Radiation-curable ink-jet ink composition and ink-jet method

By using vinylmethyloxazolidinone and monomers with multiple vinyl ether groups, the ink composition achieves low viscosity and superior adhesion, addressing the challenges of existing inkjet ink compositions.

JP7559375B2Active Publication Date: 2024-10-02SEIKO EPSON CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020108575
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-24
Publication Date
2024-10-02
Estimated Expiration
2040-06-24

AI Technical Summary

Technical Problem

Existing radiation-curable inkjet ink compositions face challenges in achieving low viscosity while maintaining excellent adhesion of the cured coating film, as they often use high viscosity monomers like dipropylene glycol diacrylate, which compromises the adhesion between the coating film and the recording medium.

Method used

Incorporating vinylmethyloxazolidinone and monomers with two or more vinyl ether groups, along with specific monofunctional and polyfunctional monomers, to reduce viscosity and enhance adhesion, scratch resistance, and curability of the coating film.

Benefits of technology

The solution results in an ink composition with reduced viscosity, improved adhesion, and enhanced curability, leading to better ejection performance and coating film quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559375000006
    Figure 0007559375000006
  • Figure 0007559375000001
    Figure 0007559375000001
  • Figure 0007559375000002
    Figure 0007559375000002
Patent Text Reader

Abstract

To provide a radiation-curable inkjet ink composition that has low viscosity and is excellent in the adhesion of a coating layer, and an inkjet method.SOLUTION: A radiation-curable inkjet ink composition contains vinyl methyl oxazolidinone, and a monomer having two or more vinyl ether groups.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a radiation curable ink jet ink composition and an ink jet method. [Background technology]

[0002] Conventionally, radiation-curable inkjet ink compositions containing 2-(2-vinyloxyethoxy)ethyl acrylate or a divinyl ether-based compound as a monomer have been known. The above monomers have a lower viscosity than other radiation-curable monomers, and contribute to lowering the viscosity of the ink composition, thereby improving the ejection properties from an inkjet head. For example, Patent Document 1 discloses an active energy-curable inkjet ink composition containing 2-(2-vinyloxyethoxy)ethyl acrylate and triethylene glycol divinyl ether as a divinyl ether-based compound. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-55198 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the active energy curable inkjet ink composition described in Patent Document 1 has a problem in that it is difficult to improve the adhesion of the cured coating film while reducing the viscosity. More specifically, the viscosity is easily increased because a relatively high viscosity monomer such as dipropylene glycol diacrylate is used in combination. In addition, 2-(2-vinyloxyethoxy)ethyl acrylate and divinyl ether compounds have multiple functional groups. Therefore, it is more difficult to ensure adhesion between the coating film and the recording medium than with monofunctional monomers. In other words, there has been a demand for a radiation curable inkjet ink composition that has low viscosity and excellent adhesion of the coating film. [Means for solving the problem]

[0005] The radiation curable inkjet ink composition contains vinylmethyloxazolidinone and a monomer having two or more vinyl ether groups.

[0006] The inkjet method includes the steps of ejecting the radiation curable inkjet ink composition from an inkjet head and depositing it on a recording medium, and irradiating the radiation curable inkjet ink composition deposited on the recording medium with radiation. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a schematic perspective view illustrating a configuration of an inkjet printer according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] 1. Radiation-curable ink-jet ink composition The radiation curable inkjet ink composition according to this embodiment contains a polymerizable compound, a photopolymerization initiator, a coloring material, various additives, and the like. The radiation curable inkjet ink composition according to this embodiment can be applied to printing of signage and the like, 3D modeling, and the like, using an inkjet method described below. In the following description, the radiation curable inkjet ink composition according to this embodiment is also simply referred to as ink. Various components contained in the ink will be described below.

[0009] 1.1. Polymerizable compounds The polymerizable compound has a polymerizable functional group. In general, the polymerizable compound includes a monofunctional monomer having one functional group and a polyfunctional monomer having multiple functional groups. Each of the polymerizable compounds of the present embodiment described below may be used alone or in combination of two or more kinds.

[0010] The polymerizable compound used in this embodiment is cured by a polymerization reaction of the functional groups when irradiated with radiation. This causes the ink to form a coating film. Examples of radiation include ultraviolet light, electron beams, infrared light, visible light, and X-rays. Among these, it is preferable to use ultraviolet light as the radiation, since the material has good curability at the peak wavelength of the radiation and the radiation source is easily available.

[0011] The ink of this embodiment contains, as a polymerizable compound, vinylmethyloxazolidinone (CAS number: 3395-98-0) and a monomer having two or more vinyl ether groups. The ink may further contain, as a polymerizable compound, a monomer represented by the following formula (1) and a monofunctional (meth)acrylate monomer. Here, a monomer having two or more vinyl ether groups is also referred to as a monomer having multiple vinyl ether groups, and a monomer represented by formula (1) is also referred to as a monomer of formula (1). H 2 C=CR 1 -CO-OR 2 -O-CH=CH-R 3 (1) (In the formula, R 1 is a hydrogen atom or a methyl group, and R 2 is a divalent organic residue having 2 to 20 carbon atoms, and R 3 is a hydrogen atom or a monovalent organic residue having 1 to 11 carbon atoms.

[0012] When the functional group of the polymerizable compound is a (meth)acryloyl group, it is preferably an acryloyl group from the viewpoint of the curability of the ink. In this specification, (meth)acryloyl refers to at least one of acryloyl and the corresponding methacryloyl, (meth)acrylate refers to at least one of acrylate and the corresponding methacrylate, and (meth)acrylic refers to at least one of acrylic and the corresponding methacrylic.

[0013] 1.1.1. Vinylmethyloxazolidinone Vinylmethyloxazolidinone is a nitrogen-containing monofunctional monomer having a vinyl group as a functional group. Although vinylmethyloxazolidinone is a monofunctional monomer, it has a relatively low viscosity, and therefore contributes to reducing the viscosity of the ink. In addition, vinylmethyloxazolidinone improves the adhesion between the coating film and the recording medium and the abrasion resistance of the coating film. In addition, by using vinylmethyloxazolidinone in combination with a monofunctional (meth)acrylate monomer described later, the stretchability of the coating film is improved.

[0014] The content of vinylmethyloxazolidinone in the ink is preferably 5% by mass or more and 40% by mass or less, more preferably 10% by mass or more and 35% by mass or less, and even more preferably 15% by mass or more and 30% by mass or less, based on the total amount of the ink. By making the content equal to or more than the specified value, the viscosity of the ink can be further reduced, and the adhesion and abrasion resistance of the coating film can be further improved. By making the content equal to or less than the specified value, the storage stability of the ink can be improved.

[0015] 1.1.2.Monomers with multiple vinyl ether groups A monomer having two or more vinyl ether groups is a polyfunctional monomer having a plurality of vinyl ether groups which are functional groups. Examples of monomers having a plurality of vinyl ether groups include divinyl ether compounds such as ethylene glycol divinyl ether, butylene glycol divinyl ether, hexanediol divinyl ether, propylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, dipropylene glycol divinyl ether, tripropylene glycol divinyl ether, and 1,4-cyclohexanedimethanol divinyl ether, trivinyl ether compounds such as trimethylolethane trivinyl ether, trimethylolpropane trivinyl ether, and glycerin trivinyl ether, tetravinyl ether compounds such as ditrimethylolpropane tetravinyl ether and pentaerythritol tetravinyl ether, and dipentaerythritol pentavinyl ether. These monomers have a relatively low viscosity compared to general monofunctional monomers, and contribute to reducing the viscosity of the ink.

[0016] Of these, from the viewpoints of reducing the viscosity of the ink and of the curing properties, diethylene glycol divinyl ether and 1,4-cyclohexanedimethanol divinyl ether are preferred, and triethylene glycol divinyl ether is more preferred.

[0017] The content of the monomer having multiple vinyl ether groups in the ink is preferably 5% by mass or more and 30% by mass or less, more preferably 10% by mass or more and 25% by mass or less, and even more preferably 15% by mass or more and 20% by mass or less, based on the total amount of the ink. When the content is equal to or more than the specified value, the viscosity of the ink can be further reduced. When the content is equal to or less than the specified value, the curing property of the ink by irradiation with radiation can be improved. The improvement in the curing property of the ink contributes to an increase in the speed of formation of the coating film, and the time required for producing printed matter containing the coating film is shortened.

[0018] 1.1.3. Monomer of formula (1) The monomer of formula (1) has, as functional groups, one each of a (meth)acryloyl group and a functional group having an unsaturated double bond between carbon atoms, such as a vinyl ether group. In formula (1), R 2 Examples of the divalent organic residue having 2 to 20 carbon atoms and represented by the formula (I) include linear, branched or cyclic alkylene groups having 2 to 20 carbon atoms which may be substituted, alkylene groups having 2 to 20 carbon atoms which have at least one type of ether bond or ester bond in the structure which may be substituted, and divalent aromatic groups having 6 to 11 carbon atoms which may be substituted.

