Method for manufacturing deposition mask unit
The described method for manufacturing vapor deposition masks through a resist film and plating connection addresses inefficiencies in existing methods, achieving precise patterning and high yield while reducing costs.
Patent Information
- Application Number
- JP2020041192
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-10
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2040-03-10
AI Technical Summary
Existing methods for manufacturing vapor deposition masks are inefficient and costly, leading to low yield and high production costs.
A method involving the formation of a resist film on a support substrate, followed by a release layer and exposure to create openings, with deposition masks secured to a support frame using a plating connection, ensuring precise patterning and high yield.
This method enables efficient and cost-effective production of vapor deposition masks with improved patterning accuracy and yield, preventing defects during manufacturing.
Smart Images

Figure 0007561504000001 
Figure 0007561504000002 
Figure 0007561504000003
Abstract
Description
[Technical field]
[0001] One embodiment of the present invention relates to a method for producing a deposition mask unit. [Background technology]
[0002] Examples of flat panel display devices include liquid crystal display devices and organic electroluminescence display devices. These display devices are structures in which thin films containing various materials such as insulators, semiconductors, and conductors are laminated on a substrate, and these thin films are appropriately patterned and connected to exhibit the function of a display device.
[0003] Methods for forming thin films are broadly classified into gas-phase methods, liquid-phase methods, and solid-phase methods. Gas-phase methods are classified into physical vapor-phase methods and chemical vapor-phase methods, and vapor deposition methods are known as a representative example of the former. The simplest vapor deposition method is vacuum vapor deposition, in which a material is heated under high vacuum to sublimate or evaporate (hereinafter, sublimation and evaporation are collectively called vaporization) the material to generate vapor, and this vapor is solidified and deposited in a target area (hereinafter, vapor deposition area) to obtain a thin film of the material. At this time, a mask that physically blocks the non-vapor deposition area is used to selectively form a thin film in the vapor deposition area and not deposit the material in other areas (hereinafter, non-vapor deposition area) (see Patent Documents 1 and 2). The mask is called a vapor deposition mask, etc. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2009-87840 A [Patent Document 2] JP 2013-209710 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of one embodiment of the present invention is to provide a method for manufacturing a deposition mask unit. For example, an object of one embodiment of the present invention is to provide a method for manufacturing a deposition mask unit efficiently, with a high yield, or at low cost. [Means for solving the problem]
[0006] One embodiment of the present invention is a method for producing a deposition mask unit, which includes disposing a resist film on a first support substrate, forming a release layer on the resist film, exposing the resist film from a side surface of the resist film toward the inside, forming at least one deposition mask having a plurality of openings on the release layer, disposing a support frame having at least one window on the release layer such that the at least one window overlaps with the plurality of openings of the at least one deposition mask, and forming a connection portion for fixing the at least one deposition mask and the support frame to each other by a plating method.
[0007] One embodiment of the present invention is a support substrate, which includes a first metal plate, a photocurable adhesive layer on the first metal plate, and a metal layer on the adhesive layer, and the adhesive layer is exposed from a side surface of the first metal plate and a side surface of the metal layer and is cured. [Brief description of the drawings]
[0008] [Figure 1] 1A and 1B are schematic top and side views of a deposition apparatus to which a deposition mask unit manufactured by a method according to one embodiment of the present invention can be applied. [Diagram 2] FIG. 2 is a schematic top view of a deposition mask unit manufactured by a method according to one embodiment of the present invention. [Diagram 3] FIG. 1 is a schematic cross-sectional view of a deposition mask unit manufactured by a method according to an embodiment of the present invention. [Figure 4] FIG. 1 is a schematic cross-sectional view of a deposition mask unit manufactured by a method according to an embodiment of the present invention. [Diagram 5]5A to 5C are schematic cross-sectional views showing a method for producing a deposition mask unit according to one embodiment of the present invention. [Figure 6] 5A to 5C are schematic cross-sectional views showing a method for producing a deposition mask unit according to one embodiment of the present invention. [Figure 7] 1A and 1B are schematic cross-sectional views and a top view illustrating a method for producing a deposition mask unit according to one embodiment of the present invention. [Figure 8] 5A to 5C are schematic cross-sectional views showing a method for producing a deposition mask unit according to one embodiment of the present invention. [Figure 9] 5A to 5C are schematic cross-sectional views showing a method for producing a deposition mask unit according to one embodiment of the present invention. [Figure 10] 1A and 1B are schematic cross-sectional views and a top view illustrating a method for producing a deposition mask unit according to one embodiment of the present invention. [Figure 11] 1A and 1B are schematic top views illustrating a method for producing a deposition mask unit according to one embodiment of the present invention. [Figure 12] 5A to 5C are schematic cross-sectional views showing a method for producing a deposition mask unit according to one embodiment of the present invention. [Figure 13] 5A to 5C are schematic cross-sectional views showing a method for producing a deposition mask unit according to one embodiment of the present invention. [Figure 14] 5A to 5C are schematic cross-sectional views showing a method for producing a deposition mask unit according to one embodiment of the present invention. [Figure 15] 5A to 5C are schematic cross-sectional views showing a method for producing a deposition mask unit according to one embodiment of the present invention. [Figure 16] 5A to 5C are schematic cross-sectional views showing a method for producing a deposition mask unit according to one embodiment of the present invention. [Figure 17] 5A to 5C are schematic cross-sectional views showing a method for producing a deposition mask unit according to one embodiment of the present invention. [Figure 18] 5A to 5C are schematic cross-sectional views showing a method for producing a deposition mask unit according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, each embodiment of the present invention will be described with reference to the drawings, etc. However, the present invention can be embodied in various forms without departing from the gist of the present invention, and should not be construed as being limited to the description of the embodiments exemplified below.
