Polyvinyl alcohol polymer

Polyvinyl alcohol polymers with controlled particle size and structure address the issue of fluid loss under high temperature and pressure, ensuring effective fluidity and cost-efficiency in cement slurries.

JP7561855B2Active Publication Date: 2024-10-04DENKA CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022540173
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-31
Filing Date
2021-07-15
Publication Date
2024-10-04
Estimated Expiration
2041-07-15

AI Technical Summary

Technical Problem

Conventional polyvinyl alcohol (PVA)-based fluid loss reducing agents fail to maintain effectiveness under severe high temperature and pressure conditions in cement slurries, leading to dissolution and reduced fluidity, necessitating increased agent use which thickens the slurry and increases costs.

Method used

Development of polyvinyl alcohol polymers with controlled particle size distribution and structure, including homopolymers and copolymers, resistant to high temperatures and pressures, achieved through specific particle size requirements and copolymerization with monofunctional and polyfunctional monomers.

Benefits of technology

The polymers exhibit excellent fluid loss reduction even under severe conditions, maintaining slurry fluidity and reducing costs by avoiding excessive agent use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561855000002
    Figure 0007561855000002
  • Figure 0007561855000003
    Figure 0007561855000003
  • Figure 0007561855000004
    Figure 0007561855000004
Patent Text Reader

Abstract

A poly(vinyl alcohol)-based polymer (PVA) having satisfactory unsusceptibility to high-temperature dissolution is provided. The PVA is obtained by saponifying any of a homopolymer obtained from a vinyl ester monomer, a copolymer of a vinyl ester monomer and a monofunctional monomer which is not a vinyl ester, a copolymer of a vinyl ester monomer and a polyfunctional monomer, and a copolymer of a vinyl ester monomer, a monofunctional monomer which is not a vinyl ester, and a polyfunctional monomer. A 0.4 mass% aqueous solution of the PVA, in a dynamic light scattering examination at a temperature of 25°C, gives a particle size distribution in which the particle diameter at 50% cumulative frequency is 50 nm or larger.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyvinyl alcohol polymer and uses thereof. [Background technology]

[0002] Polymers having a polyvinyl alcohol (PVA) skeleton (hereinafter, in this specification, these are collectively referred to as "polyvinyl alcohol-based polymers," "vinyl alcohol-based polymers," or simply "PVA") are known as hydrophilic synthetic resins, and various applications that take advantage of their properties are being developed.

[0003] One such use is as an additive to oil well cement, which is used in cementing oil wells, gas wells, and steam wells for geothermal power generation. Oil well cement is mixed with water and other additives, and filled into the gap between the steel pipe (casing) and the well to fix and protect it. For this reason, it is preferable for the cement slurry to have high fluidity so that it is easy to fill. The loss of water content from the cement slurry due to high pressure during injection and underground heat is generally called "fluid loss." Fluid loss reduces the fluidity of the cement slurry, causing poor cementing and poor hardening after hardening. For this reason, fluid loss reducing agents are usually added to the cement slurry.

[0004] It has been proposed to use polyvinyl alcohol polymers as the main component of such fluid loss reducing agents. For example, Patent Documents 1 and 2 describe PVA used in fluid loss reducing agents. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2007 / 146348 [Patent Document 2] JP 2015-196733 A Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, the pressure and temperature conditions have become more severe, especially for shale gas wells, as they have been extracted deeper. However, conventional PVA-containing fluid loss reducing agents have not yet achieved the fluid loss reduction performance required for cement slurries injected under such severe conditions of high temperature and pressure. Specifically, PVA-based fluid loss reducing agents dissolve at high temperatures, and dissolve into the well under high pressure conditions, resulting in a decrease in the fluid loss reduction effect. Therefore, PVA-based fluid loss reducing agents are required to be resistant to dissolution at high temperatures. At present, this is addressed by increasing the amount of conventional fluid loss reducing agents added, but the problem of reduced fluidity and increased costs due to the increased viscosity of the cement slurry has not been solved. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention provides the following.

