Composition for forming adhesive layer, and manufacturing method and processing method for laminate
The use of an alkali-soluble resin with a specific lowest excited triplet state in the adhesive layer composition addresses the lack of laser processability in existing laminates, enabling effective separation of supports and adherends with minimal residue.
Patent Information
- Application Number
- JP2020174012
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-15
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2040-10-15
AI Technical Summary
Existing adhesive layers in laminates do not exhibit sufficient laser processability, making it difficult to efficiently separate supports and adherends.
An adhesive layer-forming composition containing an alkali-soluble resin with unsaturated groups, specifically designed to have a calculated lowest excited triplet state (T1) of 2.90 eV or less, allowing for effective separation of supports and adherends upon light irradiation.
The composition enables efficient separation of supports and adherends with minimal residue formation and high laser processability, facilitating the handling of thin flexible displays and semiconductor chips.
Smart Images

Figure 0007560991000001 
Figure 0007560991000002 
Figure 0007560991000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition for forming an adhesive layer, and a method for producing and treating a laminate. [Background technology]
[0002] In recent years, as digital devices and other devices have become more functional, the flexible displays and semiconductor chips they are equipped with have become thinner. However, as these devices have become thinner, their strength has decreased, making it difficult to transport them using conventional automatic transport methods.
[0003] Thus, methods have been considered for easily transporting thin flexible displays, semiconductor chips, etc. For example, in this method, a laminate having an adherend such as a semiconductor wafer fixed on a support such as a glass substrate via an adhesive layer is irradiated with light from the support side toward the adhesive layer, thereby altering or decomposing the adhesive layer and reducing the adhesive force, thereby separating the support and the adherend.
[0004] For example, Patent Document 1 describes a method for manufacturing an electronic device, which includes a step of disposing an element on a substrate on which a resin layer is formed, and a step of separating the element disposed on the substrate from the substrate by irradiating the resin layer with a laser and disposing the element on another substrate. According to Patent Document 1, by using a resin for the resin layer whose difference between the glass transition temperature and the thermal decomposition temperature is 150° C. or less, softening of the resin during laser ablation can be suppressed, and therefore, when the element is separated from the substrate, the generation of debris from the softened portion can be reduced.
[0005] Patent Document 2 describes a method for treating an object, which includes the steps of forming a laminate having a support, a temporary fixing material (a separation layer and an adhesive layer), and an object to be treated, processing the object and moving the laminate, irradiating the separation layer with light, and separating the support and the object. According to Patent Document 2, the separation layer absorbs light and decomposes or changes in quality, thereby separating the support and the object.
[0006] Patent Document 3 describes a method for separating the support from the supported substrate by irradiating the separation layer with light to alter the polymer contained in the separation layer in a laminate having a support, a supported substrate, an adhesive layer disposed on the surface of the supported substrate that is supported by the support, and a separation layer disposed between the support substrate and the supported substrate. Patent Document 3 states that the separation layer is altered and loses its adhesiveness when irradiated with light, so that the support substrate and the supported substrate can be easily separated. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2016 / 158264 [Patent Document 2] International Publication No. 2017 / 056662 [Patent Document 3] Patent No. 5580800 Summary of the Invention [Problem to be solved by the invention]
[0008] However, according to the findings of the present inventors, the laminates described in Patent Documents 1 to 3 were unable to provide the desired laser processability.
[0009] The present invention has been made in consideration of these points, and aims to provide a composition for forming an adhesive layer that has excellent laser processability, and a manufacturing method and processing method for a laminate having an adhesive layer containing the composition for forming an adhesive layer. [Means for solving the problem]
[0010] The present inventors conducted research to solve the problems associated with the adhesive layer used in forming the above-mentioned laminate, and discovered that a composition for forming an adhesive layer containing an unsaturated group-containing alkali-soluble resin is suitable as an adhesive layer, thereby completing the present invention.
[0011] The adhesive layer-forming composition of the present invention is a composition for forming an adhesive layer that enables a support and an adherend to be separated from a laminate having an adhesive layer between a light-transmitting support and an adherend by irradiating light from the support side, and the adhesive layer-forming composition contains (A) an unsaturated group-containing alkali-soluble resin as an essential component, and the energy value of the lowest excited triplet state (T1) of the (A) unsaturated group-containing alkali-soluble resin calculated by quantum chemical calculation is 2.90 eV or less.
[0012] The method for producing a laminate according to the present invention includes the steps of forming an adhesive layer on the surface of either or both of a support and an adherend using the above-mentioned adhesive layer-forming composition, and adhering the support and the adherend via the formed adhesive layer.
[0013] The method for processing a laminate according to the present invention comprises the steps of preparing a laminate having a support, an adhesive layer, and an adherend, and irradiating light to separate the support and the adherend, wherein the support transmits light having a wavelength of 10 nm or more and 400 nm or less, and the laminate is capable of being separated into the support and the adherend by irradiating the adhesive layer with light. Effect of the Invention
[0014] According to the present invention, it is possible to provide a composition for forming an adhesive layer that has excellent laser processability, and a method for producing and treating a laminate having an adhesive layer that contains the composition for forming an adhesive layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited to the following embodiment. In addition, in the present invention, when the first decimal place of the content of each component is 0, the notation after the decimal point may be omitted.
[0016] 1. Composition for forming adhesive layer The adhesive layer-forming composition according to one embodiment of the present invention contains (A) an unsaturated group-containing alkali-soluble resin as an essential component.
[0017] [Component (A)] The unsaturated group-containing alkali-soluble resin, which is the component (A), preferably has a polymerizable unsaturated group and an acidic group for exhibiting alkali solubility in one molecule, and more preferably has both a polymerizable unsaturated group and a carboxy group. The above resins can be widely used without any particular limitations. In the present invention, the component (A) is preferably an unsaturated group-containing alkali-soluble resin represented by the following general formula (1).
[0018] [ka]
[0019] In formula (1), Ar are each independently an aromatic hydrocarbon group having 6 to 14 carbon atoms, and a portion of the bonded hydrogen atoms may be substituted with a substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an aryl group or arylalkyl group having 6 to 10 carbon atoms, a cycloalkyl group or cycloalkylalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, and a halogen group. R1 are each independently an alkylene group having 2 to 4 carbon atoms, and 1 are each independently a number from 0 to 3. G are each independently a (meth)acryloyl group or a substituent represented by the following general formula (2) or the following general formula (3), and Y is a tetravalent carboxylic acid residue. Z are each independently a hydrogen atom or a substituent represented by the following general formula (4), and at least one of them is a substituent represented by the following general formula (4). n is a number having an average value of 1 to 20.
[0020] [ka]
[0021] [ka]
[0022] In formulas (2) and (3), R2 is a hydrogen atom or a methyl group, R3 is a divalent alkylene group or alkylarylene group having 2 to 10 carbon atoms, R4 is a divalent saturated or unsaturated hydrocarbon group having 2 to 20 carbon atoms, and p is a number from 0 to 10.
[0023] [ka]
[0024] In formula (4), W is a divalent or trivalent carboxylic acid residue, and m is the number 1 or 2.
[0025] In addition, Y in the above general formula (1) preferably contains at least one aromatic hydrocarbon group. Examples of aromatic hydrocarbon groups include a phenyl group, a biphenyl group, a benzophenone group, a naphthalene group, and a biphenyl ether group. Among the aromatic hydrocarbon groups, a biphenyl group, a benzophenone group, or a naphthalene group is preferable. When Y is an aromatic hydrocarbon group, the LUMO (lowest unoccupied molecular orbital) value of the resin (structural unit) becomes small. This reduces the HOMO (highest occupied molecular orbital)-LUMO energy gap, and the value of the lowest excited triplet state (T1) also becomes small.
[0026] Next, a method for producing the unsaturated group-containing alkali-soluble resin (A) represented by the above general formula (1) will be described in detail.
[0027] First, an epoxy compound (a-1) having a bisarylfluorene skeleton represented by the following general formula (5) (hereinafter simply referred to as "epoxy compound (a-1)"), which may have several oxyalkylene groups in one molecule, is reacted with either or both of (meth)acrylic acid and a (meth)acrylic acid derivative represented by the following general formula (6) or the following general formula (7) to obtain a diol compound which is an epoxy (meth)acrylate. The bisarylfluorene skeleton is preferably a bisnaphtholfluorene skeleton or a bisphenolfluorene skeleton.
[0028] [ka]
[0029] In formula (5), Ar are each independently an aromatic hydrocarbon group having 6 to 14 carbon atoms, and a portion of the bonded hydrogen atoms may be substituted with an alkyl group having 1 to 10 carbon atoms, an aryl group or arylalkyl group having 6 to 10 carbon atoms, a cycloalkyl group or cycloalkylalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or a halogen group. R1 are each independently an alkylene group having 2 to 4 carbon atoms, and 1 are each independently a number from 0 to 3.
[0030] [ka]
[0031] [ka]
[0032] In formulas (6) and (7), R2 is a hydrogen atom or a methyl group, R3 is a divalent alkylene group or alkylarylene group having 2 to 10 carbon atoms, R4 is a divalent saturated or unsaturated hydrocarbon group having 2 to 20 carbon atoms, and p is a number from 0 to 10.
[0033] The reaction of the epoxy compound (a-1) with the (meth)acrylic acid or (meth)acrylic acid derivative can be carried out by a known method. For example, JP-A-4-355450 describes that a diol compound containing a polymerizable unsaturated group can be obtained by using about 2 moles of (meth)acrylic acid per mole of an epoxy compound having two epoxy groups. In the present invention, the compound obtained by the reaction is a diol (d) containing a polymerizable unsaturated group represented by formula (8) (hereinafter, also simply referred to as "diol (d) represented by general formula (8)").
