Polyester resin mixture, polyester film and method for producing same

The polyester resin mixture, incorporating cyclohexanedimethanol and specific comonomers, addresses the issue of insufficient shrinkage and fusion with polyethylene terephthalate containers, enabling efficient recycling and high transparency without additional additives.

JP7561186B2Active Publication Date: 2024-10-03SK CHEMICALS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022517370
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-27
Filing Date
2020-07-21
Publication Date
2024-10-03
Estimated Expiration
2040-07-21

AI Technical Summary

Technical Problem

Conventional heat-shrinkable polyester films do not exhibit sufficient heat shrinkage and often fuse with polyethylene terephthalate containers during recycling, making it difficult to recycle them together without separation.

Method used

A polyester resin mixture is developed by polymerizing polyethylene terephthalate with cyclohexanedimethanol and specific comonomers, such as 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol, to enhance shrinkage properties and compatibility with recycled polyethylene terephthalate.

Benefits of technology

The resulting polyester film exhibits excellent shrinkage rates and transparency, allowing it to be recycled with polyethylene terephthalate containers without deformation, even at high drying temperatures, and does not require additional additives for improved miscibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561186000001
    Figure 0007561186000001
  • Figure 0007561186000002
    Figure 0007561186000002
  • Figure 0007561186000003
    Figure 0007561186000003
Patent Text Reader

Abstract

The present invention relates to a polyester resin mixture, a polyester film, and a method for producing the same. The polyester resin mixture can provide heat-shrinkable labels that are transparent and have an excellent shrinkage rate, even when they contain not only virgin polyethylene terephthalate but also recycled polyethylene terephthalate. The heat-shrinkable labels can be recycled while still attached to PET containers, etc., and are therefore expected to be useful in providing sustainable plastics, which have recently been attracting attention.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester resin mixture, a polyester film and a method for producing the same. [Background technology]

[0002] Heat shrinkable films have the property of shrinking when heated, and are used for shrink packaging, shrink labels, etc. Such heat shrinkable films include polyvinyl chloride (PVC) films, polystyrene films, polyester films, etc., and these films are used for labels and cap seals for various containers, or direct packaging, etc.

[0003] However, films made of polyvinyl chloride are classified as regulated due to environmental issues such as the generation of hydrogen chloride gas and dioxin-causing substances when incinerated. Polystyrene films have good workability during the shrinking process and a good product appearance, but they have the disadvantages of requiring ink with a special composition when printing because they have poor chemical resistance and of shrinking spontaneously due to lack of storage stability at room temperature, resulting in deformation in size. Furthermore, when polyvinyl chloride film or polystyrene film is used as a shrink label for polyethylene terephthalate containers, the label and container must be separated in the process of recycling the polyethylene terephthalate containers, which is troublesome.

[0004] In contrast, when a polyester film is used as a label for a polyethylene terephthalate container, it can be input into a process for recycling the polyethylene terephthalate container without separating the label, improving the convenience of the process. In particular, as the amount of polyethylene terephthalate containers used increases recently, interest in polyester films that can be input into a recycling process without separating the label is increasing. However, conventional heat-shrinkable polyester films do not exhibit sufficient heat shrinkage, and the shrinkage characteristics of polyester films need to be improved. In particular, non-crystalline polyester films have a problem of adhesion to the container during the process of washing and drying the container in the recycling process of polyethylene terephthalate containers, making it impossible to recycle the container.

[0005] Therefore, research into polyester films that have better shrinkage properties than existing polyester resins and can be recycled together with polyethylene terephthalate containers is required. Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention provides a polyester resin blend capable of providing a heat shrinkable film with excellent shrink properties.

[0007] The present invention also provides a polyester film formed from the polyester resin mixture and a method for producing the same. [Means for solving the problem]

[0008] According to one embodiment of the present invention, a polyester resin mixture is provided, which comprises a polyester resin having a structure in which an acid portion derived from a dicarboxylic acid or a derivative thereof and a diol containing ethylene glycol and a comonomer are polymerized, and a diol portion derived from a dicarboxylic acid or a derivative thereof and a diol portion derived from a diol containing ethylene glycol and a comonomer are repeated, and the comonomers include cyclohexanedimethanol, 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate, and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol, and the polyester resin comprises 0.2 to 30 mol % of the diol portion derived from 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol based on the total diol portion. Effect of the Invention

[0009] The polyester resin mixture according to one embodiment of the present invention can provide a heat shrinkable label that is transparent and has an excellent shrinkage ratio, even if it contains not only virgin polyethylene terephthalate but also recycled polyethylene terephthalate. Since the heat shrinkable label can be recycled while still attached to a PET container, it is expected to be useful in providing sustainable plastics, which have been attracting attention recently. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, a polyester resin mixture and a polyester film produced therefrom according to specific embodiments of the present invention will be described.

[0011] Unless otherwise stated herein, terminology is used merely to refer to particular embodiments and is not intended to limit the invention. And, the singular includes the plural unless expressly stated to the contrary. The meaning of "comprising" as used in the specification embodies certain features, regions, integers, steps, operations, elements, components and / or components and does not exclude the presence or addition of other specific features, regions, integers, steps, operations, elements, components and / or groups.

[0012] According to one embodiment of the present invention, a polyester resin mixture is provided, which comprises a polyester resin having a structure in which an acid portion derived from a dicarboxylic acid or a derivative thereof and a diol containing ethylene glycol and a comonomer are polymerized, and a diol portion derived from a dicarboxylic acid or a derivative thereof and a diol portion derived from a diol containing ethylene glycol and a comonomer are repeated, and the comonomers include cyclohexanedimethanol, 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate, and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol, and the polyester resin comprises 0.2 to 30 mol % of the diol portion derived from 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol based on the total diol portion.

[0013] The polyester resin has a structure in which a dicarboxylic acid or its derivative and a diol are polymerized, and an acid moiety derived from the dicarboxylic acid or its derivative and a diol moiety derived from the diol are repeated. In this specification, the acid moiety and the diol moiety refer to the residues remaining after hydrogen, hydroxyl groups, or alkoxy groups are removed from the dicarboxylic acid or its derivative and the diol when they are polymerized.

[0014] In this specification, the term "dicarboxylic acid or its derivative" refers to one or more compounds selected from dicarboxylic acids and dicarboxylic acid derivatives. And, "dicarboxylic acid derivative" refers to alkyl esters of dicarboxylic acids (lower alkyl esters having 1 to 4 carbon atoms, such as monomethyl, monoethyl, dimethyl, diethyl, or dibutyl esters) or anhydrides of dicarboxylic acids. Therefore, for example, terephthalic acid or its derivatives refers to compounds that react with diols to form a terephthaloyl moiety, such as terephthalic acid; monoalkyl or dialkyl terephthalate; and terephthalic anhydride.

[0015] The polyethylene terephthalate is widely used commercially due to its low price and excellent physical / chemical properties, but it does not exhibit a sufficient heat shrinkage rate to provide a heat shrinkable label, and it has high crystallinity, requiring high processing temperatures, and has a high crystallization rate, which limits its ability to provide transparent products.

[0016] As a result of extensive research aimed at solving such problems, the present inventors have found that a polyester film having excellent transparency and shrinkage can be provided by blending polyethylene terephthalate with a polyester resin containing a diol portion derived from a comonomer containing cyclohexanedimethanol, 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate, and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol, among which the diol portion derived from 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol is within the above-mentioned range, thereby completing the present invention.

