Composition for negative electrode, negative electrode sheet and non-aqueous secondary battery, and method for producing the negative electrode sheet and non-aqueous secondary battery
A carbon-coated silicon oxide negative electrode composition with a specific binder formulation addresses volume change issues, enhancing the cycle life and performance of non-aqueous secondary batteries by improving binding and conductivity.
Patent Information
- Application Number
- JP2023511395
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-31
- Filing Date
- 2022-03-29
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2042-03-29
AI Technical Summary
Lithium ion secondary batteries using silicon oxide as a negative electrode active material face challenges with volume change during charging and discharging, leading to reduced cycle life and performance deterioration, despite advancements in carbon coating and binder technologies.
A negative electrode composition using carbon-coated silicon oxide with a binder containing a water-soluble polymer having a weight average molecular weight of 300,000 or less and a limited acid group content of 5% by mass or less, which enhances the binding and anchoring effect, resulting in improved mechanical strength and electron conductivity.
The composition achieves high capacity, low resistance, and excellent cycle characteristics in non-aqueous secondary batteries, extending the battery's lifespan and maintaining performance over repeated charging and discharging cycles.
Smart Images

Figure 0007560655000011 
Figure 0007560655000001 
Figure 0007560655000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a negative electrode composition, a negative electrode sheet, a nonaqueous secondary battery, a method for producing a negative electrode sheet, and a method for producing a nonaqueous secondary battery. [Background technology]
[0002] Secondary batteries, such as lithium-ion secondary batteries, are used as power sources for portable electronic devices such as personal computers, video cameras, mobile phones, etc. Recently, against the backdrop of the global environmental challenge of reducing carbon dioxide emissions, they have become widespread as power sources for transportation equipment such as automobiles, and for storing electricity such as nighttime electricity and electricity generated by natural energy sources.
[0003] The electrodes (positive and negative electrodes) of a lithium-ion secondary battery have electrode active material layers (positive and negative active material layers), and these electrode active material layers contain electrode active material particles that can absorb or release lithium ions during charging and discharging. Since electrons are also transported between the electrode active material particles or between the electrode active material particles and the current collector, it is necessary to ensure electronic conductivity. To improve the efficiency of this electronic conduction, the binding property between the electrode active material particles or between the electrode active material particles and the current collector is important, and the electrode active material layers usually contain a binder.
[0004] In order to realize high-capacity lithium-ion secondary batteries, the use of silicon oxide as the negative electrode active material has been actively investigated. The theoretical capacity of silicon oxide is much higher than that of graphite, etc., and it is possible to achieve high energy density of the battery. When silicon oxide is used as the negative electrode active material, it absorbs a large amount of lithium ions and expands significantly during charging, and the silicon oxide also contracts significantly during discharging. Therefore, in lithium-ion batteries using silicon oxide as the negative electrode active material, the volume of the negative electrode active material changes significantly during charging and discharging, and the battery performance is easily degraded by repeated charging and discharging. In other words, there is a limit to improving the cycle life. As a technique for dealing with such problems, for example, Patent Document 1 describes a slurry for the negative electrode of a lithium ion battery, which contains a negative electrode active material containing 20 mass % or more of silicon particles having a median diameter of 0.1 to 2 μm, poly(meth)acrylamide which is a radical copolymer of a monomer group including a (meth)acrylamide skeleton-containing monomer and a sulfonic acid group-substituted unsaturated hydrocarbon group-containing monomer and shows a specific high viscosity in an aqueous solution state of a specific concentration, and water. According to the technique described in Patent Document 1, it is said that a lithium ion secondary battery with excellent cycle life (cycle characteristics) can be obtained by using this negative electrode slurry.
[0005] It has also been proposed to coat silicon oxide with carbon and use it as an anode active material. It is said that the carbon coating can increase the electrical conductivity of silicon oxide particles and suppress side reactions between silicon oxide and electrolytes. Therefore, carbon-coated silicon oxide is expected to be a negative electrode active material for next-generation lithium-ion secondary batteries. For example, Patent Document 2 describes carbon-coated silicon oxide and a 1580 cm peak in an argon ion laser Raman spectrum. -1 Peak intensity at 1360cm -1 Patent Document 2 describes a slurry for a lithium ion battery negative electrode, which contains graphite having an R value, which is a peak intensity ratio, of 0.2 to 1.5, a binder, carbon black, and water. According to the technology described in Patent Document 2, a lithium ion secondary battery with excellent cycle life can be obtained by doping a negative electrode mixture layer formed using this negative electrode slurry with lithium ions.
[0006] Electrodes of lithium ion secondary batteries are usually formed by applying an electrode-forming composition (slurry) onto a current collector and drying it. Therefore, the slurry for forming the electrode is prepared by dispersing an electrode active material and a binder in a liquid medium. In recent years, with the background of increasing interest in environmental issues, aqueous liquid media are in demand, and various water-soluble binders suitable for aqueous slurries have been developed, for example, as described in the above-mentioned Patent Documents 1 and 2. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2018-6334 A [Patent Document 2] JP 2018-81753 A Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a negative electrode composition using carbon-coated silicon oxide as a negative electrode active material, which, when used to form a negative electrode active material layer of a nonaqueous secondary battery, can provide a nonaqueous secondary battery with high capacity and low resistance while also sufficiently extending the cycle life. Another object of the present invention is to provide a negative electrode sheet and a nonaqueous secondary battery using the negative electrode composition. Another object of the present invention is to provide a method for producing the negative electrode sheet and the nonaqueous secondary battery. [Means for solving the problem]
[0009] In view of the above problems, the present inventors have conducted extensive research into binders to be combined with carbon-coated silicon oxide from the viewpoint of the polymer structure that constitutes the binder. As a result, while the polymer is usually made high molecular weight in consideration of the mechanical strength of the binder, the inventors have found that the above technical problems can be solved to a high level by containing a specific amount or more of a water-soluble polymer in the binder, in which the weight-average molecular weight is restricted to 300,000 or less and the content of a component having an acid group that is expected to interact with an active material or between polymers is restricted to a small amount of 5 mass% or less. The present invention was completed through further research based on these findings.
