Nonwoven fabrics and conveyor belts

By applying rubber resins with specific properties on nonwoven fabrics, the grip and stability of conveyor belts are enhanced, addressing the issue of fiber shifting and ensuring stable conveyance and quality at higher speeds.

JP7561644B2Active Publication Date: 2024-10-04NIPPON FILCON CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021017205
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-23
Filing Date
2021-02-05
Publication Date
2024-10-04
Estimated Expiration
2041-02-05

AI Technical Summary

Technical Problem

Conventional nonwoven fabric conveyor belts face challenges in maintaining stable conveyance of fiber aggregates due to insufficient grip properties, especially at higher speeds, leading to issues like fiber shifting and reduced quality.

Method used

The application of rubber resins classified as JIS K6397 R or M groups on the surface of nonwoven fabrics, with specific static friction coefficients and durometer hardness ranges, enhances the grip properties by increasing frictional resistance and improving the stability of the nonwoven fabric on the belt.

Benefits of technology

The solution significantly improves the grip and stability of nonwoven fabrics on conveyor belts, ensuring uniform web spread and easy release, while maintaining high shower resistance and adhesive strength, thus enhancing the quality and efficiency of the conveyance process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561644000002
    Figure 0007561644000002
  • Figure 0007561644000003
    Figure 0007561644000003
  • Figure 0007561644000004
    Figure 0007561644000004
Patent Text Reader

Abstract

To provide a new technique for further improving grip performance in a belt suitable for conveyance of a nonwoven fabric.SOLUTION: There is provided a woven belt 12 for a nonwoven fabric in which a rubber-made resin classified into group R (rubber with unsaturated carbon bond in main chain) of JIS K 6397 is coated onto a surface side where a nonwoven fabric 18 is conveyed.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fabric used for conveying nonwoven fabric. [Background technology]

[0002] Conventionally, an apparatus has been devised in which a fiber aggregate is supplied onto a traveling endless mesh belt, and then the fiber aggregate is transported to form a nonwoven fabric. In recent years, with the increase in transport speed, one of the performance requirements for the mesh belt is a gripping property that allows the fiber aggregate supplied onto the mesh belt to be transported stably (the fiber aggregate does not float or slip during transport).

[0003] For example, in order to add excellent sheet support properties (grip properties), a two-layer nonwoven fabric has been devised which is composed of a surface layer consisting of surface side warps and surface side wefts and a back layer consisting of back side warps and back side wefts, and which comprises a first warp pair in which the surface side binding warps functioning as binding threads and the back side binding warps functioning as binding threads are arranged in a substantially perpendicular direction, a second warp pair in which the surface side warps and the back side warps functioning as binding threads are arranged overlapping each other in a perpendicular direction, and a third warp pair in which two surface side warps are adjacently arranged side by side (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-197883 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, as the conveying speed increases, there is a demand for further improvement in gripping properties.

[0006] The present invention has been made in view of the above circumstances, and one of its exemplary objects is to provide a new technique for further improving the gripping properties of a belt suitable for transporting nonwoven fabric. [Means for solving the problem]

[0007] In order to solve the above problems, in one embodiment of the nonwoven fabric of the present invention, a rubber resin classified as group R (rubber having unsaturated carbon bonds in the main chain) of JIS K6397 is applied to the surface side on which the nonwoven fabric is transported.

[0008] According to this embodiment, the gripping performance of the belt can be improved.

[0009] The rubber resin may be a styrene butadiene rubber.

[0010] Another embodiment of the present invention is also a nonwoven fabric, the surface of which, along which the nonwoven fabric is transported, is coated with a rubber resin that is classified as Group M of JIS K6397 (rubber having a polymethylene-type saturated main chain).

[0011] According to this embodiment, the gripping performance of the belt can be improved.

[0012] The rubber resin may be an acrylic rubber.

[0013] The rubber resin may be water-soluble before curing. If the rubber resin is water-soluble before curing, even if the solvent evaporates during curing, adverse effects on the environment and human health can be reduced.

[0014] The static friction coefficient of the surface side may be in the range of 0.25 to 0.90. This can improve the gripping property of the belt. If the static friction coefficient is 0.90 or less, the nonwoven fabric web during production spreads sufficiently on the belt, and the uniformity of the web is not impaired. Also, if the static friction coefficient is 0.25 or more, a sufficient gripping force against the nonwoven fabric web is obtained.

[0015] Another embodiment of the present invention is also a woven fabric for nonwoven fabric, the surface side of the woven fabric along which the nonwoven fabric is transported being coated with a resin different from the material of the yarn constituting the fabric, and the static friction coefficient of the surface side being in the range of 0.25 to 0.90.

[0016] According to this embodiment, if the static friction coefficient is 0.90 or less, the nonwoven web during production spreads sufficiently on the belt, and the uniformity of the web is not impaired. Also, if the static friction coefficient is 0.25 or more, a sufficient gripping force is obtained for the nonwoven web. Therefore, the gripping property of the belt can be improved.

[0017] The time from pressing the cotton against the multi-layer nonwoven fabric with the surface side of the nonwoven fabric being inclined vertically to releasing the cotton until the nonwoven fabric falls may be 10 seconds or less, which makes it easier to release the nonwoven fabric from the belt that transports the nonwoven fabric.

[0018] The difference between the height of the warp knuckles formed by the warp yarns on the surface side along which the nonwoven fabric is transported and the height of the weft knuckles formed by the weft yarns may be 100 μm or more, thereby making it possible to increase the frictional resistance between the surface side of the fabric for nonwoven fabric and the nonwoven fabric.

[0019] Conductive threads may be woven into the material.

[0020] The resin may have a durometer hardness after curing of 10 to 80. This can improve the gripping performance of the belt.

[0021] Yet another embodiment of the present invention is also a woven fabric for nonwoven fabric. This woven fabric for nonwoven fabric has a resin having a durometer hardness of 10 to 80 after curing applied to the surface side along which the nonwoven fabric is transported. Alternatively, the woven fabric for nonwoven fabric may have a resin having a durometer hardness of 50 to 80 after curing applied to the surface side along which the nonwoven fabric is transported. Alternatively, the woven fabric for nonwoven fabric may have a resin having a durometer hardness of 10 to 20 after curing applied to the surface side along which the nonwoven fabric is transported.

[0022] According to this embodiment, the gripping performance of the belt can be improved.

[0023] Yet another aspect of the present invention is a conveyor belt, which is made of the above-mentioned multi-layer nonwoven fabric.

[0024] Any combination of the above components and any conversion of the present invention into a method, device, system, etc. are also valid aspects of the present invention. Effect of the Invention

[0025] According to the present invention, a new fabric for nonwoven fabric that constitutes a belt suitable for transporting nonwoven fabric can be provided. [Brief description of the drawings]

[0026] [Figure 1] FIG. 1 is a diagram showing a schematic configuration of a manufacturing apparatus for manufacturing a nonwoven fabric by a spunbond method. [Diagram 2] FIG. 1 is a schematic diagram showing a schematic configuration of an apparatus for measuring the grip performance of a multi-layer fabric for nonwoven fabric against a nonwoven fabric. [Diagram 3] FIG. 1 is a schematic diagram showing a schematic configuration of an apparatus for measuring the static friction force of a multi-layer fabric for nonwoven fabric. [Figure 4] FIG. 1 is a schematic diagram for explaining a releasability evaluation test. [Diagram 5] FIG. 1 is a design drawing showing the complete design of a multi-layer nonwoven fabric according to Example 1-1. [Figure 6] 6 is a cross-sectional view taken along each warp thread in the design diagram shown in FIG. 5. [Figure 7] 1 is a graph comparing the values ​​of frictional force of the multi-layer nonwoven fabrics according to Examples 1-1 to 1-4 and the multi-layer nonwoven fabric according to Comparative Example 1. FIG. [Figure 8] FIG. 2 is a design diagram showing a complete design of a multi-layer nonwoven fabric according to Example 2. [Figure 9] 9 is a cross-sectional view taken along each warp thread in the design diagram shown in FIG. 8. [Figure 10]FIG. 1 is a design diagram showing a complete design of a multi-layer nonwoven fabric according to Example 3. [Figure 11] 11A and 11B are cross-sectional views taken along the warp threads in the design diagram shown in FIG. 10. [Figure 12] FIG. 1 is a design diagram showing a complete design of a multi-layer nonwoven fabric according to Example 4. [Figure 13] 13 is a cross-sectional view taken along each warp thread in the design diagram shown in FIG. 12. [Figure 14] FIG. 1 is a design diagram showing a complete design of a multi-layer nonwoven fabric according to Example 5. [Figure 15] 15 is a cross-sectional view taken along each warp thread in the design diagram shown in FIG. 14. [Figure 16] FIG. 1 is a design diagram showing a complete design of a multi-layer nonwoven fabric according to Example 6. [Figure 17] 17A to 17C are cross-sectional views taken along the warp threads in the design diagram shown in FIG. 16. [Figure 18] FIG. 11 is a design diagram showing the complete design of a multi-layer nonwoven fabric according to Example 7. [Figure 19] 19 is a cross-sectional view taken along each warp thread in the design diagram shown in FIG. 18. [Figure 20] FIG. 1 is a graph showing the results of measuring the static friction coefficient. [Figure 21] FIG. 11 is a design diagram showing the complete design of a multi-layer nonwoven fabric according to Example 8. [Figure 22] 22 is a cross-sectional view taken along each warp thread in the design diagram shown in FIG. 21. [Figure 23] FIG. 13 is a design diagram showing the complete design of the multi-layer nonwoven fabric according to Example 9. [Figure 24] 24 is a cross-sectional view taken along each warp thread in the design diagram shown in FIG. 23. [Diagram 25] FIG. 13 is a graph showing other static friction coefficient measurement results. [Figure 26] FIG. 1 is a diagram showing the results of a shower resistance test for the multi-layer nonwoven fabrics of Examples 1-1 to 1-4. [Figure 27] FIG. 1 is a diagram showing the results of an adhesion test for multi-layer fabrics for nonwoven fabric according to Comparative Example 1 and Examples 1-1 to 1-4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] The present invention will be described below with reference to the drawings based on the embodiments. The same or equivalent components, parts, and processes shown in each drawing are given the same reference numerals, and duplicated descriptions are omitted as appropriate. In addition, the embodiments are not intended to limit the invention, but are merely examples, and all features and combinations thereof described in the embodiments are not necessarily essential to the invention.

