High throughput silicon carbide ceramic filtration membrane and its preparation method

JP7561466B2Active Publication Date: 2024-10-04NANJING IKAKAT EMISSIONS TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023548880
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-04-25
Filing Date
2022-04-20
Publication Date
2024-10-04
Estimated Expiration
2042-04-20

Smart Images

  • Figure 0007561466000001
    Figure 0007561466000001
  • Figure 0007561466000002
    Figure 0007561466000002
  • Figure 0007561466000003
    Figure 0007561466000003
Patent Text Reader

Abstract

A high-throughput silicon carbide ceramic filtration membrane and its preparation method. The separation layer is directly coated on the carrier only once, that is, the separation layer is directly coated after the carrier is sintered, and carbon removal is further performed after sintering. The sintering process is optimized, and the composition of the membrane forming solution is optimized, so that the silicon carbide particles are prevented from entering the pores of the carrier during the capillary filtration and thin film formation process during coating, and a separation layer with an average pore size of 0.2 μm or less can be directly coated on a silicon carbide carrier with an average pore size of 10 μm or more, which effectively prevents the silicon carbide particles from entering the pores of the carrier during coating.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of ceramic filtration membranes, specifically to high throughput silicon carbide ceramic filtration membranes and methods for their preparation. [Background technology]

[0002] In the preparation of conventional silicon carbide membranes, similar to ceramic membranes, the structure is a sandwich structure, namely, a support layer, an intermediate layer and a separation layer. The support layer is the carrier of the membrane and mainly ensures the mechanical strength of the membrane. The separation layer plays a substantial filtration and separation role. Since the carrier pore size is often at least 25 times larger than the separation layer particles, in the conventional process, it is necessary to apply an intermediate layer between the support layer and the separation layer to prevent the particles from penetrating into the support layer during the preparation process of the separation layer. However, the existence of the intermediate layer objectively reduces the throughput, and the difference between the pore sizes of the carrier, intermediate layer and separation layer in the conventional process is small, usually varying between 1-5 times, so the throughput is lowered and the difficulty is increased.

[0003] As shown in Figure 1, the conventional preparation process of silicon carbide film requires at least three sinterings, and the preparation process is relatively complicated and expensive, and the product has poor yield and low throughput due to repeated coating. In the conventional process, high-temperature oxidation (700-1200°C, under aeration conditions) is required after each coating and high-temperature sintering (usually 2000-2400°C, sintering under protection conditions with inert gas such as argon) to remove the carbon remaining in the high-temperature sintering. These carbons come from organic substances such as adhesives and dispersants contained in the material or coating slurry. Since carbon is a hydrophobic substance, if the carbon is not removed, it will be very difficult for the solvent / water in the slurry to enter the carrier pores due to capillary force during coating, and ultimately the coating film cannot be formed.

[0004] Therefore, in the conventional process, it was necessary to carry out an oxidation treatment on the product after high-temperature sintering. By oxidizing the support to remove carbon, the surface becomes hydrophilic and the pore size becomes relatively large, which is advantageous for the slurry solvent / water to enter the support pores by capillary force and finally form a coating film. However, if the particle size of the coating layer particles in the coating layer slurry is large enough, the slurry solvent / water cannot enter the support by capillary force. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] (See International Search Report) Summary of the Invention

[0006] The object of the present invention is to provide a method for preparing a high-throughput silicon carbide ceramic filter body that does not remove carbon after the sintering process, i.e., a preparation method in which oxidative decarburization is not performed after sintering the support, and the remaining carbon is left. Specifically, by optimizing the coating layer slurry and preparation process, the surface tension is reduced, and the coating layer slurry can be applied by utilizing capillary force even in a situation where the support is hydrophobic, and the coating layer fine particles are applied to a support having an average pore size of 10 μm or more by utilizing the repulsive effect of the same charge generated when the support surface and the particles to be applied have the same charge.

[0007] In a first aspect of the present invention, a method for preparing a high throughput silicon carbide ceramic filter body is provided, comprising the steps of: (1) A multi-channel tubular material is prepared, and the multi-channel tubular material is sintered at a high temperature to prepare a carrier having a pore structure with a first average pore size. (2) The carrier is made to stand, and the coating layer slurry is poured into the channel from the bottom of the carrier prepared in step (1), and the coating layer slurry reaches the top of the carrier and is held for a certain period of time, after which the coating layer slurry in the channel is released to form a channel coating layer, in which the particles of the coating layer slurry are charged with the same charge as the carrier surface. (3) The channel coating layer prepared in step (2) is dried. (4) sintering the channel coating layer at a high temperature under the protective condition of an inert atmosphere to form a pore structure having a second average pore size and to prepare a separation layer; and (5) The separation layer obtained in step (4) is subjected to high-temperature oxidation sintering to remove residual carbon.

