Manufacturing method of mineral wool products
A two-step urea addition process for mineral wool production reduces formaldehyde emissions and improves stability, addressing environmental and handling concerns associated with existing phenol-formaldehyde resin methods.
Patent Information
- Application Number
- JP2022196060
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-04-27
- Filing Date
- 2022-12-08
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2039-04-26
AI Technical Summary
Existing methods for producing mineral wool products using phenol-formaldehyde resins result in high formaldehyde emissions due to the use of urea as a formaldehyde scavenger, which are not thermally stable and require additional processing steps, leading to environmental and handling concerns.
A method involving a two-step urea addition process, where a first amount of urea is added to phenol-formaldehyde resol to reduce free formaldehyde content, followed by a second addition just before application to mineral fibers, ensuring stable pre-reactants with reduced formaldehyde emissions.
The method produces mineral wool products with significantly lower formaldehyde emissions, improved stability, and reduced ammonia emissions, eliminating the need for formaldehyde scavengers and additional processing steps.
Smart Images

Figure 0007559035000001
Abstract
Description
[Technical field]
[0001] [1] The present invention relates to a method for producing mineral wool products using a binder based on phenol-formaldehyde resol. The resulting mineral wool products are primarily intended for use as thermal and acoustic insulation for objects such as buildings, transportation and air conduction ducts, appliances, etc. [Background technology]
[0002] [2] Mineral wool products are widely used for thermal and acoustic insulation, as well as fire protection, in various parts of buildings, transport or appliances. Mineral wool materials are primarily randomly interwoven masses of mineral fibers with various lengths, usually bound together by a hardened resin-based binder. Three types of mineral materials are most commonly used: glass, stone or slag. The manufacturing methods for mineral wool products are well known in the art and typically include melting the mineral materials to a suitable temperature, fiberizing the molten mixture into fine fibers, applying (mostly spraying) an uncured liquid binder composition to the individual fibers (they still have some residual heat), collecting the fibers and forming a primary fleece on a perforated conveyor, densifying the fleece and curing the binder at high temperatures. The cured mat is then cut to the desired size using cross- and end trimmers before being packaged for transportation.
[0003] [3] The most widely used binders are based on thermosetting hydrous phenol-formaldehyde resols due to their good performance and attractive low cost. Common phenol-formaldehyde resols used for this purpose are prepared by methylolation of phenol with formaldehyde and partial condensation in aqueous solution catalyzed by a strongly alkaline substance. A detailed description of the preparation and properties of phenol-formaldehyde resols suitable for use in binders for mineral wool can be found, for example, in Chapter 10 of "Phenolic Resins: A Century of Progress", edited by L. Pilato, published by Springer-Verlag in 2010.
[0004] [4] Phenol-formaldehyde resols for mineral wool production are characterized by being prepared with a stoichiometric excess of formaldehyde, which results in free, unreacted formaldehyde being mixed with the resol reaction product. In recent years, there has been growing concern over the toxicity of formaldehyde and formaldehyde-containing materials, leading to the development of approaches to address this concern.
[0005] [5] In this respect, urea has been found to be very useful, so that today it is almost always added to the resols used in mineral wool production. Urea plays a dual role: first, it acts as a formaldehyde scavenger, reacting with the free formaldehyde in the resol and thus reducing its concentration; second, it acts as a resin extender, being incorporated into the cured thermosetting binder without unacceptably reducing its properties, thus increasing the usable solids content of the binder at low cost. Commonly used urea extender levels range from 20 to 40% by weight, based on the sum of the dry weight content of the resol and the weight of urea, depending on the starting resol. It has been reported that higher levels of urea extender, if no measures are taken, lead to a deterioration of the mechanical properties of the binder, especially after aging, along with the generation of high ammonia emissions and the formation of troublesome "blue smoke" during mineral wool production.
[0006] [6] Once the reaction between the phenol and formaldehyde has been quenched, urea may be added to the phenol-formaldehyde resole. The resole and urea are then allowed to react for up to 24 hours, usually at temperatures up to 60°C. In industry, this process is often referred to as "premixing" or "prereacting", and the resulting phenol-formaldehyde-urea product is called the "premix" or "prereact". The prereact is then stored and transported prior to use. There are known disadvantages associated with the application of the urea prereacting method, in that the prereact is significantly less stable than the phenol-formaldehyde resole (the higher the proportion of urea, the less stable it is), resulting in a much shorter usable storage time. Additionally, temperatures below 10°C should be avoided for the prereact.
[0007] [7] To address stability issues, urea may instead be added to the phenol-formaldehyde resol by the mineral wool manufacturer at the production site just before the mixture is applied to the mineral fiber. Thus, long-term storage or transportation of the pre-reacted product is no longer required. In this case, the industry sometimes refers to the urea being added "cold" to distinguish it from the pre-reacted product (in which urea is frequently added to the resol reaction product while it is still warm). However, cold urea addition also has drawbacks. For example, the presence of unreacted urea that has not had sufficient time to react has been associated with increased unwanted emissions of ammonia and amines during mineral wool production. Furthermore, if urea is first added just before application to the fiber, resols with high free formaldehyde content will need to be stored, transported and handled, with concerns related to their toxicity.
[0008] [8] The combination of both pre-reaction and cold urea addition is described, for example, in U.S. Pat. No. 5,538,761, U.S. Pat. No. 5,670,585 and U.S. Patent Application Publication No. 2007191574. However, the disclosed contents of free formaldehyde in the starting resol are expressed in terms of wet weight, not in terms of dry weight, and the disclosed contents are evidence of the need for high contents of free formaldehyde.
[0009] [9] The use of urea has helped to reduce concerns about free formaldehyde content in phenol-formaldehyde resol-based binders, but has not been completely satisfactory with respect to formaldehyde release from the manufactured mineral wool products. This is because the urea-formaldehyde reaction products are not sufficiently heat stable to release formaldehyde from the manufactured mineral wool products during curing at temperatures above 100 °C.
