Method for evaluating surface defects in steel bars
The method evaluates steel bar flaws by analyzing detection data to identify their characteristics, optimizing manufacturing conditions, and improving yield by distinguishing between different flaw types, addressing the limitations of conventional detection methods.
Patent Information
- Application Number
- JP2022057151
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-03-30
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2042-03-30
AI Technical Summary
Conventional flaw detection methods for steel bars accurately detect the presence or absence of surface flaws but fail to evaluate the nature or characteristics of these flaws, which affects the direction of optimizing manufacturing conditions to reduce flaws.
A method that evaluates the properties of surface flaws in steel bars by analyzing flaw detection data, using predefined correlations between data patterns and flaw characteristics, and converting the data into a flaw density index to distinguish between different types of flaws.
Enables automatic identification of flaw characteristics without visual inspection, optimizing manufacturing conditions to improve yield by distinguishing between different types of flaws, such as longitudinal and single flaws, thereby reducing defects and improving production efficiency.
Smart Images

Figure 0007559795000005 
Figure 0007559795000006 
Figure 0007559795000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a technique for evaluating the properties of surface defects occurring on a steel bar. [Background technology]
[0002] Conventionally, inspection of surface defects in steel bar products has been carried out by moving a flaw detector, such as a magnetic leakage flux detector or an eddy current detector, along the surface of the steel bar to inspect the entire surface, as described in Patent Document 1. Then, defects of a predetermined level or more are considered defects that should be detected, and an evaluation is made as to whether or not the product has defects of a predetermined level or more. At this time, there is a technique for detecting minute defects with high accuracy, as disclosed in Patent Document 2. Furthermore, when the entire circumference of a steel bar is to be inspected, as in Patent Document 3, the flaw detector is moved relatively in the circumferential direction of the steel bar as well as in the longitudinal direction to scan the entire surface of the steel bar and determine whether or not there are defects of a specified size or larger on the surface of the steel bar. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2001-41932 A [Patent Document 2] JP 2009-68857 A [Patent Document 3] JP 2017-167057 A Summary of the Invention [Problem to be solved by the invention]
[0004] Conventional methods for detecting flaws in steel bars aim to accurately detect whether or not there are flaws of a specified magnitude on the surface of the steel bar, and are not intended to evaluate the properties (condition) of the surface flaws. However, measures to suppress defects on the surface of steel bars in future steel bar production may differ depending on the nature of the defects that occur.
[0005] In considering improvement measures, conventionally, apart from detecting the presence or absence of defects of a specified magnitude or more as described above, workers would actually visually check the condition (properties) of the defects on the surface of the steel bar having the defects, and depending on the condition of the defects confirmed, would decide on measures to suppress the occurrence of those defects in future steel bar production. As described above, conventional flaw detection methods aim to detect flaws without exception in order to determine whether or not the current steel bar is acceptable as a product, and are not intended to evaluate the nature of flaws in order to take measures on the production line.
[0006] The present invention has been made in consideration of the above points, and aims to make it possible to evaluate the properties of defects occurring in a steel bar from a plurality of pieces of inspection data obtained by inspecting the surface of the steel bar. That is, the present invention aims to provide a technology that can automatically distinguish the properties of defects from the inspection data. [Means for solving the problem]
[0007] In order to solve the problem, one aspect of the present invention is a surface defect evaluation method for evaluating the properties of surface defects in a steel bar, which involves determining in advance a correlation between the properties of the surface defects in the steel bar and the characteristics of a data pattern obtained by performing inspection along the surface of the steel bar, and identifying the properties of the surface defects in the steel bar to be evaluated from the correlation and the characteristics of the data pattern obtained by performing the inspection on the steel bar to be evaluated, which is the steel bar to be evaluated for the properties of its surface defects. Effect of the Invention