[0028] Conventionally, various methods such as the spunbond method and the meltblowing method have been devised as methods for manufacturing nonwoven fabrics. For example, the spunbond method is a method for manufacturing nonwoven fabrics by stretching a molten resin polymer and accumulating it as a sheet on a nonwoven fabric belt. Such a spunbond method is particularly suitable for high-speed production, and in recent years, belts are used at speeds of around 1000 mm / min. Therefore, in the spunbond method, the gripping force of the belt is particularly required. Figure 1 is a diagram showing the schematic configuration of a manufacturing device for manufacturing nonwoven fabrics by the spunbond method.

[0029] The nonwoven fabric manufacturing apparatus 10 shown in Fig. 1 includes an endless nonwoven fabric belt 12, a plurality of drive rollers 14 that support and drive the nonwoven fabric belt 12, an ejector 16 that spins and draws a molten resin polymer onto the nonwoven fabric belt 12 and discharges it, a suction device 20 that sucks a nonwoven fabric 18 formed by depositing the resin polymer discharged onto the nonwoven fabric belt 12 as a fibrous aggregate from the back side of the nonwoven fabric belt 12, a press roll 21 that is disposed so as to sandwich the nonwoven fabric belt 12 between the adjacent suction devices 20, and a calendar roll 24 that embosses the nonwoven fabric 18 by thermocompression bonding to a sheet-like nonwoven fabric 22. The nonwoven fabric belt 12 is formed by loop-bonding one end of a nonwoven fabric fabric to the other end.

[0030] Such nonwoven fabric belts 12 are required to have various characteristics such as no penetration of fibers, antifouling properties, washability, runnability, rigidity, static electricity removal performance, and nonwoven fabric stability (grip). In recent years, with the increase in speed of nonwoven fabric manufacturing equipment, there is a particular demand for nonwoven fabric transport stability (grip). For example, if the grip force is small, when the nonwoven fabric is transported on the nonwoven fabric belt, the nonwoven fabric formed may move on the nonwoven fabric belt and be folded, which may lead to a decrease in the yield rate of the nonwoven fabric.

[0031] Therefore, in order to improve the grip strength, which is one of the properties required for a multilayer fabric for nonwoven fabric, the inventors of the present application focused on the frictional resistance of the upper fabric, which is the side that comes into contact with the nonwoven fabric being transported.

[0032] First, an evaluation method for demonstrating the effect of a multi-layer nonwoven fabric having an upper fabric with increased surface friction resistance, a method for measuring the static friction force of the fabric, and a releasability evaluation test will be described.

[0033] [Grip evaluation method] FIG. 2 is a schematic diagram showing the schematic configuration of an apparatus for measuring the grip performance of a multi-layer fabric for nonwoven fabric against a nonwoven fabric.

[0034] The measuring device 100 includes a tensile tester 102 and a measuring tool 104. The tensile tester 102 is a precision universal testing machine Autograph AG-IS (manufactured by Shimadzu Corporation) and a load cell (100N) for a tensile tester. The measuring tool 104 is a suction box 106. The suction box 106 has a mounting portion 106a on which a multi-layer nonwoven fabric 108 is mounted, a suction hole 106b formed in the mounting portion 106a for sucking the back side of the multi-layer nonwoven fabric 108, and a roller 106c for aligning the pulling direction of the nonwoven fabric 110 arranged horizontally toward the chuck 102a of the tensile tester 102.

[0035] The measurement method is as follows: first, the multi-layer nonwoven fabric 108 is placed on the placement portion 106a of the suction box 106. The multi-layer nonwoven fabric 108 used for the measurement is a strip-like fabric with a width of 200 mm and a length of 300 mm. Next, the nonwoven fabric 110 is placed on the multi-layer nonwoven fabric 108. The nonwoven fabric 110 is a strip-like fabric with a width of 90 mm and a length of 600 mm, and one end of the nonwoven fabric 110 is fixed to the chuck 102a.

[0036] Next, the air is sucked from below the suction hole 106b by a suction device. The suction force of the suction device is 18.44 kPa, and the air volume is 1.40 m 3 / min. In this state, a tensile test is started by the tensile tester 102. The test conditions are as follows. Tensile speed: 100mm / min Stroke: 100mm N number (number of measurements): 3 Display of measurement results: Stress

[0037] [Static friction test method] FIG. 3 is a schematic diagram showing the schematic configuration of an apparatus for measuring the static friction force of a multi-layer nonwoven fabric.

[0038] 3 includes a tensile tester 102, a measurement table 122, a multi-layer nonwoven fabric 108 placed on the measurement table 122, and a weight 128 for pressing the nonwoven fabric 18 against the multi-layer nonwoven fabric 108. Cotton 124 is placed between the weight 128 and the nonwoven fabric 18.

[0039] The tensile tester 102 used a precision universal testing machine Autograph AG-IS and a load cell for a tensile tester (100N). The measurement table 122 has a pulley 122a at its end. Weights 128 of various weights are available, and in this embodiment, a weight of 100 to 975g was used. A pulled part 127 to which one end of a spring 126 connected to the tensile tester 102 is fixed is fixed to one end of the nonwoven fabric 18. Then, the weight 128 of a predetermined weight is placed on the nonwoven fabric 18 with the cotton 124 sandwiched therebetween, and the force pulling the nonwoven fabric 18 by the tensile tester 102 is gradually increased, and the force at the start of the movement is measured as the static friction force.

[0040] [Releaseability evaluation test] Fig. 4 is a schematic diagram for explaining a releasability evaluation test. In the test method shown in Fig. 4, first, the multi-layer nonwoven fabric 108 is fixed to a wall 130. Next, cotton 132 is pressed against the multi-layer nonwoven fabric 108, and the hand is released from the cotton 132, and it is observed whether the cotton 132 falls off.

[0041] Next, the nonwoven fabric composing the nonwoven fabric belt will be described. The nonwoven fabric composing the nonwoven fabric belt 12 may be a single layer or a multilayer, but the following will be described using a multilayer nonwoven fabric as an example. In the following description, the "warp thread" refers to a thread extending along the conveying direction of the nonwoven fabric when the multilayer nonwoven fabric is used as a loop-shaped nonwoven fabric belt, and the "weft thread" refers to a thread extending in a direction intersecting the warp thread. In addition, the "upper surface side fabric" refers to a fabric located on the surface side of the nonwoven fabric belt on which the nonwoven fabric is conveyed when the multilayer nonwoven fabric is used as a nonwoven fabric belt, and the "lower surface side fabric" refers to a fabric located on the back side of the nonwoven fabric belt on which the drive roller mainly comes into contact. In addition, the "surface" simply refers to the exposed surface of the upper side fabric or the lower side fabric, and the "surface" of the upper side fabric corresponds to the front side of the nonwoven fabric belt, while the "surface" of the lower side fabric corresponds to the back side of the nonwoven fabric belt.

[0042] In addition, a "design pattern" is the smallest repeating unit of a woven fabric and corresponds to the complete structure of the fabric. In other words, a "woven fabric" is formed by repeating a "complete structure" back and forth and left and right. In addition, a "knuckle" refers to a part where a warp thread passes over or under one or more weft threads and protrudes to the surface. In addition, an "off-stack structure" refers to a structure in which threads of the same direction arranged above and below are arranged so that they do not overlap vertically.

