Manufacturing method of semiconductor laser diode, semiconductor laser diode

The method aligns cavity and electrode end faces in semiconductor laser diodes by forming a continuous first semiconductor layer and convex portions, reducing threshold current density and improving durability and efficiency.

JP7560058B2Active Publication Date: 2024-10-02ASAHI KASEI KOGYO KABUSHIKI KAISHA +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021013292
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-06
Filing Date
2021-01-29
Publication Date
2024-10-02
Estimated Expiration
2041-01-29

AI Technical Summary

Technical Problem

Existing semiconductor laser diodes face issues with high threshold current density and durability due to defects in the resonator end face formed by dry etching, leading to light absorption and misalignment of cavity and electrode end faces.

Method used

A manufacturing method that forms a continuous first semiconductor layer and electrode, with a convex portion protruding from the resonator end face, using etching technology to align the cavity and electrode end faces in the same plane, and includes a pre-division inspection to remove defective wafers.

Benefits of technology

The method reduces threshold current density, enhances durability by protecting the resonator end face from corrosion, and improves luminous efficiency and reduces manufacturing costs through pre-division inspection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560058000001
    Figure 0007560058000001
  • Figure 0007560058000002
    Figure 0007560058000002
  • Figure 0007560058000003
    Figure 0007560058000003
Patent Text Reader

Abstract

To provide a Fabry-Perot type semiconductor laser diode obtained through a step of forming a resonator end face using an etching technique, in which the threshold current density of laser oscillation is reduced.SOLUTION: A manufacturing method for a semiconductor laser diode includes a step of forming a plurality of semiconductor laser diodes on a substrate and dividing the substrate for each of the semiconductor laser diodes. This manufacturing method includes a step of forming a laminate including a first semiconductor layer 21, waveguide layers 22 to 24, and a second semiconductor layer 25 in this order on a substrate 1, a step of separating between a part to become a resonance region and the other region by etching the laminate, an electrode layer formation step of forming a layer 51 to become a second electrode on the second semiconductor layer in the laminate up to a place between a resonator end face of the resonance region and a position to be divided in the dividing step, and an etching step of simultaneously or continuously removing a part 51a formed at the position outside the resonator end face of the layer to become the second electrode and forming a resonator end face 200 after the electrode layer formation step.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a semiconductor laser diode. [Background technology]

[0002] There are various types of semiconductor laser diodes with different structures. One of them is the Fabry-Perot type semiconductor laser diode, which resonates and amplifies light generated in a resonance region between the end faces of the cavity. There are two methods for forming the cavity facets: cutting along the cleavage plane of the crystal, and using an etching technique. The etching technique is generally used because it is applicable even when the cleavage planes of the substrate and the nitride semiconductor on the substrate are different, and is highly versatile.

[0003] Patent Documents 1 and 2 describe methods for forming cavity end faces using an etching technique. Patent Document 1 describes that the cavity end faces formed by dry etching are damaged by ions and have defects, which causes a problem of light absorption at the cavity end faces. It also describes that in order to solve this problem, the surface specularity of the cavity end faces is improved by wet-etching the dry-etched end faces with an etching solution.

[0004] Patent Document 2 describes a semiconductor laser diode having an underlayer which is a first semiconductor layer, a resonance region formed on part of the upper surface of the underlayer and in which the first semiconductor layer, a first guide layer, a light emitting layer, a second guide layer, and a second semiconductor layer are stacked in this order, a first electrode formed in a part of the underlayer where the resonance region is not formed, and a second electrode formed on the resonance region.

[0005] In the method for manufacturing a semiconductor laser diode described in Patent Document 2, a laminate including a first semiconductor layer, a first guide layer, a light emitting layer, a second guide layer, and a second semiconductor layer is formed on a substrate, and then the laminate is etched to separate a portion that will become a resonance region from the other portions. After that, a second electrode is formed on the second semiconductor layer by photolithography and etching, and a first electrode is formed on a portion of the base layer where the resonance region is not formed, and then a resist mask is formed with a width corresponding to the length of the cavity, and the cavity end faces are formed by photolithography and dry etching.

[0006] In the method described in Patent Document 2, after the second electrode is formed, the cavity end faces are formed by photolithography and dry etching. Therefore, in a semiconductor laser diode manufactured by this method, the cavity end faces and the end faces of the second electrode in the resonance direction of the resonance region are not in the same plane, and the cavity end faces are located outside the end faces of the electrodes in a plan view.

[0007] On the other hand, one of the challenges in realizing an ultraviolet semiconductor laser diode is to increase the output power, and one approach to achieving this is to reduce the threshold current density of laser oscillation. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 10-41585 [Patent Document 2] Japanese Patent Application Publication No. 11-145566 [Patent Document 3] JP 2008-124498 A [Patent Document 4] JP 2009-295952 A [Patent Document 5] JP 2020-47635 A Summary of the Invention [Problem to be solved by the invention]

[0009] An object of the present invention is to provide a Fabry-Perot type semiconductor laser diode obtained through a process of forming cavity end faces using an etching technique, which has a reduced threshold current density for laser oscillation and improved durability. [Means for solving the problem]

[0010] In order to solve the above problems, a method for manufacturing a semiconductor laser diode according to a first aspect of the present invention has the following features (1) to (4). (1) A method for manufacturing a semiconductor laser diode having an underlayer, a resonance region formed on a part of the upper surface of the underlayer and including a first semiconductor layer, a waveguide layer, and a second semiconductor layer stacked in this order, a first electrode formed on the first semiconductor layer near the resonance region, and a second electrode formed on the resonance region, in which the first semiconductor layer of the resonance region and the first semiconductor layer on which the first electrode is formed are continuous (both first semiconductor layers are connected without interruption). The waveguide layer includes a light-emitting layer. The underlayer may be a substrate, or may be a first semiconductor layer formed on a substrate. (2) The method includes a step of forming a plurality of the semiconductor laser diodes on a substrate and then dividing the substrate into individual semiconductor laser diodes. (3) The method includes a step of forming a laminate including a first semiconductor layer, a waveguide layer, and a second semiconductor layer in this order on a substrate. (4) An electrode layer forming step of forming a layer to become the second electrode on the second semiconductor layer of the laminate, between the resonator facet of the resonance region and the position to be divided in the dividing step, and a first etching step of removing a portion of the layer to become the second electrode formed at a position outside the resonator facet and forming the resonator facet, simultaneously or consecutively, after the electrode layer forming step.

