Composition for negative electrode, negative electrode sheet and non-aqueous secondary battery, and method for producing the negative electrode sheet and non-aqueous secondary battery

The use of a water-soluble polymer binder with carbon-coated silicon oxide in the negative electrode composition addresses the volume change issue in lithium ion batteries, resulting in high-capacity, low-resistance non-aqueous secondary batteries with improved cycle life.

JP7560656B2Active Publication Date: 2024-10-02FUJIFILM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023511396
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-09-29
Filing Date
2022-03-29
Publication Date
2024-10-02
Estimated Expiration
2042-03-29

AI Technical Summary

Technical Problem

Lithium ion secondary batteries using silicon oxide as a negative electrode active material face challenges with significant volume changes during charging and discharging, leading to reduced cycle life and performance deterioration.

Method used

A negative electrode composition is developed using carbon-coated silicon oxide with a binder containing a water-soluble polymer, which has an adsorption rate of 5 to 25% with respect to the carbon-coated silicon oxide, to form a negative electrode active material layer for non-aqueous secondary batteries, enhancing electron conductivity and mechanical stability.

Benefits of technology

The composition achieves high capacity, low resistance, and excellent cycle characteristics in non-aqueous secondary batteries by improving the binding of carbon-coated silicon oxide particles, thereby extending the battery's lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560656000017
    Figure 0007560656000017
  • Figure 0007560656000001
    Figure 0007560656000001
  • Figure 0007560656000002
    Figure 0007560656000002
Patent Text Reader

Abstract

A composition for a negative electrode, which comprises a binder comprising a water-soluble polymer and carbon-coated silicon oxide, in which the water-soluble polymer has a ratio of adsorption of the carbon-coated silicon oxide of 5 to 25%; a negative electrode sheet and a non-aqueous secondary battery, each of which is produced using the composition for a negative electrode; and a method for producing the negative electrode sheet and a method for producing the non-aqueous secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a negative electrode composition, a negative electrode sheet, a nonaqueous secondary battery, a method for producing a negative electrode sheet, and a method for producing a nonaqueous secondary battery. [Background technology]

[0002] Secondary batteries, such as lithium-ion secondary batteries, are used as power sources for portable electronic devices such as personal computers, video cameras, mobile phones, etc. Recently, against the backdrop of the global environmental challenge of reducing carbon dioxide emissions, they have become widespread as power sources for transportation equipment such as automobiles, and for storing electricity such as nighttime electricity and electricity generated by natural energy sources.

[0003] The electrodes (positive and negative electrodes) of a lithium-ion secondary battery have electrode active material layers (positive and negative active material layers), and these electrode active material layers contain electrode active material particles that can absorb or release lithium ions during charging and discharging. Since electrons are also transported between the electrode active material particles or between the electrode active material particles and the current collector, it is necessary to ensure electronic conductivity. To improve the efficiency of this electronic conduction, the binding property between the electrode active material particles or between the electrode active material particles and the current collector is important, and the electrode active material layers usually contain a binder.

[0004] In order to realize high-capacity lithium-ion secondary batteries, the use of silicon oxide as the negative electrode active material has been investigated. The theoretical capacity of silicon oxide is much higher than that of graphite, etc., and it is possible to achieve high energy density of the battery. When silicon oxide is used as the negative electrode active material, it absorbs a large amount of lithium ions and expands significantly during charging, and the silicon oxide also contracts significantly during discharging. Therefore, in lithium ion batteries using silicon oxide as the negative electrode active material, the volume of the negative electrode active material changes significantly during charging and discharging, and the battery performance is easily reduced by repeated charging and discharging. In other words, there is a limit to improving the cycle life. As a technique for dealing with such problems, for example, Patent Document 1 describes a slurry for the negative electrode of a lithium ion battery, which contains a negative electrode active material containing 20 mass % or more of silicon particles having a median diameter (D50) of 0.1 to 2 μm, poly(meth)acrylamide which is a radical copolymer of a monomer group including a (meth)acrylamide skeleton-containing monomer and a sulfonic acid group-substituted unsaturated hydrocarbon group-containing monomer and exhibits a specific high viscosity in an aqueous solution state of a specific concentration, and water. According to the technique described in the same patent document, it is said that a lithium ion secondary battery with excellent cycle life (cycle characteristics) can be obtained by using this negative electrode slurry.

[0005] It has also been proposed to coat silicon oxide with carbon and use it as an anode active material. It is said that the carbon coating can increase the electrical conductivity of silicon oxide particles and suppress side reactions between silicon oxide and electrolytes. Therefore, carbon-coated silicon oxide is expected to be a negative electrode active material for next-generation lithium-ion secondary batteries. For example, Patent Document 2 describes carbon-coated silicon oxide and a 1580 cm peak in an argon ion laser Raman spectrum. -1 Peak intensity at 1360cm -1 The patent document describes a slurry for a lithium ion battery negative electrode, which contains graphite having an R value, which is a peak intensity ratio, of 0.2 to 1.5, a binder, carbon black, and water. According to the patent document, a lithium ion secondary battery having an excellent cycle life can be obtained by doping a negative electrode mixture layer formed using the negative electrode slurry with lithium ions.

[0006] Electrodes for lithium-ion secondary batteries are usually formed by applying an electrode-forming composition (slurry) onto a current collector and drying it. Therefore, the slurry for forming the electrode is prepared by dispersing an electrode active material and a binder in a liquid medium. In recent years, with the background of increasing interest in environmental issues, there has been a demand for aqueous liquid media. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2018-6334 A [Patent Document 2] JP 2018-81753 A Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a negative electrode composition using carbon-coated silicon oxide as a negative electrode active material, which, when used to form a negative electrode active material layer of a nonaqueous secondary battery, can provide a nonaqueous secondary battery with high capacity and low resistance while also sufficiently extending the cycle life. Another object of the present invention is to provide a negative electrode sheet and a nonaqueous secondary battery using the negative electrode composition. Another object of the present invention is to provide a method for producing the negative electrode sheet and the nonaqueous secondary battery. [Means for solving the problem]

[0009] The above problems were solved by the following means. <1> The binder contains a water-soluble polymer, and carbon-coated silicon oxide. A composition for a negative electrode, wherein the water-soluble polymer has an adsorption rate of 5 to 25% with respect to the carbon-coated silicon oxide. <2> The water-soluble polymer is a chain-polymerized polymer. <1> The negative electrode composition according to claim 1 . <3> The water-soluble polymer comprises a component represented by the following general formula (1) or (2): <1> or <2> The negative electrode composition according to claim 1 . [ka] In general formula (1), R 1 represents a hydrogen atom or a methyl group, L 1 represents a single bond or a linking group, R 2indicates a substituent. * indicates a binding site for incorporation into the water-soluble polymer. In general formula (2), R 3 represents a hydrogen atom or a methyl group, R 4 and R 5 represents a hydrogen atom or a substituent. * represents a bonding site for incorporation into the water-soluble polymer. <4> The content of the water-soluble polymer is 2 parts by mass or more per 100 parts by mass of the carbon-coated silicon oxide. <1> ~ <3> 13. The negative electrode composition according to claim 12, <5> The water-soluble polymer contains two or more components represented by the general formula (1) or (2). <3> The negative electrode composition according to claim 1 . <6> A negative electrode slurry containing a dispersion medium, <1> ~ <5> 13. The negative electrode composition according to claim 12, <7> <1> ~ <6> 13. A negative electrode sheet having a layer formed using the negative electrode composition according to claim 12. <8> The positive electrode active material layer, the separator, and the negative electrode active material layer are arranged in this order. <1> ~ <6> 2. A non-aqueous secondary battery, comprising a layer formed using the negative electrode composition according to claim 1. <9> <1> ~ <6> 2. A method for producing a negative electrode sheet, comprising forming a film using the negative electrode composition according to claim 1. <10> <9> 2. A method for producing a non-aqueous secondary battery, comprising incorporating the negative electrode sheet obtained by the method for producing a non-aqueous secondary battery according to claim 1 into a negative electrode of the non-aqueous secondary battery.