[0010]
[10] Reducing formaldehyde emissions from mineral wool products has been widely studied. Most approaches involve the use of formaldehyde scavengers other than urea to irreversibly capture excess formaldehyde, such as melamine, dicyandiamide, alkanolamines, glycine, and substances with active methylene groups, among others. However, this approach has significant drawbacks. The most important are the extra cost of the scavengers used, and the need for extra processing steps and equipment. In addition, scavengers can have a detrimental effect on the stability and processability of the resin.
[0011]
[11] The present inventors have realized that there is a need in the art for an improved method for producing mineral wool products having phenol-formaldehyde resole based binders that avoids the storage, transportation, and handling of materials having high free formaldehyde content and results in mineral wool products with reduced formaldehyde emissions without the need to use formaldehyde scavengers other than urea. Summary of the Invention
[0012]
[12] In view of the above, the inventors have developed an alternative process which provides a combination of many important advantages in both the manufacture of mineral wool products and in the products themselves, which advantages are surprising and unexpected according to the prior art.
[0013]
[13] According to the present invention, the method includes a first step (step a) of providing a hydrous phenol-formaldehyde resol having free formaldehyde. In other words, the method envisages providing, under alkaline conditions, a hydrous product of methylolation and condensation of a phenolic compound with formaldehyde, where the formaldehyde is in molar stoichiometric excess relative to the phenolic compound, so that after the reaction, the reaction product remains mixed with an excess of unreacted free formaldehyde.
[0014]
[14] Advantageously, hydrous phenol-formaldehyde resols containing a low free formaldehyde content, i.e. not more than 10% by weight of free formaldehyde based on the dry weight content of the resol, can be used in the process of the invention without impairing the stability of the product obtained. Thus, in a preferred embodiment, the hydrous phenol-formaldehyde resol in this step a contains not more than 10% by weight, preferably not more than 6% by weight, more preferably at least 1% by weight of free formaldehyde based on the dry weight content of the resol, measured according to method ISO9397:1995 (hydroxylamine hydrochloride method).
[0015]
[15] In the next step (step b), the method foresees the preparation of a phenol-formaldehyde-urea pre-reactant by contacting the phenol-formaldehyde resol with a first amount of urea (U1) and reacting the mixture of resol and urea. When the phenol-formaldehyde resol containing free formaldehyde is contacted with urea in the so-called "pre-mix" step, the urea reacts with the free formaldehyde by methylolation of the urea, among other reactions. As a result, the content of free formaldehyde in the resol decreases rapidly with the amount of urea used. By phenol-formaldehyde-urea pre-reactant is meant the reaction product mixture formed after contacting urea with the resol and reacting the mixture for a sufficient time and at a sufficient temperature to cause a rapid decrease in the free formaldehyde content. It should be understood that reaction may still continue in the formed pre-reaction after the formaldehyde content has reached a lower plateau, but at a much slower rate.
[0016]
[16] In a preferred embodiment, the phenol-formaldehyde resole and urea are reacted for at least 1 hour, preferably at a temperature between 10 and 60° C., to prepare a phenol-formaldehyde-urea pre-reactant in step b.
[0017]
[17] The phenol-formaldehyde-urea pre-reactants prepared according to the preferred embodiments are stable for at least several days, and even at least several weeks. This time allows for transportation of the pre-reactant, for example from a resole manufacturer to a mineral wool manufacturer, and for its storage prior to use as part of a mineral wool binder. By stable, we mean that the pre-reactant does not undergo degradation of properties necessary for use as part of a binder in the manufacture of mineral wool. Some of the properties of the pre-reactant that are maintained for several days or weeks are sufficiently low viscosity, sufficient water dilutability, absence of sediment, and / or adequate B-stage gelation time.
[0018]
[18] In a subsequent step (step c) of the method according to the invention, the phenol-formaldehyde-urea pre-reactant formed in step b is contacted with a second amount of urea (U2). It should be understood that this step is carried out separately from step b, i.e. the preparation of the pre-reactant referred to in the previous paragraph. In a preferred embodiment, the second amount of urea (U2) is added to the pre-reactant at least 24 hours, preferably at least 72 hours, after the pre-reactant has been formed. This subsequent step c is advantageously carried out immediately before, preferably less than 48 hours, more preferably less than 24 hours before, applying the mixture to the surface of the mineral fibres in the manufacture of the mineral wool product.
[0019]
[19] The mixture of phenol-formaldehyde-urea pre-reactant obtained in step c and urea is then applied to the surface of the mineral fibers in a subsequent step d according to the method of the invention. Said mixture is applied as part of a hydrous binder optionally containing at least one additive selected from a curing catalyst (e.g. ammonium sulfate), a resin extender different from urea (e.g. carbohydrates), a dust suppressant (e.g. mineral oil), an adhesion promoter (e.g. silanes) and a water repellent (e.g. silicones). Preferably, the binder contains the optional additives in a concentration of 1-30% by weight relative to the non-hydrous content of the binder. According to a particular embodiment, the addition of a resin separate from the hydrous phenol-formaldehyde resole of step a is excluded.
[0020]
[20] In a particular embodiment, in step d, the mixture of phenol-formaldehyde-urea pre-reactant and urea from step c is applied to the surface of the fibers as part of the wet binder with a non-wet content in the range of 4-15 wt.%, preferably 6-13 wt.%, and even more preferably 8-10 wt.%, based on the weight of the wet binder.
[0021]
[21] Preferably, a mixture of phenol-formaldehyde-urea pre-reactant and urea, the binder, is applied by spraying onto the surface of the newly formed fibers emerging from the fiberizer.
[0022]
[22] The mixture of phenol-formaldehyde-urea pre-reactant and urea, which is applied to the fibers as part of the binder, is then cured in a subsequent step (step e) in the method according to the invention.
