How to cut composite materials

By forming scribe grooves on the resin layer side using an ultrashort pulse laser light source focused near the interface, the method addresses crack formation and improves bending strength in divided composite materials.

JP7561089B2Active Publication Date: 2024-10-03NITTO DENKO CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021098404
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-06-14
Publication Date
2024-10-03
Estimated Expiration
2041-06-14

AI Technical Summary

Technical Problem

Existing methods for dividing composite materials with brittle and resin layers face challenges in minimizing cracks on the end faces and achieving sufficient bending strength after division.

Method used

A method involving the use of an ultrashort pulse laser light source to form scribe grooves on the resin layer side of the composite material, setting the laser focus near the interface between the resin and brittle layers, and removing the brittle material without penetrating the brittle layer, followed by resin removal, to ensure crack-free division and sufficient bending strength.

Benefits of technology

The method effectively reduces cracks on the brittle material layer end faces and enhances bending strength in the divided composite material pieces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561089000002
    Figure 0007561089000002
  • Figure 0007561089000003
    Figure 0007561089000003
  • Figure 0007561089000004
    Figure 0007561089000004
Patent Text Reader

Abstract

To provide a method which prevents occurrence of cracking on an end face of a brittle material layer after division, and can obtain sufficient bending strength on the composite material after division.SOLUTION: A method for dividing a composite material 10 in which a brittle material layer 1 and a resin layer 2 are laminated includes: a brittle material removal step of irradiating a composite material with a laser beam L1 oscillated from an ultrashort pulse laser light source 20 along a scheduled division line DL of the composite material from the brittle material layer side, and forming a scribe groove 11; and a resin removal step of irradiating the resin layer with a laser beam L2 oscillated from the laser light source 30 along the scheduled division line, and removing a resin forming the resin layer. The brittle material removal step sets a focal point AF of the laser beam L1 at the vicinity of an interface between the brittle material layer and the resin layer, oscillates the lase beam L1 in a state where thickness of the resin layer at the irradiation position of the laser beam L1 is equal to or more than 5 μm, and forms the scribe groove that is opened on the resin layer side and does not pass through the brittle material layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for dividing a composite material in which a brittle material layer and a resin layer are laminated, and in particular to a method for dividing the composite material (composite piece) in which cracks are unlikely to occur on the end surface of the brittle material layer after division and sufficient bending strength is obtained in the divided composite material (composite piece). [Background technology]

[0002] 2. Description of the Related Art In many cases, a protective material is disposed on the outermost surface of an image display device used in a television or a personal computer to protect the image display device. A glass plate is typically used as the protective material. However, as image display devices, such as those used in smartphones, smart watches, and in-vehicle displays, become smaller, thinner, and lighter, there is an increasing demand for thin protective materials that combine protective and optical functions. Examples of such protective materials include composite materials in which a brittle material layer such as glass that provides a protective function is laminated with a resin layer such as a polarizing film that provides an optical function. This composite material needs to be cut into a predetermined shape and size according to the application.

[0003] Conventionally, a method disclosed in Patent Document 1 has been proposed as a method for dividing a composite material in which a brittle material layer and a resin layer are laminated. The method described in Patent Document 1 includes a resin removal process in which a laser beam emitted from a laser light source such as a CO2 laser light source is irradiated onto a resin layer along the planned dividing line of a composite material to remove the resin that forms the resin layer, thereby forming a processed groove along the planned dividing line, and a brittle material removal process in which, after the resin removal process, a laser beam emitted from an ultrashort pulse laser light source is irradiated onto the brittle material layer along the planned dividing line to remove the brittle material that forms the brittle material layer, thereby forming a processed mark along the planned dividing line, where the processed mark is a through hole that penetrates the brittle material layer. According to the method described in Patent Document 1, the brittle material that forms the brittle material layer is removed using laser light emitted from an ultrashort pulse laser light source, which has the advantage that cracks are less likely to occur on the end surface of the brittle material layer after cutting.

[0004] Furthermore, the method described in Patent Document 1 also provides a predetermined bending strength for the composite material after cutting. However, it is desired to provide a more sufficient bending strength.

[0005] Non-Patent Document 1 describes that in a processing technique using an ultrashort pulsed laser beam, the filamentation phenomenon of the ultrashort pulsed laser beam is utilized, and a multi-focus optical system or a Bessel beam optical system is applied to an ultrashort pulsed laser light source. Furthermore, Non-Patent Document 2 describes the two-point bending stress of a thin glass substrate. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2019-122966 A [Non-patent literature]

[0007] [Non-Patent Document 1] John Lopez et al., “Glass Cutting Using Ultrashort Pulsed Bessel Beams,” [online], October 2015, International Congress on Applications of Lasers & Electro-Optics (ICALEO), [Retrieved July 17, 2020], Internet (URL: https: / / www.researchgate.net / publication / 284617626_GLASS_CUTTING_USING_ULTRASHORT_PULSED_BESSEL_BEAMS) [Non-Patent Document 2] Suresh T. Gulati et al., “Two Point Bending of Thin Glass Substrate”, 2011, SID 11 DIGEST, p.652-654 Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made to solve the problems of the conventional technology as described above, and has an object to provide a method in which cracks are less likely to occur on the end faces of the brittle material layer after cutting, and sufficient bending strength is obtained in the composite material (composite piece) after cutting. [Means for solving the problem]

[0009] In order to solve the above problems, the inventors have conducted extensive research and found that, when the thickness of the resin layer at the irradiation position of the laser light emitted from an ultrashort pulse laser light source is equal to or greater than a predetermined value (5 μm or greater), the focus of the laser light is set near the interface between the resin layer and the brittle material layer, and the laser light is irradiated from the brittle material layer side along the planned dividing line, the brittle material only on the resin layer side of the brittle material layer is removed, and a scribe groove is formed that is integrally connected along the planned dividing line.The inventors have also found that the composite material is divided starting from the scribe groove, cracks are unlikely to occur on the end face of the brittle material layer after division, and sufficient bending strength is obtained in the composite material after division. The present invention has been completed based on the above-mentioned findings of the present inventors.

