JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-31
Filing Date
2021-07-15
Publication Date
2024-10-04
Estimated Expiration
2041-07-15

AI Technical Summary

Technical Problem

Conventional polyvinyl alcohol (PVA)-based fluid loss reducing agents fail to maintain effectiveness under severe high temperature and pressure conditions in cement slurries, leading to dissolution and reduced fluidity, necessitating increased agent use which thickens the slurry and increases costs.

Method used

Development of polyvinyl alcohol polymers with specific structural characteristics, including controlled storage modulus and angular frequency-dependent loss tangent, achieved through copolymerization with vinyl ester and polyfunctional monomers, enhancing resistance to high temperatures and pressures.

Benefits of technology

The new polyvinyl alcohol polymers exhibit excellent fluid loss reduction even under severe conditions, maintaining slurry fluidity and reducing costs by avoiding excessive agent use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561854000002
    Figure 0007561854000002
  • Figure 0007561854000003
    Figure 0007561854000003
  • Figure 0007561854000001
    Figure 0007561854000001
Patent Text Reader

Abstract

The present invention provides a PVA having excellent heat resistance and pressure resistance. This polyvinyl alcohol-based polymer is obtained through saponification of: a homopolymer formed of a vinylester monomer; a copolymer of a vinylester monomer and a monofunctional monomer other than a vinylester; a copolymer of a vinylester monomer and a polyfunctional monomer; or a copolymer of a vinylester monomer, and a polyfunctional monomer and a monofunctional monomer other than a vinylester. When an aqueous solution of the polyvinyl alcohol-based polymer is filtered using a 100-mesh (opening: 0.154 mm) filter, the concentration thereof is adjusted to 10.0 mass%, the storage modulus G' (20°C) in the range of an angular frequency of 1.0-10.0 rad / s is measured in the aqueous solution, and the results are plotted in logarithmic scales for both axes; the inclination in the plot is 1.2 or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyvinyl alcohol polymer and uses thereof. [Background technology]

[0002] Polymers having a polyvinyl alcohol (PVA) skeleton (hereinafter, in this specification, these are collectively referred to as "polyvinyl alcohol-based polymers," "vinyl alcohol-based polymers," or simply "PVA") are known as hydrophilic synthetic resins, and various applications that take advantage of their properties are being developed.

[0003] One such use is as an additive to oil well cement, which is used in cementing oil wells, gas wells, and steam wells for geothermal power generation. Oil well cement is mixed with water and other additives, and filled into the gap between the steel pipe (casing) and the well to fix and protect it. For this reason, it is preferable for the cement slurry to have high fluidity so that it is easy to fill. The loss of water content from the cement slurry due to high pressure during injection and underground heat is generally called "fluid loss." Fluid loss reduces the fluidity of the cement slurry, causing poor cementing and poor hardening after hardening. For this reason, fluid loss reducing agents are usually added to the cement slurry.

[0004] It has been proposed to use polyvinyl alcohol polymers as the main component of such fluid loss reducing agents. For example, Patent Documents 1 and 2 describe PVA used in fluid loss reducing agents. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2007 / 146348 [Patent Document 2] JP 2015-196733 A Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, the pressure and temperature conditions have become more severe, especially for shale gas wells, as they have been extracted deeper. However, conventional PVA-containing fluid loss reducing agents have not yet achieved the fluid loss reduction performance required for cement slurries injected under such severe conditions of high temperature and pressure. Specifically, PVA-based fluid loss reducing agents dissolve at high temperatures, and dissolve into the well under high pressure conditions, resulting in a decrease in the fluid loss reduction effect. Therefore, PVA-based fluid loss reducing agents are required to be resistant to dissolution at high temperatures. At present, this is addressed by increasing the amount of conventional fluid loss reducing agents added, but the problem of reduced fluidity and increased costs due to the increased viscosity of the cement slurry has not been solved. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention provides the following.

