Method for manufacturing surface-treated metal parts and aqueous surface treatment agent for processed and molded metal parts
A water-based surface treatment agent for metal components forms a film at room temperature, addressing sludge and cost issues in conventional methods by maintaining corrosion resistance and coating adhesion without heating or water washing.
Patent Information
- Application Number
- JP2023529848
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-17
- Filing Date
- 2022-06-10
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2042-06-10
AI Technical Summary
Existing surface treatment methods for metal components generate chemical sludge and require multiple processing steps, including heating and water washing, which are costly and environmentally impactful.
A method involving a water-based surface treatment agent comprising an aqueous resin, a metal compound, and a chelating agent, applied at room temperature without water washing, to form a surface treatment film, reducing sludge generation and maintaining corrosion resistance and coating adhesion.
The method achieves equivalent corrosion resistance and coating adhesion to conventional methods while significantly reducing sludge and processing costs by eliminating heating and water washing steps.
Smart Images

Figure 0007560188000001 
Figure 0007560188000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a surface-treated metal part and a water-based surface treatment agent for a processed metal part. [Background technology]
[0002] When painting the surface of a metal member, the metal member is usually subjected to a chemical conversion treatment before painting to form a chemical conversion coating on the surface of the metal member, thereby imparting corrosion resistance, paint film adhesion, and the like to the metal member.
[0003] Phosphate-based conversion coatings are generally used as conversion coatings, but in recent years, zirconium-based conversion coatings that do not contain harmful heavy metals such as nickel have also begun to be used as environmentally friendly conversion coatings.
[0004] For example, Patent Document 1 discloses a surface conditioning composition used for conditioning the surface of a metal before it is subjected to a phosphate-based chemical conversion treatment.
[0005] Patent Document 2 discloses a metal surface treatment composition containing zirconium, fluorine, and a soluble epoxy resin. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2007-297709 A [Patent Document 2] JP 2013-053326 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, both the surface conditioning composition of Patent Document 1 and the metal surface treatment composition of Patent Document 2 form a film by a chemical reaction between the surface of a metal material and a chemical conversion treatment liquid, and surface treatment processes using such surface treatment agents have problems such as the fact that the surface treatment agent cannot be used at room temperature; that chemical conversion sludge is generated as a by-product; that one or more water rinsing steps are required after the chemical conversion treatment; and that the treatment time or treatment steps are long, requiring significant equipment and costs.
[0008] Therefore, the present invention aims to provide a method for manufacturing surface-treated metal parts, which can reduce the amount of sludge generated in the chemical reaction (hereinafter simply referred to as "chemical sludge") while achieving corrosion resistance and coating adhesion equivalent to those of conventional techniques.
[0009] Another object of the present invention is to provide an aqueous surface treatment agent for processed formed metal components, which can reduce the amount of chemical conversion sludge while achieving the same corrosion resistance and coating film adhesion as those of the prior art. [Means for solving the problem]
[0010] The method for producing a surface-treated metal member according to the present invention comprises the steps of: a degreasing and water-washing step of degreasing the metal member and then washing it with water to form a degreased and water-washed metal member; a surface treatment agent contacting step in which the degreased and water-washed metal member is brought into contact with a water-based surface treatment agent to form a metal member having a liquid film on the surface; and a drying step of drying the metal member having the liquid film on its surface without washing with water to form a metal member having a surface treatment film; A method for producing a surface-treated metal member, comprising: The aqueous surface treatment agent contains an aqueous resin (A), a metal compound (B), a chelating agent (C) and water, The aqueous resin (A) comprises at least one selected from the group consisting of an aqueous epoxy resin, an aqueous polyurethane resin, and an aqueous silicone oligomer; The metal compound (B) contains one or more metal elements selected from the group consisting of magnesium, aluminum, titanium, and zirconium, the chelating agent (C) is a chelating agent having, in one molecule, at least one first metal coordination site selected from the group consisting of an amino group and a phosphonic acid group, and at least one second metal coordination site selected from the group consisting of a carboxyl group and a hydroxyl group; In the method for producing a surface-treated metal member, the solid content of the aqueous surface treatment agent is within a range of 0.01 to 6 mass % based on the total mass of the aqueous surface treatment agent, thereby making it possible to achieve corrosion resistance and coating adhesion equivalent to those of the prior art even without heating the chemical conversion treatment bath or rinsing with water after the chemical conversion treatment.
[0011] In one embodiment of the production method according to the present invention, the aqueous surface treatment agent has a solid content in the range of 0.01 to 3 mass % with respect to the total mass of the aqueous surface treatment agent.
[0012] In one embodiment of the manufacturing method according to the present invention, the metal member is a processed and formed member.
[0013] In one embodiment of the production method according to the present invention, the aqueous surface treatment agent has a fluorine ion content of less than 0.005% by mass.
[0014] In one embodiment of the production method according to the present invention, the chelating agent (C) is at least one selected from the group consisting of alcohol amines, hydroxyl group-containing organic phosphonic acid compounds, and carboxyl group-containing organic phosphonic acid compounds.
[0015] In one embodiment of the production method according to the present invention, when the number of equivalents of the metal element of the metal compound (B) is EB and the number of equivalents of the metal coordination site of the chelating agent (C) is EC, The EB relative to EC ranges from 0.50 to 4.00.
[0016] In one embodiment of the production method according to the present invention, the aqueous resin (A) is a resin having two or more groups selected from the group consisting of a primary amino group, a secondary amino group, a carboxyl group, a hydroxyl group, a urethane group, and a ureido group.
[0017] In one embodiment of the production method according to the present invention, the aqueous resin (A) contains at least one selected from the group consisting of an acrylic-modified epoxy resin, a carbon-carbon unsaturated bond-containing polyurethane resin, and an aromatic ring structure-containing polyurethane resin.
