Semiconductor Wafers

By optimizing dopant concentrations, magnetic fields, and growth pressure, semiconductor wafers with low resistivity and controlled striations are produced, addressing manufacturing challenges and enhancing device performance.

JP7559882B2Active Publication Date: 2024-10-02SUMCO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023109141
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-29
Filing Date
2023-07-03
Publication Date
2024-10-02
Estimated Expiration
2041-06-28

AI Technical Summary

Technical Problem

Existing semiconductor wafers face challenges in achieving low resistivity and controlled striation heights during manufacturing, leading to defects and increased power consumption in semiconductor devices.

Method used

Adjusting dopant concentrations in the silicon melt, applying a magnetic field during crystal pulling, and controlling growth pressure to achieve semiconductor wafers with resistivity of 0.7 mΩ·cm or less and striation heights of 6 mm or more, using methods such as rotating the crucible and applying gas pressure.

Benefits of technology

The proposed methods enable the production of semiconductor wafers with desired resistivities and striation heights, reducing power consumption and preventing abnormal growth, thereby improving the performance of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559882000003
    Figure 0007559882000003
  • Figure 0007559882000004
    Figure 0007559882000004
  • Figure 0007559882000005
    Figure 0007559882000005
Patent Text Reader

Abstract

To provide a semiconductor wafer having low resistivity hitherto not achieved.SOLUTION: A semiconductor wafer cut from a single crystal silicon having phosphorus added as a dopant has a diameter of 300 mm and a resistivity of 0.8 mΩ cm. A striation appearing in the cross-section of the semiconductor wafer has an upper convex shape having a single peak in the central part of the semiconductor wafer; and the height x of the striation and the resistivity y satisfy the following relational expression, y≥-1.556×10-6x3+1.439×10-4x2-1.469×10-2x+9.700×10-1.SELECTED DRAWING: Figure 7A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to low resistivity wafers and methods for making the wafers. [Background technology]

[0002] Wafers are thin slices of semiconductors, such as monocrystalline silicon or single-crystal silicon, that are commonly used in photovoltaic device manufacturing to produce integrated circuits, power devices, or solar cells. Wafers serve as the circuit board for the microelectronic devices built on and within the wafer, and undergo many microfabrication steps, such as doping, ion implantation, etching, thin film deposition of various materials, and photolithographic patterning. Finally, the individual microcircuits are separated by wafer dicing and packaged as integrated circuits.

[0003] The characteristics of the wafer affect the microcircuits and other semiconductor devices. Therefore, improving the wafer characteristics can improve the performance of the semiconductor devices and circuits. For example, if the wafer has a low resistivity, the semiconductor devices and circuits will consume less power and be suitable for use in mobile devices. If the silicon crystals from which the wafers are sliced ​​grow abnormally, such crystalline defects will destroy the semiconducting properties of the material. As a result, the deformed crystals must be discarded.

[0004] Figure 1 is a graph showing the known relationship between wafer resistivity and wafer dopant concentration. The curve in Figure 1 is called the Irvin curve and was obtained via ASTM F723-81. Figure 1 shows the relationship between resistivity R and dopant (carrier) concentration (atoms / cm 3) relationship. As shown in Figure 1, two curves are shown, each corresponding to a different dopant. The lower curve describes the resistivity as a function of phosphorus concentration, while the upper curve describes the resistivity as a function of boron concentration. Another reason is that phosphorus is used to negatively charge the wafer (N-type) and boron is used to positively charge the wafer (P-type). As shown in Figure 1, in both cases the aforementioned resistivity is generally inversely proportional to the dopant concentration. For equal concentrations of dopants, the resistivity of phosphorus-doped wafers is lower than that of boron-doped wafers. A higher dopant concentration can be advantageous to obtain the lowest possible resistivity without destroying the structural and electrical integrity of the wafer.

[0005] FIG. 2 is a cross-sectional view of a crystal ingot formed in the process of producing silicon single crystal from a known silicon melt. It is known that the resistivity of a silicon ingot pulled from a silicon melt decreases when the dopant concentration of the silicon melt increases, but if the dopant concentration of the silicon melt is too high, the silicon ingot pulled from the silicon melt may exhibit abnormal growth, such as dendritic growth of cells. That is, if there is a large amount of dopant in the silicon melt, the silicon crystal ingot may deform and destroy the crystallinity. The table below (Table 1) is experimental data describing the effect of dopant concentration on the abnormal growth and resistivity of a silicon ingot.

