Wafer processing sheet and wafer processing method
A wafer processing sheet with tailored storage modulus and peelability characteristics addresses the issues of adhesive residue and electrode damage, enhancing processing yield by ensuring appropriate followability and peelability during back-grinding and dicing.
Patent Information
- Application Number
- JP2022512120
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-04-01
- Filing Date
- 2021-03-26
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-03-26
AI Technical Summary
Conventional wafer processing sheets fail to provide adequate followability and peelability, leading to adhesive residue and damage to protruding electrodes during back-grinding and dicing processes, especially when the wafer surface has large irregularities.
A wafer processing sheet with a base sheet having specific storage modulus characteristics, including a storage modulus E' of 30-80°C with an exponential coefficient of -0.035 to -0.070, and a melting point of 70°C or higher, which allows for appropriate followability and excellent peelability.
The sheet effectively protects the wafer surface during processing by minimizing adhesive residue and preventing damage to protrusions, thereby improving the yield of semiconductor devices.
Smart Images

Figure 0007559052000002 
Figure 0007559052000003 
Figure 0007559052000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a wafer processing sheet and a wafer processing method. [Background technology]
[0002] When processing a wafer, a sheet is attached to protect the wafer from damage caused by the processing. For example, in a back-grinding process performed to thin a wafer having bumps or the like formed on its surface, a sheet is attached to the surface on which the bumps or the like are formed to protect the surface. Also, in a dicing process for cutting semiconductor chips from a wafer, dicing is performed with the sheet attached to the wafer.
[0003] Such sheets are required to be able to conform to the unevenness of the wafer surface (ability to conform to steps). Conventionally, the conformability of sheets has been improved by increasing the thickness of the adhesive or by providing a soft, cushioning resin layer between the base film and the adhesive. However, when the wafer surface is significantly uneven, there are problems such as insufficient conformability, or the adhesive layer penetrating deep into the recesses on the wafer surface, resulting in adhesive residue, reduced yields, and malfunction of the processed chips.
[0004] As a method for solving such problems, Patent Document 1 discloses a technology in which a base sheet is configured to have, on one side thereof, a non-adhesive portion whose diameter is smaller than the outer diameter of the semiconductor wafer to be attached, and an adhesive portion surrounding the non-adhesive portion, and the adhesive strength of the adhesive portion at 23°C is set to 500 mN or more, thereby preventing adhesive residue and a decrease in protective performance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2013-211438 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the technology described in Patent Document 1 simply provides an adhesive portion that adheres to the edge of a semiconductor wafer, and is not configured to directly protect bumps, etc. in the non-adhesive portion. Therefore, for example, in a backgrinding process, if a semiconductor wafer has protruding electrodes, the backgrinding of the semiconductor wafer is performed with only the tips of the protruding electrodes in contact with the base sheet, and therefore there is a risk that an excessive load will be applied to the protruding electrodes during backgrinding, causing the protruding electrodes to be damaged.
[0007] Furthermore, the technology described in Patent Document 1 simply provides an adhesive portion that adheres to the edge of a semiconductor wafer, and does not disclose anything about, for example, how the adhesive portion that comes into contact with the unevenness of the wafer surface can be easily peeled off without leaving any glue residue.
[0008] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a wafer processing sheet that shows appropriate conformability to the wafer surface when heated and also has excellent peelability, and a wafer processing method using the wafer processing sheet. [Means for solving the problem]
[0009] The present inventors have conducted extensive research to solve the above problems, and as a result, have found that the above problems can be solved by using a base sheet having a predetermined storage elastic modulus characteristic as a sheet that comes into contact with the main surface of a wafer, thereby completing the present invention.
[0010] That is, the present invention is as follows. [1] A base sheet is provided in contact with a main surface of a wafer, The storage modulus E' of the base sheet at 30°C to 80°C 30-80 The exponential coefficient of the exponential trend line is -0.035 to -0.070. Sheet for wafer processing. [2] The storage modulus E' of the base sheet at 30°C 30 and storage modulus E' at 80°C 80 Difference (E' 30 -E' 80 ) is 4.00×10 7 ~4.00×10 8 Pa, The wafer processing sheet according to [1]. [3] The storage modulus E' of the base sheet at 80°C 80 But, 5.00×10 5 ~1.00×10 7 Pa, A wafer processing sheet according to [1] or [2]. [4] The storage modulus E' of the base sheet in the temperature range of 80 to 110°C 80-110 But 1.00×10 6 ~1.00×10 7 Pa, The wafer processing sheet according to any one of [1] to [3]. [5] Loss modulus E″ of the base sheet at 80°C 80 But 1.50×10 4 ~1.50×10 6 Pa, The wafer processing sheet according to any one of [1] to [4]. [6] Loss modulus E″ of the base sheet at 30°C 30 But 1.00 x 10 6 ~1.50×10 8 Pa, The wafer processing sheet according to any one of [1] to [5]. [7] The melting point of the base sheet is 70°C or higher. The wafer processing sheet according to any one of [1] to [6]. [8] A lamination process of laminating a surface of the base sheet of the wafer processing sheet according to any one of [1] to [7], which has been heated, to a main surface of a wafer; A processing step of processing the wafer in a state where the base sheet and the wafer are bonded together. Wafer processing method. [9] In the processing step, a main surface of the wafer to which the base sheet is not bonded is ground to obtain a thinned wafer. A method for processing a wafer according to [8].