[0010] In order to clarify the description, the drawings may show the width, thickness, shape, etc. of each part in a schematic manner compared to the actual embodiment, but these are merely examples and do not limit the interpretation of the present invention. In this specification and each drawing, elements having the same functions as those explained in the previous drawings may be given the same reference numerals, and duplicate explanations may be omitted.
[0011] In this specification and the claims, when describing an aspect in which a structure is placed on top of another structure, the term "on top" is used, unless otherwise specified, to include both a case in which another structure is placed directly on top of a structure so as to be in contact with the structure, and a case in which another structure is placed above a structure via yet another structure.
[0012] Hereinafter, the expression "a certain structure is exposed from another structure" means a state in which a part of a certain structure is not covered by another structure, and also includes a state in which the part not covered by the other structure is covered by yet another structure.
[0013] A method for producing the deposition mask unit 100 according to an embodiment of the present invention will be described below.
[0014] 1. Vapor deposition equipment The deposition mask unit 100 produced by this production method can be used to selectively form a film in a desired deposition region when forming a film containing an organic compound, an inorganic compound, or an organic compound and an inorganic compound by a deposition method. FIGS. 1(A) and 1(B) are schematic top and side views of a typical deposition apparatus used for forming a film by deposition. The deposition apparatus is composed of multiple chambers having various functions. One of the chambers is a deposition chamber 160 shown in FIG. 1(A), which is partitioned from an adjacent chamber by a load lock door 162 and is configured so that the inside is maintained in a high vacuum reduced pressure state or a state filled with an inert gas such as nitrogen or argon. Therefore, a pressure reducing device, a gas intake and exhaust mechanism, and the like (not shown) are connected to the deposition chamber 160.
[0015] The deposition chamber 160 provides a space capable of accommodating an object on which a film is to be formed, such as a substrate. In the example shown in FIG. 1(A) and FIG. 1(B), a deposition source 164 is disposed under the substrate 180, and the deposition source 164 is filled with a material to be deposited. The material is heated and vaporized in the deposition source 164, and when the vapor of the material reaches the surface of the substrate 180 through an opening 102a (described later) of the deposition mask unit 100, it is cooled and solidified, and the material is deposited to provide a film of the material on the substrate 180 (on the lower surface of the substrate 180 in FIG. 1(B)). In the example shown in FIG. 1(A), the deposition source 164 (also called a linear source) having a roughly rectangular shape and disposed along one side of the substrate 180 is provided, but the deposition source 164 can have any shape, and may be a deposition source 164 called a point source that overlaps with the center of gravity of the substrate 180. In the case of a point source, the relative positions of the substrate 180 and the deposition source 164 are fixed, and a mechanism for rotating the substrate 180 may be provided.
[0016] When a linear source type deposition source 164 is used, the deposition chamber 160 is configured so that the substrate 180 and the deposition source 164 move relative to each other. FIG. 1A shows an example in which the deposition source 164 is fixed and the substrate 180 moves above the deposition source 164. As shown in FIG. 1B, the deposition chamber 160 further includes a holder 170 for holding the substrate 180 and the deposition mask unit 100, a moving mechanism 168 for moving the holder 170, a shutter 166, and the like. The holder 170 maintains the relative positions of the substrate 180 and the deposition mask unit 100, and the moving mechanism 168 allows the substrate 180 and the deposition mask unit 100 to move above the deposition source 164. The shutter 166 is provided above the deposition source 164 to block the vapor of the material or to allow it to reach the substrate 180, and is controlled to open and close by a control device (not shown). Although not shown, deposition chamber 160 is equipped with a sensor for monitoring the deposition rate of the material, an adhesion prevention plate for preventing contamination by the material, a pressure gauge for monitoring the pressure inside deposition chamber 160, and the like.
[0017] 2. Deposition mask unit FIG 2 is a schematic top view of the deposition mask unit 100, and FIG 3 is a schematic cross-sectional view taken along the chain line AA' in FIG 2. The deposition mask unit 100 has at least one or more deposition masks 102. In the following description, an example will be described in which one deposition mask unit 100 has multiple deposition masks 102. In FIGS. 2 and 3, a deposition mask unit 100 including six deposition masks 102 is shown.