[0011] A second aspect of the present invention is a semiconductor laser diode obtained by the manufacturing method of the first aspect, and has the following configurations (11) and (12). (11) A semiconductor device having a base layer, a resonance region formed in a part of the base region that is a part of the upper surface of the base layer, the resonance region being formed with a first semiconductor layer, a waveguide layer, and a second semiconductor layer stacked in this order, a first electrode formed on the first semiconductor layer near the resonance region, a second electrode formed on the resonance region, and a convex portion protruding from both a surface that constitutes a resonator end face of the resonance region and the upper surface of the base region. The first semiconductor layer of the resonance region and the first semiconductor layer on which the first electrode is formed are continuous (both first semiconductor layers are connected without interruption). (12) The convex portion transitions directly onto the upper surface of the base region, which is a flat surface, on the side away from the resonator end face. Effect of the Invention

[0012] According to the manufacturing method of the first aspect of the present invention, it is expected that a semiconductor laser diode having a reduced threshold current density for laser oscillation and improved durability can be obtained. In addition, by having an etching step in which the removal of the portion of the layer to become the second electrode formed at a position outside the cavity facet and the formation of the cavity facet are performed simultaneously or consecutively after the electrode layer formation step, an inspection can be performed to check the characteristics of each semiconductor laser diode before the division step.

[0013] The semiconductor laser diode of the second aspect of the present invention is a semiconductor laser diode obtained by the manufacturing method of the first aspect, and the convex portions protruding from both the faces constituting the resonator end faces of the resonance region and the upper surface of the base region protect the areas where current and heat are concentrated, so that it is expected to obtain effects such as a reduction in leakage current when current is applied, an increase in light emission efficiency, and suppression of fluctuations in the irradiation pattern. That is, the semiconductor laser diode according to the second aspect of the present invention is expected to have a reduced threshold current density for laser oscillation and improved durability. [Brief description of the drawings]

[0014] [Figure 1]2A to 2C are diagrams for explaining the steps constituting a method for manufacturing a semiconductor laser diode according to one embodiment of the present invention, showing plan views of a substrate after each step and its AA cross-sectional views thereof. [Diagram 2] FIG. 1 is a diagram for explaining each step constituting a manufacturing method of a semiconductor laser diode according to one embodiment of the present invention, in which (a) and (b) show a plan view of the substrate after each step and a cross-sectional view taken along the line AA of the substrate, and (c) shows a plan view and a front view of the substrate after the step. [Diagram 3] FIG. 3 is a plan view showing an area of ​​a substrate on which a plurality of nitride semiconductor laser diodes are to be formed, the plan view corresponding to the state shown in FIG. 2(a). [Figure 4] FIG. 3 is a cross-sectional view taken along line BB of FIG. [Diagram 5] FIG. 2(c) is a perspective view of FIG. [Figure 6] FIG. 3 is a plan view showing an area of ​​the substrate on which a plurality of nitride semiconductor laser diodes are to be formed, the plan view corresponding to the state of FIG. 2(c). [Figure 7] 1 is a cross-sectional view showing a semiconductor laser diode according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] [Findings of the present inventors] It was found that when the resonator end faces are formed using etching technology, the resonator end faces and the end faces of the second electrode in the resonance direction of the resonance region are not in the same plane, and the resonator end faces are located outside the end faces of the electrodes in a planar view, which is one of the factors that increases the threshold current density. They also found that if an inspection can be performed before the dividing step in which a terminal connected to an external power source is brought into contact with the second electrode and the first electrode to check the characteristics of each semiconductor laser diode, it is possible to remove defective wafers and reduce manufacturing costs.

[0016] [Embodiment] Hereinafter, the embodiments of the present invention will be described, but the present invention is not limited to the embodiments shown below. In the embodiments shown below, technically preferable limitations are imposed for carrying out the present invention, but these limitations are not essential requirements for the present invention.

[0017] [composition] The manufacturing method of the Fabry-Perot type semiconductor laser diode of this embodiment includes a step of forming a plurality of nitride semiconductor laser diodes on a substrate and then dividing the substrate into individual nitride semiconductor laser diodes (hereinafter referred to as a "division step"). Note that Figures 1, 2, 4, and 5 show the substrate in an area where one nitride semiconductor laser diode is formed. Figures 3 and 6 show the substrate in an area where multiple nitride semiconductor laser diodes are formed.

[0018] 1(a), a laminate 2 including a first semiconductor layer 21, a first guide layer 22, a light emitting layer 23, a second guide layer 24, and a second semiconductor layer 25 in this order is formed on a substrate 1. That is, the first guide layer 22, the light emitting layer 23, and the second guide layer 24 are formed as waveguide layers. A sapphire substrate was used as the substrate 1, and n-Al was used as the first semiconductor layer 21. x Ga (1-x) An N layer is formed, and an Al layer is formed as the first guide layer 22. x Ga (1-x) The light-emitting layer 23 is made of AlN. x Ga (1-x) An N layer is formed, and an Al layer is formed as the second guide layer 24. x Ga (1-x) An N layer is formed, and a p-Al layer is formed as the second semiconductor layer 25. x Ga (1-x) In other words, the method of this embodiment produces a nitride semiconductor laser diode.

[0019] 1(b), a mesa etching process is performed in which the laminate 2 is etched and divided into a mesa portion (a portion including a portion that becomes a resonance region) 31 and the other portions, a first portion 32 and a second portion 33. As a result, the first semiconductor layer 21 is divided in the film thickness direction into a portion (mesa side portion) 21a that constitutes the mesa portion 31 and the other portion 21b. FIG. 1(b) shows the resonance direction K of the semiconductor laser diode to be manufactured. Next, a SiO 2 After forming the insulating layer 4, which is a layer, a photolithography-etching process is performed to provide a through hole 41 for a second electrode in the insulating layer 4 on the second semiconductor layer 25 and at the same time provide a through hole 42 for a first electrode in the insulating layer 4 on the first portion 32. Figure 1(c) shows the state after this process.

[0020] Next, a resist pattern is formed on the substrate 1 in the state shown in Fig. 1(c), and then a Ni / Pt / Au layer is evaporated and a lift-off process is performed to remove the resist pattern, followed by a high-temperature heat treatment to form a patterned NiPtAu alloy layer. This results in the state shown in Fig. 2(a). Fig. 2(a) shows the resonant direction K of the semiconductor laser diode to be manufactured and the position T of a pair of resonator end faces. When this state is shown in the substrate in the range where a plurality of nitride semiconductor laser diodes are to be formed, parting lines L1 and L2 are formed as shown in Fig. 3. The positions along each parting line L1 and L2 are the positions for division in the above-mentioned division process, and among them, the position of the parting line L2 perpendicular to the resonance direction K is indicated by the symbol E in Fig. 3.