[0010] That is, the above problems were solved by the following means. <1> A composition for a negative electrode comprising a binder and carbon-coated silicon oxide, The binder contains 5% by mass or more of a water-soluble polymer, The water-soluble polymer has a weight-average molecular weight of 300,000 or less, and the proportion of a component having an acid group in the water-soluble polymer is 5 mass % or less. <2> The water-soluble polymer is a chain-polymerized polymer. <1> The negative electrode composition according to claim 1 . <3> The water-soluble polymer contains a component represented by the following general formula (1) or (2) as a component having no acid group: <1> or <2> The negative electrode composition according to claim 1 . [ka] In general formula (1), R 1 represents a hydrogen atom or a methyl group, L 1 represents a single bond or a linking group, R 2 indicates a substituent. * indicates a binding site for incorporation into the water-soluble polymer. In general formula (2), R 3 represents a hydrogen atom or a methyl group, R 4 and R 5 represents a hydrogen atom or a substituent. * represents a bonding site for incorporation into the water-soluble polymer. <4> The content of the water-soluble polymer is 2 parts by mass or more per 100 parts by mass of the carbon-coated silicon oxide. <1> ~ <3> 13. The negative electrode composition according to claim 12, <5> The water-soluble polymer contains two or more components represented by the general formula (1) or (2). <3> The negative electrode composition according to claim 1 . <6> The acid group is a carboxy group or a salt thereof. <1> ~ <5> 13. The negative electrode composition according to claim 12, <7> A negative electrode slurry containing a dispersion medium, <1> ~ <6> 13. The negative electrode composition according to claim 12, <8> <1> ~ <7> 13. A negative electrode sheet having a layer constituted of the negative electrode composition according to claim 12. <9> The positive electrode active material layer, the separator, and the negative electrode active material layer are arranged in this order. <1> ~ <7> 2. A non-aqueous secondary battery, comprising a layer made of the negative electrode composition according to claim 1. <10> <1> ~ <7> 2. A method for producing a negative electrode sheet, comprising forming a film using the negative electrode composition according to claim 1. <11> <10> 2. A method for producing a non-aqueous secondary battery, comprising incorporating the negative electrode sheet obtained by the method for producing a non-aqueous secondary battery according to claim 1 into a negative electrode of the non-aqueous secondary battery.
[0011] In this specification, the term "water-soluble polymer" refers to a polymer that dissolves at least 7 g in 1 L of water at 25° C. (a polymer whose solubility at 25° C. is 7 [g / 1 L-H2O] or more). In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In this specification, the expression "compound" (for example, when referring to a compound by adding "compound" to the end of the name) refers to the compound itself, as well as its salts and ions. It also refers to derivatives in which a part of the structure has been changed, such as by introducing a substituent, within the scope of the desired effect. In the present specification, when a substituent has a dissociable hydrogen atom (a group in which the hydrogen atom dissociates due to the action of a base), the substituent includes the form of an ion or a salt. For example, when a compound has a carboxy group, the carboxy group may be present as an anion with a hydrogen atom dissociated therefrom, and the anion may form a salt with a counter ion (cation). There are no particular limitations on the counter ion, and examples of the counter ion include alkali metal ions such as lithium ion, sodium ion, and potassium ion. In this specification, for substituents, linking groups, etc. (hereinafter referred to as substituents, etc.) that are not specified as substituted or unsubstituted, it means that the group may have an appropriate substituent. Therefore, even when it is simply described as "group" (e.g., "alkyl group") in this specification, this "group" (e.g., "alkyl group") includes not only an embodiment that does not have a substituent (e.g., "unsubstituted alkyl group"), but also an embodiment that further has a substituent (e.g., "substituted alkyl group"). This also applies to compounds that are not specified as substituted or unsubstituted. In this specification, when there are multiple substituents etc. designated by a specific symbol, or when multiple substituents etc. are simultaneously or alternatively specified, it means that the respective substituents etc. may be the same or different from each other. In addition, even if not specified otherwise, when multiple substituents etc. are adjacent, it means that they may be linked to each other or condensed to form a ring. In this specification, when a polymer has multiple components having the same designation (represented by the same general formula), each component may be the same or different from each other. In this specification, the term "nonaqueous secondary battery" includes nonaqueous electrolyte secondary batteries and all-solid-state secondary batteries. In this specification, the term "nonaqueous electrolyte" means an electrolyte that does not substantially contain water. That is, the "nonaqueous electrolyte" may contain a small amount of water within a range that does not impede the effects of the present invention. In the present invention, the "nonaqueous electrolyte" has a water concentration of 200 ppm (by mass) or less, preferably 100 ppm or less, and more preferably 20 ppm or less. Note that it is practically difficult to make a nonaqueous electrolyte completely anhydrous, and it usually contains 1 ppm or more of water. In this specification, the term "solid content" used when describing the content or content ratio means components other than the dispersion medium described below. Effect of the Invention
[0012] The negative electrode composition and negative electrode sheet of the present invention can be used to form a negative electrode active material layer, thereby imparting excellent cycle characteristics to a non-aqueous secondary battery using carbon-coated silicon oxide as a negative electrode active material, and therefore the non-aqueous secondary battery of the present invention has high capacity, low resistance, and excellent cycle characteristics. According to the method for producing a negative electrode sheet of the present invention, the above-mentioned negative electrode sheet of the present invention can be obtained. Also, according to the method for producing a nonaqueous secondary battery of the present invention, the above-mentioned nonaqueous secondary battery of the present invention can be obtained. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a vertical cross-sectional view showing a schematic diagram of a basic layered structure of a nonaqueous electrolyte secondary battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] [Negative electrode composition] The negative electrode composition of the present invention contains a binder containing a water-soluble polymer and a negative electrode active material containing carbon-coated silicon oxide. The water-soluble polymer is a polymer having a weight-average molecular weight of 300,000 or less, and the content of a component having an acid group in the water-soluble polymer is 5% by mass or less. The water-soluble polymer is contained in the binder at 5% by mass or more. By incorporating the negative electrode active material layer prepared using the negative electrode composition of the present invention into a secondary battery, the cycle life of the resulting secondary battery can be effectively increased. Although the reason for this is not yet clear, it is assumed that one of the reasons is that the binder contains a certain amount or more of a polymer that has a relatively small molecular weight of 300,000 or less and has a limited amount of acid groups to suppress an increase in apparent molecular weight, and this polymer fits into the voids in the carbon coat layer (producing an anchor effect), thereby firmly binding the water-soluble polymer to the negative electrode active material (carbon-coated silicon oxide). The negative electrode composition of the present invention can be prepared by mixing a binder containing a water-soluble polymer, a negative electrode active material containing carbon-coated silicon oxide, and, if necessary, a dispersion medium, a conductive assistant, and the like.