[0010] In this specification, the term "water-soluble polymer" refers to a polymer that dissolves at least 7 g in 1 L of water at 25° C. (a polymer whose solubility at 25° C. is 7 [g / 1 L-H2O] or more). In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. In this specification, the term "compound" is used to mean not only the compound itself, but also its salts and ions. It also means a derivative in which a part of the structure is changed, for example by introducing a substituent, within the range in which the desired effect is achieved. In the present specification, when a substituent has a dissociable hydrogen atom (a group in which the hydrogen atom dissociates due to the action of a base), the substituent includes the form of an ion or a salt. For example, when a compound has a carboxy group, the carboxy group may be present as an anion with a hydrogen atom dissociated therefrom, and the anion may form a salt with a counter ion (cation). There are no particular limitations on the counter ion, and examples of the counter ion include alkali metal ions such as lithium ion, sodium ion, and potassium ion. In this specification, for substituents, linking groups, etc. (hereinafter referred to as substituents, etc.) that are not specified as substituted or unsubstituted, it means that the group may have an appropriate substituent. Therefore, even when it is simply described as "group" (e.g., "alkyl group") in this specification, this "group" (e.g., "alkyl group") includes not only an embodiment that does not have a substituent (e.g., "unsubstituted alkyl group"), but also an embodiment that further has a substituent (e.g., "substituted alkyl group"). This also applies to compounds that are not specified as substituted or unsubstituted. In this specification, when there are multiple substituents etc. designated by a specific symbol, or when multiple substituents etc. are simultaneously or alternatively specified, it means that the respective substituents etc. may be the same or different from each other. In addition, even if not specified otherwise, when multiple substituents etc. are adjacent, it means that they may be linked to each other or condensed to form a ring. In this specification, when a polymer has multiple components having the same designation (represented by the same general formula), each component may be the same or different from each other. In this specification, the term "nonaqueous secondary battery" includes nonaqueous electrolyte secondary batteries and all-solid-state secondary batteries. In this specification, the term "nonaqueous electrolyte" means an electrolyte that does not substantially contain water. That is, the "nonaqueous electrolyte" may contain a small amount of water within a range that does not impede the effects of the present invention. In the present invention, the "nonaqueous electrolyte" has a water concentration of 200 ppm (by mass) or less, preferably 100 ppm or less, and more preferably 50 ppm or less. Note that it is practically difficult to make a nonaqueous electrolyte completely anhydrous, and it usually contains 1 ppm or more of water. In this specification, the term "solid content" used when describing the content or content ratio means components other than the dispersion medium described below. Effect of the Invention

[0011] The negative electrode composition and negative electrode sheet of the present invention can be used to form a negative electrode active material layer, thereby imparting excellent cycle characteristics to a non-aqueous secondary battery using carbon-coated silicon oxide as a negative electrode active material, and therefore the non-aqueous secondary battery of the present invention has high capacity, low resistance, and excellent cycle characteristics. According to the method for producing a negative electrode sheet of the present invention, the above-mentioned negative electrode sheet of the present invention can be obtained. Also, according to the method for producing a nonaqueous secondary battery of the present invention, the above-mentioned nonaqueous secondary battery of the present invention can be obtained. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a vertical cross-sectional view showing a schematic diagram of a basic layered structure of a nonaqueous electrolyte secondary battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] [Negative electrode composition] The negative electrode composition of the present invention contains a binder containing a water-soluble polymer and a negative electrode active material containing carbon-coated silicon oxide. The water-soluble polymer has an adsorption rate of 5 to 25% to the carbon-coated silicon oxide. In the present invention, the adsorption rate is a value determined by the method described in the Examples below. When two or more water-soluble polymers are used, the value of the polymer with the highest adsorption rate is adopted. The adsorption rate is preferably 5 to 20%, and more preferably 10 to 20%. By incorporating the negative electrode active material layer prepared using the negative electrode composition of the present invention into a secondary battery, the cycle life of the resulting secondary battery can be effectively increased. Although the reason for this is not yet clear, it is presumed that one of the reasons is that the water-soluble polymer is firmly bound to the negative electrode active material (carbon-coated silicon oxide) by, for example, fitting into the voids in the carbon coating layer (producing an anchor effect) when the polymer having the above adsorption rate is contained in the binder. The negative electrode composition of the present invention can be prepared by mixing a binder containing a water-soluble polymer, a negative electrode active material containing carbon-coated silicon oxide, and, if necessary, a dispersion medium, a conductive assistant, and the like.

[0014] (binder) The binder used in the present invention includes the water-soluble polymer described above. From the viewpoint of improving the cycle characteristics of a nonaqueous secondary battery, the adsorption rate is preferably 8% or more, and more preferably 9% or more. The structure of the water-soluble polymer is not particularly limited as long as it has the above-mentioned adsorption rate (5 to 25%). The water-soluble polymer may be either a chain-polymerized polymer or a step-polymerized polymer, and is preferably a chain-polymerized polymer. The bonding form of the chain-polymerized polymer is not particularly limited, and may be either random or block.

[0015] The water-soluble polymer preferably contains, for example, a component represented by the following general formula (1) or (2).

[0016] [ka]

[0017] In general formula (1), R 1 represents a hydrogen atom or a methyl group, L 1 represents a single bond or a linking group (divalent), R 2 indicates a substituent. * indicates a binding site for incorporation into a water-soluble polymer. In general formula (2), R 3 represents a hydrogen atom or a methyl group, R 4 and R 5 represents a hydrogen atom or a substituent. * represents a bonding site for incorporation into a water-soluble polymer.

[0018] L 1 The linking group that can be used as the linking group is not particularly limited as long as it does not have an acid group. The chemical formula weight of this linking group is preferably 14 to 1,000, more preferably 14 to 500, and further preferably 26 to 250. L 1 Examples of the linking group that can be used include an alkylene group, -O-, a carbonyl group, an imino group, and a combination thereof. As for these combinations, a linking group formed by combining 2 to 6 of the alkylene groups, -O-, carbonyl groups, and imino groups is preferred, and a linking group formed by combining 2 or 3 of them is more preferred. L 1 Specifically, any one of -C(=O)-O-, -OC(=O)-, -NH-C(=O)-O-, -OC(=O)-NH-, -NH-C(=O)-NH-, and an alkylene group is preferable, and an alkylene group is more preferable. L 1 The alkylene group which can be taken as may be either linear or branched, and the number of carbon atoms in the alkylene group is preferably 1 to 10, more preferably 1 to 8, still more preferably 1 to 6, particularly preferably 1 to 4, and is most preferably any one of a methylene group, an ethylene group, an ethylethylene group, and a propylene group. L 1 The chemical formula weight is preferably 14-200, more preferably 14-150, and further preferably 14-100.

[0019] R 2is not particularly limited as long as it is a substituent that does not have an acid group. 2 The chemical formula weight of R is preferably 15 to 200, more preferably 15 to 150, and even more preferably 15 to 100. 2 Examples of the alkyl group include a hydroxy group, an alkyloxy group, an alkyl group, an amide group and a sulfonamide group, and a hydroxy group or an alkyloxy group is preferable. The alkyl group in the alkyloxy group may be linear, branched or cyclic. The number of carbon atoms in the alkyl group is preferably 1 to 10, more preferably 1 to 8, still more preferably 1 to 6, particularly preferably 1 to 4, and is most preferably any one of a methyl group, an ethyl group and an isopropyl group. The alkyl group has the same meaning as the alkyl group in the alkyloxy group, and the preferred range is also the same.