[0017] The polyester film can be heat-shrinked at a low temperature similar to that of polyvinyl chloride film, and has an excellent shrinkage rate, so it can be used as a heat-shrinkable label for polyethylene terephthalate (PET) containers without causing deformation or clouding of the PET containers.

[0018] In addition, in the case of a typical heat shrinkable label, it is fused to a PET container during the process of washing and drying for recycling used PET containers, and is removed before the PET container is supplied to the recycle stream. However, in the case of a heat shrinkable label manufactured from the polyester resin mixture according to one embodiment of the present invention, it can be crystallized even at a high drying temperature, so there is an advantage that it can be supplied to the PET container recycle stream in a state where it is attached to the PET container.

[0019] 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate is referred to herein for brevity as Diol A, and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol is referred to herein for brevity as Diol B.

[0020] Such a polyester resin mixture will be described in detail below.

[0021] The polyester resin according to one embodiment of the present invention can be blended with various types of commonly used polyethylene terephthalates to adjust its shrinkage characteristics, crystallinity, and crystallization rate to appropriate levels, thereby providing polyester films and thick containers with high transparency and excellent shrinkage.

[0022] Therefore, the type of the polyethylene terephthalate is not particularly limited. As a non-limiting example, the polyethylene terephthalate is produced by polymerizing a dicarboxylic acid or a derivative thereof with a diol, and the dicarboxylic acid or a derivative thereof may be mainly terephthalic acid or a derivative thereof, and the diol may be mainly ethylene glycol.

[0023] The polyethylene terephthalate may contain an acid portion derived from a comonomer other than terephthalic acid or its derivative. Specifically, the comonomer may be at least one selected from the group consisting of aromatic dicarboxylic acids or their derivatives having 8 to 14 carbon atoms and aliphatic dicarboxylic acids or their derivatives having 4 to 12 carbon atoms. The aromatic dicarboxylic acids or their derivatives having 8 to 14 carbon atoms may include aromatic dicarboxylic acids or their derivatives that are commonly used in the production of polyester resins, such as isophthalic acid, dimethyl isophthalate, phthalic acid, dimethyl phthalate, phthalic anhydride, naphthalenedicarboxylic acids such as 2,6-naphthalenedicarboxylic acid, dialkyl naphthalenedicarboxylates such as dimethyl 2,6-naphthalenedicarboxylate, and diphenyl dicarboxylic acid. The aliphatic dicarboxylic acid or its derivative having 4 to 12 carbon atoms may include cyclohexanedicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid and 1,3-cyclohexanedicarboxylic acid, cyclohexanedicarboxylates such as dimethyl 1,4-cyclohexanedicarboxylate and dimethyl 1,3-cyclohexanedicarboxylate, and linear, branched or cyclic aliphatic dicarboxylic acids or their derivatives that are commonly used in the manufacture of polyester resins such as sebacic acid, succinic acid, isodecylsuccinic acid, maleic acid, maleic anhydride, fumaric acid, adipic acid, glutaric acid, azelaic acid, etc. The comonomer may be used in an amount of 0 to 50 mol%, 0 to 30 mol%, 0 to 20 mol%, or 0 to 10 mol% based on the total dicarboxylic acid or its derivative.

[0024] The polyethylene terephthalate may contain a diol portion derived from a comonomer other than ethylene glycol. Specifically, the comonomer may be an aromatic diol having 8 to 40 or 8 to 33 carbon atoms, an aliphatic diol having 2 to 20 or 2 to 12 carbon atoms, or a mixture thereof. Specific examples of the aromatic diol include bisphenol A derivatives to which ethylene oxide and / or propylene oxide are added, such as polyoxyethylene-(n)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(n)-2,2-bis(4-hydroxyphenyl)propane, or polyoxypropylene-(n)-polyoxyethylene-(n)-2,2-bis(4-hydroxyphenyl)propane (where n represents the number of polyoxyethylene or polyoxypropylene units, and may be, for example, 0 to 10). Specific examples of the aliphatic diol include diethylene glycol, triethylene glycol, propanediol (1,2-propanediol, 1,3-propanediol, etc.), 2-methyl-1,3-propanediol, ... Examples of the diol include linear, branched, or cyclic aliphatic diols such as propanediol, 2-methylene-1,3-propanediol, 2-ethyl-1,3-propanediol, 2-isopropyl-1,3-propanediol, 1,4-butanediol, 2,3-butanediol, pentanediol (1,5-pentanediol, 2,4-pentanediol, etc.), 3-methyl-1,5-pentanediol, 3-methyl-2,4-pentanediol, hexanediol (1,6-hexanediol, etc.), neopentyl glycol (2,2-dimethyl-1,3-propanediol), 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, and tetramethylcyclobutanediol. The comonomer can be used in an amount of 0 to 50 mol %, 0 to 30 mol %, 0 to 20 mol %, or 0 to 10 mol % based on the total diol.

[0025] The polyethylene terephthalate is not particularly limited, but in order to have excellent miscibility with the polyester resin and to exhibit better shrinkage properties, the polyethylene terephthalate may have an intrinsic viscosity of 0.50 to 1.2 dl / g or 0.50 to 1.0 dl / g measured at 35°C after dissolving in orthochlorophenol at a concentration of 1.2 g / dl at 150°C for 15 minutes.

[0026] The polyester resin according to the embodiment can complement not only the physical properties of virgin polyethylene terephthalate, but also the deteriorated physical properties of recycled polyethylene terephthalate to an excellent level.

[0027] Recycled polyethylene terephthalate can be understood as including polyethylene terephthalate that has been recovered after use or any product obtained therefrom. Specifically, the recycled polyethylene terephthalate can be obtained by separating recovered waste plastic according to a certain standard, crushing and washing, melt extruding and repelletizing it, or by depolymerizing recovered waste plastic to a monomer level and repolymerizing it. Such recycled polyethylene terephthalate can be repelletized and crystallized according to a processing method and then used, or can be crystallized and further polycondensed in a solid state and then used.

[0028] Recycled polyethylene terephthalate, which is obtained by depolymerizing waste plastics to a monomer level and then repolymerizing it, exhibits such good physical properties that it is difficult to distinguish it from virgin polyethylene terephthalate. However, recycled polyethylene terephthalate is less transparent and has poorer physical properties than virgin polyethylene terephthalate, so it is difficult to produce a film that can shrink to an appropriate level using recycled polyethylene terephthalate alone or mixed with virgin polyethylene terephthalate. However, the polyester resin according to one embodiment exhibits excellent miscibility with such recycled polyethylene terephthalate, making it possible to provide a polyester film that exhibits excellent shrinkage properties when mixed with recycled polyethylene terephthalate. In particular, the polyester resin according to one embodiment has excellent miscibility with recycled polyethylene terephthalate, and can provide a polyester film with excellent shrinkage even without other additives.

[0029] Therefore, the polyethylene terephthalate may be virgin polyethylene terephthalate, recycled polyethylene terephthalate, or a mixture thereof.

[0030] In particular, the polyester resin mixture according to the embodiment contains a recycled polyethylene terephthalate resin having an intrinsic viscosity of 0.50 to 1.2 dl / g or 0.50 to 1.0 dl / g measured at 35°C after dissolving in orthochlorophenol at a concentration of 1.2 g / dl at 150°C for 15 minutes, and exhibits high transparency and excellent processability.

