Diamond abrasive grains for use in grinding wheels for semiconductor components, and method for manufacturing diamond abrasive grains for use in grinding wheels for semiconductor components

Low-toughness HPHT synthetic diamonds, irradiated and annealed below 800°C, address durability and quality issues in semiconductor processing by maintaining sharp edges and reducing wear, enhancing processing accuracy and longevity.

JP7561174B2Active Publication Date: 2024-10-03ELEMENT SIX LTD +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2022201670
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-12-17
Publication Date
2024-10-03
Estimated Expiration
2042-12-17

AI Technical Summary

Technical Problem

Existing diamond abrasive grains for semiconductor processing grindstones face issues with durability and maintaining processing accuracy due to high toughness leading to dullness and difficulty in achieving high-quality cuts, while synthetic diamonds suffer from unstable supply and high cost.

Method used

The use of low-toughness type IIa natural diamonds or HPHT synthetic diamonds, irradiated with ions or electrons and annealed below 800°C, combined with specific Raman spectroscopy to control internal stress, results in diamond abrasive grains with controlled toughness and improved durability.

Benefits of technology

The solution provides diamond abrasive grains that maintain high-quality machined surfaces and extended durability by self-sharpening, reducing chipping and wear, suitable for semiconductor component processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561174000003
    Figure 0007561174000003
  • Figure 0007561174000004
    Figure 0007561174000004
  • Figure 0007561174000005
    Figure 0007561174000005
Patent Text Reader

Abstract

To provide: diamond grits for semiconductor component processing grindstones which realizes excellent quality of a processed surface of a semiconductor component and has high durability performance; and a production methods of the diamond grits for semiconductor component processing grindstones.SOLUTION: Diamond grits for semiconductor component processing grindstones employs high-pressure and high-temperature (HPHT) single-crystal diamond grits. An average of diamond peak wavenumbers measured by Raman spectroscopy performed for HPHT single-crystal diamond grits is smaller than an average of diamond peak wavenumbers measured by Raman spectroscopy performed for type IIa single-crystal diamond.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to diamond abrasive grains for use in grinding wheels for processing semiconductor members such as semiconductor substrates, and to a method for producing diamond abrasive grains for use in grinding wheels for processing semiconductor members. [Background technology]

[0002] Diamond is the hardest substance and is widely used in grinding wheels for polishing and grinding various materials such as silicon, cutting integrated circuits, etc. In recent years, abrasive grains using single-crystalline diamond have been attracting attention.

[0003] Single-crystalline diamonds include natural diamonds and synthetic diamonds. Most natural diamonds are type Ia, and contain nitrogen in the lattice or between the lattices. Although type IIa diamonds do exist, the impurity content and crystal structure vary widely, making their quality and performance unstable. Furthermore, the price of natural diamonds fluctuates depending on the amount of diamonds mined, making stable supply an issue and they are expensive. On the other hand, synthetic diamonds can be stably supplied with a more consistent quality than natural diamonds.

[0004] Meanwhile, grinding wheels using diamond abrasive grains are required to have high durability so that they can be used for a long time in addition to being able to process a large amount of material. For example, Patent Document 1 discloses a processing method using diamond that has high toughness and wear resistance. According to this document, diamond is irradiated with an electron beam to give isolated vacancy defects, thereby improving toughness and wear resistance hardness.

[0005] Also, Patent Document 2 discloses a single crystal CVD synthetic diamond material having nitrogen defects that are both highly concentrated and uniformly distributed so as to be applied to optical filtering, mechanical and jewelry applications. The synthesis method disclosed in the same document also discloses that as-grown nitrogen vacancy defects are present at a predetermined concentration or more, and may be preferably annealed and / or irradiated. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 5554449 [Patent Document 1] Patent Publication No. 2015-505810 Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the invention described in Patent Document 1, the annealing temperature is as high as 1000°C at the lowest, and many isolated vacancy defects exist in the diamond. The same document describes that isolated vacancy defects exhibit high toughness and wear resistance to inhibit the progression of cracks, and describes that many isolated vacancy defects must be formed in order to exhibit high toughness. However, since the diamond material described in Patent Document 1 has excellent toughness, the shape of the diamond is maintained even after long-term processing. In addition, even though it has excellent wear resistance, the processing point, which is the contact point between the diamond material and the workpiece, is not constantly maintained in the sharp state before processing. In polishing and grinding processing, if a diamond material having toughness and / or wear resistance is used, the grinding wheel will be dulled, and the desired processing accuracy will not be obtained. In addition, in cutting processing, a good quality cut line will gradually be lost.

[0008] In addition, paragraphs 0020 and 0032 of Patent Document 1 state that a single crystal chemical vapor deposition (hereinafter, referred to as "CVD") diamond plate may be used to form a cutting blade and heated to a temperature of about 700°C or more after irradiation with an electron beam or the like to provide branding with a unique color. However, in order to use a single crystal CVD diamond plate as an abrasive, countless processes of generation by CVD film formation and grinding are required, which is not realistic. In fact, the amount of CVD diamond obtained by one CVD film formation is about several grams, and it is almost impossible to obtain a large amount of abrasive grains for grinding wheels. In addition, among CVD diamonds, single crystal diamonds in particular are formed by gathering microcrystals of single crystal diamond in the same orientation, so it is inappropriate to use them as abrasive grains like single crystal diamonds produced by HPHT. For this reason, the cutting blade described in Patent Document 1 is not an abrasive grain and is not used for grinding wheels. In addition, the crystal structures of diamonds produced by High-Pressure High-Temperature (hereinafter referred to as "HPHT") and CVD are significantly different, so in order to obtain a highly tough HPHT diamond, as in the invention described in Patent Document 1, it is necessary to anneal at a high temperature of 1000°C or higher, as mentioned above.

[0009] As described above, the CVD diamond described in Patent Document 2 is not only used for mechanical purposes, but also for optical filtering and jewelry, so it is difficult to say that it is suitable for mechanical processing such as polishing, grinding, and cutting. In addition, the same document describes that it is used for mechanical purposes, and describes that diamond with uniformly distributed nitrogen vacancy defects is provided to solve problems such as non-uniform wear resistance and reduced fracture toughness of CVD diamond. Therefore, even if the abrasive grains are made from the CVD diamond described in Patent Document 2, the problems of grinding, polishing, and cutting remain, as in Patent Document 1.

[0010] In recent years, as electronic components become smaller, there is a demand for smaller and higher quality semiconductor materials, and there is a demand for high-quality processing of semiconductor materials in a short time. Under these circumstances, the durability of abrasive grains and grinding wheels used in processes such as polishing, grinding, and cutting must be further optimized.

[0011] Therefore, an object of the present invention is to provide diamond abrasive grains for use in grinding wheels for processing semiconductor components, which have excellent quality in the processed surface of the semiconductor components and high durability, and a method for manufacturing diamond abrasive grains for use in grinding wheels for processing semiconductor components. [Means for solving the problem]

[0012] Conventionally, in the processing of semiconductor materials, diamonds with high toughness were required from the viewpoint of providing high durability, as described in Patent Document 1 and Patent Document 2. However, the inventors of the present invention, after intensive research, thought that if diamond abrasive grains used in semiconductor processing grindstones have high toughness, the durability of the grindstones would be inferior. In diamonds with low toughness, the diamond abrasive grains used are broken by cleavage of the abrasive grains used over a long period of use, and the abrasive grain edges are formed again to form self-sharpening blades. Since sharp edges are generated on the diamond abrasive grains after breaking, high processing accuracy is maintained even after long-term use. Therefore, it is necessary to use diamond abrasive grains with low toughness, contrary to the conventional practice. In addition, if the diamond abrasive grains are hard and have low toughness, there is a possibility that an excellent processed surface can be obtained.

[0013] An example of a hard, low-toughness diamond is type IIa natural diamond, which has an extremely low nitrogen content. However, as mentioned above, natural diamonds have a large variation in impurity content and crystal structure, and their quality and performance are not stable. Furthermore, natural diamonds are expensive, with their prices fluctuating depending on the amount of diamonds mined, leaving problems with stable supply.

[0014] Therefore, the present inventors have conducted intensive research into the use of high-quality diamond by using artificially produced Ib-type synthetic diamond. Conventionally, in order to improve toughness, diamond material is irradiated with electron beam and annealed at high temperature to improve toughness, but the present inventors have considered that diamond abrasive grains with low toughness have improved self-sharpening ability of abrasive grains during processing due to cleavage and / or wear of crystals, and as a result, the durability of grindstone is not reduced, and the quality of polished and ground processed surface is also improved.

