Projection welded joint and its manufacturing method
Patent Information
- Application Number
- JP2024542407
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2044-04-24
AI Technical Summary
【0012】 本発明は、剥離強度及び耐遅れ破壊特性を向上させたプロジェクション溶接継手を提供できる。
Smart Images

Figure 0007560006000003 
Figure 0007560006000004 
Figure 0007560006000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a projection welded joint formed by projection welding a steel plate and a nut having a projection via the projection, and to a method for manufacturing the same. [Background technology]
[0002] In recent years, various high-strength steel plates (hi-tensile steel) have been increasingly used in automobile bodies from the viewpoints of weight reduction for improved fuel economy and ensuring collision safety. In addition, when resistance spot welding cannot be used in the automobile assembly process, arc welding and bolt fastening are used. Furthermore, bolt fastening is also widely used in joining dissimilar materials such as steel plates and aluminum. In bolt fastening, a nut with a projection portion (protruding portion) is projection welded (resistance welded) to the steel plate, and then another plate is fastened with a bolt to perform assembly.
[0003] One of the quality assurances for projection welding is the push-in peel strength (also simply called peel strength). As the strength of steel plates has increased in recent years, the joint between the steel plate and the nut becomes more brittle, making it difficult to ensure peel strength. Another issue is that the increased strength of steel plates increases susceptibility to delayed fracture, i.e., hydrogen embrittlement. Another issue is that hydrogen is absorbed into the weld due to the influence of anti-rust oil and plating layers on the surface of the steel plate, making delayed fracture more likely to occur.
[0004] Patent Document 1 describes a projection welded joint in which the area ratio between the joint and the nominal diameter part of the nut or bolt satisfies a predetermined relationship, and the maximum hardness of the joint and heat-affected zone is 550 HV or less. Patent Document 1 also reports that high joint strength can be obtained by increasing the pressure during projection welding. Patent Document 2 also reports that high joint strength can be obtained by tempering the joint by post-current application at a current value lower than the current value during welding after projection welding. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-157900 A [Patent Document 2] JP 2013-78784 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, with conventional methods, there is a problem that a decrease in peel strength and delayed fracture occur when projection welding high-strength steel plates, and there is room for improvement.
[0007] In view of the above problems, an object of the present invention is to provide a projection welded joint having improved peel strength and delayed fracture resistance, and a manufacturing method thereof. [Means for solving the problem]
[0008] The present inventors have made intensive studies to solve the above problems and have obtained the following findings. High-strength steel plates have a higher carbon content than conventional steel plates and are prone to embrittlement of the joint, so the peel strength of the projection welded joint is reduced. In order to improve the peel strength of a projection welded joint using a high-strength steel plate, it is effective to soften the joint surface between the nut and the steel plate to be welded to alleviate stress concentration. In addition, delayed fracture is caused by the hardness of the joint, which is the fracture origin, and the influence of segregation and inclusions present in the joint. Therefore, in order to suppress delayed fracture, it is effective to prevent hardening of the joint and reduce the residual stress. In particular, the area near the boundary between the steel plate and the nut and a part of the joint is designated as region c, and the hardness of region c is reduced to improve the delayed fracture resistance. This is because softening the hardness of region c improves the toughness of region c, and further reduces the residual stress, making delayed fracture less likely to occur.
[0009] That is, the gist and configuration of the present invention are as follows.
[0010] [1] A projection welded joint formed by projection welding a steel plate and a nut having a protrusion through the protrusion, The steel plate comprises, in mass%, C: 0.05 to 0.50%, Si: 0.1 to 2.0%, Mn: 1.5-4.0%, P: 0.10% or less, S: 0.005% or less, N: 0.010% or less, and O: 0.030% or less and optionally further comprising: Al: 2.00% or less, B: 0.0050% or less, Ca: 0.005% or less, Cr: 1.00% or less, Cu: 0.80% or less, Ni: 1.00% or less, Mo: 1.00% or less Ti: 0.200% or less, V: 0.500% or less, Nb: 0.080% or less, Sb: 0.200% or less, and Sn: 0.200% or less and the balance being Fe and unavoidable impurities, A projection welded joint, in which a minimum hardness Hvc (HV) of a region c in the steel plate defined below and a base metal hardness Hvm (HV) of the steel plate satisfy the following formula (1). Hvc / Hvm≦0.85 (1) The region c is specified as follows in a cross section of the projection welded joint that includes the center line of the nut and passes through the center of the joint between the steel plate and the nut: The end point of the inner circumferential surface side of the nut that contacts the steel plate is A, the end point of the outer circumferential surface side is B, the thickness of the steel plate in the cross section is t (mm), the points inside the steel plate that are moved 0.20 mm and 2 / 3t from point A in the thickness direction of the steel plate are A1 and A2, respectively, and the points inside the steel plate that are moved 0.20 mm and 2 / 3t from point B in the thickness direction of the steel plate are B1 and B2, respectively, and the inside of a rectangle formed by connecting points A1, B1, B2, and A2 is defined as the region c.
