Catheter shaft and manufacturing method thereof

Incorporating plate-shaped alumina particles into the catheter shaft's resin composition addresses the challenge of achieving both high pressure resistance and flexibility, enabling thinner, more robust catheters for minimally invasive treatments.

JP7561506B2Active Publication Date: 2024-10-04DIC CORP +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020045430
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-16
Publication Date
2024-10-04
Estimated Expiration
2040-03-16

AI Technical Summary

Technical Problem

Catheters used for minimally invasive treatments like PCI and EVT face challenges with calcified and curved lesions, requiring high pressure resistance and flexibility, while also needing to be thinner for less invasive procedures, presenting a contradiction in desired characteristics.

Method used

Incorporating plate-shaped alumina particles into the catheter shaft's molding material, specifically a thermoplastic resin, to enhance mechanical properties such as pressure resistance and tensile strength, allowing for a thinner yet robust design.

Benefits of technology

The resulting catheter shaft exhibits improved mechanical properties, enabling thinner profiles with higher pressure resistance and tensile strength, suitable for less invasive medical procedures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561506000002
    Figure 0007561506000002
  • Figure 0007561506000003
    Figure 0007561506000003
  • Figure 0007561506000004
    Figure 0007561506000004
Patent Text Reader

Abstract

To provide a catheter shaft excellent in mechanical properties, and a method for manufacturing the same.SOLUTION: A catheter shaft is composed of a tube-shaped molding containing a thermoplastic resin and plate-like alumina particles, in which the plate-like alumina particles have an aspect ratio represented by the following expression of 5-500. A method for manufacturing the catheter shaft includes extruding and molding a resin composition containing a thermoplastic resin and the plate-like alumina particles into a tube shape. Aspect ratio=average particle diameter L of plate-like alumina particle / average thickness D of plate-like alumina particle.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a catheter shaft and a method for manufacturing the same. [Background technology]

[0002] Percutaneous coronary intervention (PCI) is one of the medical treatments for ischemic heart disease such as angina pectoris and myocardial infarction. By expanding narrowed or blocked coronary arteries from the inside of the blood vessels using a medical balloon catheter with a balloon at the tip, ischemic heart disease can be treated without causing significant damage to the body.

[0003] 2, a medical balloon catheter has a catheter shaft 10 attached to one end of a hub 12, a balloon 11 at the tip of the catheter shaft 10, and a guidewire introduction port 14 in the middle. A pressurized fluid injection port 13 is attached to the other end of the hub 12. The balloon 11 is inserted into a stenosis in a cardiac blood vessel and expanded to form the stenosis.

[0004] In order to prevent the coronary arteries from narrowing again (restenosis) after PCI treatment, a small mesh-like metal tube called a stent may be placed inside the coronary artery by pushing it open from the inside. Since PCI is performed through a thin catheter inserted into the artery in the wrist or the groin, it is less invasive than coronary artery bypass surgery (surgical procedure) and places less of a burden on the patient's body. In addition, catheter therapy (hereinafter referred to as "EVT") for peripheral arterial disease in the entire body other than the coronary arteries is also performed.

[0005] Medical balloon catheters are disclosed in, for example, Patent Documents 1-3. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 11-244385 [Patent Document 2] JP 2004-065413 A [Patent Document 3] JP 2005-013495 A Summary of the Invention [Problem to be solved by the invention]

[0007] In recent years, catheters used in minimally invasive treatments such as PCI and EVT have been considered for use in more advanced lesions, such as calcified and tortuous lesions. Calcified lesions are harder than normal lesions, and require high pressure to be applied to expand them with a balloon catheter. For this reason, pressure resistance is required not only for the balloon that expands the lesion, but also for the catheter shaft that connects to the balloon.

[0008] In addition, there is a demand for the development of less invasive medical catheters, and to achieve this, catheter shafts need to be made thinner and thinner, which means that catheter shafts need to simultaneously have high strength and force transmission performance, as well as the opposing properties of high flexibility and thinness.

[0009] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a catheter shaft having excellent mechanical properties that can be applied to medical catheters for PCI, EVT, etc., and a method for manufacturing the same. [Means for solving the problem]

[0010] As a result of intensive research aimed at solving the above problems, the inventors discovered that by blending specific plate-like alumina particles into the molding material of the catheter shaft, the catheter shaft has excellent mechanical properties, and thus completed the present invention. That is, the present invention has the following aspects.