[0008] A polyvinyl alcohol-based polymer obtained by saponification of a homopolymer made of a vinyl ester monomer, a copolymer of a vinyl ester monomer and a monofunctional monomer other than a vinyl ester, a copolymer of a vinyl ester monomer and a polyfunctional monomer, or a copolymer of a vinyl ester monomer, a monofunctional monomer other than a vinyl ester, and a polyfunctional monomer, The storage modulus G' (20°C) in the angular frequency range of 1.0 to 10.0 rad / s measured in an aqueous solution adjusted to a concentration of 10.0 mass% after filtering an aqueous solution of a polyvinyl alcohol polymer through a 100 mesh (0.154 mm opening) filter has a slope of 1.2 or less when plotted logarithmically. A polyvinyl alcohol polymer characterized by:

[0009] In one embodiment, the angular frequency-dependent loss tangent (tan δ) of the filtered 10.0 mass% aqueous solution is preferably in the range of 1.0 to 10.0 in the angular frequency range of 0.1 to 100 rad / s. In another embodiment, the polyvinyl alcohol-based polymer preferably has a degree of saponification of 72 to 99 mol%. In another embodiment, an additive for oil well cement containing the polyvinyl alcohol-based polymer can also be provided. Effect of the Invention

[0010] The polyvinyl alcohol polymer according to the present invention exhibits an excellent fluid loss reducing effect even under severe high temperature or high pressure environments. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a double logarithmic plot of the storage modulus G′ and loss modulus G″ measured for an aqueous solution (20° C.) of a polyvinyl alcohol-based polymer according to Example 1, the aqueous solution being adjusted to a concentration of 10.0 mass % after filtering the aqueous solution through a 100 mesh (opening: 0.154 mm) filter. [Diagram 2] FIG. 1 is a double logarithmic plot of the storage modulus G' and the loss modulus G'' measured for an aqueous solution (20°C) of a polyvinyl alcohol-based polymer according to Comparative Example 1, which was adjusted to a concentration of 10.0 mass % after filtering the aqueous solution through a 100 mesh (opening: 0.154 mm) filter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the mode for carrying out the present invention will be described. Note that the embodiment described below shows an example of the embodiment of the present invention, and the scope of the present invention is not to be interpreted narrowly by this. Numerical ranges in this specification include the upper and lower limits unless otherwise specified. The polymer in this specification follows the definition of polymer by the International Union of Pure and Applied Chemistry (IUPAC) Commission on Macromolecular Nomenclature, that is, "a polymer molecule is a molecule having a large relative molecular mass and a structure composed of a large number of repetitions of units that are substantially or conceptually derived from molecules having a small relative molecular mass."

[0013] <Chemical structure of polyvinyl alcohol polymer> The polyvinyl alcohol-based polymer according to the present invention is a polymer obtained by saponifying a homopolymer made of a vinyl ester monomer, a copolymer of a vinyl ester monomer and a monofunctional monomer other than a vinyl ester, a copolymer of a vinyl ester monomer and a polyfunctional monomer, or a copolymer of a vinyl ester monomer, a monofunctional monomer other than a vinyl ester, and a polyfunctional monomer. The polyvinyl alcohol-based polymer according to the present invention has a polymer structure that can withstand high temperatures and pressures that conventional PVA cannot withstand. The presence of such a polymer structure can be determined from the rheological properties of the polymer, and more specifically, is guaranteed by the storage modulus G' of PVA under specific conditions being within a predetermined range.

[0014] In the technical field, it is empirically known that the three-dimensional arrangement of the molecular chain of a polymer is reflected in the values ​​of the storage modulus G' and the loss modulus G''. The value obtained by dividing the loss modulus G'' by the storage modulus G', i.e., G'' / G', is called the loss tangent (tan δ). In general, for fluids with fluidity, G''>G'. In the case of linear PVA, when a double logarithmic plot is made, the slope is approximately 1 for G'' and 2 for G', so the difference becomes larger as the angular frequency becomes lower. In other words, the value of tan δ is large in the low frequency region. The present inventors have found that as the gel properties of PVA become stronger, the slopes of the double logarithmic plots of G'' and G' both approach approximately 1 in a wide frequency range including the low frequency region, i.e., tan δ does not become large. Such findings are described, for example, in the following literature. Literature: https: / / aip.scitation.org / doi / abs / 10.1063 / 1.1770590 The present inventors have discovered that by controlling the structure of PVA, it is possible to obtain a storage modulus G' that was not possible with conventional PVA, and have thus completed the present invention.