[0031] In addition, the polyester resin according to the embodiment is useful for recycling resins containing 95 mol% or more of acid moieties derived from terephthalic acid and 95 mol% or more of diol moieties derived from ethylene glycol among recycled polyethylene terephthalate. The resin may be a homopolymer made of terephthalic acid and ethylene glycol, so the upper limit of the acid moieties derived from terephthalic acid and the diol moieties derived from ethylene glycol is 100 mol%, and when the acid moieties derived from terephthalic acid or the diol moieties derived from ethylene glycol are less than 100 mol%, the resin may contain up to 5 mol% of acid moieties or diol moieties derived from the above-mentioned comonomers. In particular, the resin may contain up to 5 mol% of acid moieties derived from isophthalic acid and / or up to 5 mol% of diol moieties derived from cyclohexanedimethanol.

[0032] The polyester resin is mixed with recycled polyethylene terephthalate having a crystallization temperature of 130° C. to 160° C., so that the crystallization speed of the recycled polyethylene terephthalate can be efficiently controlled.

[0033] The polyester resin can be mixed with recycled polyethylene terephthalate having a melting point of 250° C. or higher to provide a polyester resin mixture with excellent processability.

[0034] The polyester resin according to one embodiment of the present invention is obtained by polymerizing a diol containing a dicarboxylic acid or a derivative thereof, ethylene glycol, and a comonomer (the comonomer includes cyclohexanedimethanol, diol A, and diol B), and has a structure in which an acid portion derived from the dicarboxylic acid or a derivative thereof, a diol portion derived from ethylene glycol, a diol portion derived from cyclohexanedimethanol, a diol portion derived from diol A, and a diol portion derived from diol B are repeated.

[0035] The polyester resin contains 0.2 to 30 mol % of a diol portion derived from diol A and a diol portion derived from diol B based on the total diol portion, thereby providing a polyester resin mixture having excellent shrinkage properties.

[0036] Specifically, the length of the molecular chain is increased to a certain level or more due to the diol moiety derived from the diol A and the diol B, which is related to the residual stress in the polyester resin, and the residual stress increases when the polyester film produced from the polyester resin mixture is stretched. When heat is supplied to such a polyester film, the shrinkage force increases due to the release of the residual stress, and the polyester film exhibits a high shrinkage rate.

[0037] If the diol portion derived from diol A and diol B is less than 0.2 mol %, the shrinkage properties of polyethylene terephthalate cannot be improved, making it difficult to provide a polyester film with a high shrinkage ratio. If the diol portion derived from diol A and diol B exceeds 30 mol %, it is difficult to ensure a desired viscosity due to a decrease in reactivity during the polymerization of the polyester resin, and a whitening phenomenon occurs due to overstretching during the stretching of a polyester film produced from the polyester resin mixture, reducing its value as a heat shrinkable film.

[0038] In order to exhibit an excellent shrinkage rate even when mixed with a crystalline resin, polyethylene terephthalate, the polyester resin may contain a diol portion derived from diol A and a diol portion derived from diol B in an amount of about 0.2 to 30 mol%, about 0.5 to 30 mol%, about 1 to 30 mol%, about 2 to 30 mol%, about 3 to 30 mol%, about 4 to 30 mol%, about 5 to 30 mol%, about 6 to 30 mol%, about 7 to 30 mol%, about 8 to 30 mol%, about 9 to 30 mol%, or about 10 to 30 mol% based on the total diol portion.

[0039] In order to maximize the above-mentioned effects, the polyester resin may contain 0.1 to 15 mol % of a diol portion derived from diol A and / or 0.1 to 15 mol % of a diol portion derived from diol B based on the total diol portion.

[0040] Meanwhile, the polyester resin may contain 1 to 35 mol %, 1 to 32 mol %, or 1 to 30 mol % of the diol portion derived from cyclohexanedimethanol based on the total diol portion. Within such range, a polyester resin mixture having excellent shrinkage properties and transparency can be provided.

[0041] The cyclohexanedimethanol can be 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,2-cyclohexanedimethanol or mixtures thereof or can be 1,4-cyclohexanedimethanol.

[0042] The polyester resin may contain a diol moiety derived from diethylene glycol in an amount of 2 to 15 mol%, 3 to 15 mol%, 4 to 15 mol%, 5 to 15 mol%, or 10 to 13 mol% based on the total diol moiety. The diol moiety derived from diethylene glycol introduced into the polyester resin may be formed by reacting two ethylene glycols to form diethylene glycol during polymerization of the polyester resin, and reacting the diethylene glycol with a dicarboxylic acid or a derivative thereof. However, the present invention is not limited thereto, and may be formed by adding diethylene glycol as a comonomer other than ethylene glycol during the preparation of the polyester resin in order to adjust the content of the diol moiety derived from diethylene glycol to the above range. The polyester resin may contain a diol moiety derived from diethylene glycol in the above range, thereby providing a polyester resin mixture having excellent shrinkage properties and transparency. In particular, when the polyester resin is prepared by adding diethylene glycol as a comonomer other than ethylene glycol to provide a large amount of diol moiety derived from diethylene glycol, the elongation of the polyester film is improved, allowing high-magnification stretching, and a polyester film having excellent shrinkage properties at a thin thickness may be provided.

[0043] The remaining diol moiety in the polyester resin other than the above diol moiety may be a diol moiety derived from ethylene glycol.

[0044] Meanwhile, the comonomer other than ethylene glycol may include a diol that is commonly used in the preparation of polyester resins in addition to the above-mentioned monomers. Specific examples of such diols include the diols listed above as usable for polyethylene terephthalate.

[0045] For example, the polyester resin may be prepared using 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-methylene-1,3-propanediol, 2-ethyl-1,3-propanediol, 2-isopropyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,5-pentanediol, 3-methyl-2,4-pentanediol, 1,6-hexanediol, 1,2-cyclohexanediol, 1,4-cyclohexanediol, diethylene glycol, or a mixture thereof as a comonomer other than ethylene glycol, and may further include a diol portion derived from the comonomer. Such a comonomer may be appropriately used to improve the moldability and other physical properties of the polyester resin prepared. However, the comonomer other than ethylene glycol is advantageously a combination of the above-mentioned cyclohexanedimethanol, diol A and diol B, or, if necessary, diethylene glycol, in order to satisfy the above-mentioned physical properties. When the comonomer includes cyclohexanedimethanol, diol A and diol B, or, if necessary, a diol other than diethylene glycol, the content thereof may be 10 mol % or less, 5 mol % or less, or 2 mol % or less based on the total comonomer.

[0046] The polyester resin may also contain a dicarboxylic acid or a derivative thereof for producing the polyester resin together with the polyethylene terephthalate described above, which may be mainly terephthalic acid or a derivative thereof, and may contain a comonomer other than terephthalic acid or a derivative thereof. The type and content of the comonomer may be adjusted with reference to the type and content of the comonomer usable for the polyethylene terephthalate described above.

[0047] Depending on the structure described above, the polyester resin may have an intrinsic viscosity of about 0.45-1.2 dl / g, about 0.55-1.0 dl / g, about 0.60-1.0 dl / g, or about 0.60-0.9 dl / g when dissolved in orthochlorophenol at a concentration of 1.2 g / dl for 15 minutes at 150° C. and measured at 35° C. Within these ranges, the polyester resin has an appropriate molecular weight and excellent mechanical properties, and can be molded by mixing with polyethylene terephthalate under mild pressure and temperature.

