Paper

Antiviral business card paper with integrated metal ions in cellulose fibers addresses the issue of mechanical deterioration and detachment, providing effective antiviral protection and stability.

JP7561105B2Active Publication Date: 2024-10-03NIPPON PAPER IND CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021141074
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-08-31
Publication Date
2024-10-03
Estimated Expiration
2041-08-31

AI Technical Summary

Technical Problem

Existing business card papers lack antiviral properties and suffer from mechanical property deterioration due to chemically bonded inorganic compounds containing metal components, which can detach, making them unsuitable for frequent hand-to-hand distribution.

Method used

Development of antiviral paper containing cellulose fibers with metal ions and/or particles, such as Ag, Au, Pt, Pd, Ni, Mn, Fe, Ti, Al, Zn, and Cu, integrated through ionic bonding, ensuring stability and functionality.

Benefits of technology

The paper exhibits excellent antiviral activity against influenza virus and feline calicivirus, maintaining mechanical properties and functionality, suitable for business cards and other applications requiring repeated handling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561105000001
    Figure 0007561105000001
Patent Text Reader

Abstract

To provide paper sheet that is supposed to be handed from person to person, especially business card paper sheet consisting of antiviral paper with excellent antiviral activity.SOLUTION: The present invention provides paper sheet having antiviral properties, and is particularly suitable for business card paper sheet. The paper sheet of the present invention has a paper thickness of 150 μm or more as measured according to JIS P 8118 and an antiviral activity value (Mv) of 2.0 or more against influenza virus or feline calicivirus as measured according to JIS L 1922:2016 (test method for antiviral properties of textile products).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to paper that is handed from person to person, and more specifically, to business card paper made of antiviral paper containing cellulose fibers. [Background technology]

[0002] In our daily lives, paper is commonly used as a handout, for example, for distributing advertisements in front of train stations or handing out business cards to people when meeting them for the first time. Generally, business cards are used with necessary information such as the name, organization, job title, telephone number, fax number, and email address printed on so-called business card size business card paper, and are often handed to the other person when meeting for the first time. However, recently, business cards have become indispensable for business activities of companies, and in order to leave a strong impression on the customer, business cards are being printed with not only traditional text but also full-color photos of the person, the company building, products, etc. Furthermore, many people create business cards with their own designs using home printers, and studies have been conducted on patterned paper for business cards, for example, as shown in Patent Document 1.

[0003] The paper that serves as the base material for business cards is produced using the various methods described above, and is expected to be handed from person to person and stored for long periods of time. Therefore, in addition to various printing suitabilities, the paper must also have a good feel in the hand and mechanical properties such as stiffness.

[0004] On the other hand, despite the growing awareness of hygiene in recent years, no research has been done into the antibacterial and antiviral properties of business card paper, even though it is intended to be handed over from person to person.

[0005] Various techniques have been proposed to impart antibacterial properties to paper, which is the base material for paper. For example, Patent Document 2 discloses a method of imparting antibacterial properties to paper by applying an aqueous solution of nanoparticle precursors containing a metal salt and a reducing agent to an aggregate of fibers. Patent Document 3 also proposes an inorganic porous crystal-hydrophilic polymer composite in which an aqueous solution of either a silicon compound or an aluminum compound, which is a component of zeolite, is impregnated into a hydrophilic polymer substrate such as cellulose fiber, and a basic substance and the other aqueous solution are mixed and further impregnated to support zeolite inside the cellulose fiber, and it is further disclosed that antibacterial and deodorizing effects can be imparted by supporting a metal on the zeolite.

[0006] Furthermore, Patent Document 4 discloses zinc compound-containing paper having excellent deodorizing and antibacterial properties, in which a metal complex of zinc and an aqueous solution of ammonia and / or ammonium salt is formed on the surface of a base paper.

[0007] Patent Document 5 discloses a paper base material for functional sheets having deodorizing properties, etc., which contains oxidized pulp and is characterized in that the amount of carboxyl groups in the oxidized pulp is 1.0 mmol / g to 2.0 mmol / g relative to the bone dry weight of the oxidized pulp. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2004-122404 A [Patent Document 2] Special Publication No. 2019-504941 [Patent Document 3] Japanese Patent Application Publication No. 10-120923 [Patent Document 4] Patent Publication No. 2021-042512 [Patent Document 5] International Publication No. 2014 / 097929 Summary of the Invention [Problem to be solved by the invention]

[0009] However, what is described in Patent Documents 2 and 3 is a simple mixture of cellulose fibers and inorganic compounds containing metal components, and the cellulose fibers and inorganic compounds containing metal components are not strongly chemically bonded to each other. In other words, inorganic compounds containing metal components do not form a physical or chemical network like fibers, so when functional paper is produced using them, the mechanical properties as a base material, such as tensile strength and tear strength, decrease, and the inorganic compounds containing metal components fall off from the base material, making it problematic for use as antibacterial and antiviral distribution paper, especially business cards. In addition, Patent Document 4 relates to an antibacterial treatment performed by directly treating the surface of paper with a metal. Furthermore, Patent Documents 2 to 4 all relate to paper with antibacterial properties, and are not related to antiviral properties. In view of these circumstances, the present invention aims to provide paper intended to be handed from person to person, in particular business card paper made of antiviral paper containing cellulose fibers and having excellent antiviral activity. [Means for solving the problem]

[0010] The present invention includes, but is not limited to, the following aspects. [1] A paper containing cellulose fibers and an adhesive, Paper thickness measured according to JIS P 8118 is 150 μm or more. Paper with an antiviral activity value (Mv) of 2.0 or higher against influenza virus and feline calicivirus, measured in accordance with JIS L 1922:2016 (antiviral test method for textile products). [2] The paper according to [1], wherein the cellulose fibers contain one or more metal ions and / or metal particles selected from the group consisting of Ag, Au, Pt, Pd, Ni, Mn, Fe, Ti, Al, Zn and Cu. [3] The paper according to [1] or [2], wherein the cellulose fibers include, as cellulose fibers having anionic groups, oxidized cellulose fibers having carboxyl groups or carboxylate groups; and / or carboxyalkylated cellulose fibers having carboxyalkyl groups. [4] The paper according to [3], wherein the amount of anionic groups in the cellulose fibers having anionic groups is 0.01 to 3.0 mmol / g. [5] The paper described in any of [1] to [4], wherein the cellulose fibers contain Cu and / or Ag as metal ions and / or metal particles, and the content of metal ions and / or metal particles in the paper is 0.20 mg or more and 6.3 mg / g or less. [6] The paper according to any one of [1] to [5], which contains 60% by weight or more of LBKP relative to 100% by weight of the cellulose fibers. [7] The paper according to any one of [1] to [6], having an Oken smoothness of 30 seconds or more as measured in accordance with JIS P 8155. [8] The paper according to any one of [1] to [7], wherein the paper is business card paper. Effect of the Invention

[0011] According to the present invention, it is possible to provide a business card paper made of antiviral paper that contains cellulose fibers and is intended to be handed from person to person, particularly an antiviral paper with excellent antiviral properties. According to the present invention, the functional components that contribute to the antiviral activity remain firmly in the business card paper, so that the functions such as the antiviral activity are fully exhibited. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The paper containing the cellulose fibers according to the present invention is a single-layer or multi-layer paper having antiviral properties, and is suitable for use as a business card. Specifically, the paper according to the present invention has an antiviral activity value (Mv) of 2.0 or more against influenza virus or feline calicivirus, measured based on JIS L 1922:2016 (antiviral test method for textile products), and more preferably has an antiviral activity value of 2.5 or more or 3.0 or more.

[0013] The antiviral paper of the present invention may have one or more other functions in addition to the antiviral properties and suitability for business cards. Examples of the functions of the antiviral paper of the present invention include deodorizing, antibacterial, heat resistance, moisture resistance, weather resistance, solvent resistance, abrasion resistance, and electromagnetic wave blocking, and in a preferred embodiment of the present invention, the antiviral paper has a deodorizing and / or antibacterial function.

[0014] The uses of the antiviral paper according to the present invention are not particularly limited, but it can be suitably used in applications that require antiviral function and sufficient paper thickness, and that are distributed from person to person or used repeatedly, such as business card paper, postcards, coasters, and packaging materials (paper containers, cardboard, wrapping paper, confectionery boxes, paper bags, etc.).