[0015] <Preparation of polyvinyl alcohol polymer> Examples of the vinyl ester monomers mentioned above include vinyl acetate, vinyl propionate, vinyl butyrate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl pivalate, etc., and mixtures of these may also be used. From the viewpoint of ease of polymerization, vinyl acetate is preferred.

[0016] Examples of monofunctional monomers copolymerizable with vinyl ester monomers (i.e., monofunctional monomers other than vinyl esters) include the following compounds: α-olefin monomers such as ethylene and propylene; (meth)acrylic acid alkyl ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; unsaturated amide monomers such as (meth)acrylamide and N-methylol acrylamide; unsaturated carboxylic acid monomers such as (meth)acrylic acid, crotonic acid, maleic acid, itaconic acid, and fumaric acid; alkyl (methyl, ethyl, propyl, and the like) ester monomers of unsaturated carboxylic acids; anhydrides of unsaturated carboxylic acids such as maleic anhydride; sodium, potassium, ammonium, and the like salts of unsaturated carboxylic acids; sulfonic acid group-containing monomers or salts thereof such as 2-acrylamido-2-methylpropanesulfonic acid; alkyl vinyl ether monomers.

[0017] As the polyfunctional monomer copolymerizable with the vinyl ester monomer, a compound having two or more polymerizable unsaturated bonds in the molecule can be used. Examples of such compounds include the following: Divinyl ethers and divinyl sulfonic acid compounds, such as ethanediol divinyl ether, propanediol divinyl ether, butanediol divinyl ether, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, and polypropylene glycol divinyl ether; Diene compounds, such as pentadiene, hexadiene, heptadiene, octadiene, nonadiene, and decadiene; Diallyl ether compounds, such as glycerin diallyl ether, diethylene glycol diallyl ether, ethylene glycol diallyl ether, triethylene glycol diallyl ether, polyethylene glycol diallyl ether, trimethylolpropane diallyl ether, and pentaerythritol diallyl ether; Triallyl ether compounds, such as glycerin triallyl ether, trimethylolpropane triallyl ether, and pentaerythritol triallyl ether. Tetraallyl ether compounds such as pentaerythritol tetraallyl ether. Polyfunctional monomers containing allyl ester groups such as diallyl phthalate, diallyl maleate, diallyl itaconate, diallyl terephthalate, and diallyl adipate. Polyfunctional monomers containing allylamino groups such as diallylamine, diallylmethylamine, and other diallylamine compounds, and triallylamine. Polyfunctional monomers containing allylammonium groups such as diallylammonium salts such as diallyldimethylammonium chloride. Polyfunctional monomers containing two or more allyl groups such as triallyl isocyanurate, 1,3-diallyl urea, triallyl phosphate, and diallyl disulfide.Polyfunctional monomers having (meth)acrylic acid such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, glycerin di(meth)acrylate, glycerin tri(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and isocyanuric acid tri(meth)acrylate. Polyfunctional monomers having (meth)acrylamide such as N,N'-methylenebis(meth)acrylamide and N,N'-ethylenebis(meth)acrylamide. Polyfunctional aromatic monomers such as divinylbenzene and trivinylbenzene. Glycidyl group-containing monomers such as allyl glycidyl ether and glycidyl (meth)acrylate.