[0011] [1] A catheter shaft comprising a tubular molded body containing a thermoplastic resin and plate-like alumina particles, The catheter shaft has an aspect ratio of 5 to 500, the aspect ratio being represented by the following formula: Aspect ratio = average particle size L of plate-shaped alumina particles / average thickness D of plate-shaped alumina particles [2] The catheter shaft according to [1] above, wherein the content of the platelet alumina particles is 5 to 60 mass % relative to 100 mass % of the catheter shaft. [3] The catheter shaft according to [1] or [2] above, wherein the outer diameter of the catheter shaft is 0.25 to 3.3 mm. [4] The catheter shaft described in any one of [1] to [3] above, wherein the inner diameter of the catheter shaft is 0.2 to 3.0 mm. [5] The catheter shaft according to any one of [1] to [4] above, wherein the thickness of the catheter shaft, expressed as (outer diameter-inner diameter) / 2, is 0.01 to 2 mm. [6] The catheter shaft according to any one of [1] to [5], wherein the average thickness of the platelet alumina particles is 500 nm or less. [7] The catheter shaft according to any one of [1] to [6], wherein, when a scanning electron microscope photograph of a cross section of the central axis of the catheter shaft cut perpendicular to the cross section is taken, the average orientation angle between the contour line of the plate surface of the plate-like alumina particles and the contour line of the surface of the catheter shaft is 20° or less. [8] The catheter shaft according to any one of the above [1] to [7], wherein the thermoplastic resin is a polyamide resin or a polyamide elastomer. [9] A method for producing a catheter shaft according to any one of the above [1] to [8], comprising extruding a resin composition containing the thermoplastic resin and the plate-like alumina particles into a tubular shape. Effect of the Invention

[0012] According to the present invention, a catheter shaft having excellent mechanical properties and a method for producing the same can be provided. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic diagram of a catheter shaft. [Diagram 2] FIG. 1 is a schematic diagram of a medical balloon catheter. [Diagram 3] FIG. 2 is a schematic diagram of an SEM image of an orthogonal cross section of a catheter shaft. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] A catheter shaft and a method for manufacturing the same according to an embodiment of the present invention will be described below.

[0015] <Catheter shaft> The catheter shaft of this embodiment is made of a tubular molded body containing a thermoplastic resin and plate-like alumina particles.

[0016] FIG. 1 is a schematic diagram of a catheter shaft of the present embodiment.

[0017] The catheter shaft of this embodiment is not limited as long as it is a tubular molded body containing a thermoplastic resin and plate-like alumina particles, and includes a straw-shaped molded body and a hollow cylindrical molded body.

[0018] In order to realize minimal invasiveness when used as a medical catheter, the outer diameter d1 of the catheter shaft is preferably 3.3 mm or less, more preferably 2.7 mm or less, even more preferably 2.4 mm or less, and particularly preferably 1.8 mm or less. The catheter shaft of this embodiment has excellent mechanical properties such as pressure resistance and tensile strength, so that a thinner outer diameter d1 can be achieved. In order to ensure strength, the outer diameter d1 of the catheter shaft is preferably 0.25 mm or more, more preferably 0.35 mm or more, even more preferably 0.40 mm or more, and particularly preferably 0.45 mm or more. The outer diameter d1 of the catheter shaft is preferably 0.25 to 3.3 mm, more preferably 0.35 to 2.7 mm, even more preferably 0.40 to 2.4 mm, and particularly preferably 0.45 to 1.8 mm.

[0019] The inner diameter d2 of the catheter shaft is preferably 0.2 to 3.0 mm, more preferably 0.35 to 2.4 mm, further preferably 0.4 to 2.0 mm, and particularly preferably 0.8 to 1.5 mm.

[0020] The thickness of the catheter shaft, expressed by (outer diameter d1-inner diameter d2) / 2, is preferably 2 mm or less, more preferably 1.6 mm or less, and even more preferably 1.2 mm or less. The catheter shaft of this embodiment has excellent mechanical properties such as pressure resistance and tensile strength, and therefore can achieve a thinner thickness. The thickness of the catheter shaft, expressed by (outer diameter d1-inner diameter d2) / 2, is preferably 0.01 to 2 mm, more preferably 0.02 to 1.6 mm, and even more preferably 0.04 to 1.2 mm.

[0021] When a scanning electron microscope photograph of a cross section of the central axis of the catheter shaft of this embodiment cut perpendicular to the cross section is taken, the average orientation angle between the contour line of the plate surface of the plate-like alumina particle and the contour line of the surface of the catheter shaft is preferably 20° or less, more preferably 15° or less, and even more preferably 10° or less.

[0022] The catheter shaft of the embodiment has excellent mechanical properties because the plate-like alumina particles are oriented such that the average orientation angle between the plate surface of the plate-like alumina particles and the contour line of the surface of the catheter shaft is 20° or less. When the catheter shaft of the embodiment has an average orientation angle of more preferably 15° or less, and even more preferably 10° or less, it can exhibit excellent mechanical properties even when plate-like alumina particles with a relatively small aspect ratio are used, or can have even better mechanical properties even when plate-like alumina particles with a comparable aspect ratio are used.

