Laminate for tube container, tube container, and method for producing laminate for tube container

The laminate structure for tube containers with integrated layers and a check valve addresses the inefficiencies of separate manufacturing processes, enhancing productivity and cost-effectiveness while ensuring air-tightness.

JP7559468B2Active Publication Date: 2024-10-02DAI NIPPON PRINTING CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020161271
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-25
Publication Date
2024-10-02
Estimated Expiration
2040-09-25

AI Technical Summary

Technical Problem

Conventional double tube containers require separate manufacturing processes for the outer and inner layers, increasing the number of manufacturing steps and costs.

Method used

A laminate for tube containers is designed with an outer layer and an inner layer, featuring a weak seal between them, and includes holes in the outer layer to prevent air backflow, integrated with a check valve in the mouth portion, manufactured through a process involving inflation molding and lamination of sealant layers.

Benefits of technology

This approach reduces manufacturing processes and costs while effectively preventing air from entering the container, maintaining content quality by minimizing air backflow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559468000001
    Figure 0007559468000001
  • Figure 0007559468000002
    Figure 0007559468000002
  • Figure 0007559468000003
    Figure 0007559468000003
Patent Text Reader

Abstract

To provide a method of manufacturing a laminate for a tube container including a reduced number of manufacturing steps, and further provide a laminate for tube containers and a tube container whereby it is possible to prevent the reverse flow of air into a tube container even when filled with a content containing cosmetics, etc.SOLUTION: A laminate 55 constitutes a body part of a tube container, and the laminate 55 comprises an outer layer 1 and an inner layer 2 arranged in sequence from an outer surface toward an inner surface, and a weak seal part 57d is provided between the outer layer 1 and the inner layer 2, and the outer layer 1 includes a first sealant layer 56, a base material layer 58 and a second sealant layer 59, and the inner layer 2 includes a third sealant layer 60, and a hole 15 is provided at least at a part of the outer layer 1.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a laminate for a tube container, a tube container, and a method for manufacturing the laminate for a tube container. [Background technology]

[0002] Tube containers are filled and packaged with the contents, and the required amount can be squeezed out at the time of use. For this reason, tube containers are widely used as containers for foods, cosmetics, medicines, etc.

[0003] Such tube containers are usually composed of a body portion whose main component is synthetic resin, and a head member including a mouth portion (for example, Patent Document 1).

[0004] The tube container has a high degree of elasticity, so that after it is squeezed, the outside air flows back from the spout, and the air easily gets mixed into the container. For this reason, in order to maintain the quality of the cosmetics and the like stored in the tube container, a double tube container has been proposed, which is composed of an opening with a check valve that prevents the backflow of air into the tube container, an outer tube with a through hole, and an inner tube (for example, Patent Document 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 5-220900 [Patent Document 2] JP 2015-205717 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in conventional double-walled tube containers, the outer layer and the inner layer are formed in separate manufacturing processes, and then a process is required to insert the cylindrical inner layer into the cylindrical outer layer, which results in a disadvantage in that the number of manufacturing processes for the double-walled tube is increased and the cost is high. [Means for solving the problem]

[0007] The present disclosure has been made in light of the above circumstances, and aims to provide a laminate for a tube container and a tube container that reliably prevents air from flowing back into the tube container even when the tube container is filled with contents including cosmetics, etc. It also aims to provide a method for manufacturing the tube container and the laminate for a tube container.

[0008] That is, the laminate for a tube container of the present disclosure is a laminate that constitutes the body of a tube container, the laminate comprising an outer layer and an inner layer arranged in order from the outer surface to the inner surface, a weak seal portion between the outer layer and the inner layer, the outer layer comprising a first sealant layer, a base layer, and a second sealant layer, the inner layer comprising a third sealant layer, and at least a portion of the outer layer comprising a hole.

[0009] In addition, the tube container of the present disclosure comprises a cylindrical body member formed by overlapping and joining opposing ends of a laminate for a tube container to each other, and a head member joined to one end of the cylindrical body member, the head member including a shoulder portion and a mouth portion, and a check valve provided at the mouth portion.

[0010] Further, a manufacturing method of a laminate for a tube container according to the present disclosure is a manufacturing method of the laminate for a tube container, and is characterized in that it includes a step of manufacturing a hollow film by an inflation molding method, a step of flattening the hollow film after inflation molding and weakly sealing the inner surfaces together, a step of cutting both longitudinal side edge portions of the flat hollow film by a predetermined width to manufacture the second sealant layer and the third sealant layer, a winding step of winding up the second sealant layer and the third sealant layer, and a step of overlapping and laminating the base layer and the first sealant layer on the second sealant layer side of the second sealant layer and the third sealant layer pulled out from the winding. Effect of the Invention