[0021] 2(a) and 3, in the above-mentioned lithography lift-off process, second alloy layer (layer to become second electrode) 51 and first alloy layer (layer to become first electrode) 61 are formed in the resonance direction K up to between resonator end face position T and position E of parting line L2 (position to be divided in the dividing process). At this time, connector 52 that electrically connects second alloy layer 51 and second semiconductor layer 25 is formed in through hole 41 for the second electrode in insulating layer 4, and connector 62 that electrically connects first alloy layer 61 and second semiconductor layer 25 is formed in through hole 42 for the first electrode in insulating layer 4.

[0022] Next, a Ni vapor deposition film is formed on substrate 1 in the state shown in Fig. 2(a), and then a photolithography lift-off process is performed to cover the portion between a pair of cavity end face positions T in the resonance direction K with Ni mask 7, as shown in Fig. 2(b). In this state, second alloy layer 51 and first alloy layer 61 are each covered with Ni mask 7 except for portions 51a and 61a that are outside cavity end face position T in the resonance direction K.

[0023] Next, the substrate 1 in the state of FIG. 2(b) is dry-etched. This dry etching is performed using chlorine gas under conditions that the mesa portion 31 is etched to the boundary position H between the first portion 32 and the second portion 33. In this single continuous dry etching process (first etching process), the outer portion 51a of the second alloy layer 51 and the outer portion 61a of the first alloy layer 61 are removed, and the end face 5A of the second electrode 5 and the end face 6A of the first electrode 6 are generated (i.e., the second electrode 5 and the first electrode 6 are formed) as shown in FIG. 2(c), and the portion of the mesa portion 31 that is not covered by the mask 7 is removed to a predetermined depth, forming the resonator end face 200. In addition, the portion of the first portion 32 that is not covered by the mask 7 is also removed to a predetermined depth. As a result, the resonance region 310 and the underlayer 320 are formed.

[0024] Next, the substrate 1 after the dry etching is immersed in an alkaline aqueous solution to perform wet etching, and then the mask 7 is removed to obtain the substrate 1 (element precursor 10) in the state shown in Fig. 2(c). This element precursor 10 is shown in Fig. 4 as a cross-sectional view taken along line BB in Fig. 2(c) and in Fig. 5 as a perspective view. When this state is shown in the substrate in the range where a plurality of nitride semiconductor laser diodes 10A are to be formed, parting lines L1 and L2 are formed as shown in Fig. 6. Next, the substrate is divided along division lines L1 and L2 shown in FIG.

[0025] Next, as shown in FIG. 7, the cavity end face 200 of the element precursor 10, the end face 5A of the second electrode 5, and the end face 6A of the first electrode 6 are coated with SiO 2 and HfO 2 Reflective layer 9, which is a dielectric multilayer film, is formed by sputtering, thereby obtaining nitride semiconductor laser diode 10A shown in FIG. The reflective layer 9 is formed by placing a jig having a slope that inclines the substrate surface by 45° on a stand for placing the substrate in a film-forming apparatus, attaching the back surface of the substrate 1 to the slope of the jig, and making the resonator end face 200 of the element precursor 10, which is the film-forming surface, a surface facing upward at an angle of 45°, and covering the center in the resonance direction K of the upper surface of the element precursor 10 with a cover. This allows the reflective layer 9 to be formed so that the film thickness at the end face 5A of the second electrode 5 and the end face 6A of the first electrode 6 is thicker than the film thickness at the resonator end face 200, and also ensures a conductive portion D on the upper surfaces of the second electrode 5 and the first electrode 6.

[0026] 2(c), 4, and 5, the cavity facet 200 of the element precursor 10 (i.e., the nitride semiconductor laser diode 10A) is composed of the surfaces of the first semiconductor layer 21aa (part of the mesa side portion 21a of the first semiconductor layer 2), the first guide layer 22, the light emitting layer 23, the second guide layer 24, and the second semiconductor layer 25. The facet 5A of the second electrode 5 in the resonance direction K and the cavity facet 200 are in the same plane. Furthermore, the facet 6A of the first electrode 6 in the resonance direction K and the facet 32a of the first portion (portion other than the mesa portion) 32 of the first semiconductor layer 21 are also in the same plane as the cavity facet 200.

[0027] Furthermore, the nitride semiconductor laser diode 10A has protrusions 81 to 84 formed by dry etching the substrate 1 in the state shown in FIG. 2(b). The protrusions 81 protrude from both the surface of the first semiconductor layer 21aa constituting the resonator end face 200 and a first upper surface 321 of the base layer 320. The protrusions 82 protrude from both the end face 32a of the first semiconductor layer 21 that is in the same plane as the end face 6A of the first electrode 6 in the resonance direction K and a second upper surface 322 of the base layer 320.

[0028] The protrusion 81 has a triangular prism shape, with one side of the triangular prism in contact with the first semiconductor layer 21aa constituting the resonator facet 200, the other side in contact with the first upper surface 321 of the base layer 320, and the remaining side facing upward as a slope. In other words, the protrusion dimension of the protrusion 81 from the upper surface of the base layer 320 is greatest at the position where the protrusion 81 protrudes from the surface of the first semiconductor layer 21aa constituting the resonator facet 200. Furthermore, a dimension W81 of the protrusion 81 in a direction perpendicular to the resonance direction K is larger than a dimension W of the connecting body 52 in a direction perpendicular to the resonance direction K.

[0029] The protrusions 83 and 84 are the surfaces of all layers (layers constituting the mesa portion 31) constituting the resonator facet 200, and protrude from both an elongated right-angled triangular surface (see the lower diagram of FIG. 2(c)) consisting of the oblique line L1 indicating the slope of the mesa portion 31, the perpendicular line L2 extending from the apex of the mesa portion 31 to the first upper surface 321 of the base layer 320, and the side along the first upper surface 321 (see the lower diagram of FIG. 2(c)), and the triangular surface of the first upper surface 321 of the base layer 320 (see the upper diagram of FIG. 2(c)). In other words, the protrusions 83 and 84 have a triangular pyramid shape with elongated triangular side surfaces.

[0030] Moreover, the convex portions 81, 83, and 84 directly transition to the first upper surface 321 of the base layer 320, which is a flat surface, on the side away from the resonator end surface. That is, the nitride semiconductor laser diode 10A does not have the convex portions 81, 83, and 84 extending up to the end surface position in the resonating direction of the base layer 320 (for example, FIG. 5 of Patent Document 3 and FIG. 2 of Patent Document 4), nor does the convex portions 81, 83, and 84 transition to the first upper surface 321 via a concave portion (the tips of the convex portions 81, 83, and 84 descend to a position lower than the first upper surface 321 and then transition to the first upper surface 321) (for example, FIG. 3 of Patent Document 5).

