Interlayer film for laminated glass and laminated glass

A multi-layer interlayer film with specific thermoplastic resins and heat-shielding particles in laminated glass stabilizes sound insulation across temperature fluctuations, enhancing performance in low temperature ranges.

JP7561623B2Active Publication Date: 2024-10-04SEKISUI CHEMICAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020544308
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-16
Filing Date
2020-07-14
Publication Date
2024-10-04
Estimated Expiration
2040-07-14

AI Technical Summary

Technical Problem

Conventional laminated glass exhibits deteriorating sound insulation properties at relatively low temperatures due to changes in the plasticizer distribution and Young's modulus of the resin layers with temperature fluctuations.

Method used

An interlayer film for laminated glass with a multi-layer structure, comprising specific thermoplastic resins and heat-shielding particles, is designed to maintain consistent sound insulation properties across varying temperatures by controlling the glass transition temperatures and resin layer interactions.

Benefits of technology

The interlayer film enhances sound insulation in laminated glass, particularly in low temperature ranges, by stabilizing resin layer properties and absorbing sunlight for temperature regulation, thereby improving sound insulation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561623000008
    Figure 0007561623000008
  • Figure 0007561623000009
    Figure 0007561623000009
  • Figure 0007561623000010
    Figure 0007561623000010
Patent Text Reader

Abstract

Provided is an interlayer film for a laminated glass, whereby sound insulating properties of a laminated glass can be increased in a relatively low-temperature region. An interlayer film for a laminated glass pertaining to the present invention has a one-layer structure or a structure having two or more layers, and, when a laminated glass X having a longitudinal size of 25 mm and a transverse size of 300 mm is obtained by sandwiching the interlayer film between two sheets of green glass having a thickness of 2 mm, the absolute value of the difference between the secondary resonance frequency of the laminated glass X before irradiation thereof by xenon light and the secondary resonance frequency of the laminated glass X after irradiation thereof by xenon light is 60 Hz or greater, and the solar radiation transmittance of the laminated glass X is 50% or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an interlayer film for laminated glass used to obtain laminated glass. The present invention also relates to laminated glass using the interlayer film for laminated glass. [Background technology]

[0002] Even if laminated glass is broken by an external impact, the amount of glass fragments scattered is small, and therefore, laminated glass is excellent in safety. For this reason, the laminated glass is widely used in automobiles, railroad cars, aircraft, ships, buildings, etc. The laminated glass is manufactured by sandwiching an interlayer film for laminated glass between two glass sheets.

[0003] As an example of the interlayer film for laminated glass, the following Patent Document 1 discloses an interlayer film for laminated glass having a single-layer structure or a laminated structure of two or more layers. This interlayer film is a single-layer interlayer film having a single-layer structure including a first layer containing a thermoplastic resin, tungsten oxide particles, and an ultraviolet blocking agent, or a multi-layer interlayer film for laminated glass having a laminated structure of two or more layers including a first layer containing a thermoplastic resin and tungsten oxide particles and a second layer containing an ultraviolet blocking agent.

[0004] Patent Document 2 listed below discloses an interlayer film for laminated glass, which comprises a first layer containing a thermoplastic resin and at least one of an immonium compound and an aminium compound, and a second layer containing a polyvinyl acetal resin and a plasticizer, wherein the thermoplastic resin contained in the first layer is a thermoplastic resin having a hydroxyl group content of 25 mol % or less. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] WO2012 / 115198A1 [Patent Document 2] JP 2011-042552 A Summary of the Invention [Problem to be solved by the invention]

[0006] The laminated glass described in Patent Documents 1 and 2 can improve heat insulation. However, in conventional laminated glass having heat insulation performance as described in Patent Documents 1 and 2, the sound insulation of the laminated glass may change with changes in the surrounding temperature. For example, in conventional laminated glass, the sound insulation of the laminated glass may decrease in a relatively low temperature range (e.g., -10°C to 10°C).

[0007] An object of the present invention is to provide an interlayer film for laminated glass that can improve the sound insulation of laminated glass in a relatively low temperature range. Another object of the present invention is to provide laminated glass using the interlayer film for laminated glass. [Means for solving the problem]

[0008] According to a broad aspect of the present invention, there is provided an interlayer film for laminated glass having a one-layer structure or a two or more layer structure, in which, when the interlayer film is sandwiched between two sheets of green glass with a thickness of 2 mm to obtain laminated glass X having a size of 25 mm in length and 300 mm in width, the absolute value of the difference between the secondary resonance frequency of the laminated glass X before irradiation with xenon light and the secondary resonance frequency of the laminated glass X after irradiation with xenon light, as determined by the xenon light irradiation test described below, is 60 Hz or more, the loss factor of the laminated glass X at 20°C is 0.25 or more, and the solar transmittance of the laminated glass X is 50% or less (in this specification, "interlayer film for laminated glass" may be abbreviated to "interlayer film").

[0009] Xenon light irradiation test: The secondary resonance frequency of the laminated glass X at 10°C is determined by the central excitation method according to ISO16940. Under the condition of 10°C, the laminated glass X is exposed to 190 W / m 2The laminated glass X is irradiated with xenon light for 30 minutes. The secondary resonance frequency of the laminated glass X after irradiation with xenon light is obtained by a central excitation method in accordance with ISO 16940. The absolute value of the difference between the secondary resonance frequency of the laminated glass X before irradiation with xenon light and the secondary resonance frequency of the laminated glass X after irradiation with xenon light is calculated.

[0010] In a specific aspect of the interlayer film according to the present invention, the absolute value of the difference between the secondary resonance frequency of the laminated glass X before irradiation with xenon light and the secondary resonance frequency of the laminated glass X after irradiation with xenon light, as determined by the xenon light irradiation test, is 200 Hz or less.

[0011] In a specific aspect of the interlayer film according to the present invention, when the laminated glass X is stored at 10°C for 56 days or more, the secondary resonance frequency of the laminated glass X at 10°C after storage, as determined by a central vibration method in accordance with ISO16940, is 900 Hz or more.

[0012] In a specific aspect of the interlayer film according to the present invention, the interlayer film has a structure of three or more layers, and includes a first layer, a second layer arranged on a first surface side of the first layer, and a third layer arranged on a second surface side opposite the first surface of the first layer, the second layer being a surface layer of the interlayer film, the third layer being a surface layer of the interlayer film, the first layer comprising a thermoplastic resin, the second layer comprising a thermoplastic resin, and the third layer comprising a thermoplastic resin.

[0013] In a specific aspect of the interlayer film according to the present invention, the first layer contains a plasticizer, the second layer contains a plasticizer, and the third layer contains a plasticizer.

[0014] In a specific aspect of the interlayer film according to the present invention, the first layer has a glass transition temperature of 5°C or lower, the second layer has a glass transition temperature of 30°C or higher, and the third layer has a glass transition temperature of 30°C or higher.

[0015] In a specific aspect of the interlayer film according to the present invention, the thermoplastic resin contained in the first layer is a polyvinyl acetal resin, the thermoplastic resin contained in the second layer is a polyvinyl acetal resin, and the thermoplastic resin contained in the third layer is a polyvinyl acetal resin.

[0016] In a specific aspect of the interlayer film according to the present invention, the polyvinyl acetal resin contained in the first layer has a degree of acetylation of 10 mol % or less.

[0017] In a specific aspect of the interlayer film according to the present invention, the polyvinyl acetal resin contained in the first layer has a degree of acetylation of 15 mol % or more.

[0018] In a specific aspect of the interlayer film according to the present invention, the polyvinyl acetal resin contained in the first layer is a polyvinyl butyral resin.

[0019] In a specific aspect of the interlayer film according to the present invention, when the polyvinyl butyral resin contained in the first layer has a degree of butyralization of B mol % and a degree of acetylation of A mol %, the polyvinyl butyral resin contained in the first layer is a polyvinyl butyral resin that satisfies the formula: B≧−0.88×A+78.6.

[0020] In a specific aspect of the interlayer film according to the present invention, the interlayer film contains heat insulating particles.

[0021] In a specific aspect of the interlayer film according to the present invention, the second layer contains heat shielding particles, and the third layer contains heat shielding particles.

[0022] In a specific aspect of the interlayer film according to the present invention, the second layer contains heat shielding particles, the third layer contains heat shielding particles, and a layer different from both the second layer and the third layer does not contain heat shielding particles.

[0023] In a specific aspect of the interlayer film according to the present invention, the second layer contains heat shielding particles and at least one component selected from the group consisting of a phthalocyanine compound, a naphthalocyanine compound, an anthracyanine compound, and carbon black, and the third layer contains heat shielding particles and at least one component selected from the group consisting of a phthalocyanine compound, a naphthalocyanine compound, an anthracyanine compound, and carbon black.

[0024] In a specific aspect of the interlayer film according to the present invention, the component contained in the second layer is Pigment Blue 15, Pigment Green 7, or carbon black, and the component contained in the third layer is Pigment Blue 15, Pigment Green 7, or carbon black.

[0025] In a specific aspect of the interlayer film according to the present invention, the heat-shielding particles contained in the second layer are tin-doped indium oxide particles, and the heat-shielding particles contained in the third layer are tin-doped indium oxide particles.

[0026] In a specific aspect of the interlayer film according to the present invention, the interlayer film has one end and another end opposite the one end, and the thickness of the other end is greater than the thickness of the one end.

[0027] According to a broad aspect of the present invention, there is provided laminated glass comprising a first laminated glass component, a second laminated glass component, and the above-mentioned interlayer film for laminated glass, wherein the interlayer film for laminated glass is disposed between the first laminated glass component and the second laminated glass component.

[0028] According to a broad aspect of the present invention, there is provided a laminated glass comprising a first laminated glass component, a second laminated glass component, and an interlayer film for laminated glass having a one-layer structure or a two or more layer structure, the interlayer film for laminated glass being disposed between the first laminated glass component and the second laminated glass component, the absolute value of the difference between the secondary resonant frequency of the laminated glass before irradiation with xenon light and the secondary resonant frequency of the laminated glass after irradiation with xenon light, as determined by the following xenon light irradiation test, being 60 Hz or more, a loss factor at 20°C being 0.25 or more, and a solar transmittance being 50% or less.

[0029] Xenon light irradiation test: The secondary resonance frequency of the laminated glass at 10°C is determined using the central excitation method in accordance with ISO16940. Under the condition of 10°C, the laminated glass is exposed to 190W / m 2 The laminated glass is irradiated with xenon light for 30 minutes. The secondary resonance frequency of the laminated glass after irradiation with xenon light is determined using the central excitation method in accordance with ISO 16940. The absolute value of the difference between the secondary resonance frequency of the laminated glass before irradiation with xenon light and the secondary resonance frequency of the laminated glass after irradiation with xenon light is calculated.

[0030] In a specific aspect of the laminated glass according to the present invention, the first laminated glass member is green glass or a heat absorbing plate glass, and the second laminated glass member is green glass or a heat absorbing plate glass.

[0031] In a specific aspect of the laminated glass according to the present invention, the solar transmittance is 48% or less. Effect of the Invention

[0032] The interlayer film for laminated glass according to the present invention has a one-layer structure or a two or more layer structure. The interlayer film for laminated glass according to the present invention is sandwiched between two sheets of green glass with a thickness of 2 mm to obtain a laminated glass X having a length of 25 mm and a width of 300 mm. In the interlayer film for laminated glass according to the present invention, the absolute value of the difference between the secondary resonance frequency of the laminated glass X before irradiation with xenon light and the secondary resonance frequency of the laminated glass X after irradiation with xenon light, which is determined by the xenon light irradiation test, is 60 Hz or more. In the interlayer film for laminated glass according to the present invention, the laminated glass X has a loss factor of 0.25 or more at 20°C. In the interlayer film for laminated glass according to the present invention, the laminated glass X has a solar transmittance of 50% or less. Since the interlayer film for laminated glass according to the present invention has the above configuration, it is possible to increase the sound insulation of the laminated glass in a relatively low temperature range.

[0033] The laminated glass according to the present invention comprises a first laminated glass member, a second laminated glass member, and an interlayer film for laminated glass having a one-layer structure or a two or more layer structure, and the interlayer film for laminated glass is disposed between the first laminated glass member and the second laminated glass member. In the laminated glass according to the present invention, the absolute value of the difference between the secondary resonance frequency of the laminated glass before irradiation with xenon light and the secondary resonance frequency of the laminated glass after irradiation with xenon light, as determined by the xenon light irradiation test, is 60 Hz or more. The laminated glass according to the present invention has a loss factor of 0.25 or more and a solar transmittance of 50% or less at 20°C. Since the laminated glass according to the present invention has the above configuration, it can improve sound insulation in a relatively low temperature range. [Brief description of the drawings]

[0034] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic diagram of an interlayer film for laminated glass according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates a schematic diagram of an interlayer film for laminated glass according to a second embodiment of the present invention. [Diagram 3]FIG. 3 is a cross-sectional view that illustrates an example of laminated glass using the interlayer film for laminated glass shown in FIG. [Figure 4] FIG. 4 is a cross-sectional view that illustrates an example of laminated glass using the interlayer film for laminated glass shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] The present invention will be described in detail below.

[0036] (Interlayer film for laminated glass) The interlayer film for laminated glass according to the present invention (hereinafter sometimes abbreviated as "interlayer film") has a single-layer structure or a two or more-layer structure.

[0037] The interlayer film according to the present invention is sandwiched between two sheets of green glass with a thickness of 2 mm to obtain laminated glass X having a length of 25 mm and a width of 300 mm.

[0038] In the interlayer film of the present invention, the absolute value of the difference between the secondary resonance frequency of the laminated glass X before irradiation with xenon light and the secondary resonance frequency of the laminated glass X after irradiation with xenon light, as determined by the xenon light irradiation test described below, is 60 Hz or more. In the interlayer film of the present invention, the loss factor of the laminated glass X at 20°C is 0.25 or more. In the interlayer film of the present invention, the solar transmittance of the laminated glass X is 50% or less.

[0039] Xenon light irradiation test: Using the central excitation method in accordance with ISO16940, the secondary resonance frequency of the laminated glass X at 10°C is determined. Under the condition of 10°C, the laminated glass X is exposed to 190 W / m 2 The laminated glass X is irradiated with xenon light for 30 minutes. The secondary resonance frequency of the laminated glass X after irradiation with xenon light is determined by the central excitation method in accordance with ISO 16940. The absolute value of the difference between the secondary resonance frequency of the laminated glass X before irradiation with xenon light and the secondary resonance frequency of the laminated glass X after irradiation with xenon light is calculated.

[0040] The interlayer film according to the present invention has the above-mentioned features and is therefore capable of improving the sound insulation of laminated glass in a relatively low temperature range.

[0041] In laminated glass using a conventional interlayer film for laminated glass, the sound insulation of the laminated glass (for example, sound insulation at 2000 Hz to 5000 Hz) may decrease in a relatively low temperature range (for example, from -10° C. to 10° C.) For example, in a conventional interlayer film for laminated glass, the sound insulation of the laminated glass may change due to the movement of a plasticizer contained in the interlayer film between layers or the change in Young's modulus of the resin layer as the temperature changes, and as a result, the sound insulation may not be improved at relatively low temperatures.

