Asphalt Compositions Comprising Reclaimed Polymers and Epoxy-Functionalized Ethylene Copolymers
Incorporating recycled polymers and epoxy-functionalized ethylene copolymers into asphalt compositions addresses rutting and fatigue cracking issues, improving performance and sustainability by enhancing rheological and tensile properties.
Patent Information
- Application Number
- JP2021543397
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-10
- Filing Date
- 2020-01-31
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2040-01-31
AI Technical Summary
Asphalt compositions used in pavements often suffer from rutting and fatigue cracking due to excessive stiffness and thermal cracking at low temperatures, necessitating improved resistance to failure modes in various temperature conditions.
Incorporating a recycled polymer component and an epoxy-functionalized ethylene copolymer into asphalt compositions to enhance rheological and tensile properties, thereby increasing resistance to rutting and fatigue cracking.
The combination of recycled polymers and epoxy-functionalized ethylene copolymers improves asphalt compositions' resistance to rutting and fatigue cracking across varying temperatures, while also enhancing sustainability by utilizing recycled materials.
Smart Images

Figure 0007561739000001 
Figure 0007561739000002 
Figure 0007561739000003
Abstract
Description
[Technical field]
[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to U.S. Provisional Patent Application No. 62 / 799,536, filed January 31, 2019, and U.S. Provisional Patent Application No. 62 / 859,505, filed June 10, 2019, the entire disclosures of which are incorporated herein by reference.
[0002] FIELD OF THE DISCLOSURE Embodiments described herein relate generally to asphalt, and specifically to asphalt compositions that include recycled polymer components and epoxy-functionalized ethylene copolymers. [Background technology]
[0003] Asphalt compositions are often used as construction materials. For example, asphalt compositions can be used as pavements in the construction of roads. Several factors can affect the performance of a pavement, including bitumen quality, source of raw materials, traffic loads, and more recently, sustainability considerations.
[0004] Repeated loading may result in fatigue cracking or permanent deformation, known as "rutting." It is believed that the elasticity and cracking properties of the asphalt binder may play a role in such failure modes. For example, an asphalt binder with excessive stiffness may be insufficient to prevent permanent deformation due to repeated loading. Furthermore, thermal cracking may occur at relatively low temperatures when stress exceeds the tensile strength of the pavement. Thus, an asphalt composition may exhibit improved rutting, fatigue cracking, and thermal cracking resistance by having higher elastic properties in various temperature regimes. Summary of the Invention [Problem to be solved by the invention]
[0005] Therefore, there is a need for asphalt compositions with properties that may enhance resistance to failure modes such as rutting and fatigue cracking under various temperature regimes. [Means for solving the problem]
[0006] Embodiments of the present disclosure meet those needs by providing an asphalt composition that may include an asphalt binder, a recycled polymer component, and an epoxy-functionalized ethylene copolymer. Effect of the Invention
[0007] Without being bound by theory, it is believed that the recycled polymer component may enhance the resistance to permanent set with respect to the modified asphalt composition's resistance to rutting and fatigue in various temperature regimes. Additionally, it is believed that functionalization of polymers, such as the epoxy-functionalized ethylene copolymers described herein, may be an effective route to chemically bond materials to enhance the rheological and tensile properties of asphalt compositions containing bitumen.
[0008] Furthermore, incorporating recycled polymer components into asphalt compositions may be a sustainable option. Agencies in many jurisdictions around the world, including the United States Department of Transportation (DOT) and many states, have approved recycled materials that can be incorporated into asphalt compositions. Some recycled materials can include ground rubber tires (GTR), recycled asphalt pavement (RAP), and recycled asphalt shingles (RAS). In other regions, such as India and some Association of Southeast Asian Nations (ASEAN) countries, local governments have sponsored and even regulated the use of waste plastic packaging in asphalt. Post-industrial recycling (PIR) and post-consumer recycling (PCR) are generally considered plastic packaging used by consumers or industries from commercially available selected sources.
[0009] The asphalt composition embodiments described herein may incorporate recycled polymer components with epoxy-functionalized ethylene copolymers, which may provide improved resistance to rutting or fatigue cracking in various temperature regimes, as well as increased sustainability benefits. Compared to asphalt compositions containing unrecycled polymer components, the asphalt compositions described herein may have improved or equivalent resistance to rutting or fatigue cracking in various temperature regimes. However, compared to asphalt compositions having unrecycled polymer components, while having improved or equivalent properties, the asphalt compositions described herein may further increase sustainability benefits.
[0010] However, the incorporation of recycled polymers has traditionally resulted in asphalt compositions with undesirable fatigue and thermal cracking. Alternatively, some conventional asphalt compositions incorporate styrene / conjugated diene copolymers or epoxy-functionalized ethylene copolymers, either alone or in combination.
[0011] Thus, the presently described asphalt compositions that may include epoxy-functionalized ethylene copolymers may exhibit improved performance (i.e., relatively higher elasticity) compared to asphalt compositions having only recycled polymer components. Additionally, the asphalt compositions described herein may exhibit improved performance (i.e., relatively higher elasticity and resistance to fatigue and thermal cracking) over asphalt compositions that incorporate recycled polymer components and styrene / conjugated diene copolymers.
[0012] According to at least one embodiment of the present disclosure, an asphalt composition is provided. An embodiment of the asphalt composition may include, based on the total weight of the asphalt composition, about 70 to about 99.5 wt% of an asphalt binder; about 0.25 to 20 wt% of a recycled polymer component, based on the total weight of the asphalt composition; and about 0.1 to 10 wt% of an epoxy-functionalized ethylene copolymer, based on the total weight of the asphalt composition, having the formula E / X / Y / Z. E may be a copolymer unit -(CH2CH2)- derived from ethylene, and X is a copolymer unit -(CH2CR)- present at 0 to about 40 wt% of the copolymer. 1 R 2 )-, where R 1 is hydrogen, methyl, or ethyl; R 2 is a carboalkoxy, acyloxy, or alkoxy of 1 to 10 carbon atoms, and Y is a copolymer unit -(CHCR 3 R 4 )-, where R 3 is hydrogen or methyl, R 4 is carboglycidoxy or glycidoxy, and Z can be a copolymer derived from comonomers including carbon monoxide, sulfur dioxide, acrylonitrile, or other monomers, present at 0 to about 10 wt% of the copolymer. Thus, embodiments of the present disclosure can provide compositions with improved properties that can increase resistance to rutting or fatigue cracking in various temperature regimes. Embodiments of the present disclosure can also provide compositions that are sustainable or environmentally friendly.
[0013] According to at least another embodiment of the present disclosure, a method of making an asphalt composition is provided. An embodiment of the method can include combining an asphalt binder, a recycled polymer component, and an epoxy-functionalized ethylene copolymer having the formula E / X / Y / Z. E can be a copolymer unit -(CH2CH2)- derived from ethylene, and X can be a copolymer unit -(CH2CR)- present at 0 to about 40 wt% of the copolymer. 1 R 2 )-, where R 1is hydrogen, methyl, or ethyl; R 2 is a carboalkoxy, acyloxy, or alkoxy of 1 to 10 carbon atoms, and Y is a copolymer unit -(CHCR 3 R 4 )-, where R 3 is hydrogen or methyl, R 4 is carboglycidoxy or glycidoxy, and Z can optionally be a copolymer derived from comonomers including carbon monoxide, sulfur dioxide, acrylonitrile, or other monomers present at 0 to about 10 wt % of the copolymer.
[0014] These and other embodiments are described in more detail in the detailed description of the invention below. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Certain embodiments of the present application will now be described. These embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the subject matter to those skilled in the art.
[0016] The term "polymer" refers to a polymeric compound prepared by polymerizing monomers, whether of the same or different types. Thus, the general term polymer encompasses the term "homopolymer," which usually refers to a polymer prepared from only one type of monomer, and "copolymer" refers to a polymer prepared from two or more different monomers. As used herein, the term "interpolymer" refers to a polymer prepared by polymerization of at least two different types of monomers. Thus, the general term interpolymer includes copolymers or polymers prepared from two or more different types of monomers, such as terpolymers.
[0017] "Polyethylene" or "ethylene-based polymer" shall mean a polymer containing greater than 50 mole percent units derived from ethylene monomer. This includes ethylene-based homopolymers or copolymers (meaning units derived from two or more comonomers). Common forms of ethylene-based polymers known in the art include, but are not limited to, low density polyethylene (LDPE), linear low density polyethylene (LLDPE), ultra low density polyethylene (ULDPE), very low density polyethylene (VLDPE), single-site catalyzed linear low density polyethylene including both linear and substantially linear low density resins (m-LLDPE), medium density polyethylene (MDPE), and high density polyethylene (HDPE).
[0018] As used herein, the term "propylene-based polymer" refers to a polymer that contains, in polymerized form, greater than 50 mole percent units derived from propylene monomers, including propylene homopolymers, random copolymer polypropylenes, impact copolymer polypropylenes, propylene / α-olefin copolymers, and propylene / α-olefin copolymers.
[0019] The term "LLDPE" includes resins made using Ziegler-Natta catalyst systems and resins made using single-site catalysts, including, but not limited to, resins made using bismetallocene catalysts (sometimes referred to as "m-LLDPE"), phosphinimine, constrained geometry catalysts, and post-metallocene molecular catalysts, including, but not limited to, bis(biphenylphenoxy) catalysts (also referred to as polyaryloxy ether catalysts). LLDPE includes linear, substantially linear, or heterogeneous ethylene-based copolymers or homopolymers. LLDPE contains less long chain branching than LDPE and includes substantially linear ethylene polymers, as further defined in U.S. Patents 5,272,236, 5,278,272, 5,582,923, and 5,733,155, homogeneously branched linear ethylene polymer compositions such as those described in U.S. Patent 3,645,992, heterogeneously branched ethylene polymers such as those prepared according to the process disclosed in U.S. Patent 4,076,698, and blends thereof (e.g., those disclosed in U.S. Patents 3,914,342 and 5,854,045). LLDPE resins may be made by gas phase, liquid phase, or slurry polymerization, or any combination thereof, using any type of reactor or reactor configuration known in the art.