[0019] Among these, alkylene groups having 2 to 6 carbon atoms, such as an ethylene group, an n-propylene group, an isopropylene group, and a butylene group, and alkylene groups having 2 to 9 carbon atoms and an oxygen atom due to an ether bond in the structure, such as an oxyethylene group, an oxy-n-propylene group, an oxyisopropylene group, and an oxybutylene group, are preferred. Furthermore, from the viewpoint of reducing the viscosity of the ink and improving the curing property of the ink, R 2 More preferred are those having a glycol ether chain, which is an alkylene group having 2 to 9 carbon atoms and having an oxygen atom by an ether bond in the structure, such as an oxyethylene group, an oxy-n-propylene group, an oxyisopropylene group, and an oxybutylene group.

[0020] In formula (1), R 3 Examples of the monovalent organic residue having 1 to 11 carbon atoms and represented by the formula (I) include a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms which may be substituted, and an aromatic group having 6 to 11 carbon atoms which may be substituted. Among these, an alkyl group having 1 to 2 carbon atoms, such as a methyl group or an ethyl group, and an aromatic group having 6 to 8 carbon atoms, such as a phenyl group or a benzyl group, are preferred.

[0021] When each of the above organic residues is a group that may be substituted, the substituent is divided into a group that contains carbon atom and a group that does not contain carbon atom.When the above substituent is a group that contains carbon atom, the carbon atom is counted in the number of carbon atoms of the organic residue.The group that contains carbon atom is not particularly limited, but for example, carboxyl group and alkoxy group are included.The group that does not contain carbon atom is not particularly limited, but for example, hydroxyl group and halo group are included.

[0022] Specific examples of the monomer of formula (1) include 2-vinyloxyethyl (meth)acrylate, 3-vinyloxypropyl (meth)acrylate, 1-methyl-2-vinyloxyethyl (meth)acrylate, 2-vinyloxypropyl (meth)acrylate, 4-vinyloxybutyl (meth)acrylate, 1-methyl-3-vinyloxypropyl (meth)acrylate, 1-vinyloxymethylpropyl (meth)acrylate, 2-methyl-3-vinyloxypropyl (meth)acrylate, 1,1-dimethyl-2-vinyloxyethyl (meth)acrylate, and (meth)acrylic acid. 3-vinyloxybutyl, 1-methyl-2-vinyloxypropyl (meth)acrylate, 2-vinyloxybutyl (meth)acrylate, 4-vinyloxycyclohexyl (meth)acrylate, 6-vinyloxyhexyl (meth)acrylate, 4-vinyloxymethylcyclohexylmethyl (meth)acrylate, 3-vinyloxymethylcyclohexylmethyl (meth)acrylate, 2-vinyloxymethylcyclohexylmethyl (meth)acrylate, p-vinyloxymethylphenylmethyl (meth)acrylate, m-vinyloxymethylphenylmethyl (meth)acrylate, o-vinyloxymethylphenylmethyl (meth)acrylate, 2-(2-vinyloxyethoxy)ethyl (meth)acrylate, 2-(2-vinyloxyethoxy)ethyl acrylate, 2-(vinyloxyisopropoxy)ethyl (meth)acrylate, 2-(vinyloxyethoxy)propyl (meth)acrylate, 2-(vinyloxyethoxy)isopropyl (meth)acrylate, 2-(vinyloxyisopropoxy)propyl (meth)acrylate, 2-(vinyloxyisopropoxy)isopropyl (meth)acrylate, 2-(vinyloxyisopropoxy)isopropyl (meth)acrylate, 2-(vinyloxyethoxy)acrylic acid ethoxy)ethyl, (meth)acrylic acid 2-(vinyloxyethoxyisopropoxy)ethyl, (meth)acrylic acid 2-(vinyloxyisopropoxyethoxy)ethyl, (meth)acrylic acid 2-(vinyloxyisopropoxyisopropoxy)ethyl, (meth)acrylic acid 2-(vinyloxyethoxyethoxy)propyl, (meth)acrylic acid 2-(vinyloxyethoxyisopropoxy)propyl, (meth)acrylic acid 2-(vinyloxyisopropoxyethoxy)propyl, (meth)acrylic acid 2-(vinyloxyisopropoxyisopropoxy)propyl, (meth)acrylic acid 2-(vinyloxyisopropoxyisopropoxy)propyl,2-(vinyloxyethoxyethoxy)isopropyl (meth)acrylate, 2-(vinyloxyethoxyisopropoxy)isopropyl (meth)acrylate, 2-(vinyloxyisopropoxyethoxy)isopropyl (meth)acrylate, 2-(vinyloxyisopropoxyisopropoxy)isopropyl (meth)acrylate, 2-(vinyloxyethoxyethoxyethoxy)ethyl (meth)acrylate, 2-(vinyloxyethoxyethoxyethoxy)ethyl (meth)acrylate Examples of suitable acrylates include 2-(isopropenoxyethoxy)ethyl (meth)acrylate, 2-(isopropenoxyethoxyethoxy)ethyl (meth)acrylate, 2-(isopropenoxyethoxyethoxy)ethyl (meth)acrylate, 2-(isopropenoxyethoxyethoxyethoxy)ethyl (meth)acrylate, 2-(isopropenoxyethoxyethoxyethoxy)ethyl (meth)acrylate, polyethylene glycol monovinyl ether (meth)acrylate, and polypropylene glycol monovinyl ether (meth)acrylate. Of these specific examples, 2-(2-vinyloxyethoxy)ethyl acrylate is particularly preferred because of the ease of achieving a balance between the curability and viscosity of the ink.

[0023] The monomer of formula (1) has a relatively low viscosity compared to general monofunctional monomers, which contributes to reducing the viscosity of the ink. It also has excellent curability when exposed to radiation. As a result, it is possible to further reduce the viscosity of the ink and improve the curability when forming a coating film.

[0024] The content of the monomer of formula (1) in the ink is preferably 10% by mass or more and 50% by mass or less, more preferably 20% by mass or more and 45% by mass or less, and even more preferably 30% by mass or more and 40% by mass or less, based on the total amount of the ink. When the content is equal to or more than the specified value, the viscosity of the ink is further reduced and the curing property of the ink by irradiation with radiation can be further improved. When the content is equal to or less than the specified value, the odor of the ink is reduced and the adhesion between the coating film and the recording medium is improved.

[0025] 1.1.4. Monofunctional (meth)acrylate monomers The monofunctional (meth)acrylate monomer has one (meth)acryloyl group as a functional group. By using the monofunctional (meth)acrylate monomer in the ink, the crosslink density in the coating film can be suppressed, and the extensibility of the coating film can be improved.

[0026] Examples of the monofunctional (meth)acrylate monomer include a monofunctional (meth)acrylate monomer having an aromatic group, a monofunctional (meth)acrylate monomer having an alicyclic structure, a monofunctional (meth)acrylate monomer having a cyclic ether structure, and a monofunctional (meth)acrylate monomer having a crosslinked condensed ring structure.

[0027] Of these, the ink preferably contains a monofunctional (meth)acrylate monomer having an aromatic group as the monofunctional (meth)acrylate monomer. The monofunctional (meth)acrylate monomer having an aromatic group has excellent solubility for a photopolymerization initiator having an aromatic group, such as an acylphosphine oxide-based photopolymerization initiator. Therefore, the ink can be cured by irradiation with radiation by using the above-mentioned photopolymerization initiator in combination.

[0028] Examples of monofunctional (meth)acrylate monomers having an aromatic group include phenoxyethyl (meth)acrylate, benzyl (meth)acrylate, alkoxylated 2-phenoxyethyl (meth)acrylate, ethoxylated nonylphenyl (meth)acrylate, alkoxylated nonylphenyl (meth)acrylate, p-cumylphenol EO-modified (meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate.

[0029] Among these, from the viewpoint of the solubility of the photopolymerization initiator described above, benzyl (meth)acrylate or phenoxyethyl (meth)acrylate is preferred, phenoxyethyl (meth)acrylate is more preferred, and phenoxyethyl acrylate (2-phenoxyethyl acrylate) is even more preferred.

[0030] The content of the monofunctional (meth)acrylate monomer having an aromatic group in the ink is preferably 5% by mass or more and 40% by mass or less, more preferably 10% by mass or more and 35% by mass or less, and even more preferably 15% by mass or more and 30% by mass or less, based on the total amount of the ink. This further improves the solubility of the photopolymerization initiator having an aromatic group. In addition, the extensibility of the coating film is improved, and the curability of the ink, the adhesion of the coating film, and the abrasion resistance are also improved.