[0034] [ka]
[0035] (In formula (8), each Ar is independently an aromatic hydrocarbon group having 6 to 14 carbon atoms, and a portion of the bonded hydrogen atoms may be substituted with an alkyl group having 1 to 10 carbon atoms, an aryl group or arylalkyl group having 6 to 10 carbon atoms, a cycloalkyl group or cycloalkylalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or a halogen group. Each G is independently a (meth)acryloyl group, or a substituent represented by the following general formula (2) or general formula (3), each R1 is independently an alkylene group having 2 to 4 carbon atoms, and each 1 is independently a number from 0 to 3.)
[0036] [ka]
[0037] [ka]
[0038] In formulas (2) and (3), R2 is a hydrogen atom or a methyl group, R3 is a divalent alkylene group or alkylarylene group having 2 to 10 carbon atoms, R4 is a divalent saturated or unsaturated hydrocarbon group having 2 to 20 carbon atoms, and p is a number from 0 to 10.
[0039] In the synthesis of the diol (d) represented by the general formula (8) and the subsequent production of the unsaturated group-containing alkali-soluble resin represented by the general formula (1) by reacting it with a polyvalent carboxylic acid or anhydride thereof, the reaction is usually carried out in a solvent using a catalyst as necessary.
[0040] Examples of the solvent include cellosolve-based solvents such as ethyl cellosolve acetate and butyl cellosolve acetate, high-boiling ether or ester-based solvents such as diglyme, ethyl carbitol acetate, butyl carbitol acetate, and propylene glycol monomethyl ether acetate, and ketone-based solvents such as cyclohexanone and diisobutyl ketone. There are no particular limitations on the reaction conditions such as the solvent and catalyst used, but it is preferable to use, for example, a solvent that does not have a hydroxyl group and has a boiling point higher than the reaction temperature as the reaction solvent.
[0041] In addition, it is preferable to use a catalyst in the reaction between an epoxy group and a carboxy group or a hydroxyl group. JP-A-9-325494 describes ammonium salts such as tetraethylammonium bromide and triethylbenzylammonium chloride, and phosphines such as triphenylphosphine and tris(2,6-dimethoxyphenyl)phosphine.
[0042] Next, a diol (d) represented by general formula (8) obtained by the reaction of the epoxy compound (a-1) with the (meth)acrylic acid derivative is reacted with a dicarboxylic acid or tricarboxylic acid or its acid anhydride (b) and a tetracarboxylic acid or its acid dianhydride (c) to obtain an alkali-soluble resin having a carboxy group and a polymerizable unsaturated group in one molecule represented by the following general formula (1).
[0043] [ka]
[0044] In formula (1), Ar are each independently an aromatic hydrocarbon group having 6 to 14 carbon atoms, and a portion of the bonded hydrogen atoms may be substituted with an alkyl group having 1 to 10 carbon atoms, an aryl group or arylalkyl group having 6 to 10 carbon atoms, a cycloalkyl group or cycloalkylalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or a halogen group. R1 are each independently an alkylene group having 2 to 4 carbon atoms, and 1 are each independently a number from 0 to 3. G are each independently a (meth)acryloyl group or a substituent represented by the following general formula (2) or the following general formula (3), and Y is a tetravalent carboxylic acid residue. Z are each independently a hydrogen atom or a substituent represented by the following general formula (4), and at least one of them is a substituent represented by the following general formula (4). n is a number having an average value of 1 to 20.
[0045] [ka]
[0046] [ka]
[0047] (In formulas (2) and (3), R2 is a hydrogen atom or a methyl group, R3 is a divalent alkylene group or alkylarylene group having 2 to 10 carbon atoms, R4 is a divalent saturated or unsaturated hydrocarbon group having 2 to 20 carbon atoms, and p is a number from 0 to 10.)
[0048] [ka]
[0049] In formula (4), W is a divalent or trivalent carboxylic acid residue, and m is 1 or 2.
[0050] The acid component used to synthesize the unsaturated group-containing alkali-soluble resin represented by general formula (1) is a polyvalent acid component capable of reacting with the hydroxyl group in the diol (d) molecule represented by general formula (8), and it is necessary to use a dicarboxylic acid or tricarboxylic acid or an acid monoanhydride thereof (b) in combination with a tetracarboxylic acid or an acid dianhydride thereof (c). The carboxylic acid residue of the acid component may be either a saturated or unsaturated hydrocarbon group. In addition, these carboxylic acid residues may contain bonds containing heteroatoms such as -O-, -S-, and carbonyl groups.
[0051] Examples of the dicarboxylic acid or tricarboxylic acid or the acid monoanhydride thereof (b) include chain hydrocarbon dicarboxylic acid or tricarboxylic acid, alicyclic hydrocarbon dicarboxylic acid or tricarboxylic acid, aromatic hydrocarbon dicarboxylic acid or tricarboxylic acid, or the acid monoanhydride thereof, and the like.
[0052] Examples of the acid monoanhydrides of the above-mentioned chain hydrocarbon dicarboxylic acids or tricarboxylic acids include acid monoanhydrides of succinic acid, acetylsuccinic acid, maleic acid, adipic acid, itaconic acid, azelaic acid, citramalic acid, malonic acid, glutaric acid, citric acid, tartaric acid, oxoglutaric acid, pimelic acid, sebacic acid, suberic acid, diglycolic acid, and the like, and acid monoanhydrides of dicarboxylic acids or tricarboxylic acids into which any substituent has been introduced.
[0053] Examples of the acid monoanhydrides of the alicyclic hydrocarbon dicarboxylic acid or tricarboxylic acid include acid monoanhydrides of cyclobutanedicarboxylic acid, cyclopentanedicarboxylic acid, hexahydrophthalic acid, tetrahydrophthalic acid, norbornanedicarboxylic acid, and acid monoanhydrides of dicarboxylic acids or tricarboxylic acids having any substituent introduced therein.
[0054] Examples of the acid monoanhydrides of the aromatic hydrocarbon dicarboxylic acids or tricarboxylic acids include acid monoanhydrides of phthalic acid, isophthalic acid, trimellitic acid, 1,8-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, and the like, and acid monoanhydrides of dicarboxylic acids or tricarboxylic acids into which any substituent has been introduced.
[0055] Among the above dicarboxylic acid or tricarboxylic acid monoanhydrides, succinic acid, itaconic acid, tetrahydrophthalic acid, hexahydrotrimellitic acid, phthalic acid, trimellitic acid, 1,8-naphthalenedicarboxylic acid, and 2,3-naphthalenedicarboxylic acid are preferred, and tetrahydrophthalic acid, 1,8-naphthalenedicarboxylic acid, and 2,3-naphthalenedicarboxylic acid are more preferred.
[0056] In addition, in the case of dicarboxylic acids or tricarboxylic acids, it is preferable to use their acid monoanhydrides. The above-mentioned acid monoanhydrides of dicarboxylic acids or tricarboxylic acids may be used alone or in combination of two or more kinds.
[0057] Examples of the tetracarboxylic acid or its dianhydride (c) include chain hydrocarbon tetracarboxylic acid, alicyclic hydrocarbon tetracarboxylic acid, aromatic hydrocarbon tetracarboxylic acid, or dianhydrides thereof.
[0058] Examples of the chain hydrocarbon tetracarboxylic acid include butane tetracarboxylic acid, pentane tetracarboxylic acid, hexane tetracarboxylic acid, and chain hydrocarbon tetracarboxylic acids having a substituent such as an alicyclic hydrocarbon group or an unsaturated hydrocarbon group introduced therein.
[0059] Examples of the alicyclic hydrocarbon tetracarboxylic acid include cyclobutane tetracarboxylic acid, cyclopentane tetracarboxylic acid, cyclohexane tetracarboxylic acid, cycloheptane tetracarboxylic acid, norbornane tetracarboxylic acid, and alicyclic tetracarboxylic acids having a substituent such as a chain hydrocarbon group or an unsaturated hydrocarbon group introduced therein.
[0060] Examples of aromatic hydrocarbon tetracarboxylic acids include pyromellitic acid, benzophenone tetracarboxylic acid, biphenyl tetracarboxylic acid, diphenyl ether tetracarboxylic acid, diphenyl sulfone tetracarboxylic acid, naphthalene-1,4,5,8-tetracarboxylic acid, and naphthalene-2,3,6,7-tetracarboxylic acid.
[0061] In addition, bis(trimellitic anhydride) aryl esters can also be used. Bis(trimellitic anhydride) aryl esters are a group of compounds produced, for example, by the method described in International Publication No. 2010 / 074065, and are structurally dianhydrides in which two hydroxyl groups of an aromatic diol (such as naphthalenediol, biphenol, terphenyldiol, etc.) react with the carboxyl groups of two molecules of trimellitic anhydride to form an ester bond. Hereinafter, these compounds will be referred to as bis(trimellitic anhydride) esters of aromatic diols.
[0062] Among the above tetracarboxylic acids or their dianhydrides, biphenyltetracarboxylic acid, benzophenonetetracarboxylic acid, diphenylethertetracarboxylic acid, naphthalene-1,4,5,8-tetracarboxylic acid, and naphthalene-2,3,6,7-tetracarboxylic acid are preferred, and biphenyltetracarboxylic acid, benzophenonetetracarboxylic acid, naphthalene-1,4,5,8-tetracarboxylic acid, and naphthalene-2,3,6,7-tetracarboxylic acid are more preferred. In addition, in the above tetracarboxylic acids or their dianhydrides, it is preferred to use the dianhydrides. Furthermore, bis(trimellitic anhydride) esters of naphthalenediol can also be preferably used. The above tetracarboxylic acids or their dianhydrides, and bis(trimellitic anhydride) esters of aromatic diols may be used alone or in combination of two or more.