[0011] According to the present disclosure, the number of manufacturing steps is small, and the manufacturing cost is low. In addition, even when the contents containing cosmetics or the like are filled, the contents can be prevented from being deteriorated due to the backflow of air into the tube container. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a cross-sectional view showing an example of a layer structure of the laminate for tube containers according to the present embodiment. [Diagram 2] FIG. 4 is a cross-sectional view showing another example of the layer structure of the laminate for tube containers according to the present embodiment. [Diagram 3] FIG. 2 is a partial vertical cross-sectional view showing the tube container according to the present embodiment with a cap attached. [Figure 4] FIG. 2 is a partial vertical cross-sectional view showing the tube container according to the present embodiment filled with contents. [Diagram 5] 1 is a schematic diagram showing a method for producing a hollow film used in a laminate for a tube container according to the present embodiment. FIG. [Figure 6] 4A to 4C are diagrams showing a method for manufacturing a tube container. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. Figures 1 to 6 are diagrams showing one embodiment of the present disclosure. In addition, the numerical values ​​such as dimensions of each member and the names of materials described in this specification are examples of the embodiment, and are not limited thereto, and can be appropriately selected and used.

[0014] Fig. 3 is a partial cross-sectional view of the tube container according to this embodiment with the cap attached, and Fig. 4 is a partial cross-sectional view of a packaged product of the tube container filled with contents.

[0015] 3, the tube container 10 includes a body 50 formed of a laminate sheet 55, and a head member 40 produced by providing a synthetic resin to the body 50 by a method such as compression molding or injection molding. The head member 40 further includes a shoulder portion 12 and a mouth portion 11. A cap 20 is attached to the mouth portion 11 of the tube container 10. The mouth portion 11 further includes a check valve 13, which will be described later.

[0016] 3, the tube container 10 comprises a multi-layer outer layer 1 forming an outer shell, and a deformable inner layer 2 for accommodating the contents, and the outer layer 1 and the inner layer 2 are fixed by strong sealing at the connection part of the head member at the upper end and at the bottom part at the lower end. Also, a hole 15, which will be described later, is provided in a part of the outer layer 1.

[0017] The hole 15 is for air intake, and the position of the hole 15 is not limited as long as it is formed through the entire thickness of the outer layer 1. The shape of the hole 15 is not particularly limited, and examples thereof include a circle, an ellipse, a polygon such as a square, a cross, a line, a V-shape, and other suitable slit shapes. The hole 15 may further be provided with a check valve film.

[0018] The tube container 10 having such a configuration is obtained through the following manufacturing process.

[0019] A laminate sheet 55 of a cylindrical body member of a tube container according to the present disclosure described later is used, and both ends of the laminate sheet are overlapped and the outer and inner sides of the overlapped portion are heat-sealed to form a side seal portion 18, thereby manufacturing a cylindrical body. Next, the cylindrical body is placed in a mold, and a shoulder portion and a mouth portion are formed at one opening of the cylindrical body portion 50 by a method such as compression molding. In this way, the shoulder portion and the mouth portion are integrally molded at one opening of the cylindrical body portion, thereby producing a tube container 10. At the mouth portion, a check valve made of a thermoplastic resin is integrated by simultaneous molding. Then, a cap 20 is attached to the mouth portion of the tube container 10 (see FIG. 3).

[0020] At the other end of the cylindrical body 50, a bottom seal 17 is formed by bonding together two laminate sheets 55. This bottom seal 17 is formed by bonding together two laminate sheets 55 near the opening 16 after, for example, an appropriate amount of content C is filled through the opening 16 formed at the other end of the cylindrical body 50 (see FIG. 4).

[0021] Next, laminate sheet 55 for a cylindrical body part according to this embodiment will be described with reference to Figures 1 and 2. As shown in Figure 1, laminate sheet 55 for a cylindrical body part has a double structure having an outer layer 1 and an inner layer 2, and a weak seal portion 57d is formed between outer layer 1 and inner layer 2. In addition, a hole 15 is provided in a part of outer layer 1.

[0022] The outer layer 1 includes a first sealant layer 56, a first adhesive layer 57a, a base layer 58, a second adhesive layer 57b, and a second sealant layer 59, arranged in this order from the outside to the inside. The inner layer 2 includes a third sealant layer 60 .

[0023] Also, as shown in FIG. 2, in the laminate sheet 55 of the tubular body portion, the outer layer 1 includes, arranged in order from the outside to the inside, a first sealant layer 56, a first adhesive layer 57a, a base layer 58, a second adhesive layer 57b, and a second sealant layer 59. The inner layer 2 includes a third sealant layer 60, a third adhesive layer 57c, a gas barrier layer 53, a fourth adhesive layer 57e, and a fourth sealant layer 61.

[0024] In laminate sheet 55 of the cylindrical body portion shown in FIG. 1 or FIG. 2, for example, a printed layer may be provided on the inside of base material layer 58 by reverse printing.

