Dry etching method for lithium niobate
The use of chlorine and hydrogen gases with dielectric or photoresist masks in ICP etching addresses the challenges of slow etching rates and complex metal masks in LN etching, achieving higher etching rates and smoother sidewalls while reducing costs and simplifying the process.
Patent Information
- Application Number
- JP2023544098
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-23
- Filing Date
- 2021-12-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-12-09
AI Technical Summary
Conventional dry etching methods for lithium niobate (LN) face challenges such as slow etching rates, increased surface roughness, and the use of expensive and complex metal masks that can damage the crystal, leading to poor sidewall smoothness and high production costs.
A method using chlorine gas (Cl2) and hydrogen gas (H2) with inert gases like argon (Ar) in an inductively coupled plasma (ICP) etching machine, employing dielectric or photoresist masks to achieve high selectivity and smooth sidewalls, avoiding the need for metal masks.
This method enhances etching rates, reduces production costs, and improves sidewall smoothness by using dielectric or photoresist masks, which are easier to use and remove, thus simplifying the process and increasing production capacity.
Smart Images

Figure 0007559252000001 
Figure 0007559252000002 
Figure 0007559252000003
Abstract
Description
[Technical field]
[0001] This application relates to the field of semiconductor processing, and in particular to a method for dry etching lithium niobate.
[0002] This application claims priority to a Chinese patent application with application number 202110697917.1, entitled "Method for dry etching of lithium niobate", filed with the China Patent Office on June 23, 2021, the entire contents of which are incorporated herein by reference. [Background technology]
[0003] Lithium niobate (LN) crystal is a ferroelectric material with an oxygen octahedral structure. It integrates piezoelectric, electro-optical, acousto-optical, nonlinear optical properties, photorefractive effects, and is widely used in many fields such as optical modulation, optical amplification, optical switches, optical storage, and optical waveguides. It is one of the artificial crystals with the most extensive optical performance and the best comprehensive index ever discovered. With the development of integrated optics, the requirements for device performance and integration are constantly increasing, and more requirements are being placed on the LN etching process.
[0004] Dry etching is a process that utilizes the action of atoms and molecules in the plasma state with the material surface to form volatile substances or directly collide with the sample surface to etch it, and can achieve anisotropic etching, that is, the vertical etching speed is much faster than the horizontal etching speed to ensure the fidelity of the fine pattern after transfer. Inductively Coupled Plasma (ICP) etching technology in dry etching has been increasingly applied in the manufacturing of semiconductor devices due to its advantages such as high control precision, excellent uniformity in large-area etching, and low pollution.
[0005] However, LN is a material that is very difficult to etch. In conventional ICP LN etching, a combination of fluorine-based gas (e.g., CF4, CHF3, SF6) and inert gas (e.g., Ar) is generally used. Chlorine-based gas such as Cl2, which is often used in dry etching, has rarely been reported in literature and patents for use in etching LN. Nb elements in LN react with F ions to generate volatile NBF3, NBF4, and NBF5, and Li in lithium niobate reacts with F ions to generate LiF, which is less volatile, and is deposited on the etching surface, reducing the etching rate and increasing the roughness of the etching surface. The LiF deposits are removed by the ion bombardment of Ar gas, increasing the physical action in the etching reaction, improving the etching rate, and improving the smoothness of the etching surface.
[0006] Since the etching rate of LN is slow, in order to obtain a relatively deep etching depth, the mask often selects a metal film layer that can withstand etching under F-based gas, such as metal Cr, Cu, and Al. However, the production of metal thin films requires dedicated equipment, the manufacturing process is complicated, the cost is high, and it is difficult to remove after etching. Metals can damage the LN wafer during the process of forming a pattern by the lift-off process, which can result in cracks on the wafer and adversely affect subsequent processes. When a pattern is formed on a metal mask, there are often vertical stripes on the sidewall, and dry etching transfers these stripes to the LN sidewall after etching, resulting in a lack of smoothness on the LN sidewall after etching. Summary of the Invention [Problem to be solved by the invention]
[0007] Various exemplary embodiments of the present application provide a method for dry etching lithium niobate.
