins, or a copolymer of one or more types of α-olefins and other vinyl monomers. Specific examples include polyethylene (PE), polypropylene (PP), poly-1-butene, poly-4-methyl-1-pentene, ethylene-propylene copolymers such as ethylene-propylene rubber (EPR), ethylene-propylene-butene copolymers, ethylene-butene copolymers, ethylene-vinyl alcohol copolymers, and ethylene-ethyl acrylate copolymers. Both low density (LD) polyolefins and high density (HD) polyolefins can be used. Examples of polyolefin resin films include non-oriented polypropylene (CPP) film, biaxially oriented polypropylene (OPP) film, low-density polyethylene (LDPE) film, linear low-density polyethylene (LLDPE) film, medium-density polyethylene (MDPE) film, high-density polyethylene (HDPE) film, polyethylene (PE) film made by blending two or more types of polyethylene (PE), and PP / PE blend film made by blending polypropylene (PP) and polyethylene (PE).
[0116] Specific examples of resin films that can be preferably used as the support include PET film, PEN film, PPS film, PEEK film, CPP film, and OPP film. Preferred examples from the viewpoint of strength include PET film, PEN film, PPS film, and PEEK film. Preferred examples from the viewpoint of availability, dimensional stability, optical properties, etc. include PET film.
[0117] The resin film may contain known additives such as light stabilizers, antioxidants, antistatic agents, colorants (dyes, pigments, etc.), fillers, slip agents, antiblocking agents, etc. The amount of additives to be added is not particularly limited and can be appropriately set depending on the application of the pressure-sensitive adhesive sheet, etc.
[0118] The method for producing the resin film is not particularly limited, and may be any of the conventionally known general resin film forming methods such as extrusion molding, inflation molding, T-die casting, and calendar roll molding.
[0119] The support may be substantially composed of such a resin film. Alternatively, the support may include an auxiliary layer in addition to the resin film. Examples of the auxiliary layer include an optical property adjusting layer (e.g., a colored layer, an anti-reflection layer), a printed layer or a laminate layer for imparting a desired appearance to the support or the adhesive sheet, an antistatic layer, an undercoat layer, a peeling layer, or other surface treatment layer. The support may also be an optical member, which will be described later.
[0120] The thickness of the support is not particularly limited and may be selected according to the purpose and mode of use of the pressure-sensitive adhesive sheet. The thickness of the support may be, for example, 1000 μm or less, 500 μm or less, 100 μm or less, 70 μm or less, 50 μm or less, 25 μm or less, 10 μm or less, or 5 μm or less. When the thickness of the support is reduced, the flexibility of the pressure-sensitive adhesive sheet and its ability to follow the surface shape of the adherend tend to improve. In addition, from the viewpoint of handling and processability, the thickness of the support may be, for example, 2 μm or more, or may be more than 5 μm or more than 10 μm. In some embodiments, the thickness of the support may be, for example, 20 μm or more, 35 μm or more, or 55 μm or more.
[0121] The surface of the support that is to be bonded to the adhesive layer may be subjected to a conventionally known surface treatment such as corona discharge treatment, plasma treatment, ultraviolet irradiation treatment, acid treatment, alkali treatment, application of an undercoat (primer), antistatic treatment, etc., as necessary. Such a surface treatment may be a treatment for improving the adhesion between the support and the adhesive layer, in other words, the anchoring property of the adhesive layer to the support. The composition of the primer is not particularly limited, and can be appropriately selected from known ones. The thickness of the undercoat layer is not particularly limited, but is usually appropriate to be about 0.01 μm to 1 μm, and preferably about 0.1 μm to 1 μm.
[0122] The surface of the support opposite to the side bonded to the adhesive layer (hereinafter also referred to as the back side) may be subjected to a conventionally known surface treatment such as a release treatment, an adhesiveness or adhesion improving treatment, or an antistatic treatment, if necessary. For example, by surface treating the back side of the support with a release treatment agent, the unwinding force of the adhesive sheet wound into a roll can be reduced. As the release treatment agent, a silicone-based release treatment agent, a long-chain alkyl-based release treatment agent, an olefin-based release treatment agent, a fluorine-based release treatment agent, a fatty acid amide-based release treatment agent, molybdenum sulfide, silica powder, etc. can be used.
[0123] <Additional adhesive layer> In the adhesive sheet disclosed herein, the adhesive layer that can be additionally arranged apart from the above-mentioned adhesive layer (compound A-containing adhesive layer) can be, for example, an adhesive layer composed of one or more adhesives selected from various known adhesives such as acrylic adhesives, rubber adhesives (natural rubber-based, synthetic rubber-based, and mixtures thereof), silicone adhesives, polyester adhesives, urethane adhesives, polyether adhesives, polyamide adhesives, and fluorine-based adhesives. From the viewpoint of transparency, weather resistance, and the like, in some embodiments, an acrylic adhesive can be preferably used as a constituent material of the additional adhesive layer. As for other matters of the additional adhesive layer, the same configuration as the above-mentioned adhesive layer (compound A-containing adhesive layer) can be adopted, or an appropriate configuration can be adopted according to the application or purpose based on known or commonly used technology and technical common sense, so detailed explanations are omitted here.
[0124] <Characteristics of adhesive sheet> The adhesive sheet disclosed herein may have a normal peel strength of about 1.5 N / cm or more after 30 minutes at 23°C, measured by the method described in the Examples below. The normal peel strength after 30 minutes at 23°C is suitably about 2 N / cm or more, and from the viewpoint of exhibiting good adhesive strength, it is preferably about 3 N / cm or more, more preferably about 3.5 N / cm or more (e.g., about 4 N / cm or more). For example, an adhesive sheet according to one embodiment may exhibit a normal peel strength after 30 minutes at 23°C of about 5 N / cm or more. In this embodiment, the normal peel strength after 30 minutes at 23°C is preferably about 9 N / cm or more, more preferably about 10 N / cm or more, even more preferably about 11 N / cm or more, and particularly preferably about 12 N / cm or more (e.g., about 13 N / cm or more). Such a strong adhesive strength can be preferably achieved by using a solvent-based or photocurable adhesive composition. The upper limit of the normal peel strength after 30 minutes at 23° C. is not particularly limited, and may be, for example, 25 N / cm or less, 20 N / cm or less, 15 N / cm or less, or 10 N / cm or less.
[0125] The pressure-sensitive adhesive sheet disclosed herein may have a water peeling strength of less than about 1.3 N / cm after 30 minutes at 23° C., as measured by the method described in the Examples below. The water peeling strength after 30 minutes at 23° C. is suitably about 1 N / cm or less, and from the viewpoint of reworkability using water peeling, is preferably less than 1 N / cm, for example, may be less than 0.7 N / cm, or may be less than 0.3 N / cm (about 0.1 N / cm or less).
[0126] The adhesive sheet disclosed herein may have a normal peel strength after 18 hours at 60°C of about 3 N / cm or more (e.g., about 4 N / cm or more) measured by the method described in the Examples below. The normal peel strength after 18 hours at 60°C is suitably about 5 N / cm or more, and from the viewpoint of exerting sufficient adhesive strength, is preferably about 7 N / cm or more (e.g., about 8 N / cm or more). For example, an adhesive sheet according to one embodiment may exhibit a normal peel strength after 18 hours at 60°C of about 10 N / cm or more. In this embodiment, the normal peel strength after 18 hours at 60°C is preferably about 12 N / cm or more, more preferably about 14 N / cm or more (e.g., about 15 N / cm or more). The upper limit of the normal peel strength after 18 hours at 60°C is not particularly limited, and may be, for example, 25 N / cm or less, 20 N / cm or less, 18 N / cm or less, or 12 N / cm or less.
[0127] The adhesive sheet disclosed herein may have a water peeling strength of less than about 1.3 N / cm after 18 hours at 60°C, as measured by the method described in the Examples below. The water peeling strength after 18 hours at 60°C is suitably less than about 1 N / cm, and from the viewpoint of reworkability using water peeling, is preferably less than 1 N / cm, and may be, for example, less than 0.7 N / cm, or less than 0.3 N / cm (about 0.1 N / cm or less). In another embodiment, the water peeling strength after 18 hours at 60°C may be about 4 N / cm or more. In this embodiment, the water peeling strength after 18 hours at 60°C may be about 5 N / cm or more, or may be about 6 N / cm or more (for example, about 7 N / cm or more). According to an adhesive sheet exhibiting the water peeling strength after 18 hours at 60°C, the water peeling property disappears by carrying out a predetermined curing treatment (typically a heat treatment), so that the adhesive sheet can exhibit good bonding reliability (water resistance reliability) even in an environment exposed to water or the like. The upper limit of the water peel strength after 18 hours at 60° C. is not particularly limited, and may be, for example, 25 N / cm or less, 20 N / cm or less, or 12 N / cm or less.