[0031] Examples of monofunctional (meth)acrylate monomers having an alicyclic structure include isobornyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, 2-(meth)acrylic acid-1,4-dioxaspiro[4,5]dec-2-ylmethyl, dicyclopentanyl acrylate, and 3,3,5-trimethylcyclohexyl acrylate.

[0032] Among these, isobornyl acrylate and 3,3,5-trimethylcyclohexyl acrylate are preferred from the viewpoints of the curability of the ink and the abrasion resistance of the coating film.

[0033] Examples of monofunctional (meth)acrylate monomers having a cyclic ether structure include cyclic trimethylolpropane formal acrylate, tetrahydrofurfuryl acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl acrylate, etc. By using these monomers in combination with vinylmethyloxazolidinone in the ink, the odor of the ink is reduced, and the adhesion and abrasion resistance of the coating film are improved.

[0034] The bridged condensed ring structure in the monofunctional (meth)acrylate monomer having a bridged condensed ring structure refers to a structure in which two or more ring structures share a side in a one-to-one relationship, and two or more atoms of the same ring structure or different ring structures that are not adjacent to each other are linked. Examples of the monofunctional (meth)acrylate monomer having a bridged condensed ring structure include dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, and dicyclopentanyl (meth)acrylate. In addition, monofunctional (meth)acrylates having bridged condensed ring structures of the following formulae (a) and (b) may be used. By using these monofunctional (meth)acrylate monomers having a bridged condensed ring structure in combination with vinylmethyloxazolidinone, the abrasion resistance and stretchability of the coating film are improved, and the adhesion to a recording medium is further improved.

[0035] [ka]

[0036] [ka]

[0037] When a monofunctional (meth)acrylate monomer having an alicyclic structure, a cyclic ether structure, or a crosslinked condensed ring structure is used, the content of the monomer is preferably 5% by mass to 40% by mass, more preferably 10% by mass to 35% by mass, and even more preferably 15% by mass to 30% by mass, relative to the total amount of the ink. This improves the extensibility of the coating film, as well as the curing property of the ink, and the adhesion and abrasion resistance of the coating film.

[0038] The above monofunctional (meth)acrylate monomers may be used alone or in combination of two or more kinds.

[0039] Other monofunctional (meth)acrylate monomers include, for example, 2-ethylhexyl acrylate, isoamyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, isomyristyl (meth)acrylate, isostearyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, butoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, and other (meth)acrylates having an aliphatic group containing a straight or branched chain, and lactone-modified flexible (meth)acrylates.

[0040] 1.1.5. Other polymerizable compounds The ink may contain other polymerizable compounds in addition to the above-mentioned polymerizable compounds, such as monofunctional monomers, polyfunctional monomers, and oligomers as listed below. The functional group of the other polymerizable compounds is not particularly limited as long as it is capable of undergoing a polymerization reaction by radiation, and any known polymerizable functional group can be used.

[0041] Examples of monofunctional monomers include nitrogen-containing monofunctional vinyl monomers such as N-vinylcaprolactam, N-vinylformamide, N-vinylcarbazole, N-vinylacetamide, and N-vinylpyrrolidone, nitrogen-containing monofunctional acrylate monomers such as acryloylmorpholine, nitrogen-containing monofunctional acrylamide monomers such as (meth)acrylamide, N-hydroxymethyl(meth)acrylamide, diacetoneacrylamide, N,N-dimethyl(meth)acrylamide, and dimethylaminoethyl acrylate benzyl chloride quaternary salt, unsaturated carboxylic acids such as (meth)acrylic acid, itaconic acid, crotonic acid, isocrotonic acid, and maleic acid, salts of the unsaturated carboxylic acid, esters of unsaturated carboxylic acids, urethanes, amides, and anhydrides, acrylonitrile, styrene, various unsaturated polyesters, unsaturated polyethers, unsaturated polyamides, and unsaturated urethanes. Although vinylmethyloxazolidinone is a category of nitrogen-containing monofunctional vinyl monomers, it is not included in this specification.

[0042] Examples of polyfunctional monomers include dipropylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, dipropylene glycol dimethacrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, propoxylated (2) neopentyl glycol di(meth)acrylate, dimethylol-tricyclodecane di(meth)acrylate, EO (ethylene oxide) adduct di(meth)acrylate of bisphenol A, PO( Examples of the polyfunctional (meth)acrylate include bifunctional (meth)acrylates such as propylene oxide) adduct di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, and polytetramethylene glycol di(meth)acrylate, and polyfunctional (meth)acrylates having three or more functional groups such as trimethylolpropane tri(meth)acrylate, EO-modified trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, glycerin propoxy tri(meth)acrylate, caprolactone-modified trimethylolpropane tri(meth)acrylate, pentaerythritol ethoxy tetra(meth)acrylate, and caprolactam-modified dipentaerythritol hexa(meth)acrylate. Among these polyfunctional monomers, tripropylene glycol diacrylate and propoxylated (2) neopentyl glycol diacrylate are preferred.

[0043] When a polyfunctional monomer is added to the ink, the content of the polyfunctional monomer is preferably from 2% by mass to 20% by mass, more preferably from 2% by mass to 15% by mass, and even more preferably from 2% by mass to 10% by mass, relative to the total amount of the ink. This improves the curability of the ink.

[0044] An oligomer is a polymer that is a component of a polymerizable compound and has one or more functional groups. The polymerizable compound is not limited to the above-mentioned polymerizable compounds. In this specification, a polymerizable compound having a molecular weight of 1000 or less is referred to as a monomer, and a polymerizable compound having a molecular weight of more than 1000 is referred to as an oligomer.

[0045] Examples of the oligomer include urethane acrylate oligomers in which the repeating unit is a urethane, polyester acrylate oligomers in which the repeating unit is an ester, and epoxy acrylate oligomers in which the repeating unit is derived from a polymerizable compound having an epoxy group.

[0046] Among these, urethane acrylate oligomers are preferred. Of the urethane acrylate oligomers, aromatic urethane acrylate oligomers are preferred, and aliphatic urethane acrylate oligomers are more preferred. The number of functional groups possessed by the urethane acrylate oligomer is preferably 4 or less, and more preferably 2 or less. This prevents the increase in the viscosity of the ink, and improves the curability of the ink and the adhesion of the coating film.

[0047] When an oligomer is added to the ink, the content of the oligomer is preferably from 1 to 15% by mass, more preferably from 1 to 10% by mass, and even more preferably from 2 to 7% by mass, relative to the total amount of the ink. This further suppresses an increase in the viscosity of the ink, and further improves the curability of the ink and the adhesion of the coating.

[0048] 1.2. Photopolymerization initiator The photopolymerization initiator generates active species upon irradiation with radiation, and has the function of promoting the polymerization reaction of the polymerizable compound by the active species. Specifically, the active species generated from the photopolymerization initiator include radicals, acids, bases, etc.

[0049] The photopolymerization initiator is not particularly limited as long as it has the above-mentioned function, and examples thereof include known photopolymerization initiators such as acylphosphine oxide-based photopolymerization initiators, alkylphenone-based photopolymerization initiators, titanocene-based photopolymerization initiators, and thioxanthone-based photopolymerization initiators. Among these, thioxanthone-based photopolymerization initiators are preferred, and acylphosphine oxide-based photopolymerization initiators are more preferred. This improves the curability of the ink, particularly the curability in a curing process that employs UV-LED (ultraviolet light-emitting diode) light. The photopolymerization initiator may be used alone or in combination of two or more types.

[0050] Examples of the acylphosphine oxide photopolymerization initiator include 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide.

[0051] Commercially available products may be used as the acylphosphine oxide photopolymerization initiator. Examples of the commercially available products include Omnirad® 819 (bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide) from IGM RESINS BV, Omnirad 1800 (a mixture of bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide and 1-hydroxy-cyclohexyl-phenyl ketone in a mass ratio of 25:75), Omnirad TPO (2,4,6-trimethylbenzoyldiphenylphosphine oxide), and Speedcure® TPO (2,4,6-trimethylbenzoyldiphenylphosphine oxide) from Lambson Group Ltd.

[0052] The content of the acylphosphine oxide photopolymerization initiator in the ink is preferably 3% by mass or more and 15% by mass or less, more preferably 5% by mass or more and 12% by mass or less, and even more preferably 7% by mass or more and 10% by mass or less, based on the total amount of the ink. This improves the curability of the ink and ensures the solubility of the photopolymerization initiator.

[0053] Examples of the thioxanthone-based photopolymerization initiator include thioxanthone, 2-methylthioxanthone, 2,4-diethylthioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, and 2-chlorothioxanthone.

[0054] As the thioxanthone-based photopolymerization initiator, a commercially available product may be used, such as Speedcure (registered trademark) DETX (2,4-diethylthioxanthone) from Lambson Group Ltd.

