Paper product, cured product, and method for producing paper product

By optimizing the matrix resin composition with thermosetting resin and inorganic fillers, the paper product achieves enhanced bending strength and modulus through improved fiber dispersion and resin interaction.

JP7559345B2Active Publication Date: 2024-10-02SUMITOMO BAKELITE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020078059
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-27
Publication Date
2024-10-02
Estimated Expiration
2040-04-27

AI Technical Summary

Technical Problem

Existing papermaking technologies focus on reducing anisotropy in fiber orientation, but neglect the potential for improving bending strength and flexural modulus by optimizing the matrix resin composition.

Method used

A paper product is produced using a thermosetting resin composition independently dispersed with reinforcing fibers, where the resin includes inorganic fillers or modified thermosetting resins to enhance mechanical properties.

Benefits of technology

The approach significantly improves bending strength and bending elastic modulus of the cured product by uniformly dispersing reinforcing fibers and inorganic fillers within the thermosetting resin matrix.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559345000002
    Figure 0007559345000002
  • Figure 0007559345000003
    Figure 0007559345000003
  • Figure 0007559345000001
    Figure 0007559345000001
Patent Text Reader

Abstract

To provide a sheet making body capable of improving bending strength and a coefficient of bending elasticity when the sheet making body is formed into a cured matter.SOLUTION: A sheet making body 21 is obtained using a disperse medium in which a thermosetting resin composition (including thermosetting resin A) and reinforcing fiber B are independently dispersed. Inorganic fillers are finely dispersed in the thermosetting resin composition (including the thermosetting resin A).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a paper article, a cured product, and a method for producing a paper article. [Background technology]

[0002] The application of papermaking techniques, which are a technology used in papermaking, has been considered as a manufacturing method for fiber-reinforced plastics (FRP), in which monofilaments such as organic fibers, carbon fibers, and glass fibers are dispersed in a resin matrix.

[0003] For example, Patent Document 1 describes a fiber-reinforced resin that is composed of a reinforcing fiber substrate made of a group of fiber bundles of short reinforcing fibers and a matrix resin made of a thermosetting resin. Patent Document 1 describes that a certain number or more of the fiber bundles of the reinforcing fiber substrate are split to have a specific number of single yarns, the number of straight fiber bundles is a specific number or more, the orientation of the fiber bundles is two-dimensionally pseudo-isotropic, and the volume content of the reinforcing fibers is a specific number or more, thereby achieving a high degree of isotropy and exhibiting high strength. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-174605 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the technology disclosed in Patent Document 1 focuses on the reinforcing fibers contained in the paper product, and attempts to reduce the anisotropy due to the orientation of the reinforcing fibers by using reinforcing fiber bundles of short fibers in a specific range. In response to this, the present inventors focused their attention on the matrix resin of the paper product and discovered that by using a specific matrix resin to obtain a paper product, it is possible to improve the bending strength and bending modulus of the cured product, thereby completing the present invention. [Means for solving the problem]

[0006] According to the present invention, there is provided a papermaking product obtained by using a dispersion medium in which a thermosetting resin composition and reinforcing fibers are each independently dispersed, comprising: the thermosetting resin composition comprises a thermosetting resin, A paper article is provided in which an inorganic filler is finely dispersed in the thermosetting resin composition.

[0007] According to the present invention, there is also provided a papermaking product obtained by using a dispersion medium in which a thermosetting resin composition and reinforcing fibers are each independently dispersed, comprising: The thermosetting resin composition comprises a modified thermosetting resin. Effect of the Invention

[0008] According to the present invention, there is provided a paper article which, when cured, has improved bending strength and bending modulus. [Brief description of the drawings]

[0009] [Figure 1] 1 is a schematic diagram showing a cross section and a part of a plane of a paper article according to an embodiment of the present invention. FIG. [Diagram 2] 2 is a schematic cross-sectional view showing an example of a method for producing a paper article according to the present embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present invention will be described with reference to the drawings. In all the drawings, the same components are given the same reference numerals and the description will be omitted as appropriate.

[0011] <Paperwork> 1 is a schematic diagram showing a cross section and a part of a plan view of a paper article 21 according to this embodiment. The paper article 21 is a molding material in a B-stage state in which reinforcing fibers are dispersed with a thermosetting resin A as a matrix resin. The thermosetting resin A functions as a binder that bonds the reinforcing fibers B together, and also functions as a molding material for obtaining a molded article from the paper article 21 by a subsequent heat treatment.

[0012] In Fig. 1, the region of the paper product indicated by the dotted line is a partially enlarged schematic diagram of a cross section and a plan view. The paper product 21 according to this embodiment is obtained by a papermaking method described later, and has the following structural characteristics 1 to 3. (Feature 1) In a plan view of the surface of the paper article 21, the reinforcing fibers B are randomly oriented. (Feature 2) In a cross-sectional view in the thickness direction of the paper article 21, the orientation state of the reinforcing fibers B is highly controlled, and the reinforcing fibers B are oriented in a specific direction. In other words, in the thickness direction of the paper article 21, the reinforcing fibers B are in a laminated state. (Feature 3) Reinforcing fibers B are bonded together by thermosetting resin A.

[0013] Since the paper product 21 is formed by a papermaking method, the thermosetting resin A is uniformly dispersed and the paper product 21 has excellent processability. This also improves the design of the paper product 21. Furthermore, the papermaking method places few restrictions on the combination of materials that can be used to form the paper product 21.

[0014] The paper article 21 according to this embodiment has a first or second form, as described below.

