Wiring sheet and method for producing same
The wiring sheet with a pseudo sheet structure and low-modulus electrodes addresses the issue of contact resistance, achieving accurate resistance measurements and improved conductivity.
Patent Information
- Application Number
- JP2023546518
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-03-30
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2042-03-30
AI Technical Summary
The existing wiring sheets exhibit higher resistance values due to contact resistance between conductive linear bodies and electrodes, which is not accounted for in the calculated values.
A wiring sheet design with a pseudo sheet structure and electrodes having a Young's modulus of 1×10^9 Pa or less, directly contacting conductive linear bodies, and gold-plated for reduced contact resistance.
The design effectively reduces contact resistance, ensuring the measured resistance values align closer to calculated values, enhancing conductivity and heat generation efficiency.
Smart Images

Figure 0007560676000002 
Figure 0007560676000003 
Figure 0007560676000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a wiring sheet. [Background technology]
[0002] A wiring sheet having a pseudo-sheet structure in which a plurality of metal wires are arranged at intervals is known. This wiring sheet can be used, for example, as a material for heat-generating textiles, a member for generating heat in various articles, and a heating element of a heat-generating device. For example, Patent Document 1 describes a sheet having a pseudo-sheet structure in which multiple linear elements extending in one direction are arranged at intervals as a sheet used as a heating element. A pair of electrodes is provided on both ends of the multiple linear elements, thereby obtaining a wiring sheet that can be used as a heating element. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2017 / 086395 Summary of the Invention [Problem to be solved by the invention]
[0004] However, it has been found that in the sheet described in Patent Document 1, the resistance value of the wiring sheet becomes higher than the calculated value due to the contact resistance between the conductive linear body and the electrode.
[0005] An object of the present invention is to provide a wiring sheet capable of reducing the contact resistance between a conductive linear body and an electrode. [Means for solving the problem]
[0006] According to one aspect of the present invention, there is provided a wiring sheet including a pseudo sheet structure in which a plurality of conductive linear bodies are arranged at intervals, and a pair of electrodes in direct contact with the conductive linear bodies, the Young's modulus of the electrodes being 1×109 Pa super 100×10 9 A wiring sheet having a resistance of 0.1 Pa or less is provided.
[0007] In the wiring sheet according to one embodiment of the present invention, it is preferable that the relationship between the resistance value R of the electrode in the axial direction and the overall resistance value r of the conductive linear body in the axial direction satisfies the condition represented by the following formula (F1). r>R (F1)
[0008] In the wiring sheet according to one aspect of the present invention, the electrodes preferably have a thickness of 40 μm or less.
[0009] In the wiring sheet according to one aspect of the present invention, the electrodes are preferably gold-plated.
[0010] In the wiring sheet according to one aspect of the present invention, the electrode has a Young's modulus of 1×10 9 Pa super 100×10 9 It is preferable that the conductor is made of only a conductor having a resistance of 0.1 Pa or less.
[0011] The wiring sheet according to one aspect of the present invention preferably further includes a resin layer that supports the pseudo sheet structure.
[0012] The wiring sheet according to one aspect of the present invention preferably further comprises a substrate supporting the pseudo sheet structure.
[0013] According to one aspect of the present invention, there is provided a method for producing a wiring sheet according to the aspect of the present invention, comprising the steps of: applying a conductive sheet having a Young's modulus of 1×10 to the pseudo sheet structure so as to be in direct contact with the conductive linear body; 9 Pa super 100×10 9 The present invention provides a method for manufacturing a wiring sheet, comprising the steps of forming a pair of electrodes made of a conductor having a resistivity of 0.1 Pa or less.
[0014] Advantageous Effects of Invention According to one aspect of the present invention, a wiring sheet capable of reducing the contact resistance between a conductive linear object and an electrode can be provided. [Brief description of the drawings]
[0015] [Figure 1] 1 is a schematic diagram showing a wiring sheet according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing the II-II cross section of FIG. [Figure 3A] 5A to 5C are diagrams illustrating a method for manufacturing a wiring sheet according to an embodiment of the present invention. [Figure 3B] 5A to 5C are diagrams illustrating a method for manufacturing a wiring sheet according to an embodiment of the present invention. [Figure 3C] 5A to 5C are diagrams illustrating a method for manufacturing a wiring sheet according to an embodiment of the present invention. [Figure 3D] 5A to 5C are diagrams illustrating a method for manufacturing a wiring sheet according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, the present invention will be described with reference to the drawings, taking an embodiment as an example. The present invention is not limited to the contents of the embodiment. In the drawings, some parts are illustrated enlarged or reduced in size for ease of explanation.
[0017] (Wiring sheet) 1 and 2, the wiring sheet 100 according to this embodiment includes a pseudo sheet structure 2 in which a plurality of conductive linear members 21 are arranged at intervals, and a pair of electrodes 4. The pseudo sheet structure 2 is electrically connected to the electrodes 4. And the Young's modulus of electrode 4 is 1×10 9 Pa super 100×10 9 Pa or less.
[0018] The reason why wiring sheet 100 according to the present embodiment can reduce the contact resistance between conductive linear body 21 and electrode 4 is not necessarily clear, but the inventors speculate as follows. That is, it is presumed that the contact resistance between the conductive linear body 21 and the electrode 4 is related to the ease with which the conductive linear body 21 cuts into the electrode 4 when the conductive linear body 21 is crimped to the electrode 4. If the electrode 4 is too hard (if the Young's modulus of the electrode 4 is too high), the conductive linear body 21 hardly cuts into the electrode 4. On the other hand, in the wiring sheet 100 according to the present embodiment, the Young's modulus of the electrode 4 is within the above range, and therefore the conductive linear body 21 cuts into the electrode 4 to an appropriate degree. The inventors presume that in this way, the contact resistance between the conductive linear body 21 and the electrode 4 can be reduced.