[0043] In addition, the "intersection support strength of yarns" refers to the force applied between the warp and weft yarns at the knuckle portion, and generally, knuckles that are attached to one yarn tend to have a strong intersection support strength, while long knuckles that are attached to multiple yarns tend to have a low intersection support strength. Therefore, the weave that has the highest intersection support strength is a plain weave. This is because in a plain weave, all knuckles are attached to a single yarn, resulting in the highest knuckle density.

[0044] In addition, a "binding yarn" refers to at least a portion of the warp threads that make up the upper side fabric (or lower side fabric), and is a yarn that binds the upper side fabric and the lower side fabric together by weaving the weft threads of the lower side fabric (or upper side fabric) from the back side (or front side) using warp threads that should normally only be woven with the weft threads of the upper side fabric (or lower side fabric).

[0045] Fiber penetration is a phenomenon in which fibers get stuck between the knuckle intersections of threads. When fibers get stuck, problems occur, such as (1) defects in the nonwoven fabric, and (2) the breathability of the fabric in the stuck area decreases, reducing the suction effect and the grip of the nonwoven fabric.

[0046] The upper surface side warp and lower surface side warp constituting the following woven fabric are preferably in the range of about φ0.30 to 0.50 mm, but are not necessarily limited to this range. Similarly, the upper surface side weft is preferably in the range of about φ0.30 to 0.60 mm, and the lower surface side weft is preferably in the range of about φ0.40 to 0.70 mm, but are not necessarily limited to this range.

[0047] (Example 1-1) The structure of the multilayer nonwoven fabric according to Example 1-1 will be described below with reference to the drawings. Fig. 5 is a design drawing showing the complete design of the multilayer nonwoven fabric according to Example 1-1. Fig. 6 is a cross-sectional view taken along each warp in the design drawing shown in Fig. 5. In Fig. 5, the warp pairs (4U and 4U', and 8U and 8U') are shown in two rows for convenience, since the upper surface side warps are juxtaposed.

[0048] In the design drawings, warp threads are indicated by Arabic numerals, for example, 1, 2, 3.... Weft threads are indicated by Arabic numerals with a dash, for example, 1', 2', 3'.... Upper surface side threads are indicated by numerals with U or U', and lower surface side threads are indicated by numerals with L, for example, 1'U, 2'L, etc. Also, binding threads that bind the upper surface side fabric and the lower surface side fabric are indicated by numerals with b.

[0049] In the design drawings, a triangle mark indicates that the threads that would normally constitute the lower surface side warp are placed above the upper surface side weft, a cross mark indicates that the upper surface side warp is placed above the upper surface side weft, a triangle mark indicates that the threads that would normally constitute the upper surface side warp are placed below the lower surface side weft, and a circle mark indicates that the lower surface side warp is placed below the lower surface side weft. In Fig. 6, the upper surface side warp is shown by a solid line, and the lower surface side warp is shown by a dotted line.

[0050] The multilayer nonwoven fabric 40 of the first embodiment shown in Figure 5 is a multilayer fabric with a surface plain weave structure composed of, from the left, one warp pair A (1Ub and 1Lb), two warp pairs B (2U and 2L and 3U and 3L), one warp pair C (4U and 4U'), one warp pair A (5Ub and 5Lb), two warp pairs B (6U and 6L and 7U and 7L), one warp pair C (8U and 8U'), and upper surface side wefts (1'U, 2'U, 3'U, 4'U) and lower surface side wefts (1'L, 2'L, 3'L, 4'L).

[0051] Also, as shown in Figure 6, upper surface side warp 1Ub, which functions as a binding yarn that constitutes warp pair A, passes under lower surface side weft 1'L to form a back surface side knuckle, then passes between upper surface side weft 2'U and lower surface side weft 2'L, then passes over upper surface side weft 3'U to form a front surface side knuckle, and then passes between upper surface side weft 4'U and lower surface side weft 4'L to be woven together.

[0052] In addition, lower surface side warp 1Lb, which functions as a binding yarn that constitutes warp pair A, passes above upper surface side weft 1'U to form a front surface side knuckle, then passes between upper surface side weft 2'U and lower surface side weft 2'L, then passes below lower surface side weft 3'L to form a back surface side knuckle, and then passes between upper surface side weft 4'U and lower surface side weft 4'L to be woven together.

[0053] In addition, the upper surface side warp 2U that constitutes warp pair B is woven so that it passes under the upper surface side weft 1'U, then passes over the upper surface side weft 2'U to form a surface side knuckle, and then passes under the upper surface side weft 3'U, then passes over the upper surface side weft 4'U to form a surface side knuckle again.

[0054] In addition, the lower surface side warp 2L that constitutes warp pair B is woven so that it passes above the lower surface side weft 1'L, then passes below the lower surface side weft 2'L to form a back surface side knuckle, and then passes above the lower surface side weft 3'L, then passes below the lower surface side weft 4'L to form a back surface side knuckle again.

[0055] In addition, upper surface side warp 3U, which constitutes warp pair B, passes above upper surface side weft 1'U to form a surface side knuckle, then passes below upper surface side weft 2'U, then passes above upper surface side weft 3'U to form a surface side knuckle again, and then passes below upper surface side weft 4'U to be woven together.

[0056] In addition, lower surface side warp 3L, which constitutes warp pair B, passes under lower surface side weft 1'L to form a back surface side knuckle, then passes over lower surface side weft 2'L, then passes under lower surface side weft 3'L to form a back surface side knuckle again, and then passes over lower surface side weft 4'L to be woven together.

[0057] In addition, the upper surface side warp 4U that constitutes the warp pair C is woven so that it passes under the upper surface side weft 1'U, then passes over the upper surface side weft 2'U to form a surface side knuckle, and then passes under the upper surface side weft 3'U, then passes over the upper surface side weft 4'U to form a surface side knuckle again.

[0058] In addition, the upper surface side warp 4U' that constitutes the warp pair C passes above the upper surface side weft 1'U to form a surface side knuckle, then passes below the upper surface side weft 2'U, and then passes above the upper surface side weft 3'U to form a surface side knuckle, before passing below the upper surface side weft 4'U and being woven together.

[0059] In addition, the upper surface side warp 5Ub, which functions as a binding yarn that constitutes the warp pair A, passes between the upper surface side weft 1'U and the lower surface side weft 1'L, then passes above the upper surface side weft 2'U to form a surface side knuckle, and then passes between the upper surface side weft 3'U and the lower surface side weft 3'L, then passes below the lower surface side weft 4'L to form a back surface side knuckle.

[0060] In addition, the lower surface side warp 5Lb, which functions as a binding yarn that constitutes the warp pair A, passes between the upper surface side weft 1'U and the lower surface side weft 1'L, then passes under the lower surface side weft 2'L to form a back surface side knuckle, and then passes between the upper surface side weft 3'U and the lower surface side weft 3'L, before passing over the upper surface side weft 4'U to form a front surface side knuckle.

[0061] In addition, the upper surface side warp 6U that constitutes warp pair B passes above the upper surface side weft 1'U to form a surface side knuckle, then passes below the upper surface side weft 2'U, then passes above the upper surface side weft 3'U to form another surface side knuckle, and then passes below the upper surface side weft 4'U to be woven together.

[0062] In addition, the lower surface side warp 6L that constitutes warp pair B passes under the lower surface side weft 1'L to form a back surface side knuckle, then passes over the lower surface side weft 2'L, then passes under the lower surface side weft 3'L to form a back surface side knuckle again, and then passes over the lower surface side weft 4'L to be woven together.

[0063] In addition, the upper surface side warp 7U that constitutes warp pair B passes under the upper surface side weft 1'U, then passes over the upper surface side weft 2'U to form a surface side knuckle, and then passes under the upper surface side weft 3'U, then passes over the upper surface side weft 4'U to form a surface side knuckle again.

[0064] In addition, the lower surface side warp 7L that constitutes warp pair B passes above the lower surface side weft 1'L, then passes below the lower surface side weft 2'L to form a back surface side knuckle, then passes above the lower surface side weft 3'L, and then passes below the lower surface side weft 4'L to again form a back surface side knuckle.

[0065] Furthermore, the upper surface side warp 8U that constitutes the warp pair C passes above the upper surface side weft 1'U to form a surface side knuckle, then passes below the upper surface side weft 2'U, and then passes above the upper surface side weft 3'U to form another surface side knuckle, before passing below the upper surface side weft 4'U and being woven together.

[0066] Furthermore, the upper surface side warp 8U' which constitutes the warp pair C passes under the upper surface side weft 1'U, then passes over the upper surface side weft 2'U to form a surface side knuckle, then passes under the upper surface side weft 3'U, then passes over the upper surface side weft 4'U to form a surface side knuckle again.