[10] In the processing step, the wafer is diced to obtain semiconductor chips. A method for processing a wafer according to [8]. Effect of the Invention
[0011] According to the present invention, it is possible to provide a wafer processing sheet that exhibits appropriate conformability to the wafer surface when heated and also has excellent peelability, and a wafer processing method using the wafer processing sheet. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a cross-sectional view showing an example of wafer back-grinding using the wafer processing sheet of the present embodiment. [Diagram 2] FIG. 11 is a cross-sectional view for explaining the conformability of the wafer processing sheet. [Diagram 3] 1 is a graph showing the results of dynamic viscoelasticity measurement in Example 1. [Figure 4] 1 is a graph showing the results of dynamic viscoelasticity measurement in Example 1, with exponential approximation curves added, in which graph A shows the storage modulus E' on a logarithmic scale, and graph B shows the storage modulus E' on a non-logarithmic scale. [Diagram 5] 1 is a graph showing the results of dynamic viscoelasticity measurement in Example 2. [Figure 6] 1 is a graph showing the results of dynamic viscoelasticity measurement in Comparative Example 1. [Figure 7] 13 is a graph showing the results of dynamic viscoelasticity measurement in Comparative Example 2. [Figure 8]13 is a graph showing the results of dynamic viscoelasticity measurement in Comparative Example 3. [Figure 9] 13 is a graph showing the results of dynamic viscoelasticity measurement in Comparative Example 4. [Figure 10] 13 is a graph showing the results of dynamic viscoelasticity measurement in Comparative Example 5. [Figure 11] 13 is a graph showing the results of dynamic viscoelasticity measurement in Comparative Example 6. [Figure 12] 3 is a photograph showing a cross section of a base sheet in Example 1, Comparative Example 2, and Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] An embodiment of the present invention (hereinafter referred to as "the present embodiment") will be described in detail below, but the present invention is not limited to this, and various modifications are possible without departing from the gist of the present invention. In the drawings, the same elements are given the same symbols, and duplicated explanations will be omitted. Furthermore, unless otherwise specified, positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings. Furthermore, the dimensional ratios of the drawings are not limited to those shown in the drawings.
[0014] [Wafer processing sheet] The wafer processing sheet of this embodiment is a base sheet that comes into contact with the main surface of the wafer and has a storage modulus E' at 30°C to 80°C. 30-80 The exponential coefficient of the exponential approximation curve is −0.035 to −0.070.
[0015] By using a base sheet having such storage modulus characteristics, appropriate conformability is exhibited to the uneven wafer surface when heated, and excellent peelability is also exhibited after the back-grinding process and the dicing process, and adhesive residue on the wafer surface can be suppressed, etc. This makes it possible to more appropriately protect and deprotect the wafer surface in the back-grinding process and the dicing process, which can contribute to improving the yield of semiconductor devices.
[0016] First, a brief description will be given of the use of the wafer processing sheet of this embodiment. FIG. 1 shows a cross-sectional view of an example of back-grinding of a wafer using the wafer processing sheet of this embodiment. In FIG. 1, the wafer processing sheet 10 has a base sheet 11 and another layer 12 such as a buffer layer, and the semiconductor wafer 20 has a convex portion 20b on the wafer main surface 20a. The wafer processing sheet 10 of this embodiment is used by attaching the surface 11a of the base sheet 11 to the wafer main surface 20a in the processing process of the semiconductor wafer 20 such as the back-grinding process or dicing process.
[0017] More specifically, before the processing process, the base sheet 11 is heated while the wafer main surface 20a and the surface 11a of the base sheet 11 are in contact with each other (step A). When heated, the elastic modulus of the base sheet 11 decreases, and the base sheet 11 is bonded to the wafer main surface 20a so as to conform to the protrusions 20b formed on the wafer main surface 20a (step B).
[0018] Then, the temperature of the base sheet 11 is lowered, and back-grinding of the back surface 20a' of the semiconductor wafer 20 is performed (step C). The specific method of back-grinding is not particularly limited, and a known method can be used. For example, a method of grinding the back surface 20a' of the semiconductor wafer 20 while supplying a slurry containing abrasive grains to the back surface 20a' of the semiconductor wafer 20 to thin the semiconductor wafer 20 can be used. When the temperature of the base sheet 11 is lowered before back-grinding, the elastic modulus is restored while conforming to the wafer main surface 20a, and the wafer main surface 20a is protected without misalignment between the wafer main surface 20a and the surface 11a of the base sheet 11.