[0020] The term "HDPE" refers to ethylene-based polymers having a density greater than about 0.940 g / cc, and are generally prepared with Ziegler-Natta, chromium, or even metallocene catalysts.
[0021] As used herein, the term "asphalt" is a complex mixture that can be separated into two major portions of hydrocarbons, asphaltenes and maltenes. Asphaltenes can be polyaromatic and can include polyaromatic with mostly polar functional groups. One or more of the following functional groups may be present: carboxylic acid, amine, sulfide, sulfoxide, sulfone, sulfonic acid, porphyrin, porphyrin derivative, metalloporphyrin or metalloporphyrin derivative with vanadium, nickel or iron cations. The maltene phase can include polar aromatics, aromatics, and naphthenes. Without being bound by theory, it is generally believed that asphalt can be a colloidal dispersion of asphaltenes dispersed in maltenes, with polar aromatics acting as dispersants. Asphaltenes have a relatively high molecular weight (about 1500 Daltons) compared to other components of asphalt. Asphaltenes are amphoteric in nature and can form aggregates through self-association that provide asphalt with viscoelastic behavior. Asphaltene may vary in amount and function depending on the crude oil source from which the asphalt is derived. Specific examples of suitable crude asphalts include Ajax, Marathon, Wyoming Sour, Mayan, Venezuelan, Canadian, Arabian, Trinidad Lake, Salamanca, Brazilian, Argentinean, Uruguayan, Chilean, and combinations of two or more thereof. Asphalt Binder. The term "asphalt" may include "asphalt binders" including one or more of bitumen, asphaltenes; heterocyclic compounds containing sulfur, nitrogen, and oxygen; and trace metals such as iron, nickel, and vanadium. The term "asphalt" may further include aggregates. Aggregates may include stone, sand, gravel, and combinations thereof.
[0022] Reference will now be made in detail to embodiments of the asphalt composition as described herein. The embodiments of the asphalt composition may include an asphalt binder, a recycled polymer component, and an epoxy-functionalized ethylene copolymer.
[0023] In embodiments, the asphalt compositions described herein may include an asphalt binder, which may be referred to as the "asphalt component" of the asphalt composition. In some embodiments, the asphalt binder may include a petroleum derivative. The asphalt binder may include bitumen. Bitumen may be saturated and unsaturated hydrocarbons (e.g., aliphatic and aromatic hydrocarbons). Additionally, the asphalt binder may include one or more asphaltenes; heterocyclic compounds containing sulfur, nitrogen, and oxygen; and trace metals such as iron, nickel, and vanadium. In some embodiments, the asphalt binder may be commercially available. In some embodiments, the asphalt binder may be naturally occurring. In some embodiments, the asphalt binder may include about 70 weight percent (wt%) to 100 wt% bitumen, based on the total weight of the asphalt binder. In other embodiments, the asphalt binder may be at least 90% bitumen. In other embodiments, the asphalt may include up to 100 wt% bitumen.
[0024] In embodiments, the asphalt composition may comprise from about 70 weight percent (wt%) to about 99.5 wt% of the asphalt binder based on the total weight of the asphalt composition. In some embodiments, the asphalt composition may comprise from about 70 wt% to about 95 wt%, from about 70 wt% to about 90 wt%, from about 70 wt% to about 85 wt%, from about 70 wt% to about 80 wt%, from about 70 wt% to about 75 wt%, from about 75 wt% to about 99.5 wt%, from about 75 wt% to about 95 wt%, from about 75 wt% to about 90 wt%, from about 75 wt% to about 8 ... % to about 80 wt%, about 80 wt% to about 99.5 wt%, about 80 wt% to about 95 wt%, about 80 wt% to about 90 wt%, about 80 wt% to about 85 wt%, about 85 wt% to about 99.5 wt%, about 85 wt% to about 95 wt%, about 85 wt% to about 90 wt%, about 90 wt% to about 99.5 wt%, about 90 wt% to about 95 wt%, or about 95 wt% to about 99.5 wt% asphalt binder.
[0025] In embodiments, the asphalt composition may include a recycled polymer component. The recycled polymer component may include polymeric materials that have previously undergone a thermoforming or extrusion process. As used herein, the recycled polymer component may include post-industrial recycled (PIR) or post-consumer recycled (PCR) polymeric materials that have been modified in some way for reuse. In some embodiments, the recycled polymer component may be commercially sourced post-consumer or industrially used plastic packaging. In further embodiments, the recycled polymer component may include PCR plastic packaging products that have been used by consumers and modified in some way for reuse. In embodiments, the recycled polymer component may include one or more of ethylene-based polymers, propylene-based polymers, polyesters, poly(vinyl chloride), polystyrene, acrylonitrile butadiene styrene, polyamides, ethylene vinyl alcohol, ethylene vinyl acetate, polyvinyl chloride, and / or functionalized copolymers of ethylene or propylene with maleic anhydride, methacrylic acid, or acrylic acid, such as FUSABOND™, AMPLIFY™, BYNEL™, SURLYN™, NUCREL™ (used as a tie layer in a multi-layer structure). In embodiments, the recycled polymer component may include up to 99.99 wt% of one or more of ethylene-based polymers, propylene-based polymers, polyesters, poly(vinyl chloride), polystyrene, acrylonitrile butadiene styrene, polyamides, ethylene vinyl alcohol, ethylene vinyl acetate, or polyvinyl chloride, based on the total weight of the recycled polymer component. In other embodiments, the recycled polymer component may include from about 51 wt% to about 99.99 wt%, from about 60 wt% to about 99.99 wt%, from about 70 wt% to about 99.99 wt%, from about 80 wt% to about 99.99 wt%, or from about 90 wt% to about 99.99 wt% of one or more of an ethylene-based polymer, a propylene-based polymer, a polyester, poly(vinyl chloride), polystyrene, acrylonitrile butadiene styrene, a polyamide, ethylene vinyl alcohol, ethylene vinyl acetate, or polyvinyl chloride, based on the total weight of the recycled polymer component.In a further embodiment, the recycled polymer component may include an ethylene-based polymer.
[0026] In embodiments, the recycled polymer component may include one or more contaminants. The contaminants may be the result of the use of the polymeric material before it is modified for reuse. In some embodiments, the contaminants may include paper, ink, food residues, or other recycled materials in addition to the polymer resulting from the recycling process. In one particular embodiment, the recycled polymer component may include PCR polymeric material and paper resulting from plastic packaging with a paper label. In embodiments, the recycled polymer component may include at least 0.01 wt% of contaminants based on the total weight of the recycled polymer component. In other embodiments, the recycled polymer component may include at least about 0.01 wt% to about 1 wt%, about 0.01 wt% to about 5 wt%, about 0.01 wt% to about 10 wt%, about 0.01 wt% to about 20 wt%, about 0.01 wt% to about 30 wt%, or about 0.01 wt% to about 40 wt% of contaminants based on the total weight of the recycled polymer component.
[0027] In embodiments, the recycled polymer component may exhibit color characteristics. In embodiments, the recycled polymer component may include one or more contaminants, so that the recycled polymer component may exhibit color characteristics that differ from the color characteristics of the polymer prior to being recycled. For example, in embodiments, the recycled polymer component may have a non-zero yellowness index. In further embodiments, the recycled polymer component may have a yellowness index of greater than 5, as measured according to ASTM D6290. In some embodiments, for example, if the recycled polymer component has a blue color, the yellowness of the recycled polymer component may have a yellowness index of less than 0. Without being bound by theory, according to the International Commission on Illumination (CIE), L * a * b * The color space is modeled on the opponent color theory, which states that no two colors can be simultaneously red and green or yellow and blue. * (Sample L * From standard L *The difference between light and dark is defined as the difference between light and dark, with more positive values indicating lighter colors and more negative values indicating darker colors. * (Sample a * From standard a * Δb (defined as the difference between red and green, with more positive values indicating more red colors and more negative values indicating more green colors) * (Sample b * From standard b * L (defined as the difference between yellow and blue), indicates the difference between yellow and blue, with more positive values indicating more yellow and more negative values indicating more blue. * is the brightness, a * are the red / green coordinates, and b * indicates the yellow / blue coordinates. ΔL * , Δa * , and Δb * can be positive (+) or negative (-). However, the total difference ΔE * is always positive.
[0028] The incorporation of recycled polymer components into the asphalt composition can provide sustainability benefits to the asphalt composition. In further embodiments, while providing sustainability benefits, the presently described asphalt compositions can be resistant to failure modes such as rutting and cracking in various temperature regimes. Furthermore, when compared to asphalt compositions that include a non-recycled polymer component while having improved or comparable properties, the asphalt compositions described herein can further enhance sustainability benefits. In some embodiments, the recycled polymer component can include HDPE. In some embodiments, the recycled polymer component can include LLDPE. In further embodiments, the recycled polymer component can include a combination of HDPE and LLDPE.