[0015] <<First Form>> The first embodiment of the paper product according to the present invention is a paper product obtained by using a dispersion medium in which a thermosetting resin composition and reinforcing fibers are each dispersed independently, and an inorganic filler is finely dispersed in the thermosetting resin composition. In other words, the paper product according to the first embodiment is obtained by dispersing a thermosetting resin composition containing a thermosetting resin having inorganic filler finely dispersed therein and reinforcing fibers in a dispersion medium described below, and then forming the thermosetting resin composition into a paper product. As a result, in the paper product, the inorganic filler is positioned near the thermosetting resin, and the inorganic filler can increase the elastic modulus of the thermosetting resin, making it easier to improve the bending strength and bending modulus of the cured paper product as a whole.

[0016] The method for obtaining the thermosetting resin composition is not particularly limited, but for example, a thermosetting resin, an inorganic filler, and an optional additive are mixed using a mixer, and then kneaded for 5 to 10 minutes using a biaxial roll or the like at, for example, 70 to 90° C. The kneaded product thus obtained is cooled and then pulverized to obtain a powdered thermosetting resin composition (molding material) in which the inorganic filler is finely dispersed.

[0017] The average particle size (d50) of the powdered thermosetting resin composition is preferably 10 to 100 μm, more preferably 20 to 80 μm, and even more preferably 30 to 70 μm, which makes it easier to disperse the inorganic filler inside and improve the mechanical strength of the paper product obtained later. The average particle size of the thermosetting resin composition can be measured in the same manner as for the inorganic filler described below.

[0018] [Inorganic filler] In the first embodiment, the inorganic filler is used to increase the elastic modulus of the thermosetting resin. Examples of inorganic fillers include one or more selected from calcium sulfate, barium sulfate, aluminum hydroxide, magnesium hydroxide, aluminum oxide (alumina), crystalline or fused silica, surface-treated silica, talc, kaolin, clay, mica, dolomite, wollastonite, glass fiber, carbon fiber, glass beads, zircon, and molybdenum compounds. Among them, from the viewpoint of easily improving the bending strength and bending modulus of the paper product as a whole, fused silica is preferred, clay is more preferred, and a mixture of these may be used.

[0019] The inorganic filler may be surface-treated. For example, the surface treatment may be performed with a coupling agent such as a silane coupling agent. This can suppress the aggregation of the inorganic filler and provide good dispersibility. As the coupling agent, for example, primary aminosilanes such as γ-aminopropyltriethoxysilane and γ-aminopropyltrimethoxysilane can be used. When a coupling agent is used, its content is not particularly limited, but is preferably 0.05 to 3 parts by weight, and more preferably 0.1 to 2 parts by weight, based on 100 parts by weight of the inorganic filler.

[0020] The content of the inorganic filler is preferably 5 mass% or more and 70 mass% or less, more preferably 10 mass% or more and 60 mass% or less, and even more preferably 20 mass% or more and 50 mass% or less, based on the total amount of the thermosetting resin composition. By setting the content of the inorganic filler to be equal to or more than the above lower limit, the mechanical strength can be improved, whereas by setting the content of the inorganic filler to be equal to or less than the above upper limit, good mechanical strength can be stably obtained.

[0021] The average particle size of the inorganic filler is preferably from 0.1 to 100 μm, more preferably from 0.1 to 50 μm, and further preferably from 0.1 to 20 μm. By setting the average particle size of the inorganic filler to be equal to or larger than the lower limit, the mechanical strength can be improved, whereas by setting the average particle size of the inorganic filler to be equal to or smaller than the upper limit, the dispersibility can be improved and the mechanical strength can be stabilized. When a fibrous inorganic filler material is selected, it is preferable to shorten the fiber length by cutting or the like.

[0022] The average particle size of the inorganic filler is the particle size (D50) that is the cumulative 50% of the volume-based particle size distribution, and can be measured with a commercially available laser type particle size distribution analyzer (for example, SALD-7000 manufactured by Shimadzu Corporation).

[0023] <<Second Form>> The second embodiment of the paper product according to the present embodiment is a paper product obtained by using a dispersion medium in which a thermosetting resin composition and reinforcing fibers are each independently dispersed, and the thermosetting resin composition contains a modified thermosetting resin. That is, the paper product according to the second embodiment is obtained by dispersing the modified thermosetting resin and reinforcing fibers in a dispersion medium described below, and then forming the paper product. This makes it possible to stably increase the elastic modulus of the thermosetting resin, and improve the bending strength and bending modulus of the paper product as a whole.

[0024] The method for obtaining the thermosetting resin composition of the present embodiment is not particularly limited, but for example, a thermosetting resin and, for example, an elastomer component described below are mixed using a mixer, and then kneaded for 5 to 10 minutes at, for example, 70 to 90° C. using a biaxial roll or the like to obtain a kneaded product. The kneaded product obtained is cooled and then pulverized to obtain a thermosetting resin composition (molding material) containing a thermosetting resin modified by the elastomer component or the like.

[0025] As the modified thermosetting resin, a thermosetting resin described below that has been modified with an elastomer component is preferable. The elastomer component may be one or more selected from the group consisting of polyvinyl acetal resin, acrylic rubber, acrylonitrile butadiene rubber (NBR), styrene butadiene rubber (SBR), silicone rubber, butyl rubber, urethane rubber, polybutadiene, isoprene rubber, chloroprene rubber, and copolymers thereof. This makes it possible to improve the toughness of the thermosetting resin, and makes it easier to improve the bending strength and bending modulus of a paper product using the same.

[0026] Among them, polyvinyl acetal resins are preferred. The polyvinyl acetal resins are resins obtained by acetalizing polyvinyl alcohol with a carbonyl compound such as formaldehyde or acetaldehyde, and examples of the polyvinyl acetal resins include polyvinyl formal and polyvinyl butyral. Of these, at least one of them can be used. The degree of acetalization of the polyvinyl acetal resin is preferably 50% or more, more preferably 60% or more, from the viewpoint of obtaining reactivity, while it is preferably 80% or less from the viewpoint of compatibility.