[0019] Finally, the base sheet 11 is peeled off from the wafer main surface 20a (step D). At this time, from the viewpoint of suppressing adhesive residue, it is preferable that the base sheet 11 has a suitable elasticity. This prevents the sheet components from penetrating too much into the recesses when followed in step B, and further suppresses adhesive residue in the recesses caused by the sheet components that have penetrated too much into the recesses. In addition, since the sheet components do not penetrate too much into the recesses, the protrusions are less likely to be subjected to load by the sheet components that have penetrated into the recesses during peeling, and peelability tends to be excellent.
[0020] In particular, in the wafer processing sheet of this embodiment, the conformability in the above steps A to B is important. For example, as shown in FIG. 2B, if the conformability is insufficient and the gap 32 is large, it becomes difficult to adequately protect the convex portion 20b formed on the wafer main surface 20a, which is likely to lead to a decrease in yield in the processing process. In addition, if the conformability is insufficient, there is also a problem that the back surface of the wafer processing sheet 10 is likely to have wavy edges 33. On the other hand, as shown in FIG. 2C, if the conformability is too high and the base sheet penetrates into the gap 34 of the convex portion 20b, it is likely to get caught during peeling, damaging the convex portion 20b or leading to problems such as being unable to peel off.
[0021] Therefore, in the wafer processing sheet 10 of this embodiment, as shown in Fig. 2A, it is important that the sheet has a suitable conformability to provide sufficient protection while preventing the sheet from penetrating into the gaps 31 of the protrusions 20b and ensuring peelability. The configuration of the wafer processing sheet 10 will be described in detail below.
[0022] (Base sheet) (Storage modulus E') In order to adequately protect the wafer surface 20a in the above-described processing of the semiconductor wafer 20, the base sheet 11 is required to have conformability to the wafer main surface 20a. For this reason, in this embodiment, the decrease characteristic of the storage elastic modulus E' (elastic component) upon heating is specified. More specifically, in this embodiment, the decrease characteristic is the storage elastic modulus E' at 30°C to 80°C. 30-80 is expressed by the following exponential approximation curve, the exponential coefficient (hereinafter, simply referred to as "exponential coefficient k") is defined. Exponential approximation curve: y=αe kx y: Storage modulus E' x: Temperature (℃) α: coefficient e: Napier's number k: exponential coefficient
[0023] In this embodiment, the exponent coefficient k is -0.035 to -0.070, preferably -0.040 to -0.070, more preferably -0.045 to -0.070, and further preferably -0.050 to -0.070. When the exponent coefficient k is -0.035 or less, the decrease in the storage modulus E' when the temperature is increased from 30°C to 80°C is large, and the conformability is further improved at high temperatures. On the other hand, when the exponent coefficient k is -0.070 or more, excessive conformability is exhibited at high temperatures, and it is possible to suppress the decrease in releasability.
[0024] In this embodiment, the coefficient α is preferably 1.00×10 8 ~8.00×10 8 and more preferably 2.00×10 8 ~6.00×10 8 and more preferably 2.50×10 8 ~4.50×10 8 When the coefficient α is within the above range, the followability and peelability tend to be further improved.
[0025] The exponential approximation curve is used to represent the characteristics of the curve of the storage modulus E' at 30°C to 80°C, and therefore preferably has a sufficient correlation with the curve of the storage modulus E'. From this viewpoint, the coefficient of determination R 2 is preferably 0.90 to 1.00, more preferably 0.94 to 1.00, and further preferably 0.98 to 1.00. 2 When is within the above range, the exponential approximation curve more accurately represents the curve of the storage modulus E' at 30° C. to 80° C. Therefore, the exponential coefficient k more appropriately represents the characteristics of the storage modulus E'.
[0026] Storage modulus E' of the base sheet at 80°C 80 is preferably 5.00 x 10 5 ~1.00×10 7 Pa, more preferably 7.00×10 5 ~8.00×10 6Pa, and more preferably 1.00×10 6 ~7.00×10 6 Pa. Storage modulus E' 80 is 5.00 x 10 5 By having a storage modulus E' of 1 Pa or more, excessive conformability at high temperatures is suppressed, and the peelability tends to be further improved. 80 is 1.00 x 10 7 By keeping the modulus at 1 Pa or less, the conformability at high temperatures tends to be improved.
[0027] The storage modulus E' of the base sheet at 30°C 30 is preferably 5.00 x 10 6 ~1.50×10 8 Pa, more preferably 8.00×10 6 ~1.00×10 8 Pa, and more preferably 3.00×10 7 ~8.00×10 7 Pa. Storage modulus E' 30 is 5.00 x 10 6 By having a storage modulus E' of 1 Pa or more, adhesive residue is suppressed and peelability tends to be improved. 30 is 1.50 x 10 8 By ensuring that the tension is equal to or less than Pa, even if the base sheet gets caught in gaps between the protrusions during peeling, the protrusions are less likely to be damaged, and peelability tends to be further improved.