[0015] The antiviral paper according to the present invention may have a single-layer structure or a multilayer structure, but if it has a multilayer structure, at least one layer must contain cellulose fibers carrying metal ions and / or metal particles, which will be described later. Furthermore, cellulose fibers carrying metal ions and / or metal particles will exhibit excellent antiviral function regardless of which layer they are contained in, but because viruses generally adhere to the outermost layer of paper, from the viewpoint of efficiently exerting the antiviral function, it is preferable that cellulose fibers carrying metal ions and / or metal particles are contained in the outermost layer of the paper.

[0016] The paper according to the present invention contains cellulose fibers, and it is preferable that the cellulose fibers have anionic groups on the surface and contain one or more metal ions and / or metal particles selected from the group consisting of Ag, Au, Pt, Pd, Ni, Mn, Fe, Ti, Al, Zn and Cu. The anionic groups are preferably carboxyl groups or carboxylate groups, and the metal ions are preferably ionically bonded. In the present invention, it is preferable that the paper has at least one layer containing cellulose fibers carrying metal ions and / or metal particles (hereinafter also referred to as "metal-containing cellulose fibers"). From the viewpoints of high activity and safety, it is preferable that the metal ions contain Cu and / or Ag, and it is more preferable that the paper contains Cu. Ag and Cu are safer than Hg and the like, and can be used suitably for paper applications that are often directly touched by hands. In addition, Compared to Ag, Cu is known to be less susceptible to the effects of halogens, temperature, etc., and to exhibit its effects stably. Therefore, the paper of the present invention, which contains cellulose fibers carrying the metal of the present invention, particularly Cu ions and / or Cu particles, can be used in any environment or for any purpose.

[0017] The raw materials other than the metal-containing cellulose fibers are not particularly limited, and known raw materials can be used. For example, the raw materials may include one or more types of other materials such as cellulose fibers that do not support metal ions or metal particles (hereinafter also referred to as "general cellulose fibers"), synthetic fibers, resins, inorganic substances, etc. The paper of the present invention may contain a filler. The content of the filler in the paper is not particularly limited, but is preferably within a range not exceeding 20% ​​by weight of the paper weight, and may be 10% by weight or less, or 5% by weight or less. Examples of fillers include heavy calcium carbonate, light calcium carbonate, silica, diatomaceous earth, alumina, titanium oxide, magnesium oxide, pumice powder, pumice balloon, aluminum hydroxide, magnesium hydroxide, basic magnesium carbonate, dolomite, calcium sulfate, potassium titanate, barium sulfate, calcium sulfite, talc, clay, mica, asbestos, calcium silicate, montmorillonite, bentonite, graphite, aluminum powder, molybdenum sulfide, etc. Other materials are not particularly limited, but may include bulking agents, dry strength improvers, wet strength improvers, drainage improvers, retention improvers, dyes, sizing agents, aluminum sulfate, etc. The total content of materials other than the filler preferably does not exceed 10% by weight of the paper.

[0018] The method for producing the paper is not particularly limited, and any known method can be used. For example, any method may be used, including a method in which water in which the raw material is dispersed is discharged and then dehydrated by pressure or heat (so-called wet method), or a method in which the raw material is discharged in a dry state and then similarly formed into a sheet by pressure or heat (so-called dry method). Since cellulose fibers are hydrophilic, it is preferable to form the paper by the wet method. In the present invention, the metal-containing cellulose fibers can be mixed with a pulp slurry (paper material) in the same manner as in the case of ordinary paper, and the resulting sample can be used to make paper. For the papermaking, a known papermaking machine such as a Fourdrinier papermaking machine, a twin-wire papermaking machine, or a cylinder papermaking machine can be used, and the papermaking conditions are not limited. Furthermore, the paper according to the present invention may be subjected to a known surface treatment such as a calendar treatment, if necessary. Known treatment devices can be used for the surface treatment, and the conditions are not limited.

[0019] The paper of the present invention may be provided with a coating layer (clear coating layer) that does not contain a pigment on the surface of the paper as necessary. The paper of the present invention is preferably provided with a clear coating layer on one or both sides of the paper, and more preferably has a clear coating layer that contains at least starch. By having a clear coating layer, it is possible to obtain paper with excellent smoothness, surface strength, and printability. In addition, although the reason is not clear, the paper of the present invention has excellent antiviral activity and antibacterial and deodorizing functions even when the paper surface is covered with a clear coating layer.

[0020] The coating weight of the clear coating layer is 0.01 to 3.0 g / m2 in solids per side. 2 is preferable, and 0.1 to 2.0 g / m2 is more preferable. The clear coating can be formed by applying the coating liquid onto the paper using a coater (coating machine) such as a size press, a gate roll coater, a premetering size press, a curtain coater, or a spray coater. From the viewpoint of boiling and coating amount adjustment, the solid content concentration of the clear coating liquid is preferably 2 to 14 wt%, and the B type viscosity (30°C, 60 rpm) at a solid content concentration of 5 wt% is preferably 5 to 450 mPa s, and more preferably 10 to 300 mPa s.

[0021] In the present invention, starch refers to a mixture of amylose and amylopectin, and the mixing ratio generally varies depending on the plant that is the raw material of the starch. In the present invention, starches also include polymeric compounds derived from starch. Examples of the polymer include starch that has been modified, modified, or processed. Starches preferably include starches such as raw starch, oxidized starch, esterified starch, cationic starch, and self-modified starch produced by thermochemical or enzymatic modification in a paper mill using acetylated tapioca starch as a raw material, and modified starches such as aldehyde starch and hydroxyethylated starch. For the clear coating layer of the present invention, for example, cellulose derivatives such as carboxymethylcellulose, hydroxyethylcellulose, and methylcellulose, modified alcohols such as polyacrylamide, polyvinyl alcohol, carboxyl-modified polyvinyl alcohol, and acetoacetylated polyvinyl alcohol, styrene-butadiene copolymers, polyvinyl acetate, vinyl chloride-vinyl acetate copolymers, polyvinyl chloride, polyvinylidene chloride, and polyacrylic esters can also be used, and two or more of them may be used in combination. For the purpose of improving sizing properties, it is also possible to use in combination a surface sizing agent such as a styrene-based sizing agent, an olefin-based sizing agent, an acrylate-based sizing agent, a styrene-acrylic sizing agent, a cationic sizing agent, etc. In the present invention, various auxiliaries that are typically blended in clear coatings, such as dispersants, thickeners, water retention agents, defoamers, water resistance agents, colorants, conductive agents, etc., are appropriately used as necessary.

[0022] The basis weight of the paper according to the present invention is 100 to 300 g / m2, which can provide a sufficient texture and a luxurious feel when used as a card or business card. 2 The range is preferably 130 to 250 g / m 2 It is more preferable that the basis weight is in the range of 300 g / m 2 If it is larger, the paper becomes less flexible and easier to cut, which can cause problems. 2If it is smaller, the stiffness will be insufficient when used as a card or business card, giving the impression of being less luxurious, and the business card may become wrinkled when stored for a long period of time in a business card holder or case. When the paper has a multi-layer structure, it is preferable that the outermost base paper layer contains the metal ions and / or metal particles of the present invention. In addition, the basis weight of each layer is 10 g / m 2 This is preferable from the viewpoint of producing paper that is uniform and has a minimum level of strength when handled during production.

[0023] The thickness of the paper is preferably in the range of 150 to 500 μm from the viewpoint of the texture when used for business cards, etc., and the lower limit is more preferably 180 μm or more, and even more preferably 190 μm or more. The upper limit is more preferably 250 μm or less. If it is thinner than 150 μm, the stiffness, texture, strike-through, and luxurious feel may be inferior, and if it is thicker than 500 μm, problems may occur in the flexibility and cuttability of the paper, and when printed with a home inkjet printer. When the paper has a multi-layer structure, it is preferable that the thickness of each layer is 20 μm or more from the viewpoint of producing uniform paper. There is no particular limitation on the density of the paper.

[0024] It is preferable that the paper has a certain degree of sizing property in order to prevent feathering and print-through during inkjet printing. In addition, since a memo such as the date of receipt may be written on a business card, pen-writing size suitability is also required. Therefore, although the paper of the present invention is not particularly limited, it is preferable that the Stockigt sizing degree measured according to JIS P 8122 is 3 seconds or more, and the pen-writing size measured according to JAPAN TAPPI No. 12 is 4 or more.