[0128] A pressure-sensitive adhesive sheet according to a preferred embodiment may have a water peeling adhesion reduction rate A of about 40% or more (e.g., about 50% or more) calculated from the ratio (FW1 / FN1) of the water peeling force FW1 after 30 minutes at 23°C to the normal peeling force FN1 after 30 minutes at 23°C. A pressure-sensitive adhesive sheet having a high water peeling adhesion reduction rate A can be peeled off using an aqueous liquid such as water, thereby significantly reducing the load applied to the adherend during peeling. For example, a small amount of aqueous liquid is supplied to the adherend to which the pressure-sensitive adhesive sheet is attached, and the aqueous liquid is allowed to enter the interface between the pressure-sensitive adhesive sheet and the adherend from one end of the pressure-sensitive adhesive sheet to trigger peeling, and then the pressure-sensitive adhesive sheet is peeled off, thereby significantly reducing the peel strength of the pressure-sensitive adhesive sheet from the adherend. By utilizing this property, it is possible to achieve both the performance of suppressing the positional deviation or lifting of the pressure-sensitive adhesive sheet attached to the adherend and good reworkability. In some embodiments, the water peeling adhesive strength reduction rate A is suitably 60% or more, preferably 65% or more, for example, 70% or more, 75% or more, 80% or more, or 85% or more. In the pressure-sensitive adhesive sheet according to one embodiment, the water peeling adhesive strength reduction rate A is 90% or more, for example, 95% or more, or even 98% or more (typically 99% or more). The water peeling adhesive strength reduction rate A is in principle 100% or less, and typically less than 100%. The water peel adhesion loss rate A is calculated using the formula: Water peel adhesion loss rate A [%] = (1-(FW1 / FN1)) × 100; It can be found from.
[0129] The adhesive sheet according to one embodiment may have a peel strength increase rate calculated from the relationship between the normal peel strength FN1 after 30 minutes at 23°C and the normal peel strength FN2 after 18 hours at 60°C. The peel strength increase rate may be, for example, 30% or more, or 40% or more. In some embodiments, the peel strength increase rate may be, for example, 100% or more, 150% or more, or 200% or more. Such a peel strength increase rate is preferably adopted for a configuration in which the initial peel strength is relatively low. The upper limit of the peel strength increase rate is not particularly limited, and may be, for example, 1000% or less. In some other embodiments, the peel strength increase rate may be approximately 100% or less, and is suitably approximately 50% or less. The adhesive sheet having the suppressed peel strength increase rate may have excellent adhesive stability, such as being likely to exhibit stable adhesive strength throughout the period of attachment to the adherend and being unlikely to cause excessive adhesive strength increase in the usage environment to which the adhesive sheet may be exposed. The peel strength increase rate may be approximately 40% or less, or approximately 30% or less. In this embodiment, the lower limit of the rate of increase in peel force is not particularly limited, and may be about 0% or more, or may be about 10% or more (for example, about 15% or more). The peel force increase rate is calculated by the formula: Peel force increase rate [%] = ((FN2-FN1) / FN1) × 100; It can be found from.
[0130] The pressure-sensitive adhesive sheet according to one embodiment may have a post-heat water-peeling adhesive strength reduction rate of about 70% or more, calculated from the ratio (FW2 / FN2) of the water-peeling strength FW2 after 18 hours at 60°C to the normal peel strength FN2 after 18 hours at 60°C. A pressure-sensitive adhesive sheet having a high post-heat water-peeling adhesive strength reduction rate has sufficient adhesive strength after heating and excellent water-peeling properties using an aqueous liquid such as water, so that it can exhibit good reworkability even after heat treatment. The post-heat water-peeling adhesive strength reduction rate is suitably 80% or more, and may be, for example, 90% or more, 95% or more, or even 98% or more (typically 99% or more). In another embodiment, the post-heat water-peeling adhesive strength reduction rate may be 40% or less. With a pressure-sensitive adhesive sheet having a low post-heat water-peeling adhesive strength reduction rate, it becomes difficult to peel the pressure-sensitive adhesive sheet with water after the heat treatment, and a bond with good water resistance reliability can be realized. In this embodiment, the post-heat water-peeling adhesive strength reduction rate may be, for example, 30% or less, or 20% or less. The rate of decrease in water peel adhesion after heating is in principle 100% or less, and typically less than 100%. The rate of decrease in water peel adhesion after heating is calculated using the formula: Water peel adhesion loss rate [%] = (1-(FW2 / FN2)) × 100; It can be found from.
[0131] In the technology disclosed herein, the haze value of the pressure-sensitive adhesive sheet is suitably about 10% or less, and may be about 5% or less (e.g., about 3% or less). The haze value is preferably 1.0% or less. Such highly transparent pressure-sensitive adhesive sheets are suitable for optical applications requiring high light transmittance. The haze value of the pressure-sensitive adhesive sheet may be less than 1.0%, may be less than 0.7%, or may be 0.5% or less (e.g., 0 to 0.5%). These haze values for the pressure-sensitive adhesive sheet may also be preferably applied to the haze value of the pressure-sensitive adhesive layer in the technology disclosed herein.
[0132] Here, the "haze value" refers to the ratio of diffuse transmitted light to the total transmitted light when a measurement target is irradiated with visible light. It is also called the cloudiness value. The haze value can be expressed by the following formula. Th[%]=Td / Tt×100 In the above formula, Th is the haze value [%], Td is the scattered light transmittance, and Tt is the total light transmittance. The haze value can be measured according to the method described in the examples below. The haze value can be adjusted, for example, by selecting the composition, thickness, etc. of the pressure-sensitive adhesive layer.
[0133] From the viewpoint of bonding reliability, the adhesive sheet disclosed herein preferably has a normal adhesive strength N0 of 2.0 N / 10 mm or more. In some embodiments, the normal adhesive strength N0 may be, for example, 2.5 N / 10 mm or more, 3.0 N / 10 mm or more, 3.5 N / 10 mm or more, or 4.0 N / 10 mm or more. The upper limit of the normal adhesive strength N0 is not particularly limited, and may be, for example, 30 N / 10 mm or less. In some embodiments, the normal adhesive strength N0 may be 20 N / 10 mm or less, or 15 N / 10 mm or less. The normal adhesive strength N0 is measured by the method described in the Examples below.
[0134] The water peeling force N2 is preferably 60% or less (more preferably 50% or less) of the normal adhesive force N0. Although not particularly limited, the water peeling force N2 may be, for example, 10N / 10mm or less, 3.5N / 10mm or less, 3.0N / 10mm or less, 2.5N / 10mm or less, 1.6N / 10mm or less, 1.2N / 10mm or less, or 1.0N / 10mm or less. A pressure-sensitive adhesive sheet with a low water peeling force N2 can reduce the load on the adherend when peeling the pressure-sensitive adhesive sheet. This is particularly meaningful for pressure-sensitive adhesive sheets that are attached to, for example, thin adherends, brittle adherends, adherends that are easily deformed (stretched, bent, twisted, etc.), adherends with thin films that are easily damaged on the surface, and the like. The PSA sheet disclosed herein may also be suitably embodied in an embodiment in which the water peeling force N2 is, for example, 0.75 N / 10 mm or less, or 0.50 N / 10 mm or less, or 0.25 N / 10 mm or less, or 0.15 N / 10 mm or less. The lower limit of the water peeling force N2 is not particularly limited, and may be substantially 0 N / 10 mm or more than 0 N / 10 mm. In addition, from the viewpoint of improving reworkability, in the measurement of water peeling force N2, it is preferable that the pressure-sensitive adhesive sheet is peeled off from the adherend without leaving any adhesive residue on the adherend. That is, it is preferable that the pressure-sensitive adhesive sheet has excellent non-adhesive residue properties. The presence or absence of adhesive residue on the adherend can be grasped, for example, by visually observing the adherend after peeling off the pressure-sensitive adhesive sheet. The water peeling force N2 is measured by the method described in the Examples below.
[0135] The ratio (N2 / N0) of the water peeling force N2 [N / 10 mm] to the normal adhesive force N0 [N / 10 mm] may be, for example, 1 / 2.5 or less, 1 / 5 or less, or 1 / 10 or less. A smaller ratio (N2 / N0) means that the water peeling force N2 is more significantly reduced relative to the normal adhesive force N0. The adhesive sheet disclosed herein may be preferably implemented in an embodiment in which the ratio (N2 / N0) is 1 / 15 or less, 1 / 25 or less, or 1 / 35 or less. The upper limit of the ratio (N2 / N0) is not particularly limited, and may be, for example, 1 / 200 or more, 1 / 150 or more, or 1 / 100 or more.
[0136] The adhesive sheet disclosed herein preferably has a water peeling adhesion reduction rate B of 40% or more. An adhesive sheet having a large value of the water peeling adhesion reduction rate B can be easily peeled off using an aqueous liquid such as water. For example, a small amount of aqueous liquid is supplied to an adherend to which an adhesive sheet is attached, and the aqueous liquid is caused to enter the interface between the adhesive sheet and the adherend from one end of the adhesive sheet to trigger peeling, and then the adhesive sheet is peeled off, whereby the peel strength of the adhesive sheet from the adherend can be significantly reduced. By utilizing this property, it is possible to achieve both high adhesive strength during normal use and good reworkability. In some embodiments, the water peeling adhesion reduction rate B may be, for example, 50% or more, 65% or more, 75% or more, 85% or more, 90% or more, 95% or more, or 97% or more. The water peeling adhesion reduction rate B is in principle 100% or less, and typically less than 100%. The water peel adhesion loss rate B is calculated using the formula: Water peel adhesion loss rate B [%] = (1-(N2 / N0)) x 100; In the formula, N0 is the normal adhesive strength N0 [N / 10 mm], and N2 is the water peel strength N2 [N / 10 mm].