[0028] Storage modulus E' of the base sheet in the temperature range of 80 to 110°C 80-110 is preferably 1.00 x 10 6 ~1.00×10 7 Pa, more preferably 1.00×10 6 ~7.50×10 6 Pa, and more preferably 1.00×10 6 ~5.00×10 6 Pa. Storage modulus E' 80-110 is 1.00 x 10 6By being 0.1 Pa or more, the decrease in the storage modulus E' in the high temperature region tends to be slowed down. Therefore, excessive improvement in the conformability during lamination at high temperatures is suppressed, and the peelability tends to be further improved. In addition, the storage modulus E' 80-110 is 1.00 x 10 7 By setting the storage modulus E' to 0.05 Pa or less, the conformability at high temperatures tends to be improved. 80-110 is 1.00 x 10 6 ~1.00×10 7 "The storage modulus E' in the temperature range of 80 to 110°C is 1.00 x 10 Pa" means that 6 ~1.00×10 7 This means that the value falls within the range of Pa.
[0029] Storage modulus E' of the base sheet 30 and storage modulus E' 80 Difference (E' 30 -E' 80 ) is preferably 4.00×10 7 ~4.00×10 8 Pa, more preferably 4.00×10 7 ~1.00×10 8 Pa, and more preferably 4.00×10 7 ~8.00×10 7 Pa. The difference (E' 30 -E' 80 ) is 4.00 x 10 7 By setting the difference (E' 30 -E' 80 ) is 4.00 x 10 8 By ensuring that the compressive strength is equal to or less than Pa, the base sheet is prevented from conforming to the gaps between the protrusions, and the peelability tends to be further improved.
[0030] (Loss modulus E”) The base sheet of the present embodiment may further specify a loss modulus E'' (viscous component) from the viewpoint of conformability and peelability. From this viewpoint, the loss modulus E'' of the base sheet at 80°C is 80 is preferably 1.50 x 104 ~1.50×10 6 Pa, more preferably 7.50×10 4 ~1.00×10 6 Pa, and more preferably 1.00×10 5 ~9.00×10 5 Pa. Loss modulus E” 80 is 1.50 x 10 4 By having a loss modulus of elasticity E” or more, the conformability tends to be improved at high temperatures. 80 is 1.50 x 10 6 By ensuring that the compressive strength is not more than 1 Pa, excessive conformability is prevented from being exhibited at high temperatures, and the peelability tends to be further improved.
[0031] In addition, the loss modulus E" of the base sheet at 30°C 30 is preferably 1.00 x 10 6 ~1.50×10 8 Pa, more preferably 1.00×10 6 ~7.50×10 7 Pa, and more preferably 1.00×10 6 ~5.00×10 7 Pa. Loss modulus E” 30 is 1.00 x 10 6 By having a loss modulus E″ or more, damage to the convex portions due to the base sheet being caught in the gaps between the convex portions during peeling is more suppressed, and peelability tends to be further improved. In addition, the loss modulus E″ 30 is 1.50 x 10 8 By ensuring that the compressive strength is equal to or less than 1 Pa, adhesive residue is suppressed and peelability tends to be further improved.
[0032] Loss modulus E” of the base sheet 30 and loss modulus E” 80 Difference (E 30 -E” 80 ) is preferably 1.00×10 5 ~5.00×10 8 Pa, more preferably 5.00×10 5 ~1.00×10 8Pa, and more preferably 1.00×10 6 ~5.00×10 7 Pa. The difference (E 30 -E” 80 ) is 1.00 x 10 5 By setting the difference (E” 30 -E” 80 ) is 5.00 x 10 8 By making the compressive strength equal to or less than Pa, the peelability tends to be further improved.
[0033] (Melting Point) The melting point of the base sheet is preferably 70°C or higher, more preferably 80°C or higher, and even more preferably 85°C or higher. By having the melting point of the base sheet be 70°C or higher, the base sheet tends to be prevented from melting when heated. This makes it possible to prevent the base sheet from penetrating into the gaps between the convex parts, so that the peelability tends to be further improved. The upper limit of the melting point of the base sheet is not particularly limited, but is preferably 200°C, more preferably 150°C or lower, and even more preferably 120°C or lower.
[0034] Storage modulus E' and its approximate curve exponential coefficient k and coefficient of determination R 2 The loss modulus E″ and melting point can be controlled by adjusting the type of resin used in the base sheet and the composition of the base sheet.
[0035] The dynamic viscoelasticity measurement in this embodiment can be performed according to a conventional method. For example, a sample can be used that is kept in a thermo-hygrostat at a temperature of 23° C. (±2° C.) and a relative humidity of 50% (±5%). For example, a device named "Rheomeric Series RSA III" (manufactured by TA Instruments) can be used. Other conditions are not particularly limited, but measurements can be performed under the conditions described in the examples.