[0023]
[23] In a preferred embodiment, the mixture of phenol-formaldehyde-urea pre-reactant and urea is cured by passing the coated mineral fiber through an air-circulating curing oven set at a temperature above 100° C., preferably 140-180° C. Curing times are preferably in the range of 3-5 minutes.
[0024]
[24] According to the invention, the method is further characterized by the following features: (i) - the total amount of urea (Ut) is 30-35% by weight relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), and the second amount of urea (U2) used in step c is 20-35% by weight of the total amount of urea (Ut); or (ii)--the total amount of urea (Ut) is about 40% by weight relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), and the second amount of urea (U2) used in step c) is about 25% by weight of the total amount of urea; or (iii) the total amount of urea (Ut) is 42-50% by weight relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), and the second amount of urea (U2) used in step c is 15-52% by weight of the total amount of urea (Ut); or (iv) - the total amount of urea (Ut) is 42-50% by weight relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), and the second amount of urea (U2) used in step c is 63-66% by weight of the total amount of urea; or (v) the total amount of urea (Ut) is about 45% by weight relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), and the second amount of urea (U2) used in step c is about 56% by weight of the total amount of urea. In the context of the present invention, the range of 30-35 wt% is also understood to include 29.6 wt%, 29.7 wt%, 29.8 wt% and 29.9 wt%. The total amount of urea (Ut) used is the result of combining the first amount of urea (U1) used for the pre-reactant formation in step b and the second amount of urea (U2) used for the formation of the mixture of pre-reactant and urea in step c. The inventors have found that when Ut is less than 10 wt%, the formaldehyde emission increases significantly. On the other hand, Ut values above 60 wt% lead to a decrease in the mechanical properties of the binder and high ammonia emission.
[0025]
[25] In a particular embodiment, the total amount of urea (Ut) is 30-35% by weight relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), and U2 is 22-33% by weight, preferably 25-30% by weight, of the total amount of urea (Ut); or the total amount of urea (Ut) is 42-50% by weight, preferably 45-48% by weight, relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), and U2 is 15-50% by weight, preferably 20-48% by weight, preferably 25-45% by weight, preferably 30-43% by weight, preferably 35-40% by weight, of the total amount of urea (Ut).
[0026]
[26] In a preferred embodiment, the total amount of urea (Ut) is 30-35% by weight, preferably 33% by weight, based on the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), and the second amount of urea (U2) used in step c is 20-35% by weight of the total amount of urea (Ut). In another preferred embodiment, the total amount of urea (Ut) is 42-50% by weight, preferably 43-48% by weight, based on the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), and the second amount of urea (U2) used in step c is 15-52% by weight of the total amount of urea (Ut). In another preferred embodiment, the total amount of urea (Ut) is 42-50% by weight, preferably 43-48% by weight, based on the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), and the second amount of urea (U2) used in step c is 63%-66% by weight, preferably about 65% by weight, based on the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut). In another preferred embodiment, the total amount of urea (Ut) is about 40% by weight, based on the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), and the second amount of urea (U2) used in step c is about 25% by weight, based on the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut). In another preferred embodiment, the total amount of urea (Ut) is about 45% by weight relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), and the second amount of urea (U2) used in step c is about 56% by weight of the total amount of urea (Ut).
[0027]
[27] According to certain embodiments, the addition of a resin other than the hydrous phenol-formaldehyde resole of step a is excluded. In certain embodiments, the addition of sodium silicate resin, polyester resin, melamine resin, novolac resin, epoxy resin, polyamide resin, furan-based resin, phosphate ester resin, or combinations thereof is excluded.
[0028]
[28] In particular, the inventors have surprisingly found that when Ut is 30-35 wt. % relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut) and U2 is 20-35 wt. % of the total amount of urea, or when Ut is 42-50 wt. % and U2 is 15-52 wt. % or 63-66 wt. %, the formaldehyde emission in the resulting product is significantly reduced.
[0029]
[29] The inventors have surprisingly found that, starting from the same free formaldehyde content in the phenol-formaldehyde resol and using the same total amount of urea, the process according to the invention results in a mineral wool product with significantly reduced formaldehyde emissions compared to the emissions measured for a process using the same total amount of urea only during the formation of the pre-reactant. Without wishing to be bound by theory, it is believed that the split urea addition to the resol and the contact of the pre-reactant with the second amount of urea (U2) just before application to the mineral fibers modifies the reaction pathway during curing, thereby increasing the amount of formaldehyde that is irreversibly locked in the polymeric thermoset network formed during curing.
[0030]
[30] A further advantage of the method of the invention is that the first amount of urea (U1) can be added by the phenol-formaldehyde resol manufacturer himself immediately after the condensation reaction for its production is completed, to obtain a pre-reactant with significantly lower free formaldehyde than the resol obtained from the condensation. For example, the amount of urea used in this pre-mixing step can be selected so as to be sufficient to reduce the free formaldehyde content in the pre-reactant to 0.9% by weight or less, preferably 0.2% by weight or less, as measured according to ISO 11402:2004 (KCN method), as the dry weight content of the pre-reactant. A pre-reactant with such an important reduction in free formaldehyde content is less problematic with regard to potential toxicological and environmental concerns related to formaldehyde during storage, transportation and handling of this material.
[0031]
[31] Thus, in a preferred embodiment of the invention, the first amount (U1) of urea contacted with the phenol-formaldehyde resol in step b is selected to be sufficient to produce a phenol-formaldehyde-urea pre-reactant containing not more than 0.9% by weight, preferably not more than 0.2% by weight, of free formaldehyde based on the dry weight content of the pre-reactant, as measured according to ISO 11402:2004 (KCN method).