[0031] The reason why the protrusions 81 to 84 are formed by dry etching the substrate 1 in the state of FIG. 2(b) is that the dry etching rate using chlorine gas differs depending on the material. For example, Al x Ga (1-x) Under the condition of etching the N layer at 2.828 nm / s, SiO 2 When the film formation is performed under conditions such that the etching rate of the NiPtAu alloy layer is 0.585 nm / s and the etching rate of the NiPtAu alloy layer is 0.507 nm / s, the protrusions 81 to 84 are formed. Here, as shown in the lower diagram of Figure 2(b), the portion of mesa portion 31 that is not covered by mask 7 is considered to be divided into a central portion 31a which is located below the outer portion 51a of second alloy layer 51, an inclined portion 31b consisting of a right-angled triangle with the inclined surface of mesa portion 31 as its hypotenuse and the straight line indicating boundary position H as its base, and an end portion 31c consisting of a rectangle between the two.

[0032] In other words, Al x Ga (1-x) Since the etching rate of the mesa portion 31 which is a laminate of N layers is five times or more the etching rate of the NiPtAu alloy layer, when the end portion 31c which does not have the portion 51a which is the NiPtAu alloy layer thereon is etched up to the boundary position H, the central portion 31a which has the portion 51a which is the NiPtAu alloy layer thereon is etched only up to a position above the boundary position H at the position closest to the mask 7 in the resonance direction K. As a result, a protrusion 81 is formed.

[0033] In addition, since the insulating layer 4 is also formed on the slope of the mesa portion 31, the etching of the slope portion 31b is affected by the etching of the insulating layer 4 on the slope. In other words, the portion of the slope portion 31b that is etched after the insulating layer 4 on the slope is etched increases toward the lower side of the slope portion 31b. x Ga (1-x) The etching rate of the mesa portion 31, which is a laminate of N layers, is SiO 2 Since the etching rate is about five times that of the insulating layer 4, when the end portion 31c is etched up to the boundary position H, a part of the inclined portion 31b in the resonance direction K is left unetched and remains as the convex portions 83 and 84.

[0034] The portion of the first portion 32 that is not covered by the mask 7 is divided into a central portion 32b that is located under the outer portion 61a of the first alloy layer 61 and end portions 32c on both sides of the central portion 32b. x Ga (1-x) Since the etching rate of the N layer is five or more times the etching rate of the NiPtAu alloy layer, at the same time, the etching depth of the end portion 32c, which does not have the portion 61a which is the NiPtAu alloy layer thereon, becomes deeper than the etching depth of the central portion 32b, which has the portion 61a which is the NiPtAu alloy layer thereon.

[0035] That is, when the end portion 31c of the mesa portion 31 is etched up to the boundary position H, the end portion 32c of the first portion 32 is etched up to the second upper surface 322 which is lower than the first upper surface 321 of the underlayer 320, but the etching of the central portion 32b of the first portion 32 is only performed up to a position above the second upper surface 322 at the position closest to the mask 7 in the resonance direction K. As a result, a protrusion 82 is formed. The reason why the convex portions 81 to 84 have a triangular prism or pyramid shape is that the corners are intensively etched and scraped off.

[0036] In the nitride semiconductor laser diode of this embodiment, the first alloy layer 61 and the second alloy layer 51 are formed of the same material, but the first alloy layer 61 and the second alloy layer 51 may be formed of different materials. For example, a similar structure can be formed even if the first alloy layer 61 is a NiPtAu alloy layer and the second alloy layer 51 is a V / Al / Ti / Au layer.

[0037] [Action, effect] As described above, the manufacturing method of the nitride semiconductor laser diode of this embodiment includes an electrode layer formation step of forming the second alloy layer (layer that becomes the second electrode) 51 on the second semiconductor layer 25 of the laminate 2 up to between the cavity facet position T of the resonance region 310 and the dividing position E in the dividing step, and an etching step of successively removing the portion 51a of the second alloy layer (layer that becomes the second electrode) 51 outside the cavity facet position T in the resonance direction K and forming the cavity facet 200.

[0038] Therefore, according to the manufacturing method of the nitride semiconductor laser diode of this embodiment, it is possible to obtain a nitride semiconductor laser diode 10A in which the cavity facet 200 and the facet 5A in the resonance direction K of the second electrode 5 are on the same plane. As a result, the nitride semiconductor laser diode 10A obtained by the manufacturing method of this embodiment is expected to have a reduced threshold current density for laser oscillation. Moreover, in the manufacturing method of the nitride semiconductor laser diode of this embodiment, the above-mentioned etching step is performed by a dry etching method using mask 7, and then wet etching is performed with an alkaline aqueous solution without removing mask 7, thereby obtaining a nitride semiconductor laser diode having a highly flattened cavity facet 200.

[0039] Furthermore, in the manufacturing method of the nitride semiconductor laser diode of this embodiment, as shown in FIG. 6, before the substrate is divided at the division lines L1 and L2, both the second electrode 5 and the first electrode 6 are not continuous between adjacent element precursors, so that in the state shown in FIG. 6, a terminal connected to an external power source can be brought into contact with the second electrode 5 and the first electrode 6 to easily inspect the characteristics of each element. In contrast, if at least one of the second electrode 5 and the first electrode 6 is continuous between adjacent elements (for example, the method described in Patent Document 3), the above-mentioned inspection method cannot perform a correct inspection because multiple elements are driven simultaneously. By performing this inspection before division, it is possible to remove defective wafers, and manufacturing costs can be reduced. Also, if the elements are divided, the labor required to place each element in an inspection device during inspection increases significantly, increasing manufacturing costs. With elements in a wafer state, only one wafer needs to be placed, so costs can be significantly reduced.

[0040] Moreover, the nitride semiconductor laser diode 10A of this embodiment has a protrusion 81 protruding from both the surface of the first semiconductor layer 21aa constituting the cavity facet 200 of the cavity region 310 and the first upper surface (underlying region) 321 of the underlying layer 320. This protrusion 81 protects the portion where current and heat are concentrated (the surface of the first semiconductor layer 21aa constituting the cavity facet 200), making the portion less susceptible to corrosion due to air, water, etc. As a result, it can be expected to obtain effects such as a reduction in leakage current during current flow, an increase in light emission efficiency, and suppression of irradiation pattern fluctuation.

[0041] Furthermore, the protrusion 81 has a shape in which the protrusion dimension from the first upper surface 321 of the underlayer 320 is greatest at the protruding position from the surface of the first semiconductor layer 21aa that constitutes the resonator facet 200, and the protrusion dimension decreases to zero as the distance from this surface increases. Therefore, it is possible to suppress natural light emission and reflection / scattering of excess laser light while maintaining a high protective effect of the protrusion 81 on the surface of the first semiconductor layer 21aa that constitutes the resonator facet 200. Furthermore, since the dimension W81 of the protrusion 81 in the direction perpendicular to the resonance direction K is greater than the dimension W5 of the connector 52 which corresponds to the width of the substantial light emitting portion, the substantial light emitting portion is reliably protected by the protrusion 81.