[0018] From the viewpoint of reactivity with vinyl ester monomers and resistance to decomposition in saponification reaction, the monomer copolymerizable with vinyl ester monomer is preferably a compound that is not easily decomposed by alkali, and more preferably a compound having a carbonyl group or an amide group in the molecule. In a preferred embodiment, PVA is obtained by saponifying a copolymer of vinyl ester monomer and polyfunctional monomer, and a crosslinked structure is formed from the polyfunctional group, which has the effect of obtaining resistance to dissolution at high temperatures. As such a polyfunctional monomer, a compound having a ring structure is preferred, a compound having a heterocyclic structure is more preferred, and triallyl isocyanurate (TAIC) is particularly preferred.

[0019] When a vinyl ester monomer is copolymerized with a monomer other than vinyl ester, the copolymerization amount is preferably 0.001 to 1.0 mol %, more preferably 0.005 to 0.5 mol %, and even more preferably 0.01 to 0.2 mol %, of the structural units derived from the monomer other than vinyl ester relative to 100 mol % of the structural units derived from the vinyl alcohol unit in the vinyl alcohol polymer. By adjusting the copolymerization amount to this range, the dissolution resistance at high temperatures is improved and the vinyl alcohol polymer is not excessively crosslinked, which is also preferable from the viewpoint of production.

[0020] The copolymerization amount can be calculated using a total nitrogen trace analyzer. For example, when using a total nitrogen trace analyzer TN-2100H (manufactured by Nitto Seiko Analytech Co., Ltd.), the calculation can be performed according to the following procedure.

[0021] A sample of vinyl alcohol polymer is collected on a quartz board, which is set in an auto boat controller ABC-210 (manufactured by Nitto Seiko Analytech Co., Ltd.) and automatically inserted into an electric furnace, where it is burned in an argon / oxygen stream. The NO gas generated during this process is measured with a chemiluminescence detector. A calibration curve is created in advance using a standard solution (N-pyridine / toluene), and the nitrogen concentration is calculated from this calibration curve.

[0022] Example of measurement conditions Reaction tube: Double tube for ABC Electric furnace temperature Inlet Temp: 800℃, Outlet Temp: 900℃ Gas flow rate: Ar: 300 mL / min, O2: 300 mL / min, Ozone: 300 mL / min Sample size: approx. 9-15mg

[0023] Any method can be used for polymerizing the vinyl ester monomer or its copolymer, and for example, known polymerization methods such as solution polymerization, suspension polymerization, bulk polymerization, etc. From the viewpoints of ease of operation and the ability to use a solvent common to the subsequent saponification reaction, it is preferable to use a solution polymerization method in an alcohol, and it is particularly preferable to use methanol as the alcohol.

[0024] The polymer obtained as described above can be saponified by any method to prepare PVA. An example of the saponification method is a method in which an alkali catalyst is added to an alcohol solution of a polymer (such as polyvinyl ester). An example of the saponification procedure is described below.

[0025] Examples of the alcohol that can be used as a solvent for the polymer include methanol, ethanol, butanol, and preferably methanol. The concentration of the polymer in the alcohol solution can be set arbitrarily and may be, for example, 10% by mass or more and 80% by mass or less.

[0026] Next, an alkali catalyst is added to the solution to carry out a saponification reaction. Examples of the alkali catalyst include hydroxides and alcoholates of alkali metals such as sodium hydroxide, potassium hydroxide, sodium methylate, sodium ethylate, and potassium methylate. Among these, it is preferable to use sodium hydroxide. The amount of the alkali catalyst to be added is not particularly limited, but is preferably 1.0 to 100.0 millimolar equivalents relative to the polymer, and more preferably 5.0 to 30.0 millimolar equivalents. The reaction temperature during saponification is not particularly limited, but is preferably 10 to 70°C, and more preferably 30 to 55°C. The reaction time is also not particularly limited, and may be, for example, 20 minutes or more to 2 hours.

[0027] The degree of saponification can be appropriately adjusted depending on the application of the PVA, and may be, for example, 72 to 99 mol %. After the saponification reaction, a washing step for removing impurities such as sodium acetate and a drying step may be performed as necessary.

[0028] <Additives for oil well cement> In one embodiment, an additive for oil well cement containing the above-mentioned PVA can be provided, which is suitable for use in cementing oil wells, gas wells, steam wells for geothermal power generation, and the like.