[0029] In further embodiments, the recycled polymer component is from about 0.858 grams per cubic centimeter (g / cc) to about 0.918 g / cc, from about 0.858 g / cc to about 0.910 g / cc, from about 0.858 g / cc to about 0.900 g / cc, from about 0.858 g / cc to about 0.890 g / cc, from about 0.858 g / cc to about 0.880 g / cc, from about 0.858 g / cc to about 0.870 g / cc, from about 0.870 grams per cubic centimeter (g / cc) to about 0.918 g / cc, from about 0.870 g / cc to about 0.910 g / cc, from about 0.870 g / cc to about 0.900 g / cc, from about 0.870 g / cc to about 0.890 g / cc, from about 0.870 g / cc to about 0.880 g / cc, The LLDPE may have a density of from about 0.880 grams per cubic centimeter (g / cc) to about 0.918 g / cc, from about 0.880 g / cc to about 0.910 g / cc, from about 0.880 g / cc to about 0.900 g / cc, from about 0.880 g / cc to about 0.890 g / cc, from about 0.890 grams per cubic centimeter (g / cc) to about 0.918 g / cc, from about 0.890 g / cc to about 0.910 g / cc, from about 0.890 g / cc to about 0.900 g / cc, from about 0.900 grams per cubic centimeter (g / cc) to about 0.918 g / cc, from about 0.900 g / cc to about 0.910 g / cc, or from about 0.910 grams per cubic centimeter (g / cc) to about 0.918 g / cc.
[0030] In some embodiments, the recycled polymer component may include an LLDPE having a melt index I2 of less than about 20 grams per 10 minutes (g / 10min) when measured according to ASTM D1238 at 190° C. and a load of 2.16 kg. In further embodiments, the LLDPE may have a melt index I2 of less than about 0.1 g / 10 min to about 20.0 g / 10 min, about 0.1 g / 10 min to about 15.0 g / 10 min, about 0.1 g / 10 min to about 10.0 g / 10 min, about 0.1 g / 10 min to about 5 g / 10 min, about 0.1 g / 10 min to about 1.0 g / 10 min, about 0.1 g / 10 min to about 0.5 g / 10 min, about 1.0 g / 10 min to about 20.0 g / 10 min, about 1.0 g / 10 min to about 15.0 g / 10 min, about 1. The melt index I2 may be from 0 g / 10 min to about 10.0 g / 10 min, from about 1.0 g / 10 min to about 5 g / 10 min, from about 5.0 g / 10 min to about 20.0 g / 10 min, from about 5.0 g / 10 min to about 15.0 g / 10 min, from about 5.0 g / 10 min to about 10.0 g / 10 min, from about 10.0 g / 10 min to about 20.0 g / 10 min, from about 10.0 g / 10 min to about 15.0 g / 10 min, or from about 15.0 g / 10 min to about 20.0 g / 10 min.
[0031] In further embodiments, the recycled polymer component can have a density of from about 0.940 g / cc to about 0.970 g / cc, from about 0.940 g / cc to about 0.960 g / cc, from about 0.940 g / cc to about 0.950 g / cc, from about 0.950 g / cc to about 0.970 g / cc, from about 0.950 g / cc to about 0.960 g / cc, or from about 0.960 g / cc to about 0.970 g / cc.
[0032] In some embodiments, the recycled polymer component may include HDPE with a melt index I2 of less than about 20 grams per 10 minutes (g / 10min) when measured according to ASTM D1238 at 190° C. and a load of 2.16 kg. In further embodiments, the HDPE may have a melt index I2 of less than about 0.1 g / 10 min to about 20.0 g / 10 min, about 0.1 g / 10 min to about 15.0 g / 10 min, about 0.1 g / 10 min to about 10.0 g / 10 min, about 0.1 g / 10 min to about 5 g / 10 min, about 0.1 g / 10 min to about 1.0 g / 10 min, about 0.1 g / 10 min to about 0.5 g / 10 min, about 1.0 g / 10 min to about 20.0 g / 10 min, about 1.0 g / 10 min to about 15.0 g / 10 min, about 1.0 The melt index I2 may be from about 1.0 g / 10 min to about 5 g / 10 min, from about 5.0 g / 10 min to about 20.0 g / 10 min, from about 5.0 g / 10 min to about 15.0 g / 10 min, from about 5.0 g / 10 min to about 10.0 g / 10 min, from about 10.0 g / 10 min to about 20.0 g / 10 min, from about 10.0 g / 10 min to about 15.0 g / 10 min, or from about 15.0 g / 10 min to about 20.0 g / 10 min.
[0033] In embodiments, the asphalt composition may include from about 0.25 weight percent (wt%) to about 20 wt% of the recycled polymer component, based on the total weight of the asphalt composition. In some embodiments, the asphalt composition may comprise from about 0.25 wt% to about 20 wt%, from about 0.25 wt% to about 15 wt%, from about 0.25 wt% to about 10 wt%, from about 0.25 wt% to about 5 wt%, from about 0.25 wt% to about 1 wt%, from about 1 wt% to about 20 wt%, from about 1 wt% to about 15 wt%, from about 1 wt% to about 10 wt%, from about 1 wt% to about 5 wt%, from about 5 wt% to about 20 wt%, from about 5 wt% to about 15 wt%, from about 5 wt% to about 10 wt%, from about 10 wt% to about 20 wt%, from about 10 wt% to about 15 wt%, or from about 15 wt% to about 20 wt%, based on the total weight of the asphalt composition.
[0034] In an embodiment, the asphalt composition may include an epoxy-functionalized ethylene copolymer, which may be represented by the formula E / X / Y / X, including copolymer units E, X, Y, and Z.
[0035] In an embodiment, E is 、 The copolymer units derived from ethylene may be -(CH2CH2)-.
[0036] In an embodiment, X is a copolymer unit -(CHCR 1 R 2 In some embodiments, R 1 can be hydrogen, methyl, or ethyl. In some embodiments, R 2 is a carboalkoxy, acyloxy, or alkoxy of 1 to 10 carbon atoms. In further embodiments, the epoxy-functionalized ethylene copolymer may comprise from about 0 wt% to about 40 wt% X, from about 0 wt% to about 30 wt% X, from about 0 wt% to about 20 wt% X, from about 0 wt% to about 10 wt% X, from about 10 wt% to about 40 wt% X, from about 10 wt% to about 30 wt% X, from about 10 wt% to about 20 wt% X, from about 20 wt% to about 40 wt% X, from about 20 wt% to about 30 wt% X, or from about 30 wt% to about 40 wt% X, based on the total weight of the epoxy-functionalized ethylene copolymer.
[0037] In an embodiment, Y is a copolymer unit -(CHCR 3 R 4 In some embodiments, R 3 can be hydrogen or methyl. In some embodiments, R 4can be carboglycidoxy or glycidoxy. In some embodiments, Y can be selected from the group consisting of glycidyl acrylate, glycidyl methacrylate, glycidyl butyl acrylate, glycidyl vinyl ether, and combinations of two or more of glycidyl acrylate, glycidyl methacrylate, glycidyl butyl acrylate, and glycidyl vinyl ether. In further embodiments, the epoxy-functionalized ethylene copolymer comprises from about 0 wt% to about 25 wt% Y, from about 0 wt% to about 20 wt% Y, from about 0 wt% to about 15 wt% Y, from about 0 wt% to about 10 wt% Y, from about 0 wt% to about 5 wt% Y, from about 5 wt% to about 25 wt% Y, from about 5 wt% to about 25 wt% Y, or from about 5 wt% to about 30 wt% Y, based on the total weight of the epoxy-functionalized ethylene copolymer. % to about 20 wt% Y, about 5 wt% to about 15 wt% Y, about 5 wt% to about 10 wt% Y, about 10 wt% to about 25 wt% Y, about 10 wt% to about 20 wt% Y, about 10 wt% to about 15 wt% Y, about 15 wt% to about 25 wt% Y, about 15 wt% to about 20 wt% Y, or about 20 wt% to about 25 wt% Y.
[0038] In embodiments, Z may be a copolymer derived from comonomers including carbon monoxide, sulfur dioxide, acrylonitrile, or other monomers. In further embodiments, the epoxy-functionalized ethylene copolymer may optionally comprise from about 0 wt% to about 10 wt% Z, from about 0 wt% to about 8 wt% Z, from about 0 wt% to about 6 wt% Z, from about 0 wt% to about 4 wt% Z, from about 0 wt% to about 2 wt% Z, from about 2 wt% to about 10 wt% Z, from about 2 wt% to about 8 wt% Z, from about 2 wt% to about 6 wt% Z, from about 2 wt% to about 4 wt% Z, from about 4 wt% to about 10 wt% Z, from about 4 wt% to about 8 wt% Z, from about 4 wt% to about 6 wt% Z, from about 6 wt% to about 10 wt% Z, from about 6 wt% to about 8 wt% Z, or from about 8 wt% to about 10 wt% Z, based on the total weight of the epoxy-functionalized ethylene copolymer.
[0039] In embodiments, the epoxy-functionalized ethylene copolymer may include ethylene vinyl acetate glycidyl methacrylate terpolymer, ethylene n-butyl acrylate glycidyl methacrylate terpolymer, or ethylene methyl acrylate glycidyl methacrylate terpolymer.
[0040] In embodiments, the asphalt composition may comprise from about 0.1 weight percent (wt%) to about 10 wt% of the epoxy-functionalized ethylene copolymer based on the total weight of the asphalt composition. In some embodiments, the asphalt composition may comprise from about 0.1 wt% to about 5 wt%, from about 0.1 wt% to about 1 wt%, from about 0.1 wt% to about 0.5 wt%, from about 0.5 wt% to about 10 wt%, from about 0.5 wt% to about 5 wt%, from about 0.5 wt% to about 1 wt%, from about 1 wt% to about 10 wt%, from about 1 wt% to about 5 wt%, or from about 5 wt% to about 10 wt% of the epoxy-functionalized ethylene copolymer based on the total weight of the asphalt composition.