[0042] Moreover, the nitride semiconductor laser diode 10A of the present embodiment has a protrusion 82. This protrusion 82 protects the end face 32a of the first portion 32 of the first semiconductor layer 21 that has been damaged by etching, and makes the end face 32a less susceptible to corrosion due to air, water, and the like. Moreover, the nitride semiconductor laser diode 10A of this embodiment has protrusions 83 and 84. These protrusions 83 and 84 protect both ends in the width direction of each layer constituting the cavity facet that has been damaged by etching, making these parts less susceptible to corrosion due to air, water, etc. As a result, it is expected that an effect similar to that of the protrusion 81 can be obtained.

[0043] Furthermore, since the protrusions 81, 83, 84 transition directly to the first upper surface 321 of the base layer 320, which is a flat surface, on the side away from the cavity end facets, the following effects can be expected to be obtained. That is, since the convex portions 81, 83, and 84 do not reach the end face position in the resonance direction of the underlayer 320, but the first upper surface 321 exists, the convex portions 81, 83, and 84 are protected from damage due to external physical impact. For example, when the side surface of the chip is sandwiched by a collet during assembly, the convex portions 81, 83, and 84 can be prevented from coming into direct contact with the collet, so that damage to the convex portions 81, 83, and 84 is prevented. The same can be said about the convex portion 82.

[0044] Furthermore, since the convex portions 81, 83, and 84 do not extend to the end face position in the resonance direction of the underlayer 320, and the first upper surface 321 exists, it is possible to prevent the convex portions 81, 83, and 84 from being destroyed even if chipping or cracking occurs on the end face of the element during the division process. Furthermore, since the element division line can be kept away from the light-emitting portion of the semiconductor, damage to the light-emitting portion due to heat and shock during division can be suppressed. The same can be said for the convex portion 82 when chipping or cracking occurs on the end face of the element during the division process.

[0045] Furthermore, on the side away from the resonator end face, the heat diffusion performance and deterioration resistance are improved compared to when the convex portions 81, 83, and 84 transition to the first upper surface 321 via the concave portions. This is because heat and current are concentrated in the base near these convex portions, and the semiconductor is prone to deterioration due to reaction with the outside air (oxygen, carbon), but without the concave portions, heat is more easily diffused, and the surface area is smaller due to the absence of the concave portions, so reaction with the outside air is less likely to occur, and deterioration is less likely to occur. In addition, natural light from inside the semiconductor is also emitted from underlayer 320, but if first upper surface 321 of underlayer 320 has irregularities, the light extraction efficiency of this natural light increases, resulting in noise in the laser light. Therefore, by transitioning convex portions 81, 83, and 84 to first upper surface 321 without passing through concave portions, it is possible to reduce noise in the laser light compared to transitioning to first upper surface 321 through concave portions.

[0046] Furthermore, in the nitride semiconductor laser diode 10A of this embodiment, a reflective layer 9 is formed on the cavity facet 200 and the facet 5A in the resonance direction K of the second electrode 5, and the film thickness of the reflective layer 9 is thicker on the facet 5A of the second electrode 5 than on the facet 200. In other words, a thick reflective layer that can impart a high corrosion suppression effect is formed on the facet 5A of the second electrode 5, and a reflective layer with a design film thickness (thinner than the reflective layer formed on the facet 5A) is formed on the cavity facet 200, thereby improving the durability of the nitride semiconductor laser diode.

[0047] [Differences between the first and second aspects and the embodiment] In the manufacturing method of the semiconductor laser diode of this embodiment, before the electrode layer forming step, a step of forming an insulating layer 4 on the second semiconductor layer 25 and a step of providing through holes 41, 42 at predetermined positions (positions corresponding to the electrode layer forming positions) of the insulating layer 4 are performed. As a result, the first electrode 6 and the second electrode 5 are connected to the second semiconductor layer 25 by the connectors 62, 52, respectively, and by performing the etching step via the insulating layer 4, convex portions 83, 84 are generated in the obtained semiconductor laser diode 10A. In the semiconductor laser diode 10A of this embodiment, the protrusions 83, 84 and the protrusions 81, 82 have the same protrusion dimension outward in the resonance direction K, but this protrusion dimension does not have to be the same; for example, the protrusion dimension of the protrusions 83, 84 may be larger than that of the protrusions 81, 82.

[0048] 2(b), the area covered by the mask 7 in the resonance direction K is the same for the mesa portion 31 and the first portion 32 and the second portion 33 other than the mesa portion, but the entire upper surface of the first portion 32 may be covered. In that case, the first electrode 6 is formed to have a longer dimension in the resonance direction K than the second electrode 5, and the second upper surface 322 and the convex portion 82 are not formed. In the manufacturing method of the semiconductor laser diode of this embodiment, dry etching using a mask 7 is performed as an etching process for successively removing portions 51a, 61a of the second alloy layer 51 and the first alloy layer 61 outside the cavity facet position T and forming the cavity facet 200. However, in the state of Figure 2(a), FIB processing may be performed without using a mask, in which a focused ion beam (FIB) is irradiated only outside the cavity facet position T in the resonance direction K.

[0049] Although the semiconductor laser diode 10A of this embodiment does not have a ridge semiconductor layer, a ridge semiconductor layer may be provided above a part of the second semiconductor layer 25. By providing the ridge semiconductor layer, light emission in the light emitting layer can be controlled to occur only in the region below the ridge semiconductor layer, so that the current density of the semiconductor laser diode can be increased and the laser oscillation threshold can be reduced.

[0050] In the manufacturing method of the semiconductor laser diode of this embodiment, the laminate 2 is mesa-etched to divide the first semiconductor layer 21 into a portion 21a including a portion that becomes a resonance region and the other portion 21b in the film thickness direction, and the first electrode 6 is formed on the upper surface of the other portion 21b generated by this etching. That is, the surface on which the first electrode 6 is formed (the second upper surface 322 of the base layer made of the first semiconductor layer) is formed by mesa etching. After that, patterning is performed using an etching mask different from that used for mesa etching, and then etching is performed again until the upper surface 321 of the base region reaches the position of the upper surface of the mesa-etched end face 32a, so that the upper surface of the base region becomes the upper surface of the first semiconductor layer. The depth of this re-etching may not be aligned with the position of the upper surface of the end face 32a, but may be etched below the base layer 320 made of the first semiconductor layer, for example, down to the substrate 1, so that the upper surface of the base region becomes the upper surface of the substrate 1 instead of the upper surface of the first semiconductor layer.