[0042] In contrast, the interlayer film according to the present invention has the above-mentioned configuration and can therefore improve the sound insulation of the laminated glass in a relatively low temperature range (for example, -10°C to 10°C). For example, when the laminated glass is exposed to sunlight in a low-temperature environment, the interlayer film according to the present invention can increase the temperature of the interlayer film, thereby improving the sound insulation. In particular, when the interlayer film contains heat-shielding particles, the heat-shielding particles can absorb sunlight and effectively increase the temperature of the interlayer film, thereby making it possible to further effectively improve the sound insulation of the laminated glass.

[0043] The interlayer film according to the present invention has a one-layer structure or a two or more layer structure. The interlayer film according to the present invention may have a one-layer structure, or a two or more layer structure. The interlayer film according to the present invention may have a two-layer structure, a three-layer structure, or a three or more layer structure. The interlayer film according to the present invention includes a first layer. The interlayer film according to the present invention may be a single-layer interlayer film including only the first layer, or may be a multi-layer interlayer film including the first layer and another layer.

[0044] The interlayer film may have only the first layer, or may have a second layer in addition to the first layer. The interlayer film preferably has the second layer as a surface layer in the interlayer film. The second layer is preferably a surface layer of the interlayer film. When the interlayer film has the second layer, the second layer is disposed on the first surface side of the first layer.

[0045] The interlayer film may have a structure of three or more layers, and may include a third layer in addition to the first and second layers. The interlayer film preferably includes a third layer as a surface layer in the interlayer film. The third layer is preferably a surface layer of the interlayer film. When the interlayer film includes the second layer and the third layer, the third layer is disposed on the second surface side opposite to the first surface of the first layer.

[0046] Other layers may be provided between the first layer and the second layer, and between the first layer and the third layer.

[0047] The interlayer film according to the present invention is sandwiched between two sheets of green glass each having a thickness of 2 mm to produce laminated glass X having dimensions of 25 mm in length and 300 mm in width.

[0048] The laminated glass X is produced in order to carry out the xenon light irradiation test and to measure the loss factor, secondary resonance frequency and solar transmittance of the laminated glass X.

[0049] The laminated glass X is preferably produced as follows.

[0050] An interlayer film is sandwiched between two sheets of green glass with a thickness of 2 mm to obtain a laminate. The obtained laminate is placed in a rubber bag and degassed at a vacuum of 2.6 kPa for 20 minutes, then transferred to an oven in the degassed state and held at 90°C for an additional 30 minutes to perform vacuum pressing to pre-bond the laminate. The pre-bonded laminate is compressed in an autoclave for 20 minutes under conditions of 135°C and a pressure of 1.2 MPa to obtain laminated glass X having a length of 25 mm and a width of 300 mm.

[0051] The laminated glass X may be prepared by peeling off the interlayer in the laminated glass from the laminated glass member.

[0052] In the present invention, the laminated glass X is subjected to the following xenon light irradiation test.

[0053] Xenon light irradiation test: Using the central excitation method in accordance with ISO16940, the secondary resonance frequency of the laminated glass X at 10°C is determined. Under the condition of 10°C, the laminated glass X is exposed to 190 W / m 2 The laminated glass X is irradiated with xenon light for 30 minutes. The secondary resonance frequency of the laminated glass X after irradiation with xenon light is determined by the central excitation method in accordance with ISO 16940. The absolute value of the difference between the secondary resonance frequency of the laminated glass X before irradiation with xenon light and the secondary resonance frequency of the laminated glass X after irradiation with xenon light is calculated.

[0054] More specifically, the xenon light irradiation test of the laminated glass X is carried out as follows.

[0055] (1) The secondary resonance frequency of the laminated glass X at 10°C is determined by the central excitation method in accordance with ISO 16940.

[0056] (2) Under windless conditions at 10°C, the laminated glass X is subjected to a load of 190 W / m 2 The laminated glass X is irradiated with xenon light of 190 W / m for 30 minutes. An example of an apparatus for irradiating xenon light is a solar simulator apparatus (e.g., "HAL-320" manufactured by Asahi Spectroscopy). An example of an apparatus for measuring illuminance is an illuminometer (e.g., "KEYSIGHT U1252B, Sensor EKO Pyranometer ML-01" manufactured by Keysight Technologies). The distance between the main surface of the laminated glass X and the light source (e.g., a xenon lamp) is set at 100 mm for an illuminance of 190 W / m. 2 There is no particular limitation as long as the arrangement is such that

[0057] (3) The secondary resonance frequency of the laminated glass X after irradiation with xenon light is determined by a central excitation method in accordance with ISO 16940. In this case, the secondary resonance frequency is determined within 2 minutes (preferably within 1 minute) after irradiation with xenon light.

[0058] (4) Calculate the absolute value of the difference between the secondary resonance frequency of the laminated glass X before irradiation with xenon light obtained in (1) above and the secondary resonance frequency of the laminated glass X after irradiation with xenon light obtained in (3) above.

[0059] In order to exert the effects of the present invention, the absolute value of the difference between the secondary resonance frequency of the laminated glass X before irradiation with xenon light and the secondary resonance frequency of the laminated glass X after irradiation with xenon light is 60 Hz or more.

[0060] The absolute value of the difference between the secondary resonance frequency of the laminated glass X before irradiation with xenon light and the secondary resonance frequency of the laminated glass X after irradiation with xenon light is preferably 75 Hz or more, more preferably 100 Hz or more, preferably 200 Hz or less, and more preferably 120 Hz or less. When the absolute value of the difference is equal to or more than the above lower limit and equal to or less than the above upper limit, the effects of the present invention can be more effectively exhibited.

[0061] From the viewpoint of exerting the effects of the present invention more effectively, the secondary resonance frequency of the laminated glass X at 10° C. before irradiation with xenon light is preferably 900 Hz or more, more preferably 910 Hz or more, even more preferably 925 Hz or more, and is preferably 1000 Hz or less, more preferably 965 Hz or less, and even more preferably 950 Hz or less.

[0062] In order to more effectively exert the effects of the present invention, the secondary resonance frequency of the laminated glass X after irradiation with xenon light is preferably 750 Hz or more, more preferably 815 Hz or more, and preferably 850 Hz or less, more preferably 843 Hz or less.

[0063] The following methods can be used to control the absolute value of the difference and the secondary resonance frequency within the preferred ranges. (1) A method of adjusting the content of a plasticizer. Generally, the secondary resonance frequency increases when the content of a plasticizer is reduced. (2) A method of controlling the Young's modulus of the first layer, the second layer, or the third layer described below. Generally, the secondary resonance frequency increases when the Young's modulus is increased. (3) A method of controlling the heat-shielding performance of the intermediate film. Generally, the absolute value of the difference increases when the heat-shielding performance of the intermediate film is improved. (4) A method of controlling the thickness of the second layer (surface layer) or the third layer (surface layer) described below. Generally, the secondary resonance frequency decreases when the thickness of the second layer or the third layer is increased. (5) A method of controlling the thickness of the first layer (intermediate layer) described below. Generally, the secondary resonance frequency decreases when the thickness of the first layer is increased. By appropriately combining these methods, the absolute value of the difference and the secondary resonance frequency can be controlled within the preferred ranges.

[0064] When the laminated glass X is stored at 10°C for 56 days or more, the secondary resonance frequency of the laminated glass X after storage at 10°C, as determined by a central vibration method in accordance with ISO16940, is preferably 900Hz or more, more preferably 920Hz or more, and preferably 1050Hz or less, more preferably 975Hz or less. When the secondary resonance frequency is equal to or more than the lower limit and equal to or less than the upper limit, the effects of the present invention can be more effectively exhibited. The secondary resonance frequency is preferably measured after storing the laminated glass X at 10°C for 56 days.

[0065] In order to exert the effects of the present invention, the loss factor of the laminated glass X at 20° C. is 0.25 or more.

[0066] To more effectively exert the effects of the present invention, the loss coefficient of the laminated glass X at 20° C. is preferably 0.26 or more, more preferably 0.28 or more, and is preferably 0.5 or less, more preferably 0.4 or less.

[0067] The loss factor of the laminated glass X at 20° C. is measured by the central vibration method in accordance with ISO16940.

[0068] In order to exert the effects of the present invention and to enhance the heat shielding property, the solar transmittance of the laminated glass X is 50% or less.

[0069] From the viewpoint of more effectively exerting the effects of the present invention and more effectively improving the heat shielding property, the solar transmittance of the laminated glass X is preferably 10% or more, more preferably 15% or more, and is preferably 48% or less, more preferably 44% or less.

[0070] The solar transmittance of the laminated glass X is measured using a spectrophotometer (for example, "U-4100" manufactured by Hitachi High-Technologies Corporation) in accordance with JIS R3106:1998.

[0071] Hereinafter, specific embodiments of the present invention will be described with reference to the drawings.

[0072] FIG. 1 is a cross-sectional view that illustrates a schematic diagram of an interlayer film for laminated glass according to a first embodiment of the present invention.

[0073] The interlayer film 11 shown in FIG. 1 is a multi-layer interlayer film having a structure of two or more layers. The interlayer film 11 is used to obtain laminated glass. The interlayer film 11 is an interlayer film for laminated glass. The interlayer film 11 includes a first layer 1, a second layer 2, and a third layer 3. The interlayer film 11 has a three-layer structure. The second layer 2 is disposed and laminated on a first surface 1a of the first layer 1. The third layer 3 is disposed and laminated on a second surface 1b opposite to the first surface 1a of the first layer 1. The first layer 1 is an intermediate layer. The second layer 2 and the third layer 3 are each a protective layer, and in this embodiment, are surface layers. The first layer 1 is disposed and sandwiched between the second layer 2 and the third layer 3. Therefore, the intermediate film 11 has a multilayer structure in which the second layer 2, the first layer 1, and the third layer 3 are laminated in this order (second layer 2 / first layer 1 / third layer 3).

[0074] Other layers may be disposed between the second layer 2 and the first layer 1, and between the first layer 1 and the third layer 3. It is preferable that the second layer 2 and the first layer 1, and the first layer 1 and the third layer 3 are directly laminated to each other. Examples of the other layers include a layer containing polyethylene terephthalate or the like.

[0075] FIG. 2 is a cross-sectional view that illustrates a schematic diagram of an interlayer film for laminated glass according to a second embodiment of the present invention.

[0076] The interlayer film 11A shown in Fig. 2 is a single-layer interlayer film having a one-layer structure. The interlayer film 11A is a first layer. The interlayer film 11A is used to obtain laminated glass. The interlayer film 11A is an interlayer film for laminated glass.

[0077] From the viewpoint of further improving the sound insulation of the laminated glass, the glass transition temperature of the first layer is preferably -10°C or higher, more preferably -5°C or higher, and preferably 5°C or lower, more preferably 2°C or lower.

[0078] From the viewpoint of further improving the sound insulation of the laminated glass, the glass transition temperature of the second layer is preferably 30°C or higher, more preferably 32°C or higher, and preferably 40°C or lower, more preferably 38°C or lower.

[0079] From the viewpoint of further improving the sound insulation of the laminated glass, the glass transition temperature of the third layer is preferably 30°C or higher, more preferably 32°C or higher, and preferably 40°C or lower, more preferably 38°C or lower.

[0080] The glass transition temperature is determined by viscoelasticity measurement, which is specifically performed as follows.

[0081] The test pieces are stored for 12 hours in an environment with a room temperature of 23±2°C and a humidity of 25±5%. Then, the viscoelasticity is measured using a TA Instruments viscoelasticity measuring device "ARES-G2". Using a parallel plate with a diameter of 8 mm as a jig, the measurements are performed under the following conditions: shear mode, temperature drop rate of 3°C / min from 100°C to -20°C, frequency of 1Hz, and strain of 1%.

[0082] The viscoelasticity measurement may be performed using the interlayer film itself. In this case, the peaks of tan δ derived from the first layer, the second layer, and the third layer may be read from the measurement results. For an interlayer film having a structure of two or more layers, each layer may be peeled off and the glass transition temperature of the layer to be measured may be measured. In the case of laminated glass, the laminated glass may be cooled with liquid nitrogen or the like, and then the laminated glass member and the interlayer film may be peeled off, and the viscoelasticity measurement may be performed using the peeled interlayer film.

[0083] The interlayer film according to the present invention, the first layer, the second layer, and the third layer, as well as each component used in the interlayer film, will be described in detail below.

[0084] (thermoplastic resin) The intermediate film preferably contains a thermoplastic resin (hereinafter, may be referred to as thermoplastic resin (0)). Examples of the thermoplastic resin include polyvinyl acetate resin, polyester resin, polyvinyl acetal resin, vinyl acetate resin, polystyrene resin, ethylene-vinyl acetate copolymer resin, ethylene-acrylic acid copolymer resin, polyurethane resin, ionomer resin, polyvinyl alcohol resin, polyolefin resin such as aliphatic polyolefin, and (meth)acrylic resin (polymer having a (meth)acryloyl group). Polyoxymethylene (or polyacetal) resin is included in polyvinyl acetal resin. Thermoplastic resins other than these may be used as the thermoplastic resin. The thermoplastic resin may be a thermoplastic elastomer.

[0085] The intermediate film preferably contains a polyvinyl acetal resin (hereinafter, may be referred to as polyvinyl acetal resin (0)) as the thermoplastic resin (0). The thermoplastic resin (0) contained in the intermediate film is preferably polyvinyl acetal resin (0). The first layer (including a single-layer intermediate film) preferably contains a thermoplastic resin (hereinafter, may be referred to as thermoplastic resin (1)). The first layer preferably contains a polyvinyl acetal resin (hereinafter, may be referred to as polyvinyl acetal resin (1)) as the thermoplastic resin (1). The thermoplastic resin (1) contained in the first layer is preferably polyvinyl acetal resin (1). The second layer preferably contains a thermoplastic resin (hereinafter, may be referred to as thermoplastic resin (2)). The second layer preferably contains a polyvinyl acetal resin (hereinafter, may be referred to as polyvinyl acetal resin (2)) as the thermoplastic resin (2). The thermoplastic resin (2) contained in the second layer is preferably a polyvinyl acetal resin (2). The third layer preferably contains a thermoplastic resin (hereinafter, may be referred to as a thermoplastic resin (3)). The third layer preferably contains a polyvinyl acetal resin (hereinafter, may be referred to as a polyvinyl acetal resin (3)) as the thermoplastic resin (3). The thermoplastic resin (3) contained in the third layer is preferably a polyvinyl acetal resin (3). The thermoplastic resin (1), the thermoplastic resin (2), and the thermoplastic resin (3) may be the same or different. Since sound insulation is further improved, the thermoplastic resin (1) is preferably different from the thermoplastic resin (2) and the thermoplastic resin (3). The polyvinyl acetal resin (1), the polyvinyl acetal resin (2), and the polyvinyl acetal resin (3) may be the same or different. Since the sound insulation property is further improved, it is preferable that the polyvinyl acetal resin (1) is different from the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3).The thermoplastic resin (0), the thermoplastic resin (1), the thermoplastic resin (2), and the thermoplastic resin (3) may each be used alone or in combination of two or more thereof. The polyvinyl acetal resin (0), the polyvinyl acetal resin (1), the polyvinyl acetal resin (2), and the polyvinyl acetal resin (3) may each be used alone or in combination of two or more thereof.

[0086] Examples of the thermoplastic resin include polyvinyl acetal resin, ethylene-vinyl acetate copolymer resin, ethylene-acrylic acid copolymer resin, polyurethane resin, polyvinyl alcohol resin, ionomer resin, etc. Thermoplastic resins other than these may also be used.