[0025] The paper of the present invention has excellent smoothness, and therefore has excellent ink adhesion during printing and a good feel when touched. Therefore, although not particularly limited, the Oken smoothness measured in accordance with JIS P 8155 is preferably 30 seconds or more and 250 seconds or less, and more preferably 45 seconds or more and 200 seconds or less.

[0026] When the paper according to the present invention has a multi-layer structure, each layer may be produced one by one and then laminated by a known method, or each layer may be formed by sequentially laminating them. Alternatively, the paper may be produced by a so-called simultaneous multi-layer method in which the raw materials for each layer are simultaneously ejected and multiple layers are formed at once. There is no particular restriction on the method for bonding each layer, and known methods can be used. For example, a method using an adhesive, a method of passing between heated rolls, or a method of fusing the layers together by applying hot air can be mentioned. When the paper according to the present invention has a multi-layer structure, the outermost layer may be laminated with one or more layers, or may have an adhesive layer on the outermost layer for adhering to other substrates, as in the case of so-called adhesive label paper. It may also be a simple laminate of single-layer papers, or may have one or more layers with a three-dimensional structure, as in cardboard.

[0027] The paper according to the present invention may be printed on the outermost layer as necessary. The printing method is not particularly limited, but may be, for example, a gravure printing machine, an offset printing machine, an inkjet printing machine, a letterpress printing machine, a flexographic printing machine, a thermal transfer printing machine, or a toner printing machine. The gravure printing machine is a printing machine that transfers ink to a substrate via a roll-shaped plate cylinder on which an image is engraved, and is a printing machine that has been used conventionally. The offset printing machine is a printing machine that transfers ink to a substrate once on a blanket and then transfers it again. The letterpress printing machine is a letterpress printing machine that applies pressure to the ink applied to the relief plate to press it against the substrate. The flexographic printing machine is a letterpress printing machine that uses a flexible, elastic resin plate. The thermal transfer printing machine is a printing machine that uses ink ribbons of each color and transfers color materials from the ink ribbon to the substrate by heat. A toner printer is an electrophotographic printer that transfers toner attached to a charged drum to a print medium using static electricity. The paper of the present invention has excellent printability and is therefore suitable for business cards.

[0028] When the paper according to the present invention contains cellulose fibers carrying metal ions and / or metal particles, the total amount of metal ions and particles per gram of paper is preferably 0.20 mg / g or more, more preferably 0.25 mg / g or more, even more preferably 0.30 mg / g or more, and most preferably 0.60 mg / g or more, and preferably 6.3 mg / g or less, and may be 5.0 mg / g or less, or 4.0 mg / g or less. By setting the total content of metal ions and / or metal particles in paper to between 0.20 mg / g and 6.3 mg / g per gram of paper, it is possible to easily obtain paper with excellent antiviral properties, while also suppressing the increased environmental burden and discoloration of the paper caused by excess metal ions and / or metal particles.

[0029] The content of metal ions and metal particles in paper can be measured (quantified) by, for example, inductively coupled plasma optical emission spectrometry (ICP-OES).

[0030] The content of the metal-containing cellulose fibers is preferably 0.5% by weight or more relative to the paper. If the content of the metal-containing cellulose fibers is too low, sufficient antiviral function may not be imparted. The upper limit of the content is not particularly limited and can be appropriately adjusted depending on the desired level of antiviral, deodorizing, antibacterial, etc., but may be 100% by weight. The content of the metal-containing cellulose fibers may be, for example, 1 to 80% by weight, 2 to 60% by weight, 3 to 40% by weight, etc. As described above, since the content of metal-containing cellulose fibers is preferably 0.5% by weight or more of the paper, the content of general cellulose fibers in the paper is preferably 99.5% by weight or less. There is no particular lower limit for the content of general cellulose fibers, and the paper does not necessarily need to contain general cellulose fibers.

[0031] The paper according to the present invention comprises cellulose fibers. The type of cellulose fibers in the present invention is not particularly limited, and any type can be used as necessary. Two or more types of cellulose fibers may be mixed in any ratio. The origin of the cellulose fibers is not particularly limited, and examples include cellulose fibers derived from plants, animals, algae, and microorganisms. Among these, cellulose fibers derived from plants or microorganisms are preferred, and cellulose fibers derived from plants are particularly preferred. Examples of cellulose fibers derived from plants include wood, bamboo, hemp, jute, kenaf, agricultural waste, and pulp (softwood unbleached kraft pulp (NUKP), softwood bleached kraft pulp (NBKP), hardwood unbleached kraft pulp (LUKP), hardwood bleached kraft pulp (LBKP), softwood unbleached sulfite pulp (NUSP), softwood bleached sulfite pulp (NBSP), thermomechanical pulp (TMP), recycled pulp, and waste paper pulp). Examples of cellulose fibers derived from animals include cellulose fibers derived from ascidians, and examples of cellulose fibers derived from microorganisms include cellulose fibers derived from acetic acid bacteria (Acetobacter).

[0032] The number average fiber diameter and number average fiber length of the cellulose raw material used in the present invention are not particularly limited, and any number average fiber diameter and number average fiber length can be used as necessary. Two or more types of cellulose fibers having different number average fiber diameters and number average fiber lengths may be mixed in any ratio. For example, in the case of softwood kraft pulp (NBKP), which is one of the common pulps, the number average fiber diameter is about 30 to 60 μm and the number average fiber length is about 3 to 5 mm, and in the case of hardwood bleached kraft pulp (LBKP), the number average fiber diameter is about 10 to 30 μm and the number average fiber length is about 1 to 2 mm.

[0033] The paper of the present invention preferably contains LBKP and / or recycled paper pulp as cellulose fibers. LBKP and recycled paper pulp have relatively short fiber length, and by containing these pulps, paper with excellent smoothness can be obtained, and the paper thus obtained is excellent in surface properties and printability (especially printed surface feel). It is particularly preferable to contain 60% by weight or more of LBKP, which has excellent whiteness.

[0034] [Modification of cellulose fibers] Cellulose fibers have three hydroxyl groups per glucose unit and can be subjected to various chemical modification treatments. In the present invention, it is preferable to carry out a chemical modification treatment having an anionic group after the treatment. Examples of cellulose fibers into which anionic groups have been introduced include oxidized cellulose fibers having carboxyl groups or carboxylate groups, phosphoric acid esterified cellulose fibers having phosphoric acid groups, phosphite esterified cellulose fibers having phosphoric acid groups, and sulfonated cellulose fibers having sulfate groups. In the present invention, in order to introduce metal ions or metal particles into at least a portion of the cellulose fibers in a step described below, it is preferable to carry out modification (oxidation) to introduce carboxyl groups or carboxylate groups into at least a portion of the cellulose fibers. In this specification, the anionic groups introduced into the cellulose fibers are sometimes referred to as acid groups.

[0035] Here, the carboxyl group refers to a group represented by -COOH, and the carboxylate group refers to a group represented by -COO-. The counter ion of the carboxylate group is not particularly limited. As described below, when a metal particle is formed through an ionic bond with the carboxylate group, this metal ion becomes the counter.