[0067] The multilayer nonwoven fabric 40 according to Example 1-1 has a resin (e.g., a rubber resin classified as group M of JIS K6397 (rubber having a polymethylene-type saturated main chain)) different from the material of the yarn constituting the fabric applied to the surface side along which the nonwoven fabric is transported. This improves the grip of the belt. Here, the rubber resin according to Example 1-1 is an acrylic rubber (a rubber-like copolymer of acrylic acid esters and other substances (ethylene and acrylonitrile)). The rubber resin may also be water-soluble.

[0068] The acrylic rubber applied to the multi-layer nonwoven fabric according to Example 1-1 had a hardness of 15 after curing in terms of durometer hardness (Shore A).

[0069] (Example 1-2) The multi-layer nonwoven fabric according to Example 1-2 has a perfect structure similar to that of the multi-layer nonwoven fabric according to Example 1-1, and a resin different from the material of the threads constituting the fabric is applied to the surface side on which the nonwoven fabric is conveyed. Specifically, it differs from Example 1-1 in that a rubber resin classified as group R (rubber having an unsaturated carbon bond in the main chain) of JIS K6397 is applied. This improves the grip of the belt. Here, the rubber resin according to Example 1-2 is styrene butadiene rubber. The rubber resin may be water-soluble.

[0070] The styrene-butadiene rubber applied to the multi-layer nonwoven fabric of Example 1-2 had a hardness of 80 after curing in terms of durometer hardness (Shore A).

[0071] (Examples 1-3) The multi-layer nonwoven fabric of Example 1-3 is coated with the same styrene-butadiene rubber as the rubber resin coated on the surface of the multi-layer nonwoven fabric of Example 1-2, but the concentration of the resin is changed in order to increase the hardness of the resin. The hardness of the styrene-butadiene rubber coated on the multi-layer nonwoven fabric of Example 1-3 after curing was 50 in durometer hardness (Shore A).

[0072] (Examples 1 to 4) The multi-layer nonwoven fabric of Example 1-4 is coated with the same styrene-butadiene rubber as the rubber resin coated on the surface of the multi-layer nonwoven fabric of Example 1-2, but the concentration of the resin is changed in order to increase the hardness of the resin. The hardness of the styrene-butadiene rubber coated on the multi-layer nonwoven fabric of Example 1-4 after curing was 15 in durometer hardness (Shore A).

[0073] Comparative Example 1 The multilayer fabric for nonwoven fabric of Comparative Example 1 is substantially the same as the multilayer fabric for nonwoven fabric 40 of Example 1-1, except that no rubber resin is applied to the surface side on which the nonwoven fabric is transported.

[0074] Comparative Example 2 The multilayer fabric for nonwoven fabric of Comparative Example 2 is substantially the same as the multilayer fabric for nonwoven fabric of Comparative Example 1, except that an adhesive resin (e.g., silicone resin) is applied to the surface side on which the nonwoven fabric is transported.

[0075] Comparative Example 3 The multilayer nonwoven fabric of Comparative Example 3 is substantially the same as the multilayer nonwoven fabric of Comparative Example 1, except that the surface side on which the nonwoven fabric is transported is embossed.

[0076] Fig. 7 is a graph comparing the frictional force values ​​of the multilayer woven fabrics for nonwoven fabric according to Examples 1-1 to 1-4 and the multilayer woven fabric for nonwoven fabric according to Comparative Example 1. As shown in Fig. 7, the frictional force of the multilayer woven fabric for nonwoven fabric according to Example 1-1 is 0.20 [kgf] or more, which is four times or more the frictional force (less than 0.05 [kgf]) of the multilayer woven fabric for nonwoven fabric according to Comparative Example 1. In other words, the nonwoven fabric belt using the multilayer woven fabric for nonwoven fabric according to Example 1-1 can improve gripping properties.

[0077] Moreover, the frictional force of the multi-layered nonwoven fabric according to Example 1-2 is 0.084 [kgf], the frictional force of the multi-layered nonwoven fabric according to Example 1-3 is 0.141 [kgf], and the frictional force of the multi-layered nonwoven fabric according to Example 1-4 is 0.297 [kgf], all of which are about 2 to 6 times the frictional force (less than 0.05 [kgf]) of the multi-layered nonwoven fabric according to Comparative Example 1. That is, the gripping property can be improved not only for the acrylic rubber in Example 1-1, but also for the nonwoven fabric belts using the multi-layered nonwoven fabrics according to Examples 1-2 to 1-4 in which styrene butadiene rubber is applied to the surface side. Moreover, by adjusting the concentration of the rubber resin when applying, the amount of application can be changed, and the magnitude of the frictional force can be adjusted. In other words, the hardness of the surface side of the fabric to which the rubber resin is applied can be adjusted by the amount of application of the rubber resin, and the magnitude of the frictional force of the multi-layered nonwoven fabric can be adjusted.

[0078] FIG. 20 is a graph showing the results of measuring the coefficient of static friction. The horizontal axis of the graph represents the weight [kg] of the weight, the vertical axis of the graph represents the tensile stress [kgf], and the slope of a linear approximation curve (with an intercept of 0) represents the coefficient of static friction. The coefficient of static friction of the multilayer nonwoven fabric (line L1) according to Comparative Example 1 is about 0.18. In contrast, the coefficient of static friction of the multilayer nonwoven fabric (lines L2, L3, L4) according to Example 1-1 to which acrylic rubber is applied is in the range of 0.32 to 0.47. The coefficient of static friction (grip force) can be adjusted by adjusting the concentration of the resin to be applied and the moving speed of the belt (multilayer nonwoven fabric) during application.

[0079] The difference in the inclination of lines L2 to L4 is caused by the difference in the resin concentration during application. Specifically, while the belt was moved in the length direction at a moving speed of 22 m / min, resin-containing solutions with resin mass % concentrations of 20% (line L2), 50% (line L3), and 80% (line L4) were applied to the surface of the multilayer nonwoven fabric according to Example 1-1 using a fixed spray.

[0080] Fig. 25 is a graph showing the results of other static friction coefficient measurements. As in Fig. 20, the static friction coefficient of the multilayer nonwoven fabric (line L1) according to Comparative Example 1 is about 0.18. In contrast, the static friction coefficients of the multilayer nonwoven fabrics (lines L5, L6, L7) according to Examples 1-2 to 1-4, which are coated with styrene-butadiene rubber and have different surface hardness, are in the range of 0.33 to 0.82. The static friction coefficient (grip force) can be adjusted by adjusting the concentration of the resin to be applied, the hardness of the resin after curing, and the moving speed of the belt (multilayer nonwoven fabric) during application.

[0081] The difference in the inclination of lines L5 to L7 is caused by the difference in the resin concentration during application. Specifically, while the belt was moved in the length direction at a speed of 22 m / min, a resin-containing solution with a resin mass percentage concentration of 20% (line L2), 50% (line L3), or 80% (line L4) was applied to the surface of the multilayer nonwoven fabric according to each example using a fixed spray.

[0082] Next, the results of the release evaluation test are shown in Table 1.

[0083] [Table 1]

[0084] As shown in Table 1, the cotton immediately fell off in the nonwoven multilayer fabric according to Comparative Example 1, which was not subjected to any processing, and the nonwoven multilayer fabric according to Example 1-1, which was coated with a rubber resin. On the other hand, in the nonwoven multilayer fabric according to Comparative Example 2 and the nonwoven multilayer fabric according to Comparative Example 3, the cotton remained attached to the nonwoven multilayer fabric and did not fall off. Whether the cotton falls off or not corresponds to whether the nonwoven fabric 18 is easily peeled off from the nonwoven fabric belt 12 (releasability) in the process of producing the nonwoven fabric shown in FIG. 1.

[0085] Thus, in the multilayer nonwoven fabric 40 according to Example 1-1, the time from pressing cotton against the multilayer nonwoven fabric with the surface side on which the nonwoven fabric is transported tilted vertically to releasing the cotton until the fabric falls is 10 seconds or less. As a result, the multilayer nonwoven fabric according to Example 1-1 makes it easier for the nonwoven fabric to be released from the belt transporting the nonwoven fabric. Although there is basically a trade-off between grip performance and release performance, the nonwoven fabric belt made of the multilayer nonwoven fabric according to the present embodiment coated with a rubber resin can achieve both high grip performance and good release performance.

[0086] In addition, when the surface side of the multi-layer nonwoven fabric according to the present embodiment is coated with a rubber resin or a resin different from the material of the yarn constituting the fabric, the static friction coefficient of the surface side is preferably in the range of 0.25 to 0.90. This allows the nonwoven fabric belt using the multi-layer nonwoven fabric according to the present embodiment to improve gripping properties. The static friction coefficient of the surface side of the multi-layer nonwoven fabric may be adjusted, for example, by setting the difference between the height of the warp knuckle (position of the x mark shown in FIG. 5) formed by the warp yarn on the surface side where the nonwoven fabric is transported and the height of the weft knuckle (for example, the position adjacent to the x mark shown in FIG. 5) to 100 μm or more. This allows the friction resistance between the surface side of the nonwoven fabric fabric and the nonwoven fabric to be increased. In addition, due to the height difference of the knuckles, the resin applied to the lower knuckle is protected from surface wear by the higher knuckle.