[0036] The melting point of the base sheet can be measured in accordance with JIS K7121.
[0037] The base sheet is mainly composed of a resin, and may contain additives as necessary. The resin may be used alone or in combination of two or more kinds.
[0038] (resin) The resin used in the base sheet is not particularly limited, and examples thereof include ionomer resin, ethylene-vinyl acetate copolymer, soft polypropylene resin, ethylene-(meth)acrylic acid copolymer resin, ethylene-butadiene copolymer resin, hydrogenated resin of ethylene-butadiene copolymer, ethylene-1-butene copolymer resin, soft acrylic resin, etc. Among these, ionomer resin and ethylene-vinyl acetate copolymer are preferred, and ionomer resin is more preferred. By using such a resin, the followability and peelability tend to be further improved. The resin may be used alone or in combination of two or more kinds.
[0039] The ionomer resin is not particularly limited as long as it is a resin in which a specific polymer is intermolecularly bonded by a metal ion, and examples thereof include polyolefin-based ionomers, acrylic-based ionomers, polystyrene-based ionomers, and polyester-based ionomers. These ionomer resins may be used alone or in combination of two or more. Among these, polyolefin-based ionomers and acrylic-based ionomers are preferred, and polyolefin-based ionomers are more preferred. By using such resins, the followability and peelability tend to be further improved.
[0040] The polyolefin ionomer is not particularly limited, but examples thereof include ethylene-methacrylate copolymers, ethylene-acrylate copolymers, and ethylene-methacrylate-acrylate copolymers.
[0041] The acrylic ionomer is not particularly limited, but examples thereof include an acrylic acid ester-acrylate copolymer, an acrylic acid ester-methacrylate copolymer, a methacrylic acid ester-acrylate copolymer, and a methacrylic acid ester-methacrylate copolymer.
[0042] The polystyrene ionomer is not particularly limited, but examples thereof include styrene-styrene sulfonate copolymers, styrene-acrylate copolymers, styrene-methacrylate copolymers, styrene-styrene carboxylate copolymers, and styrene-N-methyl 4-vinylpyridinium salt copolymers.
[0043] The polyester ionomer is not particularly limited, but examples thereof include sulfoterephthalic acid copolymerized polyethylene terephthalate, sulfoisophthalic acid copolymerized polyethylene terephthalate, sulfoterephthalic acid copolymerized polybutylene terephthalate, and sulfoisophthalic acid copolymerized polybutylene terephthalate.
[0044] The metal ions constituting the salt of the ionomer resin are not particularly limited, and examples thereof include monovalent metal ions such as sodium ions and lithium ions, divalent metal ions such as zinc ions, calcium ions and magnesium ions, and trivalent metal ions such as aluminum ions. The polymer and metal ions in the ionomer resin can be used in any combination based on the valence of the ionic functional group in the polymer and the metal ion.
[0045] The ethylene-vinyl acetate copolymer is not particularly limited as long as it is a copolymer of ethylene and vinyl acetate. The content of vinyl acetate in the ethylene-vinyl acetate copolymer is preferably 1 to 35 mol%, more preferably 3 to 25 mol%, and even more preferably 3 to 15 mol%, based on the total number of moles of structural units derived from ethylene and vinyl acetate. By having the content of vinyl acetate within the above range, the followability and peelability tend to be further improved.
[0046] The soft polypropylene resin is not particularly limited, but may be, for example, a polypropylene resin blended with a rubber component. The rubber component used here is not particularly limited, but may be, for example, a styrene-butadiene copolymer rubber, a styrene-butadiene-styrene block copolymer rubber, a styrene-isoprene-styrene block copolymer rubber, an ethylene-propylene copolymer rubber, etc.
[0047] The weight average molecular weight (Mw) of the resin used in the above-mentioned base sheet is preferably 10,000 to 1,000,000, and more preferably 50,000 to 500,000.
[0048] (Thickness) The thickness of the base sheet is preferably 50 to 500 μm, more preferably 70 to 400 μm, and further preferably 100 to 300 μm. By having the thickness of the base sheet within the above range, sufficient conformability to the irregularities on the wafer surface is exhibited, and the strength of the sheet is also maintained, so that the sheet is less likely to break when peeled off, and peelability also tends to be improved.
[0049] (Other ingredients) The base sheet may contain other additives, such as known plasticizers, heat stabilizers, colorants, organic lubricants, inorganic lubricants, surfactants, and processing aids, as necessary.
[0050] (other layers) The wafer processing sheet 10 of this embodiment may have another layer 12 on the surface opposite to the surface 11a of the base sheet 11 that contacts the wafer main surface 20a (see FIG. 1). The other layer 12 is not particularly limited, but examples thereof include an adhesive layer for fixing the base sheet 11 attached to the wafer 20 to a stage, and a buffer layer interposed between the base sheet 11 and the stage.