[0018] Each deposition mask 102 includes a plurality of openings 102a penetrating the deposition mask 102. In each deposition mask 102, areas other than the openings 102a are referred to as non-openings. The non-openings surround the plurality of openings 102a. The deposition mask unit 100 further includes a support frame 110 that supports the deposition mask 102, and the deposition mask 102 is fixed to the support frame 110 via at least one connecting portion 120. The number of connecting portions 120 can be the same as the number of deposition masks 102 (see FIG. 2). Each connecting portion 120 surrounds the plurality of openings 102a of the corresponding deposition mask 102 and contacts the support frame 110 and the deposition mask 102.
[0019] During deposition, the deposition mask unit 100 and the substrate 180 are arranged so that the deposition region and the openings 102a overlap, and the non-deposition region and the non-openings overlap, and the vapor of the material passes through the openings 102a, and the material is deposited on the deposition region. There is no restriction on the arrangement of the multiple openings 102a, but for example, when a film is formed on each of multiple pixels provided in the display region of the display device, the multiple openings 102a are provided so as to overlap the region on the substrate 180 where the pixels are provided. Therefore, when multiple pixels are arranged in a matrix, the multiple openings 102a are also arranged in a matrix. When multiple display devices are manufactured using one deposition mask unit 100, the display regions of the multiple display devices are formed on a large substrate 180 called mother glass. In this case, the multiple openings 102a are provided so as to form multiple opening groups 102b corresponding to the multiple display regions, respectively. The distance between adjacent opening groups 102b is greater than the distance between adjacent openings 102a in each opening group 102b.
[0020] The support frame 110 has at least one window 110a (FIG. 3). When the deposition mask unit 100 has a plurality of deposition masks 102, the at least one window 110a includes a plurality of windows 110a. In this case, the number of the windows 110a may be the same as the number of the deposition masks 102. Each window 110a is provided so as to overlap with a plurality of openings 102a of the deposition masks 102. That is, the plurality of openings 102a are exposed from the support frame 110 through one of the windows 110a. Each opening group 102b is also exposed from the support frame 110 through one of the windows 110a. A part of the support frame 110 contacts the connection portion 120 between adjacent opening groups 102b.
[0021] 4(A) and 4(B) are schematic cross-sectional views of a region Ra sandwiched between adjacent windows 110a and a region Rb (see FIG. 3) at an end of the deposition mask unit 100, respectively. As shown in FIG. 4(A), the support frame 110 is not in direct contact with the deposition mask 102, and is fixed to a non-opening portion of the deposition mask 102 via a connecting portion 120. Although not shown, the support frame 110 may overlap a part of the deposition mask 102. The same is true for the region Rb, and as shown in FIG. 4(B), the support frame 110 is not in direct contact with the deposition mask 102, and is fixed to a non-opening portion of the deposition mask 102 via a connecting portion 120. In this region Rb, the support frame 110 may also overlap a part of the deposition mask 102.
[0022] As shown in FIG. 4(A) and FIG. 4(B), it is preferable that the connection portion 120 does not contact the upper surface of the support frame 110. In other words, it is preferable that the connection portion 120 is separated from the upper surface of the support frame 110. Although a method for producing the deposition mask unit 100 will be described later, by separating the connection portion 120 from the upper surface of the support frame 110, it is possible to prevent adjacent connection portions 120 from being integrated through the support frame 110 and causing distortion of the support frame 110, and it is possible to stabilize the shape of the deposition mask unit 100. In FIG. 4(A) and FIG. 4(B), the top layer of the connection portion 120 is located on the same plane as the upper surface of the support frame 110, but the top layer of the connection portion 120 may be lower than the upper surface of the support frame 110. That is, the top layer of the connection portion 120 may be located between the upper surface of the support frame 110 and the deposition mask 102.
[0023] The deposition mask 102 and the connection parts 120 contain a zero-valent metal such as nickel, copper, titanium, or chromium, and preferably contain nickel. The deposition mask 102 and the connection parts 120 may be made of the same material composition. The support frame 110 also contains a zero-valent metal, and the metal is selected from nickel, iron, cobalt, chromium, manganese, and the like. For example, the support frame 110 may be an alloy containing iron and chromium, or an alloy of iron, nickel, and manganese, and the alloy may contain carbon.
[0024] 3. Method for manufacturing deposition mask unit An example of a method for producing the deposition mask unit 100 will be described with reference to FIGS. 5(A) to 18(B). 3-1. Formation of peeling layer First, a flat surface is formed for forming the deposition mask 102. Specifically, a resist mask 132 is formed on a first support substrate 130 (FIG. 5(A)).
[0025] The first support substrate 130 is a substrate having a function of supporting a release layer 134 or a second support substrate 138 (described later) formed or disposed thereon. The first support substrate 130 includes glass, quartz, plastic, or a metal such as copper, aluminum, titanium, iron, nickel, cobalt, chromium, molybdenum, or manganese, or an alloy thereof. When the first support substrate 130 includes an alloy, the alloy may be, for example, an alloy including iron and chromium, or an alloy of iron, nickel, and manganese, and the alloy may include carbon. When a substrate including glass, quartz, or plastic is used, a substrate on which a film of the above-mentioned metal or alloy is formed may be used. As described later, a release layer 134 is formed on the first support substrate 130. When the release layer 134 is formed by electrolytic plating, it is preferable to use a metal substrate or an alloy substrate as the first support substrate 130 because it can also function as an electrode for supplying power during electrolytic plating.