[0019] (base material) The base material 1 can directly or indirectly support the pseudo sheet structure 2. The base material 1 does not necessarily have to be provided. The base material 1 is a member that is provided as necessary. Examples of the substrate 1 include a resin film, paper, metal foil, nonwoven fabric, cloth, and glass. Substrate 1 is preferably transparent or has visibility. With such a configuration, the light transmittance of wiring sheet 100 can be improved. Furthermore, base material 1 may have elasticity. When base material 1 has elasticity, the elasticity of wiring sheet 100 can be ensured even when pseudo sheet structure 2 is provided on base material 1. Examples of resin films include polyethylene films, polypropylene films, polybutene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polyethylene naphthalate films, polybutylene terephthalate films, polyurethane films, ethylene-vinyl acetate copolymer films, ionomer resin films, ethylene-(meth)acrylic acid copolymer films, ethylene-(meth)acrylic acid ester copolymer films, polystyrene films, polycarbonate films, and polyimide films, as well as crosslinked films and laminated films thereof. Examples of the nonwoven fabric include spunbond nonwoven fabric, needle punch nonwoven fabric, melt blown nonwoven fabric, and spunlace nonwoven fabric. Examples of the cloth include woven fabric and knitted fabric. Examples of the glass include glass plate, glass fiber, and glass film. For the reasons mentioned above, the substrate 1 is preferably a resin film, a nonwoven fabric, a cloth, or glass, more preferably a resin film or glass, and particularly preferably a polyethylene terephthalate film or a glass plate. The thickness of the substrate 1 is not particularly limited. The thickness of the substrate 1 is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 50 μm or more. The thickness of the substrate 1 is preferably 10 mm or less, more preferably 5 mm or less, and even more preferably 3 mm or less.
[0020] (pseudo seat structure) The pseudo sheet structure 2 has a structure in which a plurality of conductive linear bodies 21 are arranged at intervals from one another. That is, the pseudo sheet structure 2 is a structure in which a plurality of conductive linear bodies 21 are arranged at intervals from one another to form a flat or curved surface. The conductive linear bodies 21 extend in one direction and have a straight or wavy shape in a plan view of the wiring sheet 100. The pseudo sheet structure 2 has a structure in which a plurality of conductive linear bodies 21 are arranged in a direction perpendicular to the axial direction of the conductive linear bodies 21. The conductive linear body 21 may be linear or wavy in plan view of the wiring sheet 100. Examples of the wave shape include a sine wave, a rectangular wave, a triangular wave, and a sawtooth wave. If the pseudo sheet structure 2 has such a structure, breakage of the conductive linear body 21 can be suppressed when the wiring sheet 100 is stretched in the axial direction of the conductive linear body 21.
[0021] The volume resistivity of the conductive linear body 21 is 1×10 -9 It is preferable that the resistance is Ω·m or more, and 1×10 -8 The volume resistivity of the conductive linear body 21 is preferably 1×10-3 It is preferable that the resistance is Ω·m or less, and 1×10 -4 It is more preferable that the volume resistivity is Ω·m or less. When the volume resistivity of the conductive linear members 21 is in the above range, the surface resistance of the pseudo sheet structure 2 tends to decrease. The volume resistivity of the conductive linear body 21 was measured as follows. Silver paste was applied to both ends of the conductive linear body 21, and the resistance was measured at a portion 300 mm from each end. The cross-sectional area (unit: m 2 ) is multiplied by the resistance value, and the obtained value is divided by the measured length (0.3 m) to calculate the volume resistivity of the conductive linear body 21.
[0022] The cross-sectional shape of the conductive linear body 21 is not particularly limited and may be polygonal, flat, elliptical, circular, or the like. From the viewpoint of compatibility with the resin layer 3, an elliptical or circular shape is preferable. When the cross section of the conductive linear member 21 is circular, the thickness (diameter) D (see FIG. 2) of the conductive linear member 21 is preferably 3 μm or more and 75 μm or less. From the viewpoints of suppressing an increase in sheet resistance and improving heat generation efficiency and dielectric breakdown resistance characteristics when the wiring sheet 100 is used as a heating element, the diameter D of the conductive linear member 21 is more preferably 5 μm or more, and even more preferably 8 μm or more. Moreover, the diameter D of the conductive linear member 21 is more preferably 60 μm or less, even more preferably 40 μm or less, and particularly preferably 25 μm or less. When the cross section of the conductive linear body 21 is elliptical, it is preferable that the major axis of the conductive linear body 21 is in the same range as the diameter D described above.
[0023] The diameter D of the conductive linear body 21 is determined by observing the conductive linear body 21 of the pseudo sheet structure 2 using a digital microscope, measuring the diameter of the conductive linear body 21 at five randomly selected points, and averaging the measured values.
[0024] The interval L (see FIG. 2) between the conductive linear members 21 is preferably 0.3 mm or more, more preferably 0.5 mm or more, and even more preferably 0.8 mm or more. The interval L between the conductive linear members 21 is preferably 50 mm or less, more preferably 30 mm or less, and even more preferably 20 mm or less. If the spacing between the conductive linear bodies 21 is within the above range, the conductive linear bodies are relatively densely packed, thereby improving the functionality of the wiring sheet 100, such as maintaining a low resistance of the pseudo sheet structure and making the distribution of temperature rise uniform when the wiring sheet 100 is used as a heating element.