[0018] In one embodiment of the production method according to the present invention, the chelating agent (C) comprises one or more selected from the group consisting of monoethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, ethylenediaminetetraacetic acid, hydroxyethylethylenediaminetetraacetic acid, triethylenetetraminehexaacetic acid, 1,3-diamino-2-hydroxypropanetetraacetic acid, 1-hydroxyethane-1,1-diphosphonic acid, and 2-phosphonobutane-1,2,4-butanetricarboxylic acid.
[0019] The aqueous surface treatment agent according to the present invention is an aqueous surface treatment agent for processed formed metal members, The aqueous surface treatment agent contains an aqueous resin (A), a metal compound (B), a chelating agent (C) and water, The aqueous resin (A) comprises at least one selected from the group consisting of an aqueous epoxy resin, an aqueous polyurethane resin, and an aqueous silicone oligomer; The metal compound (B) contains one or more metal elements selected from the group consisting of magnesium, aluminum, titanium, and zirconium, the chelating agent (C) is at least one selected from the group consisting of alcohol amines, hydroxyl group-containing organic phosphonic acid compounds, and carboxyl group-containing organic phosphonic acid compounds; The aqueous surface treatment agent has a solid content in the range of 0.01 to 6 mass % based on the total mass of the aqueous surface treatment agent, which makes it possible to achieve corrosion resistance and coating film adhesion equivalent to those of the conventional technology even without heating the chemical conversion treatment bath or rinsing with water after the chemical conversion treatment.
[0020] In one embodiment of the aqueous surface treatment agent according to the present invention, the aqueous surface treatment agent has a solid content in the range of 0.01 to 3 mass % with respect to the total mass of the aqueous surface treatment agent. Effect of the Invention
[0021] According to the present invention, it is possible to provide a method for producing a surface-treated metal member, which can reduce the amount of chemical conversion sludge while achieving the same corrosion resistance and coating adhesion as the conventional techniques. Also, according to the present invention, it is possible to provide an aqueous surface treatment agent for processed molded metal members, which can reduce the amount of chemical conversion sludge while achieving the same corrosion resistance and coating adhesion as the conventional techniques. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, embodiments of the present invention will be described. These descriptions are intended to be illustrative of the present invention and are not intended to limit the present invention in any way.
[0023] In the present invention, two or more embodiments can be combined in any manner.
[0024] In the present invention, the terms film and coating can be used interchangeably.
[0025] In the present invention, the term "solid content" is a concept that encompasses solid content, non-volatile content, and active ingredients.
[0026] In this specification, unless otherwise specified, numerical ranges are intended to include the upper and lower limits of the range. For example, 0.01 to 6% by mass means a range of 0.01% by mass or more and 6% by mass or less.
[0027] In this specification, the aqueous resin (A), the metal compound (B), and the chelating agent (C) may be simply referred to as "component A," "component B," and "component C," respectively.
[0028] In this specification, the surface treatment agent contacting step may be simply referred to as the "contacting step."
[0029] In the present invention, a primary amino group refers to "-NH", a secondary amino group refers to ">NH", a urethane group refers to "a structure represented by -NH-(C=O)-O-", and a ureido group refers to "a structure represented by -NH-(C=O)-NH-".
[0030] In this specification, (meth)acrylic acid means "one or more selected from the group consisting of acrylic acid and methacrylic acid."
[0031] (Method of manufacturing surface-treated metal members) The method for producing a surface-treated metal member according to the present invention comprises the steps of: a degreasing and water-washing step of degreasing the metal member and then washing it with water to form a degreased and water-washed metal member; a surface treatment agent contacting step in which the degreased and water-washed metal member is brought into contact with a water-based surface treatment agent to form a metal member having a liquid film on the surface; and a drying step of drying the metal member having the liquid film on its surface without washing with water to form a metal member having a surface treatment film; A method for producing a surface-treated metal member, comprising: The aqueous surface treatment agent contains an aqueous resin (A), a metal compound (B), a chelating agent (C) and water, The aqueous resin (A) comprises at least one selected from the group consisting of an aqueous epoxy resin, an aqueous polyurethane resin, and an aqueous silicone oligomer; The metal compound (B) contains one or more metal elements selected from the group consisting of magnesium, aluminum, titanium, and zirconium, the chelating agent (C) is a chelating agent having, in one molecule, at least one first metal coordination site selected from the group consisting of an amino group and a phosphonic acid group, and at least one second metal coordination site selected from the group consisting of a carboxyl group and a hydroxyl group; In the method for producing a surface-treated metal member, the aqueous surface treatment agent has a solid content in the range of 0.01 to 6 mass % based on the total mass of the aqueous surface treatment agent.
[0032] Hereinafter, each step of the method for producing a surface-treated metal member according to the present invention will be described.
[0033] ·Degreasing and washing process In the degreasing and water-washing process, the metal component is degreased and then washed with water to form a degreased and water-washed metal component. The degreasing removes oil or dirt adhering to the surface of the metal component. The water-washing after the degreasing removes the degreaser on the surface of the metal component after the degreasing process.
[0034] The metal member is not particularly limited, and a known metal member can be used. Examples of the metal member include an iron-based substrate, an aluminum-based substrate, a zinc-based substrate, and a magnesium-based substrate. The iron-based substrate refers to a substrate in which the substrate is one or more selected from the group consisting of iron and iron alloys. The aluminum-based substrate refers to a substrate in which the substrate is one or more selected from the group consisting of aluminum and aluminum alloys. The zinc-based substrate refers to a substrate in which the substrate is one or more selected from the group consisting of zinc and zinc alloys. The magnesium-based substrate refers to a substrate in which the substrate is one or more selected from the group consisting of magnesium and magnesium alloys.
[0035] In one embodiment of the manufacturing method according to the present invention, the metal member is a processed and molded member, for example, a processed and molded member that has been subjected to laser processing, press processing, or the like.
[0036] The degreasing method is not particularly limited, and for example, the degreasing agent and degreasing conditions described in Patent Document 2 can be adopted.
[0037] Surface treatment agent contact process In the surface treatment agent contact step, the degreased and water-washed metal component is brought into contact with a water-based surface treatment agent to form a metal component having a liquid film on its surface.