[0048] The polyester resin may have a glass transition temperature of 60°C to 80°C, 62°C to 78°C, or 63°C to 75°C, depending on the structure described above.

[0049] In addition, the content of the oligomer introduced into the polyester resin may be 3.0 area % or less, 2.0 area % or less, 1.5 area % or less, or 1.0 area % or less with respect to the total polyester resin area. The oligomer means a compound having a molecular weight of 500 to 1000 g / mol, and the polyester resin may not contain an oligomer, so the lower limit of the oligomer content may be 0 area %. As an example, the content of the oligomer introduced into the polyester resin may be 0.1 to 3 area %, 0.1 to 2 area %, 0.1 to 1.5 area %, or 0.1 to 1.2 area % with respect to the total polyester resin area. Within this range, it is possible to provide a polyester film that can prevent an increase in haze due to precipitation of oligomers during stretching at high temperatures, maintain high transparency even after stretching, and minimize the defective rate in the subsequent printing process.

[0050] The polyester resin may be prepared by esterification or transesterification of the above dicarboxylic acid or its derivative with the above diol; and polycondensation of the esterification or transesterification product.

[0051] The esterification or transesterification reaction does not necessarily require a catalyst, but a catalyst is selectively used to shorten the reaction time. Examples of such catalysts include sodium and magnesium methylates, acetates, borates, fatty acid salts, and carbonates of Zn, Cd, Mn, Co, Ca, Ba, etc., metallic Mg, and oxides of Pb, Zn, Sb, Ge, etc.

[0052] The esterification or transesterification reaction may be carried out in a batch, semi-continuous or continuous manner, and each raw material is added separately, but it is preferable to add the diol in the form of a slurry containing the dicarboxylic acid or its derivative. The diol is added in a ratio of about 1.2 to 3.0 moles per mole of the dicarboxylic acid or its derivative.

[0053] A polycondensation catalyst, a stabilizer, a coloring agent, a crystallizing agent, an antioxidant, a branching agent, etc. may be added to the slurry before the esterification or transesterification reaction is started or to the product after the reaction is completed. However, the timing of adding the above-mentioned additives is not limited thereto, and they may be added at any time during the polyester resin production process.

[0054] The polycondensation catalyst may be selected from one or more of the usual titanium, germanium, antimony, aluminum, and tin compounds. Among them, titanium catalysts can copolymerize a large amount of cyclohexanedimethanol with terephthalic acid or its derivatives, and can perform the same level of reaction even with a small amount of antimony catalysts, and are cheaper than germanium catalysts. Examples of useful titanium catalysts include tetraethyl titanate, acetyl tripropyl titanate, tetrapropyl titanate, tetrabutyl titanate, polybutyl titanate, 2-ethylhexyl titanate, octylene glycol titanate, lactate titanate, triethanolamine titanate, acetylacetonate titanate, ethyl acetoacetic ester titanate, isostearyl titanate, titanium dioxide, titanium dioxide / silicon dioxide coprecipitate, and titanium dioxide / zirconium dioxide coprecipitate. The amount of the polycondensation catalyst used varies depending on the desired hue and the stabilizer and coloring agent used, but since it affects the hue of the polymerized polyester resin, it is used so that the amount of titanium element is about 1 to 100 ppm, more preferably about 1 to 50 ppm, based on the weight of the polyester resin. If the amount of titanium element is less than about 1 ppm, the desired degree of polymerization cannot be achieved, and if it exceeds about 100 ppm, the hue of the polyester resin becomes yellow, making it difficult to obtain a transparent polyester film.

[0055] The stabilizer may generally be a phosphorus-based compound such as phosphoric acid, trimethyl phosphate, triethyl phosphate, or triethyl phosphonoacetate, and the amount of the stabilizer may be 10 to 200 ppm based on the amount of phosphorus element relative to the weight of the polyester resin. If the amount of the stabilizer is less than 10 ppm, the stabilizing effect may be insufficient, and the hue of the polyester resin may turn yellow, and if the amount of the stabilizer is more than 200 ppm, the polyester resin may not have a desired high degree of polymerization. In addition, examples of coloring agents added to improve the hue of the polyester resin include ordinary coloring agents such as cobalt acetate and cobalt propionate, and the amount of the stabilizer may be 10 to 200 ppm based on the amount of cobalt element relative to the weight of the polyester resin. If necessary, anthraquinone compounds, perinone compounds, azo compounds, methine compounds, etc. can be used as organic colorants, and commercially available products include toners such as Polysynthren Blue RLS and Solvaperm Red BB from Clarient. The amount of the organic colorant added can be adjusted to 0 to 50 ppm based on the weight of the polyester resin. If the colorant is used at a content outside the above range, the yellow color of the polyester resin may not be sufficiently separated or the physical properties may be deteriorated.

[0056] Examples of the crystallizing agent include a crystal nucleating agent, an ultraviolet absorber, a polyolefin resin, and a polyamide resin. Examples of the antioxidant include a hindered phenol antioxidant, a phosphate antioxidant, a thioether antioxidant, or a mixture thereof. Examples of the branching agent include a general branching agent having three or more functional groups, such as trimellitic anhydride, trimethylol propane, trimellitic acid, or a mixture thereof.

[0057] The esterification reaction is carried out at a temperature of about 200 to 300° C., about 230 to 280° C., about 230 to 265° C., or about 245 to 255° C. and a pressure of 0 to 10.0 kgf / cm 2 (0-7355.6mmHg), 0-5.0kgf / cm 2 (0~3677.8mmHg), 0.1~3.0kgf / cm 2 (73.6~2206.7mmHg) or 1.0~3.0kgf / cm 2 The transesterification reaction can be carried out at a temperature of 150 to 270°C or 180 to 260°C and a pressure of 0 to 5.0 kgf / cm. 2 (0~3677.8mmHg) or 0.1~3.0kgf / cm 2 (73.6 to 2206.7 mmHg). The pressures listed outside the parentheses here are gauge pressures (kgf / cm 2 pressures given in brackets refer to absolute pressures (given in mmHg).

[0058] If the reaction temperature and pressure are outside the above ranges, the physical properties of the polyester resin may be deteriorated. The reaction time (average residence time) is usually 1 to 24 hours or 100 to 300 minutes, and varies depending on the reaction temperature, pressure, and the molar ratio of the diol to the dicarboxylic acid or its derivative used.

[0059] The product obtained by the esterification or transesterification reaction is produced by polycondensation reaction into a polyester resin with a higher degree of polymerization. In general, the polycondensation reaction is carried out at a temperature of 150 to 300°C, 200 to 290°C, 260 to 290°C, 260 to 280°C, or 265 to 275°C and under reduced pressure conditions of 400 to 0.01 mmHg, 100 to 0.05 mmHg, or 10 to 0.1 mmHg. Here, the pressure means the range of absolute pressure. The reduced pressure condition of 400 to 0.01 mmHg is for removing the by-product of the polycondensation reaction, such as glycol, and the unreacted product, such as cyclohexane dimethanol. Therefore, if the reduced pressure condition is out of the above range, the by-product and the unreacted product may not be sufficiently removed. In addition, if the polycondensation reaction temperature is out of the above range, the physical properties of the polyester resin may be deteriorated. The polycondensation reaction is carried out for a time required to reach a desired intrinsic viscosity, for example, for an average residence time of 1 to 24 hours.