[0011] [2] A method for manufacturing a projection welded joint by projection welding a steel plate and a nut having a protrusion via the protrusion, The steel plate comprises, in mass%, C: 0.05 to 0.50%, Si: 0.1 to 2.0%, Mn: 1.5-4.0%, P: 0.10% or less, S: 0.005% or less, N: 0.010% or less, and O: 0.030% or less and optionally further comprising: Al: 2.00% or less, B: 0.0050% or less, Ca: 0.005% or less, Cr: 1.00% or less, Cu: 0.80% or less, Ni: 1.00% or less, Mo: 1.00% or less Ti: 0.200% or less, V: 0.500% or less, Nb: 0.080% or less, Sb: 0.200% or less, and Sn: 0.200% or less and the balance being Fe and unavoidable impurities, The projection welding is A main current application process in which a current is applied at a current value I1 (kA) for a current application time t1 (ms) to form a joint between the steel plate and the nut; The de-energization time t that satisfies the following formula (2) c1 a de-energization step of providing a de-energization period of (ms); a first post-current application step of applying a current at a current value I (kA) that satisfies the following formula (3) for a current application time t (ms) that satisfies the following formula (4); a second post-current application step of applying current at a current value I3 (kA) that satisfies the following formula (5) for a current application time t3 (ms) that satisfies the following formula (6); A method for manufacturing a projection welded joint having the above structure. 800 <t c1 (2) 1.10I1≦I2≦1.80I1 (3) 50≦t2≦200 (4) I3≦0.70I2 (5) 300≦t3≦1000 (6) Effect of the Invention
[0012] The present invention can provide a projection welded joint having improved peel strength and delayed fracture resistance. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a cross-sectional view including a center line of a nut used in one embodiment of the present invention. [Diagram 2] 1 is a partial cross-sectional view of a projection welded joint according to one embodiment of the present invention, the cross-sectional view including the center line of a nut and passing through the center of a joint between a steel plate and a nut. [Diagram 3] FIG. 2 is a top view of a nut provided with three protrusions and a nut provided with four protrusions, both used in one embodiment of the present invention. [Figure 4] FIG. 13 is a diagram showing region c and hardness measurement points in region c in a cross section of a projection welded joint according to one embodiment of the present invention. [Diagram 5]1 is a diagram showing a measurement area 30 for base metal hardness Hvm and hardness measurement points in the area 30 in a cross section of a projection welded joint according to one embodiment of the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of a projection welded joint and a manufacturing method thereof according to the present invention will be described. Note that the embodiment described below is an example of the present invention, and the configuration of the present invention is not limited to this specific example.
[0015] [Steel plate] First, the composition of the steel plate in the projection welded joint according to the present invention will be described. In the following description, the "%" in the composition refers to "mass %" unless otherwise specified.
[0016] C: 0.05 to 0.50% C is an element that contributes to strengthening of the steel plate. If the C content of the steel plate is less than 0.05%, the strength of the steel plate is low, and it is extremely difficult to manufacture a steel plate with a tensile strength of 780 MPa or more. Therefore, the C content of the steel plate is set to 0.05% or more. It is preferable that the C content of the steel plate is set to 0.10% or more. On the other hand, if the C content of the steel plate exceeds 0.50%, the strength of the steel plate increases, but the amount of hard martensite becomes excessive, and the number of microvoids increases. Furthermore, the joint becomes excessively hard and embrittlement progresses, making it difficult to improve the peel strength. Therefore, the C content of the steel plate is set to 0.50% or less. It is preferable that the C content of the steel plate is set to 0.45% or less.
[0017] Si: 0.1 to 2.0% When the Si content of the steel plate is 0.1% or more, it is effective in strengthening the steel plate. In addition, since Si is a ferrite-forming element, it is advantageous in forming ferrite at the end of the joint. Therefore, the Si content of the steel plate is set to 0.1% or more. The Si content of the steel plate is preferably set to 0.2% or more. On the other hand, if the Si content of the steel plate exceeds 2.0%, the steel plate is strengthened, but may have a negative effect on toughness. Therefore, the Si content of the steel plate is set to 2.0% or less. The Si content is preferably set to 1.8% or less.
[0018] Mn: 1.5-4.0% When the Mn content is 1.5% or more, high peel strength can be obtained without long-term cooling. Therefore, the Mn content of the steel plate is set to 1.5% or more. The Mn content of the steel plate is preferably set to 2.0% or more. On the other hand, when the Mn content of the steel plate exceeds 4.0%, embrittlement of the welded portion or cracks associated with embrittlement become prominent, making it difficult to improve the peel strength. Therefore, the Mn content of the steel plate is set to 4.0% or less. The Mn content of the steel plate is preferably set to 3.5% or less.
[0019] P:0.10% or less P is an unavoidable impurity, but if the P content of the steel plate exceeds 0.10%, strong segregation appears at the end of the joint of the welded portion, making it difficult to improve the peel strength. Therefore, the P content of the steel plate is set to 0.10% or less. The P content of the steel plate is preferably 0.05% or less, and more preferably 0.02% or less. There is no particular lower limit for the P content of the steel plate. However, since excessive reduction leads to an increase in costs, the P content of the steel plate is preferably 0.005% or more.
[0020] S: 0.005% or less S is an element that segregates at grain boundaries and embrittles steel sheets, and is an element that is inevitably included. Furthermore, if the S content of a steel sheet exceeds 0.005%, it reduces sulfides and the local deformability of the steel sheet. Therefore, the S content of the steel sheet is set to 0.005% or less. The S content of the steel sheet is preferably 0.004% or less, and more preferably 0.003% or less. There is no particular lower limit for the S content of the steel sheet. However, since excessive reduction leads to an increase in costs, the S content of the steel sheet is preferably 0.001% or more.