[0008] Depending on the nature (state) of the defects that occur on the surface, the direction in which the operating conditions for steel bar manufacturing should be optimized to reduce defects varies. In contrast, according to the aspect of the present invention, the characteristics of the surface defects that have actually occurred are evaluated from the flaw detection data without being evaluated visually, which makes it easy to identify (evaluate) which type of flaw has occurred in which steel bar product. As a result, according to the present invention, the optimum process for each product is performed to prevent defects. Manufacturing conditions This makes it easier to check the quality, leading to improved yields. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a conceptual diagram showing an example of equipment for flaw evaluation according to an embodiment of the present invention. [Diagram 2] 1A to 1C are diagrams illustrating two examples of flaw detection charts and an example of detecting the presence or absence of flaws using the flaw detection charts. [Diagram 3] 13 is a diagram showing the relationship between a first section D1 and a second section D2. FIG. [Figure 4] FIG. 1 is a diagram for explaining indexing of features of a flaw detection chart (data pattern). [Diagram 5] FIG. 1 shows examples of the nature of defects, where (a) is a longitudinal defect 1, (b) is a longitudinal defect 2, and (c) is an example of a single defect. [Figure 6] FIG. 1 shows examples of the characteristics (features) of the inspection chart (data pattern) for each type of defect and the corresponding defect density index, where (a) is an example for longitudinal defect 1, (b) is an example for longitudinal defect 2, and (c) is an example for a single defect. [Figure 7] FIG. 10 is a diagram for explaining the characteristics of each flaw in the flaw inspection chart, where (a) is an example of a longitudinal flaw 1, (b) is an example of a longitudinal flaw 2, and (c) is an example of a single flaw. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment based on the present invention will be described with reference to the drawings. (composition) The steel bars are manufactured in a steel bar factory equipped with, for example, a heating furnace, a roughing mill, an intermediate rolling mill, and a finishing rolling mill. The surface quality of the manufactured steel bars is evaluated, for example, by a magnetic leakage flux flaw detector in a finishing factory. The flaw detection facility of this embodiment includes a flaw detection device and a flaw detection control unit 3, as shown in FIG.
[0011] <Flaw detection equipment> As shown in Figure 1, the flaw detection device uses a flaw detector 2 placed close to the surface of the steel bar 1 to scan the surface of the steel bar 1 to be inspected in the circumferential and longitudinal directions (axial direction), continuously detecting flaws around the entire surface of the steel bar 1. As for the flaw detector 2 and the method of flaw detection using the flaw detector 2, it is sufficient to adopt a conventionally known configuration of the flaw detector 2 and a conventionally known flaw detection method, and there are no particular limitations on the configuration of the flaw detector 2 and the flaw detection method. The flaw detector of this embodiment includes a flaw detector 2, such as a magnetic leakage flux flaw detector or an eddy current flaw detector. The flaw detector 2 detects flaws in the entire surface of the steel bar 1 to be inspected.
[0012] <Flaw detection control section 3> As shown in FIG. 1, the flaw detection control unit 3 includes a flaw detection data generating unit 3A, a flaw determining unit 3B, and a flaw properties evaluating unit 3C.
[0013] <Flaw detection data generation unit 3A> The flaw detection data generating unit 3A continuously acquires detection signals from the flaw detector 2 at a preset sampling period in synchronization with the relative movement of the flaw detector 2 with respect to the surface of the steel bar 1, and continuously obtains maximum output information for each predetermined scan interval (first section D1) based on the acquired detection signals, and stores the information sequentially in a storage unit such as a database. The above detection signals are acquired, for example, for the entire surface of the steel bar 1 to be inspected. The interval between the first sections D1 is determined in advance based on the dimensions of the surface flaw to be measured. The interval between the first sections D1 can be, for example, 30 mm.
[0014] By the processing of this flaw detection data generating unit 3A, continuous flaw detection data (detection information) is acquired along the scanning direction (flaw detection direction). The continuous flaw detection data is composed of discrete values at preset scanning interval units. Hereinafter, a collection of flaw detection data continuously acquired along the surface of the steel bar 1 will be referred to as a flaw detection chart 10. The flaw detection chart 10 can be expressed, for example, as shown in Fig. 2. Fig. 2 illustrates two types of flaw detection charts 10, in which the horizontal axis indicates the scanning direction (flaw detection direction) and the vertical axis indicates the maximum output value of the detection signal for each predetermined scanning interval (first section D1).
[0015] <Flaw determination section 3B> The flaw determination unit 3B determines whether or not the flaw exceeds a first threshold value TH1 set as a threshold value for determining whether the product is acceptable, as shown in Fig. 2, based on the flaw detection chart 10 consisting of a sequence of multiple flaw detection data acquired by the flaw detection data generation unit 3A. The first threshold value TH1 is determined in advance as a threshold value that makes it possible to determine whether the product is acceptable, based on the acquired flaw detection data of the steel bar 1 and the state of surface flaws in the steel bar product.