[0055] When a thioxanthone-based photopolymerization initiator is used in the ink, the content thereof is preferably from 0.5% to 10% by mass, more preferably from 1% to 3% by mass, relative to the total amount of the ink, which improves the curability of the ink.

[0056] 1.3.Colorants The coloring material colors the coating film formed from the ink. By coloring the coating film of the ink, it becomes possible to color the recording medium and form a color image on the recording medium. A pigment or a dye is used as the coloring material. The ink of the present invention is not limited to containing a coloring material, and may be a clear ink that does not contain a coloring material.

[0057] Pigments The pigment improves the light resistance of the coloring material in the ink coating, and both inorganic and organic pigments can be used as the pigment.

[0058] As the pigment, any of known organic pigments and inorganic pigments can be used. As the organic pigment, for example, azo pigments such as azo lake pigments, insoluble azo pigments, condensed azo pigments, and chelate azo pigments, phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, thioindigo pigments, isoindolinone pigments, isoindoline pigments, quinophthalone pigments, and polycyclic pigments such as diketopyrrolopyrrole pigments, dye lake pigments such as basic dye lakes and acid dye lakes, nitro pigments, nitroso pigments, aniline black, and daylight fluorescent pigments can be used. As the inorganic pigment, for example, metal oxide pigments such as titanium dioxide, zinc oxide, and chromium oxide, and carbon black can be used. In addition, luster pigments such as pearl pigments and metallic pigments can be used.

[0059] Examples of black pigments include CI (Colour Index Generic Name) Pigment Black 1, 7, and 11. Among these, it is preferable to use carbon black, which is CI Pigment Black 7.

[0060] Specific examples of carbon black include Mitsubishi Chemical's No. 2300, No. 900, MCF88, No. 33, No. 40, No. 45, No. 52, MA7, MA8, MA100, and No. 2200B; Columbia Carbon's Raven (registered trademark) 5750, 5250, 5000, 3500, 1255, and 700; CABOT's Rega1 (registered trademark) 400R, 330R, and 660R, Mogul (registered trademark) L, and Monarch (registered trademark) 700, 800, 880, 900, 1000, 1100, 1300, and 1400; and Degussa's Color Black FW1, FW2, FW2V, FW18, FW200, S150, S160, and S170, Printex (registered trademark) 35, U, V, and 140U, and Special Black. 6, 5, 4A, and 4 are examples.

[0061] Examples of white pigments include CI Pigment White 6, 18, and 21.

[0062] Examples of yellow pigments include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 16, 17, 24, 34, 35, 37, 53, 55, 65, 73, 74, 75, 81, 83, 93, 94, 95, 97, 98, 99, 108, 109, 110, 113, 114, 117, 120, 124, 128, 129, 133, 138, 139, 147, 151, 153, 154, 155, 167, 172, and 180.

[0063] Examples of magenta pigments include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 40, 41, 42, 48(Ca), 48(Mn), 57(Ca), 57:1, 88, 112, 114, 122, 123, 144, 146, 149, 150, 166, 168, 170, 171, 175, 176, 177, 178, 179, 184, 185, 187, 202, 209, 219, 224, 245, and CI Pigment Violet. 19, 23, 32, 33, 36, 38, 43, and 50 are listed.

[0064] Examples of cyan pigments include CI Pigment Blue 1, 2, 3, 15, 15:1, 15:2, 15:3, 15:34, 15:4, 16, 18, 22, 25, 60, 65, and 66, and CI Vat Blue 4 and 60.

[0065] Examples of pigments for colors other than those mentioned above include CI Pigment Green 7 and 10, CI Pigment Brown 3, 5, 25 and 26, and CI Pigment Orange 1, 2, 5, 7, 13, 14, 15, 16, 24, 34, 36, 38, 40, 43 and 63.

[0066] One type of pigment may be used alone, or two or more types may be used in combination. When a pigment is used, a dispersant, which will be described later, may be used in combination. The average particle size of the pigment is preferably 300 nm or less, and more preferably 50 nm or more and 200 nm or less. When the average particle size of the pigment is within the above range, the ink ejection property and dispersion stability are improved, and the image quality of the coating film is excellent. The average particle size here refers to the volume-based particle size distribution (50%) measured by dynamic light scattering.

[0067] When a pigment is added to the ink, the content thereof is from 0.2% by mass to 20.0% by mass, preferably from 1.0% by mass to 20.0% by mass, more preferably from 1.0% by mass to 15.0% by mass, and even more preferably from 1.0% by mass to 10.0% by mass, relative to the total amount of the ink.

[0068] 1.3.2.Dye As the dye, known acid dyes, direct dyes, reactive dyes, and basic dyes can be used. One type of dye may be used alone, or two or more types may be used in combination.

[0069] Examples of dyes include CI Acid Yellow 17, 23, 42, 44, 79, 142, CI Acid Red 52, 80, 82, 249, 254, 289, CI Acid Blue 9, 45, 249, CI Acid Black 1, 2, 24, 94, CI Food Black 1, 2, CI Direct Yellow 1, 12, 24, 33, 50, 55, 58, 86, 132, 142, 144, 173, CI Direct Red 1, 4, 9, 80, 81, 225, 227, CI Direct Blue 1, 2, 15, 71, 86, 87, 98, 165, 199, 202, CI Direct Black 19, 38, 51, 71, 154, 168, 171, 195, and CI Reactive Red. 14, 32, 55, 79, 249, and CI Reactive Black 3, 4, and 35.

[0070] When a dye is added to the ink, the content thereof is from 0.2% by mass to 20.0% by mass, preferably from 1.0% by mass to 20.0% by mass, more preferably from 1.0% by mass to 15.0% by mass, and even more preferably from 1.0% by mass to 10.0% by mass, relative to the total amount of the ink.

[0071] 1.4 Additives The ink preferably contains a fluorescent whitening agent as an additive, and may contain other additives such as a dispersant, a polymerization inhibitor, a surfactant, and a photosensitizer, as necessary.

[0072] 1.4.1.Fluorescent whitening agents For example, the fluorescent brightening agent absorbs light with a wavelength of about 300 nm to 450 nm and emits fluorescence with a wavelength of about 400 nm to 500 nm. That is, when ultraviolet light is used as radiation, the fluorescent brightening agent increases the long wavelength region of the ultraviolet light irradiated to the ink, thereby improving the curing property.

[0073] Examples of fluorescent brightening agents include naphthalene benzoxazolyl derivatives, thiophene benzoxazolyl derivatives, stilbene benzoxazolyl derivatives, coumarin derivatives, styrene biphenyl derivatives, pyrazolone derivatives, stilbene derivatives, styryl derivatives of benzene and biphenyl, bis(benzazol-2-yl) derivatives, carbostyryl, naphthalimide, derivatives of dibenzothiophene-5,5'-dioxide, pyrene derivatives, and pyridotriazole. One or more types of fluorescent brightening agents may be used alone, or two or more types may be used in combination.

[0074] The fluorescent whitening agent may be a commercially available product, such as TELALUX (registered trademark) OB (2,5-bis(5-tert-butyl-2-benzoxazolyl)thiophene) and KCB (1,4-bis(2-benzoxazolyl)naphthalene) from Clariant Japan.

[0075] The content of the fluorescent whitening agent in the ink is preferably from 0.07% to 0.70% by mass, more preferably from 0.10% to 0.50% by mass, relative to the total amount of the ink, which improves the curing properties of the ink.

[0076] 1.4.2. Other Additives The dispersant provides dispersibility to the pigment in the ink. By using the dispersant, the pigment is stably dispersed in the ink, and the ink has improved resistance to settling during storage and ejection stability from an inkjet head.

[0077] The dispersant may be, for example, a known dispersant commonly used in the preparation of a pigment dispersion, such as a polymer dispersant.Specific examples of the dispersant include polyoxyalkylene polyalkylene polyamines, vinyl polymers and copolymers, acrylic polymers and copolymers, polyesters, polyamides, polyimides, polyurethanes, amino polymers, silicon-containing polymers, sulfur-containing polymers, fluorine-containing polymers, and epoxy resins.The dispersant may be used alone or in combination of two or more.

[0078] As the polymer dispersant, commercially available products may be used, and examples thereof include the Ajisper (registered trademark) series from Ajinomoto Fine-Techno Co., Ltd., the Solsperse (registered trademark) series such as Solsperse 36000 from Lubrizol Corporation, the Disperbyk series from BYK Additives & Instruments, and the Disparlon (registered trademark) series from Kusumoto Chemicals Co., Ltd.

[0079] The content of the dispersant in the ink is preferably from 0.05% to 1.00% by mass, more preferably from 0.10% to 0.50% by mass, relative to the total amount of the ink, which further improves the storage stability and ejection stability of the ink.

[0080] The polymerization inhibitor improves the storage stability of the ink by suppressing the progress of unintended polymerization reactions of the polymerizable compound during storage, etc. One type of polymerization inhibitor may be used alone, or two or more types may be used in combination.