[0021] N: 0.010% or less N is an element that is inevitably contained, and if the N content of the steel plate exceeds 0.010%, the aging resistance of the steel plate deteriorates. Therefore, the N content of the steel plate is set to 0.010% or less. The N content of the steel plate is preferably set to 0.008% or less. There is no particular lower limit for the N content of the steel plate. However, since an excessive reduction leads to an increase in costs, the N content of the steel plate is preferably set to 0.001% or more.
[0022] O: 0.030% or less If the O content of a steel plate exceeds 0.030%, nonmetallic inclusions are generated, deteriorating the cleanliness and toughness of the steel plate. Therefore, the O content of the steel plate is set to 0.030% or less. The O content of the steel plate is preferably set to 0.020% or less. There is no particular lower limit for the O content of the steel plate. However, since an excessive reduction leads to an increase in costs, the O content of the steel plate is preferably set to 0.005% or more.
[0023] In addition to the above-mentioned composition, the steel sheet used in the present invention may contain, if necessary, one or more elements selected from Al, B, Ca, Cr, Cu, Ni, Mo, Ti, V, Nb, Sb, and Sn, with the balance being Fe and unavoidable impurities.
[0024] Al: 2.00% or less Al is an element that can control the structure by refining austenite grains, but adding a large amount of it deteriorates toughness. Therefore, when Al is added, the Al content is set to 2.00% or less. The Al content is preferably set to 1.50% or less. In addition, although there is no particular lower limit for the Al content, from the viewpoint of fully obtaining the effect of adding Al, the Al content is preferably set to 0.01% or more, and more preferably set to 1.20% or more.
[0025] B: 0.0050% or less B is an element that can improve hardenability and strengthen steel sheets, but if a large amount is added, the effect is saturated. Therefore, when B is added, the B content is set to 0.0050% or less. The B content is preferably set to 0.0010% or less. In addition, although there is no particular lower limit for the B content, from the viewpoint of fully obtaining the effect of the addition of B, the B content is preferably set to 0.0003% or more.
[0026] Ca: 0.005% or less Ca is an element that can contribute to improving the workability of steel sheets, but adding a large amount of Ca deteriorates toughness. Therefore, when Ca is added, the Ca content is set to 0.005% or less. The Ca content is preferably set to 0.004% or less. In addition, although there is no particular lower limit for the Ca content, from the viewpoint of fully obtaining the effect of adding Ca, the Ca content is preferably set to 0.001% or more.
[0027] Cr:1.00% or less Cr is an element that can improve the strength of steel plate by improving hardenability, but adding a large amount of Cr may deteriorate the toughness of the joint. Therefore, when Cr is added, the Cr content is set to 1.00% or less. The Cr content is preferably set to 0.80% or less. In addition, although there is no particular lower limit for the Cr content, the Cr content is preferably set to 0.01% or more from the viewpoint of fully obtaining the effect of the addition of Cr.
[0028] Cu: 0.80% or less Cu is an element that can contribute to improving the strength of steel plate, but adding a large amount of Cu deteriorates toughness. Therefore, when Cu is added, the Cu content is set to 0.80% or less. The Cu content is preferably set to 0.60% or less. In addition, although there is no particular lower limit for the Cu content, from the viewpoint of fully obtaining the effect of adding Cu, the Cu content is preferably set to 0.006% or more.
[0029] Ni: 1.00% or less Ni is an element that can contribute to improving the strength of steel plate, but adding a large amount of Ni deteriorates toughness. Therefore, when Ni is added, the Ni content is set to 1.00% or less. The Ni content is preferably set to 0.80% or less. In addition, although there is no particular lower limit for the Ni content, from the viewpoint of fully obtaining the effect of the addition of Ni, the Ni content is preferably set to 0.005% or more.
[0030] Mo: 1.00% or less Mo is an element that can contribute to improving the strength of steel plate, but adding a large amount of Mo deteriorates toughness. Therefore, when Mo is added, the Mo content is set to 1.00% or less. The Mo content is preferably set to 0.80% or less. There is no particular lower limit for the Mo content, but from the viewpoint of fully obtaining the effect of the addition of Mo, the Mo content is preferably set to 0.006% or more.
[0031] Ti:0.200% or less Ti is an element that can improve hardenability and strengthen steel sheets, but if added in large quantities, it forms carbides, which undergo precipitation hardening and significantly deteriorate toughness. Therefore, when Ti is added, the Ti content is set to 0.200% or less. The Ti content is preferably set to 0.150% or less. There is no particular lower limit for the Ti content, but from the viewpoint of fully obtaining the effects of the addition of Ti, the Ti content is preferably set to 0.003% or more.
[0032] V:0.500% or less V is an element that can strengthen steel by controlling the structure through precipitation hardening, but adding a large amount of V leads to a deterioration in the toughness of the joint. Therefore, when V is added, the V content is set to 0.500% or less. The V content is preferably set to 0.300% or less. There is no particular lower limit for the V content, but from the viewpoint of fully obtaining the effect of the V addition, the V content is preferably set to 0.005% or more.