[0137] <Application> The use of the pressure-sensitive adhesive sheet disclosed herein is not particularly limited, and it can be used for various applications. For example, by taking advantage of the feature of having both good reworkability by water peeling and sufficient adhesive strength without impairing the optical properties of the adherend, it can be used for applications such as fixing, joining, molding, decoration, protection, and support of the optical member in a form attached to an optical member constituting various mobile devices (portable devices), automobiles, home appliances, etc. The material constituting at least the surface of the optical member can be, for example, glass such as an alkali glass plate or non-alkali glass; metal materials such as stainless steel (SUS) and aluminum; ceramic materials such as alumina and silica; resin materials such as acrylic resin, ABS resin, polycarbonate resin, polystyrene resin, transparent polyimide resin, etc. The pressure-sensitive adhesive sheet disclosed herein may be attached to a painted surface with a paint such as an acrylic, polyester, alkyd, melamine, urethane, acid epoxy crosslinking, or a composite of these (for example, an acrylic melamine, an alkyd melamine), or a plated surface such as a zinc-plated steel plate. Suitable examples of the adherend include inorganic materials such as the above-mentioned glass, the above-mentioned ceramic materials, the above-mentioned metal materials, etc. The adhesive sheet disclosed herein may be, for example, a component of an optical member with an adhesive sheet, which includes an optical member having at least a part of its surface made of such a material and the above-mentioned adhesive sheet, and in which the adhesive surface of the above-mentioned adhesive sheet is bonded to the surface of the above-mentioned optical member.
[0138] The optical applications of the technology disclosed herein include, for example, applications for bonding optical members (for bonding optical members) and applications for manufacturing products (optical products) using the optical members. The pressure-sensitive adhesive sheet disclosed herein can be preferably used as an optical pressure-sensitive adhesive sheet for such applications.
[0139] The optical member refers to a member having optical properties (for example, polarization, light refraction, light scattering, light reflectivity, light transmittance, light absorption, light diffraction, optical rotation, visibility, etc.). The optical member is not particularly limited as long as it has optical properties, but examples thereof include members constituting devices (optical devices) such as display devices (image display devices) and input devices, or members used in these devices, such as polarizing plates, wave plates, retardation plates, optical compensation films, brightness improvement films, light guide plates, reflective films, anti-reflection films, hard coat (HC) films, impact absorbing films, antifouling films, photochromic films, light control films, transparent conductive films (ITO films), design films, decorative films, surface protection plates, prisms, lenses, color filters, transparent substrates, and further members in which these are laminated (these may be collectively referred to as "functional films"). The above "plate" and "film" each include plate-like, film-like, sheet-like and other forms. For example, "polarizing film" includes "polarizing plate", "polarizing sheet", and the like.
[0140] Examples of the display device include a liquid crystal display device, an organic EL (electroluminescence) display device, a PDP (plasma display panel), and electronic paper. In particular, the technology disclosed herein is preferably applied to a foldable display device or a display device for vehicle use that includes expensive components. Examples of the input device include a touch panel.
[0141] The optical member is not particularly limited, and examples thereof include members (e.g., sheet-shaped, film-shaped, or plate-shaped members) made of glass, acrylic resin, polycarbonate, polyethylene terephthalate, metal thin film, etc. In this specification, the term "optical member" also includes members (design films, decorative films, surface protection films, etc.) that play a role in decoration or protection while maintaining the visibility of a display device or an input device.
[0142] The embodiment of bonding an optical member using the adhesive sheet disclosed herein is not particularly limited, and may be, for example, (1) an embodiment in which optical members are bonded to each other via the adhesive sheet disclosed herein, (2) an embodiment in which an optical member is bonded to a member other than an optical member via the adhesive sheet disclosed herein, or (3) an embodiment in which the adhesive sheet disclosed herein includes an optical member and the adhesive sheet is bonded to an optical member or a member other than an optical member. In the above embodiment (3), the adhesive sheet having an optical member may be, for example, an adhesive sheet whose support is an optical member (e.g., an optical film). In this way, an adhesive sheet having an optical member as a support may also be understood as an adhesive-type optical member (e.g., an adhesive-type optical film). In addition, when the adhesive sheet disclosed herein is an adhesive sheet having a support and the functional film is used as the support, the adhesive sheet may also be understood as an "adhesive-type functional film" having the adhesive layer disclosed herein on at least one side of the functional film.
[0143] <Removal method> Also, according to this specification, a method for peeling a pressure-sensitive adhesive sheet attached to an adherend from the adherend is provided. The method may include a water peeling step of peeling the pressure-sensitive adhesive sheet from the adherend while advancing the intrusion of the aqueous liquid into the interface in accordance with the movement of the peel front, in a state where an aqueous liquid is present at the interface between the adherend and the pressure-sensitive adhesive sheet at the peel front of the pressure-sensitive adhesive sheet from the adherend. Here, the peel front refers to a location where the pressure-sensitive adhesive sheet starts to separate from the adherend when the peeling of the pressure-sensitive adhesive sheet from the adherend progresses. According to the water peeling step, the aqueous liquid can be effectively used to peel the pressure-sensitive adhesive sheet from the adherend. The peeling method may be preferably carried out, for example, in an embodiment in which any of the pressure-sensitive adhesive sheets disclosed herein are peeled from the adherend.
[0144] The aqueous liquid used in the above-mentioned peeling method may be water or a mixed solvent mainly composed of water, containing a small amount of additives as necessary. As the solvent other than water constituting the mixed solvent, a lower alcohol (e.g., ethyl alcohol) or a lower ketone (e.g., acetone) that can be mixed uniformly with water may be used. As the additive, a known surfactant or the like may be used. From the viewpoint of avoiding contamination of the adherend, in some embodiments, an aqueous liquid that does not substantially contain additives may be preferably used. From the viewpoint of environmental hygiene, it is particularly preferable to use water as the aqueous liquid. The water is not particularly limited, and for example, distilled water, ion-exchanged water, tap water, etc. may be used in consideration of the purity required depending on the application and the ease of availability.
[0145] In some embodiments, the peeling method can be preferably carried out in a manner similar to the measurement of the water peeling force described below, in which an aqueous liquid is supplied onto the adherend near the outer edge of the adhesive sheet attached to the adherend, the aqueous liquid is allowed to penetrate into the interface between the adhesive sheet and the adherend from the outer edge of the adhesive sheet, and then the peeling of the adhesive sheet is allowed to proceed without supplying new water (i.e., using only the aqueous liquid supplied onto the adherend before the start of peeling). If the water that is allowed to penetrate into the interface between the adhesive sheet and the adherend in accordance with the movement of the peeling front during the water peeling process runs out midway, additional water may be supplied intermittently or continuously after the start of the water peeling process. For example, when the adherend has water absorption properties or when the aqueous liquid is likely to remain on the adherend surface or adhesive surface after peeling, an embodiment in which additional water is supplied after the start of the water peeling process can be preferably adopted.
[0146] The amount of the aqueous liquid supplied before the start of peeling is not particularly limited as long as it is an amount that can introduce the aqueous liquid from outside the adhesion range of the adhesive sheet to the interface between the adhesive sheet and the adherend. The amount of the aqueous liquid may be, for example, 5 μL or more, usually 10 μL or more is appropriate, and may be 20 μL or more. There is no particular limit to the upper limit of the amount of the aqueous liquid. In some embodiments, from the viewpoint of improving workability, etc., the amount of the aqueous liquid may be, for example, 10 mL or less, 5 mL or less, 1 mL or less, 0.5 mL or less, 0.1 mL or less, or 0.05 mL or less. By reducing the amount of the aqueous liquid, the operation of removing the aqueous liquid by drying, wiping, etc. after peeling of the adhesive sheet can be omitted or simplified.
[0147] The operation of injecting the aqueous liquid into the interface between the adhesive sheet and the adherend from the outer edge of the adhesive sheet at the start of peeling can be carried out, for example, by inserting the tip of a tool such as a cutter knife or needle into the interface at the outer edge of the adhesive sheet, scratching and lifting the outer edge of the adhesive sheet with a hook or claw, or attaching a highly adhesive adhesive tape or suction cup to the back surface near the outer edge of the adhesive sheet to lift the edge of the adhesive sheet. By forcibly injecting the aqueous liquid into the interface from the outer edge of the adhesive sheet in this way, a state in which the aqueous liquid is present at the interface between the adherend and the adhesive sheet can be efficiently formed. In addition, it is possible to suitably achieve both good water peelability after the operation of forcibly injecting the aqueous liquid into the interface to trigger peeling, and high water resistance reliability when such an operation is not performed.
[0148] The pressure-sensitive adhesive sheet to be peeled off by the peeling method includes a pressure-sensitive adhesive layer, and the pressure-sensitive adhesive layer is composed of a pressure-sensitive adhesive containing compound A. The pressure-sensitive adhesive sheet is preferably, for example, any of the pressure-sensitive adhesive sheets disclosed herein. Therefore, the peeling method is suitable as a peeling method for any of the pressure-sensitive adhesive sheets disclosed herein.
[0149] The water peeling step according to some embodiments can be preferably carried out in an embodiment in which the peel front is moved at a speed of 10 mm / min or more. Moving the peel front at a speed of 10 mm / min or more corresponds to peeling the PSA sheet at a pulling speed of 20 mm / min or more, for example, under the condition of a peel angle of 180 degrees. The speed at which the peel front is moved may be, for example, 25 mm / min or more, 50 mm / min or more, 150 mm / min or more, 300 mm / min or more, or 500 mm / min or more. According to the peeling method disclosed herein, by peeling the PSA sheet from the adherend while progressing the penetration of the aqueous liquid into the interface, good water peelability can be exhibited even at such a relatively high peeling speed. There is no particular upper limit to the speed at which the peel front is moved. The speed at which the peel front is moved may be, for example, 1000 mm / min or less.
[0150] The peeling method disclosed herein is, for example, a method in which the peeling area of the PSA sheet per 10 μL of aqueous liquid (e.g., water) volume used in the method is, for example, 50 cm 2 More than 100cm, preferably 100cm 2 The present invention can be implemented in the above-described manner.
[0151] The peeling method disclosed herein can be preferably applied to peeling off an adhesive sheet attached to a non-water-absorbent smooth surface such as a glass plate, a metal plate, a resin plate, etc. The peeling method disclosed herein can also be preferably used as a method for peeling off an adhesive sheet from any of the optical members described above. In particular, it is suitable as a method for peeling off an adhesive sheet attached to a glass plate such as an alkali glass or non-alkali glass.