[0060] In order to reduce the content of unreacted substances such as cyclohexanedimethanol remaining in the polyester resin, the vacuum reaction may be intentionally maintained for a long time at the end of the esterification reaction or the transesterification reaction or at the beginning of the polycondensation reaction, i.e., when the viscosity of the resin is not high enough, to allow the unreacted raw materials to flow out of the system. When the viscosity of the resin becomes high, it becomes difficult for the raw materials remaining in the reactor to flow out of the system. For example, the reaction product obtained by the esterification reaction or the transesterification reaction before the polycondensation reaction may be left for 0.2 to 3 hours under reduced pressure conditions of about 400 to 1 mmHg or about 200 to 3 mmHg to effectively remove the unreacted substances such as ethylene glycol and cyclohexanedimethanol remaining in the polyester resin. At this time, the temperature of the product may be adjusted to be the same as the esterification reaction or the transesterification reaction temperature, or the polycondensation reaction temperature, or to a temperature between them.

[0061] By adding the step of discharging unreacted raw materials out of the system as described above, the content of unreacted substances such as cyclohexanedimethanol remaining in the polyester resin can be reduced, and as a result, a polyester resin can be produced that can achieve the desired physical properties at a more excellent level.

[0062] On the other hand, the intrinsic viscosity of the polymer after the polycondensation reaction is preferably 0.30 to 1.0 dl / g. If the intrinsic viscosity is less than 0.30 dl / g, the reaction rate in the solid-state reaction is significantly reduced, and if the intrinsic viscosity is more than 1.0 dl / g, the viscosity of the melt during melt polymerization increases, which increases the possibility of the polymer discoloring due to the shear stress between the stirrer and the reactor, and the amount of by-products such as acetaldehyde also increases.

[0063] The polyester resin according to the embodiment may have a higher degree of polymerization by additionally carrying out a solid-state reaction after the polycondensation reaction, if necessary.

[0064] Specifically, the polymer obtained by the polycondensation reaction is discharged outside the reactor and granulated. The granulation method can be either the strand cutting method, in which the polymer is extruded into strands, solidified in a cooling liquid, and then cut with a cutter, or the underwater cutting method, in which the die hole is immersed in the cooling liquid, extruded directly into the cooling liquid, and cut with a cutter. In general, in order to cut without problems in the strand cutting method, the temperature of the cooling liquid must be kept low and the strands must be well solidified. In the underwater cutting method, it is better to maintain the temperature of the cooling liquid according to the polymer and make the shape of the polymer uniform. However, in the case of crystalline polymers, the temperature of the cooling liquid can be intentionally kept high to induce crystallization during extrusion.

[0065] By washing the particulate polymer with water, it is possible to remove unreacted raw materials such as cyclohexanedimethanol that dissolve in water. The smaller the particle, the greater the surface area relative to the weight of the particle, so the smaller the particle size, the more advantageous it is. To achieve this goal, the particles are produced to have an average weight of about 15 mg or less. For example, the particulate polymer is washed by leaving it in water at a temperature equal to the glass transition temperature of the polymer or about 5 to 20°C lower for 5 minutes to 10 hours.

[0066] The particulate polymer undergoes a crystallization stage to prevent it from fusing during the solid-state reaction. It can be carried out in air, inert gas, water vapor, water vapor-containing inert gas atmosphere, or in solution, and the crystallization process is carried out at 110°C to 210°C or 120°C to 210°C. If the temperature is low, the rate at which the particle crystals are generated becomes too slow, and if the temperature is high, the particle surfaces melt faster than the rate at which the crystals are formed, causing the particles to stick together and fuse. As the heat resistance of the particles increases as they crystallize, it is possible to divide the crystallization into several stages and raise the temperature for each stage.

[0067] The solid-state reaction is carried out under an inert gas atmosphere such as nitrogen, carbon dioxide, or argon, or under reduced pressure conditions of 400-0.01 mmHg, at a temperature of 180-220°C, for an average residence time of 1-150 hours. This solid-state reaction further increases the molecular weight and removes the raw materials that remain unreacted in the melting reaction, as well as cyclic oligomers and acetaldehyde that are produced during the reaction.

[0068] The crystallized polymer is dissolved in orthochlorophenol at a concentration of 1.2 g / dl at 150° C. for 15 minutes and solid-state polymerized to reach an intrinsic viscosity of 0.65 dl / g or more, 0.70 dl / g or more, 0.75 dl / g or more, or 0.80 dl / g or more, measured at 35° C.

[0069] Meanwhile, the polyester resin mixture can provide a polyester film that is transparent and has excellent heat shrinkage properties without any special additives even if it contains up to about 50% by weight of recycled polyethylene terephthalate as polyethylene terephthalate. Therefore, the mixing ratio of polyethylene terephthalate and polyester resin in the polyester resin mixture is not particularly limited.

[0070] As non-limiting examples, the polyester resin mixture may include polyethylene terephthalate and polyester resin in a weight ratio of 1:99 to 99:1, 1:99 to 80:20, 1:99 to 70:30, 1:99 to 60:40, 1:99 to 50:50, or 5:95 to 50:50.

[0071] For example, when the polyester resin mixture contains polyethylene terephthalate and polyester resin in a weight ratio of 1:99 to 50:50 or 5:95 to 50:50, it is possible to provide a polyester film exhibiting excellent shrinkage properties.

[0072] The polyester resin mixture has a diol moiety derived from cyclohexanedimethanol contained in the polyethylene terephthalate and polyester resin of 0.5 to 32 mol % based on the total diol moiety contained in the polyethylene terephthalate and polyester resin, thereby providing a polyester film having excellent transparency and shrinkage properties, and the polyester film can exhibit excellent chemical resistance during printing.

[0073] The polyester resin mixture according to the embodiment includes recycled polyethylene terephthalate, and has an advantage that the compatibility of the polyester resin with the recycled polyethylene terephthalate is very good, and therefore no additives are required to complement the physical properties of the recycled polyethylene terephthalate. However, as a non-limiting example, the polyester resin mixture may include additives commonly used in the technical field to which the present invention pertains.

[0074] Meanwhile, according to another embodiment of the present invention, there is provided a polyester film formed from the polyester resin mixture and a method for producing the same.

[0075] The polyester film is transparent and exhibits excellent shrinkage properties when formed from the polyester resin mixture according to the embodiment.

[0076] For example, the polyester film may exhibit high transparency when it has a thickness of 50 μm and a haze of 5% or less, 4% or less, 3% or less, 2.5% or less, 2% or less, or 1% or less, as measured according to ASTM D1003-97. Theoretically, a haze of 0% is most preferable, so the lower limit may be 0% or more.

[0077] In addition, since the polyester film has a low shrinkage start temperature of 65° C. or less, when used as a heat shrinkable label for a PET container, it can be molded with excellent quality without causing deformation or clouding of the PET container. Moreover, the polyester film exhibits a maximum shrinkage rate of 55% or more, 60% or more, 65% or more, 70% or more, or 75% or more at 95° C., thereby providing a heat shrinkable film with excellent quality. The upper limit of the maximum shrinkage rate is not particularly limited, and may be 85% or less, for example.

[0078] The polyester film may be a monolayer film or may be a multilayer film containing two or more layers.

[0079] When the polyester film is a single-layer film, it is suitable to produce the film from a polyester resin mixture in which polyethylene terephthalate and polyester resin are mixed in a weight ratio of 1:99 to 50:50 or 5:95 to 50:50 in order to exhibit excellent shrinkage properties.

[0080] When the polyester film is a multi-layer film, the multi-layer film may include a core layer and a skin layer.