[0010] That is, in order to solve the above-mentioned problems, the present invention provides a method for dividing a composite material in which a brittle material layer and a resin layer are laminated, the method comprising: a brittle material removal step of irradiating the brittle material layer side with a laser beam oscillated from an ultrashort pulse laser light source along a planned division line of the composite material from the brittle material layer side to remove the brittle material that forms the brittle material layer, thereby forming a scribe groove that is integrally connected along the planned division line; and a resin removal step of irradiating the resin layer along the planned division line with a laser beam oscillated from a laser light source to remove the resin that forms the resin layer, wherein in the brittle material removal step, a focus of the laser beam oscillated from the ultrashort pulse laser light source is set in the vicinity of the interface between the resin layer and the brittle material layer, and the laser beam is oscillated from the ultrashort pulse laser light source in a state in which the thickness of the resin layer at the irradiation position of the laser beam oscillated from the ultrashort pulse laser light source is 5 μm or more, and the scribe groove that opens on the resin layer side and does not penetrate the brittle material layer is formed.

[0011] According to the composite dividing method of the present invention, in the brittle material removal step, laser light emitted from an ultrashort pulse laser light source is irradiated to remove the brittle material that forms the brittle material layer, thereby forming a scribe groove in the brittle material layer. Therefore, the composite is divided starting from this scribe groove, and cracks are less likely to occur on the end face of the brittle material layer after division (the end face in the direction perpendicular to the thickness direction of the composite (the lamination direction of the brittle material layer and the resin layer)). Furthermore, according to the method for dividing a composite material according to the present invention, the scribe groove formed in the brittle material removing step opens on the resin layer side and does not penetrate the brittle material layer. In other words, in the brittle material removing step, the brittle material is removed only on the resin layer side of the brittle material layer to form the scribe groove. Therefore, the composite material is divided starting from the scribe groove, and as the present inventors have found, the divided composite material can have sufficient bending strength. Although the mechanism by which the scribe groove is formed by the present invention is not entirely clear, the inventors presume that by setting the focus of the laser light near the interface between the resin layer and the brittle material layer, the energy of the laser light is concentrated and absorbed near the interface between the resin layer and the brittle material layer, generating heat, and this heat is then conducted to the brittle material layer, removing the brittle material at the point where the heat is conducted, thereby forming the scribe groove.

[0012] In the composite dividing method according to the present invention, "irradiating the composite with laser light from the brittle material layer side along the planned dividing line" means irradiating the composite with laser light from the brittle material layer side along the planned dividing line when viewed from the thickness direction of the composite (lamination direction of the brittle material layer and the resin layer). In addition, in the composite dividing method according to the present invention, "irradiating the resin layer with laser light along the planned dividing line" means irradiating the resin layer with laser light along the planned dividing line when viewed from the thickness direction of the composite. In addition, in the method for dividing a composite material according to the present invention, "the vicinity of the interface between the resin layer and the brittle material layer" means the interface itself between the resin layer and the brittle material layer, and a portion of the resin layer close to the interface (for example, a portion that is 20 μm or less, preferably 10 μm or less, away from the interface in the thickness direction of the composite material). "Setting the focal point of the laser light emitted from the ultrashort pulse laser light source near the interface between the resin layer and the brittle material layer" means setting the position of the focal point of the laser light in the thickness direction of the composite material near the interface between the resin layer and the brittle material layer. Furthermore, in the composite material dividing method according to the present invention, the type of laser light source used in the resin removing step is not particularly limited as long as the resin forming the resin layer can be removed by the oscillating laser light. However, it is preferable to use a CO2 laser light source or a CO laser light source that oscillates a laser light with a wavelength in the infrared range, since it is possible to increase the relative moving speed (processing speed) of the laser light with respect to the composite material.

[0013] In the composite cutting method according to the present invention, it is also possible to carry out the resin removal step first, followed by the brittle material removal step. However, in this case, the resin cannot be completely removed along the planned cutting line in the resin removal step, and it becomes necessary to intentionally leave the resin for a thickness of 5 μm or more. The amount of remaining resin can vary depending on the power of the laser light emitted from the laser light source in the resin removal step, the relative moving speed (processing speed) of the laser light with respect to the composite material, etc., so it takes time to adjust them, while leaving too much resin may cause problems in cutting the composite material. For this reason, in the composite material dividing method according to the present invention, it is preferable to carry out the resin removing step after the brittle material removing step. According to the above-mentioned preferred method, since the scribe grooves are formed by the brittle material removal step performed first, there is no problem in completely removing the resin along the planned dividing line in the resin removal step performed after the scribe grooves are formed. This makes it possible to avoid the trouble of adjusting the power of the laser light, etc., and the risk of problems occurring in dividing the composite material.

[0014] Preferably, the composite material dividing method according to the present invention further includes, after the brittle material removing step and the resin removing step, a composite material dividing step of dividing the composite material by applying an external force along the planned dividing line. According to the above-mentioned preferable method, it is possible to reliably cut the composite material.

[0015] According to the findings of the inventors, the smaller the depth of the scribed grooves, the more sufficient bending strength can be obtained in the composite material after cutting, whereas if the depth of the scribed grooves is too small, cutting of the composite material is hindered. Therefore, in the method for dividing a composite material according to the present invention, the depth of the scribed groove is preferably 3 μm or more and 50 μm or less. The lower limit is more preferably 5 μm or more, and even more preferably 10 μm or more. The upper limit is more preferably 30 μm or less, more preferably 20 μm or less, more preferably 18 μm or less, and even more preferably 16 μm or less. In the above-mentioned preferred method, "depth of the scribed groove" means the distance between the end of the scribed groove on the resin layer side (open end of the scribed groove) and the bottom of the scribed groove on the brittle material layer side (end opposite to the open end of the scribed groove). In addition, in the above-mentioned preferred method, "the depth of the scribed groove is 3 μm or more and 50 μm or less" means that the average value of the depth of the scribed groove along the intended division line is 3 μm or more and 50 μm or less.

[0016] In the method for dividing a composite material according to the present invention, the depth of the scribe groove is preferably 10% to 50% of the thickness of the brittle material layer, more preferably 15% or more as the lower limit, and 35% or less as the upper limit.

[0017] In the composite material cutting method according to the present invention, the wavelength of the laser light oscillated from the ultrashort pulse laser light source is, for example, not less than 500 nm and not more than 2500 nm.