[0026] The resist mask 132 is formed so as to surround the contour of the peeling layer 134 formed on the first support substrate 130 in order to determine the shape of the peeling layer 134 formed on the first support substrate 130. Therefore, although not shown, the resist mask 132 is provided so as to have a closed shape on the first support substrate 130. There is no restriction on the method of forming the resist mask 132, and it is sufficient to form a known negative or positive resist on the first support substrate 130 by exposure and development through a photomask. The resist may be liquid or solid. In the latter case, the resist is also called a resist film. In addition, in order to facilitate the peeling process described later, it is preferable to form the resist mask 132 so that its outer side surface 132a is separated from the end of the first support substrate 130.
[0027] Thereafter, a release layer 134 is formed on the first support substrate 130 (FIG. 5(B)). As described later, the release layer 134 is a functional layer for accelerating the release of the second support substrate 138 from the deposition mask unit 100 formed thereon, or for growing a plating layer that becomes the deposition mask 102, and may be made of a metal thin film such as nickel, molybdenum, or tungsten. The release layer 134 may be formed to a thickness of, for example, 20 μm to 200 μm, or 40 μm to 150 μm, by using an electroless plating method, an electrolytic plating method (hereinafter, electroless plating method and electrolytic plating method are collectively referred to as plating method), a sputtering method, or a chemical vapor deposition (CVD) method.
[0028] A resist film 136 is formed on the second support substrate 138 (FIG. 5(C)). The second support substrate 138 is a substrate having a function of holding the deposition mask 102 and the support frame 110 when forming the deposition mask unit 100, and may include materials that can be used for the first support substrate 130. For example, both the first support substrate 130 and the second support substrate 138 may be alloys of iron, nickel, and manganese. In this case, the compositions of these metals may differ between the first support substrate 130 and the second support substrate 138.
[0029] The resist film 136 contains a negative photocurable resin. That is, it contains a polymer or oligomer that is cured by light. The thickness of the resist film 136 can be selected arbitrarily, and may be appropriately selected from the range of, for example, 20 μm to 500 μm, 50 μm to 200 μm, or 50 μm to 100 μm. In order to ensure the film thickness, the resist film 136 may be laminated.
[0030] As an optional configuration, the resist film 136 may be exposed to light (primary exposure) (FIG. 5(C)). This primary exposure may be performed by irradiating light through the upper surface of the resist film 136, i.e., the surface opposite to the second support substrate 138. Note that this primary exposure is performed so that the resist film 136 is not completely hardened and maintains its flexibility. In other words, the exposure is performed so that the resist film 136 after exposure is still elastically deformable. By performing the primary exposure in this manner, the upper surface of the resist film 136 can maintain its adhesiveness, and as a result, sufficient adhesive strength can be maintained between the resist film 136 and the peeling layer 134.
[0031] Next, the first support substrate 130 and the second support substrate 138 are bonded together so that the peeling layer 134 and the resist film 136 are in contact with each other (FIG. 5(D)). At this time, there is no restriction on the up-down relationship between the first support substrate 130 and the second support substrate 138, and the latter may be placed on the former, or the former may be placed on the latter. The surface of the resist film 136 has viscosity before exposure, and the primary exposure is also performed so that the viscosity is maintained. Therefore, by bonding the first support substrate 130 and the second support substrate 138 together, the peeling layer 134 and the resist film 136 are fixed to each other. In addition, by performing the primary exposure, the flexibility of the resist film 136 decreases compared to before exposure, so that the peeling layer 134 can be stably fixed on the resist film 136, and patterning accuracy in the subsequent process can be ensured.
[0032] Thereafter, peeling is performed at the interface between the peeling layer 134 and the first support substrate 130, and the first support substrate 130 is removed (FIG. 6(A)). The peeling may be performed by fixing one of the first support substrate 130 and the second support substrate 138 and physically removing the other. The peeling layer 134 formed outside the resist mask 132 is removed together with the first support substrate 130 (FIG. 6(A)). When the shape of the resist film 136 is larger than the shape of the peeling layer 134, the end of the resist film 136 is exposed from the peeling layer 134 as shown in FIG. 6(B). In this case, the end exposed from the peeling layer 134 may be removed physically or by using a developer (FIG. 6(C)).
[0033] Here, edge exposure is performed on the resist film 136. Specifically, exposure is performed using a light source 140 so that light emitted from the light source 140 is irradiated onto the resist film 136 through the side surface 136a of the resist film 136 (FIG. 7(A)). For example, exposure may be performed so that the direction of travel of light with the maximum intensity emitted from the light source 140 passes through the side surface 136a directly from the light source or after being reflected on the upper surface of the second support substrate 138. Edge exposure is preferably performed on all the side surfaces 136a of the resist film 136. That is, as shown in FIG. 7(B), it is preferable to perform edge exposure while moving the light source 140 at a constant speed along the outer periphery of the resist film 136. At this time, the direction of the light source 140 is appropriately adjusted so that the light emitted from the light source 140 passes through the side surface 136a of the resist film 136.
