Method for producing silicon single crystals

By controlling oxygen concentration and pulling rate with a magnetic field and thermal stress adjustment, the method effectively suppresses internal dislocations in silicon single crystals, enhancing slip resistance and producing high-quality wafers.

JP7561498B2Active Publication Date: 2024-10-04GLOBALWAFERS JAPAN
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020023535
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-02-14
Publication Date
2024-10-04
Estimated Expiration
2040-02-14

AI Technical Summary

Technical Problem

Existing methods for producing silicon single crystals using the Czochralski method fail to effectively suppress internal dislocations, which are not visible on the crystal surface and can only be detected after wafer slicing, leading to unusable wafers.

Method used

Control the oxygen concentration and pulling rate during crystal growth by applying a horizontal magnetic field and adjusting thermal stress to suppress internal dislocations, using a correlation formula to set the oxygen concentration (A) and pulling speed (B) within specific ranges.

Benefits of technology

The method ensures improved slip resistance and prevents the occurrence of internal dislocations, allowing for higher pulling speeds and reducing the introduction of interstitial atoms, thereby producing high-quality silicon single crystals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561498000001
    Figure 0007561498000001
  • Figure 0007561498000002
    Figure 0007561498000002
  • Figure 0007561498000003
    Figure 0007561498000003
Patent Text Reader

Abstract

To provide a method for producing a silicon single crystal whereby it is possible to keep an oxygen level required for improving the slip resistance by thermal stress in the crystal and to prevent the occurrence of internal rearrangement when pulling up the silicon single crystal.SOLUTION: In a step for growing a straight barrel portion of a silicon single crystal, a correlational formula between the oxygen level A(×1018atoms / cm3) in the single crystal and the single crystal pulling-up speed B (mm / min) is expressed as: B=-1 / 4A+0.75, and the oxygen level in the single crystal is controlled to A or more and the single crystal-pulling up speed is controlled to B or more.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a silicon single crystal by pulling the silicon single crystal by the Czochralski method (CZ method), and in particular to a method for producing a silicon single crystal capable of suppressing internal dislocations (dislocation generation) during pulling of the silicon single crystal. [Background technology]

[0002] The growth of silicon single crystals by the CZ method is carried out by filling a quartz crucible 51 placed in a chamber 50 as shown in FIG. 9 with polysilicon as a raw material, heating and melting the polysilicon using a heater 52 provided around the quartz crucible 51 to form silicon melt M, immersing a seed crystal (seed) P attached to a seed chuck in the silicon melt, and lifting up the seed chuck while rotating the seed chuck and the quartz crucible 51 in the same direction or in opposite directions.

[0003] Generally, prior to the start of pulling, after the temperature of the silicon melt M has stabilized, a seed crystal P is brought into contact with the silicon melt M to perform necking, which melts the tip of the seed crystal P. The necking is an essential process for removing dislocations that occur in the silicon single crystal due to thermal shock caused by the contact between the seed crystal P and the silicon melt M. This necking forms a neck portion P1, which generally needs to have a diameter of 3 to 4 mm and a length of 30 to 40 mm or more.

[0004] In addition, the processes that follow after the start of pulling include the process of forming a shoulder portion C1, which expands the crystal to the diameter of the body portion after necking is completed, the process of forming the body portion C2, which grows the single crystal that will become the product, and the process of forming a tail portion (not shown), which gradually reduces the diameter of the single crystal after the body portion formation process.

[0005] However, if dislocations occur in the crystal during the silicon single crystal pulling process, the wafers cut from the dislocation-caused crystal contain many dislocations and therefore cannot be used for device manufacture. In response to such problems, Patent Document 1 (JP 2006-347853 A) discloses a method for growing silicon single crystals in which dislocations caused by thermal stress are suppressed by including a hydrogen atom-containing gas in the atmospheric gas used when growing the single crystal.

[0006] Specifically, the hydrogen molecular partial pressure of the gas of the hydrogen atom-containing substance in the atmospheric gas is set to 40 to 400 Pa, and the concentration of oxygen gas in the atmospheric gas is set to a volume ratio that satisfies α-2β≧3%, where α is the hydrogen molecular equivalent concentration of the gas of the hydrogen atom-containing substance, and β is the oxygen gas concentration.