[0041] In some embodiments, the epoxy-functionalized ethylene copolymer may have a melt flow index, as determined by ASTM D1238-65T, Condition E, of about 1000 g / 10 min or less, about 0.3 g / 10 min to about 1000 g / 10 min, about 0.3 g / 10 min to about 500 g / 10 min, about 0.3 g / 10 min to about 250 g / 10 min, or about 0.3 g / 10 min to about 100 g / 10 min.
[0042] Without being bound by theory, it is believed that functionalization of polymers may be an effective route to chemically bond materials to enhance the rheological and tensile properties of asphalt compositions containing bitumen. In comparison, non-functionalized modifications may require approximately twice as much epoxy-functionalized ethylene copolymer to achieve the same specifications of the asphalt composition. Therefore, a sustainable option may include incorporating recycled polymer components into the asphalt composition. Furthermore, by incorporating epoxy-functionalized ethylene copolymers into the asphalt composition, it may be possible to incorporate more recycled polymer components, thereby increasing the sustainability benefits.
[0043] Without being bound by theory, it is believed that epoxy-functionalized ethylene copolymers may be relatively compatible with ethylene-based polymers compared to other polymers. Thus, embodiments of asphalt compositions having an ethylene-based polymer as a recycled polymer component with epoxy-functionalized ethylene copolymers may show relatively improved performance results compared to some other embodiments using other polymers. In further embodiments, asphalt compositions having recycled polymer components including LLDPE, HDPE, or combinations thereof and epoxy-functionalized ethylene copolymers may show relatively improved results compared to some other embodiments with other polymers.
[0044] The asphalt composition may optionally further comprise one or more polymers in addition to the recycled polymer component, referred to herein as "additional polymers." The one or more additional polymers should not react with the asphalt or the epoxy-functionalized ethylene copolymers described herein. Because the one or more additional polymers should not react with the asphalt or the epoxy-functionalized ethylene copolymers, they are sometimes referred to as "diluent" polymers.
[0045] In some embodiments, the one or more additional polymers may include a styrene / conjugated diene copolymer. In further embodiments, the one or more additional polymers may include a polystyrene-butadiene-styrene (SBS) copolymer. Styrene / conjugated diene block copolymers include polymers derived from or including copolymer units of styrene and a conjugated diene, such as butadiene, isoprene, ethylene butene, or 1,3-pentadiene. Styrene / conjugated diene copolymers may be di-, tri-, or polyblock copolymers with linear or radial (star or branched) architecture, with or without random junctions. Suitable styrene / conjugated diene copolymers include, for example, diblock AB type copolymers, linear (triblock) ABA type copolymers, and radial (AB) n A refers to copolymer units derived from styrene and B refers to copolymer units derived from a conjugated diene. Preferred styrene / conjugated diene copolymers include linear (triblock) ABA type structures or radial (AB) n It has a mold structure.
[0046] In an embodiment, the styrene / conjugated diene copolymer may comprise about 10 wt% to about 50 wt% or about 20 wt% to about 40 wt% of copolymer units derived from styrene, based on the total weight of the styrene / conjugated diene copolymer. In an embodiment, the styrene / conjugated diene block copolymer may comprise about 50 wt% to about 90 wt% or about 60 wt% to about 80 wt% of copolymer units derived from conjugated diene, based on the total weight of the styrene / conjugated diene copolymer. In a further embodiment, the styrene / conjugated diene block copolymer may comprise about 50 wt% to about 90 wt% or about 60 wt% to about 80 wt% of copolymer units derived from butadiene or isoprene, based on the total weight of the styrene / conjugated diene copolymer. In a further embodiment, 20 to 40 wt% of the copolymer units may be derived from styrene, with the remainder being complementarily derived from conjugated diene. As used herein, the term "complementarily" refers to a set of values that have a single sum, such as, for example, the sum of the weight percentages of the components in a composition.
[0047] The styrene / conjugated diene copolymer may have a weight average molecular weight of from about 10,000 Daltons to about 1,000,000 Daltons. The weight average molecular weight of the styrene / conjugated diene copolymer may be determined using conventional gel permeation chromatography. In other embodiments, the styrene / conjugated diene copolymer may have a molecular weight of from about 10,000 daltons to about 750,000 daltons, from about 10,000 daltons to about 600,000 daltons, from about 10,000 daltons to about 500,000 daltons, from about 30,000 daltons to about 1,000,000 daltons, from about 30,000 daltons to about 750,000 daltons, from about 30,000 daltons to about 600,000 daltons, from about 30,000 daltons to about 500,000 daltons, from about 100,000 daltons to about 1,000,000, from about 100,000 daltons to about 750,000 daltons, from about 100,000 daltons The polymer may have a weight average molecular weight of about 1 to about 600,000 daltons, about 100,000 daltons to about 500,000 daltons, about 150,000 daltons to about 1,000,000 daltons, about 150,000 daltons to about 750,000 daltons, about 150,000 daltons to about 600,000 daltons, about 150,000 daltons to about 500,000 daltons, about 200,000 daltons to about 1,000,000 daltons, 200,000 daltons to about 750,000 daltons, about 200,000 daltons to about 600,000 daltons, or about 200,000 daltons to about 500,000 daltons. In some embodiments, the weight average molecular weight of the styrene and butadiene copolymer is from about 10,000 daltons to about 600,000 daltons, or from about 30,000 daltons to about 400,000 daltons.
[0048] The melt flow index of the styrene / conjugated diene copolymer, as determined by ASTM Test Method D 1238, Condition G, can be from about 0 g / 10 min to about 200 g / 10 min, from about 0 g / 10 min to about 100 g / 10 min, or from about 0 g / 10 min to 10 g / 10 min, from about 0.1 g / 10 min to about 200 g / 10 min, from about 0.1 g / 10 min to about 100 g / 10 min, or from about 0.1 g / 10 min to 10 g / 10 min.
[0049] The styrene / conjugated diene copolymers can be prepared by anionic polymerization of the monomers in the presence of an initiator consisting of an organometallic compound of an alkali metal, in particular an organolithium compound such as an alkyllithium, in particular butyllithium, the preparation being carried out at a temperature below 0° C. in a solution in a solvent consisting at least in part of a polar solvent such as tetrahydrofuran or diethyl ether.
[0050] In embodiments, the asphalt composition may include one or more additives. The one or more additives may enable the asphalt composition to have improved stability and may affect the rheological properties of the asphalt composition. In some embodiments, the one or more additives may enable the asphalt composition to include crosslinking with sulfur. In further embodiments, the one or more additives may include a sulfur-based additive. Commercially available sulfur-based additives may include BGA from Ergon, Inc., which includes hydrotreated naphthenic oil, elemental sulfur, rheological additives, and other components.
[0051] In embodiments, the asphalt composition may include an acid. In some embodiments, the acid may be polyphosphoric acid. In further embodiments, the polymer reinforced asphalt composition may include from about 0.05 wt% to about 1 wt%, from about 0.05 wt% to about 0.8 wt%, from about 0.05 wt% to about 0.6 wt%, from about 0.05 wt% to about 0.4 wt%, from about 0.05 wt% to about 0.2 wt%, from about 0.2 wt% to about 1 wt%, from about 0.05 wt% to about 0.2 ... The acid may comprise from about 0.2 wt% to about 0.8 wt%, from about 0.2 wt% to about 0.6 wt%, from about 0.2 wt% to about 0.4 wt%, from about 0.4 wt% to about 1 wt%, from about 0.4 wt% to about 0.8 wt%, from about 0.4 wt% to about 0.6 wt%, from about 0.6 wt% to about 1 wt%, from about 0.6 wt% to about 0.8 wt%, or from about 0.8 wt% to about 1 wt%.
[0052] In embodiments, the asphalt composition may include an anhydride. In further embodiments, the asphalt composition may include from about 0.05 wt% to about 1 wt%, from about 0.05 wt% to about 0.8 wt%, from about 0.05 wt% to about 0.6 wt%, from about 0.05 wt% to about 0.4 wt%, from about 0.05 wt% to about 0.2 wt%, from about 0.2 wt% to about 1 ... % to about 0.8 wt%, about 0.2 wt% to about 0.6 wt%, about 0.2 wt% to about 0.4 wt%, about 0.4 wt% to about 1 wt%, about 0.4 wt% to about 0.8 wt%, about 0.4 wt% to about 0.6 wt%, about 0.6 wt% to about 1 wt%, about 0.6 wt% to about 0.8 wt%, or about 0.8 wt% to about 1 wt% anhydrous.
[0053] In an embodiment, the asphalt composition may have an upper continuous grade that is higher than the unmodified asphalt binder source. The upper continuous grade may be determined by the G * / sin(δ)=1. In other embodiments, the asphalt composition may have a surface layer continuous grading of about 52°C to about 100°C, about 52°C to about 94°C, about 52°C to about 88°C, about 52°C to about 82°C, about 52°C to about 76°C, about 52°C to about 70°C, about 52°C to about 64°C, or about 52°C to about 58°C.
[0054] In embodiments, the asphalt composition may have a phase angle less than that of the unmodified binder. The phase angle defines the resistance of the asphalt binder to shear deformation in the linear viscoelastic region and may depend on the magnitude of the shear strain. In most asphalt applications, a phase angle less than 75° is desirable. In other embodiments, the asphalt composition may have a phase angle of about 55° to about 75°, about 55° to 70°, about 55° to about 65°, about 55° to about 60°, about 60° to about 75°, about 60° to about 70°, about 60° to about 65°, about 65° to about 75°, about 65° to about 70°, or about 70° to about 75°.