[0087] The thermoplastic resin is preferably a polyvinyl acetal resin. By using a polyvinyl acetal resin in combination with a plasticizer, the adhesive strength of the layer containing the polyvinyl acetal resin and the plasticizer to the laminated glass member or other layer is further increased.

[0088] The polyvinyl acetal resin can be produced, for example, by acetalizing polyvinyl alcohol (PVA) with an aldehyde. The polyvinyl acetal resin is preferably an acetalized product of polyvinyl alcohol. The polyvinyl alcohol can be obtained, for example, by saponifying polyvinyl acetate. The degree of saponification of the polyvinyl alcohol is generally within the range of 70 mol% to 99.9 mol%.

[0089] The average degree of polymerization of the polyvinyl alcohol (PVA) is preferably 200 or more, more preferably 500 or more, even more preferably 1500 or more, even more preferably 1600 or more, particularly preferably 2600 or more, most preferably 2700 or more, and preferably 5000 or less, more preferably 4000 or less, and even more preferably 3500 or less. When the average degree of polymerization is equal to or more than the lower limit, the penetration resistance of the laminated glass is further improved. When the average degree of polymerization is equal to or less than the upper limit, the interlayer film is easily formed.

[0090] The average degree of polymerization of the polyvinyl alcohol is determined by a method in accordance with JIS K6726 "Testing method for polyvinyl alcohol."

[0091] The number of carbon atoms in the acetal group contained in the polyvinyl acetal resin is not particularly limited. The aldehyde used in producing the polyvinyl acetal resin is not particularly limited. The number of carbon atoms in the acetal group in the polyvinyl acetal resin is preferably 3 to 5, and more preferably 3 or 4. When the number of carbon atoms in the acetal group in the polyvinyl acetal resin is 3 or more, the glass transition temperature of the interlayer film becomes sufficiently low.

[0092] The aldehyde is not particularly limited. In general, an aldehyde having 1 to 10 carbon atoms is preferably used. Examples of the aldehyde having 1 to 10 carbon atoms include propionaldehyde, n-butylaldehyde, isobutyraldehyde, n-valeraldehyde, 2-ethylbutyraldehyde, n-hexylaldehyde, n-octylaldehyde, n-nonylaldehyde, n-decylaldehyde, formaldehyde, acetaldehyde, and benzaldehyde. The aldehyde is preferably propionaldehyde, n-butylaldehyde, isobutyraldehyde, n-hexylaldehyde, or n-valeraldehyde, more preferably propionaldehyde, n-butylaldehyde, or isobutyraldehyde, and even more preferably n-butylaldehyde. The aldehydes may be used alone or in combination of two or more.

[0093] The intermediate film preferably contains a polyvinyl butyral resin as the thermoplastic resin (0). The intermediate film preferably contains a polyvinyl butyral resin as the polyvinyl acetal resin (0). The thermoplastic resin (0) contained in the intermediate film is preferably a polyvinyl butyral resin. The first layer preferably contains a polyvinyl butyral resin as the thermoplastic resin (1). The first layer preferably contains a polyvinyl butyral resin as the polyvinyl acetal resin (1). The thermoplastic resin (1) contained in the first layer is preferably a polyvinyl butyral resin. The second layer preferably contains a polyvinyl butyral resin as the thermoplastic resin (2). The second layer preferably contains a polyvinyl butyral resin as the polyvinyl acetal resin (2). The thermoplastic resin (2) contained in the second layer is preferably a polyvinyl butyral resin. The third layer preferably contains a polyvinyl butyral resin as the thermoplastic resin (3). The third layer preferably contains a polyvinyl butyral resin as the polyvinyl acetal resin (3). The thermoplastic resin (3) contained in the third layer is preferably a polyvinyl butyral resin. The polyvinyl butyral resins contained in the intermediate film, the first layer, the second layer, and the third layer may each be of one type or two or more types in combination.

[0094] The hydroxyl group content (hydroxyl group amount) of the polyvinyl acetal resin (0) is preferably 15 mol% or more, more preferably 18 mol% or more, and preferably 40 mol% or less, more preferably 35 mol% or less. When the hydroxyl group content is equal to or more than the lower limit, the adhesive strength of the interlayer film is further increased. When the hydroxyl group content is equal to or less than the upper limit, the flexibility of the interlayer film is increased, making it easier to handle the interlayer film.

[0095] The hydroxyl group content (hydroxyl group amount) of the polyvinyl acetal resin (1) is preferably 15 mol% or more, more preferably 17 mol% or more, even more preferably 20 mol% or more, preferably 28 mol% or less, more preferably 27 mol% or less, even more preferably 25 mol% or less, and particularly preferably 24 mol% or less. When the hydroxyl group content is equal to or more than the lower limit, the mechanical strength of the interlayer film is further increased. In particular, when the hydroxyl group content of the polyvinyl acetal resin (1) is 15 mol% or more, the reaction efficiency is high and the productivity is excellent, and when it is 28 mol% or less, the sound insulation of the laminated glass is further increased. In addition, when the hydroxyl group content is equal to or less than the upper limit, the flexibility of the interlayer film is increased, and the handling of the interlayer film is facilitated.

[0096] The hydroxyl group content of each of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) is preferably 25 mol% or more, more preferably 28 mol% or more, more preferably 30 mol% or more, even more preferably 31.5 mol% or more, even more preferably 32 mol% or more, and particularly preferably 33 mol% or more. The hydroxyl group content of each of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) is preferably 38 mol% or less, more preferably 37 mol% or less, even more preferably 36.5 mol% or less, and particularly preferably 36 mol% or less. When the hydroxyl group content is the lower limit or more, the adhesive strength of the interlayer film is further increased. When the hydroxyl group content is the upper limit or less, the flexibility of the interlayer film is increased, and the handling of the interlayer film is facilitated.

[0097] From the viewpoint of further improving the sound insulation, the hydroxyl group content of the polyvinyl acetal resin (1) is preferably lower than the hydroxyl group content of the polyvinyl acetal resin (2). From the viewpoint of further improving the sound insulation, the hydroxyl group content of the polyvinyl acetal resin (1) is preferably lower than the hydroxyl group content of the polyvinyl acetal resin (3). From the viewpoint of further improving the sound insulation, the absolute value of the difference between the hydroxyl group content of the polyvinyl acetal resin (1) and the hydroxyl group content of the polyvinyl acetal resin (2) is preferably 1 mol % or more, more preferably 5 mol % or more, even more preferably 9 mol % or more, particularly preferably 10 mol % or more, and most preferably 12 mol % or more. From the viewpoint of further improving sound insulation, the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin (1) and the hydroxyl content of the polyvinyl acetal resin (3) is preferably 1 mol% or more, more preferably 5 mol% or more, even more preferably 9 mol% or more, particularly preferably 10 mol% or more, and most preferably 12 mol% or more. The absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin (1) and the hydroxyl content of the polyvinyl acetal resin (2), and the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin (1) and the hydroxyl content of the polyvinyl acetal resin (3) are preferably 20 mol% or less.

[0098] The hydroxyl content of the polyvinyl acetal resin is a molar fraction calculated by dividing the amount of ethylene groups to which hydroxyl groups are bonded by the total amount of ethylene groups in the main chain, and expressed as a percentage. The amount of ethylene groups to which hydroxyl groups are bonded can be measured, for example, in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral."

[0099] The degree of acetylation (amount of acetyl groups) of the polyvinyl acetal resin (0) is preferably 0.1 mol% or more, more preferably 0.3 mol% or more, even more preferably 0.5 mol% or more, and preferably 30 mol% or less, more preferably 25 mol% or less, and even more preferably 20 mol% or less. When the degree of acetylation is equal to or more than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetylation is equal to or less than the upper limit, the moisture resistance of the interlayer film and the laminated glass is increased.

[0100] The degree of acetylation (amount of acetyl groups) of the polyvinyl acetal resin (1) is preferably 10 mol% or less, and also preferably 15 mol% or more. When the degree of acetylation of the polyvinyl acetal resin (1) is 10 mol% or less, the degree of acetylation of the polyvinyl acetal resin (1) is preferably 0.1 mol% or more, more preferably 1.1 mol% or more, preferably 9 mol% or less, and more preferably 7 mol% or less. When the degree of acetylation of the polyvinyl acetal resin (1) is 15 mol% or more, the degree of acetylation of the polyvinyl acetal resin (1) is preferably 16 mol% or more, more preferably 17 mol% or more, preferably 25 mol% or less, more preferably 23 mol% or less, and even more preferably 19 mol% or less. When the degree of acetylation is the lower limit or more, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetylation is the upper limit or less, the moisture resistance of the interlayer film and the laminated glass is increased. In addition, when the degree of acetylation of the polyvinyl acetal resin (1) is equal to or higher than the lower limit and equal to or lower than the upper limit, it becomes easy to control the absolute value of the difference and the secondary resonance frequency within the preferred ranges, and the effects of the present invention can be more effectively achieved. In addition, when the degree of acetylation of the polyvinyl acetal resin (1) is 0.1 mol% or more and 25 mol% or less, the penetration resistance is excellent. The degree of acetylation of the polyvinyl acetal resin (1) may be 10 mol% or less, or 15 mol% or more.

[0101] The degree of acetylation of each of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) is preferably 0.01 mol% or more, more preferably 0.5 mol% or more, and preferably 10 mol% or less, more preferably 2 mol% or less. When the degree of acetylation is equal to or more than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetylation is equal to or less than the upper limit, the moisture resistance of the interlayer film and the laminated glass is increased.

[0102] The degree of acetylation is a molar fraction calculated by dividing the amount of ethylene groups to which acetyl groups are bonded by the total amount of ethylene groups in the main chain, expressed as a percentage. The amount of ethylene groups to which acetyl groups are bonded can be measured, for example, in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral."

[0103] The degree of acetalization of the polyvinyl acetal resin (0) (the degree of butyralization in the case of a polyvinyl butyral resin) is preferably 60 mol% or more, more preferably 63 mol% or more, preferably 85 mol% or less, more preferably 75 mol% or less, and even more preferably 70 mol% or less. When the degree of acetalization is equal to or more than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetalization is equal to or less than the upper limit, the reaction time required to produce the polyvinyl acetal resin is shortened.

[0104] The degree of acetalization of the polyvinyl acetal resin (1) (the degree of butyralization in the case of a polyvinyl butyral resin) is preferably 47 mol% or more, more preferably 60 mol% or more, preferably 85 mol% or less, more preferably 80 mol% or less, and even more preferably 75 mol% or less. When the degree of acetalization is equal to or more than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetalization is equal to or less than the upper limit, the reaction time required for producing the polyvinyl acetal resin is shortened. In addition, when the degree of acetalization of the polyvinyl acetal resin (1) (the degree of butyralization in the case of a polyvinyl butyral resin) is equal to or more than the lower limit and equal to or less than the upper limit, it becomes easy to control the absolute value of the difference and the secondary resonance frequency within the preferred ranges, and the effects of the present invention can be more effectively exhibited.

[0105] When the degree of acetalization of the polyvinyl acetal resin (1) is B mol % and the degree of acetylation is A mol %, the polyvinyl acetal resin (1) is preferably a polyvinyl acetal resin that satisfies the formula: B ≧ −0.88×A + 78.6 In this case, it becomes easy to control the absolute value of the difference and the secondary resonance frequency within the preferred ranges, and the effects of the present invention can be more effectively exhibited.

[0106] When the polyvinyl acetal resin (1) is a polyvinyl butyral resin, it is particularly preferable that the polyvinyl butyral resin is a polyvinyl butyral resin that satisfies the formula: B≧−0.88×A+78.6, where the butyralization degree of the polyvinyl butyral resin is B mol % and the acetylation degree of the polyvinyl butyral resin is A mol %. In this case, it becomes easier to control the absolute value of the difference and the secondary resonance frequency within the preferred ranges, and the effects of the present invention can be exhibited even more effectively.

[0107] The degree of acetalization of each of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) (the degree of butyralization in the case of a polyvinyl butyral resin) is preferably 55 mol% or more, more preferably 60 mol% or more, preferably 75 mol% or less, more preferably 71 mol% or less. When the degree of acetalization is equal to or more than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetalization is equal to or less than the upper limit, the reaction time required to produce the polyvinyl acetal resin is shortened.

[0108] The degree of acetalization is determined as follows. The amount of ethylene groups to which hydroxyl groups are bonded and the amount of ethylene groups to which acetyl groups are bonded are subtracted from the total amount of ethylene groups in the main chain. The mole fraction is determined by dividing the obtained value by the total amount of ethylene groups in the main chain. The resulting percentage is the degree of acetalization.

[0109] The hydroxyl group content (hydroxyl group amount), acetalization degree (butyralization degree), and acetylation degree are preferably calculated from the results measured by a method conforming to JIS K6728 "Testing Method for Polyvinyl Butyral". However, measurements according to ASTM D1396-92 may also be used. When the polyvinyl acetal resin is a polyvinyl butyral resin, the hydroxyl group content (hydroxyl group amount), acetalization degree (butyralization degree), and acetylation degree can be calculated from the results measured by a method conforming to JIS K6728 "Testing Method for Polyvinyl Butyral".

[0110] In 100% by weight of the thermoplastic resin contained in the interlayer, the content of the polyvinyl acetal resin is preferably 10% by weight or more, more preferably 30% by weight or more, even more preferably 50% by weight or more, still more preferably 70% by weight or more, particularly preferably 80% by weight or more, and most preferably 90% by weight or more. The main component (50% by weight or more) of the thermoplastic resin in the interlayer is preferably a polyvinyl acetal resin.

[0111] (Plasticizer) The interlayer preferably contains a plasticizer. The first layer (including a single-layer interlayer) preferably contains a plasticizer (hereinafter, may be referred to as plasticizer (1)). The second layer preferably contains a plasticizer (hereinafter, may be referred to as plasticizer (2)). The third layer preferably contains a plasticizer (hereinafter, may be referred to as plasticizer (3)). By using a plasticizer or by using a polyvinyl acetal resin and a plasticizer in combination, the impact resistance and penetration resistance are further improved, and the adhesive strength of the layer containing the polyvinyl acetal resin and the plasticizer to the laminated glass member or other layers is appropriately increased. The plasticizer is not particularly limited. The plasticizer (1), the plasticizer (2), and the plasticizer (3) may be the same or different. The plasticizer (1), the plasticizer (2), and the plasticizer (3) may each be used alone or in combination of two or more.

[0112] The plasticizer may be an organic ester plasticizer such as a monobasic organic acid ester or a polybasic organic acid ester, or an organic phosphoric acid plasticizer such as an organic phosphoric acid plasticizer or an organic phosphorous acid plasticizer. The plasticizer is preferably an organic ester plasticizer. The plasticizer is preferably a liquid plasticizer.

[0113] The monobasic organic acid ester may be a glycol ester obtained by reacting a glycol with a monobasic organic acid. The glycol may be triethylene glycol, tetraethylene glycol, or tripropylene glycol. The monobasic organic acid may be butyric acid, isobutyric acid, caproic acid, 2-ethylbutyric acid, heptyl acid, n-octylic acid, 2-ethylhexyl acid, n-nonyl acid, or decyl acid.

[0114] Examples of the polybasic organic acid ester include ester compounds of a polybasic organic acid and an alcohol having a linear or branched structure with 4 to 8 carbon atoms. Examples of the polybasic organic acid include adipic acid, sebacic acid, and azelaic acid.