[0029] Cementing, which is carried out when drilling a well, is the process of injecting cement into the gap between the drilled well and the steel pipe inserted into it. A widely used method of cementing is to mix cement with various additives, such as fluid loss additives, in a dry state, then turn the mixture into a slurry using high-pressure water and pump it in.

[0030] Using PVA as a fluid loss reducing agent reduces the loss of water content from the cement slurry during cementing (i.e. reduces fluid loss) and makes it possible to maintain the fluidity of the cement slurry. If the fluid loss is large, the fluidity of the cement slurry is lost and it becomes difficult to perform sufficient cementing.

[0031] Fluid loss evaluation is one of the evaluation items for oil well cement defined by the American Petroleum Institute (API). The fluid loss test method is described in Recommended Practice for Testing Well Cements, API Recommended Practice 10B-2, April 2013.

[0032] <Oil well cement composition> In one embodiment, an oil well cement composition containing an oil well cement and the additive for oil well cement can be provided. The oil well cement is not particularly limited as long as it is a cement used in cementing oil wells, gas wells, steam wells for geothermal power generation, etc.

[0033] Preferably, the content of the additive for oil well cement in the above composition is 0.01 to 10% bwoc, more preferably 0.05 to 5% bwoc. By setting the range in this way, the fluid loss can be effectively reduced. Note that "bwoc" (by weight of cement) means based on the weight of cement, and refers to the weight of the dry additive added to the cement composition based only on the solid content of the cement.

[0034] <Oil well cement slurry> In one embodiment, an oil well cement slurry containing oil well cement, the above additive for oil well cement, and water can also be provided. Preferably, the water content of the above cement slurry is 20 to 40% by mass.

[0035] The method of incorporating the additive for oil well cement into the cement slurry is not particularly limited. For example, there are a method of mixing the composition containing oil well cement and the additive with water after preparing the composition, a method of mixing oil well cement, the additive, and water without preparing the composition, and the like.

Examples

[0036] Hereinafter, the present invention will be described in more detail based on examples. Note that the examples described below show an example of a typical embodiment of the present invention, and the present invention is not limited to the following examples.

[0037] <Preparation of PVA> [Example 1] Into a polymerization kettle equipped with a reflux condenser, a dropping funnel, and a stirrer, 100 parts by mass of vinyl acetate, 67 parts by mass of methanol, 0.16 part by mass of triallyl isocyanurate (TAIC) as a polyfunctional monomer, and 5.0 x 10 -6 parts by mass of Peroyl NPP (manufactured by NOF Corporation) as an initiator were charged, and polymerization was carried out at a temperature below the boiling point for 5.0 hours while stirring under a nitrogen atmosphere. Next, the unreacted vinyl acetate monomer was removed outside the polymerization system to obtain a methanol solution of a polyvinyl acetate - TAIC copolymer.

[0038] A methanol solution of sodium hydroxide was added to the obtained vinyl acetate-TAIC copolymer solution (0.008 mol% of sodium hydroxide with respect to the copolymer). Then, a saponification reaction was carried out at 45 °C for 45 minutes to obtain PVA with a saponification degree of 88.2 mol%.

[0039] [Examples 2 - 3, Comparative Examples 1 - 3] Except that the charged amounts were changed as shown in Table 1 below, PVA of Examples 2 - 3 and Comparative Examples 1 - 3 was obtained by the same procedure as in Example 1.

[0040] [Measurement of Physical Properties of PVA] [Saponification Degree] It was measured and calculated in accordance with "3.5 Saponification Degree" of JIS K 6726:1994 of Japanese Industrial Standards.

[0041] [Measurement of Storage Elastic Modulus G', Loss Elastic Modulus G'', and Loss Tangent (tanδ)] The storage elastic modulus G', loss elastic modulus G'', and loss tangent (tanδ) were determined by the following method.