[0007] According to the method disclosed in Patent Document 1, hydrogen elements in the gas of the hydrogen-atom-containing substance penetrate into the interstitial spaces of the silicon crystal, which is equivalent to increasing the concentration of interstitial atoms in the silicon crystal, and it is possible to reduce the number of interstitial atoms taken into the crystal from the silicon melt during the silicon solidification process. This makes it possible to suppress slip dislocations originating from dislocation clusters (defects of about 10 μm in size formed as agglomerates of excess interstitial silicon) that are generated by thermal stress.

[0008] Incidentally, Patent Document 2 (JP Patent Publication No. 2002-187796) discloses a method in which, when a magnetic field is applied to pull up a single crystal, if dislocations occur in the single crystal being grown, the heater output is increased from the single crystal production conditions without applying a magnetic field, thereby melting the dislocated single crystal, and then a magnetic field is applied again while the heater output is set to the single crystal production conditions, and the single crystal is pulled up again.

[0009] According to this method, when the single crystal is pulled up after melt-back (re-melting) without applying a magnetic field, foreign matter on the surface of the molten liquid is prevented from being incorporated into the single crystal, making it possible to suppress the occurrence of dislocations during the shoulder formation process, thereby achieving a significant improvement in yield. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Patent Publication No. 2006-347853 [Patent Document 2] JP 2002-187796 A Summary of the Invention [Problem to be solved by the invention]

[0011] Generally, as the pulling speed of a single crystal decreases, the amount of interstitial atoms introduced increases, and the amount of strain introduced into the crystal tends to increase. On the other hand, as the amount of oxygen introduced into the crystal increases, the slip resistance tends to increase. If the amount of strain in the crystal increases and the balance between strain and slip resistance is lost, dislocations are introduced from the center of the crystal where the stress is high. Since such dislocations occur inside the crystal (called internal dislocations), the crystal habit lines, which are indicators of whether or not there is a dislocation, do not disappear on the crystal surface, and inspection after slicing into wafers is necessary to confirm the dislocations. However, the inventions disclosed in Patent Documents 1 and 2 are based on dislocations that can be determined based on the presence or absence of crystal habit lines, and do not take into consideration internal dislocations.

[0012] The present inventors focused on the relationship between the crystal pulling speed, which affects the amount of distortion, and the crystal oxygen concentration, which affects the slip resistance required to maintain balance with the distortion, and as a result of extensive research, they discovered that internal dislocations in the crystal can be suppressed by controlling the crystal oxygen concentration and the pulling speed when growing silicon single crystals by the CZ method, which led to the invention.

[0013] The present invention has been made under the circumstances described above, and has an object to provide a method for producing a silicon single crystal that can ensure an oxygen concentration in the crystal to improve slip resistance and prevent the occurrence of internal dislocations when pulling up the silicon single crystal. [Means for solving the problem]

[0014] The method for producing a silicon single crystal according to the present invention, which has been made to solve the above problems, is a method for producing a silicon single crystal by pulling up a silicon single crystal by the Czochralski method in order to produce a wafer having a diameter of 300 mm, and the method comprises applying a horizontal magnetic field having a magnetic flux density of 2500 Gauss or more and 3000 Gauss or less during pulling up the silicon single crystal, and increasing the oxygen concentration in the silicon single crystal to A(×10 18 atoms / cm 3 ) and the pulling speed of the silicon single crystal is B (mm / min), B≧-1 / 4A+0.75 、0.4≦A<1.8 The oxygen concentration A in the silicon single crystal and the pulling speed B of the silicon single crystal are controlled so as to obtain In the silicon single crystal straight body growing step, the temperature of a water-cooled body surrounding the silicon single crystal is adjusted to set the thermal stress in the crystal axis portion of the straight body to 18 MPa or less in terms of Mises stress. It is characterized by the fact that

[0015] As described above, according to the present invention, the oxygen concentration in the crystal and the pulling rate during growth of the crystal body were controlled to be equal to or higher than their respective threshold values ​​determined based on the correlation equations, thereby growing a silicon single crystal. This makes it possible to ensure an oxygen concentration in the crystal that improves slip resistance, and also ensures a pulling speed equal to or greater than the threshold determined by the correlation equation. This suppresses the introduction of interstitial atoms, making it difficult for distortion to accumulate inside the crystal, and thus making it possible to suppress the occurrence of internal dislocations caused by distortion in the crystal.