[0020] R 4 and R 5 Each of the chemical formula weights is preferably 1-200, more preferably 1-150, and further preferably 1-60. R 4 and R 5 The substituent which may be taken as the aryl group is preferably an alkyl group. The alkyl group is the same as R 2 The meaning of the alkyl group in the alkyloxy group that can be taken as R is the same as that of the alkyl group in the alkyloxy group that can be taken as R, and the preferred range is also the same. 4 and R 5 It is also preferable that the alkyl group which can be taken as the alkyl group further has a substituent. Examples of such a substituent include a hydroxy group, an alkylcarbonyl group, an amide group, and a urethane bond-containing group (-NH-CO-OR b (R b represents an alkyl group. 4 and R 5 As the substituent of the alkyl group which may be taken as the substituent, a hydroxy group is preferred. The alkyl group in the alkylcarbonyl group is the same as R 2 The alkyl group in the alkyloxy group that can be taken as R has the same meaning and preferable range. b The alkyl group represented by the above R2 The alkyl group has the same meaning as the alkyl group in the alkyloxy group which can be taken as the above, and the preferred range is also the same. R 4 and R 5 are preferably both hydrogen atoms, or one of them is a hydrogen atom and the other is a hydroxyalkyl group.

[0021] The constituent represented by the above general formula (1) or (2) preferably does not have an acid group.

[0022] The proportion of the component represented by the general formula (1) or (2) in the water-soluble polymer (the sum of the proportion of the component represented by the general formula (1) and the proportion of the component represented by the general formula (2) in the water-soluble polymer) is not particularly limited as long as the water-soluble polymer as a whole exhibits the above-mentioned adsorption rate. For example, the proportion of the component represented by the general formula (1) or (2) can be 30% by mass or more. In addition, the proportion of the component represented by the general formula (1) or (2) is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. From the viewpoint of improving the cycle characteristics of the secondary battery, the water-soluble polymer used in the present invention preferably contains two or more components represented by general formula (1) or (2), more preferably contains 2 to 6 components represented by general formula (1) or (2), and even more preferably contains 2 to 4 components represented by general formula (1) or (2). By containing two or more components represented by general formula (1) or (2), the water-soluble polymer can improve both the adsorption rate to the carbon-coated silicon oxide and the mechanical properties of the negative electrode sheet when used in the negative electrode sheet, and as a result, the cycle characteristics of the secondary battery can be further improved. In addition, examples of a form containing two or more components represented by general formula (1) or (2) include a form containing two or more components represented by general formula (1) and no component represented by general formula (2), a form containing two or more components represented by general formula (2) and no component represented by general formula (1), and a form containing both a component represented by general formula (1) and a component represented by general formula (2).

[0023] Preferred specific examples of the component represented by the above general formula (1) are shown below, but the present invention is not limited to these.

[0024] [ka]

[0025] Preferred specific examples of the component represented by the above general formula (2) are shown below, but the present invention is not limited to these.

[0026] [ka]

[0027] When the water-soluble polymer contains a component other than the component represented by the general formula (1) or (2) as a component not having an acid group, such a component is not particularly limited. For example, a component derived from a vinyl monomer such as styrene, maleimide, N-vinylacetamide, vinyl ester, or vinyl ether can be mentioned.

[0028] The water-soluble polymer may have a component having an acid group. The "acid group" of the component having an acid group means a group having a dissociable proton or a salt thereof. For example, a carboxy group, a sulfo group, a phosphoric acid group (-OP(=O)(OH)2), a phosphonic acid group (-P(=O)(OH)2) or a salt thereof is mentioned, and a carboxy group and a sulfo group or a salt thereof is preferred, and a carboxy group or a salt thereof is more preferred. Examples of the salt form include an alkali metal salt (e.g., a lithium salt, a sodium salt, a potassium salt, etc.).

[0029] The constituent having an acid group is not particularly limited, and the constituent usually contains 1 to 3 acid groups, preferably 1 or 2, and more preferably 1. The constituent having an acid group that the water-soluble polymer may have is preferably, for example, a constituent represented by the following general formula (3).

[0030] [ka]

[0031] In the formula, R 6 R represents a hydrogen atom or an acid group. 7 represents a hydrogen atom or a methyl group, L 2 represents a single bond or a linking group (divalent), R 8 indicates an acid group. * indicates a bonding site for incorporation into a water-soluble polymer.

[0032] L 2 The linking group which can be taken as is not particularly limited, and examples thereof include an alkylene group, an arylene group, a carbonyl group, -O- or an imino group, or a linking group which is a combination of two or more of these.

[0033] L 2 The alkylene group may be either linear or branched, and the number of carbon atoms in the alkylene group is preferably 1 to 10, more preferably 1 to 8, still more preferably 1 to 6, and particularly preferably 1 to 4. Specific examples of this alkylene group include a methylene group, an ethylene group, a propylene group, and a dimethylethylene group.

[0034] L 2 The number of carbon atoms in the arylene group which can be taken as the alkyl group is preferably 6 to 30, more preferably 6 to 20, further preferably 6 to 15, and further preferably 6 to 10. Specific examples of the arylene group include a phenylene group and a naphthylene group.

[0035] The above "linking group combining two or more types" is a linking group combining at least two types of an alkylene group, an arylene group, a carbonyl group, -O-, and an imino group, and is preferably a linking group combining 2 to 10 types, more preferably a linking group combining 2 to 7 types, and even more preferably a linking group combining 2 to 4 types. Specific examples of the above-mentioned "linking group combining two or more types" include a "carbonyl group-imino group-alkylene group" and a "carbonyl group-O-alkylene group".

[0036] The proportion of components having acid groups in the water-soluble polymer is preferably 30% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, even more preferably 3% by mass or less, particularly preferably 2% by mass or less, and it is most preferable that the water-soluble polymer does not have any components having acid groups.

[0037] Preferred specific examples of the component represented by the above general formula (3) are shown below, but the present invention is not limited to these.

[0038] [ka]

[0039] The weight average molecular weight of the water-soluble polymer used in the present invention is preferably 900,000 or less, more preferably 800,000 or less, and particularly preferably 700,000 or less. On the other hand, the weight average molecular weight of the water-soluble polymer is preferably 10,000 or more, more preferably 40,000 or more, and even more preferably 100,000 or more. From the viewpoint of the flex resistance of the negative electrode sheet, the weight-average molecular weight of the water-soluble polymer is also preferably 350,000 or more. In this specification, the weight average molecular weight of a polymer is a value obtained by measurement according to the method described in the Examples section below.

[0040] The above-mentioned adsorption rate of the water-soluble polymer used in the present invention is influenced by various factors. For example, physical interaction with the carbon coating layer, anchoring effect on the voids of the carbon coating layer, charge interaction with silicon oxide, etc. are included. Therefore, it is difficult to unequivocally explain whether such a polymer structure can realize the target adsorption rate, but it is presumed that the adsorption rate for carbon-coated silicon oxide can be changed into various ranges by controlling the type or amount of hydrophilic groups and hydrophobic groups in the polymer, or by controlling the molecular weight of the polymer.

[0041] In the binder used in the present invention, the content of the water-soluble polymer is preferably 5% by mass or more, and from the viewpoint of improving the cycle characteristics of the secondary battery, more preferably 10% by mass or more, and even more preferably 20% by mass or more. The binder used in the present invention may be composed of the water-soluble polymer.