[0087] The multilayer nonwoven fabric according to the present embodiment may be coated with a resin having a hardness in a predetermined range on the surface side along which the nonwoven fabric is transported. Specifically, a resin having a durometer hardness of 10 to 80 after curing is preferred. If the hardness is less than 10 (soft), the releasability decreases. On the other hand, if the hardness is more than 80 (hard), the gripping ability decreases. This makes it possible to realize a multilayer nonwoven fabric that has both releasability and gripping ability. The durometer hardness according to the present embodiment is measured using a cylindrical indenter of a standard type A rubber hardness tester (DM-104A: manufactured by Muratec KDS Co., Ltd.).

[0088] [Shower resistance test] When the belt made of the multilayer nonwoven fabric according to the present embodiment is continuously used, dirt adheres to and accumulates on the belt. Therefore, dirt needs to be washed off with a high-pressure shower, and high shower resistance is required. Here, high shower resistance means that the resin applied to the surface of the fabric is not easily peeled off when washed with a high-pressure shower. If the shower resistance is low, the grip performance of the multilayer nonwoven fabric decreases due to peeling of the resin.

[0089] The specific test method was to spray water on the surface of the multi-layer nonwoven fabric with a shower pressure of 2.5 to 20 MPa. The shower was sprayed over a range of 10 cm in the warp direction of the multi-layer nonwoven fabric, and the shower was moved back and forth at a moving speed of 20 cm / min. After that, the above-mentioned grip property evaluation was performed.

[0090] FIG. 26 is a diagram showing the results of a shower resistance test for the multilayer nonwoven fabrics of Examples 1-1 to 1-4. As shown in FIG. 26, it can be seen that the multilayer nonwoven fabric of Example 1-1, in which acrylic rubber is applied to the surface side, has a reduced grip strength at a shower pressure of 6 MPa. On the other hand, the multilayer nonwoven fabrics of Examples 1-2 and 1-3 have almost no reduction in grip strength even at a shower pressure of 20 MPa, and are therefore highly shower resistant. Also, it can be seen that the multilayer nonwoven fabric of Examples 1-2 and 1-3 have almost no reduction in grip strength even at a shower pressure of 20 MPa, and are therefore highly shower resistant. Also, the multilayer nonwoven fabric of Example 1-4 suppresses a reduction in grip strength up to a shower pressure of about 15 MPa.

[0091] From the above, in terms of shower resistance, a multi-layer nonwoven fabric having a rubber resin classified as Group R (rubber having unsaturated carbon bonds in the main chain) of JIS K6397 applied to the surface side is preferable. More preferably, the durometer hardness of the applied resin after curing is 80 or less (60 or less).

[0092] [Adhesion test] If the adhesive strength of the resin on the surface of the multi-layer nonwoven fabric is high, the nonwoven fabric is less likely to float off the belt surface, enabling stable transportation. On the other hand, the releasability when moving from the belt to the next process decreases, so an appropriate adhesive strength is required depending on the nonwoven fabric manufacturing equipment and manufacturing conditions.

[0093] The specific test method is explained below. First, a belt sample made of a multi-layer nonwoven fabric of the size used in the grip evaluation is set in the test machine. Next, one end of a tissue paper with a width of 90 mm and a length of 394 mm is clamped with a chuck and draped over the belt sample so that the entire tissue paper is placed on it. After that, a cylindrical weight weighing 2.4 kg is rolled over the tissue paper to bring the tissue paper and the belt sample into close contact. Then, the chuck clamping one end of the tissue paper is pulled upwards by 80 cm at a speed of 150 cm / min, and the tensile stress (adhesive force) [kgf] applied to the tissue paper at that time is measured.

[0094] Fig. 27 shows the results of an adhesion test on the multilayer nonwoven fabrics according to Comparative Example 1 and Examples 1-1 to 1-4. As shown in Fig. 27, the multilayer nonwoven fabric according to Example 1-1 has high adhesion, so the nonwoven fabric on the belt can be stably transported. On the other hand, the multilayer nonwoven fabrics according to Examples 1-2 to 1-4 have higher adhesion than Comparative Example 1 and lower adhesion than Example 1-1, so they can achieve stable transportation and good releasability.

[0095] As described above, by applying a resin having a durometer hardness of 50 to 80 after curing, a multi-layer nonwoven fabric having improved grip and high shower resistance can be realized. In addition, by applying a resin having a durometer hardness of 10 to 20, a multi-layer nonwoven fabric having very high grip can be obtained, so applying such a resin to the surface side of the woven fabric on which the nonwoven fabric is transported is suitable for the production of nonwoven fabrics that require particularly strong grip. On the other hand, if a resin having a durometer hardness of more than 80 is applied, it becomes difficult to improve the grip. In addition, if a resin having a durometer hardness of less than 10 is applied, release failure and peeling of the resin are likely to occur.

[0096] Example 2 Hereinafter, the configuration of the multilayer nonwoven fabric according to Example 2 will be described with reference to the drawings. Fig. 8 is a design diagram showing the complete design of the multilayer nonwoven fabric according to Example 2. Fig. 9 is a cross-sectional view taken along each warp thread in the design diagram shown in Fig. 8.

[0097] In the following design drawings, warp threads are indicated by Arabic numerals, e.g., 1, 2, 3.... Bonding threads are indicated by numerals with an F and non-bonding threads are indicated by numerals with an S. Weft threads are indicated by Arabic numerals with a dash, e.g., 1', 2', 3'.... Upper surface side wefts are indicated by numerals with an U and lower surface side wefts are indicated by numerals with an L, e.g., 1'U, 2'L, etc.

[0098] In addition, in the design drawings, a ■ mark indicates that the bonding yarn is positioned above the upper surface side weft, a square mark indicates that the bonding yarn is positioned below the lower surface side weft, and an × mark indicates that the non-bonding yarn is positioned above the upper surface side weft.

[0099] The multi-layer nonwoven fabric 50 according to Example 2 is a multi-layer fabric, and the upper surface side weft and the lower surface side weft are arranged so as not to overlap each other vertically. The overlap of the yarns in the design drawing is represented by the numbers indicating the yarns on the left side of the design drawing.

[0100] The multilayer nonwoven fabric 50 according to Example 2 shown in FIG. 8 is a multilayer fabric having a surface plain weave structure constituted by binding yarns F, non-binding yarns S, upper surface side wefts U, and lower surface side wefts L.

[0101] As shown in Fig. 8, the binding yarn 4F passes above the upper surface side weft 1'U to form a front side knuckle, then passes above the lower surface side weft 2'L, then passes below the upper surface side weft 3'U, and then passes below the lower surface side weft 4'L and the lower surface side weft 6'L to form a back side knuckle, then passes below the upper surface side weft 7'U, and then passes above the lower surface side weft 8'L.

[0102] In addition, the binding yarn 3F is paired with the adjacent binding yarn 4F. The binding yarn 3F forms a surface side knuckle above the upper surface side weft 5'U. The binding yarn 3F and the binding yarn 4F form a knuckle above the upper surface side weft 1'U and the upper surface side weft 5'U, forming a single upper surface side warp design on the surface.

[0103] The non-bonding yarn 1S passes above the upper surface side weft yarn 1'U to form a surface side knuckle, then passes below the upper surface side weft yarn 3'U, then passes above the upper surface side weft yarn 5'U to form a surface side knuckle, and then passes below the upper surface side weft yarn 7'U.

[0104] In addition, the non-bonding yarn 2S passes under the upper surface side weft 1'U, then passes over the upper surface side weft 3'U to form a surface side knuckle, and then passes under the upper surface side weft 5'U, then passes over the upper surface side weft 7'U to form a surface side knuckle.

[0105] In the multilayer nonwoven fabric 50 of Example 2, as shown in FIG. 8, each of the bonding yarns F and the non-bonding yarns S is formed in pairs of two, with non-bonding yarns 1S, 2S forming pairs with bonding yarns 3F, 4F, and non-bonding yarns 5S, 6S forming pairs with bonding yarns 7F, 8F.

[0106] Next, the wefts shown in Fig. 8 will be described. There is no limit to the diameter of the upper surface side wefts (1'U, 3'U, 5'U, 7'U) and the lower surface side wefts (2'L, 4'L, 6'L, 8'L). However, the lower surface side wefts are preferably thicker in order to increase the rigidity of the fabric, and the upper surface side wefts are preferably thinner than the lower surface side wefts in order to increase the surface density. The upper surface side wefts and the lower surface side wefts in the multilayer nonwoven fabric 50 have an off-stack structure. By adopting an off-stack structure, the multilayer nonwoven fabric 50 has improved adhesion between the upper surface side wefts and the lower surface side wefts, and the spatial density is reduced, thereby suppressing fiber loss.