[0008] A polyvinyl alcohol-based polymer obtained by saponification of a homopolymer made of a vinyl ester monomer, a copolymer of a vinyl ester monomer and a monofunctional monomer other than a vinyl ester, a copolymer of a vinyl ester monomer and a polyfunctional monomer, or a copolymer of a vinyl ester monomer, a monofunctional monomer other than a vinyl ester, and a polyfunctional monomer, The particle size distribution of a 0.4% by mass aqueous solution of a polyvinyl alcohol polymer, as measured by dynamic light scattering at 25°C, has a cumulative particle size of 50% or more. A polyvinyl alcohol polymer characterized by:

[0009] In one embodiment, the average particle size (median size) determined by the dynamic light scattering measurement is preferably 60 nm or more. In another embodiment, the passing rate of a 1.0% by mass aqueous solution of the vinyl alcohol-based polymer through a 300 mesh (0.045 mm mesh size) filter is preferably 95% by mass or more in terms of solid content. In another embodiment, the passing rate of a 1.0% by mass aqueous solution of the vinyl alcohol-based polymer through a membrane filter with a pore size of 0.45 μm is preferably 10% by mass or less in terms of solid content. In another embodiment, the average degree of polymerization of the vinyl alcohol-based polymer measured by the method described in JIS K 6726:1994 is preferably 2500 to 6000. In another embodiment, an additive for oil well cement containing a polyvinyl alcohol-based polymer can also be provided. Effect of the Invention

[0010] The polyvinyl alcohol polymer according to the present invention exhibits an excellent fluid loss reducing effect even under severe high temperature or high pressure environments. [Brief description of the drawings]

[0011] [Figure 1] 3 shows the particle size distribution of the polyvinyl alcohol polymer of Example 2, determined by dynamic light scattering measurement. [Diagram 2] 3 shows the particle size distribution of the polyvinyl alcohol polymer of Example 3, determined by dynamic light scattering measurement. [Diagram 3] 1 shows the particle size distribution of the polyvinyl alcohol polymer according to Comparative Example 3, determined by dynamic light scattering measurement. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the mode for carrying out the present invention will be described. Note that the embodiment described below shows an example of the embodiment of the present invention, and the scope of the present invention is not to be interpreted narrowly by this. Numerical ranges in this specification include the upper and lower limits unless otherwise specified. The polymer in this specification follows the definition of polymer by the International Union of Pure and Applied Chemistry (IUPAC) Commission on Macromolecular Nomenclature, that is, "a polymer molecule is a molecule having a large relative molecular mass and a structure composed of a large number of repetitions of units that are substantially or conceptually derived from molecules having a small relative molecular mass."

[0013] <Chemical structure of polyvinyl alcohol polymer> The polyvinyl alcohol-based polymer according to the present invention is a polymer obtained by saponifying a homopolymer made of a vinyl ester monomer, a copolymer of a vinyl ester monomer and a monofunctional monomer other than a vinyl ester, a copolymer of a vinyl ester monomer and a polyfunctional monomer, or a copolymer of a vinyl ester monomer, a monofunctional monomer other than a vinyl ester, and a polyfunctional monomer. The polyvinyl alcohol-based polymer according to the present invention has a polymer structure that can withstand high temperatures and pressures that cannot be used with conventional PVA. The presence of such a polymer structure can be judged from the particle size distribution of the polymer particles in the dilute aqueous solution, and more specifically, is guaranteed by the particle size at a cumulative frequency of 50% obtained from the particle size distribution of PVA particles under specific conditions being within a specified range.

[0014] The present inventors have discovered that by controlling the structure of PVA, a particle size distribution that could not be obtained with conventional PVA can be obtained, and have completed the present invention.

[0015] <Preparation of polyvinyl alcohol polymer> Examples of the vinyl ester monomers mentioned above include vinyl acetate, vinyl propionate, vinyl butyrate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl pivalate, etc., and mixtures of these may also be used. From the viewpoint of ease of polymerization, vinyl acetate is preferred.