[0034] The light source 140 may be configured arbitrarily, and is configured to emit light (e.g., ultraviolet light with a wavelength of 365 nm or visible light) that is effective for curing the photocurable resin contained in the resist film 136. The light from the light source 140 may be a laser or incoherent light. The output of the light source 140 may also be appropriately selected depending on the size and thickness of the resist film 136, the photosensitivity of the photocurable resin contained in the resist film 136, the moving speed of the light source 140, and the like, and may be appropriately selected, for example, from a range of 1000 mW to 6000 mW, 2000 mW to 6000 mW, or 3000 mW to 5000 mW. The moving speed of the light source 140 may also be adjusted depending on the size of the resist film 136 and the output of the light source 140, and may be appropriately selected, for example, from a range of 0.1 cm / s to 20 cm / s, 1.0 cm / s to 10 cm / s, or 1.0 cm / s to 5.0 cm / s.
[0035] As a result, the outer periphery 136b of the resist film 136 is hardened, and the inner portion 136c surrounded by the outer periphery 136b maintains an unhardened or semi-hardened state by the primary exposure (FIG. 7(C)). By making the inner portion 136c unhardened or semi-hardened, the peeling layer 134 can be fixed more stably, so that the peeling layer 134 is prevented from being unintentionally peeled off in the subsequent process, and the accuracy of patterning performed on the peeling layer 134 can be ensured. Furthermore, as will be described in detail later, forming the outer periphery 136b improves the manufacturing yield of the deposition mask unit 100, and it is possible to provide the deposition mask unit 100 efficiently and at low cost.
[0036] Through the above steps, the peeling layer 134 is formed on the second support substrate 138 via the resist film 136. The upper surface of the peeling layer 134 in this state (the surface opposite to the second support substrate 138) is the surface that was in contact with the first support substrate 130 before peeling. Therefore, by using the first support substrate 130 with high flatness, a flat surface can be formed on the upper surface of the peeling layer 134.
[0037] 3-2. Formation of deposition mask Next, a resist mask 144 is formed on the peeling layer 134. The resist mask 144 is selectively formed in an island shape in a region where a plurality of openings 102a and a dummy pattern 106 described later are formed. Specifically, a negative or positive resist 142 is formed on the peeling layer 134 (FIG. 8(A)), and the resist mask 144 is formed by exposure and development through a photomask (FIG. 8(B)). The resist 142 may be a liquid or a resist film. Note that the resist mask 144 is preferably formed also on the outer edge of the peeling layer 134 so that the peeling layer 134 can be easily peeled off from the deposition mask unit 100 in a peeling process described later.
[0038] In developing the resist 142 after exposure, a developer is brought into contact with the resist 142, and then a cleaning liquid containing water is used to clean the first support substrate 130 and the resist mask 144. Immediately after cleaning, droplets of the cleaning liquid remain on the second support substrate 138, but these droplets are removed by blowing them away by supplying compressed nitrogen or air parallel or obliquely to the upper surface of the first support substrate 130 (see the arrow in FIG. 8(B)).
[0039] In this developing step, it is preferable to selectively remove only the uncured resist 142. However, the material contained in the resist 142 and the material contained in the resist film 136 are both photocurable resins, and their basic structures are the same or similar. Therefore, the uncured resist 142 is not necessarily more soluble in a developer than the resist film 136. For this reason, if the outer peripheral portion 136b (see FIG. 7(C)) cured by the above-mentioned edge exposure is not provided, the photocurable resin originating from the resist film 136 will dissolve in the developer. As a result, the cleaning liquid used during cleaning will also contain a small amount of photocurable resin.
[0040] Under such circumstances, when compressed nitrogen or air hits the side surface of the peeling layer 134 (arrow at the left end in FIG. 8(B)), turbulence occurs, and this turbulence may cause droplets of the cleaning liquid containing the photocurable resin to scatter and adhere to the resist mask 144. When the droplets adhere to the resist mask 144 and the solvent in the droplets subsequently evaporates, the photocurable resin precipitates on the resist mask 144. As a result, the shape of the resist mask 144 changes, and it becomes impossible to control the pattern of the openings 102a of the deposition mask 102 to be formed later according to the pattern of the photomask. This causes a decrease in the manufacturing yield of the deposition mask unit 100.
[0041] However, as described above, in one embodiment of the present invention, the resist film 136 is subjected to end exposure before the formation of the resist 142. Therefore, the outer peripheral portion 136b is constituted by the cured resist film 136 and is not dissolved in the developer. In addition, the uncured or semi-cured inner portion 136c is surrounded by the cured outer peripheral portion 136b and is not in contact with the developer. Therefore, the inner portion 136c of the resist film 136 is not dissolved by the developer, and the photocurable resin derived from the resist film 136 is not contained in the cleaning liquid. For this reason, even if droplets of the cleaning liquid adhere to the resist mask 144, the photocurable resin derived from the resist film 136 does not adhere to the resist mask 144. As a result, the resist mask 144 that is precisely patterned according to the pattern of the photomask can be formed, and the pattern of the openings 102a of the deposition mask 102 can be precisely controlled. This contributes to efficient manufacturing and high yield of the deposition mask unit 100.