[0008] Preferably, the preparation of the carrier specifically includes the following processes: A silicon carbide powder having a first particle size mismatch is mixed with a first auxiliary agent and water, and then a multi-channel tubular material is extruded and sintered to form a pore structure having a first average pore size in the channel walls by recrystallization of the material to produce a carrier. Preferably, the silicon carbide powder having the first particle size mismatch degree includes silicon carbide powder I and silicon carbide powder II, and the median diameter of silicon carbide powder I is 5 to 30 times the median diameter of silicon carbide powder II. More preferably, the median diameter of silicon carbide powder I is between 10 and 30 μm, and the median diameter of silicon carbide powder II is between 0.5 and 6 μm. Preferably, the first auxiliary agent includes an adhesive, a plasticizer, and a dispersant. More preferably, the mass ratio of the silicon carbide powder I, silicon carbide powder II, adhesive, plasticizer, dispersant, and water is (50-75):(10-20):(4-8):(1-3):(1-3):(10-20). Preferably, the method further comprises drying the multi-channel tubular blank prior to high temperature sintering the blank.

[0009] Preferably, the coating layer slurry is prepared by mixing silicon carbide powder having a second particle size mismatch degree, a second auxiliary agent, and water, the silicon carbide powder having the second particle size mismatch degree includes silicon carbide powder III and silicon carbide powder IV, and the median diameter of the silicon carbide powder III is 3 to 8 times the median diameter of the silicon carbide powder IV. Preferably, the silicon carbide powder III has a median diameter between 0.5 and 6 μm, and the silicon carbide powder IV has a median diameter between 0.1 and 3 μm. Preferably, the second auxiliary agent contains an adhesive, a plasticizer, a dispersant, an antifoaming agent and a surfactant, and the mass ratio of silicon carbide powder III, silicon carbide powder IV, adhesive, plasticizer, dispersant, antifoaming agent, surfactant and water is (5-15):(5-15):(3-10):(5-15):(0-1.5):(0-1.5):(1-5):(50-80). Preferably, the pH value of the coating layer slurry is between 6-10. Preferably, the coating layer slurry is first The material is pretreated by adding alumina balls with a diameter of 8 to 10 mm and rolling polishing for 12 to 48 hours before being placed in the channel. Preferably, the coating layer slurry enters the channel at a speed of 20-100 mm / s. Preferably, in step (2), the predetermined time is 3 to 15 seconds.

[0010] Preferably, the process of high-temperature sintering of the channel coating layer and the material includes a degumming treatment, for example, by heating to 300-500°C under argon atmosphere protection and keeping the temperature for 2-5 hours to degumm the material and the channel coating layer. After degumming is complete, high temperature sintering is performed to achieve recrystallization for the silicon carbide particles. Preferably, the sintering temperature of the channel coating layer recrystallization is lower than the sintering temperature of the raw material recrystallization. More preferably, the sintering temperature of the channel coating layer recrystallization is between 1600 and 2000°C, and the sintering temperature of the raw material recrystallization is between 2000 and 2400°C. Preferably, the particles in the coating layer slurry carry the same charge as the carrier surface.

[0011] A second aspect (viewpoint) of the present invention provides a high-throughput silicon carbide ceramic filtration membrane comprising a carrier and a separation layer and not including an intermediate layer, prepared based on the above-mentioned method for preparing a high-throughput silicon carbide ceramic filtration membrane. Particularly preferably, the first average pore size is 10 μm or more and the second average pore size is 0.2 μm or less.Particularly preferably, the second average pore size is 0.15 μm to 0.2 μm.

[0012] In a third aspect of the present invention, there is provided a high throughput silicon carbide ceramic filtration membrane, comprising a porous carrier and a porous separating layer, but no intermediate layer, wherein the average pore size of the pores in the porous carrier is 20 times or more larger than the average pore size of the pores in the porous separating layer. Preferably, the average pore size of the pores in the porous carrier is 10 μm or more, and the average pore size of the pores in the porous separating layer is 0.2 μm or less. Preferably, the average pore size of the pores in the separating layer having the above-mentioned pores is between 0.15 μm and 0.2 μm.

[0013] Compared with the prior art, the present invention adjusts and optimizes the preparation process of ceramic filtration membranes, eliminates the intermediate layer and intermediate layer preparation processes in the conventional process, optimizes the formulation of the coating layer slurry, and does not carry out oxidation or carbon removal after the support is sintered and prepared, but uses the remaining carbon to block the pores of the support to a certain extent, thereby reducing the probability of the silicon carbide particles of the separation layer penetrating into the pores of the support, and at the same time, combines the repulsive effect of the particles of the coating layer slurry and the same charge on the surface of the support to prevent the particles from penetrating into the pores of the support during capillary filtration and thin film formation when the coating layer slurry is applied.