[0027] The content of the elastomer component is, for example, preferably 1% by weight or more and 40% by weight or less, more preferably 2% by weight or more and 20% by weight or less, and even more preferably 3% by weight or more and 10% by weight or less, based on the entire thermosetting resin composition (100% by weight).

[0028] Below, the contents common to the first and second embodiments will be described.

[0029] [Thermosetting resin A] The thermosetting resin is used as a matrix resin in the paper product. Specifically, the thermosetting resin may be a phenol resin, an epoxy resin, a melamine resin, a polyurethane, or an unsaturated polyester resin. The thermosetting resin may be one or more of the above specific examples. The thermosetting resin may be a phenol resin, for example, from the above specific examples. This can improve the strength of the molded product. Therefore, the anisotropy of the bending strength can be reduced. It is also preferable from the viewpoint of improving the dispersibility of the reinforcing fibers.

[0030] (Phenol Resin) Specific examples of the phenolic resin include novolac-type phenolic resin, resol-type phenolic resin, and aryl alkylene-type phenolic resin. As the phenolic resin, one of these may be used alone, or two or more types having different weight average molecular weights may be used in combination, or one or more types may be used in combination with their prepolymers. As the phenolic resin, it is preferable to use, for example, novolac-type phenolic resin or resol-type phenolic resin from the above specific examples.

[0031] The novolac type phenolic resin can be appropriately selected according to the purpose as long as it is a resin obtained by reacting a phenol with an aldehyde in the absence of a catalyst or in the presence of an acid catalyst. For example, random novolac type and high ortho novolac type phenolic resins can also be used. There can be. The novolac type phenolic resin can usually be obtained by reacting the aldehydes with the phenols at a molar ratio (aldehydes / phenols) controlled to be 0.5 or more and 1.0 or less.

[0032] Specific examples of phenols used in preparing this novolac type phenolic resin include phenol, o-cresol, m-cresol, p-cresol, xylenol, alkylphenols, catechol, resorcin, etc. These phenols may be used alone or in combination of two or more.

[0033] Specific examples of aldehydes used in preparing the novolac phenolic resin include aldehyde compounds such as formaldehyde, paraformaldehyde, and benzaldehyde, as well as sources of these aldehyde compounds, or solutions of these aldehyde compounds. These aldehydes may be used alone or in combination of two or more.

[0034] Specific examples of acid catalysts used in preparing the novolac phenolic resin include organic carboxylic acids such as oxalic acid and acetic acid, organic sulfonic acids such as benzenesulfonic acid, paratoluenesulfonic acid, and methanesulfonic acid, organic phosphonic acids such as 1-hydroxyethylidene-1,1'-diphosphonic acid and 2-phosphonobutane-1,2,4-tricarboxylic acid, and inorganic acids such as hydrochloric acid, sulfuric acid, and phosphoric acid. These may be used alone or in combination of two or more.

[0035] The resol type phenolic resin can be appropriately selected according to the application, so long as it is a resin obtained by reacting a phenol with an aldehyde in the presence of a basic catalyst. Incidentally, this resol type phenolic resin can usually be obtained by reacting the aldehydes while controlling the molar ratio of the phenols to the aldehydes (aldehydes / phenols) to be 1.3 or more and 1.7 or less.

[0036] Specific examples of phenols used in preparing this resol type phenolic resin include phenol, o-cresol, m-cresol, p-cresol, xylenol, alkylphenols, catechol, and resorcin. These phenols may be used alone or in combination of two or more.

[0037] Specific examples of aldehydes used in preparing the resol-type phenolic resin include aldehyde compounds such as formaldehyde, paraformaldehyde, and benzaldehyde, as well as sources of these aldehyde compounds, or solutions of these aldehyde compounds. These aldehydes may be used alone or in combination of two or more.

[0038] Specific examples of basic catalysts used in preparing resol-type phenolic resins include alkali metal hydroxides such as sodium hydroxide, lithium hydroxide, and potassium hydroxide, oxides and hydroxides of alkaline earth metals such as calcium, magnesium, and barium, sodium carbonate, aqueous ammonia, amines such as triethylamine and hexamethylenetetramine, and divalent metal salts such as magnesium acetate and zinc acetate. These may be used alone or in combination of two or more.

[0039] (Epoxy resin) The above epoxy resins are not limited to those mentioned above, and any monomer, oligomer, or polymer having two or more epoxy groups in one molecule can be used, regardless of its molecular weight or molecular structure. It is. Specific examples of epoxy resins include biphenyl type epoxy resins; bisphenol type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AD ​​type, and tetramethylbisphenol F type epoxy resins; stilbene type epoxy resins; novolac type epoxy resins such as phenol novolac type epoxy resins and cresol novolac type epoxy resins; polyfunctional epoxy resins such as triphenyl type epoxy resins exemplified by triphenol methane type epoxy resins and alkyl-modified triphenol methane type epoxy resins; phenol aralkyl type epoxy resins having a phenylene skeleton, naphthol aralkyl type epoxy resins having a phenylene skeleton, and phenol aralkyl type epoxy resins having a biphenylene skeleton. phenol aralkyl type epoxy resins such as aryl type epoxy resins (biphenyl aralkyl type epoxy resins) and naphthol aralkyl type epoxy resins having a biphenylene skeleton; naphthol type epoxy resins such as dihydroxynaphthalene type epoxy resins and epoxy resins obtained by glycidyl etherification of dihydroxynaphthalene dimers; triazine nucleus-containing epoxy resins such as triglycidyl isocyanurate and monoallyl diglycidyl isocyanurate; bridged cyclic hydrocarbon compound modified phenol type epoxy resins such as dicyclopentadiene modified phenol type epoxy resins; brominated type epoxy resins such as brominated bisphenol A type and brominated phenol novolac type; tris(hydroxyphenyl)methane type epoxy resins. As the epoxy resin, one of these may be used alone, or two or more different types may be used in combination.