[0042] Next, a metal film is grown by plating in the area not covered by the resist mask 144 to form the deposition mask 102 and the dummy pattern 106 (FIG. 9(A)). The plating pattern may be formed in one step or in several steps. When plating is performed in several steps, plating may be performed so that different metals are formed in different steps. Furthermore, plating may be performed so that the upper surface of the plating pattern is lower or higher than the upper surface of the resist mask 144. In the latter case, the upper surface of the plating pattern may be flattened by polishing the surface. Thereafter, the resist mask 144 is removed by etching with a stripping solution and / or ashing to form the deposition mask 102 having the multiple openings 102a and the dummy pattern 106 (FIG. 9(B)).
[0043] In the region Ra between the adjacent windows 110a, as shown in the schematic cross-sectional view of FIG. 10(A), a dummy pattern (hereinafter, a first dummy pattern) 106-1 is formed on the peeling layer 134 at the same time as the deposition mask 102 is formed. A groove (hereinafter, a first groove) 104-1 is formed between the first dummy pattern 106-1 and the deposition mask 102, and the first groove 104-1 separates the first dummy pattern 106-1 from the deposition mask 102. Therefore, as shown in the schematic top view of FIG. 10(B), one first dummy pattern 106-1 surrounds one deposition mask 102. Since the first dummy pattern 106-1 and the deposition mask 102 are formed at the same time, they can have the same composition and thickness.
[0044] The same is true for the region Rb at the end of the deposition mask unit 100. As shown in FIG. 11A, a dummy pattern (hereinafter, a second dummy pattern) 106-2 is formed on the peeling layer 134 at the same time as the deposition mask 102 is formed. A groove (hereinafter, a second groove) 104-2 is formed between the second dummy pattern 106-2 and the deposition mask 102, and the second groove 104-2 separates the second dummy pattern 106-2 from the deposition mask 102. As shown in the top schematic diagram of FIG. 11B, the second dummy pattern 106-2 surrounds the multiple deposition masks 102 and the multiple first dummy patterns 106-1 not shown in FIG. 11B. Since the second dummy pattern 106-2 and the deposition mask 102 are also formed at the same time, they can also have the same composition and thickness.
[0045] 3-3. Protection of openings As described below, the support frame 110 is placed on the deposition mask 102, and then the connection parts 120 are formed by plating, thereby fixing the deposition mask 102 and the support frame 110 to each other. Therefore, in order to prevent the openings 102a from being plated with metal when the connection parts 120 are formed, a plurality of resist masks 148 are used to protect the openings 102a.
[0046] 9(C), first, the resist film 146 is arranged so as to cover the multiple deposition masks 102. The resist film 146 is arranged so as to cover all of the openings 102a of the multiple deposition masks 102 and the dummy patterns 106 including the first dummy pattern 106-1 and the second dummy pattern 106-2. The resist film 146 is preferably formed to a thickness such that it is not covered by the connection portion 120 to be formed later. Therefore, the thickness of the resist film 146 may be selected from the range of 50 μm to 500 μm, 60 μm to 200 μm, or 100 μm to 200 μm.
[0047] Next, the resist film 146 is exposed using a photomask 150. The photomask 150 has a light-shielding portion 150a and a light-transmitting portion 150b. As shown in FIG. 12(A), the photomask 150 is configured and arranged so that, in the region Ra, the portion of the resist film 146 overlapping with the opening 102a of the deposition mask 102 and the portion overlapping with a part of the non-opening portion of the deposition mask 102 are exposed, and the portion overlapping with the first dummy pattern 106-1 and the portion overlapping with the other part of the non-opening portion of the deposition mask 102 are not exposed. That is, the light-transmitting portion 150b overlaps with the opening 102a of the deposition mask 102 and the part of the non-opening portion, and the light-shielding portion 150a overlaps with the first dummy pattern 106-1 and the other part of the non-opening portion.
[0048] On the other hand, in region Rb, as shown in FIG. 13(A), the photomask 150 is configured and arranged such that the light-transmitting portion 150b overlaps with the opening 102a of the deposition mask 102 and a portion of the non-opening portion, and the light-shielding portion 150a overlaps with the second dummy pattern 106-2 and another portion of the non-opening portion of the deposition mask 102.
[0049] The resist film 146 is a negative resist and contains a polymer or oligomer that is hardened by light. The solubility of the exposed portion in a developer is significantly reduced, and the exposed portion remains as a mask after development. On the other hand, the unexposed portion is removed by development. Therefore, in the region Ra, the multiple resist masks 148 generated by development cover the multiple openings 102a and a part of the non-opening portions, and the other part of the non-opening portions and the first dummy pattern 106-1 are exposed from the resist mask 148 (FIG. 12(B)). On the other hand, in the region Rb, the resist mask 148 covers the multiple openings 102a and a part of the non-opening portions, and the other part of the non-opening portions and the second dummy pattern 106-2 are exposed from the resist mask 148 (FIG. 13(B)). As will be described later, a connection portion 120 is formed in the non-opening portion exposed from the resist mask 148, thereby joining the deposition mask 102 and the support frame 110.