[0115] Examples of the organic ester plasticizer include triethylene glycol di-2-ethylpropanoate, triethylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylhexanoate, triethylene glycol dicaprylate, triethylene glycol di-n-octanoate, triethylene glycol di-n-heptanoate, tetraethylene glycol di-n-heptanoate, dibutyl sebacate, dioctyl azelate, dibutyl carbitol adipate, ethylene glycol di-2-ethylbutyrate, 1,3-propylene glycol di-2-ethylbutyrate, 1,4-butylene glycol di-2-ethylbutyrate, di Examples of suitable plasticizers include ethylene glycol di-2-ethylbutyrate, diethylene glycol di-2-ethylhexanoate, dipropylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylpentanoate, tetraethylene glycol di-2-ethylbutyrate, diethylene glycol dicaprylate, dihexyl adipate, dioctyl adipate, hexylcyclohexyl adipate, a mixture of heptyl adipate and nonyl adipate, diisononyl adipate, diisodecyl adipate, heptylnonyl adipate, dibutyl sebacate, oil-modified alkyd sebacate, and a mixture of phosphoric acid ester and adipate. Other organic ester plasticizers may also be used. Other adipic acid esters than the above-mentioned adipic acid esters may also be used.

[0116] The organic phosphoric acid plasticizers include tributoxyethyl phosphate, isodecylphenyl phosphate, and triisopropyl phosphate.

[0117] The plasticizer is preferably a diester plasticizer represented by the following formula (1).

[0118] [ka]

[0119] In the above formula (1), R1 and R2 each represent an organic group having 2 to 10 carbon atoms, R3 represents an ethylene group, an isopropylene group or an n-propylene group, and p represents an integer of 3 to 10. In the above formula (1), R1 and R2 each represent an organic group having 5 to 10 carbon atoms, and more preferably an organic group having 6 to 10 carbon atoms.

[0120] The plasticizer preferably includes triethylene glycol di-2-ethylhexanoate (3GO), triethylene glycol di-2-ethylbutyrate (3GH) or triethylene glycol di-2-ethylpropanoate.The plasticizer more preferably includes triethylene glycol di-2-ethylhexanoate or triethylene glycol di-2-ethylbutyrate, and even more preferably includes triethylene glycol di-2-ethylhexanoate.

[0121] In the first layer, the content of the plasticizer (1) relative to 100 parts by weight of the thermoplastic resin (1) (when the thermoplastic resin (1) is a polyvinyl acetal resin (1), 100 parts by weight of the polyvinyl acetal resin (1)) is defined as the content (1). The content (1) is preferably 40 parts by weight or more, more preferably 50 parts by weight or more, even more preferably 60 parts by weight or more, preferably 85 parts by weight or less, more preferably 75 parts by weight or less, even more preferably 71 parts by weight or less, and particularly preferably 68 parts by weight or less. When the content (1) is equal to or more than the lower limit, the flexibility of the interlayer film is increased, and the interlayer film is easy to handle. When the content (1) is equal to or less than the upper limit, the penetration resistance of the laminated glass is further increased. When the content (1) is equal to or more than the lower limit and equal to or less than the upper limit, it is easy to control the absolute value of the difference and the secondary resonance frequency within the preferred ranges, and the effect of the present invention can be further effectively exhibited.

[0122] In the second layer, the content of the plasticizer (2) relative to 100 parts by weight of the thermoplastic resin (2) (when the thermoplastic resin (2) is a polyvinyl acetal resin (2), 100 parts by weight of the polyvinyl acetal resin (2)) is defined as the content (2). The content (2) is preferably 10 parts by weight or more, more preferably 15 parts by weight or more, even more preferably 20 parts by weight or more, particularly preferably 24 parts by weight or more, preferably 40 parts by weight or less, more preferably 35 parts by weight or less, even more preferably 33 parts by weight or less, and particularly preferably 32 parts by weight or less. When the content (2) is equal to or more than the lower limit, the flexibility of the interlayer film is increased, and the handling of the interlayer film becomes easier. When the content (2) is equal to or less than the upper limit, the bending rigidity is further increased.

[0123] In the third layer, the content of the plasticizer (3) relative to 100 parts by weight of the thermoplastic resin (3) (when the thermoplastic resin (3) is a polyvinyl acetal resin (3), 100 parts by weight of the polyvinyl acetal resin (3)) is defined as the content (3). The content (3) is preferably 10 parts by weight or more, more preferably 15 parts by weight or more, even more preferably 20 parts by weight or more, particularly preferably 24 parts by weight or more, preferably 40 parts by weight or less, more preferably 35 parts by weight or less, even more preferably 33 parts by weight or less, and particularly preferably 32 parts by weight or less. When the content (3) is equal to or more than the lower limit, the flexibility of the interlayer film is increased, and the handling of the interlayer film becomes easier. When the content (3) is equal to or less than the upper limit, the bending rigidity is further increased.

[0124] The content (1) and the content (2) may be the same or different. The content (1) and the content (3) may be the same or different. From the viewpoint of improving the sound insulation of the laminated glass, it is preferable that the content (1) and the content (2) are the same, or the content (1) is greater than the content (2), and it is more preferable that the content (1) is greater than the content (2). From the viewpoint of improving the sound insulation of the laminated glass, it is preferable that the content (1) and the content (3) are the same, or the content (1) is greater than the content (3), and it is more preferable that the content (1) is greater than the content (3).

[0125] From the viewpoint of further improving the sound insulation of the laminated glass, the absolute value of the difference between the content (2) and the content (1) and the absolute value of the difference between the content (3) and the content (1) are each preferably 10 parts by weight or more, more preferably 15 parts by weight or more, and even more preferably 20 parts by weight or more. The absolute value of the difference between the content (2) and the content (1) and the absolute value of the difference between the content (3) and the content (1) are each preferably 80 parts by weight or less, more preferably 75 parts by weight or less, and even more preferably 70 parts by weight or less.

[0126] (Heat-shielding material) The intermediate film preferably contains a heat-shielding substance. The first layer (including a single-layer intermediate film) preferably contains a heat-shielding substance. The second layer preferably contains a heat-shielding substance. The third layer preferably contains a heat-shielding substance. Only one type of the heat-shielding substance may be used, or two or more types may be used in combination. The heat-shielding substance may also correspond to a colorant, which will be described later.

[0127] The heat-shielding material preferably contains at least one component X selected from among a phthalocyanine compound, a naphthalocyanine compound, an anthracyanine compound, and carbon black, or contains heat-shielding particles. In this case, the component X may also function as a colorant. In order to further improve the heat-shielding property, it is more preferable that the heat-shielding material contains the component X and the heat-shielding particles. The heat-shielding material may contain at least one component X1 selected from among a phthalocyanine compound, a naphthalocyanine compound, and an anthracyanine compound, or may contain heat-shielding particles. In order to further improve the heat-shielding property, it is more preferable that the heat-shielding material contains the component X1 and heat-shielding particles. The heat-shielding material may contain carbon black or may contain heat-shielding particles. In order to further improve the heat-shielding property, it is more preferable that the heat-shielding material contains carbon black and heat-shielding particles.

[0128] Ingredient X: The interlayer film preferably contains at least one component X selected from a phthalocyanine compound, a naphthalocyanine compound, an anthracyanine compound, and carbon black. The first layer preferably contains the component X. The second layer preferably contains the component X. The third layer preferably contains the component X. The component X is a heat-shielding material. Only one type of the component X may be used, or two or more types may be used in combination.

[0129] There is no particular limitation on the above-mentioned component X. As the component X, conventionally known phthalocyanine compounds, naphthalocyanine compounds, anthracyanine compounds, and carbon black can be used.

[0130] From the viewpoint of further improving the heat insulation property of the laminated glass, the above-mentioned component X is preferably at least one selected from the group consisting of phthalocyanine, phthalocyanine derivatives, naphthalocyanine, naphthalocyanine derivatives, and carbon black, and more preferably at least one of phthalocyanine and phthalocyanine derivatives.

[0131] From the viewpoint of effectively increasing the heat shielding property and maintaining the visible light transmittance at a higher level for a long period of time, the above component X preferably contains a vanadium atom or a copper atom. The above component X preferably contains a vanadium atom, and also preferably contains a copper atom. The above component X is more preferably at least one of phthalocyanine containing a vanadium atom or a copper atom and a derivative of phthalocyanine containing a vanadium atom or a copper atom. From the viewpoint of further increasing the heat shielding property of the interlayer film and the laminated glass, the above component X preferably has a structural unit in which an oxygen atom is bonded to a vanadium atom.

[0132] From the viewpoint of further improving the heat insulating property of the laminated glass, the above-mentioned component X is preferably Pigment Blue 15, Pigment Green 7, or carbon black. Pigment Blue 15 and Pigment Green 7 are phthalocyanine compounds containing copper atoms.

[0133] In 100% by weight of the layer (first layer, second layer or third layer) containing the component X, the content of the component X is preferably 0.001% by weight or more, more preferably 0.005% by weight or more, even more preferably 0.01% by weight or more, and particularly preferably 0.02% by weight or more. In 100% by weight of the layer (first layer, second layer or third layer) containing the component X, the content of the component X is preferably 0.2% by weight or less, more preferably 0.1% by weight or less, even more preferably 0.05% by weight or less, and particularly preferably 0.04% by weight or less. When the content of the component X is the above lower limit or more and the above upper limit or less, the heat shielding property is sufficiently high and the visible light transmittance is sufficiently high. For example, it is possible to make the visible light transmittance 70% or more.

[0134] In 100% by weight of the layer (first layer, second layer or third layer) containing the component X1, the content of the component X1 is preferably 0.001% by weight or more, more preferably 0.005% by weight or more, even more preferably 0.01% by weight or more, and particularly preferably 0.02% by weight or more. In 100% by weight of the layer (first layer, second layer or third layer) containing the component X1, the content of the component X1 is preferably 0.2% by weight or less, more preferably 0.1% by weight or less, even more preferably 0.05% by weight or less, and particularly preferably 0.04% by weight or less. When the content of the component X1 is the above lower limit or more and the above upper limit or less, the heat shielding property is sufficiently high and the visible light transmittance is sufficiently high. For example, it is possible to make the visible light transmittance 70% or more.

[0135] In 100% by weight of the layer (first layer, second layer or third layer) containing the carbon black, the content of the carbon black is preferably 0.001% by weight or more, more preferably 0.005% by weight or more, even more preferably 0.01% by weight or more, and particularly preferably 0.02% by weight or more. In 100% by weight of the layer (first layer, second layer or third layer) containing the carbon black, the content of the carbon black is preferably 0.2% by weight or less, more preferably 0.1% by weight or less, even more preferably 0.05% by weight or less, and particularly preferably 0.04% by weight or less. When the content of the carbon black is the above lower limit or more and the above upper limit or less, the heat shielding property is sufficiently high and the visible light transmittance is sufficiently high. For example, it is possible to make the visible light transmittance 70% or more.

[0136] Heat shielding particles: The intermediate film preferably contains heat-shielding particles. The first layer (including a single-layer intermediate film) preferably contains the heat-shielding particles. The second layer preferably contains the heat-shielding particles. The third layer preferably contains the heat-shielding particles. It is also preferable that the second layer contains the heat-shielding particles, the third layer contains the heat-shielding particles, and both the second layer and the third layer are different layers that do not contain heat-shielding particles. The heat-shielding particles are a heat-shielding material. By using the heat-shielding particles, infrared rays (heat rays) can be effectively blocked. Only one type of the heat-shielding particles may be used, or two or more types may be used in combination.

[0137] By including the heat-shielding particles, it becomes easy to control the absolute value of the difference and the secondary resonance frequency within the preferred ranges, and the effects of the present invention can be exhibited even more effectively.

[0138] From the viewpoint of further enhancing the heat shielding property of the laminated glass, the heat shielding particles are more preferably metal oxide particles.The heat shielding particles are preferably particles formed of a metal oxide (metal oxide particles).

[0139] Infrared rays, which have wavelengths of 780 nm or more, longer than visible light, have a smaller amount of energy than ultraviolet rays. However, infrared rays have a large thermal effect, and when infrared rays are absorbed by a substance, they are released as heat. For this reason, infrared rays are generally called heat rays. By using the above heat-shielding particles, infrared rays (heat rays) can be effectively blocked. Note that heat-shielding particles refer to particles that can absorb infrared rays.

[0140] Specific examples of the heat shielding particles include metal oxide particles such as aluminum-doped tin oxide particles, indium-doped tin oxide particles, antimony-doped tin oxide particles (ATO particles), gallium-doped zinc oxide particles (GZO particles), indium-doped zinc oxide particles (IZO particles), aluminum-doped zinc oxide particles (AZO particles), niobium-doped titanium oxide particles, sodium-doped tungsten oxide particles, cesium-doped tungsten oxide particles, thallium-doped tungsten oxide particles, rubidium-doped tungsten oxide particles, tin-doped indium oxide particles (ITO particles), tin-doped zinc oxide particles, and silicon-doped zinc oxide particles, as well as lanthanum hexaboride (LaB6) particles. Heat shielding particles other than these may also be used. Metal oxide particles are preferred because of their high heat ray shielding function, and ATO particles, GZO particles, IZO particles, ITO particles, or tungsten oxide particles are more preferred, with ITO particles or tungsten oxide particles being particularly preferred. In particular, tin-doped indium oxide particles (ITO particles) are preferred because they have a high heat ray shielding function and are easily available, and tungsten oxide particles are also preferred.

[0141] From the viewpoint of further improving the heat insulating property of the laminated glass, the tungsten oxide particles are preferably metal-doped tungsten oxide particles. The "tungsten oxide particles" include metal-doped tungsten oxide particles. Specific examples of the metal-doped tungsten oxide particles include sodium-doped tungsten oxide particles, cesium-doped tungsten oxide particles, thallium-doped tungsten oxide particles, and rubidium-doped tungsten oxide particles.

[0142] From the viewpoint of further increasing the heat insulating property of the laminated glass, cesium-doped tungsten oxide particles are particularly preferred. From the viewpoint of further increasing the heat insulating property of the laminated glass, the cesium-doped tungsten oxide particles are represented by the formula: Cs 0.33 Tungsten oxide particles represented by WO3 are preferred.

[0143] The average particle size of the heat shielding particles is preferably 0.01 μm or more, more preferably 0.02 μm or more, and preferably 0.1 μm or less, more preferably 0.05 μm or less. When the average particle size is equal to or more than the lower limit, the heat shielding properties are sufficiently high. When the average particle size is equal to or less than the upper limit, the dispersibility of the heat shielding particles is high.

[0144] The "average particle size" refers to the volume average particle size. The average particle size can be measured using a particle size distribution measuring device (manufactured by Nikkiso Co., Ltd., "UPA-EX150") or the like.

[0145] From the viewpoint of further improving the heat shielding property of the laminated glass, it is preferable that the second layer contains the heat shielding particles and component X, and the third layer contains the heat shielding particles and component X.

[0146] In 100% by weight of the layer (first layer, second layer or third layer) containing the heat shielding particles, the content of the heat shielding particles is preferably 0.01% by weight or more, more preferably 0.1% by weight or more, even more preferably 1% by weight or more, and particularly preferably 1.5% by weight or more. In 100% by weight of the layer (first layer, second layer or third layer) containing the heat shielding particles, the content of the heat shielding particles is preferably 6% by weight or less, more preferably 5.5% by weight or less, even more preferably 4% by weight or less, particularly preferably 3.5% by weight or less, and most preferably 3% by weight or less. When the content of the heat shielding particles is equal to or more than the lower limit and equal to or less than the upper limit, the heat shielding property is sufficiently high and the visible light transmittance is sufficiently high.