[0042] From the viewpoint of improving the cycle characteristics of the secondary battery, the content of the water-soluble polymer in the negative electrode composition is preferably 2 parts by mass or more, more preferably 4 parts by mass or more, and even more preferably 8 parts by mass or more, per 100 parts by mass of the carbon-coated silicon oxide, while the content of the water-soluble polymer in the negative electrode composition is preferably 30 parts by mass or less, more preferably 24 parts by mass or less, and even more preferably 18 parts by mass or less, per 100 parts by mass of the carbon-coated silicon oxide. By including the water-soluble polymer in the negative electrode composition in an amount of 2 parts by mass or more per 100 parts by mass of carbon-coated silicon oxide, the carbon-coated silicon oxide can be coated, and the cycle characteristics of the secondary battery can be improved.

[0043] The binder used in the present invention can contain polymers other than the above water-soluble polymers as long as the effects of the present invention are not impaired. Examples of such polymers include, for example, water-insoluble polymers, and polymers having an adsorption rate of less than 5% or exceeding 20% with respect to carbon-coated silicon oxide. Specific examples of such polymers include, for example, Polymer B described in Table 1 below, but are not limited thereto.

[0044] (Negative electrode active material) The negative electrode active material used in the present invention contains carbon-coated silicon oxide (SiOx (0 < x ≤ 1.5)). The carbon-coated silicon oxide can reversibly occlude and release lithium ions. The entire surface of the silicon oxide may be carbon-coated, or there may be a portion that is not carbon-coated. Note that even if the entire surface of the silicon oxide is carbon-coated, the carbon-coated layer itself is in a state of having a large number of voids. The ratio of carbon atoms in the carbon-coated silicon oxide (in the total of the carbon-coated layer and silicon oxide) is not particularly limited, and from the viewpoint of achieving both conductivity and capacitance, for example, 0.2 to 5% by mass is preferable, 0.5 to 5% by mass is more preferable, 0.5 to 3% by mass is still more preferable, and 1 to 3% by mass is particularly preferable. Commercially available products can be used for the carbon-coated silicon oxide, and it can also be prepared by carbon-coating silicon oxide, for example, with reference to JP-A-2019-204686.

[0045] The negative electrode active material used in the present invention may contain a negative electrode active material other than the carbon-coated silicon oxide. Hereinafter, in the description of the negative electrode active material used in the present invention, a negative electrode active material other than the carbon-coated silicon oxide is referred to as "other negative electrode active material". It is preferable that the other negative electrode active material can reversibly occlude and release lithium ions. The material thereof is not particularly limited as long as it has the above characteristics, and examples include carbonaceous materials, metal oxides, metal composite oxides, lithium alloys, and negative electrode active materials capable of forming an alloy with lithium. The lithium alloy is not particularly limited as long as it is an alloy that is usually used as a negative electrode active material for secondary batteries, and an example thereof is a lithium aluminum alloy. The negative electrode active material capable of forming an alloy with lithium is not particularly limited as long as it is a material that is commonly used as a negative electrode active material for secondary batteries. Examples of such active materials include negative electrode active materials having tin atoms, and metals such as Al and In. Examples of the negative electrode active material containing tin atoms include Sn, SnO, SnO2, SnS, SnS2, and the above-mentioned active materials containing silicon atoms and tin atoms. Also included are composite oxides with lithium oxide, such as Li2SnO2. Among these, as the other negative electrode active material, carbonaceous materials are preferably used from the viewpoint of reliability.

[0046] The carbonaceous material used as the other negative electrode active material is a material substantially made of carbon. For example, carbon black such as petroleum pitch, graphite (natural graphite, artificial graphite such as vapor-grown graphite, etc.), and carbonaceous materials obtained by burning various synthetic resins such as PAN (polyacrylonitrile)-based resins or furfuryl alcohol resins can be mentioned. In addition, various carbon fibers such as PAN-based carbon fibers, cellulose-based carbon fibers, pitch-based carbon fibers, vapor-grown carbon fibers, dehydrated PVA (polyvinyl alcohol)-based carbon fibers, lignin carbon fibers, glassy carbon fibers, and activated carbon fibers, mesophase microspheres, graphite whiskers, and plate-like graphite can also be mentioned.

[0047] Other metal oxides and metal composite oxides that can be used as negative electrode active materials are not particularly limited as long as they are oxides that can absorb and release lithium, and amorphous oxides are preferred, and chalcogenides that are reaction products of metal elements and elements of group 16 of the periodic table are also preferred. The term "amorphous" as used herein means that the oxide has a broad scattering band with a peak in the 2θ value range of 20° to 40° in an X-ray diffraction method using CuKα rays, and may have crystalline diffraction lines. Among the compound group consisting of the above amorphous oxides and chalcogenides, the amorphous oxides of metalloid elements and the above chalcogenides are more preferred, and the oxides (excluding oxides containing Si) consisting of one or more of the elements of Groups 13 (IIIB) to 15 (VB) of the periodic table, Al, Ga, Si, Sn, Ge, Pb, Sb and Bi, or a combination of two or more of them, or chalcogenides are particularly preferred.Specific examples of preferred amorphous oxides and chalcogenides include Ga2O3, GeO, PbO, PbO2, Pb2O3, Pb2O4, Pb3O4, Sb2O3, Sb2O4, Sb2O8Bi2O3, Sb2O5, Bi2O3, Bi2O4, GeS, PbS, PbS2, Sb2S3 and Sb2S5.

[0048] The metal (composite) oxide and the above chalcogenide preferably contain at least one of titanium and lithium as a constituent from the viewpoint of high current density charge / discharge characteristics. Examples of the metal composite oxide containing lithium (lithium composite metal oxide) include composite oxides of lithium oxide and the above metal (composite) oxide or the above chalcogenide, more specifically Li2SnO2.

[0049] Other negative electrode active materials preferably contain titanium atoms. More specifically, TiNb2O7 (niobium titanate oxide [NTO]), Li4Ti5O 12 Lithium titanate (LTO) is preferred because it has excellent rapid charge / discharge characteristics due to its small volumetric change when absorbing and releasing lithium ions, and because it suppresses electrode deterioration and can improve the life of lithium ion secondary batteries.

[0050] The shape of the carbon-coated silicon oxide and other negative electrode active materials is not particularly limited, but is preferably particulate. The volume-based median diameter D50 of the carbon-coated silicon oxide and other negative electrode active materials is preferably 0.1 to 60 μm. To obtain a desired particle size, a conventional grinder or classifier is used. For example, a mortar, a ball mill, a sand mill, a vibration ball mill, a satellite ball mill, a planetary ball mill, a swirling airflow type jet mill, or a sieve is preferably used. During grinding, wet grinding in the presence of water or an organic solvent such as methanol can also be performed. In order to obtain a desired particle size, it is preferable to perform classification. The classification method is not particularly limited, and a sieve, a wind classifier, or the like can be used as desired. Classification can be performed both dry and wet.

[0051] The median diameter D50 of the carbon-coated silicon oxide is preferably from 0.1 to 30 μm, more preferably from 0.5 to 20 μm, and particularly preferably from 2 to 8 μm. The median diameter D50 can be determined by a laser diffraction method, for example, using SALD-2300 (product name) manufactured by Shimadzu Corporation.

[0052] When carbon-coated silicon oxide is used in combination with other negative electrode active materials, a combination of carbon-coated silicon oxide and a carbonaceous material is preferred, and a combination of carbon-coated silicon oxide and graphite is particularly preferred. When carbon-coated silicon oxide and graphite are combined, the blending ratio (carbon-coated silicon oxide / graphite, by mass) is preferably 0.1 or more, more preferably 0.2 or more, and even more preferably 0.3 or more. There is no particular upper limit to the blending ratio of carbon-coated silicon oxide to graphite, but 4 or less is practical, preferably 3 or less, and more preferably 2 or less. The content of carbon-coated silicon oxide in the negative electrode active material is not particularly limited and can be, for example, 10 to 90 mass %, preferably 10 to 50 mass %, and more preferably 15 to 40 mass %. When forming a negative electrode active material layer, the unit area (cm 2The mass (mg) (weight per unit area) of the carbon-coated silicon oxide and other negative electrode active materials is not particularly limited and can be appropriately determined according to the designed battery capacity.