[0016] Examples of monofunctional monomers copolymerizable with vinyl ester monomers (i.e., monofunctional monomers other than vinyl esters) include the following compounds: α-olefin monomers such as ethylene and propylene; (meth)acrylic acid alkyl ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; unsaturated amide monomers such as (meth)acrylamide and N-methylol acrylamide; unsaturated carboxylic acid monomers such as (meth)acrylic acid, crotonic acid, maleic acid, itaconic acid, and fumaric acid; alkyl (methyl, ethyl, propyl, and the like) ester monomers of unsaturated carboxylic acids; anhydrides of unsaturated carboxylic acids such as maleic anhydride; sodium, potassium, ammonium, and the like salts of unsaturated carboxylic acids; sulfonic acid group-containing monomers or salts thereof such as 2-acrylamido-2-methylpropanesulfonic acid; alkyl vinyl ether monomers.

[0017] As the polyfunctional monomer copolymerizable with the vinyl ester monomer, a compound having two or more polymerizable unsaturated bonds in the molecule can be used. Examples of such compounds include the following: Divinyl ethers and divinyl sulfonic acid compounds, such as ethanediol divinyl ether, propanediol divinyl ether, butanediol divinyl ether, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, and polypropylene glycol divinyl ether; Diene compounds, such as pentadiene, hexadiene, heptadiene, octadiene, nonadiene, and decadiene; Diallyl ether compounds, such as glycerin diallyl ether, diethylene glycol diallyl ether, ethylene glycol diallyl ether, triethylene glycol diallyl ether, polyethylene glycol diallyl ether, trimethylolpropane diallyl ether, and pentaerythritol diallyl ether; Triallyl ether compounds, such as glycerin triallyl ether, trimethylolpropane triallyl ether, and pentaerythritol triallyl ether. Tetraallyl ether compounds such as pentaerythritol tetraallyl ether. Polyfunctional monomers containing allyl ester groups such as diallyl phthalate, diallyl maleate, diallyl itaconate, diallyl terephthalate, and diallyl adipate. Polyfunctional monomers containing allylamino groups such as diallylamine, diallylmethylamine, and other diallylamine compounds, and triallylamine. Polyfunctional monomers containing allylammonium groups such as diallylammonium salts such as diallyldimethylammonium chloride. Polyfunctional monomers containing two or more allyl groups such as triallyl isocyanurate, 1,3-diallyl urea, triallyl phosphate, and diallyl disulfide.Polyfunctional monomers having (meth)acrylic acid such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, glycerin di(meth)acrylate, glycerin tri(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and isocyanuric acid tri(meth)acrylate. Polyfunctional monomers having (meth)acrylamide such as N,N'-methylenebis(meth)acrylamide and N,N'-ethylenebis(meth)acrylamide. Polyfunctional aromatic monomers such as divinylbenzene and trivinylbenzene. Glycidyl group-containing polyfunctional monomers such as allyl glycidyl ether and glycidyl (meth)acrylate.

[0018] From the viewpoint of reactivity with vinyl ester monomers and resistance to decomposition in saponification reaction, the monomer copolymerizable with vinyl ester monomer is preferably a compound that is not easily decomposed by alkali, and more preferably a compound having a carbonyl group or an amide group in the molecule. In a preferred embodiment, PVA is obtained by saponifying a copolymer of vinyl ester monomer and polyfunctional monomer, and a crosslinked structure is formed from the polyfunctional group, which has the effect of obtaining resistance to dissolution at high temperatures. As such a polyfunctional monomer, a compound having a ring structure is preferred, a compound having a heterocyclic structure is more preferred, and triallyl isocyanurate (TAIC) is particularly preferred.

[0019] When a vinyl ester monomer is copolymerized with a monomer other than vinyl ester, the copolymerization amount is preferably 0.001 to 1.0 mol %, more preferably 0.005 to 0.5 mol %, and even more preferably 0.01 to 0.2 mol %, of the structural units derived from the monomer other than vinyl ester relative to 100 mol % of the structural units derived from the vinyl alcohol unit in the vinyl alcohol polymer. By adjusting the copolymerization amount to this range, the dissolution resistance at high temperatures is improved and the vinyl alcohol polymer is not excessively crosslinked, which is also preferable from the viewpoint of production.