[0015] Here, Patent Documents 1 and 2 each state that diamonds change color, but do not specifically disclose a method for controlling the color. This is because the color changes depending on the state of the raw material, such as the state before irradiation with electron beams or the state before annealing. In the inventions described in these documents, the annealing temperature is increased to a certain temperature or higher to improve toughness, but it is considered that high toughness is sufficient, and no specific control means for discoloration are disclosed. For this reason, in order to control the toughness appropriately so that it is not too high, it is not possible to control it only by the color of the diamond.

[0016] Furthermore, the effect of irradiation with electron beams or annealing on the diamond structure was reconsidered. In diamonds containing nitrogen, the bond length between carbon and nitrogen in the crystal is shorter than the bond between carbon and carbon. For this reason, it is considered that the diamond crystal has compressive stress. On the other hand, when diamond is irradiated with electron beams, the bonds in the nitrogen vicinity region in the diamond crystal or the bonds between carbons are damaged, and the compressive stress of the diamond is relaxed. It is presumed that the damaged parts are rebonded by annealing and the damage is restored. In view of this, in Patent Document 1 and Patent Document 2, the annealing temperature had to be increased because high toughness was required. Thus, although various diamond colors are disclosed in these documents, the correlation between toughness and diamond color is unknown, so the state of the diamond structure cannot be determined by the color of the diamond.

[0017] The present inventors have noticed that diamond abrasive grains used in grinding and polishing wheels and diamond abrasive grains used in cutting members must have low toughness, unlike the diamond materials disclosed in Patent Document 1 and Patent Document 2, as described above. Therefore, detailed studies have been conducted on the structure of diamonds that exhibit low toughness. As a result, the present inventors have noticed that diamond abrasive grains with desired low toughness can be obtained by highly precisely adjusting the internal stress of diamond crystals. Then, the present inventors have come to the conclusion that a suitable low toughness can be obtained if the natural diamond is of type IIa, which contains very little nitrogen and has very little internal crystal stress, and have performed detailed analysis by Raman spectroscopy.

[0018] As a result, it was found that, although annealing at a high annealing temperature exceeding 800°C was conventionally performed to obtain high durability performance through high toughness, when the annealing temperature was deliberately lowered to less than 800°C and annealing was performed for a specified time, a temperature range was found to exist in which the desired low toughness was exhibited. It was also found that, for diamonds that were only irradiated with electron beams, the internal stress was relaxed, so that the measurement results by Raman spectroscopy shifted to the low fraction side, and as the annealing temperature increased, the internal stress increased, so that the measurement results shifted to the high wavenumber side.

[0019] Based on these findings, further research has revealed that when annealing temperature is lowered, diamond approaches the natural diamond of type IIa.Furthermore, when the average wave number obtained by Raman spectroscopy measurement is lower than that of natural diamond of type IIa, desired low toughness can be obtained for the first time, and when used as grindstone, high quality machined surface can be obtained for a long period of time, and the present invention has been completed. The present invention, which has been made based on these findings, is as follows.

[0020] (1) Diamond abrasive grains for semiconductor component processing grindstones using HPHT single crystal diamond abrasive grains, Diamond abrasive grains for use in grinding wheels for processing semiconductor components, characterized in that the average value of diamond peak wavenumbers obtained by diamond peak measurement by Raman spectroscopy performed on the HPHT single crystal diamond abrasive grains is smaller than the average value of diamond peak wavenumbers obtained by measurement by Raman spectroscopy performed on type IIa single crystal diamond.

[0021] (2) Diamond abrasive grains for use in cutting, polishing, or grinding of semiconductor components, as described in (1).

[0022] (3) Diamond abrasive grains for use in grinding wheels for processing semiconductor components, as described in (1) or (2), which have crystal nuclei and / or crystal defects derived from carbon compounds.

[0023] (4) Diamond abrasive grains for use in grinding wheels for processing semiconductor members according to any one of (1) to (3), which have smooth crystal faces.

[0024] (5) Diamond abrasive grains for use in a grinding wheel for processing semiconductor members according to any one of (1) to (4), having an average particle size of 0.25 to 50 μm or less.

[0025] (6) A method for producing diamond abrasive grains for use in semiconductor component processing wheels, as described in any one of (1) to (5), comprising irradiating HPHTIb type synthetic diamond particles with at least one of ions, electrons, protons, neutrons, and gamma rays, and then annealing the particles at a temperature of less than 800°C for 10 to 240 minutes.

[0026] (7) A method for producing diamond abrasive grains for use in a grinding wheel for processing semiconductor components, as described in (6), comprising mixing raw materials consisting of amorphous carbon and a carbon compound having a hydrogen and / or hydroxyl group in a mass ratio of amorphous carbon:carbon compound=7:3-4:6, and synthesizing the diamond abrasive grains by maintaining the mixture under conditions of a pressure of 5-10 GPa and a temperature of 1300-1800°C for 1-300 seconds.

[0027] (8) A method for producing diamond abrasive grains for use in semiconductor component processing wheels, as described in (6) or (7), in which the amorphous carbon is carbon black, and the carbon compound is at least one of an aliphatic hydrocarbon, an alcohol, and a polyhydric alcohol.

[0028] (9) A method for producing diamond abrasive grains for use in semiconductor component processing wheels, as described in (8), in which the aliphatic hydrocarbon is polyethylene, the alcohol is methanol, and the polyhydric alcohol is pentaerythritol or xylitol. [Brief description of the drawings]

[0029] [Figure 1] FIG. 1 shows the results of measurements taken by Raman spectroscopy using a 785 nm laser on diamonds produced under various conditions. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a hub blade for illustrating an overview of the process of forming a protective layer on the hub blade. [Diagram 3] Figure 3 is a schematic cross-sectional view of a hub blade, Figure 3(A) is a schematic cross-sectional view showing the state of the base after the grinding wheel has been formed, and Figure 3(B) is an enlarged schematic cross-sectional view of the outer circumferential portion of the base shown in Figure 3(A). [Figure 4] Figure 4 is a schematic cross-sectional view of a hub blade, where Figure 4(A) is a schematic cross-sectional view showing the state of the base after the base has been removed, and Figure 4(B) is an enlarged schematic cross-sectional view of the outer circumferential portion of the base shown in Figure 4(A). [Diagram 5] Figure 5 is a schematic cross-sectional view of a hub blade, Figure 5(A) is a schematic cross-sectional view showing the state of the base after the protective layer has been removed, and Figure 5(B) is an enlarged schematic cross-sectional view of the outer circumferential portion of the base shown in Figure 5(A). [Figure 6] FIG. 6 is a perspective view showing a schematic diagram of the completed electroplated grindstone. [Figure 7]FIG. 7 shows the relationship between the cut length and the amount of wear when cutting silicon substrates with cutting wheels using diamond abrasive grains of type Ib synthetic diamond (As), diamond after electron beam irradiation (XP), and diamond annealed at 650°C after electron beam irradiation (XP-AN). [Figure 8] FIG. 8 is a graph showing the cutting life of the hub blade grinding wheels using the three types of diamond abrasive grains shown in FIG. [Figure 9] FIG. 9 is a perspective view of a grinding device equipped with a grinding wheel using abrasive grains. [Figure 10] FIG. 10 is a graph showing the surface roughness of the ground surface obtained by grinding with the grinding wheel using the three types of diamond abrasive grains shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail with reference to the accompanying drawings, but the present invention is not limited to the following embodiments. 1. Diamond abrasives for semiconductor component processing (1) Processing wheel The grindstone for processing semiconductor materials using the diamond abrasive grains for the grindstone for processing semiconductor materials according to the present invention can form a high-quality processed surface, and is therefore used to process semiconductor materials. For example, the grindstone for cutting can be a hub blade. For example, the grindstone for grinding and polishing can be a grind wheel.

[0031] Hub blades are cutting wheels that are mainly used in dicing machines. They are made by electroplating nickel or nickel alloy with diamond grains dispersed on the outer periphery of a disk-shaped hub base made of aluminum or stainless steel.

[0032] Conventional silicon substrates were thick and easy to process because the wafers themselves had rigidity. However, in recent years, electronic devices have become smaller, and the electronic components mounted on them are also required to be thinner and smaller, and similar specifications are also required for the chips obtained by cutting the silicon substrates that make up the electronic components. For this reason, silicon substrates with low rigidity and a thickness of 0.1 mm or less have come to be used, and if the cutting wheel has a short life, chipping on the cut surface becomes significant.

[0033] A grinding wheel is a grinding / polishing wheel with multiple roughly rectangular grinding stones attached to the end of a disk base, and the grinding wheel grinding stones rotate and come into contact with the substrate, grinding and polishing the substrate. The substrate rubs against the grinding stones when they come into contact, and the frictional heat generated by this causes the grinding stones to wear out easily. A processed grinding wheel is made by binding diamond abrasive grains with a binder such as resin or glass (vitrified).

