Method, manufacturing system and component for producing layers - Patents.com
The method of using preformed fusible sections on components addresses the limitations of existing layer production by achieving high deposition rates and improved process quality, resulting in efficient and cost-effective production of corrosion-resistant and wear-resistant components.
Patent Information
- Application Number
- JP2023508016
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-08-07
- Filing Date
- 2021-07-22
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2041-07-22
AI Technical Summary
Existing methods for producing layers on components, particularly for corrosion-resistant and wear-resistant coatings, face limitations such as low deposition rates, process instability, and inefficiency, especially for rotationally symmetrical components, with current welding and laser processes failing to achieve time- and cost-effective application of thicker layers.
A method involving the use of preformed fusible sections, such as helically shaped wire elements, which are placed on a base and melted to form a material bond, allowing for high deposition rates and reduced process complexity, using a laser unit with lower beam quality requirements.
Achieves deposition rates up to 20 kg/h, significantly faster than previous methods, with improved process quality and reduced equipment costs, enabling the production of components with homogeneous microstructures and reduced heat-affected zones.
Smart Images

Figure 0007561270000001 
Figure 0007561270000002 
Figure 0007561270000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a layer, in particular to a method for coating and / or producing a component, a manufacturing system and a component. [Background technology]
[0002] Coating with corrosion- and / or wear-resistant materials is one of the processes to make components functional and increase their service life. For example, overlay welding is a coating process often used in industry. In overlay welding, both the base material and the filler material are melted or fused so that after solidification a layer is formed that is bonded to the base material.
[0003] By creating multiple layers on each top surface, a component that is at least partially productively manufactured can be created. In addition, the process is also used for repair welding, since the appearance and / or function of the component can be restored by adding layers.
[0004] The filler material can be processed as powder, wire and / or strip. One drawback of known processes for producing layers is that the achievable deposition rates are significantly below the metal removal rates of modern milling processes. In comparison with current turning processes, this drawback is even more pronounced, since these processes have higher metal removal rates than milling processes. In particular for rotationally symmetric components, there are currently no welding and / or laser processes that allow the time- and cost-effective application of thicker layers or corresponding additive manufacturing methods. These connections are very important, especially in production chains where the timing of ablation and deposition processes is coordinated with one another.
[0005] Coating and / or productive deposition of components can be performed using various processes. Possible processes include flame spraying, cold gas atomization, arc welding, plasma powder overlay welding, plasma spraying and selected laser processes. In the case of powder charge materials, the machining area can be enlarged relatively easily by increasing the nozzle and focal diameter. Alternatively, acceleration of the machining process can be achieved by increasing the relative movement.
[0006] However, these processes can only produce thin layers close to the contour. Thick layers, especially at armor plates or heels, usually cannot be produced this way. In addition, powder-based processes often have low material efficiency because part of the powder supply is not used for the build-up. This is because some powder particles remain loose on the component and / or machine. In addition, powder-based processes can be hazardous to health.
[0007] The deposition rate for wire-based processes can generally be increased by using multiple wires. Alternatively, it is possible to increase the feed rate of one or more wires. However, these options for increasing the deposition rate are associated with the drawback that they lead to process instabilities. To reduce the instabilities of these processes caused by feeding the wire at high deposition rates, additional energy sources are used. For example, the wire is inductively preheated or a portion of the melting power is provided by an arc welding process. These hybrid processes are often described as combining positive features, but are a compromise between precise controllability and the increased cost of the laser device and the low-cost energy supply of the additional energy source.
[0008] For example, DE 2605841 A1 teaches a process in which a wire is wound around a shaft and is continuously welded to this shaft. However, due to the elasticity of the wire, positioning the wire on the shaft creates play, especially since only a loose fit can be formed due to the elasticity of the wire. Because of this, the wire is not firmly placed on the shaft and can continue to shift. In addition, this process is not suitable for current coating and / or productive component manufacturing applications, since wire feeding and welding must be performed on a single processing device. Therefore, the efficiency of this process is low and the quality produced does not meet current requirements due to the presence of a loose fit. Summary of the Invention [Problem to be solved by the invention]
[0009] It is therefore an object of the present invention to provide a method for producing a layer, in particular for coating and / or producing a component, a manufacturing system and a component, which are able to mitigate or eliminate one or more of the above mentioned drawbacks. In particular, it is an object of the present invention to provide a method which allows to produce a layer and / or to manufacture a component while improving the reliability of the method and / or increasing the application speed. [Means for solving the problem]
[0010] According to a first aspect, the above mentioned object is achieved by a method for forming a layer, in particular for coating and / or producing a component, comprising the steps of placing a preformed fusible part on a base and melting said preformed fusible part to form a material bond between said base and said preformed fusible part.