[0006] Table 1: For a 200 mm wafer with phosphorus (P) dopant and 4 mm striation height and 0.4 mm / min pull speed

[0007] [Table 1]

[0008] From the above data, the dopant concentration is 9.7×10 19 atoms / cm 3In summary, under these growth conditions, the maximum dopant concentration to achieve a minimum resistivity of 0.8 mΩ cm until abnormal growth is observed is approximately 9.5 × 10 19 atoms / cm 3 It is.

[0009] Incidentally, different dopants have different effects on reducing the resistivity of the wafer. Figures 4A and 4B compare two known dopants in terms of their effect on reducing the resistivity of a 150 mm wafer. In Figures 4A and 4B, the wafers are doped with antimony (Sb) and arsenic (As), respectively. Both wafers were obtained from crystals with a striation height of 3 mm and pulled at 0.7 mm / min. Figures 4A and 4B show that arsenic is more effective in reducing resistivity without forming abnormal growths. Here, arsenic (Figure 4B) results in a minimum resistivity of about 1.5 mΩ·cm before the occurrence of abnormal growths, compared to 9.0 mΩ·cm for antimony (Figure 4A).

[0010] During the manufacturing process of single crystal silicon wafers, striations occur on the cross-sectional surface of the wafer as a result of, for example, the rate at which the single crystal is pulled from the melt during the manufacturing process of the silicon single crystal. The striation height of a silicon ingot can be measured as described in U.S. Patent No. 8,888,911, the disclosure of which is incorporated herein in its entirety. SUMMARY OF THE DISCLOSURE

[0011] In view of the above problems, embodiments of the present disclosure provide a heretofore unattainable low resistivity wafer. This can be achieved by adjusting the desired amount of dopant in the molten silicon from which the single crystal to provide the wafer is grown. The embodiments also include a low resistivity wafer with a desired striation height.

[0012] Embodiments include a semiconductor wafer including a dopant having a resistivity of 0.7 mΩ·cm or less and a striation height of 6 millimeters (mm) or more.Embodiments include a semiconductor wafer including phosphorus as a dopant.Embodiments include a semiconductor wafer having a diameter of about 200 mm.

[0013] Embodiments include a semiconductor wafer having a resistivity of 0.5 mΩ·cm or less.

[0014] Embodiments include a semiconductor wafer including a dopant having a resistivity of 0.8 mΩ·cm or less and a striation height of 13 millimeters (mm) or more.Embodiments include a semiconductor wafer including phosphorus as a dopant.Embodiments include a semiconductor wafer having a diameter of about 300 mm.

[0015] Embodiments include a semiconductor wafer including a dopant having a resistivity of 0.7 mΩ·cm or less and a striation height of 22 millimeters (mm) or more.Embodiments include a semiconductor wafer including phosphorus as a dopant.Embodiments include a semiconductor wafer having a diameter of about 300 mm.

[0016] Embodiments include a semiconductor wafer including a dopant having a resistivity of 1.6 mΩ·cm and a striation height of 13 millimeters (mm) or greater.Embodiments include a semiconductor wafer including arsenic as a dopant.Embodiments include a semiconductor wafer having a diameter of about 300 mm.

[0017] An embodiment includes a method of manufacturing a semiconductor wafer by adding a dopant to a silicon melt, rotating and pulling a crystal from the silicon melt, and subjecting the silicon melt to a magnetic field of 3000 Gauss (G) (0.3 Tesla (T)) or greater during pulling. In an embodiment, the semiconductor wafer cut from the crystal has a resistivity of 0.8 mΩ·cm or less and a striation height of 13 mm or greater. Illustrative features include manufactured wafers having a diameter equal to about 300 mm.

[0018] Embodiments include a method for manufacturing a semiconductor wafer in which the dopant added to the silicon melt is phosphorus. Embodiments include a method for manufacturing a semiconductor wafer that comprises applying pressure to the silicon melt (hereinafter referred to as "growth pressure") to reduce or inhibit evaporation of the dopant. In embodiments, the growth pressure is applied via application of a gas, such as, for example, argon gas.