[0033] Nb: 0.080% or less Nb is an element that can improve the cross tensile strength and delayed fracture resistance after resistance welding by forming fine carbonitrides, but adding a large amount of Nb not only significantly reduces elongation but also significantly impairs toughness. Therefore, when Nb is added, the Nb content is set to 0.080% or less. The Nb content is preferably set to 0.070% or less, and more preferably set to 0.060% or less. In addition, the lower limit of the Nb content is not particularly limited, but from the viewpoint of fully obtaining the effect of the addition of Nb, the Nb content is preferably set to 0.005% or more.
[0034] Sb: 0.200% or less Sb is an element that can suppress nitridation and oxidation of the steel sheet surface, but adding a large amount of Sb reduces toughness. Therefore, when Sb is added, the Sb content is set to 0.200% or less. There is no particular lower limit for the Sb content, but from the viewpoint of fully obtaining the effect of the addition of Sb, the Sb content is preferably set to 0.002% or more.
[0035] Sn: 0.200% or less Sn is an element that can suppress nitridation and oxidation of the steel sheet surface, and adding Sn stabilizes the material, but adding a large amount of Sn reduces toughness. Therefore, when Sn is added, the Sn content is set to 0.200% or less. There is no particular lower limit for the Sn content, but from the viewpoint of fully obtaining the effect of adding Sn, the Sn content is preferably set to 0.002% or more.
[0036] The steel plate having the above-mentioned composition preferably has a tensile strength of 980 MPa or more, more preferably 1180 MPa or more. However, when the tensile strength of the steel plate is 980 MPa or more, the carbon content is high, so that when conventional projection welding is performed, there is a problem that the joint is easily embrittled and the indentation peel strength is reduced. According to the present invention, even in the case of a high-strength steel plate having a tensile strength of 980 MPa or more, the hardness of the region c is softened, and the stress concentration is alleviated, thereby suppressing the peel strength from decreasing. Furthermore, by reducing the residual stress in the region c, the peel strength of the projection weld is improved, and the delayed fracture resistance property can be improved. The above-mentioned effect can be obtained even when a steel plate having a tensile strength of less than 980 MPa is used. On the other hand, the upper limit of the tensile strength of the steel plate is not particularly limited, but the tensile strength is generally 2000 MPa or less.
[0037] From the viewpoint of targeting general steel sheets for automobiles, the thickness of the steel sheet is preferably 0.8 mm to 2.3 mm.
[0038] The steel sheet used in the present invention may have a plating layer on the surface of the steel sheet, and may be, for example, a steel sheet having a zinc plating layer (galvanized steel sheet). The zinc plating layer includes known zinc plating layers, such as a hot-dip galvanized layer, an electrogalvanized layer, a Zn-Al plating layer, and a Zn-Ni layer. The steel sheet used in the present invention may be subjected to a zinc plating process and then an alloying process to form a steel sheet having an alloyed zinc plating layer. The zinc plating layer may be applied to only one side of the steel sheet, or may be applied to both sides.
[0039] [nut] The nut used in the present invention is a nut having a protrusion. FIG. 1 shows a cross section including a center line 12 of a nut 10 used in one embodiment of the present invention. The nut 10 has a protrusion 16 on a surface 14 perpendicular to the center line 12. In FIG. 1, two protrusions 16 are provided symmetrically at 180° intervals with the center line 12 as the rotation axis on the surface 14 perpendicular to the center line 12. The protrusions 16 may be provided at three or four points symmetrically with the center line 12 as the rotation axis. The shapes of the nut 10 and the protrusions 16 may adopt, for example, a square welded nut (1C type) and various protrusion shapes described in JIS B 1196:2010, respectively.
[0040] The composition of the nut is not particularly limited, but for example, S25C (JIS G4051) may be adopted. In particular, when the C content in the composition of the nut is 0.05 mass% or more, the hardness of the region c is preferably obtained. Therefore, the C content of the nut is preferably 0.05 mass% or more, and more preferably 0.07 mass% or more. On the other hand, when the C content in the composition of the nut is 0.40 mass% or less, the hardness of the region c is preferably obtained. Therefore, the C content of the nut is preferably 0.40 mass% or less, and more preferably 0.38 mass% or less.
[0041] When three or more protrusions are provided on a surface perpendicular to the center line of the nut used in the present invention, the contact position between the protrusions and the steel plate becomes three or more during projection welding described below, and the contact state can be suitably stabilized. Therefore, the number of protrusions provided on the surface perpendicular to the center line of the nut used in the present invention is preferably three or more. On the other hand, when four or less protrusions are provided on a surface perpendicular to the center line of the nut used in the present invention, it is possible to suitably prevent the occurrence of weakly contacted protrusions during projection welding, which leads to unbalanced heat input, and suitably suppress the decrease in strength of the joint. Therefore, the number of protrusions provided on the surface perpendicular to the center line of the nut used in the present invention is preferably four or less.
[0042] [Projection welded joint] The projection welded joint according to the present invention is a projection welded joint formed by projection welding the above-mentioned steel plate and nut via the protrusion of the nut to form a joint between the steel plate and the nut. Here, the "joint between the steel plate and the nut" refers to the portion where the steel plate and the nut are joined by fusion joining or solid-state joining, and is a portion originating from the protrusion of the nut.