[0036] The amount of anionic groups in cellulose fibers having anionic groups (acid groups) can be measured, for example, by the following method. 60 ml of a 0.5% by mass slurry (aqueous dispersion) of a cellulose fiber sample having anionic groups (acid groups) is prepared, and a 0.1 M aqueous hydrochloric acid solution is added to adjust the pH to 2.5. A 0.05 N aqueous sodium hydroxide solution is then added dropwise to measure the electrical conductivity until the pH reaches 11, and the amount of sodium hydroxide (a) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity is gradual, is measured. The amount of anionic groups [mmol / g] of the cellulose fiber having anionic groups (acid groups) is then calculated using the following formula. In the formula, x is a value corresponding to the valence of the acid group, which is 1 for carboxyl groups, carboxylate groups, phosphorous groups, and sulfonic acid groups, and 2 for phosphate groups. a [ml] x 0.05 / weight of cellulose fiber having anionic groups (acid groups) [g] / x

[0037] In the case of carboxyalkylated cellulose fibers having carboxyalkyl groups, the amount of anionic groups resulting from the carboxyalkylation treatment can be quantified by the following method. (1) Accurately weigh out approximately 2.0 g of carboxymethyl cellulose (bone dry) and place it in a 300 mL Erlenmeyer flask equipped with a stopper. (2) Add 100 mL of concentrated nitric acid to 1,000 mL of methanol, add 100 mL of the resulting nitric acid-methanol solution, and shake for 3 hours to convert the carboxymethylcellulose salt (carboxymethylated cellulose) into hydrogen-type carboxymethyl cellulose. (3) Accurately weigh out 1.5 to 2.0 g of hydrogen-type carboxymethyl cellulose (bone dry) and place it in a 300 mL Erlenmeyer flask equipped with a stopper. (4) Wet the hydrogen-form carboxymethyl cellulose with 15 mL of 80% methanol, add 100 mL of 0.1 N NaOH, and shake at room temperature for 3 hours. (5) Back-titrate excess NaOH with 0.1N H2SO4 using phenolphthalein as an indicator. (6) Calculate the degree of carboxyalkyl substitution (DS) according to the following formula: A = [(100 × F'-(0.1N H2SO4) (mL) × F) × 0.1] / (bone-dry mass of hydrogen-type carboxyalkylated cellulose (g)) DS = 0.162 x A / (1-0.058 x A) A: The amount of 1N NaOH required to neutralize 1 g of hydrogen-type carboxyalkylated cellulose (mL) F': factor of 0.1N NaOH F: Factor of 0.1N H2SO4

[0038] A method for introducing anionic groups into glucose units on the surface of cellulose fibers will be described below.

[0039] (1-1) Oxidation In the present invention, the method of modification (oxidation) to introduce carboxyl groups or carboxylate groups into cellulose fibers is not particularly limited as long as the cellulose fibers after modification contain carboxyl groups or carboxylate groups, and any known method can be used. One example is a method in which a cellulose raw material is oxidized in water using an oxidizing agent in the presence of a substance selected from the group consisting of an N-oxyl compound, and a bromide, an iodide, or a mixture thereof. According to this method, the primary hydroxyl group at the C6 position of the glucopyranose ring on the cellulose surface is selectively oxidized to generate a group selected from the group consisting of an aldehyde group, a carboxyl group, and a carboxylate group. The concentration of the cellulose raw material during the reaction is not particularly limited, but is preferably 5% by weight or less.

[0040] The term "N-oxyl compound" refers to a compound that can generate a nitroxy radical. An example of a nitroxy radical is 2,2,6,6-tetramethylpiperidine 1-oxyl (TEMPO). Any compound that can promote the desired oxidation reaction can be used as the N-oxyl compound.

[0041] The amount of the N-oxyl compound used is not particularly limited as long as it is a catalytic amount capable of oxidizing cellulose fibers. For example, it is preferably 0.01 mmol or more, more preferably 0.02 mmol or more, per 1 g of bone-dry cellulose. The upper limit is preferably 10 mmol or less, more preferably 1 mmol or less, and even more preferably 0.5 mmol or less. Therefore, the amount of the N-oxyl compound used is preferably 0.01 to 10 mmol, more preferably 0.01 to 1 mmol, and even more preferably 0.02 to 0.5 mmol, per 1 g of bone-dry cellulose.

[0042] Bromides are compounds containing bromine, such as alkali metal bromides that can be dissociated and ionized in water, such as sodium bromide. Iodides are compounds containing iodine, such as alkali metal iodides. The amount of bromide or iodide used may be selected within a range that can promote the oxidation reaction. The total amount of bromide and iodide is preferably 0.1 mmol or more, more preferably 0.5 mmol or more, per 1 g of bone dry cellulose. The upper limit is preferably 100 mmol or less, more preferably 10 mmol or less, and even more preferably 5 mmol or less. Therefore, the total amount of bromide and iodide is preferably 0.1 to 100 mmol, more preferably 0.1 to 10 mmol, and even more preferably 0.5 to 5 mmol, per 1 g of bone dry cellulose.

[0043] The oxidizing agent is not particularly limited, but examples thereof include halogens, hypohalous acids, halous acids, perhalogen acids, salts thereof, halogen oxides, peroxides, etc. Among them, hypohalous acids or salts thereof are preferred, hypochlorous acid or salts thereof are more preferred, and sodium hypochlorite is even more preferred, because they are inexpensive and have a low environmental impact.

[0044] The amount of the oxidizing agent used is preferably 0.5 mmol or more, more preferably 1 mmol or more, and even more preferably 3 mmol or more, per 1 g of bone-dry cellulose. The upper limit is preferably 500 mmol or less, more preferably 50 mmol or less, and even more preferably 25 mmol or less. Therefore, the amount of the oxidizing agent used is preferably 0.5 to 500 mmol, more preferably 0.5 to 50 mmol, more preferably 1 to 25 mmol, and most preferably 3 to 10 mmol, per 1 g of bone-dry cellulose.

[0045] When an N-oxyl compound is used, the amount of the oxidizing agent used is preferably 1 mol or more per mol of the N-oxyl compound. The upper limit is preferably 40 mol. Therefore, the amount of the oxidizing agent used is preferably 1 to 40 mol per mol of the N-oxyl compound.

[0046] Conditions such as pH and temperature during the oxidation reaction are not particularly limited, and generally, the oxidation reaction proceeds efficiently even under relatively mild conditions. The reaction temperature is preferably 4°C or higher, more preferably 15°C or higher. The upper limit is preferably 40°C or lower, more preferably 30°C or lower. Therefore, the temperature is preferably 4 to 40°C, and may be about 15 to 30°C, that is, room temperature.

[0047] The pH of the reaction solution is preferably at least 8, and more preferably at least 10. The upper limit is preferably not more than 12, and more preferably not more than 11. Therefore, the pH of the reaction solution is preferably 8 to 12, and more preferably about 10 to 11. Usually, as the oxidation reaction proceeds, carboxyl groups are generated in the cellulose, so the pH of the reaction solution tends to decrease. Therefore, in order to efficiently proceed with the oxidation reaction, it is preferable to add an alkaline solution such as an aqueous sodium hydroxide solution to maintain the pH of the reaction solution within the above range. The reaction medium during oxidation is preferably water, because it is easy to handle and does not easily cause side reactions.

[0048] The reaction time in the oxidation can be appropriately set according to the degree of progress of the oxidation, and is usually 0.5 hours or more. The upper limit is usually 6 hours or less, preferably 4 hours or less. Therefore, the reaction time in the oxidation is usually 0.5 to 6 hours, for example, about 0.5 to 4 hours.

[0049] The oxidation may be carried out in two or more separate reaction stages. For example, the oxidized cellulose obtained by filtering after the completion of the first reaction stage can be oxidized again under the same or different reaction conditions, allowing efficient oxidation without reaction inhibition by table salt produced as a by-product in the first reaction stage.

[0050] Another example of a modification (oxidation) method for introducing a carboxyl group or a carboxylate group is a method of oxidation by ozone treatment, in which at least the hydroxyl groups at positions 2 and 6 of the glucopyranose ring constituting cellulose are oxidized and the cellulose chain is decomposed.

[0051] Ozone treatment is usually carried out by contacting the cellulose raw material with a gas containing ozone. The ozone concentration in the gas is 50 g / m 3 The upper limit is 250 g / m 3 It is preferable that the thickness is less than 220 g / m 3 It is more preferable that the ozone concentration in the gas is 50 to 250 g / m or less. 3 It is preferable that the thickness is 50 to 220 g / m 3 It is more preferable that:

[0052] The amount of ozone added is preferably 0.1 parts by weight or more, and more preferably 5 parts by weight or more, based on 100% by weight of the solid content of the cellulose raw material. The upper limit is usually 30% by weight or less. Therefore, the amount of ozone added is preferably 0.1 to 30% by weight, and more preferably 5 to 30% by weight, based on 100% by weight of the solid content of the cellulose raw material.