[0014] By optimizing the process of the present invention, it is possible to directly coat a silicon carbide membrane separation layer with an average pore size of 150 nm on a silicon carbide carrier with an average pore size of 10 μm or more, and complete the preparation of a filtration membrane by sintering the silicon carbide membrane twice at the ultrafiltration application level. This avoids the disadvantages of traditional ceramic membranes that require a multi-layer structure (carrier, intermediate layer and separation layer) and at least three sintering steps, and eliminates the need for the preparation of the intermediate layer, which greatly reduces production costs and improves the pass rate of the products.

[0015] At the same time, the ceramic filtration membrane prepared in the present invention is composed only of a silicon carbide carrier and a separation layer, which realizes the preparation of a separation layer with a high pore size on a large pore size carrier, and does not contain an intermediate layer. Therefore, compared with conventional filtration membrane products with the same pore size specifications, the present invention has a significantly increased throughput, and tests have shown that the increase in throughput has reached more than 30%.

[0016] It should be understood that all combinations of the above-mentioned features, and the additional features further detailed below, may be considered part of the inventive subject matter of the present disclosure, provided such features are not mutually inconsistent, and all combinations of subject matter claimed are considered part of the inventive subject matter of the present disclosure. [Brief description of the drawings]

[0017] In the drawings, identical or nearly identical components shown in each drawing may be represented by the same reference numerals. For the sake of clarity, not all components are labeled in each drawing. Various aspects of the present invention will now be described, by way of example, with reference to the drawings, in which:

[0018] [Figure 1] Figure 1 is a flow chart of the ceramic filtration membrane preparation process, which adopts three-stage sintering and oxidation in the conventional process. [Diagram 2] FIG. 2 is a process flow chart of a ceramic filtration membrane in which the preparation of an intermediate layer is omitted in an exemplary embodiment of the present invention. [Diagram 3] FIG. 3 is an example of a process for preparing a ceramic filtration membrane in an exemplary embodiment of the present invention. [Figure 4] FIG. 4 is an example of a process for preparing a silicon carbide support in the process for preparing a ceramic filtration membrane in an exemplary embodiment of the present invention. [Diagram 5] FIG. 5 is an example of a process for preparing a separation layer and removing carbon in a process for preparing a ceramic filtration membrane in an exemplary embodiment of the present invention. [Figure 6]FIG. 6 is a schematic diagram of a ceramic body including a carrier, intermediate and separating layers prepared using the conventional process shown in FIG. [Figure 7] FIG. 7 is a schematic diagram of a silicon carbide ceramic membrane obtained using the ceramic filtration membrane preparation method of Example 1, in which no intermediate layer is included. [Figure 8] FIG. 8 is a pore size measurement diagram of the support of the silicon carbide ceramic membrane obtained by using the ceramic filtration membrane preparation method of Example 1, in which the average support pore size is 10.5 μm. [Figure 9] FIG. 9 is a pore size measurement diagram of the separation layer of the silicon carbide ceramic membrane obtained by using the ceramic filtration membrane preparation method of Example 1, in which the average separation layer pore size is 0.15 μm. [Figure 10] FIG. 10 is a support pore size diagram of the silicon carbide ceramic membrane obtained by using the ceramic filtration membrane preparation method of Example 2, in which the intermediate layer is not included, and the average support pore size is 15 μm. [Figure 11] FIG. 11 is a pore size measurement diagram of the separation layer of the silicon carbide ceramic membrane obtained by using the ceramic filtration membrane preparation method of Example 2, in which the average separation layer pore size is 0.2 μm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] In order to further understand the technical contents of the present invention, specific embodiments are given herein and described in conjunction with the accompanying drawings.

[0020] In this disclosure, each aspect of the present invention is described with reference to the drawings, which show a number of illustrative examples. The examples of the present disclosure are not meant to include all aspects of the present invention. The various concepts and examples introduced above, and the concepts and embodiments described in more detail below, can be implemented in any one of many ways, as the concepts and examples disclosed in the present invention are not limited to any embodiment. In addition, some aspects disclosed in the present invention can be used alone or in any suitable combination with other aspects disclosed in the present invention.

[0021] In the preparation process of the conventional sandwich-structured ceramic membrane as shown in Fig. 1, at least three sinterings are required during the preparation process, and after each coating and high-temperature sintering, high-temperature oxidation is required to remove the carbon remaining from the high-temperature sintering, so the preparation process is relatively complicated, the cost is high, and the product requires multiple coatings, resulting in low yields. Fig. 6 shows an example of a typical sandwich-structured ceramic membrane prepared by a conventional sintering process, which has a typical carrier, intermediate layer and separation layer structure, and the average pore size of the intermediate layer is about twice that of the separation layer, and the existence of the intermediate layer and the low ratio of the pore sizes of the intermediate layer and the separation layer affect and significantly reduce the throughput.