[0040] The upper limit of the weight average molecular weight of the thermosetting resin is, for example, preferably not more than 10,000, more preferably not more than 9,000, and even more preferably not more than 8,000. This reduces the viscosity of the slurry when it is formed, and can further improve the dispersibility of the reinforcing fibers and the thermosetting resin. The lower limit of the weight average molecular weight of the thermosetting resin is, for example, preferably 2000 or more, more preferably 3000 or more, and even more preferably 4000 or more. This can improve the mechanical strength of the molded product. Therefore, the anisotropy of the bending strength can be further reduced.

[0041] The lower limit of the content of the thermosetting resin in the paper product is, for example, preferably 30 parts by mass or more, more preferably 35 parts by mass or more, even more preferably 40 parts by mass or more, and even more preferably 45 parts by mass or more, based on the total solid content of the paper product, which can further improve the random orientation of the reinforcing fibers in the paper product. The upper limit of the content of the thermosetting resin in the paper product is, for example, preferably 70 parts by mass or less, more preferably 65 parts by mass or less, even more preferably 60 parts by mass or less, and even more preferably 55 parts by mass or less, based on the total solid content of the paper product. This is preferable from the viewpoint of improving the moldability of the paper product, making it easier to mold it into a desired shape, and enabling the molded product to be used in applications requiring a precise structure. In this embodiment, the total solid content of the paper product refers to the total of the raw material components excluding the dispersion medium.

[0042] [Reinforced fiber B] The reinforcing fibers according to the present embodiment are not limited, and specifically, metal fibers; inorganic fibers such as carbon fibers, glass fibers, and ceramic fibers; natural fibers such as wood fibers, cotton, hemp, and wool; regenerated fibers such as rayon fibers; semi-synthetic fibers such as cellulose fibers; synthetic fibers such as polyamide fibers, aramid fibers, polyimide fibers, polyvinyl alcohol fibers, polyester fibers, acrylic fibers, polyparaphenylene benzoxazole fibers, polyethylene fibers, polypropylene fibers, polyacrylonitrile fibers, and ethylene vinyl alcohol fibers can be used. As the reinforcing fibers, one or more of the above specific examples can be used in combination. As the reinforcing fibers, it is preferable to use inorganic fibers or synthetic fibers, for example, from the above specific examples. In addition, it is preferable to use, for example, glass fibers or carbon fibers as inorganic fibers. Furthermore, it is preferable to use, for example, aramid fibers as synthetic fibers. This can suitably reinforce paper-made bodies and molded products. It is also preferable from the viewpoint of further improving the dispersibility of the reinforcing fibers in the slurry.

[0043] (Other Ingredients) In addition to the thermosetting resins and reinforcing fibers described above, the paper product according to this embodiment may contain, for example, pulp fibers, paper-making agents, ion exchange agents, fillers, flocculants, conductivity imparting agents, flame retardants, flame retardant assistants, pigments, dyes, lubricants, release agents, compatibilizers, dispersants, crystal nucleating agents, plasticizers, heat stabilizers, antioxidants, coloring inhibitors, ultraviolet absorbers, flowability modifiers, foaming agents, antibacterial agents, vibration damping agents, deodorizing agents, sliding property modifiers, and antistatic agents. Representative components will be described below.

[0044] (Pulp fiber) The paper product according to the present embodiment may further include pulp fibers obtained by fibrillating organic fibers. Pulp fibers are not particularly limited, but include pulp-like fibers obtained by fibrillating organic fibers such as cellulose fibers such as linter pulp and wood pulp, natural fibers such as kenaf, jute, and bamboo, para-type wholly aromatic polyamide fibers and their copolymers, aromatic polyester fibers, polybenzazole fibers, meta-type aramid fibers and their copolymers, acrylic fibers, acrylonitrile fibers, polyimide fibers, and polyamide fibers. As the pulp fibers, one or a combination of two or more of the above specific examples may be used.

[0045] The method for fibrillating the organic fibers is not particularly limited, but the organic fibers can be dispersed in water to form a slurry, which is then beaten with a beater or refiner to produce the fibrillated organic fibers. The slurry concentration during beating is optional, but a solid content concentration of 0.1 to 10 mass% is preferred.

[0046] (Papermaking chemicals) A papermaking agent can be added to the paper product of this embodiment for the purpose of improving material yield, etc. The papermaking agent is not particularly limited, but examples thereof include thermoplastic resins such as acrylic polymers, vinyl polymers, polyurethanes, polyamides, polyesters, and polyethylene oxides, and one or more selected from these are used. The thermoplastic resin used as the papermaking agent preferably has at least one functional group selected from amino groups, epoxy groups, carboxyl groups, oxazoline groups, carboxylate groups, and acid anhydride groups, and may have two or more functional groups. Among these, thermoplastic resins having amino groups are more preferable.

[0047] (Ion exchange agent) The paper product of the present embodiment may contain an ion exchange agent, which is a powdery material having ion exchange ability. Specific examples of the ion exchange agent include clay minerals, scaly silica fine particles, hydrotalcites, fluorine taeniolite, and swellable synthetic mica. The ion exchange agent may be one or more of the above specific examples in combination. This is advantageous in terms of efficiently producing an aggregate of the thermosetting resin and the reinforcing fibers while maintaining the fiber length of the reinforcing fibers long.

[0048] The clay minerals may be natural or synthetic, and are not particularly limited. Examples of the clay minerals include smectite, halloysite, kanemite, kenyaite, zirconium phosphate, and titanium phosphate. The hydrotalcites are not particularly limited as long as they have ion exchange capacity. Examples of the fluorine taeniolite include, but are not limited to, lithium-type fluorine taeniolite, sodium-type fluorine taeniolite, etc. Examples of the swellable synthetic mica include, but are not limited to, sodium-type tetrasilicon fluorine mica, lithium-type tetrasilicon fluorine mica, etc., and one type may be used alone or two or more types may be used in combination.