[0015] (binder) The binder used in the present invention contains the above-mentioned water-soluble polymer in an amount of 5% by mass or more based on the total amount of the binder. The water-soluble polymer used in the present invention may be either a chain-polymerized polymer or a step-polymerized polymer, and is preferably a chain-polymerized polymer. The bonding form of the chain-polymerized polymer is not particularly limited, and may be either random or block.
[0016] The main component constituting the water-soluble polymer, which does not have an acid group, is not particularly limited. The water-soluble polymer preferably contains, as the component not having an acid group, a component represented by the following general formula (1) or (2), for example.
[0017] [ka]
[0018] In general formula (1), R 1 represents a hydrogen atom or a methyl group, L 1 represents a single bond or a linking group (divalent), R 2 indicates a substituent. * indicates a binding site for incorporation into a water-soluble polymer. In general formula (2), R 3 represents a hydrogen atom or a methyl group, R 4 and R 5 represents a hydrogen atom or a substituent. * represents a bonding site for incorporation into a water-soluble polymer.
[0019] L 1 The linking group that can be used as the linking group is not particularly limited as long as it does not have an acid group. The chemical formula weight of this linking group is preferably 14 to 1,000, more preferably 14 to 500, and further preferably 26 to 250. L 1Examples of the linking group that can be used include an alkylene group, -O-, a carbonyl group, an imino group, and a combination thereof. As for these combinations, a linking group formed by combining 2 to 6 of the alkylene groups, -O-, carbonyl groups, and imino groups is preferred, and a linking group formed by combining 2 or 3 of them is more preferred. L 1 Specifically, any one of -C(=O)-O-, -OC(=O)-, -NH-C(=O)-O-, -OC(=O)-NH-, -NH-C(=O)-NH-, and an alkylene group is preferable, and an alkylene group is more preferable. L 1 The alkylene group which can be taken as may be either linear or branched, and the number of carbon atoms in the alkylene group is preferably 1 to 10, more preferably 1 to 8, still more preferably 1 to 6, particularly preferably 1 to 4, and is most preferably any one of a methylene group, an ethylene group, an ethylethylene group, and a propylene group. L 1 The chemical formula weight is preferably 14-200, more preferably 14-150, and further preferably 14-80.
[0020] R 2 is not particularly limited as long as it is a substituent that does not have an acid group. 2 The chemical formula weight of R is preferably 15 to 200, more preferably 15 to 150, and even more preferably 15 to 100. 2 Examples of the alkyl group include a hydroxy group, an alkyloxy group, an alkyl group, an amide group and a sulfonamide group, and a hydroxy group or an alkyloxy group is preferable. The alkyl group in the alkyloxy group may be linear, branched or cyclic. The number of carbon atoms in the alkyl group is preferably 1 to 10, more preferably 1 to 8, still more preferably 1 to 6, particularly preferably 1 to 4, and is most preferably any one of a methyl group, an ethyl group and an isopropyl group. The alkyl group has the same meaning as the alkyl group in the alkyloxy group, and the preferred range is also the same.
[0021] R 4 and R5 The substituent that can be used as R is not particularly limited as long as it is a substituent that does not have an acid group. 4 and R 5 The chemical formula weight of each of R is preferably 15 to 200, more preferably 15 to 150, and further preferably 15 to 60. 4 and R 5 The substituent which may be taken as the aryl group is preferably an alkyl group. The alkyl group is the same as R 2 The meaning of the alkyl group in the alkyloxy group that can be taken as R is the same as that of the alkyl group in the alkyloxy group that can be taken as R, and the preferred range is also the same. 4 and R 5 The alkyl group which can be taken as the alkyl group preferably further has a substituent. Examples of such substituents include a hydroxy group, an alkylcarbonyl group, an amide group, and a urethane bond-containing group (-NH-CO-OR b (R b represents an alkyl group. 4 and R 5 The substituent of the alkyl group which may be taken as the substituent is preferably a hydroxy group. The alkyl group in the alkylcarbonyl group is the same as R 2 The meaning and preferred range of the alkyl group in the alkyloxy group that can be taken as R b The alkyl group represented by the above R 2 The alkyl group has the same meaning as the alkyl group in the alkyloxy group which can be taken as the above, and the preferred range is also the same. R 4 and R 5 are preferably both hydrogen atoms, or one of them is a hydrogen atom and the other is a hydroxyalkyl group.
[0022] The water-soluble polymer used in the present invention may contain one kind of component not having an acid group alone or two or more kinds in combination. The proportion of the component represented by the general formula (1) or (2) in the water-soluble polymer (the sum of the proportion of the component represented by the general formula (1) and the proportion of the component represented by the general formula (2) in the water-soluble polymer) is preferably 30% by mass or more, more preferably 50% by mass or more, even more preferably 70% by mass or more, particularly preferably 90% by mass or more, and most preferably 95% by mass or more. From the viewpoint of improving the cycle characteristics of the secondary battery, the water-soluble polymer used in the present invention preferably contains two or more kinds of components represented by general formula (1) or (2), more preferably contains 2 to 6 kinds of components represented by general formula (1) or (2), and even more preferably contains 2 to 4 kinds of components represented by general formula (1) or (2). Examples of the form containing two or more kinds of components represented by general formula (1) or (2) include a form containing two or more kinds of components represented by general formula (1) and no component represented by general formula (2), a form containing two or more kinds of components represented by general formula (2) and no component represented by general formula (1), and a form containing both a component represented by general formula (1) and a component represented by general formula (2).
[0023] Preferred specific examples of the component represented by the above general formula (1) are shown below, but the present invention is not limited to these examples.
[0024] [ka]
[0025] Preferred specific examples of the component represented by the above general formula (2) are shown below, but the present invention is not limited to these examples.
[0026] [ka]
[0027] When the water-soluble polymer contains a component other than the component represented by the general formula (1) or (2) as a component not having an acid group, such a component is not particularly limited. For example, a component derived from a vinyl monomer such as styrene, maleimide, N-vinylacetamide, vinyl ester, or vinyl ether can be mentioned.
[0028] The "acid group" of the constituent having an acid group that the water-soluble polymer may have means a group having a dissociable proton or a salt thereof. Examples of the acid group include a carboxy group, a sulfo group, a phosphoric acid group (-OP(=O)(OH)2), a phosphonic acid group (-P(=O)(OH)2) or a salt thereof, with a carboxy group and a sulfo group or a salt thereof being preferred, and a carboxy group or a salt thereof being more preferred. Examples of the salt form include an alkali metal salt (e.g., a lithium salt, a sodium salt, a potassium salt, etc.).