[0107] As is clear from the design drawing, the multi-layer nonwoven fabric 50 has a structure in which there are fewer knuckles on the reverse side than on the obverse side.

[0108] As described above, the multi-layer nonwoven fabric 50 is formed by bonding an upper side fabric consisting of upper side warps (1S, 2S, 3F, 5S, 6S, 7F) and upper side wefts (1'U, 3'U, 5'U, 7'U) and a lower side fabric consisting of lower side warps (4F, 8F) and lower side wefts (2'L, 4'L, 6'L, 8'L). The first warp threads (3F, 7F) of the upper side warps function as first bonding yarns bonding the upper side fabric and the lower side fabric, and the second warp threads (4F, 8F) of the lower side warps function as second bonding yarns bonding the upper side fabric and the lower side fabric.

[0109] In the multilayer nonwoven fabric 50 of Example 2, a resin different from the material of the yarn constituting the fabric (for example, a rubber resin classified as Group M of JIS K6397 (rubber having a polymethylene type saturated main chain)) is applied to the surface side along which the nonwoven fabric is transported.

[0110] In this way, the multilayer fabric 50 for nonwoven fabric has a resin applied to the upper fabric side, which is the side that comes into contact with the nonwoven fabric being transported, that increases the static friction coefficient, thereby improving stability (grip) when transporting the nonwoven fabric.

[0111] On the other hand, the upper surface side warp has a third warp (1S, 2S, 5S, 6S) which passes above the upper surface side weft, and then passes below the adjacent upper surface side weft and above the lower surface side weft, so that the upper surface side weft (1'U, 3'U, 5'U, 7'U) does not protrude from the surface side on which the nonwoven fabric is conveyed.

[0112] Furthermore, in the multilayer nonwoven fabric 50, the number of upper surface side warps (6) is greater than the number of lower surface side warps (2) in the complete design. This results in a denser design on the side (front side) where the nonwoven fabric is transported, improving fiber support, smoothness, and knuckle intersection support, while the opposite back side is less dense, improving breathability.

[0113] Furthermore, in the multilayer nonwoven fabric 50 of Example 2, as in the schematic diagram shown in Figure 6, the upper surface side wefts (1'U, 3'U, 5'U, 7'U) are woven so that their intersections with the upper surface side warps (1S, 2S, 5S, 6S) do not protrude from the upper surface of the upper surface side warps.

[0114] As described above, the multilayer nonwoven fabric 50 includes a pair of first and second binding yarns 3F and 4F. The first binding yarn 3F passes under two or more lower surface side wefts 8'L, 2'L to form a first lower surface side intersection, and the second binding yarn 4F passes under two or more lower surface side wefts (4L', 6'L) to form a second lower surface side intersection. The first and second lower surface side intersections are arranged alternately in the conveyance direction of the nonwoven fabric.

[0115] In this way, on the back side of the lower side fabric of the multilayer fabric 50 for nonwoven fabric, each binding yarn passes under two or more lower side wefts to form each lower side intersection. Therefore, each binding yarn is more exposed on the back side of the lower side fabric, and the area that rubs (wears) against the machine or roll is larger. As a result, the wear resistance is increased, and the life of the multilayer fabric when used as a belt can be extended.

[0116] In the multi-layer nonwoven fabric 50 of Example 2, the upper side warp density of the upper side fabric is preferably in the range of 50-90% and the lower side warp density of the lower side fabric is preferably in the range of 10-40%.

[0117] Example 3 Hereinafter, the configuration of the multilayer nonwoven fabric according to Example 3 will be described with reference to the drawings. Fig. 10 is a design diagram showing the complete design of the multilayer nonwoven fabric according to Example 3. Fig. 11 is a cross-sectional view taken along each warp thread in the design diagram shown in Fig. 10.

[0118] The multi-layer nonwoven fabric 60 according to Example 3 is a multi-layer fabric, and the upper surface side weft and the lower surface side weft are arranged so as not to overlap each other vertically. The overlap of the yarns in the design drawing is represented by the numbers indicating the yarns on the left side of the design drawing.

[0119] 10, a multi-layer nonwoven fabric 60 according to Example 3 is a multi-layer fabric formed of binding yarn F, upper surface side weft U, and lower surface side weft L. The upper surface side weft is thinner than the lower surface side weft.

[0120] As shown in Fig. 11, the binding yarn 1F passes above the lower surface side weft 1'L, then passes above the upper surface side weft 2'U to form a front side knuckle, then passes above the lower surface side weft 3'L, and passes below the lower surface side weft 5'L and lower surface side weft 7'L to form a back side knuckle, and then passes below the upper surface side weft 8'U.

[0121] The binding yarn 2F passes under the lower surface side weft 1'L and the lower surface side weft 3'L to form a back surface side knuckle, then passes under the upper surface side weft 4'U and over the upper surface side weft 6'U to form a front surface side knuckle, then passes over the lower surface side weft 7'L and under the upper surface side weft 8'U.

[0122] The binding yarn 3F passes above the lower surface side weft 1'L, then passes below the lower surface side weft 3'L and lower surface side weft 5'L to form a back surface side knuckle, and then passes below the upper surface side weft 6'U, then passes above the lower surface side weft 7'L and upper surface side weft 8'U to form a front surface side knuckle.

[0123] The binding yarn 4F passes under the lower surface side weft 1'L, then passes over the lower surface side weft 3'L and the upper surface side weft 4'U to form a front side knuckle, then passes over the lower surface side weft 5'L and under the upper surface side weft 6'U, and forms a back side knuckle under the lower surface side weft 7'L. Then it passes under the upper surface side weft 8'U.

[0124] The multilayer nonwoven fabric 60 of Example 3 has a resin (e.g., a rubber resin classified in the M group of JIS K6397 (rubber having a polymethylene type saturated main chain)) different from the material of the yarn constituting the fabric applied to the surface side along which the nonwoven fabric is transported.

[0125] In this way, the multilayer fabric 60 for nonwoven fabric has a resin applied to the upper fabric side, which is the side that comes into contact with the nonwoven fabric being transported, that increases the static friction coefficient, thereby improving stability (grip) when transporting the nonwoven fabric.

[0126] Example 4 Hereinafter, the configuration of the multilayer nonwoven fabric according to Example 4 will be described with reference to the drawings. Fig. 12 is a design diagram showing the complete design of the multilayer nonwoven fabric according to Example 4. Fig. 13 is a cross-sectional view taken along each warp thread in the design diagram shown in Fig. 12.

[0127] The multi-layer nonwoven fabric 70 according to Example 4 is a multi-layer fabric, and the upper surface side weft and the lower surface side weft are arranged so as not to overlap each other vertically. The overlap of the yarns in the design drawing is represented by the numbers indicating the yarns on the left side of the design drawing.

[0128] 12, a multi-layer nonwoven fabric 70 according to Example 4 is a multi-layer fabric formed of binding yarn F, upper surface side weft U, and lower surface side weft L. The upper surface side weft is thicker than the lower surface side weft.

[0129] As shown in Fig. 13, the binding yarn 1F passes above the upper surface side weft 7'U and the upper surface side weft 1'U to form a front side knuckle, then passes above the lower surface side weft 2'L and below the upper surface side weft 3'U, and then passes below the lower surface side weft 4'L to form a back side knuckle. Next, it passes below the upper surface side weft 5'U, and then passes above the lower surface side weft 6'L.

[0130] The binding yarn 2F passes under the upper surface side weft 1'U, then over the lower surface side weft 2'L, and over the upper surface side weft 3'U and upper surface side weft 5'U to form a front side knuckle, then over the lower surface side weft 6'L, then under the upper surface side weft 7'U, and under the lower surface side weft 8'L to form a back side knuckle.

[0131] The binding yarn 3F passes above the upper surface side weft 1'U and the upper surface side weft 3'U to form a front side knuckle, then passes above the lower surface side weft 4'L and then below the lower surface side weft 6'L to form a back side knuckle, then passes below the upper surface side weft 7'U and then above the lower surface side weft 8'L.

[0132] The binding yarn 4F passes under the upper surface side weft 1'U, then passes under the lower surface side weft 2'L to form a back surface side knuckle, then passes under the upper surface side weft 3'U and over the lower surface side weft 4'L, then passes over the upper surface side weft 5'U and over the upper surface side weft 7'U to form a front surface side knuckle, and then passes over the upper surface side weft 8'L.

[0133] The multilayer nonwoven fabric 70 of Example 4 has a resin (e.g., a rubber resin classified in the M group of JIS K6397 (rubber having a polymethylene type saturated main chain)) different from the material of the yarn constituting the fabric applied to the surface side along which the nonwoven fabric is transported.