[0022] As shown in FIG. 2, the present invention aims to provide an improved method for preparing ceramic filtration membranes, which eliminates the intermediate layer and its preparation process, and adopts a process of directly coating a separation layer on the carrier in one go. That is, after sintering the carrier, the separation layer is directly coated, and carbon removal is performed after sintering. By optimizing the sintering process and optimizing the composition of the membrane forming solution, it is possible to prevent silicon carbide particles from entering the pore structure of the carrier during the capillary filtration and thin film formation process during coating, and to realize a separation layer with an average pore size of 150 nm directly coated on a silicon carbide carrier with an average pore size of 10 μm or more, which effectively prevents silicon carbide particles in the coating layer slurry from entering the pores of the carrier during coating. This avoids the disadvantage that the traditional ceramic membrane preparation process requires multiple coatings, that is, at least two coatings (first coating the intermediate layer on the carrier, then coating the separation layer on the intermediate layer) and three sinterings, thereby reducing production costs and increasing the pass rate of products. The elimination of the intermediate layer also allows for significantly higher throughput than ceramic membranes of comparable pore size.

[0023] The preparation method of the present invention is particularly applicable to preparing a ceramic filtration membrane for a separation layer having a pore structure with a pore size difference of 20 times or more based on a large pore size carrier, and the ceramic filtration membrane structure to be prepared is composed only of a large pore size carrier and a separation layer attached to the carrier surface, and in particular, the average pore size value of the carrier pores (first pore size D1) is 20 times or more the average pore size value of the separation layer pores (second pore size D2). In the following examples, an example will be given in which a separation layer with a pore structure with an average pore size of less than 0.2 μm is directly applied to a silicon carbide carrier having a pore structure with an average pore size of 10 μm or more.

[0024] As shown in the figures, an exemplary realization of the preparation method of the present invention will now be described in more detail.

[0025] The preparation process shown in FIG. 3 includes the following steps: preparing a multi-channel tubular material, and sintering the multi-channel tubular material at high temperature to prepare a carrier having a pore structure with a first average pore size; standing the carrier, and introducing a coating layer slurry into the channel from the bottom of the prepared carrier until the coating layer slurry reaches the top of the carrier and is held for a certain time, and then releasing the coating layer slurry in the channel to form a channel coating layer, in which the particles of the coating layer slurry are charged with the same charge as the carrier surface; drying the channel coating layer; and under the protective condition of an inert atmosphere, sintering the channel coating layer at high temperature to form a pore structure with a second average pore size to prepare a separation layer; and performing high-temperature oxidation sintering on the separation layer to remove residual carbon.

[0026] As one specific example of the present invention, take the preparation of silicon carbide ceramic filtration membranes with high throughput and low cost as an example. The process includes: mixing silicon carbide powder having a first particle size mismatch with a first auxiliary agent and water, extruding a multi-channel tubular blank, and then sintering the blank at a high temperature to form a pore structure having a first average pore size in the channel wall by recrystallization of the blank, thereby preparing a carrier; The carrier is made to stand, and the coating layer slurry is poured into each channel from the bottom of the carrier, and after the coating layer slurry reaches the top of the carrier and is held for a predetermined time, the coating layer slurry in the channel is released to form a channel coating layer; wherein the coating layer slurry is prepared by mixing silicon carbide powder having a second particle size mismatch degree, a second auxiliary agent, and water, and the pH value of the slurry is controlled to be between 6 and 10; drying the channel coating layer; and sintering the channel coating layer at a high temperature under a protective atmosphere to form a pore structure having a second average pore size to form a separation layer; and performing high-temperature oxidative sintering on the separation layer to remove any remaining carbon in the separation layer.

[0027] It is particularly preferred that the method includes drying the multi-channel tubular material before the material recrystallizes. For example, the multi-channel tubular material is dried in a drying chamber for 24-48 hours. The environmental conditions controlled in the drying chamber are a relative humidity of 20-60% and a temperature of 25-50°C. During the drying process, hot air is passed through the material channels at a flow rate of 0.5-2 m / s.

[0028] Preferably, the silicon carbide powder having the first particle size mismatch degree includes silicon carbide powder I and silicon carbide powder II, and the median diameter of silicon carbide powder I is 5 to 30 times the median diameter of silicon carbide powder II. In particular, the median diameter of silicon carbide powder I is between 10 and 30 μm, and the median diameter of silicon carbide powder II is between 0.5 and 6 μm.

[0029] Exemplary first auxiliaries include adhesives, plasticizers, and dispersants. Particularly preferably, the mass ratio of silicon carbide powder I, silicon carbide powder II, adhesive, plasticizer, dispersant, and water is (50-75):(10-20):(4-8):(1-3):(1-3):(10-20).