[0038] Water-based surface treatment agent The aqueous surface treatment agent used in the production method of the present invention contains an aqueous resin (A), a metal compound (B), a chelating agent (C) and water, The aqueous resin (A) comprises at least one selected from the group consisting of an aqueous epoxy resin, an aqueous polyurethane resin, and an aqueous silicone oligomer; The metal compound (B) contains one or more metal elements selected from the group consisting of magnesium, aluminum, titanium, and zirconium, the chelating agent (C) is a chelating agent having, in one molecule, at least one first metal coordination site selected from the group consisting of an amino group and a phosphonic acid group, and at least one second metal coordination site selected from the group consisting of a carboxyl group and a hydroxyl group; The solid content of the aqueous surface treatment agent is within a range of 0.01 to 6% by mass with respect to the total mass of the aqueous surface treatment agent.
[0039] Component A Component A includes at least one selected from the group consisting of an aqueous epoxy resin, an aqueous polyurethane resin, and an aqueous silicone oligomer. From the viewpoint of the corrosion resistance of the chemical conversion coating on the metal member, Component A is preferably an aqueous epoxy resin.
[0040] A preferred embodiment of the water-based epoxy resin is an acrylic-modified epoxy resin, which has the advantage of ensuring good adhesion of the chemical conversion coating to the metal member.
[0041] Examples of commercially available acrylic modified epoxy resins include those sold under the trade names "MODEPIX 301", "MODEPIX 302", "MODEPIX 303" and "MODEPIX 304" manufactured by Arakawa Chemical Industries Co., Ltd.
[0042] In addition to the above, the aqueous epoxy resin may be, for example, the aqueous epoxy resins described in Patent Document 1, JP-A-2005-008975, etc.
[0043] The aqueous epoxy resin may be used alone or in combination of two or more kinds.
[0044] The aqueous polyurethane resin is not particularly limited, and for example, the aqueous polyurethane resins described in JP-A-2005-008975 can be used.
[0045] In one embodiment, the component A has at least one selected from the group consisting of a carbon-carbon unsaturated bond and an aromatic ring structure in the molecule.
[0046] In one embodiment of the manufacturing method according to the present invention, the aqueous resin (A) is a resin having two or more types of groups selected from the group consisting of a primary amino group (-NH2), a secondary amino group (>NH), a carboxyl group, a hydroxyl group, a urethane group, and a ureido group. From the viewpoint of enhancing the corrosion resistance of the chemical conversion coating, it is preferable that the aqueous resin (A) is a resin having two or more types of the functional groups.
[0047] The aqueous polyurethane resin is not particularly limited, and examples thereof include those obtained by reacting a polyol compound with a diisocyanate compound, further chain-extending the reacted compound with a diamine or the like, and dispersing the reacted compound in water.
[0048] Commercially available aqueous polyurethane resins may be used, such as those available under the trade names "HUX-320" and "HUX-550" from ADEKA Corporation, "Superflex (registered trademark)" from Daiichi Kogyo Seiyaku Co., Ltd., and "Hydran (registered trademark)" from DIC Corporation.
[0049] The aqueous polyurethane resin may be used alone or in combination of two or more kinds.
[0050] The aqueous silicone oligomer is not particularly limited, and for example, the silicone oligomer (A) described in Japanese Patent No. 6058843 can be used.
[0051] The silicone oligomer may be a commercially available one. Examples of commercially available products include methyl methoxy oligomers such as "KC-89", "KR-500", "X-40-9225", "X-40-9246", and "X-40-9250" manufactured by Shin-Etsu Chemical Co., Ltd.; phenyl methoxy oligomers such as "KR-217"; aminosilane oligomers such as condensates of "KBM-903", methyl / phenyl methoxy oligomers such as "KR-9218", "KR-213", "KR-510", "X-40-9227", "X-40-9247", and "KR-401N"; and methyl methoxy oligomers such as "MSE-100" manufactured by Wacker Silicone Co., Ltd.
[0052] The aqueous silicone oligomer may be used alone or in combination of two or more kinds.
[0053] In one embodiment of the production method according to the present invention, the aqueous resin (A) contains at least one selected from the group consisting of an acrylic-modified epoxy resin, a carbon-carbon unsaturated bond-containing polyurethane resin, and an aromatic ring structure-containing polyurethane resin.
[0054] The amount of the A component may be appropriately adjusted, for example, 20 to 80% by mass relative to the total solid content in the aqueous surface treatment agent. In one embodiment, the amount of the A component is 20% by mass or more, 30% by mass or more, 40% by mass or more, 50% by mass or more, 60% by mass or more, or 70% by mass or more relative to the total solid content in the aqueous surface treatment agent. In another embodiment, the amount of the A component is 80% by mass or less, 70% by mass or less, 60% by mass or less, 50% by mass or less, 40% by mass or less, or 30% by mass or less relative to the total solid content in the aqueous surface treatment agent.
[0055] ·B component Component B contains one or more metal elements selected from the group consisting of magnesium, aluminum, titanium and zirconium. Component B, together with Component A, functions to impart good corrosion resistance.
[0056] Examples of component B include carbonates, phosphates, nitrates, sulfates, acetates, oxides, hydroxides, organic acid salts, complex compounds, etc., each containing the above metal element. Component B may be a single salt or a double salt.
[0057] Examples of the magnesium-containing component B include magnesium nitrate, magnesium sulfate, magnesium acetate, and magnesium oxide.
[0058] Examples of the aluminum-containing component B include aluminum nitrate, aluminum sulfate, aluminum acetate, and aluminum oxide.
[0059] Examples of the titanium-containing component B include titanium nitrate, titanyl nitrate, titanyl sulfate, titanium sulfate, titanium oxide, diisopropoxytitanium bisacetylacetone, a reaction product of lactic acid and titanium alkoxide, titanium laurate, titanium acetylacetonate, and barium titanate.