[0053] The content of the carbon-coated silicon oxide and other negative electrode active materials in the negative electrode composition is not particularly limited, and is preferably 10 to 98 mass%, and more preferably 15 to 95 mass%, in total, based on 100 mass% of the solid content.

[0054] (dispersion medium) The negative electrode composition of the present invention can also contain a dispersion medium to form a negative electrode slurry. When a non-aqueous electrolyte secondary battery is produced using the negative electrode composition of the present invention, an aqueous medium containing water can be used as the dispersion medium. The "aqueous medium containing water" refers to water or a mixture of water and a water-soluble organic solvent. The "water-soluble organic solvent" refers to an organic solvent that is compatible with water, such as N-methylpyrrolidone, methanol, ethanol, acetone, and tetrahydrofuran.

[0055] (Conductive assistant) The negative electrode composition of the present invention may also contain a conductive assistant. The conductive assistant is not particularly limited, and may be any known conductive assistant. For example, it may be an electron conductive material such as graphites such as natural graphite and artificial graphite, carbon blacks such as acetylene black, ketjen black, and furnace black, amorphous carbon such as needle coke, carbon fibers such as vapor-grown carbon fibers or carbon nanotubes, carbonaceous materials such as graphene or fullerene, metal powders or metal fibers such as copper and nickel, or conductive polymers such as polyaniline, polypyrrole, polythiophene, polyacetylene, and polyphenylene derivatives. In the present invention, when a negative electrode active material and a conductive assistant are used in combination, among the above conductive assistants, those that do not insert or release Li when the secondary battery is charged and discharged and do not function as a negative electrode active material are considered to be conductive assistants. Therefore, among the conductive assistants, those that can function as a negative electrode active material in the negative electrode active material layer when the secondary battery is charged and discharged are classified as negative electrode active materials rather than conductive assistants. Whether or not a conductive assistant functions as a negative electrode active material when the secondary battery is charged and discharged is not unique, but is determined by the combination with the negative electrode active material.

[0056] The conductive assistant may be used alone or in combination of two or more kinds. The content of the conductive assistant in the negative electrode composition is preferably 1 to 30 mass %, more preferably 1 to 15 mass %, and further preferably 3 to 10 mass %, based on 100 mass % of the solid content.

[0057] The shape of the conductive assistant is not particularly limited, but is preferably particulate. The median diameter D50 of the conductive assistant is not particularly limited, but is, for example, preferably 0.01 to 50 μm, and more preferably 0.02 to 10.0 μm.

[0058] (Other additives) The negative electrode composition of the present invention may contain, as desired, other components in addition to the above-mentioned components, such as a lithium salt, an ionic liquid, a thickener, an antifoaming agent, a leveling agent, a dehydrating agent, an antioxidant, etc. In addition, the composition may contain a crosslinking agent (such as one that undergoes a crosslinking reaction by radical polymerization, condensation polymerization, or ring-opening polymerization) for chemically crosslinking the water-soluble polymer, and further a polymerization initiator (such as one that generates an acid or radicals by heat or light). With regard to the above-mentioned conductive assistant and other additives, reference can be made to, for example, International Publication No. 2019 / 203334 and Japanese Patent Application Laid-Open No. 2015-46389.

[0059] [Negative electrode sheet] The negative electrode sheet of the present invention has a layer (negative electrode active material layer) that is constructed (formed) using the negative electrode composition of the present invention. The negative electrode sheet of the present invention may have a negative electrode active material layer, and may be a sheet in which the negative electrode active material layer is formed on a substrate (current collector), or may be a sheet formed only of the negative electrode active material layer without having a substrate. This negative electrode sheet is usually a sheet having a configuration in which the negative electrode active material layer is laminated on the current collector. The negative electrode sheet of the present invention may have other layers such as a protective layer (release sheet) and a coating layer. The negative electrode sheet of the present invention can be suitably used as a material constituting the negative electrode active material layer of a secondary battery.

[0060] [Method of manufacturing negative electrode sheet] The negative electrode sheet of the present invention can be obtained by forming a negative electrode active material layer using the negative electrode composition of the present invention. For example, a current collector or the like is used as a substrate, and the negative electrode composition of the present invention is applied thereon (with or without another layer) to form a coating film, which is then dried to obtain an electrode sheet having a negative electrode active material layer (coated and dried layer) on the substrate.

[0061] [Non-aqueous secondary battery] The nonaqueous secondary battery of the present invention refers to any device in which ions pass between positive and negative electrodes via an electrolyte upon charging and discharging, and energy is stored and released at the positive and negative electrodes. That is, the nonaqueous secondary battery of the present invention includes both batteries and capacitors (e.g., lithium ion capacitors). From the viewpoint of the amount of energy stored, it is preferable that the nonaqueous secondary battery of the present invention is used for battery applications (not as a capacitor).

[0062] The nonaqueous secondary battery of the present invention will be described taking a nonaqueous electrolyte secondary battery as an example, however, the secondary battery of the present invention is not limited to a nonaqueous electrolyte secondary battery and broadly includes all nonaqueous secondary batteries including all-solid-state secondary batteries. A nonaqueous electrolyte secondary battery according to a preferred embodiment of the present invention includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode. The positive electrode includes a positive electrode current collector and a positive electrode active material layer in contact with the positive electrode current collector, and the negative electrode includes a negative electrode current collector and a negative electrode active material layer in contact with the negative electrode current collector. In the nonaqueous electrolyte secondary battery of the present invention, the negative electrode active material layer is formed using the electrode composition of the present invention.

[0063] FIG. 1 is a cross-sectional view showing a schematic of the laminated structure of a general non-aqueous electrolyte secondary battery 10, including the working electrodes when the battery is operated. The non-aqueous electrolyte secondary battery 10 has a laminated structure having, as viewed from the negative electrode side, a negative electrode current collector 1, a negative electrode active material layer 2, a separator 3, a positive electrode active material layer 4, and a positive electrode current collector 5, in this order. The space between the negative electrode active material layer and the positive electrode active material layer is filled with a non-aqueous electrolyte (not shown), and is separated by the separator 3. The separator 3 has pores, and functions as a positive and negative electrode separator that insulates between the positive and negative electrodes while allowing the electrolyte and ions to pass through during normal battery use. With this structure, for example, in the case of a lithium-ion secondary battery, electrons (e - ) is supplied, and at the same time, lithium ions (Li + ) moves and accumulates in the negative electrode. On the other hand, during discharge, the lithium ions (Li + ) is returned to the positive electrode side through the electrolyte, and electrons are supplied to the operating part 6. In the illustrated example, a light bulb is used as the operating part 6, and it is lit by the discharge. In the present invention, the negative electrode current collector 1 and the negative electrode active material layer 2 are collectively referred to as the negative electrode, and the positive electrode active material layer 4 and the positive electrode current collector 5 are collectively referred to as the positive electrode.

[0064] In the non-aqueous secondary battery of the present invention, the positive electrode active material material, the non-aqueous electrolyte, the solid electrolyte material, and other members are not particularly limited, except that the negative electrode active material layer is formed using the negative electrode composition of the present invention. These materials and members can be appropriately applied to those used in normal non-aqueous secondary batteries. In addition, for the method of producing the non-aqueous secondary battery of the present invention, a normal method can be appropriately adopted, except that the negative electrode active material layer is formed using the negative electrode composition of the present invention. For example, JP-A-2016-201308, JP-A-2005-108835, JP-A-2012-185938, and WO 2020 / 067106 can be appropriately referred to.