[0030] Preferably, the adhesive may be selected from methylhydroxyethyl cellulose or polyvinyl alcohol, the plasticizer is polyethylene glycol or phthalate ester, and the dispersant is an acrylic polymer.

[0031] Preferably, the silicon carbide powder having the second particle size mismatch degree includes silicon carbide powder III and silicon carbide powder IV, and the median diameter of the silicon carbide powder III is 3 to 8 times the median diameter of the silicon carbide powder IV. In particular, the median diameter of the silicon carbide powder III is between 0.5 and 6 μm, and the median diameter of the silicon carbide powder IV is between 0.1 and 3 μm.

[0032] Particularly preferably, by controlling the median diameters of both the silicon carbide powder III and the silicon carbide powder IV to be between 0.1 and 1.5 μm, a pore structure having a pore diameter of 200 μm or less can be effectively prepared.

[0033] It should be understood that the median size in the embodiments of the present invention is also referred to as the midpoint particle size.

[0034] Exemplary second auxiliary agents include adhesives, plasticizers, dispersants, antifoaming agents and surfactants, in which the mass ratio of silicon carbide powder III, silicon carbide powder IV, adhesives, plasticizers, dispersants, antifoaming agents, surfactants and water is (5-15):(5-15):(3-10):(5-15):(0-1.5):(0-1.5):(1-5):(50-80).

[0035] Preferably, the adhesive may be at least one of methylhydroxyethyl cellulose and polyvinyl alcohol, the plasticizer may be polyethylene glycol or phthalate ester, the dispersant may be an acrylic polymer, the defoamer may be silicone polyethers, and the surfactant may be alcohols.

[0036] The coating layer slurry after uniformly mixing based on the above-mentioned mass ratio is first The material is treated by a pretreatment method in which alumina balls with a diameter of 8 to 10 mm are added and roll-polished for 12 to 48 hours before being placed in the channel.

[0037] Preferably, in some embodiments of the present invention, the coating layer slurry is controlled to be injected into the channel at a speed of 20-100 mm / s. More preferably, the coating layer slurry is held for 3-15 seconds after reaching the top of the carrier to achieve effective coating and form a coating layer by capillary action.

[0038] In this way, by optimizing the composition of the coating layer slurry, after the support is sintered and prepared, carbon oxide removal is not performed, and the remaining carbon is used to block the pores of the support to a certain extent, thereby reducing the probability that the silicon carbide microparticles of the separation layer will enter the pores of the support, and by combining the repulsive effect of the particles of the coating layer slurry and the same charge on the surface of the support, the intrusion of microparticles into the pores of the support during capillary filtration and thin film formation when the coating layer slurry is applied is prevented.

[0039] Optionally, during the process of disposing the coating layer slurry, various methods can be used, such as adjusting the properties of the fluid (slurry) or adjusting the pH, to control the particles (silicon carbide particles) and the carrier surface to have the same charge, and this can be achieved by using one or a combination of two or more of these methods.

[0040] For example, in disposing a separation layer coating layer slurry prepared by mixing silicon carbide powder having a second particle size mismatch degree, a second auxiliary agent, and water, the pH value of the slurry can be controlled to be between 6 and 10, so that the particles in the coating layer slurry carry a charge of the same polarity as the carrier surface, and the repulsive action of the same polarity charge prevents the particles in the coating layer slurry from entering the pore size of the carrier.

[0041] As shown in Figures 4 and 5, in some embodiments of the present invention, degumming is included in the high-temperature sintering of the channel coating layer and the high-temperature sintering of the material. For example, the material and the coating layer are degummed by heating up to 300-500°C under argon atmosphere protection conditions and keeping the temperature for 2-5 hours.

[0042] After the degumming is complete, the mixture is heated again to the recrystallization temperature range and recrystallized. Finally, it is cooled to room temperature in the furnace.

[0043] In a specific implementation, the sintering temperature of the channel coating layer recrystallization is lower than the sintering temperature of the raw material recrystallization, preferably, the sintering temperature of the channel coating layer recrystallization is between 1600-2000°C, and the sintering temperature of the raw material recrystallization is between 2000-2400°C.

[0044] The raw materials of the above materials and the slurry are all commercially available. Preferably, the purity of silicon carbide powder I is greater than 98%, the purity of silicon carbide powder II is greater than 99%, and the purity of silicon carbide powder III and silicon carbide powder IV is greater than 99%. EXAMPLES

[0045] The above preparation methods are described below in conjunction with specific examples.