[0032]
[32] The lower amount of urea used in the premixing step in the method of the present invention results in a higher pre-reactant stability compared to the situation where the same total amount of urea (Ut) is used but not divided (this is all of the urea applied in the premixing step). The pre-reactant obtained in the preferred embodiment is stable for at least one week, and usually even several weeks. By stable, it is meant that the properties of the pre-reactant that are important for its usability in the manufacture of mineral wool do not substantially deteriorate during this time. Such properties are, for example, good water dilutability, low viscosity, absence of sediment, or adequate B-stage gelation time, to name the most important ones.
[0033]
[33] The relatively low amount of urea used in the premixing step in the process of the present invention also paves the way for the use of phenol-formaldehyde resols with a relatively low content of free formaldehyde. It has been reported that the addition of a large molar stoichiometric excess of urea relative to the free formaldehyde in the resol for the preparation of the pre-reactant can result in troublesome precipitation of phenol-formaldehyde tetradimers and a decrease in the stability of the pre-reactant. In the process of the present invention, due to the relative reduction in the amount of urea used in the preparation of the pre-reactant, resols with a lower content of free formaldehyde, for example, 10% by weight or less of free formaldehyde relative to the dry weight content of the resol, can be used without unacceptably impairing the stability of the pre-reactant formed.
[0034]
[34] The present invention also relates to mineral wool products with reduced formaldehyde emissions obtainable by the methods according to the embodiments described herein, as well as the use of these mineral wool products for the insulation of buildings, transport, air conduction ducts or appliances.
[0035]
[35] Furthermore, a particular embodiment of the present invention relates to a method for preparing a phenol-formaldehyde-urea pre-reactant having a low free formaldehyde content, comprising providing a phenol-formaldehyde resol containing 10% by weight or less, preferably 6% by weight or less, and preferably at least 1% by weight of free formaldehyde based on the dry weight content of the resol, contacting the resol with a sufficient amount of urea to reduce the free formaldehyde content in the pre-reactant to 0.9% by weight or less, preferably 0.2% by weight or less, based on the dry weight content of the pre-reactant, according to ISO11402:2007 (KCN method), and reacting the resol and urea mixture, preferably for at least 1 hour, more preferably for at least 2 hours. Also preferably, the amount of urea in this embodied method for preparing the pre-reactant is at least 5% by weight, more preferably at least 10% by weight, and preferably at most 20% by weight based on the dry weight content of the pre-reactant. In these embodiments, the phenol-formaldehyde resol is preferably substantially free of nitrogenated compounds (compounds containing at least one nitrogen atom), and in particular is substantially free of compounds selected from urea, ammonia, ammonium inorganic or organic salts, alkanolamines, alkylamines and / or melamine.
[0036] definition
[36] Substantially free means in accordance with this specification that the concentration of the corresponding compound in the resole, pre-reactant or binder is sufficiently low that it can be ignored. However, in this context it should be understood that the compound in question may be present in trace amounts, for example from unintentional cross-contamination, preferably at a concentration of 0.1% by weight relative to the dry weight of the resole, pre-reactant or binder.
[0037]
[37] In the context of this disclosure, dry weight content is defined as the weight fraction of residue remaining after drying 3 g of a water-containing composition (resole, pre-reactant or binder) at 135 °C for 1 h in a ventilated oven, e.g. as measured according to ISO 3251:2008.
[0038]
[38] The term binder refers to the aqueous mixture of ingredients that is applied to fibers in the manufacture of mineral wool products and then cured to produce bonds at the intersections of the fibers through the cured binder. Binders are generally prepared in situ, which means that they are prepared continuously at the mineral wool manufacturing plant, usually just prior to being applied to the fibers.
[0039]
[39] Curing means that the material in question undergoes a curing reaction (hardening or crosslinking reaction) when heated, for example to 100 °C in a curing oven (thermosetting). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0040]
[40] The hydrous phenol-formaldehyde resols suitable for the process of the present invention are water-soluble curable resols having free formaldehyde, which are produced by methylolation and condensation of phenolic compounds with formaldehyde in the presence of an alkaline catalyst by methods known in the art. In the resol, the molar ratio of phenol:formaldehyde is <1. Phenol-formaldehyde resols are reactive mixtures with methylol functional groups that undergo a self-curing reaction under the influence of heat or acid. Thus, resols are partially reacted thermosetting resins, also known as resins, prepolymers or precondensates, which are stable at low temperatures and alkaline pH and can be further condensed into thermosetting resins in a curing reaction by application of heat and / or acidic pH values. Those skilled in the art know how such resols are generally produced and recognize how to modify different reaction phases and parameters to obtain the characteristics described in the preferred embodiments of the present invention. Such parameters include, for example, the molar ratio of phenol:formaldehyde, the type and amount of catalyst, and the condensation reaction time and temperature.
[0041]
[41] The molar ratio of phenol:formaldehyde for the preparation of the resole of the present process is preferably in the range of 1:2 to 1:6. A stoichiometric excess of formaldehyde ensures the predominant formation of low molecular weight species by methylolation and condensation, lower solution viscosity, and low free phenol content in the resole. A molar excess of formaldehyde also has the consequence that the aqueous resole after reaction contains free, unreacted formaldehyde.
[0042]
[42] For clarity of this description, the appropriate resole will be referred to as a phenol-formaldehyde resole, but it should be understood that this does not mean that the resole contains only unsubstituted phenol and formaldehyde as components. Other components may be present in the resole without departing from the scope of the invention. Such components may be, for example, alkylphenols, phenol esters, or substituted phenol derivatives such as resorcinol and its derivatives, or formaldehyde-related compounds such as paraformaldehyde, or higher aldehydes such as butyraldehyde, acrolein, or glyoxal. Other compounds having hydroxy or carboxy groups can also react with the phenol and formaldehyde (e.g., carbohydrates or alkanolamines), and even compounds having functional groups different from hydroxy or carboxy (e.g., hexamethylenetetramine) can be included in the reaction. However, it is preferred that the sum of the weights of unsubstituted phenol and formaldehyde in the resole is at least 80% by weight, preferably at least 90% by weight, of the dry weight of the resole.