[0019] According to embodiments of the present disclosure, wafers having desired dopants, desired resistivity, and desired striation height to achieve desired performance can be obtained by the above method. [Brief description of the drawings]

[0020] Embodiments of the present disclosure are further described in the following detailed description, which provide non-limiting examples of the present disclosure, with reference to the several drawings mentioned, in which like reference numerals refer to like parts throughout the several views of the drawings. [Figure 1] FIG. 1 is a graph illustrating the relationship between wafer resistivity and wafer dopant concentration according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a photograph of a cross section of a single crystal ingot showing the formation of abnormal growth. [Figure 3A] FIG. 3A illustrates the relationship between striation height before abnormal growth occurs and minimum achievable resistivity according to an embodiment of the present disclosure. [Figure 3B] FIG. 3B illustrates the relationship between striation height before abnormal growth occurs and minimum achievable resistivity according to an embodiment of the present disclosure. [Figure 3C] FIG. 3C illustrates the relationship between striation height before abnormal growth occurs and minimum achievable resistivity according to an embodiment of the present disclosure. [Figure 3D] FIG. 3D illustrates the relationship between striation height before abnormal growth occurs and minimum achievable resistivity according to an embodiment of the present disclosure. [Figure 3E] FIG. 3E illustrates the relationship between striation height before abnormal growth occurs and minimum achievable resistivity according to an embodiment of the present disclosure. [Figure 3F] FIG. 3F illustrates the relationship between striation height before abnormal growth occurs and minimum achievable resistivity according to an embodiment of the present disclosure. [Figure 4A] FIG. 4A shows the effect of lowering the resistivity of the wafer between the two dopants. [Figure 4B] FIG. 4B shows the effect of lowering the resistivity of the wafer between the two dopants. [Figure 5A] FIG. 5A shows striation height for a 200 mm wafer according to an embodiment of the present disclosure. [Figure 5B] FIG. 5B illustrates the striation height of a 300 mm wafer according to an embodiment of the present disclosure. [Figure 6] FIG. 6 illustrates a method for measuring striation height in a cross-sectional view of a silicon wafer according to an embodiment of the present disclosure. [Figure 7A] FIG. 7A illustrates a positive striation height according to an embodiment. [Figure 7B] FIG. 7B illustrates a negative striation height according to an embodiment. [Figure 8A] FIG. 8A shows the relationship between the magnetic field applied during the manufacturing process of the silicon single crystal wafer according to the embodiment and the above-mentioned striation height. [Figure 8B] FIG. 8B shows the relationship between the magnetic field applied during the manufacturing process of the silicon single crystal wafer according to the embodiment and the above-mentioned striation height. [Figure 9A] FIG. 9A illustrates the effect of silicon ingot pull rate on the amount of dopant concentration that can be tolerated before abnormal growth occurs, for various striation heights. [Figure 9B] FIG. 9B illustrates the effect of silicon ingot pull rate on the amount of dopant concentration that can be tolerated before abnormal growth occurs, for various striation heights. [Figure 9C] FIG. 9C illustrates the effect of silicon ingot pull rate on the amount of dopant concentration that can be tolerated before abnormal growth occurs, for various striation heights. [Figure 10A]FIG. 10A shows the effect of silicon ingot pull rate on the decrease in resistivity of wafers with various striation heights before abnormal growth occurs. [Figure 10B] FIG. 10B shows the effect of silicon ingot pull rate on the decrease in resistivity of wafers with various striation heights before abnormal growth occurs. [Figure 10C] FIG. 10C shows the effect of silicon ingot pull rate on the decrease in resistivity of wafers with various striation heights before abnormal growth occurs. [Figure 11] FIG. 11 shows a crystal pulling apparatus equipped with gas supply ports and pressure control valves. [Figure 12A] FIG. 12A is a graph showing the relationship between wafer resistivity and gas flow rate. [Figure 12B] FIG. 12B is a graph showing the relationship between wafer resistivity and gas pressure. Disclosed embodiments

[0021] The matters described herein are given by way of example only to exemplify the embodiments of the present disclosure, and are described for the purpose of providing what is believed to be the most effective and easiest to understand explanation of the principles and conceptual features of the embodiments. In this respect, it is not intended to show structural details of the embodiments beyond the extent necessary for a fundamental understanding of the present invention, and the description in conjunction with the drawings will make clear to those skilled in the art how some forms of the embodiments are actually embodied.