[0046] [Example 1] 1) Molding and sintering of silicon carbide materials Selection of raw materials: Silicon carbide powder I, silicon carbide powder II, methylhydroxyethyl cellulose, polyethylene glycol, acrylic polymer and water are taken and prepared according to the mass ratio of 60:18:6:2:2:12. The median diameter of silicon carbide powder I is 20 times that of silicon carbide powder II. The median diameter of silicon carbide powder I is 20 μm and the purity is greater than 98%, while the median diameter of silicon carbide powder II is 1 μm and the purity is greater than 99%.

[0047] Mixing of ingredients: Mix the selected ingredients at room temperature (20-25 degrees Celsius) based on the proportions in the following order: add liquid first and then powder to form a homogenous mixture.

[0048] Molding: The resulting mixture is fed into an extruder and molded into a multi-channel tubular material under an extrusion pressure of 120 MPa.

[0049] Drying: The material is extruded and dried in a drying room for 24 hours. The relative humidity is 50-60%, the temperature is 25-30℃, and hot air is passed through the material channel at a flow rate of 2m / s.

[0050] High-temperature sintering and recrystallization: After drying, the material is sintered at high temperature under argon atmosphere protection conditions. The temperature is raised to 500°C, kept at that temperature for 2 hours, and the material is degummed. After degumming is completed, the temperature is raised to 2400°C. The sintering temperature rise process lasts for 18 hours, during which the material is sintered with recrystallization, kept at that temperature for 5 hours, and finally cooled to room temperature in the furnace.

[0051] 2) Application of silicon carbide coating layer Preparation of slurry: Mix silicon carbide powder III, silicon carbide powder IV, methylhydroxyethyl cellulose, phthalate ester, acrylic polymer dispersant, silicone polyether antifoaming agent, alcohol surfactant PEG and water uniformly in a mass ratio of 15:10:5:8:1.5:1.5:3:56, control the pH to 8-9, add alumina balls with a diameter of 8-10 mm, and perform rolling polishing for 48 hours to obtain a coating layer slurry. The median diameter of silicon carbide powder III is five times the median diameter of silicon carbide powder IV. Silicon carbide powder III has a median diameter of 1.5 μm and a purity of greater than 99%, and silicon carbide powder IV has a median diameter of 0.3 μm and a purity of greater than 99%.

[0052] Coating layer application: The carrier is held vertically, and the coating layer slurry is poured into the carrier channel from the bottom at a speed of 80 mm / s. When the coating layer slurry reaches the top of the carrier, the process is stopped for 4 seconds, and finally the coating layer slurry in the carrier channel is released to form a coating layer by utilizing capillary action.

[0053] Drying of the coating layer: The prepared silicon carbide membrane is dried in a drying room for 24 hours at a relative humidity of 50-60% and a temperature of 25-30°C, with hot air passing through the material channel at a flow rate of 2 m / s.

[0054] High-temperature sintering and recrystallization: The dried silicon carbide film is sintered at high temperature under argon atmosphere protection conditions. The temperature is raised to 500°C and kept at that temperature for 2 hours to degumm the silicon carbide film. After degumming is completed, the temperature is raised to 1600°C, recrystallization sintering is performed, the temperature is kept at that temperature for 5 hours, and finally the film is cooled to room temperature in the furnace. The sintering temperature rise process takes 20 hours.

[0055] Oxidation sintering: The obtained silicon carbide membrane is subjected to oxidation sintering at 800°C under aeration conditions, which removes residual carbon and increases the mechanical strength of the membrane. The obtained product is a 100% recrystallized silicon carbide membrane, with a separation layer of about 47.9 μm thick, attached to the carrier surface, and without an intermediate layer, as shown in Figure 7.

[0056] As a result of the measurements, the average pore size of the pore structure of the prepared ceramic membrane support was 10.5 μm (see Figure 8), and the average pore size of the pore structure of the separation layer was 0.15 μm (see Figure 9). This enabled the preparation of a large pore size support, and based on this, the application and preparation of a separation layer with a small average pore size (0.15 μm) was realized, ensuring the quality of the filtered water while also ensuring high throughput through the large pore size support.

[0057] [Example 2] 1) Molding and sintering of silicon carbide materials Selection of raw materials: Silicon carbide powder I, silicon carbide powder II, methylhydroxyethyl cellulose, polyethylene glycol, acrylic polymer and water are taken and prepared according to the mass ratio of 65:15:5:1:1:13. The median diameter of silicon carbide powder I is 15 times that of silicon carbide powder II. The median diameter of silicon carbide powder I is 30 μm and the purity is greater than 98%, while the median diameter of silicon carbide powder II is 2 μm and the purity is greater than 99%.

[0058] Mixing of ingredients: Mix the selected ingredients at room temperature (20-25 degrees Celsius) based on the proportions in the following order: add liquid first and then powder to form a homogenous mixture.

[0059] Molding: The resulting mixture is fed into an extruder and molded into a multi-channel tubular material under an extrusion pressure of 120 MPa.