[0025] In this specification, the terms "outside" and "inside" refer to the "outside" and "inside" when the tube container 10 is produced using the laminate sheet 55 for the cylindrical body portion.

[0026] Next, each layer of the laminate sheet 55 of the cylindrical body will be described.

[0027] The second sealant layer 59 and the third sealant layer 60 are layers for weakly sealing the outer layer 1 and the inner layer 2. The first sealant layer 56 is a layer for bonding the laminate sheets 55 of the cylindrical body portion together.

[0028] The second sealant layer 59 and the third sealant layer 60 are formed by using a hollow film that has been crushed into a flat shape, and cutting off both longitudinal edge portions of the flat hollow film by a predetermined width. The second sealant layer 59 and the third sealant layer 60 have a weak seal portion 57d between their opposing inner surfaces. The seal strength of the weak seal portion 57d is preferably 0.1 N / 15 mm or more and 2 N / 15 mm or less, and more preferably 1 N / 15 mm or more and 2 N / 15 mm or less. If the seal strength is within the above range, the laminate sheet 55 of the cylindrical body portion does not peel off during processing, and when used as the inner layer of a tube container, the inner surfaces can be easily peeled off when the contents are pushed out, which is preferable.

[0029] The hollow film is not particularly limited as long as it has the suitability for inflation molding and heat sealing, and for example, a polyolefin film can be used. More specifically, for example, a low density polyethylene film (LDPE), a medium density polyethylene film (MDPE), a high density polyethylene film (HDPE), a linear low density polyethylene film (LLDPE), a polypropylene film, an acid-modified polyolefin resin film obtained by modifying a polyolefin resin such as polyethylene or polypropylene with acrylic acid, methacrylic acid, maleic acid, maleic anhydride, fumaric acid, itaconic acid, or other unsaturated carboxylic acid, a polyvinyl acetate resin film, a polyester resin film, a polystyrene resin film, a polyacrylonitrile, a saturated polyester, a polyvinyl alcohol, or other resin film can be used.

[0030] In the present embodiment, among the above, a low-density polyethylene film is preferable because it is easy to handle.

[0031] In this embodiment, for example, a resin composition can be prepared by using one or more of the above resins as the main component and optionally adding desired additives thereto, and then the resin composition prepared as above can be used.

[0032] In addition, as the material, for example, antiblocking agents, lubricants (fatty acid amides, etc.), flame retardants, inorganic or organic fillers, etc. may be added arbitrarily.

[0033] In the present embodiment, the thickness is preferably 10 μm or more and 200 μm or less, and more preferably 60 μm or more and 150 μm or less. If it is within the above range, it can be easily manufactured by an inflation molding method.

[0034] The hollow films used for the second sealant layer 59 and the third sealant layer 60 in this embodiment are preferably obtained by an inflation molding method. That is, the inflation film is already cylindrical and can be used in the form in which it is produced.

[0035] Fig. 5 is an explanatory diagram illustrating an inflation molding method for obtaining a hollow film used for the second sealant layer 59 and the third sealant layer 60 of this embodiment. In Fig. 5, 100 is an extruder, 101 is an inflation die, and the molten resin 120 extruded in a tubular shape from the extruder 100 through the inflation die 101 is inflated by air supplied from an air supply pipe 103 while being pulled up vertically, and is flattened while being air-cooled, and the inner surfaces of the hollow films are overlapped to form a weak seal portion 57d on the entire surface, and the hollow film is taken up by a take-up device to obtain a take-up roll 121 in which the hollow film is wound in a flat shape. In Fig. 5, 105 is an air ring for air cooling, 106 is a guide roller, 107 is a stabilizer, 108 is a pinch roll, and 110 is a take-up device.

[0036] Next, the first sealant layer 56 and the fourth sealant layer 61 are layers for bonding the laminate sheets 55 of the cylindrical body portion together. The materials constituting the first sealant layer and the fourth sealant layer 61 may be any materials that can be melted and fused by heat.

[0037] It is preferable that the first sealant layer 56 allows the printed layer formed on the base layer 58 to be seen through.

[0038] The first sealant layer 56 and the fourth sealant layer 61 are layers for bonding the laminate sheets 55 of the cylindrical body portion together. The first sealant layer may be made of a material similar to that of the second sealant layer described above.

[0039] In the present embodiment, the first sealant layer 56 and the fourth sealant layer 61 can be prepared, for example, by preparing a resin composition using one or more of the above-mentioned resins as the main component and optionally adding desired additives thereto, and then using the resin composition prepared above, for example, a film or sheet can be formed using a T-die method, an inflation molding method, or other molding method.

[0040] The materials for the first sealant layer 56 and the fourth sealant layer 61 may contain, for example, an antiblocking agent, a lubricant (fatty acid amide, etc.), a flame retardant, an inorganic or organic filler, etc., as desired.