[0023] The method for evaluating the average orientation angle is to use a scanning electron microscope (e.g., JCM-7000) to observe the state of a cross section of the target catheter shaft sample cut perpendicular to the central axis of the sample, confirm the orientation state of the plate-like alumina particles reflected in the SEM image, and, when the straight line of the contour of the surface of the catheter shaft is set to an angle of 0°, estimate the orientation angle (-90°<θ<90°) of each plate-like alumina particle relative to a line parallel to this straight line, and define the average of these absolute values ​​as the average orientation angle of the target catheter shaft.

[0024] In the catheter shaft of this embodiment, the plate-like alumina particles are preferably dispersed in the thermoplastic resin matrix, and more preferably, the primary particles of the plate-like alumina particles are dispersed in the thermoplastic resin matrix. The term "dispersed" as used herein refers to a state in which the plate-like alumina particles or the primary particles of the plate-like alumina particles are not in contact with each other.

[0025] The content of the plate-like alumina particles is preferably 5 to 60 mass %, more preferably 5 to 50 mass %, and particularly preferably 10 to 40 mass %, relative to 100 mass % of the catheter shaft. When the content of the plate-like alumina particles is equal to or greater than the lower limit, the catheter shaft has excellent mechanical properties. When the content of the plate-like alumina particles is equal to or less than the upper limit, the plate-like alumina particles can be prevented from contacting each other in the thermoplastic resin matrix, the flowability of the resin composition containing the thermoplastic resin and the plate-like alumina particles in a molten state can be favorably maintained, the plate-like alumina particles can be favorably dispersed in the catheter shaft, and the catheter shaft can be stably formed.

[0026] The content of the thermoplastic resin is preferably 40 to 95% by mass, more preferably 50 to 95% by mass, and particularly preferably 60 to 90% by mass, based on 100% by mass of the catheter shaft. When the content of the thermoplastic resin is equal to or more than the lower limit, it is preferable because excellent moldability can be imparted to the resin composition. On the other hand, when the content of the resin is equal to or less than the upper limit, it is preferable because the mechanical properties of the catheter shaft are excellent.

[0027] The catheter shaft of this embodiment has excellent mechanical properties such as pressure resistance and tensile strength, which will be described later, and can be applied to less invasive medical catheters such as those for PCI and EVT.

[0028] The catheter shaft of this embodiment can be used as a medical catheter 1, for example, as shown in Fig. 2. The medical catheter 1 has a catheter shaft 10 attached to one end of a hub 12, a balloon 11 at the tip of the catheter shaft 10, and a guidewire introduction port 14 in the middle. A pressurized fluid injection port 13 is attached to the other end of the hub 12. The balloon 11 is inserted into a stenosis in a cardiac blood vessel and expanded to form the stenosis.

[0029] The catheter shaft of the medical catheter can be formed as a single layer or a multi-layer. The catheter shaft of the present embodiment can be used as an outer shaft of the medical catheter or as an inner shaft of the medical catheter.

[0030] The method for producing the catheter shaft will be described in detail later. The thermoplastic resin and the plate-like alumina particles will be described below.

[0031] [Thermoplastic resin] As the thermoplastic resin, a thermoplastic resin used as a molding material for medical catheter shafts can be used. It is believed that by blending the plate-like alumina particles with a thermoplastic resin as a molding material for the catheter shaft, the material strength of the catheter shaft can be increased. As such a thermoplastic resin, specifically, polyamide resins such as nylon 11 (polyamide 11) and nylon 12 (polyamide 12), or polyamide elastomers such as polyether block amide can be suitably used.

[0032] [Plate-shaped alumina particles] The plate-like alumina particles can be produced by known and commonly used production methods such as a hydrothermal method and a flux method. Among them, the preferred production method is a method for producing alumina particles in which an aluminum compound is calcined in the presence of a shape control agent consisting of a molybdenum compound and silicon or a compound containing a silicon atom. The plate-like alumina particles obtained by the preferred manufacturing method according to the present invention contain molybdenum within the particles and have a polygonal plate shape. Furthermore, as long as the effects of the present invention are not impaired, impurities from the raw materials or shape control agents may be contained. The plate-like alumina particles may further contain organic compounds, etc.

[0033] In the present invention, "plate-like" refers to an aspect ratio, calculated by dividing the average particle diameter by the thickness, of 2 or more. In this specification, the "thickness of the plate-like alumina particles" is a value measured using a scanning electron microscope (SEM). The "average particle diameter of the plate-like alumina particles" is the volume-based median diameter D from the volume-based cumulative particle size distribution measured using a laser diffraction / scattering particle size distribution measuring device. 50 The value calculated as follows.

[0034] The plate-like alumina particles preferably have an average thickness of 0.01 to 0.5 μm, an average particle diameter of 0.1 to 500 μm, and an aspect ratio, which is the ratio of the average particle diameter to the average thickness, of 5 to 500. When the aspect ratio of the plate-like alumina particles is 5 or more, it is preferable because the particles can have two-dimensional orientation characteristics, and when the aspect ratio of the plate-like alumina particles is 500 or less, it is because the particles have excellent mechanical strength. More preferably, the average thickness is 0.03 to 3 μm, the average particle diameter is 1 to 50 μm, and the aspect ratio, which is the ratio of the average particle diameter to the average thickness, is 15 to 100.

