Manufacturing method of laminate and laminate

The described manufacturing method for optical laminates uses UV cleaning and carbonated water washing to address the challenge of particulate foreign matter and haze in photomasks, ensuring high precision and reliability in semiconductor manufacturing.

JP7561813B2Active Publication Date: 2024-10-04聚光ルミナ カンパニー リミテッド
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022186958
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-20
Filing Date
2022-11-22
Publication Date
2024-10-04
Estimated Expiration
2042-11-22

AI Technical Summary

Technical Problem

The challenge in semiconductor manufacturing is the removal of particulate foreign matter and suppression of unintended haze during exposure processes, particularly due to residual ions and defects on the surface of optical laminates used in photomasks.

Method used

A manufacturing method involving ultraviolet cleaning and carbonated water washing steps, along with optional hydrogen water rinsing, to reduce residual ions and particles on the laminate surface, using a sputtering method for the light-shielding film and controlled heat treatment to minimize optical property changes.

Benefits of technology

The method effectively removes surface particles and ions, reducing haze and defects, maintaining laminate integrity and enhancing the reliability of photomasks for finer semiconductor patterns.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561813000001
    Figure 0007561813000001
  • Figure 0007561813000002
    Figure 0007561813000002
  • Figure 0007561813000003
    Figure 0007561813000003
Patent Text Reader

Abstract

To provide a method of producing a laminate capable of effectively suppressing the occurrence of unintended haze in an exposure process by removing particles, etc. present on an outer surface of the laminate, and to provide a laminate or the like.SOLUTION: An embodiment relates to a method of producing a laminate, a laminate, and the like, the method including: a preparation step of providing a processing object which is a laminate precursor on which a light shielding film is disposed; and a carbonated water washing step of applying a carbonated water washing process of adding ultraviolet rays and carbonated water to the processing object to provide a washed laminate, wherein the light shielding film includes a transition metal, oxygen, nitrogen, or carbon, the laminate has a residual ion content as measured by ion chromatography, the residual ion content includes sulfur-based ions and nitrate-based ions, the amount of the sulfur-based ions is more than 0ng / cm2 and 0.1ng / cm2 or less, and the amount of the nitrate-based ions is more than 0ng / cm2 and 0.1ng / cm2 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The embodiments relate to a method for producing a laminate and the laminate that are applied to optical applications. [Background technology]

[0002] Optical laminates are used in the semiconductor manufacturing process. For example, in the case of semiconductor photomasks, they are enlarged to about 3 to 4 times their original size and used for exposure in the semiconductor manufacturing process. As semiconductor wiring becomes finer and more complex, the performance required for the optical laminate is becoming increasingly difficult, such as requiring a higher level of line pattern precision and almost perfect removal of particulate foreign matter.

[0003] The blank mask may include a light-transmitting substrate, a thin film such as a light-shielding film, etc. The light-transmitting substrate may be manufactured by processing a material having light-transmitting properties into a shape, and then performing a polishing process and a cleaning process.

[0004] As the circuit patterns developed on the wafer become finer, it is required to more effectively suppress defects that may occur during the manufacturing process of the blank mask. Certain ions remaining on the surface of the blank mask (such as a metal-containing thin film) may grow into particulate foreign matter when affected by the energy of exposure light or exposed to other chemicals. In addition, when certain conditions are met, the ions may increase haze and transfer unintended distorted patterns during exposure. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Korean Patent No. 10-0316374 [Patent Document 2] Korean Patent No. 10-0745065 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the embodiment is to provide a method for manufacturing a laminate, a laminate, etc., which can remove particles, etc. present on the outer surface of the laminate and effectively suppress the occurrence of unintended haze during the exposure process.

[0007] Another object of the embodiment is to provide a blank mask having reduced defects, a manufacturing method thereof, etc. [Means for solving the problem]

[0008] In order to achieve the above object, a method for manufacturing a laminate in an embodiment includes: a preparation step of providing a treatment object, which is a pre-treatment laminate having a light-shielding film disposed thereon; and a carbonated water cleaning step of applying a first cleaning step of adding ultraviolet light and carbonated water to the treatment object to provide a cleaned laminate.

[0009] The light-shielding film contains a transition metal and oxygen, nitrogen, or carbon.

[0010] The laminate has a residual ion content measured by an ion chromatography method, the residual ions include sulfur-based ions and nitrate-based ions, and the sulfur-based ion content is 0 ng / cm 2 Super 0.1ng / cm 2 The content of nitrate ions is 0 ng / cm or less. 2 Super 0.1ng / cm 2 It may be the following.

[0011] The light-shielding film may be manufactured in a manufacturing step of a light-shielding film using a sputtering method.

[0012] The sputtering method is a method in which a target containing a transition metal is disposed and sputtering is performed in the presence of a reactive gas containing an oxygen atom-containing gas, a nitrogen atom-containing gas, or a carbon atom-containing gas.

[0013] In the carbonated water washing step, the ultraviolet light has a wavelength of 1 mW / cm2 in the range of 190 nm to 290 nm.2 ~11mW / cm 2 The light may be irradiated with a light amount of .

[0014] In the carbonated water washing step, the carbonated water may have an electrical conductivity of 1 μS / cm or more and 10 μS / cm or less.

[0015] An ultraviolet ray cleaning step may be further included before the carbonated water cleaning step.

[0016] The ultraviolet cleaning step is a step of irradiating the treatment object with ultraviolet light having a wavelength of 120 nm or more and less than 190 nm.

[0017] In the carbonated water cleaning step, the carbonated water may be applied along with megasonics.

[0018] The carbonated water wash step may further include a second wash.

[0019] The second cleaning is a process in which both carbonated water and hydrogen water are applied to the object to be treated as cleaning liquids.

[0020] The change in optical density of the laminate before the preparation step and the laminate after the carbonated water washing step may be 0% or more and 0.1% or less.

[0021] The change in thickness of the laminate before the treatment in the preparation step and the laminate after the carbonated water washing step may be 0 angstroms or more and 5 angstroms or less.