[0034] However, the abrasive grains that make up the grindstones on conventional grinding wheels are diamond grains with high toughness, so the efficiency of grinding and polishing deteriorates as the time of use increases. For this reason, it becomes necessary to increase the rotation speed of the grinding wheel to shorten the grinding and polishing time. However, increasing the rotation speed causes the substrate to heat up. In addition, the grindstones can be damaged, resulting in a short lifespan.

[0035] In contrast to these, the grindstones used in the hub blades and grind wheels are equipped with the diamond abrasive grains for semiconductor component processing grindstones according to the present invention. Unlike conventional products, the diamond abrasive grains for semiconductor component processing grindstones according to the present invention have low toughness, so even silicon substrates with low rigidity do not chip for a long period of time. Details of the diamond abrasive grains for semiconductor component processing grindstones according to the present invention will be described later.

[0036] (2) Semiconductor materials In the present invention, the semiconductor member refers to a substrate such as a silicon substrate, a resin substrate, a glass plate, a GaN substrate, or a sapphire substrate, a semiconductor substrate having one or more semiconductor films laminated thereon, a semiconductor substrate molded with a resin, or a semiconductor chip cut from a semiconductor substrate. The semiconductor member also includes a semiconductor wafer having a plurality of semiconductor chips.

[0037] (3) Diamond abrasive grains In Ib type diamond, the interatomic distance is shortened by the bond between carbon and nitrogen due to the presence of nitrogen atoms, so that the state is given compressive stress. When irradiated with electron beams, etc., the vicinity of nitrogen and / or the bond between carbon atoms are damaged. It is presumed that this damage relieves the compressive stress in the crystal, and the toughness of Ib type diamond is reduced. Therefore, the diamond abrasive grain with moderate damage formed as in the present invention becomes close to the characteristics of IIa diamond with very few nitrogen atoms, so that in cutting processing where stress such as impact is applied, the diamond abrasive grain is broken one after another by continued use, and self-sharpens, so that it exhibits excellent durability.

[0038] On the other hand, it is presumed that the diamond material described in Patent Document 1 exhibits high toughness because, when the annealing temperature is high, the number of recombination sites of the damaged parts increases, and the recombination restores the carbon bonds within the crystal, which acts to inhibit the progress of cracks. For this reason, it is necessary to prevent the bond damage near the nitrogen and between carbon atoms from becoming more than necessary.

[0039] Diamonds with such damaged areas are repaired by rebonding the damaged areas through annealing. When rebonding occurs, compressive stress is again applied, and the toughness and / or wear resistance is moderately increased compared to conventional diamonds. In this state, the diamond abrasive grains have weak self-sharpening performance due to improved toughness and / or wear resistance, and the diamond abrasive grains are less likely to be broken due to their durability. Therefore, the self-sharpening performance of the abrasive grains cannot be improved, and in order for the abrasive grains to demonstrate their durability in grinding / polishing and cutting processes, it is important to repair the damaged areas by annealing appropriately, and there is an appropriate temperature range.

[0040] In this way, the diamond abrasive grains for semiconductor processing grindstones according to the present invention can control the durability of the semiconductor processing grindstones because their strength and toughness affect various processes. As a result, chipping during processing is suppressed, and high-quality processed surfaces can be obtained. In this way, the diamond abrasive grains for semiconductor processing grindstones according to the present invention, which have a technical concept that takes into account the toughness of diamond abrasive grains, can confirm the stress inside the crystal by the wavenumber shift of the Raman peak through Raman spectroscopy. This measurement is obtained by irradiating a 785nm laser.

[0041] The Raman peak of diamond abrasive grains is significantly shifted to the lower end compared to type IIa diamond by irradiating type Ib single crystal diamond abrasive grains with an electron beam. Then, when the annealing temperature is increased in the range of 500 to 1100 ° C, it gradually shifts to the higher wave number side. When it exceeds 800 ° C, it shows a wave number distribution similar to that of type IIa diamond abrasive grains. Therefore, at less than 800 ° C, it shifts to a lower wave number than natural IIa diamond, and diamond with relaxed internal crystal stress is obtained. Thus, diamond abrasive grains with an annealing temperature of less than 800 ° C are low-toughness abrasive grains with relaxed internal stress, and have a structure suitable for use as a grindstone for processing semiconductor materials.

[0042] In the present invention, the wavenumber distribution obtained by Raman spectroscopy is obtained by tallying up the frequency of each wavenumber of the obtained Raman peak. The average value of the wavenumber is calculated by multiplying the frequency of each wavenumber by the wavenumber, and dividing the calculated total by the frequency. The wavenumber shift represents the internal stress of the diamond abrasive grain. In the present invention, the average value of the wavenumber of the obtained diamond abrasive grain is lower than that of the natural diamond of IIa type. When the average value of the wavenumber is lower than that of the natural diamond of IIa type, the diamond exhibits low toughness, and when used as a grindstone, a high-quality processed surface is maintained for a long period of time. The difference ratio calculated by subtracting the average value of the wavenumber obtained from the average value of the wavenumber of IIa type, dividing the subtracted value by the average value of the wavenumber of IIa type, and multiplying by 100 is preferably 0.0001% or more, more preferably 0.0005% or more, even more preferably 0.0010% or more, particularly preferably 0.0014% or more, and most preferably 0.0020% or more. The upper limit is not particularly limited, but is preferably 1.0000% or less, more preferably 0.1000% or less, even more preferably 0.0100% or less, and particularly preferably 0.0030% or less.

[0043] In this way, the diamond abrasive grains for semiconductor component processing wheels according to the present invention have a moderate degree of residual damage in the vicinity of nitrogen and carbon bonding compared to conventional diamond abrasive grains. This goes against common technical knowledge, and it is only by using this method that the durability of the semiconductor component processing wheel and the high quality of the processed surface can be obtained.

[0044] In addition, the diamond abrasive grains for semiconductor material processing grindstone according to the present invention are manufactured by HPHT, and therefore, unlike diamond manufactured by CVD, they are monocrystalline with no grain boundaries. Even if damage is controlled with CVD diamond, it is difficult to control the internal stress throughout the grain due to grain boundaries, so they cannot show adequate toughness. Therefore, for diamond abrasive grains that attempt to achieve higher toughness and / or durability, it is necessary to use HPHT diamond abrasive grains.

[0045] The particle size of the diamond abrasive grains for semiconductor material processing grindstone of the present invention is preferably 0.25 to 50 μm. Within this range, the particles are not too large and can be used in a wide range of applications. For example, when used for hub blades, the particle size is preferably 1 to 30 μm, and more preferably 1 to 5 μm. When used for glide wheels, the particle size is preferably 0.25 to 50 μm, more preferably 3 to 40 μm, and most preferably 3 to 30 μm. In the present invention, for example, the volume average diameter D50 value measured by a laser diffraction scattering type particle size distribution measuring instrument (for example, manufactured by Malvern Instruments, model: Mastersizer2000, manufactured by Microtrac Bell, model: MicrotracMT3000, MicrotracUPA, etc.) can be used as the average particle size.

[0046] The diamond abrasive grain of the present invention may also have crystal nuclei and / or crystal defects derived from carbon compounds. In the case of conventional diamond grains, if crystal nuclei or crystal defects remain, crystal interfaces are formed on the surfaces that contain them, resulting in polycrystals. However, the single crystal diamond of the present invention has the same crystal orientation in the entire region including these and their surroundings, and the synthesized diamond grain is single crystal.

[0047] As described below, the single crystal diamond particles of the present invention can be produced preferably without using a metal catalyst, and therefore have extremely high purity, and since the components of the decomposed carbon compounds other than carbon do not remain within the single crystal diamond particles but are released to the outside, the particles have very few defects.

[0048] The crystal nuclei and / or crystal defects derived from carbon compounds can be easily confirmed in TEM images. However, these defects are observed only on the surface of the sample by chance, and do not reach deep inside the particles. Even if such slight defects exist, the crystal orientation is aligned in the entire area including the crystal nuclei and their surroundings. Furthermore, the crystal nuclei and crystal defects are derived from the carbon compounds described below. The crystal nuclei and crystal defects are a residual structure of the carbon compounds before their formation to some extent.

[0049] The single crystal diamond abrasive grain of the present invention may have a smooth crystal surface. As described later, even if irradiated and annealed as necessary, the smooth surface is maintained. In addition, the use of single crystal diamond abrasive grains with a smooth surface is particularly effective when used in the grindstone for processing semiconductor materials of the present invention. When single crystal diamond abrasive grains have a smooth surface, stress is applied uniformly to the abrasive grains, so that a uniform self-sharpening edge is generated, and high performance as a grindstone is maintained.