[0060] Drying: The material is extruded and dried in a drying room for 24 hours. The relative humidity is 50-60%, the temperature is 25-30℃, and hot air is passed through the material channel at a flow rate of 2m / s.

[0061] High-temperature sintering and recrystallization: After drying, the material is sintered at high temperature under argon atmosphere protection conditions. The temperature is raised to 500°C, kept at that temperature for 2 hours, and the material is degummed. After degumming is completed, the temperature is raised to 2400°C. The sintering temperature rise process takes 25 hours, and the material is sintered at high temperature and kept at that temperature for 5 hours, and finally cooled to room temperature in the furnace.

[0062] 2) Application of silicon carbide coating layer Preparation of slurry: Silicon carbide powder III, silicon carbide powder IV, methylhydroxyethyl cellulose, phthalate ester, acrylic polymer dispersant, silicone polyether antifoaming agent, alcohol surfactant PEG and water are mixed uniformly in a mass ratio of 15:15:6:6:1.5:1.5:4:51, the pH is controlled to 7-8, alumina balls with a diameter of 8-10 mm are added and the mixture is subjected to rolling polishing for 48 hours to obtain a coating layer slurry. The median diameter of silicon carbide powder III is five times the median diameter of silicon carbide powder IV. Silicon carbide powder III has a median diameter of 1.5 μm and a purity of greater than 99%, and silicon carbide powder IV has a median diameter of 0.3 μm and a purity of greater than 99%.

[0063] Coating layer application: The carrier is held vertically, and the coating layer slurry is poured into the carrier channel from the bottom at a speed of 80 mm / s. When the coating layer slurry reaches the top of the carrier, the process is stopped for 3 seconds, and finally the coating layer slurry in the carrier channel is released to form a coating layer by utilizing capillary action.

[0064] Drying of the coating layer: The prepared silicon carbide membrane is dried in a drying room for 24 hours at a relative humidity of 50-60% and a temperature of 25-30°C, with hot air passing through the material channel at a flow rate of 2 m / s.

[0065] High-temperature sintering and recrystallization: The dried silicon carbide film is sintered at high temperature under argon atmosphere protection conditions. The temperature is raised to 500°C and kept at that temperature for 2 hours to degumm the silicon carbide film. After degumming is completed, the temperature is raised to 1800°C. The sintering temperature rise process takes 25 hours, recrystallization sintering is performed, the temperature is kept at that temperature for 5 hours, and finally the film is cooled to room temperature in the furnace.

[0066] Oxidation sintering: The obtained silicon carbide membrane is subjected to oxidation sintering at 800℃ under ventilation conditions, which removes residual carbon and increases the mechanical strength of the membrane. The resulting product is a 100% recrystallized silicon carbide membrane.

[0067] As a result of the measurement, the average pore size of the pore structure of the prepared ceramic membrane support was 15 μm (see FIG. 10), the average pore size of the pore structure of the separation layer was 0.2 μm (see FIG. 11), and no intermediate layer was included.

[0068] Based on the ceramic membrane prepared in the above examples, the ceramic membranes prepared in Examples 1 and 2 were tested. The test results showed that the average pore size of the pore structure of the carrier of the prepared ceramic membrane was 10 μm or more (FIGS. 8 and 10), and the average pore size of the pore structure of the separation layer was 0.2 μm or less (FIGS. 9 and 11), which realized the preparation of a large pore carrier, and based on this, realized the application and preparation of a separation layer with a small pore size. In particular, the technology of the present invention realizes the preparation of a ceramic filtration membrane in which the difference between the pore size of the separation layer and the pore size of the carrier reaches 20 times or more. By using the raw materials and preparation process of the above examples, it is possible to realize the preparation of a silicon carbide ceramic membrane in which the average pore size of the carrier is 10 μm or more and the average pore size of the separation layer is 0.2 μm or less, and particularly preferably, the average pore size of the separation layer is controlled within the range of 0.15 μm to 0.2 μm, thereby realizing the preparation of a low-cost, high-throughput ceramic filtration membrane.

[0069] Testing was carried out on the silicon carbide ceramic membrane prepared in Example 1 of the present invention, and at the same time, a conventional sandwich structure ceramic membrane with an average pore size close to (0.15 μm) was selected to compare with the ceramic membrane prepared in the present invention. The ratio of the throughput of pure water between the conventional silicon carbide membrane (sandwich structure) and the new silicon carbide membrane (removing the middle layer) was 3000LMH / bar vs 4000LMH / bar, which shows that the throughput of the ceramic membrane prepared in the process of the present invention is obviously improved by more than 30%. In addition, the results of the porosity test showed that the ceramic body prepared in the present invention has a porosity of more than 42%, realizing high throughput filtration.