[0018] In the composite material cutting method according to the present invention, the pulse width of the laser light oscillated from the ultrashort pulse laser light source is, for example, not less than 350 femtoseconds and not more than 10,000 femtoseconds. Effect of the Invention

[0019] According to the present invention, cracks are unlikely to occur on the end faces of the brittle material layer after cutting, and it is possible to obtain sufficient bending strength for the composite material after cutting. [Brief description of the drawings]

[0020] [Figure 1] 1A to 1C are explanatory diagrams for explaining a schematic procedure of a composite material dividing method according to one embodiment of the present invention. [Diagram 2] 1A to 1C are explanatory diagrams for explaining a schematic procedure of a composite material dividing method according to one embodiment of the present invention. [Diagram 3] 2 is an explanatory diagram for explaining a schematic example of a method for setting the focus of laser light oscillated from the ultrashort pulse laser light source shown in FIG. 1. FIG. [Figure 4]FIG. 2 is a cross-sectional view showing a schematic configuration of a composite piece after being cut in a composite cutting step of a cutting method according to one embodiment of the present invention. [Diagram 5] FIG. 1 is a diagram for explaining a schematic overview of a test according to Example 1. [Figure 6] FIG. 1 is a diagram showing test results according to Examples 1 and 2 and Comparative Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, a composite material dividing method according to one embodiment of the present invention (hereinafter, simply referred to as a "dividing method") will be described with reference to the attached drawings as appropriate. 1 and 2 are explanatory diagrams for explaining the procedure of a composite cutting method according to an embodiment of the present invention. Fig. 1(a) is a cross-sectional view showing a brittle material removing step of the cutting method according to the present embodiment, Fig. 1(b) is a cross-sectional view showing a resin removing step of the cutting method according to the present embodiment, and Fig. 1(c) is a cross-sectional view showing a composite cutting step of the cutting method according to the present embodiment. Fig. 2(a) is an upper plan view (plan view seen from the brittle material layer side) showing the composite after the brittle material removing step of the cutting method according to the present embodiment, and Fig. 2(b) is a lower plan view (plan view seen from the resin layer side) showing the composite after the resin removing step of the cutting method according to the present embodiment. The cutting method according to this embodiment is a method for cutting a composite material 10 in which a brittle material layer 1 and a resin layer 2 are laminated, in the thickness direction (the lamination direction of the brittle material layer 1 and the resin layer 2, the vertical direction in Figure 1, the Z direction).

[0022] The brittle material layer 1 and the resin layer 2 are laminated by any suitable method. For example, the brittle material layer 1 and the resin layer 2 can be laminated by a so-called roll-to-roll method. That is, the brittle material layer 1 and the resin layer 2 can be laminated by conveying the long brittle material layer 1 and the long resin layer 2 in the longitudinal direction, and attaching them to each other so that their longitudinal directions are aligned. It is also possible to laminate the brittle material layer 1 and the resin layer 2 after cutting them into a predetermined shape. The brittle material layer 1 and the resin layer 2 are typically laminated via any suitable adhesive or adhesive.

[0023] Examples of the brittle material that forms the brittle material layer 1 include glass, and single crystal or polycrystalline silicon. Glass can be classified according to composition, such as soda-lime glass, borate glass, aluminosilicate glass, quartz glass, and sapphire glass. Glass can be classified according to alkali content, such as non-alkali glass and low-alkali glass. The content of alkali metal components (e.g., Na2O, K2O, Li2O) in the glass is preferably 15% by weight or less, more preferably 10% by weight or less.

[0024] The thickness of the brittle material layer 1 is preferably 200 μm or less, more preferably 150 μm or less, even more preferably 120 μm or less, and particularly preferably 100 μm or less. On the other hand, the thickness of the brittle material layer 1 is preferably 5 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more. If the thickness of the brittle material layer 1 is in such a range, lamination with the resin layer 2 by a roll-to-roll method is possible.

[0025] When the brittle material forming the brittle material layer 1 is glass, the light transmittance of the brittle material layer 1 at a wavelength of 550 nm is preferably 85% or more. When the brittle material forming the brittle material layer 1 is glass, the refractive index of the brittle material layer 1 at a wavelength of 550 nm is preferably 1.4 to 1.65. When the brittle material forming the brittle material layer 1 is glass, the density of the brittle material layer 1 is preferably 2.3 g / cm 3 ~3.0g / cm 3 and more preferably 2.3 g / cm 3 ~2.7g / cm 3 It is.

[0026] When the brittle material forming the brittle material layer 1 is glass, a commercially available glass plate may be used as it is, or may be polished to a desired thickness and used as the brittle material layer 1. Examples of commercially available glass plates include "7059", "1737" and "EAGLE2000" manufactured by Corning Incorporated, "AN100" manufactured by Asahi Glass Co., Ltd., "NA-35" manufactured by NH Techno Glass Co., Ltd., "OA-10" manufactured by Nippon Electric Glass Co., Ltd., and "D263" or "AF45" manufactured by Schott.

[0027] Examples of the resin layer 2 include a single layer film formed of a plastic material such as polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), acrylic resin such as polymethyl methacrylate (PMMA), cyclic olefin polymer (COP), cyclic olefin copolymer (COC), polycarbonate (PC), urethane resin, polyvinyl alcohol (PVA), polyimide (PI), polytetrafluoroethylene (PTFE), polyvinyl chloride (PVC), polystyrene (PS), triacetyl cellulose (TAC), polyethylene naphthalate (PEN), ethylene-vinyl acetate (EVA), polyamide (PA), silicone resin, epoxy resin, liquid crystal polymer, and various resin foams, or a laminate film consisting of multiple layers.

[0028] When the resin layer 2 is a laminated film composed of multiple layers, various adhesives such as acrylic adhesives, urethane adhesives, silicone adhesives, and epoxy adhesives may be interposed between the layers. Also, an adhesive layer or adhesive layer made of the above-mentioned adhesives or adhesives may be formed on the surface of the resin layer 2. Furthermore, on the surface of the resin layer 2, a conductive inorganic film such as an indium tin oxide (ITO), Ag, Au, or Cu film may be formed. The cutting method according to this embodiment is particularly suitable for use in cases where the resin layer 2 is any of various optical films such as polarizing films, surface protection films, and retardation films used in displays. The thickness of the resin layer 2 is preferably 20 to 500 μm.

[0029] In the example shown in Figure 1, the resin layer 2 is a surface protection film composed of a base film 21 made of PET or the like and an adhesive layer 22 formed on one side of the base film 21, and the composite material 10 is illustrated as an example in which a brittle material layer 1 and a resin layer 2 are laminated via the adhesive layer 22.

[0030] The cutting method according to the present embodiment includes a brittle material removing step, a resin removing step, and a composite material cutting step. Each step will be described below in order.