[0050] 2. Manufacturing method of diamond abrasive grains for grinding stones for semiconductor components The manufacturing method of diamond abrasive grains for semiconductor material grinding stone according to the present invention is a manufacturing method of single crystal diamond using high temperature and high pressure method, and can be manufactured in the same manner as conventional methods except that the manufacturing method of diamond abrasive grains is different from conventional methods. The raw material is a mixture of carbon raw material such as graphite and amorphous carbon and catalytic metal such as Fe, Co, Ni, Mn, etc. The impurity concentration of these raw materials is less than 100 ppm, and the arithmetic mean particle size is 5 to 1000 μm. The mixing ratio of carbon raw material and catalytic metal is 3:7 to 7:3.

[0051] This is introduced into the pressure medium used in conventional HPHT, and diamond is synthesized at a temperature and pressure in the thermodynamically stable region of diamond in the graphite phase equilibrium diagram. The pressure is more preferably 6 GPa or more, and the temperature is more preferably 1400 ° C or more. The pressure is more preferably 9.5 GPa or less, more preferably 8 GPa or less, and the temperature is more preferably 1700 ° C or less, more preferably 1600 ° C or less. From the viewpoint of diamond yield, it is preferable to raise the pressure to the above range and then raise the temperature to the above range. Examples of synthesis apparatuses used in HPHT include anvil-cylinder types such as belt types represented by uniaxial presses, toroidal types and chechevitsa types of anvil-opposed types, tetrahedral types of multiaxial presses, and multi-anvil types.

[0052] The time during which the raw material is exposed to the thermodynamically stable region is preferably 30 minutes or less. Within this time, a high conversion rate from the carbon source raw material to diamond can be obtained. There is no particular lower limit, but it is sufficient if it is 1 second or more.

[0053] The pressure profile and temperature profile are not particularly limited, and the pressurization rate and temperature increase rate may be set within the range of the device specifications.

[0054] Next, the diamond particles produced by the HPHT method may be pulverized to obtain a desired abrasive grain size. The pulverization method is not particularly limited, but may be performed using a pulverizer such as a ball mill or a jet mill. As described above, the grain size of the obtained pulverized powder is preferably 0.25 to 50 μm.

[0055] The ground diamond particles are then irradiated with at least one of ions, electrons, protons, neutrons, and gamma rays to produce diamond abrasive grains. The irradiation conditions are not particularly limited and may be the same as those of the conventional method. 15 e - / cm 2 ~1×10 19 e - / cm 2 The dose may be 100°C or more. The irradiation energy may be appropriately adjusted within the range of 30keV to 12Mev. The temperature of the diamond particles during irradiation may not be higher than the annealing temperature described later, so as not to increase the toughness of the diamond abrasive grains. The temperature may be room temperature, or may be 100°C or more and less than 800°C.

[0056] Then, annealing is performed at a temperature of less than 800°C for 10 to 240 minutes. Conventionally, annealing was performed at a high temperature of at least 1000°C or more to obtain high toughness. In contrast, in the manufacture of diamond abrasive grains of the present invention, annealing must be performed at a lower temperature than conventionally in order to prevent the toughness from improving as much as possible. The lower limit of the annealing temperature is not particularly limited, but in order to obtain a moderate toughness, it is preferably room temperature or higher, and more preferably 100°C or higher. The annealing time does not greatly affect the characteristics of the diamond abrasive grains, but in order to prevent the manufacturing time from becoming too long, it is sufficient to be within the above-mentioned range, and more preferably 30 to 120 minutes. The temperature rise and fall rate is not particularly limited, but is not particularly limited as long as it is within the range that the annealing device can control, and may be, for example, 5 to 20°C / min.

[0057] When used in polishing and grinding wheels, the annealing temperature is preferably 600°C or higher and lower than 800°C, more preferably 600 to 700. In these wheels, the toughness is slightly improved by annealing in a range of toughness lower than conventionally, which causes fine fracture of the diamond abrasive grains during processing, lowers surface roughness or reduces chipping, improves the durability of the wheel, and provides a high-quality processed surface.

[0058] When used in a cut-off wheel, the annealing temperature is preferably room temperature or higher but lower than 800° C., and more preferably room temperature to 650° C. When low-toughness diamond abrasive grains are used in a cut-off wheel that is subjected to stress similar to that of an impact, the durability of the wheel is improved and a high-quality machined surface can be obtained.

[0059] Although the above-mentioned process has been described in the order of manufacturing diamond abrasive grains, irradiation, and annealing, the desired characteristics can be obtained even if the order of annealing and irradiation is reversed.

[0060] In addition, a raw material that does not use a metal catalyst may be selected as a method for manufacturing diamond abrasive grains. For example, diamond may be synthesized by exposing a raw material consisting of amorphous carbon and a carbon compound to pressure and temperature in the thermodynamically stable region of diamond in the phase equilibrium diagram of carbon. When metal impurities are not included, the influence of irradia-tion on diamond bonds is significant, so it is thought that the diamond shifts to the lower fraction side. This is significant in the range of annealing temperatures below 800°C. Furthermore, the diamond abrasive grains used in the semiconductor processing grindstone according to the present invention do not contain metal impurities, and also have crystal nuclei and / or crystal defects derived from carbon compounds, so that by using them in the grindstone, a sharper and more uniform self-sharpening blade is generated, making it easier to obtain a high-quality processed surface and excellent processing performance.

[0061] The "amorphous carbon" used in the manufacturing method of the present invention refers to carbon that is amorphous and does not have a fixed crystal structure. Among these, solid carbon that is easy to handle is preferable, and carbon black is preferable. In addition, it may contain unavoidable impurities. In the present invention, those having a certain crystal structure such as diamond and graphite are excluded from the "amorphous carbon" of the present invention. In addition, "carbon compounds" described later are also excluded from the "amorphous carbon".

[0062] In the manufacturing method according to the present invention, single crystal diamond can be manufactured without being limited by the purity of the raw material. Preferably, the amorphous carbon including carbon black has an impurity concentration of less than 30 ppm and an arithmetic mean particle size of 16 to 200 nm. More preferably, it is 16 to 100 nm, and even more preferably, it is 16 to 70 nm. If it is within this range, there is no need to complicate the temperature profile and pressure profile.

[0063] The carbon compound used in the present invention is not particularly limited as long as it is a compound containing C, and includes, for example, inorganic compound materials including carbon monoxide, carbon dioxide, hydrocyanic acid, cyanates, and thiocyanates, and organic materials. However, amorphous carbon and metal salts are not included. The carbon compound is not particularly limited, but is not limited to any material that can be thermally decomposed and carbonized, such as tires, toner, hair, wood, and waste plastics. When using such recycled resources, they can be used as raw materials if they are crushed into small pieces so that carbonization by thermal decomposition is easy. In addition, solids such as coal, coke, charcoal, soot, and glassy carbon, liquids such as naphtha (gasoline), kerosene, light oil, and heavy oil, and gases such as natural gas are also included.

[0064] In addition, the carbon compound is preferably an organic compound, is preferably liquid or solid at room temperature, and is particularly preferably solid so as to be easy to handle as raw material.In order to ensure that the elements that do not contribute to diamond do not remain during synthesis and are decomposed during synthesis and released to the outside, the organic compound is more preferably made of hydrogen, oxygen, and carbon, and is particularly preferably made of hydrogen and / or hydroxyl group and carbon.

[0065] In addition to the above, the carbon compounds used in the present invention include aliphatic, aromatic, and alicyclic hydrocarbons, which may be saturated or unsaturated, and may be monomeric, oligomeric, or polymeric. Examples of such alkanes include methane, ethane, propane, butane, pentane, hexane, heptane, octane, nonane, and decane; alkenes such as ethene (ethylene), propene (propylene), butene (butylene), pentene, hexene, heptene, octene, nonene, and decene; alkynes such as ethyne (acetylene), propyne (methylacetylene), butyne, pentine, hexyne, heptyne, octyne, nonine, and decyne; cycloalkanes such as cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane, cyclooctane, cyclononane, and cyclodecane; and alkadiene alkanes such as propadiene (allene), butadiene, pentadiene (piperylene), hexadiene, heptadiene, octadiene, nonadiene, and decadiene. These may have substituents such as alcohols with hydroxyl groups, such as methanol, ethanol, and propanol, sulfone groups, nitro groups, nitroso groups, epoxy groups, aldehyde groups, amino groups, acyl groups, carbonyl groups, and carboxyl groups, and may be oligomers of these or polymers such as polyethylene, polypropylene, and polyethylene terephthalate.