[0065] The nonaqueous secondary battery of the present invention can be mounted in electronic devices such as notebook computers, pen-input computers, mobile computers, electronic book players, mobile phones, cordless phone sub-units, pagers, handheld terminals, portable fax machines, portable copiers, portable printers, headphone stereos, video movie machines, liquid crystal televisions, handheld cleaners, portable CDs, mini-discs, electric shavers, transceivers, electronic organizers, calculators, portable tape recorders, radios, backup power sources, and memory cards. It can also be mounted in consumer devices such as automobiles, electric vehicles, motors, lighting equipment, toys, game equipment, road conditioners, watches, strobes, cameras, and medical equipment (pacemakers, hearing aids, shoulder massagers, etc.). It can also be combined with solar cells.

[0066] The present invention will be described in more detail with reference to examples. However, the present invention is not to be construed as being limited to these examples except as defined in the present invention. EXAMPLES

[0067] [Synthesis of Polymer A] <Synthesis of Polymer 1 (Polymer No. 1 in Table 1 below)> Polymer 1 shown in Table 1 below was synthesized as follows. A 500 mL separable flask was charged with 108.1 g of ion-exchanged water, and while stirring at 75°C under a nitrogen atmosphere, a mixture containing 17.5 g of 2-hydroxyethyl acrylate, 52.5 g of N-(2-hydroxyethyl)acrylamide, and 24.9 g of ion-exchanged water and a mixture containing 1.26 g of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate and 33.3 g of ion-exchanged water were simultaneously added dropwise over 1 hour. After the dropwise addition was completed, the mixture was stirred at 75°C for 2 hours to obtain a polymer solution with a solid content of 29.8% by mass.

[0068] <Synthesis of polymers 2 to 19 and c1 to c3 (synthesis of polymers No. 2 to 19 and c1 to c3 in Table 1 below) Polymers 2 to 19 and c1 to c3 were synthesized in the same manner as in the synthesis of Polymer 1, except that the monomers shown in Table 1 below were used in the mass ratios shown in Table 1 below as monomers from which the constituent components were derived.

[0069] <Synthesis of Polymers 20 to 23, c4, and c5 (Synthesis of Polymers No. 20 to 23, c4, and c5 in Table 3 below) Polymers 20 to 23, c4 and c5 were synthesized in the same manner as in the synthesis of Polymer 1, except that the monomers shown in Table 3 below were used in the mass ratios shown in Table 3 below as monomers from which the constituent components were derived.

[0070] <Synthesis of Polymers 25 to 28, c6, and c7 (Synthesis of Polymers No. 25 to 28, c6, and c7 in Table 5 below) Polymers 25 to 28, c6 and c7 were synthesized in the same manner as in the synthesis of Polymer 1, except that the monomers shown in Table 3 below were used in the mass ratios shown in Table 5 below as monomers from which the constituent components were derived.

[0071] [Carbon-coated silicon oxide] In preparing a negative electrode composition described below, active materials 1 to 3 (all manufactured by Osaka Titanium Co., Ltd.) shown in Table A below were used as carbon-coated silicon oxide. [Table A]

[0072] (Measurement of weight average molecular weight) The weight average molecular weight (Mw) of the polymer shown in Table 1 below is a weight average molecular weight calculated as sodium polyacrylate by gel permeation chromatography (GPC), and is a value measured under the following conditions. Measuring instrument: HLC-8220GPC (product name, manufactured by Tosoh Corporation) Columns: TOSOH TSKgel 5000PWXL (product name, manufactured by Tosoh Corporation), TOSOH TSKgel G4000PWXL (product name, manufactured by Tosoh Corporation), and TOSOH TSKgel G2500PWXL (product name, manufactured by Tosoh Corporation) were connected. Guard column: TSKgel guardcolumn PWXL (product name, manufactured by Tosoh Corporation) Carrier: 200mM sodium nitrate aqueous solution Rinse solution: Ultrapure water Carrier flow rate: Sample pump 1.0ml / min Reference pump 0.223mL / min Initial pump pressure: Sample pump 4.4MPa Reference pump 0.8MPa Sample concentration: 0.10% by mass Column temperature: 40℃ Detector temperature: 40℃ Collection time: 45 minutes (runtime 47.0 minutes) Detector: RI (refractive index) detector

[0073] (Measurement of adsorption rate) 40 mg of the aqueous polymer solution was poured into a 50 mL sample bottle in terms of solid content, and diluted with ion-exchanged water to 40.00 g including the polymer to obtain an aqueous polymer solution with a polymer concentration of 0.1% by mass. 800 mg of carbon-coated silicon oxide was placed in a 15 mL sample bottle. 8 g of the above polymer aqueous solution with a polymer concentration of 0.1% by mass was added to the sample bottle, and then the mixture was stirred at 80 rpm at 25°C for 1 hour using a mix rotor. After standing at 25°C for 30 minutes, the supernatant was filtered through a 0.45 μm filter to obtain a filtrate. GPC measurement was performed under the above conditions, and the adsorption rate (%) was calculated by applying the peak height (1) of the polymer aqueous solution and the peak height (2) of the filtrate to the following formula. The adsorption rate is shown in Table 2 below, together with the weight average molecular weight (adsorption molecular weight) obtained by GPC measurement. Adsorption rate (%) = 100 - {100 × peak height (2) / peak height (1)} The adsorption molecular weight was calculated from the difference between the GPC data of the aqueous polymer solution and the GPC data of the filtrate. The carbon-coated silicon oxide was the same as that used in the negative electrode composition.

[0074] [Preparation of negative electrode composition 1 (composition No. 1 in Table 2 below)] In a 60 mL ointment container (Umano Chemical Co., Ltd.), 30 parts by mass of the active material 1 described in Table A above, 70 parts by mass of graphite (product name: MAG-D, Hitachi Chemical Co., Ltd.), 5 parts by mass of acetylene black (product name: Denka Black, Denka Co., Ltd.), 5 parts by mass of polymer 1, and 22.5 parts by mass of distilled water were added and dispersed for 10 minutes at 2000 rpm using a foaming mixer (product name, THINKY Co., Ltd.). 27 parts by mass of distilled water was added to the dispersed liquid, and dispersed for 10 minutes at 2000 rpm using a foaming mixer, to obtain a negative electrode composition 1.

[0075] [Preparation of non-aqueous electrolyte secondary battery (2032 type coin battery) 1 (battery No. 1 in Table 2 below)] The obtained negative electrode composition 1 was applied onto a copper foil having a thickness of 20 μm using an applicator and dried for 1 hour at 80° C. Thereafter, pressure was applied using a press machine and then dried in a vacuum at 150° C. for 6 hours to obtain a negative electrode sheet having a negative electrode active material layer having a thickness of 25 μm. A disk having a diameter of 13.0 mm was cut out from the negative electrode sheet and used to form a negative electrode. Lithium foil (50 μm thick, 14.5 mmφ) and a polypropylene separator (25 μm thick, 16.0 mmφ) were stacked in this order, and 200 μL of 1M LiPF6 ethylene carbonate / ethyl methyl carbonate (volume ratio 1:2) electrolyte was impregnated into the separator. 200 μL of electrolyte was further impregnated into the separator, and the negative electrode sheet was stacked so that the negative electrode active material layer surface was in contact with the separator. Then, a 2032-type coin case was crimped to prepare a nonaqueous electrolyte secondary battery 1 (a battery having a laminate consisting of Li foil-separator-negative electrode active material layer-copper foil).

[0076] [Preparation of negative electrode compositions 2 to 19 and c1 to c3 (compositions No. 2 to 19 and c1 to c3 in Table 2 below)] Negative electrode compositions 2 to 19 and c1 to c3 were prepared in the same manner as in the preparation of the negative electrode composition 1, except that polymer 1 was replaced with polymers 2 to 19 and c1 to c3 shown in Table 1 below.