[0025] The interval L between the conductive linear members 21 is measured by observing the conductive linear members 21 of the pseudo sheet structure 2 using a digital microscope and measuring the interval between two adjacent conductive linear members 21. The interval between two adjacent conductive linear bodies 21 is the length along the direction in which the conductive linear bodies 21 are arranged, and is the length between opposing portions of the two conductive linear bodies 21 (see FIG. 2). When the conductive linear bodies 21 are arranged at uneven intervals, the interval L is the average value of the intervals between all adjacent conductive linear bodies 21.
[0026] The conductive linear body 21 is not particularly limited, but is preferably a linear body including a metal wire (hereinafter also referred to as a "metal wire linear body"). Since metal wire has high thermal conductivity, high electrical conductivity, and high handling properties, when a metal wire linear body is used as the conductive linear body 21, the resistance value of the pseudo sheet structure 2 is reduced while light transmittance is easily improved. Furthermore, when the wiring sheet 100 (pseudo sheet structure 2) is used as a heating body, rapid heat generation is easily achieved. Furthermore, as described above, a linear body with a small diameter is easily obtained. In addition to a metal wire, examples of the conductive linear body 21 include a linear body containing a carbon nanotube and a linear body in which a thread is provided with a conductive coating.
[0027] The metal wire linear body may be a linear body made of a single metal wire, or may be a linear body made of a plurality of twisted metal wires. Examples of the metal wire include wires containing metals such as copper, aluminum, tungsten, iron, molybdenum, nickel, titanium, silver, and gold, or alloys containing two or more metals (for example, steels such as stainless steel and carbon steel, brass, phosphor bronze, zirconium-copper alloys, beryllium copper, iron-nickel, nichrome, nickel-titanium, Kanthal, Hastelloy, and rhenium-tungsten). The metal wire may be plated with gold, tin, zinc, silver, nickel, chromium, nickel-chromium alloys, or solder, or may be coated with a carbon material or polymer described below. In particular, wires containing one or more metals selected from tungsten and molybdenum and alloys containing them are preferable from the viewpoint of forming a conductive linear body 21 that is thin, has high strength, and has a low volume resistivity. It is particularly preferable that the metal wires are gold-plated, which can suppress migration of the metal wires. The metal wire may be a metal wire coated with a carbon material. When the metal wire is coated with a carbon material, the metallic luster is reduced, and the presence of the metal wire can be easily made less noticeable. In addition, when the metal wire is coated with a carbon material, metal corrosion is also suppressed. Examples of the carbon material that coats the metal wire include amorphous carbon (for example, carbon black, activated carbon, hard carbon, soft carbon, mesoporous carbon, and carbon fiber), graphite, fullerene, graphene, and carbon nanotubes.
[0028] The conductive linear body 21 may be a linear body having a conductive coating applied to the thread. Examples of the thread include threads spun from resins such as nylon and polyester. Examples of the conductive coating include coatings of metals, conductive polymers, carbon materials, etc. The conductive coating can be formed by plating or deposition. A linear body having a conductive coating applied to the thread can improve the conductivity of the linear body while maintaining the flexibility of the thread. In other words, it becomes easier to reduce the resistance of the pseudo sheet structure 2.
[0029] (Resin layer) The resin layer 3 is a layer containing resin. The pseudo sheet structure 2 can be supported directly or indirectly by this resin layer 3. The resin layer 3 is not necessarily provided. The resin layer 3 is a member that is provided as necessary. The resin layer 3 is preferably a layer containing an adhesive. When forming the pseudo sheet structure 2 on the resin layer 3, the adhesive makes it easy to attach the conductive linear body 21 to the resin layer 3. The resin layer 3 is preferably stretchable. In such a case, the stretchability of the wiring sheet 100 can be ensured.
[0030] When the resin layer 3 contains an adhesive, the adhesive applied to the resin layer 3 is not particularly limited. For example, a drying-solidifying adhesive, a heat-melting adhesive, a curing adhesive (curing adhesive), a pressure-sensitive adhesive, and the like can be used as the adhesive. The drying-solidifying adhesive refers to an adhesive that is solidified by removing moisture or solvent by drying an adhesive composition after application. The curing adhesive refers to an adhesive that is solidified by applying an adhesive composition, optionally drying it, and then causing a chemical reaction. The curing adhesive includes (1) an adhesive that is solidified by performing at least one of a heating treatment and an energy ray irradiation treatment to cause a chemical reaction such as a polymerization reaction, and (2) an adhesive that is solidified by reacting with moisture (moisture). The heat-melting adhesive refers to an adhesive that melts with heat and bonds by cooling. The pressure-sensitive adhesive refers to an adhesive (adhesive) that bonds by the adhesiveness of a pressure-sensitive adhesive (pressure-sensitive adhesive). For example, an adhesive that is moistened to exhibit stickability can be used as the adhesive of the resin layer 3.
[0031] The resin layer 3 may be a layer containing an adhesive (pressure-sensitive adhesive). The adhesive of the adhesive layer is not particularly limited. For example, examples of the adhesive include an acrylic adhesive, a urethane adhesive, a rubber adhesive, a polyester adhesive, a silicone adhesive, and a polyvinyl ether adhesive. Among these, the adhesive is preferably at least one selected from the group consisting of an acrylic adhesive, a urethane adhesive, and a rubber adhesive, and more preferably an acrylic adhesive.
[0032] Examples of acrylic adhesives include acrylic polymers containing structural units derived from alkyl (meth)acrylates having a straight-chain alkyl group or a branched-chain alkyl group (i.e., polymers obtained by polymerizing at least alkyl (meth)acrylates), acrylic polymers containing structural units derived from (meth)acrylates having a cyclic structure (i.e., polymers obtained by polymerizing at least (meth)acrylates having a cyclic structure), etc. Here, "(meth)acrylate" is used as a term indicating both "acrylate" and "methacrylate", and the same applies to other similar terms.