[0011] The invention is based on the recognition that the complexity of known wire-based processes results in process limitations that can only be overcome with high technical efforts. The method described reduces the process complexity compared to known processes, in particular because no control of the wire feed is required and, as a consequence, possible process errors can be reduced. In particular, attempts to achieve high application speeds with wire-based processes have shown that adequate process quality is often not achieved. The method described allows a high process quality to be achieved due to the reduced process complexity. In particular, it is possible to melt several wires arranged next to each other, surrounded for example by preformed fusible parts.
[0012] The invention is also based on the realization that the filler can be decoupled from the melting process. The placement of the preformed fusible part on the base can be performed completely independent of the melting of the preformed fusible part. The placement of the preformed fusible part on the base can therefore be understood as a set-up process. The subsequent melting process is independent of this set-up process. Thus, the often cost-intensive melting equipment can be fully used to melt the preformed fusible part without set-up times, especially in the form of the placement of the preformed fusible part on the base.
[0013] The invention is also based on the recognition that very high deposition rates can be achieved by the above-mentioned methods. For example, laser deposition welding can have a deposition rate of 2 kg / h. Also, powder-based processes can achieve deposition rates of, for example, up to 14 kg / h. Using a laser spraying process, deposition rates of, for example, 0.5-1.5 kg / h can be achieved. The inventors have found that deposition rates of up to 20 kg / h are achievable using the methods described in the previous paragraph. Compared to currently used powder-based processes, deposition rates of about 1.5 times can be achieved. Compared to previously available wire-based processes, deposition rates of 7 times can be achieved.
[0014] Another finding is that the equipment costs do not increase significantly. It has been found that high beam quality is not required to melt the preformed fusible portion. A relatively low beam quality is sufficient since a deep penetration effect is not required, whereas a locally focused energy with good beam quality is required to produce the deep penetration effect. As a result, only a relatively large focal spot is required, as is used in heat conduction welding.
[0015] The preformed fusible part can be designed in different ways. In particular, the fusible part can be formed as a spring, a wire mesh, a sleeve and / or a half shell. In particular, the preformed fusible part is preferably thin-walled. Thin-walled means that it is weldable in such a way that a material bond is generated, in particular by a fusible unit, in particular a fusible unit with a laser unit. The material bond between the base part and the preformed fusible part is generated in particular by melting the fusible part and the base part.
[0016] This method makes it possible to structure a production cycle: in a first step, for example, the fusible part can be preformed, in particular by means of a spring winding machine; in a second step, the fusible part can be placed on the base; in a third step, melting takes place. These steps can be carried out partly in parallel, which ensures optimal timing of the various steps.
[0017] It is conceivable that progressive components can be produced by arranging preformed fusible parts of different materials. This can be important in different applications. For example, some layers can be provided to give the component extra strength, while other layers, especially the outer facing ones, can be provided to improve wear resistance. The material bond between the base and the preformed fusible part is preferably essentially along the entire surface of the fusible part facing the base. In particular, substantially means that an area of more than 50%, more than 75%, more than 90%, more than 95%, in particular more than 97.5% of the surface of the fusible part facing the base is materially bonded to the base.
[0018] In a preferred embodiment of the process, the preformed fusible portion is formed as a helical wire element, preferably with two or more adjacent windings of the helical wire element in contact with each other. In particular, it is preferred that substantially all windings are adjacent to each other. The helical wire element can be, for example, a spring. It is particularly preferred that the helical wire element is designed as a tension spring element, i.e. with the windings in contact with each other.
[0019] The helical shaped wire element preferably has more than 3, more than 5, more than 10, in particular more than 20 windings. For example, the helical shaped wire element may have 18 windings. Winding wire into a spring is a process that has been known for a long time and is a process with high process reliability. This process reliability means that it is possible to provide helical shaped wire elements with consistent properties, in particular enabling a process with high process reliability for the melting process.