[0022] In order to achieve the above object, a laminate according to another embodiment is a laminate having a light-shielding film disposed thereon, the light-shielding film including a transition metal and at least one of oxygen and nitrogen, the light-shielding film having a reflectance of 35% or less for light having a wavelength of 193 nm, and the laminate having a residual ion content measured by an ion chromatography method, the residual ions including sulfur-based ions and nitrate-based ions, the sulfur-based ion content being 0 ng / cm2 Super 0.1ng / cm 2 The content of nitrate ions is 0 ng / cm or less. 2 Super 0.1ng / cm 2 The following is the result.

[0023] The residual ions may include halogen ions, and the content of the halogen ions is 0 ng / cm 2 Super 0.1ng / cm 2 It may be the following.

[0024] The transition metal may include chromium, and the halide ion may include a fluorine ion or a chloride ion.

[0025] The residual ions may include ammonium ions, and the content of the ammonium ions may be less than 0 ng / cm 2 Super 1.0ng / cm 2 It may be the following.

[0026] The residual ions may include ionic impurities, such as the sulfur ions, the nitrate ions, the halogen ions, and the ammonium ions, and the content of the ionic impurities is 0 ng / cm 2 Super 1.5ng / cm 2 It may be the following.

[0027] The residual ions may include sodium ions, phosphate ions, potassium ions, magnesium ions, and calcium ions, and the sum of the sodium ion content, the phosphate ion content, the potassium ion content, the magnesium ion content, and the calcium ion content is 0 ng / cm 2 More than 0.01ng / cm 2 It may be the following.

[0028] The laminate may be a photomask blank or a photomask. Effect of the Invention

[0029] The laminate manufacturing method and laminate of the embodied examples can effectively prevent unintended haze from occurring during the exposure process by removing particles present on the outer surface or surface of the laminate while minimizing changes in the properties of the laminate. BEST MODE FOR CARRYING OUT THEINVENTION

[0030] Although the present invention is described in detail below so that those skilled in the art can easily implement the present invention, the present invention may be embodied in many different forms and should not be construed as limited to the embodiments set forth herein.

[0031] As used herein, terms of degree such as "about," "substantially," and the like are used in a numerical or approximate sense when the tolerances of manufacturing and materials inherent in the referred meaning are given, and are used to prevent unscrupulous infringers from unfairly taking advantage of disclosures in which precise or absolute numerical values ​​are referred to to aid in the understanding of the embodiments.

[0032] Throughout this specification, the term "combinations thereof" in a Markush form phrase means a mixture or combination of one or more selected from the group of elements set forth in the Markush form phrase, including one or more selected from the group of elements.

[0033] Throughout this specification, the phrase "A and / or B" means "A, B, or A and B."

[0034] Throughout this specification, terms such as "first", "second" or "A", "B" are used to distinguish identical terms from one another, unless otherwise specified.

[0035] In this specification, the term "B is located on A" means that B can be located on A, or B can be located on A with another layer located therebetween, and is not to be interpreted as being limited to B being located in contact with the surface of A.

[0036] In this specification, the term "singular" is to be construed as including the singular or plural as the context requires, unless otherwise specified.

[0037] In this specification, ppm is based on weight unless otherwise specified.

[0038] In this specification, room temperature is any one of temperatures between about 20°C and about 25°C.

[0039] In this specification, humidity means relative humidity.

[0040] In this specification, light intensity refers to the intensity of the light source.

[0041] The embodiments will be described in more detail below.

[0042] Manufacturing method of laminate To achieve the above object, a method for manufacturing a laminate according to an embodiment of the present invention includes a preparation step and a carbonated water washing step.

[0043] The method for producing the laminate may include a step of producing a light-shielding film, a preparation step, and a step of washing with carbonated water.

[0044] The method for producing the laminate may include a preparation step, an ultraviolet ray cleaning step, and a carbonated water cleaning step.

[0045] The method for producing the laminate may include a step of producing a light-shielding film, a preparation step, an ultraviolet ray cleaning step, and a carbonated water cleaning step.

[0046] The method for manufacturing the laminate may include a preparation step, a carbonated water washing step, and a rinsing step.

[0047] The method for producing the laminate may include a step of producing a light-shielding film, a preparation step, a carbonated water washing step, and a rinsing step.

[0048] The method for manufacturing the laminate may include a preparation step, an ultraviolet cleaning step, a carbonated water cleaning step, and a rinsing step.

[0049] The method for manufacturing the laminate may include a step of manufacturing a light-shielding film, a preparation step, a UV cleaning step, a carbonated water cleaning step, and a rinsing step.

[0050] The preparation step is a step of providing a processing target, which is a pre-processing laminate having a light-shielding film (described later) disposed thereon.

[0051] The preparation step may include a process of placing and fixing the processing object in the chamber, or placing an apparatus in which a number of processing objects are arranged side by side in the chamber.

[0052] The ultraviolet cleaning step is a step of irradiating the treatment object with ultraviolet light having a wavelength of 120 nm or more and less than 190 nm. The wavelength of the ultraviolet light may be 138 nm or more and less than 185 nm, or 154 nm or more and less than 178 nm.

[0053] The irradiation of ultraviolet light may be performed by a light source, and one or more light sources may be arranged, in which case light of a uniform intensity may be irradiated onto the surface of the substrate to be cleaned.

[0054] The UV cleaning step is performed at 20 mW / cm 2 More than 55mW / cm 2 The UV cleaning step may be performed with a light intensity of 30 mW / cm 2 More than 50mW / cm 2 The UV cleaning step may be performed at a light intensity of 35 mW / cm 2 More than 45mW / cm 2 The following light amounts may be used:

[0055] The ultraviolet cleaning step can efficiently remove compounds that strongly absorb wavelengths in the range of about 100 nm to about 190 nm before performing the subsequent steps. Specifically, the ultraviolet cleaning step can transfer light energy to particles including organic matter, induce chemical bonds in the organic matter to be broken, and promote decomposition and removal of the particles including organic matter, thereby further improving the reliability of the manufacturing method overall.

[0056] The carbonated water cleaning step is a step of providing a cleaned laminate by applying a carbonated water cleaning process in which ultraviolet light and carbonated water are applied to the treatment object.

[0057] The carbonated water washing step may be selectively applied as a first wash, a second wash, or a third wash, which will be described below.

[0058] The first wash is a process where UV light and carbonated water are both applied.