[0016] In addition, Silicone The lower limit of the oxygen concentration A in the crystal is 0.4×10 18 atoms / cm 3 The upper limit is 1.8×10 18 atoms / cm 3 It is desirable that: Also, In the silicon single crystal straight body growing step, a temperature of a water-cooled body surrounding the silicon single crystal is adjusted; It is desirable that the thermal stress in the crystal axis portion of the straight body portion be 18 MPa or less in terms of the Mises stress. When the oxygen concentration and the pulling rate are controlled to be equal to or higher than the respective threshold values ​​determined based on the correlation equation, the thermal stress in the crystal axis portion can be reduced to a small thermal stress of 18 MPa or less, which is a von Mises stress. Effect of the Invention

[0017] According to the present invention, it is possible to provide a method for producing a silicon single crystal that can ensure an oxygen concentration in the crystal to improve the slip resistance due to thermal stress, and can prevent the occurrence of internal dislocations when pulling up the silicon single crystal. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a cross-sectional view of a single crystal pulling apparatus for carrying out a method for producing a silicon single crystal according to the present invention. [Diagram 2] FIG. 2 is a flow chart showing a process for producing a silicon single crystal using the single crystal pulling apparatus of FIG. [Diagram 3] FIG. 3 is a graph for explaining the method for producing a silicon single crystal according to the present invention. [Figure 4] FIG. 4 is a graph showing the results of Experiment 1 of the present invention. [Diagram 5] FIG. 5 is a photograph showing the results of an example of the present invention and a comparative example. [Figure 6] FIG. 6 is a graph showing the results of Experiment 2 of the present invention. [Figure 7] FIG. 7 is a graph showing the results of Experiment 3 of the present invention. [Figure 8] FIG. 8 is a simulation image showing the results of an embodiment of the present invention. [Figure 9] FIG. 9 is a cross-sectional view for explaining a process of pulling a silicon single crystal by the Czochralski method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The method for producing a silicon single crystal according to the present invention will be described below with reference to the drawings. Fig. 1 is a cross-sectional view of a single crystal pulling apparatus for carrying out the method for producing a silicon single crystal according to the present invention. Fig. 2 is a flow chart showing the flow of the method for producing a silicon single crystal using the single crystal pulling apparatus of Fig. 1.

[0020] This single crystal pulling apparatus 1 comprises a furnace body 10 formed by stacking a pull chamber 10b on top of a cylindrical main chamber 10a, and is equipped with a carbon susceptor (or graphite susceptor) 2 that is rotatable about a vertical axis and movable up and down within this furnace body 10, and a quartz glass crucible 3 (hereinafter simply referred to as crucible 3) held by the carbon susceptor 2.

[0021] The crucible 3 has a straight body portion 3a and a bottom portion 3b formed below the straight body portion 3a, and is rotatable about a vertical axis together with the rotation of the carbon susceptor 2. Further, below the carbon susceptor 2, there are provided a rotation drive unit 14 such as a rotation motor for rotating the carbon susceptor 2 around a vertical axis, and an elevation drive unit 15 for moving the carbon susceptor 2 up and down. The rotation drive unit 14 is connected to a rotation drive control unit 14a, and the elevation drive unit 15 is connected to an elevation drive control unit 15a.

[0022] The single crystal pulling apparatus 1 also includes a side heater 4 that uses resistance heating to melt the semiconductor raw material (raw polysilicon) loaded in the crucible 3 to form silicon melt M (hereinafter simply referred to as melt M), and a pulling mechanism 9 that winds up a wire 6 and pulls up the grown single crystal C. A seed crystal P is attached to the tip of the wire 6 of the pulling mechanism 9.