[0020] Alternatively or additionally, the windings of the helical wire element can be spaced apart from each other. Such helical wire elements can be used, for example, to manufacture drills or extruder screws. The distance between the windings can be designed to be specific to the component.
[0021] It is further preferred that the preformed fusible portion comprises two or more helically shaped wire elements, preferably made from or including two or more different materials, so that a spring-spring concept with a double spring pitch can be realized.
[0022] A further preferred embodiment of the method is characterized in that the melting is performed by means of a laser unit. The laser unit is especially designed for generating and / or emitting a laser beam. The laser unit is preferably a fiber-guided diode laser unit. Furthermore, the laser unit may be a direct beam laser unit. Furthermore, the laser unit may be a fiber laser, a disk laser and / or a CO2 laser. The laser unit may also include other types of laser sources. It is further preferred that the laser unit has a power of more than 5 kW, preferably more than 50 kW, in particular more than 100 kW.
[0023] The laser unit preferably produces a round or rectangular focus. For example, the round focus may have a diameter of 4.6 mm. Furthermore, the laser unit may have a spot width of more than 5 mm, in particular about 40 mm. Furthermore, other focus dimensions can be used. For example, the focus may be elliptical or have a temperature-optimized profile. The above-mentioned method does not place high demands on the beam quality of the laser beam, so that in particular fiber-guided diode laser units or direct beam laser units can be used.
[0024] In a further preferred embodiment of the process, the preformed fusible section is placed onto the base by a pressure lock and / or form lock method.
[0025] The pressure locking configuration of the preformed fusible portion to the base can be achieved, for example, by using a helical wire element. The helical wire element can have, for example, an inner diameter that is smaller than the outer diameter of the base, resulting in an interference fit. However, due to the nature of the helical wire element, the wire element may be pressed onto the base without being twisted to increase the inner diameter. A spring force pressure locks the helical wire element to the base. The form locking configuration of the preformed fusible portion can be formed, for example, on a shoulder of the base.
[0026] It is further preferred that the preformed fusible portion is arranged around the base. Arrangement of the preformed fusible portion around the base means in particular that the preformed fusible portion is arranged along the outer and / or inner circumference of the base. For example, coatings of shafts are usually applied on the outer circumference. Furthermore, an arrangement on the inner circumference of a tube may be preferred in order to protect against corrosion by an inner coating.
[0027] A further preferred development of the method is characterized in that the welding is performed through a preformed fusible part in such a way that the base melts at least in a cross section, the cross-sectional melting of the base being particularly related to melting near the surface.
[0028] A further preferred embodiment of the method is characterized in that the base comprising the preformed fusible part is rotated during melting. The base is preferably rotated around its longitudinal axis and / or its axis of symmetry. By rotating the base comprising the preformed fusible part, the process is further simplified. In this way, the laser beam only needs to be guided along the longitudinal axis or axis of symmetry of the base and / or the fusible part. The radial feed is in particular realized by a rotary movement.
[0029] Furthermore, it is preferred that the feed direction is essentially parallel to the longitudinal axis and / or the axis of symmetry of the base. The feed direction in particular relates to the feed of the fusible unit, in particular the laser beam and / or the laser unit. In addition, the feed can be realized by a component. The longitudinal axis and / or the axis of symmetry of the base is preferably coaxially aligned with the longitudinal axis and / or the axis of symmetry of the fusible part.
[0030] A further preferred embodiment of the method is characterized in that the melting occurs at a feed rate of 500 mm / min to 2000 mm / min, in particular 700 mm / min to 900 mm / min. The feed rate can be realized by a fusible unit, in particular a laser unit and / or component. The feed rate is preferably oriented parallel to the aforementioned feed direction.
[0031] Further preferred embodiments of the method are characterized in that the preformed fusible portion has an inner peripheral outer contour that corresponds to the outer peripheral outer contour of the round body, and / or the preformed fusible portion has an outer peripheral outer contour that corresponds to the inner peripheral outer contour of the base.
[0032] In particular, it is preferred that the outer peripheral contour and / or the inner peripheral contour of the base is rotationally symmetric, which in particular means radially symmetric.
[0033] Another preferred embodiment of the method is characterized by a base having a rounded outer periphery. Furthermore, it is preferred that the preformed fusible portion has a rounded inner periphery. The rounded outer periphery of the base can mean, for example, that the base has a round cross section. In particular, this cross section has an orthogonal cross section that is aligned parallel to the longitudinal axis and / or the axis of symmetry of the base. The rounded outer periphery of the base and the corresponding extension, in particular the rounded inner periphery of the preformed fusible portion with a diameter, allow the preformed fusible portion to be arranged on the outer periphery of the base in an advantageous manner.