[0147] (Coloring agent) The intermediate film preferably contains a coloring agent. By coloring the intermediate film with a coloring agent, it is possible to improve the design and privacy protection. In addition, by coloring the intermediate film with a coloring agent, it is possible to further improve the heat shielding performance and reduce the solar radiation transmittance. The coloring agent may be used alone or in combination of two or more kinds. Note that the coloring agent may also correspond to the above-mentioned heat shielding material.

[0148] From the viewpoint of effectively suppressing excessive color unevenness, the first layer (including a single-layer interlayer film) preferably contains a colorant. The first layer is preferably a colored layer. From the viewpoint of effectively suppressing excessive color unevenness, the intermediate layer of the interlayer film preferably contains a colorant, and is preferably a colored layer. When the first layer contains a colorant, the second layer may or may not contain a colorant. When the first layer is a colored layer, the second layer may or may not be a colored layer. When the first layer contains a colorant, the third layer may or may not contain a colorant. When the first layer is a colored layer, the third layer may or may not be a colored layer. The surface layer of the interlayer film may or may not contain a colorant, and may or may not be a colored layer.

[0149] From the viewpoint of further increasing the heat shielding property and decreasing the solar radiation transmittance, the second layer preferably contains a colorant, and the third layer preferably contains a colorant. From the viewpoint of further increasing the heat shielding property and decreasing the solar radiation transmittance, the second layer is preferably a colored layer, and the third layer is preferably a colored layer. In these cases, the first layer may or may not contain a colorant, and may or may not be a colored layer.

[0150] The colorant includes pigments and dyes.

[0151] Whether a colorant is a dye or a pigment can be determined from the classification according to the color index.

[0152] In this specification, for colorants and the like not listed in the color index, "pigment" and "dye" may be defined as follows. A polyvinyl butyral resin (polyvinyl alcohol polymerization degree 1700, hydroxyl group content 30 mol%, acetylation degree 1 mol%, butyralization degree 69 mol%) is prepared. 100 parts by weight of this polyvinyl butyral resin, 40 parts by weight of triethylene glycol di-2-ethylhexanoate (3GO), and a colorant with a content of 0.015% by weight relative to the total amount of the polyvinyl butyral resin, 3GO, and colorant (100% by weight) are kneaded and extruded to obtain a resin film (single layer) with a thickness of 760 μm. When a laminated glass is produced using this resin film and two pieces of clear glass (thickness 2.5 mm) with a visible light transmittance of 90% measured in accordance with JIS R3106:1998, the colorant that gives the haze value of the resulting laminated glass of 0.35% or more is defined as a pigment. The colorant having a haze value of less than 0.35% is a dye.

[0153] The pigment may be an organic pigment or an inorganic pigment. The organic pigment may be an organic pigment having a metal atom or an organic pigment not having a metal atom. The pigment may be used alone or in combination of two or more kinds.

[0154] Examples of the organic pigment include a phthalocyanine compound, a quinacridone compound, an azo compound, a pentaphene compound, a dioxazine compound, a perylene compound, an indole compound, and a dioxazine compound.

[0155] The color tone of the organic pigment is preferably yellow, orange, red, violet, blue or green.

[0156] Examples of the inorganic pigment include carbon black, iron oxide, zinc oxide, and titanium oxide.

[0157] The intermediate film preferably contains, as the pigment, a phthalocyanine compound, a quinacrylonitrile compound, an azo compound, a pentaphene compound, a dioxazine compound, a perylene compound, an indole compound, or carbon black. The intermediate film may contain, as the pigment, a phthalocyanine compound, a quinacrylonitrile compound, a perylene compound, or an indole compound, or may contain carbon black.

[0158] Examples of the dye include pyrene-based dyes, aminoketone-based dyes, anthraquinone-based dyes, azo-based dyes, etc. The dyes may be used alone or in combination of two or more.

[0159] Examples of the pyrene-based dyes include Solvent Green 5 (CAS 79869-59-3) and Solvent Green 7 (CAS 6358-69-6).

[0160] Examples of the aminoketone dyes include Solvent Yellow 98 (CAS12671-74-8), Solvent Yellow 85 (CAS12271-01-1), Solvent Red 179 (CAS8910-94-5), and Solvent Red 135 (CAS71902-17-5).

[0161] Examples of the anthraquinone dyes include Solvent Yellow 163 (CAS13676091-0), Solvent Red 207 (CAS15958-69-6), Disperse Red 92 (CAS12236-11-2), Solvent Violet 13 (CAS81-48-1), Disperse Violet 31 (CAS6408-72-6), Solvent Blue 97 (CAS61969-44-6), Solvent Blue 45 (CAS37229-23-5), Solvent Blue 104 (CAS116-75-6) and Disperse Blue 214 (CAS104491-84-1).

[0162] Examples of the azo dyes include Solvent Yellow 30 (CAS 3321-10-4), Solvent Red 164 (CAS 70956-30-8), and Disperse Blue 146 (CAS 88650-91-3).

[0163] In 100% by weight of the colored layer (first layer, second layer or third layer) containing the coloring agent, the content of the coloring agent is preferably 0.0001% by weight or more, more preferably 0.0003% by weight or more, even more preferably 0.0005% by weight or more, and particularly preferably 0.0008% by weight or more. In 100% by weight of the colored layer (first layer, second layer or third layer) containing the coloring agent, the content of the coloring agent is preferably 3% by weight or less, more preferably 2% by weight or less, even more preferably 1% by weight or less, and particularly preferably 0.5% by weight or less. When the content of the coloring agent is the above lower limit or more and the above upper limit or less, it is possible to achieve good coloring and further improve the heat shielding property.

[0164] (Metal Salts) The interlayer preferably contains at least one metal salt (hereinafter, may be referred to as metal salt M) of an alkali metal salt and an alkaline earth metal salt. The first layer (including a single-layer interlayer) preferably contains the metal salt M. The second layer preferably contains the metal salt M. The third layer preferably contains the metal salt M. The alkaline earth metals refer to six metals, namely, Be, Mg, Ca, Sr, Ba, and Ra. The use of the metal salt M makes it easy to control the adhesion between the interlayer and a laminated glass member such as a glass plate, or the adhesion between each layer in the interlayer. Only one type of the metal salt M may be used, or two or more types may be used in combination.

[0165] The metal salt M preferably contains at least one metal selected from the group consisting of Li, Na, K, Rb, Cs, Mg, Ca, Sr and Ba. The metal salt contained in the interlayer film preferably contains at least one metal selected from the group consisting of K and Mg.

[0166] Moreover, the metal salt M is more preferably an alkali metal salt of an organic acid having 2 to 16 carbon atoms or an alkaline earth metal salt of an organic acid having 2 to 16 carbon atoms, and further preferably a magnesium salt of a carboxylate having 2 to 16 carbon atoms or a potassium salt of a carboxylate having 2 to 16 carbon atoms.

[0167] Examples of the magnesium salt of a carboxylate having 2 to 16 carbon atoms and the potassium salt of a carboxylate having 2 to 16 carbon atoms include magnesium acetate, potassium acetate, magnesium propionate, potassium propionate, magnesium 2-ethylbutyrate, potassium 2-ethylbutanoate, magnesium 2-ethylhexanoate, and potassium 2-ethylhexanoate.

[0168] The total content of Mg and K in the layer (first layer, second layer or third layer) containing the metal salt M is preferably 5 ppm or more, more preferably 10 ppm or more, even more preferably 20 ppm or more, and preferably 300 ppm or less, more preferably 250 ppm or less, and even more preferably 200 ppm or less. When the total content of Mg and K is equal to or more than the above lower limit and equal to or less than the above upper limit, the adhesion between the interlayer film and the glass plate or the adhesion between the layers in the interlayer film can be controlled more satisfactorily.

[0169] (UV protection agent) The interlayer film preferably contains an ultraviolet ray shielding agent. The first layer (including a single-layer interlayer film) preferably contains an ultraviolet ray shielding agent. The second layer preferably contains an ultraviolet ray shielding agent. The third layer preferably contains an ultraviolet ray shielding agent. By using an ultraviolet ray shielding agent, the visible light transmittance is more unlikely to decrease even when the interlayer film and the laminated glass are used for a long period of time. The ultraviolet ray shielding agent may be used alone or in combination of two or more kinds.

[0170] The ultraviolet shielding agent includes an ultraviolet absorbing agent. The ultraviolet shielding agent is preferably an ultraviolet absorbing agent.

[0171] Examples of the ultraviolet ray shielding agent include ultraviolet ray shielding agents containing metal atoms, ultraviolet ray shielding agents containing metal oxides, ultraviolet ray shielding agents having a benzotriazole structure (benzotriazole compounds), ultraviolet ray shielding agents having a benzophenone structure (benzophenone compounds), ultraviolet ray shielding agents having a triazine structure (triazine compounds), ultraviolet ray shielding agents having a malonic acid ester structure (malonic acid ester compounds), ultraviolet ray shielding agents having an oxalic acid anilide structure (oxalic acid anilide compounds), and ultraviolet ray shielding agents having a benzoate structure (benzoate compounds).

[0172] Examples of the ultraviolet shielding agent containing the metal atom include platinum particles, platinum particles whose surfaces are coated with silica, palladium particles, and palladium particles whose surfaces are coated with silica, etc. It is preferable that the ultraviolet shielding agent is not a heat shielding particle.

[0173] The ultraviolet shielding agent is preferably an ultraviolet shielding agent having a benzotriazole structure, an ultraviolet shielding agent having a benzophenone structure, an ultraviolet shielding agent having a triazine structure, or an ultraviolet shielding agent having a benzoate structure. The ultraviolet shielding agent is more preferably an ultraviolet shielding agent having a benzotriazole structure or an ultraviolet shielding agent having a benzophenone structure, and further preferably an ultraviolet shielding agent having a benzotriazole structure.

[0174] Examples of the ultraviolet shielding agent containing the metal oxide include zinc oxide, titanium oxide, and cerium oxide. Furthermore, the ultraviolet shielding agent containing the metal oxide may be surface-coated. Examples of the surface-coating material of the ultraviolet shielding agent containing the metal oxide include insulating metal oxides, hydrolyzable organic silicon compounds, and silicone compounds.

[0175] The insulating metal oxide includes silica, alumina, zirconia, etc. The insulating metal oxide has a band gap energy of, for example, 5.0 eV or more.

[0176] Examples of the ultraviolet shielding agent having the benzotriazole structure include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole (BASF's "Tinuvin P"), 2-(2'-hydroxy-3',5'-di-t-butylphenyl)benzotriazole (BASF's "Tinuvin 320"), 2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole (BASF's "Tinuvin 326"), and 2-(2'-hydroxy-3',5'-di-amylphenyl)benzotriazole (BASF's "Tinuvin 328"), etc. Since the ultraviolet shielding agent has excellent ultraviolet shielding performance, it is preferable that the ultraviolet shielding agent has a benzotriazole structure containing a halogen atom, and more preferably has a benzotriazole structure containing a chlorine atom.

[0177] Examples of the ultraviolet screening agent having a benzophenone structure include octabenzone ("Chimassorb 81" manufactured by BASF).

[0178] Examples of the ultraviolet screening agent having a triazine structure include "LA-F70" manufactured by ADEKA Corporation and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol ("Tinuvin 1577FF" manufactured by BASF).

[0179] Examples of the ultraviolet screening agent having a malonic acid ester structure include dimethyl 2-(p-methoxybenzylidene)malonate, tetraethyl-2,2-(1,4-phenylenedimethylidene)bismalonate, and 2-(p-methoxybenzylidene)-bis(1,2,2,6,6-pentamethyl-4-piperidinyl)malonate.

[0180] Commercially available ultraviolet screening agents having the above malonic acid ester structure include Hostavin B-CAP, Hostavin PR-25, and Hostavin PR-31 (all manufactured by Clariant).

[0181] Examples of ultraviolet screening agents having the above-mentioned oxalic acid anilide structure include oxalic acid diamides having an aryl group substituted on the nitrogen atom, such as N-(2-ethylphenyl)-N'-(2-ethoxy-5-t-butylphenyl)oxalic acid diamide, N-(2-ethylphenyl)-N'-(2-ethoxy-phenyl)oxalic acid diamide, and 2-ethyl-2'-ethoxy-oxalanilide ("Sanduvor VSU" manufactured by Clariant).

[0182] Examples of the ultraviolet screening agent having a benzoate structure include 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate ("Tinuvin 120" manufactured by BASF).

[0183] The content of the ultraviolet shielding agent in 100% by weight of the layer (first layer, second layer or third layer) containing the ultraviolet shielding agent is preferably 0.1% by weight or more, more preferably 0.2% by weight or more, even more preferably 0.3% by weight or more, and particularly preferably 0.5% by weight or more. The content of the ultraviolet shielding agent in 100% by weight of the layer (first layer, second layer or third layer) containing the ultraviolet shielding agent is preferably 2.5% by weight or less, more preferably 2% by weight or less, even more preferably 1% by weight or less, and particularly preferably 0.8% by weight or less. When the content of the ultraviolet shielding agent is the above lower limit or more and the above upper limit or less, the decrease in visible light transmittance after a period of time can be further suppressed. In particular, when the content of the ultraviolet shielding agent is 0.2% by weight or more in 100% by weight of the layer containing the ultraviolet shielding agent, the decrease in visible light transmittance of the interlayer film and the laminated glass after a period of time can be significantly suppressed.

[0184] (Antioxidants) The interlayer film preferably contains an antioxidant. The first layer (including a single-layer interlayer film) preferably contains an antioxidant. The second layer preferably contains an antioxidant. The third layer preferably contains an antioxidant. Only one type of antioxidant may be used, or two or more types may be used in combination.

[0185] The antioxidants include phenol-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants. The phenol-based antioxidants are antioxidants having a phenol skeleton. The sulfur-based antioxidants are antioxidants containing sulfur atoms. The phosphorus-based antioxidants are antioxidants containing phosphorus atoms.

[0186] The antioxidant is preferably a phenol-based antioxidant or a phosphorus-based antioxidant.

[0187] The phenol-based antioxidants include 2,6-di-t-butyl-p-cresol (BHT), butyl hydroxyanisole (BHA), 2,6-di-t-butyl-4-ethylphenol, stearyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2'-methylenebis-(4-methyl-6-butylphenol), 2,2'-methylenebis-(4-ethyl-6-t-butylphenol), 4,4'-butylidene-bis-(3-methyl-6-t-butylphenol), 1,1,3-tris-(2-methyl-hydroxy-5- t-butylphenyl)butane, tetrakis[methylene-3-(3',5'-butyl-4-hydroxyphenyl)propionate]methane, 1,3,3-tris-(2-methyl-4-hydroxy-5-t-butylphenol)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis(3,3'-t-butylphenol)butyric acid glycol ester, and bis(3-t-butyl-4-hydroxy-5-methylbenzenepropanoic acid)ethylenebis(oxyethylene). One or more of these antioxidants are preferably used.