[0081] The polymerization inhibitor is not particularly limited, but examples thereof include 4-methoxyphenol (hydroquinone monomethyl ether), 4-hydroxy-2,2,6,6-tetramethylpiperidine-N-oxyl, hydroquinone, cresol, t-butylcatechol, 3,5-di-t-butyl-4-hydroxytoluene, 2,2'-methylenebis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-butylphenol), and 4,4'-thiobis(3-methyl-6-t-butylphenol), hindered amine compounds, 2,2,6,6-tetramethylpiperidinyl-1-oxyl, and derivatives of 2,2,6,6-tetramethylpiperidinyl-1-oxyl.

[0082] Among the above polymerization inhibitors, 2,2,6,6-tetramethylpiperidinyl-1-oxyl or its derivatives are preferred. The derivatives of 2,2,6,6-tetramethylpiperidinyl-1-oxyl are not particularly limited, but include, for example, 4-acetamido-2,2,6,6-tetramethylpiperidinyl-1-oxyl, 4-amino-2,2,6,6-tetramethylpiperidinyl-1-oxyl, 4-carboxy-2,2,6,6-tetramethylpiperidinyl-1-oxyl, 4-(2-chloroacetamido)-2,2,6,6-tetramethylpiperidinyl-1-oxyl, 4-cyano-2,2,6,6-tetramethylpiperidinyl-1-oxyl, 4-hydroxy ... Benzoate-2,2,6,6-tetramethylpiperidinyl-1-oxyl, 4-(2-iodoacetamido)-2,2,6,6-tetramethylpiperidinyl-1-oxyl, 4-isothiocyanate-2,2,6,6-tetramethylpiperidinyl-1-oxyl, 4-methacryloyloxy-2,2,6,6-tetramethylpiperidinyl-1-oxyl, 4-methoxy-2,2,6,6-tetramethylpiperidinyl-1-oxyl, 4-oxo-2,2,6,6-tetramethylpiperidinyl-1-oxyl, 4-(2-propynyloxy)-2,2,6,6-tetramethylpiperidinyl-1-oxyl are listed. Among these, 4-hydroxy-2,2,6,6-tetramethylpiperidinyl-1-oxyl is more preferred. By using these, the storage stability of the ink is further improved.

[0083] When a polymerization inhibitor is added to the ink, the content thereof is preferably from 0.05% by mass to 1.00% by mass, and more preferably from 0.05% by mass to 0.50% by mass, relative to the total amount of the ink.

[0084] The surfactant improves the abrasion resistance of the coating film. Examples of the surfactant include acetylene glycol surfactants, fluorine surfactants, and silicone surfactants. Among these, silicone surfactants are preferred, and polyester-modified silicone or polyether-modified silicone is more preferred. As such surfactants, commercially available products can be used, and examples include polyester-modified silicones such as BYK (registered trademark)-347, -348, BYK-UV3500, -3510, and -3530, and polyether-modified silicones such as BYK-3570, all of which are manufactured by BYK Additives & Instruments. These may be used alone or in combination of two or more types.

[0085] When a surfactant is added to the ink, the content thereof is preferably from 0.1% by mass to 1.0% by mass, and more preferably from 0.2% by mass to 0.8% by mass, relative to the total amount of the ink.

[0086] The photosensitizer absorbs radiation and becomes excited, promoting the generation of active species from the photopolymerization initiator. Examples of photosensitizers include aliphatic amines, amines containing aromatic groups, piperidine, reaction products of epoxy resins and amines, and amine compounds such as triethanolamine triacrylate, urea compounds such as allylthiourea and o-tolylthiourea, sulfur compounds such as sodium diethyldithiophosphate and soluble salts of aromatic sulfinic acids, nitrile compounds such as N,N-diethyl-p-aminobenzonitrile, phosphorus compounds such as tri-n-butylphosphine and sodium diethyldithiophosphide, nitrogen compounds such as Michler's ketone, N-nitrisohydroxylamine derivatives, oxazolidine compounds, tetrahydro-1,3-oxazine compounds, condensates of formaldehyde or acetaldehyde with diamines, and chlorine compounds such as carbon tetrachloride and hexachloroethane. These may be used alone or in combination of two or more.

[0087] When a photosensitizer is added to the ink, the content is preferably 0.5% by mass or more and 3.0% by mass or less with respect to the total amount of the ink.

[0088] 2. Ink preparation method In preparing the ink, the above-mentioned components are mixed and thoroughly stirred so that the components are uniformly mixed. In the ink preparation process, the mixture of the photopolymerization initiator and at least a part of the polymerizable compound may be subjected to at least one of ultrasonic treatment and heating treatment. This reduces the amount of dissolved oxygen in the prepared ink, improving the ejection stability and storage stability of the ink.

[0089] 3. Ink properties The viscosity of the ink at 25°C is preferably 30 mPa·s (millipascal seconds) or less, more preferably 25 mPa·s or less, even more preferably 20 mPa·s or less, and particularly preferably 15 mPa·s or less. This improves the ejection properties of the ink from the inkjet head, and prevents the ink droplets from deflecting or scattering. The ink viscosity is measured using Anton Paar's rheometer MCR-301, a viscoelasticity measuring device, at a set ink temperature of 25°C, by increasing the shear rate from 10 to 1000 and reading the viscosity at a shear rate of 200.

[0090] The surface tension of the ink at 20°C is preferably 20 mN / m or more and 40 mN / m or less. This makes it difficult for the ink to wet the nozzle surface of the inkjet head that has been treated to be liquid repellent. This allows the ink to be ejected normally and in an appropriate amount from the inkjet head, preventing the ink droplets from deflecting or scattering. The surface tension of the ink is measured by checking the surface tension when a platinum plate is wetted with the ink in an environment of 20°C using an automatic surface tensiometer CBVP-Z manufactured by Kyowa Interface Science Co., Ltd.

[0091] 4. Inkjet device An inkjet device used in the inkjet method of the present embodiment, which will be described later, will be described with reference to Fig. 1, taking as an example a serial type inkjet printer. In Fig. 1, the scale of each component is different from the actual scale so that each component is large enough to be recognizable.

[0092] The inkjet printer 1 according to this embodiment is what is known as a serial type printer. A serial printer is a printer in which an inkjet head is mounted on a carriage that moves in a specific direction, and printing is performed while the inkjet head moves in conjunction with the movement of the carriage. Hereinafter, the inkjet printer 1 will also be referred to simply as the printer 1.

[0093] 1, the printer 1 has an inkjet head 3, a carriage 4, a main scanning mechanism 5, a platen roller 6, a light source 11, and a control unit (not shown) that controls the overall operation of the printer 1. The carriage 4 mounts the inkjet head 3 and the light source 11, and is capable of detachably mounting ink cartridges 7a, 7b, 7c, 7d, and 7e as containers that contain ink to be supplied to the inkjet head 3.

[0094] The main scanning mechanism 5 has a timing belt 8 connected to the carriage 4, a motor 9 that drives the timing belt 8, and a guide shaft 10. The guide shaft 10, as a support member for the carriage 4, is installed in the main scanning direction, which is the scanning direction of the carriage 4. The carriage 4 is driven by the motor 9 via the timing belt 8, and is capable of reciprocating along the guide shaft 10. In this way, the main scanning mechanism 5 moves the carriage 4 back and forth in the main scanning direction.

[0095] The platen roller 6 transports the recording medium 2, to which the ink is to be applied, in a sub-scanning direction perpendicular to the main scanning direction. Therefore, the recording medium 2 is transported in the sub-scanning direction, which is approximately the same as the length direction of the recording medium 2. The carriage 4 is capable of reciprocating in the main scanning direction, which is approximately the same as the width direction of the recording medium 2. Therefore, the inkjet head 3 and the light source 11 are capable of scanning relatively to the recording medium 2 in the main scanning direction and the sub-scanning direction.

[0096] The ink cartridges 7a, 7b, 7c, 7d, and 7e are five independent ink cartridges. The ink cartridges 7a, 7b, 7c, 7d, and 7e contain color inks that contain coloring materials and clear inks that do not contain coloring materials.

[0097] For example, color inks such as black, cyan, magenta, and yellow, and clear ink can be separately stored in the ink cartridges 7a, 7b, 7c, 7d, and 7e and used as an ink set. In FIG. 1, the number of ink cartridges is five, but this is not limited to this. Also, the ink cartridge for clear ink may be omitted, and an ink cartridge for another color ink such as white ink may be provided.

[0098] A supply port (not shown) for supplying the accommodated ink to the inkjet head 3 is provided at the bottom of each of the ink cartridges 7a, 7b, 7c, 7d, and 7e.