[0043] The projection welded joint according to the present invention is characterized in that the minimum hardness Hvc (HV) of a region c in the steel plate, as defined below, and the base metal hardness Hvm (HV) of the steel plate satisfy the following formula (1): Hvc / Hvm≦0.85 (1)
[0044] FIG. 2 shows a cross section of a projection welded joint 100 according to an embodiment of the present invention, which includes the center line 12 of the nut 10 and passes through the center of the joint between the steel plate 20 and the nut 10. The end point of the inner peripheral surface side of the nut 10 that contacts the steel plate 20 is A, the end point of the outer peripheral surface side is B, and the thickness of the steel plate in the cross section is t (mm). The points inside the steel plate 20 that are moved from point A by 0.20 mm and 2 / 3t in the thickness direction of the steel plate 20 are A1 and A2, respectively, and the points inside the steel plate 20 that are moved from point B by 0.20 mm and 2 / 3t in the thickness direction of the steel plate 20 are B1 and B2, respectively, and the inside of the rectangle formed by connecting points A1, B1, B2, and A2 is area c. Note that FIG. 2 also shows a measurement area 30 for the base metal hardness Hvm.
[0045] Since the joint is derived from the protrusion of the nut, the center of the joint corresponds to the position where the center of the protrusion of the nut was. Figure 3 shows a top view of (a) a nut 10A provided with three protrusions 16 and (b) a nut 10B provided with four protrusions 16 used in one embodiment of the present invention. The cutting line shown in Figure 3 is a line passing through the center line of the nut and the center of the protrusion 16. After projection welding the steel plate and the nut, the projection welded joint is cut along the cutting line shown in Figure 3 to obtain a cross section as shown in Figure 2.
[0046] When the ratio Hvc / Hvm of the minimum hardness Hvc of region c to the base metal hardness Hvm of the steel plate is 0.85 or less, region c is sufficiently softened, and thus the indentation peel strength and delayed fracture resistance are improved. Therefore, Hvc / Hvm of the projection welded joint according to the present invention is set to 0.85 or less. Hvc / Hvm is preferably 0.83 or less, and more preferably 0.80 or less. On the other hand, when Hvc / Hvm is 0.55 or more, region c can be suitably tempered. Therefore, Hvc / Hvm is preferably 0.55 or more.
[0047] The minimum hardness Hvc of region c is obtained as follows. FIG. 4 shows an enlarged view of region c. In region c, hardness measurement points 32 are set at 0.20 mm pitches in a direction perpendicular to the thickness direction of the steel plate from a point moved 0.10 mm or 0.30 mm in the direction from point B2 to point B1. At each of the hardness measurement points 32 in region c, a measurement load of 300 gf is applied with an indenter for 15 seconds in accordance with JIS Z 2244 (2020), and the Vickers hardness is measured. The lowest value among the obtained measurement results is taken as the minimum hardness Hvc of region c.
[0048] When the minimum hardness Hvc of region c is 250HV or more, the stress concentration caused by softening region c can be suitably alleviated. Therefore, the minimum hardness Hvc of region c is preferably 250HV or more. On the other hand, when the minimum hardness Hvc of region c is 650HV or less, the stress concentration caused by softening region c can be suitably alleviated. Therefore, the minimum hardness Hvc of region c is preferably 650HV or less.
[0049] The base metal hardness Hvm of the steel plate is obtained as follows. As shown in FIG. 2, in the cross section of the projection welded joint 100, a point C1 is located 7.00 mm away from point B on the line formed by the surface of the steel plate 20. A point C2 is located 0.60 mm away from point C1 on the line formed by the surface of the steel plate 20, a point C3 is located inside the steel plate 20 located 0.60 mm away from point C2 in the thickness direction of the steel plate 20, and a point C4 is located inside the steel plate 20 located 0.60 mm away from point C1 in the thickness direction of the steel plate 20. The inside of the square formed by connecting points C1, C2, C3, and C4 is the measurement area 30 of the base metal hardness Hvm. Point C1 is located 7.00 mm away from point B in order to avoid heat effects during welding. FIG. 5 shows an enlarged view of the measurement area 30 of the base metal hardness Hvm. The hardness measurement points 32 are set at 0.20 mm intervals in the thickness direction of the steel plate 20 and in the direction perpendicular to the thickness direction from a point moved 0.20 mm from point C1 in the thickness direction of the steel plate 20. At the nine hardness measurement points 32 shown in FIG. 5, a measurement load of 300 gf is applied for 15 seconds with an indenter in accordance with JIS Z 2244 (2020), and the Vickers hardness is measured at each point. The average value obtained is the base material hardness Hvm. As described above, the base material hardness Hvm of the steel plate is measured at its cross section, so the presence or absence of a plating layer does not affect it.
[0050] When the base material hardness Hvm of the steel plate is 400HV or more, the softening effect can be suitably obtained in region c. Therefore, the base material hardness Hvm of the steel plate is preferably 400HV or more. On the other hand, when the base material hardness Hvm of the steel plate is 700HV or less, the softening effect can be suitably obtained in region c. Therefore, the base material hardness Hvm of the steel plate is preferably 700HV or less, and more preferably 650HV or less.