[0066] In addition, similar to single crystal diamond, the Raman spectrum shows a peak at 1330-1340 cm -1 It is preferable that a shoulder peak is observed near the sp 3 It is preferable that the organic compound has a carbon atom with a hybrid orbital, and the number of carbon atoms is preferably 1 to 10, more preferably 4 to 6, and particularly preferably 5. In particular, the organic compound is preferably a polyhydric alcohol. As the polyhydric alcohol, a trihydric to octahydric alcohol is preferable, and a tetrahydric alcohol is more preferable. All the carbon elements in the polyhydric alcohol are sp 3 It is more preferred that the orbital has a hybrid structure.

[0067] Diamonds are sp 3 It is a tetrahedral structure with hybrid orbitals, and when this carbon structure exists in a carbon compound, it acts as a crystal nucleus during synthesis. Therefore, in order to promote the growth of diamond more efficiently, it is necessary to make the carbon compound sp 3It is preferable that the carbon structure has a hybrid orbital, and it is preferable that the carbon compound has a structure close to the tetrahedral structure of diamond. In addition to these, it is most preferable that the carbon compound has a tetrahedral structure with five carbon atoms. It may have a hydroxyl group at the end of these, and it is preferable that the polyhydric alcohol is a polyhydric alcohol from the viewpoint of being released as a desorbed gas when heated.

[0068] The reason why the use of the above-mentioned preferred amorphous carbon and carbon compound in the present invention enables single crystal diamond having excellent durability to be synthesized at low cost, in high yield, and in a short time is believed to be as follows. Conventional high-temperature, high-pressure methods use molten metal and graphite. When the molten metal melts at high temperatures, the graphite is decomposed by the molten metal to produce diamond. However, amorphous carbon, which is carbon that does not have a fixed crystal structure, has a random structure, so it is easier to convert the structure into diamond compared to carbon that has a specific structure. For this reason, the high energy required for the structural change of graphite by molten metal, as in the conventional method, is not required, and sp 3 It is speculated that if there is an organic compound with hybrid orbitals, it can act as a starting point for the conversion of carbon to diamond, making it easier to produce diamond. In addition, hydroxyl groups in the raw materials exposed to high temperature and pressure react with amorphous carbon and are released as CO or CO2. 3 The carbon with hybrid orbital becomes the crystal nucleus, which is the smallest structure of diamond crystal.Then, this crystal nucleus becomes the starting point, and amorphous carbon is converted into diamond structure.Therefore, it is presumed that the present invention can produce the single crystal diamond particle with few defects and excellent durability at low cost and high yield.

[0069] Examples of polyhydric alcohols include ethylene glycol, propylene glycol, diethylene glycol, trimethylene glycol, tetraethylene glycol, triethylene glycol, dipropylene glycol, 1,4-butanediol, 1,3-butanediol, 2,3-butanediol, 1,2-butanediol, 2-methyl-1,3-propanediol, 3-methyl-1,2-butanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,2-pentanediol, 1,5-pentanediol, 1,4-pentanediol, 2,4-pentanediol, 2,3-dimethyltrimethylene glycol, tetramethylene glycol, and 3-methyl-4,3-pentanediol. Examples of such glyceryl ethers include glyceryl ether, 3-methyl-1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 1,6-hexanediol, 1,5-hexanediol, 1,4-hexanediol, 2,5-hexanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, hydroxypivalic acid neopentyl glycol ester, glycerin, trimethylolethane, trimethylolpropane, diglycerin, xylitol, triglycerin, 1,2,6-hexanetriol, pentaerythritol, dipentaerythritol, tris(2-hydroxyethyl)isocyanuric acid, sorbitol, perseitol, and sucrose.

[0070] Among these, trihydric alcohols include glycerin and trimethylolpropane. Tetrahydric alcohols include pentaerythritol and diglycerin. Pentahydric alcohols include xylitol. Hexahydric alcohols include sorbitol. Heptahydric alcohols include perseitol. Octahydric alcohols include sucrose. Among these, tetrahydric alcohols are preferred, and pentaerythritol is most preferred.

[0071] The above carbon compounds may be used alone or in combination of two or more. The carbon compound may contain unavoidable impurities. Even if the carbon compound contains unavoidable impurities, the above-mentioned effects are not affected.

[0072] In the present invention, the combination of amorphous carbon and a carbon compound is preferably such that the amorphous carbon is carbon black and the carbon compound is sp 3 Polyhydric alcohols having hybrid orbitals and tetrahedral structures, most preferably a combination of carbon black and pentaerythritol, can be converted into diamond at 95% or more, preferably 99% or more, based on the total weight of the raw materials.

[0073] From the viewpoint of pressure attenuation due to volumetric shrinkage during conversion of amorphous carbon to diamond, the mixing ratio of amorphous carbon to carbon compound is preferably (amorphous carbon):(carbon compound)=7:3-4:6, and particularly preferably 6:4-5:5, in terms of mass ratio. After weighing out the amorphous carbon and carbon compound in the above range, the starting materials are mixed. A general mixing method may be used. For example, the starting materials are put into a powder mixer and mixed for about 1-30 minutes under atmospheric pressure or reduced pressure. This produces a mixed powder of 100 μm or less.

[0074] The mixed powder obtained as described above can be used to manufacture diamond abrasive grains under the same conditions as in the case of raw materials using a metal catalyst. EXAMPLES

[0075] The present invention will be described with reference to the following examples, which are not intended to limit the scope of the present invention. In order to verify the effects of the present invention, hub blades and grinding wheels were produced using the diamond abrasive grains shown in Table 1, and each was evaluated.

[0076] (1) Preparation of diamond abrasive grains In this embodiment, Ib type diamond particles synthesized by HPHT were prepared as follows. The raw materials were graphite with an arithmetic mean particle size of 30 μm and FeNiCo alloy with an arithmetic mean particle size of 30 μm as a catalyst metal, and 50 g of graphite and 50 g of FeNiCo alloy powder were weighed and put into a powder mixer to obtain a mixed powder.

[0077] Diamond synthesis was carried out in a "toroidal" type high pressure chamber. The applied pressure was calibrated using the approximate curve of the phase transition of Bi, Tl, and Ba at room temperature, which is commonly used in the HPHT method, and was taken as the pressure indicated by the oil pressure gauge. The heating temperature was calibrated with the input power and temperature using a thermocouple, and was taken as the temperature calculated from the input power. The raw material was heated by a direct heating method in which an electric current was passed through a graphite heater. Using this equipment configuration, the mixed powder was exposed to HPHT in air at a temperature of 1250°C and a pressure of 5.5 MPa.

[0078] The sample synthesized by the high-temperature high-pressure method is mixed with the pressure medium at the end of the decompression process, so the pressure medium particles are first removed using a sieve and then washed with deionized water. Next, the powder is placed in a liquid of bromoform (CHBg3) to separate the carbon black and diamond particles. The diamond particles are filtered and washed with deionized water to obtain diamond particles.

[0079] The diamond particles thus produced were subjected to elutriation. The average particle size of the obtained diamond particles was 30 μm in arithmetic mean particle size. The average particle size of the obtained diamond particles was measured using a laser diffraction scattering type particle size distribution measuring device (e.g., manufactured by Malvern Instruments, model: Mastersizer2000) with the volume average particle size D50 as the average particle size.

[0080] The resulting abrasive grains were then irradiated with an electron beam. The electron irradiation was performed for 2 hours at 4.5 MeV, 20 mA, and a 50% scanning width using an apparatus manufactured by Isotron plc. The total dose received by the sample was 1.95 × 10 18 e - / cm 2The result was then annealed in air under the conditions shown in Table 1 to obtain single crystal diamond abrasive grains. The fact that they were single crystals was confirmed by TEM images.

[0081] The obtained diamond abrasive grains were subjected to Raman spectroscopy measurement. The Raman spectroscopy measurement was performed using a Raman spectroscopic analyzer (manufactured by WITech Corporation: Laser Raman Spectroscopic Analyzer, Model No. alpha300R), and each diamond abrasive grain was measured as shown in Figure 1.

[0082] FIG. 1 shows the results of mapping measurements obtained by irradiating a 785 nm laser by Raman spectroscopy on diamonds created under various conditions. In FIG. 1, IIa is a natural diamond, Ib (As Received) is an Ib type synthetic diamond, XP is an Ib (As Received) diamond irradiated with an electron beam, XP-AN500 is a diamond obtained by annealing XP at 500°C, XP-AN650 is a diamond obtained by annealing XP at 650°C, XP-AN800 is a diamond obtained by annealing XP at 800°C, XP-AN950 is a diamond obtained by annealing XP at 950°C, and XP-AN1100 is a diamond obtained by annealing XP at 1100°C. In FIG. 1, when the wavenumber distribution shifts to the high wavenumber side, the toughness increases due to compressive stress. On the other hand, when the wavenumber distribution shifts to the low wavenumber side, the toughness decreases due to tensile stress. The average wavenumber distribution for each sample is shown in Table 1. The arithmetic mean particle size of the diamond abrasive grains is 30 μm.