[0031] <Brittle material removal process> As shown in Figures 1(a) and 2(a), in the brittle material removal process, laser light (ultrashort pulse laser light) L1 oscillated (pulsed) from an ultrashort pulse laser light source 20 is irradiated from the brittle material layer 1 side along the planned dividing line of the composite 10 to remove the brittle material that forms the brittle material layer 1, thereby forming a scribe groove 11 that is integrally connected along the planned dividing line. In the example shown in FIG. 1 and FIG. 2, a straight line DL extending in the Y direction among two orthogonal directions (X direction and Y direction) in the plane (XY two-dimensional plane) of the composite material 10 is illustrated as the planned division line. The planned division line DL can be actually drawn on the composite material 10 as a visually recognizable display, or its coordinates can be input in advance to a control device (not shown) that controls the relative positional relationship between the laser light L1 and the composite material 10 on the XY two-dimensional plane. The planned division line DL shown in FIG. 1 and FIG. 2 is a virtual line whose coordinates are input in advance to the control device and is not actually drawn on the composite material 10. Note that the planned division line DL is not limited to a straight line and may be a curved line. By determining the planned division line DL according to the application of the composite material 10, the composite material 10 can be divided into any shape according to the application.

[0032] As an example of the manner in which the laser light L1 is irradiated along the planned dividing line DL of the composite material 10 (an example of scanning the laser light L1), it is possible to place the sheet-shaped composite material 10 on an XY two-axis stage (not shown) and fix it (for example, by suction), and drive the XY two-axis stage by a control signal from a control device to change the relative position of the composite material 10 on the XY two-dimensional plane with respect to the laser light L1. It is also possible to fix the position of the composite material 10 and change the position of the laser light L1 irradiated to the composite material 10 on the XY two-dimensional plane by deflecting the laser light L1 oscillated from the ultrashort pulse laser light source 20 using a galvanometer mirror or a polygon mirror driven by a control signal from a control device. Furthermore, it is also possible to use both the scanning of the composite material 10 using the above-mentioned XY two-axis stage and the scanning of the laser light L1 using a galvanometer mirror or the like in combination.

[0033] The brittle material forming the brittle material layer 1 is removed by utilizing the filamentation phenomenon of the laser light L1 emitted from the ultrashort pulse laser light source 20, or by applying a multi-focus optical system (not shown) or a Bessel beam optical system (not shown) to the ultrashort pulse laser light source 20. The use of the filamentation phenomenon of ultrashort pulsed laser light and the application of a multi-focus optical system or a Bessel beam optical system to an ultrashort pulsed laser light source are described in the above-mentioned Non-Patent Document 1. Trumpf, Germany, also sells products related to glass processing in which a multi-focus optical system is applied to an ultrashort pulsed laser light source. As described above, the use of the filamentation phenomenon of ultrashort pulsed laser light and the application of a multi-focus optical system or a Bessel beam optical system to an ultrashort pulsed laser light source are publicly known, and therefore further detailed description will be omitted here.

[0034] The wavelength of the laser light L1 emitted from the ultrashort pulse laser light source 20 is preferably 500 nm or more and 2500 nm or less, which shows high light transmittance when the brittle material forming the brittle material layer 1 is glass. In order to effectively induce a nonlinear optical phenomenon (multiphoton absorption), the pulse width of the laser light L1 is preferably 100 picoseconds or less, and more preferably 50 picoseconds or less. The pulse width of the laser light L1 is set, for example, to 350 femtoseconds or more and 10000 femtoseconds or less. The oscillation form of the laser light L1 may be single pulse oscillation or burst mode multi-pulse oscillation.

[0035] In the brittle material removal process, the focus of the laser light L1 emitted from the ultrashort pulse laser light source 20 is set near the interface between the resin layer 2 and the brittle material layer 1. As a result, the scribe groove 11 formed in the brittle material removal process opens on the resin layer 2 side and does not penetrate the brittle material layer 1 (does not open on the side opposite to the resin layer 2 side). In other words, in the brittle material removal process, the scribe groove 11 is formed by removing the brittle material only on the resin layer 2 side of the brittle material layer 1. This point will be explained in more detail below.

[0036] FIG. 3 is an explanatory diagram for explaining a schematic example of a method for setting the focus of the laser light L1 oscillated from the ultrashort pulse laser light source 20. As shown in FIG. In the example shown in FIG. 3, a multi-focus optical system is applied to the ultrashort pulse laser light source 20. Specifically, the multi-focus optical system shown in FIG. 3 is composed of three axicon lenses 21a, 21b, and 21c. As shown in FIG. 3, if the spatial intensity distribution of the laser light L1 oscillated from the ultrashort pulse laser light source 20 is assumed to be a Gaussian distribution, the laser light L1 oscillated in the range from point A to point B, where the intensity is relatively high, follows the optical path shown by the broken line in FIG. 3 and converges at a focal point AF. In the brittle material removal process of this embodiment, the focal point set near the interface between the resin layer 2 and the brittle material layer 1 is the focal point AF where the laser light L1 oscillated in the range from point A to point B, where the intensity is relatively high, is converged. The range from point A to point B is, for example, a range where the intensity of the laser light L1 is 90% or more of the maximum intensity of the spatial intensity distribution of the laser light L1. In the brittle material removal process, the positional relationship between the focal point AF and the composite material 10 is adjusted so that the focal point AF of the laser light L1 is located near the interface between the resin layer 2 and the brittle material layer 1, specifically, at a distance H from the interface. This distance H is preferably set to 0 μm to 20 μm, and more preferably 0 μm to 10 μm. The spot diameter of the laser light L1 at the focal point AF is set to preferably 5 μm or less, and more preferably 3 μm or less.

[0037] In addition, when the filamentation phenomenon of the laser light L1 is utilized, the laser light L1 self-converges due to the Kerr effect when passing through the brittle material layer 1, and the spot diameter becomes smaller as it advances. Then, when the laser light L1 converges to an energy threshold at which ablation occurs in the brittle material layer 1, the brittle material of the brittle material layer 1 is removed and a scribe groove 11 is formed. As described above, by setting the position at which the laser light L1 converges to the energy threshold at which ablation occurs (corresponding to the focus AF described above) near the interface between the resin layer 2 and the brittle material layer 1, it is possible to form a scribe groove 11 that opens on the resin layer 2 side and does not penetrate the brittle material layer 1.