[0134] In this way, the multilayer fabric 70 for nonwoven fabric has a resin applied to the upper fabric side, which is the side that comes into contact with the nonwoven fabric being transported, that increases the static friction coefficient, thereby improving stability (grip) when transporting the nonwoven fabric.

[0135] Example 5 Hereinafter, the configuration of the multilayer nonwoven fabric according to Example 5 will be described with reference to the drawings. Fig. 14 is a design diagram showing the complete design of the multilayer nonwoven fabric according to Example 5. Fig. 15 is a cross-sectional view taken along each warp thread in the design diagram shown in Fig. 14.

[0136] The multi-layer nonwoven fabric 80 according to Example 5 is a multi-layer fabric, and the upper surface side weft and the lower surface side weft are arranged so as to overlap each other vertically. The overlap of the yarns in the design drawing is represented by the numbers indicating the yarns on the left side of the design drawing.

[0137] A multi-layer nonwoven fabric 80 according to Example 5 shown in FIG. 14 is a multi-layer fabric constituted by binding yarns F, upper surface side wefts U, and lower surface side wefts L.

[0138] As shown in Fig. 15, the binding yarn 1F passes above the upper surface side weft 1'U to form a front surface side knuckle, then passes between the upper surface side weft 2'U and the lower surface side weft 2'L, and then passes below the lower surface side weft 3'L to form a back surface side knuckle. Then, it passes between the upper surface side weft 4'U and the lower surface side weft 4'L.

[0139] The binding yarn 2F passes between the upper surface side weft 1'U and the lower surface side weft 1'L, then passes above the upper surface side weft 2'U to form a surface side knuckle, and then passes between the upper surface side weft 3'U and the lower surface side weft 3'L, then passes below the lower surface side weft 4'L to form a back surface side knuckle.

[0140] The binding yarn 3F passes between the upper surface side weft 1'U and the lower surface side weft 1'L, then passes under the lower surface side weft 2'L to form a back surface side knuckle, and then passes between the upper surface side weft 3'U and the lower surface side weft 3'L, then passes over the upper surface side weft 4'U to form a front surface side knuckle.

[0141] The binding yarn 4F passes below the lower surface side weft 1'L to form a back surface side knuckle, then passes between the upper surface side weft 2'U and the lower surface side weft 2'L, and then passes above the upper surface side weft 3'U to form a front surface side knuckle. Then it passes between the upper surface side weft 4'U and the lower surface side weft 4'L.

[0142] The multilayer nonwoven fabric 80 of Example 5 has a resin (e.g., a rubber resin classified in the M group of JIS K6397 (rubber having a polymethylene type saturated main chain)) different from the material of the yarn constituting the fabric applied to the surface side along which the nonwoven fabric is transported.

[0143] In this way, the multilayer fabric 80 for nonwoven fabric has a resin applied to the upper fabric side, which is the side that comes into contact with the nonwoven fabric being transported, that increases the static friction coefficient, thereby improving stability (grip) when transporting the nonwoven fabric.

[0144] Example 6 Hereinafter, the structure of the multilayer nonwoven fabric according to Example 6 will be described with reference to the drawings. Fig. 16 is a design diagram showing the complete design of the multilayer nonwoven fabric according to Example 6. Fig. 17 is a cross-sectional view taken along each warp thread in the design diagram shown in Fig. 16.

[0145] The multi-layer nonwoven fabric 90 according to Example 6 is a multi-layer fabric, and the upper surface side weft and the lower surface side weft are arranged so as to overlap each other vertically. The overlapping of the yarns in the design drawing is represented by the numbers indicating the yarns on the left side of the design drawing.

[0146] A multi-layer nonwoven fabric 90 according to Example 6 shown in FIG. 16 is a multi-layer fabric constituted by binding yarns F, upper surface side wefts U, and lower surface side wefts L.

[0147] As shown in Fig. 17, the binding yarn 1F passes above the upper surface side weft 1'U and upper surface side weft 2'U to form a front side knuckle, then passes below the lower surface side weft 3'L to form a back side knuckle, and then passes between the upper surface side weft 4'U and lower surface side weft 4'L.

[0148] The binding yarn 2F passes between the upper surface side weft 1'U and the lower surface side weft 1'L, passes above the upper surface side weft 2'U and the upper surface side weft 3'U to form a surface side knuckle, and then passes below the lower surface side weft 4'L to form a back surface side knuckle.

[0149] The binding yarn 3F passes above the upper surface side weft 4'U and the upper surface side weft 1'U to form a front side knuckle, then passes below the lower surface side weft 2'L to form a back side knuckle, and then passes between the upper surface side weft 3'U and the lower surface side weft 3'L.

[0150] The binding yarn 4F passes under the lower surface side weft 1'L to form a back surface side knuckle, then passes between the upper surface side weft 2'U and the lower surface side weft 2'L, and passes over the upper surface side weft 3'U and the upper surface side weft 4'U to form a front surface side knuckle.

[0151] The multilayer nonwoven fabric 90 of Example 6 has a resin (e.g., a rubber resin classified in the M group of JIS K6397 (rubber having a polymethylene type saturated main chain)) different from the material of the yarn constituting the fabric applied to the surface side along which the nonwoven fabric is transported.

[0152] In this way, the multilayer fabric 90 for nonwoven fabric has a resin applied to the upper fabric side, which is the side that comes into contact with the nonwoven fabric being transported, that increases the static friction coefficient, thereby improving stability (grip) when transporting the nonwoven fabric.

[0153] Example 7 Hereinafter, the configuration of the multilayer nonwoven fabric according to Example 7 will be described with reference to the drawings. Fig. 18 is a design diagram showing the complete design of the multilayer nonwoven fabric according to Example 7. Fig. 19 is a cross-sectional view taken along each warp thread in the design diagram shown in Fig. 18.

[0154] The multi-layer nonwoven fabric 92 according to Example 7 is a multi-layer fabric, and the upper surface side weft and the lower surface side weft are arranged so as to overlap each other vertically. The overlap of the yarns in the design drawing is represented by the numbers indicating the yarns on the left side of the design drawing.

[0155] A multi-layer nonwoven fabric 92 according to Example 7 shown in FIG. 18 is a multi-layer fabric constituted by binding yarns F, upper surface side wefts U, and lower surface side wefts L.

[0156] As shown in Figure 19, the binding yarn 1F passes above the upper surface side weft 1'U to form a surface side knuckle, then passes between the upper surface side weft 2'U and the lower surface side weft 2'L, and passes below the lower surface side weft 3'L and the lower surface side weft 4'L to form a back surface side knuckle.

[0157] The binding yarn 2F passes under the lower surface side weft 4'L and the lower surface side weft 1'L to form a back surface side knuckle, then passes over the upper surface side weft 2'U to form a front surface side knuckle, and then passes between the upper surface side weft 3'U and the lower surface side weft 3'L.

[0158] The binding yarn 3F passes between the upper surface side weft 1'U and the lower surface side weft 1'L, then passes under the lower surface side weft 2'L and the lower surface side weft 3'L to form a back surface side knuckle, and then passes over the upper surface side weft 4'U to form a front surface side knuckle.

[0159] The binding yarn 4F passes under the lower surface side weft 1'L and lower surface side weft 2'L to form a back surface side knuckle, then passes over the upper surface side weft 3'U to form a front surface side knuckle, and then passes between the upper surface side weft 4'U and lower surface side weft 4'L.

[0160] The multilayer nonwoven fabric 92 of Example 7 has a resin (e.g., a rubber resin classified in the M group of JIS K6397 (rubber having a polymethylene type saturated main chain)) different from the material of the yarn constituting the fabric applied to the surface side along which the nonwoven fabric is transported.

[0161] In this way, the multilayer fabric 92 for nonwoven fabric has a resin applied to the upper fabric side, which is the side that comes into contact with the nonwoven fabric being transported, that increases the static friction coefficient, thereby improving stability (grip) when transporting the nonwoven fabric.

[0162] Example 8 Fig. 21 is a design drawing showing the complete design of the multi-layer nonwoven fabric according to Example 8. Fig. 22 is a cross-sectional view taken along each warp thread in the design drawing shown in Fig. 21.

[0163] The multilayer nonwoven fabric 94 of Example 8 shown in Figure 21 is a multilayer fabric with a surface plain weave structure composed of, from the left, warp pair A (1Ub and 1Lb), warp pair B (2U and 2L), warp pair C (3Ub and 3Lb), warp pair D (4U and 4L), and upper surface side wefts (1'U, 2'U, 3'U, 4'U) and lower surface side wefts (1'L, 2'L, 3'L, 4'L).