[0033] The acrylic polymer (including homopolymers and copolymers) may be crosslinked with a crosslinking agent. Examples of the crosslinking agent include epoxy crosslinking agents, isocyanate crosslinking agents, aziridine crosslinking agents, and metal chelate crosslinking agents. When crosslinking the acrylic polymer, at least one of a hydroxyl group and a carboxyl group that react with these crosslinking agents can be introduced into the acrylic polymer as a functional group derived from the monomer component of the acrylic polymer.
[0034] The resin layer 3 is not particularly limited, and may be, for example, curable or not curable. For example, when the resin layer 3 contains an adhesive, or when the resin layer 3 contains a pressure-sensitive adhesive, the resin layer 3 may be curable or not curable. The resin layer 3 is preferably a curable resin layer from the viewpoint that the resin layer 3 can constitute the outermost layer of the wiring sheet 100. If the resin layer 3 is a curable resin layer, the surface of the resin layer 3 is likely to have excellent scratch resistance. In addition, the resin layer 3 is more preferably an energy ray curable resin layer from the viewpoint of ease of application. Examples of the energy ray curable resin layer include ultraviolet rays, visible light, infrared rays, and electron beams. In addition, "energy ray curing" also includes heat curing by heating using energy rays.
[0035] In this specification, curing does not simply mean that the curable resin reacts, but also means that the tackiness of the surface of the cured resin layer 3 is suppressed (preferably, the tackiness is eliminated), and that the surface of the cured resin layer 3 has excellent scratch resistance.
[0036] Furthermore, when resin layer 3 constitutes the outermost layer of wiring sheet 100, resin layer 3 preferably has little tackiness, and more preferably has no tackiness. Furthermore, from this viewpoint, resin layer 3 is preferably a curable resin, and more preferably a curable adhesive layer containing an energy ray curable resin.
[0037] In this specification, tackiness refers to a sticky feeling that occurs on the surface of a substance. In this embodiment, tackiness refers to a sticky feeling that occurs on the surface of the resin layer 3.
[0038] When the resin layer 3 is an energy ray curable resin layer, it may contain an energy ray curable resin. For example, when the resin layer 3 is a layer containing an adhesive, the resin layer 3 is formed from an adhesive composition containing an energy ray curable resin in addition to the adhesive. Also, for example, when the resin layer 3 is a layer containing an adhesive, the resin layer 3 is formed from an adhesive composition containing an energy ray curable resin. As the energy ray curable resin, for example, a compound having at least one polymerizable double bond in the molecule can be mentioned. As the compound having at least one polymerizable double bond in the molecule, an acrylate compound having a (meth)acryloyl group is preferable. Examples of the acrylate-based compound include (meth)acrylates containing a chain aliphatic skeleton, (meth)acrylates containing a cyclic aliphatic skeleton, oligoester (meth)acrylates, urethane (meth)acrylate oligomers, epoxy-modified (meth)acrylates, polyalkylene glycol (meth)acrylates, polyether (meth)acrylates other than polyalkylene glycol (meth)acrylates, and itaconic acid oligomers. The energy ray curable resin may be used alone or in combination of two or more. When the energy ray curable resin contains two or more types, the combination of the energy ray curable resins and the ratio thereof can be selected according to the purpose.
[0039] The weight average molecular weight (Mw) of the energy ray curable resin is preferably 100 or more, and more preferably 300 or more. The weight average molecular weight (Mw) of the energy ray curable resin is preferably 30,000 or less, and more preferably 10,000 or less.
[0040] When the resin layer 3 is an energy ray-curable resin layer, the energy ray-curable resin may be combined with a thermoplastic resin described later, and the combination and ratio of the energy ray-curable resin and the thermoplastic resin can be selected according to the purpose.
[0041] When the resin layer 3 is a thermosetting resin layer, the resin layer 3 contains a thermosetting resin. The thermosetting resin used in the resin layer 3 is not particularly limited, and specifically includes epoxy resin, phenol resin, melamine resin, urea resin, polyester resin, urethane resin, acrylic resin, benzoxazine resin, phenoxy resin, amine-based compound, and acid anhydride-based compound. These can be used alone or in combination of two or more. Among these, from the viewpoint of suitability for curing using an imidazole-based curing catalyst, it is preferable to use one or more of epoxy resin, phenol resin, melamine resin, urea resin, amine-based compound, and acid anhydride-based compound as the thermosetting resin. In particular, from the viewpoint of showing excellent curability, it is preferable to use epoxy resin, phenol resin, a mixture thereof, or a mixture of epoxy resin and at least one selected from the group consisting of phenol resin, melamine resin, urea resin, amine-based compound, and acid anhydride-based compound as the thermosetting resin.
[0042] When the resin layer 3 is a moisture-curable resin layer, the resin layer 3 contains a moisture-curable resin. The moisture-curable resin used in the resin layer 3 is not particularly limited, and examples thereof include moisture-curable urethane resin (a resin produced by curing an isocyanate group with moisture) and modified silicone resin.
[0043] When at least one of an energy ray curable resin and a thermosetting resin is used in the resin layer 3, it is preferable that a photopolymerization initiator, a thermal polymerization initiator, and the like are used in the resin layer 3. When the resin layer 3 contains an energy ray curable resin, a crosslinked structure is formed in the resin layer 3 by using a photopolymerization initiator, and the like. When the resin layer 3 contains a thermosetting resin, a crosslinked structure is formed in the resin layer 3 by using a thermal polymerization initiator, and the like. Therefore, the conductive linear body 21 is more likely to be protected by the resin layer 3 more firmly.