[0029] The constituent having an acid group is not particularly limited, and the constituent usually contains 1 to 3 acid groups, preferably 1 or 2, and more preferably 1. When the water-soluble polymer contains a constituent having an acid group, it is preferable that the water-soluble polymer contains, for example, a constituent represented by the following general formula (3).
[0030] [ka]
[0031] In the formula, R 6 R represents a hydrogen atom or an acid group. 7 represents a hydrogen atom or a methyl group, L 2 represents a single bond or a linking group (divalent), R 8 indicates an acid group. * indicates a bonding site for incorporation into a water-soluble polymer.
[0032] L 2 The linking group which can be taken as is not particularly limited, and examples thereof include an alkylene group, an arylene group, a carbonyl group, an ether bond (-O-) or an imino group, or a linking group which is a combination of two or more of these.
[0033] L 2 The alkylene group which can be taken as may be either linear or branched, and the alkylene group preferably has 1 to 10 carbon atoms, more preferably 1 to 8 carbon atoms, further preferably 1 to 6 carbon atoms, particularly preferably 1 to 4 carbon atoms, and is most preferably any one of a methylene group, an ethylene group, a propylene group, and a dimethylethylene group.
[0034] L 2 The number of carbon atoms in the arylene group which can be taken as the alkyl group is preferably from 6 to 30, more preferably from 6 to 20, further preferably from 6 to 15, and particularly preferably from 6 to 10. Specific examples of the arylene group include a phenylene group and a naphthylene group.
[0035] The above "linking group combining two or more types" is a linking group combining at least two types of an alkylene group, an arylene group, a carbonyl group, an ether bond (-O-), and an imino group, and is preferably a linking group combining 2 to 10 types, more preferably a linking group combining 2 to 7 types, and even more preferably a linking group combining 2 to 4 types. Specific examples of the above-mentioned "linking group combining two or more types" include "carbonyl group-imino group-alkylene group" and "carbonyl group-ether bond-alkylene group".
[0036] The proportion of components having an acid group in the water-soluble polymer is 5% by mass or less, preferably 4% by mass or less, more preferably 3% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less, and it is most preferable that the water-soluble polymer does not have any components having an acid group.
[0037] Preferred specific examples of the component represented by the above general formula (3) are shown below, but the present invention is not limited to these examples.
[0038] [ka]
[0039] The weight-average molecular weight of the water-soluble polymer used in the present invention is 300,000 or less, preferably 290,000 or less, more preferably 280,000 or less, and even more preferably 270,000 or less. On the other hand, the weight-average molecular weight of the water-soluble polymer is preferably 10,000 or more, more preferably 40,000 or more, even more preferably 100,000 or more, particularly preferably 140,000 or more, and most preferably 170,000 or more. In this specification, the weight average molecular weight of a polymer is a value obtained by measurement according to the method described in the Examples section below.
[0040] In the binder used in the present invention, the content of the water-soluble polymer is 5% by mass or more, and from the viewpoint of improving the cycle characteristics of the secondary battery, the content is preferably 10% by mass or more, and more preferably 20% by mass or more. The binder used in the present invention may be composed of the water-soluble polymer.
[0041] From the viewpoint of improving the cycle characteristics of the secondary battery, the content of the water-soluble polymer in the negative electrode composition is preferably 2 parts by mass or more, more preferably 4 parts by mass or more, and even more preferably 8 parts by mass or more, relative to 100 parts by mass of the carbon-coated silicon oxide, while the content of the water-soluble polymer in the negative electrode composition is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, relative to 100 parts by mass of the carbon-coated silicon oxide.
[0042] The binder used in the present invention may contain a polymer other than the water-soluble polymer. Examples of such a polymer include a water-insoluble polymer, a water-soluble polymer having a weight-average molecular weight of more than 300,000, and a water-soluble polymer having an acid group-containing component content of more than 5% by mass. A specific example of such a polymer is polymer B shown in Table 1 below, but polymer B is not limited to "polymer B shown in Table 1 below."
[0043] (Negative electrode active material) The negative electrode active material used in the present invention contains carbon-coated silicon oxide (SiOx (0 < x ≤ 1.5)). The carbon-coated silicon oxide can reversibly occlude and release lithium ions. The entire surface of the silicon oxide may be carbon-coated, or there may be a portion that is not carbon-coated. Even if the entire surface of the silicon oxide is carbon-coated, the carbon coating layer itself is in a state of having a large number of voids. The ratio of carbon atoms in the carbon-coated silicon oxide (in the total of the carbon coating layer and silicon oxide) is not particularly limited. For example, 0.5 to 5% by mass is preferable, and 1 to 3% by mass is more preferable. Commercially available products of carbon-coated silicon oxide may be used, or it can also be prepared by carbon-coating silicon oxide, for example, referring to Japanese Patent Application Laid-Open No. 2019-204686.
[0044] The negative electrode active material used in the present invention may contain a negative electrode active material other than the carbon-coated silicon oxide. Hereinafter, in the description of the negative electrode active material used in the present invention, a negative electrode active material other than the carbon-coated silicon oxide is referred to as "other negative electrode active material". Other negative electrode active materials are preferably those that can reversibly occlude and release lithium ions. The material thereof is not particularly limited as long as it has the above characteristics, and examples include carbonaceous materials, metal oxides, metal composite oxides, lithium alloys, and negative electrode active materials capable of forming an alloy with lithium. The lithium alloy is not particularly limited as long as it is an alloy commonly used as a negative electrode active material for secondary batteries. For example, a lithium aluminum alloy can be mentioned. The negative electrode active material capable of forming an alloy with lithium is not particularly limited as long as it is a material commonly used as a negative electrode active material for secondary batteries. Examples of such active materials include negative electrode active materials having tin atoms, and various metals such as Al and In. Examples of the negative electrode active material containing tin atoms include Sn, SnO, SnO2, SnS, SnS2, and the above-mentioned active materials containing silicon atoms and tin atoms. Also included are composite oxides with lithium oxide, such as Li2SnO2. Among these, as the other negative electrode active material, carbonaceous materials are preferably used from the viewpoint of reliability.