[0022] In this specification, when the terms "about" or "substantially" are used in connection with a numerical value, it is intended that the associated numerical value be within a tolerance of approximately ±10% of the stated numerical value. Furthermore, when percentages are referred to herein, it is intended that these percentages are based on weight (i.e., weight percent). The term "up to" refers to an amount from zero to the stated upper limit, including all values ​​therebetween. When a range is specified, all values ​​within that range are included, for example to the nearest 0.1%. Furthermore, when the terms "generally" and "substantially" are used in connection with a geometric shape, it is intended that the geometric tolerance is within the scope of the disclosure, although no precision of the geometric shape is required. Tubular members of the described characteristics may be cylindrical or may have other tubular cross-sectional shapes, such as square, rectangular, oval, triangular, etc.

[0023] In the drawings, the dimensions of layers and regions may be exaggerated for clarity. Like numbers refer to like elements throughout. The same numerals refer to the same parts throughout the specification. Spatial relative terms such as "beneath," "below," "lower," "above," and "upper" are used herein to facilitate describing the relationship of one element or feature to another element or feature as illustrated in the figures. Spatial relative terms are intended to include various orientations of the device during use or operation in addition to the orientation depicted. For example, if the device in the drawings is turned over, elements described as "below" or "beneath" a different element or feature would be oriented "above" that different element or feature. Thus, the word "below" can include both an up and down orientation. The device is otherwise oriented (rotated 90 degrees or in any other direction) and the spatial relative descriptors used herein should be interpreted accordingly.

[0024] The embodiments are described herein with reference to cross-sectional illustrations that are schematic illustrations of idealized features (and intermediate structures) thereof. As such, variations from the shapes of the illustrations as a result, for example, of manufacturing techniques and / or tolerances, are expected. Thus, the embodiments should not be construed as limited to the particular shapes of regions illustrated herein but should include, for example, deviations in shapes that result from manufacturing. The regions illustrated in the drawings are schematic in nature and their shapes are not intended to illustrate the actual shapes of materials and are not intended to limit the scope of the embodiments.

[0025] In an embodiment, a method for forming a silicon single crystal includes rotating silicon from a silicon melt and rotating a crucible containing the silicon melt. During the pulling process, striations are formed at the melt-crystal interface, thus resulting in high striations along the cross section of the silicon crystal. There may be a relationship between the striation height and abnormal growth of the silicon crystal, and between the striation height and the resistivity of the aforementioned wafer. In particular, increasing the striation height allows for additional dopant concentration in the silicon melt, thus lowering the resistivity of the crystal and the resulting wafer without causing abnormal growth.

[0026] 3A-3F show the relationship between striation height and resistivity of silicon wafers with different dopants according to embodiments of the present disclosure. FIGS. 3A-3C show three different diameters of arsenic (As) wafers: 150 mm, 200 mm, and 300 mm, all of which show that the limit of lowering resistivity (without forming abnormal growth) improves with increasing striation height. As FIG. 3A shows, according to the present invention, a 300 mm As wafer can obtain a resistivity as low as 1.6 mΩ·cm without forming abnormal growth with a striation height of 13 mm. Furthermore, according to the present invention, resistivities lower than 1.6 mΩ·cm are possible with further increasing the striation height. In one embodiment, a 300 mm As wafer is subjected to a resistivity of about 4.0×10 19 atoms / cm 3An arsenic concentration of about 5.1×10 was used with a crucible rotation rate of about 0.2 revolutions per minute (rpm), a crystal pull rate of about 0.2 mm / min, and a magnetic field of about 0.3 Tesla (T) (or 3000 Gauss (G)), resulting in a striation height of about 13 mm and a resistivity of about 1.6 mΩ·cm. Similarly, as shown in FIG. 3B, a 200 mm As wafer can obtain a resistivity as low as 1.4 mΩ·cm with a striation height of 5 mm. Furthermore, the present invention shows that resistivities lower than 1.4 mΩ·cm are possible by further increasing the striation height. In another embodiment, a resistivity of about 5.1×10 19 atoms / cm 3 A concentration of 1.0 μm of As was used for the 200 mm wafers, with a crucible rotation speed of about 6 rpm and a crystal pulling speed of about 0.2 mm / min, resulting in a striation height of 5 mm and a resistivity of about 1.4 mΩ·cm. In this case, no magnetic field was applied. Finally, as shown in Figure 3C, the 150 mm As wafers can obtain a low resistivity of 1.4 mΩ·cm with a striation height of about -1 mm. It is also possible to reduce the resistivity without forming abnormal growth by increasing the striation height in all three wafers.

[0027] The linear regression relationship between resistivity, represented as the "Y" axis, and striation height, represented as the "X" axis, for each wafer size of As-doped wafers is shown below.