[0083] [Table 1]

[0084] In Table 1, when "difference from IIa" is "-", it means that it is shifted to the higher wavenumber side than IIa, and when "difference from IIa" is "+", it means that it is shifted to the lower wavenumber side than IIa. As shown in Figure 1 and Table 1, it can be seen that the wavenumber distribution of XP is shifted to the lower wavenumber side compared to Ib (AsReceived) regardless of the annealing temperature. And, as the annealing temperature increases, the wavenumber distribution shifts to the higher wavenumber side, and at 800 ° C, it shifts to the higher wavenumber side than natural diamond, and tends to deviate from the appropriate grinding / polishing wheel or cutting wheel. Thus, XP and low-toughness diamond abrasive grains with an annealing temperature of less than 800 ° C have a structure suitable for semiconductor material processing wheels.

[0085] (1) Evaluation using hub blades (1-1) Making the hub blade A nickel plating layer containing abrasive grains was formed by electrodeposition in a nickel plating bath in which diamond abrasive grains for semiconductor processing grindstones were dispersed on an annular base made of aluminum. Then, a grindstone was formed in which abrasive grains were dispersed in the plating layer formed on the base. A part of the base overlapping the grindstone was removed with a chemical solution. When removing the protective layer, a part of the protective layer was removed to expose the area of ​​the grindstone that was covered by the protective layer. The details are as follows.

[0086] First, a nickel plating layer was formed on a ring-shaped base made of a material containing aluminum. Figure 2 is a schematic cross-sectional view for explaining an overview of the process of forming a protective layer (nickel plating layer) on the hub blade.

[0087] The base 4 and the nickel electrode 6 were immersed in the nickel plating solution in the plating bath 2. The base 4 was made of aluminum metal material and had a disk shape (annular shape), and a mask 4a corresponding to the shape of a grindstone described later was provided on its surface. As shown in Fig. 2, the mask 4a used had a part of the surface of the base 4 exposed at its outer periphery.

[0088] The base 4 was connected to a negative terminal (negative electrode) of a DC power supply 10 via a switch 8. On the other hand, the nickel electrode 6 was connected to a positive terminal (positive electrode) of the DC power supply 10.

[0089] After the base 4 and the nickel electrode 6 were immersed in the nickel plating solution in the plating bath 2, a direct current was passed through the nickel plating solution with the base 4 as the cathode and the nickel electrode 6 as the anode, forming a nickel plating layer on the surface of the base 4 not covered by the mask 4a. Specifically, as shown in Fig. 2, a switch 8 arranged between the base 4 and a direct current power source 10 was short-circuited while a fan 14 was rotated by a rotary drive source 12 such as a motor to stir the nickel plating solution. As a result, a nickel plating layer was formed as a protective layer 16 on the area of ​​the base 4 not covered by the mask 4a, and the abrasive grains and the nickel plating layer were laminated on the protective layer 16, forming a grinding wheel in which the abrasive grains were distributed approximately evenly in the nickel plating layer.

[0090] The nickel plating solution is an electrolyte in which materials containing nickel (ions), such as nickel sulfate and nickel nitrate, are dissolved, and the diamond abrasive grains shown in Table 1 were mixed into the volume of nickel plating solution B. Nickel plating solution A is nickel plating solution B (Watts bath) containing 270 g / L of nickel sulfate, 45 g / L of nickel chloride, and 40 g / L of boric acid, and 6 L was used in this example.

[0091] Fig. 3 is a schematic cross-sectional view of a hub blade, Fig. 3(A) is a schematic cross-sectional view showing the state of the base 4 after the grindstone is formed, and Fig. 3(B) is a schematic cross-sectional view showing an enlarged outer peripheral portion of the base 4 shown in Fig. 3(A). As shown in Fig. 3(A) and Fig. 3(B), the grindstone 36 is formed to a desired thickness and overlaps the protective layer 16, and the formation of the grindstone is completed.

[0092] Thereafter, a part of the base 4 overlapping the grindstone 16 was removed with a chemical solution. Fig. 4 is a schematic cross-sectional view of the hub blade, Fig. 4(A) is a cross-sectional view showing the state of the base 4 after the base has been removed, and Fig. 4(B) is an enlarged cross-sectional view of the outer periphery of the base 4 shown in Fig. 4(A). As shown in Figs. 4(A) and 4(B), the mask 4a used in the step of forming the grindstone was removed before the base removal step was carried out.

[0093] When removing the base 4, a chemical solution (chemical solution for etching) was applied to the outer periphery of the base 4 to remove a part of the outer periphery of the base 4 as shown in Figures 4(A) and 4(B). A sodium hydroxide solution that dissolves aluminum was used as the chemical solution. As a result, a part of the protective layer 16 that was covered by the base 4 was exposed.

[0094] In this embodiment, a protective layer 16 is provided between the base 4 and the grinding wheel 36, so that even if the above-mentioned chemical solution passes through the nickel plating layer (grinding wheel 36), the base 4 will not be removed by the passing chemical solution.

[0095] Thereafter, a part of the protective layer 16 was removed to expose the area of ​​the grinding wheel 36 that had been covered with the protective layer 16. Figure 5 is a cross-sectional schematic diagram of the hub blade, Figure 5(A) is a cross-sectional schematic diagram showing the state of the base 4 after the protective layer has been removed, and Figure 5(B) is an enlarged cross-sectional schematic diagram of the outer periphery of the base 4 shown in Figure 5(A).

[0096] When removing the protective layer, a chemical solution (chemical solution for etching) was applied to the protective layer 16 exposed after removing the base, and a part of the protective layer 16 was removed as shown in Figures 5(A) and 5(B). A part of the grindstone 36 was exposed.

[0097] 6 is a perspective view showing a schematic diagram of the completed electroplated grindstone. Through the above-mentioned procedure, a hub-type electroplated grindstone 1 is completed in which an annular grindstone part 36 is fixed to the outer periphery of a disk-shaped base 4.

[0098] (1-2) Hub blade evaluation The amount of blade wear and cutting life of each of the hub blades manufactured as described above were evaluated under the following evaluation conditions. A silicon wafer with a thickness of 400 μm was used as the workpiece, and cutting was performed while supplying cutting water to the contact area between the hub blade using various diamond abrasive grains and the silicon wafer as described above. The rotation speed of the cutting blade was about 30,000 rpm. The cutting feed rate of the chuck table when cutting each planned dividing line of the silicon wafer was constant at 120 mm / sec, and 100,000 mm was cut. The cutting depth of the silicon wafer was set so that the bottom end of the cutting blade cut through the silicon wafer and cut 30 μm into the dicing tape.

[0099] Blade wear and cutting life FIG. 7 is a diagram showing the relationship between the cutting length and the wear amount when cutting a silicon substrate with a cutting wheel using diamond abrasive grains of Ib type synthetic diamond (As-Received), diamond after electron beam irradiation (XP), and diamond annealed at 650°C after electron beam irradiation (XP-Anneal). FIG. 8 is a graph showing the cutting life of the hub blade using the three types of diamond shown in FIG. 7. Note that FIG. 9 shows the percentage (%) of each blade wear amount when As-Received is taken as 100% in the blade wear amount after cutting 100000mm in FIG. 8. As shown in FIG. 7 and FIG. 8, the XP and XP-AN of this embodiment both have about 70% less blade wear amount than As-Received, and have a longer cutting life.

[0100] (2) Evaluation using a grind wheel (2-1) Wafer grinding with a grinding wheel and preparation of the grinding wheel A resinoid grinding wheel was produced in which the abrasive grains were bonded together using a binder structure in which various diamond abrasive grains shown in Table 1 were dispersed in a synthetic resin binder made of phenol. The average grain size of the diamond abrasive grains was 30 μm. Silicon wafers were ground using a grinding machine equipped with this grinding wheel. Details are explained below.

[0101] 9 is a perspective view of a grinding device equipped with a grinding wheel using abrasive grains, in which the X-axis direction is the width direction of the grinding device 100, the Y-axis direction is the depth direction of the grinding device 100, and the Z-axis direction is the vertical direction.

[0102] As shown in FIG. 9, the grinding apparatus 100 includes a first cassette 111 and a second cassette 112 in which a plurality of wafers W, which are workpieces, are accommodated, a common carry-in / out means 113 which serves both as a carry-out means for carrying the wafers W out of the first cassette 111 and as a carry-in means for carrying the ground wafers W into the second cassette 112, an alignment means 114 for aligning the center of the wafer W, transport means 115 and 116 for transporting the wafers W, and a suction means for sucking the wafers W. The apparatus is equipped with three chuck tables 117-119 that hold the wafers, a turntable 120 that rotatably supports and rotates each of these chuck tables 117-119, grinding means 30, 40 that are processing means that perform grinding processing as processing on the wafers W held on each of the chuck tables 117-119, cleaning means 151 that cleans the wafers W after grinding, and cleaning means 152 that cleans the chuck tables 117-119 after grinding.