[0188] Examples of the phosphorus-based antioxidant include tridecyl phosphite, tris(tridecyl)phosphite, triphenyl phosphite, trinonylphenyl phosphite, bis(tridecyl)pentaerythritol diphosphite, bis(decyl)pentaerythritol diphosphite, tris(2,4-di-t-butylphenyl)phosphite, bis(2,4-di-t-butyl-6-methylphenyl)ethyl ester phosphorous acid, and 2,2'-methylenebis(4,6-di-t-butyl-1-phenyloxy)(2-ethylhexyloxy)phosphorus, etc. One or more of these antioxidants are preferably used.

[0189] Commercially available examples of the antioxidant include "IRGANOX 245" manufactured by BASF, "IRGAFOS 168" manufactured by BASF, "IRGAFOS 38" manufactured by BASF, "Sumilizer BHT" manufactured by Sumitomo Chemical Co., Ltd., "H-BHT" manufactured by Sakai Chemical Industry Co., Ltd., and "IRGANOX 1010" manufactured by BASF.

[0190] In order to maintain the high visible light transmittance of the interlayer film and laminated glass for a long period of time, the content of the antioxidant is preferably 0.1 wt% or more in 100 wt% of the layer containing the antioxidant (the first layer, the second layer, or the third layer). In addition, since the effect of adding the antioxidant becomes saturated, the content of the antioxidant is preferably 2 wt% or less in 100 wt% of the layer containing the antioxidant.

[0191] (Other ingredients) The intermediate film, the first layer, the second layer and the third layer may each contain additives such as a coupling agent, a dispersant, a surfactant, a flame retardant, an antistatic agent, an adhesion modifier other than a metal salt, a moisture resistant agent, a fluorescent brightening agent, an infrared absorbing agent, etc. These additives may be used alone or in combination of two or more kinds.

[0192] (Infrared reflective layer) The intermediate film may include an infrared reflective layer. The infrared reflective layer is a layer that reflects infrared rays. The infrared reflective layer is not particularly limited as long as it has the ability to reflect infrared rays.

[0193] The infrared reflective layer may be disposed between the first layer and the second layer, or between the first layer and the third layer, and the second layer or the third layer may be the infrared reflective layer.

[0194] The infrared reflective layer may be disposed on the second layer on a surface opposite to the first layer, or on the third layer on a surface opposite to the first layer. In this case, the intermediate film may have a fourth layer disposed on the infrared reflective layer on a surface opposite to the second layer, or on the infrared reflective layer on a surface opposite to the third layer.

[0195] Examples of the infrared reflective layer include a resin film with a metal foil, a multilayer laminate film in which a metal layer and a dielectric layer are formed on a resin layer, a film containing graphite, a multilayer resin film, a liquid crystal film, etc. These films have the ability to reflect infrared rays.

[0196] The infrared reflective layer is preferably a resin film with metal foil, a film containing graphite, a multilayer resin film, or a liquid crystal film, and more preferably a resin film with metal foil, a multilayer resin film, or a liquid crystal film. These films have excellent infrared reflective properties. Therefore, by using these films, a laminated glass can be obtained that has higher heat shielding properties and can maintain a high visible light transmittance for a longer period of time.

[0197] The infrared reflective layer is more preferably a multilayer resin film or a liquid crystal film, which is more transparent to electromagnetic waves than a metal foil-coated resin film, and therefore allows the use of laminated glass without interfering with the use of electronic devices in the vehicle.

[0198] The resin film with metal foil includes a resin film and a metal foil laminated on the outer surface of the resin film. Examples of materials for the resin film include polyethylene terephthalate resin, polyethylene naphthalate resin, polyvinyl acetal resin, ethylene-vinyl acetate copolymer resin, ethylene-acrylic acid copolymer resin, polyurethane resin, polyvinyl alcohol resin, polyolefin resin, polyvinyl chloride resin, and polyimide resin. Examples of materials for the metal foil include aluminum, copper, silver, gold, palladium, and alloys containing these.

[0199] The multilayer laminate film in which a metal layer and a dielectric layer are formed on the resin layer is a multilayer laminate film in which metal layers and dielectric layers are alternately laminated on a resin layer (resin film) in any number of layers. In the multilayer laminate film in which a metal layer and a dielectric layer are formed on the resin layer, it is preferable that all of the metal layers and dielectric layers are alternately laminated, but there may be a structural portion in which some of the layers are not alternately laminated, such as metal layer / dielectric layer / metal layer / dielectric layer / metal layer / metal layer / dielectric layer / metal layer.

[0200] The material of the resin layer (resin film) in the multilayer laminate film may be the same as the material of the resin film in the resin film with metal foil. The material of the resin layer (resin film) in the multilayer laminate film may be polyethylene, polypropylene, polylactic acid, poly(4-methylpentene-1), polyvinylidene fluoride, cyclic polyolefin, polymethyl methacrylate, polyvinyl chloride, polyvinyl alcohol, polyamides such as nylon 6, 11, 12, 66, polystyrene, polycarbonate, polyethylene terephthalate, polyethylene naphthalate, polyester, polyphenylene sulfide, and polyetherimide. The material of the metal layer in the multilayer laminate film may be the same as the material of the metal foil in the resin film with metal foil. A coating layer of metal or mixed oxide of metals may be applied to both sides or one side of the metal layer. The material of the coating layer may be ZnO, Al2O3, Ga2O3, InO3, MgO, Ti, NiCr, and Cu.

[0201] The material of the dielectric layer in the multi-layer laminate film may be, for example, indium oxide.

[0202] The multilayer resin film is a laminated film in which a plurality of resin films are laminated. Examples of materials for the multilayer resin film include materials similar to those for the resin layers (resin films) in the multilayer laminate film. The number of resin films laminated in the multilayer resin film is 2 or more, may be 3 or more, or may be 5 or more. The number of resin films laminated in the multilayer resin film may be 1000 or less, may be 100 or less, or may be 50 or less.

[0203] The multilayer resin film may be a multilayer resin film in which two or more types of thermoplastic resin layers having different optical properties (refractive indexes) are laminated alternately or randomly in any number of layers. Such a multilayer resin film is configured to obtain a desired infrared reflection performance.

[0204] The liquid crystal film may be a film in which any number of cholesteric liquid crystal layers that reflect light of any wavelength are laminated together, and such a liquid crystal film is configured to provide a desired infrared reflecting performance.

[0205] The laminate of the infrared reflective layer and the second laminated glass member may be a second laminated glass member with a metal foil, in which case the metal foil functions as the infrared reflective layer.

[0206] Since the infrared reflective layer has excellent infrared reflecting performance, it is preferable that the infrared reflective layer has an infrared transmittance of 40% or less at at least one wavelength in the range of 800 nm to 2000 nm. The infrared transmittance of the infrared reflective layer used in the examples described later satisfies the above-mentioned preferable conditions. At at least one wavelength in the range of 800 nm to 2000 nm, the infrared transmittance is more preferably 30% or less, and even more preferably 20% or less.

[0207] Specifically, the transmittance of the infrared reflective layer at each wavelength in the range of 800 nm to 2000 nm is measured as follows. A single infrared reflective layer is prepared. Using a spectrophotometer (Hitachi High-Tech Corporation's "U-4100"), the spectral transmittance of the infrared reflective layer at each wavelength in the range of 800 nm to 2000 nm is measured in accordance with JIS R3106:1998.

[0208] From the viewpoint of effectively enhancing the heat shielding property of the laminated glass, the infrared reflectance of the infrared reflective layer at wavelengths of 800 nm to 1200 nm is preferably 20% or more, more preferably 22% or more, and even more preferably 25% or more.

[0209] Specifically, the infrared reflectance of the infrared reflective layer at wavelengths of 800 nm to 1200 nm is measured as follows. Using a spectrophotometer (Hitachi High-Technologies Corporation's "U-4100"), the reflectance of the infrared reflective layer at each wavelength of 800 nm to 1200 nm is obtained in accordance with JIS R3106:1998. Of the reflectances at each wavelength, it is preferable that the lowest reflectance is equal to or greater than the lower limit.

[0210] From the viewpoint of effectively increasing the transparency of the laminated glass, the infrared reflective layer preferably has a visible light transmittance at a wavelength of 380 nm to 780 nm of 20% or more, more preferably 50% or more, and even more preferably 70% or more.

[0211] The visible light transmittance is measured at wavelengths of 380 nm to 780 nm using a spectrophotometer (Hitachi High-Technologies Corporation, "U-4100") in accordance with JIS R3211:1998.

[0212] (Other details of interlayer film for laminated glass) The thickness of the interlayer film is not particularly limited. From the viewpoint of practical use and of sufficiently increasing the penetration resistance and bending rigidity of the laminated glass, the average thickness of the interlayer film is preferably 0.1 mm or more, more preferably 0.25 mm or more, and preferably 3 mm or less, more preferably 1.5 mm or less. When the average thickness of the interlayer film is equal to or more than the lower limit, the penetration resistance and bending rigidity of the laminated glass are further increased. When the average thickness of the interlayer film is equal to or less than the upper limit, the transparency of the interlayer film is further improved.

[0213] The average thickness of the intermediate film is T. The average thickness of the first layer is preferably 0.035T or more, more preferably 0.0625T or more, even more preferably 0.1T or more, preferably 0.4T or less, more preferably 0.375T or less, even more preferably 0.25T or less, and particularly preferably 0.15T or less. When the average thickness of the first layer is 0.4T or less, the bending rigidity is further improved. In addition, when the average thickness of the first layer is equal to or more than the lower limit and equal to or less than the upper limit, it becomes easy to control the absolute value of the difference and the secondary resonance frequency within the preferred ranges, and the effects of the present invention can be more effectively exhibited.

[0214] The average thickness of each of the second layer and the third layer is preferably 0.3T or more, more preferably 0.3125T or more, even more preferably 0.375T or more, preferably 0.97T or less, more preferably 0.9375T or less, and even more preferably 0.9T or less. The average thickness of each of the second layer and the third layer may be 0.46875T or less, or may be 0.45T or less. In addition, when the average thickness of each of the second layer and the third layer is not less than the lower limit and not more than the upper limit, the bending rigidity of the laminated glass is further increased. In addition, when the average thickness of each of the second layer and the third layer is not less than the lower limit and not more than the upper limit, it becomes easy to control the absolute value of the difference and the secondary resonance frequency within the preferred range, and the effect of the present invention can be more effectively exhibited.

[0215] The sum of the average thickness of the second layer and the average thickness of the third layer is preferably 0.625 T or more, more preferably 0.75 T or more, even more preferably 0.85 T or more, and preferably 0.97 T or less, more preferably 0.9375 T or less, and even more preferably 0.9 T or less. When the sum is equal to or greater than the lower limit and equal to or less than the upper limit, the bending rigidity of the laminated glass is further increased. When the sum is equal to or greater than the lower limit and equal to or less than the upper limit, it becomes easy to control the absolute value of the difference and the secondary resonance frequency within the preferred ranges, and the effects of the present invention can be more effectively exhibited.

[0216] The intermediate film has one end and the other end opposite to the one end. The one end and the other end are opposite ends of the intermediate film. The intermediate film may be an intermediate film having a uniform thickness, or an intermediate film having a varying thickness. The intermediate film may be an intermediate film having the same thickness at the one end and the other end, or an intermediate film having a thickness at the other end greater than the thickness at the one end. The cross-sectional shape of the intermediate film may be rectangular or wedge-shaped.

[0217] The distance between one end and the other end of the intermediate film is L. The intermediate film preferably has a minimum thickness in a region from 0L to 0.4L from the one end to the other end, and a maximum thickness in a region from 0L to 0.4L from the other end to the one end. It is more preferable that the intermediate film has a minimum thickness in a region from 0L to 0.3L from the one end to the other end, and a maximum thickness in a region from 0L to 0.3L from the other end to the one end. It is even more preferable that the intermediate film has a minimum thickness in a region from 0L to 0.2L from the one end to the other end, and a maximum thickness in a region from 0L to 0.2L from the other end to the one end. It is even more preferable that the intermediate film has a minimum thickness in a region from 0L to 0.1L from the one end to the other end, and a maximum thickness in a region from 0L to 0.1L from the other end to the one end. It is particularly preferred that the interlayer has a minimum thickness at one end and a maximum thickness at the other end.

[0218] The interlayer film may have a uniform thickness portion. The uniform thickness portion refers to a portion in which the thickness does not change by more than 10 μm within a distance range of 10 cm in the direction connecting the one end and the other end of the interlayer film. Accordingly, the uniform thickness portion refers to a portion in which the thickness does not change by more than 10 μm within a distance range of 10 cm in the direction connecting the one end and the other end of the interlayer film. Specifically, the uniform thickness portion refers to a portion in which the thickness does not change at all in the direction connecting the one end and the other end of the interlayer film, or a portion in which the thickness changes by 10 μm or less within a distance range of 10 cm in the direction connecting the one end and the other end of the interlayer film.

[0219] The maximum thickness of the interlayer is preferably 0.1 mm or more, more preferably 0.25 mm or more, even more preferably 0.5 mm or more, particularly preferably 0.8 mm or more, and is preferably 3.8 mm or less, more preferably 2 mm or less, and even more preferably 1.5 mm or less.

[0220] The distance L between one end and the other end of the interlayer is preferably 3 m or less, more preferably 2 m or less, particularly preferably 1.5 m or less, and is preferably 0.5 m or more, more preferably 0.8 m or more, particularly preferably 1 m or more.

[0221] The interlayer film may be wound into a roll of the interlayer film. The roll may include a winding core and the interlayer film wound around the outer periphery of the winding core.

[0222] The method for producing the interlayer film according to the present invention is not particularly limited. In the case of a single-layer interlayer film, the method for producing the interlayer film according to the present invention includes a method of extruding a resin composition using an extruder. In the case of a multi-layer interlayer film, the method for producing the interlayer film according to the present invention includes, for example, a method of forming each layer using each resin composition for forming each layer, and then laminating the obtained layers, as well as a method of laminating each layer by co-extruding each resin composition for forming each layer using an extruder. The extrusion molding method is preferable because it is suitable for continuous production.

[0223] In view of the excellent manufacturing efficiency of the interlayer film, it is preferable that the second layer and the third layer contain the same polyvinyl acetal resin. In view of the excellent manufacturing efficiency of the interlayer film, it is more preferable that the second layer and the third layer contain the same polyvinyl acetal resin and the same plasticizer. In view of the excellent manufacturing efficiency of the interlayer film, it is even more preferable that the second layer and the third layer are formed from the same resin composition.

[0224] The intermediate film preferably has an uneven shape on at least one of both surfaces. The intermediate film more preferably has an uneven shape on both surfaces. The method for forming the uneven shape is not particularly limited, and examples thereof include a lip embossing method, an embossing roll method, a calendar roll method, and a profile extrusion method. The embossing roll method is preferred because it can form a large number of uneven embossments that are quantitatively uniform uneven patterns.

[0225] (Laminated glass) The laminated glass according to the present invention includes a first laminated glass member, a second laminated glass member, and the above-mentioned interlayer film for laminated glass. In the laminated glass according to the present invention, the above-mentioned interlayer film for laminated glass is disposed between the first laminated glass member and the second laminated glass member.