[0063] The reaction of the diol (d) represented by the general formula (8) with the acid components (b) and (c) is not particularly limited, and any known method can be used. For example, JP-A-9-325494 describes a method of reacting an epoxy (meth)acrylate with a tetracarboxylic dianhydride at a reaction temperature of 90 to 140° C.
[0064] Here, it is preferable to react the compound so that the terminals of the compound become carboxy groups, and so that the molar ratio of the compound with the epoxy (meth)acrylate (d), dicarboxylic acid or tricarboxylic acid or their monoanhydrides (b), and tetracarboxylic dianhydride (c) is (d):(b):(c)=1.0:0.01-1.0:0.2-1.0.
[0065] For example, when an acid monoanhydride (b) and an acid dianhydride (c) are used, it is preferable to react them so that the molar ratio [(d) / [(b) / 2+(c)]] of the amount of the acid component to the diol (d) containing a polymerizable unsaturated group is 0.5 to 1.0. Here, when the molar ratio is 1.0 or less, the content of the diol containing an unreacted polymerizable unsaturated group is not increased, so the stability over time of the alkali-soluble resin composition can be improved. On the other hand, when the molar ratio exceeds 0.5, the terminal of the alkali-soluble resin represented by the general formula (2) does not become an acid anhydride, so that the content of the unreacted acid dianhydride can be suppressed from increasing, so the stability over time of the alkali-soluble resin composition can be improved. In addition, in order to adjust the acid value and molecular weight of the alkali-soluble resin represented by the general formula (2), the molar ratio of each component (b), (c) and (d) can be arbitrarily changed within the above-mentioned range.
[0066] In the adhesive layer-forming composition of the present invention, the content of the unsaturated group-containing alkali-soluble resin (A) represented by the above general formula (1) is preferably 10% by mass or more and 90% by mass or less, more preferably 30% by mass or more and 80% by mass or less, based on the total mass of the solid content. If the content of the above component (A) is 10% by mass or more based on the total mass of the solid content, it is easy to absorb irradiated light (e.g., ultraviolet light) and change in quality, so that the support and the adherend can be easily separated. If the content is 90% by mass or less, the crosslink density of the adhesive layer after curing is not too high, so that it is easy to be ablated when irradiated with light, and residue is unlikely to be generated.
[0067] The energy of the lowest excited triplet state (T1) of the unsaturated group-containing alkali-soluble resin (A) calculated by quantum chemical calculation is 2.90 eV or less, and preferably 2.0 eV or more and 2.90 eV or less. By using the component (A) whose lowest excited triplet state (T1) is 2.0 eV or more, the activation energy of the decomposition reaction of the resin can be lowered and the decomposition reaction can be promoted. In addition, by using the component (A) whose lowest excited triplet state (T1) is 2.9 eV or less, the decomposition of the resin and the gasification of the decomposition product can be easily promoted by the energy of the laser, and the adhesive layer can be efficiently peeled off by the pressure of the generated gas.
[0068] In the present invention, when the unsaturated group-containing alkali-soluble resin (A) represented by general formula (1) is used, the lowest excited triplet state (T1) energy is 2.9 eV or less when Y represented by general formula (1) contains at least one aromatic hydrocarbon group. In order for Y to contain at least one aromatic hydrocarbon group, it is preferable to use the above-mentioned aromatic hydrocarbon tetracarboxylic acid or its acid dianhydride.
[0069] By using biphenyltetracarboxylic acid, benzophenonetetracarboxylic acid, naphthalene-1,4,5,8-tetracarboxylic acid, naphthalene-2,3,6,7-tetracarboxylic acid, etc. as the aromatic hydrocarbon tetracarboxylic acid or its dianhydride, the Y has a structure containing an aromatic hydrocarbon group. In addition, a resin having an energy of the lowest excited triplet state (T1) of the unsaturated group-containing alkali-soluble resin (A) represented by general formula (1) of 2.9 eV or less can be obtained. In addition, by using a naphthalene compound such as naphthalene-1,4,5,8-tetracarboxylic acid or naphthalene-2,3,6,7-tetracarboxylic acid as the aromatic hydrocarbon tetracarboxylic acid or its dianhydride, a resin having an energy of the lowest excited triplet state (T1) of 2.0 eV or more and 2.9 eV or less can be obtained.
[0070] In addition, a resin having an energy of the lowest excited triplet state (T1) of 2.0 eV or more and 2.9 eV or less can be obtained by using the above-mentioned biphenyl tetracarboxylic acid or benzophenone tetracarboxylic acid as the aromatic hydrocarbon tetracarboxylic acid or its dianhydride, and using a naphthalene compound such as 1,8-naphthalenedicarboxylic acid or 2,3-naphthalenedicarboxylic acid as the monoanhydride of an aromatic dicarboxylic acid or tricarboxylic acid.
[0071] The energy of the lowest excited triplet state (T1) of the unsaturated group-containing alkali-soluble resin (A) represented by general formula (1) calculated by quantum chemical calculation can be calculated, for example, using the "Gaussian16, Revision B.01" software package (Gaussian Inc.). The calculation method is to carry out a ground state structure optimization calculation for the molecular structure (molecular coordinates) of the structural unit of the component (A) (terminals substituted with hydrogen) with a charge of 0 and a multiplicity of 1, using the density functional theory (DFT) with the functional B3LYP and the basis function 6-31G(d) (Gaussian input line "#B3LYP / 6-31G(d)OPT"). Next, in the optimized molecular structure, the charge is set to 0 and the multiplicity is set to 1, and the lowest excited triplet energy (T1) is calculated by the time-dependent density functional method (TDDFT) using the functional B3LYP and the basis function 6-31G(d) (Gaussian input line "#B3LYP / 6-31G(d)td=(50-50,nstates=4)"). In this way, the energy value of the lowest excited triplet state (T1) of the (A) component can be obtained. Note that for the DFT and TDDFT calculations, computational chemistry software with similar functions may be used instead.
[0072] The acid value of the unsaturated group-containing alkali-soluble resin (A) represented by general formula (1) is preferably 50 mgKOH / g or more and 200 mgKOH / g or less, and more preferably 60 mgKOH / g or more and 150 mgKOH / g or less. When the acid value is 50 mgKOH / g or more, residues are less likely to remain during alkaline development, and when the acid value is 200 mgKOH / g or less, the penetration of the alkaline developer is not too fast, so peeling development can be suppressed. The acid value can be determined by titration with a 1 / 10N-KOH aqueous solution using a potentiometric titrator "COM-1600" (manufactured by Hiranuma Sangyo Co., Ltd.).
[0073] In addition, the weight average molecular weight (Mw) of the unsaturated group-containing alkali-soluble resin (A) represented by the general formula (1) is preferably 1000 or more and 100000 or less, more preferably 1500 or more and 30000 or less, and even more preferably 2000 or more and 15000 or less, as measured by gel permeation chromatography (GPC) (HLC-8220GPC, manufactured by Tosoh Corporation) in terms of polystyrene. When the weight average molecular weight (Mw) is 1000 or more, the adhesion between the support and the adherend can be improved. When the weight average molecular weight (Mw) is less than 100000, the solution viscosity of the photosensitive resin composition is easily adjusted to a level suitable for application, and application to the surface of the support or adherend does not take too much time.
[0074] The adhesive layer-forming composition according to one embodiment of the present invention includes (B) a photopolymerizable monomer having at least one ethylenically unsaturated bond, and (C) a photopolymerization initiator and / or (D) a sensitizer. Each component will be described below.
[0075] [(B) Component] (B) Examples of photopolymerizable monomers having at least one or more ethylenically unsaturated bonds include trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, sorbitol penta(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, sorbitol hexa(meth)acrylate, alkylene oxide-modified hexa(meth)acrylate of phosphazene, caprolactone-modified dipentaerythritol hexa(meth)acrylate, and other (meth)acrylic acid esters, dendrimer-type multifunctional acrylates, etc. These photopolymerizable monomers may be used alone or in combination of two or more.
[0076] The content of the (B) component is preferably 5 parts by mass or more and 200 parts by mass or less per 100 parts by mass of the (A) component. When the content of the (B) component is 5 parts by mass or more per 100 parts by mass of the (A) component, the resin contains a sufficient number of photoreactive functional groups, so that a sufficient crosslinked structure can be formed, improving chemical resistance. When the content is 200 parts by mass or less, the crosslink density of the adhesive layer after curing is prevented from becoming excessively high, so that the adhesive layer is easily ablated when irradiated with light, and residue is less likely to be generated.