[0045] The carbonaceous material used as the other negative electrode active material is a material substantially made of carbon. For example, carbon black such as petroleum pitch, graphite (natural graphite, artificial graphite such as vapor-grown graphite, etc.), and carbonaceous materials obtained by burning various synthetic resins such as PAN (polyacrylonitrile)-based resins or furfuryl alcohol resins can be mentioned. In addition, various carbon fibers such as PAN-based carbon fibers, cellulose-based carbon fibers, pitch-based carbon fibers, vapor-grown carbon fibers, dehydrated PVA (polyvinyl alcohol)-based carbon fibers, lignin carbon fibers, glassy carbon fibers, and activated carbon fibers, mesophase microspheres, graphite whiskers, and plate-like graphite can also be mentioned.
[0046] Other metal oxides and metal composite oxides that can be used as negative electrode active materials are not particularly limited as long as they are oxides that can absorb and release lithium, and amorphous oxides are preferred, and chalcogenides that are reaction products of metal elements and elements of group 16 of the periodic table are also preferred. The term "amorphous" as used herein means that the oxide has a broad scattering band with a peak in the 2θ value range of 20° to 40° in an X-ray diffraction method using CuKα rays, and may have crystalline diffraction lines. Among the compound group consisting of the above amorphous oxides and chalcogenides, the amorphous oxides of metalloid elements and the above chalcogenides are more preferred, and the oxides (excluding oxides containing Si) consisting of one or more of the elements of Groups 13 (IIIB) to 15 (VB) of the periodic table, Al, Ga, Si, Sn, Ge, Pb, Sb and Bi, or a combination of two or more of them, or chalcogenides are particularly preferred.Specific examples of preferred amorphous oxides and chalcogenides include Ga2O3, GeO, PbO, PbO2, Pb2O3, Pb2O4, Pb3O4, Sb2O3, Sb2O4, Sb2O8Bi2O3, Sb2O5, Bi2O3, Bi2O4, GeS, PbS, PbS2, Sb2S3 and Sb2S5.
[0047] The metal (composite) oxide and the above chalcogenide preferably contain at least one of titanium and lithium as a constituent from the viewpoint of high current density charge / discharge characteristics. Examples of the metal composite oxide containing lithium (lithium composite metal oxide) include composite oxides of lithium oxide and the above metal (composite) oxide or the above chalcogenide, more specifically Li2SnO2.
[0048] Other negative electrode active materials preferably contain titanium atoms. More specifically, TiNb2O7 (niobium titanate oxide [NTO]), Li4Ti5O 12 Lithium titanate (LTO) is preferred because it has excellent rapid charge / discharge characteristics due to its small volumetric change when absorbing and releasing lithium ions, and because it suppresses electrode deterioration and can improve the life of lithium ion secondary batteries.
[0049] The shape of the carbon-coated silicon oxide and other negative electrode active materials is not particularly limited, but is preferably particulate. The volume-based median diameter D50 of the carbon-coated silicon oxide and other negative electrode active materials is preferably 0.1 to 60 μm. To obtain a desired particle size, a conventional grinder or classifier is used. For example, a mortar, a ball mill, a sand mill, a vibration ball mill, a satellite ball mill, a planetary ball mill, a swirling airflow type jet mill, or a sieve is preferably used. During grinding, wet grinding in the presence of water or an organic solvent such as methanol can also be performed. In order to obtain a desired particle size, it is preferable to perform classification. The classification method is not particularly limited, and a sieve, a wind classifier, or the like can be used as desired. Classification can be performed both dry and wet.
[0050] The median diameter D50 of the carbon-coated silicon oxide is preferably from 0.1 to 30 μm, more preferably from 0.5 to 20 μm, and particularly preferably from 2 to 8 μm. The median diameter D50 can be determined by a laser diffraction method, for example, using SALD-2300 (product name) manufactured by Shimadzu Corporation.
[0051] When carbon-coated silicon oxide is used in combination with other negative electrode active materials, a combination of carbon-coated silicon oxide and a carbonaceous material is preferred, and a combination of carbon-coated silicon oxide and graphite is particularly preferred. When carbon-coated silicon oxide and graphite are combined, the mass ratio (carbon-coated silicon oxide / graphite) is preferably 0.1 or more, more preferably 0.2 or more, and even more preferably 0.3 or more. There is no particular upper limit to the mass ratio of carbon-coated silicon oxide to graphite, but 4 or less is practical. The content of carbon-coated silicon oxide in the negative electrode active material is not particularly limited and can be, for example, 10 to 90 mass %, preferably 10 to 50 mass %, and more preferably 15 to 40 mass %. When forming a negative electrode active material layer, the unit area (cm 2The mass (mg) (weight per unit area) of the carbon-coated silicon oxide and other negative electrode active materials is not particularly limited and can be appropriately determined according to the designed battery capacity.
[0052] The content of the carbon-coated silicon oxide and other negative electrode active materials in the negative electrode composition is not particularly limited, and is preferably 10 to 98 mass%, and more preferably 15 to 95 mass%, in total, based on 100 mass% of the solid content.
[0053] (dispersion medium) The negative electrode composition of the present invention can also contain a dispersion medium to form a negative electrode slurry. When a non-aqueous electrolyte secondary battery is prepared using the negative electrode composition of the present invention, an aqueous medium containing water can be used as the dispersion medium. The "aqueous medium containing water" is water or a mixture of water and a water-soluble organic solvent. The "water-soluble organic solvent" is an organic solvent that does not undergo phase separation when mixed with water, and examples of such organic solvents include N-methylpyrrolidone, methanol, ethanol, acetone, and tetrahydrofuran.
[0054] (Conductive assistant) The negative electrode composition of the present invention may also contain a conductive assistant. The conductive assistant is not particularly limited, and may be any known conductive assistant. For example, it may be an electron conductive material such as graphites such as natural graphite and artificial graphite, carbon blacks such as acetylene black, ketjen black, and furnace black, amorphous carbon such as needle coke, carbon fibers such as vapor-grown carbon fibers or carbon nanotubes, carbonaceous materials such as graphene or fullerene, metal powders or metal fibers such as copper and nickel, or conductive polymers such as polyaniline, polypyrrole, polythiophene, polyacetylene, and polyphenylene derivatives. In the present invention, when a negative electrode active material and a conductive assistant are used in combination, among the above conductive assistants, those that do not insert or release Li when the secondary battery is charged and discharged and do not function as a negative electrode active material are considered to be conductive assistants. Therefore, among the conductive assistants, those that can function as a negative electrode active material in the negative electrode active material layer when the secondary battery is charged and discharged are classified as negative electrode active materials rather than conductive assistants. Whether or not a conductive assistant functions as a negative electrode active material when the secondary battery is charged and discharged is not unique, but is determined by the combination with the negative electrode active material.