[0038] By adjusting the power of the laser light L1 oscillated from the ultrashort pulse laser light source 20, it is possible to adjust the strength of the energy used to form the scribe groove 11 (to remove the brittle material) (the strength in the range from point A to point B). This makes it possible to adjust the depth of the scribe groove 11. The smaller the depth of the scribe groove 11, the more sufficient bending strength can be obtained in the composite material 10 after cutting. On the other hand, if the depth of the scribe groove 11 is too small, it will be difficult to cut the composite material 10 in the composite cutting process described below. For this reason, the depth of the scribe groove 11 is preferably 3 μm or more and 50 μm or less. The lower limit is more preferably 5 μm or more, and even more preferably 10 μm or more. The upper limit is more preferably 30 μm or less, more preferably 20 μm or less, more preferably 18 μm or less, and even more preferably 16 μm or less. When the thickness of the brittle material layer 1 is small (for example, when the thickness is 50 μm or less), the depth of the scribe groove 11 is preferably 3 μm or more and 20 μm or less. Moreover, the depth of the scribe grooves 11 is preferably 10% to 50% of the thickness of the brittle material layer 1. The lower limit is more preferably 15% or more, and the upper limit is more preferably 35% or less.

[0039] <Resin removal process> The resin removing step in this embodiment is performed after the brittle material removing step. 1(b) and 2(b), in the resin removal step, the resin layer 2 is irradiated with laser light L2 emitted from a laser light source 30 along the planned dividing line DL of the composite material 10 to remove the resin forming the resin layer 2. As a result, a processed groove 23 is formed along the planned dividing line DL. The manner in which the laser light L2 is irradiated along the planned division line DL (the manner in which the laser light L2 is scanned) can be the same as the manner in which the laser light L1 described above is irradiated along the planned division line DL, so detailed explanation will be omitted here.

[0040] In this embodiment, the laser light source 30 is a CO2 laser light source that oscillates laser light L2 with a wavelength of 9 to 11 μm in the infrared range. However, the present invention is not limited to this, and it is also possible to use, as the laser light source 30, a CO laser light source that oscillates laser light L2 with a wavelength of 5 μm. Also, a visible light and ultraviolet (UV) pulsed laser light source can be used as the laser light source 30. Examples of visible light and UV pulsed laser light sources include those emitting laser light L2 with a wavelength of 532 nm, 355 nm, 349 nm, or 266 nm (high-order harmonics of a solid-state laser light source using Nd:YAG, Nd:YLF, or YVO4 as a medium), an excimer laser light source emitting laser light L2 with a wavelength of 351 nm, 248 nm, 222 nm, 193 nm, or 157 nm, and an F2 laser light source emitting laser light L2 with a wavelength of 157 nm. It is also possible to use a pulsed laser light source that emits laser light L2 having a wavelength outside the ultraviolet range and a pulse width on the order of femtoseconds or picoseconds as the laser light source 30. If the laser light L2 emitted from this pulsed laser light source is used, it is possible to induce ablation processing based on a multiphoton absorption process. Furthermore, as the laser light source 30, it is also possible to use a semiconductor laser light source or a fiber laser light source that oscillates the laser light L2 with a wavelength in the infrared region. As described above, in this embodiment, a CO2 laser light source is used as the laser light source 30, and therefore, hereinafter, the laser light source 30 will be referred to as the "CO2 laser light source 30."

[0041] The oscillation form of the CO2 laser light source 30 may be pulse oscillation or continuous oscillation. The spatial intensity distribution of the laser light L2 may be a Gaussian distribution, or may be shaped into a flat-top distribution using a diffractive optical element (not shown) or the like in order to suppress damage to the brittle material layer 1 that is not the target of removal by the laser light L2. There is no restriction on the polarization state of the laser light L2, and it may be any of linear polarization, circular polarization, and random polarization.

[0042] By irradiating the resin layer 2 (base film 21 and adhesive layer 22) with the laser light L2 along the planned dividing line DL of the composite material 10, a local temperature rise occurs due to infrared light absorption of the resin irradiated with the laser light L2 (portions of the base film 21 and adhesive layer 22 irradiated with the laser light L2) among the resins forming the resin layer 2, and the resin is scattered, so that the resin is removed from the composite material 10, and a processed groove 23 is formed in the composite material 10. In order to prevent the scattered resin removed from the composite material 10 from reattaching to the composite material 10, it is preferable to provide a dust collection mechanism in the vicinity of the planned dividing line DL. In order to prevent the groove width of the processed groove 23 from increasing, it is preferable to focus the laser light L2 so that the spot diameter at the irradiation position on the resin layer 2 is 300 μm or less, and it is more preferable to focus the laser light L2 so that the spot diameter is 200 μm or less.

[0043] In the case of a resin removal method based on the principle of local temperature rise caused by infrared light absorption by resin irradiated with laser light L2, it is possible to roughly estimate the input energy required to form the processed groove 23 from the thickness of the resin layer 2, regardless of the type of resin or the layer structure of the resin layer 2. Specifically, the input energy required to form the processed groove 23, expressed by the following formula (1), can be estimated based on the thickness of the resin layer 2 using the following formula (2). Input energy [mJ / mm] = average power of laser light L2 [mW] / processing speed [mm / sec] (1) Input energy [mJ / mm] = 0.5 × thickness of resin layer 2 [μm] (2) The input energy to be actually set is preferably set to 20% to 180% of the input energy estimated by the above formula (2), and more preferably set to 50% to 150%. The reason for providing a margin for the estimated input energy in this way is that it is considered that the input energy required to form the groove 23 varies depending on the light absorptance (light absorptance at the wavelength of the laser light L2) of the resin forming the resin layer 2 and the thermal properties such as the melting point and decomposition point of the resin. Specifically, for example, a sample of the composite material 10 to which the cutting method according to the present embodiment is applied is prepared, and a preliminary test is performed to form the groove 23 in the resin layer 2 of this sample with a plurality of input energies within the above preferred range, and an appropriate input energy can be determined.

[0044] In the resin removal process of this embodiment, the resin layer 2 is irradiated with the laser light L2 oscillated from the laser light source 30 from the resin layer 2 side. In the example shown in Figs. 1(a) and (b), the CO2 laser light source 30 is disposed below the composite material 10 in the Z direction so as to face the resin layer 2, and the ultrashort pulse laser light source 20 is disposed above the composite material 10 in the Z direction so as to face the brittle material layer 1. Then, after the scribe groove 11 is formed with the laser light L1 oscillated from the ultrashort pulse laser light source 20 in the brittle material removal process, the oscillation of the laser light L1 is stopped, and the processed groove 23 is formed with the laser light L2 oscillated from the CO2 laser light source 30 in the resin removal process. However, the present invention is not limited to this, and it is also possible to adopt a method in which the ultrashort pulse laser light source 20 and the CO2 laser light source 30 are both placed on the same side of the composite material 10 (upper or lower in the Z direction), and the composite material 10 is turned upside down so that the brittle material layer 1 faces the ultrashort pulse laser light source 20 in the brittle material removal process, and the resin layer 2 faces the CO2 laser light source 30 in the resin removal process.