[0077] [(C) component] Examples of the (C) photopolymerization initiator include biimidazole compounds such as 2-[4-(methylthio)benzoyl]-2-(4-morpholinyl)propane, 2-(o-chlorophenyl)-4,5-phenylbiimidazole, 2-(o-chlorophenyl)-4,5-di(m-methoxyphenyl)biimidazole, 2-(o-fluorophenyl)-4,5-diphenylbiimidazole, 2-(o-methoxyphenyl)-4,5-diphenylbiimidazole, and 2,4,5-triarylbiimidazole; 2-trichloromethyl-5-styryl-1,3,4-oxo-1,3,4-triphenylbiimidazole; halomethyldiazole compounds such as sadiazole, 2-trichloromethyl-5-(p-cyanostyryl)-1,3,4-oxadiazole, and 2-trichloromethyl-5-(p-methoxystyryl)-1,3,4-oxadiazole; 2,4,6-tris(trichloromethyl)-1,3,5-triazine, 2-methyl-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-phenyl-4,6-bis(trichloromethyl)-1,3,5-triazine, and 2-(4-chlorophenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine; Halomethyl-s-triazines such as triazine, 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxynaphthyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxystyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(3,4,5-trimethoxystyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine, and 2-(4-methylthiostyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine. Triazine compounds, 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime), 1-(4-phenylsulfanylphenyl)butane-1,2-dione-2-oxime-O-benzoate, 1-(4-methylsulfanylphenyl)butane-1,2-dione-2-oxime-O-acetate, 1-(4-methylsulfanylphenyl)butan-1-oneoxime-O-acetate and other O-acyloxime compounds, benzyl dimethyl ketal, thioxanthone, 2-chlorothioxanthone, 2,Examples of the photopolymerization initiator include sulfur compounds such as 4-diethylthioxanthone, 2-methylthioxanthone, and 2-isopropylthioxanthone, anthraquinones such as 2-ethylanthraquinone, octamethylanthraquinone, 1,2-benzanthraquinone, and 2,3-diphenylanthraquinone, organic peroxides such as azobisisobutyronitrile, benzoyl peroxide, and cumene peroxide, and thiol compounds such as 2-mercaptobenzimidazole, 2-mercaptobenzoxazole, and 2-mercaptobenzothiazole. These photopolymerization initiators may be used alone or in combination of two or more.
[0078] The content of the (C) component is preferably 0.1 parts by mass or more and 30 parts by mass or less, and more preferably 0.3 parts by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the total amount of the (A) component and the (B) component. When the content of the (C) component is 0.1 parts by mass or more, the photopolymerization speed is moderate, so that the decrease in sensitivity can be suppressed. In addition, when the content is 30 parts by mass or less, the sensitivity is suppressed from increasing excessively, and scorching, peeling residue, etc., which occur when ablation is performed by irradiating light, are unlikely to occur. In addition, when the adhesive layer forming composition is used to form a pattern by photolithography, the (C) component is contained, and when a pattern is not formed or a pattern is formed by a method other than photolithography, the (C) component may not be contained.
[0079] [(D) component] Examples of the (D) photosensitizer include acetophenones such as triethanolamine, triisopropanolamine, benzophenone, 4,4'-bisdimethylaminobenzophenone (Michler's ketone), 4-phenylbenzophenone, 4,4'-dichlorobenzophenone, hydroxybenzophenone, 4,4'-diethylaminobenzophenone, acetophenone, 2,2-diethoxyacetophenone, p-dimethylacetophenone, p-dimethylaminopropiophenone, dichloroacetophenone, trichloroacetophenone, and p-tert-butylacetophenone; benzoin ethers such as benzoin, benzoin methyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; 2-dimethylaminoethylbenzoic acid, 4-dimethylaminobenzoic acid ethyl, and 4-dimethylaminobenzoic acid (n-butoxybenzoic acid); Benzophenones such as 4-dimethylaminobenzoic acid isoamyl, 4-dimethylaminobenzoic acid 2-ethylhexyl, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, 4-benzoyl-4'-methyl-diphenyl sulfide, acrylated benzophenone, 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone, and 3,3'-dimethyl-4-methoxybenzophenone; thioxanthones such as 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 2,4-dichlorothioxanthone; aminobenzophenones such as 4,4'-bisdiethylaminobenzophenone; 10-butyl-2-chloroacridone, 2-ethylanthraquinone, 9,10-phenanthrenequinone, and camphorquinone. These photosensitizers may be used alone or in combination of two or more.
[0080] The content of the (D) component is preferably 0.5 parts by mass or more and 400 parts by mass or less, and more preferably 1 part by mass or more and 300 parts by mass or less, relative to 100 parts by mass of the total amount of the (C) component. If the content of the (D) component is 0.5 parts by mass or more, the sensitivity of the photopolymerization initiator can be improved, and the photopolymerization speed can be increased. Also, if the content is 400 parts by mass or less, excessive promotion of the reaction is suppressed, and scorching, peeling residue, and the like that occur when ablation is performed by irradiating light are less likely to occur.
[0081] [(E) component] The adhesive layer-forming composition of the present invention may also contain an epoxy compound having two or more epoxy groups as the component (E).
[0082] (E) Examples of epoxy compounds having two or more epoxy groups include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol fluorene type epoxy compounds, phenol novolac type epoxy compounds, cresol novolac type epoxy compounds (e.g., EPPN-501H: manufactured by Nippon Kayaku Co., Ltd.), phenol aralkyl type epoxy compounds, phenol novolac compounds containing a naphthalene skeleton (e.g., NC-7000L: manufactured by Nippon Kayaku Co., Ltd.), biphenyl type epoxy compounds (e.g., jERYX4000 (manufactured by Mitsubishi Chemical Corporation), naphthol aralkyl type epoxy compounds, trisphenolmethane type epoxy compounds, tetrakisphenolethane type epoxy compounds, glycidyl ethers of polyhydric alcohols, glycidyl esters of polycarboxylic acids, copolymers of monomers having (meth)acrylic groups containing glycidyl (meth)acrylate as a unit, such as copolymers of methacrylic acid and glycidyl methacrylate, 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate (e.g., celloxide, 2021P: manufactured by Daicel Corporation), butanetetracarboxylic acid tetra(3,4-epoxycyclohexylmethyl) modified ε-caprolactone (e.g., Epolead GT401: manufactured by Daicel Corporation), epoxy compounds having epoxycyclohexyl groups such as HiREM-1 manufactured by Shikoku Kasei Kogyo Co., Ltd., polyfunctional epoxy compounds having a dicyclopentadiene skeleton (e.g., HP7200 series: manufactured by DIC Corporation), 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol (e.g., EHPE3150: manufactured by Daicel Corporation), epoxidized polybutadiene (e.g., NISSO-PB·JP-100: manufactured by Nippon Soda Co., Ltd.), and epoxy compounds having a silicone skeleton.
[0083] (E) Among the epoxy compounds having two or more epoxy groups, bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol fluorene type epoxy compounds, phenol novolac type epoxy compounds, cresol novolac type epoxy compounds, and biphenyl type epoxy compounds are preferred, and biphenyl type epoxy compounds are more preferred. By using a biphenyl type epoxy compound, it is possible to achieve both the light absorption ability required for separation by light irradiation and the patterning property of the photosensitive resin composition during photocuring, and also to increase the degree of freedom in designing the photosensitive resin composition.
[0084] The epoxy equivalent of the epoxy compound of component (E) is preferably 100 g / eq or more and 300 g / eq or less, more preferably 100 g / eq or more and 250 g / eq or less. The number average molecular weight (Mn) of the epoxy compound of component (E) is preferably 100 to 5000. When the epoxy equivalent is 100 g / eq or more and 300 g / eq or less, and the number average molecular weight (Mn) of the epoxy compound is 100 to 5000, a cured film having good solvent resistance can be obtained. When the epoxy equivalent is 300 g / eq or less, sufficient alkali resistance can be maintained even when an alkaline chemical solution is used in a post-process. These compounds may be used alone or in combination of two or more kinds.
[0085] The content of the (E) component is preferably 0 parts by mass or more and 60 parts by mass or less, more preferably 5 parts by mass or more and 50 parts by mass or less, based on the total mass of the solid content. When the content of the (E) component is 5 parts by mass or more based on the total mass of the solid content, a sufficient crosslinked structure can be formed, improving chemical resistance. When the content is 60 parts by mass or less, the crosslink density of the adhesive layer after curing is prevented from becoming excessively high, so that the adhesive layer is easily ablated when irradiated with light, and residue is less likely to be generated. Depending on the combination with the (A) component or the (B) component, the necessary chemical resistance, etc. can be ensured even if the content of the (E) component is 0 parts by mass.
[0086] [Component (F)] The adhesive layer-forming composition according to one embodiment of the present invention may contain a solvent as the component (F).
[0087] Examples of the solvent contained in the (F) adhesive layer-forming composition include alcohols such as methanol, ethanol, n-propanol, isopropanol, ethylene glycol, propylene glycol, 3-methoxy-1-butanol, ethylene glycol monobutyl ether, 3-hydroxy-2-butanone, and diacetone alcohol; terpenes such as α- or β-terpineol; ketones such as acetone, methyl ethyl ketone, cyclohexanone, and N-methyl-2-pyrrolidone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; cellosolve, methyl cellosolve, ethyl cellosolve, carbitol, methyl carbitol, ethyl carbitol, butyl carbitol, diethylene glycol ethyl methyl ether, and propylene glycol monomethyl ether. Examples of the solvent include glycol ethers such as propylene glycol monoethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, triethylene glycol monomethyl ether, and triethylene glycol monoethyl ether, and esters such as ethyl acetate, butyl acetate, ethyl lactate, 3-methoxybutyl acetate, 3-methoxy-3-butyl acetate, 3-methoxy-3-methyl-1-butyl acetate, cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, carbitol acetate, ethyl carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate. By dissolving and mixing using these, a uniform solution-like composition can be obtained. These solvents may be used alone or in combination of two or more to obtain the necessary characteristics such as coatability. The amount of the solvent varies depending on the target viscosity, but is preferably 60 to 90% by mass in the photosensitive resin composition solution.
[0088] The adhesive layer-forming composition according to one embodiment of the present invention may contain additives such as a curing agent, a curing accelerator, a thermal polymerization inhibitor and an antioxidant, a plasticizer, a filler, a leveling agent, an antifoaming agent, a surfactant, and a coupling agent, as necessary.