[0016] The flaw determination unit 3B, for example, determines whether the detected output value for each piece of flaw detection data in the flaw detection chart 10 is equal to or less than the first threshold value TH1. When the flaw determination unit 3B detects flaw detection data determined to exceed the first threshold value TH1, it determines that the area including the flaw detection data contains a flaw that will cause the product to fail, and outputs the information. The examples shown in (a) and (b) of FIG. 2 illustrate a case where there is a flaw that will cause the product to fail. This determines whether the inspected steel bar 1 is acceptable as a product.
[0017] <Defect Characteristics Evaluation Section 3C> The defect characteristics evaluation unit 3C evaluates the characteristics of the surface defects occurring on the steel bar 1 being inspected based on the characteristics of a data pattern (data chart) that is set based on an arrangement of multiple inspection data along the surface of the steel bar 1 obtained by inspection. Here, the steel bar that is the subject of evaluation for evaluating the properties of the surface defects is the steel bar to be evaluated.
[0018] For this evaluation, for example, the correlation between the properties of the surface flaws of the steel bar 1 and the data pattern is obtained in advance, and identification data for identifying the properties of the surface flaws is obtained from the correlation.The properties of the surface flaws of the steel bar 1 are then evaluated from the characteristics of the obtained data pattern with reference to the previously obtained identification data. For example, the identification data is compared with the characteristics of the acquired data pattern to identify the nature of the surface flaws of the steel bar 1. In this embodiment, the plurality of flaw detection data constituting the data pattern are data obtained by detecting flaws on the entire surface of the steel bar 1.
[0019] Next, a first method of evaluation processing in the flaw property evaluation unit 3C in this embodiment will be described. In the first method, for the flaw inspection chart 10 consisting of a collection of flaw inspection data continuously acquired along the surface of the steel bar 1 generated by the flaw inspection data generating unit 3A, as shown in FIG. 3, it is judged whether or not the second threshold value TH2 is exceeded for each first section D1 (predetermined scan interval). That is, it is judged whether each flaw inspection data is equal to or less than the second threshold value TH2, and if it is not satisfied, it is determined that the first section D1 has a surface defect. Hereinafter, the surface defect is also referred to as a detected defect. Also, the number of detected defects is referred to as the number of detected defects.
[0020] Furthermore, in the first method, the surface of the steel bar 1 is divided into second sections D2 larger than the first sections D1 along the surface of the steel bar 1 as shown in Figures 3 and 4. In this embodiment (Figures 3 and 4), the division direction of the second sections D2 is the same as the inspection direction. In the first method, the flaw property evaluation unit 3C first obtains the number of first sections that are present in each second section D2 and are equal to or greater than the second threshold value TH2, as shown in Fig. 4, for each second section D2, and expresses the flaw detection data as the number of first sections that are present in each second section D2 and are equal to or greater than the second threshold value TH2 (the number of detected flaws). That is, the flaw detection data consisting of flaw outputs is grouped, and the flaw detection data is converted into a format that expresses the number of detected flaws consisting of the number of sections that are present in each second section D2 and are equal to or greater than the second threshold value TH2.
[0021] In this embodiment, for example, the length (size) of the second section D2 is an integer multiple of the first section D1. In this embodiment, as shown in Fig. 3, the length (size) of the second section D2 is 10 times the length (size) of the first section D1. In this case, the number of detected defects is in the range of 0 to 10. It is preferable to set the second sections D2 so that each first section D1 is exclusively included in one of the second sections D2.
[0022] Next, the flaw property evaluation unit 3C extracts second sections with one or more detected flaws, and for the extracted second sections, calculates an index by taking the average number of detected flaws per second section, and uses the index as a feature for identifying the properties of the surface flaws of the steel bar 1. Note that if there is no flaw inspection data with one or more detected flaws, the index is set to zero. In this specification, the above index is referred to as a flaw density index. In the case of the flaw inspection chart 10 shown in FIG. 4, the flaw density index is 6.0. Then, the flaw property evaluation unit 3C evaluates the property of the flaw generated in the steel bar 1 to be inspected based on the determined flaw concentration index value. For example, a correlation between the nature of a flaw and the value of the flaw density index is obtained using flaw detection data from a past flaw detection inspection, and the nature of the flaw is identified by the obtained flaw density index.