[0035] The average thickness, average particle size, aspect ratio, etc. of the plate-like alumina particles of the present invention can be controlled by selecting the proportions of the molybdenum compound, the aluminum compound, and the shape-controlling agent used, the type of the shape-controlling agent, and the state in which the shape-controlling agent and the aluminum compound are present.

[0036] <Catheter shaft manufacturing method> In the method for producing a catheter shaft of this embodiment, a resin composition containing the thermoplastic resin and the plate-like alumina particles is extruded into a tubular shape. There are no particular limitations on the method, so long as it is a method of extruding a resin composition containing a thermoplastic resin and plate-like alumina particles having an aspect ratio of 5 to 500 into a tubular shape, and any molding method such as a known extrusion molding method or extrusion tube molding method can be used.

[0037] As the plate-like alumina particles, those mentioned above are used, and the preferred properties of the plate-like alumina particles, such as the average thickness and aspect ratio, are the same as those mentioned above, so a description thereof will be omitted here.

[0038] The catheter shaft of the present embodiment is formed by molding a resin composition containing a thermoplastic resin and predetermined plate-like alumina particles into a tubular shape, and the plate-like alumina particles can be oriented so that the average orientation angle between the contour line of the plate surface of the plate-like alumina particles and the contour line of the surface of the catheter shaft is 20° or less.

[0039] The content of the plate-like alumina particles is preferably 5 to 60 mass%, more preferably 5 to 50 mass%, and even more preferably 10 to 40 mass%, based on 100 mass% of the resin composition. When the content of the plate-like alumina particles is equal to or more than the lower limit, it is preferable because a catheter shaft having excellent mechanical properties can be obtained. On the other hand, when the content of the plate-like alumina particles is equal to or less than the upper limit, it is preferable because a resin composition having excellent moldability can be obtained.

[0040] Examples of the thermoplastic resin include the above-mentioned known and commonly used thermoplastic resins, of which polyamide resins such as nylon 11 and nylon 12, and polyamide elastomers such as polyether block amide are more preferred.

[0041] The content of the thermoplastic resin is preferably 40 to 95% by mass, more preferably 50 to 95% by mass, and particularly preferably 60 to 90% by mass, based on 100% by mass of the resin composition. When the content of the resin is equal to or more than the lower limit, it is preferable because excellent moldability can be imparted to the resin composition. On the other hand, when the content of the resin is equal to or less than the upper limit, it is preferable because the mechanical properties of the catheter shaft are excellent.

[0042] The resin composition can be obtained by mixing the plate-like alumina particles, the thermoplastic resin, and, if necessary, other ingredients. There is no particular limitation on the mixing method, and the mixture can be mixed by a known, commonly used method.

[0043] Examples of a method for mixing the thermoplastic resin with the plate-like alumina particles include a method in which the thermoplastic resin, the plate-like alumina particles, and other components as necessary are mixed in advance using various mixers such as a tumbler or a Henschel mixer, and then melt-kneaded using a mixer such as a Banbury mixer, a roll, a Brabender, a single-screw kneading extruder, a twin-screw kneading extruder, a kneader, a mixing roll, etc. The temperature for melt-kneading is not particularly limited, but is usually in the range of 100 to 350°C, and preferably in the range of 200 to 300°C.

[0044] The resin composition is preferably obtained by simply dry-blending raw materials containing the plate-like alumina particles and the thermoplastic resin, and then melt-kneading the mixture to obtain a pellet-shaped resin composition. Next, the pellet-like resin composition is press-molded while still in a fluid state into a desired tubular shape, and then cooled to room temperature in air or water to produce a continuous tubular molded product.

[0045] The molding temperature is not limited as long as the thermoplastic resin melts but does not decompose, but it is preferable to select an appropriate temperature with reference to the melt-kneading temperature. Specifically, molding can be performed by pressing the pellet-shaped resin composition into a die (metal mold, die) at a temperature equal to or higher than the temperature used in the melt-kneading. That is, a melt of the pellet-shaped resin composition is pressed into a die provided with an annular (double cylindrical) slit roughly corresponding to the tube outer diameter d1 and the tube inner diameter d2, and extruded out of the slit, thereby making it possible to pressure-mold a continuous tube-shaped molded body. The continuous tubular molded article thus obtained can be cut in the longitudinal direction of the cylinder to a desired length to produce a catheter shaft of a predetermined length.