[0045] In the resin removal step, resin residue may be left at the bottom of the formed processed groove 23 as long as it does not interfere with cutting of the composite material 10 in the composite material cutting step described below. However, in order to reliably divide the composite material 10, it is preferable to further include a cleaning step of removing the resin residue that forms the resin layer 2 by cleaning the processed grooves 23 formed in the resin removal step. In the cleaning process, various wet and dry cleaning methods can be applied. Examples of wet cleaning methods include chemical immersion, ultrasonic cleaning, dry ice blasting, and micro- and nano-fine bubble cleaning. Examples of dry cleaning methods include laser, plasma, ultraviolet light, and ozone.

[0046] <Composite material cutting process> As shown in Fig. 1(c), in the composite material dividing step, after the brittle material removing step and the resin removing step, an external force is applied along the planned dividing line DL to divide the composite material 10. In the example shown in Fig. 1(c), the composite material 10 is divided into composite material pieces 10a and 10b. Examples of methods for applying an external force to the composite material 10 include mechanical breaking (mountain folding), heating the area near the planned cutting line DL with infrared laser light, applying vibration with an ultrasonic roller, and suction and lifting with a suction cup. When dividing the composite material 10 by mountain folding, it is preferable to apply an external force so that the resin layer 2 side of the brittle material layer 1 where the scribe groove 11 is formed becomes a starting point for division, making the resin layer 2 side convex (the brittle material layer 1 side becomes concave).

[0047] FIG. 4 is a cross-sectional view that shows a schematic configuration of composite material pieces 10a, 10b after being cut in the composite material cutting step of the cutting method according to this embodiment. As shown in FIG. 4, in each of the composite pieces 10a, 10b, the surface roughness of a first region 12 on the resin layer 2 side at one end face (cut end face) of the brittle material layer 1 is greater than the surface roughness of a second region 13 on the opposite side of the end face to the resin layer 2. The first region 12 corresponds to the region where the scribe groove 11 is formed, and the second region 13 corresponds to the region where the scribe groove 11 is not formed. Therefore, the thickness of the first region 12 (the dimension of the first region 12 along the thickness direction (Z direction) of the brittle material layer 1) is preferably 10% or more and 40% or less of the thickness of the brittle material layer 1. The lower limit is more preferably 15% or more. The upper limit is more preferably 35% or less. One end face (cut end face) of the brittle material layer 1 of the composite pieces 10a, 10b protrudes toward the one end face side (left side of the paper in FIG. 4) further than the end face (cut end face) on the same side of the resin layer 2. The protrusion amount 14 varies depending on the spot diameter at the irradiation position of the laser light L2 oscillated from the CO2 laser light source 30 on the resin layer 2, and is, for example, 200 μm or less, 100 μm or less, or 50 μm or less. The lower limit of the protrusion amount 14 is preferably as small as possible, and is, for example, 1 μm or more, or 5 μm or more.

[0048] According to the cutting method of this embodiment described above, in the brittle material removal process, the laser light L1 emitted from the ultrashort pulse laser light source 20 is irradiated to remove the brittle material that forms the brittle material layer 1, thereby forming a scribe groove 11 in the brittle material layer 1. Therefore, in the composite cutting process, the composite 10 is cut starting from this scribe groove 11, and cracks are less likely to occur on the end face of the brittle material layer 1 after cutting. Furthermore, according to the dividing method of this embodiment, the scribe grooves 11 formed in the brittle material removing step open on the resin layer 2 side and do not penetrate the brittle material layer 1. In other words, in the brittle material removing step, the scribe grooves 11 are formed by removing the brittle material only on the resin layer 2 side of the brittle material layer 1. Therefore, in the composite dividing step, the composite 10 is divided starting from the scribe grooves 11, and sufficient bending strength can be obtained in the divided composite pieces 10a, 10b.

[0049] In this embodiment, the resin removing step is performed after the brittle material removing step, but the present invention is not limited to this, and it is also possible to perform the brittle material removing step after the resin removing step. In other words, it is also possible to form the scribe groove 11 after forming the processed groove 23. However, in this case, in the brittle material removal process, the focal point AF of the laser light L1 emitted from the ultrashort pulse laser light source 20 is set near the interface between the resin layer 2 and the brittle material layer 1, so that resin residue must be generated at the bottom of the processed groove 23 when the brittle material removal process is performed. Specifically, the brittle material removal process must be performed when the thickness of this resin residue (i.e., the thickness of the resin layer 2 at the irradiation position of the laser light L1 emitted from the ultrashort pulse laser light source 20) is 5 μm or more.

[0050] Hereinafter, an example of the results of a test performed to cut the composite material 10 using the cutting method according to this embodiment (Examples 1 and 2) and the cutting methods according to comparative examples (Comparative Examples 1 and 2) will be described.

[0051] <Example 1> 5 is a diagram for explaining a schematic overview of the test according to Example 1. Hereinafter, the overview of the test according to Example 1 will be explained with reference to FIGS. In the composite material 10 used in Example 1, the brittle material layer 1 is made of alkali-free glass and has a thickness of 30 μm. The resin layer 2 is a surface protection film and has a total thickness of 58 μm. Specifically, this surface protection film is formed by applying an acrylic adhesive to one side of a substrate film 21 made of a PET film having a thickness of 38 μm and drying the film to form an adhesive layer (acrylic adhesive layer) 22 having a thickness of 20 μm after drying. The composite material 10 is configured such that the brittle material layer 1 and the resin layer 2 are laminated via the adhesive layer 22. As shown in FIG. 5(a), the composite material 10 is a square having an in-plane (XY two-dimensional plane) dimension of 150 mm×150 mm. The dashed straight line shown in FIG. 5(a) is the planned division line.

[0052] In Example 1, first, the brittle material removing step was performed, then the resin removing step was performed, and finally, the composite material cutting step was performed.