[0023] [Second threshold TH2] Here, the second threshold value TH2 is determined in advance as a threshold value that enables more meaningful determination of inspection data (number of detected defects) for classifying the characteristics of defects, for example, from the correlation between the characteristics of the surface defects of the steel bar 1 previously obtained and the characteristics of the data pattern. Alternatively, the second threshold value TH2 is determined according to the first threshold value TH1. For example, when the number of rejected steel bars 1 is small, the second threshold value TH2 is set to a value lower than the first threshold value TH1. When the number of rejected steel bars 1 is large, the second threshold value TH2 is set to the value of the first threshold value TH1.
[0024] [Range of indicators for identifying defects] The nature of defects on the surface of the steel bar 1 can be of various types, for example, as shown in FIG. 5, and the seriousness of the defect and the cause of its occurrence during manufacturing vary depending on the type of defect.
[0025] Fig. 5(a) shows an example in which multiple longitudinal defects have occurred along the entire circumference of the surface of a steel bar 1. In the following description, such defects are referred to as longitudinal defects 1. When the defects are longitudinal defects 1, the grinding load is extremely high. 5(b) shows an example in which multiple longitudinal flaws have occurred in a partial area of the surface of the steel bar 1. In the following description, such flaws are referred to as longitudinal flaws 2. When the flaws are longitudinal flaws 2, the grinding load is high. In the following description, longitudinal flaw 1 and longitudinal flaw 2 will be collectively referred to as longitudinal flaw. Fig. 5(c) shows an example of a single defect such as a crack or a chip. In the following description, such a defect is called a single defect. When the defect is a single defect, the grinding load is low.
[0026] When the defect type is longitudinal flaw 1 or longitudinal flaw 2, grinding is required over a wider area than when the defect type is a single flaw, which may result in the product falling short of the dimensional tolerance and being rejected, leading to a decrease in yield. Also, measures to suppress longitudinal flaws are different from measures to suppress single flaws.
[0027] FIG. 6 shows 10 examples of flaw detection charts for the following types of flaws: longitudinal flaw 1 (FIG. 6(a)), longitudinal flaw 2 (FIG. 6(b)), and single flaw (FIG. 6(c)), along with examples of longitudinal flaws in each case. As shown in Figure 6, longitudinal defects are significantly larger than single defects. FIG. 7 shows other examples of the flaw detection chart 10 when the flaw characteristics are longitudinal flaw 1 (FIG. 7(a)), longitudinal flaw 2 (FIG. 7(b)), and single flaw (FIG. 7(c)). As shown in Fig. 7(a), in the case of longitudinal flaw 1, the flaw output value is expressed as a high value overall. Also, as shown in Fig. 7(b), in the case of longitudinal flaw 2, the flaw output value is expressed as a high value in a partial region. On the other hand, as shown in Fig. 7(c), a single flaw is expressed as a single high flaw output value.
[0028] Thus, the inventors have considered that the characteristics of the flaws are correlated with the characteristics (the chart pattern) of the flaw detection chart 10. The inventors have then considered expressing this correlation as an index. Then, we took statistics and evaluated the flaw detection charts 10 and the characteristics of the flaws at that time for a large number of steel bars 1 in the past. Table 1 shows the results when the defect type is longitudinal defect 1.
[0029] [Table 1]
[0030] Table 2 shows the results when the defect type is longitudinal defect 2.
[0031] [Table 2]
[0032] Table 3 shows the results when the defect type is a single defect.
[0033] [Table 3]
[0034] Tables 1 to 3 show the maximum and average values of data obtained for the flaw detection chart 10 of the flaw detection data consisting of flaw output values. As can be seen from Tables 1 to 3, the maximum value of the flaw does not allow the properties of the flaw to be evaluated significantly. On the other hand, it was found that when the average value or the average value + σ of the output values of the flaw detection chart 10 is used as an index, the properties of the flaw can be evaluated with the average value or the average value + σ. Note that the present disclosure also includes the case where the properties of the flaw are evaluated with the average value or the average value + σ of the data obtained from the flaw detection chart 10 itself as an index. However, in the example of the flaw characteristics shown in Table 4, when the above-mentioned "average value + σ" was used as the index, as shown in Table 4, it was not possible to distinguish between longitudinal flaws and single flaws.