[0152] The matters disclosed in this specification include the following. (1) A pressure-sensitive adhesive composition comprising an acrylic polymer, The optical pressure-sensitive adhesive composition further comprises at least one compound A selected from a surfactant and a compound having a polyoxyalkylene skeleton. (2) The pressure-sensitive adhesive composition according to (1) above, wherein the monomer components forming the acrylic polymer contain less than 20% by weight of alkoxyalkyl (meth)acrylate and less than 20% by weight of alkoxypolyalkylene glycol (meth)acrylate. (3) The pressure-sensitive adhesive composition according to the above (1) or (2), wherein the content of the compound A is less than 1 part by weight based on 100 parts by weight of the acrylic polymer. (4) The weight average molecular weight of the acrylic polymer is 40×10 4 The pressure-sensitive adhesive composition according to any one of the above (1) to (3). (5) The pressure-sensitive adhesive composition according to any one of the above (1) to (4), which is an optical pressure-sensitive adhesive composition. (6) The pressure-sensitive adhesive composition according to any one of the above (1) to (5), which is a solvent-based pressure-sensitive adhesive composition or a solventless pressure-sensitive adhesive composition. (7) The pressure-sensitive adhesive composition according to any one of the above (1) to (6), wherein the compound A is a nonionic surfactant. (8) The pressure-sensitive adhesive composition according to any one of the above (1) to (7), wherein the compound A has an HLB of 10 or more. (9) The monomer component forming the acrylic polymer is a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 20 carbon atoms at the ester terminal; A monomer having a nitrogen atom; The pressure-sensitive adhesive composition according to any one of the above (1) to (8). (10) The nitrogen atom-containing monomer is represented by the general formula (1): [ka] (In general formula (1), R 1 is a divalent organic group; and (meth)acrylamide. (11) The SP value of the acrylic polymer is 18.0 to 23.0 (MJ / m 3 )1 / 2 The pressure-sensitive adhesive composition according to any one of the above (1) to (10), (12) The pressure-sensitive adhesive composition according to any one of the above (1) to (11), further comprising a peel strength increasing agent. (13) The pressure-sensitive adhesive composition according to the above (12), wherein the peel strength increasing agent is a compound having an alkoxysilyl group.
[0153] (14) An optical pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive composition according to any one of (1) to (13) above. (15) The pressure-sensitive adhesive sheet according to (14) above, wherein the pressure-sensitive adhesive layer has a thickness of 10 μm or more and 200 μm or less. (16) The pressure-sensitive adhesive sheet according to (14) or (15) above, wherein the pressure-sensitive adhesive sheet has a normal peel strength FN1 of 3 N / cm or more, measured after the pressure-sensitive adhesive sheet is attached with its adhesive surface to an adherend and left to stand at 23°C for 30 minutes at a tensile speed of 60 mm / min and a peel angle of 180°. (17) The pressure-sensitive adhesive sheet according to any one of (14) to (16) above, wherein the pressure-sensitive adhesive sheet is attached with the pressure-sensitive adhesive surface to an adherend and left to stand at 23° C. for 30 minutes, and then a drop of water is dropped onto the adherend and the water is allowed to penetrate into one end of the interface between the pressure-sensitive adhesive layer and the adherend, and the water peel force FW1 measured under conditions of a tensile speed of 60 mm / min and a peel angle of 180° is less than 1 N / cm without the need for additional water supply. (18) The pressure-sensitive adhesive sheet according to any one of (14) to (17) above, wherein the pressure-sensitive adhesive sheet has a normal peel strength FN2 of 7 N / cm or more, measured under conditions of a tensile speed of 60 mm / min and a peel angle of 180° after the pressure-sensitive adhesive sheet is attached with its pressure-sensitive adhesive surface to an adherend and left at 60°C for 18 hours. (19) The pressure-sensitive adhesive sheet according to any one of (14) to (18) above, wherein the pressure-sensitive adhesive sheet is attached with the pressure-sensitive adhesive surface to an adherend and left at 60° C. for 18 hours, and then a drop of water is dropped onto the adherend and the water is allowed to penetrate into one end of the interface between the pressure-sensitive adhesive layer and the adherend, and the water peel force FW2 is measured under conditions of a tensile speed of 60 mm / min and a peel angle of 180° without the need for additional water supply, and is less than 1 N / cm. (20) The pressure-sensitive adhesive sheet according to any one of (14) to (18) above, wherein after the pressure-sensitive adhesive surface of the pressure-sensitive adhesive sheet is attached to an adherend and left at 60°C for 18 hours, one drop of water is dropped onto the adherend and the water is allowed to penetrate into one end of the interface between the pressure-sensitive adhesive layer and the adherend, and then, without the need for additional water supply, the water peel force FW2 is measured under conditions of a pulling speed of 60 mm / min and a peel angle of 180°, and is 6 N / cm or more. (21) The pressure-sensitive adhesive sheet according to any one of (14) to (20) above, which has a water peel adhesion loss rate A of 60% or more. (22) The pressure-sensitive adhesive sheet according to any one of (14) to (21) above, which has an increase in peel strength of 20% or more. (23) The pressure-sensitive adhesive sheet according to any one of (14) to (22) above, which has a post-heat water peel adhesion loss rate of 80% or more. (24) The pressure-sensitive adhesive sheet according to any one of (14) to (23) above, which has a haze value of less than 0.7%.
[0154] (25) A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer, the adhesive surface of the pressure-sensitive adhesive sheet is attached to an alkaline glass plate as an adherend, and then allowed to stand at 23°C for 30 minutes. After that, the normal peel strength FN1 measured under conditions of a pulling speed of 60 mm / min and a peel angle of 180° is 2 N / cm or more; A pressure-sensitive adhesive sheet having a water peeling adhesion reduction rate A of 50% or more, where the water peeling adhesion reduction rate A is calculated from the water peeling adhesion force FW1 [N / cm] measured at a tensile tester under conditions of a tensile speed of 60 mm / min and a peel angle of 180 degrees and the normal peeling strength FN1 [N / cm] according to the following formula: (1-(FW1 / FN1))×100; after 30 minutes from attaching the adhesive surface of the pressure-sensitive adhesive sheet to an alkaline glass plate as an adherend in a measurement environment of 23°C and 50% RH, 10 μL to 40 μL of distilled water is dropped onto the adherend and the distilled water is allowed to penetrate into one end of the interface between the pressure-sensitive adhesive layer and the adherend, based on JIS Z0237. (26) A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer, The pressure-sensitive adhesive sheet has an adhesive surface attached to a surface of an alkali glass plate prepared by the float method, the surface having a contact angle with distilled water of 5 degrees to 10 degrees, and an adhesive strength (normal adhesive strength) N0 of 2.0 N / 10 mm or more after one day at room temperature, and a water peeling adhesive strength reduction rate B of 40% or more. Here, the water peeling adhesive strength reduction rate B is determined by: attaching the adhesive surface to a surface of an alkali glass plate prepared by the float method, the surface having a contact angle with distilled water of 5 degrees to 10 degrees, the adhesive surface being attached to a surface of an alkali glass plate prepared by the float method, the surface having a contact angle with distilled water of 5 degrees to 10 degrees after one day at room temperature; dropping 20 μL of distilled water onto the adherend, allowing the distilled water to penetrate into one end of the interface between the pressure-sensitive adhesive layer and the adherend; and then measuring the adhesive strength according to 10.4.1 of JIS Z0237:2009. Method 1: An adhesive sheet calculated according to the 180° peel adhesive strength against a test plate, specifically, using a tensile testing machine at a test temperature of 23°C, a tensile speed of 300 mm / min, and a peel angle of 180°, from the water peel strength N2 [N / 10 mm] and adhesive strength (normal adhesive strength) N0 [N / 10 mm] according to the following formula: (1-(N2 / N0)) x 100. (27) The pressure-sensitive adhesive sheet according to (25) or (26) above, wherein the pressure-sensitive adhesive sheet has a normal peel strength FN1 of 3 N / cm or more, measured under conditions of a tensile speed of 60 mm / min and a peel angle of 180° after the pressure-sensitive adhesive sheet is attached with its adhesive surface to the adherend and left to stand at 23°C for 30 minutes. (28) The pressure-sensitive adhesive sheet according to any one of (25) to (27) above, wherein after the pressure-sensitive adhesive surface of the pressure-sensitive adhesive sheet is attached to the adherend and left to stand at 23° C. for 30 minutes, one drop of water is dropped onto the adherend and the water is allowed to penetrate into one end of the interface between the pressure-sensitive adhesive layer and the adherend, and then, without the supply of additional water, the water peel force FW1 measured under conditions of a tensile speed of 60 mm / min and a peel angle of 180° is less than 1 N / cm. (29) The pressure-sensitive adhesive sheet according to any one of (25) to (28) above, wherein the pressure-sensitive adhesive sheet has a normal peel strength FN2 of 7 N / cm or more, measured under conditions of a tensile speed of 60 mm / min and a peel angle of 180° after the pressure-sensitive adhesive sheet is attached with its pressure-sensitive adhesive surface to the adherend and left to stand at 60°C for 18 hours. (30) The pressure-sensitive adhesive sheet according to any one of (25) to (29) above, wherein after the pressure-sensitive adhesive surface of the pressure-sensitive adhesive sheet is attached to the adherend and left to stand at 60°C for 18 hours, one drop of water is dropped onto the adherend and the water is allowed to penetrate into one end of the interface between the pressure-sensitive adhesive layer and the adherend, and then, without the need for additional water supply, the water peel force FW2 is measured under conditions of a tensile speed of 60 mm / min and a peel angle of 180°, and is less than 1 N / cm. (31) The pressure-sensitive adhesive sheet according to any one of (25) to (29) above, wherein the pressure-sensitive adhesive sheet is attached with the pressure-sensitive adhesive surface to the adherend and left to stand at 60° C. for 18 hours, and then a drop of water is dropped onto the adherend and the water is allowed to penetrate into one end of the interface between the pressure-sensitive adhesive layer and the adherend, and the water peel force FW2 is measured at a tensile speed of 60 mm / min and a peel angle of 180° without the need for additional water supply, and is 6 N / cm or more. (32) The pressure-sensitive adhesive sheet according to any one of (25) to (31) above, which has a water peel adhesion loss rate A of 60% or more. (33) The pressure-sensitive adhesive sheet according to any one of (25) to (32) above, which has an increase in peel strength of 20% or more. (34) The pressure-sensitive adhesive sheet according to any one of (25) to (33) above, which has a post-heat water peel adhesion loss rate of 80% or more. (35) The pressure-sensitive adhesive sheet according to any one of (25) to (34) above, which has a haze value of less than 0.7%. (36) The pressure-sensitive adhesive sheet according to any one of (25) to (35) above, wherein the pressure-sensitive adhesive layer has a thickness of 10 μm or more and 200 μm or less.