[0008] One embodiment of the present application provides a method for dry etching lithium niobate, the method including step 1 of feeding a patterned lithium niobate into an etching machine, and etching gases of Cl2, H 2、 and introducing a mixture of an inert gas such as Ar gas or He gas into an etching cavity of the etching machine, igniting the etching machine with RF to start etching, and step 3 terminating the etching when an etching time is reached.
[0009] In one embodiment, the lithium niobate in step 1 may be a lithium niobate wafer, the splitting direction of which is not limited, and the wafer is the material to be etched.
[0010] In one embodiment, the lithium niobate sample in step 1 is a wafer made of a lithium niobate thin film grown above a substrate, so the direction of division is not limited, and the lithium niobate thin film-containing wafer is the material to be etched. The substrate may be a silicon substrate or other substrate, and a thin film material such as silica may be present on the substrate.
[0011] In one embodiment, the lithium niobate sample in step 1 may use a hard mask such as a SiO thin film, a SiN thin film or a Si thin film as a mask material in dry etching, and the sample must complete patterning before etching.
[0012] In one embodiment, the sample in step 1 uses photoresist as a mask material in dry etching, and the sample must be patterned before etching. In the dry etching method for lithium niobate described in the present application, the proportion of H2 in the total gas flow rate in the etching gas in step 2 is 20% to 80%.
[0013] In one embodiment, the proportion of Cl2 in the total gas flow rate of the etching gas in step 2 is 5% to 60%.
[0014] In one embodiment, the etcher has an upper RF power range of 200w to 1200w and a lower RF power range of 30w to 600w during the etching.
[0015] In one embodiment, the etcher has a cavity pressure during the etching of less than 20 mT.
[0016] In one embodiment, the etching machine has a coolant temperature range of 0°C to 80°C during the etching. Effect of the Invention
[0017] The dry etching method of lithium niobate adopted in this application is different from the conventional fluorine-based etching system of lithium niobate, and uses Cl2 / H2 gas to etch lithium niobate. This application can use dielectric materials and photoresists as masks, so that when applied to the production line, it can not only optimize the production process, but also greatly improve production capacity and save costs.
[0018] According to the dry etching method of lithium niobate adopted in the present application, a conventional photoresist mask or a dielectric material such as SiO, SiN, or Si can be used as a hard mask for dry etching of lithium niobate, and good selectivity and good morphology can be obtained.
[0019] The lithium niobate dry etching method adopted in the present application has a high selectivity to the lithium niobate mask, allowing the thickness of the dielectric mask or photoresist mask to be made thinner, simplifying the mask patterning and removal processes.
[0020] In conventional production lines, metal masks such as Cr, Al, and Cu were often used for etching lithium niobate. LN etching using a metal mask has many drawbacks.
[0021] The metal masks employed in the prior art have complicated manufacturing processes, high costs, require specialized equipment for deposition of the metal masks, and require photolithography to be performed first and then transfer the pattern to the metal film layer using a complicated process to pattern the metal masks, whereas in the lithium niobate dry etching method employed in the present application, the photoresist masks employed are patterned only through photolithography processes, the deposition cost of the dielectric mask is low, the patterning is easy, and the patterning can even be completed in the same etch cavity as the dry etching step.
[0022] The metal mask used in the prior art is difficult to remove after etching, and the removal cost is high. On the other hand, in the lithium niobate dry etching method used in the present application, the dielectric and photoresist used are easily removed after dry etching, the removal cost is low, the method is mature, and even the mask removal process can be performed without breaking the vacuum after etching.
[0023] During the deposition and patterning of metal masks on lithium niobate wafers, the associated processes are prone to damage the lithium niobate crystals, causing the crystals to crack. The lithium niobate dry etching method adopted in this application can avoid the occurrence of cracks by using a dielectric mask or a photoresist mask.
[0024] The lithium niobate dry etching method adopted in this application is an effective means for reducing costs and simplifying the process of lithium niobate devices, and can provide a new process path in the production line, greatly saving production costs and improving production capacity. [Brief description of the drawings]
[0025] [Figure 1] FIG. 1 is a schematic diagram of an etching result 1 of an LN wafer using a SiO mask according to one embodiment of the present application. [Diagram 2] FIG. 2 is a schematic diagram of an etching result 2 of an LN wafer using the SiO mask of the embodiment shown in FIG. [Diagram 3] FIG. 1 is a schematic diagram showing an etching result 1 of an LN wafer using a PR mask according to an embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram of an etching result 2 of an LN wafer using the PR mask of the embodiment shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] In order to make the objectives and technical solutions of the embodiments of the present application clearer, the technical solutions of the embodiments of the present application will be described clearly and completely below with reference to the drawings of the embodiments of the present application. It is clear that the described embodiments are only a part of the embodiments of the present application, not all of them. All other embodiments obtained by those skilled in the art based on the described embodiments of the present application without creative efforts shall be within the scope of protection of the present application.