[0044] Examples of the photopolymerization initiator include benzophenone, acetophenone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin benzoic acid, benzoin methyl benzoate, benzoin dimethyl ketal, 2,4-diethylthioxanthone, 1-hydroxycyclohexyl phenyl ketone, benzyl diphenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, 2-chloroanthraquinone, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenyl-phosphine oxide.
[0045] Examples of the thermal polymerization initiator include hydrogen peroxide, peroxodisulfates (ammonium peroxodisulfate, sodium peroxodisulfate, potassium peroxodisulfate, etc.), azo compounds (2,2'-azobis(2-amidinopropane) dihydrochloride, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobisisobutyronitrile, 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), etc.), and organic peroxides (benzoyl peroxide, lauroyl peroxide, peracetic acid, persuccinic acid, di-t-butyl peroxide, t-butyl hydroperoxide, cumene hydroperoxide, etc.).
[0046] These polymerization initiators can be used alone or in combination of two or more. When forming a crosslinked structure using these polymerization initiators, the amount of the polymerization initiator used is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, relative to 100 parts by mass of at least one of the energy ray curable resin and the thermosetting resin. The amount of the polymerization initiator used is preferably 100 parts by mass or less, more preferably 10 parts by mass or less, relative to 100 parts by mass of at least one of the energy ray curable resin and the thermosetting resin.
[0047] The resin layer 3 may not be curable, and may be, for example, a layer made of a thermoplastic resin composition. The thermoplastic resin layer can be softened by including a solvent (water, solvent, etc.) in the thermoplastic resin composition. This makes it easier to arrange the conductive linear body 21 on the resin layer 3 when forming the conductive linear body 21 on the resin layer 3. On the other hand, the thermoplastic resin layer can be dried and solidified by volatilizing the solvent in the thermoplastic resin composition.
[0048] Examples of the thermoplastic resin include polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyvinyl acetate, polyurethane, polyether, polyethersulfone, polyimide, and acrylic resin. Examples of the solvent include alcohol-based solvents, ketone-based solvents, ester-based solvents, ether-based solvents, hydrocarbon-based solvents, and alkyl halide-based solvents, as well as water.
[0049] The resin layer 3 may contain an inorganic filler. By containing an inorganic filler, the hardness of the cured resin layer 3 can be further improved. In addition, the thermal conductivity of the resin layer 3 is improved.
[0050] Examples of inorganic fillers include inorganic powders (e.g., powders of silica, alumina, talc, calcium carbonate, titanium white, red iron oxide, silicon carbide, metals, and boron nitride), beads obtained by sphering inorganic powders, single crystal fibers, and glass fibers. Among these, silica fillers and alumina fillers are preferred as inorganic fillers. The inorganic fillers may be used alone or in combination of two or more.
[0051] The resin layer 3 may contain other components, such as well-known additives, such as an organic solvent, a flame retardant, a tackifier, an ultraviolet absorber, an antioxidant, a preservative, an antifungal agent, a plasticizer, an antifoaming agent, and a wettability adjuster.
[0052] The thickness of resin layer 3 is appropriately determined depending on the application of wiring sheet 100. For example, from the viewpoint of adhesiveness, the thickness of resin layer 3 is preferably 3 μm or more, and more preferably 5 μm or more. Moreover, the thickness of resin layer 3 is preferably 150 μm or less, and more preferably 100 μm or less.
[0053] (electrode) The electrodes 4 are used to supply a current to the conductive linear body 21. The electrodes 4 are in direct contact with the conductive linear body 21. The electrodes 4 are disposed so as to be electrically connected to both ends of the conductive linear body 21. In this embodiment, the Young's modulus of the electrode 4 is 1×10 9 Pa super 100×10 9 It is necessary that the pressure is less than or equal to Pa. Young's modulus of electrode 4 is 1×10 9 If the Young's modulus of the electrode 4 is less than 100×10 Pa, the electrode 4 becomes easily deformed, and as a result, the volume resistivity tends to become too high, and the resistance value of the electrode 4 may become too high. 9 If it exceeds Pa, the contact resistance between the conductive linear body 21 and the electrode 4 cannot be reduced. From a similar viewpoint, the Young's modulus of the electrode 4 is 10×10 9 Pa or more, and 20×10 9 More preferably, the pressure is 30×10 Pa or more. 9 More preferably, the pressure is 50×10 Pa or more. 9 The Young's modulus of the electrode 4 is particularly preferably 90×10 Pa or more. 9 Pa or less, and 80×10 9 Pa or less, and more preferably 70×10 9 It is particularly preferable that the pressure is 0.1 Pa or less. The Young's modulus of the electrode 4 can be measured by a continuous stiffness measurement method. Specifically, it can be measured by the method described in the examples below.
[0054] The electrode 4 can be formed using a known electrode material having a Young's modulus within the above range. Examples of the electrode material include a conductive paste (such as silver paste) and a metal foil (such as a solder alloy foil). Electrode 4 has a Young's modulus of 1×10 9 Pa super 100×10 9 It is preferable that the electrode 4 is made only of a conductor having a resistivity of not more than 1 Pa. Use of such an electrode 4 can more reliably reduce the contact resistance between the conductive linear body 21 and the electrode 4. From the same viewpoint, it is also preferable that the electrode 4 is made only of a conductor formed from a conductive paste. Examples of the conductive paste include silver paste, copper paste, and carbon paste. Among these, silver paste is preferred from the viewpoint of low volume resistivity.