[0041] In this embodiment, the thickness of the first sealant layer 56 is preferably thinner than the thickness of the third sealant layer 60 or the fourth sealant layer 61. By not making the first sealant layer too thick, it is possible to prevent a decrease in the visibility of a printed layer when the printed layer is provided on the inside of the base layer 58 by reverse printing. This makes it possible to prevent a decrease in the design of the cylindrical body of the tube container.

[0042] In this embodiment, the thickness of the first sealant layer 56 and the fourth sealant layer 61 is preferably 10 μm or more and 200 μm or less, and more preferably 30 μm or more and 180 μm or less.

[0043] The base layer 58 may be made of any material that is strong, tough, and heat-resistant as a basic material constituting the tube container 10 .

[0044] Examples of materials that can be used to form the base layer 58 include films or sheets of polyester-based resins, polyamide-based resins, polyaramid-based resins, polyolefin-based resins, polycarbonate-based resins, polyacetal-based resins, fluorine-based resins, and other tough resins.

[0045] Among the above, polyester resins, particularly polyethylene terephthalate (PET) resins, are preferred in terms of printability. Here, polyethylene terephthalate resins refer to pure polyethylene terephthalate resins and various modified polyethylene terephthalate resins.

[0046] Any of an unstretched film, a uniaxially or biaxially stretched film, and the like can be used as the base layer 58. Among them, in the present embodiment, a biaxially stretched polyester resin film is preferred because of its excellent printability.

[0047] In the present embodiment, the thickness of the base layer 58 is preferably 10 μm or more and 25 μm or less.

[0048] The print layer is a layer for forming a pattern or the like on the tube container.

[0049] The printing layer can be formed on the above-mentioned base material layer 58 by a printing method such as gravure printing, letterpress printing, screen printing, transfer printing, flexographic printing, ink-jet printing, or the like.

[0050] The design is not particularly limited, and examples include letters, figures, symbols, patterns, and the like.

[0051] It is preferable that the print layer is formed on the back surface of the base layer 58 rather than on the outermost surface, since this can prevent damage to the design layer due to external impact.

[0052] The printing layer may be an ink composition obtained by adding one or more of ordinary ink vehicles as the main component, optionally containing one or more of plasticizers, stabilizers, antioxidants, light stabilizers, ultraviolet absorbers, curing agents, crosslinking agents, lubricants, antistatic agents, fillers, and other additives as necessary, and further adding colorants such as dyes and pigments, and thoroughly kneading the mixture with a solvent, diluent, etc. to prepare an ink composition. Examples of such ink vehicles include linseed oil, tung oil, soybean oil, hydrocarbon oil, rosin, rosin ester, rosin modified resin, shellac, alkyd resin, phenolic resin, maleic acid resin, natural resin, hydrocarbon resin, polyvinyl chloride resin, polyacetic acid resin, polystyrene resin, polyvinyl butyral resin, acrylic or methacrylic resin, polyamide resin, polyester resin, polyurethane resin, epoxy resin, urea resin, melamine resin, aminoalkyd resin, nitrocellulose, ethyl cellulose, chlorinated rubber, cyclized rubber, and others, and one or more of these may be used in combination.

[0053] The laminate sheet 55 of the cylindrical body further has a gas barrier layer 53 disposed between the third sealant layer 60 and the fourth sealant layer 61, and this gas barrier layer 53 can be a metal foil or a layer having a base film and a vapor-deposited film vapor-deposited on the base film.

[0054] The gas barrier layer 53 is a layer for suppressing the permeation of oxygen gas, water vapor, etc. In addition, a material having not only a gas barrier property against oxygen gas, water vapor, etc. but also a property of retaining aroma of the contents can be used.

[0055] Specifically, the gas barrier layer 53 is a barrier layer containing a metal element or an inorganic oxide, and may be, for example, one or more selected from the group consisting of aluminum foil, aluminum vapor deposition film, aluminum oxide vapor deposition film, and silicon oxide vapor deposition film. Among these, aluminum foil is preferred from the viewpoint of aroma retention.

[0056] As the base film on which the vapor deposition film is provided, films or sheets of various resins such as polyethylene resins, polypropylene resins, cyclic polyolefin resins, fluorine resins, polystyrene resins, acrylonitrile-styrene copolymers (AS resins), acrylonitrile-butadiene-styrene copolymers (ABS resins), polyvinyl chloride resins, fluorine resins, poly(meth)acrylic resins, polycarbonate resins, polyester resins such as polyethylene terephthalate and polyethylene naphthalate, polyamide resins such as various nylons, polyimide resins, polyamideimide resins, polyarylphthalate resins, silicone resins, polysulfone resins, polyphenylene sulfide resins, polyethersulfone resins, polyurethane resins, acetal resins, cellulose resins, and others can be used. Among these, polyethylene terephthalate (PET) is preferred in terms of adhesive strength with the vapor deposition film, aroma retention, and resistance to contents.