[0103] In the grinding apparatus 100, the wafer W accommodated in the first cassette 111 is transported to the alignment means 114 by the transport operation of the transport-in / out means 113, where the wafer W is centered and then transported and placed on one of the chuck tables 117-119 by the transport means 115. In the figure, the wafer W is transported and placed on the chuck table 117. The three chuck tables 117-119 in this embodiment are arranged at equal intervals in the circumferential direction of the turntable 120, and each of them is rotatable and moves on the XY plane with the rotation of the turntable 120. The chuck tables 117-119 are arranged directly below the grinding means 130 by rotating a predetermined angle, for example, 120 degrees counterclockwise, while suction-holding the wafer W.

[0104] The grinding means 130 grinds the wafer W held on the chuck tables 117-119, and is provided on a wall 122 erected at the end of the base 121 in the Y-axis direction. The grinding means 130 is guided by a pair of guide rails 131 arranged in the Z-axis direction on the wall 122, and is supported by a support 133 that moves up and down by driving a motor 132, and is configured to move up and down in the Z-axis direction with the up and down movement of the support 133. The grinding means 130 includes a motor 134 that rotates a rotatably supported spindle 134a, and a grinding wheel 136 that is attached to the tip of the spindle 134a via a wheel mount 135 and grinds the back surface of the wafer W. The grinding wheel 136 includes a grinding stone 137 for rough grinding that is fixed to the lower surface of the grinding wheel 136 in an annular shape.

[0105] Rough grinding was performed as follows. The grinding wheel 136 was rotated by rotating the spindle 134a by the motor 134, and was fed downward in the Z-axis direction for grinding, so that the rotating grinding stone 137 came into contact with the back surface of the wafer W, thereby grinding the back surface of the wafer W held on the chuck table 117 and positioned immediately below the grinding means 130. Here, when rough grinding of the wafer W held on the chuck table 117 was completed, the turntable 120 was rotated counterclockwise by a predetermined angle, and the roughly ground wafer W was positioned immediately below the grinding means 140.

[0106] The grinding means 140 grinds the wafer W held on the chuck tables 117-119, is guided by a pair of guide rails 141 arranged in the Z-axis direction on the wall 122, is supported by a support part 143 that moves up and down by driving a motor 142, and is configured to move up and down in the Z-axis direction with the up and down movement of the support part 143. The grinding means 140 includes a motor 144 that rotates a rotatably supported spindle 144a, and a grinding wheel 146 that is attached to the tip of the spindle 144a via a wheel mount 145 and grinds the back surface of the wafer W. The grinding wheel 146 includes a grinding wheel 147 for finish grinding that is fixed to the lower surface of the grinding wheel 146 in an annular shape. In other words, the grinding means 140 has the same basic configuration as the grinding means 130, and is configured differently only in the types of the grinding wheels 137 and 147.

[0107] The finish grinding was performed as follows. The grinding wheel 146 was rotated by the rotation of the spindle 144a by the motor 144, and was fed downward in the Z-axis direction for grinding, so that the rotating grinding stone 147 came into contact with the back surface of the wafer W held by the chuck table 117 and positioned directly below the grinding means 140, thereby grinding the back surface of the wafer W. Here, when the finish grinding of the wafer W held by the chuck table 117 was completed, the turntable 120 was rotated counterclockwise by a predetermined angle, and returned to the initial position shown in FIG. 11. At this position, the wafer W whose back surface has been finish ground was transported by the transport means 116 to the cleaning means 151, and after the grinding debris was removed by cleaning, it was transported into the second cassette 112 by the transport operation of the transport means 113. The cleaning means 152 washed the chuck table 117, which had been vacant after the finish-ground wafer W was picked up by the transport means 116, with pure water. Similarly, rough grinding, finish grinding, and loading / unloading of the wafers W held on the other chuck tables 118 and 119 were performed in accordance with the rotational position of the turntable 120 .

[0108] Here, the grinding wheels 137 and 147 contain diamond abrasive grains. The grinding wheels 137 and 147 are made by kneading the diamond abrasive grains with vitrified.

[0109] A silicon wafer is used as the wafer W, which is the workpiece, and the average grain size of the diamond abrasive grains used in the grinding wheel 137 is 30 μm.

[0110] (2-2) Evaluation of grind wheels The grinding wheel was evaluated based on the surface roughness of the wafer after grinding.

[0111] Surface roughness The surface roughness of the silicon wafer ground using each grinding wheel was measured using a Chapman MP3300. FIG. 10 is a graph showing the surface roughness of the ground surface ground using the grinding wheels using the three types of diamond abrasive grains shown in FIG. 7. As shown in FIG. 10, the results showed that the surface roughness of both XP and XP-AN in this embodiment was smaller than that of As. Among the examples, it was found that the surface roughness of XP-AN was superior to that of XP in the grinding wheels.

[0112] The raw material of diamond particles was changed as follows. Carbon black powder with an arithmetic mean particle size of 40 nm (product name: Tokai Carbon Co., Ltd., Toka Black #4500) and charcoal with an arithmetic mean particle size of 20 to 40 nm were used as amorphous carbon, and pentaerythritol (Tokyo Chemical Industry Co., Ltd., product code (P0039)) and xylitol (Tokyo Chemical Industry Co., Ltd., product code (X0018)) were weighed as shown in Table 2, and the pressure, temperature, and processing time were set to the conditions in Table 1, and the mixture was put into a powder mixer to obtain a mixed powder. Other than this, diamond abrasive grains were manufactured in the same manner as above and evaluated in the same manner as above. As a result, for all of Samples 1 to 6 in Table 2, results equal to or better than those described above were obtained.

[0113] [Table 2] [Explanation of symbols]

[0114] 1 Electroplated grinding wheel 2 Plating bath 4 Foundation 4a Mask 6 copper electrode 8. Switch 10 DC power supply 12 Rotational drive source 14 Fan 16 Protective layer (copper plating layer) 22 Plating bath 26 Nickel Electrode 28 Switch 30 DC power supply 32 Rotational drive source 34 Fans 36 Grindstone Department A Copper plating solution B Nickel plating solution C Additives 10 Grinding equipment 11 First Cassette 12 Second Cassette 13 Carrying in / out means 15,16 Means of transportation 17~19 Chuck table 20 Turntable 30,40 Grinding means 37,47 Grinding wheels

Claims

1. A diamond abrasive for a semiconductor member processing grindstone using HPHT single crystal diamond abrasive, the average value of the diamond peak wavenumber obtained by diamond peak measurement by Raman spectroscopy performed on the HPHT single crystal diamond abrasive grain is smaller than the average value of the diamond peak wavenumber obtained by measurement by Raman spectroscopy performed on a type IIa single crystal diamond, The HPHT single crystal diamond abrasive grains are annealed at a temperature of less than 800° C.

1. A diamond abrasive grain for use as a grinding wheel for processing semiconductor components.

2. The diamond abrasive grains for use as a grinding wheel for processing semiconductor members according to claim 1, which are used for cutting, polishing, or grinding.

3. 3. The diamond abrasive grain for use as a grinding wheel for processing semiconductor components according to claim 1 or 2, which has crystal nuclei and / or crystal defects derived from a carbon compound.

4. 3. The diamond abrasive grain for use as a grinding wheel for processing semiconductor components according to claim 1 or 2, which has a smooth crystal face.

5. 3. The diamond abrasive grains for use as a grinding wheel for processing semiconductor components according to claim 1 or 2, having an average particle size of 0.25 to 50 μm or less.

6. The method for producing diamond abrasive grains for semiconductor material processing grindstones according to claim 1 or 2, comprising irradiating HPHTIb type synthetic diamond particles with at least one of ions, electron beams, proton beams, neutron beams, and gamma rays, and then annealing the particles at a temperature of less than 800°C for 10 to 240 minutes.

7. 7. The method for producing diamond abrasive grains for use in semiconductor component processing wheels according to claim 6, comprising mixing raw materials consisting of amorphous carbon and a carbon compound having a hydrogen and / or hydroxyl group in a mass ratio of amorphous carbon:carbon compound=7:3 to 4:6, and synthesizing the diamond abrasive grains by maintaining the mixture under conditions of a pressure of 5 to 10 GPa and a temperature of 1300 to 1800°C for 1 to 300 seconds.

8. 8. The method for producing diamond abrasive grains for use in a grinding wheel for processing semiconductor components according to claim 7, wherein the amorphous carbon is carbon black, and the carbon compound is at least one of an aliphatic hydrocarbon, an alcohol, and a polyhydric alcohol.