[0046] A coupling agent may be added externally to the resin composition, since this can further increase the fluidity of the resin composition and the filling ability of the plate-like alumina particles and the like. By adding a coupling agent externally, the adhesion between the resin composition and the plate-like alumina particles can be further increased, and the adhesion between the resin composition and the plate-like alumina particles can be improved, which can improve the mechanical properties of the catheter shaft. Furthermore, the coupling agent may be added to the resin composition after it has been localized by a so-called surface treatment, such as by being attached to the surface of the plate-like alumina particles or by being coated by a reaction. As a method for providing the surface of the plate-like alumina particles, dip coating or chemical vapor deposition (CVD) can be adopted. Among them, the thermal CVD method is preferable because it does not require vacuum equipment, is relatively simple, and provides more effective performance improvement.

[0047] Examples of the coupling agent include alkyltrimethoxysilanes or alkyltrichlorosilanes having an alkyl group having 1 to 22 carbon atoms, such as methyltrimethoxysilane, dimethyldimethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, isopropyltrimethoxysilane, isopropyltriethoxysilane, pentyltrimethoxysilane, hexyltrimethoxysilane, and octenyltrimethoxysilane; 3,3,3-trifluoropropyltrimethoxysilane, tridecafluoro-1,1,2,2-tetrahydrooctyl)trichlorosilanes; phenyltrimethoxysilane, phenyltriethoxysilane, p-chloromethylphenyltrimethoxysilane, and p-chloromethylphenyltriethoxysilanes; γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, and γ-glycidoxypropyltrimethoxysilane. Examples of organic silane compounds include epoxy silanes such as ethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and glycidoxyoctyltrimethoxysilane, amino silanes such as γ-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, γ-aminopropyltrimethoxysilane, and γ-ureidopropyltriethoxysilane, mercapto silanes such as 3-mercaptopropyltrimethoxysilane, p-styryltrimethoxysilane, vinyltrichlorosilane, vinyltris(β-methoxyethoxy)silane, vinyltrimethoxysilane, vinyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, and vinyl silanes of high molecular type such as epoxy, amino, and vinyl. The organic silane compounds may be contained alone or in combination of two or more.

[0048] The above-mentioned coupling agents may be used alone or in combination of two or more kinds.

[0049] The amount of the coupling agent added is not particularly limited, but is preferably 0.01 to 5% by mass, and more preferably 0.1 to 3% by mass, relative to 100% by mass of the resin composition.

[0050] The resin composition may contain additives such as a colorant (pigment, dye) and a softener (plasticizer) in addition to the coupling agent. EXAMPLES

[0051] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In addition, "%" represents "% by mass" unless otherwise specified.

[0052] <Synthesis of plate-shaped alumina particles> [Synthesis Example 1] 50 g of aluminum hydroxide (manufactured by Nippon Light Metals Co., Ltd., average particle size 12 μm), 0.65 g of silicon dioxide (Kanto Chemical Co., Ltd.), and 1.72 g of molybdenum trioxide (manufactured by Taiyo Koko Co., Ltd.) were mixed in a mortar to obtain a mixture. The obtained mixture was placed in a crucible, heated to 1100°C at 5°C / min in a ceramic electric furnace, and held at 1200°C for 10 hours for firing. After that, the temperature was lowered to room temperature at 5°C / min, and the crucible was removed to obtain 34.2 g of light blue powder. The obtained powder was crushed in a mortar until it passed through a 106 μm sieve.

[0053] Next, the obtained powder was dispersed in 150 mL of 0.5% ammonia water, and the dispersion solution was stirred at room temperature (25 to 30°C) for 0.5 hours. After that, the ammonia water was removed by filtration, and the molybdenum remaining on the particle surface was removed by washing with water and drying, yielding 33.5 g of a light blue powder. SEM observation of the obtained powder confirmed that it had a polygonal plate shape, had very few aggregates, and was a plate-shaped particle with excellent handleability. Furthermore, X-ray diffraction (XRD) measurement revealed sharp peak scattering due to α-alumina, and no alumina crystal peaks other than the α crystal structure were observed, confirming that it was a plate-shaped alumina with a dense crystal structure. Furthermore, the results of fluorescent X-ray quantitative analysis confirmed that the obtained particles contained 0.8% molybdenum in molybdenum trioxide equivalent and 1.9% silicon in silicon dioxide equivalent by mass.

[0054] [Synthesis Example 2] 142.3 g of aluminum hydroxide (manufactured by Nippon Light Metals Co., Ltd., average particle size 2 μm), 2.8 g of silicon dioxide (manufactured by Kanto Chemical Co., Ltd., special grade), and 4.7 g of molybdenum trioxide (manufactured by Taiyo Koko Co., Ltd.) were mixed in a mortar to obtain a mixture. The obtained mixture was placed in a crucible, heated to 1200°C at 5°C / min in a ceramic electric furnace, and held at 1200°C for 10 hours for firing. After that, the temperature was lowered to room temperature at 5°C / min, and the crucible was removed to obtain 95 g of light blue powder. The obtained powder was crushed in a mortar until it passed through a 106 μm sieve.