[0081] The resin layer may be formed on one or both sides of the base layer, and at least one surface of the polyester film may be a resin layer. In this structure, by adjusting the types and blending ratio of polyethylene terephthalate and polyester resin so that the base layer exhibits excellent shrinkage characteristics, and adjusting the types and blending ratio of polyethylene terephthalate and polyester resin so that the resin layer exhibits crystallinity, it is possible to provide a heat shrinkable film that has excellent shrinkage characteristics and can be recycled with PET containers without causing a fusion phenomenon even when supplied to a PET container recycle stream.

[0082] As an example, if the base layer contains polyethylene terephthalate and polyester resin in a weight ratio of 0:100 to 50:50, and the resin layer contains polyethylene terephthalate and polyester resin in a weight ratio of 10:90 to 100:0, excellent shrinkage properties and crystallinity can be exhibited simultaneously.

[0083] Meanwhile, the polyester film may include two or more substrate layers and two or more resin layers. As a non-limiting example, the polyester film may have a structure in which a first resin layer is formed on a first substrate layer, a second substrate layer is formed on the first resin layer, and a second resin layer is further formed on the second substrate layer.

[0084] Regardless of whether the polyester film is a single-layer film or a multi-layer film, the weight ratio of polyethylene terephthalate and polyester resin contained in the entire polyester film is controlled to 5:95 to 50:50, thereby exhibiting excellent shrinkage properties and crystallinity at the same time.

[0085] The method for producing the polyester film will now be described in detail.

[0086] The method for producing the polyester film includes the steps of: forming a polyester resin mixture to produce an unstretched film; and stretching the unstretched film.

[0087] The polyester resin mixture is prepared by preparing polyethylene terephthalate and polyester resin in chip or pellet form, drying them, and mixing them with an agitator. Specifically, polyethylene terephthalate and polyester resin are molded into chip or pellet form by a twin-screw extruder. Then, the polyethylene terephthalate in chip or pellet form is dried at about 120 to 160°C, and separately, the polyester resin in chip or pellet form is dried at about 50 to 75°C, and the components are mixed using an agitator to prepare the polyester resin mixture. Alternatively, the polyethylene terephthalate in chip or pellet form and the polyester resin in chip or pellet form may be dried together at about 50 to 160°C, and the components are mixed using an agitator to prepare the polyester resin mixture.

[0088] The polyester resin mixture is then molded to produce an unstretched film. The polyester resin mixture is molded at temperatures of about 230°C to 310°C, about 240°C to 300°C, or about 250°C to 290°C to minimize thermal decomposition of the polymer, maintain the long chain structure of the polymer, and minimize the problem of damage or breakage of the film during the subsequent stretching process.

[0089] Specifically, a mixture of polyethylene terephthalate in the form of chips or pellets and a polyester resin is fed to an extruder, and the cylinder temperature is adjusted to the above-mentioned range to obtain an unstretched film.

[0090] If the polyester film has a multi-layer structure, two or more layers can be molded sequentially or simultaneously, that is, one layer can be molded on top of the other layer, or two or more layers can be molded at the same time by coextrusion or the like.

[0091] The unstretched film obtained by the above method is cooled to an appropriate temperature. Although not particularly limited, the produced unstretched film is closely attached to a cooling roll at about 10 to 70°C, wound up, and supplied to the next process.

[0092] In the step of stretching the unstretched film, the unstretched film is stretched in the machine direction and / or the transverse direction to provide a uniaxially stretched film or a biaxially stretched film.

[0093] The stretching temperature of the unstretched film may be a temperature equal to or higher than the glass transition temperature of the polyester resin. Specifically, the unstretched film is stretched at a temperature of 55°C to 180°C or 60°C to 170°C.

[0094] The unstretched film is stretched at a high ratio. For example, the unstretched film is uniaxially stretched at a transverse stretch ratio of 1.5 to 6 times or a longitudinal stretch ratio of 1.1 to 5 times. For another example, the unstretched film is biaxially stretched at a transverse stretch ratio of 1.5 to 6 times and a longitudinal stretch ratio of 1.1 to 5 times.

[0095] The polyester film may have a semi-crystallization time of 0.1 to 100 minutes, 0.1 to 80 minutes, 0.1 to 70 minutes, 0.1 to 60 minutes, 0.1 to 50 minutes, 0.1 to 40 minutes, 0.1 to 30 minutes, 0.1 to 20 minutes, 0.1 to 10 minutes, 0.1 to 7 minutes, 0.1 to 6 minutes, 0.1 to 5 minutes, 0.1 to 4 minutes, 0.1 to 3 minutes, 0.1 to 2 minutes, 0.1 to 1 minute, or 0.5 to 1 minute so that fusion problems do not occur when the polyester film is supplied to a recycle stream together with PET containers.

[0096] The thickness of the polyester film is not particularly limited, but may be 3 μm to 350 μm. If the polyester film is a multi-layer film, the percentage of the resin layer thickness to the base layer thickness (resin layer thickness / base layer thickness×100) may be 2.5% to 50%, and the percentage of the resin layer thickness to the polyester film thickness (resin layer thickness / polyester film thickness×100) may be 1% to 50%.

[0097] The polyester film can be applied to various technical fields to which the present invention belongs, and is expected to be usefully used as a heat shrinkable label for PET containers and the like due to its excellent shrinkage properties and transparency.

[0098] The functions and effects of the present invention will be described in more detail below with reference to specific examples of the present invention, however, these are presented as examples of the present invention and do not limit the scope of the invention in any way.

[0099] The following physical properties were measured by the following methods.

[0100] (1) Intrinsic viscosity (IV) The sample was dissolved in o-chlorophenol at a concentration of 1.2 g / dl at 150°C for 15 minutes, and the intrinsic viscosity of the sample was measured using an Ubbelohde viscometer. Specifically, the temperature of the viscometer was maintained at 35°C, and the efflux time t0, which is the time it takes for the solvent to pass through a specific internal section of the viscometer, and the time t, which is the time it takes for the solution to pass through, were determined. The t0 and t values ​​were then substituted into equation 1 to calculate the specific viscosity, and the calculated specific viscosity value was substituted into equation 2 to calculate the intrinsic viscosity.

[0101]

number

[0102] In the above formula 2, A is the Huggins constant, 0.247, and c is the concentration value, 1.2 g / dl.

[0103] (2) Glass transition temperature (Tg) The Tg of polyester resin was measured by DSC (differential scanning calorimetry). The measuring device used was a Mettler Toledo DSC 1 model. Specifically, the polyester resin sample used for analysis was dried for 5 to 10 hours under a nitrogen atmosphere at 60°C using a dehumidifying dryer (Moretto model D2T). Therefore, Tg was measured when the moisture content remaining in the sample was less than 500 ppm. Approximately 6 to 10 mg of the dried sample was taken and filled into an aluminum pan, heated at room temperature to 280°C at a rate of 10°C / min (first scan), and annealed at 280°C for 3 minutes. After that, the sample was rapidly cooled to room temperature and then heated again at room temperature to 280°C at a rate of 10°C / min (second scan) to obtain a DSC curve. The Tg value was analyzed by the second DSC scan using the glass transition function in the DSC menu of the related program (STARe software) provided by Mettler Toledo. In this case, Tg was defined as the temperature at which the DSC curve obtained during the second scan first changes into a step-like shape during the heating process and the maximum slope of the curve appears, and the scan temperature range was set from -20°C to 15°C, which is the midpoint calculated by the program, to 15°C to 20°C.