[0099] The components of the ink cartridges 7a to 7e are made of materials that are resistant to evaporation and deterioration of the ink components, deterioration of the components due to the ink components, etc. In this embodiment, an ink cartridge is exemplified as the ink container, but the ink container is not limited to this, and other than the ink cartridge, an ink pack, an ink bottle, etc. may be used as the ink container.

[0100] An inkjet head 3 and a light source 11 are disposed on the side of the carriage 4 facing the recording medium 2. The inkjet head 3 has a nozzle surface (not shown) on the surface facing the recording medium 2. A polymer film containing a fluorine compound and a silicone compound, or a co-deposition plating film containing nickel and a fluorine compound may be formed as a liquid-repellent film on the nozzle surface. Although not shown, a nozzle row consisting of a plurality of ejection nozzles is disposed on the nozzle surface individually corresponding to each ink. Each ink is supplied to the inkjet head 3 from the ink cartridges 7a, 7b, 7c, 7d, and 7e, respectively, and ejected as droplets from the ejection nozzles by an actuator (not shown) in the inkjet head 3. The ejected ink droplets land on and adhere to the recording medium 2.

[0101] In the inkjet head 3, a piezoelectric element is used as an actuator, which is a driving means, but is not limited to this. For example, an electromechanical conversion element that displaces a vibration plate as an actuator by electrostatic adsorption, or an electrothermal conversion element that ejects ink as droplets by bubbles generated by heating may be used as the driving means.

[0102] The light source 11 is arranged alongside the inkjet head 3 in the main scanning direction. The light source 11 is a radiation emitting device, and includes a light emitting element (not shown), such as a UV-LED. The radiation emitted from the light source 11 is not limited to ultraviolet light, and may be infrared light, an electron beam, visible light, X-rays, or the like. Here, a lamp or the like may be used as the light source 11 instead of a light emitting element such as an LED (light emitting diode) or an LD (semiconductor laser), but it is preferable to use a light emitting element from the viewpoint of miniaturization, cost reduction, and the like.

[0103] When the ink droplets attached to the recording medium 2 are irradiated with radiation from the light source 11, a photopolymerization reaction of the polymerizable compound in the ink proceeds, causing the ink droplets to harden and form an ink coating. This results in coloring of the recording medium 2, formation of images, colors, characters, patterns, etc. on the recording medium 2, and formation of a clear ink coating.

[0104] The light source 11 is not limited to being arranged next to the inkjet head 3 in the main scanning direction, and the light source 11 may be offset from the inkjet head 3 in the sub-scanning direction opposite to the direction in which the recording medium 2 is transported. The light source 11 is not limited to being arranged on the carriage 4, and may be separate from the carriage 4.

[0105] In this embodiment, an on-carriage type printer 1 is exemplified as an inkjet device, but this is not limiting. The inkjet device may be, for example, an off-carriage type such as a large format printer in which the ink container is not mounted on the carriage. In addition, the inkjet device used in this embodiment is not limited to a serial printer, and may be a line head printer in which the inkjet head is formed to be as wide as or wider than the width of the recording medium 2 and printing is performed without moving the inkjet head.

[0106] 5. Recording medium The recording medium 2 is appropriately selected depending on the purpose of the printed matter produced from the ink and the recording medium. The material for forming the recording medium 2 is not particularly limited, but examples thereof include plastics such as polyvinyl chloride (PVC), polyethylene terephthalate, polypropylene, polyethylene, polycarbonate, cellulose diacetate, cellulose triacetate, cellulose propionate, cellulose butyrate, cellulose acetate butyrate, cellulose nitrate, polyethylene terephthalate, polyethylene, polystyrene, polypropylene, polycarbonate, and polyvinyl acetal, as well as those whose surfaces have been treated, glass, paper, metal, and wood.

[0107] The recording medium 2 may be in the form of, for example, a roll or a single sheet, a board, or a cloth.

[0108] 6. Inkjet method The inkjet method according to this embodiment includes an application process in which the above-mentioned ink is ejected from the inkjet head 3 of the printer 1 and adhered to the recording medium 2, and a curing process in which the ink adhered to the recording medium 2 is irradiated with radiation.

[0109] 6.1.Coating process In the coating process, color inks are ejected from the inkjet head 3 of the printer 1 onto the recording medium 2 to adhere to it. More specifically, a piezoelectric element is driven to eject ink filled in a pressure generating chamber of the inkjet head 3 from an ejection nozzle. This type of ejection method is also called an inkjet method. At this time, a multi-pass method may be used in which the carriage 4 repeats reciprocating movement in the main scanning direction multiple times relative to a predetermined position on the recording medium 2. That is, the transport of the recording medium 2 in the sub-scanning direction is stopped for a certain period of time to eject color inks in multiple passes, and then the recording medium 2 is transported a short distance before performing the multi-pass method again.

[0110] By depositing color ink onto the recording medium 2 while moving the inkjet head 3 relatively to the recording medium 2, a liquid layer of color ink is formed on the recording medium 2, which serves as a base for a desired image or the like.

[0111] 6.2.Curing process In the curing process, a coating film is formed from the liquid layer of the ink formed on the recording medium 2. More specifically, radiation is irradiated from the light source 11 toward a predetermined position on the recording medium 2. The radiation irradiated area on the recording medium 2 need only include the area where the ink is applied. The radiation irradiation causes a photopolymerization reaction of the polymerizable compound in the ink in the liquid layer on the recording medium 2 to proceed, and the ink hardens to become a coating film.

[0112] When a clear ink is used to form a coating film, the steps of applying and curing the clear ink may be carried out before or after the steps of applying and curing the color inks.

[0113] According to this embodiment, the following effects can be obtained.

[0114] In the ink, the viscosity can be reduced and the adhesion of the coating film can be improved. That is, it is possible to provide an ink having a low viscosity and excellent adhesion of the coating film.

[0115] In the inkjet method, the viscosity of the ink is reduced, which improves the ejection properties of the ink from the inkjet head 3. In addition, a coating film with improved adhesion to the recording medium 2 can be formed.

[0116] 7. Examples and Comparative Examples The effects of the present invention will be described in more detail below with reference to examples and comparative examples. Tables 1, 2, and 3 show the composition and evaluation results for each ink of Examples 1 to 34 and Comparative Examples 1 to 4. In the composition columns of Tables 1 to 3, the units of values ​​are mass%, and columns with no value or - sign mean that the component is not contained. In Tables 1 to 3, abbreviations are used for the names of some components. The abbreviations will be described later. Hereinafter, the inks of Examples 1 to 34 are collectively referred to as the inks of the examples, the inks of Comparative Examples 1 to 4 are collectively referred to as the inks of the comparative examples, and the inks of the examples and comparative examples are collectively referred to as the inks. The present invention is not limited in any way by the following examples.

[0117] 7.1. Preparation of ink Each ink was prepared according to the composition in Tables 1 to 3. Specifically, the pigment (coloring material), the dispersant, and a portion of the polymerizable compound were weighed and placed in a tank for dispersion with a bead mill. Next, ceramic beads with a diameter of 1 mm were placed in the tank and dispersed with a bead mill to prepare each pigment dispersion in which the pigment was dispersed in the polymerizable compound.

[0118] Separately from the pigment dispersion, the remaining additives such as the polymerizable compound, photopolymerization initiator, and fluorescent whitening agent other than the components blended in the pigment dispersion were weighed and added to a stainless steel mixing tank. Then, the mixture was stirred using a mechanical stirrer to completely dissolve the solids such as the photopolymerization initiator in the polymerizable compound. Next, the pigment dispersion was weighed and stirred for another hour in an environment of about 20°C. After that, filtration was performed using a membrane filter with a pore size of 5 μm to prepare the inks of the examples and comparative examples.