[0023] The side heater 4 is connected to a heater drive control unit 4a that controls the amount of power supplied, and the lifting mechanism 9 is connected to a rotation drive control unit 9a that controls the rotation drive thereof. In addition, in this single crystal pulling apparatus 1, a magnetic field applying electromagnetic coil 8 is installed outside the furnace body 2. When a predetermined current is applied to this magnetic field applying electromagnetic coil 8, a horizontal magnetic field of a predetermined strength is applied to the silicon melt M in the crucible 3. An electromagnetic coil control unit 8a that controls the operation of the magnetic field applying electromagnetic coil 8 is connected to the magnetic field applying electromagnetic coil 8.

[0024] That is, in this embodiment, the MCZ method (Magnetic field applied CZ method) is carried out in which a magnetic field is applied into the molten liquid M to grow a single crystal, thereby controlling the convection of the silicon molten liquid M and stabilizing the single crystallization.

[0025] In addition, a radiation shield 7 is disposed above the molten liquid M formed in the crucible 3 to surround the single crystal C. This radiation shield 7 has openings at the top and bottom, and serves to block excess radiant heat from the side heaters 4 and the molten liquid M to the single crystal C being grown, and to straighten the gas flow in the furnace. The gap between the lower end of the radiation shield 7 and the melt surface is controlled to maintain a predetermined distance according to the desired characteristics of the single crystal to be grown.

[0026] A cylindrical water-cooling body 12 is disposed inside the radiation shield 7. Cooling water is supplied to this water-cooling body 12 by cooling water supply means 12a, and is configured to maintain a predetermined temperature by circulating the water.

[0027] In addition, this single crystal pulling apparatus 1 is equipped with a computer 11 having a memory device 11a and an arithmetic and control device 11b, and the rotation drive control unit 14a, the lift drive control unit 15a, the electromagnetic coil control unit 8a, the rotation drive control unit 9a, and the cooling water supply means 12a are each connected to the arithmetic and control device 11b.

[0028] In the single crystal pulling apparatus 1 configured as above, when growing a single crystal C having a diameter of, for example, 300 mm, pulling is performed as follows: First, raw polysilicon (e.g., 350 kg) is loaded into the crucible 3, and a crystal growing process is started based on a program stored in the storage device 11a of the computer 11.

[0029] First, a predetermined atmosphere (mainly an inert gas such as argon gas) is created inside the furnace body 10, and the raw material polysilicon loaded in the crucible 3 is melted by heating with the side heater 4 to become a molten liquid M (step S1 in FIG. 2). Furthermore, the crucible 3 is rotated at a predetermined height position at a predetermined rotation speed (rpm) (step S2 in FIG. 2).

[0030] Next, a predetermined current is passed through the magnetic field applying electromagnetic coil 8, and a horizontal magnetic field is started to be applied to the melt M with a magnetic flux density set within a range of 1000 to 4000 Gauss (for example, 2500 Gauss) (step S3 in FIG. 2). Further, the wire 6 is lowered to bring the seed crystal P into contact with the molten liquid M, and necking is carried out to melt the tip of the seed crystal P, thereby starting the formation of a neck portion P1 (step S4 in FIG. 2). Once the neck portion P1 is formed, the pulling conditions are adjusted using parameters such as the power supplied to the side heater 4, the pulling speed, and the strength of the applied magnetic field, and the seed crystal P begins to rotate at a predetermined rotation speed in the direction opposite to the rotation direction of the crucible 3.

[0031] Then, the crystal diameter is gradually enlarged to form a shoulder portion C1 (step S5 in FIG. 2), and the process proceeds to forming a straight body portion C2 that will become the product portion (step S6 in FIG. 2). In the growth of the body portion C2, the computer 11 calculates the crystal oxygen concentration A (×10 18 atoms / cm 3 ), and the vertical axis y is the pulling speed B (mm / min). The values ​​of A and B determined by the correlation equation of the linear function B=-1 / 4A+0.75 are set as thresholds, and the pulling speed and the oxygen concentration of the crystal are controlled so that they are equal to or greater than these thresholds.

[0032] Specifically, the value of the crystal oxygen concentration is set to be the target oxygen concentration value of the wafer to be produced, for example. If A is the target oxygen concentration value, then the correlation equation is entered with the oxygen concentration value A (×10 18 atoms / cm 3) is substituted, the pulling speed value B=-1 / 4A+0.75 (mm / min) is set as the pulling speed threshold. That is, the computer 11 performs pulling control so that the oxygen concentration is equal to or higher than the target value A, and also performs pulling control at a pulling speed equal to or higher than B.