[0053] In the brittle material removal process, a Coherent "Monaco 1035-80-60" (oscillation wavelength 1035 nm, pulse width of laser light L1 350 to 10000 femtoseconds, maximum pulse oscillation repetition frequency 50 MHz, average power 60 W) was used as the ultrashort pulse laser light source 20, and the laser light L1 oscillated at a predetermined output from the ultrashort pulse laser light source 20 was irradiated onto the composite material 10 from the brittle material layer 1 side via a multi-focus optical system. The focus AF (see FIG. 3) of the laser light L1 was set at the center in the thickness direction of the adhesive layer 22 of the resin layer 2 (a position 10 μm from the interface with the brittle material layer 1, i.e., a distance H=10 μm). The relative movement speed (processing speed) of the laser light L1 with respect to the composite material 10 was set to 125 mm / sec, and the repetition frequency of the pulse oscillation was set to 125 kHz. The laser light L1 was scanned along the intended dividing line so as to divide a composite piece 10c having in-plane dimensions of 110 mm x 60 mm, as shown in Figure 5(a). As a result, a scribe groove 11 (see Figures 1(a) and 2(a)) was formed in the brittle material layer 1, the scribe groove 11 being integrally connected along the intended dividing line and having an (average) depth of 10 μm and a groove width of approximately 3 μm.

[0054] Next, in the resin removal process, a CO2 laser light source 30 was used, manufactured by Coherent Corporation, "DIAMOND J-3-9.4" (oscillation wavelength 9.4μm, pulse oscillation repetition frequency 15kHz, laser light L2 power 13W, Gaussian beam), and the laser light L2 emitted from the CO2 laser light source 30 was focused to a spot diameter of 120μm using a focusing lens, and was irradiated onto the resin layer 2 of the composite material 10. The relative movement speed (processing speed) of the laser light L2 with respect to the composite material 10 was set to 400mm / sec, and the laser light L2 was scanned along the planned division line, resulting in the formation of a processed groove 23 (see Fig. 1(b) and Fig. 2(b)) with a groove width of 150μm in the resin layer 2. In the resin removal step of Example 1, the input energy estimated by the above formula (2) is 29 mJ / mm. On the other hand, the actual input energy is 33 mJ / mm according to the above formula (1), which is 114% of the estimated input energy.

[0055] Finally, in the composite cutting process, the composite material 10 was manually folded along the intended cutting line so that the resin layer 2 side was convex (the brittle material layer 1 side was concave), thereby cutting the composite piece 10c.

[0056] <Example 2> In the composite material 10 used in Example 2, the brittle material layer 1 is formed from alkali-free glass and has a thickness of 100 μm. The resin layer 2 is formed by applying an epoxy adhesive to one side of a polarizing film and drying it to form an adhesive layer (epoxy adhesive layer) having a thickness of 1 μm after drying. The polarizing film used has a structure of TAC film (thickness 40 μm) / PVA polarizer (thickness 5 μm) / acrylic film (thickness 40 μm) / acrylic pressure-sensitive adhesive layer (thickness 30 μm) / separator (PET film, thickness 38 μm) in order from the side where the adhesive layer is formed. The composite material 10 has a structure in which the brittle material layer 1 and the resin layer 2 are laminated via an adhesive layer. The composite material 10 used in Example 2 is also a square shape with in-plane (XY two-dimensional plane) dimensions of 150 mm×150 mm, similar to Example 1.

[0057] In Example 2, the scribe groove 11 was formed under the same conditions as in Example 1, except that in the brittle material removing step, the focal point AF of the laser light L1 was set to the center in the thickness direction of the adhesive layer of the resin layer 2 (a position 0.5 μm from the interface with the brittle material layer 1, i.e., a distance H=0.5 μm). The resin removing step and the composite cutting step were also performed under the same conditions as in Example 1, and the composite piece 10c was cut.

[0058] <Comparative Example 1> In the composite material 10 used in Comparative Example 1, the brittle material layer 1 is formed of alkali-free glass and has a thickness of 30 μm, similar to that of Example 1. The resin layer 2 is formed by applying an epoxy adhesive to one side of a TAC film (thickness 40 μm) and drying it to form an adhesive layer (epoxy adhesive layer) having a thickness of 1 μm after drying. The composite material 10 is configured such that the brittle material layer 1 and the resin layer 2 are laminated via the adhesive layer. The composite material 10 used in Comparative Example 1 is also a square with in-plane (XY two-dimensional plane) dimensions of 150 mm × 150 mm, similar to Examples 1 and 2.

[0059] In Comparative Example 1, first, the resin removing step was performed, then the brittle material removing step was performed, and finally, the composite material cutting step was performed.

[0060] In the resin removal process, a CO2 laser light source 30 was used, manufactured by Coherent, Inc., "DIAMOND J-3-9.4" (oscillation wavelength 9.4 μm, pulse oscillation repetition frequency 15 kHz, laser light L2 power 18 W, Gaussian beam), and the laser light L2 emitted from the CO2 laser light source 30 was focused to a spot diameter of 120 μm using a focusing lens, and irradiated onto the resin layer 2 of the composite material 10. The relative movement speed (processing speed) of the laser light L2 with respect to the composite material 10 was set to 400 mm / sec, and the laser light L2 was scanned along the planned division line, forming a processed groove 23 with a groove width of 150 μm in the resin layer 2. No resin residue was generated at the bottom of the processed groove 23. In the resin removal step of Comparative Example 1, the input energy estimated by the above formula (2) is 21 mJ / mm. On the other hand, the actual input energy is 45 mJ / mm according to the above formula (1), which is 214% of the estimated input energy.

[0061] Next, in the brittle material removal process, an ultrashort pulse laser light source 20 having an oscillation wavelength of 1035 nm, a pulse width of 8500 femtoseconds for the laser light L1, a repetition frequency of pulse oscillation of 125 kHz, and an average power of 13 W was used, and the laser light L1 oscillated at a predetermined output from the ultrashort pulse laser light source 20 was irradiated onto the composite material 10 from the opposite side to the processed groove 23 (the brittle material layer 1 side) via a multi-focus optical system. The focal point AF of the laser light L1 was set at a position 25 μm away from the interface between the brittle material layer 1 and the resin layer 2 toward the brittle material layer 1 side. The relative moving speed (processing speed) of the laser light L1 with respect to the composite material 10 was set to 125 mm / sec, and the laser light L1 was scanned along the planned division line, resulting in the formation of perforations (diameter of about 0.7 to 0.9 μm) with a pitch of 1 μm as processing marks in the brittle material layer 1.