[0119] [Table 1]

[0120] [Table 2]

[0121] [Table 3]

[0122] Details of the abbreviations and product names used in Tables 1 to 3 are as follows:

[0123] Vinylmethyloxazolidinone VMOX: Vinylmethyloxazolidinone. BASF. Monomers with multiple vinyl ether groups DVE-2: Diethylene glycol divinyl ether. BASF. DVE-3: Triethylene glycol divinyl ether. BASF. CHDM-di: 1,4-Cyclohexanedimethanol divinyl ether. Trade name SR420, Sartomer Corporation. Monomer of formula (1) VEEA: 2-(2-vinyloxyethoxy)ethyl acrylate. Trade name, Nippon Shokubai Co., Ltd. Monofunctional (meth)acrylate monomer having an aromatic group PHEA: Phenoxyethyl acrylate. Product name: Viscoat #192, Osaka Organic Chemical Industry Co., Ltd. Monofunctional (meth)acrylate monomer with alicyclic structure IBXA: Isobornyl acrylate. Osaka Organic Chemical Industry Co., Ltd. TMCHA: 3,3,5-trimethylcyclohexyl acrylate. Osaka Organic Chemical Industry Co., Ltd. Monofunctional (meth)acrylate monomer having a cyclic ether structure CTFA: Cyclic trimethylolpropane formal acrylate. Product name: Viscoat #200, Osaka Organic Chemical Industry Co., Ltd. MEDOL-10: (2-methyl-2-ethyl-1,3-dioxolan-4-yl) methyl acrylate. Trade name, Osaka Organic Chemical Industry Co., Ltd. Monofunctional (meth)acrylate monomer having a crosslinked condensed ring structure FA-512AS: Dicyclopentenyloxyethyl acrylate. Hitachi Chemical Co., Ltd. Other polymerizable compounds Monofunctional monomers nVC: N-vinylcaprolactam. ISP Japan. ACMO: Acryloylmorpholine. KJ Chemicals. Other polymerizable compounds Polyfunctional monomers TPGDA: Tripropylene glycol diacrylate. Product name: Viscoat #310HP, Osaka Organic Chemical Industry Co., Ltd. NPG(2PO)DA: Propoxylated (2) neopentyl glycol diacrylate. Trade name SR9003, Sartomer Corporation. Other polymerizable compounds Oligomers EC6101: Aliphatic urethane acrylate oligomer. Trade name ETERCURE(R) 6101, Changxing Materials Co., Ltd. CN9893: Aliphatic urethane acrylate oligomer. Trade name, Sartomer Corporation.

[0124] Photoinitiator Omnirad 819: Trade name. Bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. IGM RESINS BV. Speedcure TPO: Trade name. 2,4,6-trimethylbenzoyldiphenylphosphine oxide. Lambson Group Ltd. Speedcure® DETX: Trade name. 2,4-diethylthioxanthone. Produced by Lambson Group Ltd.

[0125] Optical brightener TELALUX® OB: (2,5-bis(5-tert-butyl-2-benzoxazolyl)thiophene). Trade name, Clariant Japan K.K. TELALUX® KCB (1,4-bis(2-benzoxazolyl)naphthalene), trade name, Clariant Japan K.K.

[0126] Polymerization Inhibitor LA-7RD: 4-hydroxy-2,2,6,6-tetramethylpiperidinyl-1-oxyl. Trade name: Adeka STAB (registered trademark) LA-7RD, ADEKA Corporation. MEHQ: 4-Methoxyphenol. Kanto Chemical Co., Ltd.

[0127] Surfactants BYK-UV3500: Silicone surfactant. Trade name, BYK Additives&Instruments.

[0128] Pigments PB-15:3: CI Pigment Blue 15:3. Clariant Japan.

[0129] Dispersants Solsperse® 36000: Trade name, manufactured by Lubrizol.

[0130] Here, the ink of Example 1 is at a level in which DVE-3 is used as a monomer having multiple vinyl ether groups, VEEA is used as a monomer of formula (1), and PHEA having an aromatic group is used as a monofunctional (meth)acrylate.

[0131] The ink of Example 2 is at a level where the amount of VMOX is increased and the amounts of VEEA and PHEA are decreased compared to the ink of Example 1.

[0132] The ink of Example 3 is at a level where the amount of VMOX is increased and the amount of PHEA is decreased compared to the ink of Example 2.

[0133] The ink of Example 4 contains a reduced amount of VMOX and an increased amount of PHEA compared to the ink of Example 1.

[0134] The ink of Example 5 contains a reduced amount of VMOX and an increased amount of PHEA compared to the ink of Example 4.

[0135] The ink of Example 6 is at the same level as the ink of Example 1, except that DVE-3 is replaced with DVE-2.

[0136] The ink of Example 7 is at the same level as the ink of Example 1 except that DVE-3 is replaced with CHDM-di.

[0137] The ink of Example 8 is a level where DVE-2, DVE-3, and CHDM-di are used in combination with the ink of Example 1 as monomers having multiple vinyl ether groups.

[0138] The ink of Example 9 is at a level where the amount of DVE-3 is increased and the amount of VEEA is decreased compared to the ink of Example 1.

[0139] The ink of Example 10 is at a level where the amount of DVE-3 is increased and the amount of VEEA is decreased compared to the ink of Example 9.

[0140] The ink of Example 11 is at a level where the amount of DVE-3 is reduced compared to the ink of Example 1, and the amount of the reduced amount is replaced with NPG(2PO)DA, which is a polyfunctional monomer of another polymerizable compound.

[0141] The ink of Example 12 contains a reduced amount of DVE-3 and an increased amount of NPG(2PO)DA compared to the ink of Example 11.

[0142] The ink of Example 13 contains increased amounts of DVE-3 and PHEA and a reduced amount of VEEA compared to the ink of Example 11.

[0143] The ink of Example 14 is the same as the ink of Example 13 except that it does not contain VEEA and contains increased amounts of VMOX and DVE-3.

[0144] The ink of Example 15 contains reduced amounts of VMOX, DVE-3, and PHEA and an increased amount of VEEA compared to the ink of Example 1.

[0145] The ink of Example 16 contains a reduced amount of VMOX and an increased amount of VEEA compared to the ink of Example 15.

[0146] The ink of Example 17 contains increased amounts of VMOX and DVE-3 and reduced amounts of VEEA and PHEA compared to the ink of Example 15.

[0147] The ink of Example 18 contains reduced amounts of VMOX and VEEA and increased amounts of DVE-3 and PHEA compared to the ink of Example 15.

[0148] The ink of Example 19 is a level different from the ink of Example 1 in that IBXA having an alicyclic structure is used as the monofunctional (meth)acrylate.

[0149] The ink of Example 20 is at a level where the amount of VMOX is increased and the amount of IBXA is decreased compared to the ink of Example 19.

[0150] The ink of Example 21 contains reduced amounts of VMOX and VEEA and an increased amount of IBXA compared to the ink of Example 19.

[0151] The ink of Example 22 is at a level different from that of Example 1 in that TMCHA having an alicyclic structure is used as the monofunctional (meth)acrylate.

[0152] The ink of Example 23 is at a level different from that of Example 1 in that CTFA having a cyclic ether structure is used as the monofunctional (meth)acrylate.

[0153] The ink of Example 24 contains an increased amount of VMOX and a decreased amount of CTFA compared to the ink of Example 23.

[0154] The ink of Example 25 has reduced amounts of VMOX and VEEA, and reduced amounts of CTFA, compared to the ink of Example 23.

[0155] The ink of Example 26 is a level different from the ink of Example 1 in that MEDOL-10 having a cyclic ether structure is used as the monofunctional (meth)acrylate.

[0156] The ink of Example 27 is a standard ink in which FA-512AS having a crosslinked condensed ring structure is used as the monofunctional (meth)acrylate in comparison with the ink of Example 1.

[0157] The ink of Example 28 contains a reduced amount of FA-512AS compared to the ink of Example 27, and also contains PHEA, IBXA, and CTFA.

[0158] The ink of Example 29 has an increased amount of DVE-3 and decreased amounts of VEEA and NPG(2PO)DA compared to the ink of Example 11.

[0159] The ink of Example 30 is at a level where NPG(2PO)DA is replaced with TPGDA compared to the ink of Example 29.

[0160] The ink of Example 31 has a reduced amount of VEEA compared to the ink of Example 1, and the reduced amount is replaced with EC6101, which is an oligomer of another polymerizable compound.

[0161] The ink of Example 32 contains a reduced amount of VEEA compared to the ink of Example 1, and the reduced amount is replaced with CN9893, which is an oligomer of another polymerizable compound.

[0162] The ink of Example 33 contains a reduced amount of VEEA compared to the ink of Example 1, and the reduced amount is replaced with NPG(2PO)DA and EC6101.

[0163] The ink of Example 34 is the same as that of Example 1 except that the fluorescent brightener was changed from TELALUX OB to TELALUX KCB.

[0164] The ink of Comparative Example 1 is a level where, compared to the ink of Example 1, VMOX is not blended and the amount of PHEA is increased.

[0165] The ink of Comparative Example 2 is the same as the ink of Example 1 except that it does not contain DVE-3 and that the reduced amount is replaced with NPG(2PO)DA.

[0166] The ink of Comparative Example 3 has a reduced amount of PHEA compared to the ink of Comparative Example 1, and the reduced amount is replaced with nVC, which is a monofunctional monomer of another polymerizable compound.

[0167] The ink of Comparative Example 4 is at a level where the amount of PHEA is reduced compared to the ink of Comparative Example 1, and the reduced amount is replaced with ACMO, which is a monofunctional monomer of another polymerizable compound.

[0168] Evaluation The inks of the Examples and Comparative Examples were evaluated as described below, and the evaluation results are shown in the columns of evaluation results in Tables 1 to 3.