[0104] (3) Oligomer content 0.3g of the polyester resin prepared in Preparation Example was dissolved in 15mL of o-chlorophenol at 150℃ for 15 minutes, cooled to room temperature, and then 9mL of chloroform was added. Gel permeation chromatography was performed using a Tosoh column and an RI detector. From the molecular weight graph of the polyester resin obtained in this way, the ratio of the molecular weight area of ​​500~1000g / mol to the total molecular weight area was calculated and defined as the oligomer content of the polyester resin.

[0105] (4) Maximum shrinkage rate The polyester films prepared in the Examples and Comparative Examples were cut into 5 cm x 5 cm squares, which were then immersed in 95°C warm water for 10 seconds and then removed. The ratio of the reduced length to the initial length was calculated using the following formula 3 and defined as the maximum shrinkage at 95°C.

[0106] [Formula 3] Maximum shrinkage rate (%) = (initial length - length measured after immersion) / initial length x 100 (5) Shrinkage start temperature The polyester films manufactured in the examples and comparative examples were cut into 5cm x 5cm squares, which were then immersed in warm water at various temperatures in the range of 55°C to 100°C for 10 seconds and then removed. The ratio of the reduced length to the initial length was calculated using Equation 3, and the temperature at which the film shrunk to 2% or less was defined as the shrinkage initiation temperature.

[0107] (6) Hayes The polyester films produced in the examples and comparative examples were cut to a size of 10 cm x 10 cm (longitudinal length x horizontal length) to prepare test pieces. The parallel transmittance and diffuse transmittance of the test pieces were measured using a Minolta CM-3600A measuring instrument according to the ASTM D1003-97 measurement method. The transmittance is defined as the sum of the parallel transmittance and the diffuse transmittance, and the haze is defined as the percentage of the diffuse transmittance relative to the transmittance (haze = diffuse transmittance / transmittance x 100). Therefore, the transmittance and haze were calculated from the parallel transmittance and diffuse transmittance of the test pieces.

[0108] (7) Whether or not the polyester film and PET container are fused together Polyester film and polyethylene terephthalate containers (PET containers) were simultaneously crushed to obtain flakes with a bulk density of about 250-600g / L. The polyester foil pieces and PET container flakes obtained in this way were left at 160℃ for 1 hour, and the presence or absence of fusion between the polyester foil pieces and the PET container flakes was observed with the naked eye. If any fusion was observed, it was indicated by "O", and if not, it was indicated by "X".

[0109] (8) Crystallization half time The half-crystallization time of the polyester film was measured by DSC (differential scanning calorimetry). Specifically, the polyester film was rapidly heated to 140°C and then maintained at 140°C, and the time (unit: min) at which half of the total heat generated during crystallization was generated was measured.

[0110] Production Example 1: Production of polyester resin Terephthalic acid, ethylene glycol, diethylene glycol, 1,4-cyclohexanedimethanol, 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate (hereinafter, diol A), and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol (hereinafter, diol B) were added to a 3 kg batch reactor connected to a column and a condenser capable of being cooled by water. The monomers were added in appropriate amounts so that the acid portion derived from terephthalic acid was 100 mol% of the total acid portion contained in the produced polyester resin, and the diol portion derived from 1,4-cyclohexanedimethanol was 7 mol%, the diol portion derived from diethylene glycol was 12 mol%, the diol portion derived from diol A was 13 mol%, the diol portion derived from diol B was 2 mol%, and the diol portion derived from ethylene glycol was 66 mol% of the total diol portion. In addition, 0.3g of tetrabutyl titanate was used as a catalyst, 0.4g of phosphoric acid as a stabilizer, and 2.1g of cobalt acetate as a coloring agent. Next, nitrogen was injected into the reactor until the pressure in the reactor was 1.0kgf / cm above normal pressure. 2 The pressure was increased by 1495.6 mmHg (absolute pressure: 1495.6 mmHg).

[0111] The temperature of the reactor was then raised to 220°C over 90 minutes, maintained at 220°C for 2 hours, and then raised to 260°C over 2 hours. The temperature of the reactor was then maintained at 260°C until the mixture in the reactor was observed with the naked eye and became transparent, and an esterification reaction was carried out. When the esterification reaction was completed, the nitrogen in the pressurized reactor was discharged to the outside, the pressure in the reactor was reduced to normal pressure, and the mixture in the reactor was transferred to a 3 kg reactor capable of vacuum reaction.

[0112] The reactor pressure was then lowered to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes under normal pressure, and the reactor temperature was raised to 270°C over 1 hour, and the polycondensation reaction was carried out while maintaining the reactor pressure at 1 Torr (absolute pressure: 1 mmHg) or less. The stirring speed was set to be fast at the beginning of the polycondensation reaction, or the stirring speed was appropriately adjusted when the stirring force weakened due to the increase in viscosity of the reactants accompanying the progress of the polycondensation reaction or the temperature of the reactants rose above the set temperature. The polycondensation reaction was carried out until the intrinsic viscosity (IV) of the mixture (melt) in the reactor was 0.77 dl / g. When the intrinsic viscosity of the mixture in the reactor reached a desired level, the mixture was discharged outside the reactor and made into strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg.

[0113] Production Examples 2 to 8 and Comparative Production Examples 1 to 4: Production of polyester resins Polyester resins were produced in the same manner as in Production Example 1, except that the contents of the diol moiety derived from 1,4-cyclohexanedimethanol, the diol moiety derived from diethylene glycol, the diol moiety derived from diol A, and the diol moiety derived from diol B relative to the total diol moiety in the polyester resin were changed as shown in Table 1.

[0114] [Table 1]

[0115] In Table 1, CHDM is the mol % of the diol portion derived from 1,4-cyclohexanedimethanol relative to the total diol portion, DEG is the mol % of the diol portion derived from diethylene glycol relative to the total diol portion, diol A is the mol % of the diol portion derived from diol A relative to the total diol portion, diol B is the mol % of the diol portion derived from diol B relative to the total diol portion, and the remaining diol portion is the diol portion derived from ethylene glycol.

[0116] Example 1: Preparation of polyester resin mixture and polyester film 1) Manufacture of polyester resin mixtures The polyester resin prepared in Preparation Example 1 was mixed with recycled PET resin in a weight ratio of 95:5 to prepare a polyester resin mixture.

[0117] Specifically, the recycled PET resin, which was obtained by crushing and washing waste plastic and then melt-extruding the flakes to re-pelletize them, was dry-mixed at room temperature with the polyester resin pelletized separately, and dried at a temperature of 50°C to 150°C to produce a polyester resin mixture.

[0118] The composition of recycled PET resin varies depending on the region where the waste plastic is collected, the method of sorting the waste plastic, and the method of re-pelletizing it. The recycled PET resin used in this experiment is a copolymer made of terephthalic acid, isophthalic acid, and ethylene glycol, with an isophthalic acid content of 3 mol% or less of the total dicarboxylic acid, an intrinsic viscosity (IV) of 0.74 dl / g, a crystallization temperature of 130°C, and a melting point of 250°C.

[0119] The polyester resin mixture prepared by mixing the polyester resin with recycled PET resin in a weight ratio of 95:5 was used as a polyester resin mixture for forming a base layer, and the polyester resin prepared in Preparation Example 1 was mixed with recycled PET resin in a weight ratio of 90:10 in the same manner as described above to prepare a polyester resin mixture for forming a resin layer.