[0050] Through the steps up to this point, a plurality of resist masks 148 are formed, covering all of the openings 102a.
[0051] 3-4. Creating a support frame The support frame 110 is formed by etching a metal plate 112. Specifically, a resist 152 is formed on the metal plate 112 containing a metal or alloy including nickel, iron, cobalt, chromium, manganese, etc., and exposed through a photomask 156 (FIG. 14(A)), followed by development to form a resist mask 154 (FIG. 14(B)). The resist 152 may be a liquid resist or a film-like resist. The resist 152 may be either negative or positive. In the case of a negative type, as shown in FIG. 14(A), the photomask 156 may be configured and positioned so that the light-transmitting portion 156b overlaps the region where the support frame 110 is to be formed, and the light-shielding portion 156a overlaps the region to be removed by etching, i.e., the region where the window 110a is to be formed. Thereafter, the support frame 110 is obtained by removing the region other than the region covered by the resist mask 154 by development (FIG. 14(C)). The resist mask 154 is then removed with a stripper and / or by ashing.
[0052] 3-5. Arrangement of support frames and formation of joints Next, the support frame 110 is placed on the support substrate 138. Specifically, the deposition mask 102 is placed on the second support substrate 138 via the peeling layer 134 so as to overlap the first dummy pattern 106-1 and the second dummy pattern 106-2 (FIGS. 15(A) and 16(A)). That is, the support frame 110 is placed so that one window 110a overlaps the multiple openings 102a and one resist mask 148. At this time, an adhesive 158 may be provided on the support frame 110, and the support frame 110 may be bonded to the first dummy pattern 106-1 and the second dummy pattern 106-2 by the adhesive 158. The adhesive 158 may be, for example, an acrylic adhesive or an epoxy adhesive, or a resist film similar to the resist film 146. When a resist film is used, the thickness of the resist film may be smaller than that of the resist film 146. Specifically, the thickness of the resist film serving as adhesive 158 can be selected from the range of 1 μm to 20 μm, or 1 μm to 10 μm. When using a resist film as adhesive 158, the resist film does not need to be exposed to light in order to maintain its adhesive strength.
[0053] As an optional configuration, a protective film 159 may be formed on the upper surface of the support frame 110 (FIGS. 15(A) and 16(A)). A resist film similar to the resist film 146 may be used as the protective film 159. In this case, the resist film may or may not be exposed to light. By forming the protective film 159, when the connection parts 120 are subsequently formed by plating, the connection parts 120 are not formed on the upper surface of the support frame 110, and adjacent deposition masks 102 can be prevented from being directly connected by the connection parts 120.
[0054] Thereafter, the connection parts 120 are formed by plating. The connection parts 120 grow mainly from the supporting frame 110 and the non-opening parts of the deposition mask 102 that are exposed from the resist mask 148, and as a result, as shown in Fig. 15(B) and Fig. 16(B), the connection parts 120 are formed in contact with the upper surface of the non-opening part of the deposition mask 102 and the side surface 110b that constitutes the window 110a of the support frame 110. In this way, the deposition mask 102 and the support frame 110 are fixed together.
[0055] 16(B), a plating layer 121 is also formed on the left side of the support frame 110, i.e., on the outermost periphery, at the same time as the connection portion 120. Since the plating layer 121 is located outside the substrate 180 in the deposition process using the deposition mask unit 100, this does not pose a problem, but if necessary, a resist mask 148 may be used in the state shown in FIG. 16(A) to cover the outermost periphery so as to prevent the plating layer 121 from being formed.
[0056] At this time, the connection portion 120 is formed so as not to cover the upper surface of the resist mask 148. This is because if the connection portion 120 covers the upper surface of the resist mask 148, defects may occur when the resist mask 148 is subsequently removed with a stripping solution. Specifically, when the resist mask 148 swells with the stripping solution, the volume expands, which causes stress to be generated in the connection portion 120 on the resist mask 148, and as a result, the connection portion 120 may be damaged. By forming the connection portion 120 so as not to cover the upper surface of the resist mask 148, this defect can be effectively suppressed. By providing the resist film 146 to have a thickness in the above-mentioned range, it is possible to allow the deposition mask 102 to be fixed to the support frame 110 with sufficient bonding strength to the connection portion 120, and the connection portion 120 can be formed so as not to cover the upper surface of the resist mask 148.
[0057] 3-6. Removal of the support substrate and release layer Thereafter, the resist mask 148 is removed by etching using a peeling liquid (FIGS. 17(A) and 18(A)). At this time, the protective film 159 is also removed. Furthermore, the second support substrate 138 and the release layer 134 are sequentially peeled off. By removing the adhesive 158 simultaneously with or after the peeling of the release layer 134, the first dummy pattern 106-1 and the second dummy pattern 106-2 are removed together with the adhesive 158 (FIGS. 17(B) and 18(B)).