[0051] [Additional information on the configuration of the first and second aspects] (substrate) Specific examples of materials that form the substrate include Si, SiC, MgO, and Ga. 2 O 3 , Al 2 O 3 , ZnO, GaN, InN, AlN, or mixed crystals thereof. For ease of assembly, the substrate is preferably a thin rectangular plate, but is not limited thereto. From the viewpoint of growing high-quality crystals, the off-angle of the substrate is preferably greater than 0 degrees and less than 2 degrees. The thickness of the substrate is not particularly limited as long as the purpose is to laminate an AlGaN layer on top, but is preferably 50 μm or more and 1 mm or less.

[0052] The substrate is used for the purposes of supporting the thin films formed as the layers that make up the semiconductor laser diode, improving crystallinity, and dissipating heat to the outside. For this reason, it is preferable to use an AlN substrate, which is a material with high thermal conductivity and allows AlGaN to grow with high quality. There is no particular restriction on the crystal quality of the substrate, but to form a thin film with high luminous efficiency, a threading dislocation density of 1×10 9 cm -2 Less than or equal to 1×10 is preferred 8 cm -2 The following is more preferable. The growth surface of the substrate is preferably the commonly used +c-plane AlN because of its low cost, but it may be -c-plane AlN, a semi-polar plane substrate, or a non-polar plane substrate. When growing III-composition-gradient AlGaN, which is widely used as a p-type semiconductor, +c-plane AlN is preferable from the viewpoint of increasing the effect of polarization doping.

[0053] (First semiconductor layer) The thickness of the first semiconductor layer is not particularly limited. For example, the thickness may be 100 nm or more in order to reduce the resistance of the first semiconductor layer, or 10 μm or less in order to suppress the occurrence of cracks during the formation of the first semiconductor layer. The material for forming the first semiconductor layer is Al. x1 Ga (1-x1) N (0≦x1≦1). The material forming the first semiconductor layer may contain impurities such as a Group V element other than N, such as P, As, or Sb, a Group III element, such as In or B, or C, H, F, O, Si, Cd, Zn, or Be.

[0054] In addition, Al x Ga (1-x) The Al composition ratio x of N can be determined by exposing a cross section along the a-plane of AlGaN using a focused ion beam (FIB) device, observing the cross section with a transmission electron microscope, and performing energy dispersive X-ray analysis (EDX) of the cross section. The Al composition ratio x can be defined as the ratio of the number of moles of Al to the sum of the number of moles of Al and Ga, and can be defined using the values ​​of the number of moles of Al and Ga quantified by EDX.

[0055] When the first semiconductor layer is an n-type semiconductor, for example, Si is 1×10 19 cm -3It is possible to make it n-type by doping. If the first semiconductor layer is a p-type semiconductor, for example, Mg is added at 3×10 19 cm -3 It is possible to make the layer p-type by doping. The impurity concentration may be uniform or non-uniform throughout the layer, or may be non-uniform only in the thickness direction or only in the horizontal direction of the substrate. In addition, an intermediate layer such as an AlN layer or an AlGaN layer may be formed between the substrate 1 and the first semiconductor layer 21aa. In this case, this intermediate layer may be used as the base layer 320.

[0056] (Waveguide layer) The waveguide layer is a layer including a light-emitting layer, and is, for example, a layer in which a first guide layer, a light-emitting layer, and a second guide layer are laminated in this order, but may not include either or both of the first guide layer and the second guide layer.

[0057] (First guide layer) The first guide layer is formed on the first semiconductor layer of the first semiconductor layer. The first guide layer has a refractive index different from that of the first semiconductor layer in order to confine the light emitted from the light emitting layer in the light emitting section (the section composed of the first guide layer, the light emitting layer, and the second guide layer). Examples of materials that can be used to form the first guide layer include mixed crystals of AlN and GaN. A specific example of the material for forming the first guide layer is Al. x2 Ga (1-x2) N(0 <x2<1)である。 The first guide layer is made of Al x2 Ga (1-x2) The Al composition ratio x2 of N is the Al x1 Ga (1-x1) The Al composition ratio x1 of N may be smaller than that of the first semiconductor layer. This makes it possible for the first guide layer to have a larger refractive index than the first semiconductor layer, and to confine the light emitted from the light emitting layer in the light emitting section. The material forming the first guide layer may contain impurities such as a Group V element other than N, such as P, As, or Sb, a Group III element, such as In or B, or C, H, F, O, Si, Cd, Zn, or Be.

[0058] When the first guide layer is an n-type semiconductor, for example, Si is 1×10 19 cm -3 It is possible to make it n-type by doping. If the first guide layer is a p-type semiconductor, for example, Mg is added at 3×10 19 cm -3 It is possible to make the first guide layer p-type by doping. The first guide layer may have a dopant only in a part of the thickness direction. In other words, a part of the thickness direction of the first guide layer may be a combination of an n-type semiconductor and an undoped layer, or a p-type semiconductor and an undoped layer. The first guide layer may be an undoped layer.

[0059] The first guide layer may have a gradient structure. For example, the first guide layer may be Al x2 Ga (1-x2) The first guide layer may have a layer structure in which the Al composition ratio x2 of N changes continuously or stepwise from 0.6 to 0.5. The thickness of the first guide layer is not particularly limited. The thickness of the first guide layer may be 10 nm or more in order to efficiently confine the light emitted from the light emitting layer in the light emitting portion, and the thickness of the first guide layer may be 2 μm or less in order to reduce the resistance of the first guide layer. The first guide layer may have an AlGaN layer that serves as a blocking layer within the range in which the purpose of confining light in the light emitting portion is maintained.

[0060] (Light Emitting Layer) Examples of materials for forming the light-emitting layer include AlN, GaN, and mixed crystals thereof. x3 Ga (1-x3) N(0≦x3≦1). The Al of the light-emitting layer x3 Ga (1-x3) The Al composition ratio x of N is set to the Al of the first guide layer in order to efficiently confine the carriers injected from the first and second electrodes to the light emitting section. x2 Ga (1-x2) The Al composition ratio x3 of N may be smaller than the Al composition ratio x2. For example, the light emitting layer may be an Al x3 Ga (1-x3) It may be formed of N. In addition, the material forming the light emitting layer may contain impurities such as Group V elements other than N, such as P, As, or Sb, Group III elements, such as In or B, or C, H, F, O, Si, Cd, Zn, or Be.