[0043]
[43] Advantageously, resols with a low free formaldehyde content, i.e. resols containing 10% or less by weight of free formaldehyde relative to the dry weight content of the resol, can be used in the process of the invention. According to a particular embodiment of the invention, the free formaldehyde content in the resol is preferably 10% or less by weight, more preferably 6% or less by weight, and preferably at least 1% by weight, relative to the dry weight content of the resol, when measured according to the method of ISO9397:1995 (hydroxylamine hydrochloride method). The main advantage of using resols with these levels of free formaldehyde content in the process of the invention is that the mineral wool products obtained by applying the process of these embodiments have satisfactory mechanical performance and, in addition, emit less formaldehyde. In particular, if the free formaldehyde content in the resol is sufficiently low, the formaldehyde emission can be reduced to 10 μg / m 3less than 8 μg / m 3 It is possible to produce mineral wool products with less than 1000 mg / kg of formaldehyde per 1000 g of mineral wool. The formaldehyde emissions from mineral wool products are related to the emissions when the product is stored under controlled conditions for 28 days in a test vessel equipped with an air exchanger and the formaldehyde concentration in the air inside the vessel is then measured according to standard method ISO 16000-3:2011.
[0044]
[44] According to the method of a particular embodiment, the phenol-formaldehyde resole preferably has a dry weight content of 40-60% by weight. The content of unreacted free phenol in the resole is preferably at most 6% by weight, more preferably at most 2% by weight, based on the dry weight content of the resole. The water dilutability of the resole in demineralized water at 20°C is suitably greater than 10 parts by weight (this means that at least 10 g of water can be added to 1 g of resole before permanent turbidity appears), preferably greater than 20 parts, more preferably greater than 50 parts. The resole viscosity is preferably at most 50 mPa.s at 20°C, more preferably at most 30 mPa.s, measured on an aqueous resole solution with a dry weight content of 45% by weight. The pH of the resole solution is preferably higher than 8, more preferably higher than 8.5, even more preferably higher than 8.9. The B-stage gel time of the resole is preferably in the range of 2-15 minutes at 130°C. The methods used to determine these values are known to those skilled in the art and will be briefly described in some detail below.
[0045]
[45] In a preferred embodiment, the phenol-formaldehyde resol has a total nitrogen concentration of less than 1.0% by weight, preferably less than 0.6% by weight, based on the dry weight content of the resol, before contacting it with urea to form the phenol-formaldehyde-urea pre-reactant. Preferably, the resol is substantially free of nitrogenated compounds (compounds containing at least one nitrogen atom), in particular substantially free of compounds selected from urea, ammonia, ammonium inorganic or organic salts, alkanolamines, alkylamines and / or melamine.
[0046]
[46] According to certain embodiments of the invention, the phenol-formaldehyde resol is substantially free of formaldehyde scavengers selected from the group of amines, tannins, sulfites and bisulfites, compounds having methylene active groups, glycine, resorcinol and its derivatives, alkanolamines, and mixtures thereof.
[0047]
[47] Resoles having the properties described in the preferred embodiments herein are available from resole manufacturers such as Momentive Performance Materials or Prefere Resins.
[0048]
[48] The process according to the invention comprises a step (step b) of contacting the phenol-formaldehyde resol with a first amount of urea (U1) to react the resol and urea mixture to prepare a phenol-formaldehyde-urea pre-reactant. The contacting step can be carried out by adding urea (both in solid or liquid form) to the aqueous resol composition, usually under efficient stirring. After contacting the urea and resol, they are mixed vigorously and allowed to react by leaving the mixture for at least 1 hour, preferably at least 2 hours, either in the same reactor used for the preparation of the resol or in a separate vessel. The temperature during this step b, which includes the contacting, mixing and phase reaction leading to the pre-reactant, is in the range of 10-100°C, preferably 15-80°C, preferably 18-70°C, preferably 20-60°C, preferably 30-50°C, more preferably 35-45°C. In a preferred embodiment, the temperature of step b does not exceed 70°C, more preferably the temperature of step b is between 20-60°C. Higher temperatures in the range 10-100°C accelerate the condensation reaction and therefore the reaction must be stopped sooner to avoid the condensation proceeding beyond a desired point. In a preferred embodiment, the phenol-formaldehyde resol and a first amount of urea (U1) are reacted in step b of the process of the present invention at a temperature between 10 and 60°C for at least 1 hour to prepare a pre-reactant.
[0049]
[49] In a preferred embodiment of the invention, in step b, the first amount (U1) of urea contacted with the phenol-formaldehyde resol is selected to be sufficient to produce a phenol-formaldehyde-urea pre-reactant containing not more than 0.9% by weight, preferably not more than 0.2% by weight, of free formaldehyde based on the dry weight content of the pre-reactant, measured according to ISO 11402:2004 (KCN method).
[0050]
[50] The first amount of urea (U1) is preferably in the range of 34-85% by weight, such as 44% by weight, preferably 48-85% by weight, preferably 65-80% by weight, such as 75% by weight, based on the total amount of urea (Ut).
[0051]
[51] Particularly good results of pre-reactant stability, low free formaldehyde pre-reactant content and low formaldehyde emissions were achieved when using a resole containing less than 6% by weight of free formaldehyde, based on the dry weight content of the resole, in contact with a first amount of urea (U1) of at least 34% by weight, more preferably at least 48% by weight, more preferably at least 65% by weight, based on the total amount of urea (Ut).