[0053] The ozone treatment temperature is usually 0°C or higher, and preferably 20°C or higher. The upper limit is usually 50°C or lower. Therefore, the ozone treatment temperature is preferably 0 to 50°C, and more preferably 20 to 50°C. The ozone treatment time is usually 1 minute or more, and preferably 30 minutes or more. The upper limit is usually 360 minutes or less. Therefore, the ozone treatment time is usually about 1 to 360 minutes, and preferably about 30 to 360 minutes. When the ozone treatment conditions are within the above-mentioned ranges, excessive oxidation and decomposition of cellulose can be prevented, and the yield of oxidized cellulose is good.

[0054] The resultant product obtained after the ozone treatment may be further subjected to a post-oxidation treatment using an oxidizing agent. The oxidizing agent used in the post-oxidation treatment is not particularly limited, but examples thereof include chlorine compounds such as chlorine dioxide and sodium chlorite; oxygen, hydrogen peroxide, persulfuric acid, and peracetic acid. Examples of the method of the post-oxidation treatment include a method in which the oxidizing agent is dissolved in a polar organic solvent such as water or alcohol to prepare an oxidizing agent solution, and the cellulose raw material is immersed in the oxidizing agent solution.

[0055] The amount of anionic groups in oxidized cellulose fibers having carboxyl or carboxylate groups is preferably 0.01 to 3.0 mmol / g, and more preferably 0.20 to 2.2 mmol / g. If the amount of anionic groups is less than 0.01 mmol / g, the amount of metal particles present on the surface of the cellulose fibers may be insufficient in the step of supporting metal ions or metal particles on the cellulose fibers described below, and antiviral, deodorizing, and antibacterial functions may be poor. On the other hand, if the amount of anionic groups exceeds 3.0 mmol / g, aggregation of the metal particles may occur, and antiviral, deodorizing, and antibacterial functions may be poor, and cellulose cleavage may occur more easily as a side reaction during the oxidation reaction, resulting in a reduced yield. The amount of anionic groups (carboxyl groups, carboxylate groups) contained in the oxidized cellulose fibers can be adjusted by controlling the oxidation conditions, such as the amount of oxidizing agent added and the reaction time.

[0056] (1-2) Etherification Regarding etherification, any method may be used as long as it contains a carboxyl group or a carboxylate group in the functional group after the reaction in order to introduce metal ions into the cellulose fiber in a later step, and a known method can be used. Examples include carboxyalkyl etherification such as carboxymethyl (etherification), carboxyethyl (etherification), carboxypropyl (etherification), and carboxybutyl (etherification), and carboxyphenyl (etherification). As an example of one of these, the carboxymethylation method will be described below.

[0057] The method of carboxymethylation is not particularly limited, and known methods can be used. For example, a method of mercerizing the cellulose raw material as the starting raw material and then etherifying it can be used. A common solvent is used during the carboxymethylation reaction. Examples of the solvent include water, alcohol (e.g., lower alcohol), and mixed solvents thereof. Examples of the lower alcohol include methanol, ethanol, N-propyl alcohol, isopropyl alcohol, N-butanol, isobutanol, and tertiary butanol.

[0058] The mixing ratio of the lower alcohol in the mixed solvent is usually 60% by weight or more or 95% by weight or less, and preferably 60 to 95% by weight. The amount of the solvent is usually 3 times by weight relative to the cellulose raw material. The upper limit is not particularly limited, but is 20 times by weight. Therefore, the amount of the solvent is preferably 3 to 20 times by weight.

[0059] Mercerization is usually carried out by mixing the bottom raw material with a mercerizing agent. Examples of the mercerizing agent include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide. The amount of the mercerizing agent used is preferably 0.5 times mol or more, more preferably 1.0 times mol or more, and even more preferably 1.5 times mol or more per anhydrous glucose residue of the bottom raw material. The upper limit is usually 20 times mol or less, preferably 10 times mol or less, and more preferably 5 times mol or less, and therefore, 0.5 to 20 times mol is preferable, 1.0 to 10 times mol is more preferable, and 1.5 to 5 times mol is even more preferable.

[0060] The reaction temperature for mercerization is usually 0°C or higher, preferably 10°C or higher. The upper limit is usually 70°C or lower, preferably 60°C or lower. Therefore, the reaction temperature is usually 0 to 70°C, preferably 10 to 60°C. The reaction time is usually 15 minutes or more, preferably 30 minutes or more. The upper limit is usually 8 hours or less, preferably 7 hours or less. Therefore, it is usually 15 minutes to 8 hours, preferably 30 minutes to 7 hours.

[0061] The etherification reaction is usually carried out by adding a carboxymethylating agent to the reaction system after mercerization. An example of the carboxymethylating agent is sodium monochloroacetate. The amount of the carboxymethylating agent added is usually preferably 0.05 times mol or more, more preferably 0.5 times mol or more, and even more preferably 0.8 times mol or more per glucose residue of the cellulose raw material. The upper limit is usually 10.0 times mol or less, preferably 5 times mol or less, and more preferably 3 times mol or less, and therefore preferably 0.05 to 10.0 times mol, more preferably 0.5 to 5 times mol, and even more preferably 0.8 to 3 times mol.

[0062] The reaction temperature is usually 30°C or higher, preferably 40°C or higher, and the upper limit is usually 90°C or lower, preferably 80°C or lower. Therefore, the reaction temperature is usually 30 to 90°C, preferably 40 to 80°C. The reaction time is usually 30 minutes or more, preferably 1 hour or more. The upper limit is usually 10 hours or less, preferably 4 hours or less. Therefore, the reaction time is usually 30 minutes to 10 hours, preferably 1 hour to 4 hours. The reaction liquid may be stirred during the carboxymethylation reaction as necessary.

[0063] When the cellulose raw material is modified by carboxymethylation, the degree of carboxymethyl substitution per anhydroglucose unit in the obtained carboxymethylated cellulose fiber is preferably 0.01 or more, more preferably 0.05 or more, and even more preferably 0.10 or more. The upper limit is preferably 0.50 or less, more preferably 0.40 or less, and even more preferably 0.35 or less. Therefore, the degree of carboxymethyl substitution is preferably 0.01 to 0.50, more preferably 0.05 to 0.40, and even more preferably 0.10 to 0.30.

[0064] (1-3) Esterification In the present invention, any method for modifying (esterifying) cellulose fibers to introduce phosphate groups and phosphite groups may be used, and any known method can be used.

[0065] The phosphated cellulose fibers having a phosphate group and the phosphite cellulose fibers having a phosphite group are cellulose fibers esterified with a compound having a phosphate group or a phosphite group. Examples of the compound having a phosphate group or a phosphite group include phosphoric acid, polyphosphoric acid, phosphorous acid, phosphonic acid, polyphosphonic acid, and esters and salts thereof. These compounds are low cost and easy to handle.

[0066] Specific examples of compounds having a phosphate group or a phosphite group include phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, sodium pyrophosphate, sodium metaphosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, tripotassium phosphate, potassium pyrophosphate, potassium metaphosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, ammonium pyrophosphate, ammonium metaphosphate, phosphorous acid, sodium hydrogen phosphite, ammonium hydrogen phosphite, potassium hydrogen phosphite, sodium dihydrogen phosphite, sodium phosphite, lithium phosphite, potassium phosphite, magnesium phosphite, calcium phosphite, triethyl phosphite, triphenyl phosphite, and pyrophosphorous acid. Among these, phosphoric acid, sodium salt of phosphoric acid, potassium salt of phosphoric acid, ammonium salt of phosphoric acid, phosphorous acid, sodium salt of phosphorous acid, potassium salt of phosphorous acid, and ammonium salt of phosphorous acid are preferred, and sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium hydrogen phosphite, and sodium dihydrogen phosphite are more preferred, because they have high esterification efficiency and are easily applicable industrially. Compounds having a phosphoric acid group or a phosphorous group may be used alone or in combination of two or more.

[0067] The esterification reaction is carried out, for example, by reacting a cellulose raw material with a compound having a phosphate group or a phosphite group. Examples of a method for reacting a cellulose raw material with a compound having a phosphate group or a phosphite group include a method of mixing a powder or an aqueous solution of the compound having a phosphate group or a phosphite group with the cellulose raw material, and a method of adding an aqueous solution of the compound having a phosphate group or a phosphite group to a slurry of the cellulose raw material. Among these, the method of mixing an aqueous solution of a compound having a phosphate group or a phosphite group with a cellulose raw material or a slurry thereof is preferred because it increases the uniformity of the reaction and the efficiency of esterification. The pH of the aqueous solution of the compound having a phosphate group or a phosphite group is preferably 7 or less from the viewpoint of increasing the efficiency of introducing the phosphate group or the phosphite group, and more preferably 3 to 7 from the viewpoint of suppressing hydrolysis.