[0055] The conductive assistant may be used alone or in combination of two or more. The content of the conductive assistant in the negative electrode composition is preferably 10 to 90 mass %, more preferably 30 to 80 mass %, and further preferably 50 to 70 mass %, based on 100 mass % of the solid content.
[0056] The shape of the conductive assistant is not particularly limited, but is preferably particulate. The median diameter D50 of the conductive assistant is not particularly limited, but is, for example, preferably 0.01 to 50 μm, and more preferably 0.02 to 10.0 μm.
[0057] (Other additives) The negative electrode composition of the present invention may contain, as desired, other components in addition to the above-mentioned components, such as a lithium salt, an ionic liquid, a thickener, an antifoaming agent, a leveling agent, a dehydrating agent, an antioxidant, etc. In addition, the composition may contain a crosslinking agent (such as one that undergoes a crosslinking reaction by radical polymerization, condensation polymerization, or ring-opening polymerization) for chemically crosslinking the water-soluble polymer, and further a polymerization initiator (such as one that generates an acid or radicals by heat or light). With regard to the above-mentioned conductive assistant and other additives, reference can be made to, for example, International Publication No. 2019 / 203334 and Japanese Patent Application Laid-Open No. 2015-46389.
[0058] [Negative electrode sheet] The negative electrode sheet of the present invention has a layer (negative electrode active material layer) that is constructed (formed) using the negative electrode composition of the present invention. The negative electrode sheet of the present invention may have a negative electrode active material layer, and may be a sheet in which the negative electrode active material layer is formed on a substrate (current collector), or may be a sheet formed only of the negative electrode active material layer without having a substrate. This negative electrode sheet is usually a sheet having a configuration in which the negative electrode active material layer is laminated on the current collector. The negative electrode sheet of the present invention may have other layers such as a protective layer (release sheet) and a coating layer. The negative electrode sheet of the present invention can be suitably used as a material constituting the negative electrode active material layer of a secondary battery.
[0059] [Method of manufacturing negative electrode sheet] The negative electrode sheet of the present invention can be obtained by forming a negative electrode active material layer using the negative electrode composition of the present invention. For example, a current collector or the like is used as a substrate, and the negative electrode composition of the present invention is applied thereon (with or without another layer) to form a coating film, which is then dried to obtain an electrode sheet having a negative electrode active material layer (coated and dried layer) on the substrate.
[0060] [Non-aqueous secondary battery] The nonaqueous secondary battery of the present invention refers to any device in which ions pass between positive and negative electrodes via an electrolyte upon charging and discharging, and energy is stored and released at the positive and negative electrodes. That is, the nonaqueous secondary battery of the present invention includes both batteries and capacitors (e.g., lithium ion capacitors). From the viewpoint of the amount of energy stored, it is preferable that the nonaqueous secondary battery of the present invention is used for battery applications (not as a capacitor).
[0061] The nonaqueous secondary battery of the present invention will be described taking a nonaqueous electrolyte secondary battery as an example, however, the secondary battery of the present invention is not limited to a nonaqueous electrolyte secondary battery and broadly includes all nonaqueous secondary batteries including all-solid-state secondary batteries. A nonaqueous electrolyte secondary battery according to a preferred embodiment of the present invention includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode. The positive electrode includes a positive electrode current collector and a positive electrode active material layer in contact with the positive electrode current collector, and the negative electrode includes a negative electrode current collector and a negative electrode active material layer in contact with the negative electrode current collector. In the nonaqueous electrolyte secondary battery of the present invention, the negative electrode active material layer is formed using the electrode composition of the present invention.
[0062] FIG. 1 is a cross-sectional view showing a schematic of the laminated structure of a general non-aqueous electrolyte secondary battery 10, including the working electrodes when the battery is operated. The non-aqueous electrolyte secondary battery 10 has a laminated structure having, as viewed from the negative electrode side, a negative electrode current collector 1, a negative electrode active material layer 2, a separator 3, a positive electrode active material layer 4, and a positive electrode current collector 5, in this order. The space between the negative electrode active material layer and the positive electrode active material layer is filled with a non-aqueous electrolyte (not shown), and is separated by the separator 3. The separator 3 has pores, and functions as a positive and negative electrode separator that insulates between the positive and negative electrodes while allowing the electrolyte and ions to pass through during normal battery use. With this structure, for example, in the case of a lithium-ion secondary battery, electrons (e - ) is supplied, and at the same time, lithium ions (Li + ) moves and accumulates in the negative electrode. On the other hand, during discharge, the lithium ions (Li + ) is returned to the positive electrode side through the electrolyte, and electrons are supplied to the operating part 6. In the illustrated example, a light bulb is used as the operating part 6, and it is lit by the discharge. In the present invention, the negative electrode current collector 1 and the negative electrode active material layer 2 are collectively referred to as the negative electrode, and the positive electrode active material layer 4 and the positive electrode current collector 5 are collectively referred to as the positive electrode.
[0063] In the non-aqueous secondary battery of the present invention, the positive electrode active material material, the non-aqueous electrolyte, the solid electrolyte material, and other members are not particularly limited, except that the negative electrode active material layer is formed using the negative electrode composition of the present invention. These materials and members can be appropriately applied to those used in normal non-aqueous secondary batteries. In addition, for the method of producing the non-aqueous secondary battery of the present invention, a normal method can be appropriately adopted, except that the negative electrode active material layer is formed using the negative electrode composition of the present invention. For example, JP-A-2016-201308, JP-A-2005-108835, JP-A-2012-185938, and WO 2020 / 067106 can be appropriately referred to.
[0064] The nonaqueous secondary battery of the present invention can be mounted in electronic devices such as notebook computers, pen-input computers, mobile computers, electronic book players, mobile phones, cordless phone sub-units, pagers, handheld terminals, portable fax machines, portable copiers, portable printers, headphone stereos, video movie machines, liquid crystal televisions, handheld cleaners, portable CDs, mini-discs, electric shavers, transceivers, electronic organizers, calculators, portable tape recorders, radios, backup power sources, and memory cards. It can also be mounted in consumer devices such as automobiles, electric vehicles, motors, lighting equipment, toys, game equipment, road conditioners, watches, strobes, cameras, and medical equipment (pacemakers, hearing aids, shoulder massagers, etc.). It can also be combined with solar cells.