[0020] The copolymerization amount can be calculated using a total nitrogen trace analyzer. For example, when using a total nitrogen trace analyzer TN-2100H (manufactured by Nitto Seiko Analytech Co., Ltd.), the calculation can be performed according to the following procedure.

[0021] A sample of vinyl alcohol polymer is collected on a quartz board, which is set in an auto boat controller ABC-210 (manufactured by Nitto Seiko Analytech Co., Ltd.) and automatically inserted into an electric furnace, where it is burned in an argon / oxygen stream. The NO gas generated during this process is measured with a chemiluminescence detector. A calibration curve is created in advance using a standard solution (N-pyridine / toluene), and the nitrogen concentration is calculated from this calibration curve.

[0022] Example of measurement conditions Reaction tube: Double tube for ABC Electric furnace temperature Inlet Temp: 800℃, Outlet Temp: 900℃ Gas flow rate: Ar: 300 mL / min, O2: 300 mL / min, Ozone: 300 mL / min Sample size: approx. 9-15mg

[0023] Any method can be used for polymerizing the vinyl ester monomer or its copolymer, and for example, known polymerization methods such as solution polymerization, suspension polymerization, bulk polymerization, etc. From the viewpoints of ease of operation and the ability to use a solvent common to the subsequent saponification reaction, it is preferable to use a solution polymerization method in an alcohol, and it is particularly preferable to use methanol as the alcohol.

[0024] The polymer obtained as described above can be saponified by any method to prepare PVA. An example of the saponification method is a method in which an alkali catalyst is added to an alcohol solution of a polymer (such as polyvinyl ester). An example of the saponification procedure is described below.

[0025] Examples of the alcohol that can be used as a solvent for the polymer include methanol, ethanol, butanol, and preferably methanol. The concentration of the polymer in the alcohol solution can be set arbitrarily and may be, for example, 10% by mass or more and 80% by mass or less.

[0026] Next, an alkali catalyst is added to the solution to carry out a saponification reaction. Examples of the alkali catalyst include hydroxides and alcoholates of alkali metals such as sodium hydroxide, potassium hydroxide, sodium methylate, sodium ethylate, and potassium methylate. Among these, it is preferable to use sodium hydroxide. The amount of the alkali catalyst to be added is not particularly limited, but is preferably 1.0 to 100.0 millimolar equivalents relative to the polymer, and more preferably 5.0 to 30.0 millimolar equivalents. The reaction temperature during saponification is not particularly limited, but is preferably 10 to 70°C, and more preferably 30 to 55°C. The reaction time is also not particularly limited, and may be, for example, 20 minutes or more to 2 hours.

[0027] The degree of saponification can be appropriately adjusted depending on the application of the PVA, and may be, for example, 72 to 99 mol %. After the saponification reaction, a washing step for removing impurities such as sodium acetate and a drying step may be performed as necessary.

[0028] <Physical properties of polyvinyl alcohol polymer> The particle size distribution of the PVA particles in the dilute aqueous solution obtained by the above-mentioned production method can be quantified by subjecting a 0.4 mass% aqueous solution of PVA to dynamic light scattering measurement at a temperature of 25°C. In the present invention, the particle size of the PVA particles at a cumulative frequency of 50% in the particle size distribution must be 50 nm or more, and is more preferably in the range of 70 to 1000 nm. The cumulative frequency is determined from the scattering intensity distribution frequency obtained by dynamic light scattering measurement.

[0029] The average particle size of PVA in the dilute aqueous solution can be set according to the application, and is preferably, for example, 60 to 2000 nm, more preferably 70 to 1500 nm. In this specification, the average particle size of PVA in the dilute aqueous solution is determined by cumulant analysis of the particle size distribution obtained by performing dynamic light scattering measurement on a 0.4 mass% aqueous solution of PVA at a temperature of 25°C.

[0030] When used as an additive for oil well cement, if the average particle size of PVA in a dilute solution is 60 nm or more, the PVA in the cement slurry is less likely to flow out, improving the fluid loss reduction performance. If the average particle size of PVA in a dilute solution is 2000 nm or more, it is not preferable from the viewpoint of productivity.

