Release film and method for producing same
The release film with alternating inorganic and organic layers addresses the peeling challenge of ultra-thin copper foils at high temperatures, ensuring effective peeling and metal recovery for 5G electronic products.
Patent Information
- Application Number
- JP2023032320
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-12-30
- Filing Date
- 2023-03-02
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-02
AI Technical Summary
Ultra-thin copper foils used in electronic products for 5G support are difficult to peel off at high temperatures, affecting performance.
A release film comprising alternating inorganic and organic layers, with inorganic layers made of nickel, cobalt, tungsten, or molybdenum alloys, and organic layers containing nitrogen-containing heterocyclic compounds, providing a favorable release effect at both room temperature and high temperatures.
The release film enables easy peeling of copper foils at both room temperature and high temperatures, enhancing the performance of electronic products and allowing metal recovery through electrochemical means.
Smart Images

Figure 0007561903000001 
Figure 0007561903000002 
Figure 0007561903000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a release film, and more particularly to a release film and a method for producing the same. [Background technology]
[0002] With the development of 5th generation mobile networks (5G), the demand for compatible electronic products is also increasing. However, the ultra-thin copper foil currently used for circuit boards in the above electronic products cannot be easily peeled off at high temperatures, which affects the performance of the electronic products. Summary of the Invention [Problem to be solved by the invention]
[0003] The present invention provides a release film having a favorable release effect and a method for producing the same. [Means for solving the problem]
[0004] A release film according to the present invention includes at least one inorganic layer and at least one organic layer, and the material of the inorganic layer includes nickel, cobalt, tungsten, molybdenum, or an alloy thereof.
[0005] In one embodiment of the present invention, the inorganic and organic layers are stacked alternately.
[0006] In one embodiment of the present invention, the material of the organic layer comprises a nitrogen-containing heterocyclic compound or a derivative thereof.
[0007] In one embodiment of the present invention, the material of the organic layer comprises benzotriazole (1,2,3-benzotriazole, BTA) or a derivative thereof.
[0008] In one embodiment of the present invention, the inorganic layer has a thickness of 10 nanometers to 100 nanometers.
[0009] In one embodiment of the present invention, the release film has a thickness of 80 nanometers to 150 nanometers.
[0010] In one embodiment of the present invention, the release film has a release force of 0 grams per centimeter (g / cm) to 20 grams per centimeter at room temperature and a release force of 0 grams per centimeter to 50 grams per centimeter at a temperature of 390°C.
[0011] The method for producing a release film of the present invention includes forming at least one inorganic layer on a substrate, and forming at least one organic layer on the inorganic layer to form a release film having an inorganic layer and an organic layer. The material of the inorganic layer includes nickel, cobalt, tungsten, molybdenum, or an alloy thereof.
[0012] In one embodiment of the present invention, the inorganic layer is formed by a sputtering method or an electroplating method.
[0013] In one embodiment of the present invention, the organic layer is formed by an impregnation method. Effect of the Invention
[0014] As described above, the release film of the present invention and the release film produced by the production method thereof comprise at least one inorganic layer and at least one organic layer, and the material of the inorganic layer comprises nickel, cobalt, tungsten, molybdenum or alloy thereof, so that the release film has a good release effect, and the metal in the inorganic layer of the release film can be further recovered by electrochemical technology.
[0015] In order to make the above features and advantages of the present invention more easily understandable, the present invention will be described in detail below with reference to the embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, the embodiments of the present invention will be described in detail. The implementation details provided in the embodiments are only for illustrative purposes and are not intended to limit the scope of the present invention. Those skilled in the art can modify or change these implementation details according to the needs of actual implementation.
[0017] <Release film> The present invention provides a release film comprising at least one inorganic layer and at least one organic layer. The release film preferably comprises at least two inorganic layers and at least two organic layers. The lamination method of the inorganic layer and the organic layer is not particularly limited, and a suitable lamination method can be selected as necessary. In this embodiment, the lamination method of the inorganic layer and the organic layer is preferably alternately laminated with each other.