[0028] 300mm As-doped wafer: y = 2.886×10 -6 x 3 + 3.319×10 -4 x 2 - 4.192×10 -2 x + 2.082.

[0029] 200mm As-doped wafer: y = -5.514×10 -6 x 3 + 3.872×10 -4 x 2 - 2.216×10 -2 x + 1.500.

[0030] 150mm As-doped wafer: y = -3.884×10 -6 x 3 + 2.592×10 -4 x 2 - 1.743×10 -2 x + 1.389.

[0031] 3D-3F show phosphorus (P) wafers of three different diameters: 150 mm, 200 mm, and 300 mm, all of which improve the limit of lowering resistivity (without forming abnormal growth) as the striation height increases. As FIG. 3D shows, in accordance with the present invention, a 300 mm P wafer can obtain a resistivity as low as 0.8 mΩ·cm without forming abnormal growth at a striation height of 13 mm. Furthermore, in accordance with the present invention, resistivities lower than 0.8 mΩ·cm are possible by further increasing the striation height. In one embodiment, a resistivity of about 9.5×10 19 atoms / cm 3 A phosphorus concentration of about 1.3×10 was used for a 300 mm wafer, with a crucible rotation speed of about 0.2 rpm, a crystal pull rate of about 0.2 mm / min, and a magnetic field of about 0.3 T, resulting in a striation height of about 13 mm and a resistivity of about 0.8 mΩ·cm. Similarly, as shown in FIG. 3E, a 200 mm P wafer can obtain a resistivity as low as 0.6 mΩ·cm with a striation height of 16 mm. Furthermore, the present invention shows that resistivities lower than 0.6 mΩ·cm are possible by further increasing the striation height. In one embodiment, a resistivity of about 1.3×1020 atoms / cm 3 A phosphorus concentration of about 1.0 μm was used for the 200 mm wafers, with a crucible rotation speed of about 0.2 rpm, a crystal pulling speed of about 0.2 mm / min, and a magnetic field of about 0.3 T, resulting in a striation height of about 16 mm and a resistivity of about 0.6 mΩ·cm. Finally, as shown in Figure 3F, the 150 mm P wafers can obtain a low resistivity of 0.6 mΩ·cm with a striation height of about 13 mm. It is also possible to reduce the resistivity without forming abnormal growth by increasing the striation height in all the wafers.

[0032] The linear regression relationship between resistivity, represented as the "Y" axis, and striation height, represented as the "X" axis, for each wafer size of P-doped wafers is shown below.

[0033] 300mm P-doped wafer: y = -1.556×10 -6 x 3 + 1.439×10 -4 x 2 - 1.469×10 -2 x + 9.700×10 -1 .

[0034] 200mm P-doped wafer: y = -1.588×10 -6 x 3 + 1.331×10 -4 x 2 - 1.195×10 -2 x + 7.649×10 -1 .

[0035] 150mm P-doped wafer: y = -1.478×10 -6 x 3 + 7.824×10 -5 x 2- 9.744×10 -3 x + 7.176×10 -1 .

[0036] Table 2 below shows numerical evidence of the minimum resistivity achievable within a range of striation heights for various types of wafers (at fixed dopant concentrations).

[0037] [Table 2]

[0038] 5A and 5B show striation height measurements for 200 mm and 300 mm wafers according to embodiments of the present disclosure. Both wafers are doped with phosphorus. FIG. 5A shows that the 200 mm wafer can obtain a resistivity of about 0.6 mΩ·cm with a striation height of 18 mm. FIG. 5B shows that the 300 mm wafer can obtain a resistivity of 0.8 mΩ·cm with a striation height of 25 mm. From these figures, it can be seen that it is more difficult to achieve a low resistivity with a large 300 mm wafer than with a small 200 mm wafer when using the same dopant, even with a larger striation height.

[0039] FIG. 6 is a graph showing a method for measuring striation height of a silicon wafer according to an embodiment of the present disclosure. In FIG. 6, the striations are measured by first breaking the wafer and etching the cross-sectional image with, for example, a combination of HF, CrO3, and HO. After etching, a photograph of the etched cross-sectional image is taken, for example, by optical microscopy. Based on the photograph, the striation angles are measured at various intervals (i.e., 10 mm intervals). The measured striation angles are plotted on a curve whose x-axis represents the distance from the edge of the wafer towards the center of the wafer. Said curve represents the striation shape and height as shown in FIG. 6.