[0077] [Preparation of non-aqueous electrolyte secondary batteries 2 to 19 and c1 to c3 (batteries No. 2 to 19 and c1 to c3 in Table 2 below)] Non-aqueous electrolyte secondary batteries 2 to 19 and c1 to c3 were produced in the same manner as in the production of the non-aqueous electrolyte secondary battery 1, except that negative electrode compositions 2 to 19 and c1 to c3 shown in Table 2 below were used instead of the negative electrode composition 1.

[0078] [Test Example 1] Evaluation of cycle characteristics The discharge capacity retention rate of each coin battery was measured using a charge / discharge evaluation device: TOSCAT-3000 (product name, manufactured by Toyo Systems Co., Ltd.). Charging was performed at a C rate of 0.2C (a rate at which the battery is fully charged in 5 hours) until the battery voltage reached 0.02V. Discharging was performed at a C rate of 0.2C until the battery voltage reached 1.5V. Each coin battery was initialized by repeating three cycles of charging and discharging, with one charge and one discharge constituting one charge / discharge cycle. After the initialization, charging was performed at 0.5C until the voltage reached 0.02V. Discharging was performed at 0.5C until the voltage reached 1.5V. This one charge and one discharge constitutes one charge / discharge cycle, and 50 charge / discharge cycles were repeated to evaluate the cycle characteristics. When the discharge capacity at the first cycle after initialization (initial discharge capacity) was taken as 100%, the discharge capacity retention rate at the 50th cycle (100 x "discharge capacity at the 50th cycle" / "initial discharge capacity") was calculated, and the cycle characteristics were evaluated according to the following evaluation rank. Table 1 shows the polymer types and their characteristics, and Table 2 shows the test evaluation results using each composition. -Evaluation rank of discharge capacity retention rate (cycle characteristics)- 1: 95% or more 2: 90% or more, less than 95% 3: 85% or more, but less than 90% 4: Less than 85%

[0079] [Table 1]

[0080] [Table 2]

[0081] <Notes for Tables 1 and 2> The abbreviations of the monomers from which the components are derived are explained. Also, the structures of the components derived from the monomers are described. (Components not having an acid group) HEA: 2-hydroxyethyl acrylate HEAA: N-(2-hydroxyethyl)acrylamide Aam: Acrylamide MEA: 2-Methoxyethyl acrylate [ka]

[0082] (Components having acid groups) AA: Sodium acrylate AMPS: 2-acrylamido-2-methylpropanesulfonic acid [ka]

[0083] Latex: copolymer latex of styrene / 2-ethylhexyl acrylate / acrylic acid = 40 / 55 / 5 (mass ratio), Mw = 1.2 million, average primary particle size on a volume basis of 3 μm (solid content 15 mass %), this latex is water-insoluble. High acid group polymer: Random copolymer synthesized in the same manner as polymer 1 above ("HEAA / HEA / AA", HEAA:HEA:AA = 70:20:10 (mass ratio), Mw = 150,000) High molecular weight polymer: Random copolymer synthesized in the same manner as polymer 1 above ("HEAA / HEA", HEAA:HEA = 50:50 (mass ratio), Mw = 400,000)

[0084] "Content in polymer A (% by mass)": means the content in polymer A of a component having an acid group. "Content 1 (parts by mass)": When the content of carbon-coated silicon oxide in the negative electrode composition is taken as 100 parts by mass, this means the content of polymer A relative to 100 parts by mass of carbon-coated silicon oxide. "Content in binder (% by mass)" means the percentage of the content of the water-soluble polymer defined in the present invention relative to the total polymer contained in the binder. "Content 2 (parts by mass)": When the content of carbon-coated silicon oxide in the negative electrode composition is taken as 100 parts by mass, it means the content of polymer B relative to 100 parts by mass of carbon-coated silicon oxide. The content of "latex" is the content of solid content. "Water-soluble / water-insoluble": "Water" means that 7 g or more was dissolved in 1 L of water at 25° C., and "Non-water" means that less than 7 g was dissolved in 1 L of water at 25° C. All of the polymers A, including those used in the comparative examples, are water-soluble.

[0085] The polymer A used in the negative electrode compositions No. c1 to c3 had an adsorption rate of less than 5% to the carbon-coated silicon oxide. The batteries No. c1 and c3 produced using the negative electrode compositions No. c1 to c3 had poor cycle characteristics. In contrast, it is clear that the batteries (Nos. 1 to 19) produced using the negative electrode compositions (Nos. 1 to 19) of the present invention are excellent in cycle characteristics.

[0086] [Preparation of negative electrode compositions 20 to 24, c4 and c5 (compositions No. 20 to 24, c4 and c5 in Table 4 below)] Negative electrode compositions 20 to 24, c4, and c5 were prepared in the same manner as the negative electrode composition 1, except that the active material 1 and polymer 1 used in the preparation of the negative electrode composition 1 were replaced with the polymers and active materials shown in Table 4 below.

[0087] [Preparation of Nonaqueous Electrolyte Secondary Batteries 20 to 24, c4, and c5 (Batteries No. 20 to 24, c4, and c5 in Table 4 below)] Non-aqueous electrolyte secondary batteries 20 to 24, c4, and c5 were produced in the same manner as in the production of the non-aqueous electrolyte secondary battery 1, except that negative electrode compositions 20 to 24, c4, and c5 shown in Table 4 below were used instead of the negative electrode composition 1.

[0088] [Preparation of negative electrode sheets 20 to 24, c4 and c5 (negative electrode sheets No. 20 to 24, c4 and c5 in Table 4 below)] The negative electrode composition 20 was applied onto a copper foil having a thickness of 20 μm using an applicator and dried at 80° C. for 1 hour. It was further dried under vacuum at 100° C. for 6 hours to obtain a negative electrode sheet 20. The negative electrode sheet 20 was 50 mm wide, 150 mm long, and 90 μm thick, and the thickness of the negative electrode active material layer was 70 μm. Negative electrode sheets 21 to 24, c4, and c5 were prepared in the same manner as the negative electrode sheet 20, except that negative electrode compositions 21 to 24, c4, and c5 shown in Table 4 below were used instead of negative electrode composition 20.

[0089] The nonaqueous electrolyte secondary batteries 20 to 24, c4 and c5 were used to evaluate cycle characteristics according to the above-mentioned Test Example 1. In addition, the negative electrode sheets 20 to 24, c4 and c5 were used to evaluate bending resistance according to the later-described Test Example 2. The polymer types and their properties are shown in Table 3 below, and the results of the cycle characteristic evaluation and flex resistance evaluation are shown in Table 4 below.

[0090] [Test Example 2] Evaluation of bending resistance A test piece measuring 10 mm in width, 100 mm in length, and 90 μm in thickness was cut out from the produced negative electrode sheet, and this test piece was set in a cylindrical mandrel bending tester (BEVS 1603 (trade name, manufactured by Allgood Corporation). The test piece was wrapped around a mandrel rod so that the current collector of the test piece was in contact with the mandrel rod. The diameter of the mandrel rod was gradually reduced from 32 mm, and the diameter at which a crack first occurred in the negative electrode active material layer of the test piece was assigned to the following evaluation rank to evaluate bending resistance. -Bending resistance evaluation rank- 1: Less than 10mm 2: 10mm to less than 20mm 3: 20mm to less than 25mm 4: 25mm or more

[0091] [Table 3]

[0092] [Table 4]

[0093] <Notes for Tables 3 and 4> The meanings of "HEA," "AA," "HEAA," "Aam," "Content in polymer A (mass%)," "Content 1 (parts by mass)," "Content in binder (mass%)," and "Water" are the same as those in the "Notes to Tables 1 and 2" above.