[0059] In the carbonated water cleaning step, the ultraviolet light may have any one of wavelengths ranging from 190 nm to 290 nm. In the carbonated water cleaning step, the ultraviolet light may have any one of wavelengths ranging from 230 nm to 280 nm. In the carbonated water cleaning step, the ultraviolet light may have an intensity of 1 mW / cm 2 More than 11mW / cm 2 In the carbonated water washing step, the ultraviolet light may be irradiated with a light amount of 3 mW / cm 2 More than 10mW / cm 2 In the carbonated water washing step, the ultraviolet light may be irradiated with a light amount of 4 mW / cm 2 More than 9mW / cm 2 The following light doses may be applied: In this case, it is possible to apply carbonated water to minimize damage to the substrate while still allowing for efficient cleaning.

[0060] In the carbonated water cleaning step, the carbonated water may have an electrical conductivity of 1 μS / cm or more and 10 μS / cm or less. The carbonated water may have an electrical conductivity of 2 μS / cm or more and 8 μS / cm or less. The carbonated water may have an electrical conductivity of 3 μS / cm or more and 7 μS / cm or less. By using carbonated water having the above electrical conductivity, damage to the surface of the laminate can be minimized and an excellent cleaning effect can be obtained.

[0061] In the carbonated water washing step, carbonated water is washed over an area of ​​504 cm 2 of the laminate. 2 The carbonated water may be supplied at a rate of 1,500 to 4,000 ml / min per 504 cm2 of the laminate. 2 The carbonated water may be supplied at a rate of 2,000 to 3,000 ml / min per nozzle. The carbonated water may be supplied through one nozzle, or through two or more nozzles.

[0062] The combined application of UV light and carbonated water provides excellent cleaning results while reducing surface damage to the laminate and improving process efficiency.

[0063] Megasonics may be applied together with the carbonated water, which is the cleaning liquid. The megasonics may be applied through a megasonics generator attached to the nozzle when the cleaning liquid is sprayed through the nozzle, but is not limited thereto.

[0064] When cleaning the front surface of the laminate (the surface where the light-shielding film is exposed), the megasonics can be applied at 0.5 MHz to 1.3 MHz and 5 W to 12 W. When cleaning the rear surface of the laminate (the surface where the quartz is exposed), the megasonics can be applied at 1 MHz to 1.8 MHz and 20 W to 45 W. When both megasonics are applied, more efficient cleaning can be achieved.

[0065] The second cleaning is a process in which both carbonated water and hydrogen water are applied. The second cleaning may be performed after the first cleaning. This refers to a process in which both carbonated water (DICO2) and hydrogen water (DIH2) are applied as cleaning liquids, and the carbonated water and hydrogen water may be applied in a volume ratio of 1:0.1 to 10, or a volume ratio of 1:0.5 to 2. The specific description of the carbonated water applied here is as described above, so the description will be omitted.

[0066] The hydrogen water may have a hydrogen content of 0.7 ppm to 3 ppm, or may have a hydrogen content of 0.9 ppm to 2 ppm.

[0067] Megasonics may also be applied in the second cleaning, the specific details of which are as described above.

[0068] The third cleaning is a process of cleaning the surface with hydrogen water. The concentration of hydrogen water, whether or not megasonics is applied, and the specific conditions thereof are as described above. The third cleaning may be applied together with the first or second cleaning.

[0069] The rinsing step is a step of rinsing the laminate with carbonated water and / or hydrogen water.

[0070] In the rinsing step, carbonated water is added to the laminated body in an amount of 504 cm 2 The liquid can be supplied to the rear surface of the laminate (the surface where the quartz is exposed, the surface farthest from the light-shielding film) at a rate of 500 to 2,000 ml / min per minute.

[0071] In the rinsing step, the carbonated water may have an electrical conductivity of 1 μS / cm or more and 10 μS / cm or less. The carbonated water may have an electrical conductivity of 2 μS / cm or more and 8 μS / cm or less. The carbonated water may have an electrical conductivity of 3 μS / cm or more and 7 μS / cm or less. The carbonated water may have a concentration measured by electrical conductivity that is the same as the concentration in the carbonated water washing step, or may have a different concentration.

[0072] The rinsing step may be performed by applying ozone water. The ozone water is applied only to the rear surface of the laminate, and is not substantially applied to the front surface (the surface on which the light-shielding film is exposed). This makes it possible to more efficiently control changes in the optical properties of the laminate caused by cleaning.

[0073] The ozone water may have an ozone concentration of 40 to 120 ppm (weight basis). The ozone water may have an ozone concentration of 50 to 110 ppm (weight basis), or 80 to 105 ppm (weight basis). The ozone water may be produced using an ozone generator manufactured by MKS.

[0074] The ozone water is applied to the laminated body having an area of ​​504 cm 2 The liquid can be supplied to the rear surface of the laminate (the surface where the quartz is exposed, the surface farthest from the light-shielding film) at a rate of 300 to 1,000 ml / min per minute.

[0075] In the method for manufacturing the laminate, a separate ozone water is not applied to the light-shielding film during the preparation step to the rinsing step, thereby minimizing chemical changes or loss of the surface layer of the light-shielding film.

[0076] The carbonated water and hydrogen water described above are substantially free of ozone. The meaning of the fact that the carbonated water and / or hydrogen water are substantially free of ozone includes the case where the carbonated water and / or hydrogen water contains a trace amount of ozone that is not capable of functioning as ozone water, and for example, the ozone concentration may be 10 ppm or less.

[0077] When the carbonated water or the carbonated water and the hydrogen water are used, the loss of the light-shielding film caused by ozone can be substantially suppressed, and the change in physical properties of the light-shielding film that may occur during the process of cleaning can be minimized.

[0078] It is believed that the durability of the light-shielding film varies depending on the form of the oxide film of transition metal M and oxygen O. Specifically, it is believed that the oxide film is more stable when it is in the form of M2O3. However, when the M2O3 oxide film comes into contact with ozone, a part of it may change to the form of MO3. MO3 may cause surface loss of the light-shielding film itself or change in the physical properties of the entire light-shielding film. This is believed to be because the M2O3 oxide film is not easily damaged or removed during cleaning, but the MO3 oxide film is relatively easily damaged or removed during cleaning.