[0035] [Table 4]
[0036] Therefore, in this embodiment, in order to improve the accuracy of distinction, as shown in Figures 3 and 4, each piece of inspection data of the inspection chart 10 is grouped in units of second sections D2 wider than the first sections D1, and the average value of the number of flaws present in each second section D2 is taken as the flaw concentration index as described above. However, only for the second sections D2 that have flaws, the average value of the number of flaws is taken as an index (feature value) expressing the characteristics of the property (pattern) of the inspection chart 10. It was found that by using this flaw density index, it is possible to more clearly distinguish between longitudinal flaws and single flaws, as shown in Figure 6 and Table 4.
[0037] In this embodiment, the range of the index is a defect density index. 3 A flaw was evaluated as a longitudinal flaw when the flaw density index was 10 or less. A flaw density index of less than 3 (greater than 0) was evaluated as a single flaw.
[0038] (Operation etc.) In this embodiment, flaws are detected along the surface of a steel bar 1 by a flaw detector 2 of the flaw detection device. Using the flaw detection chart 10 obtained by the flaw detection and a preset first threshold value TH1, it is determined whether or not there is a flaw that would cause the product to be unacceptable (see FIG. 2). Note that the first threshold value TH1 is set to a different value depending on the quality required for each product.
[0039] Furthermore, in this embodiment, the properties of the flaws occurring in the steel bar 1 are evaluated from the flaw detection data. That is, in this embodiment, it is not necessary to directly look at the state of the flaws on the surface of the steel bar 1 to evaluate the properties of the flaws, and the properties of the flaws occurring in the steel bar 1 can be evaluated for all of the manufactured steel bars 1 from a chart (data pattern) of the flaw detection data for flaw detection. The evaluation of the nature of the defects may be performed only on the steel bars 1 that are rejected as products.
[0040] At this time, in this embodiment (first method), in order to evaluate the properties of the flaws, the flaw inspection chart 10 (arrangement of flaw inspection data) consisting of detection output values is converted into a flaw inspection chart 10 consisting of an array of flaw inspection data consisting of the number of flaws. Then, as a feature of the data pattern (properties) of the flaw inspection chart 10 after the conversion, a flaw density index consisting of average values is calculated to index the flaw inspection chart 10, and the properties of the flaws are evaluated using the flaw density index. As a result, in this embodiment, it is possible to more clearly and simply distinguish between longitudinal flaws and single flaws.
[0041] Furthermore, since the characteristics of the defects occurring in each steel bar 1 can be evaluated from the flaw detection data without actually visually inspecting each steel bar 1, it is possible to automatically and quickly evaluate the tendency of defects occurring during the production of steel bar 1. Then, the manufacturing conditions for producing the steel bar 1 can be optimized in accordance with the occurring defects. As shown in FIG. 5, longitudinal defects require more extensive grinding to remove than single defects, and the optimal conditions for heating and rolling during the production of steel bar 1 to suppress longitudinal defects are different from the optimal conditions for heating and rolling to suppress single defects.
[0042] In this manner, in this embodiment, by evaluating the properties of the defects and optimizing the manufacturing conditions for manufacturing the steel bar 1, it is possible to significantly reduce the number of steel bars 1 that have defects that render them unusable as products. As a result, the yield is improved. In addition, compared with longitudinal flaws, single flaws have a possibility of being able to pass as products by grinding. In the present embodiment, the steel bars 1 having single flaws can be easily selected from among the rejected steel bars 1, which also leads to an improvement in yield.
[0043] (Modification) (1) In the above embodiment, an example was given in which the defect characteristics were classified into two characteristics (longitudinal defects and single defects), but the index range may be set so as to classify the defect characteristics into three or more characteristics. (2) In addition, in the above explanation, the average value (defect density index) is calculated as an index that ignores the order of the converted flaw detection data (number of flaws), and the flaw density index is used as an index that expresses the characteristics of the data pattern to identify the nature of the flaws. The characteristics of the data pattern may be obtained by considering the order of the arrangement of the inspection data. For example, longitudinal flaws are characterized in that flaws of a predetermined size or larger appear continuously in the longitudinal direction. The characteristics of the data pattern may be obtained based on the dependency of the occurrence of such longitudinal flaws along the longitudinal direction.
[0044] (3) In the above embodiment, the characteristics of the flaws are evaluated from the characteristics (data pattern) of the flaw detection chart 10 after the flaw detection data consisting of the detection output values is converted into flaw detection data consisting of the number of flaws. The nature of the flaw may be evaluated based on the characteristics of a sequence (data pattern) of flaw detection data consisting of detected flaw output values.