[0055] In embodiments, the asphalt composition may have an elastic recovery of at least 50%. Elastic recovery can be used to measure the percentage a sample recovers after tensile deformation using an extensometer. Without being bound by theory, it is believed that a higher elastic recovery means a more elastic behavior of the sample after deformation. Elastic recovery can be determined according to Texas Department of Transportation procedure TEX-539-C, AASHTO T301, or ASTM 6084. In other embodiments, the asphalt composition may have an elastic recovery of about 50% to about 90%, about 50% to about 80%, or about 50% to about 70%.
[0056] In an embodiment, the asphalt composition may have a separation difference of 2.2° C. measured according to ASTM D5976. In some embodiments, the separation difference may be from about 0° C. to about ±2° C., from about 0° C. to about ±1° C., or from about ±1° C. to about ±2° C.
[0057] To produce an asphalt composition, the asphalt binder can be blended with the recycled polymer component and the epoxy-functionalized ethylene copolymer. In some embodiments, the asphalt binder can be heated to blend with the recycled polymer component, the epoxy-functionalized ethylene copolymer, or both. In some embodiments, the asphalt binder can be heated up to 200°C. In other embodiments, the asphalt can be heated to a temperature of about 100°C to about 200°C, about 100°C to about 180°C, about 100°C to about 160°C, about 100°C to about 140°C, about 100°C to about 120°C, about 120°C to about 200°C, about 120°C to about 180°C, about 120°C to about 160°C, about 120°C to about 140°C, about 140°C to about 200°C, about 140°C to about 180°C, about 140°C to about 160°C, about 160°C to about 200°C, about 160°C to about 180°C, or about 180°C to about 200°C.
[0058] In some embodiments, the epoxy-functionalized ethylene copolymer, recycled polymer component, or combinations thereof can be first blended with the asphalt binder to produce an asphalt composition. In some further embodiments, the epoxy-functionalized ethylene copolymer, recycled polymer component, or combinations thereof can be blended with the asphalt binder for about 0.5 hours to about 4 hours, about 0.5 hours to about 3 hours, about 0.5 hours to about 2 hours, about 0.5 hours to about 1 hour, about 1 hour to about 5 hours, about 1 hour to about 4 hours, about 1 hour to about 3 hours, about 1 hour to about 2 hours, about 2 hours to about 5 hours, about 2 hours to about 4 hours, about 2 hours to about 3 hours, about 3 hours to about 5 hours, about 3 hours to about 4 hours, or about 4 hours to about 5 hours. In other embodiments, the epoxy-functionalized ethylene copolymer, recycled polymer component, or combination can be added and blended to produce an embodiment of the asphalt composition described herein.
[0059] In some embodiments of making an asphalt composition, after the asphalt, recycled polymer component, and epoxy-functionalized ethylene copolymer are blended, additional polymer, acid, or anhydride may be added and blended for about 0.5 hours to about 2 hours, about 0.5 hours to about 1 hour, or about 1 hour to about 2 hours.
[0060] In another embodiment, the recycled polymer component can be added directly to the aggregate without the asphalt binder to produce the asphalt composition. In some embodiments, the aggregate can be heated prior to mixing the recycled polymer component and the asphalt binder. In some embodiments, the asphalt binder can be mixed with the epoxy-functionalized ethylene copolymer separately from the recycled polymer component and aggregate. In further embodiments, a mixture of the asphalt binder and the epoxy-functionalized ethylene copolymer can be mixed with a mixture of the recycled polymer component and aggregate.
[0061] Test Method
[0062] The American Association of State Highway and Transportation Officials (AASHTO) is a standard setting organization that publishes specifications, testing protocols, and guidelines for asphalt compositions that may be used in the design and construction of highways. Test methods used herein include the following:
[0063] Rheological properties (surface layer continuity, phase angle, and elastic recovery)
[0064] Dynamic Shear Rheometer measurements of fracture temperature and phase angle were performed in accordance with AASHTO T315-12, "Standard Method of Test for Determining the Rheological Properties of Asphalt Binder Using a Dynamic Shear Rheometer (DSR)." This method characterizes the viscous and elastic behavior of asphalt binders at moderate (i.e., 52°C) to elevated temperatures (i.e., 100°C). The Dynamic Shear Rheometer test method uses a parallel plate geometry to measure the dynamic shear modulus (G) of unaged and aged asphalt binders under dynamic or oscillatory shear. * ) and phase angle (δ). The linear viscoelastic properties of the asphalt binder are derived from these values. * ) can be considered as the total resistance of the sample to deformation when subjected to repeated shear. The phase angle (δ) can be considered as the lag between the applied shear stress and the resulting shear strain. The surface continuous grain size is G * It is determined as the temperature at which / sin(δ)=1.
[0065] The phase angle defines the resistance of the asphalt binder to shear deformation in the linear viscoelastic region. The higher the phase angle (δ), the more viscous the material. A purely elastic material may have a phase angle (δ) of about 0 degrees. A purely viscous material may have a phase angle (δ) of about 90 degrees. The phase angle may depend on the magnitude of the shear strain. The phase angle of both unmodified and modified asphalt decreases with increasing shear strain. For most asphalt applications, a phase angle less than 75° is desirable.
[0066] Elastic recovery was measured according to Texas Department of Transportation procedure TEX-539-C, AASHTO T301 or ASTM 6084. Elastic recovery is used to measure the percentage of a sample that recovers after tensile deformation using an extensometer. It is believed that a higher elastic recovery percentage means the sample has a more elastic behavior after deformation.
[0067] Combined stress creep recovery
[0068] Rotating thin film heat aged samples were studied using multiple stress creep recovery (MSCR) at 67°C in accordance with AASHTO T350-14, "Standard Method of Test for Multiple Stress Creep Recovery (MSCR) Test of Asphalt Binder Using a Dynamic Shear Rheometer (DSR)". Percent recovery values from MSCR testing are considered to be a measure of the elastic response of the sample. Non-recoverable creep compliance is considered to be an indication of the asphalt binder's resistance to permanent deformation after repeated exposure to loads of known stresses.
[0069] Medium Temperature Test
[0070] Mid-temperature testing at 25°C using AASHTO T315 was performed after aging according to AASHTO T240-13 "Standard Method of Test for Effect of Heat and Air on a Moving Film of Asphalt Binder (Rolling Thin-Film Oven Test)" and AASHTO R28-12 "Standard Practice for Accelerated Aging of Asphalt Binder Using a Pressurized Aging Vessel (PAV)". Residues were tested after aging to perform mid-temperature testing. Asphalt binders need to be elastic to allow for dissipation of energy to prevent cracking, but also not too rigid to prevent cracking. In asphalt applications, G * A lower value of sin(δ) typically indicates improved performance. In a further embodiment, the maximum G * The sin(δ) value may be 5000 kPa.
[0071] rigidity
[0072] The average of the two measurements was used to determine the stiffness and m-value of the sample beams aged at -12°C using AASHTO T313-12, "Standard Method of Test for Determining the Flexural Creep Stiffness of Asphalt Binder Using the Bending Beam Rheometer (BBR)". Low temperature cracking performance is believed to be related to the creep stiffness and the slope of the logarithm of creep stiffness versus logarithm of time curve of the asphalt binder.
[0073] Separation properties
[0074] Separation properties were measured according to ASTM D7173, "Standard practice for determining the separation tendency of polymer from polymer modified asphalt." Comparison of the softening point properties of samples heat aged at 163±5°C for 48 hours and of the upper and lower sections is believed to provide information on the stability of the polymer modified asphalt formulation. A separation difference of 2.2°C or less is considered a passing result.
[0075] Force ductility ratio
[0076] The force ductility ratio was determined by measuring the tensile stress exerted on specimens pulled apart at 5 cm / min in a 4°C water bath as specified in AASHTO T300. This test may serve as an indication of the presence of polymers in the asphalt sample if the material ruptures during elongation. When plotted as a function of force versus elongation, if two peaks are present, the force ductility ratio can be defined as the ratio of the second to the first peak, or the ratio of the force at 30 cm to the first peak. EXAMPLES
[0077] The following examples are illustrative of features of the present disclosure and are not intended to limit the scope of the disclosure. The following experiments analyzed the performance of embodiments of the asphalt compositions described herein.
[0078] To prepare the comparative examples and examples described below, a modified blending kettle was made using a 1 quart kettle that could be equipped with a heating mantle. The lid of the 1 quart kettle was modified to include a central hole about 1 cm in diameter to accommodate the stirrer shaft and a second hole about 3 mm in diameter to accommodate a thermocouple probe. The lid can be sealed onto the sample kettle where the stirrer shaft is threaded through the lid and the stirrer shaft and motor are placed into the mixed sample.
[0079] Examples 1 to 4
[0080] Materials used to prepare Examples 1-4 included asphalt binder supplied by Valero (TX) as the asphalt binder, Natura PCR, a LLDPE-rich post-consumer recycled resin with a Yellowness Index of 35.56 supplied by Avangard Innovative (Houston TX) as the recycled polymer component, ELVALOY™ RET EP1177 supplied by DowDuPont (Wilmington DE) as the epoxy functionalized ethylene copolymer, and polyphosphoric acid (PPA) supplied by Innophos (Cranbury NJ).