[0031] From the viewpoint of the strength of the cement after hardening and the manufacturing process of PVA, it is preferable that the PVA particles do not contain excessively large gel particles. More specifically, the passing rate of a 1.0 mass% aqueous solution of PVA through a 300 mesh (opening: 0.045 mm) filter is preferably 95 mass% or more, and more preferably in the range of 97 to 100 mass%, calculated as solid content.

[0032] Here, the 300 mesh filter passing rate can be calculated by the following procedure. The dried PVA is dissolved in water at 25°C to obtain an aqueous solution with a concentration of 1.0 mass%. 100 mL of the resulting PVA aqueous solution is filtered through a 300 mesh filter (openings 0.045 mm). The mass of PVA remaining on the filter is measured. The percentage of PVA that has passed through the filter is calculated from the measured mass of the PVA residue.

[0033] From the viewpoint of dissolution resistance, the PVA particles preferably have a particle size distribution that makes it difficult for them to pass through a membrane filter having a pore size of 0.45 μm. More specifically, the passing rate of a 1.0 mass % aqueous solution of PVA through a membrane filter having a pore size of 0.45 μm is preferably 10 mass % or less, and more preferably in the range of 0 to 5 mass %, calculated as solid content.

[0034] Here, the passing rate of a 0.45 μm membrane filter can be calculated by the following procedure. An aqueous PVA solution adjusted to a concentration of 1.0% by mass is filtered under reduced pressure (10 mmHg) for 10 minutes using a 0.45 μm filter (manufactured by ADVANTEC, Material: Mixed Cellulose ester, pore size: 0.45 μm, diameter: 47 mm). The passing rate is calculated from the amount of solids in the filtrate.

[0035] The average degree of polymerization of PVA can be measured by the method described in JIS K6726: 1994. From the viewpoint of productivity, the average degree of polymerization is preferably in the range of 2,500 to 6,000, and more preferably in the range of 2,800 to 5,000.

[0036] <Additives for oil well cement> In one embodiment, an additive for oil well cement containing the above-mentioned PVA can be provided, which is suitable for use in cementing oil wells, gas wells, steam wells for geothermal power generation, and the like.

[0037] Cementing, which is carried out when drilling a well, is the process of injecting cement into the gap between the drilled well and the steel pipe inserted into it. A widely used method of cementing is to mix cement with various additives, such as fluid loss additives, in a dry state, then turn the mixture into a slurry using high-pressure water and pump it in.

[0038] Using PVA as a fluid loss reducing agent reduces the loss of water content from the cement slurry during cementing (i.e. reduces fluid loss) and makes it possible to maintain the fluidity of the cement slurry. If the fluid loss is large, the fluidity of the cement slurry is lost and it becomes difficult to perform sufficient cementing.

[0039] Fluid loss evaluation is one of the evaluation items for oil well cement defined by the American Petroleum Institute (API). The fluid loss test method is described in Recommended Practice for Testing Well Cements, API Recommended Practice 10B-2, April 2013.

[0040] <Oil well cement composition> In one embodiment, an oil well cement composition containing an oil well cement and the additive for oil well cement can be provided. The oil well cement is not particularly limited as long as it is a cement used in cementing oil wells, gas wells, steam wells for geothermal power generation, etc.

[0041] The content of the oil well cement additive in the above composition is preferably 0.01-10% bwoc, more preferably 0.05-5% bwoc. By setting the content in this range, fluid loss can be effectively reduced. Note that "bwoc" (by weight of cement) means based on the weight of cement, and refers to the weight of the additive in a dry state added to the cement composition based only on the solid content of cement.

[0042] <Oil well cement slurry> In one embodiment, there is also provided an oil well cement slurry containing an oil well cement, the oil well cement additive, and water. The cement slurry preferably has a water content of 20 to 40 mass %.

[0043] The method of incorporating an additive for oil well cement into the cement slurry is not particularly limited. For example, there are methods such as mixing the composition containing the oil well cement and the additive with water after preparing the composition, and methods of mixing the oil well cement, the additive, and water without preparing the composition.