[0018] The material of the inorganic layer includes nickel, cobalt, tungsten, molybdenum or alloys thereof. For example, the material of the inorganic layer may include nickel-molybdenum-tungsten alloy (Ni / Mo / W), nickel-cobalt-tungsten alloy (Ni / Co / W), nickel-tungsten-cobalt-molybdenum alloy (Ni / W / Co / Mo) or other suitable alloys, with nickel-cobalt-tungsten alloy (Ni / Co / W) or nickel-tungsten-cobalt-molybdenum alloy (Ni / W / Co / Mo) being preferred. The nickel-molybdenum-tungsten alloy (Ni / Mo / W) may include 5% to 75% by weight of nickel, 5% to 35% by weight of molybdenum, 5% to 35% by weight of tungsten and inevitable impurities. Nickel-cobalt-tungsten alloy (Ni / Co / W) may contain 5% to 75% by weight of nickel, 5% to 35% by weight of cobalt, 5% to 35% by weight of tungsten, and unavoidable impurities. Nickel-tungsten-cobalt-molybdenum alloy (Ni / W / Co / Mo) may contain 5% to 75% by weight of nickel, 5% to 35% by weight of tungsten, 5% to 35% by weight of cobalt, 5% to 35% by weight of molybdenum, and unavoidable impurities. When the material of the inorganic layer contains tungsten, molybdenum, or a combination thereof, the release film has a favorable release effect at both room temperature and high temperature (e.g., about 400°C). When the material of the inorganic layer contains nickel, cobalt, or a combination thereof, the inorganic layer has a favorable uniformity, and thus the release film has a favorable release effect. When the release film has at least two inorganic layers, the materials of each inorganic layer may be the same or different. For example, when the release film has two inorganic layers, the material of the inorganic layer formed first (i.e., the first inorganic layer formed directly on the substrate) may be a nickel-molybdenum-tungsten alloy (Ni / Mo / W), and the material of the inorganic layer formed later may be a nickel-cobalt-tungsten alloy (Ni / Co / W).
[0019] The material of the organic layer is not particularly limited, and a suitable material can be selected as necessary. In this embodiment, the material of the organic layer may include a nitrogen-containing heterocyclic compound, a derivative thereof, or other suitable material. The nitrogen-containing heterocyclic compound may include benzotriazole, a derivative thereof, or other suitable nitrogen-containing heterocyclic compound. For example, the nitrogen-containing heterocyclic compound may include benzotriazole, methylbenzotriazole (5-methyl-1H-benzotriazole, 5M-BTA), a compound represented by the following chemical formula 1 (CBT-1), 5-carboxybenzotriazole (benzotriazole-5-carboxylic acid, CBT-5), 2-carboxybenzotriazole (CBTA), or 1-[(1',2'-dicarbonyl)ethyl]benzotriazole (BT-M), with benzotriazole or 2-carboxybenzotriazole being preferred, and 2-carboxybenzotriazole being more preferred. By providing the release film with an organic layer, the uniformity of the inorganic layer that is in direct contact with the organic layer can be improved. For example, when the release film has two organic layers, the material of the first organic layer formed (i.e., the first organic layer formed on the first inorganic layer) may be benzotriazole, and the material of the second organic layer may be 2-carboxybenzotriazole. [ka]
[0020] The thickness of the inorganic layer and the organic layer are not particularly limited, and a suitable thickness can be selected as required. In this embodiment, the thickness of the inorganic layer is 10 nanometers to 100 nanometers, and preferably 30 nanometers to 50 nanometers. When the thickness of the inorganic layer is within the above range, the release film has a good release effect. The thickness of the release film is not particularly limited, and a suitable thickness can be selected as required. In this embodiment, the thickness of the release film is 80 nanometers to 150 nanometers, and preferably 90 nanometers to 130 nanometers. When the thickness of the release film is within the above range, the release film has a good release effect.
[0021] In this embodiment, the release film has a peel strength of 0 to 20 grams / centimeter at room temperature, preferably 7 to 12 grams / centimeter, and a peel strength of 0 to 50 grams / centimeter at a temperature of 390° C., preferably 7 to 12 grams / centimeter.
[0022] <Method of producing release film> The present invention also provides a method for producing a release film, comprising forming at least one inorganic layer on a substrate, and forming at least one organic layer on the inorganic layer to form a release film having an inorganic layer and an organic layer, thereby forming a release film having the preferred release effect, and further recovering metals in the inorganic layer of the release film through electrochemical technology.
[0023] The method of forming the inorganic layer is not particularly limited, and a suitable method can be selected as necessary. In this embodiment, the inorganic layer can be formed by a sputtering method, an electroplating method, or other suitable method. When the release film has at least two inorganic layers, the methods of forming each inorganic layer can be the same or different. For example, when the release film has two inorganic layers, the inorganic layer formed first (i.e., the first inorganic layer formed directly on the substrate) can be formed by a sputtering method, and the inorganic layer formed later can be formed by an electroplating method.
[0024] The method of forming the organic layer is not particularly limited, and a suitable method can be selected as necessary. In this embodiment, the organic layer can be formed by impregnation method or other suitable method. When the release film has at least two organic layers, the method of forming each organic layer can be the same or different.