[0081] To prepare Examples 1, 2, 3, and 4, 450 grams (g) or 650 g of asphalt was poured into the modified blending kettle (described above) and a lid and agitator assembly was attached to the kettle. The modified blending kettle was heated to 165° C. and once the temperature stabilized, the epoxy-functionalized ethylene copolymer, recycled polymer component, and polyphosphoric acid were added to the modified blending kettle in the ratios shown in Table 1. The epoxy-functionalized ethylene copolymer was added first and mixed for 2 hours. The recycled polymer component was added second and mixed for 2 hours. The polyphosphoric acid was then added and mixed for 1 hour. The samples were then stored in a 163° C. oven overnight before testing. [Table 1]
[0082] Example 5
[0083] Materials used to prepare Example 5 included asphalt binder (PG58-28) supplied by Marathon Petroleum Corporation (Detroit MI) as the asphalt binder, LLDPE-rich post-industrial recycled (PIR) resin with a yellowness index of 12.36 as the recycled polymer component containing approximately 75% LLDPE, 20% polyamide, and 5% ethylene vinyl alcohol, ELVALOY™ RET EP1177 supplied by Dow Inc. (Midland MI) as the epoxy functionalized ethylene copolymer, and polyphosphoric acid (PPA) supplied by Innophos (Cranbury NJ).
[0084] To prepare Example 5, 300 grams (g) or asphalt was poured into the modified blending kettle (as described above). Using a high shear blender, the PIR was processed at 185°C until the blend was uniform (usually 10-30 minutes). The blend was then transferred to the lid and stirrer assembly described above (low shear blending). The modified blending kettle was heated to 185°C and once the temperature was stable, the epoxy functionalized ethylene copolymer was added in the ratio shown in Table 2 and mixed for 2 hours. Polyphosphoric acid was then added and mixed for 1 hour. The samples were then stored in a 163°C oven overnight before testing was performed. [Table 2]
[0085] Comparative Examples 1 to 4
[0086] The materials used to prepare Comparative Examples 1-4 included asphalt binder supplied by Valero (TX) as the asphalt binder, Natura PCR, an LLDPE-rich post-consumer recycled resin with a Yellowness Index of 35.56 supplied by Avangard Innovative (Houston TX) as the recycled polymer component, ELVALOY™ RET EP1177 supplied by DowDuPont (Wilmington DE) as the epoxy functionalized ethylene copolymer, and polyphosphoric acid (PPA) supplied by Innophos (Cranbury NJ).
[0087] To prepare Comparative Examples 1, 2, 3, and 4, 450 grams (g) or 650 g of asphalt was poured into the modified blending kettle (as described above) and the lid and agitator assembly was attached to the kettle. The modified blending kettle was heated to 165° C. and once the temperature was stable, either the epoxy-functionalized ethylene copolymer or the recycled polymer component was added in the ratios shown in Table 3 and mixed for 2 hours. Polyphosphoric acid was then added and mixed for 1 hour. The samples were then stored in a 163° C. oven overnight before testing. [Table 3]
[0088] Comparative Example 5
[0089] The materials used to make Comparative 5 included asphalt binder supplied by Valero (TX) as the asphalt binder, Natura PCR, an LLDPE-rich post-consumer recycled resin supplied by Avangard Innovative (Houston TX) with a Yellowness Index of 35.56 as the recycled polymer component, D1101 supplied by Kraton (Houston TX) as the styrene / conjugated diene copolymer, and BGA supplied by Ergon, Inc. as the additive.
[0090] To prepare Comparative Example 5, 650 g of asphalt was poured into the modified blending kettle (as described above) and the lid and stirrer assembly was attached to the kettle. The modified blending kettle was heated to 165° C. and once the temperature stabilized, the styrene / conjugated diene copolymer was added in the ratio shown in Table 4 and mixed for 2 hours. BGA was then added and mixed for 1 hour. The sample was then stored in a 163° C. oven overnight before testing. [Table 4]
[0091] Comparative Examples 6 to 8
[0092] The materials used to prepare Comparative Examples 6-8 below include asphalt binder (PG58-28) supplied by Marathon Petroleum Corporation (Detroit MI) as the asphalt binder, LLDPE-rich post-industrial recycled (PIR) resin with a yellowness index of 12.36 as the recycled polymer component containing approximately 75% LLDPE, 20% polyamide, and 5% ethylene vinyl alcohol, ELVALOY™ RET EP1177 supplied by Dow Inc. (Midland MI) as the epoxy-functionalized ethylene copolymer, polyphosphoric acid (PPA) supplied by Innophos (Cranbury NJ), D1101 supplied by Kraton (Houston TX) as the styrene / conjugated diene copolymer, and sulfur supplied by Sigma Aldrich as the additive.
[0093] To prepare Comparative Examples 6, 7, and 8, approximately 300-400 grams (g) of asphalt was poured into the modified blending kettle (as described above). A high shear blender was used to process the post-industrial recycled (PIR) and SBS at 155°C-185°C until the blend was homogenous (usually 10-30 minutes). The blend was then transferred to the lid and agitator assembly described above (low shear blending). The modified blending kettle was heated to 185°C and once the temperature was stable, the epoxy functionalized ethylene copolymer was added in the ratios shown in Table 5 and mixed for 2 hours. Polyphosphoric acid was then added and mixed for 1 hour. For the SBS blends, sulfur was added and mixed for 2 hours. The samples were then stored overnight in a 163°C oven before testing was performed. [Table 5]
[0094] Comparison of Comparative Examples 1 to 8 and Examples 1 to 5
[0095] Table 6 provides a summary of the compositions of Examples 1-5 and Comparative Examples 1-8 grouped by the amount of recycled polymer component (RPC). [Table 6]
[0096] For Examples 1-5 and Comparative Examples 1-8, dynamic shear rheometer fracture temperature and phase angle were measured according to AASHTO T315-12, combined stress creep recovery was measured according to AASHTO T350-14, and intermediate temperature testing was performed at 25°C using AASHTO T315 after aging according to AASHTO T240-13 and AASHTO R28-12. Dynamic shear rheometer measurements for surface layer continuum grain size, phase angle, and elastic recovery, 3.2 kPA (%R 3.2 ) 、 3.2kPA(J nr,3.2 The combined stress creep recovery measurements for percent recovery in Z factor and Z factor and the results of the intermediate temperature tests are shown in Table 7. [Table 7]
[0097] As shown in Tables 6 and 7, all of Examples 1-4 showed higher continuous grading compared to Comparative Example 1, which did not contain either the recycled polymer component or the epoxy-functionalized ethylene copolymer, indicating that the recycled polymer component and the epoxy-functionalized ethylene copolymer increase the value of the asphalt sample. Furthermore, Examples 1-4 having a mixture of recycled polymer component (PCR) and epoxy-functionalized ethylene copolymer were found to have increased (improved) upper continuous grading compared to Comparative Examples 2-4, which contained only one of the recycled polymer component (PCR) (Comparative Examples 2-3) or the epoxy-functionalized ethylene copolymer (Comparative Example 4). Also, Examples 2 and 3 were found to have increased (improved) upper continuous grading compared to Comparative Example 5, which had a combination of recycled polymer component (PCR) with styrene / conjugated diene copolymer and BGA.
[0098] As shown in Tables 6 and 7, Comparative Example 7 with 2% PIR showed only a 3°C improvement in continuous gradation compared to Comparative Example 6, which did not contain any recycled polymer component or epoxy-functionalized ethylene copolymer, indicating that the recycled polymer component did not significantly increase the absolute value, improve the phase angle, or demonstrate high elastic recovery of the asphalt samples. Example 5, which had a mixture of recycled polymer component (PIR) and epoxy-functionalized ethylene copolymer, was found to increase (improve) the surface layer continuous gradation compared to Comparative Examples 6 and 7.
[0099] As previously mentioned, in most asphalt applications, a phase angle of less than 75° is desirable. In Examples 1-4, it was found that the combination of recycled polymer component and epoxy-functionalized ethylene copolymer reduced (improved) the phase angle, while Comparative Examples 1-5 exhibited higher (poor) phase angles than Examples 1-4. Furthermore, in Example 5, it was found that the combination of recycled polymer component and epoxy-functionalized ethylene copolymer reduced (improved) the phase angle, while Comparative Examples 6-8 exhibited higher (poor) phase angles than Example 5.
[0100] As explained before, a higher elastic recovery is believed to mean a higher elastic behavior of the sample after deformation. As shown in Table 7, Examples 1-4, which include a combination of recycled polymer components and epoxy-functionalized ethylene copolymer, showed increased (improved) elastic recovery compared to Comparative Examples 1-3, which showed low (poor) elastic recovery or failure. Examples 2 and 4 also showed increased (improved) elastic recovery compared to Comparative Examples 4 and 5, which have epoxy-functionalized ethylene copolymer alone or a combination of recycled polymer components with styrene / conjugated diene copolymer and BGA. Example 5, which has a combination of recycled polymer components and epoxy-functionalized ethylene copolymer, was found to have increased (improved) elastic recovery compared to Comparative Examples 6 and 7.
[0101] Also, as shown in Table 7, Examples 1-4, which include a combination of recycled polymer component (PCR) and epoxy-functionalized ethylene copolymer, increased (improved) recovery and reduced non-recoverable creep compliance (J) when compared to Comparative Examples 1-3, which showed lower (less satisfactory) recovery. nr ) was found to reduce the saturation temperature. Furthermore, Comparative Example 5 and Example 1 had similar J nr,3.2 values, which may indicate similar resistance to creep. However, Example 1 showed a significantly improved recovery rate compared to Comparative Example 5. Example 5, which has a combination of recycled polymer component (PIR) and epoxy-functionalized ethylene copolymer, showed a lower (poorer) recovery rate compared to Comparative Examples 6 and 7. 、 Increase (improve) the recovery rate and reduce irrecoverable creep compliance (J nr ) was found to reduce creep resistance. Additionally, Example 5 may exhibit improved creep resistance and significantly improved recovery rates compared to Comparative Examples 6 and 7. 、 Improved J nr,3.2 had value.