[0079] By applying the carbonated water washing step of the embodiment, it is possible to provide a laminate in which loss of the light-shielding film and changes in physical properties are minimized, and detection of trace amounts of foreign matter and residual ions is minimized.

[0080] A detailed description of the laminate itself, such as the form of the oxide on the surface and the level of residual ions found in the laminate after cleaning, will be omitted since they will be described in detail later.

[0081] The laminate includes a light-shielding film disposed on a support, and can be manufactured in a manufacturing step of the light-shielding film by applying a sputtering method.

[0082] A specific description of the support will be omitted since it overlaps with the description of the laminate described later.

[0083] The light-shielding film can be manufactured by a sputtering method.

[0084] The sputtering method is a method in which a target containing a transition metal is placed and sputtering is performed in an atmosphere containing a reactive gas including an oxygen atom-containing gas, a nitrogen atom-containing gas, or a carbon atom-containing gas, and the atmosphere may contain both a reactive gas and an inert gas.

[0085] The target may be a single target containing a transition metal.

[0086] The targets may be applied in combination with two or more targets, including one target containing a transition metal.

[0087] The target containing a transition metal may contain 90 at% or more of the transition metal.The target containing a transition metal may contain 95 at% or more of the transition metal.The target containing a transition metal may contain 99 at% of the transition metal.

[0088] The target containing a transition metal may be a target made of a transition metal contained in a light-shielding film. In this case, "made of a transition metal" may mean a target made of one type of transition metal or a target made of two or more types of transition metals. In this case, "made of a transition metal" includes a case where the transition metal contains unavoidable impurities, and is not interpreted as being limited to a target made of only a transition metal in the strict sense.

[0089] The transition metal may include at least one of Cr, Ta, Ti, and Hf. The transition metal may include Cr.

[0090] The reactive gas reacts with the transition metal to form a sputtering film. For example, any one selected from the group consisting of a transition metal oxide, a transition metal nitride, a transition metal carbide, and combinations thereof may be formed as the light-shielding film. The light-shielding film may be entirely amorphous or may be partially amorphous containing crystals.

[0091] Examples of oxygen atom-containing gases include oxygen, carbon oxides (CO, CO2, etc.), and nitrogen oxides (NO, NO2, N2O, N2O3, etc.). Examples of nitrogen atom-containing gases include nitrogen and nitrogen oxides (NO, NO2, N2O, N2O3, etc.). Examples of carbon atom-containing gases include carbon oxides (CO, CO2, etc.), and methane. To introduce oxygen atoms into the light-shielding film, it is preferable to use an oxygen-containing compound rather than oxygen itself, since the reaction can be more easily controlled.

[0092] The inert gas may be, for example, helium gas, argon gas, or the like, but is not limited thereto.

[0093] The sputtering is performed by the steps of: i) placing a target and a support in a chamber and injecting an atmospheric gas into the chamber; ii) applying power to the sputtering equipment; and iii) forming a film on the support by transition metal particles detached from the target together with oxygen, nitrogen, or carbon contained in a reactive gas.

[0094] The release of the transition metal particles may be performed by a sputtering gas, which refers to a gas that is ionized in a plasma atmosphere and collides with a target.

[0095] The sputtering gas may be argon (Ar) gas.

[0096] The power source applied for sputtering may be a DC power source or an RF power source.

[0097] The power applied to the sputtering can be set to 1.5 kW or more and 2.5 kW or less.

[0098] The light-shielding film may be heat-treated, which can remove unnecessary stress generated during the formation of the light-shielding film and improve the physical properties of the light-shielding film, such as improving the smoothness of the light-shielding film.

[0099] When the heat treatment is performed in an oxygen-containing atmosphere, a light-shielding film surface layer having an increased oxygen content can be formed on the surface of the light-shielding film.

[0100] When the heat treatment is performed in a nitrogen-containing atmosphere, a light-shielding film surface layer having an increased nitrogen content can be formed on the surface of the light-shielding film.

[0101] The heat treatment may be carried out at a temperature of about 150°C or more and about 330°C or less.

[0102] The heat treatment may be carried out for a period of not less than about 5 minutes and not more than about 30 minutes.

[0103] The light-shielding film thus produced has the characteristics of the laminate which will be described in detail below.

[0104] The method for manufacturing the laminate may include a preparation step, an ultraviolet cleaning step, a carbonated water cleaning step, and a rinsing step as a cleaning process of the laminate.

[0105] Laminate The laminate to be treated includes a light-shielding film.

[0106] A light-shielding film is disposed on the laminate to be processed.

[0107] Specifically, the laminate may include a light-shielding film disposed on a support.

[0108] The light-shielding film may cover the entire surface of the support, or may cover only a portion of the surface.

[0109] The support may be a light-transmitting substrate.

[0110] The support may be a light-transmitting substrate on which a light-shielding film is directly disposed.

[0111] The support may be a light-transmitting substrate having a phase shift film disposed thereon, and a light-shielding film disposed thereon.

[0112] The support may be one in which a light-shielding film is partially disposed. Specifically, the light-shielding film may be disposed on a light-transmitting substrate in direct contact with the light-transmitting substrate. Alternatively, the light-shielding film may be disposed on a phase shift film disposed on a light-transmitting substrate. Furthermore, the support may be one in which the above-mentioned arrangements are mixed on one substrate.

[0113] The object to be treated may be a laminate including a light-shielding film. The laminate may have an optical application. The object to be treated may be a photomask blank or a photomask.

[0114] The light-transmitting substrate may be a quartz substrate, etc. In this case, the light-transmitting substrate means a substrate having a transmittance of about 85% to about 100%, and the exposure light may be, but is not limited to, ArF light.

[0115] The phase shift film can be any phase shift film used in the field of photomasks. For example, the phase shift film may contain molybdenum and / or silicon, or may contain an oxide or nitride thereof.

[0116] The laminate may include both a portion (light-transmitting portion) that does not have a phase shift film on the support and a portion (phase shifting portion) that has a phase shift film. The phase difference between the light-transmitting portion and the phase shifting portion may be about 160° to about 230°, or about 168° to about 185°.