[0051] As long as the wafer processing sheet 10 of this embodiment is used for the purpose of protecting the wafer main surface 20a before processing, the layer structure other than the base sheet 11 is not particularly limited, and other layers 12 can be used in combination according to the type of processing. The other layers 12 may be a single layer or a laminate of layers having the same or different functions.
[0052] In addition, since the wafer processing sheet 10 of this embodiment has a surface 11a that contacts the wafer main surface 20a of the base sheet 11, it is preferable that the surface 11a that contacts the surface of the wafer main surface 20a on which the convex portion 20b is formed does not have an adhesive layer or the like.
[0053] [Wafer Processing Method] The method for processing a wafer according to the present embodiment includes a lamination step of laminating a heated surface of the base sheet of the wafer processing sheet to a main surface of a wafer, and a processing step of processing the wafer in a state where the base sheet and the wafer are laminated together. Each step will be described below with reference to FIG.
[0054] [Lamination process] In the lamination step, the heated surface 11a of the base sheet 11 of the wafer processing sheet 10 is laminated to the main surface 20a of the wafer. In the lamination step, the base sheet 11 may be laminated to the wafer main surface 20a in a pre-heated state, or the base sheet 11 may be laminated to the wafer main surface 20a and then heated.
[0055] By bonding the surface 11a of the base sheet 11 and the main surface 20a of the wafer in a heated state, the surface 11a can be bonded to the main surface 20a of the wafer in a state where it conforms to the main surface 20a of the wafer (see B in FIG. 1). In this way, the convex portions 20b are sunk into the base sheet 11, so that the main surface 20a of the wafer having the convex portions 20b can be protected.
[0056] The heating temperature is preferably 60 to 150° C., more preferably 70 to 120° C., and further preferably 80 to 120° C. The heating time of the base sheet 11 is preferably 3 to 120 seconds, and more preferably 5 to 90 seconds. By keeping the heating conditions within the above range, the conformability of the base sheet 11 tends to be further improved.
[0057] [Processing process] The processing step for processing the wafer 20 in a state where the base sheet 11 and the wafer 20 are bonded together is not particularly limited, and any wafer processing process can be appropriately applied. For example, the processing step includes a back-grinding process in which the back surface 20a' of the wafer to which the base sheet 11 is not bonded is ground to obtain a thinned wafer 21, and a dicing process in which the wafer 20 is diced to obtain semiconductor chips. Among these, the wafer processing method of the present embodiment can be suitably used for the back-grinding process.
[0058] The specific method of back grinding is not particularly limited, and known methods can be used. For example, a method of grinding while supplying a slurry containing abrasive grains to the back surface 20a' of the wafer is exemplified. The thickness of the thinned wafer 21 obtained by this is not particularly limited as long as it is a thickness suitable for the processing purpose, but as an example, it is preferably 300 μm or less, more preferably 150 μm or less, and even more preferably 50 μm or less.
[0059] In the back grinding process, a load is applied in the thickness direction of the wafer, which tends to damage the protrusions 20b and the like, resulting in a decrease in yield. In contrast, by using the wafer processing sheet of this embodiment, processing can be performed with at least a portion of the protrusions 20b embedded in the base sheet 11, which makes it possible to avoid damage to the protrusions 20b and the like.
[0060] In addition, the wafer processing sheet of this embodiment has a predetermined viscoelastic property, so that the base sheet 11 follows the main surface 20a of the wafer 20, making it possible to protect the main surface 20a of the wafer 20 and achieve a suitable degree of adhesion. This makes it possible to solve problems such as glue residue on the main surface 20a of the wafer 20, which occurs when using an adhesive sheet in a conventional form in which the convex portion 20b is in contact with the adhesive. In addition, unlike conventional wafer processing sheets in which an adhesive layer is attached to the outer periphery of the wafer 20, there is no need to attach the adhesive layer to the outer periphery of the wafer 20 with high positional accuracy, so the processing process can be simplified.
[0061] [Peeling process] The wafer processing method of the present embodiment may include a peeling step of peeling off the thinned wafer 21 and the base sheet 11. The method of peeling off the base sheet 11 is not particularly limited, but for example, as shown in FIG. 1, the peeling can be performed by bending the base sheet 11 in a direction F so that one end of the base sheet 11 moves away from the thinned wafer 21.
[0062] The peeling step may be carried out at room temperature or under heating. The temperature at which the peeling step is carried out is preferably 10 to 70°C, more preferably 20 to 60°C.
[0063] When using a conventional wafer processing sheet having an adhesive layer, there is a problem of adhesive residue on the main surface 20a of the wafer 20. However, the wafer processing sheet of the present embodiment has a predetermined viscoelasticity property, so it can be peeled off without leaving any adhesive residue.