[0055] The electrode 4 is preferably gold-plated, which can suppress migration of the electrode 4. The width of one of the pair of electrodes 4 is preferably 10 mm or less, more preferably 5 mm or less, and even more preferably 3 mm or less, in a plan view of the pseudo sheet structure 2. The lower limit of the width of one of the pair of electrodes 4 may be, for example, 0.1 mm or more. The thickness of the electrode 4 is preferably 40 μm or less, more preferably 30 μm or less, and even more preferably 20 μm or less. If the thickness of the electrode 4 is equal to or less than the above-mentioned upper limit, deformation of the conductive linear body 21 tends to be small when the conductive linear body 21 and the electrode 4 are brought into contact with each other, and conduction tends to be stable. The lower limit of the thickness of the electrode 4 may be, for example, 1 μm or more.
[0056] It is preferable that the relationship between the resistance value R of the electrode 4 in the axial direction and the total resistance value r of the conductive linear body 21 in the axial direction satisfies the condition expressed by the following formula (F1). r>R (F1) When the condition expressed by the formula (F1) is satisfied, the heat generation of the electrode 4 can be reduced. The value of R / r is preferably 0.0001 or more, and more preferably 0.0005 or more. The value of R / r is preferably 0.3 or less, and more preferably 0.0.15 or less. When wiring sheet 100 is used as a heating element, pseudo sheet structure 2 needs to have a certain degree of resistance in order to generate heat, while electrodes 4 preferably allow a current to flow as easily as possible. The resistance value R in the axial direction of the electrode 4 and the overall resistance value r in the axial direction of the conductive linear body 21 can be measured using a tester. First, the resistance value R in the axial direction of the electrode 4 and the resistance value (per one) of the conductive linear body 21 in the axial direction are measured. Since the resistance value in the axial direction of the conductive linear body 21 is inversely proportional to the cross-sectional area of the conductive linear body 21, the overall resistance value r in the axial direction of the conductive linear body 21 is calculated by dividing the resistance value (per one) of the conductive linear body 21 in the axial direction by the number of conductive linear bodies 21.
[0057] (Method of manufacturing wiring sheet) Next, a method for manufacturing the wiring sheet according to this embodiment will be described. The method for manufacturing an interconnect sheet according to this embodiment can produce the interconnect sheet 100 according to this embodiment described above. The method for manufacturing an interconnect sheet is not particularly limited. In one aspect of the method for producing the wiring sheet according to the present embodiment, a conductive sheet having a Young's modulus of 1×10 is placed on pseudo sheet structure 2 so as to be in direct contact with conductive linear body 21. 9 Pa super 100×10 9 The method includes a step of forming a pair of electrodes 4 made of a conductor having a resistivity of not more than Pa (electrode formation step). The method for manufacturing a wiring sheet according to this embodiment may further include a step of forming pseudo sheet structure 2 (pseudo sheet structure forming step). By carrying out the pseudo sheet structure forming step and the electrode forming step in this order, wiring sheet 100 can be produced.
[0058] In the pseudo sheet structure forming process, first, as shown in FIG. 3A, an adhesive for forming the resin layer 3 is applied on the release film 5 to form a coating film. Next, the coating film is dried to form the resin layer 3. Next, the conductive linear bodies 21 are arranged on the resin layer 3 to form the pseudo sheet structure 2. For example, in a state where the resin layer 3 with the release film 5 is arranged on the outer circumferential surface of a drum member, the conductive linear bodies 21 are wound spirally on the resin layer 3 while rotating the drum member. Then, the bundle of the conductive linear bodies 21 wound spirally is cut along the axial direction of the drum member. This forms the pseudo sheet structure 2 and places it on the resin layer 3. Then, the resin layer 3 with the release film 5 on which the pseudo sheet structure 2 is formed is taken out of the drum member, and another release film 5' is attached to the pseudo sheet structure 2, thereby obtaining a laminate having the pseudo sheet structure 2 as shown in FIG. 3A. According to this method, for example, it is easy to adjust the spacing L between adjacent conductive linear bodies 21 in the pseudo sheet structure 2 by moving the payout portion of the conductive linear body 21 along a direction parallel to the axis of the drum member while rotating the drum member. The release film 5 is not particularly limited, and may be any film having releasability. The release film 5 may be, for example, a release sheet including a release substrate and a release agent layer formed by applying a release agent onto the release substrate. The release agent layer provided on the release substrate may be provided on only one side of the release substrate, or may be provided on both sides of the release substrate. Examples of the release substrate include a paper substrate, a laminated paper obtained by laminating a thermoplastic resin onto a substrate such as paper or nonwoven fabric, and a thermoplastic resin film. Examples of the release agent include an olefin resin, a rubber elastomer, a long-chain alkyl resin, an alkyd resin, a fluorine resin, and a silicone resin.
[0059] In the electrode formation step, first, one release film 5' is peeled off from the laminate as shown in Fig. 3A. Then, strip-shaped conductive paste is applied to both ends of the substrate 1 and cured to form two electrodes 4, and the substrate 1 with the electrodes 4 is produced as shown in Fig. 3B. Next, as shown in Figure 3C, the laminate from which one release film 5 has been peeled off is bonded to a substrate 1 with an electrode 4 so that a pair of electrodes 4 are positioned at both ends of the conductive linear body 21 in the pseudo sheet structure 2, and then the other release film 5 is peeled off. In this manner, wiring sheet 100 as shown in FIG. 3D can be produced.
[0060] (Effects of the embodiment) According to this embodiment, the following advantageous effects can be obtained. (1) According to this embodiment, the Young's modulus of the electrode 4 is 1×10 9 Pa super 100×10 9 Since the pressure is less than or equal to 1 Pa, the contact resistance between the conductive linear body 21 and the electrode 4 can be reduced.