[0102] The Z factor of an asphalt composition is %R 3.2 Against J nr,3.2 The formula %R on the plot 3.2 =29.371(J nr,3.2 ) -0.2633 Z-factor is defined by how above (positive number) or below (negative number) a sample is relative to the "29 line," or "29 line." Traditionally, unmodified asphalt compositions have negative Z-factor values (below the 29 line), while polymer-modified asphalt compositions can have positive Z-factor values (above the 29 line). Here, each of Examples 1-5 had a positive Z-factor value. Examples 1-4 also had a higher Z-factor than Comparative Example 5. Comparative Examples 2-3 and 8 showed negative Z-factor values, which was surprising for modified asphalt compositions.
[0103] As mentioned above, G * The maximum allowable value of sin(δ) is 5000 kPa at grain temperature, and G *As shown in Table 7, Examples 1-4 having a combination of recycled polymer component and epoxy-functionalized ethylene copolymer have lower G * It was found that Example 5, which has a combination of recycled polymer components and epoxy-functionalized ethylene copolymer, has a lower G sin(δ) value compared to Comparative Examples 7 and 8. * It was found to have a sin(δ) value.
[0104] The stiffness and m values of the aged Comparative Examples 1-5 and Examples 1-4 were tested using AASHTO T313-12 as described above. The stiffness and m value results are shown in Table 8. [Table 8]
[0105] In Examples 1-4, the combination of recycled polymer component and epoxy-functionalized ethylene copolymer was found to meet stiffness values of less than 300 MPa and m values of greater than 0.300. Thus, Examples 1-4 appear to exhibit comparable stiffness and m values compared to Comparative Examples 2-3 and 5.
[0106] The separation properties provided in Table 9 for Comparative Examples 2, 3, and 5 and Examples 1 and 4 were measured according to ASTM D5976, as previously described. [Table 9]
[0107] As stated above, a separation difference of 2.2°C or less is considered a passing result. The results provided in Table 9 show that Comparative Examples 2 and 3, which have only recycled polymer components, did not pass the separation test. Examples 1 and 4, which have a combination of recycled polymer components and epoxy-functionalized ethylene copolymer, passed the separation test.
[0108] The force ductility ratios of Comparative Example 8 and Example 5 were tested using AASHTO T300 as previously described. The results for 4° C. are provided in Table 10. [Table 10]
[0109] In Example 5, the combination of recycled polymer component and epoxy functionalized ethylene copolymer was found to have a force ductility ratio of 0.4 compared to Comparative Example 8, which had a ratio of 0. It is believed that a higher force ductility ratio would result in improved performance. A minimum force ductility ratio of 0.3 is required as specified by Michigan DOT for the PG64-28P specification.
[0110] Based on these results in Tables 7-10, Examples 1-4 show that embodiments of the present disclosure can provide asphalt compositions including an asphalt binder, a recycled polymer component, and an epoxy-functionalized ethylene copolymer, which can improve the performance of the asphalt composition compared to asphalt compositions including only recycled polymer components or only epoxy-functionalized ethylene copolymer. Examples 1-5 further show that embodiments of the present disclosure can provide sustainable asphalt compositions with improved efficiency that can be achieved by incorporating recycled polymer components. Furthermore, the incorporation of epoxy-functionalized ethylene can allow for the incorporation of more recycled polymer components, potentially resulting in improved performance results.
[0111] Comparative Examples 9 to 11 and Examples 6 to 7
[0112] The materials used to produce Comparative Examples 9-11 and Examples 6-7 included REVAP produced by Petrobras (Sao Jose dos Campos-SP-Brazil) as the asphalt binder. Comparative Example 10 and Examples 6-7 included ELVALOY™ RET 5160 supplied by DowDuPont (Wilmington DE-US) as the epoxy-functionalized ethylene copolymer and polyphosphoric acid (PPA) supplied by Arkema Quimica Ltda (Rio Claro-SP-Brazil). Comparative Example 11 and Examples 6-7 included HDPE-rich post-consumer recycled resin (PCR) with traces of polypropylene and LDPE in the recycled polymer component used to produce Examples 9-13. The PCR resin was supplied from a Wortex recycled extrusion single screw line with a diameter of 60 mm and L / D of 42. The PCR had a melt index of 0.3352 ± 0.0060 (measured at 190 °C and 2.16 kg load), a melt index of 38.9057 ± 1.2153 (measured at 190 °C and 21.60 kg load), and a melt loss of 0.9602 ± 0.0004 g / cm 3 When measured according to ASTM D6290, the PCR had a yellowness index of -32.33 and a blue color (measured Δb * (as indicated by -4.86).
[0113] To prepare Comparative Examples 9-11 and Examples 6-7, 2000 grams (g) of asphalt was poured into a modified blending kettle attached to a lid and agitator assembly. The modified blending kettle was heated to 180° C., and once the temperature stabilized, one or more of the epoxy-functionalized ethylene copolymer, the recycled polymer component, and the polyphosphoric acid were added in the ratios shown in Table 11. The epoxy-functionalized ethylene copolymer and the recycled polymer component were added and mixed in a turbulent system for 1.5 hours. The polyphosphoric acid was then added and mixed for 0.5 hours. The samples were then stored in a 163° C. oven overnight before testing.
[0114] Table 11 provides a summary of the compositions of Comparative Examples 9-11 and Examples 6-7, grouped by the amount of recycled polymer component (RPC). [Table 11]
[0115] Comparison of Comparative Examples 9 to 11 and Examples 6 to 7
[0116] In the cases of Comparative Examples 9 to 11 and Examples 6 to 7, the combined stress creep recovery (MSCR), recovery rate (%R 3.2 ), J nr,3.2 The surface layer continuous particle size temperature and phase angle of the complex dynamic shear rheometer (DSR) were measured according to the method previously described in this disclosure. * The surface layer continuous performance grain size temperature is defined when / sin(δ) is equal to 1.0 kPa. The properties of Comparative Examples 9 to 11 and Examples 6 to 7 are shown in Tables 12 to 16. [Table 12] [Table 13] [Table 14] [Table 15] [Table 16]
[0117] As shown in Table 12, Comparative Example 9 represents a sample that does not contain any recycled polymer component or epoxy-functionalized ethylene copolymer, and Comparative Example 9 has a J of 33.6. nr,3.2 and %R of 0.0% 3.2These results did not meet the minimum requirements per method AASHTO T350. As shown in Table 13, Comparative Example 10, which contained an epoxy-functionalized ethylene copolymer but no recycled polymer component, had a %R value higher than 35% (47.6%) when both properties were measured at 76°C. 3.2 and J of 0.51 to 1.00 (0.86) nr,3.2 As shown in Table 14, Comparative Example 11, which contained the recycled polymer component but no epoxy-functionalized ethylene copolymer, performed poorly compared to Comparative Example 10, showing a J nr,3.2 was 2.99 and R% was 0.1%. Therefore, according to the AASHTO T350 method, the composition containing only PCR appears to perform below the minimum required standard (S) level for traffic loads.
[0118] Furthermore, as shown in Table 15, Example 6 had a J nr,3.2 is 0.67, %R 3.2 The J value is 30%, and Example 6 meets the standard (S) traffic load rating. As shown in Table 16, Example 7 shows comparable performance compared to the standard formulation Comparative Example 10 when evaluated at 3.2 kPa and 76° C., with a J value of 0.46. nr,3.2 and a %R of 43% 3.2 Thus, Example 7 exhibited properties that met the same classification as high (H) level traffic load according to method AASHTO T350.
[0119] As mentioned above, the Z factor of an asphalt composition is calculated by %R 3.2 Against J nr,3.2 The formula %R on the plot 3.2 =29.371(J nr,3.2 ) -0.2633, or "29 line", by how above (positive number) or below (negative number) the sample is. Traditionally, unmodified asphalt compositions have negative Z-factor values (below the 29 line), while polymer-modified asphalt compositions can have positive Z-factor values (above the 29 line). Here, Comparative Example 10 had a positive Z-factor value, and Example 7 had positive Z-factor values at only 70°C and 76°C. It was not unexpected that Comparative Example 9, which is the exact asphalt composition, would show a negative value. However, Comparative Example 11, Example 6, and Example 7 (58°C and 64°C) showed negative Z-factor values, which was surprising for the modified asphalt compositions.
[0120] The phase separation properties provided in Table 17 for Comparative Example 10 and Examples 6-7 were measured according to ASTM D7173, as previously described. [Table 17]
[0121] Based on these results in Tables 11-17, Examples 6-7 show that embodiments of the present disclosure can provide asphalt compositions including an asphalt binder, a recycled polymer component, and an epoxy-functionalized ethylene copolymer, which can improve the performance of the asphalt composition compared to asphalt compositions including only recycled polymer components or only epoxy-functionalized ethylene copolymer. Examples 6-7 can further show that embodiments of the present disclosure can provide sustainable asphalt compositions, which can be achieved by incorporating recycled polymer components. Furthermore, the incorporation of epoxy-functionalized ethylene can allow the incorporation of more recycled polymer components with performance results that meet industry standards and are comparable to comparative asphalt compositions without sustainability improvements.