[0052]
[52] In the next step c, the phenol-formaldehyde-urea pre-reactant formed in step b is contacted with a second amount of urea (U2) to produce a mixture of pre-reactant and urea. The start of this step c is separated in time from the end of step b, preferably by at least 24 hours, more preferably by at least 72 hours. This step c is typically performed by the mineral wool manufacturer at their facility just before the mixture of pre-reactant and urea is applied to the mineral fibers in the manufacture of the mineral wool product. In contrast, the preparation of the phenol-formaldehyde-urea pre-reactant is typically performed by the resole manufacturer, who ships the finished pre-reactant to the mineral wool manufacturer.
[0053]
[53] In step c, the phenol-formaldehyde-urea pre-reactant and the second amount of urea (U2) can be contacted and thoroughly mixed in a vessel adapted for this purpose or, less preferred at present, said contacting and mixing can be carried out continuously "in-line" in the mineral wool production line and the mixture transported to a binder application station. The mixture of pre-reactant and the second amount of urea (U2) is preferably maintained at a temperature below 50°C, preferably below 40°C, more preferably below 30°C, more preferably between 20 and 25°C, all the way up to its application on the surface of the mineral fibres to avoid premature progression of the condensation reactants.
[0054]
[54] The phenol-formaldehyde-urea pre-reactant and the second amount of urea (U2) are contacted and mixed immediately prior to, and preferably less than 48 hours, and more preferably less than 24 hours, before applying the resulting mixture to the surface of the mineral fibers.
[0055]
[55] The process according to the invention provides for the total amount of urea (Ut), i.e. the sum of the first (U1) and second (U2) amounts of urea used in steps b and c relative to the sum of the dry weight of the phenol-formaldehyde resol and the total amount of urea (Ut), to be used in the following ranges: (i) if the total amount of urea (Ut) is 30-35% by weight relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), the second amount of urea (U2) used in step c is 20-35% by weight of the total amount of urea (Ut); or (ii) when the total amount of urea (Ut) is about 40% by weight based on the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), the second amount of urea (U2) used in step c is about 25% by weight of the total amount of urea; or (iii) when the total amount of urea (Ut) is between 42 and 50% by weight relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), the second amount of urea (U2) used in step c is between 15 and 52% by weight of the total amount of urea (Ut); or (iv) when the total amount of urea (Ut) is 42-50% by weight relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), the second amount of urea (U2) used in step c is 63-66% by weight of the total amount of urea; or (v) when the total amount of urea (Ut) is about 45% by weight relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), the second amount of urea (U2) used in step c is about 56% by weight of the total amount of urea. The inventors have surprisingly found that when this combination of features is used, the formaldehyde emissions from the mineral wool product produced are significantly reduced compared to when the same total amount of urea is used only in the preparation of the pre-reactant (without "cold" urea addition).
[0056]
[56] To produce a mineral wool product according to the method of the invention, in a further step d, a mixture of the phenol-formaldehyde-urea pre-reactant from step c and a second amount of urea (U2) is applied to the surface of the mineral fibres. The mixture of said pre-reactant and the second amount of urea (U2) is applied to the fibres as part of a binder. The binder optionally contains additives used to aid in the manufacture of the mineral wool product or to improve the properties of the mineral wool product. The binder is preferably a hydrous composition containing non-hydrous content in the range of 4-15% by weight based on the hydrous binder weight.
[0057]
[57] The optional additives contained in the binder in addition to the phenol-formaldehyde-urea pre-reactant and the second amount of urea (U2) are preferably present in a concentration of more than 1% and less than 30% by weight, more preferably in a concentration of 5-25% by weight, more preferably in a concentration of 10-20% by weight, and even more preferably in a concentration of 15-18% by weight, based on the non-water content of the binder. The optional additives include at least one additive selected from the following group of substances: i) curing catalysts such as ammonium sulfate; ii) resin extenders different from urea, such as carbohydrates; iii) dust suppressants, such as mineral oils; iv) adhesion promoters, such as silanes; and v) water repellents, such as silicones, more particularly reactive silicones. It is particularly preferred to include up to 10% by weight of molasses and / or glucose as resin extenders.
[0058]
[58] In certain embodiments, resins are excluded from the optional additives. In certain embodiments, the addition of sodium silicate resins, polyester resins, melamine resins, novolac resins, epoxy resins, polyamide resins, furan-based resins, phosphate ester resins, or combinations thereof are excluded.
[0059]
[59] In a preferred embodiment, the mixture of the phenol-formaldehyde-urea pre-reactant and the second amount of urea (U2) is largely diluted with fresh or treated water and optionally mixed with additives to prepare the binder. If no additives are used, the binder can include only the mixture of the pre-reactant and the second amount of urea (U2), preferably diluted with water to the desired concentration.
[0060]
[60] The concentrations of the different components in the binder are preferably in the range of 40-90% by weight of phenol-formaldehyde resol, 30-50% by weight of total urea (the sum of the first (U1) and second (U2) amounts of urea) and 1-20% by weight of additives, based on the non-wet weight of the binder.
[0061]
[61] In a preferred embodiment, the mixture of the phenol-formaldehyde-urea pre-reactant and the second amount of urea (U2) is applied in spray form to the individual fine mineral fibers attenuated from the hot molten mineral mixture by the fiberizer. The spray can be produced by a spray nozzle or similar device oriented in such a way that the sprayed mixture is directed toward the surface of the attenuated fibers. The mixture is brought into contact with the surface of the mineral fibers while they are still warm. The impregnated fibers are collected on a perforated conveyor in a forming chamber, where the primary uncured mat is formed. Most of the water contained in the binder evaporates at this stage.
[0062]
[62] The primary mat is then densified and transported by a series of conveyors to a heated curing oven. The binder is then cured at a temperature in excess of 100°C, preferably between 140 and 180°C, more preferably between 150 and 170°C, and even more preferably between 155 and 165°C. Curing times are preferably in the range of 2 to 5 minutes. The cured mineral wool mat is then trimmed and formed to its final dimensions, and optionally rolled and packaged.