[0055] Next, 50 g of the obtained light blue powder was dispersed in 150 mL of 0.5% ammonia water, and the dispersion solution was stirred at room temperature (25 to 30°C) for 0.5 hours, after which the ammonia water was removed by filtration, and the molybdenum remaining on the particle surface was removed by washing with water and drying, to obtain 47 g of light blue powder. The obtained powder was confirmed to have a polygonal plate shape by SEM observation, with very few aggregates, and to be a plate-shaped particle with excellent handleability. Furthermore, when X-ray diffraction (XRD) measurement was performed, a sharp peak scattering due to α-alumina appeared, and no alumina crystal peak other than the α crystal structure was observed, confirming that the particles were plate-shaped alumina particles with a dense crystal structure. In addition, the α conversion rate was 99% or more (almost 100%). Furthermore, from the results of fluorescent X-ray quantitative analysis, it was confirmed that the obtained particles contained 0.3 mass% molybdenum in terms of molybdenum trioxide and 2.2 mass% silicon in terms of silicon dioxide.

[0056] <Spherical alumina particles> For comparison, spherical alumina particles (DAW-07) manufactured by Denka Co., Ltd. were used.

[0057] (Measurement of average particle size L) The above plate-like alumina particle and spherical alumina particle samples were measured using a laser diffraction particle size distribution analyzer HELOS (H3355) & RODOS (manufactured by Japan Laser Co., Ltd.) under conditions of a dispersion pressure of 3 bar and a suction pressure of 90 mbar. 50 (μm) was obtained and calculated as the average particle size L. The evaluation results are shown in Table 1.

[0058] (Measurement of average thickness D) For the above sample, a scanning electron microscope (SEM) was used to measure the thickness of 50 pieces, and the average value was adopted as the average thickness D (μm). The evaluation results are shown in Table 1.

[0059] The aspect ratio L / D of the above sample was calculated using the following formula. The evaluation results are shown in Table 1.

[0060] (Aspect ratio L / D) Aspect ratio = average particle size L of plate-shaped alumina particles / average thickness D of plate-shaped alumina particles

[0061] The alpha conversion rate and Mo content of the plate-like alumina particles obtained in Synthesis Example 1 and Synthesis Example 2 were analyzed by the following methods.

[0062] (Analysis of Alpha Conversion Rate) The prepared sample was placed on a measurement sample holder with a depth of 0.5 mm, and packed flat with a constant load. It was then set in a wide-angle X-ray diffractometer (Rigaku Corporation, Rint-Ultma) and measured under the conditions of Cu / Kα radiation, 40 kV / 30 mA, scan speed 2 degrees / min, and scan range 10 to 70 degrees. The α conversion rate was calculated from the ratio of the strongest peak heights of α-alumina and transition alumina.

[0063] (Analysis of molybdenum and silicon content in plate-shaped alumina particles) Using a Primus IV X-ray fluorescence analyzer (Rigaku Corporation), approximately 70 mg of the prepared sample was placed on filter paper, covered with PP film, and subjected to composition analysis. The molybdenum amount determined from the results of X-ray fluorescence (XRF) analysis was calculated as molybdenum trioxide (mass %) relative to 100% by mass of the plate-like alumina particles.The silicon amount determined from the results of X-ray fluorescence (XRF) analysis was calculated as silicon dioxide (mass %) relative to 100% by mass of the plate-like alumina particles.

[0064] <Making the catheter shaft> [Example 1] The plate-like alumina particles of Synthesis Example 1 (24 parts by mass) and polyamide 11 (RILSAN (registered trademark) BESVO A MED) (76 parts by mass) manufactured by Arkema Inc. were melted, kneaded, and extruded using a twin-screw kneading extruder, and the extruded strands were cooled and cut to obtain a pellet-shaped resin composition.

[0065] The obtained pellet-like resin composition was heated and melted at 220 to 240°C in a twin-screw extruder (2D25S manufactured by Toyo Seiki Seisakusho) and extrusion molded to obtain a tubular molded product as the catheter shaft of Example 1. The catheter shaft of Example 1 had an outer diameter of 1.32 mm, an inner diameter of 1.14 mm, and a thickness of 0.09 mm.

[0066] [Example 2] The plate-like alumina particles of Synthesis Example 2 (11 parts by mass) and polyamide 11 (RILSAN (registered trademark) BESVO A MED) (89 parts by mass) manufactured by Arkema Inc. were melted, kneaded, and extruded using a twin-screw kneading extruder, and the extruded strands were cooled and cut to obtain a pellet-shaped resin composition.

[0067] The obtained pellet-like resin composition was heated and melted at 220 to 240°C in a twin-screw extruder (2D25S manufactured by Toyo Seiki Seisakusho) and extrusion molded to obtain a tubular molded product as the catheter shaft of Example 2. The catheter shaft of Example 2 had an outer diameter of 1.32 mm, an inner diameter of 1.14 mm, and a thickness of 0.09 mm.