[0049] Among these, clay minerals are more preferable, and smectite is even more preferable in that it is available in a wide range of products, from natural to synthetic. The smectite is not particularly limited as long as it has ion exchange ability, but examples thereof include montmorillonite, beidellite, nontronite, saponite, hectorite, sauconite, and stevensite. The montmorillonite is a hydrous silicate of aluminum, but it may be bentonite that contains montmorillonite as a main component and also contains minerals such as quartz, mica, feldspar, and zeolite. When used in applications where coloring or impurities are a concern, synthetic smectite with fewer impurities is preferred.

[0050] Examples of powdered substances having the above-mentioned ion exchange capacity include Kunipia (bentonite) and Sumecton SA (synthetic saponite) manufactured by Kunimine Industries Co., Ltd., Sunlovely (flake-like silica microparticles) manufactured by AGC Si-Tech Co., Ltd., Somasif (swellable synthetic mica) and Lucentite (synthetic smectite) manufactured by Co-op Chemical Co., Ltd., and hydrotalcite STABIACE HT-1 (hydrotalcite) manufactured by Sakai Chemical Industry Co., Ltd., but are not limited to these.

[0051] (filling material) Examples of the filler include crushed glass, mica, talc, kaolin, sericite, bentonite, xonotlite, sepiolite, smectite, montmorillonite, wollastonite, silica, calcium carbonate, glass beads, glass flakes, glass microballoons, clay, molybdenum disulfide, titanium oxide, zinc oxide, antimony oxide, aluminum oxide, zinc oxide, calcium polyphosphate, graphite, barium sulfate, magnesium sulfate, zinc borate, calcium borate, aluminum borate whiskers, and potassium titanate whiskers.

[0052] (Flocculant) The paper article according to the present embodiment may contain, for example, a flocculant, which allows the thermosetting resin and the reinforcing fibers to be aggregated on the flock. As the flocculant, specifically, cationic polymer flocculant, anionic polymer flocculant, nonionic polymer flocculant, amphoteric polymer flocculant, etc. can be used. Examples of such flocculants include cationic polyacrylamide, anionic polyacrylamide, Hoffman polyacrylamide, Mannick polyacrylamide, amphoteric copolymer polyacrylamide, cationic starch, amphoteric starch, polyethylene oxide, etc. These polymer flocculants may be used alone or in combination of two or more. In addition, as the polymer flocculant, the polymer structure, molecular weight, amount of functional groups such as hydroxyl groups and ionic groups, etc. can be used without any particular limitation depending on the required characteristics. In addition, examples of polymer flocculants that can be commercially obtained include polyethylene oxide manufactured by Wako Pure Chemical Industries, Ltd., Kanto Chemical Industry Co., Ltd., and Sumitomo Seika Chemicals Co., Ltd.; cationic PAM Harifix manufactured by Harima Chemicals Co., Ltd.; anionic PAM Hermide B-15; amphoteric PAM Hermide RB-300; and cationic starch SC-5 manufactured by Sanwa Starch Co., Ltd., but are not limited to these.

[0053] In addition to the above-mentioned constituent materials, the paper product of this embodiment can contain a variety of additives for the purpose of adjusting production conditions or expressing required physical properties, such as stabilizers such as antioxidants and ultraviolet absorbers for improving characteristics, release agents, plasticizers, flame retardants, resin curing catalysts and curing accelerators, pigments, paper strength improvers such as dry strength improvers and wet strength improvers, retention improvers, drainage improvers, size fixing agents, defoaming agents, sizing agents such as rosin-based sizing agents for acidic papermaking, rosin-based sizing agents for neutral papermaking, alkyl ketene dimer sizing agents, alkenyl succinic anhydride sizing agents, special modified rosin-based sizing agents, and coagulants such as aluminum sulfate, aluminum chloride, and polyaluminum chloride.

[0054] <Manufacturing method of paper product> The method for producing the paper article according to this embodiment is, for example, a wet papermaking method. The method for producing a paper article according to this embodiment includes a slurry preparation step of preparing a slurry containing a dispersion medium in which the above-mentioned thermosetting resin composition and reinforcing fibers are each independently dispersed; an aggregation step of adding a flocculant to the dispersion liquid to form an aggregate; a separation step of placing the slurry in a container having a mesh on the bottom surface and separating the dispersion medium from the aggregate; and a dehydration step of dehydrating and pressing the aggregate to produce a paper article. Each step will be described in detail below with reference to FIG.

[0055] (Slurry preparation process) In the slurry preparation step, as shown in Fig. 2(a), a slurry containing a thermosetting resin composition containing a thermosetting resin A, reinforcing fibers B, and a dispersion medium is prepared. That is, the slurry contains a dispersion medium in which the thermosetting resin and the reinforcing fibers are each independently dispersed. The slurry may further contain other components than the flocculant among the raw material components of the paper product described above. The method for preparing the slurry is not limited, but for example, a method in which the slurry is stirred in a vessel equipped with a stirrer can be mentioned.

[0056] The thermosetting resin composition is preferably in the form of granules or powder, from the viewpoint of obtaining an appropriate dispersion medium.

[0057] (dispersion medium) The dispersion medium is not limited, and specific examples thereof include water, alcohols such as ethanol, 1-propanol, 1-butanol, and ethylene glycol, ketones such as acetone, methyl ethyl ketone, 2-heptanone, and cyclohexanone, esters such as ethyl acetate, butyl acetate, methyl acetoacetate, and methyl acetoacetate, and ethers such as tetrahydrofuran, isopropyl ether, dioxane, and furfural. The dispersion medium may be one or a combination of two or more of the above specific examples.

[0058] Here, the slurry may contain, in addition to the above materials, a poly(meth)acrylic acid ester emulsion and pulp fibers.