[0060] Examples of the zirconium-containing component B include zirconyl nitrate, zirconyl acetate, zirconium acetate, zirconium sulfate, zirconyl sulfate, titanium sulfate, basic zirconium sulfate, zirconium oxyphosphate, zirconium phosphate, sodium zirconium phosphate, ammonium zirconyl carbonate, ammonium zirconium carbonate, potassium zirconium carbonate, basic zirconium carbonate, zirconium oxide, zirconium hydroxide, zirconium acetylacetonate, and calcium zirconate.
[0061] As the component B, a metal compound containing zirconium can be suitably used, and for example, ammonium zirconium carbonate, potassium zirconium carbonate, etc. can be particularly suitably used.
[0062] The component B may be used alone or in combination of two or more.
[0063] The amount of the B component may be appropriately adjusted, and is, for example, 10 to 70% by mass relative to the total solid content in the aqueous surface treatment agent. In one embodiment, the amount of the B component is 10% by mass or more, 20% by mass or more, 25% by mass or more, 30% by mass or more, 40% by mass or more, 50% by mass or more, or 60% by mass or more relative to the total solid content in the aqueous surface treatment agent. In another embodiment, the amount of the B component is 70% by mass or less, 60% by mass or less, 50% by mass or less, 40% by mass or less, 30% by mass or less, or 20% by mass or less relative to the total solid content in the aqueous surface treatment agent.
[0064] In one embodiment of the production method according to the present invention, when the number of equivalents of the metal element in the metal compound (B) is EB and the number of equivalents of the metal coordination site in the chelating agent (C) is EC, EB relative to EC is in the range of 0.50 to 4.00.
[0065] An example of the calculation of EB for EC will be described based on Example 1 described later. Ammonium zirconium carbonate (NH4)2ZrO(CO3)2, which is component B, is treated as 263.33 g / mol, and diethanolamine is treated as 105.14 g / mol. (NH4)2ZrO(CO3)2: 99.6 parts by mass in Example 1 is 99.6 / 263.33 = 0.378 mol = 378 mmol. Here, 1 mol of (NH4)2ZrO(CO3)2 contains 1 mol of Zr, so EB is 378 mmol. Meanwhile, diethanolamine: 9.9 parts by mass (effective ingredient equivalent) in Example 1 is 9.9 / 105.14 = 0.0942 mol = 94.2 mmol. Since the number of metal coordination sites of diethanolamine is 3 (2 hydroxyl groups, 1 NH group), the number of moles of metal coordination sites, i.e., EC, is 94.2 mmol × 3 = 282.6 mmol. Then, EB / EC = 378 / 282.6 = 1.337 = approximately 1.34.
[0066] ·C component Component C is a chelating agent having, per molecule, at least one first metal coordination site selected from the group consisting of amino groups and phosphonic acid groups, and at least one second metal coordination site selected from the group consisting of carboxyl groups and hydroxyl groups.
[0067] Examples of the chelating agent that can be preferably used include alcohol amines, hydroxyl group-containing organic phosphonic acid compounds, and carboxyl group-containing organic phosphonic acid compounds.
[0068] Examples of the alcohol amine include monoethanolamine, diethanolamine, triethanolamine, N-butylethanolamine, N-methylethanolamine, 2-amino-2-methyl-1-propanol, dimethylethanolamine, dibutylethanolamine, and methyldiethanolamine.
[0069] Examples of hydroxy group-containing organic phosphonic acid compounds include hydroxymethanediphosphonic acid, 1-hydroxyethane-1,1-diphosphonic acid, and 1-hydroxypropane-1,1-diphosphonic acid.
[0070] Examples of the carboxyl group-containing organic phosphonic acid compound include 2-hydroxyphosphonoacetic acid and 2-phosphonobutane-1,2,4-butanetricarboxylic acid.
[0071] In one embodiment of the production method according to the present invention, the chelating agent (C) is at least one selected from the group consisting of alcohol amines, hydroxyl group-containing organic phosphonic acid compounds, and carboxyl group-containing organic phosphonic acid compounds.
[0072] As the component C, alcohol amines can be particularly preferably used.
[0073] In one embodiment of the production method according to the present invention, the chelating agent (C) comprises one or more selected from the group consisting of monoethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, ethylenediaminetetraacetic acid, hydroxyethylethylenediaminetetraacetic acid, triethylenetetraminehexaacetic acid, 1,3-diamino-2-hydroxypropanetetraacetic acid, 1-hydroxyethane-1,1-diphosphonic acid, and 2-phosphonobutane-1,2,4-butanetricarboxylic acid.
[0074] The component C may be used alone or in combination of two or more.
[0075] The amount of the C component may be appropriately adjusted, and is, for example, 2 to 30% by mass relative to the total solid content in the aqueous surface treatment agent. In one embodiment, the amount of the C component is 2% by mass or more, 5% by mass or more, 10% by mass or more, 15% by mass or more, 20% by mass or more, or 25% by mass or more relative to the total solid content in the aqueous surface treatment agent. In another embodiment, the amount of the C component is 30% by mass or less, 25% by mass or less, 20% by mass or less, 15% by mass or less, 10% by mass or less, or 5% by mass or less relative to the total solid content in the aqueous surface treatment agent.
[0076] The aqueous surface treatment agent contains water. The amount of water can be set so that the solid content of the aqueous surface treatment agent is within the range of 0.01 to 6 mass % relative to the total mass of the aqueous surface treatment agent. The aqueous surface treatment agent can contain an organic solvent within a range that does not impair the effects of the present invention.
[0077] The solid content of the aqueous surface treatment agent is within a range of 0.01 to 6 mass % relative to the total mass of the aqueous surface treatment agent, and is preferably 0.1 to 3 mass % or 0.1 to 1 mass %.
[0078] The aqueous surface treatment agent may be free of fluorine ions, or may contain fluorine ions as unavoidable impurities.
[0079] In one embodiment of the production method according to the present invention, the aqueous surface treatment agent does not contain fluorine ions or contains fluorine ions as unavoidable impurities.