[0051] [Manufacturing method of projection welded joints] The method for producing a projection welded joint according to the present invention is a method for producing a projection welded joint by projection welding a steel plate and a nut having a protrusion via the protrusion. The steel plate has the above-mentioned composition, and the projection welding includes a main current application step in which a current is applied at a current value I1 (kA) for a current application time t1 (ms) to form a joint between the steel plate and the nut, and a non-current application time t2 (ms) that satisfies the following formula (2): c1 the manufacturing method comprising: a non-energization process having a non-energization period of t1 (ms), a first post-energization process in which current is applied at a current value I2 (kA) that satisfies the following formula (3) for a current application time t2 (ms) that satisfies the following formula (4), and a second post-energization process in which current is applied at a current value I3 (kA) that satisfies the following formula (5) for a current application time t3 (ms) that satisfies the following formula (6). 800 <t c1 (2) 1.10I1≦I2≦1.80I1 (3) 50≦t2≦200 (4) I3≦0.70I2 (5) 300≦t3≦1000 (6)
[0052] [Main energization process] The main current application process is a process for forming a joint between a steel plate and a nut. In the main current application process, a current is applied at a current value I1 for a current application time t1 to form a joint. Note that, as long as a joint can be formed, the conditions of the main current application process described below are not particularly limited.
[0053] When the current value I1 in the main current application step is 7.0 kA or more, the steel plate and the nut can be suitably joined. When the current value I1 is less than 7.0 kA, after joining the steel plate and the nut, when the center of the joint is cut and the cross section is checked with a microscope, a gap is often observed between the steel plate and the nut. Therefore, the current value I1 in the main current application step is preferably 7.0 kA or more, and more preferably 8.0 kA or more. On the other hand, when the current value I1 is 30.0 kA or less, the joint expands too much, the molten metal splashes out of the nut as a splash, and the projection part of the nut is completely crushed and does not function as a joint. Therefore, the current value I1 is preferably 30.0 kA or less, and more preferably 28.0 kA or less.
[0054] When the energization time t1 of the main energization step is 70 ms or more, the joint can be suitably and stably obtained. Therefore, the energization time t1 of the main energization step is preferably 70 ms or more, more preferably 100 ms or more, and even more preferably 160 ms or more. On the other hand, when the energization time t1 is 500 ms or less, the joint expands too much, the molten metal splashes out of the nut as a splash, and the projection part of the nut is completely crushed and does not function as a joint. This can be suitably prevented. Therefore, the energization time t1 of the main energization step is preferably 500 ms or less, and more preferably 400 ms or less.
[0055] When the pressure applied in the main current application process is 3.0 kN or more, the current diameter is of a suitable size, and the occurrence of splashing can be suitably prevented. Therefore, the pressure applied in the main current application process is preferably 3.0 kN or more, and more preferably 3.5 kN or more. On the other hand, when the pressure applied in the main current application process is 6.0 kN or less, the current diameter is suitably prevented from expanding, and the joint can be suitably secured. Therefore, the pressure applied in the main current application process is preferably 6.0 kN or less, and more preferably 5.5 kN or less. Note that the pressure applied may be limited by the capacity of the device used, and may be appropriately adjusted so that the required joint diameter is obtained.
[0056] [First de-energization step and first post-energization step] After the main current step, softening is performed on the projection welded joint, particularly on region c. Specifically, after the main current step, a de-current step, a first post-current step, and a second post-current step are performed. By softening region c, stress concentration during a peel test is alleviated and residual stress is reduced, thereby making it possible to avoid delayed fracture.
[0057] In the first current-deactivation step, the projection welded joint is cooled so as to sufficiently lower the temperature of region c in order to obtain a softening effect.
[0058] In the first de-energization step, the cooling time t c1 The weld is cooled by keeping the current off for ms. 800 <t c1 (2) Cooling time t of the first de-energization step c1 If the cooling time t is less than 800 ms, the area c cannot be sufficiently softened. As a result, even if the subsequent processes are performed, the area c will have an embrittled structure, which will easily cause stress concentration during the indentation peel test and make it easier for cracks to grow. Therefore, c1 The cooling time t c1 is preferably 850 ms or more, and more preferably 900 ms or more. c1 If the cooling time t is long, the processing time will increase. c1 It is preferable that the delay time is 2500 ms or less.
[0059] Following the first non-current passing step, a first post-current passing step is performed. Current is passed to raise the temperature of region c to an appropriate temperature range. The "appropriate temperature range" refers to a temperature range for softening the hardness of region c. In the first post-current passing step, current is passed at a current value I2 (kA) that satisfies the following formula (3) for a current passing time t2 (ms) that satisfies the following formula (4). 1.10I1≦I2≦1.80I1 (3) 50≦t2≦200 (4)
[0060] The inventors have found that the region c can be softened by performing the first post-current step at a current value equal to or greater than that of the main current step. The post-current step softens the region c and reduces its hardness, thereby making it possible to alleviate the stress concentration applied to the region c during the indentation peel test.
[0061] If the current value I2 in the first post-current step is less than 1.10I1, the region c cannot be effectively softened. Therefore, the current value I2 in the first post-current step is set to 1.10I1 or more, and preferably 1.20I1 or more. On the other hand, if the current value I2 in the first post-current step exceeds 1.80I1, the temperature of the region c will be A c3 The temperature at which the transformation from ferrite to austenite is completed is likely to be exceeded, resulting in embrittlement. As a result, the welded portion cannot have sufficient toughness. Therefore, the current value I2 in the first post-current step is set to 1.80I1 or less, and preferably 1.70I1 or less.