[0061] [Modifications of the embodiment] The present invention is not limited to the above-described embodiment, and includes modifications and improvements within the scope of the present invention that can achieve the object of the present invention. For example, in the above-described embodiment, interconnect sheet 100 includes substrate 1, but is not limited to this. For example, interconnect sheet 100 does not have to include substrate 1. In such a case, interconnect sheet 100 can be used by being attached to an adherend by resin layer 3. EXAMPLES
[0062] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0063] [Preparation Example 1] A curable adhesive was obtained by blending 100 parts by mass of a phenoxy resin (manufactured by Mitsubishi Chemical Corporation, product name "YX7200B35") with 170 parts by mass of a polyfunctional hydrogenated bisphenol A diglycidyl ether epoxy compound (manufactured by Mitsubishi Chemical Corporation, product name "YX8000"), 0.2 parts by mass of a silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-4803"), 2 parts by mass of a thermal cationic polymerization initiator (manufactured by Sanshin Chemical Industry Co., Ltd., product name "SAN-AID SI-B3"), and 2 parts by mass of a thermal cationic polymerization initiator (manufactured by Sanshin Chemical Industry Co., Ltd., product name "SAN-AID SI-B7").
[0064] [Example 1] (Preparation of pseudo-sheet structure) The adhesive obtained in Preparation Example 1 was applied to a 38 μm thick release film (manufactured by Lintec Corporation, product name "SP-PET382150") and dried to form a resin layer with a thickness of 15 μm after drying. The resin layer was then cut into a rectangle of 250 mm x 320 mm to produce an adhesive sheet. A gold-plated tungsten wire (diameter 10 μm, manufactured by Tokusai Corporation, product name "Au(0.1)-TWG", hereinafter referred to as "wire") was prepared as the conductive linear body. Next, the adhesive sheet was wound around a drum member whose outer periphery was made of rubber, with the surface of the pressure-sensitive adhesive layer facing outward, without any wrinkles, and both ends of the adhesive sheet in the circumferential direction were fixed with double-sided tape. The wire wound around the bobbin was attached to the surface of the pressure-sensitive adhesive layer of the adhesive sheet located near the end of the drum member, and the wire was wound around the drum member while being unwound, and the drum member was moved little by little in a direction parallel to the drum axis so that the wire was wound around the drum member while drawing a spiral at equal intervals of 3 mm. As a result, a pseudo-sheet structure was formed with 80 wires lined up on the surface of the adhesive layer. The wire was then cut, and the pseudo-sheet structure was removed from the drum member. The pseudo-sheet structure was cut into a rectangle of 40 mm x 82 mm so that 12 wires were taken out, and a laminate formed with a pseudo-sheet structure was produced.
[0065] (Preparation of substrate with electrodes) A glass plate (thickness 2 mm) was used as the substrate, and silver paste (manufactured by Jujo Chemical Co., Ltd., product name "#2 TF silver paste") was applied at an electrode distance of 2 mm. 78mm After screen printing so that the thickness was 17 μm, it was dried at 150°C for 30 minutes to form two strip-shaped electrodes with a thickness of 17 μm (resistance value: 0.74 Ω). After that, a nickel layer (thickness: 1 μm) and a gold layer (thickness: 50 nm) were laminated in that order on the silver paste by electroless plating to produce a substrate with electrodes (resistance value: 0.56 Ω).
[0066] (Creating wiring sheets) The laminate was attached to the electrode-attached substrate so that the two electrodes were located at both ends of the conductive linear body of the pseudo-sheet structure, and the release film was peeled off.Then, the laminate was heated and pressed at 120°C, 0.5 MPa, and for 30 minutes to obtain a wiring sheet.
[0067] [Example 2] A wiring sheet was obtained in the same manner as in Example 1, except that in producing a substrate with electrodes, electroless plating was not performed on the strip electrodes.
[0068] [Comparative Example 1] (Preparation of substrate with electrodes) A copper foil (thickness: 18 μm, manufactured by JX Metals Corporation, product name "BHY-82F-HA") with a 15 μm coating of the adhesive obtained in Preparation Example 1 was attached to a glass plate as a substrate so that the width was 2 mm and the distance between the electrodes was 70 mm. The adhesive obtained in Preparation Example 1 was then cured at 120°C for 30 minutes to form two electrodes (resistance value: 0.04 Ω) to produce a substrate with electrodes. (Creating wiring sheets) The adhesive obtained in Preparation Example 1 was applied to a 38 μm thick release film (manufactured by Lintec Corporation, product name "SP-382150") and dried to form a resin layer with a thickness of 15 μm after drying. The resin layer was then cut into a rectangle of 250 mm x 320 mm to produce an adhesive sheet. A gold-plated tungsten wire (diameter 12 μm, manufactured by Tokusai Corporation, product name "Au(0.1)-TWG", hereinafter referred to as "wire") was prepared as the conductive linear body. Next, the adhesive sheet was wound around a drum member whose outer periphery was made of rubber, with the surface of the pressure-sensitive adhesive layer facing outward, without any wrinkles, and both ends of the adhesive sheet in the circumferential direction were fixed with double-sided tape. The wire wound around the bobbin was attached to the surface of the pressure-sensitive adhesive layer of the adhesive sheet located near the end of the drum member, and the wire was wound around the drum member while being unwound, and the drum member was moved little by little in a direction parallel to the drum axis so that the wire was wound around the drum member while drawing a spiral at equal intervals of 4 mm. As a result, a pseudo-sheet structure was formed with 60 wires arranged on the surface of the adhesive layer. The wire was then cut, and the pseudo-sheet structure was removed from the drum member. The pseudo-sheet structure was cut into a rectangle of 36 mm x 74 mm so that 8 wires were taken out, and a laminate formed with a pseudo-sheet structure was produced.