[0068] [Example 3] The plate-like alumina particles of Synthesis Example 2 (24 parts by mass) and polyamide 11 (RILSAN (registered trademark) BESVO A MED) (76 parts by mass) manufactured by Arkema Inc. were melted, kneaded, and extruded using a twin-screw kneading extruder, and the extruded strands were cooled and cut to obtain a pellet-shaped resin composition.

[0069] The obtained pellet-like resin composition was heated and melted at 220 to 240°C in a twin-screw extruder (2D25S manufactured by Toyo Seiki Seisakusho) and extrusion molded to obtain a tubular molded product as the catheter shaft of Example 3. The catheter shaft of Example 3 had an outer diameter of 1.32 mm, an inner diameter of 1.14 mm, and a thickness of 0.09 mm.

[0070] [Example 4] The plate-like alumina particles of Synthesis Example 2 (37 parts by mass) and polyamide 11 (RILSAN (registered trademark) BESVO A MED) (63 parts by mass) manufactured by Arkema Inc. were melted, kneaded, and extruded using a twin-screw kneading extruder, and the extruded strands were cooled and cut to obtain a pellet-shaped resin composition.

[0071] The obtained pellet-like resin composition was heated and melted at 220 to 240°C in a twin-screw extruder (2D25S manufactured by Toyo Seiki Seisakusho) and extrusion molded to obtain a tubular molded product as the catheter shaft of Example 4. The catheter shaft of Example 4 had an outer diameter of 1.32 mm, an inner diameter of 1.14 mm, and a thickness of 0.09 mm.

[0072] [Comparative Example 1] A pellet-shaped resin composition of polyamide 11 (RILSAN (registered trademark) BESVO A MED) manufactured by Arkema Inc. was heated and melted at 220 to 240°C in a twin-screw extruder (2D25S manufactured by Toyo Seiki Seisakusho) and extrusion molded to obtain a tubular molded product as the catheter shaft of Comparative Example 1. The catheter shaft of Comparative Example 1 had an outer diameter of 1.32 mm, an inner diameter of 1.14 mm, and a thickness of 0.09 mm.

[0073] [Comparative Example 2] Spherical alumina particles (DAW-07) (24 parts by mass) manufactured by Denka Company Ltd. and polyamide 11 (RILSAN (registered trademark) BESVO A MED) (76 parts by mass) manufactured by Arkema K.K. were melted, kneaded, and extruded using a twin-screw kneading extruder, and the extruded strands were cooled and cut to obtain a pellet-shaped resin composition.

[0074] The obtained pellet-like resin composition was heated and melted at 220 to 240°C in a twin-screw extruder (2D25S manufactured by Toyo Seiki Seisakusho) and extrusion molded to obtain a tubular molded product as the catheter shaft of Comparative Example 2. The catheter shaft of Comparative Example 2 had an outer diameter of 1.32 mm, an inner diameter of 1.14 mm, and a thickness of 0.09 mm.

[0075] <Measurement of average orientation angle> The average orientation angle of the plate-like alumina particles in the catheter shafts of Examples 1 to 4 was measured according to the following procedure. (1) The catheter shaft was cut to a length of approximately 5 mm. (2) Furthermore, a sample having an approximately rectangular shape was extracted by cutting perpendicularly to the cross-section, and embedded in epoxy resin. The sample was then polished using a Buehler Automet 250pro polishing machine to make the cross section of the central axis of the catheter shaft visible. (3) Using a JEOL JCM-7000 scanning electron microscope (SEM), the cross-sections of the central axes of the samples were observed, and the orientation of the plate-like alumina particles reflected in the SEM images with a field of view of 250 μm × 190 μm was confirmed.

[0076] (4) The straight line of the contour of the outer surface of the catheter shaft was set at an angle of 0°, and the orientation angle (-90°<θ<90°) between the contour line of the plate surface of each plate-like alumina particle and a line parallel to that straight line was estimated. The average of the absolute values ​​of these orientation angles was then calculated to calculate the average orientation angle of the plate-like alumina particles in the catheter shaft.

[0077] More specifically, the angle of the sample was adjusted so that the straight line of the contour of the outer surface of the catheter shaft sample was placed in the field of view and the straight line of the contour of the surface was parallel to the long side of the screen in the field of view.The field of view was then moved to the inside of the cross section of the sample, and an image was taken with the field of view after the movement. FIG. 3 is a schematic diagram of an SEM image of a cross section of the central axis of a catheter shaft. As shown in the schematic diagram of FIG. 3, each plate-like alumina particle was observed to have a roughly needle-like shape on the cross section of the catheter shaft. The coordinates of the two longitudinal ends of the plate-like alumina particles that appeared needle-like in the photograph were measured, and the angle between the direction of the straight line of the surface outline, i.e., the long side direction of the photograph, was calculated from these values. Then, photographs were taken in any field of view, and measurements were made for at least 100 plate-like alumina particles, and the average absolute value of their orientation angles was calculated. The results are shown in Table 1.