[0062] As described above, in the first post-current application step, the temperature is rapidly increased in a short time, so the current application time t2 in the temperature increase process is set to 50 ms or more. The current application time t2 is preferably set to 60 ms or more. On the other hand, if the current application time t2 exceeds 200 ms, the temperature of the region c will rise to A c3 Therefore, the current application time t2 is set to 200 ms or less, and preferably to 180 ms or less.
[0063] In the projection welding according to the present invention, after the first post-current step, a second post-current step is performed in which current is applied at a current value I3 (kA) that satisfies the following formula (5) for a current application time t3 (ms) that satisfies the following formula (6). By performing the second post-current step, the region c can be softened more effectively, and residual stress can be reduced, making it easier to alleviate stress concentration. I3≦0.70I2 (5) 300≦t3≦1000 (6)
[0064] If the current value I3 of the second post-current process exceeds 0.70I2, appropriate temperature control cannot be performed to more effectively soften the region c. Therefore, the current value I3 of the second post-current process is set to 0.70I2 or less, preferably 0.65I2 or less, and more preferably 0.60I2 or less. On the other hand, if the current value I3 of the second post-current process is 0.15I2 or more, the stress concentration caused by the softening of the region c can be suitably alleviated. Therefore, the current value I3 of the second post-current process is preferably set to 0.15I2 or more, and more preferably 0.20I2 or more.
[0065] The second post-current process is a process for softening the region c, and when the current conduction time t3 is 300 ms or more, the softening can be effectively performed. Therefore, the current conduction time t3 of the second post-current process is set to 300 ms or more, preferably 350 ms or more, and more preferably 400 ms or more. On the other hand, when the current conduction time t3 exceeds 1000 ms, the temperature rises and there is a possibility that the temperature may rise again to near the melting point. Therefore, the current conduction time t3 of the second post-current process is set to 1000 ms or less, and preferably 900 ms or less.
[0066] Following the second post-current step, a non-current step and a post-current step may be repeatedly performed. By repeating the non-current step and the post-current step, the effect of softening the region b is increased, which is preferable. On the other hand, if the non-current step and the post-current step are repeated too many times, the effect becomes saturated, so the number of times the steps are repeated is preferably less than 10 times, and more preferably less than 4 times.
[0067] As described above, the projection welding method of the present invention can soften region c by appropriately controlling the welding conditions in the post heat treatment step, thereby mitigating stress concentration and reducing residual stress. That is, the projection welded joint obtained by this welding method can improve the push-in peel strength. Therefore, even when welding a steel plate containing a relatively large amount of C in its composition, specifically, a high-strength steel plate having a tensile strength of 980 MPa or more and a C content of 0.05 to 0.50 mass % as described above, the peel strength can be further improved.
[0068] Regarding steps and conditions not described in this specification, conventional methods can be used. EXAMPLES
[0069] As an example of the present invention, a projection welded joint was produced by projection welding a steel plate and a nut. For the test specimens, steel plates (Steel Plates A to M) with tensile strengths of 780 MPa to 1800 MPa and thicknesses of 1.0 to 1.8 mm were used. Table 1 shows the tensile strengths (TS), thicknesses, and chemical compositions of Steel Plates A to M used. The remainder of the chemical compositions shown in Table 1 is Fe and unavoidable impurities, and "-" indicates that the content of the element is below the lower detection limit.
[0070] As test pieces, cold-rolled steel sheets or GA steel sheets (galvannealed steel sheets) of each steel sheet were prepared. The size of the test piece was 50 mm on the long side and 50 mm on the short side, and a hole with a diameter of 11 mm was drilled in the center of the test piece. In addition, an M8 welding nut was prepared with three protrusions symmetrically provided at 120° intervals on the center line of the nut. The test piece was set in an AC welding machine so that the center of the hole of the test piece and the center of the screw hole of the nut were aligned, and welding was performed under the welding conditions shown in Table 2 to obtain a welded body. The steel type of the M8 welding nut was S25C (JIS G4051). The resistance welding conditions were such that welding was performed using a servo motor pressure type resistance welding machine attached to a welding gun with a single-phase AC (50 Hz), and a projection welded joint was produced. The pair of electrode tips used were flat electrodes with a diameter of 30 mm. A bolt was fixed in the nut hole of the obtained projection welded joint to produce a bolted test piece.
[0071] [Table 1]
[0072] [Table 2]
[0073] For the projection welded joints and bolted test pieces thus obtained, the hardness, peel strength, and delayed fracture resistance of the base metal and region c were measured by the methods described below.
[0074] [Hardness rating] The hardness of the base material and region c was measured as follows. The projection welded joint was cut at a position that included the center line of the nut and passed through the center of the joint between the steel plate and the nut to obtain a test piece, which was ultrasonically cleaned and then filled with resin to obtain a sample. The plate thickness cross section of the obtained sample was polished and etched using a picric acid solution. The hardness measurement was performed on the plate thickness cross section of the etched sample as described above, and the results are shown in Table 2. In the "Hardness judgment" column in Table 2, if the hardness measurement result satisfies formula (1) (i.e., if Hvc / Hvm≦0.85 is satisfied), it is indicated as a pass, and if it does not satisfy formula (1), it is indicated as a fail, with "×".