[0155] (37) An optical member with a pressure-sensitive adhesive sheet, comprising: the pressure-sensitive adhesive sheet according to any one of (14) to (35) above; and an optical member bonded to one surface of the pressure-sensitive adhesive sheet. (38) A method for removing a pressure-sensitive adhesive sheet attached to an adherend, comprising the steps of: A peeling method comprising a water peeling step of peeling the adhesive sheet from the adherend while progressing the penetration of the aqueous liquid into the interface in accordance with the movement of the peel front, in a state where an aqueous liquid is present at the interface between the adherend and the adhesive sheet at the peel front of the adhesive sheet from the adherend. (39) The peeling method according to the above (38), wherein the pressure-sensitive adhesive sheet is the pressure-sensitive adhesive sheet according to any one of the above (14) to (36). (40) The method for peeling according to (38) or (39) above, wherein in the water peeling step, the peeling front is moved at a speed of 10 mm / min or more. EXAMPLES
[0156] Some examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in these examples. In the following description, "parts" and "%" are by weight unless otherwise specified.
[0157] <Evaluation method> [Measurement of normal peel strength after 30 minutes at 23℃] Under a measurement environment of 23°C and 50% RH, the adhesive sheet to be measured is cut to a size of 10 mm wide and 120 mm long to prepare a test piece. Under the same environment, the adhesive surface of the test piece is pressed against the surface of the adherend by rolling a 2 kg roller back and forth once. The test piece is attached to the adherend so that the distance from the outer edge of the test piece to the outer edge of the adherend is at least 1 mm, preferably 3 mm or more. After leaving it under the same environment for 30 minutes, a cutter knife is inserted into the interface between the test piece and the adherend to peel one end of the test piece in the longitudinal direction from the adherend, and the peel strength is measured using a tensile tester under conditions of a tensile speed of 60 mm / min and a peel angle of 180 degrees in accordance with JIS Z0237. The measurement is performed three times, and the average value is taken as the normal peel strength [N / cm] after 30 minutes at 23°C. An alkaline glass plate (manufactured by Matsunami Glass Industry Co., Ltd., thickness 1.35 mm, blue plate edge polished product) is used as the adherend. Alternatively, an equivalent of an alkali glass plate manufactured by Matsunami Glass Industry Co., Ltd. can be used. As a tensile tester, a universal tensile compression tester (apparatus name "tensile compression tester, TCM-1kNB" manufactured by Minebea Co., Ltd.) or an equivalent can be used. The peel strength is measured so that the peeling of the test piece attached to the adherend proceeds from bottom to top. In addition, in a pressure-sensitive adhesive sheet in which a bonding mode in which a part or all of the pressure-sensitive adhesive layer is photocured after bonding to the adherend is applied, the test piece after being attached to the adherend is irradiated with light through the above-mentioned alkali glass plate in an environment of 23°C and 50% RH. In addition, when the measurement target is a double-sided pressure-sensitive adhesive sheet, a PET film can be attached to one of the adhesive surfaces of the double-sided pressure-sensitive adhesive sheet as described below to back it up, and the measurement can be performed.
[0158] [Measurement of water peeling force after 30 minutes at 23℃] Under a measurement environment of 23°C and 50% RH, the pressure sensitive adhesive sheet to be measured is cut to a size of 10 mm in width and 120 mm in length to prepare a test piece. Under the same environment, the pressure sensitive adhesive surface of the test piece is pressed against the surface of the adherend by rolling a 2 kg roller back and forth once. After leaving it under the same environment for 30 minutes, a drop of distilled water (about 10 μL to about 40 μL) is dropped on the surface of the adherend exposed from one end in the longitudinal direction of the test piece near the end. Then, a cutter knife is inserted into the interface between the test piece and the adherend to allow the water to enter the interface, and then, without supplying new water, the peel strength is measured using a tensile tester at a tensile speed of 60 mm / min and a peel angle of 180 degrees in accordance with JIS Z0237. The measurement is performed three times, and the average value is taken as the water peel strength [N / cm] after 30 minutes at 23°C. The adherend, tensile tester, and other items are basically the same as those in the measurement of normal peel strength after 30 minutes at 23°C.
[0159] [Measurement of normal peel strength after 18 hours at 60℃] Under a measurement environment of 23°C and 50% RH, the adhesive sheet to be measured is cut to a size of 10 mm wide and 120 mm long to prepare a test piece. Under the same environment, the adhesive surface of the test piece is pressed against the surface of the adherend by rolling a 2 kg roller back and forth once. This is left in an environment of 60°C for 18 hours, and then left in an environment of 23°C and 50% RH for 30 minutes, and a cutter knife is inserted into the interface between the test piece and the adherend to peel one end of the longitudinal direction of the test piece from the adherend, and the peel strength is measured using a tensile tester under conditions of a tensile speed of 60 mm / min and a peel angle of 180 degrees in accordance with JIS Z0237. The measurement is performed three times, and the average value is taken as the normal peel strength [N / cm] after 18 hours at 60°C. The adherend, tensile tester, and other items are basically the same as those for the measurement of the normal peel strength after 30 minutes at 23°C.
[0160] [Measurement of water peeling strength after 18 hours at 60℃] Under a measurement environment of 23°C and 50% RH, the adhesive sheet to be measured is cut to a size of 10 mm in width and 120 mm in length to prepare a test piece. Under the same environment, the adhesive surface of the test piece is pressed against the surface of the adherend by rolling a 2 kg roller back and forth once. After leaving it in an environment of 60°C for 18 hours, it is left in an environment of 23°C and 50% RH for 30 minutes, and one drop (about 10 μL to about 40 μL) of distilled water is dropped on the surface of the adherend exposed from one end in the vicinity of one end in the longitudinal direction of the test piece. Then, a cutter knife is inserted into the interface between the test piece and the adherend to allow the water to enter the interface, and then, without supplying new water, the peel strength is measured using a tensile tester in accordance with JIS Z0237 under the conditions of a tensile speed of 60 mm / min and a peel angle of 180 degrees. The measurement is performed three times, and the average value is taken as the water peel strength [N / cm] after 18 hours at 60°C. The adherend, tensile tester, and other items are basically the same as for the measurement of normal peel strength after 30 minutes at 23°C.
[0161] [Haze value] The adhesive surface of the adhesive layer (a 50 μm thick adhesive layer in the examples described below) is attached to one side of an alkali glass with a haze value of 0.1% to form a laminate of the adhesive layer and the alkali glass, and then the haze value is measured using a haze meter ("MR-100", manufactured by Murakami Color Research Laboratory). In the measurement, the alkali glass with the adhesive layer attached is positioned so that the adhesive layer faces the light source. Since the haze value of the alkali glass is 0.1%, the haze value [%] of the adhesive layer is determined by subtracting 0.1% from the measured value.
[0162] [Normal adhesive strength N0] The adhesive sheet to be measured is cut into a rectangular shape of 10 mm width and 120 mm length to prepare a test piece. The adhesive surface of the test piece is attached to the adherend with a hand roller to prepare a sample for evaluation. The sample is placed in an autoclave and treated for 15 minutes under conditions of a pressure of 5 atm and a temperature of 50°C. The evaluation sample removed from the autoclave is kept in an environment of 23°C and 50% RH for one day, and then, under the same environment, a cutter knife is inserted into the interface between the test piece and the adherend to peel one end of the test piece in the longitudinal direction from the adherend, and the peel strength is measured in accordance with JIS Z0237:2009, "10.4.1 Method 1: 180° peel adhesion to test plate", specifically, at a test temperature of 23°C, a tensile speed of 300 mm / min, and a peel angle of 180 degrees using a tensile testing machine.
[0163] [Water peeling force N2] The adhesive sheet to be measured is cut into a rectangular shape of 10 mm width and 120 mm length to prepare a test piece. The adhesive surface of the test piece is attached to the adherend with a hand roller to prepare a sample for evaluation. The sample is placed in an autoclave and treated for 15 minutes under conditions of a pressure of 5 atm and a temperature of 50°C. The evaluation sample taken out of the autoclave is kept in an environment of 23°C and 50% RH for one day, and then, under the same environment, 20 μL of distilled water is dropped on the surface of the adherend exposed from one end of the test piece in the vicinity of one end in the longitudinal direction of the test piece. Then, a cutter knife is inserted into the interface between the test piece and the adherend to allow the water to penetrate into the interface, and the peel strength is measured according to "10.4.1 Method 1: 180° peel adhesion to test plate" of JIS Z0237:2009, specifically, at a test temperature of 23°C, a tensile tester at a tensile speed of 300 mm / min, and a peel angle of 180°. Note that the water used in measuring the water peel force N2 is only 20 μL of distilled water dropped onto the adherend before peeling begins.