[0034] Furthermore, the preformed fusible portion, in particular the helical shaped wire element, is preferably formed from or includes a metallic material, for example the metallic material may be or include steel, nickel-based alloys, titanium, copper, cobalt-based alloys and / or aluminum, and the preformed fusible portion, in particular the helical shaped wire element, may further include or be formed from other fusible materials, for example plastics.
[0035] In a further preferred embodiment of the process, the preformed fusible portion has a thickness of 0.1 mm to 5 mm, in particular 1 mm to 2 mm. Furthermore, the helical shaped wire element may have a diameter of 5 mm to 1000 mm, preferably 20 mm to 100 mm, more preferably 30 mm to 40 mm.
[0036] Furthermore, it may be preferred that the wire of the helical shaped wire element has a circular, elliptical, triangular, rectangular and / or polygonal cross section. For example, the wire may have a thickness of 0.1 mm to 5 mm, in particular 1 mm to 2 mm.
[0037] In another preferred embodiment of the method, the pre-formed fusible portion includes a first wire element and a second wire element, the first wire element and the second wire element being formed from or including different materials.
[0038] In a further preferred embodiment of the method, the placement of the preformed fusible portion is performed independently of the location of melting of the preformed fusible portion. It is further preferred that the placement of the preformed fusible portion is performed in a first processing step and the melting is performed in a second processing step different from the first processing step.
[0039] In another preferred embodiment of the process, the method includes a step of checking the placement of the pre-formed fusible part on the base before fusing. Checking the placement can be done, for example, by a 3D scanning process. In particular, the relative position of the fusible part on the base is checked. For example, this can be done by moving a reference point of the fusible part away from a reference position of the base, for example a first end and / or a second end of the base.
[0040] In a further preferred embodiment of the process, it comprises a step of performing a heat treatment of the arranged base including the preformed fusible portion prior to melting, which reduces thermal stresses in particular in the base and / or the preformed fusible portion. In addition, the melting power, in particular the laser power, required to melt the preformed fusible portion is reduced by the heat treatment.
[0041] In a further preferred embodiment of the method, the method includes the step of disposing a second preformed fusible portion and / or a further preformed fusible portion on the melted preformed fusible portion to produce an at least partially productively produced component. It is further preferred to include the step of melting the second preformed fusible portion and / or the further preformed fusible portion to form a material bond between the base and / or preformed fusible portion and the second preformed fusible portion and / or the further preformed fusible portion. In disposing the second preformed fusible portion and / or the further preformed fusible portion, it is preferred that the previously disposed and melted preformed fusible portion solidifies.
[0042] According to a further aspect, the above-mentioned object is achieved by a manufacturing system configured to carry out a method according to one of the above-mentioned embodiments. Preferably, the manufacturing system comprises a first processing unit arranged and configured to generate a preformed fusible portion, in particular a helical shaped wire element. In addition, the manufacturing system may comprise a second processing unit arranged and configured to place a preformed fusible portion on a base.
[0043] Furthermore, the manufacturing system may include a third processing unit arranged and configured to melt the preformed fusible portion so that a material bond is formed between the base and the preformed fusible portion. In particular, the manufacturing system preferably includes the second processing unit and the third processing unit. Also, the first processing unit may be additionally provided. As an alternative to the first processing unit, the preformed fusible portion may be provided elsewhere, for example by an external supply.
[0044] According to a further aspect, the above mentioned object is achieved by a component obtainable by a method according to one of the above described embodiments.
[0045] The component obtained by the method according to the first aspect is different from conventionally coated components. Metallographic examination allows the microstructure and chemical phases to be examined at the interface between the base and the preformed fusible portion, adjacent to the interface. At the interface, according to a further aspect, chemical intermixing of the materials of the base and the preformed fusible portion occurs within the component, resulting in a metallurgical bond. Chemical intermixing can be detected, for example, using energy dispersive X-ray spectroscopy, also called EDX analysis.
[0046] In processes of electrolytic plating or coating from the gas phase, such as PVD or CVD, metallurgical compounds are formed and the base is essentially unaffected by heat. In comparison with other welding processes, the difference is that, in particular in the component according to the further aspect, straight and homogeneous interfaces are formed, which results in a relatively small heat-affected zone.