[0063]
[63] In a particular embodiment, the mixture of the phenol-formaldehyde-urea pre-reactant and the second amount of urea (U2) is applied to the fibers as part of the binder in an amount that produces a solid binder content of between 1.5% and 15% by weight, preferably between 3% and 12% by weight, and more preferably between 5% and 10% by weight, based on the weight of the mineral fibers in the final mineral wool product after curing. The amount of cured binder based on the weight of the mineral fibers in the mineral wool product is measured as LOI (loss on ignition) according to ISO 29771:2008, and thus in a preferred embodiment, the mineral wool product obtained by the method of the present invention has an LOI of between 1.5% and 15% by weight.
[0064]
[64] When the phenol-formaldehyde resole contains less than 6% by weight of free formaldehyde based on the dry weight content of the resole, the second amount of urea (U2) is in the range of 20-35% by weight based on the total amount of urea (Ut), and the total amount of urea (Ut) is 30-35% by weight based on the sum of the dry weight of the resole and the total amount of urea (Ut), or the second amount of urea (U2) is in the range of 63-66% by weight based on the total amount of urea (Ut), and the total amount of urea (Ut) is 42-50% by weight based on the sum of the dry weight of the resole and the total amount of urea (Ut), and no further formaldehyde scavenger is required, surprisingly, the mineral wool product produced according to this embodiment of the method of the present invention has a formaldehyde content of less than 10 μg / m when measured according to ISO 16000-3:2011. 3 Less than or equal to 8 μg / m 3Thus, in one embodiment, the present invention provides a method for producing a cellulose ester resin having a formaldehyde emission of less than 10 μg / m2 obtained by the method of the present invention, as measured according to ISO 16000-3:2011. 3 Formaldehyde emissions of less than 8 μg / m 3 The present invention relates to a mineral wool product having a formaldehyde emission of less than 1.5% by weight. In a preferred embodiment, the mineral wool product obtained by the method of the present invention further has an LOI of 1.5% by weight to 15% by weight. The mineral wool product obtained by the method of the present invention exhibits a non-acidic behavior with respect to pH, i.e., when said mineral wool product is in contact with water, the water does not have an acidic pH.
[0065] Test Method
[65] The free formaldehyde content of a resole is measured, for example, by a procedure using hydroxylamine hydrochloride, according to the international standard ISO 9397:1995. This method involves the following general principle: the formaldehyde present in the resole is converted to an oxime using hydroxylamine hydrochloride. The hydrochloric acid formed during this reaction is then measured by potentiometric back titration with sodium hydroxide solution. The free formaldehyde content of the resole is then calculated from the amount of sodium hydroxide relative to its dry content.
[0066]
[66] The free formaldehyde content of the phenol-formaldehyde-urea pre-reactant is measured using the KCN method according to ISO 11402: 2004. Alternative methods for measuring the free formaldehyde content are HPLC or NMR.
[0067]
[67] The free or unreacted phenol content of the resole is measured, for example, according to the international standard ISO 8974:2002, which determines the free phenol content using a weighted amount of an internal standard added to the test portion or by gas chromatography using a stock solution of the internal standard. The internal standard used is 1-octanol. The free phenol content of the resole is then calculated relative to its dry weight content.
[0068]
[68] The nitrogen content in phenol-formaldehyde resols is measured, for example, by the Kjeldahl method.
[0069]
[69] The dilutability (or miscibility) of aqueous resols is measured at 20 °C with demineralized water according to the international standard ISO 8989:1995 method. Resol dilutability is a measure of the mass of demineralized water relative to the mass of hydrous resole that will produce permanent turbidity in the liquid resole. The method involves adding water to the resole until turbidity persists for a minimum of 30 seconds after stirring.
[0070]
[70] The viscosity of the resole is measured at 20° C. using a Brookfield viscometer, for example, at spindle 1 and 60 rpm. The viscosity referred to in this invention is based on a hydrous resole having a dry weight content of 45% by weight.
[0071]
[71] The B-stage gel time of resols is measured at 130 °C according to the international standard ISO 8987:2005.
[0072]
[72] The content of hardened binder in mineral wool products (LOI) is determined according to the international standard ISO 29771:2008.
[0073]
[73] Formaldehyde emissions from mineral wool products are measured from freshly manufactured samples, for example according to ISO 16000-3:2011. The method involves placing fresh samples in a 212 L glass vessel equipped with ventilation and set at a temperature of 23 ± 1 °C, a relative humidity of 50 ± 5%, an air flow of 0.2 ± 0.1 m / s, and an air exchange rate of 0.5 h to 1 ± 5%, for a period of 28 days. Other settings include a test vessel volume of 1 m 3 per 1m 2 The loading rate of the sample surface area of 0.5 m 3 / m 2h. The formaldehyde released at the time of measurement (in this example, after 28 days) was measured from the air sample in the container collected on a sorbent cartridge coated with 2,4-dinitrophenylhydrazine (DNPH) in μg / m 3 was measured and the hydrazones formed were subsequently analyzed by high performance liquid chromatography (HPLC). EXAMPLES
[0074]
[74] A phenol-formaldehyde resole characterized as having a pH of 9.6, a viscosity of 20 mPa.s, a dilution in demineralized water of >50, a B-stage gel time of 3 minutes, and a dry weight content of 45% by weight, supplied by a commercial supplier, was used in the manufacture of glass wool products. The resole was further characterized as having a phenol content of less than 2% by weight, a nitrogen content of less than 0.6% by weight, and a free formaldehyde content of 6% by weight, based on the dry weight content of the resole.
[0075]
[75] In the present example, two amounts of urea U1 and U2 were added to the phenol-formaldehyde resol in two separate steps. The first amount U1 was used to prepare the phenol-formaldehyde-urea pre-reactant and was added to the same reaction vessel in which the resol was prepared once the condensation reaction had stopped. The mixture was allowed to react in the same reaction vessel for several hours. After one week, before the manufacture of the glass wool product, the second amount of urea U2 was added to the pre-reactant and mixed with stirring at about 25°C for one hour.