[0040] 7A and 7B illustrate positive and negative striation height formation during the process of making a single crystal ingot according to an embodiment. The striation height describes the height of the solid-liquid interface when the silicon crystal ingot is pulled from the silicon melt. As shown in FIG. 7A, when the striation height is positive, it means that the solid-liquid interface is higher than the surface of the silicon melt, and the solid-liquid interface is convex. As shown in FIG. 7B, when the striation height is negative, it means that the solid-liquid interface is lower than the surface of the silicon melt, and the solid-liquid interface is concave.

[0041] 8A and 8B are graphs showing the relationship between the magnetic field applied during the manufacturing process of a silicon single crystal wafer according to the embodiment and the aforementioned striation height. The size of the single crystal wafer shown in FIG. 8A is 300 mm, and the size of the single crystal wafer shown in FIG. 8B is 200 mm. The graphs shown in FIGS. 8A and 8B show the relationship between the magnetic field and the striation height during the pulling process. In particular, these figures show that an increase in the magnetic field increases the striation height in both the 300 mm and 200 mm wafers. FIGS. 8A and 8B show how the magnetic field tends to affect the striation height, but are not intended to indicate a lower or upper limit for the striation height in any way. Factors other than the magnetic field, such as the rotation speed of the crucible containing the silicon melt, the crystal pulling speed, and the amount of dopant concentration, may also cause the striations to have different heights.

[0042] 9A-9C and 10A-10C respectively show the effect of silicon ingot pull rate on dopant concentration and wafer resistivity, according to an embodiment. FIGS. 9A-9C and 10A-10C include experiments using wafers with three representative striation heights, 24 mm, 0 mm, and -20 mm. FIGS. 9A-9C show that each of the three striation heights allows for higher dopant concentration (and therefore lower resistivity) without forming abnormal growth when the pull rate is reduced. FIGS. 10A-10C confirm the results of FIGS. 9A-9C, showing that all three striation heights result in lower resistivity as the pull rate is reduced. FIGS. 9A-9C further show that larger striation heights tend to result in higher wafer dopant concentration (and therefore lower resistivity) for a given pull rate before abnormal growth occurs. Again, Figures 10A through 10C confirm the above, with the maximum striation height of 24 mm exhibiting the lowest resistivity over the range of pull rates exemplified in this experiment.

[0043] FIG. 11 shows a crystal pulling apparatus including a gas supply port and a pressure control valve. FIGS. 12A and 12B are graphs showing resistivity vs. gas flow rate and resistivity vs. gas pressure, respectively. An embodiment of the present invention includes a method for manufacturing a semiconductor wafer, in which the dopant added to the silicon melt is phosphorus. Additionally, an embodiment includes a method for manufacturing a semiconductor wafer, comprising applying pressure to the silicon melt to reduce or inhibit evaporation of the dopant (hereinafter referred to as "growth pressure"). An embodiment includes applying the growth pressure through application of a gas, such as, for example, argon gas. In FIG. 11, the growth pressure can be adjusted by controlling the flow rate of gas from a gas supply port (A). The flow rate can also be controlled by a pressure control valve (B) that releases the gas using a pressure control valve, such as a butterfly valve. An embodiment includes a method for manufacturing a semiconductor wafer having a resistivity of 0.7 mΩ·cm or less. Inhibiting evaporation of the dopant leads to a decrease in the resistivity of the wafer. For example, Figure 12B shows that increasing the pressure from 17 kilopascals (kPa) to 27 kPa (at a fixed gas flow rate of 80 liters / min) reduces the wafer resistivity by about 0.19 mΩ·cm (about 17%). Figure 12A shows that decreasing the gas flow rate from 80 liters / min to 40 liters / min (at a fixed gas pressure of 17 kPa) reduces the wafer resistivity by about 0.08 mΩ·cm (about 7%).

[0044] The above examples are merely illustrative and should not be construed as limiting the present disclosure. The present disclosure has been described with reference to examples of embodiments, but the words used herein are understood to be descriptive and exemplary, rather than limiting. Changes may be made within the scope of the appended claims without departing from the scope and spirit of the present disclosure in its form, as detailed or amended herein. Although the embodiments have been described herein with reference to specific structures, materials, and features, the embodiments are not intended to be limited to those disclosed herein, but rather the embodiments are intended to cover all functionally equivalent structures, methods, and uses within the scope of the appended claims.