[0169] 7.2.1.Ink Viscosity The viscosity of the ink at 25°C was measured within 1 hour after the ink preparation using the ink viscosity measuring method described above, and evaluated according to the following evaluation criteria. The ink viscosity evaluated here was used as the initial viscosity of the ink in the storage stability evaluation described later. Evaluation criteria AA: Viscosity is 15 mPa·s or less. A: Viscosity is greater than 15 mPa·s and less than 20 Pa·s. B: Viscosity is greater than 20 mPa·s and less than 25 mPa·s. C: Viscosity is greater than 25 mPa·s and less than 30 mPa·s. D: Viscosity exceeds 30 mPa·s.

[0170] 7.2.2. Odor of coating film The ink was applied to the recording medium to a thickness of 10 μm using a bar coater. The recording medium used was a vinyl chloride film (trade name: JT5829R, manufactured by MACtac). Next, a UV-LED was used to apply 400 mJ / cm 2 The ink was irradiated with radiation at an energy of 1000 rpm to form a coating film of the ink. Then, a sensory evaluation was performed in an environment of about 25° C. on the odor generated from the coating film, and the odor was evaluated according to the following evaluation criteria. Evaluation criteria A: Odorless or barely detectable odor. B: It's a faint smell and I can tell what it is. C: The odor is easily detectable. D: Strong or intense odor.

[0171] 7.2.3. Ink curing First, ink was printed on a recording medium by an inkjet method. Specifically, a polyvinyl chloride film JT5829R manufactured by MACtac was used as a recording medium. An inkjet printer PX-G930 manufactured by Seiko Epson was used as an inkjet device. The ink printing pattern was a solid image with a recording resolution of 600 dpi (dots per inch) horizontally and 600 dpi vertically. The printer was modified to use a plastic film as a recording medium and to eject radiation-curable ink.

[0172] Next, the curing property of the ink applied on the recording medium was evaluated. Specifically, the ink on the recording medium was irradiated with different irradiation energies using a UV-LED with a peak wavelength of 395 nm as a light source device. Then, the irradiation energy at which the ink became tack-free and a coating film was formed was investigated. The irradiation energy required for the ink to become tack-free was evaluated according to the following evaluation criteria. Evaluation criteria A: Irradiation energy is 200mJ / cm 2 is less than. B: Irradiation energy is 200 mJ / cm 2 More than 350mJ / cm 2 is less than. C: Irradiation energy is 350 mJ / cm 2 More than 500mJ / cm 2 is less than. D: Irradiation energy is 500 mJ / cm 2 That's all.

[0173] 7.2.4. Coating adhesion In the same manner as in the evaluation of the curing properties of the ink described above, the ink was applied onto a polyvinyl chloride film JT5829R. Then, the ink was irradiated with 400 mJ / cm using the above UV-LED. 2 A coating film was formed with an irradiation energy of 100 nm to 150 nm. A cross-cut test was carried out on the obtained coating film in accordance with JIS K5600-5-6 to evaluate the adhesion between the coating film and a recording medium.

[0174] Specifically, a cutter was used as a cutting tool, and the blade of the cutter was placed perpendicularly against the coating film to make multiple cuts in the coating film. The cuts were made into a 10 x 10 grid with a distance of 1 mm between adjacent cuts. A transparent adhesive tape with a width of 25 mm cut to a length of 75 mm was attached to the grid, and the tape was rubbed and pressed sufficiently with a finger so that there was no gap between the coating film. Next, within 5 minutes after the tape was attached, the end of the tape was lifted so that the angle between the tape and the coating film surface was about 60°, and the tape was instantly peeled off from the coating film within 0.5 to 1.0 seconds. Thereafter, the peeling state of the coating film was visually observed and evaluated according to the following evaluation criteria. Evaluation criteria AA: No peeling of the coating was observed on the grid. A: Peeling of the coating is observed in less than 10% of the grid. B: Peeling of the coating is observed in 10% or more but less than 35% of the grid. C: Peeling of the coating is observed in 35% or more but less than 50% of the grid. D: Peeling of the coating is observed on more than 50% of the grid.

[0175] 7.2.5. Ink storage stability As an index of the storage stability of the ink, the change in the viscosity of the ink after being left at 60°C for 14 days was investigated. Specifically, the ink was placed in a 30 ml brown glass tube, sealed, and placed in a thermostatic chamber adjusted to 60°C for 14 days. The ink was then removed from the thermostatic chamber and allowed to cool to 25°C, after which the viscosity was measured by the method described above and used as the viscosity after being left. The rate of change in the viscosity of the ink after being left relative to its initial viscosity was calculated and evaluated according to the following evaluation criteria. Evaluation criteria A: The viscosity change rate is less than +5%. B: The rate of change in viscosity is +5% or more but less than +10%. C: The viscosity change rate is +10% or more.

[0176] 7.2.6. Summary of evaluation results As shown in Tables 1, 2, and 3, the viscosity of the ink of the Examples was rated B or higher, which corresponds to good, except for Examples 11, 12, 14, and 33. In particular, Examples 3, 17, 20, and 24 were rated AA, which corresponds to excellent. Examples 11, 12, 14, and 33 were rated C, which corresponds to fair. In addition, the adhesion of the coating film of the Examples was rated A or higher, which corresponds to excellent, except for Examples 4 and 5. In particular, Examples 31 and 33 were rated AA, which corresponds to excellent. Example 4 was rated B, which corresponds to good, and Example 5 was rated C, which corresponds to fair. This shows that the ink of the Examples has low viscosity and excellent adhesion of the coating film.

[0177] The odor of the inks of the Examples was rated B or higher, which corresponds to good, except for Examples 12 and 16, and was rated C, which corresponds to fair, for Examples 12 and 16. The curability of the inks of the Examples was rated B or higher, which corresponds to good, except for Example 10, and was rated C, which corresponds to fair, for Example 10. The storage stability of the inks of the Examples was rated A, which corresponds to good, except for Examples 2 and 3, and was rated B, which corresponds to fair, for Example 2, and was rated C, which corresponds to poor, for Example 3. From the above, it was shown that the inks of the Examples are easy to improve in odor, curability, and storage stability.

[0178] On the other hand, the ink of the comparative example was rated D, which corresponds to poor viscosity or poor adhesion, indicating that viscosity reduction and coating adhesion are incompatible. [Explanation of symbols]

[0179] 1...inkjet printer, 2...recording medium, 3...inkjet head.

Claims

1. Vinylmethyloxazolidinone and a monomer having two or more vinyl ether groups. Including, The content of the monomer having two or more vinyl ether groups is 5% by mass or more based on the total amount. The content is 30% by mass or less, The content of the vinylmethyloxazolidinone is 5% by mass or more and 40% by mass or less based on the total amount. is as follows: Further comprising a monofunctional (meth)acrylate monomer; Radiation curable ink jet ink composition.

2. Vinylmethyloxazolidinone and a monomer having two or more vinyl ether groups. Including, A radiation-curable ink-jet ink composition further comprising a monomer represented by the following formula (1): Composition. H 2 C=CR 1 -CO-OR 2 -O-CH=CH-R 3 ・・・(1) (In the formula, R 1 is a hydrogen atom or a methyl group, R 2 is a divalent organic compound having 2 to 20 carbon atoms. is a residue, R 3 is a hydrogen atom or a monovalent organic residue having 1 to 11 carbon atoms.

3. The radiation-curable ink according to claim 1 , further comprising a monomer represented by the following formula (1): Jet ink composition. H 2 C=CR 1 -CO-OR 2 -O-CH=CH-R 3 ・・・(1) (In the formula, R 1 is a hydrogen atom or a methyl group, R 2 is a divalent organic compound having 2 to 20 carbon atoms. is a residue, R 3 is a hydrogen atom or a monovalent organic residue having 1 to 11 carbon atoms.

4. The content of the monomer represented by the formula (1) is 10% by mass or more and 50% by mass or less based on the total amount.

4. The radiation-curable inkjet ink according to claim 2, wherein the Composition.

5. The monofunctional (meth)acrylate monomer may be a monofunctional (meth)acrylate having an aromatic group. The radiation curable ink-jet ink composition of claim 1 comprising an acrylate monomer. 。

6. The radiation-curable composition according to any one of claims 1 to 5, further comprising a fluorescent whitening agent. Inkjet ink composition.

7. The radiation curable inkjet ink composition according to any one of claims 1 to 6. ejecting the object from an inkjet head and depositing the object on a recording medium; The radiation-curable inkjet ink composition applied to the recording medium is then subjected to radiation. and exposing the ink to radiation.

Citation Information

Patent Citations

  • Active energy ray-curable inkjet ink composition

    JP2014055198A

  • Radiation-curable inkjet composition and inkjet method

    JP2021042321A

  • Radiation-curable inkjet composition and inkjet method

    JP2021042322A

  • Carbon-based porous material, preparation method therefor and use thereof

    WO2018014659A1

  • Printing ink

    WO2018197852A1