[0080] The method of contacting the degreased and water-washed metal member with the aqueous surface treatment agent is not particularly limited, and examples thereof include an immersion method, a spray method, a roll coating method, a bar coating method, etc. Alternatively, the aqueous surface treatment agent may be poured onto the degreased and water-washed metal member to contact it.
[0081] The conditions for contacting the degreased and water-washed metal member with the aqueous surface treatment agent are not particularly limited, including temperature and time. The temperature of the aqueous surface treatment agent during contact can be, for example, 10 to 40° C., which is the same as the outside air temperature. The contact time can be set arbitrarily depending on the conditions of the equipment and members to be used, and can be, for example, 10 to 30 seconds.
[0082] In the present invention, by using the above-mentioned aqueous surface treatment agent, the temperature of the aqueous surface treatment agent in the contact step can be set to a temperature lower than conventionally, such as room temperature. When the aqueous surface treatment agent freezes in a cold environment, the aqueous surface treatment agent may be heated to the minimum necessary level to melt the aqueous surface treatment agent, but the aqueous surface treatment agent does not need to be heated in a normal environment. In one embodiment, the contact step does not involve a heating means for maintaining the temperature of the aqueous surface treatment agent at 40° C. or higher, 38° C. or higher, or 35° C. or higher.
[0083] The solid content of the liquid film formed on the surface of the metal member in the contact step is, for example, in the range of 0.01 to 6 mass %.
[0084] The solid content of the liquid film formed in the surface treatment agent contact step is in the range of 0.01 to 6 mass % in each case.
[0085] ·Drying process In the drying step, the metal member having the liquid film on its surface is dried without washing with water to form a metal member having a surface treatment film. By drying without washing with water, it is possible to reduce wastewater costs and industrial waste costs. In addition, the present invention does not generate sludge that is generated in the chemical conversion reaction.
[0086] Conventional reactive conversion coatings have the following three problems if water rinsing is not performed, and water rinsing is performed to avoid these problems. The first problem is that the reactive conversion coating solution remains on the surface of the metal component, making it impossible to control the film reaction and resulting in the failure to obtain the desired film; the second problem is that general reactive conversion coating agents are acidic, and if they remain on the surface of metal components such as steel sheets, they can cause process rust; the third problem is that reactive conversion coatings produce conversion sludge during treatment, which adheres to the surface of the metal component, and this adhesion can lead to abnormal appearance of the paint after conversion.
[0087] In contrast, in the present invention, the above-mentioned aqueous surface treatment agent is a non-reactive type, and the formation of the surface treatment film does not involve a chemical conversion reaction. Since no chemical conversion reaction is involved, no sludge is generated, which is generated by the chemical conversion reaction. Therefore, the manufacturing method of the present invention does not require the water washing required in the above-mentioned conventional reactive chemical conversion treatment.
[0088] The drying temperature and drying time after application of the surface treatment agent are not particularly limited, and may be any temperature and time that evaporates unnecessary components (e.g., moisture, organic solvent, etc.) from the coating. For example, a method such as drying for 3 minutes in a hot air dryer (such as "PHH-202" manufactured by Espec Corp.) at 100°C can be used. If necessary, air blowing or the like may be performed before drying to remove excess treatment solution before drying.
[0089] The dry thickness of the surface treatment film formed by drying is not particularly limited, and is, for example, 0.001 to 1.0 μm. In one embodiment, the dry thickness of the surface treatment film is 0.002 to 1.0 μm or 0.002 to 0.5 μm. In another embodiment, the dry thickness of the surface treatment film is 0.002 μm or more, 0.005 μm or more, 0.010 μm or more, 0.050 μm or more, 0.100 μm or more, 0.500 μm or more, or 1.000 μm or more. In yet another embodiment, the dry thickness of the surface treatment film is 2.000 μm or less, 1.000 μm or less, 0.500 μm or less, 0.100 μm or less, 0.050 μm or less, 0.010 μm or less, or 0.005 μm or less.
[0090] Other processes The method for producing a surface-treated metal member of the present invention may include any other steps in addition to the degreasing and water-washing step, the contacting step, and the drying step, such as a coating step in which a coating composition is applied onto the metal member or onto the surface treatment film after the drying step to form a coating film.
[0091] The coating composition used in the coating step is not particularly limited and may be appropriately selected depending on the application.
[0092] The coating method in the coating step is not particularly limited, and any known coating method can be used, such as a dipping method, a spray method, a roll coating method, a bar coating method, a brush coating method, a roller coating method, etc. In one embodiment, the coating method in the coating step is a spray method.
[0093] (Water-based surface treatment agent) The aqueous surface treatment agent according to the present invention is an aqueous surface treatment agent for processed formed metal members, The aqueous surface treatment agent contains an aqueous resin (A), a metal compound (B), a chelating agent (C) and water, The aqueous resin (A) comprises at least one selected from the group consisting of an aqueous epoxy resin, an aqueous polyurethane resin, and an aqueous silicone oligomer; The metal compound (B) contains one or more metal elements selected from the group consisting of magnesium, aluminum, titanium, and zirconium, the chelating agent (C) is at least one selected from the group consisting of alcohol amines, hydroxyl group-containing organic phosphonic acid compounds, and carboxyl group-containing organic phosphonic acid compounds; The aqueous surface treatment agent has a solid content in the range of 0.01 to 6 mass % with respect to the total mass of the aqueous surface treatment agent.
[0094] The aqueous surface treatment agent described in the contact step of the method for producing the surface-treated metal member (hereinafter, sometimes referred to as the "first aqueous surface treatment agent") and the aqueous surface treatment agent according to the present invention (hereinafter, sometimes referred to as the "second aqueous surface treatment agent") differ in the scope of the C component, but the other components and amounts are similar. More specifically, in the first aqueous surface treatment agent, the C component is a chelating agent having one or more first metal coordination sites selected from the group consisting of amino groups and phosphonic acid groups and one or more second metal coordination sites selected from the group consisting of carboxyl groups and hydroxyl groups in one molecule, whereas in the second aqueous surface treatment agent, the C component is one or more selected from the group consisting of alcohol amines, hydroxyl group-containing organic phosphonic acid compounds, and carboxyl group-containing organic phosphonic acid compounds, and the C component of the first aqueous surface treatment agent is broader in a higher concept than the C component of the second aqueous surface treatment agent.