[0226] The laminated glass according to the present invention comprises a first laminated glass member, a second laminated glass member, and an interlayer film for laminated glass having a one-layer structure or a two or more layer structure. In the laminated glass according to the present invention, the interlayer film for laminated glass is disposed between the first laminated glass member and the second laminated glass member. In the laminated glass according to the present invention, the absolute value of the difference between the secondary resonance frequency of the laminated glass before irradiation with xenon light and the secondary resonance frequency of the laminated glass after irradiation with xenon light, which is determined by the xenon light irradiation test described below, is preferably 60 Hz or more. The laminated glass according to the present invention preferably has a loss factor at 20°C of 0.25 or more and a solar transmittance of 50% or less.

[0227] Xenon light irradiation test: The secondary resonance frequency of the laminated glass at 10°C is determined using the central excitation method in accordance with ISO16940. Under the condition of 10°C, the laminated glass is exposed to 190W / m 2 The laminated glass is irradiated with xenon light for 30 minutes. The secondary resonance frequency of the laminated glass after irradiation with xenon light is determined using the central excitation method in accordance with ISO 16940. The absolute value of the difference between the secondary resonance frequency of the laminated glass before irradiation with xenon light and the secondary resonance frequency of the laminated glass after irradiation with xenon light is calculated.

[0228] More specifically, the xenon light irradiation test of the laminated glass is carried out as follows.

[0229] (1) The secondary resonance frequency of the above laminated glass at 10°C is determined by the central excitation method in accordance with ISO 16940.

[0230] (2) Under windless conditions at 10°C, the above laminated glass is subjected to a temperature of 190 W / m 2 The laminated glass is irradiated with xenon light of 190 W / m for 30 minutes. An example of an apparatus for irradiating xenon light is a solar simulator apparatus (e.g., "HAL-320" manufactured by Asahi Spectroscopy). An example of an apparatus for measuring illuminance is an illuminometer (e.g., "KEYSIGHT U1252B, Sensor EKO Pyranometer ML-01" manufactured by Keysight Technologies). The distance between the main surface of the laminated glass and the light source (e.g., xenon lamp) is set at 100 mm for an illuminance of 190 W / m. 2 There is no particular limitation as long as the arrangement is such that

[0231] (3) The secondary resonance frequency of the laminated glass after irradiation with xenon light is determined by a central excitation method in accordance with ISO 16940. In this case, the secondary resonance frequency is determined within 2 minutes (preferably within 1 minute) after irradiation with xenon light.

[0232] (4) Calculate the absolute value of the difference between the secondary resonance frequency of the laminated glass before irradiation with xenon light obtained in (1) above and the secondary resonance frequency of the laminated glass after irradiation with xenon light obtained in (3) above.

[0233] Since the laminated glass according to the present invention has the above-mentioned configuration, it is possible to improve the sound insulation in a relatively low temperature range.

[0234] The absolute value of the difference between the secondary resonance frequency of the laminated glass before irradiation with xenon light and the secondary resonance frequency of the laminated glass after irradiation with xenon light is preferably 75 Hz or more, more preferably 100 Hz or more, preferably 200 Hz or less, more preferably 120 Hz or less. When the absolute value of the difference is equal to or more than the above lower limit and equal to or less than the above upper limit, the effects of the present invention can be more effectively exhibited.

[0235] From the viewpoint of exerting the effects of the present invention more effectively, the secondary resonance frequency of the laminated glass at 10° C. before irradiation with xenon light is preferably 900 Hz or more, more preferably 910 Hz or more, even more preferably 925 Hz or more, and is preferably 1000 Hz or less, more preferably 965 Hz or less.

[0236] From the viewpoint of more effectively exerting the effects of the present invention, the secondary resonance frequency of the laminated glass after irradiation with xenon light is preferably 750 Hz or more, more preferably 815 Hz or more, and preferably 850 Hz or less, more preferably 843 Hz or less.

[0237] To more effectively exert the effects of the present invention, the loss factor of the laminated glass at 20° C. is preferably 0.26 or more, more preferably 0.28 or more, and is preferably 0.5 or less, more preferably 0.4 or less.

[0238] The loss factor of the above laminated glass at 20°C is measured by the central vibration method in accordance with ISO16940.

[0239] From the viewpoint of more effectively exerting the effects of the present invention and more effectively improving the heat shielding property, the solar transmittance of the laminated glass is preferably 10% or more, more preferably 15% or more, and is preferably 48% or less, more preferably 44% or less.

[0240] The solar transmittance of the laminated glass is measured using a spectrophotometer (for example, "U-4100" manufactured by Hitachi High-Technologies Corporation) in accordance with JIS R3106:1998.

[0241] FIG. 3 is a cross-sectional view that illustrates an example of laminated glass using the interlayer film for laminated glass shown in FIG.

[0242] The laminated glass 31 shown in Fig. 3 includes a first laminated glass member 21, a second laminated glass member 22, and an interlayer film 11. The interlayer film 11 is disposed and sandwiched between the first laminated glass member 21 and the second laminated glass member 22.

[0243] A first laminated glass member 21 is laminated on a first surface 11a of the interlayer film 11. A second laminated glass member 22 is laminated on a second surface 11b opposite to the first surface 11a of the interlayer film 11. The first laminated glass member 21 is laminated on an outer surface 2a of the second layer 2. The second laminated glass member 22 is laminated on an outer surface 3a of the third layer 3.

[0244] FIG. 4 is a cross-sectional view that illustrates an example of laminated glass using the interlayer film for laminated glass shown in FIG.

[0245] 4 includes a first laminated glass member 21, a second laminated glass member 22, and an interlayer film 11A. The interlayer film 11A is disposed and sandwiched between the first laminated glass member 21 and the second laminated glass member 22.

[0246] A first laminated glass member 21 is laminated on a first surface 11a of the interlayer film 11A. A second laminated glass member 22 is laminated on a second surface 11b of the interlayer film 11A opposite to the first surface 11a.

[0247] As described above, the laminated glass according to the present invention includes a first laminated glass component, a second laminated glass component, and an interlayer film, and the interlayer film is the interlayer film for laminated glass according to the present invention. In the laminated glass according to the present invention, the interlayer film is disposed between the first laminated glass component and the second laminated glass component.

[0248] The first laminated glass member is preferably a first glass plate, and the second laminated glass member is preferably a second glass plate.

[0249] Examples of the first and second laminated glass members include glass plates and PET (polyethylene terephthalate) films. The laminated glass includes not only a laminated glass having an intermediate film sandwiched between two glass plates, but also a laminated glass having an intermediate film sandwiched between a glass plate and a PET film or the like. The laminated glass is a laminate including glass plates, and preferably includes at least one glass plate. It is preferable that the first and second laminated glass members are glass plates or PET (polyethylene terephthalate) films, respectively, and that the laminated glass includes at least one glass plate as the first and second laminated glass members. It is particularly preferable that both the first and second laminated glass members are glass plates.

[0250] The glass plate includes inorganic glass and organic glass. The inorganic glass includes float plate glass, heat absorbing plate glass, heat reflecting plate glass, polished plate glass, patterned plate glass, lined plate glass, green glass, etc. The organic glass is a synthetic resin glass that replaces inorganic glass. The organic glass includes polycarbonate plate and poly(meth)acrylic resin plate, etc. The poly(meth)acrylic resin plate includes polymethyl(meth)acrylate plate, etc.

[0251] The first laminated glass member and the second laminated glass member are preferably green glass or heat absorbing plate glass, respectively. The first laminated glass member is preferably green glass or heat absorbing plate glass, more preferably green glass, because it has a high infrared transmittance and further improves the heat shielding properties of the laminated glass. The second laminated glass member is preferably green glass or heat absorbing plate glass, more preferably green glass, because it has a low infrared transmittance and further improves the heat shielding properties of the laminated glass. The first laminated glass member is preferably clear glass, and the second laminated glass member is preferably heat absorbing plate glass. The heat absorbing plate glass is a heat absorbing plate glass conforming to JIS R3208.

[0252] The thickness of each of the first laminated glass member and the second laminated glass member is preferably 1 mm or more, preferably 5 mm or less, and more preferably 3 mm or less. When the first and second laminated glass members are glass plates, the thickness of the glass plates is preferably 0.5 mm or more, more preferably 0.7 mm or more, preferably 5 mm or less, and more preferably 3 mm or less. When the first and second laminated glass members are PET films, the thickness of the PET films is preferably 0.03 mm or more, and preferably 0.5 mm or less.

[0253] The method for producing the laminated glass is not particularly limited. For example, an interlayer film is sandwiched between the first laminated glass member and the second laminated glass member, and the interlayer film is removed by passing the first laminated glass member and the second laminated glass member through a pressing roll or by placing the glass member in a rubber bag and sucking the glass member under reduced pressure. Then, the glass member is pre-bonded at about 70°C to 110°C to obtain a laminate. Next, the laminate is placed in an autoclave or pressed to be pressure-bonded at about 120°C to 150°C and a pressure of 1MPa to 1.5MPa. In this manner, a laminated glass can be obtained. When producing the laminated glass, each layer in the interlayer film may be laminated.

[0254] The interlayer film and the laminated glass can be used in automobiles, railroad vehicles, aircraft, ships, buildings, etc. The interlayer film and the laminated glass can be used for purposes other than these. The interlayer film and the laminated glass are preferably interlayer films and laminated glasses for vehicles or buildings, and more preferably interlayer films and laminated glasses for vehicles. The interlayer film and the laminated glass can be used for automobile front glass, side glass, rear glass, roof glass, etc. The interlayer film and the laminated glass are preferably used in automobiles. The interlayer film is used to obtain laminated glass for automobiles.

[0255] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0256] In the polyvinyl acetal resin used, n-butyl aldehyde with 4 carbon atoms was used for acetalization. For the polyvinyl acetal resin, the degree of acetalization (degree of butyralization), the degree of acetylation, and the content of hydroxyl groups were measured by a method conforming to JIS K6728 "Testing Method for Polyvinyl Butyral." When measured by ASTM D1396-92, the values ​​were similar to those obtained by a method conforming to JIS K6728 "Testing Method for Polyvinyl Butyral."

[0257] The following materials were prepared:

[0258] (thermoplastic resin) Polyvinyl acetal resin 1 (polyvinyl butyral resin (PVB1), average degree of polymerization 3000, hydroxyl group content 17 mol%, acetylation degree 12 mol%, acetalization degree (butyralization degree) 71 mol%) Polyvinyl acetal resin 2 (polyvinyl butyral resin (PVB2), average degree of polymerization 3000, hydroxyl group content 18 mol%, acetylation degree 8 mol%, acetalization degree (butyralization degree) 74 mol%) Polyvinyl acetal resin 3 (polyvinyl butyral resin (PVB3), average degree of polymerization 3000, hydroxyl group content 19 mol%, acetylation degree 1 mol%, acetalization degree (butyralization degree) 80 mol%) Polyvinyl acetal resin 4 (polyvinyl butyral resin (PVB4), average degree of polymerization 3000, hydroxyl group content 15 mol%, acetylation degree 16 mol%, acetalization degree (butyralization degree) 69 mol%) Polyvinyl acetal resin 5 (polyvinyl butyral resin (PVB5), average degree of polymerization 3000, hydroxyl group content 18 mol%, acetylation degree 16 mol%, acetalization degree (butyralization degree) 66 mol%) Polyvinyl acetal resin 6 (polyvinyl butyral resin (PVB6), average degree of polymerization 1700, hydroxyl group content 30 mol%, acetylation degree 1 mol%, acetalization degree (butyralization degree) 69 mol%)

[0259] (Plasticizer) Triethylene glycol di-2-ethylhexanoate (3GO)

[0260] (Heat-shielding material or coloring agent) Heat shielding particles: Tin-doped indium oxide particles (ITO particles, average particle size 0.01 μm) Cesium-doped tungsten oxide particles (CWO particles, average particle size 0.02 μm) Ingredient X: Pigment Blue 15 (Phthalocyanine compound containing copper atoms) Pigment Green 7 (Phthalocyanine compound containing copper atoms) Pigment Black 1 (Carbon Black) Phthalocyanine compound X (a phthalocyanine compound containing vanadium atoms, "FDN-001" manufactured by Yamada Chemical Industry Co., Ltd.) others: Solvent Red 146 (SR146, anthraquinone dye, 1-amino-4-hydroxy-2-phenoxy-9,10-anthraquinone) Pigment Blue 60 (P.B60, anthraquinone dye, 6,15-dihydrodinaphtho[2,3-a:2,3-h]phenazine-5,9,14,18-tetraone)

[0261] (UV protection agent) Tinuvin 326 (2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole, BASF "Tinuvin 326")

[0262] (Antioxidants) BHT (2,6-di-t-butyl-p-cresol)

[0263] The following laminated glass components were prepared.

[0264] (Laminated glass components) Green glass 1 (thickness 2 mm, solar transmittance (Ts2100) 70%) Green glass 2 (thickness 1.9 mm, solar transmittance (Ts2100) 70%) Heat absorbing plate glass 1 (thickness 2 mm, solar transmittance (Ts2100) 62%) Heat absorbing plate glass 2 (thickness 1.9 mm, solar transmittance (Ts2100) 62%)

[0265] Example 1 Preparation of the composition for forming the first layer: The following components were mixed and thoroughly kneaded with a mixing roll to obtain a composition for forming a first layer.

[0266] Polyvinyl acetal resin 1 (PVB1) 100 parts by weight Triethylene glycol di-2-ethylhexanoate (3GO) 73 parts by weight Tinuvin 326 in an amount of 0.2% by weight in the resulting first layer BHT in an amount to give 0.2% by weight in the resulting first layer

[0267] Preparation of compositions for forming the second and third layers: The following components were mixed and thoroughly kneaded with a mixing roll to obtain compositions for forming the second layer and the third layer.

[0268] Polyvinyl acetal resin 6 (PVB6) 100 parts by weight Triethylene glycol di-2-ethylhexanoate (3GO) 36 parts by weight ITO particles in an amount of 0.16% by weight in the resulting second and third layers Tinuvin 326 in an amount of 0.2% by weight in the resulting second and third layers BHT in an amount of 0.2% by weight in the resulting second and third layers

[0269] Preparation of the interlayer: The composition for forming the first layer and the compositions for forming the second layer and the third layer were co-extruded using a co-extruder to produce an intermediate film (thickness 800 μm) having a laminated structure of the second layer (thickness 345 μm) / the first layer (thickness 110 μm) / the third layer (thickness 345 μm).

[0270] Laminated glass preparation: An interlayer film was sandwiched between two sheets of green glass with a thickness of 2 mm to obtain a laminate. The obtained laminate was placed in a rubber bag and degassed at a vacuum degree of 2.6 kPa for 20 minutes, then transferred to an oven in the degassed state and further held at 90°C for 30 minutes to perform vacuum pressing to pre-press the laminate. The pre-pressed laminate was pressed for 20 minutes in an autoclave under conditions of 135°C and a pressure of 1.2 MPa to obtain a laminated glass. The laminated glass was cut to obtain a laminated glass (1) having a size of 25 mm in length and 300 mm in width. The laminated glass was also cut to obtain a laminated glass (2) having a size of 500 mm in length and 500 mm in width.

[0271] Comparative Example 1 Interlayer films and laminated glasses (1) and (2) were obtained in the same manner as in Example 1, except that no heat-shielding material was used and the content of the plasticizer was changed as shown in Table 1.

[0272] (Examples 2 to 5) Interlayer films and laminated glasses (1) and (2) were obtained in the same manner as in Example 1, except that the type of polyvinyl acetal resin, the content of plasticizer, and the thicknesses of the first, second, and third layers were changed as shown in Tables 1 and 2.