[0075] [Peel strength evaluation] Using the obtained bolt fastening test piece, the maximum load when the nut peeled off from the steel plate was measured by a push-in peel test according to JIS B1196:2010, and this measured value was taken as the peel strength (kN). In the present invention, the lower limit (3.73 kN) of JIS B1196:2010 was used as the standard for peel strength, and when it was less than 3.73 kN, it was evaluated as "X" as the peel strength was inferior, when it was 3.73 kN or more and less than 6.00 kN, it was evaluated as "△" as the peel strength was equivalent to the conventional peel strength, and when it was 6.00 kN or more, it was evaluated as "○" as the peel strength was excellent. Table 2 shows the measured peel strength and its evaluation results.
[0076] [Evaluation of delayed fracture resistance] After leaving the projection welded joints for 24 hours, the joints were cut and embedded in resin, and the cross sections of the welded joints were then observed. The cross sections were visually inspected to evaluate the occurrence of delayed fracture. Those that experienced delayed fracture were rated as "X", and those that did not experience delayed fracture were rated as "O".
[0077] As shown in Table 2, the projection welded joints of the invention examples were good welded joints having excellent peel strength and delayed fracture resistance. In contrast, good projection welded joints were not obtained in the comparative examples. [Industrial Applicability]
[0078] The present invention can provide a projection welded joint having improved peel strength and delayed fracture resistance. [Explanation of symbols]
[0079] 100 Projection welded joint 10 Nut 10A Nut with three prongs 10B Nut with four prongs 12 Nut centerline 14 Surface perpendicular to the center line of the nut 16 Protrusion 20 steel plate 30 Measurement area for base material hardness Hvm 32 hardness measurement points
Claims
1. A projection welded joint formed by projection welding a steel plate and a nut having a protrusion via the protrusion, The steel plate comprises, in mass%, C: 0.05-0.50%, Si: 0.1-2.0%, Mn: 1.5-4.0%, P: 0.10% or less, S: 0.005% or less, N: 0.010% or less, and O: 0.030% or less and optionally further comprising: Al: 2.00% or less, B: 0.0050% or less, Ca: 0.005% or less, Cr: 1.00% or less, Cu: 0.80% or less, Ni: 1.00% or less, Mo: 1.00% or less, Ti: 0.200% or less, V: 0.500% or less, Nb: 0.080% or less, Sb: 0.200% or less, and Sn: 0.200% or less and the balance being Fe and unavoidable impurities; A projection welded joint, wherein the minimum hardness Hvc (HV) of the steel plate in a region c defined below and the base metal hardness Hvm (HV) of the steel plate satisfy the following formula (1). Hvc / Hvm≦0.85 (1) The region c is specified as follows in a cross section of the projection welded joint that includes the center line of the nut and passes through the center of the joint between the steel plate and the nut: the end point on the inner circumferential surface side of the nut that contacts the steel plate is A, the end point on the outer circumferential surface side is B, the thickness of the steel plate in the cross section is t (mm), the points inside the steel plate that are moved 0.20 mm and 2 / 3t from point A in the thickness direction of the steel plate are A1 and A2, respectively, and the points inside the steel plate that are moved 0.20 mm and 2 / 3t from point B in the thickness direction of the steel plate are B1 and B2, respectively, and the inside of a rectangle formed by connecting points A1, B1, B2, and A2 is defined as the region c.
2. A method for manufacturing a projection welded joint by projection welding a steel plate and a nut having a protrusion via the protrusion, comprising: The steel plate comprises, in mass%, C: 0.05-0.50%, Si: 0.1-2.0%, Mn: 1.5-4.0%, P: 0.10% or less, S: 0.005% or less, N: 0.010% or less, and O: 0.030% or less and optionally further comprising: Al: 2.00% or less, B: 0.0050% or less, Ca: 0.005% or less, Cr: 1.00% or less, Cu: 0.80% or less, Ni: 1.00% or less, Mo: 1.00% or less, Ti: 0.200% or less, V: 0.500% or less, Nb: 0.080% or less, Sb: 0.200% or less, and Sn: 0.200% or less and the balance being Fe and unavoidable impurities; The projection welding is Current value I 1 (kA) and current flow time t 1 A main current application process in which a current is applied for (ms) to form a joint between the steel plate and the nut; The non-energizing time t satisfies the following formula (2): c1 a de-energization step of providing a de-energization period of (ms); A current value I that satisfies the following formula (3) 2 (kA), and the current application time t 2 a first post-current application step of applying current for (ms); A current value I that satisfies the following formula (5) 3 (kA), and the current application time t 3 A second post-current application step of applying current for (ms); A method for manufacturing a projection welded joint having the above structure. 800<t c1 ...(2) 1.10I 1 ≦I 2 ≦1.80I 1 ...(3) 50≦t 2 ≦200 ... (4) I 3 ≦0.70I 2 ...(5) 300≦t 3 ≦1000 ... (6)
Citation Information
Patent Citations
Projection welding method
JP2004050280A
Nut projection-welding coupling
JP2010116592A
Projection welding joint and projection welding method
JP7020597B1
Method for producing rivet joint, rivet joint, and automobile part
WO2023047840A1
Projection weld joint and method for production thereof
JP2012157900A
Cited By
Projection welding joint, and method for manufacturing a projection welding joint
JP7890655B1