[0064] As described above, the present invention is not limited to the above-described embodiment, and various modifications are possible without departing from the spirit of the present invention. In other words, the above-described embodiment is merely illustrative in all respects and should not be interpreted as being restrictive.
[0065] For example, the lamination in the lamination step may be performed under reduced pressure in addition to normal pressure. A curable resin may be used instead of or in addition to the other layer 12. When using a curable resin, for example, the curable resin is supplied onto the film, and the surface opposite the surface 11a of the base sheet 11 that contacts the wafer main surface 20a is pressed against the film so as to spread the curable resin on the surface opposite the surface 11a. Then, the wafer processing sheet 10 can be fixed onto the film by curing the curable resin.
[0066] Furthermore, while FIG. 1 mainly shows an example of back grinding, the wafer processing sheet of this embodiment can also be used in dicing and other wafer processing processes. EXAMPLES
[0067] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.
[0068] Example 1 Using a T-die method, an ethylene-methacrylic acid-acrylic acid ester zinc salt copolymer was formed into a substrate sheet (Gunze Co., Ltd., product name "HMD-150") having a thickness of 150 μm.
[0069] Example 2 Using a T-die method, an ethylene-vinyl acetate copolymer was formed into a substrate sheet having a thickness of 150 μm (manufactured by Riken Technos Corporation, product name "EU90B", vinyl acetate content 6 mol%).
[0070] Comparative Example 1 Using the T-die method, an ethylene methacrylic acid copolymer (a resin manufactured by Mitsui DuPont Polychemicals, product name "Nucrel N0407") was formed into a substrate sheet having a thickness of 150 μm.
[0071] Comparative Example 2 Using an inflation method, low-density polyethylene was formed into a base sheet (manufactured by Aicello, product name "N-280") having a thickness of 150 μm.
[0072] Comparative Example 3 A linear low-density polyethylene was formed into a substrate sheet (manufactured by Aicello, product name "N-165") having a thickness of 150 μm by inflation method.
[0073] Comparative Example 4 Using the T-die method, a hydrogenated styrene-based thermoplastic elastomer (manufactured by Asahi Kasei Corporation, resin product name "H1041") was formed into a substrate sheet with a thickness of 150 μm.
[0074] Comparative Example 5 Using the T-die method, unstretched polypropylene was formed into a substrate sheet (manufactured by Futamura Corporation, product name "FRTK-S") having a thickness of 150 μm.
[0075] Comparative Example 6 Using the T-die method, the urethane resin was formed into a substrate sheet (manufactured by Nihon Matai Co., Ltd., product name "Esmer URS") having a thickness of 150 μm.
[0076] [Dynamic viscoelasticity measurement] Dynamic viscoelasticity measurements were performed on each of the above base sheets under the following conditions. First, the base sheets were kept in a thermohygrostat at a temperature of 23°C (±2°C) and a relative humidity of 50% (±5%) for 40 hours. The obtained base sheets were used as samples and dynamic viscoelasticity measurements were performed under normal atmospheric conditions (dry conditions). The dynamic viscoelasticity measuring device used was the "Rheomeric Series RSA III" (manufactured by TA Instruments). (Measurement conditions) Measurement device: "Rheomeric Series RSA III" (manufactured by TA Instruments) Sample: Length 1cm x Width 0.5cm x Thickness 0.2cm Test length: 1cm Sample pretreatment: Keep in an atmosphere of 23°C and 50% relative humidity for 40 hours Test mode: Tensile Frequency: 1.6Hz (10rad / sec) Temperature range: 0~150℃ Heating rate: 5℃ / min Distortion range: 0.10% Initial load: 148g Measurement interval: 1point / ℃
[0077] The storage modulus E' and loss modulus E" obtained by the above measurement are shown in Figs. 3, 5 to 11. Based on Figs. 3, 5 to 11, the storage modulus E' at 30°C to 80°C 30-80 The exponential approximation curve was obtained, and the exponential coefficient and the like were specified. The storage modulus E' and the loss modulus E" as well as the values related to the exponential approximation curve are summarized in Table 1. Note that, as an example, FIG. 4 shows the exponential approximation curve and the coefficient of determination R 2 4(a) is a graph showing the storage modulus E' on a logarithmic scale, and is a graph showing the temperature range of 30°C to 80°C from FIG. 3. FIG. 4(b) is a graph showing the storage modulus E' of FIG. 4(a) in a format not showing the logarithmic scale in order to express the shape of the exponential approximation curve. Exponential approximation curve: y=αe kx y: Storage modulus E' x: Temperature (℃) α: coefficient e: Napier's number k: exponential coefficient
[0078] [Follow-up test] The base sheet obtained as described above was used as a wafer processing sheet, and was pressed against the surface of the wafer on which the protrusions were formed at 100° C. for 1 minute to be attached. The wafer used had a diameter of 8 inches and a thickness of 725 μm. The protrusions formed on the wafer were 230 μm high bumps (protruding electrodes) formed in an area other than the 3.0 mm area around the periphery.