[0045] The present disclosure is not limited to the above-mentioned features, and various modifications and variations are possible without departing from the scope of the present disclosure.

Claims

1. A semiconductor wafer having a diameter of 300 mm cut from single crystal silicon doped with phosphorus as a dopant, The resistivity of the semiconductor wafer is 0.8 mΩ cm or less, The striations appearing in a cross section of the semiconductor wafer have an upward convex shape having a single peak at the center of the semiconductor wafer, The height x of the striations and the resistivity y are related by the following formula: y ≧ -1.556×10 -6 x 3 + 1.439×10 -4 x 2 - 1.469×10 -2 x + 9.700×10 -1 Fulfilling A semiconductor wafer, wherein the range of the height x of the striations is -15≦x≦35.

2. A semiconductor wafer having a diameter of 200 mm cut from single crystal silicon doped with phosphorus as a dopant, The resistivity of the semiconductor wafer is 0.6 mΩ cm or less, The striations appearing in a cross section of the semiconductor wafer have an upward convex shape having a single peak at the center of the semiconductor wafer, The height x of the striations and the resistivity y are related by the following formula: y ≧ -1.588×10 -6 x 3 + 1.331×10 -4 x 2 - 1.195×10 -2 x + 7.649×10 -1 Fulfilling A semiconductor wafer, wherein the range of the height x of the striations is -15≦x≦30.

3. A semiconductor wafer having a diameter of 150 mm cut from single crystal silicon doped with phosphorus as a dopant, The resistivity of the semiconductor wafer is 0.6 mΩ cm or less, The striations appearing in a cross section of the semiconductor wafer have an upward convex shape having a single peak at the center of the semiconductor wafer, The height x of the striations and the resistivity y are related by the following formula: y ≧ -1.478×10 -6 x 3 + 7.824×10 -5 x 2 - 9.744×10 -3 x + 7.176×10 -1 Fulfilling A semiconductor wafer, wherein the range of the height x of the striations is -16≦x≦25.

4. A semiconductor wafer having a diameter of 300 mm cut from single crystal silicon doped with arsenic as a dopant, The resistivity y of the semiconductor wafer is 1.6 mΩ cm or less, The striations appearing in a cross section of the semiconductor wafer have an upward convex shape having a single peak at the center of the semiconductor wafer, The height x of the striations and the resistivity y are related by the following formula: y ≧ 2.886×10 -6 x 3 + 3.319×10 -4 x 2 - 4.192×10 -2 x + 2.082 Fulfilling A semiconductor wafer, wherein the range of the height x of the striations is -15≦x≦35.

5. A semiconductor wafer having a diameter of 200 mm cut from single crystal silicon doped with arsenic as a dopant, The resistivity of the semiconductor wafer is 1.4 mΩ cm or less, The striations appearing in a cross section of the semiconductor wafer have an upward convex shape having a single peak at the center of the semiconductor wafer, The height x of the striations and the resistivity y are related by the following formula: y ≧ -5.514×10 -6 x 3 + 3.872×10 -4 x 2 - 2.216×10 -2 x + 1.500 Fulfilling A semiconductor wafer, wherein the range of the height x of the striations is -15≦x≦30.

6. A semiconductor wafer having a diameter of 150 mm cut from single crystal silicon doped with arsenic as a dopant, The resistivity of the semiconductor wafer is 1.4 mΩ cm or less, The striations appearing in a cross section of the semiconductor wafer have an upward convex shape having a single peak at the center of the semiconductor wafer, The height x of the striations and the resistivity y are related by the following formula: y ≧ -3.884×10 -6 x 3 + 2.592×10 -4 x 2 - 1.743×10 -2 x + 1.389 Fulfilling A semiconductor wafer, wherein the range of the height x of the striations is -15≦x≦25.

Citation Information

Patent Citations

  • Semiconductor single crystal manufacturing apparatus

    JP2009035455A

  • Method of manufacturing silicon epitaxial wafer

    JP2011044505A

  • Method of producing single crystal silicon

    JP2011057476A

  • Method for calculating solid-liquid interface height between single crystal and raw material melt and method for manufacturing single crystal

    JP2017206400A

  • n-TYPE SILICON SINGLE CRYSTAL PRODUCTION METHOD, n-TYPE SILICON SINGLE CRYSTAL INGOT, SILICON WAFER, AND EPITAXIAL SILICON WAFER

    WO2018198663A1