[0027] The basic principle of the dry etching method for lithium niobate described in this application is as follows.
[0028] In the dry etching of lithium niobate, it is very important that the product exists in gaseous form under vacuum conditions and can be pumped out. Nb compounds generally have a low boiling point, exist in gaseous form under high vacuum conditions and are easy to pump out, and do not affect the progress of etching. On the other hand, Li compounds generally have a high boiling point and are difficult to volatilize even under high vacuum conditions. They are prone to forming deposits that hinder the progress of etching, reduce the steepness of the sidewall, and cause sidewall roughness.
[0029] LiF, which is generated when a conventional fluorine-based gas etches lithium niobate, has a boiling point of 1717°C at room temperature. In the present application, H2, Cl2, and Li2NbO3 undergo a chemical reaction, and the LI compound contains LiH and LiCl, where LiH has a boiling point of 950°C at room temperature and pressure, and LiCl has a boiling point of 1383°C at room temperature and pressure. LiH and LiCl have lower boiling points and are more volatile than LiF, which is advantageous for reducing the slope and roughness of the sidewall caused by deposition and obtaining a steep etching form and a smooth etching surface. In the conventional fluorine-based LN etching system, the steepness of the obtained sidewall is generally about 60° to 75°, while when etching LN with this system, a steep sidewall slope of 80° or more can be obtained.
[0030] The present invention can etch LN using conventional PR masks or dielectrics such as SiO, SiN, and Si as hard masks, and can obtain good selectivity and good morphology, which is an effective means for reducing costs and simplifying processes for LN processes, and avoids the disadvantages of etching LN using metal masks, such as complicated manufacturing processes, high costs, difficult removal, and lift-off processes that are prone to damage LN crystals and rough LN sidewalls. In addition, SiO and PR masks are easy to smooth the sidewalls, which is advantageous for obtaining smooth LN sidewalls after etching.
[0031] In the process of the present application, Cl2 and H2 are used as the main etching gas, and an appropriate amount of inert gas is added as auxiliary, and the etching uses ME (Main Etch) step with stable parameters. The power of the upper RF is 200w-1200w, the power of the lower RF is 30w-600w, the proportion of H2 in the total gas flow is 20%-80%, the proportion of Cl2 in the total gas flow is 5%-60%, the cavity pressure is less than 20mT, and the temperature of the coolant during the process is 0℃-80℃. When the etching material is crystalline LN or thin film LN, the pattern is not limited, and with appropriate parameters, the etching process can obtain an ideal morphology, a faster etching rate, and a relatively high selectivity to the mask. Example 1
[0032] In this embodiment shown in Figures 1 and 2, the machine used in the etching process was an Inductively Coupled Plasma (ICP) etcher, model HAASRODE-E200. The sample used was an LN wafer with a size of 1cm*1cm, a film layer structure of 2.1μmSiO / 500umZ-cutLNSub, and a SiO hard mask already patterned. The pattern was a line with a CD of about 3μm.
[0033] The sample was transferred into the etcher chamber. Appropriate etching parameters were set, for example, upper RF power 600w, lower RF power 100w, cavity pressure 5mT, process temperature 20°C, ME time of process 10min, Cl2, H2 and Ar mixture was introduced, ignited by RF to start etching.
[0034] The sample was transferred into the etcher chamber. Appropriate etching parameters were set, for example, upper RF power 600w, lower RF power 100w, cavity pressure 5mT, process temperature 20℃, and process ME time 10min. A mixture of Cl2, H2 and Ar was introduced and ignited by RF to start etching. When the etching time, which is the time length required for the etching process, was reached, the etching was stopped. After etching was completed, the sample was taken out and the cross section was photographed using SEM to inspect the etching morphology.