[0089] Examples of curing agents include amine compounds, polyvalent carboxylic acid compounds, phenolic resins, amino resins, dicyandiamide, Lewis acid complex compounds, etc., which contribute to the curing of epoxy resins. Examples of curing accelerators include tertiary amines, quaternary ammonium salts, tertiary phosphines, quaternary phosphonium salts, boric acid esters, Lewis acids, organometallic compounds, imidazoles, etc., which contribute to the curing acceleration of epoxy resins. Examples of thermal polymerization inhibitors and antioxidants include hydroquinone, hydroquinone monomethyl ether, pyrogallol, tert-butylcatechol, phenothiazine, hindered phenol compounds, etc. Examples of plasticizers include dibutyl phthalate, dioctyl phthalate, tricresyl phosphate, etc. Examples of fillers include glass fiber, silica, mica, alumina, etc. Examples of defoamers and leveling agents include silicone-based, fluorine-based, and acrylic compounds. Examples of surfactants include fluorine-based surfactants, silicone-based surfactants, etc. Examples of coupling agents include 3-(glycidyloxy)propyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-ureidopropyltriethoxysilane, and the like.
[0090] The adhesive layer-forming composition of the present invention can be used by coating it on the required area, and can also be used through a process of forming a required pattern by photolithography.
[0091] 2. Manufacturing method of laminate A method for producing a laminate according to one embodiment of the present invention includes the steps of: (1) forming an adhesive layer containing the above-mentioned adhesive layer-forming composition on the surface of one or both of a support and an adherend; and (2) bonding the support and the adherend via the formed adhesive layer. Each step will be described below.
[0092] [Step of forming adhesive layer] The adhesive layer forming step is a step of forming an adhesive layer containing the above-mentioned adhesive layer forming composition on the surface of either one or both of the support and the adherend.
[0093] (Support) There are no limitations on the type of support, so long as an adhesive layer can be formed on the surface thereof.
[0094] In the present invention, the support is preferably laser transmissive. In particular, the support is more preferably transmissive to light (laser) having a wavelength of 10 nm or more and 400 nm or less, and even more preferably transmissive to light (laser) having a wavelength of 100 nm or more and 400 nm or less. Examples of the support having the laser transmissive property include glass substrates, acrylic substrates, sapphire substrates, and quartz substrates. However, for glass substrates and acrylic substrates, it is necessary to use substrates having a composition that has sufficient transmittance for the wavelength of light to be used. Of the above supports, glass substrates are preferred.
[0095] (adherent) Examples of the adherend include a semiconductor wafer, a semiconductor chip, a light emitting element, an optical glass wafer, a metal foil, a polishing pad, a resin coating film, a wiring layer, and the like.
[0096] (adhesive layer) The adhesive layer is formed by applying an adhesive to the surface of either one or both of the above-mentioned support and the above-mentioned adherend. The above-mentioned adhesive is preferably an adhesive layer forming composition containing the above-mentioned (A) unsaturated group-containing alkali-soluble resin. The above-mentioned unsaturated group-containing alkali-soluble resin has a low crosslink density after curing, and is therefore easily ablated when irradiated with a laser, and therefore has excellent laser processability.
[0097] Examples of the method for applying the adhesive include known methods such as immersion in a solution, spin coating, ink jetting, spraying, and methods using a roller coater, land coater, slit coater or spinner.
[0098] After the adhesive is applied by the above application method, the solvent is dried (prebaked) to form an adhesive layer. Note that prebaking is performed by heating using an oven, a hot plate, etc. The heating temperature and heating time in prebaking are appropriately selected depending on the solvent used, and for example, prebaking is performed at a temperature of 60 to 110°C for 1 to 3 minutes.
[0099] The thickness of the adhesive layer can be selected arbitrarily. In the present invention, the thickness of the adhesive layer is preferably 0.1 μm or more and 50 μm or less, and more preferably 0.5 μm or more and 30 μm or less. When the thickness of the adhesive layer is 0.1 μm or more, the adhesive layer can have sufficient holding power to adhere the adherend. Also, when the thickness is 50 μm or less, the adhesive layer can be sufficiently cured by light or heat curing.
[0100] In addition, this process may include an exposure process and a development process for patterning the adhesive layer after applying the adhesive to the surface of either one or both of the above-mentioned support and the above-mentioned adherend. By patterning the adhesive layer, the adhesive layer can be formed only in the portion where the adherend is to be adhered, and in the process of separating the support and the adherend (described later), peeling failure and positional deviation of the adherend can be suppressed.
[0101] Examples of light used in the exposure step include visible light, ultraviolet light, far ultraviolet light, electron beams, X-rays, and the like. Among the above-mentioned light, ultraviolet light (wavelength 250 to 400 nm) is preferred. In addition, in the development step, a developer suitable for alkaline development is used. Examples of the developer include aqueous solutions of sodium carbonate, potassium carbonate, potassium hydroxide, diethanolamine, tetramethylammonium hydroxide, and the like. These developers can be appropriately selected according to the characteristics of the resin layer, and a surfactant may be added as necessary. The development temperature is preferably 20 to 35°C, and fine images can be precisely formed using a commercially available developing machine, ultrasonic cleaner, or the like. After the alkaline development, the film is usually washed with water. As the development treatment method, a shower development method, a spray development method, a dip (immersion) development method, a puddle (liquid puddle) development method, and the like can be applied.
[0102] [Step of bonding the support and the adherend] The step of adhering the support and the adherend is a step of adhering the support and the adherend via the adhesive layer.
[0103] As a method for bonding the support and the adherend, for example, there is a method of contacting the adherend (wherein the adhesive is applied to the surface that contacts the adhesive layer) with the surface of the adhesive layer formed on the surface of the support and pressurizing the adherend while heating it. In addition, as for the bonding conditions between the support and the adherend, the temperature during pressurization is preferably from room temperature to 200°C, more preferably from 30°C to 150°C. The pressure during bonding is preferably from 0.01 MPa to 20 MPa, more preferably from 0.03 MPa to 15 MPa. In addition, if necessary, after completion of the pressurized thermocompression bonding, the heat curing can be performed at a temperature of 120°C to 250°C. By bonding the support and the adherend under the above conditions, the adherend is more firmly fixed to the surface of the support via the adhesive layer.
[0104] In the bonding step, the support and the adherend may be bonded by photocuring. An example of a method for photocuring the adhesive layer is a method of irradiating light using a high-pressure mercury lamp. The bonding conditions for the support and the adherend are preferably such that the wavelength of the irradiated light is 200 to 500 nm. The exposure dose of the irradiated light is 25 mJ / cm. 2 More than 3000mJ / cm 2 It is preferable that the concentration is less than 50 mJ / cm 2 More than 2000mJ / cm 2 It is more preferable that:
[0105] In this manner, the laminate of the present invention is formed.
[0106] The laminate can be separated from the support by irradiating the adhesive layer from the support side with a laser (described later) having a wavelength of 10 nm or more and 400 nm or less.
[0107] 3. Processing method of laminate A method for treating a laminate according to one embodiment of the present invention includes the steps of (1) preparing the laminate described above, and (2) irradiating the laminate with light to separate the support and the adherend. Each step will be described below.
[0108] [Step of preparing laminate] The step of preparing a laminate is a step of forming a laminate as described above, or of preparing an already formed laminate.
[0109] [Step of separating the support and the adherend] The step of separating the support and the adherend is a step of separating the support and the adherend by irradiating the adhesive layer with light.
[0110] The light to be irradiated is not particularly limited as long as it can separate the support and the adherend. In the present invention, the light is preferably ultraviolet light, and the wavelength of the ultraviolet light is more preferably 10 nm or more and 400 nm or less, and even more preferably 100 nm or more and 400 nm or less. If the wavelength of the ultraviolet light is 10 nm or more, the polymer, which is a component of the adhesive layer, absorbs the light and changes its quality, reducing the strength and adhesive force, so that the support and the adherend can be easily separated. In addition, if the wavelength is 400 nm or less, the adhesive layer in the processed part absorbs light, so that the generation of residue of the cured film can be suppressed.
[0111] Examples of the ultraviolet light source include a low mercury lamp, a high pressure mercury lamp, an extra-high pressure mercury lamp, a metal halide lamp, a far ultraviolet light laser, etc. Among the above light sources, a laser is preferable.
[0112] Examples of the laser include solid-state lasers, liquid lasers, and gas lasers. Examples of the solid-state laser include semiconductor pumped lasers. Examples of the liquid laser include dye lasers. Examples of the gas laser include excimer lasers. Among the lasers, semiconductor pumped lasers are preferred.
[0113] Examples of the semiconductor pumped laser include Nd:YAG laser, Nd:YLF laser, Nd:glass laser, Nd:YVO4 laser, Yb:YAG laser, Yb-doped fiber laser, Er:YAG laser, Tm:YAG laser, etc. Examples of the excimer laser include KrF laser, XeCl laser, ArF laser, F2 laser, etc. Among the above lasers, the Nd:YAG laser is preferred.
[0114] The output and cumulative light quantity of the light irradiated onto the adhesive layer vary depending on the type of light source, etc., but when the irradiated light is a laser, the output can be from 0.1 mW to 200 W. The cumulative light quantity can be 1 mJ / cm2. 2 More than 50J / cm2 It is preferable that the integrated light amount is 0.1 mJ / cm or less. 2 If the intensity is more than 50 J / cm, burning and peeling residue are less likely to occur during ablation. 2 If the ablation speed is equal to or less than this, the ablation speed can be appropriately controlled to perform appropriate processing.