[0078] <Pressure Test> The catheter shafts of Examples 1 to 4 and Comparative Examples 1 and 2 were subjected to pressure resistance tests according to the following procedure. (1) The catheter shaft was cut to a length of 50 mm. (2) One end of the cut catheter shaft was clamped to securely seal it, and the other end was connected to a connector for adding pressurized fluid, thereby connecting it to the pressurized fluid source of a pressure tester Hydraulic Pressure Tester Model HPT-1000 (Confluent Medical Technologies). (3) The catheter shaft connected to the pressurized fluid source was immersed in a thermostatic water bath Model WB10 (PolyScience) containing warm water at 37°C. (4) Using a pressure tester, the pressure of the fluid was increased from 0 atm by 1 atm every 5 seconds, and the pressure at the time of bursting was measured as the pressure resistance value (atm). 1 atm = 101.325 Pa. The results are shown in Table 1.

[0079] <Tensile test> The catheter shafts of Examples 1 to 4 and Comparative Examples 1 and 2 were subjected to tensile tests according to the following procedure. (1) The catheter shaft was cut to a length of 45 mm. (2) Immerse in a 37°C thermostatic water bath for 2 hours. (3) The catheter shaft was removed from the thermostatic water bath and placed in a tabletop material testing machine STA-1225 (manufactured by A&D Co., Ltd.) with the chuck distance set to 25 mm. (4) The tensile tests were performed at a tensile speed of 100 mm / min, and data was continuously acquired from the benchtop material testing machine, and the load at break was measured as the tensile breaking load (N). Note that the load at break was the maximum load in the tensile tests of all catheter shafts. The results are shown in Table 1.

[0080] [Table 1]

[0081] As shown in Table 1, the catheter shafts of Examples 1 to 4 containing plate-like alumina particles had higher pressure resistance and were more excellent in pressure resistance than the catheter shafts of Comparative Examples 1 and 2. By adding plate-like alumina particles to the molding material of the catheter shaft, the mechanical strength of the catheter shaft was improved. The catheter shafts of Examples 1 to 4 have better pressure resistance than the catheter shaft of Comparative Example 1 made of a material currently available on the market, so that it is possible to apply thinner catheter shafts. In addition, the catheter shaft of Comparative Example 2 containing spherical alumina particles had a smaller tensile breaking load than the catheter shaft of Comparative Example 1, whereas the catheter shafts of Examples 1 to 4 containing plate-like alumina particles maintained the same tensile breaking load value as the catheter shaft of Comparative Example 1.

[0082] The catheter shaft of the present invention has excellent mechanical properties such as pressure resistance and tensile strength, and can therefore be applied to less invasive medical catheters such as those for PCI and EVT. [Explanation of symbols]

[0083] 1 Medical catheter, 10 Catheter shaft, 11 Balloon, 12 Branch hub, 13 Pressurized fluid injection port, 14 Guide wire introduction port.

Claims

1. A catheter shaft made of a tubular molded body containing a thermoplastic resin and plate-like alumina particles, The plate-like alumina particles have an aspect ratio represented by the following formula of 5 to 500, A catheter shaft in which, when a scanning electron microscope photograph of a cross section of the central axis of the catheter shaft cut in a direction perpendicular to the cross section is taken, the average orientation angle between the outline of the plate surface of the plate-like alumina particles and the outline of the surface of the catheter shaft is 20° or less. Aspect ratio = average particle size L of plate-like alumina particles / average thickness D of plate-like alumina particles

2. 2. The catheter shaft according to claim 1, wherein the content of the platelet alumina particles is 5 to 60 mass % relative to 100 mass % of the catheter shaft.

3. The catheter shaft according to claim 1 or 2, wherein the outer diameter of the catheter shaft is 0.25 to 3.3 mm.

4. The catheter shaft according to any one of claims 1 to 3, wherein the inner diameter of the catheter shaft is 0.2 to 3.0 mm.

5. The catheter shaft according to any one of claims 1 to 4, wherein the thickness of the catheter shaft, expressed as (outer diameter - inner diameter) / 2, is 0.01 to 2 mm.

6. The catheter shaft according to any one of claims 1 to 5, wherein the average thickness of the plate-like alumina particles is 500 nm or less.

7. The catheter shaft according to any one of claims 1 to 6, wherein the thermoplastic resin is a polyamide resin or a polyamide elastomer.

8. The method for producing a catheter shaft according to any one of claims 1 to 7, wherein a resin composition containing the thermoplastic resin and the plate-like alumina particles is extruded into a tubular shape.

Citation Information

Patent Citations

  • Medical baloon catheter shaft and its manufacturing method

    JP1999244385A

  • Medical catheter containing inorganic crystal

    JP2001293082A

  • Balloon catheter

    JP2004065413A

  • Medical care tube

    JP2004141296A

  • Medical tube

    JP2005013495A