[0120] 2) Polyester film manufacturing The polyester resin mixture for forming the base layer and the polyester resin mixture for forming the resin layer were co-extruded through a die at a temperature of 260°C to 290°C, and then cooled to 20°C to 50°C to produce an unstretched film with a three-layer structure in which the first and second resin layers were formed on both sides of the base layer. The unstretched film was then reheated to 75°C to 90°C and stretched five times in the transverse direction to produce a polyester film.

[0121] The polyester film thus produced had a base layer thickness of 40 μm, and each resin layer had a thickness of 5 μm.

[0122] Examples 2 to 13 and Comparative Examples 1 to 7: Production of polyester resin mixtures and polyester films Polyester resin mixtures and polyester films were produced in the same manner as in Example 1, except that the type of polyester resin and the content of recycled PET resin in the polyester resin mixture for forming the base layer and the polyester resin mixture for forming the resin layer were changed as shown in Table 2 below.

[0123] [Table 2]

[0124] Test example: Evaluation of the physical properties of polyester film The polyester films produced in the examples and comparative examples were evaluated by the above-mentioned methods, and the results are shown in Table 3.

[0125] [Table 3]

[0126] Referring to Table 3, in Examples 1 to 13, polyester resins containing 0.2 to 30 mol % of diol moieties derived from diol A and diol B based on the total diol moiety are mixed with recycled PET resin to effectively slow down the crystallization rate of recycled PET resin to provide highly transparent polyester films, and it is confirmed that the polyester films are not fused to PET container flakes at a high temperature of 160° C. due to the elevated crystallization temperature. In particular, the polyester films according to Examples 1 to 13 have a very low shrinkage initiation temperature and a significantly improved maximum shrinkage rate compared to films made from recycled PET resin, and are expected to be useful as heat shrinkable films.

[0127] In contrast, the polyester films of Comparative Examples 1 to 5 were produced by mixing a polyester resin not containing a diol moiety derived from diol A and diol B with recycled PET resin, and therefore did not exhibit a sufficiently low shrinkage initiation temperature and a sufficient shrinkage rate. In addition, the polyester resin not containing a diol moiety derived from diol A and diol B exhibits non-crystalline properties, and when the blending ratio of recycled PET resin is low, it is confirmed that the polyester film exhibits non-crystalline properties and is fused with PET container flakes, making it impossible to provide a polyester film that can be recycled continuously.

Claims

1. Polyethylene terephthalate; and a polyester resin having a structure in which a dicarboxylic acid or a derivative thereof and a diol containing ethylene glycol and a comonomer are polymerized, and an acid portion derived from the dicarboxylic acid or a derivative thereof and a diol portion derived from the diol containing ethylene glycol and a comonomer are repeated, the comonomers include cyclohexanedimethanol, 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate, and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol; The polyester resin contains 0.2 to 30 mol % of a diol portion derived from 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate and 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol based on the total diol portion; The content of oligomers having a molecular weight of 500 to 1000 g / mol introduced into the polyester resin is 3.0% or less by area based on the total area of ​​the polyester resin.

2. 2. The polyester resin blend of claim 1, wherein the polyethylene terephthalate is virgin polyethylene terephthalate, recycled polyethylene terephthalate, or a mixture thereof.

3. 2. The polyester resin mixture according to claim 1, wherein the polyester resin contains 0.1 to 15 mol % of a diol portion derived from 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate based on the total diol portion.

4. 2. The polyester resin mixture according to claim 1, wherein the polyester resin contains 0.1 to 15 mol % of a diol portion derived from 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol based on the total diol portion.

5. 2. The polyester resin mixture according to claim 1, wherein the polyester resin contains 1 to 35 mol % of a diol portion derived from cyclohexanedimethanol based on the total diol portion.

6. 2. The polyester resin mixture according to claim 1, wherein the polyester resin contains 2 to 15 mol % of a diol portion derived from diethylene glycol based on the total diol portion.

7. 2. The polyester resin blend of claim 1, wherein the comonomer further comprises 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-methylene-1,3-propanediol, 2-ethyl-1,3-propanediol, 2-isopropyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,5-pentanediol, 3-methyl-2,4-pentanediol, 1,6-hexanediol, 1,2-cyclohexanediol, 1,4-cyclohexanediol, diethylene glycol, or a mixture thereof.

8. the polyester resin comprises acid moieties derived from terephthalic acid or a derivative thereof, or comprises acid moieties derived from terephthalic acid or a derivative thereof and a comonomer of a dicarboxylic acid or a derivative thereof; The polyester resin mixture according to claim 1, wherein the dicarboxylic acid comonomer or a derivative thereof is at least one selected from the group consisting of isophthalic acid, dimethyl isophthalate, phthalic acid, dimethyl phthalate, phthalic anhydride, 2,6-naphthalenedicarboxylic acid, dimethyl 2,6-naphthalenedicarboxylate, diphenyldicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, dimethyl 1,4-cyclohexanedicarboxylate, dimethyl 1,3-cyclohexanedicarboxylate, sebacic acid, succinic acid, isodecylsuccinic acid, maleic acid, maleic anhydride, fumaric acid, adipic acid, glutaric acid, and azelaic acid.

9. A polyester film formed from the polyester resin mixture of claim 1.

10. The polyester film of claim 9, wherein the polyester film has a haze of 5% or less when measured according to ASTM D1003-97 at a thickness of 50 μm.

11. The polyester film described in claim 9, wherein the polyester film has a shrinkage onset temperature of 65°C or less.

12. The polyester film described in claim 9, wherein the polyester film has a maximum shrinkage rate of 55% to 85% at 95°C.

13. The polyester film of claim 9, wherein the polyester film is a monolayer film.

14. The polyester film described in claim 9, wherein the polyester film is a multilayer film including a substrate layer and a resin layer.

15. A polyester film as described in claim 14, wherein the base layer contains polyethylene terephthalate and polyester resin in a weight ratio of 0:100 to 50:50, and the resin layer contains polyethylene terephthalate and polyester resin in a weight ratio of 10:90 to 100:

0.

16. The polyester film described in claim 9, wherein the polyester film is uniaxially stretched at a transverse stretch ratio of 1.5 to 6 times or a longitudinal stretch ratio of 1.1 to 5 times.

17. The polyester film of claim 9, wherein the polyester film is biaxially stretched at a transverse stretch ratio of 1.5 to 6 times and a longitudinal stretch ratio of 1.1 to 5 times.

18. The polyester film of claim 9, wherein the polyester film has a half-crystallization time of 0.1 minutes to 100 minutes.

19. The polyester film described in Claim 14, wherein the percentage of the resin layer thickness relative to the substrate layer thickness is 2.5% to 50%.

20. A polyester film described in claim 13 or 14, wherein the weight ratio of polyethylene terephthalate and polyester resin contained in the entire polyester film is 5:95 to 50:

50.

21. A method for producing a polyester film, comprising the steps of: molding the polyester resin mixture described in claim 1 to produce an unstretched film; and stretching the unstretched film.

Citation Information

Patent Citations

  • Heat shrinking film

    JP1998204273A

  • Reactor grade copolyester for shrink film

    JP2003531214A

  • Copolyester resin and molded product using the same

    JP2016516878A

  • Heat-shrinkable film containing copolyester resin

    JP2016521806A

  • Heat-shrinkable film-forming composition containing polyethylene terephthalate resin and copolymerized polyester resin, and heat-shrinkable film

    JP2016521807A