[0095] The one or more compounds selected from the group consisting of alcohol amines, hydroxyl group-containing organic phosphonic acid compounds and carboxyl group-containing organic phosphonic acid compounds, which are component C of the second aqueous surface treatment agent, are as described for component C of the first aqueous surface treatment agent.
[0096] The second aqueous surface treatment agent is for treating the surface of a processed and molded metal member, such as a processed and molded metal member that has been subjected to laser processing, press processing, or the like.
[0097] In the aqueous surface treatment agent of the present invention, additives such as inorganic or organic general rust inhibitors and surface conditioners may be used in addition to the components A to C, so long as they do not impair the purpose of the agent. Examples of such additives include imidazole and benzotriazole. EXAMPLES
[0098] The present invention will be described in more detail below by way of examples. However, these examples are intended to illustrate the present invention and are not intended to limit the present invention in any way.
[0099] The materials of the aqueous surface treatment agents used in the examples are as follows: Component A Water-based epoxy resin: Trade name "EPICLON (registered trademark) H-502-42W" manufactured by DIC Corporation, water-based modified phenoxy resin, solid content 39 to 43 mass%, having hydroxyl groups and carboxyl groups, referred to as "Epiclon" in Tables 1 and 2 Water-based epoxy resin: Trade name "MODEPICS (registered trademark) 301" manufactured by Arakawa Chemical Industries, Ltd., solid content 32 to 34%, having hydroxyl groups and carboxyl groups, referred to as "MODEPICS" in Tables 1 and 2 Water-based polyurethane resin: ADEKA Corporation's product name "HUX-320", solid content 30-34%, aromatic ring structure-containing polyurethane resin with urethane groups and carboxyl groups. In Table 1, it is referred to as "HUX320". Water-based polyurethane resin: ADEKA Corporation's product name "HUX-550", solid content 26.5-29.5%, aromatic ring structure-containing polyurethane resin with urethane groups and carboxyl groups, referred to as "HUX550" in Table 1 Water-based silicone oligomer: A solution of hydrolysis condensation product of Shin-Etsu Chemical Co., Ltd.'s product name "KBM-903", solid content 20%, containing hydroxyl groups and primary amino groups, referred to as "903 condensation product" in Table 1 ·Comparison A component Acrylic resin: "NP-900A" manufactured by Saiden Chemical Industry Co., Ltd., solid content 47-49%, referred to as "900A" in Table 2 ·B component Ammonium zirconium carbonate: Trade name "Zircosol AC-7" manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd., (NH4)2ZrO(CO3)2, solid content 29%, referred to as "AC-7" in Tables 1 and 2 Zirconyl nitrate: Trade name "EKZ-5" manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd., ZrO(NO3)2, solid content 40%, indicated as "ZN" in Table 1 Titanium diisopropoxybis(triethanolamine): Matsumoto Fine Chemical Co., Ltd.'s trade name "Orgatics TC-400", Ti(Oi-C3H7)2(C6H 14 O3N)2, solids content 79%, in Table 1 it is called "TC400" Aluminum acetate: "Basic aluminum acetate" reagent manufactured by Fujifilm Wako Pure Chemical Industries, Al(OH)(CH3COO)2, 100% solids, referred to as "Al acetate" in Table 1 Magnesium oxide: "Magnesium oxide" reagent manufactured by Fujifilm Wako Pure Chemical Industries, MgO, 100% solid content, referred to as "MgO" in Table 1 ·C component Diethanolamine: "Diethanolamine" reagent manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., alcoholamine, molecular weight 105.14, has one amino group as the first metal coordination site and two hydroxyl groups as the second metal coordination sites; active ingredient concentration 99% or more, referred to as "diethanolamine" in Tables 1 and 2. Triethanolamine: 2,2',2"-nitrilotriethanol, a reagent manufactured by Fujifilm Wako Pure Chemical Industries, an alcoholamine with a molecular weight of 149.19, which has one amino group as the first metal coordination site and three hydroxyl groups as the second metal coordination sites; active ingredient concentration of 98% or more; in Tables 1 and 2, referred to as "triethanolamine" 1-Hydroxyethane-1,1-diphosphonic acid: Trade name "PH-210" manufactured by Chelest Co., Ltd., molecular weight 206.03, has two phosphonic acid groups as the first metal coordination site and one hydroxyl group as the second metal coordination site; solid content 60%, represented as "HEDP" in Table 1 2-Phosphonobutane-1,2,4-tricarboxylic acid: trade name "PH-430" manufactured by Chelest Corporation, molecular weight 270.13, has one phosphonic acid group as the first metal coordination site and three carboxyl groups as the second metal coordination sites; solid content 50%, represented as "PBTC" in Table 1 ·Comparison C component Citric acid: Fujifilm Wako Pure Chemical Industries, molecular weight 192.123, solid content 100%, indicated as "CA" in Table 2 Acetylacetone: Fujifilm Wako Pure Chemical Industries, molecular weight 100.117, active ingredient concentration 99% or more, indicated as "AA" in Table 2 Surface treatment agent for zinc phosphate treatment: Nippon Paint Surf Chemicals' product name "Surfdyne 6350"
[0100] The other materials are as follows: Degreaser: Nippon Paint Surf Chemicals' product name "Surf Cleaner 53NF" Surface conditioner: Nippon Paint Surf Chemicals' product name "Surf Fine GL1" Powder paint: Nippon Paint Industrial Coatings' product name "Bilusia PL1000" Metal parts: Cold-rolled steel plate (SPC270D, manufactured by Pultec) Cellophane tape: Product name "Cellotape (registered trademark)" manufactured by Nichiban Co., Ltd.