[0115] As a method of irradiating the adhesive layer with light (laser), it is preferable to irradiate the entire surface of the adhesive layer with a laser from the support side. The method of irradiating the laser is not particularly limited, and can be performed by a known method.
[0116] The laminate is capable of separating the support and the adherend by irradiating the adhesive layer with light (laser).
[0117] The method for treating a laminate according to one embodiment of the present invention may include a step of processing the prepared laminate prior to the step of separating the support and the adherend.
[0118] Methods for processing the laminate include thinning of adherends such as dicing and back grinding, photofabrication, stacking of semiconductor chips, mounting of various elements, resin sealing, and the like.
[0119] The method for treating a laminate according to an embodiment of the present invention may further include a step of transferring the processed laminate from one device to another. A method for transferring the laminate includes using a robot arm or the like.
[0120] In this manner, the laminate of the present invention is processed. EXAMPLES
[0121] Hereinafter, the embodiments of the present invention will be described in detail based on examples and comparative examples, but the present invention is not limited to these.
[0122] First, synthesis examples of the unsaturated group-containing alkali-soluble resin, component (A), will be described. Unless otherwise specified, the resins in these synthesis examples were evaluated as follows.
[0123] In addition, when the same model of measuring equipment is used, the name of the equipment manufacturer is omitted from the second place. In addition, in the examples, all glass substrates used to prepare the substrates with cured films for measurement are used after the same treatment. In addition, when the first decimal place of the content of each component is 0, the notation after the decimal point may be omitted.
[0124] [Solid content concentration] 1 g of the resin solution obtained in Synthesis Example was impregnated into a glass filter (weight: W0(g)), weighed [W1(g)], and the weight after heating at 160°C for 2 hours [W2(g)] was calculated from the following formula. Solid content concentration (weight%) = 100 × (W2-W0) / (W1-W0)
[0125] [Acid value] The resin solution was dissolved in dioxane and titrated with a 1 / 10N KOH aqueous solution using a potentiometric titrator "COM-1600" (manufactured by Hiranuma Sangyo Co., Ltd.) to determine the content.
[0126] [Molecular weight] Measurement was performed using gel permeation chromatography (GPC) "HLC-8220GPC" (manufactured by Tosoh Corporation, solvent: tetrahydrofuran, columns: TSKgelSuper H-2000 (2 columns) + TSKgelSuper H-3000 (1 column) + TSKgelSuper H-4000 (1 column) + TSKgelSuper H-5000 (1 column) (manufactured by Tosoh Corporation), temperature: 40°C, rate: 0.6 ml / min), and the weight average molecular weight (Mw) was calculated as a value converted into standard polystyrene (manufactured by Tosoh Corporation, PS-oligomer kit).
[0127] The abbreviations used in the Synthesis Examples are as follows. BPFE: Bisphenol fluorene type epoxy resin (epoxy resin with general formula (1) where Ar is a benzene ring and l is 0, epoxy equivalent 256g / eq) BNFE: Bisnaphtholfluorene type epoxy resin (epoxy resin with general formula (1) where Ar is a naphthalene ring and l is 0, epoxy equivalent 281g / eq) YD-7011R: Bisphenol A type epoxy resin (Epototo YD-7011R, manufactured by Nippon Steel Chemical & Material Co., Ltd., "Epototo" is a registered trademark of the company) YX8000: Hydrogenated epoxy resin ("jER YX8000", epoxy equivalent 205g / eq, manufactured by Mitsubishi Chemical Corporation; "jER" is a registered trademark of the company) BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride BTDA: 3,3',4,4'-benzophenonetetracarboxylic dianhydride HPMDA: 1,2,4,5-cyclohexanetetracarboxylic dianhydride THPA: 1,2,3,6-Tetrahydrophthalic anhydride TPP: Triphenylphosphine AA: Acrylic acid PGMEA: Propylene glycol monomethyl ether acetate
[0128] [Synthesis Example 1] In a 250 mL four-neck flask equipped with a reflux condenser, BPFE (50.00 g, 0.10 mol), AA (14.07 g, 0.20 mol), TPP (0.26 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (25.00 g) was charged and adjusted so that the solid content was 50 mass%.
[0129] Next, BPDA (14.37 g, 0.05 mol) and THPA (7.43 g, 0.05 mol) were added to the obtained reaction product and stirred at 115 to 120 ° C for 6 hours to obtain an unsaturated group-containing alkali-soluble resin (A)-1. The solid content concentration of the obtained resin solution was 57.0 mass%, the acid value (solid content equivalent) was 96 mg KOH / g, and the Mw by GPC analysis was 3600.
[0130] [Synthesis Example 2] In a 250 mL four-neck flask equipped with a reflux condenser, BPFE (50.00 g, 0.10 mol), AA (14.07 g, 0.20 mol), TPP (0.26 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (25.00 g) was charged and adjusted so that the solid content was 50 mass%.
[0131] Next, BTDA (15.73 g, 0.05 mol) and THPA (7.43 g, 0.05 mol) were added to the obtained reaction product and stirred at 115 to 120° C. for 6 hours to obtain an unsaturated group-containing alkali-soluble resin (A)-2. The solid content concentration of the obtained resin solution was 57.4 mass%, the acid value (solid content equivalent) was 105 mg KOH / g, and the Mw by GPC analysis was 3200.
[0132] [Synthesis Example 3] In a 250 mL four-neck flask equipped with a reflux condenser, BPFE (50.00 g, 0.10 mol), AA (14.07 g, 0.20 mol), TPP (0.26 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (25.00 g) was charged and adjusted so that the solid content was 50 mass%.
[0133] Next, naphthalene-1,4,5,8-tetracarboxylic dianhydride (13.09 g, 0.05 mol) and THPA (7.43 g, 0.05 mol) were added to the obtained reaction product and stirred at 115 to 120 ° C for 6 hours to obtain an unsaturated group-containing alkali-soluble resin (A)-3. The solid content concentration of the obtained resin solution was 56.6 mass%, the acid value (solid content equivalent) was 101 mg KOH / g, and the Mw by GPC analysis was 3300.
[0134] [Synthesis Example 4] In a 250 mL four-neck flask equipped with a reflux condenser, BPFE (50.00 g, 0.10 mol), AA (14.07 g, 0.20 mol), TPP (0.26 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (25.00 g) was charged and adjusted so that the solid content was 50 mass%.
[0135] Next, naphthalene-2,3,6,7-tetracarboxylic dianhydride (13.09 g, 0.05 mol) and THPA (7.43 g, 0.05 mol) were added to the obtained reaction product and stirred at 115 to 120 ° C for 6 hours to obtain an unsaturated group-containing alkali-soluble resin (A)-4. The solid content concentration of the obtained resin solution was 56.6 mass%, the acid value (solid content equivalent) was 99 mg KOH / g, and the Mw by GPC analysis was 3400.
[0136] [Synthesis Example 5] In a 250 mL four-neck flask equipped with a reflux condenser, BPFE (50.00 g, 0.10 mol), AA (14.07 g, 0.20 mol), TPP (0.26 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (25.00 g) was charged and adjusted so that the solid content was 50 mass%.
[0137] Next, BPDA (14.37 g, 0.05 mol) and 1,8-naphthalenedicarboxylic anhydride (9.68 g, 0.05 mol) were added to the obtained reaction product, and the mixture was stirred at 115 to 120 ° C for 6 hours to obtain an unsaturated group-containing alkali-soluble resin (A)-5. The solid content concentration of the obtained resin solution was 57.6 mass%, the acid value (solid content equivalent) was 97 mg KOH / g, and the Mw by GPC analysis was 3700.
[0138] [Synthesis Example 6] In a 250 mL four-neck flask equipped with a reflux condenser, BPFE (50.00 g, 0.10 mol), AA (14.07 g, 0.20 mol), TPP (0.26 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (25.00 g) was charged and adjusted so that the solid content was 50 mass%.
[0139] Next, BPDA (14.37 g, 0.05 mol) and 2,3-naphthalenedicarboxylic anhydride (9.68 g, 0.05 mol) were added to the obtained reaction product, and the mixture was stirred at 115 to 120° C. for 6 hours to obtain an unsaturated group-containing alkali-soluble resin (A)-6. The solid content of the obtained resin solution was 57.6 mass%, the acid value (solid content equivalent) was 95 mgKOH / g, and the Mw by GPC analysis was 3600.
[0140] [Synthesis Example 7] In a 250 mL four-neck flask equipped with a reflux condenser, BPFE (50.00 g, 0.10 mol), AA (14.07 g, 0.20 mol), TPP (0.26 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (25.00 g) was charged and adjusted so that the solid content was 50 mass%.
[0141] Next, BPDA (10.06 g, 0.03 mol) and THPA (11.89 g, 0.08 mol) were added to the obtained reaction product and stirred at 115 to 120 ° C for 6 hours to obtain an unsaturated group-containing alkali-soluble resin (A)-7. The solid content concentration of the obtained resin solution was 57.0 mass%, the acid value (solid content equivalent) was 98 mg KOH / g, and Mw by GPC analysis was 2300.
[0142] [Synthesis Example 8] In a 250 mL four-neck flask equipped with a reflux condenser, BPFE (50.00 g, 0.10 mol), AA (14.07 g, 0.20 mol), TPP (0.26 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (25.00 g) was charged and adjusted so that the solid content was 50 mass%.