[0061] When the light-emitting layer is an n-type semiconductor, for example, Si is 1×10 19 cm -3 It is possible to make it n-type by doping. If the light-emitting layer is a p-type semiconductor, for example, Mg is added at 3×10 19 cm -3 It is possible to make the light-emitting layer a p-type layer by doping it. The light-emitting layer may be an undoped layer. The light-emitting layer is, for example, Al x5 Ga (1-x5) A well layer formed of N and a layer adjacent to the well layer, for example, Al x4 Ga (1-x4) The semiconductor device may have a barrier layer made of N, and may have a multiple quantum well (MQW) structure in which well layers and barrier layers are alternately stacked one by one.

[0062] The Al composition ratio x5 of the well layer is smaller than the Al composition ratio x4 of each of the first guide layer and the second guide layer. Also, the Al composition ratio x5 of the well layer is smaller than the Al composition ratio x4 of the barrier layer. The Al composition ratio x4 of the barrier layer may be the same as the Al composition ratio x4 of each of the first guide layer and the second guide layer, or may be higher or lower than the Al composition ratio x4 of each of the first guide layer and the second guide layer. The average Al composition ratio of the well layers and the barrier layers is the Al composition ratio x of the light emitting layer. By having a light emitting layer with a multiple quantum well structure, the light emitting efficiency and light intensity of the light emitting layer can be improved.

[0063] The light-emitting layer may have a double quantum well structure, for example, "barrier layer / well layer / barrier layer / well layer / barrier layer". The thickness of each of these well layers may be, for example, 4 nm, the thickness of each of these barrier layers may be, for example, 8 nm, and the thickness of the light-emitting layer may be 32 nm. The number of quantum wells in the multiple quantum well layer may be one (i.e., a single quantum well instead of a multiple quantum well), two, three, four, or five. A single well layer is preferable for the purpose of increasing the carrier density in one well layer.

[0064] (Second guide layer) The second guide layer is formed on the light emitting layer. The second guide layer has a refractive index different from that of the second semiconductor layer in order to confine the light emitted by the light emitting layer in the light emitting portion. Examples of materials for forming the second guide layer include AlN, GaN, and mixed crystals thereof. Specific examples of materials for forming the second guide layer include Al x6 Ga (1-x6) N(0≦x6≦1). Second guide layer Al x6 Ga (1-x6) The Al composition ratio of N is x6. x5 Ga (1-x5) The Al composition ratio of N may be greater than x5. This allows carriers to be confined in the light emitting layer. The material forming the second guide layer may contain impurities such as a Group V element other than N, such as P, As, or Sb, a Group III element, such as In or B, or C, H, F, O, Si, Cd, Zn, or Be.

[0065] When the second guide layer is an n-type semiconductor, for example, Si is 1×10 19 cm -3 It is possible to make it n-type by doping. If the second guide layer is a p-type semiconductor, for example, Mg is added at 3×10 19 cm -3 It is possible to make the second guide layer p-type by doping it. The second guide layer may be an undoped layer. The second guide layer is made of Al x6 Ga (1-x6) For example, the second guide layer may have a structure in which the Al composition ratio x6 of N is graded. x6Ga (1-x6) It may have a layer structure in which the Al composition ratio x6 of N changes continuously or stepwise from 0.5 to 0.6.

[0066] The thickness of the second guide layer is not particularly limited. The thickness of the second guide layer may be 10 nm or more in order to efficiently confine the light emitted from the light emitting layer in the light emitting portion. The thickness of the second guide layer may be 2 μm or less in order to reduce the resistance of the second guide layer. Second guide layer Al x6 Ga (1-x6) The Al composition ratio x6 of N(0≦x6≦1) and the Al of the first guide layer x4 Ga (1-x4) The Al composition ratio x4 of N (0≦x4≦1) may be the same value or different values.

[0067] (Second semiconductor layer) When the second semiconductor layer is an n-type semiconductor, for example, Si is 1×10 19 cm -3 It is possible to make it n-type by doping. If the second semiconductor layer is a p-type semiconductor, for example, Mg is added at 3×10 19 cm -3 It is possible to make it p-type by doping. The dopant concentration may be uniform or non-uniform in the direction perpendicular to the substrate, and may be uniform or non-uniform in the in-plane direction of the substrate. The second semiconductor layer may have a structure in which the Al composition ratio of AlGaN is graded. When the second semiconductor layer has a layered structure, the second semiconductor layer may be an undoped layer that does not have a dopant. The second semiconductor layer may have a laminated structure further including a layer with a high doping concentration on the top layer.

[0068] The second semiconductor layer may have a laminated structure of two or more layers. In that case, it is preferable that the Al composition ratio decreases toward the upper layer in order to efficiently transport carriers to the light emitting layer. The second semiconductor layer is made of Al x7 Ga (1-x7) The Al composition ratio x7 of N may be 0.x7 Ga (1-x7) By using p-type (p-) GaN in which the Al composition ratio x7 of N is 0, the contact resistance of the second electrode disposed on the second semiconductor layer can be reduced.

[0069] (first electrode) When the first electrode is an n-type electrode, the material for the first electrode can be a material corresponding to an n-type electrode of a general nitride semiconductor light-emitting element, so long as the first electrode is used for the purpose of injecting electrons into the first semiconductor layer. For example, when the first electrode is an n-type electrode, Ti, Al, Ni, Au, Cr, V, Zr, Hf, Nb, Ta, Mo, W and alloys thereof, ITO, etc. are applicable as the material for the first electrode.

[0070] When the first electrode is a p-type electrode, the material for the first electrode can be the same as that for the p-type electrode layer of a general nitride semiconductor light-emitting device, so long as the first electrode is used for the purpose of injecting holes into the nitride semiconductor light-emitting device. For example, when the first electrode is a p-type electrode, Ni, Au, Pt, Ag, Rh, Pd, Cu and alloys thereof, ITO, etc. are applied as the material for the first electrode. When the first electrode is a p-type electrode, Ni, Au or alloys thereof, or ITO, which have a small contact resistance between the first electrode and the ridge semiconductor layer 17, may be used.

[0071] The first electrode may have a pad electrode on the upper part for the purpose of uniformly diffusing the current over the entire area of ​​the first electrode. Examples of materials for forming the pad electrode include Au, Al, Cu, Ag, and W. From the viewpoint of electrical conductivity, the pad electrode may be formed of Au, which has high electrical conductivity among these materials. Specifically, the structure of the first electrode may include a structure in which a first contact electrode made of an alloy of Ni and Au is formed on the first semiconductor layer, and a first pad electrode made of Au is formed on the first contact electrode. The first electrode is formed to a thickness of, for example, 240 nm.

[0072] (Second electrode) When the second electrode is an n-type electrode, the material for forming the second electrode can be a material corresponding to the n-type electrode of a general semiconductor laser diode, as long as the second electrode is used for the purpose of injecting electrons into the first semiconductor layer. For example, when the second electrode is an n-type electrode, Ti, Al, Ni, Au, Cr, V, Zr, Hf, Nb, Ta, Mo, W and alloys thereof, ITO, etc. are applicable as the material for forming the second electrode.