[0059] The poly(meth)acrylic acid ester emulsion may be added after mixing and stirring the thermosetting resin A, the reinforcing fiber B, the pulp fiber if necessary, and other components if necessary in a dispersion medium, or may be mixed simultaneously with the above components. In order to disperse each component to a higher degree, the poly(meth)acrylic acid ester emulsion is preferably added after mixing and stirring the above components in a dispersion medium. Furthermore, by blending the pulp fibers, the reinforcing fibers B can be highly dispersed. Alternatively, the thermosetting resin A, the reinforcing fiber B, and the polyether oxide may be mixed in a dispersion medium to obtain a first slurry, and then the first mixed aqueous slurry may be mixed with a poly(meth)acrylic acid ester emulsion to prepare a second slurry.

[0060] (Agglutination process) In the aggregation step, an aggregating agent is added to the dispersion liquid to form aggregates. Here, the above-mentioned flocculant can be used as the flocculant. Note that, when the thermosetting resin and the reinforcing fibers are sufficiently flocculated to form an aggregate, for example, the flocculation step does not need to be performed.

[0061] (separation process) In the separation step, the slurry is placed in a container with a mesh 60 on the bottom as shown in Fig. 2(b) to separate the dispersion medium from the aggregates. As a result, a sheet-like aggregate remains on the mesh as shown in Fig. 2(c). The aggregates contain, for example, the raw material components of the slurry.

[0062] In this embodiment, the shape of the mesh 60 can be appropriately selected to adjust the shape of the resulting paper article 21. For example, when a flat sheet-shaped mesh 60 is used, a paper article 10 having a sheet-like shape is obtained. Also, when a mesh 60 having a three-dimensional shape such as a corrugated shape or unevenness is used, a paper article 21 having a three-dimensional shape is obtained. The shape of the paper article 21 can be appropriately selected according to the shape of the molded body 20 obtained by hardening and molding it, the shape of the mold, etc. Also, the thickness of the paper article 21 can be adjusted by adjusting the amount of each of the above materials in the material slurry, or by preparing a slurry again and performing the separation process.

[0063] (Dehydration process) In the dehydration step, the aggregate is dehydrated and pressed to produce a paper body. The conditions for the dehydration press are, for example, a temperature of 20°C to 30°C and a pressure of 1kgf / cm 2 More than 50kgf / cm 2 It can be as follows: Here, the dehydration press is preferably performed so that the dehydration rate of the paper product is 20% or less, for example. Note that the dehydration rate according to this embodiment refers to the mass of the dispersion medium contained in the aggregate (paper product) after the dehydration treatment, when the mass of the dispersion medium contained in the aggregate before the dehydration treatment is taken as 100%.

[0064] <Method of manufacturing molded products> Next, a method for producing the molded product will be described. The method for producing a molded product according to this embodiment includes, for example, a drying step in which the paper body is heat-treated, and a molding step in which the paper body is molded under heat and pressure into a molded product. The details are explained below.

[0065] (drying process) In the drying process, the paper body is heat treated as shown in Fig. 2(d), which further removes the dispersion medium from the paper body. The drying method is not limited, and for example, an oven 70 as shown in FIG. 2(d) can be used. Here, the drying temperature can be set to a temperature equal to or higher than the melting point of the thermosetting resin and equal to or lower than the reaction temperature. The reaction temperature is the temperature at which the calculated reaction rate exceeds 0% for the first time during the temperature rise process in differential scanning calorimetry (DSC) measurement. Here, the reaction rate is calculated as follows. First, a temperature profile is measured by DSC measurement for a paper product that has not undergone a curing reaction. The heat generation amount calculated from the temperature profile of the curing reaction obtained by this is defined as A [mJ / mg], which is converted per unit mass of the heat generation peak of the curing reaction. Next, for the paper product for which the reaction rate is to be calculated, the heat generation amount B [mJ / mg] converted per unit mass of the heat generation peak of the curing reaction is calculated in the same manner. Using the above A and B, the reaction rate is calculated from the following formula. (Formula) (Reaction rate) = B / A × 100 [%]

[0066] (molding process) In the molding step, the paper body is molded in a die under heat and pressure to produce a molded product. The molded product according to the present embodiment is obtained by molding the paper product under heat and pressure in a die. The molded product can be produced by heating and pressurizing the sheet-like or three-dimensional paper product 21 using a die having a desired shape. Examples of molding methods include press molding.

[0067] The cured state of the molded product according to this embodiment is a B-stage cured state. Here, when the heating temperature in the molding step is set to a temperature equal to or higher than the melting point and equal to or lower than the reaction temperature of the above-mentioned thermosetting resin, the molded product can be brought into a B-stage cured state.

[0068] <Method of manufacturing the cured product> The molded product according to the present embodiment may be further heat-treated at a temperature higher than the reaction temperature to become a cured product in a C-stage cured state. Here, the heat treatment at a temperature higher than the reaction temperature may be performed, for example, simultaneously with the molding step.

[0069] The glass transition temperature of the cured product is, for example, preferably 180° C. or higher, more preferably 230° C. or higher, and even more preferably 260° C. or higher, which can improve heat resistance. The glass transition temperature of the cured product may be, for example, 300° C. or lower.

[0070] [Application] The uses of the papermaking product, molding, and cured product according to the present embodiment are not limited as long as they require small anisotropy in mechanical properties such as bending strength. Specifically, the papermaking product, molding, and cured product according to the present embodiment can be suitably used as a protective member, a portable member, and the like. Specific examples of protective materials include electronic device components such as electronic device casings, transportation equipment components such as the bodies of automobiles and airplanes, and wall materials for industrial materials such as pressure vessels and buildings, which protect the contents. Protective materials are required to have properties that prevent damage such as cracks even when loads and deformations are applied from all directions. Examples of portable members include electronic device members such as the housings and internal members of portable electronic devices such as mobile phones and smartphones, and items carried by humans such as sporting goods members such as tennis rackets and golf clubs. In applications of portable members, the portable member is required to have properties that prevent damage such as cracks even if a large load or deformation is applied due to dropping the portable member or using the portable member in a way that the user did not expect from the seller. The papermaking product, molded product, and cured product according to this embodiment have small anisotropy in bending strength, and therefore can be suitably used for applications such as protective members and portable members.