[0164] 21 and 22, the multilayer nonwoven fabric 94 according to Example 8 has a plain weave weave for both the upper fabric on the front side and the lower fabric on the back side. A nonwoven belt using the multilayer nonwoven fabric 94 with a regular plain weave weave on the front side has a large number of fiber support points in the fabric that supports the nonwoven web, improving the support of the nonwoven web. Furthermore, the plain weave upper fabric has a high intersection support strength and prevents fibers from penetrating.

[0165] Moreover, the multi-layered nonwoven fabric 94 according to Example 8 is woven under conditions in which the difference between the height h1 (height from the reference position X) of the first knuckle by the warp binding yarns (1Ub, 1Lb, 3Ub, 3Lb) and the height h2 (height from the reference position X) of the second knuckle by the upper surface side warp yarns (2U, 4U) is about 80 μm, as shown in FIG. 22. That is, the height difference |h1-h2| between the first knuckle and the second knuckle is larger than the height difference |h1-h2| of the knuckle in the conventional multi-layered nonwoven fabric, thereby improving the gripping property against the nonwoven fabric. In Example 8, the height h1 of the first knuckle is higher than the height h2 of the second knuckle. The reference position X may be any position as long as the height difference between the knuckles can be calculated.

[0166] In addition, the multi-layer nonwoven fabric 94 according to Example 8 can provide height differences in the knuckles of the warp yarns, so that the resin applied to the lower knuckles is protected from wear. As a result, the effect of improving gripping properties by the resin can be sustained for a long time.

[0167] Example 9 Fig. 23 is a design drawing showing the complete design of the multi-layer nonwoven fabric according to Example 9. Fig. 24 is a cross-sectional view taken along each warp thread in the design drawing shown in Fig. 23.

[0168] In the multilayer nonwoven fabric 96 of Example 9, an upper side fabric composed of upper side warps (1Ub, 2U) and upper side wefts (1'U, 2'U, 3'U, 4'U) and a lower side fabric composed of lower side warps (1Lb, 2L) and lower side wefts (1'L, 2'L, 3'L, 4'L) are bound together by warp binding yarns (1Ub, 1Lb). The multilayer nonwoven fabric 96 of Example 9 has the same weaving method and knuckle size as the multilayer nonwoven fabric 94 of Example 8, except that the upper side warps (3Ub, 4U) and lower side warps (3Lb, 4L) in the multilayer nonwoven fabric 94 of Example 8 are not included. In the multilayer fabric for nonwoven fabric of Example 9, the height difference |h1-h2| between the first knuckle and the second knuckle is also larger than the height difference |h1-h2| between the knuckles in the conventional multilayer fabric for nonwoven fabric, thereby improving the grip on the nonwoven fabric.

[0169] In addition, the multi-layer nonwoven fabric 96 according to Example 9 can provide height differences in the knuckles of the warp yarns, so that the resin applied to the lower knuckles is protected from wear. As a result, the effect of improving gripping properties by the resin can be sustained for a long time.

[0170] (Modification) Some of the warp yarns form loops at both ends further outside than the weft yarns included in the complete design, and a pintle wire is passed through each loop so that the upper surface side fabric is located on the surface side along which the nonwoven fabric is transported, thereby making each multi-layer nonwoven fabric into an endless nonwoven fabric belt.

[0171] The diameter of each yarn is, for example, in the range of 0.10 to 1.20 mm. For example, the upper surface side warp may have a diameter of 0.40 mm, the lower surface side warp may have a diameter of 0.40 mm, the upper surface side weft may have a diameter of 0.50 mm, and the lower surface side weft may have a diameter of 0.50 mm.

[0172] The yarns used for the warp and weft in the above-mentioned embodiments and examples may be appropriately selected depending on the purpose and the place of use. For example, the cross-sectional shape of the yarn is not limited to a circle, and yarns such as square or star-shaped yarns, elliptical yarns, hollow yarns, and yarns with a core-sheath structure may be used. The material of the yarn may be freely selected within a range that satisfies the desired characteristics, and polyethylene terephthalate, polyester, polyamide, polyphenylene sulfide, polyvinylidene fluoride, polypropylene, aramid, polyether ether ketone, polyethylene naphthalate, polytetrafluoroethylene, cotton, wool, metal, thermoplastic polyurethane, thermoplastic elastomer, and the like may be used. Of course, it is also possible to use yarns in which various substances are blended or contained in copolymers or these materials according to the purpose. In general, it is preferable to use polyester monofilaments, which have rigidity and excellent dimensional stability, as yarns constituting nonwoven fabrics. In addition, conductive carbon yarns may be woven into the yarn.

[0173] The resin may be applied to the belt by a coater roll, spray, brush, or immersion. In particular, when the resin is applied by spraying, the resin is less unevenly applied, and the possibility of the resin blocking the mesh is reduced. In addition, the gripping force of the belt may be increased by weaving a high-friction thread into the surface that has been previously coated with the resin according to the present embodiment. The nonwoven fabric according to the present embodiment is suitable for use in the manufacture of nonwoven fabrics by the spunbond method, meltblowing method, hydroentanglement, dry method, airlaid method, calendar method, wet method, chemical bond method, thermal bond method, and needle punch method.

[0174] Although the present invention has been described above with reference to the above-mentioned embodiment, the present invention is not limited to the above-mentioned embodiment, and suitable combinations or substitutions of the configurations of the embodiment are also included in the present invention. In addition, it is possible to suitably rearrange the combinations and processing order in the embodiment based on the knowledge of a person skilled in the art, and to make modifications such as various design changes to the embodiment, and the embodiment to which such modifications have been made is also included in the scope of the present invention. [Explanation of symbols]

[0175] 10 Nonwoven fabric manufacturing equipment, 12 Nonwoven fabric belts, 18 Nonwoven fabric, 40,50,60,70,80,90,92,108 Multi-layer fabrics for nonwoven fabrics, 132 Cotton.

Claims

1. A nonwoven fabric having a rubber resin classified as Group R (rubber having unsaturated carbon bonds in the main chain) of JIS K6397 applied to the surface side on which the nonwoven fabric is transported.

2. 2. The nonwoven fabric according to claim 1, wherein the rubber resin is styrene-butadiene rubber.

3. The surface on which the nonwoven fabric is transported is coated with a rubber resin that is classified as Group M of JIS K6397 (rubber having a polymethylene-type saturated main chain). A fabric for nonwoven fabric, characterized in that the difference between the height of warp knuckles formed by warp yarns on the surface side along which the nonwoven fabric is transported and the height of weft knuckles formed by weft yarns is 100 μm or more.

4. 4. The nonwoven fabric according to claim 3, wherein the rubber resin is an acrylic rubber.

5. 5. The nonwoven fabric according to claim 1, wherein the rubber resin is water-soluble before curing.

6. The fabric for nonwoven fabric according to any one of claims 1 to 5, characterized in that the static friction coefficient of the surface side is in the range of 0.25 to 0.

90.

7. The surface of the nonwoven fabric that is being transported is coated with a resin that is different from the material of the threads that make up the fabric. The static friction coefficient of the surface side is in the range of 0.25 to 0.90, A fabric for nonwoven fabric, characterized in that the difference between the height of warp knuckles formed by warp yarns on the surface side along which the nonwoven fabric is transported and the height of weft knuckles formed by weft yarns is 100 μm or more.

8. A nonwoven fabric as described in any one of claims 1 to 7, characterized in that when cotton is pressed against a multilayer nonwoven fabric inclined with the surface side along which the nonwoven fabric is transported being vertically inclined, the time from when the cotton is released until the fabric falls is 10 seconds or less.

9. 2. The nonwoven fabric according to claim 1, wherein the difference between the height of the warp knuckles formed by the warp yarns on the surface side along which the nonwoven fabric is transported and the height of the weft knuckles formed by the weft yarns is 100 μm or more.

10. 10. The nonwoven fabric according to claim 1, wherein conductive yarn is woven into the fabric.

11. 8. The nonwoven fabric according to claim 7, wherein the resin has a durometer hardness of 10 to 80 after curing.

12. A resin having a durometer hardness of 10 to 80 after curing is applied to the surface side along which the nonwoven fabric is conveyed, A fabric for nonwoven fabric, characterized in that the difference between the height of warp knuckles formed by warp yarns on the surface side along which the nonwoven fabric is transported and the height of weft knuckles formed by weft yarns is 100 μm or more.

13. The woven fabric according to claim 12, characterized in that the durometer hardness is 50 to 80.

14. The woven fabric according to claim 12, characterized in that the durometer hardness is 10 to 20.

15. A conveyor belt for spunbond nonwoven fabrics, comprising the nonwoven fabric according to any one of claims 1 to 14.

Citation Information

Patent Citations

  • Photo thyristor

    JP1994021436A

  • Dryer canvas for papermaking

    JP2004300621A

  • Industrial fabric with silicone-coated surface

    JP2006512502A

  • Bilayer fabric for nonwoven fabric

    JP2017197883A

  • Fabric belt for producing web material, in particular for producing spunbonded fabric

    US20170260664A1