[0117] The light-shielding film may be a film containing a transition metal and oxygen, nitrogen, or carbon.

[0118] The transition metal may include at least one of Cr, Ta, Ti, and Hf. The transition metal may include Cr.

[0119] Specifically, the light-shielding film may include Cr and any one selected from the group consisting of oxygen, nitrogen, carbon, and combinations thereof.

[0120] Specifically, the light-shielding film may include any one selected from the group consisting of CrO, CrON, CrOCN, and combinations thereof.

[0121] The light-shielding film may have a substantially two-layer structure. For example, the light-shielding film surface layer may be configured so that the oxygen or nitrogen content is higher on the surface side of the light-shielding film in order to control the surface strength of the light-shielding film. The light-shielding film other than the light-shielding film surface layer is referred to as a light-shielding film lower layer in order to distinguish it from the light-shielding film surface layer.

[0122] The light-shielding film surface layer may have a thickness of 30 to 80 nm, or 40 to 70 nm. The light-shielding film lower layer and the light-shielding film surface layer may have a thickness ratio of 1:0.02 to 0.25, or 1:0.04 to 0.18. However, the boundary between the light-shielding film surface layer and the light-shielding film lower layer may not be clearly observed. In such a case, the region with an oxygen content of 25 atomic % or less can be treated as the light-shielding film surface layer.

[0123] When the above-mentioned carbonated water cleaning step is applied to the surface layer of the light-shielding film, the change in physical properties before and after the cleaning process can be minimized, and damage to the surface layer of the light-shielding film can be substantially suppressed.

[0124] The change in thickness of the laminate between the laminate before the preparation step and the laminate after the carbonated water washing step may be about 0 Å to about 5 Å. The change in thickness may be about 0 Å to about 2 Å, or about 0.1 Å to about 1.5 Å. The change in thickness shows a tendency for the thickness to become thinner. This is believed to be due to the detachment of some metal oxides due to the above-mentioned oxidation reaction. However, the change in thickness may also be an increase in thickness, and is not to be interpreted as being limited to a decrease in thickness.

[0125] The laminate may have a transmittance change of about 0% to 0.05% between the laminate before the preparation step and the laminate after the carbonated water washing step, or the transmittance change may be about 0% to 0.03%, or about 0% to 0.008%.

[0126] The change in optical density of the laminate before the preparation step and the laminate after the carbonated water washing step may be about 0% to about 0.1%. The change in optical density may be about 0% to about 0.05%, or about 0% to about 0.01%. The change in optical density indicates a tendency for optical density to decrease, which is considered to be associated with the change in thickness. However, the change in optical density is not limited to a decrease.

[0127] The change in reflectance of the laminate before the preparation step and after the carbonated water washing step may be about 0% to about 0.5%. The change in reflectance may be about 0% to about 0.25%.

[0128] The laminate after treatment (washing) may be one in which very fine particles of 50 nm or less in size are substantially not detectable, where by very fine particles are substantially not detectable, it is meant that when one laminate is inspected, very fine particles are not detected, or there are no more than two, or no more than one, or none at all.

[0129] The laminate after the treatment may also have a controlled residual ion content as described below. In this case, a low residual ion content means that the residual ion content measured by a specific method is less than the content described below.

[0130] The laminate of the embodiment is characterized by a small content of residual ions as measured by ion chromatography.

[0131] Ultrafine particles that are adsorbed to the laminate and are not completely removed even during the cleaning process, or ions remaining in the laminate itself, can adversely affect the quality of the laminate. When the laminate is used, elements that become unstable due to repeated energy irradiation can move to the surface, and residual ions inside the laminate can meet with other ions and cause unintended reactions. This can result in the formation of particulate impurities or the generation of haze in some parts of the laminate.

[0132] If the amount of residual ions detected during the post-cleaning inspection process is small, the formation of particulate impurities and / or the occurrence of haze can be reduced. Furthermore, the suppression of the formation of particulate impurities and the suppression of the occurrence of haze have recently been evaluated as more important properties as semiconductor designs evolve to finer lines.

[0133] The measurement of residual ions using ion chromatography is performed according to the method described in the Examples. Briefly, the process of measuring residual ions is as follows: one laminate stored in a product storage box is placed in a clean bag, 100 ml of deionized water is poured into it, and the clean bag is then placed in a water bath prepared at 90°C. The laminate is then left for 120 minutes so that ions can be sufficiently released from the surface of the laminate. The deionized water collected from the clean bag is detected by ion chromatography to determine the concentration. The size of the laminate is approximately 5 inches to 7 inches wide, approximately 5 inches to 7 inches long, and approximately 0.1 inches to 0.5 inches high. In the case where the size (surface area) of the laminate changes, the amount of deionized water can be changed in proportion to the size of the laminate.

[0134] The residual ions may include sulfur-based ions.

[0135] Sulfur ions include sulfate ions (SO4 2- ) including SOx.

[0136] The residual ions may include nitrate ions.

[0137] Nitrate ions are nitrite ions (NO2 - ), nitrate ion (NO3 - ) including NOx.

[0138] The content of the sulfur-based ions is about 0.1 ng / cm 2 or less, or about 0.8 ng / cm 2The content of the sulfur-based ions may be about 0 ng / cm or less. 2 may be greater than about 0.1 ng / cm 2 or about 0.3 ng / cm 2 It may be super.

[0139] The content of the nitrate ions is about 0.1 ng / cm 2 or less, or about 0.05 ng / cm 2 The content of the nitrate ions may be about 0 ng / cm or less. 2 or about 0.1 ng / cm 2 It may be super.

[0140] The above-mentioned contents of the sulfur-based ions and the nitrate-based ions are excellent residual ion contents for applying the laminate as a photomask, and in particular, can substantially suppress the generation of haze that may occur during the use of the photomask.

[0141] The residual ions may include halogen ions.

[0142] The halogen ions can include fluorine ions, chloride ions, or both.

[0143] The content of the halogen ions is about 0.1 ng / cm 2 or less, about 0.05 ng / cm 2 or less, or about 0.03 ng / cm 2 The halogen ion content may be about 0 ng / cm or less. 2 Greater than or about 0.01ng / cm 2 It may be more than that.