[0047] Micrographs of components produced by conventional overlay welding processes show that layers are usually formed by a number of weld beads arranged next to each other. The boundary of the boundary and the direction of the heat affected zone are usually wavy in such components, and the heat affected zone is relatively large. In addition, the production of the weld beads arranged next to each other leads to a remelting and / or tempering of the adjacent weld beads already produced. This leads to structural modifications in the area between two adjacent weld beads, which can be analyzed by etching the metallographic section or by energy dispersive X-ray spectroscopy. In contrast, according to a further embodiment, the component is characterized by a homogeneous microstructure.
[0048] For further advantages, further aspect embodiment variants and further embodiment details which may be considered, reference is made to the above description of the corresponding features and further embodiments of the process. Preferred embodiments are described by way of example with reference to the accompanying drawings, which show: [Brief description of the drawings]
[0049] [Figure 1] FIG. 1 is a schematic two-dimensional view of an exemplary embodiment of a base portion and a pre-formed fusible portion.
[0050] [Diagram 2] FIG. 2 is a schematic two-dimensional view of a typical process set-up for melting a preformed fusible portion.
[0051] [Diagram 3] FIG. 3 is another schematic two-dimensional view of the setup shown in FIG.
[0052] [Figure 4] FIG. 4 is a schematic diagram of the processing unit.
[0053] [Diagram 5] FIG. 5 is a schematic process.
[0054] In the drawings, identical or essentially functionally identical or similar elements are indicated with the same reference numbers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0055] FIG. 1 shows a preformed fusible portion 100 formed as a helical shaped wire element 101. The preformed fusible portion 100 extends from a first fusible portion end 102 to a second fusible portion end 104. A first winding 106 is provided adjacent to the first fusible portion end 102. A second winding 108 is provided adjacent to the second fusible portion end 104. A number of additional windings 110 are provided between the first winding 106 and the second winding 108. The windings 106, 108, 110 are adjacent to one another. By abutting one another it is meant in particular that there is no gap between two adjacent windings. Alternatively or additionally, it is also conceivable that the windings 106, 108, 110 are spaced apart from one another.
[0056] Also, the preformed fusible portion 100 may be formed, for example, as a sleeve, which may be arranged to be locked under pressure against the base portion 200 by a corresponding inner circumferential shape. Further geometries of the preformed fusible portion have already been described above.
[0057] Also shown in FIG. 1 is a base 200 extending from a first base end 202 to a second base end 204. Adjacent to the first base end 202 is a coating 206, which is coated by the method. Additionally, the base 200 includes a threaded portion 208 adjacent to the second base end 204. The base 200 is formed as a rotationally symmetric component having a longitudinal axis 210 which also serves as an axis of symmetry 212. Also shown in FIG. 1 is a mandrel 10, which is provided for clamping the base 200 in a lathe. Notably, the mandrel 10 is part of the lathe and is not typically part of the base 200.
[0058] In FIG. 2, the preformed fusible part 100 is placed on the base 200. The preformed fusible part 100 is melted by a laser beam 2 from a laser unit 1. The laser unit 1 is moved in a feed direction 4 parallel to a longitudinal axis 210 of the base 200. By moving the laser unit 1 in the feed direction 4, the laser beam is moved continuously from the first fusible part end 102 towards the second fusible part end 104. As a result, the first winding 106 and the further winding facing the first winding 106 are melted, which are shown as melted parts 112 in FIG. 2. The original structure with the windings is melted away. While the laser unit 1 is moved in the feed direction 4, the base 200 including the preformed fusible part 100 rotates around the longitudinal axis 210 at a rotation speed.
[0059] The rotation speed depends on the diameter of the base 200, the focal spot size and the laser power of the laser unit 1. For example, the rotation speed may be between 1 revolution per minute and 20 revolutions per minute. For example, the resulting feed speed may be between 500 mm / min and 2000 mm / min, in particular between 700 mm / min and 900 mm / min.
[0060] The component 400 is formed by materially bonding the fusion portion 100 to the base portion 200 .
[0061] Figure 3 shows another view of the assembly shown in Figure 2. In Figure 3, the longitudinal axis 210 of the base 200 is perpendicular to the image plane. In particular, the base 200 is shown as having a rounded outer shape. Additionally, the preformed fusible portion 100 is shown as having a rounded inner shape.