[0033] In this manner, when growing a single crystal C having the above-mentioned crystal oxygen concentration A, the pulling speed is controlled to be equal to or faster than B, thereby suppressing the introduction of interstitial atoms, making it difficult for distortion to accumulate inside the crystal, and suppressing the occurrence of internal dislocations caused by distortion in the crystal. The range of the crystal oxygen concentration A is 0.4(×10 18 atoms / cm 3 ) or more than 1.8(×10 18 atoms / cm 3 ) is desirable. This is because the limit of low oxygen concentration is 0.4(×10 18 atoms / cm 3 ), which is 1.8(×10 18 atoms / cm 3 ) or more, there is a risk of dislocations occurring during crystal pulling. The pulling speed B is preferably in the range of 0.3 (mm / min) or more and less than 1.1 (mm / min) because if the pulling speed B is less than 0.3 (mm / min), the rate of dislocations occurring during crystal pulling increases, and if it is 1.1 (mm / min) or more, there is a risk of the crystal being deformed.

[0034] The oxygen in the single crystal is introduced as follows: When the silicon melt M flows in contact with (along) the side wall of the crucible 3, silicon is chemically active at its melting point, so that the silicon melt M reacts with the quartz component of the crucible 3, dissolves the side wall of the crucible 3, and O (oxygen) is taken into the silicon melt M.

[0035] In order to control the oxygen concentration in the single crystal grown from the silicon melt M into which O (oxygen) has been introduced in this manner, the flow (convection) of the silicon melt M can be controlled, preferably by adjusting the furnace pressure (increasing the furnace pressure decreases the oxygen concentration in the crystal).

[0036] In addition, by adjusting the temperature of the water-cooling body 12, the temperature of the growing body portion C2 is cooled, for example, from 1412°C to 800°C, and the thermal stress in the crystal axis portion is suppressed to, for example, 18 MPa or less in terms of Mises stress. In this way, the thermal stress inside the crystal is kept low, and the oxygen concentration in the crystal is controlled to be equal to or higher than the target value A during the growth of the body portion C2, thereby ensuring the amount of oxygen introduced into the crystal and improving the slip resistance.

[0037] As the formation of the body portion C2 of the silicon single crystal C progresses, the carbon susceptor 2 housing the crucible 3 is moved upward to maintain the position of the melt surface M1 relative to the radiation shield 7 and side heater 4, which are fixed in position. Moreover, by applying a magnetic field having a magnetic flux density set, for example, in the range of 1000 to 4000 Gauss, more preferably 2000 to 3000 Gauss, natural convection of the molten liquid M is suppressed.) If the magnetic flux density of the horizontal magnetic field is set low, in the range of 800 to 1000 Gauss, the molten liquid M becomes unstable and crystal deformation is likely to occur.

[0038] Then, when the body portion C2 is formed to a predetermined length, the process proceeds to the final tail portion process (step S7 in FIG. 2). In this tail portion process, the contact area between the lower end of the crystal and the molten liquid M gradually decreases, and the single crystal C and the molten liquid M are separated, thereby producing a silicon single crystal.

[0039] As described above, according to the present embodiment, the oxygen concentration in the crystal and the pulling speed during the growth of the crystal body are controlled to be equal to or higher than the respective threshold values ​​determined based on the correlation equations, and a silicon single crystal is grown. Furthermore, the thermal stress in the crystal axis during the growth of the body is suppressed to a von Mises stress of 18 MPa or less. This ensures an oxygen concentration in the crystal that improves slip resistance, and also ensures a pulling speed equal to or greater than the threshold determined by the correlation equation. This suppresses the introduction of interstitial atoms, making it difficult for distortion to accumulate inside the crystal, and thus suppresses the occurrence of internal dislocations caused by distortion in the crystal. EXAMPLES

[0040] The method for producing a silicon single crystal according to the present invention will be further described based on examples. (Experiment 1) In experiment 1, 360 kg of raw polysilicon was put into the crucible in the single crystal pulling apparatus having the configuration shown in the above embodiment, and a silicon single crystal having a diameter of 307 mm was pulled. In order to suppress natural convection of the silicon melt, the magnetic flux density of the horizontal magnetic field applied during pulling was set to 2500 Gauss.