[0058] Through the above steps, the deposition mask unit 100 can be fabricated.
[0059] As described above, in this embodiment, during development for forming the resist mask 144 for determining the shapes of the opening 102a and the dummy pattern 106, the inner portion 136c of the resist film 136 for fixing the peeling layer 134 and the second support substrate 138 is prevented from contacting the developer by the outer peripheral portion 136b that is hardened by edge exposure. Therefore, in the cleaning step after development, droplets containing a photocurable resin originating from the resist film 136 are not scattered on the resist mask 144, and the precise patterning of the resist mask 144 is prevented from being destroyed. This effectively prevents the occurrence of defects in the manufacture of the deposition mask unit 100, and makes it possible to provide the deposition mask unit 100 efficiently and with a high yield.
[0060] The above-mentioned embodiments of the present invention may be combined as appropriate as long as they are not mutually inconsistent. In addition, a method in which a person skilled in the art appropriately adds or omits steps or modifies conditions based on the manufacturing method of each embodiment is also included in the scope of the present invention as long as it includes the gist of the present invention.
[0061] Even if there are other effects and advantages different from those brought about by the aspects of each of the above-mentioned embodiments, those which are clear from the description in this specification or which can be easily predicted by a person skilled in the art are naturally understood to be brought about by the present invention. [Explanation of symbols]
[0062] 100: deposition mask unit, 102: deposition mask, 102a: opening, 102b: opening group, 104-1: first groove, 104-2: second groove, 106: dummy pattern, 106-1: first dummy pattern, 106-2: second dummy pattern, 110: support frame, 110a: window, 110b: side, 112: metal plate, 120: connection portion, 121: plating layer, 130: first support substrate, 132: resist mask, 132a: side, 134: peeling layer, 136: resist film, 136a: side, 136b: outer periphery, 136c: inside, 138 : second support substrate, 140: light source, 142: resist, 144: resist mask, 146: resist film, 146a: exposed portion, 146b: unexposed portion, 148: resist mask, 150: photomask, 150a: light-shielding portion, 150b: light-transmitting portion, 152: resist, 154: resist mask, 156: photomask, 156a: light-shielding portion, 156b: light-transmitting portion, 158: adhesive, 159: protective film, 160: deposition chamber, 162: load lock door, 164: deposition source, 166: shutter, 168: moving mechanism, 170: holder, 180: substrate
Claims
1. disposing a resist film on a first supporting substrate; forming a release layer on the resist film; exposing the resist film from a side surface of the resist film toward the inside; forming at least one deposition mask having a plurality of openings on the release layer; placing a support frame having at least one window on the release layer such that the at least one window overlaps the plurality of openings of the at least one deposition mask; and forming a connection portion for fixing the at least one deposition mask and the support frame to each other by a plating method; the connection portion is formed so as to contact a side surface of the support frame on the window side and an upper surface of the deposition mask.
2. The exposure is performed using a light source, The method according to claim 1 , wherein the exposure is performed such that the direction of travel of light having the maximum intensity emitted from the light source passes through the side surface.
3. The method of claim 2 , wherein the light source is configured to emit ultraviolet light.
4. The method of claim 2 , wherein the exposure is performed while moving the light source along the periphery of the resist film.
5. the release layer is formed as a thin film including a metal layer on a second support substrate; The method further comprises: bonding the first support substrate and the second support substrate together such that the release layer and the resist film are in contact with each other; The method of claim 1 , comprising transferring the release layer onto the second support substrate by peeling the first support substrate.
6. The method further includes exposing the resist film from an upper surface of the resist film before bonding the first support substrate and the second support substrate together, The method of claim 5 , wherein the exposure of the resist film is performed such that the resist film remains flexible.
7. 10. The method of claim 1, further comprising removing the portion of the resist film exposed from the release layer prior to the exposing of the resist film.
8. 10. The method of claim 1, further comprising, prior to the positioning of the support frame, forming a second resist mask on the at least one deposition mask, the second resist mask covering the plurality of openings and spaced apart from the sides to expose portions of the at least one deposition mask.
9. The method according to claim 8 , wherein the connection portion is formed in a portion exposed from the second resist mask.
10. the at least one deposition mask includes a plurality of deposition masks, the at least one window comprises a plurality of windows; The method of claim 1 , wherein the support frame is positioned such that each of the plurality of windows overlaps a corresponding one of the plurality of openings in the deposition mask.
Citation Information
Patent Citations
Forming method of submicrom photo-resist pattern
JP1986222127A
Vapor deposition mask and manufacturing method of vapor deposition mask, organic el element, electronic equipment
JP2009087840A
Reflection type mask, exposure apparatus, exposure method, and device manufacturing method
JP2011077480A
Vapor-deposition mask, method of manufacturing the same, and method of manufacturing organic el display device
JP2013209710A
Mask and method for producing same
WO2020009088A1