[0101] Examples 1 to 17 and Comparative Examples 1 to 3 Each component was mixed with water in the proportions shown in Tables 1 and 2 to prepare an aqueous surface treatment agent. The amount of each component is expressed as parts by mass of solid content. The solid content of the aqueous surface treatment agent is also shown in Tables 1 and 2. The value of the number of equivalents EB of the metal element in component B relative to the number of equivalents EC of the metal coordination site in component C is also shown in Tables 1 and 2. In preparing the aqueous surface treatment agents of Examples 1 to 17 and Comparative Examples 1 to 3, no fluoride ions were added.
[0102] As the surface treatment agent for Comparative Example 4, Surfdyne 6350, a surface treatment agent for zinc phosphate treatment, was used.
[0103] [Table 1]
[0104] [Table 2]
[0105] ·Degreasing and washing process A cold-rolled steel sheet, which is a metal member, was degreased by immersion in a degreaser heated to 40° C. for 120 seconds, and then thoroughly rinsed with tap water to obtain a degreased and water-washed metal member.
[0106] Surface treatment agent contact process The aqueous surface treatment agent prepared in Example 1 was sprayed onto the degreased and water-washed metal member for 30 seconds at room temperature of 25° C. without heating, so that the metal member was brought into contact with the aqueous surface treatment agent, and a liquid film of the aqueous surface treatment agent was formed on the surface of the metal member.
[0107] ·Drying process The metal member having the liquid film on its surface was dried in a dryer at a temperature of 100° C. without being washed with water to obtain a metal member having a surface treatment film. The dry thickness of the surface treatment film was 0.06 μm.
[0108] Painting process Next, a powder coating was sprayed onto the surface treatment film to a dry film thickness of 60 μm or more, and then dried to form a coating film.
[0109] In Examples 2 to 17 and Comparative Examples 1 to 3, the same four steps as in Example 1 were carried out, except that the aqueous surface treatment agent in Example 1 was replaced with the aqueous surface treatment agent in each Example or Comparative Example, and a surface treatment film and a coating film were formed in that order from the metal member side. The dry film thickness of the surface treatment film was in the range of 0.002 to 0.5 μm in all cases except for Example 17. The dry film thickness of the surface treatment film in Example 17 was in the range of 0.002 to 1.0 μm.
[0110] In Comparative Example 4, a degreasing and water washing step was carried out in the same manner as in Example 1. Then, a surface conditioning treatment was carried out by immersion at room temperature for 30 seconds using a surface conditioner. Then, a chemical conversion treatment was carried out by immersion at 35°C for 2 minutes using a zinc phosphate treatment agent. Then, after thorough water washing with tap water, a water washing with pure water was also carried out. Then, a drying step and a painting step were carried out in the same manner as in Example 1, and a surface treatment film and a coating film were formed in that order from the metal member side. The dry film thickness of the surface treatment film was 2 μm. In Comparative Example 4, sludge was generated during the chemical conversion treatment using the zinc phosphate treatment agent.
[0111] The metal members having the surface treatment films and coating films obtained in each of the Examples and Comparative Examples were subjected to the following tests to evaluate the corrosion resistance and coating adhesion. The results are shown in Tables 1 and 2.
[0112] - Preparation of corrosion-resistant test plates A cross-cut (cut length 5 cm) was made on the coating surface of the metal member to prepare a test plate.
[0113] Corrosion resistance (SST) test The test plate was subjected to a salt spray test (SST) for 500 hours under the conditions of JIS Z 2371:2015. Cellophane tape was then applied to the cross-cut area, and the cellophane tape was peeled off to measure the maximum peel width on one side from the cross-cut area. The test plate was then scored according to the following criteria. 4 and 5 points are pass. 5 points: No peeling 4 points: Peeling occurs, maximum peeling width is less than 3 mm 3 points: Maximum peel width is 3 mm or more and less than 5 mm 2 points: Maximum peel width is 5 mm or more and less than 10 mm 1 point: Maximum peel width is 10mm or more
[0114] Corrosion resistance (CCT) test The test plates were subjected to a combined cycle test (CCT) for up to 500 hours under the conditions of JASO M609. The maximum blister width from the cross cut was measured and a score was given according to the following criteria. 4 and 5 points are pass. 5 points: Blister present, maximum blister width less than 3 mm 4 points: Maximum swelling width is 3mm or more but less than 5mm 3 points: Maximum swelling width is 5mm or more but less than 7mm 2 points: Maximum swelling width is 7mm or more but less than 10mm 1 point: Maximum swelling width is 10mm or more
[0115] Corrosion resistance (SDT) test The test panels were subjected to a saltwater immersion test (SDT) for 500 hours at 25°C in saltwater with a NaCl concentration of 3%. As with the SST test, the maximum peel width on one side from the cross-cut was measured. The test panels were scored according to the following criteria. 4 and 5 points are pass. 5 points: No peeling 4 points: Peeling occurs, maximum peeling width is less than 3 mm 3 points: Maximum peel width is 3 mm or more and less than 5 mm 2 points: Maximum peel width is 5 mm or more and less than 10 mm 1 point: Maximum peel width is 10mm or more
[0116] - Preparation of test panels for coating adhesion A test plate was prepared by making a checkerboard pattern of 100 squares spaced 1 mm apart on the coating surface of a metal member.