[0144] When chromium is included as the transition metal, the content of the halogen ions may be high, which is believed to be because chromium has a high affinity for chloride ions and the like, and thus attracts chloride ions and the like in the air or in the treatment solution.

[0145] The residual ions may include ammonium ions.

[0146] The content of the ammonia ions is about 1.0 ng / cm 2 or less, about 0.7 ng / cm 2 or less, or about 0.5 ng / cm 2 The ammonium ion content may be about 0 ng / cm or less. 2 may be greater than about 0.1 ng / cm 2 or about 0.3 ng / cm 2 When the content of the ammonium ions is within the above range, the generation of particulate impurities and the generation of haze can be substantially suppressed.

[0147] The residual ions may include sulfur ions, nitrate ions, halogen ions, and ammonium ions, and more specifically, SO4 2- , NO2 - , NO3 - , Cl - and NH4 + are called ionic impurities.

[0148] The content of the ionic impurities is about 1.5 ng / cm 2 or less, about 1.0 ng / cm 2 or less, or about 0.7 ng / cm 2 The content of the ionic impurities may be about 0 ng / cm 2 may be greater than about 0.1 ng / cm 2 or about 0.3 ng / cm 2 It may be super.

[0149] It is believed that the content of ionic impurities in a laminate having such characteristics is very well controlled when a light-shielding film is formed, and when such a laminate is used as a photomask or the like, it is easier to control defects.

[0150] The residual ions may include sodium ions.

[0151] The residual ions may include phosphate ions.

[0152] The residual ions may include potassium ions.

[0153] The residual ions may include magnesium ions.

[0154] The residual ions may include calcium ions.

[0155] The sum of the sodium ion content, the phosphate ion content, the potassium ion content, the magnesium ion content, and the calcium ion content is about 0 ng / cm 2 More than about 0.01ng / cm 2 In such a case, by well controlling the concentration of residual ions in the laminate, it is possible to provide a photomask that substantially reduces the possibility of occurrence of particulate defects and reduces the degree of occurrence of haze.

[0156] The light-shielding film may have a reflectance to the exposure light of about 35% or less, or about 30% or less. The reflectance may be about 20% or more, about 23% or more, or about 25% or more.

[0157] The exposure light may be light with a wavelength of about 193 nm.

[0158] The exposure light may be ArF light.

[0159] The light-shielding film serves to block at least a part of light of an intended wavelength. Therefore, the light-shielding film may have a relatively high surface reflectance compared to a light-transmitting film. However, if the reflectance of the light-shielding film is too high, the accuracy of the inspection result for checking the presence or absence of defects in the laminate may decrease. The inspection process is a process for checking the presence or absence of surface defects and impurities in the light-shielding film, and is applied to the manufacturing process of the photomask blank. That is, if the surface reflectance of the light-shielding film is too high, the reliability of the laminate may decrease. Therefore, it is necessary to adjust the surface reflectance of the light-shielding film. The inspection light may be applied in the same manner as the exposure light or in a different manner, and the reflectance based on the exposure light has been presented above.

[0160] In order to obtain effects such as adjusting the surface reflectance of the light-shielding film and improving durability, the characteristics of the surface layer of the light-shielding film and the lower layer of the light-shielding film may be controlled differently. For this purpose, the surface layer of the light-shielding film may be laminated so that the distribution of oxygen or nitrogen is higher than that of the lower layer of the light-shielding film, or a method of performing an oxidation treatment or a nitridation treatment on the surface of an already formed light-shielding film may be applied.

[0161] When the light-shielding film contains a compound in the form of M2O3 (M is a transition metal, O is oxygen), a part of the compound may be changed to the form of MO3 by a process such as oxidation. For example, when chromium is used as the transition metal, a part of Cr2O3 may be changed to CrO3 by an oxidation process, cleaning, etc., so that the content of CrO3 in the surface layer of the light-shielding film may be substantially high. Since Cr2O3 has a relatively strong property against external forces and damage, CrO3 is more easily lost than Cr2O3. Therefore, a light-shielding film containing a large amount of CrO3 is more likely to lose the film itself during a process such as cleaning. This may cause various changes in optical properties such as changes in thickness, optical density, transmittance, and reflectance. In addition, it is considered that a light-shielding film containing a large amount of CrO3 is more likely to lose the film itself when a relatively strong oxidation cleaning process is performed. However, if cleaning is not sufficient, residual ions and impurities in the laminate may not be sufficiently removed.

[0162] The light-shielding film provides a method for manufacturing a laminate that minimizes changes in the optical properties of the light-shielding film, such as reflectance, while reducing the content of impurities and residual ions by applying a manufacturing method including the above-mentioned cleaning process.

[0163] The light-shielding film contains a transition metal and at least one of oxygen and nitrogen.

[0164] The light-shielding film may contain the transition metal at about 35 at% or more, about 40 at% or more, about 45 at% or more, or about 50 at% or more. The light-shielding film may contain the transition metal at about 75 at% or less, about 70 at% or less, about 65 at% or less, or about 60 at% or less. In this case, the transition metal content of the light-shielding film means the average value of the transition metal content in the entire light-shielding film including the light-shielding film lower layer and the light-shielding film surface layer.

[0165] The light-shielding film may contain oxygen in an amount of about 15 at% or more, about 20 at% or more, or about 25 at% or more. The light-shielding film may contain oxygen in an amount of about 55 at% or less, about 50 at% or less, or about 45 at% or less. In this case, the oxygen content of the light-shielding film means the average oxygen content of the entire light-shielding film including the light-shielding film lower layer and the light-shielding film surface layer.

[0166] The light-shielding film may contain nitrogen at about 15 at% or more, about 20 at% or more, or about 25 at% or more. The light-shielding film may contain nitrogen at about 55 at% or less, about 50 at% or less, or about 45 at% or less. In this case, the nitrogen content of the light-shielding film means the average nitrogen content of the entire light-shielding film including the light-shielding film lower layer and the light-shielding film surface layer.

[0167] The light-shielding film may contain carbon at about 1 at% or more, about 2 at% or more, or about 3 at% or more. The light-shielding film may contain carbon at about 10 at% or less, or about 8 at% or less. In this case, the carbon content of the light-shielding film means the average carbon content of the entire light-shielding film including the light-shielding film lower layer and the light-shielding film surface layer.