[0069] [Resistance value evaluation] An ohmmeter was connected to the electrodes of the wiring sheet to measure the resistance value (actual value) of the wiring sheet.Then, the difference rate (unit: %) between the actual resistance value and the calculated resistance value was calculated using the following formula.The results are shown in Table 1. Difference rate between actual value and calculated value = [(actual value - calculated value) / calculated value] x 100 (%) Here, the calculated resistance value is a resistance value calculated from the resistance value and number of the conductive linear bodies and the resistance value of the electrodes. The specific calculation method is shown below. [Example 1] Based on the wire resistance (per wire): 59.2 Ω, number of wires: 12, and electrode resistance: 0.56 Ω, the result was calculated as (59.2 / 12) Ω + 0.56 Ω, giving approximately 5.49 Ω. [Example 2] Based on the wire resistance (per wire): 59.2 Ω, number of wires: 12, and electrode resistance: 0.74 Ω, the result was calculated as (59.2 / 12) Ω + 0.74 Ω, giving a value of approximately 5.67 Ω. [Comparative Example 1] Based on the wire resistance (per wire): 36.9 Ω, number of wires: 8, and electrode resistance: 0.04 Ω, the result was calculated as (36.9 / 8) Ω + 0.04 Ω, giving approximately 4.65 Ω. The rate of difference between the measured value and the calculated value is caused by the contact resistance between the electrode and the conductive linear body, so a small rate of difference between the measured value and the calculated value means that the contact resistance is small.
[0070] [Elasticity measurement] The Young's modulus of the electrode was measured by a continuous stiffness measurement method. Specifically, the Young's modulus of the electrode provided on the glass substrate was measured at 25° C. under the following conditions using a nanoindenter (manufactured by MTS Systems). The obtained results are shown in Table 1. Indenter shape: triangular pyramid Maximum indentation depth: 500 nm Vibration frequency: 75Hz
[0071] [Calculation of R / r value] The specific calculation method for R / r is shown below. [Example 1] The wire resistance (per wire): 59.2 Ω, number of wires: 12, electrode resistance: 0.56 Ω, calculated as 0.56 Ω / (59.2 / 12) Ω to be approximately 0.1135. [Example 2] The wire resistance (per wire): 59.2 Ω, number of wires: 12, electrode resistance: 0.74 Ω, so the result was 0.74 Ω / (59.2 / 12) Ω, giving a value of 0.1500. [Comparative Example 1] The wire resistance (per wire): 36.9 Ω, number of wires: 8, electrode resistance: 0.04 Ω, calculated as 0.04 Ω / (36.9 / 8) Ω, resulting in approximately 0.0087.
[0072] [Table 1]
[0073] From the results shown in Table 1, the Young's modulus of the electrode is 1×10 9 Pa super 100×109 It was found that when the Young's modulus of the electrode was less than 1 Pa (Examples 1 and 2), the difference rate between the measured value and the calculated value was smaller than when the Young's modulus of the electrode was too high (Comparative Example 1). This confirmed that the present invention can reduce the contact resistance between the conductive linear body and the electrode. In addition, when comparing Example 1 and Example 2, it was found that Example 1, in which the Young's modulus of the electrode was relatively high and the electrode was gold-plated, had a smaller discrepancy rate between the actual measured value and the calculated value. [Explanation of symbols]
[0074] Reference Signs List 1: substrate, 2: pseudo sheet structure, 21: conductive linear body, 3: resin layer, 4: electrode, 5,5': release film, 100: wiring sheet.
Claims
1. A wiring sheet comprising a pseudo sheet structure in which a plurality of conductive linear bodies are arranged at intervals, and a pair of electrodes in direct contact with the conductive linear bodies, the conductive linear body is a wire containing one or more metals selected from tungsten, molybdenum, and alloys containing these metals; The cross-sectional shape of the conductive linear body is polygonal, flat, elliptical, or circular, The Young's modulus of the electrode is 1×10 9 Pa super 62.6×10 9 Pa or less, Wiring sheet.
2. The wiring sheet according to claim 1 , A relationship between a resistance value R in the axial direction of the electrode and a total resistance value r in the axial direction of the conductive linear body satisfies the condition represented by the following formula (F1): Wiring sheet. r>R...(F1)
3. The wiring sheet according to claim 1 or 2, The thickness of the electrode is 40 μm or less. Wiring sheet.
4. The wiring sheet according to claim 1 , The electrodes are gold plated. Wiring sheet.
5. The wiring sheet according to claim 1 , The electrode has a Young's modulus of 1×10 9 Pa super 62.6×10 9 The conductor is made of only conductors having a viscosity of 0.1 Pa or less. Wiring sheet.
6. The wiring sheet according to claim 1 , A resin layer is provided to support the pseudo sheet structure. Wiring sheet.
7. The wiring sheet according to claim 1 , A substrate is provided to support the pseudo sheet structure. Wiring sheet.
8. A method for producing the wiring sheet according to any one of claims 1 to 7, comprising the steps of: A conductive sheet having a Young's modulus of 1×10 is placed on the pseudo sheet structure so as to be in direct contact with the conductive linear body. 9 Pa super 62.6×10 9 forming a pair of electrodes made of a conductor having a viscosity of 0.01 Pa or less; A method for manufacturing a wiring sheet.
Citation Information
Patent Citations
Electric device, piezoelectric motor, robot, hand and feed pump
JP2017092326A
Manufacturing method of sheet-like conductive member, and sheet-like conductive member
JP2020119856A
Sheet, heating element, and heating device
WO2017086395A1
Wiring sheet
WO2021261465A1