Examples

[0044] Hereinafter, the present invention will be described in more detail based on examples. It should be noted that the examples described below show an example of a typical embodiment of the present invention, and the present invention is not limited to the following examples.

[0045] <Preparation of PVA> [Example 1] Into a polymerization kettle equipped with a reflux condenser, a dropping funnel, and a stirrer, 100 parts by mass of vinyl acetate, 43 parts by mass of methanol, 0.090 parts by mass of triallyl isocyanurate (TAIC) as a polyfunctional monomer, and 5.0×10 -6 parts by mass of Peroyl NPP (manufactured by NOF Corporation) as an initiator were charged, and polymerization was carried out at a temperature below the boiling point for 5.0 hours while stirring under a nitrogen atmosphere. Next, the unreacted vinyl acetate monomer was removed outside the polymerization system to obtain a methanol solution of a polyvinyl acetate-TAIC copolymer.

[0046] A methanol solution of sodium hydroxide was added to the obtained methanol solution of the vinyl acetate-TAIC copolymer (0.008 mol% of sodium hydroxide with respect to the copolymer). Then, a saponification reaction was carried out at 45°C for 45 minutes to obtain PVA with a saponification degree of 88.1 mol%.

[0047] [Examples 2 to 5, Comparative Examples 1 to 5] PVAs of Examples 2 to 5 and Comparative Examples 1 to 5 were obtained in the same procedure as in Example 1 except that the charged amounts were changed as shown in Table 1 below.

[0048] <Measurement of Physical Properties of PVA> [Saponification Degree] It was measured and calculated in accordance with JIS K 6726:1994 "3.5 Saponification Degree" of Japanese Industrial Standards.

[0049] [Average degree of polymerization] The average degree of polymerization was measured and calculated in accordance with JIS K 6726:1994 "3.7 Average degree of polymerization". However, before injecting the approximately 1% by mass PVA aqueous solution prepared for measuring the average degree of polymerization into the Ostwald meter, it was filtered through a 300 mesh (0.045 mm mesh) filter. The concentration of PVA used to calculate the average degree of polymerization was the concentration value after filtration.

[0050] [Copolymerization amount] The copolymerization amount was calculated using a total nitrogen trace analyzer TN-2100H (manufactured by Nitto Seiko Analytech Co., Ltd.) according to the following procedure. The PVA obtained above was collected on a quartz board, which was set in an auto boat controller ABC-210 (manufactured by Nitto Seiko Analytech Co., Ltd.) and automatically inserted into an electric furnace, where it was burned in an argon / oxygen stream. The NO gas generated during this process was measured with a chemiluminescence detector. A calibration curve was created in advance using a standard solution (N-pyridine / toluene), and the nitrogen concentration was calculated from the calibration curve. Measurement conditions Reaction tube: Double tube for ABC Electric furnace temperature Inlet Temp: 800℃, Outlet Temp: 900℃ Gas flow rate: Ar: 300 mL / min, O2: 300 mL / min, Ozone: 300 mL / min Sample size: approx. 9-15mg

[0051] [Cumulative frequency 50% diameter and average particle diameter] The particle size of PVA at 50% cumulative frequency was measured by dynamic light scattering measurement as follows. A 0.4% by mass PVA aqueous solution was prepared and filtered through a 300 mesh (0.045 mm mesh size) filter, after which the filtrate was placed in a quartz cell and measured with a dynamic light scattering measurement device (Otsuka Electronics Co., Ltd., ELS-Z2). The measurement conditions were 25°C, solvent: water, solvent refractive index: 1.33, solvent viscosity: 0.89 (cP), and the particle size value at 50% cumulative frequency was obtained from the obtained scattering intensity distribution frequency. In addition, from this measurement result, the average particle size of PVA was obtained by cumulant method analysis. Graphs of the scattering intensity distribution and cumulative frequency distribution of Example 2, Example 3, and Comparative Example 3 are shown in Figures 1 to 3, respectively.