[0042] An aqueous PVA solution of 10 mass% or more was prepared, and the solution was filtered through a 100 - mesh (aperture 0.154 mm) filter. The concentration of the filtered aqueous solution was measured. When the concentration was 10 mass% or more, pure water was added to adjust the concentration to 10 mass%. The dynamic viscoelasticity of the adjusted solution was measured using a rheometer measuring device (Anton Paar MCR). A cone - plate CP50 - 2 (diameter: 50 mm, angle 2°) was used as the plate. The measurement conditions were: temperature 30 °C, shear strain (vibration) 1 → 5% (logarithmic slope), angular frequency 628.3 → 0.06 rad / s (linear slope), and the storage elastic modulus G' and loss elastic modulus G'' were obtained. The loss tangent (tanδ) was calculated by (loss elastic modulus G'' / storage elastic modulus G').

[0043] Double - logarithmic plots of the storage elastic modulus G' and loss elastic modulus G'' obtained as described above are shown in Figure 1 for Example 1 and Figure 2 for Comparative Example 1, respectively.

[0044] [Measurement of Fluid Loss] The fluid loss reduction effect of PVA was measured according to the fluid loss evaluation method of the American Petroleum Institute (API) standard 10B-2 (April 2013). The specific measurement procedure is shown below.

[0045] Class G oil well cement was blended with PVA and retarder (CR-270, Flotek Industries) 0.4bwoc in the amounts shown in Table 1, and mixed with water according to the procedure described in API Standard 10B-2 (April 2013) to obtain a cement slurry with a water content of 30% by mass. The resulting cement slurry was placed in a fluid loss evaluation tester (Model 7120, Chandler Engineering) and tested at the temperature shown in Table 1 under a pressure of 1000 psi according to the procedure described in API Standard 10B-2 (April 2013), and the fluid loss amount was calculated.

[0046] The evaluation was performed at temperatures ranging from 40°C to 140°C and with PVA amounts ranging from 0.4 to 1.2% bwoc, as shown in Table 1. In Table 1, "-" indicates that fluid loss measurements were not performed.

[0047] [Table 1]

[0048] From the results of the examples, it was confirmed that the additive for oil well cement of the present invention has good fluid loss reducing performance.

Claims

1. A polyvinyl alcohol-based polymer obtained by saponifying a copolymer of vinyl acetate and triallyl isocyanurate, the content of structural units derived from triallyl isocyanurate is 0.001 to 1.0 mol % relative to 100 mol % of structural units derived from vinyl alcohol units in the polyvinyl alcohol-based polymer; The storage modulus G' (20°C) in the angular frequency range of 1.0 to 10.0 rad / s measured in an aqueous solution adjusted to a concentration of 10.0% by mass after filtering an aqueous solution of a polyvinyl alcohol-based polymer through a 100 mesh (0.154 mm mesh) filter has a slope of 1.2 or less when the storage modulus G' (20°C) in the angular frequency range of 1.0 to 10.0 rad / s is plotted logarithmically. A polyvinyl alcohol polymer characterized by:

2. The polyvinyl alcohol-based polymer according to claim 1, wherein the value of angular frequency-dependent loss tangent (tan δ) measured in an aqueous solution adjusted to a concentration of 10.0% by mass after filtering the aqueous solution of the polyvinyl alcohol-based polymer through a 100 mesh (mesh size: 0.154 mm) filter is in the range of 1.0 to 10.0 in an angular frequency range of 0.1 to 100 rad / s.

3. The polyvinyl alcohol-based polymer according to claim 1 or 2, wherein the degree of saponification of the polyvinyl alcohol-based polymer is 72 to 99 mol%.

4. An additive for oil well cement comprising the polyvinyl alcohol polymer according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Hydrophilic nonionic rigid gel

    JP1980104301A

  • Polyvinyl alcohol-made medical hydrogel and manufacture therefor

    JP2000157625A

  • Additive for slurry, drilling mud, and cement slurry

    JP2015196733A

  • Fluid loss additive with improved rheological properties

    WO2007146348A2

  • Additive for oil well cement and cement slurry using said additive for oil well cement

    WO2019163490A1