[0164] In the measurement of the normal adhesive strength N0 and the water peeling strength N2, the adherend is an alkali glass plate prepared by the float method, and the contact angle of the surface to which the test piece is attached to distilled water is 5 degrees to 10 degrees. For example, an alkali glass plate (thickness 1.35 mm, blue plate edge polished product) manufactured by Matsunami Glass Industry Co., Ltd. or its equivalent can be used as the adherend. The test piece is attached to the adherend so that the distance from the outer edge of the test piece to the outer edge of the adherend is at least 10 mm or more, preferably 15 mm or more. In the case of a pressure-sensitive adhesive sheet containing a photocrosslinkable pressure-sensitive adhesive layer, the sample taken out of the autoclave is irradiated with light through the alkali glass plate under an environment of 23°C and 50% RH, and then the peel strength is measured. The light irradiation conditions (wavelength, irradiation intensity, irradiation time, etc.) are appropriately set according to the composition and thickness of the pressure-sensitive adhesive layer (for example, the conditions described below). As a tensile tester, a universal tensile / compression tester (device name "Tension / Compression Tester, TCM-1kNB" manufactured by Minebea Co., Ltd.) or an equivalent can be used. The peel strength is measured so that the peeling of the test piece attached to the adherend proceeds from bottom to top. When making the measurement, if necessary, the test piece can be reinforced by attaching a suitable backing material to the back side of the adhesive sheet (the surface opposite to the adhesive surface to be measured). As a backing material, for example, a PET film with a thickness of about 25 μm can be used.
[0165] The contact angle of the above-mentioned alkali glass plate is measured as follows. That is, in a measurement atmosphere of 23°C and 50% RH, the measurement is performed by the sessile drop method using a contact angle meter (manufactured by Kyowa Interface Science Co., Ltd., product name "DMo-501 type", control box "DMC-2", control and analysis software "FAMAS (version 5.0.30)"). The amount of distilled water dropped is 2 μL, and the contact angle is calculated by the Θ / 2 method from the image taken 5 seconds after the drop (performed with N5).
[0166] Other matters concerning the measurement of normal adhesive strength N0 and water peeling strength N2 shall basically conform to the measurement of normal peeling strength after 30 minutes at 23°C. Similarly, for matters not specified regarding the measurement of normal peeling strength after 30 minutes at 23°C, the contents of the measurement method for normal adhesive strength N0 and water peeling strength N2 shall be referred to as appropriate.
[0167] <Example 1> (Preparation of Pressure-Sensitive Adhesive Composition) In a reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer and a stirrer, 64.5 parts of n-butyl acrylate (BA), 6 parts of cyclohexyl acrylate (CHA), 9.6 parts of N-vinyl-2-pyrrolidone (NVP), 5 parts of isostearyl acrylate (iSTA) and 14.9 parts of 4-hydroxybutyl acrylate (4HBA) were charged as monomer components, 0.07 parts of α-thioglycerol as a chain transfer agent, and 122 parts of ethyl acetate as a polymerization solvent. 0.2 parts of 2,2'-azobisisobutyronitrile (AIBN) were added as a thermal polymerization initiator, and solution polymerization was carried out under a nitrogen atmosphere to obtain a solution containing an acrylic polymer with Mw of 600,000.
[0168] To the solution obtained above, 0.33 parts of 3-glycidoxypropyltrimethoxysilane (trade name: KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) as a silane coupling agent, 0.1 parts of nonionic surfactant A (polyoxyethylene sorbitan monolaurate, HLB 13.3, trade name: Rheodol TW-L106, manufactured by Kao Corporation) as compound A, 0.1 parts of an isocyanate-based crosslinking agent (trimethylolpropane / xylylene diisocyanate adduct (manufactured by Mitsui Chemicals, Takenao Corporation) per 100 parts of the monomer components used in preparing the solution, A solvent-based pressure-sensitive adhesive composition was prepared by adding 0.09 parts of Tono D-110N (solid content concentration 75% by mass) based on solid content, 0.4 parts of an acrylic oligomer, 0.02 parts of dioctyltin dilaurate (Tokyo Fine Chemical Co., Ltd., Envirizer OL-1) as a crosslinking accelerator, 3 parts of acetylacetone as a crosslinking retarder, 2.7 parts of dipentaerythritol hexaacrylate (DPHA) as a polyfunctional monomer, and 0.22 parts of Irgacure 184 (Ciba Specialty Chemicals) as a photopolymerization initiator, and mixing them uniformly.
[0169] The acrylic oligomer used was synthesized by the following method. [Synthesis of acrylic oligomers] 100 parts of toluene, 60 parts of dicyclopentanyl methacrylate (DCPMA) (trade name: FA-513M, Hitachi Chemical Co., Ltd.), 40 parts of methyl methacrylate (MMA), and 3.5 parts of α-thioglycerol as a chain transfer agent were charged into a four-neck flask. Then, after stirring at 70°C under a nitrogen atmosphere for 1 hour, 0.2 parts of AIBN were charged as a thermal polymerization initiator, and the mixture was reacted at 70°C for 2 hours, and then at 80°C for 2 hours. Thereafter, the reaction liquid was charged under a temperature atmosphere of 130°C, and the toluene, chain transfer agent, and unreacted monomers were dried and removed to obtain a solid acrylic oligomer. The Tg of this acrylic oligomer was 144°C, and the Mw was 4300.
[0170] (Preparation of adhesive sheet) The adhesive composition obtained above was applied to a 38 μm thick release film R1 (Mitsubishi Plastics, MRF#38) with one side of the polyester film being the release surface, and dried at 135° C. for 2 minutes to form an adhesive layer with a thickness of 50 μm. A 50 μm PET film was attached to this adhesive layer to obtain a laminated sheet in which a PET film (backing film), an adhesive layer (support-less double-sided adhesive sheet), and a release film R1 were laminated in this order. The surface of the adhesive sheet in this example that is attached to the adherend is protected by the release film R1.
[0171] <Example 2> An adhesive composition was prepared in the same manner as in Example 1, except that nonionic surfactant B (polyoxyethylene sorbitan monooleate, HLB 10.0, product name: Rheodol TW-O106V, manufactured by Kao Corporation) was used instead of nonionic surfactant A as compound A, and an adhesive sheet according to this example was obtained.
[0172] <Example 3> An adhesive composition was prepared in the same manner as in Example 1, except that nonionic surfactant C (polyoxyethylene lauryl ether, HLB 9.7, product name: Emulgen 105, manufactured by Kao Corporation) was used instead of nonionic surfactant A as compound A, and an adhesive sheet according to this example was obtained.
[0173] <Example 4> An adhesive composition was prepared in the same manner as in Example 1, except that nonionic surfactant D (sorbitan monolaurate, HLB 8.6, product name: Rheodol SP-L10, manufactured by Kao Corporation) was used instead of nonionic surfactant A as compound A, and an adhesive sheet according to this example was obtained.
[0174] <Example 5> An adhesive composition was prepared in the same manner as in Example 1, except that nonionic surfactant E (sorbitan monooleate, HLB 4.3, product name: Rheodol SP-O10V, manufactured by Kao Corporation) was used instead of nonionic surfactant A as compound A, and an adhesive sheet according to this example was obtained.
[0175] <Example 6> An adhesive composition was prepared in the same manner as in Example 1, except that an anionic surfactant (sodium lauryl sulfate, product name: EMAL 10G, manufactured by Kao Corporation) was used instead of the nonionic surfactant A as compound A, and an adhesive sheet according to this example was obtained.
[0176] <Example 7> An adhesive composition was prepared in the same manner as in Example 1, except that 0.05 parts of nonionic surfactant F (polyoxyethylene lauryl ether, HLB 12.1, product name: Emulgen 108, manufactured by Kao Corporation) was used instead of 0.1 parts of nonionic surfactant A, and an adhesive sheet according to this example was obtained.
[0177] <Example 8> An adhesive composition was prepared in the same manner as in Example 1, except that the amount of nonionic surfactant A used was changed to 2 parts per 100 parts of the monomer component, and an adhesive sheet according to this example was obtained.
[0178] <Example 9> An adhesive composition was prepared in the same manner as in Example 4, except that the amount of nonionic surfactant D used was changed to 2 parts per 100 parts of the monomer component, and an adhesive sheet according to this example was obtained.
[0179] <Example 10> An adhesive composition was prepared in the same manner as in Example 1, except that Compound A was not used, and an adhesive sheet according to this example was obtained.
[0180] <Example 11> (Preparation of Pressure-Sensitive Adhesive Composition) A monomer mixture (100 parts) containing 2-ethylhexyl acrylate (2EHA), NVP, hydroxyethyl acrylate (HEA) and isobornyl acrylate (IBXA) in a weight ratio of 80 / 35 / 5 / 30 was placed in a four-neck flask together with 0.05 parts of Irgacure 651 (manufactured by Ciba Specialty Chemicals) and 0.05 parts of Irgacure 184 (manufactured by Ciba Specialty Chemicals) as photopolymerization initiators, and irradiated with ultraviolet light under a nitrogen atmosphere until the viscosity (BH viscometer, No. 5 rotor, 10 rpm, measurement temperature 30°C) reached approximately 15 Pa s, to prepare a monomer syrup containing a partial polymer of the monomer mixture. To 100 parts of this monomer syrup, 0.15 parts of nonionic surfactant G (polyoxyethylene sorbitan monolaurate, HLB 16.7, product name: Rheodol TW-L120, manufactured by Kao Corporation) as compound A was added, and further 0.13 parts of 1,6-hexanediol diacrylate (HDDA) and 0.33 parts of a photopolymerization initiator (product name: Irgacure 651, manufactured by Chiba Specialty Chemicals) were added and mixed uniformly to prepare an ultraviolet-curable adhesive composition.