[0041] The temperature of the water-cooled body surrounding the single crystal was adjusted, the distance from the surface of the single crystal to the surface of the water-cooled body was set to 55 mm, and the von Mises stress was adjusted to 18 MPa or less. The magnetic field strength was set to 3000 Gauss. As the inert gas, Ar gas was used, and the flow rate of the inert gas was set to 130 L / min. The pressure inside the furnace was set to 15 to 80 Torr. The rotation speed of the crucible was set to 0.5 rpm, and the rotation speed of the single crystal was set to 9.5 rpm (the rotation directions were opposite to each other).

[0042] In addition, in experiment 1, 110 pulling trials were performed. The target crystal oxygen concentration was set for each trial, and the pulling speed was changed. The results of each trial in Experiment 1 are shown in the graph in FIG. In the graph of FIG. 4, the vertical axis y represents the average pulling speed (mm / min), and the horizontal axis x represents the oxygen concentration at the center of the crystal (10 18 atoms / cm 3 ) is a plot of the average pulling rate and the oxygen concentration at the center of the crystal in each trial. In each trial, the obtained single crystal was processed into an etched wafer and the presence or absence of internal dislocations was confirmed by shining oblique light on it and transmitting it through the surface. In each trial, as shown in Figure 4, those without internal dislocations are indicated with ◇, and those with internal dislocations are indicated with ×.

[0043] From the graph in FIG. 4, the correlation equation is y=-1 / 4x+0.75 (y is the average pulling speed (mm / min), x is the oxygen concentration at the center of the crystal (10 18 atoms / cm 3 In the above, it was found that when the value A of y when x=B is set as the threshold value of the average pulling speed, and when the crystal oxygen concentration is equal to or greater than B and the pulling speed is equal to or greater than A, there are no internal dislocations.

[0044] Fig. 5(a) shows a photograph of a case where there are no internal dislocations when inspecting for the presence or absence of internal dislocations, and Fig. 5(b) shows a photograph of a case where there are internal dislocations. In the example of the results shown in Fig. 5(b), several cross-shaped reflections of about 5 to 20 mm in size are seen, but since the crystal habit lines have not disappeared, they can be confirmed as internal dislocations.

[0045] As a result of this experiment 1, as shown in the graph in Figure 4, it was confirmed that no internal dislocations occur when the single crystal is pulled up at a value equal to or higher than the value of y obtained by substituting the target oxygen concentration for x in the correlation equation y = -1 / 4x + 0.75.

[0046] (Experiment 2) In experiment 2, the conditions of magnetic flux density, inert gas flow rate, furnace pressure, and rotation speed of the crucible and single crystal, which affect the flow (convection) of the silicon melt, were changed from those of experiment 1. The other conditions were the same as those of experiment 1. Specifically, the magnetic flux density was 2000 Gauss, the flow rate of the inert gas was 130 l / min, the pressure inside the furnace was 15 to 80 Torr, and the rotation speed of the crucible was 0.5 rpm and the rotation speed of the single crystal was 9.5 rpm (the rotation directions were opposite to each other).

[0047] The results of each trial in Experiment 2 are shown in the graph of FIG. 6. In the graph of FIG. 6, the vertical axis y represents the average pulling speed (mm / min) and the horizontal axis x represents the oxygen concentration at the center of the crystal (10 18 atoms / cm 3 ) are plotted against the average pulling speed and the oxygen concentration at the center of the crystal in each trial. In each trial, those without internal dislocations are indicated by ◇, and those with internal dislocations are indicated by ×. As a result of experiment 2, as shown in the graph in Figure 6, when the target oxygen concentration was substituted for x in the correlation equation y = -1 / 4x + 0.75, and the single crystal was pulled at a value equal to or higher than the y value, no internal dislocations were generated.