[0076]
[76] A binder mixture was prepared by mixing the obtained pre-reactant and a second amount of urea U2 with water, ammonium sulfate, mineral oil and aminopropyltrimethoxysilane. The binder was applied to the glass wool fiber surface in the form of droplets by spraying in a ring shape as the fibers from the disk fiberizer, attenuated by a hot air blower, fell onto a perforated conveyor belt. The glass fibers with the binder were collected in the form of an uncured mat, densified and transported to a curing oven, where the binder was cured by heating at 140-180 °C for 3-5 minutes. After curing, the glass wool mat produced had a density of 29.5 kg / m 3 and a thickness of 100 mm. The cured binder content, measured as LOI, was 6.5 wt. % relative to the weight of the fiber.
[0077]
[77] In the comparative example, all the urea was added in one step without any splits to form the pre-reactant, and then the same procedure was repeated, except that no urea was added to the pre-reactant.
[0078]
[78] Table 1 shows the amounts of urea U1 and U2 as weight percent relative to the total amount of urea in the inventive and comparative examples, as well as the formaldehyde emission results obtained after 28 days from the manufactured glass wool products. [Table 1]
[0079]
[79] The phenol-formaldehyde-urea pre-reactants of Examples 1-6 contained <0.2 wt. % free formaldehyde based on the dry weight of the pre-reactant.
Claims
1. A method for producing mineral wool comprising the steps of: a) providing a hydrous phenol-formaldehyde resol containing free formaldehyde; b) preparing a phenol-formaldehyde-urea pre-reactant by contacting the resole with a first amount of urea (U1) and reacting the mixture; c) contacting the pre-reactant with a second amount of urea (U2), wherein the second amount of urea (U2) is added to the pre-reactant separated in time by at least 24 hours after the pre-reactant is formed; d) applying the resulting mixture of the pre-reactant and the second amount of urea (U2) as part of the binder, optionally together with additives, to the surface of the mineral fibers; and e) curing the binder on the surface of the mineral fibers; The phenol-formaldehyde resole in step a contains at most 6% by weight of free formaldehyde based on the dry weight content of the resole; (i) the total amount of urea (Ut) is 30-35% by weight relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), and the second amount of urea (U2) used in step c) is 20-35% by weight of the total amount of urea (Ut); or (ii) the total amount of urea (Ut) is 42-50% by weight relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), and the second amount of urea (U2) used in step c) is 63-66% by weight of the total amount of urea (Ut).
2. 2. The method according to claim 1, wherein the total amount of urea (Ut) is 30-35% by weight relative to the sum of the dry weight content of the phenol-formaldehyde resol and the total amount of urea (Ut), and the second amount of urea (U2) used in step c is 22-33% by weight of the total amount of urea (Ut).
3. 3. The process according to claim 2, wherein the second amount (U2) of urea used in step c) is 25-30% by weight of the total amount (Ut) of urea.
4. The method of any one of claims 1 to 3, wherein the addition of a resin separate from the hydrous phenol-formaldehyde resol of step a is excluded.
5. 5. The method of any one of claims 1 to 4, wherein the phenol-formaldehyde resole has a water dilution at 20°C of more than 10 parts by weight, a viscosity of up to 50 mPa.s at 20°C and a dry weight content of 45% by weight, a pH greater than 8, and a B-stage gel time in the range of 2 to 15 minutes at 130°C.
6. The method according to any one of claims 1 to 5, wherein in step b, the phenol-formaldehyde resol and the first amount of urea (U1) are reacted for at least 1 hour.
7. The method according to claim 6, wherein in step b, the phenol-formaldehyde resol and the first amount of urea (U1) are reacted at 10-60° C. to prepare a pre-reactant.
8. 2. The method of claim 1, wherein in step c, a second amount of urea (U2) is added to the pre-reactant separated in time by at least 72 hours after the pre-reactant is formed.
9. 9. The method according to any one of claims 1 to 8, wherein in step c, the pre-reactant is contacted with a second amount of urea (U2) less than 48 hours before applying the mixture to the surface of the fibre in step d.
10. 10. The method according to any one of the preceding claims, wherein in step d, the mixture of the pre-reactant and the second amount of urea (U2) is applied to the mineral fibres as part of a binder comprising additives in a concentration of 1-30% by weight relative to the non-moisture content of the binder.
11. 11. The method according to any one of claims 1 to 10, wherein the first amount (U1) of urea in step b) is selected to produce a pre-reactant containing not more than 0.9% by weight of free formaldehyde relative to the dry weight content of the pre-reactant.
12. 12. The method according to claim 11, wherein the first amount (U1) of urea in step b is selected to produce a pre-reactant containing not more than 0.2% by weight of free formaldehyde relative to the dry weight content of the pre-reactant.
13. The method according to any one of claims 1 to 12, wherein the phenol-formaldehyde resol in step a has a total nitrogen concentration of less than 1.0 wt. % based on the dry weight content of the resol.
14. 14. The method of claim 13, wherein the phenol-formaldehyde resole in step a has a total nitrogen concentration of less than 0.6 wt. % based on the dry weight content of the resole.
15. 15. The method of any one of claims 1 to 14, wherein the phenol-formaldehyde resol in step b is substantially free of formaldehyde scavengers selected from the group of amines, tannins, sulfites and bisulfites, compounds with methylene active groups, glycine, resorcinol and its derivatives, alkanolamines, and mixtures thereof.
Citation Information
Patent Citations
Water-soluble phenolic resole-urea composition
JP1988061043A
Incombustible binder for inorganic fiber
JP1992091153A
Thermal insulation product and method for manufacturing same
JP2004503807A
Process for preparing binder-treated fiberglass exhibiting lowered formaldehyde and ammonia emissions and product prepared thereby
US5538761A