[0071] The present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. Below, examples of reference forms are given. 1. A paper product obtained by using a dispersion medium in which a thermosetting resin composition and reinforcing fibers are each independently dispersed, the thermosetting resin composition comprises a thermosetting resin, The paper article has an inorganic filler finely dispersed in the thermosetting resin. 2. A paper product obtained by using a dispersion medium in which a thermosetting resin composition and reinforcing fibers are each independently dispersed, The thermosetting resin composition comprises a modified thermosetting resin. 3. The paper article according to 1 or 2, wherein the thermosetting resin comprises one or more resins selected from the group consisting of phenolic resins, epoxy resins, melamine resins, polyurethanes, and unsaturated polyester resins. 4. The papermaking product according to any one of 1. to 3., wherein the reinforcing fibers include one or more fibers selected from metal fibers, carbon fibers, glass fibers, ceramic fibers, polyamide fibers, aramid fibers, polyimide fibers, polyvinyl alcohol fibers, polyester fibers, acrylic fibers, polyparaphenylene benzoxazole fibers, polyethylene fibers, polypropylene fibers, polyacrylonitrile fibers, and ethylene vinyl alcohol fibers. 5. The paper product according to any one of 1 to 4, wherein the content of the thermosetting resin is 20% by mass or more and 80% by mass or less based on the total amount of the paper product. 6. The papermaking product according to 1, wherein the inorganic filler is one or more selected from calcium carbonate, calcium sulfate, barium sulfate, aluminum hydroxide, magnesium hydroxide, aluminum oxide (alumina), crystalline or fused silica, surface-treated silica, talc, kaolin, clay, mica, dolomite, wollastonite, glass fiber, carbon fiber, glass beads, zircon, and molybdenum compounds. 7. The papermaking product according to 1. or 6., wherein the content of the inorganic filler is 5% by mass or more and 70% by mass or less based on the total amount of the thermosetting resin composition. 8. The papermaking product according to any one of 1, 6 and 7, wherein the inorganic filler has an average particle size of 0.1 to 100 μm. 9. The paper product according to 2., wherein the modified thermosetting resin is modified with an elastomer component. 10. The papermaking product according to 9., wherein the elastomer component is one or more selected from the group consisting of polyvinyl acetal resin, acrylic rubber, acrylonitrile butadiene rubber (NBR), styrene butadiene rubber (SBR), silicone rubber, butyl rubber, urethane rubber, polybutadiene, isoprene rubber, chloroprene rubber, and copolymers thereof. 11. The papermaking product according to 10, wherein the polyvinyl acetal resin has a degree of acetalization of 50 to 80%. 12. A cured product obtained by curing the papermaking article described in any one of 1. to 11. 13. A step of kneading a thermosetting resin and an inorganic filler to obtain a thermosetting resin composition; A step of dispersing the thermosetting resin composition and reinforcing fibers in a dispersion medium, and then removing the dispersion medium by a papermaking method to obtain a paper body; A method for producing a paper article comprising the steps of: 14. A step of dispersing a thermosetting resin composition containing a modified thermosetting resin and reinforcing fibers in a dispersion medium, and then removing the dispersion medium by a papermaking method to obtain a paper body; A method for producing a paper article comprising the steps of: EXAMPLES

[0072] The present invention will be described in detail below using examples, but the present invention is not limited to the descriptions of these examples. Details of the components used in each of the Examples and Comparative Examples are given below.

[0073] [Examples 1 to 7] <Preparation of Thermosetting Resin Composition> First, raw material 1 shown below was used and mixed in a mixer according to the compounding ratio shown in Table 1. The resulting mixture was then kneaded with a biaxial roll at 80°C for 5 minutes, cooled, and pulverized to obtain a thermosetting resin composition having an average particle size of 50 μm. This resulted in a thermosetting resin composition in which inorganic filler was finely dispersed in the thermosetting resin.

[0074] (raw material 1) thermosetting resin Phenolic resin 1: Resol type phenolic resin "51723" manufactured by Sumitomo Bakelite Co., Ltd. Phenolic resin 2: Novolac type phenolic resin "A1087" manufactured by Sumitomo Bakelite Co., Ltd. Inorganic Filler Inorganic filler 1: Clay (calcined aluminum silicate) "Satenton SP-33" (average particle size 1.3 μm) manufactured by BASF Inorganic filler 2: Silica "FB-105" (average particle size 18 μm) manufactured by Denka Elastomer Component Elastomer 1: Polyvinyl alcohol (acetalization degree 66 mol%) "S-LEC BX-5" manufactured by Sekisui Chemical Co., Ltd. Elastomer 2: Polyvinyl alcohol (acetal content 74 mol%) "S-LEC KS-10" manufactured by Sekisui Chemical Co., Ltd.