[0068] The lower limit of the amount of the compound having a phosphate group or a phosphite group added is preferably 0.2 parts by weight or more, more preferably 1 part by weight or more, calculated as phosphorus atoms, per 100 parts by weight of the cellulose raw material. This range tends to improve the yield of phosphated cellulose fibers and phosphited cellulose fibers. On the other hand, the upper limit is preferably 500 parts by weight or less, more preferably 400 parts by weight or less. This range allows efficient production at a yield commensurate with the amount of the compound having a phosphate group or a phosphite group added.

[0069] When reacting the cellulose raw material with a compound having a phosphate group or a phosphite group, a basic compound may be further added to the reaction system. Examples of methods for adding the basic compound to the reaction system include a method of adding the basic compound to a slurry of the cellulose raw material, a method of adding the basic compound to an aqueous solution of a compound having a phosphate group or a phosphite group, or a method of adding the basic compound to a slurry of the cellulose raw material and a compound having a phosphate group or a phosphite group. The basic compound is not particularly limited, but a nitrogen-containing compound that exhibits basicity is preferable. Note that "exhibiting basicity" usually means that an aqueous solution of the basic compound exhibits a pink to red color in the presence of a phenolphthalein indicator, or that the pH of the aqueous solution of the basic compound is greater than 7.

[0070] The nitrogen-containing compound exhibiting basicity is not particularly limited as long as it can achieve the effects of the present invention. Among them, compounds having an amino group are preferred. For example, urea, methylamine, ethylamine, trimethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, pyridine, ethylenediamine, and hexamethylenediamine can be mentioned. Among them, urea is preferred because it is low-cost and easy to handle.

[0071] The amount of the basic compound added is preferably 2 to 1000 parts by weight, and more preferably 100 to 700 parts by weight. The reaction temperature is preferably 0 to 95°C, and more preferably 30 to 90°C. The reaction time is not particularly limited, but is usually about 1 to 600 minutes, and preferably 30 to 480 minutes. When the reaction conditions are within any of these ranges, it is possible to prevent cellulose from being easily dissolved due to excessive introduction of phosphate groups and phosphite groups into the cellulose, and the yield of phosphated cellulose fibers and phosphite cellulose fibers is likely to be improved.

[0072] After reacting the cellulose raw material with a compound having a phosphate group or a phosphite group, a suspension is usually obtained. The suspension is dehydrated as necessary, and it is preferable to carry out a heat treatment after dehydration. This makes it possible to suppress hydrolysis of the cellulose raw material. The heating temperature is preferably 100 to 170°C, and it is more preferable to heat the cellulose raw material at 130°C or less (more preferably 110°C or less) while water is contained during the heat treatment, and then heat the cellulose raw material at 100 to 170°C after removing the water.

[0073] It is preferable that the phosphated cellulose fibers and the phosphite cellulose fibers are subjected to a washing treatment such as boiling and then washing with cold water.

[0074] In the phosphated cellulose fibers and phosphited cellulose fibers, the anion group (phosphate group, phosphite group) contained in the phosphated cellulose fibers and phosphited cellulose fibers is preferably 0.1 to 3.5 mmol / g.

[0075] (1-4) Sulfonation Sulfonated cellulose fibers are cellulose fibers that have been sulfonated with a compound having a sulfate group. Examples of compounds having a sulfate group include sulfuric acid, sulfamic acid, chlorosulfonic acid, sulfur trioxide, and esters and salts thereof. These compounds are low cost and easy to handle.

[0076] In the present invention, sulfamic acid is preferably used. Sulfamic acid not only has a lower solubility for cellulose than sulfuric anhydride or an aqueous sulfuric acid solution, but also has a low acidity, making it possible to maintain the degree of polymerization. In addition, there are no restrictions on the handling of sulfuric anhydride or an aqueous sulfuric acid solution, which are highly acidic and corrosive, and sulfamic acid is not designated as a specific substance under the Air Pollution Control Law, so that it has a small impact on the environment.

[0077] The amount of sulfamic acid used can be appropriately adjusted taking into consideration the amount of anion groups (sulfate groups) introduced into the cellulose fiber. For example, sulfamic acid can be used in an amount of preferably 0.01 to 50 mol, more preferably 0.1 to 30 mol, per mol of glucose unit in the cellulose molecule.

[0078] [Supporting metal ions and / or metal particles on cellulose fibers] In the present invention, excellent antiviral, deodorizing and antibacterial functions are exhibited by further containing metal ions and / or metal particles of one or more metal elements selected from the group consisting of Ag, Au, Pt, Pd, Ni, Mn, Fe, Ti, Al, Zn and Cu in cellulose fibers containing anionic groups, particularly carboxyl groups or carboxylate groups. Among these, the use of one or more ions selected from the group consisting of Ag and Cu is preferred because it further improves the antiviral, deodorizing and antibacterial functions, and Cu ions and / or metal particles are more preferred. Cellulose fibers having anionic groups have metal ions or metal particles chemically bonded to the cellulose fibers. This means that when the fibers are incorporated into paper, the metal components are less likely to be detached from the paper. The fibers also have good mechanical properties such as tensile strength, meaning that there is no decrease in performance or strength.

[0079] The method for supporting the metal ions on the cellulose fibers is not particularly limited, and may involve, for example, mixing a previously prepared dispersion of cellulose fibers with an aqueous solution of a metal compound, or applying a dispersion containing cellulose fibers onto a substrate to form a membrane, and then dripping an aqueous solution of a metal compound onto the membrane to impregnate it. At this time, the membrane may remain fixed on the substrate, or may be peeled off from the substrate. Although the detailed mechanism is unclear, it is speculated that these methods allow metal ions derived from metal compounds to form ionic bonds or coordinate with sodium ions that are already ionically bonded to anionic groups such as carboxylate groups through counterion exchange, thereby adding metal ions to cellulose fibers. This counterion exchange is thought to occur due to the difference in ionization tendency between metal ions.

[0080] The aqueous metal compound solution herein refers to an aqueous solution of a metal salt. Examples of the metal salt include complexes (complex ions), halides, nitrates, sulfates, and acetates.

[0081] The concentration of the aqueous metal compound solution is not particularly limited, but is preferably 0.2 to 2.2 mmol, more preferably 0.4 to 1.8 mmol, per 1 g of cellulose fiber. The time for contacting the metal compound may be appropriately adjusted.

[0082] The temperature during contact with the metal compound is not particularly limited, but is preferably in the range of 2 to 50° C. Furthermore, the pH of the liquid during contact is not particularly limited, but since a low pH makes it difficult for metal ions to bind to carboxyl groups, it is preferably in the range of 7 to 13, and particularly preferably in the range of 8 to 12.

[0083] In the present invention, the effect is achieved by introducing metal ions into the cellulose fibers as described above, but some of the metal ions may be reduced to form metal particles. If necessary, it is also possible to partially form metal particles on the surface of the cellulose fibers by reducing some of the metal ions bound to the obtained metal ion-containing cellulose fibers by adding a reducing agent or the like. However, it is preferable from the viewpoint of antiviral, antibacterial, and deodorizing functions to use the entire amount of the metal compound as metal ions without carrying out any special reduction treatment.

[0084] The mechanism by which metal particles are generated in the cellulose fibers by reducing the metal compound in the metal-containing cellulose fibers obtained above is not clear, but is presumed to be as follows. The metal compound or ions derived from the metal compound in the metal compound-containing cellulose fibers are reduced to metal by the reduction reaction. At this time, the generated metal is supported on the surface of the cellulose fibers. Metals generated in the same manner and adjacent to each other are integrated to form particles. Meanwhile, metal compounds and the like that exist in the vicinity of the cellulose fibers but are not bonded to the cellulose fibers are also reduced to generate metal. This metal quickly integrates with the metal on the surface of the cellulose fibers to form metal particles.