[0057] In this embodiment, the thickness of the film supporting the gas barrier layer 53 is preferably 6 μm or more and 25 μm or less, and more preferably 10 μm or more and 20 μm or less.

[0058] Furthermore, the resin film supporting the gas barrier layer 53 may be subjected to an adhesion enhancing treatment such as corona discharge treatment, ozone treatment, or plasma treatment on a necessary surface, if necessary.

[0059] The resin film supporting the gas barrier layer 53 preferably has an anchor coating agent layer on the surface that is bonded to the gas barrier layer 53. By having the anchor coating agent layer, the adhesion to the gas barrier layer 53 and the resistance to contents are further improved.

[0060] The anchor coating agent layer is a layer formed by applying and drying an anchor coating agent. Examples of the anchor coating agent that can be used include an isocyanate-based anchor coating agent, an organic titanium-based anchor coating agent, a polybutadiene-based anchor coating agent, and a polyethyleneimine-based anchor coating agent.

[0061] The amount of anchor coating agent applied after drying is 0.05g / m 2 More than 0.5g / m 2 It is preferable that the thickness is 0.05 μm or less, or 0.05 μm or more and 0.5 μm or less.

[0062] In the above, in order to obtain sufficient barrier properties, the thickness of the vapor-deposited layer is preferably from 5 to 300 nm, more preferably from 10 to 200 nm, and even more preferably from 10 to 100 nm. More specifically, in the above PVD method, the thickness of the vapor-deposited layer made of aluminum oxide is preferably 20 to 100 nm, and more preferably about 30 to 50 nm. In the above CVD method, the thickness of the vapor-deposited layer made of silicon oxide is preferably 5 to 50 nm, and more preferably 10 to 30 nm. In the above, in the case of a vapor-deposited layer made of a metal oxide or an inorganic oxide, if the thickness of the vapor-deposited layer exceeds 200 nm, cracks or the like are likely to occur in the vapor-deposited layer, and there is a risk that the barrier properties will decrease due to warping, and there are problems such as high material costs, which are undesirable. Also, if the thickness is less than 10 nm, it is undesirable because it becomes difficult to achieve oxygen barrier properties.

[0063] Adhesive layers such as the first adhesive layer 57a, the second adhesive layer 57b, the third adhesive layer 57c, and the fourth adhesive layer 57e are layers for adhering the first sealant layer 56, the base layer 58, the gas barrier layer 53, the second sealant layer 59, the third sealant layer 60, the fourth sealant layer 61, etc. These adhesive layers can be appropriately selected depending on the resin that constitutes the layers to be adhered.

[0064] As the adhesive layer, for example, anchor coating agents such as isocyanate-based (urethane-based), polyethyleneimine-based, polybutadiene-based, and organic titanium-based, or anchor coating agents such as polyurethane-based, polyacrylic-based, polyester-based, epoxy-based, polyvinyl acetate-based, cellulose-based, and other laminating adhesives, laminating adhesives, etc. can be used as desired.

[0065] As the adhesive layer, for example, polyethylene, polypropylene, linear low-density polyethylene, ethylene-vinyl alcohol, ethylene-methacrylic acid copolymer, ethylene-acrylic acid copolymer, ionomer, maleic anhydride modified polyolefin resin, etc. can be suitably used.

[0066] In this embodiment, the thickness of the adhesive layer is preferably 3 μm or more and 60 μm or less.

[0067] The adhesive strength of the adhesive layer (strong seal portion) is preferably 3.0 N / 15 mm or more and 10.0 N / 15 mm or less, and more preferably 5.0 N / 15 mm or more and 8.0 N / 15 mm or less.

[0068] The method for laminating the first sealant layer 56, the base layer 58, the second sealant layer 59, etc., which are the outer layers, and the method for laminating the third sealant layer 60, the gas barrier layer 53, the fourth sealant layer 61, which are the inner layers, can be, for example, wet lamination, dry lamination, solventless dry lamination, extrusion lamination, T-die coextrusion molding, coextrusion lamination molding, inflation molding, or any other method. When carrying out the above-mentioned lamination, if necessary, the film can be subjected to pretreatment such as corona treatment or ozone treatment.

[0069] Furthermore, the laminate sheet 55 of the cylindrical body may have an intermediate layer between the base layer 58 and the second sealant layer 59, if necessary. The intermediate layer is provided to adjust the thickness of the laminate sheet of the cylindrical body. An olefin resin may be used for the intermediate layer. More specifically, it is preferable to use a polyethylene film such as low density polyethylene, linear low density polyethylene, or medium density polyethylene as the intermediate layer. The thickness of the intermediate layer is preferably, for example, 50 μm to 200 μm.

[0070] Next, the head member 40 of the tube container 10 will be described.

[0071] The head member 40 has a mouth portion 11 and a shoulder portion 12 provided below the mouth portion 11 .