[0143] Next, BPDA (19.25 g, 0.07 mol) and THPA (0.30 g, 0.002 mol) were added to the obtained reaction product and stirred at 115 to 120 ° C for 6 hours to obtain an unsaturated group-containing alkali-soluble resin (A)-8. The solid content concentration of the obtained resin solution was 56.3 mass%, the acid value (solid content equivalent) was 97 mg KOH / g, and the Mw by GPC analysis was 4700.
[0144] [Synthesis Example 9] In a 250 mL four-neck flask equipped with a reflux condenser, BNFE (50.00 g, 0.09 mol), AA (12.82 g, 0.20 mol), TPP (0.23 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (25.00 g) was charged and adjusted so that the solid content was 50 mass%.
[0145] Next, BPDA (13.09 g, 0.04 mol) and THPA (6.77 g, 0.04 mol) were added to the obtained reaction product and stirred at 115 to 120 ° C for 6 hours to obtain an unsaturated group-containing alkali-soluble resin (A)-9. The solid content concentration of the obtained resin solution was 56.1 mass%, the acid value (solid content equivalent) was 91 mg KOH / g, and the Mw by GPC analysis was 3500.
[0146] [Synthesis Example 10] In a 250 mL four-neck flask equipped with a reflux condenser, BNFE (50.00 g, 0.09 mol), AA (12.82 g, 0.20 mol), TPP (0.23 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (25.00 g) was charged and adjusted so that the solid content was 50 mass%.
[0147] Next, BTDA (14.33 g, 0.04 mol) and THPA (6.77 g, 0.04 mol) were added to the obtained reaction product and stirred at 115 to 120 ° C for 6 hours to obtain an unsaturated group-containing alkali-soluble resin (A)-10. The solid content concentration of the obtained resin solution was 56.5 mass%, the acid value (solid content equivalent) was 90 mg KOH / g, and the Mw by GPC analysis was 2700.
[0148] [Synthesis Example 11] In a 250 mL four-neck flask equipped with a reflux condenser, BPFE (50.00 g, 0.10 mol), AA (14.07 g, 0.20 mol), TPP (0.26 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (25.00 g) was charged and adjusted so that the solid content was 50 mass%.
[0149] Next, HPMDA (10.95 g, 0.05 mol) and THPA (7.43 g, 0.05 mol) were added to the obtained reaction product and stirred at 115 to 120 ° C for 6 hours to obtain an unsaturated group-containing alkali-soluble resin (A)-11. The solid content concentration of the obtained resin solution was 56.0 mass%, the acid value (solid content equivalent) was 105 mg KOH / g, and the Mw by GPC analysis was 4000.
[0150] [Synthesis Example 12] In a 250 mL four-neck flask equipped with a reflux condenser, YD-7011R (50.00 g, 0.05 mol), AA (7.59 g, 0.11 mol), TPP (0.14 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (20.00 g) was charged and adjusted so that the solid content was 50 mass%.
[0151] Next, BPDA (5.42 g, 0.02 mol) and THPA (6.41 g, 0.04 mol) were added to the obtained reaction product and stirred at 115 to 120 ° C for 6 hours to obtain an unsaturated group-containing alkali-soluble resin (A)-12. The solid content concentration of the obtained resin solution was 53.7 mass%, the acid value (solid content equivalent) was 68 mg KOH / g, and the Mw by GPC analysis was 7300.
[0152] [Synthesis Example 13] In a 250 mL four-neck flask equipped with a reflux condenser, 3',4'-epoxycyclohexylmethyl 3',4'-epoxycyclohexanecarboxylate (25.00 g, 0.10 mol), AA (14.28 g, 0.20 mol), TEAB (0.63 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105 ° C for 20 hours to obtain a reaction product. Then, PGMEA (20.00 g) was charged and adjusted so that the solid content was 50 mass %.
[0153] Next, BPDA (10.29 g, 0.03 mol) and THPA (11.97 g, 0.08 mol) were added to the obtained reaction product and stirred at 120 to 125 ° C for 8 hours. Furthermore, GMA (11.60 g, 0.08 mol) was added and stirred at 105 to 110 ° C for 8 hours to obtain an unsaturated group-containing alkali-soluble resin (A)-13. The solid content concentration of the obtained resin solution was 64.8 mass%, the acid value (solid content equivalent) was 55 mg KOH / g, and Mw by GPC analysis was 4200.
[0154] [Synthesis Example 14] In a 250 mL four-neck flask equipped with a reflux condenser, YX8000 (50.00 g, 0.12 mol), AA (17.58 g, 0.24 mol), TPP (0.32 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105 ° C for 20 hours to obtain a reaction product. Then, PGMEA (20.00 g) was charged and adjusted so that the solid content was 50 mass %.
[0155] Next, HPMDA (13.67 g, 0.06 mol) and THPA (9.28 g, 0.06 mol) were added to the obtained reaction product and stirred at 115 to 120 ° C for 6 hours to obtain an unsaturated group-containing alkali-soluble resin (A)-14. The solid content concentration of the obtained resin solution was 58.3 mass%, the acid value (solid content equivalent) was 115 mg KOH / g, and the Mw by GPC analysis was 4000.
[0156] The compositions for forming the adhesive layer of Examples 1 to 12 and Comparative Examples 1 to 4 were prepared in the blend amounts (unit: mass %) shown in Table 1. The blend components used in Table 1 are as follows.
[0157] (Alkali-soluble resin containing unsaturated groups) (A)-1: Resin solution obtained in Synthesis Example 1 (solid content concentration: 57.0% by mass) (A)-2: Resin solution obtained in Synthesis Example 2 (solid content concentration: 57.4% by mass) (A)-3: Resin solution obtained in Synthesis Example 3 (solid content concentration: 56.6% by mass) (A)-4: Resin solution obtained in Synthesis Example 4 (solid content concentration: 56.6% by mass) (A)-5: Resin solution obtained in Synthesis Example 5 (solid content concentration: 57.6% by mass) (A)-6: Resin solution obtained in Synthesis Example 6 (solid content concentration: 57.6% by mass) (A)-7: Resin solution obtained in Synthesis Example 7 (solid content concentration: 57.0% by mass) (A)-8: Resin solution obtained in Synthesis Example 8 (solid content concentration: 56.3% by mass) (A)-9: Resin solution obtained in Synthesis Example 9 (solid content concentration: 56.1% by mass) (A)-10: Resin solution obtained in Synthesis Example 10 (solid content concentration: 56.5% by mass) (A)-11: Resin solution obtained in Synthesis Example 11 (solid content concentration: 56.0% by mass) (A)-12: Resin solution obtained in Synthesis Example 12 (solid content concentration: 53.7% by mass) (A)-13: Resin solution obtained in Synthesis Example 13 (solid content concentration: 64.8% by mass) (A)-14: Resin solution obtained in Synthesis Example 14 (solid content concentration: 58.3% by mass)
[0158] (Photopolymerizable monomer) (B): Mixture of dipentaerythritol pentaacrylate and hexaacrylate (DPHA, manufactured by Nippon Kayaku Co., Ltd.)
[0159] (Photopolymerization initiator) (C): 2-[4-(methylthio)benzoyl]-2-(4-morpholinyl)propane ("Omnirad907" manufactured by IGMResins BV, "Omnirad" is a registered trademark of the company)
[0160] (Photosensitizer) (D): Michler's ketone
[0161] (Epoxy compounds) (E): Biphenyl-type epoxy resin (jER YX4000, manufactured by Mitsubishi Chemical Corporation)
[0162] (solvent) (F): Propylene glycol monomethyl ether acetate (PGMEA)
[0163] [Table 1]
[0164] [evaluation] (A) The energy of the lowest excited triplet state (T1) of the unsaturated group-containing alkali-soluble resin was calculated, and the following evaluations were performed using the cured films obtained by curing the adhesive layer-forming compositions of Examples 1 to 12 and Comparative Examples 1 to 4.
[0165] [Calculation method for the energy of the lowest excited triplet state (T1)] The energy of the lowest excited triplet state (T1) of the unsaturated group-containing alkali-soluble resins ((A)-1 to 11) was calculated by quantum chemical calculation based on the structural unit of the (A) component represented by the following general formula (9). To calculate the energy of the lowest excited triplet state (T1), the "Gaussian16, Revision B.01" software package (Gaussian Inc.) was used. Specifically, the lowest excited triplet energy (T1) was obtained by the following calculation method. First, a ground state structure optimization calculation was performed on the molecular structure (molecular coordinates) of the structural unit of the (A) component represented by the general formula (9) (terminals substituted with hydrogen) with a charge of 0 and a multiplicity of 1, using the density functional theory (DFT) with the functional B3LYP and the basis function 6-31G(d) (Gaussian input line "#B3LYP / 6-31G(d)OPT"). Next, the lowest excited triplet energy (T1) was calculated for the optimized molecular structure using a charge of 0 and a multiplicity of 1 by the time-dependent density functional method (TDDFT) with the functional B3LYP and the basis set 6-31G(d) (Gaussian input line "#B3LYP / 6-31G(d)td=(50-50,nstates=4)"). Note that for DFT and TDDFT calculations, computational chemistry software with similar functions may be used instead.
[0166] [ka]
[0167] The energies of the lowest excited triplet state (T1) of the unsaturated group-containing alkali-soluble resins ((A)-12, 13, and 14) were calculated by the above-mentioned quantum chemical calculations based on the structural units of the (A) component represented by the following general formulas (10), (11), and (12), respectively.