[0085] The reduction reaction may be carried out by a known method, but is preferably carried out while reducing the metal compound without cleaving the bond between the metal compound and the cellulose fiber. Examples of such reduction methods include a gas phase reduction method using hydrogen and a liquid phase reduction method using a reducing agent such as an aqueous solution of sodium borohydride. The conditions for the gas phase reduction, such as time and temperature, may be appropriately adjusted, but for example, the reaction may be carried out at 50 to 60°C for about 1 to 3 hours. The gas phase reduction reaction is preferably carried out in a state in which the oxidized cellulose fibers do not contain water or solvent. In the reduction reaction, the membrane may remain fixed on the substrate, or may be peeled off from the substrate. In the case of liquid phase reduction, a membrane is obtained from the above dispersion, and this can be subjected to the reduction reaction with or without drying. The dispersion can also be subjected to the liquid phase reduction reaction without drying. The reaction temperature in the liquid phase reduction is preferably 4 to 40°C, more preferably room temperature.

[0086] The average particle size of the metal particles is determined from a transmission electron microscope image or X-ray diffraction. In the present invention, the average particle size of the metal particles is preferably in the range of 1 to 50 nm when determined from a transmission electron microscope image. Specifically, a method for determining the average particle size from a transmission electron microscope image includes a method of preparing a transmission electron microscope image of cellulose fibers, determining the circle equivalent diameters of primary particles of a plurality of metal particles from the image, and averaging these values.

[0087] The presence of metal ions and / or metal particles in cellulose fibers can be confirmed by scanning electron microscope images and ICP emission spectroscopy of the extract with strong acid. In other words, the presence of metal ions cannot be confirmed by scanning electron microscope images, while the presence of metals can be confirmed by ICP emission spectroscopy. In contrast, for example, when the above-mentioned metals are reduced from ions and exist as metal particles, the metal particles can be confirmed by scanning electron microscope images, so the presence or absence of metal ions can be determined. In addition, the presence or absence of metal ions can also be determined by scanning electron microscope images and element mapping. In other words, the presence of metal ions cannot be confirmed by scanning electron microscope images, but the presence of metal ions can be confirmed by element mapping.

[0088] In the step of supporting the metal ions or metal particles, the total content of the metal ions and / or metal particles relative to the cellulose fibers is preferably in the range of 10 to 100 mg / g, more preferably in the range of 15 to 80 mg / g, and particularly preferably in the range of 20 to 60 mg / g. If the total content is less than 10 mg / g, the antiviral, deodorizing, and antibacterial functions may be deteriorated. On the other hand, if the total content exceeds 100 mg / g, the metal ions may be easily eluted during production, which may increase the load on wastewater treatment.

[0089] [Beating] The cellulose fibers in the present invention may be beaten at least once between the time before the modification treatment and the time after the metal loading treatment, but it is preferable to perform the beating treatment before the metal loading treatment, since the fibers can be efficiently fibrillated without agglomeration. The beating treatment here refers to a treatment that applies a mechanical shear force to the fibers. The beating treatment fibrillates a part of the cellulose fibers, increasing the surface area, and generally strengthens the interfiber bond during drying. In the present invention, the beating treatment, particularly for metal-containing cellulose fibers, can further enhance the antiviral, deodorizing, and antibacterial effects after loading metal ions and / or metal particles. On the other hand, excessive beating treatment and excessive fineness of cellulose fibers is not preferable because it reduces the yield when blended with pulp for papermaking, or the fibers do not remain in the paper, resulting in reduced antiviral, deodorizing, and antibacterial functions. Canadian Standard Freeness (CSF) can be used as an index of the degree of beating. Specifically, if the CSF is less than 30 ml, the antiviral, deodorizing, and antibacterial functions are reduced due to reduced paper retention, and if the CSF is more than 600 ml, fibrillation is insufficient, resulting in reduced antiviral, deodorizing, and antibacterial functions. In this way, by setting the freeness (CSF) of cellulose fibers to 30 to 600 ml, the antiviral, deodorizing, and antibacterial functions are improved.

[0090] The apparatus used for beating is not particularly limited, and any known apparatus can be used. Examples of beating apparatus include refiners, beaters, PFI mills, kneaders, dispersers, and other apparatuses that act on pulp fibers with metal or blades around a rotating shaft, apparatuses that use friction between pulp fibers, as well as high-pressure homogenizers, ultra-high-pressure homogenizers, nanomizers, various mills, and stone-mill type grinders.

[0091] Prior to beating or, if necessary, prior to the dispersion treatment carried out before beating, a pretreatment may be carried out as necessary. Pretreatments include, for example, mixing, stirring, emulsification, and dispersion, and may be carried out using a known device (e.g., a high-speed shear mixer).

[0092] In the present invention, the cellulose fibers may be nanofiberized. The surface area of ​​the nanofiberized portion increases, and antiviral, deodorizing, and antibacterial functions can be improved. On the other hand, if the fibers are completely nanofiberized, the fibers are completely disintegrated, and when mixed with pulp to produce a paper, the yield decreases, or the fibers do not remain in the paper, and the effects of the cellulose fibers decrease. Here, nanofiberization refers to defibrating the cellulose fibers to fibers with a fiber diameter of 100 nm or less. To form nanofibers, any known device similar to that used for beating can be used. EXAMPLES

[0093] The present invention will be described in more detail below with reference to specific examples, but the present invention is not limited to the following specific examples. In this specification, unless otherwise specified, concentrations and the like are based on weight, and numerical ranges are described as including their endpoints.

[0094] 1-1. Preparation of Cu ion-loaded oxidized cellulose fibers 275 BDkg (bone dry) of bleached, unbeaten kraft pulp (brightness 85%) derived from coniferous trees was added to 500 ml of an aqueous solution containing 1.07 kg (0.25 mmol per 1 g of bone dry cellulose) of TEMPO (Sigma Aldrich) and 28.3 kg of sodium bromide (1.0 mmol per 1 g of bone dry cellulose), and the mixture was stirred until the pulp was uniformly dispersed. Next, an aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 5.2 mmol / g, and the oxidation reaction was started at room temperature. The pH of the system decreased during the reaction, but 3M aqueous solution of sodium hydroxide was gradually added to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system did not change (time required for the oxidation reaction: about 90 minutes). After the reaction mixture was dehydrated using a screw press, washing with a sufficient amount of water and filtering were repeated twice to obtain water-impregnated oxidized cellulose fibers (solid content: 10% by mass, pulp yield: 90%, carboxyl group content: 1.68 mmol / g). Water was added to the obtained oxidized cellulose fibers to make a dispersion with a solid concentration of 2%, and the pH was adjusted to 9.0. Next, CuCl2 (FUJIFILM Wako Pure Chemical Industries, Ltd.) was added while stirring so that the concentration per 1 g of oxidized cellulose fibers was 1.0 mmol / g, and the mixture was further stirred for 30 minutes to incorporate Cu ions into the oxidized cellulose fibers. The unreacted metal salts were then removed by washing with sufficient amounts of water and filtering twice to obtain water-impregnated oxidized cellulose fibers carrying Cu ions (solid content: 30% by mass). The metal ion content in the resulting oxidized cellulose fibers carrying Cu ions was 43.8 mg / g, and the Canadian Standard Freeness (CSF) of the oxidized cellulose fibers carrying Cu ions was 500 ml. 1-2.Paper manufacturing (1) Example 1 LBKP (Nippon Paper Industries, CSF: 470ml) was used as the cellulose fiber, and Cu ion-supported oxidized cellulose fiber was mixed with it at 3% by weight of the total cellulose fiber (no light calcium carbonate was added). 0.80% by weight of cationic starch and 0.1% by weight of AKD-based sizing agent (Seiko PMC, AD1614) were added to 100% by weight of cellulose fiber to prepare a pulp slurry. The obtained pulp slurry was used to make paper at a speed of 540m / min using a papermaking machine. Next, 5.6 parts of anionic sizing agent (Harima Chemicals) and 3.5 parts of raw salt were added to 100 parts by weight of oxidized starch (Nippon Corn Starch, SK20) to prepare a surface treatment liquid with a solid concentration of 11% by mass. This was then applied using a gate roll coater (GRC) (amount applied on both sides: approximately 1.6 g / m 2 After drying, the paper is calendered to a basis weight of approximately 180 g / m 2 I got the paper. (2) Example 2 Paper was obtained in the same manner as in Example 1, except that the basis weight was set to about 170 g / m2, the calender line pressure after drying was increased, and the paper thickness was set to 181 μm. (3) Example 3 The cellulose fiber was mixed with 5% by weight of NBKP (Nippon Paper Co., Ltd., CSF: 550 ml) and 4% by weight of Cu ion-supported oxidized cellulose fiber, resulting in a basis weight of approximately 190 g / m 2 Paper was obtained in the same manner as in Example 1, except that: (3) Comparative Example 1 A paper was produced in the same manner as in Example 1, except that the Cu ion-supported oxidized cellulose fibers were not blended. (4) Comparative Example 2 Paper was obtained in the same manner as in Example 1, except that the basis weight was about 80 g / m2.