[0075] <Preparation of paper-made object> The obtained thermosetting resin composition was used to prepare the following raw material 2. Note that "volume %" refers to the volume percentage relative to the total solid content (100 volume %) of the papermaking product of Example 1. (raw material 2) Thermosetting resin composition: 55% by volume of the thermosetting resin composition obtained above Reinforced fiber: PAN-based carbon fiber (Toray, T800SC, average fiber length 6 mm) 40% by volume Pulp: Aramid pulp (Teijin Ltd., Twaron (registered trademark) 1094) 5% by volume

[0076] The above-mentioned raw material 2 was added to water as a dispersion medium and stirred for 20 minutes to obtain a slurry with a solid concentration of 0.15% by weight. To the resulting slurry, a poly(meth)acrylic acid ester emulsion ("Himoc DR-9300" manufactured by Himo Corporation) prepared in advance was added so as to be 300 ppm relative to the solid content in the slurry, thereby flocculating the solid content in the slurry. The slurry containing the aggregates was then filtered through a 30-mesh metal screen, and the sheet-like aggregates remaining on the screen were pressed at a pressure of 3 MPa to dehydrate them to a dehydration rate of 20%. The dehydrated aggregates were dried at 70°C for 3 hours to obtain a sheet-like paper product in a B-stage state. The dehydration rate refers to the mass of water contained in the preform (paper product) after dehydration, when the mass of water contained in the preform (before dehydration) is taken as 100%. As a result, a paper article was obtained in which the inorganic filler was finely dispersed in the thermosetting resin.

[0077] [Reference examples 1 and 2] First, the raw materials were prepared in the proportions shown in Table 1, and a thermosetting resin composition was prepared in which the thermosetting resin and the inorganic filler were not kneaded. In other words, the inorganic filler was not finely dispersed in the thermosetting resin. Then, a papermaking body was produced in the same manner as in the above examples.

[0078] <Preparation of cured product> The obtained papermaking product was heated at 180°C and 80 MPa for 15 minutes, and then treated at 180°C for 8 hours to obtain a cured product.

[0079] The following measurements were carried out on the obtained cured product, and the results are shown in Table 1. · Flexural test: Measurement of flexural modulus (GPa) and flexural strength (MPa) The flexural modulus (GPa) and flexural strength (MPa) were measured in accordance with ISO178.

[0080] [Table 1] [Explanation of symbols]

[0081] 21 Paper model 60 mesh 70 Oven A Thermosetting resin B Fiber filler

Claims

1. A paper product in which reinforcing fibers are dispersed in a thermosetting resin composition, the thermosetting resin composition is a kneaded product containing a thermosetting resin and an inorganic filler, and a content of the inorganic filler is 5% by mass or more and 50% by mass or less with respect to a total amount of the thermosetting resin composition; The paper article has an inorganic filler finely dispersed in the thermosetting resin.

2. A paper product in which reinforcing fibers are dispersed in a thermosetting resin composition, The thermosetting resin composition is a kneaded product containing a thermosetting resin modified with an elastomer component, and the content of the elastomer component is 1% by weight or more and 40% by weight or less based on the total amount of the thermosetting resin composition.

3. 3. The paper product according to claim 1, wherein the thermosetting resin comprises one or more resins selected from the group consisting of phenolic resins, epoxy resins, melamine resins, polyurethanes, and unsaturated polyester resins.

4. 4. The papermaking product according to claim 1, wherein the reinforcing fibers include one or more selected from the group consisting of metal fibers, carbon fibers, glass fibers, ceramic fibers, polyamide fibers, aramid fibers, polyimide fibers, polyvinyl alcohol fibers, polyester fibers, acrylic fibers, polyparaphenylene benzoxazole fibers, polyethylene fibers, polypropylene fibers, polyacrylonitrile fibers, and ethylene vinyl alcohol fibers.

5. The paper product according to claim 1 , wherein the content of the thermosetting resin is 20% by mass or more and 80% by mass or less based on the total amount of the paper product.

6. 2. The papermaking product according to claim 1, wherein the inorganic filler is one or more selected from the group consisting of calcium carbonate, calcium sulfate, barium sulfate, aluminum hydroxide, magnesium hydroxide, aluminum oxide (alumina), crystalline or fused silica, surface-treated silica, talc, kaolin, clay, mica, dolomite, wollastonite, glass fiber, carbon fiber, glass beads, zircon, and molybdenum compounds.

7. The papermaking product according to claim 1 or 6, wherein the inorganic filler has an average particle size of 0.1 to 100 μm.

8. 3. The papermaking product according to claim 2, wherein the elastomer component is one or more selected from the group consisting of polyvinyl acetal resin, acrylic rubber, acrylonitrile butadiene rubber (NBR), styrene butadiene rubber (SBR), silicone rubber, butyl rubber, urethane rubber, polybutadiene, isoprene rubber, chloroprene rubber, and copolymers thereof.

9. The papermaking product according to claim 8, wherein the polyvinyl acetal resin has a degree of acetalization of 50 to 80%.

10. A cured product obtained by curing the paper article according to any one of claims 1 to 9.

11. A step of kneading a thermosetting resin and an inorganic filler to obtain a thermosetting resin composition; A step of dispersing the thermosetting resin composition and reinforcing fibers in a dispersion medium, and then removing the dispersion medium by a papermaking method to obtain a paper body; A method for producing a paper article comprising the steps of:

12. A step of kneading a thermosetting resin and an elastomer component to obtain a thermosetting resin composition containing a thermosetting resin modified by the elastomer component; A step of dispersing a thermosetting resin composition containing the modified thermosetting resin and reinforcing fibers in a dispersion medium, and then removing the dispersion medium by a papermaking method to obtain a paper body; A method for producing a paper article comprising the steps of:

13. The method for producing a paper article according to claim 11 or 12, wherein the thermosetting resin composition is in a powder form.

14. The method for producing a paperboard according to any one of claims 11 to 13, wherein the average particle size (d50) of the thermosetting resin composition is 10 to 100 µm.

Citation Information

Patent Citations

  • Modified inorganic filler

    JP1985038473A

  • gasket material

    JP1995505660A

  • Production of composite formed product

    JP1998102394A

  • Fiber-reinforced resin

    JP2008174605A

  • Modified phenol resin, method for manufacturing the same, phenol resin composition, refractory composition, resin coated sand for use in mold, molding material, nonwoven fabric, cured product, carbonized product, and activated carbon

    JP2011021093A