[0070] A strength test was carried out on the coating layer structure of the ceramic membrane prepared in this Example 1, and the separation layer (i.e., membrane) in the test results had a fairly high mechanical strength, with a bending strength of 25 MPa or more. Measurements of multiple test membranes showed that they could hold a strength of around 35 MPa.

[0071] Although the present invention has been described above with reference to preferred embodiments, they are not intended to limit the present invention. Those skilled in the art to which the present invention pertains may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be considered as being based on the definition of the claims. [Explanation of symbols]

[0072] (none)

Claims

1. 1. A method for preparing a high throughput silicon carbide ceramic filtration membrane, the method comprising: (1) preparing a multi-channel tubular material, and sintering the multi-channel tubular material at a high temperature of 2000-2400° C. under an inert atmosphere to prepare a carrier having a pore structure with a first average pore size; (2) standing the carrier upright, pouring a coating layer slurry into a channel from the bottom of the carrier prepared in step (1), and releasing the coating layer slurry in the channel after the coating layer slurry reaches the top of the carrier and is held for a predetermined time to form a channel coating layer, in which the particles of the coating layer slurry are charged with the same charge as the surface of the carrier; (3) drying the channel covering layer formed in the step (2); (4) sintering the channel covering layer at a high temperature of 1600 to 2000° C. under an inert atmosphere to form a pore structure having a second average pore size to prepare a separation layer; (5) performing oxidation sintering on the separation layer obtained in the step (4) under an aeration condition to remove residual carbon; Including, In the step (1), the multi-channel tubular blank is prepared by mixing silicon carbide powder having a first particle size mismatch and a first additive with water, and extruding the resulting mixture; The silicon carbide powder having a first particle size mismatch degree includes silicon carbide powder I and silicon carbide powder II, the median diameter of the silicon carbide powder I is 5 to 30 times the median diameter of the silicon carbide powder II, the median diameter of the silicon carbide powder I is between 10 and 30 μm, and the median diameter of the silicon carbide powder II is between 0.5 and 6 μm; The first auxiliary agent includes an adhesive, a plasticizer, and a dispersant; In the step (2), the coating layer slurry is prepared by mixing a silicon carbide powder having a second particle size mismatch degree and a second auxiliary agent with water; The silicon carbide powder having the second particle size mismatch degree includes silicon carbide powder III and silicon carbide powder IV, the median diameter of the silicon carbide powder III is 3 to 8 times the median diameter of the silicon carbide powder IV, the median diameter of the silicon carbide powder III is between 0.5 and 6 μm, and the median diameter of the silicon carbide powder IV is between 0.1 and 3 μm; The second auxiliary agent includes an adhesive, a plasticizer, a dispersant, an antifoaming agent, and a surfactant, and the mass ratio of the silicon carbide powder III, the silicon carbide powder IV, the adhesive, the plasticizer, the dispersant, the antifoaming agent, the surfactant, and the water is (5 to 15):(5 to 15):(3 to 10):(5 to 15):(0 to 1.5):(0 to 1.5):(1 to 5):(50 to 80); The pH value of the coating layer slurry is between 6 and 10; 1. A method for preparing a high throughput silicon carbide ceramic filtration membrane, comprising:

2. The method for preparing a high-throughput silicon carbide ceramic filtration membrane as described in claim 1, characterized in that in the step (1), the mass ratio of the silicon carbide powder I, the silicon carbide powder II, the adhesive, the plasticizer, the dispersant and the water is (50-75):(10-20):(4-8):(1-3):(1-3):(10-20).

3. A method for preparing a high-throughput silicon carbide ceramic filtration membrane as described in claim 1, characterized in that in step (1), the method further comprises drying the multi-channel tubular material before high-temperature sintering the multi-channel tubular material at a temperature of 2000 to 2400°C.

4. The coating layer slurry is first The method for preparing a high-throughput silicon carbide ceramic filtration membrane according to claim 1, characterized in that: alumina balls with a diameter of 8-10 mm are added, and roll-polished for 12-48 hours are used as a pretreatment method, before being put into the channel.

5. The method for preparing a high throughput silicon carbide ceramic filtration membrane as described in claim 1, characterized in that the coating layer slurry is fed into the channel at a speed of 20 to 100 mm / s.

6. The method for preparing a high-throughput silicon carbide ceramic filtration membrane as described in claim 1, wherein in step (2), the predetermined time is 3 to 15 seconds.

Citation Information

Patent Citations

  • Preparation method of pure silicon carbide porous ceramic membrane

    CN104261867A

  • Preparation method of high-strength uniform-hole silicon carbide ceramic membrane

    CN105175005A

  • Composite filter membrane for water treatment

    CN106145264A

  • Anionic antibacterial ceramic separation membrane and preparation method thereof

    CN106731888A

  • Production of porous ceramic

    JP1999116352A