[0122] It will be apparent that modifications and variations are possible without departing from the scope of the present disclosure, as defined in the appended claims. More specifically, although certain aspects of the present disclosure are identified herein as preferred or particularly advantageous, it is contemplated that the present disclosure is not necessarily limited to those aspects. The present invention may include the following aspects. [1] An asphalt composition comprising: About 70 to about 99.5 wt. % of an asphalt binder, based on the total weight of the asphalt composition; About 0.25 to 20 wt.% of a recycled polymer component, based on the total weight of the asphalt composition; and about 0.1 to 10 wt. %, based on the total weight of the asphalt composition, of an epoxy-functionalized ethylene copolymer having the formula E / X / Y / Z. where E is a copolymer unit derived from ethylene -(CH 2 CH 2 )-and X is a copolymer unit -(CH 2 CR 1 R 2 )-, where R 1 is hydrogen, methyl, or ethyl; R 2 is a carboalkoxy, acyloxy, or alkoxy of 1 to 10 carbon atoms; Y is a copolymer unit -(CH 2 CR 3 R 4 )-, where R 3 is hydrogen or methyl, R 4 is carboglycidoxy or glycidoxy, An asphalt composition, wherein Z is a copolymer derived from comonomers including carbon monoxide, sulfur dioxide, acrylonitrile, or other monomers, present at 0 to about 10 wt % of said copolymer. [2] The asphalt composition of [1], wherein the recycled polymer component comprises, based on the total weight of the recycled polymer component, 1 wt% to 99.99 wt% of one or more of an ethylene-based polymer, a propylene-based polymer, a polyester, a poly(vinyl chloride), a polystyrene or a polyamide, ethylene vinyl alcohol, ethylene vinyl acetate, or polyvinyl chloride. [3] The asphalt composition according to [1] or [2], wherein the recycled polymer component comprises 51 wt% to 99.99 wt% of one or more ethylene-based polymers, based on the total weight of the recycled polymer component. [4] The asphalt composition according to any one of [1] to [3], wherein the recycled polymer component has a density of about 0.858 grams per cubic centimeter (g / cc) to about 0.970 g / cc. [5] The recycled polymer component has a melt index I of less than about 20 grams per 10 minutes (g / 10 min), measured according to ASTM D1238 at 190° C. and a load of 2.16 kg. 2 The asphalt composition according to any one of [1] to [4], [6] The asphalt composition according to any one of [1] to [5], wherein Y is selected from the group consisting of glycidyl acrylate, glycidyl methacrylate, glycidyl butyl acrylate, glycidyl vinyl ether, and a combination of two or more of glycidyl acrylate, glycidyl methacrylate, glycidyl butyl acrylate, and glycidyl vinyl ether. [7] The asphalt composition according to any one of [1] to [6], wherein the epoxy-functionalized ethylene copolymer is an ethylene vinyl acetate glycidyl methacrylate terpolymer, an ethylene n-butyl acrylate glycidyl methacrylate terpolymer, or an ethylene methyl acrylate glycidyl methacrylate terpolymer. [8] The asphalt composition according to any one of [1] to [7], further comprising a styrene / conjugated diene copolymer. [9] The asphalt composition according to any one of [1] to [8], further comprising an acid or an anhydride.
[10] The asphalt composition according to [8], wherein the acid is polyphosphoric acid.
[11] The asphalt composition according to [8], comprising 0.05 wt% to 1 wt% of an acid or anhydride, based on the total weight of the asphalt composition.
[12] The asphalt composition according to any one of [1] to
[11] , wherein the asphalt composition has a surface layer continuous grain size exceeding 58°C.
[13] The asphalt composition according to any one of [1] to
[12] , wherein the asphalt composition has an elastic recovery of more than 50%.
[14] The asphalt composition according to any one of [1] to
[13] , wherein the recycled polymer component further contains at least 0.01 wt% of a contaminant based on the total weight of the recycled polymer component.
[15] The asphalt composition according to any one of [1] to
[14] , wherein the recycled polymer component has a non-zero yellowness index when measured according to ASTM D6290.
[16] 1. A method for producing an asphalt composition, comprising: combining an asphalt binder, a recycled polymer component, and an epoxy-functionalized ethylene copolymer having the formula E / X / Y / Z; where E is a copolymer unit derived from ethylene -(CH 2 CH 2 )-and X is a copolymer unit -(CH 2 CR 1 R 2 )-, where R 1 is hydrogen, methyl, or ethyl; R 2 is a carboalkoxy, acyloxy, or alkoxy of 1 to 10 carbon atoms; Y is a copolymer unit -(CH 2 CR 3 R 4 )-, where R 3 is hydrogen or methyl, R 4 is carboglycidoxy or glycidoxy, 1. A method for producing an asphalt composition, wherein Z is a copolymer derived from a comonomer including carbon monoxide, sulfur dioxide, acrylonitrile, or other monomer, present at 0 to about 10 wt % of said copolymer.
Claims
1. An asphalt composition comprising: 70 to 99.5 wt % of an asphalt binder, based on the total weight of the asphalt composition; and 0.25 to 20 wt % of a recycled polymer component, based on the total weight of the asphalt composition, the recycled polymer component comprising 51 wt % to 99.99 wt % of an ethylene-based polymer, based on the total weight of the recycled polymer component, the recycled polymer component being selected from linear low density polyethylene (LLDPE)-rich post-consumer recycled resins, LLDPE-rich post-industrial recycled resins, or combinations thereof; 0.1 to 10 wt %, based on the total weight of the asphalt composition, of an epoxy-functionalized ethylene copolymer having the formula E / X / Y / Z. In the formula, E represents a copolymer unit derived from ethylene -(CH 2 CH 2 ) - and X is a copolymer unit -(CH 2 CR 1 R 2 )-, where R 1 is hydrogen, methyl, or ethyl; R 2 is a carboalkoxy, acyloxy, or alkoxy of 1 to 10 carbon atoms; Y is a copolymer unit -(CH 2 CR 3 R 4 )-, where R 3 is hydrogen or methyl; R 4 is carboglycidoxy or glycidoxy, Z is a copolymer derived from comonomers including carbon monoxide, sulfur dioxide, acrylonitrile, or other monomers, present at 0-10 wt % of said copolymer; The asphalt composition further comprising an acid or an anhydride.
2. 10. The asphalt composition of claim 1, wherein the recycled polymer component has a density of from 0.858 grams per cubic centimeter (g / cc) to 0.970 g / cc.
3. The recycled polymer component has a melt index I of less than 20 grams per 10 minutes (g / 10 min), measured according to ASTM D1238 at 190° C. and a load of 2.16 kg. 2 The asphalt composition according to claim 1 or 2, having
4. The asphalt composition of any one of claims 1 to 3, wherein Y is selected from the group consisting of glycidyl acrylate, glycidyl methacrylate, glycidyl butyl acrylate, glycidyl vinyl ether, and combinations of two or more of glycidyl acrylate, glycidyl methacrylate, glycidyl butyl acrylate, and glycidyl vinyl ether.
5. 5. The asphalt composition of any one of claims 1 to 4, wherein the epoxy-functionalized ethylene copolymer is an ethylene vinyl acetate glycidyl methacrylate terpolymer, an ethylene n-butyl acrylate glycidyl methacrylate terpolymer, or an ethylene methyl acrylate glycidyl methacrylate terpolymer.
6. The asphalt composition of any one of claims 1 to 5, further comprising a styrene / conjugated diene copolymer.
7. The asphalt composition according to any one of claims 1 to 6, wherein the acid is polyphosphoric acid.
8. 8. The asphalt composition of any one of claims 1 to 7, comprising from 0.05 wt% to 1 wt% of an acid or anhydride, based on the total weight of the asphalt composition.
9. The asphalt composition according to any one of claims 1 to 8, wherein the asphalt composition has a surface layer continuous grading greater than 58°C.
10. The asphalt composition of any one of claims 1 to 9, wherein the asphalt composition has an elastic recovery of greater than 50%.
11. The asphalt composition of any one of claims 1 to 10, wherein the recycled polymer component further comprises at least 0.01 wt.% of contaminants, based on the total weight of the recycled polymer component.
12. The asphalt composition of any one of claims 1 to 11, wherein the recycled polymer component has a non-zero Yellowness Index when measured according to ASTM D6290.
13. 1. A method for producing an asphalt composition, comprising: The method includes combining an asphalt binder, a recycled polymer component, an acid or anhydride, and an epoxy-functionalized ethylene copolymer having the formula E / X / Y / Z; where E is a copolymer unit derived from ethylene -(CH 2 CH 2 ) - and X is a copolymer unit -(CH 2 CR 1 R 2 )-, where R 1 is hydrogen, methyl, or ethyl; R 2 is a carboalkoxy, acyloxy, or alkoxy of 1 to 10 carbon atoms; Y is a copolymer unit -(CH 2 CR 3 R 4 )-, where R 3 is hydrogen or methyl; R 4 is carboglycidoxy or glycidoxy, Z is a copolymer derived from comonomers including carbon monoxide, sulfur dioxide, acrylonitrile, or other monomers, present at 0-10 wt % of said copolymer; 1. A method for producing an asphalt composition, wherein the recycled polymer component comprises 51 wt% to 99.99 wt% ethylene-based polymer, based on a total weight of the recycled polymer component, and the recycled polymer component is selected from linear low density polyethylene (LLDPE)-rich post-consumer recycled resins, LLDPE-rich post-industrial recycled resins, or combinations thereof.
Citation Information
Patent Citations
Mixture of bitumen, rubber power and polymer, used as binder for road
JP1999079813A
Film for farming
JP2001045880A
Agricultural film
JP2013192488A
Photodegradable film with excellent tensile and darting properties.
JP2013513695A
Multilayer structure, membrane formed therefrom, and package formed therefrom
JP2017532232A