[0181] The adhesive composition obtained above was applied to a 38 μm-thick release film R1 (Mitsubishi Plastics, MRF#38) with one side of a polyester film being the release surface, and a 38 μm-thick release film R2 (Mitsubishi Plastics, MRE#38) with one side of a polyester film being the release surface was placed over it to block air, and the adhesive layer was cured by irradiating ultraviolet light to form a 50 μm-thick adhesive layer. Next, the release film R2 covering the adhesive layer was peeled off, and a 50 μm-thick PET film was attached to obtain a laminated sheet in which a PET film (backing film), an adhesive layer (support-less double-sided adhesive sheet), and a release film R1 were laminated in this order. The surface of the adhesive sheet in this example that is attached to the adherend is protected by the release film R1.
[0182] <Example 12 to Example 14> The adhesive composition of each example was prepared in the same manner as in Example 11, except that the amount of nonionic surfactant G used was changed to 0.25 parts (Example 12), 0.5 parts (Example 13), or 1.0 part (Example 14) per 100 parts of monomer syrup, and the adhesive sheet of each example was obtained.
[0183] <Example 15> An adhesive composition was prepared in the same manner as in Example 12, except that PEG400 (polyethylene glycol, average molecular weight 360 to 440) was used as compound A instead of nonionic surfactant G, and an adhesive sheet according to this example was obtained.
[0184] <Example 16 and Example 17> The adhesive composition of each example was prepared in the same manner as in Example 15, except that the amount of PEG400 used was changed to 0.5 part (Example 16) or 1.0 part (Example 17) per 100 parts of monomer syrup, and the adhesive sheet of each example was obtained.
[0185] <Example 18> An adhesive composition was prepared in the same manner as in Example 11, except that Compound A was not used, and an adhesive sheet according to this example was obtained.
[0186] <Example 19> An acrylic polymer-containing solution prepared in the same manner as in Example 1 was mixed with 0.1 parts of a nonionic surfactant G (polyoxyethylene sorbitan monolaurate, HLB 16.7, product name: Rheodol TW-L120, manufactured by Kao Corporation) as compound A, and 0.2 parts of an isocyanate-based crosslinking agent (trimethylolpropane / xylylene diisocyanate adduct (Takenate D-110N, manufactured by Mitsui Chemicals, Inc., solid content concentration 75% by mass) based on the solid content per 100 parts of the monomer components used in the preparation of the solution. A solvent-based pressure-sensitive adhesive composition was prepared by adding 0.09 parts of the above-mentioned acrylic oligomer, 0.4 parts of an acrylic oligomer (the same as the acrylic oligomer used in Example 1), 0.02 parts of dioctyltin dilaurate (Embirizer OL-1, manufactured by Tokyo Fine Chemical Co., Ltd.) as a crosslinking accelerator, 3 parts of acetylacetone as a crosslinking retarder, 2.7 parts of DPHA as a polyfunctional monomer, and 0.22 parts of Irgacure 184 (manufactured by Chiba Specialty Chemicals) as a photopolymerization initiator, and mixing them uniformly. A laminate sheet was obtained in the same manner as in Example 1, except that the above solvent-based adhesive composition was used, in which a PET film (backing film), a 50 μm thick adhesive layer (support-less double-sided adhesive sheet), and a release film R1 were laminated in that order.
[0187] <Example 20> An adhesive composition according to this example was prepared in the same manner as in Example 19, except that the amount of nonionic surfactant G used was changed to 0.3 parts per 100 parts of the monomer component, and an adhesive sheet according to this example was obtained.
[0188] <Example 21> An adhesive composition was prepared in the same manner as in Example 20, except that nonionic surfactant H (polyoxyethylene lauryl ether, HLB 15.3, product name: Emulgen 120, manufactured by Kao Corporation) was used instead of nonionic surfactant G as compound A, and an adhesive sheet according to this example was obtained.
[0189] <Example 22> (Preparation of Pressure-Sensitive Adhesive Composition) A reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer and a stirrer was charged with 64.5 parts of BA, 6 parts of CHA, 18 parts of NVP, 5 parts of iSTA and 14.9 parts of 4HBA as monomer components, 0.07 parts of α-thioglycerol as a chain transfer agent and 122 parts of ethyl acetate as a polymerization solvent, and 0.2 parts of AIBN was added as a thermal polymerization initiator to carry out solution polymerization under a nitrogen atmosphere, thereby obtaining a solution containing an acrylic polymer with Mw of 600,000. To the solution obtained above, 0.1 parts of nonionic surfactant G (polyoxyethylene sorbitan monolaurate, HLB 16.7, trade name: Rheodol TW-L120, manufactured by Kao Corporation) as compound A, 0.09 parts of isocyanate-based crosslinking agent (trimethylolpropane / xylylene diisocyanate adduct (manufactured by Mitsui Chemicals, Takenate D-110N, solid content concentration 75 mass%) based on solid content, 0.4 parts of acrylic oligomer (the same as the acrylic oligomer used in Example 1), 0.02 parts of dioctyltin dilaurate (manufactured by Tokyo Fine Chemicals, Envirizer OL-1) as a crosslinking accelerator, 3 parts of acetylacetone as a crosslinking retarder, 2.7 parts of DPHA as a polyfunctional monomer, and 0.22 parts of Irgacure 184 (manufactured by Ciba Specialty Chemicals) as a photopolymerization initiator were added and mixed uniformly to prepare a solvent-based pressure-sensitive adhesive composition. A laminate sheet was obtained in the same manner as in Example 1, except that the above solvent-based adhesive composition was used, in which a PET film (backing film), a 50 μm thick adhesive layer (support-less double-sided adhesive sheet), and a release film R1 were laminated in that order.
[0190] <Example 23> An adhesive composition according to this example was prepared in the same manner as in Example 22, except that the amount of nonionic surfactant G used was changed to 0.3 parts per 100 parts of the monomer component, and an adhesive sheet according to this example was obtained.
[0191] <Example 24> A monomer syrup containing a partial polymerization product of the monomer mixture was prepared by photopolymerization under a nitrogen atmosphere by irradiating with ultraviolet light until the viscosity (BH viscometer, No. 5 rotor, 10 rpm, measurement temperature 30°C) reached approximately 15 Pa s. To 100 parts of this monomer syrup, 9 parts of HEA, 8 parts of 4HBA, 0.1 part of DPHA as a polyfunctional monomer, and 0.1 part of nonionic surfactant G (polyoxyethylene sorbitan monolaurate, HLB 16.7, product name: Rheodol TW-L120, manufactured by Kao Corporation) were added and mixed uniformly to prepare an ultraviolet-curable pressure-sensitive adhesive composition. A laminated sheet was obtained in the same manner as in Example 11, except that the above ultraviolet-curable adhesive composition was used, in which a PET film (backing film), a 50 μm thick adhesive layer (support-less double-sided adhesive sheet), and a release film R1 were laminated in that order.
[0192] <Example 25~Example 26> The adhesive composition of each example was prepared in the same manner as in Example 24, except that the amount of nonionic surfactant G used was changed to 0.3 parts (Example 25) or 0.5 parts (Example 26) per 100 parts of monomer syrup, and the adhesive sheet of each example was obtained.
[0193] <Performance evaluation> The obtained pressure-sensitive adhesive sheet was measured for normal peel strength [N / cm] and water peel strength [N / cm] after 30 minutes at 23°C, and normal peel strength [N / cm] and water peel strength [N / cm] after 18 hours at 60°C. The results are shown in Tables 1 to 4. In Tables 3 and 4, the solvent-type pressure-sensitive adhesives of Examples 19 to 21 are described as "solvent-type B" and the solvent-type pressure-sensitive adhesives of Examples 22 to 23 are described as "solvent-type C" for the purpose of identifying the difference in basic composition from the solvent-type pressure-sensitive adhesives of Examples 1 to 10 (based on this relationship, the solvent-type pressure-sensitive adhesives of Examples 1 to 10 are also referred to as "solvent-type A"). Similarly, the photocurable pressure-sensitive adhesives of Examples 24 to 26 are described as "photocurable B" for the purpose of identifying the difference in basic composition from the photocurable pressure-sensitive adhesives of Examples 11 to 18 (based on this relationship, the photocurable pressure-sensitive adhesives of Examples 11 to 18 are also referred to as "photocurable A"). Furthermore, the normal adhesive strength N0 [N / 10 mm] and water peel strength N2 [N / 10 mm] of the obtained pressure-sensitive adhesive sheet were measured. In addition, in Examples 1 to 23, all peel strength measurements were performed by attaching the pressure-sensitive adhesive sheet to an alkaline glass plate as an adherend using the above-mentioned method, irradiating light through the alkaline glass plate in an environment of 23°C and 50% RH, and then performing the above-mentioned method. More specifically, after the pressure-sensitive adhesive sheet was attached to the adherend, the adhesive sheet was irradiated with light using a high-pressure mercury lamp (300 mW / cm 2 ) with an accumulated light dose of 3000mJ / cm 2 The adhesive layer included in the pressure-sensitive adhesive sheets according to Examples 1 to 23 was photocured by irradiating the adhesive with ultraviolet light, and then the peel strength was measured. For Examples 24 to 26, the pressure-sensitive adhesive sheet was attached to the adherend, and then the peel strength was measured without irradiating the adhesive with light after the above-mentioned lamination.