[0079] Thereafter, the temperature was lowered once to room temperature (25°C), and the base sheet was peeled off from the wafer at room temperature. The cross section of the base sheet after peeling was observed, and the cross-sectional shape was evaluated to be one of A to C shown in Fig. 2. The results are shown in Table 1. Fig. 12 shows photographs showing the cross sections of the base sheets in Example 1, Comparative Example 2, and Comparative Example 3.
[0080] [Peeling Test] After the base sheet was peeled off from the wafer as described above, the surface of the wafer was observed and the peelability was evaluated according to the following criteria. (Evaluation criteria for glue residue) A: No residue of the base sheet is found on the wafer surface B: A small amount of the base sheet remains on the wafer surface. C: Remaining base sheet is observed on the wafer surface (Evaluation criteria for damage to convex parts) A: No damage was observed on the convex part of the wafer, or the wafer could be peeled off easily. B: Slight damage was observed on the convex part of the wafer, or a small amount of force was required to peel off the wafer, which may damage the convex part. C: Damage was observed on the convex part of the wafer, or the force required for peeling was likely to damage the convex part.
[0081] [Table 1]
[0082] In Comparative Examples 1 and 4, although there is relatively no problem with the conformability, adhesive residue occurs on the wafer surface, which may result in a decrease in yield in the processing process. In addition, in Comparative Examples 2 and 5, the conformability is too high, and as a result, the base sheet enters the gaps between the convex parts, which damages the convex parts during peeling, or there is a high possibility that the convex parts will be damaged, and adhesive residue is likely to occur. In addition, in Comparative Examples 3 and 6, the conformability is low, so the protection of the convex parts is insufficient. As a result, the back grinding of the semiconductor wafer is performed with only the tips of the convex parts in contact with the base sheet, and in processing processes such as back grinding, excessive load is applied to the convex parts, which causes the convex parts to be damaged, which may result in a decrease in yield in the processing process. [Industrial Applicability]
[0083] The wafer processing sheet of the present invention has industrial applicability as a protective sheet used in backgrinding, dicing, and other wafer processing processes. [Explanation of symbols]
[0084] 10...wafer processing sheet, 11...base material sheet, 11a...surface, 12...layer, 20...semiconductor wafer, 20a...main surface, 20b...projection, 20a'...rear surface, 21...thinned wafer, 31...gap, 32...void, 33...wavy, 34...gap
Claims
1. A base sheet is provided in contact with a main surface of a wafer, Storage modulus E' of the base sheet at 30°C to 80°C 30-80 The exponential coefficient of the exponential approximation curve is −0.035 to −0.
070. Sheet for wafer processing.
2. Storage modulus E' of the base sheet at 30°C 30 and storage modulus E' at 80°C 80 The difference between 30 -E' 80 ) is 4.00 x 10 7 ~4.00 x 10 8 Pa, The wafer processing sheet according to claim 1 .
3. Storage modulus E' of the base sheet at 80°C 80 But, 5.00 x 10 5 ~1.00 x 10 7 Pa, The wafer processing sheet according to claim 1 or 2.
4. Storage modulus E' of the base sheet in the temperature range of 80 to 110°C 80-110 But, 1.00 x 10 6 ~1.00 x 10 7 Pa, The wafer processing sheet according to any one of claims 1 to 3.
5. Loss modulus E″ of the base sheet at 80° C. 80 But 1.50 x 10 4 ~1.50 x 10 6 Pa, The wafer processing sheet according to any one of claims 1 to 4.
6. Loss modulus E" of the base sheet at 30 ° C. 30 But, 1.00 x 10 6 ~1.50 x 10 8 Pa, The wafer processing sheet according to any one of claims 1 to 5.
7. The melting point of the base sheet is 70° C. or higher. The wafer processing sheet according to any one of claims 1 to 6.
8. A lamination step of laminating a surface of the base sheet of the wafer processing sheet according to any one of claims 1 to 7 to a main surface of a wafer, A processing step of processing the wafer in a state where the base sheet and the wafer are bonded together. Wafer processing method.
9. In the processing step, a main surface of the wafer to which the base sheet is not bonded is ground to obtain a thinned wafer. The wafer processing method according to claim 8.
10. In the processing step, the wafer is diced to obtain semiconductor chips. The wafer processing method according to claim 8.
Citation Information
Patent Citations
Adhesive film for protecting front surface of semiconductor wafer, and method of working rear surface of the semiconductor wafer using the adhesive film
JP2005183764A
Surface protection sheet
JP2013211438A
Adhesive film for semiconductor bonding
JP2016086026A
Resin composition for laminated film and laminated film
JP2019014768A
Fluoroelastomer composition
WO2020188125A1