[0045] (4) As a second method for evaluating the nature of the flaw, the nature of the flaw may be evaluated using machine learning. For example, the characteristics of surface defects detected in the past are classified into two or more types, and machine learning is performed by associating the data of the flaw inspection chart 10 of the steel bar 1 with each of the characteristics of the surface defects. Then, the machine learning results are referred to to evaluate which flaw the obtained flaw inspection chart 10 represents. (5) It is preferable to classify the nature of the defect in accordance with the cause of the defect.
[0046] (others) The present disclosure may also have the following configuration. (1) A surface defect evaluation method for evaluating the properties of surface defects on a steel bar, comprising the steps of: A correlation is previously determined between the characteristics of the surface flaw of the steel bar and the characteristics of a data pattern obtained by performing flaw detection along the surface of the steel bar, The properties of the surface defects of the steel bar to be evaluated are identified based on the above correlation and the characteristics of the data pattern obtained by performing flaw detection on the steel bar to be evaluated, which is the steel bar to be evaluated for the properties of the surface defects. (2) The characteristics of the data pattern are set based on a sequence of multiple inspection data along the surface of the steel bar obtained by the inspection. (3) The characteristics of the above data pattern are converted into an index, and the properties of the surface defects of the steel bar are evaluated based on the index.
[0047] (4) Dividing the surface of the steel bar into a plurality of first sections along the inspection direction, and determining whether the inspection data for each first section is equal to or greater than a preset threshold value; Dividing the surface of the steel bar into a second section larger than the first section along the surface of the steel bar; Calculate the number of first sections that are equal to or greater than the threshold in each second section; The characteristics of the data pattern are indexed based on the number of detected defects consisting of the number of first sections that are equal to or greater than the threshold value. (5) The second sections in which the number of detected defects is one or more are extracted, and the average number of detected defects per second section is regarded as a characteristic of the data pattern. (6) The plurality of flaw detection data constituting the data pattern are made up of flaw detection data obtained by detecting flaws on the entire surface of the steel bar. [Explanation of symbols]
[0048] 1 steel bar 2 Flaw detector 3. Flaw detection control section 3A Flaw detection data generation section 3B Defect detection section 3C Defect Characterization Section 10 Flaw detection chart TH1 First Threshold TH2 Second Threshold D1 1st Section D2 Second Section
Claims
1. A surface defect evaluation method for evaluating the properties of surface defects of a steel bar, comprising: A correlation is previously determined between the characteristics of the surface flaw of the steel bar and the characteristics of a data pattern obtained by performing flaw detection along the surface of the steel bar, Based on the correlation and the characteristics of a data pattern obtained by performing flaw detection on the steel bar to be evaluated, which is the steel bar to be evaluated for the properties of the surface flaw, the properties of the surface flaw of the steel bar to be evaluated are identified; The characteristics of the above data pattern are indexed, and the properties of the surface defects of the steel bar are evaluated based on the index. Dividing the surface of the steel bar into a plurality of first sections along the inspection direction, and determining whether or not the inspection data for each first section is equal to or greater than a preset threshold value; Dividing the surface of the steel bar into a second section along the surface of the steel bar, the second section being larger than the first section; Calculate the number of first sections that are equal to or greater than the threshold and that are present in each second section; indexing the characteristics of the data pattern based on the number of detected defects consisting of the number of first sections that are equal to or greater than the threshold value; A method for evaluating surface defects in steel bars, comprising the steps of:
2. The features of the data pattern are set based on a sequence of a plurality of inspection data along the steel bar surface obtained by the inspection.
2. The method for evaluating surface defects of a steel bar according to claim 1.
3. extracting the second sections in which the number of detected defects is one or more, and regarding the extracted second sections, an average value of the number of detected defects per second section is set as a characteristic of the data pattern; 3. A method for evaluating surface defects in a steel bar according to claim 1 or 2.
4. The plurality of flaw detection data constituting the data pattern are made up of flaw detection data obtained by detecting flaws on the entire surface of the steel bar. A method for evaluating surface defects in a steel bar according to any one of claims 1 to 3.
Citation Information
Patent Citations
Method for signal processing in eddy current flaw detection
JP1986265563A
Signal processing for eddy current flaw detection
JP1987266454A
Induction heating flaw detector
JP1993142171A
Method and apparatus for inspecting flaw with magnetic particle
JP1996082616A
Leakage flux flaw detecting-apparatus and method for judging defect
JP2001041932A