[0072] The mouth portion 11 has a threaded portion onto which a cap 20 is screwed. In addition, a check valve is provided inside the mouth portion 11. The check valve is disposed to prevent outside air from flowing into the tube container.

[0073] Additionally, shoulder portion 12 has a shape in which the diameter gradually increases from the mouth portion 11 side toward the body portion 50 side. This shoulder portion 12 has a circular shape in horizontal cross section.

[0074] The head member 40 is made of a resin material such as high density polyethylene (HDPE). In addition to the high density polyethylene, an ethylene-α-olefin copolymer polymerized using a metallocene catalyst may also be used as the head member 40 of the tube container 10.

[0075] Next, the check valve will be described.

[0076] As shown in Fig. 3, the check valve 13 can be disposed on the upper end surface of the mouth of the tube. The check valve 13 may be a separate member, not integral with the mouth, as long as it is disposed to prevent outside air from entering the tube container.

[0077] The check valve 13 can be formed by punching into any desired shape, such as a cross, a *, or a star.

[0078] When a tube container with a check valve is pressed with a finger, the inside of the tube container is pressurized, the check valve opens, and the contents can be pushed out. On the other hand, when the pressure inside the tube container with a check valve is reduced, the check valve closes, isolating the container from the outside, and prevents outside air from being drawn in (creasing an airbag), allowing the valve to be opened and closed reliably.

[0079] There are no particular limitations on the sheet for forming the check valve 13, so long as it can be heat-sealed to the material used for the mouth. If the material cannot be heat-sealed to the material used for the mouth, a heat-sealable material may be laminated thereon, or the material may be bonded via an adhesive.

[0080] It is more preferable that the sheet forming the check valve 13 has a certain degree of rigidity, is not affected by the contents, and can be bonded to the upper end surface of the mouth of the tube container by heat sealing or adhesive. The sheet forming the check valve 13 can be, for example, a single layer or a laminate of oriented or unoriented films such as polyester, polycarbonate, polypropylene, polyethylene, and polyamide.

[0081] The thickness of the check valve 13 is preferably, for example, not less than 15 μm and not more than 200 μm.

[0082] Next, the cylindrical body 50 will be described. The body 50 of the tube container 10 shown in Fig. 3 has a generally cylindrical shape. This body 50 is composed of a laminated laminate sheet 55 (see Figs. 1 and 2), and is obtained by rolling this laminate sheet 55 into a cylindrical shape, overlapping opposing ends, and joining them together by, for example, heat sealing. Therefore, the body 50 has side seal parts 18 in which the laminate sheets are joined together along the longitudinal direction.

[0083] The thickness of the body 50 is preferably, for example, 100 μm or more and 210 μm or less for each of the outer layer and the inner layer. A thickness of 100 μm or more allows the body of the tube container 10 to maintain a predetermined strength. This allows the shape retention of the tube container 10 to be maintained. Furthermore, a thickness of 210 μm or less allows the manufacturing cost of the laminate sheet 55 of the cylindrical body to be reduced, and also ensures moldability when the head member is molded by compression molding.

[0084] Examples of the heat sealing (welding) method used in producing the cylindrical body of the tube container 10 include bar sealing, rotary roll sealing, belt sealing, impulse sealing, high frequency sealing, ultrasonic sealing, and flame sealing.

[0085] In addition, the head member 40 and the cylindrical body portion 50 of the tube container 10 according to the present embodiment are joined by thermal welding when the head member 40 is molded by compression molding. However, the present invention is not limited to this, and the head member and the cylindrical body portion of the tube container 10 may be joined by injection molding.

[0086] Next, a method for producing the above-mentioned tube container 10 by using a compression molding method will be described with reference to FIG.

[0087] 6(a), this cylindrical body portion (body portion 50) is inserted into a mandrel 72, and a die 71 for compression molding the head member 40 is attached to one end of the mandrel 72. That is, the cylindrical body portion (body portion 50), which has been molded into a cylindrical shape in advance, is inserted into the mandrel 72, whose tip portion serves as a core for compression molding the head member 40, and is then advanced to a predetermined position into the cavity of the die 71 for molding the head member 40.

[0088] Next, molten resin is supplied from a resin supply device into the metal mold 71 to compression mold the head member 40. In this case, the opening of one end of the body portion 50 is inserted into the metal mold 71 to mold the head member 40, and at the same time, the cylindrical body portion 50 is fused integrally to the head member 40. Thereafter, the integrated head member 40 and body portion 50 are removed from the metal mold 71 and mandrel 72 to obtain a tube container 10 as shown in Fig. 6(b).

[0089] Furthermore, the cap 20 is produced by injection molding using an injection molding machine (not shown). Then, the cap 20 is screwed onto the mouth of the head member 40 of the tube container 10, thereby obtaining the tube container 10.

[0090] In the present disclosure, the tube container 10 manufactured as described above can be filled with the contents to be packed through the opening at the lower end, and then the opening can be heat-sealed to form a bottom weld, thereby producing a tube package (packaged product).