[0062] 4 shows a schematic diagram of a manufacturing system 500 having processing units 502-506. The first processing unit 502 is arranged and configured to generate the preformed fusible portion 100, in particular the helical shaped wire element 101. The first processing unit 502 can be, for example, a spring winding machine. The second processing unit 504 is arranged and configured to place the preformed fusible portion 100 on the base 200. The third processing unit 506 is arranged and configured to melt the preformed fusible portion 100 such that a material bond is formed between the base 200 and the preformed fusible portion 100.
[0063] 5 shows a schematic process. In step 300, a preformed fusible portion 100 is produced. In particular, this can be done using a spring winding machine, which can wind wire into a spring. This forms a helical shaped wire element that serves as the preformed fusible portion. In step 302, the preformed fusible portion 100 is placed on the base portion 200. This can be done in particular by pressing the preformed fusible portion 100 onto the base portion 200, in particular onto the coating portion 206.
[0064] In step 304, the placement of the pre-formed fusible portion 100 on the base 200 is verified. This can be done, for example, by using a 3D scanning process. In particular, the placement check verifies that the pre-formed fusible portion 100 is placed in the desired location on the base 200, and in particular, in the desired coating portion 206.
[0065] In step 306, the base 200 together with the preformed fusible portion 100, in particular with the preformed fusible portion 100 disposed thereon, is heat treated. This heat treatment can be performed at a temperature of, for example, 300° C. to 800° C. Alternatively or additionally, step 306 can be performed after step 308. As a result, preceding and / or subsequent heat treatments are possible. For example, furnace heating, induction heating, resistance heating, burner heating, and / or laser heating can be used for this heat treatment.
[0066] Finally, in step 308 , the preformed fusible portion 100 is melted to form a material bond between the base portion 200 and the preformed fusible portion 100 .
[0067] The method described above reduces the complexity of the process, which allows shorter process times and improved component quality. In addition, the method allows the production of progressive components and defined coatings, which on the one hand improves the quality of the components produced and on the other hand broadens the field of application of the components produced. In particular, the simplified process allows wire-based overlay welding to be applied to companies that cannot afford to invest heavily in high-precision manufacturing equipment. In this way, a high-quality process is possible at low cost.
[0068] The method can be used to form coatings, especially on the outer and inner surfaces of components that are at risk of corrosion. Possible applications include process engineering and energy technology, especially in the petrochemical industry. Furthermore, the process can be used to coat components for waste incineration plants. Furthermore, the method can be used for components for automotive engineering, especially for components used in electric drive vehicles, preferably passenger cars and / or trucks. The components thus produced can also be used in rail vehicles, industrial trucks and construction machines. Furthermore, the method can be used to manufacture shafts and axles for ships and aircraft. Applications in hydraulic systems are also conceivable.
[0069] This method is also used for components that are subject to high wear damage. For example, wear damage can occur in inner tubes that carry fluids with abrasive particles. Another application is the productive production of components. Due to the relatively high deposition rate, this method can also be used for mass production under economical conditions. This is different from all productive processes developed so far, which are essentially dedicated to one-off and small batch production. Furthermore, this method can be used to produce structures that were previously impossible to manufacture or were only produced at great expense. For example, in order to ensure the supply of oil in gear shafts, long holes or through holes are provided through which oil is supplied. This method can be used to produce these holes in a simple manner, for example by providing empty spaces at the positions where the through holes of the preformed fusible parts should be produced. [Explanation of symbols]
[0070] 1 Laser unit 2 Laser beam 4 Feed direction 10. Horn 100 Preformed Fusible Section 101 Spiral Wire Element 102 first fusible portion end 104 Second fusible portion end 106 First Winding 108 Second Winding 110 Windings 112 Melting section 200 base 202 first base end 204 second base end 206 Coating Department 208 Screw part 210 Longitudinal axis 212 Axis of Symmetry 400 Components 500 Manufacturing System 502 First Processing Unit 504 Second Processing Unit 506 3rd Processing Unit
Claims
1. 1. A method for producing a layer, comprising: - preforming a helical shaped fusible portion (101); - moving the helical shaped fusible portion (101) onto a base (200); - melting the helical fusible portion (101) to form a material bond between the base portion (200) and the helical fusible portion (101); A method comprising:
2. The method of claim 1, wherein two or more adjacent windings (106, 108, 110) of the helical fusible portion (101) abut each other.