[0168] The light-shielding film surface layer may contain the transition metal at about 10 at% or more, about 15 at% or more, or about 20 at% or more. The light-shielding film surface layer may contain the transition metal at about 45 at% or less, about 40 at% or less, about 35 at% or less, or about 30 at% or less.

[0169] The light-shielding film surface layer may contain oxygen at about 35 at% or more, about 40 at% or more, or about 42 at% or more. The light-shielding film surface layer may contain oxygen at about 65 at% or less, about 60 at% or less, about 55 at% or less, or about 50 at% or less.

[0170] The light-shielding film surface layer may contain nitrogen at about 1 at% or more, about 3 at% or more, or about 5 at% or more. The light-shielding film surface layer may contain nitrogen at about 25 at% or less, about 20 at% or less, or about 15 at% or less.

[0171] The light-shielding film surface layer may contain carbon in an amount of about 3 at% or more, about 5 at% or more, or about 10 at% or more. The light-shielding film surface layer may contain carbon in an amount of about 35 at% or less, about 30 at% or less, or about 25 at% or less.

[0172] The present invention will be described in more detail with reference to the following specific examples. The following examples are merely illustrative for the purpose of aiding understanding of the present invention, and are not intended to limit the scope of the present invention.

[0173] Experimental Example: Preparation Example (Production of laminate having light-shielding film) A synthetic quartz light-transmitting substrate measuring 6 inches wide, 6 inches long, and 0.25 inches thick was prepared with a phase shift film having a phase difference of approximately 180° for light with a wavelength of 193 nm on the same substrate, and was used to manufacture the following light-shielding film.

[0174] Phase shift films are manufactured by the sputtering method. During film formation, an excess amount of nitrogen gas is injected to induce the production of high-concentration NH4, and the No x The phase shift film was formed by reactive sputtering using a target with a composition ratio of Mo of 10.75 at% and Si of 89.25 at%. A power of 2 kW was applied, gas was introduced, and the film was formed by sputtering while rotating the light-transmitting substrate. During film formation, nitrogen (N2) gas and argon gas were introduced to maintain a remaining amount of 70 volume %, and the ammonium concentration on the surface was adjusted to 50 ng / cm. 2 ~110ng / cm 2 The phase shift film thus formed was heat-treated at 400° C. for 40 minutes, and then cooled at 25° C. for 40 minutes.

[0175] The light-shielding film was also produced by sputtering.

[0176] The substrate on which the phase shift film was formed was placed in the chamber of the DC sputtering equipment, and the T / S distance of the chromium target was set to 255 mm, and the angle between the substrate and the target was set to 25°. The atmospheric gas used was nitrogen (N2) and carbon dioxide (CO2) in a volume ratio of 1:3 to 3.5. The power applied during film formation was approximately 1.5kW to approximately 1.85kW.

[0177] Sputtering was performed while rotating the substrate, and a chromium-containing light-shielding film was formed. Then, heat treatment was performed at the same temperature of 200°C to 300°C for 15 minutes, and the light-shielding film after heat treatment was cooled by applying dry air for 5 minutes in an atmosphere of 20°C to 30°C. A light-shielding film with a total thickness of about 460 to about 580 angstroms was formed on the phase shift film, and a laminate was prepared.

[0178] The element contents of the light-shielding film thus formed were confirmed to be 35.5-41.9 atomic % chromium, 8.4-10.5 atomic % nitrogen, 33.0-36.3 atomic % oxygen, and 14.0-15.4 atomic % carbon, depending on the depth. Trace amounts of Si (0-6.5 atomic %) were also confirmed.

[0179] (Light-shielding film cleaning: Example) (1) UV cleaning step Through the UV treatment method, UV (ultraviolet rays, wavelength 172 nm), a type of electromagnetic radiation, was irradiated under the conditions of RT (23°C) and humidity 45% ± 5% under uniform radiation exposure conditions. The irradiation was 40 mW / cm 2 The process was carried out at high power, using N2, O2, etc. as process gases, and a strong exhaust (0.01~1kPa) was used during the process to prevent contamination sources from recombining on the mask surface or back contamination due to bounce back. Through this UV treatment, compounds that strongly absorb wavelengths in the range of about 100nm to about 190nm were removed in advance before the subsequent cleaning process.

[0180] (2) Carbonated water washing step Cleaning was performed using UV (wavelength 254 nm) and the cleaning solution, carbonated water (DICO2), simultaneously (first cleaning).

[0181] At this time, cleaning using carbonated water or the like as a cleaning liquid was performed by applying megasonics, and megasonics were applied together with the spraying of the cleaning liquid from the nozzle. When cleaning the front surface (light-shielding film surface) of the laminate, megasonics of 1 MHz and 10 W were applied together with the cleaning liquid, and when cleaning the rear surface (quartz surface) of the laminate, megasonics of 1.5 MHz and 40 W were applied together with the cleaning liquid. At this time, carbonated water with an electrical conductivity of 3 to 6 μS / cm was applied.

[0182] Next, the surface was washed using a washing solution containing hydrogen water and carbonated water (second washing). The hydrogen water used had a hydrogen concentration of 1.0 to 2.0 ppm. The concentration of the carbonated water and the megasonics applied to the front and back were the same as described above. The hydrogen water and the carbonated water were applied in a volume ratio of 4:3.

[0183] Thereafter, the surface was washed with hydrogen water (DIH2) (third washing). The hydrogen ion concentration of the hydrogen water and the application of megasonics were the same as described above.

[0184] (3) Rinse step After cleaning is completed, the wafer is rinsed with carbonated water (DICO2) and then dried using the ramp-up method.

[0185] (Light-shielding film cleaning: Comparative example) All other steps were the same as in the above washing method, except that no carbonated water (DICO2) was added during the washing process.

[0186] The characteristics of the light-shielding film were measured before and after cleaning, and are shown in Table 3 below.

[0187] Experimental Example: Measurement Example 1 (Sampling and pretreatment) Storage / pretreatment conditions: Stored in a shipping box, unloaded through a shipping box port (SBP) and loaded into a pod. All samples were placed in independent pods and processed individually, and the washed laminates were placed in separate washed product storage boxes for ion chromatography (IC) testing. All conditions (control variables) were kept the same except for the change in process conditions for evaluation (control variables).