[0073] When the second electrode is a p-type electrode, the material for forming the second electrode can be the same as that for the p-type electrode layer of a general nitride semiconductor light-emitting device, so long as the second electrode is used for the purpose of injecting holes into the nitride semiconductor light-emitting device. For example, when the second electrode is a p-type electrode, Ni, Au, Pt, Ag, Rh, Pd, Cu and alloys thereof, ITO, etc. are applied as the material for forming the second electrode. When the second electrode is a p-type electrode, Ni, Au or alloys thereof, or ITO, which have a small contact resistance between the second electrode and the second semiconductor layer, may be used.

[0074] The second electrode may have a pad electrode on the upper part for the purpose of uniformly diffusing the current over the entire area of ​​the second electrode. Examples of materials for forming the pad electrode include Au, Al, Cu, Ag, and W. From the viewpoint of electrical conductivity, the pad electrode may be formed of Au, which has high electrical conductivity among these materials. Specifically, the second electrode may have a structure in which a second contact electrode made of an alloy of a material selected from Ti, Al, Ni, and Au is formed on the second semiconductor layer, and a second pad electrode made of Au is formed on the second contact electrode. The second electrode is formed to a thickness of, for example, 60 nm. The second electrode and the first electrode may be formed to different thicknesses, or may be formed to the same thickness as the first electrode. [Explanation of symbols]

[0075] 1 Board 2. Laminate 21 First semiconductor layer 21a: Mesa side portion of the first semiconductor layer (portion constituting the mesa portion of the first semiconductor layer) 21aa: A portion of the first semiconductor layer that becomes a resonant region (the first semiconductor layer that constitutes the resonator end face) 21b: A portion that will become the base layer of the first semiconductor layer 22 First guide layer (waveguide layer) 23 Light emitting layer (waveguide layer) 24 Second guide layer (waveguide layer) 25 Second semiconductor layer 31 Mesa portion (portion including the resonance region) 32 First part (part other than the mesa part) 33 Second part (part other than the mesa part) 4. Insulation Layer 5 Second electrode 5A End face of the second electrode in the resonance direction 51 Second alloy layer (layer that will become the second electrode) 51a: A portion of the second alloy layer formed outside the cavity end face position 52 Connectors 6 First electrode 6A End face of the first electrode in the resonance direction 61 First alloy layer (layer that will become the first electrode) 61a: A portion of the first alloy layer formed outside the cavity end face position 62 Connectors 7. Mask 81 Convex 82 Convex 83 Convex 84 Convex 9 Reflective layer 200 Resonator end face 310 Resonance region 320 Base layer 321 First top surface of base layer 322 Second upper surface of base layer K resonance direction

Claims

1. A method for manufacturing a semiconductor laser diode comprising: an underlayer; a resonance region formed on a part of an upper surface of the underlayer, the resonance region being formed by laminating a first semiconductor layer, a waveguide layer, and a second semiconductor layer in this order; a first electrode formed on the first semiconductor layer in the vicinity of the resonance region; and a second electrode formed on the resonance region, the first semiconductor layer of the resonance region being continuous with the first semiconductor layer on which the first electrode is formed, the method comprising the steps of: forming a plurality of the semiconductor laser diodes on a substrate and then dividing the substrate into individual semiconductor laser diodes; forming a stack including a first semiconductor layer, a waveguide layer, and a second semiconductor layer in this order on the substrate; an electrode layer forming step of forming a layer to become the second electrode on the second semiconductor layer of the laminate, between the resonator end face of the resonance region and the position to be divided in the dividing step; a first etching step for simultaneously or consecutively removing a portion of the layer to become the second electrode formed at a position outside the cavity end face and forming the cavity end face after the electrode layer forming step; A method for manufacturing a semiconductor laser diode having the structure described above.

2. The method further includes a mesa etching step of etching the laminate to divide the first semiconductor layer into a portion including a portion that becomes the resonance region and the other portion in a thickness direction, 2. The method for manufacturing a semiconductor laser diode according to claim 1, wherein said first electrode is formed on the upper surface of said other portion produced by said etching.

3. The first etching step is performed by a dry etching method using a mask, 3. The method for producing a semiconductor laser diode according to claim 1, further comprising the step of: after said first etching step, performing wet etching with an alkaline aqueous solution without removing said mask.

4. A base layer and a resonance region formed in a part of an underlying region that is a part of an upper surface of the underlying layer, the resonance region being formed by laminating a first semiconductor layer, a waveguide layer, and a second semiconductor layer in this order; a first electrode formed on the first semiconductor layer in the vicinity of the resonance region; A second electrode formed on the resonance region; a protrusion protruding from both a surface constituting a resonator end face of the resonance region and an upper surface of the base region; having the first semiconductor layer in the resonance region and the first semiconductor layer on which the first electrode is formed are continuous; the upper surface of the base region is a flat surface on a side of the protrusion away from the cavity end surface, The semiconductor laser diode has no recess between the tip of the protrusion and the upper surface.

5. 5. The semiconductor laser diode according to claim 4, wherein said cavity end face and an end face of said second electrode in the resonance direction of said resonance region are in the same plane.

6. 6. The semiconductor laser diode according to claim 4, wherein the protrusion has a maximum protruding dimension from the upper surface of the underlayer at a protruding position from the surface constituting the cavity end face.

7. the second electrode is formed on the second semiconductor layer via an insulating layer; a connector that electrically connects the second electrode and the second semiconductor layer is formed in the through hole of the insulating layer; the protrusion has a triangular prism shape, one side of the triangular prism is in contact with the first semiconductor layer constituting the cavity end face, the other side is in contact with the upper surface of the base layer, and the remaining side is present upward as an inclined surface, 7. The semiconductor laser diode according to claim 4, wherein a dimension of the protrusion in a direction perpendicular to the resonance direction of the resonance region in a plan view is larger than a dimension of the connector.

8. The semiconductor laser diode according to any one of claims 4 to 7, wherein a reflective layer is formed on the end face of the cavity and an end face of the second electrode in a resonance direction of the resonance region, and the film thickness of the reflective layer on the end face of the second electrode is thicker than that of the cavity end face.

Citation Information

Patent Citations

  • Manufacture of group iii nitride semiconductor laser diode

    JP1997283861A

  • Manufacture of group iii nitride semiconductor laser diode

    JP1998041585A

  • Manufacture of 3-nitride semiconductor laser diode

    JP1999145566A

  • Semiconductor laser element and fabrication thereof

    JP2000106470A

  • Method for manufacturing nitride semiconductor laser device and nitride semiconductor laser device

    JP2003174228A