[0091] In the above, examples of the contents to be filled and packaged include toothpaste, cosmetics, hair dye, glue, mustard greens, wasabi paste, cream, paint, ointment, medicines, and the like.

[0092] When the tube container 10 is filled with the contents C, as the contents C are pushed out from the mouth 11, the force of the pushing causes the check valve 13 to rise, and the contents C are pushed out from the tip of the mouth 11. When the pushing out of the contents C is stopped, the check valve 13 is pulled downward, sealing the mouth 11. By moving up and down in this manner, it is possible to reliably prevent the intake of outside air.

[0093] Furthermore, when the extrusion of the content C of this tube container 10 is stopped, the check valve 13 seals the tip of the mouth 11, creating a reduced pressure state inside the inner layer 2 of the tube container, which causes the inner layer 2 to deform. At this time, the outer layer 1 of the tube container also tries to deform, but the outer layer 1 and the inner layer 2 peel off from each other, creating a gap between them, and when the gap becomes reduced pressure, it sucks in outside air through the hole 15, allowing it to return to its original state.

[0094] Next, a specific example of the above embodiment will be described.

[0095] Example 1 First, a linear low-density polyethylene resin was melted using an extruder, and then the molten resin extruded in a tubular shape from the extruder was drawn vertically using a downward inflation device while being inflated with air pressure to form a cylindrical film, which was then flattened by sandwiching it between rolls while being cooled with water to form a hollow film having a thickness of 80 μm and a weak seal portion 57d. Next, both longitudinal side edges of the flat hollow film were cut off by a predetermined width to produce a second sealant layer 59 and a third sealant layer 60.

[0096] Next, a beautiful pattern print layer was formed on the back side of the base layer, a biaxially oriented polyethylene terephthalate film (thickness 12 μm), using polyurethane gravure ink.

[0097] Next, a polyurethane adhesive for dry lamination (a two-component curing urethane adhesive with a polyester resin as the main agent and an aliphatic polyisocyanate as the curing agent) was applied at a rate of 4 g / m2 to the surface of the biaxially oriented polyethylene terephthalate film by roll coating. 2 After coating and drying, the laminate was laminated on one side of the second sealant layer 59 and heat sealed.

[0098] Next, 4 g / m of a polyurethane adhesive for dry lamination was applied to the surface of the base layer side of the laminated film obtained above. 2 After coating and drying, a linear low density polyethylene (LLDPE) film having a thickness of 130 μm was laminated for the first sealant to obtain a base sheet for the outer layer 1.

[0099] On the other hand, a polyurethane adhesive for dry lamination (a two-component curing urethane adhesive of base material: polyester resin, curing agent: aliphatic polyisocyanate) was applied at a rate of 4 g / m2 to the surface of the third sealant layer 60 by roll coating. 2 After coating and drying, a 7 μm thick aluminum foil was laminated as a gas barrier layer 53 by dry lamination.

[0100] Next, 4 g / m of a polyurethane adhesive for dry lamination was applied to the surface of the gas barrier layer 53 side of the laminated film obtained above. 2 After coating and drying, a linear low density polyethylene (LLDPE) film having a thickness of 130 μm was laminated for a fourth sealant to obtain a base sheet for the inner layer 2.

[0101] Next, holes 15 were formed at predetermined positions in the original sheet of outer layer 1. Holes 15 were formed by a carbon dioxide laser. The layer structure was as follows.

[0102] (Outer layer) 1st sealant LLDPE film (130 μm) / Adhesive layer DL adhesive / Base layer biaxially oriented polyethylene terephthalate film (12 μm) / Picture print layer / Adhesive layer DL adhesive / 2nd sealant layer LLDPE film (80 μm)

[0103] (Inner layer) 3rd sealant layer LLDPE film (80μm) / gas barrier layer aluminum foil 7μm / 4th sealant layer LLDPE film (130μm)

[0104] Using the laminate sheet 55 for the cylindrical body obtained above, one side edge and the other side edge were overlapped using a mandrel to form a cylindrical shape, and the back layer and front layer of the laminate at the overlapping portion were welded by a thermal welding method to obtain a cylindrical molded body.

[0105] Subsequently, a head member with a check valve was integrally molded with this cylindrical molded body by insert injection molding to obtain a tube container 10 according to Example 1 of the present disclosure. High density polyethylene (HDPE) was used as the material for the head member.

[0106] In this manner, the tube container 10 was produced.

[0107] In parallel with the production of the tube container 10, the cap 20 was produced by injection molding. The obtained cap 20 was then screwed onto the mouth of the head member 40 of the tube container, thereby producing the tube container 10 with the cap.