[0273] Example 6 Interlayer films and laminated glasses (1) and (2) were obtained in the same manner as in Example 1, except that the type of polyvinyl acetal resin and the content of plasticizer were changed as shown in Table 2, and that CWO particles were used as heat shielding particles in the content shown in Table 2.

[0274] Example 7 Interlayer films and laminated glasses (1) and (2) were obtained in the same manner as in Example 1, except that the type of polyvinyl acetal resin, the content of plasticizer, and the type of laminated glass member were changed as shown in Table 2.

[0275] Example 8 Interlayer films and laminated glasses (1) and (2) were obtained in the same manner as in Example 1, except that the type of polyvinyl acetal resin, the content of plasticizer, and the type of laminated glass component were changed as shown in Table 3, and Pigment Blue 15 was used as the heat-shielding material and colorant in the content shown in Table 3.

[0276] Example 9 Interlayer films and laminated glasses (1) and (2) were obtained in the same manner as in Example 1, except that the type of polyvinyl acetal resin, the content of plasticizer, and the type of laminated glass component were changed as shown in Table 3, and Pigment Green 7 was used as the heat-shielding material and colorant in the content shown in Table 3.

[0277] Example 10 Interlayer films and laminated glasses (1) and (2) were obtained in the same manner as in Example 1, except that the type of polyvinyl acetal resin, the content of plasticizer, and the type of laminated glass member were changed as shown in Table 3, Pigment Blue 15 was used as the heat-shielding material and colorant in the content shown in Table 3, and ITO particles were used as the heat-shielding material in the content shown in Table 3. In Example 10, Pigment Blue 15 was used in an amount that would result in 0.022 wt % in the resulting second and third layers, and ITO particles were used in an amount that would result in 0.16 wt % in the resulting second and third layers.

[0278] Example 11 Interlayer films and laminated glasses (1) and (2) were obtained in the same manner as in Example 1, except that the type of polyvinyl acetal resin, the content of plasticizer, and the type of laminated glass component were changed as shown in Table 4, and Pigment Black 1, Solvent Red 146, and Pigment Blue 60 were used as the heat-shielding substance and colorant in the amounts shown in Table 4. In Example 11, Pigment Black 1 was used in an amount that would result in 0.001 wt % in the resulting second and third layers, Solvent Red 146 in an amount that would result in 0.0005 wt % in the resulting second and third layers, and Pigment Blue 60 in an amount that would result in 0.0007 wt % in the resulting second and third layers.

[0279] Example 12 The type of polyvinyl acetal resin, the content of plasticizer, and the type of laminated glass member were changed as shown in Table 4. In addition, phthalocyanine compound X was used as the heat-shielding material and colorant in the content shown in Table 4, and ITO particles and CWO particles were used as the heat-shielding material in the content shown in Table 4. Except for these, interlayer films and laminated glasses (1) and (2) were obtained in the same manner as in Example 1. In Example 12, ITO particles were used in an amount that would result in 0.24 wt % in the resulting second and third layers, CWO particles in an amount that would result in 0.01 wt % in the resulting second and third layers, and phthalocyanine compound X in an amount that would result in 0.0008 wt % in the resulting second and third layers.

[0280] Example 13 Interlayer films and laminated glasses (1) and (2) were obtained in the same manner as in Example 4, except that the plasticizer content was changed as shown in Table 4, and the thickness of one end and the thickness of the other end of the interlayer film were changed as shown in Table 4 to produce an interlayer film whose other end was thicker than the thickness of one end (wedge-shaped interlayer film). In Example 13, the laminated glass was cut so that a position 5 cm from one end of the laminated glass corresponding to one end of the interlayer film toward the other end was present in the laminated glasses (1) and (2), and the evaluation described below was performed at this position.

[0281] Example 14 Nano90s (multilayer resin film manufactured by Sumitomo 3M) was prepared as an infrared reflective layer. Using this infrared reflective layer, an interlayer film having a laminated structure of the fourth layer (390 μm) / infrared reflective layer (100 μm) / second layer (thickness 345 μm) / first layer (thickness 110 μm) / third layer (thickness 345 μm) was produced. In addition, using the obtained interlayer film and the laminated glass member shown in Table 5, laminated glasses (1) and (2) were produced in the same manner as in Example 1. The composition of each layer is shown in Table 5.

[0282] (evaluation) The laminated glasses (1) obtained in Examples 1 to 6 and 13 and Comparative Example 1 correspond to the laminated glass X described above.

[0283] (1) Solar transmittance The solar direct transmittance (Tds) of the obtained laminated glass (1) at wavelengths of 300 nm to 2500 nm was measured using a spectrophotometer (Hitachi High-Technologies Corporation, "U-4100") in accordance with JIS R3106:1998.

[0284] (2)Visible light transmittance The visible light transmittance (Tv) of the obtained laminated glass (1) in the wavelength range of 380 nm to 780 nm was measured using a spectrophotometer (Hitachi High-Technologies Corporation, "U-4100") in accordance with JIS R3211:1998.

[0285] (3) Loss factor (20°C) The loss factor of the obtained laminated glass (1) at 20° C. was measured by the central vibration method in accordance with ISO16940.

[0286] (4) Xenon light irradiation test Under windless conditions at 10°C, the laminated glass (1) and (2) obtained had a thermal resistance of 190 W / m 2 The sample was irradiated with xenon light for 30 minutes.

[0287] (4-1) Secondary resonance frequency The surface temperature of the laminated glass (1) was measured before and after the irradiation with xenon light. In addition, the secondary resonance frequency at 10°C was determined for the laminated glass (1) before the irradiation with xenon light by the central excitation method in accordance with ISO16940. In addition, within 2 minutes after the irradiation with xenon light, the secondary resonance frequency was determined for the laminated glass (1) after the irradiation with xenon light by the central excitation method in accordance with ISO16940. From the obtained secondary resonance frequency, the absolute value of the difference between the secondary resonance frequency of the laminated glass (1) before the irradiation with xenon light and the secondary resonance frequency of the laminated glass (1) after the irradiation with xenon light was calculated.

[0288] (4-2) Sound transmission loss (4000Hz) A reverberation chamber conforming to ISO 10140-5 was prepared, in which a first reverberation chamber, which is a sound source chamber, and a second reverberation chamber, which is a sound receiving chamber, were connected. The laminated glass (2) before xenon light irradiation was installed between the first reverberation chamber and the second reverberation chamber. The sound transmission loss was measured at 10°C and a frequency of 4000 Hz using a sound transmission loss measuring device "Intensity Probe SI-50, Multichannel Analyzer SA-02" manufactured by Rion. Specifically, the sound transmission loss (dB) conforming to JIS A1441-1 was measured by the intensity method. The center frequency was measured in 1 / 3 octave band. In addition, within 2 minutes after the xenon light irradiation, the sound transmission loss (dB) at a frequency of 4000 Hz was also measured for the laminated glass (2) after the xenon light irradiation in the same manner. From the obtained sound transmission loss, the absolute value of the difference between the sound transmission loss of the laminated glass (2) before irradiation with xenon light and the sound transmission loss of the laminated glass (2) after irradiation with xenon light was calculated.

[0289] Details and results are shown in the following Tables 1 to 6. In the tables, the ultraviolet shielding agent and antioxidant are omitted. In the tables, the content of the heat shielding material or coloring agent is shown as the content in 100% by weight of the second and third layers.

[0290] [Table 1]

[0291] [Table 2]

[0292] [Table 3]

[0293] [Table 4]

[0294] [Table 5]

[0295] [Table 6] [Explanation of symbols]

[0296] 1...First layer 1a...First surface 1b…Second surface 2...Second layer 2a…Outer surface 3...Third layer 3a…Outer surface 11...Interlayer 11A...Interlayer (first layer) 11a...First surface 11b…Second surface 21...First laminated glass member 22...Second laminated glass member 31, 31A…Laminated glass

Claims

1. An interlayer film for laminated glass having a structure of three or more layers, Contains a heat insulating material or coloring agent, A first layer; and a second layer disposed on a first surface side of the first layer; a third layer disposed on a second surface side of the first layer opposite the first surface, the first layer comprises a polyvinyl acetal resin and a plasticizer; In the first layer, a content of the plasticizer relative to 100 parts by weight of the polyvinyl acetal resin is 60 parts by weight or more and 85 parts by weight or less, When the interlayer film is sandwiched between two sheets of green glass having a thickness of 2 mm and a solar transmittance (Ts2100) of 70% to obtain laminated glass X having a length of 25 mm and a width of 300 mm, the absolute value of the difference between the secondary resonance frequency of the laminated glass X before irradiation with xenon light and the secondary resonance frequency of the laminated glass X after irradiation with xenon light, which is determined by the following xenon light irradiation test, is 60 Hz or more; The loss coefficient of the laminated glass X at 20°C is 0.25 or more, The laminated glass X has a solar transmittance of 50% or less. Xenon light irradiation test: The secondary resonance frequency of the laminated glass X at 10°C is determined by the central excitation method in accordance with ISO 16940. 2 The laminated glass X is irradiated with xenon light of 1000 nm for 30 minutes. The secondary resonance frequency of the laminated glass X after irradiation with xenon light is determined by a central excitation method in accordance with ISO 16940. The absolute value of the difference between the secondary resonance frequency of the laminated glass X before irradiation with xenon light and the secondary resonance frequency of the laminated glass X after irradiation with xenon light is calculated.

2. 2. The interlayer film for laminated glass according to claim 1, wherein an absolute value of a difference between a secondary resonance frequency of the laminated glass X before irradiation with xenon light and a secondary resonance frequency of the laminated glass X after irradiation with xenon light, which is determined by the xenon light irradiation test, is 200 Hz or less.

3. 3. The interlayer film for laminated glass according to claim 1, wherein when the laminated glass X is stored at 10°C for 56 days or more, the laminated glass X after storage has a secondary resonance frequency at 10°C of 900 Hz or more as determined by a central vibration method in accordance with ISO 16940.

4. The second layer is a surface layer of an intermediate film, the third layer is a surface layer of an interlayer film; the second layer comprises a thermoplastic resin; The interlayer film for laminated glass according to any one of claims 1 to 3, wherein the third layer contains a thermoplastic resin.

5. The thermoplastic resin contained in the second layer is a polyvinyl acetal resin, The interlayer film for laminated glass according to claim 4 , wherein the thermoplastic resin contained in the third layer is a polyvinyl acetal resin.

6. The second layer comprises a plasticizer, The interlayer film for laminated glass according to any one of claims 1 to 5, wherein the third layer contains a plasticizer.

7. The first layer has a glass transition temperature of 5° C. or less; The second layer has a glass transition temperature of 30° C. or higher; The interlayer film for laminated glass according to any one of claims 1 to 6, wherein the third layer has a glass transition temperature of 30°C or higher.

8. The interlayer film for laminated glass according to any one of claims 1 to 7, wherein the polyvinyl acetal resin contained in the first layer has a degree of acetylation of 10 mol % or less.

9. The interlayer film for laminated glass according to any one of claims 1 to 7, wherein the polyvinyl acetal resin contained in the first layer has a degree of acetylation of 15 mol % or more.

10. The interlayer film for laminated glass according to any one of claims 1 to 9, wherein the polyvinyl acetal resin contained in the first layer is a polyvinyl butyral resin.

11. 11. The interlayer film for laminated glass according to claim 10, wherein when the polyvinyl butyral resin contained in the first layer has a degree of butyralization of B mol % and a degree of acetylation of A mol %, the polyvinyl butyral resin contained in the first layer is a polyvinyl butyral resin that satisfies the formula: B≧−0.88×A+78.

6.

12. The interlayer film for laminated glass according to any one of claims 1 to 11, comprising heat shielding particles.

13. the second layer includes heat insulating particles; The interlayer film for laminated glass according to any one of claims 1 to 11, wherein the third layer contains heat shielding particles.

14. the second layer includes heat insulating particles; the third layer includes heat insulating particles; The interlayer film for laminated glass according to any one of claims 1 to 11, wherein a layer different from both the second layer and the third layer does not contain heat shielding particles.

15. the second layer contains heat-shielding particles and at least one component selected from the group consisting of a phthalocyanine compound, a naphthalocyanine compound, an anthracyanine compound, and carbon black; The interlayer film for laminated glass according to any one of claims 1 to 11, wherein the third layer contains heat shielding particles and at least one component selected from the group consisting of a phthalocyanine compound, a naphthalocyanine compound, an anthracyanine compound, and carbon black.

16. the component contained in the second layer is Pigment Blue 15, Pigment Green 7, or carbon black; The interlayer film for laminated glass according to claim 15, wherein the component contained in the third layer is Pigment Blue 15, Pigment Green 7, or carbon black.

17. the heat-shielding particles included in the second layer are tin-doped indium oxide particles; The interlayer film for laminated glass according to any one of claims 13 to 16, wherein the heat shielding particles contained in the third layer are tin-doped indium oxide particles.

18. A wire has one end and another end opposite the one end, The interlayer film for laminated glass according to any one of claims 1 to 17, wherein the thickness of the other end is greater than the thickness of the one end.

19. a first laminated glass member; a second laminated glass member; and The interlayer film for laminated glass according to any one of claims 1 to 18, The laminated glass, wherein the interlayer film for laminated glass is disposed between the first laminated glass member and the second laminated glass member.

20. a first laminated glass member; a second laminated glass member; and and an interlayer film for laminated glass, the interlayer film for laminated glass is disposed between the first laminated glass member and the second laminated glass member; The interlayer film for laminated glass has a structure of three or more layers, The interlayer film for laminated glass contains a heat-shielding material or a colorant, the interlayer film for laminated glass comprises a first layer, a second layer disposed on a first surface side of the first layer, and a third layer disposed on a second surface side of the first layer opposite to the first surface, the first layer comprises a polyvinyl acetal resin and a plasticizer; In the first layer, a content of the plasticizer relative to 100 parts by weight of the polyvinyl acetal resin is 60 parts by weight or more and 85 parts by weight or less, the absolute value of the difference between the secondary resonance frequency of the laminated glass before irradiation with xenon light and the secondary resonance frequency of the laminated glass after irradiation with xenon light, which is determined by the following xenon light irradiation test, is 60 Hz or more; The loss factor at 20°C is 0.25 or more, A laminated glass having a solar transmittance of 50% or less. Xenon light irradiation test: The secondary resonance frequency of the laminated glass at 10°C is determined by the central excitation method in accordance with ISO 16940. 2 The laminated glass is irradiated with xenon light of 1000 nm for 30 minutes. The secondary resonance frequency of the laminated glass after irradiation with xenon light is determined by a central excitation method in accordance with ISO 16940. The absolute value of the difference between the secondary resonance frequency of the laminated glass before irradiation with xenon light and the secondary resonance frequency of the laminated glass after irradiation with xenon light is calculated.

21. The first laminated glass member is green glass or a heat absorbing glass plate, 21. The laminated glass according to claim 19 or 20, wherein the second laminated glass component is green glass or a heat absorbing glazing.

22. The laminated glass according to any one of claims 19 to 21, having a solar transmittance of 48% or less.

Citation Information

Patent Citations

  • Laminated glass

    JP2008184348A

  • Interlayer film for laminated glass and laminated glass

    JP2011042552A

  • Intermediate film for laminated glasses, and laminated glass

    WO2012115198A1

  • Interlayer for laminated glass, and laminated glass

    WO2017135447A1