[0065] The present invention will be described in more detail with reference to examples. However, the present invention is not to be construed as being limited to these examples except as defined in the present invention. EXAMPLES
[0066] [Synthesis of Polymer A] <Synthesis of Polymer 1 (Polymer No. 1 in Table 1 below)> Polymer 1 shown in Table 1 below was synthesized as follows. A 500 mL separable flask was charged with 108.1 g of ion-exchanged water, and a mixture containing 17.5 g of 2-hydroxyethyl acrylate, 52.5 g of N-(2-hydroxyethyl)acrylamide, and 24.9 g of ion-exchanged water, and a mixture containing 1.26 g of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate and 33.3 g of ion-exchanged water were simultaneously dropped into the flask over 1 hour while stirring at 75°C under a nitrogen atmosphere. After the dropwise addition, the mixture was stirred at 75°C for 2 hours to obtain a polymer solution with a solid content of 29.8% by mass.
[0067] <Synthesis of polymers 2 to 19 and c1 to c3 (synthesis of polymers No. 2 to 19 and c1 to c3 in Table 1 below) Polymers 2 to 19 and c1 to c3 were synthesized in the same manner as in the synthesis of Polymer 1, except that the monomers shown in Table 1 below were used in the mass ratios shown in Table 1 below as monomers from which the constituent components were derived.
[0068] (Measurement of weight average molecular weight) The weight average molecular weight (Mw) of the polymer shown in Table 1 below is a weight average molecular weight calculated as sodium polyacrylate by gel permeation chromatography (GPC), and is a value measured under the following conditions. Measuring instrument: HLC-8220GPC (product name, manufactured by Tosoh Corporation) Columns: TOSOH TSKgel 5000PWXL (product name, manufactured by Tosoh Corporation), TOSOH TSKgel G4000PWXL (product name, manufactured by Tosoh Corporation), and TOSOH TSKgel G2500PWXL (product name, manufactured by Tosoh Corporation) were connected. Guard column: TSKgel guardcolumn PWXL (product name, manufactured by Tosoh Corporation) Carrier: 200mM sodium nitrate aqueous solution Rinse solution: Ultrapure water Carrier flow rate: Sample pump 1.0mL / min Reference pump 0.223mL / min Initial pump pressure: Sample pump 4.4MPa Reference pump 0.8MPa Sample concentration: 0.10% by mass Column temperature: 40℃ Detector temperature: 40℃ Collection time: 45 minutes (runtime 47.0 minutes) Detector: RI (refractive index) detector
[0069] [Preparation of negative electrode composition 1 (composition No. 1 in Table 1 below)] A 60 ml ointment container (manufactured by Umano Chemical Co., Ltd.) was charged with 30 parts by mass of carbon-coated silicon oxide (SiOC, carbon atom content ratio 1.3 mass%, average primary particle diameter: 5 μm, manufactured by Osaka Titanium Co., Ltd.), 70 parts by mass of graphite (trade name: mag-d, manufactured by Hitachi Chemical Co., Ltd.), 5 parts by mass of acetylene black (trade name: Denka Black, manufactured by Denka Co., Ltd.), 5 parts by mass of polymer 1, and 22.5 parts by mass of distilled water, and dispersed for 10 minutes at 2000 rpm using a foaming mixer (trade name, manufactured by THINKY Co., Ltd.). 27 parts by mass of distilled water was added to the dispersed liquid, and the mixture was dispersed for 10 minutes at 2000 rpm using a foaming mixer, to obtain a negative electrode composition 1.
[0070] [Preparation of negative electrode compositions 2 to 19 and c1 to c3 (compositions No. 2 to 19 and c1 to c3 in Table 1 below)] Negative electrode compositions 2 to 19 and c1 to c3 were prepared in the same manner as in the preparation of the negative electrode composition 1, except that polymer 1 was replaced with polymers 2 to 19 and c1 to c3 shown in Table 1 below.
[0071] [Preparation of non-aqueous electrolyte secondary battery (2032 type coin battery) 1 (battery No. 1 in Table 1 below)] The obtained negative electrode composition 1 was applied onto a copper foil having a thickness of 20 μm using an applicator and dried for 1 hour at 80° C. Thereafter, pressure was applied using a press machine and then dried in a vacuum at 150° C. for 6 hours to obtain a negative electrode sheet having a negative electrode active material layer having a thickness of 25 μm. A disk having a diameter of 13.0 mm was cut out from the negative electrode sheet and used to form a negative electrode. Lithium foil (thickness 50 μm, 14.5 mmφ) and a polypropylene separator (thickness 25 μm, 16.0 mmφ) were stacked in this order, and 200 μL of 1M LiPF6 ethylene carbonate / ethyl methyl carbonate (volume ratio 1:2) electrolyte was impregnated into the separator. 200 μL of electrolyte was further impregnated into the separator, and the negative electrode sheet was stacked so that the negative electrode active material layer surface was in contact with the separator. Then, a 2032-type coin case was crimped to prepare a nonaqueous electrolyte secondary battery 1 (a battery having a laminate consisting of Li foil-separator-negative electrode active material layer-copper foil).
[0072] [Preparation of non-aqueous electrolyte secondary batteries 2 to 19 and c1 to c3 (batteries No. 2 to 19 and c1 to c3 in Table 1 below)] Non-aqueous electrolyte secondary batteries 2 to 19 and c1 to c3 were produced in the same manner as in the production of the non-aqueous electrolyte secondary battery 1, except that negative electrode compositions 2 to 19 and c1 to c3 shown in Table 1 below were used instead of the negative electrode composition 1.