[0108] The tube container 10A filled with the contents does not have an outer layer and an inner layer peeled off during processing of the laminate sheet 55 of the cylindrical body, and when used as the inner layer of the tube container, the outer layer and the inner layer can be easily peeled off from each other when the contents are pushed out, eliminating the need for a manufacturing step of inserting a cylindrical inner layer into a cylindrical outer layer, and the tube container 10A can be manufactured at high productivity and low cost.

[0109] In addition, when the contents are pushed out of the mouth of the tube container 10A filled with the contents, the force of the pushing causes the check valve to rise, and the contents are pushed out from the tip of the mouth. When the pushing of the contents is stopped, the check valve is pulled downward, sealing the mouth. By moving up and down in this way, it is possible to reliably prevent the intake of outside air.

[0110] When the extrusion of the contents from the tube container 10A filled with the contents was stopped, the check valve sealed the tip of the mouth, reducing the pressure inside the inner layer of the tube container and causing the inner layer to deform. At this time, the outer layer of the tube container also tried to deform, but the outer layer and the inner layer peeled off, creating a gap between them, and when the gap was reduced in pressure, it sucked in outside air through the hole 15 and restored the container to its original state.

[0111] [Heat seal strength] The laminate for tube containers in the example obtained above was cut into strips of 15 mm x 100 mm, and the heat seal strength between the outer layer 1 and the inner layer 2 was measured using a tensile tester. The peel speed was 50 mm / min, the load cell was 100 N, and the measurement was performed three times. As a result, the heat seal strength was 1.4 N.

[0112] [Resistance to contents] The tube container of the embodiment obtained above was filled with 130g of toothpaste as the content, and stored for 3 months under the conditions of 40°C and 90% RH. The tube container after storage was then disassembled to prepare test pieces for measuring the laminate strength, and the laminate strength between the gas barrier layer and the base layer, or between the gas barrier layer and the second sealant layer, was measured. As a result, both were not peelable, and the laminate for the tube container of the embodiment showed good laminate strength after storage for evaluating the resistance to contents. [Explanation of symbols]

[0113] 1 outer layer 2. Inner layer 10 Tube container 10A Tube container filled with contents 11 Mouth 12 Shoulder 13. Check valve 15 holes 16 Opening 17 Bottom seal 18 Side seal part 20 Cap 40 Head Component 50 Torso 53 Gas barrier layer 55 Laminate for tube containers (laminate sheet for cylindrical body) 56 First sealant layer 57a First adhesive layer (strong seal part) 57b Second adhesive layer (strong seal part) 57c Third adhesive layer (strong seal area) 57d Weak seal part 57e 4th adhesive layer (strong seal part) 58 Base material layer 59 Second sealant layer 60 3rd sealant layer 61 4th sealant layer 71 Mold 72 Mandrel 100 Extruder 101 Inflation Die 103 Air supply pipe 105 Air cooling air ring 106 Guide roller 107 Stabilizer 108 Pinch Roll 110 Winding device 120 Molten resin extruded into a hollow shape 121 Winding roll (hollow film)

Claims

1. A laminate constituting a body of a tube container, The laminate includes an outer layer and an inner layer arranged in this order from the outer surface to the inner surface, A weak seal portion is provided between the outer layer and the inner layer, the outer layer includes a first sealant layer, a substrate layer, and a second sealant layer; the inner layer includes a third sealant layer; At least a portion of the outer layer has holes, a cylindrical body member in which opposing ends of the laminate for a tube container are overlapped and joined to each other, the interlayer seal strength between the second sealant layer and the third sealant layer being 0.1 N / 15 mm or more and 2 N / 15 mm or less; a head member joined to one end of the cylindrical body member, the head member includes a shoulder portion and a mouth portion; A tube container characterized in that the mouth portion is provided with a check valve.

2. 2. The tube container according to claim 1, wherein the inner layer further comprises a gas barrier layer.

3. A method for manufacturing a laminate constituting a body of a tube container, comprising the steps of: The laminate includes an outer layer and an inner layer arranged in this order from the outer surface to the inner surface, A weak seal portion is provided between the outer layer and the inner layer, the outer layer includes a first sealant layer, a substrate layer, and a second sealant layer; the inner layer includes a third sealant layer; At least a portion of the outer layer has holes, The seal strength between the second sealant layer and the third sealant layer is 0.1 N / 15 mm or more and 2 N / 15 mm or less; A step of producing a hollow film by an inflation molding method; a step of flattening the hollow film after inflation molding and weakly sealing the inner surfaces of the film; a step of cutting off both side edges of the flat hollow film in a longitudinal direction by a predetermined width to produce the second sealant layer and the third sealant layer; a winding step of winding up the second sealant layer and the third sealant layer; laminating the base layer and the first sealant layer on the second sealant layer side of the second sealant layer and the third sealant layer unwound from the winding; A method for producing a laminate for a tube container, comprising:

Citation Information

Patent Citations

  • Laminated sheet for forming body part of tube container

    JP1993220900A

  • Blown tube container

    JP1997002497A