[0094] The polymer A used in the negative electrode compositions of No. c4 and c5 has an adsorption rate of less than 5% on the carbon-coated silicon oxide. The batteries of No. c4 and c5 made using the negative electrode compositions of No. c4 and c5 had poor cycle characteristics. The electrode sheet of No. c4 also had poor bending resistance. In contrast, the batteries (Nos. 20 to 24) made using the negative electrode compositions of the present invention (Nos. 20 to 24) are found to have excellent cycle characteristics. Also, a comparison of the negative electrode sheets 22 and 24 with the negative electrode sheets 20, 21, and 23 shows that the use of a water-soluble polymer with a larger weight-average molecular weight can improve flex resistance.

[0095] It was confirmed that in negative electrode compositions 20 to 24, even if the content of active material 2 (30 parts by mass) and the content of graphite (70 parts by mass) were changed to "active material 2 (10 parts by mass), graphite (90 parts by mass)," "active material 2 (20 parts by mass), graphite (80 parts by mass)," "active material 2 (40 parts by mass), graphite (60 parts by mass)," "active material 2 (50 parts by mass), graphite (50 parts by mass)," or "active material 2 (60 parts by mass), graphite (40 parts by mass)," batteries with excellent cycle characteristics and negative electrode sheets with excellent flex resistance could be obtained.

[0096] [Preparation of negative electrode compositions 25 to 29, c6 and c7 (compositions No. 25 to 29, c6 and c7 in Table 6 below)] Negative electrode compositions 25 to 29, c6 and c7 were prepared in the same manner as the negative electrode composition 1, except that the active material 1 and polymer 1 used in the preparation of the negative electrode composition 1 were replaced with the polymers and active materials shown in Table 6 below.

[0097] [Preparation of Nonaqueous Electrolyte Secondary Batteries 25 to 29, c6, and c7 (Batteries No. 25 to 29, c6, and c7 in Table 6 below)] Non-aqueous electrolyte secondary batteries 25 to 29, c6, and c7 were produced in the same manner as in the production of the non-aqueous electrolyte secondary battery 1, except that negative electrode compositions 25 to 29, c6, and c7 shown in Table 6 below were used instead of negative electrode composition 1.

[0098] [Preparation of negative electrode sheets 25 to 29, c6 and c7 (negative electrode sheets No. 25 to 29, c6 and c7 in Table 6 below)] Negative electrode sheets 25 to 29, c6, and c7 were produced in the same manner as for producing the negative electrode sheet 20, except that negative electrode compositions 25 to 29, c6, and c7 were used instead of negative electrode composition 20.

[0099] The nonaqueous electrolyte secondary batteries 25 to 29, c6 and c7 were used to evaluate the cycle characteristics according to the above Test Example 1. The negative electrode sheets 25 to 29, c6 and c7 were used to evaluate the flex resistance according to the above Test Example 2. The polymer types and their properties are shown in Table 5 below, and the results of the cycle characteristic evaluation and flex resistance evaluation are shown in Table 6 below.

[0100] [Table 5]

[0101] [Table 6]

[0102] <Notes for Tables 5 and 6> The meanings of "HEA," "AA," "HEAA," "Aam," "Content in polymer A (mass%)," "Content 1 (parts by mass)," "Content in binder (mass%)," and "Water" are the same as those in the "Notes to Tables 1 and 2" above.

[0103] The polymer A used in the negative electrode compositions No. c6 and c7 had an adsorption rate of less than 5% on the carbon-coated silicon oxide. The batteries No. c6 and c7 made using the negative electrode compositions No. c6 and c7 had poor cycle characteristics. In contrast, the batteries (Nos. 25 to 29) made using the negative electrode compositions of the present invention (Nos. 25 to 29) are excellent in cycle characteristics and flex resistance. In addition, a comparison of the negative electrode sheets 27 and 29 with the negative electrode sheets 25, 26, and 28 shows that the flex resistance can be further improved by using a water-soluble polymer with a larger weight-average molecular weight.

[0104] It was confirmed that in negative electrode compositions 25 to 29, even if the content of active material 3 (30 parts by mass) and the content of graphite (70 parts by mass) were changed to "active material 3 (10 parts by mass), graphite (90 parts by mass)," "active material 3 (20 parts by mass), graphite (80 parts by mass)," "active material 3 (40 parts by mass), graphite (60 parts by mass)," "active material 3 (50 parts by mass), graphite (50 parts by mass)," or "active material 3 (60 parts by mass), graphite (40 parts by mass)," batteries with excellent cycle characteristics and negative electrode sheets with excellent flex resistance could be obtained.

[0105] Although the present invention has been described in conjunction with embodiments thereof, we do not intend to limit our invention to any of the details of the description unless specifically stated otherwise, and believe that the appended claims should be broadly construed without departing from the spirit and scope of the invention as set forth in the appended claims.

[0106] This application claims priority based on Patent Application No. 2021-060334 filed in Japan on March 31, 2021, and Patent Application No. 2021-159546 filed in Japan on September 29, 2021, the contents of which are incorporated herein by reference as part of the present specification. [Explanation of symbols]

[0107] 10 Nonaqueous electrolyte secondary battery 1 Negative electrode current collector 2 Negative electrode active material layer 3. Separator 4 Cathode active material layer 5 Positive electrode current collector 6. Working part (light bulb)

Claims

1. A binder including a water-soluble polymer that is a chain-polymerized polymer, and carbon-coated silicon oxide, the water-soluble polymer has an adsorption rate of 5 to 25% with respect to the carbon-coated silicon oxide; The water-soluble polymer contains a component represented by the following general formula (1) or (2), and the component represented by the general formula (1) or (2) does not have an acid group, A composition for a negative electrode, wherein the proportion of the component represented by the general formula (1) or (2) in the water-soluble polymer is 95 mass % or more. 【Chemistry 1】 In formula (1), R 1 represents a hydrogen atom or a methyl group, L 1 represents a single bond or a linking group, R 2 represents a substituent, and * represents a bonding site for incorporation into the water-soluble polymer. In formula (2), R 3 represents a hydrogen atom or a methyl group, R 4 and R 5 represent a hydrogen atom or a substituent, and * represents a bonding site for incorporation into the water-soluble polymer.

2. 2. The negative electrode composition according to claim 1, wherein the content of the water-soluble polymer is 2 parts by mass or more per 100 parts by mass of the carbon-coated silicon oxide.

3. The negative electrode composition according to claim 1 or 2, wherein the water-soluble polymer contains two or more components represented by the general formula (1) or (2).

4. The negative electrode composition according to any one of claims 1 to 3, which is a negative electrode slurry containing a dispersion medium.

5. A negative electrode sheet having a layer formed using the negative electrode composition according to any one of claims 1 to 4.

6. A non-aqueous secondary battery having a positive electrode active material layer, a separator, and a negative electrode active material layer in this order, the negative electrode active material layer being a layer formed using the negative electrode composition according to any one of claims 1 to 4.

7. A method for producing a negative electrode sheet, comprising forming a film using the negative electrode composition according to any one of claims 1 to 4.

8. A method for producing a non-aqueous secondary battery, comprising incorporating the negative electrode sheet obtained by the method according to claim 7 into a negative electrode of the non-aqueous secondary battery.

Citation Information

Patent Citations

  • Composite particle for electrochemical element electrode, electrochemical element electrode material, and electrochemical element electrode

    JP2013055044A

  • Slurry for lithium ion battery negative electrode, method for manufacturing the same, negative electrode for lithium ion battery, and lithium ion battery

    JP2018006334A

  • Negative electrode for nonaqueous electrolyte solution based electrochemical element, method for manufacturing the same, lithium ion secondary battery, and method for manufacturing the same

    JP2018081753A

  • Lithium-ion secondary cell provided with negative electrode for high energy density cell

    WO2018155609A1