[0073] [Test example] Evaluation of cycle characteristics The discharge capacity retention rate of each coin battery was measured using a charge / discharge evaluation device: TOSCAT-3000 (product name, manufactured by Toyo Systems Co., Ltd.). Charging was performed at a C rate of 0.2C (a rate at which the battery is fully charged in 5 hours) until the battery voltage reached 0.02V. Discharging was performed at a C rate of 0.2C until the battery voltage reached 1.5V. Each coin battery was initialized by repeating three cycles of charging and discharging, with one charge and one discharge constituting one charge / discharge cycle. After initialization, charging was performed at 0.5C until the voltage reached 0.02V. Discharging was performed at 0.5C until the voltage reached 1.5V. This one charge and one discharge constitutes one charge / discharge cycle, and 50 charge / discharge cycles were repeated to evaluate cycle characteristics. When the discharge capacity at the first cycle after initialization (initial discharge capacity) was taken as 100%, the discharge capacity retention rate at the 50th cycle (100 x "discharge capacity at the 50th cycle" / "initial discharge capacity") was calculated, and cycle characteristics were evaluated according to the following evaluation ranks. The results are shown in Table 1 below. In this test, evaluation ranks of "1" to "3" are pass. -Evaluation rank of discharge capacity retention rate (cycle characteristics)- 1: 95% or more 2: 90% or more, less than 95% 3: 85% or more, but less than 90% 4: Less than 85%
[0074] [Table 1]
[0075] The abbreviations of the monomers from which the components are derived are explained. Also, the structures of the components derived from the monomers are described. (Components not having an acid group) HEA: 2-hydroxyethyl acrylate HEAA: N-(2-hydroxyethyl)acrylamide Aam: Acrylamide MEA: 2-Methoxyethyl acrylate [ka]
[0076] (Components having acid groups) AA: Sodium acrylate AMPS: 2-acrylamido-2-methylpropanesulfonic acid [ka]
[0077] Latex: copolymer latex of styrene / 2-ethylhexyl acrylate / acrylic acid = 40 / 55 / 5 (mass ratio), Mw = 1.2 million, average primary particle diameter 3 μm (solid content 15 mass %), this latex is water-insoluble. Water-soluble high acid group polymer: Random copolymer synthesized in the same manner as polymer 1 above ("HEAA / HEA / AA", HEAA:HEA:AA = 70:20:10 (mass ratio), Mw = 150,000) Water-soluble high molecular weight polymer: Random copolymer synthesized in the same manner as polymer 1 above ("HEAA / HEA", HEAA:HEA = 50:50 (mass ratio), Mw = 400,000)
[0078] "Acid group content (mass %) in polymer A" means the content of components in polymer A having an acid group. "Content 1 (parts by mass)": means the content of polymer A relative to 100 parts by mass of SiOC when the content of SiOC in the negative electrode composition is taken as 100 parts by mass. "Content in binder (% by mass)" means the content of the water-soluble polymer defined in the present invention in the binder. "Content 2 (parts by mass)": In the negative electrode composition, when the content of SiOC is 100 parts by mass, it means the content of polymer B relative to 100 parts by mass of SiOC. The content of "latex" is the content of solid content. All of the polymers A, including those in the comparative examples, are water-soluble.
[0079] The polymer A used in the negative electrode compositions No. c1 and c3 has a content of a component having an acid group exceeding 5 mass%. The batteries No. c1 and c3 fabricated using the negative electrode compositions No. c1 and c3 had poor cycle characteristics. The polymer A used in the negative electrode composition No. c2 has a content of components having an acid group of 5 mass% or less, but has a weight average molecular weight of more than 300,000. The battery No. c2 made using the negative electrode composition No. c2 had poor cycle characteristics. In contrast, it is clear that the batteries (Nos. 1 to 19) produced using the negative electrode compositions (Nos. 1 to 19) of the present invention are excellent in cycle characteristics.
[0080] Although the present invention has been described in conjunction with embodiments thereof, we do not intend to limit our invention to any of the details of the description unless specifically stated otherwise, and believe that the appended claims should be construed broadly without departing from the spirit and scope of the invention as set forth in the appended claims.
[0081] This application claims priority based on Japanese Patent Application No. 2021-060333, filed in Japan on March 31, 2021, the contents of which are incorporated herein by reference as part of the present specification. [Explanation of symbols]
[0082] 10 Nonaqueous electrolyte secondary battery 1 Negative electrode current collector 2 Negative electrode active material layer 3. Separator 4 Cathode active material layer 5 Positive electrode current collector 6. Working part (light bulb)
Claims
1. A composition for a negative electrode comprising a binder and carbon-coated silicon oxide, The binder contains 5% by mass or more of a water-soluble polymer which is a chain-polymerized polymer, the water-soluble polymer has a weight average molecular weight of 300,000 or less, and a proportion of a component having an acid group in the water-soluble polymer is 5 mass % or less; The negative electrode composition, wherein the water-soluble polymer contains a component represented by the following general formula (1) or (2) as a component having no acid group: [Case 1] In formula (1), R 1 represents a hydrogen atom or a methyl group, L 1 represents a single bond or a linking group, R 2 represents a substituent, and * represents a bonding site for incorporation into the water-soluble polymer. In formula (2), R 3 represents a hydrogen atom or a methyl group, R 4 and R 5 represent a hydrogen atom or a substituent, and * represents a bonding site for incorporation into the water-soluble polymer.
2. 2. The negative electrode composition according to claim 1, wherein the content of the water-soluble polymer is 2 parts by mass or more per 100 parts by mass of the carbon-coated silicon oxide.
3. The negative electrode composition according to claim 1 or 2, wherein the water-soluble polymer contains two or more components represented by the general formula (1) or (2).
4. 4. The negative electrode composition according to claim 1, wherein the acid group is a carboxy group or a salt thereof.
5. The negative electrode composition according to any one of claims 1 to 4, which is a negative electrode slurry containing a dispersion medium.
6. A negative electrode sheet having a layer constituted of the negative electrode composition according to any one of claims 1 to 5.
7. A non-aqueous secondary battery comprising a positive electrode active material layer, a separator, and a negative electrode active material layer in this order, the negative electrode active material layer being a layer constituted by the negative electrode composition according to any one of claims 1 to 5.
8. A method for producing a negative electrode sheet, comprising forming a film using the negative electrode composition according to any one of claims 1 to 5.
9. A method for producing a non-aqueous secondary battery, comprising incorporating the negative electrode sheet obtained by the method according to claim 8 into a negative electrode of the non-aqueous secondary battery.
Citation Information
Patent Citations
Composite particle for electrochemical element electrode, electrochemical element electrode material, electrochemical element electrode, and electrochemical element
JP2013051203A
Composite particle for electrochemical device electrode, electrochemical device electrode material, and electrochemical device electrode
JP2013084351A
Lithium ion rechargeable battery cells
JP2013179059A
Slurry for lithium ion battery negative electrode, method for manufacturing the same, negative electrode for lithium ion battery, and lithium ion battery
JP2018006334A
Negative electrode for nonaqueous electrolyte solution based electrochemical element, method for manufacturing the same, lithium ion secondary battery, and method for manufacturing the same
JP2018081753A