[0035] According to the experimental results after etching, taken together with Figures 1 and 2, the ER was 46.7 nm / min, the LN / SiO selectivity was 1.57, and the slope was about 81°. The sidewalls were smooth and the roughness of the bottom was based on the values before etching. In the conventional LN fluorine-based etching system, the obtained sidewall slope was generally about 60° to 75°, while when etching LN with this system, a sidewall slope of more than 80° could be obtained. Example 2
[0036] In Example 2 shown in Figures 3 and 4, the machine used in the etching process is an inductively coupled plasma etching machine of model HAASRODE-E200.The sample used is an LN wafer with a size of 1cm*1cm and a film layer structure of 1.8μmPR / 500umZ-cutLNSub, and the pattern is a groove with a CD of about 2μm.
[0037] The sample was transferred into the etching chamber. Appropriate etching parameters were set, for example, upper RF power 600w, lower RF power 80w, cavity pressure 5mT, process temperature 20℃, ME time of process 10min, Cl2, H2 and Ar mixed gas were introduced, ignited by RF to start etching. After etching was completed, the sample was taken out and the cross section was photographed using SEM to inspect the etching form of the sample.
[0038] The ER was 53.7 nm / min, the LN / PR selectivity was 1.34, the steepness was about 71°, and the sidewalls and bottom were smooth. According to the experimental results of the above two examples, the selectivity of lithium niobate to dielectric material or photoresist in etching was about 1:1 in both cases. In the conventional fluorine-based etching system for lithium niobate, the steepness of the obtained sidewall was generally about 60° to 75°, while when etching lithium niobate with this system, a steepness of the sidewall of 80° or more could be obtained. In addition, SiO and PR masks are easy to make the sidewall smooth, and the products during etching are easier to volatilize than in the conventional process, so that the deposition of the sidewall is reduced, which is advantageous for obtaining a smooth sidewall after etching.
[0039] The above is merely a preferred embodiment of the present invention, but the scope of protection of the present application is not limited thereto, and any modifications or replacements that a person skilled in the art can easily conceive within the technical scope disclosed in the present application shall be included in the scope of protection of the present application. Therefore, the scope of protection of the present application should be in accordance with the scope of protection of the claims.
Claims
1. A method for dry etching lithium niobate, comprising the steps of: Step 1: loading patterned lithium niobate into an etcher; Etching gas Cl 2 , H 2 Step 2: introducing the mixture of fluorine and an inert gas into an etching cavity of the etcher and starting the etcher by RF ignition; and step 3 of terminating the etching when the etching time is reached. The lithium niobate in step 1 is a lithium niobate wafer, and the lithium niobate wafer is a wafer to be etched, or the lithium niobate in step 1 is a lithium niobate thin-film-containing wafer made of a lithium niobate thin-film grown above a substrate to be etched; The lithium niobate wafer or the lithium niobate thin film-containing wafer uses a SiO thin film, a SiN thin film, or a Si thin film as a mask material after completing patterning in dry etching, and the SiO thin film, the SiN thin film, or the Si thin film is a hard mask; The method, wherein the lithium niobate wafer or the lithium niobate thin film containing wafer uses photoresist as a mask material to complete patterning in dry etching.
2. In the etching gas in the step 2, the H 2 The method according to claim 1, wherein the ratio of is 20% to 80%.
3. The Cl content in the total gas flow rate of the etching gas in step 2 2 The method according to claim 1, wherein the ratio of is 5% to 60%.
4. 2. The method of claim 1, wherein the etcher has a top RF power range of 200w to 1200w and a bottom RF power range of 30w to 600w during the etch.
5. 10. The method of claim 1, wherein the etcher has a cavity pressure of less than 20 mT during the etch.
6. The method of claim 1 , wherein the etching machine has a coolant temperature range of 0° C. to 80° C. during the etching.
Citation Information
Patent Citations
Through hole etching method of single crystal thin film on substrate
CN110211922A
Etching method for lithium niobate material
CN110364441A
Method of etching high-permittivity multicomponent oxide film and refractory metal film, manufacture of thin-film capacitor, and plasma apparatus for film formation
JP1994151383A
Method and device for plasma processing, and memory medium
JP2007165827A
Selective etching of high dielectric constant films with h2 doping
JP2009508334A