[0095] 2-1. Paper performance evaluation The obtained papers were evaluated for antiviral function and the like by the methods described below.

[0096] [Copper content] The content (mg / g) of metal ions and metal particles per gram of sheet was measured by inductively coupled plasma optical emission spectrometry (ICP-OES) according to the following procedure. (1) Dry the sample before measurement (50°C, 1 day). (2) Weigh out 0.1 g of the dried sample to be measured and place it in a 50 ml beaker. (3) Take 10 ml of concentrated nitric acid with a whole pipette and add it to the beaker containing the measurement sample to create a measurement sample solution (10 times dilution). (4) Leave the sample to stand for 30 minutes, then filter it through a syringe filter to remove any fiber from the sample. (5) Take 1 ml of the filtered sample liquid with a micropipette and add it to a test tube containing 49 ml of distilled water (50-fold dilution). (6) Close the test tube tightly and shake to mix. (7) Measure (quantify) the content of metal ions and metal particles using ICP-OES (Agilent Technology, ICP-OES 5110). (8) From the quantitative results (ppb) by ICP-OES, calculate the content of metal ions and metal particles per gram of sheet (mg / g) according to the following formula. (Quantitative result by ICP-OES (ppb) x 10 x 50) / (Weight of measurement sample (g)) x 1000 / 1000000000

[0097] [Metal elution amount] Regarding copper, the amount of metal ions and metal particles eluted per 0.8 g of sheet into 100 ml of ultrapure water was measured by inductively coupled plasma optical emission spectrometry (ICP-OES) according to the following procedure. (1) Dry the sample before measurement (50°C, 1 day). (2) Put ultrapure water into a 300 ml cup (30°C, 100 ml) (3) Place 0.8 g of the dried sample in the cup (2) and cover. (4) Leave the sample at rest for 30 minutes at 30°C, then filter the sample through a syringe filter to remove any fiber content. (5) Place 49 ml of the filtered sample solution into a test tube and add 1 ml of concentrated nitric acid using a micropipette. (6) Close the test tube tightly and shake to mix. (7) Measure (quantify) the content of metal ions and metal particles using ICP-OES (Agilent Technology, ICP-OES 5110). (8) From the quantitative results obtained by ICP-OES, the amount of metal ions and metal particles dissolved in 100 ml of ultrapure water per 0.8 g of sheet is calculated according to the following formula. Quantitative results by ICP-OES (ppb) x 50 / 49

[0098] [Anti-virus function] The antiviral function test was performed according to JIS L 1922:2016, and the antiviral activity value (Mv) was calculated. The weight of the sheet used in the test was 0.4 g, and the following two types of viruses were used as test viruses. Influenza virus (H3N2, ATCC VR-1679) Feline calicivirus (Strain: F-9 ATCC VR-782)

[0099] [Deodorizing function] The deodorizing function test was conducted using the SEK Mark Textile Product Certification Standard (JEC301, Textile Evaluation Technology Council) method, with ammonia as the target, using a test sample size of 100 cm 2 The deodorizing function was evaluated according to the following criteria. ◎ (Very good): Ammonia reduction rate is 80% or more ○ (Good): Ammonia reduction rate is between 70% and 80% × (Poor): Ammonia reduction rate is less than 70%

[0100] [Antibacterial function] A qualitative test was carried out using the halo method in accordance with JIS L1902 "Antibacterial test methods and antibacterial effects for textile products." Specifically, an agar medium containing E. coli was prepared, a test sample (5cm x 5cm) was placed on top of it, and after culturing at 37°C for 17 hours, the presence or absence of a "growth inhibition zone" of the test bacteria formed around the sample was confirmed. The antibacterial function was evaluated according to the following criteria. ○: A growth inhibition zone is observed and the plant has antibacterial properties. ×: No growth inhibition zone was observed, and the product had no antibacterial function.

[0101] 2-2. Paper quality evaluation The paper obtained was evaluated for its paper quality as follows. [Basis weight] Measured according to JIS P8124. [Paper thickness] Measured according to JIS P8118. [ISO whiteness] Measured according to JIS P8148 using a color difference meter (Murakami Color, CMS-35SPX). [ISO opacity] Measured according to JIS P8149. [Hue] Measured according to JIS P8150. [Stockigt sizing degree] Measured according to JIS P8122. [Pen size] Measured according to JAPAN TAPPI No. 12. [Oken smoothness] Measured according to JIS P 8155.

[0102] 2-3. Business card suitability evaluation The obtained papers were evaluated for the qualities required for business cards as follows.

[0103] [Hand feel] When the end of the short side of a sample measuring the size of a business card (55 mm x 91 mm) was held with the fingers and slowly shook up and down, samples that lacked tension and collapsed were rated as "X", and samples that were taut but did not collapse were rated as "O". [Suitable for offset printing] A printing test chart was printed on one side of paper using a Roland offset sheet-fed printing press at a printing speed of 8,000 sheets per hour using NEX NV-M blue, red, yellow, and black inks (manufactured by Toyo Ink Co., Ltd.). The printed surface texture (ink adhesion, strike-through) was visually observed and evaluated according to the following criteria. 〇: Good △: Fairly good ×: Defective. [Inkjet printability] After printing using an inkjet printer (CANON, CX-G4400), the degree of feathering was visually observed and evaluated according to the following criteria. 〇: Good △: Fairly good ×: Defective.

[0104] [Table 1]

[0105] As is clear from the above results, according to the present invention, paper having excellent antiviral, deodorizing and antibacterial properties, and particularly suitable for business cards, can be produced.

Claims

1. A business card paper having a clear coating layer containing cellulose fibers and an adhesive, Paper thickness measured according to JIS P 8118 is 150 μm or more, The business card paper has an antiviral activity value (Mv) of 2.0 or more against influenza virus and feline calicivirus, measured according to JIS L 1922:2016 (Testing method for antiviral activity of textile products).

2. 2. The business card paper according to claim 1, wherein the cellulose fibers contain one or more metal ions and / or metal particles selected from the group consisting of Ag, Au, Pt, Pd, Ni, Mn, Fe, Ti, Al, Zn and Cu.

3. 3. The business card paper according to claim 1, wherein the cellulose fibers include, as cellulose fibers having anionic groups, oxidized cellulose fibers having carboxyl groups or carboxylate groups; and / or carboxyalkylated cellulose fibers having carboxyalkyl groups.

4. 4. The business card paper according to claim 3, wherein the amount of anionic groups in the cellulose fibers having anionic groups is 0.01 to 3.0 mmol / g.

5. A business card paper according to any one of claims 1 to 4, wherein the cellulose fibers contain Cu and / or Ag as metal ions and / or metal particles, and the content of metal ions and / or metal particles in the paper is 0.20 mg or more and 6.3 mg / g or less.

6. The business card paper according to any one of claims 1 to 5, containing 60% by weight or more of LBKP relative to 100% by weight of the cellulose fibers.

7. 7. The business card paper according to claim 1, wherein the Oken smoothness measured in accordance with JIS P 8155 is 30 seconds or more.

8. Business card paper described in any one of claims 1 to 7, wherein the clear coating layer contains a surface sizing agent and the pen writing sizing degree of the business card paper is 4 or more.

Citation Information

Patent Citations

  • Sheet having cuts

    JP1994247081A

  • Inorganic porous crystal-hydrophilic polymeric complex

    JP1998120923A

  • Thermal transfer photographic paper

    JP1998230684A

  • Base paper sheet for printing

    JP2004122404A

  • Functional sheet

    JP2017141531A