[0048] (Experiment 3) In experiment 3, the conditions that affect the flow (convection) of the silicon melt, such as the magnetic flux density, the flow rate of the inert gas, the furnace pressure, and the rotation speed of the crucible and the single crystal, were changed from those in experiments 1 and 2. The other conditions were the same as those in experiments 1 and 2. Specifically, the magnetic flux density was 3000 Gauss, the flow rate of the inert gas was 130 l / min, the pressure inside the furnace was 15 to 80 Torr, and the rotation speed of the crucible was 2.0 rpm and the rotation speed of the single crystal was 9.5 rpm (the rotation directions were opposite to each other).

[0049] The results of each trial in Experiment 3 are shown in the graph of FIG. 7. In the graph of FIG. 7, the vertical axis y represents the average pulling speed (mm / min) and the horizontal axis x represents the oxygen concentration at the center of the crystal (10 18 atoms / cm 3 ) are plotted against the average pulling speed and the oxygen concentration at the center of the crystal in each trial. In each trial, those without internal dislocations are indicated by ◇, and those with internal dislocations are indicated by ×. As a result of experiment 3, as shown in the graph in Figure 7, when the target oxygen concentration was substituted for x in the correlation equation y = -1 / 4x + 0.75, and the single crystal was pulled at a value equal to or higher than the y value, no internal dislocations were generated.

[0050] From the results of Experiments 1 to 3, it was found that the average pulling speed (mm / min) and the oxygen concentration at the center of the crystal (10 18 atoms / cm 3 ) it was possible to define a correlation equation y = -1 / 4x + 0.75, and by substituting the target oxygen concentration for x in the correlation equation y = -1 / 4x + 0.75, it was confirmed that no internal dislocations would occur if the single crystal was pulled up to a value of y or higher.

[0051] (Experiment 4) In experiment 4, the pulling speed was set to 0.55 mm / min and the crystal oxygen concentration was set to 1.1E18 atoms / cm 3 The thermal stress generated inside the crystal under these conditions was confirmed by simulation. In this simulation, we used STR's comprehensive heat transfer analysis software CGSim_Basic, and used a thermal expansion coefficient of 2.6×10 -6 K -1 , Young's modulus 185GPa, Poisson's ratio 0.28, density 2330kg / m 3 was set to. The simulation results are shown in Figure 8. In Figure 8, it was confirmed that the thermal stress in the crystal axis portion approximately 150 mm above the solid-liquid interface was small at 18 MPa, and that slip resistance could be improved.

[0052] From the results of Experiments 1 to 4 above, it was confirmed that the present invention can prevent the occurrence of internal dislocations caused by strain during the growth of the body portion of a single crystal. [Explanation of symbols]

[0053] 1. Single crystal pulling device 2 Carbon susceptor 3. Quartz glass crucible (crucible) 4 Side heater 6 Wire 7 Radiation Shield 8. Magnetic field application electromagnetic coil 9 Lifting mechanism 10 Furnace body 11. Computers 11a Storage device 11b Arithmetic and control device 12 Water cooling body 14 Rotation drive unit 15 Lifting drive unit C Silicon single crystal M Silicon melt C1 Shoulder C2 Straight body part

Claims

1. A method for producing a silicon single crystal by pulling a silicon single crystal by the Czochralski method to produce a wafer having a diameter of 300 mm, comprising the steps of: During pulling of the silicon single crystal, a horizontal magnetic field having a magnetic flux density of 2500 Gauss or more and 3000 Gauss or less is applied; In the silicon single crystal straight body portion growing step, The oxygen concentration in the silicon single crystal is A (×10 18 atoms / cm 3 ) and the pulling speed of the silicon single crystal is B (mm / min), B≧−1 / 4A+0.75, 0.4≦A<1.

8. Controlling the oxygen concentration A in the silicon single crystal and the pulling speed B of the silicon single crystal; A method for producing a silicon single crystal, characterized in that, in a process for growing the straight body portion of the silicon single crystal, the temperature of a water-cooled body surrounding the silicon single crystal is adjusted to set the thermal stress in the crystal axis portion of the straight body portion to 18 MPa or less in terms of Mises stress.

Citation Information

Patent Citations

  • Method of manufacturing silicon single crystal

    JP2002187796A

  • Method for manufacturing silicon wafer

    JP2006306640A

  • Method for growing silicon single crystal

    JP2006347853A

  • Method for producing epitaxial wafer

    JP2008150283A

  • Method for growing silicon single crystal

    JP2009292702A