9. 9. The method for manufacturing diamond abrasive grains for use in semiconductor component processing wheels as described in claim 8, wherein the aliphatic hydrocarbon is polyethylene, the alcohol is methanol, and the polyhydric alcohol is pentaerythritol or xylitol.

10. A diamond abrasive grain for use as a grinding wheel for processing semiconductor components, as described in claim 3, having a smooth crystal surface.

11. Diamond abrasive grains for use in semiconductor component processing wheels as described in claim 3, having an average particle size of 0.25 to 50 μm or less.

12. Diamond abrasive grains for use in semiconductor component processing wheels as described in claim 4, having an average particle size of 0.25 to 50 μm or less.

13. A method for manufacturing diamond abrasive grains for use in semiconductor component processing wheels as described in claim 3, comprising irradiating HPHTIb type synthetic diamond particles with at least one of ions, electron beams, proton beams, neutron beams, and gamma beams, and then annealing the particles at a temperature of less than 800°C for 10 to 240 minutes.

14. A method for producing diamond abrasive grains for use in semiconductor component processing wheels as described in claim 13, comprising mixing raw materials consisting of amorphous carbon and a carbon compound having a hydrogen and / or hydroxyl group in a mass ratio of amorphous carbon:carbon compound=7:3 to 4:6, and synthesizing the diamond abrasive grains by holding the mixture under conditions of a pressure of 5 to 10 GPa and a temperature of 1300 to 1800°C for 1 to 300 seconds.

15. A method for manufacturing diamond abrasive grains for semiconductor component processing wheels as described in claim 14, wherein the amorphous carbon is carbon black, and the carbon compound is at least one of an aliphatic hydrocarbon, an alcohol, and a polyhydric alcohol.

16. A method for manufacturing diamond abrasive grains for semiconductor component processing wheels as described in claim 15, wherein the aliphatic hydrocarbon is polyethylene, the alcohol is methanol, and the polyhydric alcohol is pentaerythritol or xylitol.

17. A method for manufacturing diamond abrasive grains for use in semiconductor component processing wheels as described in claim 4, comprising irradiating HPHTIb type synthetic diamond particles with at least one of ions, electron beams, proton beams, neutron beams, and gamma rays, and then annealing the particles at a temperature of less than 800°C for 10 to 240 minutes.

18. A method for producing diamond abrasive grains for use in semiconductor component processing wheels as described in claim 17, comprising mixing raw materials consisting of amorphous carbon and a carbon compound having a hydrogen and / or hydroxyl group in a mass ratio of amorphous carbon:carbon compound=7:3 to 4:6, and synthesizing the diamond abrasive grains by holding the mixture under conditions of a pressure of 5 to 10 GPa and a temperature of 1300 to 1800°C for 1 to 300 seconds.

19. A method for manufacturing diamond abrasive grains for semiconductor component processing wheels as described in claim 18, wherein the amorphous carbon is carbon black, and the carbon compound is at least one of an aliphatic hydrocarbon, an alcohol, and a polyhydric alcohol.

20. A method for manufacturing diamond abrasive grains for semiconductor component processing wheels as described in claim 19, wherein the aliphatic hydrocarbon is polyethylene, the alcohol is methanol, and the polyhydric alcohol is pentaerythritol or xylitol.

21. A method for manufacturing diamond abrasive grains for use in semiconductor component processing wheels as described in claim 5, comprising irradiating HPHTIb type synthetic diamond particles with at least one of ions, electron beams, proton beams, neutron beams, and gamma beams, and then annealing the particles at a temperature of less than 800°C for 10 to 240 minutes.

22. A method for producing diamond abrasive grains for use in semiconductor component processing wheels as described in claim 21, comprising mixing raw materials consisting of amorphous carbon and a carbon compound having a hydrogen and / or hydroxyl group in a mass ratio of amorphous carbon:carbon compound=7:3 to 4:6, and synthesizing the diamond abrasive grains by holding the mixture under conditions of a pressure of 5 to 10 GPa and a temperature of 1300 to 1800°C for 1 to 300 seconds.

23. A method for manufacturing diamond abrasive grains for semiconductor component processing wheels as described in claim 22, wherein the amorphous carbon is carbon black, and the carbon compound is at least one of an aliphatic hydrocarbon, an alcohol, and a polyhydric alcohol.

24. A method for manufacturing diamond abrasive grains for semiconductor component processing wheels as described in claim 23, wherein the aliphatic hydrocarbon is polyethylene, the alcohol is methanol, and the polyhydric alcohol is pentaerythritol or xylitol.

25. A method for manufacturing diamond abrasive grains for use in semiconductor component processing wheels as described in claim 10, comprising irradiating HPHTIb type synthetic diamond particles with at least one of ions, electron beams, proton beams, neutron beams, and gamma beams, and then annealing the particles at a temperature of less than 800°C for 10 to 240 minutes.

26. A method for producing diamond abrasive grains for use in semiconductor component processing wheels as described in claim 25, comprising mixing raw materials consisting of amorphous carbon and a carbon compound having a hydrogen and / or hydroxyl group in a mass ratio of amorphous carbon:carbon compound=7:3 to 4:6, and synthesizing the diamond abrasive grains by holding the mixture under conditions of a pressure of 5 to 10 GPa and a temperature of 1300 to 1800°C for 1 to 300 seconds.

27. ​​A method for manufacturing diamond abrasive grains for semiconductor component processing wheels as described in claim 26, wherein the amorphous carbon is carbon black, and the carbon compound is at least one of an aliphatic hydrocarbon, an alcohol, and a polyhydric alcohol.

28. A method for manufacturing diamond abrasive grains for semiconductor component processing wheels as described in claim 27, wherein the aliphatic hydrocarbon is polyethylene, the alcohol is methanol, and the polyhydric alcohol is pentaerythritol or xylitol.

29. A method for manufacturing diamond abrasive grains for use in semiconductor component processing wheels as described in claim 11, comprising irradiating HPHTIb type synthetic diamond particles with at least one of ions, electron beams, proton beams, neutron beams, and gamma beams, and then annealing the particles at a temperature of less than 800°C for 10 to 240 minutes.

30. A method for producing diamond abrasive grains for use in semiconductor component processing wheels as described in claim 29, comprising mixing raw materials consisting of amorphous carbon and a carbon compound having a hydrogen and / or hydroxyl group in a mass ratio of amorphous carbon:carbon compound=7:3 to 4:6, and synthesizing the diamond abrasive grains by holding the mixture under conditions of a pressure of 5 to 10 GPa and a temperature of 1300 to 1800°C for 1 to 300 seconds.

31. A method for manufacturing diamond abrasive grains for semiconductor component processing wheels as described in claim 30, wherein the amorphous carbon is carbon black, and the carbon compound is at least one of an aliphatic hydrocarbon, an alcohol, and a polyhydric alcohol.

32. A method for manufacturing diamond abrasive grains for semiconductor component processing wheels as described in claim 31, wherein the aliphatic hydrocarbon is polyethylene, the alcohol is methanol, and the polyhydric alcohol is pentaerythritol or xylitol.

33. A method for manufacturing diamond abrasive grains for use in semiconductor component processing wheels as described in claim 12, comprising irradiating HPHTIb type synthetic diamond particles with at least one of ions, electron beams, proton beams, neutron beams, and gamma beams, and then annealing the particles at a temperature of less than 800°C for 10 to 240 minutes.

34. A method for producing diamond abrasive grains for use in semiconductor component processing wheels as described in claim 33, comprising mixing raw materials consisting of amorphous carbon and a carbon compound having a hydrogen and / or hydroxyl group in a mass ratio of amorphous carbon:carbon compound=7:3 to 4:6, and synthesizing the diamond abrasive grains by holding the mixture under conditions of a pressure of 5 to 10 GPa and a temperature of 1300 to 1800°C for 1 to 300 seconds.

35. A method for manufacturing diamond abrasive grains for semiconductor component processing wheels as described in claim 34, wherein the amorphous carbon is carbon black, and the carbon compound is at least one of an aliphatic hydrocarbon, an alcohol, and a polyhydric alcohol.

36. A method for manufacturing diamond abrasive grains for semiconductor component processing wheels as described in claim 35, wherein the aliphatic hydrocarbon is polyethylene, the alcohol is methanol, and the polyhydric alcohol is pentaerythritol or xylitol.

Citation Information

Patent Citations

  • Voltage detector of variable input resistance type

    JP1980054449A

  • Diamond light-emitting device and manufacture thereof

    JP1990000385A

  • Surface-reinforced diamond and its production

    JP1999071197A

  • Diamond single crystal substrate

    JP2005272191A

  • Method for manufacturing a fancy orange single-crystal CVD diamond and the resulting product

    JP2012530676A