[0168] [ka]
[0169] [ka]
[0170] [ka]
[0171] (Preparation of substrates with cured films for evaluating laser processability) The photosensitive resin composition shown in Table 1 was previously exposed to a low-pressure mercury lamp with an illumination intensity of 1000 mJ / cm at a wavelength of 254 nm. 2 The coating was applied to a 125 mm×125 mm synthetic quartz glass substrate (hereinafter referred to as "quartz glass substrate"), the surface of which had been cleaned by irradiating with ultraviolet light of 1000 nm, using a spin coater so that the film thickness after heat curing would be 1.0 μm, and a dry film was produced by pre-baking at 90° C. for 1 minute using a hot plate. Next, the film was main-cured (post-baked) at 250° C. for 30 minutes using a hot air dryer, to obtain substrates with cured films according to Examples 1 to 12 and Comparative Examples 1 to 4.
[0172] [Laser processability evaluation] (Evaluation method) After the main curing (post-baking), the cured film (coating film) was irradiated from the quartz glass substrate side with a laser (laser wavelength: 266 nm) using a flash lamp pumped Nd:YAG Q-SW laser oscillator "Callisto" (manufactured by V-Technology Co., Ltd.).2 The cured film (coating film) was processed (coating film removed) with a laser energy of 0.01 μm, and the processed cured film (coating film) was observed under an optical microscope.
[0173] (Evaluation Criteria) ○: 20mJ / cm 2 There is no paint residue in the laser irradiated area in the following cases. △: 20mJ / cm 2 Super 50mJ / cm 2 There is no paint residue in the laser irradiated area in the following cases. ×:50mJ / cm 2 There is paint residue in the laser irradiated area.
[0174] (Preparation of substrate with cured film for evaluation of development residue) The adhesive layer-forming composition shown in Table 1 was applied to a 125 mm x 125 mm glass substrate "#1737" (manufactured by Corning Incorporated) (hereinafter referred to as "glass substrate") using a spin coater so that the film thickness after heat curing treatment would be 3.0 μm, and the substrate was prebaked at 90°C for 1 minute using a hot plate to produce a hardened film (coating film). Next, the illuminance of 365 nm wavelength was 30 mW / cm 2 300mJ / cm2 ultra-high pressure mercury lamp 2 The exposed portion was exposed to ultraviolet light to cause a photocuring reaction.
[0175] Next, the exposed film was developed at 1 kgf / cm using a 0.8% TMAH (tetramethylammonium hydroxide) developer at 23°C. 2 After 10 seconds of development from the development time (break time = BT) when the pattern begins to appear, the shower pressure was increased to 5 kgf / cm 2 The unexposed portions of the exposed film were removed to form a dot pattern with a diameter of 30 μm on the glass substrate, and the substrate was post-cured (post-baked) at 250° C. for 30 minutes using a hot air dryer to obtain substrates with cured films according to Examples 1 to 12 and Comparative Examples 1 to 4.
[0176] [Development residue evaluation] (Evaluation method) The dot pattern of 30 μm diameter of the cured film (coating film) of the obtained substrate with the cured film was observed with an optical microscope and a scanning electron microscope (SEM) for jagged edges of the pattern and residues on the substrate originating from the adhesive layer-forming composition.
[0177] (Evaluation Criteria) ○: No residue was observed on the pattern edge or on the substrate. △: Residue was observed on the pattern edge and part of the substrate. ×: Significant residues on the pattern edges and on the substrate -: No pattern formed
[0178] (Preparation of substrates with cured films for chemical resistance evaluation) The photosensitive resin composition shown in Table 1 was applied to a glass substrate "#1737" using a spin coater so that the film thickness after heat curing would be 3.0 μm, and the substrate was prebaked at 90° C. for 3 minutes using a hot plate to produce a dry film. Then, the substrate was heated at a wavelength of 365 nm and exposed to an illumination intensity of 30 mW / cm 2 100mJ / cm2 ultra-high pressure mercury lamp 2 After that, the coating was post-baked at 230° C. for 30 minutes using a hot air dryer to obtain substrates with cured films according to Examples 1-12 and Comparative Examples 1-4.
[0179] [Chemical resistance evaluation] (Evaluation method) The cured film (coating film) on the obtained substrate with the cured film was immersed in acetone, 5 wt% aqueous sodium hydroxide solution, and 5 wt% hydrochloric acid for 30 minutes each, and then washed and dried. The thickness of the cured film (coating film) after the test was then measured using a stylus-type step shape measuring device "P-17" (manufactured by KLA Tencor Corporation). A grade of △ or higher was deemed to be a pass.
[0180] The remaining film rate in the chemical resistance evaluation was calculated from the following formula, where the film thickness before the test was L1 and the film thickness after the test was L2. Remaining film rate (%)=L2 / L1×100
[0181] (Evaluation Criteria) ○: Residual film rate is 90% or more △: Residual film rate is 80% or more and less than 90% ×: Residual film rate is less than 80%
[0182] The evaluation results are shown in Table 2.
[0183] [Table 2]
[0184] It has been found that a laminate using an adhesive layer-forming composition containing an unsaturated group-containing alkali-soluble resin of the present invention as an adhesive layer has excellent laser processability. This is believed to be because the unsaturated group-containing alkali-soluble resin has a low crosslink density after curing and is therefore easily ablated when irradiated with a laser.
[0185] In addition, it was found that when Y of the unsaturated group-containing alkali-soluble resin represented by general formula (1) of the present invention is an aromatic hydrocarbon group, the energy value of the lowest excited triplet state (T1) can be set to 2.90 eV or less, and the resin has excellent laser processability. This is because when Y is an aromatic hydrocarbon group, the LUMO (lowest unoccupied molecular orbital) value of the resin (structural unit) becomes small. This is thought to be because the HOMO (highest occupied molecular orbital)-LUMO energy gap becomes small, and the value of the lowest excited triplet state (T1) also becomes small.
[0186] In addition, it was found that the adhesive layer-forming composition containing an epoxy compound having two or more epoxy groups as component (E) has excellent chemical resistance. This is believed to be because the inclusion of component (E) allows a sufficient crosslinking structure to be formed. [Industrial Applicability]
[0187] The present invention can provide a laminate having an adhesive that can be used in the manufacture of various products, and in particular, can provide a laminate suitable for a process in which the laminate is temporarily attached to a support such as a semiconductor wafer and processed.
Claims
1. A laminate having an adhesive layer between a light-transmitting support and an adherend, A composition for forming an adhesive layer, which enables the support and the adherend to be separated from the laminate by irradiating light from the support side, The adhesive layer-forming composition contains (A) an unsaturated group-containing alkali-soluble resin as an essential component, the energy value of the lowest excited triplet state (T1) of the unsaturated group-containing alkali-soluble resin (A) calculated by quantum chemical calculation is 2.90 eV or less; The (A) unsaturated group-containing alkali-soluble resin is a resin represented by the following general formula (1): Composition for forming adhesive layer. 【Chemistry 1】 (In formula (1), Ar's are each independently an aromatic hydrocarbon group having 6 to 14 carbon atoms, and a portion of the bonded hydrogen atoms may be substituted with a substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an aryl group or arylalkyl group having 6 to 10 carbon atoms, a cycloalkyl group or cycloalkylalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, and a halogen group. R 1's are each independently an alkylene group having 2 to 4 carbon atoms, and 1's are each independently a number from 0 to 3. G's are each independently a (meth)acryloyl group or a substituent represented by the following general formula (2) or the following general formula (3), and Y is a tetravalent carboxylic acid residue containing at least one aromatic hydrocarbon group. Z's are each independently a hydrogen atom or a substituent represented by the following general formula (4), and at least one Z is a substituent represented by the following general formula (4). n is a number having an average value of 1 to 20.) 【Chemistry 2】 【Chemistry 3】 (In formulas (2) and (3), R 2 is a hydrogen atom or a methyl group, R 3 is a divalent alkylene group or alkylarylene group having 2 to 10 carbon atoms, R 4 is a divalent saturated or unsaturated hydrocarbon group having 2 to 20 carbon atoms, and p is a number from 0 to 10.) 【Chemistry 4】 (In formula (4), W is a divalent or trivalent carboxylic acid residue, and m is the number 1 or 2.)
2. (B) a photopolymerizable monomer having at least one ethylenically unsaturated bond; (C) a photopolymerization initiator and / or (D) a sensitizer; The adhesive layer-forming composition according to claim 1 .
3. The adhesive layer-forming composition according to claim 1 or 2, further comprising (E) an epoxy compound having two or more epoxy groups.
4. The adhesive layer forming composition according to any one of claims 1 to 3, wherein the (A) unsaturated group-containing alkali-soluble resin has a weight average molecular weight of 1,000 or more and 100,000 or less and an acid value of 50 mg KOH / g or more and 200 mg KOH / g or less.
5. A step of forming an adhesive layer on one or both of the surfaces of a support and an adherend using the adhesive layer-forming composition according to any one of claims 1 to 4; a step of adhering the support and the adherend via the formed adhesive layer; A method for producing a laminate comprising the steps of:
6. A step of preparing a laminate having a support, an adhesive layer formed using the adhesive layer-forming composition according to any one of claims 1 to 4, and an adherend; A step of separating the support and the adherend by irradiating with light; A method for treating a laminate, comprising: the support transmits light having a wavelength of 10 nm or more and 400 nm or less; The laminate treatment method, wherein the laminate is capable of being separated into the support and the adherend by irradiating the adhesive layer with light.
Citation Information
Patent Citations
Seed for epitaxial congelation
JP1980080800A
Photosensitive resin composition containing silica sol and cured product using the same
JP2014002374A
Photosensitive resin composition for insulation film, and cured product
JP2014206727A
Photosensitive resin composition, cured film formed by curing the same, and display device with that cured film
JP2020173433A
Electronic device and method for producing electronic device
WO2016158264A1