[0188] (Ion chromatography evaluation) The evaluation was carried out using a ThermoScientific Dionex ICS-2100 ion chromatography model according to the following method. The same method was applied to each of the samples in Table 1.

[0189] (Ion extraction) The prepared laminate sample was placed in a clean bag immediately after opening the product storage box, and 100 ml of deionized water was poured in. The clean bag containing the sample was placed in a water bath prepared at 90°C for 120 minutes so that the ions could be sufficiently extracted onto the surface of the laminate.

[0190] (Eluent Delivery) An isocratic process was performed to obtain an eluent that helps separate ions, and to keep the concentration and composition of the eluent constant during subsequent processes.

[0191] Measurement: The eluent and sample were injected into the measuring device, and ions were separated and detected.

[0192] The ion exchange column used was a ThermoScientific Dinex ICS-2100 ion chromatography model, and the concentration of the ions was quantified using the signal obtained from the electrical conductivity of the separated ions and the RT (retention time) of the ions. The results are shown in Tables 1 and 2 below, respectively.

[0193] Experimental Example: Measurement Example 2 (Sampling and pretreatment) Storage / pretreatment conditions: All laminates were placed in independent pods and processed individually. After cleaning, the laminates were placed in separate pods that had been cleaned for ellipsometer measurement. All other conditions (control variables) were kept the same except for the changes in process conditions for evaluation (control variables).

[0194] (Ellipsometer evaluation) Using Nanoview's MG-PRO model, measurements were taken at 7 x 7 points (total 49 points) of the sample.

[0195] Measurement results (Residual ion content) The results of the ion chromatography (IC) test are shown in Tables 1 and 2 below. As an example, the results of measuring a sample that had been washed with carbonated water are shown, and as a comparative example, the results of measuring a sample that did not use carbonated water are shown.

[0196] The calculation of ion content was according to the following formula: ng / laminated body = (IC analysis result - Blank) x amount of DIW, ng / cm 2 = (ng / laminar structure) / 504(laminar structure area, cm 2 ) ppb=100ml standard.

[0197] [Table 1]

[0198] [Table 2]

[0199] Experimental Example: Additional Comparative Example and Measurement Example 3 (Additional Comparative Examples) The light-shielding film was formed and cleaned in the same manner as in the previous embodiment, except that ozone water was used as the cleaning liquid instead of carbonated water, and the ozone concentration of the ozone water was 80 to 105 ppm.

[0200] In the additional comparative example, changes in optical properties, etc., before and after cleaning were evaluated in the same manner as in the above-mentioned examples.

[0201] (Changes in light characteristics before and after cleaning) In the examples, a total of 23 repeated experiments were carried out to confirm the changes in thickness and optical properties of the laminate before and after cleaning, and the results are shown in Table 3. In addition, in the additional comparative examples, a total of 15 experiments were carried out to confirm the changes in thickness and optical properties of the laminate before and after cleaning, and the results are shown in Table 4.

[0202] [Table 3]

[0203] [Table 4]

[0204] Referring to Tables 1 and 2, it was confirmed that the laminate using carbonated water for cleaning suppressed the generation of ions that may cause haze when used as a photomask. Also, referring to Tables 3 and 4, it was confirmed that cleaning using carbonated water had excellent removal activity of foreign matter and ions, but only slight changes in the film. This effect is even clearer when compared with the additional comparative example using ozone, and it was confirmed that even when using laminates including the same light-shielding film, there was a difference in the rate of change of about 2 times in thickness, about 10 times in transmittance, and about 7 times in optical density depending on the cleaning process.

[0205] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the appended claims also fall within the scope of the present invention.

Claims

1. The method includes a preparation step of providing a processing target, which is a pre-processed laminate having a light-shielding film disposed thereon, and a carbonated water cleaning step of applying a first cleaning step of adding ultraviolet light and carbonated water to the processing target to provide a cleaned laminate, the light-shielding film contains a transition metal and oxygen, nitrogen, or carbon; The laminate has a content of residual ions measured by an ion chromatography method, the residual ions including sulfur-based ions and nitrate-based ions; The sulfur-based ion content is 0 ng / cm 2 Super 0.1ng / cm 2 is as follows: The content of the nitrate ions is 0 ng / cm 2 Super 0.1ng / cm 2 The method for producing a laminate is as follows:

2. the light-shielding film is manufactured in a manufacturing step of a light-shielding film using a sputtering method, 2. The method for producing a laminate according to claim 1, wherein the sputtering method is a method in which a target containing a transition metal is placed and sputtering is performed in the presence of a reactive gas containing an oxygen atom-containing gas, a nitrogen atom-containing gas, or a carbon atom-containing gas.

3. In the carbonated water washing step, the ultraviolet light has a wavelength of 1 mW / cm2 in any one of the wavelengths ranging from 190 nm to 290 nm. 2 ~11mW / cm 2 The method for producing a laminate according to claim 1 , wherein the light is irradiated with a light amount of

4. The method for producing a laminate according to claim 1 , wherein in the carbonated water washing step, the carbonated water has an electrical conductivity of 1 μS / cm or more and 10 μS / cm or less.

5. The method further includes a UV cleaning step prior to the carbonated water cleaning step, The method for producing a laminate according to claim 1 , wherein the ultraviolet cleaning step is a step of irradiating the treatment object with ultraviolet light having a wavelength of 120 nm or more and less than 190 nm.

6. The method for producing a laminate according to claim 1 , wherein in the carbonated water washing step, the carbonated water is applied together with megasonics.

7. The carbonated water wash step further comprises a second wash; The method for manufacturing a laminate according to claim 1 , wherein the second cleaning is a process of applying both carbonated water and hydrogen water as cleaning liquids to the object to be treated after the first cleaning.

Citation Information

Patent Citations

  • Method for cleaning optical part and exposure device

    JP2002336804A

  • Photomask cleaning method and cleaning device

    KR100316374B1

  • Method for removing a growth particle on Phase Shift Mask

    KR100745065B1

  • Mask blank and method of producing the same, and transfer mask and method of producing the same

    WO2012086744A1