[0194] [Table 1]
[0195] [Table 2]
[0196] [Table 3]
[0197] [Table 4]
[0198] As shown in Table 1, in Example 10, which used a solvent-based adhesive that did not contain at least one compound A selected from a surfactant and a compound having a polyoxyalkylene skeleton, the water peeling force after 30 minutes at 23°C was 1.4 N / cm, whereas in Examples 1 to 9, which used a solvent-based adhesive containing compound A, the water peeling force after 30 minutes at 23°C was less than 1.3 N / cm. The inclusion of compound A improved the water peeling force. In particular, in Examples 1, 2, and 7, which used nonionic surfactants A, B, or F as compound A, excellent results were obtained, with the water peeling force after 30 minutes at 23°C being less than 1.0 N / cm. This is thought to be because these nonionic surfactants had a relatively high HLB (specifically, HLB 10 or more). In addition, in Examples 1 to 7, the normal peeling force after 30 minutes at 23°C was approximately 4 N / cm or more, and they had good adhesive strength, whereas in Examples 8 and 9, in which the amount of compound A was increased to 2 parts, the water peeling force tended to decrease, but the above-mentioned decrease in the normal peeling force was observed. A tendency for the haze value to increase was also observed in Examples 8 and 9. In addition, in Examples 1 to 10, the release force increasing agent was contained, and the normal release force after 18 hours at 60°C was significantly increased (about twice or more) compared to after 30 minutes at 23°C.
[0199] The photocurable adhesives shown in Table 2 showed better water peeling properties. Specifically, in Examples 11 to 17 using a photocurable adhesive using Compound A, the water peeling strength after 30 minutes at 23°C was less than 1.0 N / cm, which was superior to Example 18 (water peeling strength of 3.7 N / cm) in which Compound A was not used. In addition, in Examples 11 to 13 and Examples 15 to 16 in which the amount of Compound A used was less than 1 part, the normal peeling strength after 30 minutes at 23°C was approximately 4 N / cm or more, and had high adhesive strength, while in Examples 14 and 17 in which the amount of Compound A was increased to 1 part, a decrease in the normal peeling strength was observed (less than 4 N / cm). In addition, in these photocurable adhesives, the normal peeling strength after 18 hours at 60°C was higher than that after 30 minutes at 23°C, while the water peeling strength after 18 hours at 60°C was comparable to that after 30 minutes at 23°C.
[0200] As shown in Table 3, in Examples 19 to 23 using a solvent-based adhesive containing Compound A having a high HLB, better water peelability was confirmed. In these examples, the normal peel strength after 30 minutes at 23°C also tended to be higher than in Examples 1 to 9. In addition, in these examples, a peel strength increasing agent was not used, and the increase in normal peel strength after 18 hours at 60°C was suppressed, and excellent water peelability was maintained even after 18 hours at 60°C. Among them, Examples 22 to 23 showed high normal peel strength both after 30 minutes at 23°C and after 18 hours at 60°C, while maintaining water peelability. As shown in Table 4, Examples 24 to 26 using a photocurable adhesive also had good normal peel strength and excellent water peelability. In these examples, a peel strength increasing agent was not used, and the increase in normal peel strength after 18 hours at 60°C was suppressed, and excellent water peelability was also obtained even after 18 hours at 60°C.
[0201] Although not shown in the table, the pressure-sensitive adhesive sheets according to Examples 1 to 9, 11 to 17, and 19 to 26 satisfied the requirement that the normal adhesive strength N0 was 2.0 N / 10 mm or more and the water peeling adhesive strength reduction rate B was 40% or more. The water peeling adhesive strength reduction rate B was calculated from the water peeling strength N2 [N / 10 mm] and the normal adhesive strength N0 [N / 10 mm] by the following formula: (1-(N2 / N0)) x 100. In the above examples, the normal peeling strength and the water peeling strength were both higher at a pulling speed of 300 mm / min (normal adhesive strength N0 and water peeling strength N2) than at a pulling speed of 60 mm / min (normal peeling strength and water peeling strength after 30 minutes at 23°C). This tendency is a general tendency of pressure-sensitive adhesives.
[0202] Although specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above. [Explanation of symbols]
[0203] 1,2 Adhesive sheet 10 Adhesive layer 10A One surface (adhesive side) 10B Other surface 20 Support 20A front page 20B Second side (back) 30,31,32 Release Liner 50 Adhesive sheet with release liner 70 Optical Components 100 Adhesive sheet attached material
Claims
1. An optical pressure-sensitive adhesive composition comprising an acrylic polymer, The monomer components forming the acrylic polymer contain less than 20% by weight of alkoxyalkyl (meth)acrylate and less than 20% by weight of alkoxypolyalkylene glycol (meth)acrylate, The monomer component contains 5% by weight or more of a hydroxyl group-containing monomer, The pressure-sensitive adhesive composition further comprises at least one compound A selected from a surfactant and a compound having a polyoxyalkylene skeleton, The HLB of the compound A is 10 or more, The SP value of the acrylic polymer is 18.0 to 21.0 (MJ / m 3 ) 1 / 2 The optical pressure-sensitive adhesive composition according to claim 1,
2. An optical pressure-sensitive adhesive composition comprising an acrylic polymer, The monomer component forming the acrylic polymer contains 5% by weight or more of a hydroxyl group-containing monomer, The pressure-sensitive adhesive composition further comprises at least one compound A selected from a surfactant and a compound having a polyoxyalkylene skeleton, The HLB of the compound A is 10 or more, The content of the compound A is less than 1 part by weight based on 100 parts by weight of the acrylic polymer, The SP value of the acrylic polymer is 18.0 to 21.0 (MJ / m 3 ) 1 / 2 The pressure-sensitive adhesive composition.
3. The pressure-sensitive adhesive composition according to claim 1 or 2, which is a solvent-based pressure-sensitive adhesive composition or a solventless pressure-sensitive adhesive composition.
4. The pressure-sensitive adhesive composition according to any one of claims 1 to 3, wherein the compound A is a nonionic surfactant.
5. The monomer components forming the acrylic polymer are a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 20 carbon atoms at the ester terminal; A monomer having a nitrogen atom; The pressure-sensitive adhesive composition according to any one of claims 1 to 4, comprising:
6. The nitrogen atom-containing monomer is represented by the general formula (1): 【Chemistry 1】 (In general formula (1), R 1 is a divalent organic group; 6. The pressure-sensitive adhesive composition according to claim 5, wherein the monomer is one or more monomers selected from the group consisting of N-vinyl cyclic amides represented by the following formula:
7. The pressure-sensitive adhesive composition according to any one of claims 1 to 6, further comprising a peel strength increasing agent.
8. The pressure-sensitive adhesive composition according to claim 7 , wherein the peel strength increasing agent is a compound having an alkoxysilyl group.
9. An optical pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive composition according to any one of claims 1 to 8.
10. A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer, The pressure-sensitive adhesive layer contains an acrylic polymer, The monomer component forming the acrylic polymer contains 5% by weight or more of a hydroxyl group-containing monomer, The SP value of the acrylic polymer is 18.0 to 21.0 (MJ / m 3 ) 1 / 2 and the adhesive surface of the pressure-sensitive adhesive sheet is attached to an alkaline glass plate as an adherend, and the sheet is allowed to stand at 23° C. for 30 minutes. After that, the normal peel strength FN1 measured under conditions of a pulling speed of 60 mm / min and a peel angle of 180° is 2 N / cm or more; A pressure-sensitive adhesive sheet having a water peeling adhesion reduction rate A of 50% or more, wherein the water peeling adhesion reduction rate A is calculated from the water peeling adhesion force FW1 [N / cm] measured at a tensile tester under conditions of a tensile speed of 60 mm / min and a peel angle of 180° and the normal peeling strength FN1 [N / cm] according to the following formula: (1-(FW1 / FN1))×100; after 30 minutes from attaching the adhesive surface of the pressure-sensitive adhesive sheet to an alkaline glass plate as an adherend in a measurement environment of 23° C. and 50% RH, 10 μL to 40 μL of distilled water is dropped onto the adherend and the distilled water is allowed to penetrate into one end of the interface between the pressure-sensitive adhesive layer and the adherend, according to JIS Z0237.
11. The pressure-sensitive adhesive sheet according to claim 9 or 10, wherein the pressure-sensitive adhesive layer has a thickness of 10 μm or more and 200 μm or less.
12. An optical member with a pressure-sensitive adhesive sheet comprising: the pressure-sensitive adhesive sheet according to any one of claims 9 to 11; and an optical member bonded to one surface of the pressure-sensitive adhesive sheet.
13. A method for removing the pressure-sensitive adhesive sheet according to any one of claims 9 to 11 attached to an adherend, comprising the steps of: A peeling method comprising a water peeling step of peeling the adhesive sheet from the adherend while progressing the penetration of the aqueous liquid into the interface in accordance with the movement of the peel front, in a state where an aqueous liquid is present at the interface between the adherend and the adhesive sheet at the peel front of the adhesive sheet from the adherend.
Citation Information
Patent Citations
Acrylic self-adhesive composition
JP1998168407A
Pressure sensitive adhesive composition for protective film for optical member surface, and protective film for optical member surface
JP2007297446A
Acrylic adhesive composition for polarizing plates
JP2009516048A
Acrylic adhesive composition
JP2009519372A
Pressure-sensitive adhesive agent and optical film
JP2010159346A