[0062] Finally, in the composite cutting process, similar to Examples 1 and 2, the composite material 10 was manually folded in half along the intended cutting line so that the resin layer 2 side was convex (the brittle material layer 1 side was concave), thereby cutting the composite material piece 10c.

[0063] <Comparative Example 2> The configuration of the composite material 10 used in Comparative Example 2 was the same as that in Example 2. The conditions of the resin removing step, the brittle material removing step, and the composite material cutting step performed in Comparative Example 2 were the same as those in Comparative Example 1.

[0064] <Evaluation details> The composite material pieces 10c obtained in the above-described Examples 1 and 2 and Comparative Examples 1 and 2 were evaluated for absorbance, bending strength, and breaking yield. The details of each of these evaluation items will be described below.

[0065] [Absorbance] For Example 1, the absorbance of the resin layer 2 (total thickness 58 μm) was measured at an oscillation wavelength of 1035 nm of the ultrashort pulse laser light source 20. For Example 2 and Comparative Examples 1 and 2, the absorbance of the adhesive layer (thickness 1 μm) of the resin layer 2 was measured at an oscillation wavelength of 1035 nm of the ultrashort pulse laser light source 20. Specifically, the above-mentioned measurement sites (resin layer 2 for Example 1, adhesive layer for Example 2 and Comparative Examples 1 and 2) were taken out of the composite piece 10c, and light with a wavelength of 1035 nm was irradiated using a Hitachi spectrophotometer "U-4100" to measure the transmittance (I / I0). Then, the absorbance A was calculated by the following formula (3). A=-log 10 (I / I0) (3)

[0066] [Bending strength] When calculating the bending strength, a two-point bending test was performed on the composite piece 10c. In the two-point bending test, first, as shown in FIG. 5(b), the composite piece 10c was placed on the fixed part 40 of a one-axis stage having a fixed part 40 and movable parts 50a and 50b, and the composite piece 10c was sandwiched between the movable parts 50a and 50b. At this time, as described later, the composite piece 10c was placed on the fixed part 40 so that the brittle material layer side of the composite piece 10c was bent in a convex manner (i.e., the brittle material layer 1 side was on the upper side) by moving the movable part 50b. Next, as shown in FIG. 5(c), while the position of the movable part 50a was fixed, the movable part 50b was moved toward the movable part 50a at a speed of 20 mm / min, and a bending stress was applied to the composite piece 10c. The bending strength of the composite piece 10c was evaluated based on the value of the distance D between the movable parts 50a and 50b when the composite piece 10c broke.

[0067] Specifically, the above-mentioned interval D is substituted into the formula (3) (which is the same as the formula (4) below) described in Non-Patent Document 2 to obtain the maximum stress σ max was calculated and this was taken as the bending strength.

number

[0068] For Examples 1 and 2 and Comparative Examples 1 and 2, the bending strength (maximum stress σ max ) was calculated for each of the 10 composite pieces 10c, and the average value was calculated.

[0069] [Break yield] The quality of the end faces of the composite pieces 10c was observed with an optical microscope, and if the length of the cracks occurring on all four end faces of the brittle material layer 1 was 50 μm or less, it was evaluated as "separable," and if a crack longer than 50 μm occurred on any end face, it was evaluated as "unseparable." For Examples 1 and 2 and Comparative Examples 1 and 2, the above evaluation was performed on 10 composite pieces 10c each, and the separation yield was calculated by the following formula (5). Breaking yield = Number of "breakable" composite pieces 10c / 10 x 100 = Number of “separable” composite pieces 10c × 10 [%] (5)

[0070] <Test Results> FIG. 6 is a diagram showing the test results for Examples 1 and 2 and Comparative Examples 1 and 2. As shown in FIG. 6, according to Examples 1 and 2, while maintaining the cutting yield at a value equivalent to that of Comparative Examples 1 and 2 (i.e., cracks are less likely to occur on the end surface of the brittle material layer 1 after cutting, similar to that of Comparative Examples 1 and 2), it was found that the bending strength of the composite piece 10c after cutting is higher than that of Comparative Examples 1 and 2. [Explanation of symbols]

[0071] 1...brittle material layer 2. Resin layer 10...Composite material 11. Scribe groove 20. Ultrashort pulse laser light source 30···Laser light source (CO2 laser light source) 23... Machining groove AF...Focus DL... Planned division line L1: Laser light L2: Laser light

Claims

1. A method for dividing a composite material in which a brittle material layer and a resin layer are laminated, comprising the steps of: a brittle material removing step of irradiating the brittle material layer with a laser beam emitted from an ultrashort pulse laser source along a planned dividing line of the composite material from the brittle material layer side to remove the brittle material that forms the brittle material layer, thereby forming a scribe groove that is integrally connected along the planned dividing line; a resin removing step of irradiating the resin layer with a laser light emitted from a laser light source along the planned dividing line to remove a resin forming the resin layer, In the brittle material removal step, a focus of the laser light emitted from the ultrashort pulse laser light source is set in the vicinity of the interface between the resin layer and the brittle material layer, and a laser light is emitted from the ultrashort pulse laser light source in a state where the thickness of the resin layer at an irradiation position of the laser light emitted from the ultrashort pulse laser light source is 5 μm or more, to form the scribe groove that opens on the resin layer side and does not penetrate the brittle material layer. How to separate composite materials.

2. The resin removing step is carried out after the brittle material removing step. A method for dividing a composite material according to claim 1.

3. Further comprising a composite material dividing step of dividing the composite material by applying an external force along the planned dividing line after the brittle material removing step and the resin removing step. A method for dividing a composite material according to claim 1 or 2.

4. The depth of the scribed groove is 3 μm or more and 50 μm or less. A method for dividing a composite material according to any one of claims 1 to 3.

5. The depth of the scribed groove is 20 μm or less. The method for dividing a composite material according to claim 4.

6. The depth of the scribe groove is 10% or more and 50% or less of the thickness of the brittle material layer. A method for dividing a composite material according to any one of claims 1 to 3.

7. The wavelength of the laser light emitted from the ultrashort pulse laser light source is 500 nm or more and 2500 nm or less. A method for dividing a composite material according to any one of claims 1 to 6.

8. The pulse width of the laser light emitted from the ultrashort pulse laser light source is 350 femtoseconds or more and 10,000 femtoseconds or less. A method for dividing a composite material according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • How to break a glass sheet

    JP1998506087A

  • Method for cutting stacked body

    JP2009280447A

  • Segmentation method of composite material

    JP2019122966A