[0052] [300mesh passage rate] The PVA obtained above was dissolved in water at 25°C to obtain an aqueous solution with a concentration of 1.0 mass%. 100 mL of the obtained aqueous solution of PVA was filtered through a 300 mesh (0.045 mm opening) filter, and the mass of PVA remaining on the filter was measured. The proportion of PVA that passed through the filter was calculated from the measured mass of the PVA residue.

[0053] [0.45μm membrane filter penetration rate] The aqueous solution of PVA obtained above was adjusted to a concentration of 1.0% by mass and filtered under reduced pressure (10 mmHg) for 10 minutes using a 0.45 μm filter (manufactured by ADVANTEC, Material: Mixed Cellulose ester, pore size: 0.45 μm, diameter: 47 mm). The passing rate was calculated from the amount of solids in the filtrate.

[0054] [Fluid loss measurement] The fluid loss reduction effect of PVA was measured according to the fluid loss evaluation method of the American Petroleum Institute (API) standard 10B-2 (April 2013). The specific measurement procedure is shown below.

[0055] Class G oil well cement was blended with PVA and retarder (CR-270, Flotek Industries) 0.4bwoc in the amounts shown in Table 1, and mixed with water according to the procedure described in API Standard 10B-2 (April 2013) to obtain a cement slurry with a water content of 30% by mass. The resulting cement slurry was placed in a fluid loss evaluation tester (Model 7120, Chandler Engineering) and tested at the temperature shown in Table 1 under a pressure of 1000 psi according to the procedure described in API Standard 10B-2 (April 2013), and the fluid loss amount was calculated.

[0056] The evaluation was performed at temperatures ranging from 40°C to 140°C and with PVA amounts ranging from 0.4 to 1.2% bwoc, as shown in Table 1. In Table 1, "-" indicates that fluid loss measurements were not performed.

[0057] [Table 1]

[0058] From the results of the examples, it was confirmed that the additive for oil well cement of the present invention has good fluid loss reducing performance.

Claims

1. A polyvinyl alcohol-based polymer obtained by saponification of a copolymer of a vinyl ester monomer and triallyl isocyanurate, a particle size at a cumulative frequency of 50% in a particle size distribution measured by dynamic light scattering at a temperature of 25° C. of a 0.4% by mass aqueous solution of the polyvinyl alcohol-based polymer is 50 nm or more; The passing rate of a 1.0% by mass aqueous solution of the polyvinyl alcohol-based polymer through a membrane filter having a pore size of 0.45 μm is 10% by mass or less in terms of solid content. A polyvinyl alcohol polymer characterized by:

2. The polyvinyl alcohol-based polymer according to claim 1, wherein a mean particle size of a particle size distribution of a 0.4% by mass aqueous solution of the polyvinyl alcohol-based polymer as measured by dynamic light scattering at a temperature of 25°C is 60 nm or more.

3. The polyvinyl alcohol-based polymer according to claim 1 or 2, wherein a 1.0% by mass aqueous solution of the polyvinyl alcohol-based polymer has a passing rate through a 300 mesh filter (mesh opening: 0.045 mm) of 95% by mass or more in terms of solid content.

4. The polyvinyl alcohol-based polymer according to any one of claims 1 to 3, wherein a passing rate of a 1.0 mass% aqueous solution of the polyvinyl alcohol-based polymer through a membrane filter having a pore size of 0.45 µm is in the range of 0 to 5 mass% in terms of solid content.

5. The polyvinyl alcohol-based polymer according to any one of claims 1 to 4, wherein the polyvinyl alcohol-based polymer has an average degree of polymerization of 2500 to 6000 as measured by the method described in JIS K 6726:1994.

6. An additive for oil well cement comprising the polyvinyl alcohol polymer according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Hydrophilic nonionic rigid gel

    JP1980104301A

  • Crosslinked polymer particle and method for producing the same

    JP2006206895A

  • Crosslinked polymer particle and process for producing the same

    JP2008069346A

  • Method for producing polyvinyl alcohol / water mixed liquid

    JP2011173944A

  • Additive for slurry, drilling mud, and cement slurry

    JP2015196733A