3. 3. The method according to claim 1 or 2, wherein the melting is performed by a laser unit (1).
4. 4. The method according to claim 3, wherein the laser unit (1) is a fiber-guided diode laser unit and / or a direct beam laser unit.
5. 5. The method according to claim 4, wherein the laser unit (1) has a power of more than 5 kW.
6. The helical fusible portion (101) is - placed on said base (200) in a pressure-locked and / or form-locked manner; and / or - arranged circumferentially on said base (200); 6. The method according to any one of claims 1 to 5.
7. 7. The method according to any one of claims 1 to 6, wherein welding is performed over the helical fusible portion (101) such that the base portion (200) is melted at least in cross section.
8. the base (200) having the helical shaped fusible portion (101) is rotated during the melting; 8. The method according to any one of claims 1 to 7.
9. 9. The method of claim 8, wherein the base (200) having the helical shaped fusible portion (101) is rotated about a longitudinal axis (210) of the base (200) or about an axis of symmetry (212) of the base (200) during the melting.
10. 10. The method of claim 9, wherein a feed direction is oriented substantially parallel to the longitudinal axis (210) and / or to the axis of symmetry (212) of the base (200).
11. 11. The method according to any one of claims 1 to 10, wherein the melting is carried out at a feed rate of 500 mm / min to 2000 mm / min.
12. the helical fusible portion (101) has an inner circumferential shape that corresponds to the outer circumferential shape of the base portion (200); 12. The method according to any one of claims 1 to 11.
13. The method of claim 12, wherein the peripheral shape of the base (200) is rotationally symmetric.
14. the base (200) has a rounded periphery, and / or The helical fusible portion (101) has a rounded inner circumference.
14. The method according to any one of claims 1 to 13.
15. The method according to any one of the preceding claims, wherein the helical shaped fusible portion (101) is made of or comprises steel.
16. the helical fusible portion (101) has a thickness of 0.1 mm to 5 mm; and / or the helical fusible portion (101) has a diameter of 5 mm to 1000 mm; and / or the wire of the helical fusible portion (101) has a circular, elliptical, triangular, rectangular and / or polygonal cross section; 16. The method according to any one of claims 1 to 15.
17. 17. The method of any one of claims 1 to 16, wherein the helically shaped fusible portion (101) comprises a first wire element and a second wire element, the first wire element and the second wire element being formed from or comprising different materials.
18. 18. The method according to any one of claims 1 to 17, wherein the positioning of the helical shaped fusible portion (101) is performed independently of the location of the melting of the helical shaped fusible portion (101).
19. 20. The method of claim 18, wherein the positioning of the helically shaped fusible portion (101) occurs in a first processing step and the melting occurs in a second processing step different from the first processing step.
20. 20. The method according to any one of claims 1 to 19, comprising the step of checking the arrangement of the helical shaped fusible portion (101) on the base (200) before melting, in particular by a 3D scanning process.
21. 21. The method according to any one of claims 1 to 20, comprising the step of heat treating the base (200) on which the helical shaped fusible portion (101) is arranged prior to melting.
22. - disposing a second helical shaped fusible portion and / or a further helical shaped fusible portion on the molten helical shaped fusible portion (101) to at least partially produce a productively produced component; 22. The method of any one of claims 1 to 21, comprising:
23. - melting the second helical fusible portion and / or the further helical fusible portion to form a material bond between the base portion (200) and / or the helical fusible portion (101) and the second helical fusible portion; 23. The method of claim 22, comprising:
24. A first processing unit (502) arranged and configured to preform a helical shaped fusible portion (101); and a second processing unit (504) arranged and configured to move the helical shaped fusible portion (101) onto the base (200); and a third processing unit (506) arranged and configured to melt the helical shaped fusible portion (101) to form a material bond between the base portion (200) and the helical shaped fusible portion (101); A manufacturing system comprising:
Citation Information
Patent Citations
Method of producing metallic coatings on convexly curved surfaces of machine parts
AT387173B
Turbine rotor and its build-up welding method
JP1988248587A
Method for lining inner face of cylinder
JP1992341576A
Production of product of aluminum alloy
JP1995290270A
Method for preventing erosion, and member having erosion preventing portion
JP2008036652A