[0117] Coating adhesion test Cellophane tape was applied to the scratched area of the test panel, and the cellophane tape was then peeled off, and the number of 1 mm square pieces of coating film remaining on the test panel that had not peeled off was counted. Then, a score was given based on the following criteria. 4 points and 5 points are pass. 5 points: 100 coatings remaining 4 points: 80 to less than 100 paint particles remaining 3 points: 60 to less than 80 paint particles remaining 2 points: 40 or more but less than 60 remaining coatings 1 point: Less than 40 coatings remaining
[0118] Storage stability test The aqueous surface treatment agents obtained in the Examples and Comparative Examples and the zinc phosphate treatment surface treatment agent of Comparative Example 4 were left to stand in a thermostatic chamber at 40° C. for 30 days. The treatment agents were then visually inspected for the presence or absence of gelation or sediment and evaluated according to the following criteria. The results are shown in Tables 1 and 2. Pass: No gelation or sedimentation Fail: Gelling or sedimentation
[0119] According to the present invention, it is possible to provide a method for producing a surface-treated metal member, which can reduce the amount of chemical conversion sludge while achieving the same corrosion resistance and coating adhesion as the conventional technology. Also, according to the present invention, it is possible to provide a water-based surface treatment agent for processed molded metal members, which can reduce the amount of chemical conversion sludge while achieving the same corrosion resistance and coating adhesion as the conventional technology. [Industrial Applicability]
[0120] According to the present invention, it is possible to provide a method for producing a surface-treated metal member, which can reduce the amount of chemical conversion sludge while achieving the same corrosion resistance and coating adhesion as the conventional techniques. Also, according to the present invention, it is possible to provide an aqueous surface treatment agent for processed molded metal members, which can reduce the amount of chemical conversion sludge while achieving the same corrosion resistance and coating adhesion as the conventional techniques.
Claims
1. a degreasing and water-washing step of degreasing the metal member and then washing it with water to form a degreased and water-washed metal member; a surface treatment agent contacting step in which the degreased and water-washed metal member is brought into contact with a water-based surface treatment agent to form a metal member having a liquid film on the surface; and a drying step of drying the metal member having the liquid film on its surface without washing with water to form a metal member having a surface treatment film; A method for producing a surface-treated metal member, comprising: The aqueous surface treatment agent contains an aqueous resin (A), a metal compound (B), a chelating agent (C) and water, The aqueous resin (A) includes at least one selected from the group consisting of an aqueous epoxy resin, an aqueous polyurethane resin, and an aqueous silicone oligomer, The metal compound (B) contains one or more metal elements selected from the group consisting of magnesium, aluminum, titanium, and zirconium, the chelating agent (C) is a chelating agent having, in one molecule, at least one first metal coordination site selected from the group consisting of an amino group and a phosphonic acid group, and at least one second metal coordination site selected from the group consisting of a carboxyl group and a hydroxyl group; the solid content of the aqueous surface treatment agent is within a range of 0.01 to 6 mass % based on the total mass of the aqueous surface treatment agent; When the number of equivalents of the metal element of the metal compound (B) is EB and the number of equivalents of the metal coordination site of the chelating agent (C) is EC, EB to EC is in the range of 0.40 to 4.26; A method for manufacturing a surface-treated metal member.
2. The method according to claim 1, wherein the aqueous surface treatment agent has a solid content in the range of 0.01 to 3 mass % based on the total mass of the aqueous surface treatment agent.
3. The manufacturing method according to claim 1 or 2, wherein the metal member is a processed member.
4. The method according to claim 1 or 2, wherein the aqueous surface treatment agent does not contain fluorine ions or contains fluorine ions as unavoidable impurities.
5. 3. The method according to claim 1, wherein the chelating agent (C) is at least one selected from the group consisting of alcohol amines, hydroxyl group-containing organic phosphonic acid compounds, and carboxyl group-containing organic phosphonic acid compounds.
6. A manufacturing method described in claim 1 or 2, wherein EB relative to EC is in the range of 0.50 to 4.
00.
7. 3. The method according to claim 1, wherein the aqueous resin (A) is a resin having two or more groups selected from the group consisting of a primary amino group, a secondary amino group, a carboxyl group, a hydroxyl group, a urethane group, and a ureido group.
8. The method according to claim 1 or 2, wherein the aqueous resin (A) comprises at least one selected from the group consisting of an acrylic-modified epoxy resin, a carbon-carbon unsaturated bond-containing polyurethane resin, and an aromatic ring structure-containing polyurethane resin.
9. The production method according to claim 1 or 2, wherein the chelating agent (C) comprises one or more selected from the group consisting of monoethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, ethylenediaminetetraacetic acid, hydroxyethylethylenediaminetetraacetic acid, triethylenetetraminehexaacetic acid, 1,3-diamino-2-hydroxypropanetetraacetic acid, 1-hydroxyethane-1,1-diphosphonic acid, and 2-phosphonobutane-1,2,4-butanetricarboxylic acid.
10. A water-based surface treatment agent for processed metal parts, comprising: The aqueous surface treatment agent contains an aqueous resin (A), a metal compound (B), a chelating agent (C) and water, The aqueous resin (A) includes at least one selected from the group consisting of an aqueous epoxy resin, an aqueous polyurethane resin, and an aqueous silicone oligomer, The metal compound (B) contains one or more metal elements selected from the group consisting of magnesium, aluminum, titanium, and zirconium, the chelating agent (C) is at least one selected from the group consisting of alcohol amines, hydroxyl group-containing organic phosphonic acid compounds, and carboxyl group-containing organic phosphonic acid compounds; the solid content of the aqueous surface treatment agent is within a range of 0.01 to 6 mass % based on the total mass of the aqueous surface treatment agent; When the number of equivalents of the metal element of the metal compound (B) is EB and the number of equivalents of the metal coordination site of the chelating agent (C) is EC, An aqueous surface treatment agent having an EB to EC ratio in the range of 0.40 to 4.
26.
11. The aqueous surface treatment agent according to claim 10, wherein the aqueous surface treatment agent has a solid content in the range of 0.01 to 3 mass % based on the total mass of the aqueous surface treatment agent.
Citation Information
Patent Citations
Method for coating a metal surface with a polymer-rich composition
JP2006519308A
Surface conditioning composition, method for producing the same, and surface conditioning method
JP2007297709A
Metal surface-treating composition
JP2013053326A
Chromium-free metal surface treatment agent
JP2014208874A
Surface-conditioning composition, method for production thereof, and surface conditioning method
WO2007020985A1