[0025] The substrate is not particularly limited, and can select a suitable substrate as required.For example, the substrate can include copper foil, aluminum foil, plastic film or other suitable substrate.The thickness of the substrate can be 18 micrometers to 100 micrometers, and preferably 18 micrometers to 50 micrometers.
[0026] For example, the method for producing a release film may include the following: A material of an inorganic layer is plated on a substrate by a sputtering method to form a first inorganic layer; Then, a material of an organic layer is plated on the first inorganic layer by an impregnation method to form a first organic layer; By forming the first organic layer, the uniformity of the first inorganic layer can be improved; Then, a material of an inorganic layer can be further plated on the first organic layer by an electroplating method to form a second inorganic layer; Then, a material of an organic layer is plated on the second inorganic layer by an impregnation method to form a second organic layer.
[0027] The present invention will now be described in detail with reference to examples. The examples provided below are intended to be used to illustrate the present invention, and the scope of the present invention includes the scope of the appended claims and its substitutions and modifications, and is not limited to the scope of the examples.
[0028] Release film examples Examples 1 to 5 and Comparative Examples 2 to 4 of the release film will be described below.
[0029] Example 1 100 grams of nickel tungsten cobalt molybdenum alloy (Ni / W / Co / Mo) (nickel 5% to 75% by weight, tungsten 5% to 35% by weight, cobalt 5% to 35% by weight, molybdenum 5% to 35% by weight and unavoidable impurities) was plated on copper foil (thickness: 18 micrometers) by sputtering to form a first inorganic layer. Next, 1 gram of benzotriazole was dissolved in 1000 milliliters of water to form an organic matter-containing solution. Then, the organic matter-containing solution was impregnated into the first inorganic layer to form a first organic layer. This resulted in the release film of Example 1.
[0030] Example 2 The release film of Example 2 was produced by the same process as Example 1, with the difference being that the organic substance-containing solution forming the first organic layer was changed to an organic substance-containing solution formed by dissolving 1 gram of 2-carboxybenzotriazole in 1000 milliliters of water, thereby obtaining the release film of Example 2.
[0031] Example 3 The release film of Example 3 was manufactured by the same process as Example 1, with the difference being that a second inorganic layer and a second organic layer were further formed on the first organic layer. Specifically, 100 grams of nickel tungsten cobalt molybdenum alloy (Ni / W / Co / Mo) (nickel 5% to 75% by weight, tungsten 5% to 35% by weight, cobalt 5% to 35% by weight, molybdenum 5% to 35% by weight, and unavoidable impurities) was plated on the first organic layer by electroplating to form a second inorganic layer. Then, 5 grams of benzotriazole was dissolved in 1000 milliliters of water to form an organic matter-containing solution. Then, the organic matter-containing solution was impregnated to form a second organic layer on the second inorganic layer. This resulted in the release film of Example 3.
[0032] Example 4 The release film of Example 4 was manufactured by the same process as Example 2, with the difference being that a second inorganic layer and a second organic layer were further formed on the first organic layer. Specifically, 100 grams of nickel tungsten cobalt molybdenum alloy (Ni / W / Co / Mo) (nickel 5% to 75% by weight, tungsten 5% to 35% by weight, cobalt 5% to 35% by weight, molybdenum 5% to 35% by weight, and unavoidable impurities) was plated on the first organic layer by electroplating to form a second inorganic layer. Then, 5 grams of 2-carboxybenzotriazole was dissolved in 1000 milliliters of water to form an organic matter-containing solution. Then, the organic matter-containing solution was impregnated to form a second organic layer on the second inorganic layer. This resulted in the release film of Example 4.
[0033] Example 5 100 grams of nickel molybdenum tungsten alloy (Ni / Mo / W) (nickel 5% to 75% by weight, molybdenum 5% to 35% by weight, tungsten 5% to 35% by weight, and unavoidable impurities) was plated on copper foil (thickness: 18 micrometers) by sputtering to form a first inorganic layer. Then, 5 grams of benzotriazole was dissolved in 1000 milliliters of water to form an organic substance-containing solution. Then, the organic substance-containing solution was impregnated to form a first organic layer on the first inorganic layer. Then, 100 grams of nickel cobalt tungsten alloy (Ni / Co / W) (nickel 5% to 75% by weight, cobalt 5% to 35% by weight, tungsten 5% to 35% by weight, and unavoidable impurities) was plated on the first organic layer by electroplating to form a second inorganic layer. Then, 5 grams of 2-carboxybenzotriazole was dissolved in 1000 milliliters of water to form an organic matter-containing solution.Then, the organic matter-containing solution was impregnated into the second inorganic layer to form a second organic layer.Therefore, the release film of Example 5 was obtained.
[0034] Comparative Example 2 100 grams of nickel tungsten cobalt molybdenum alloy (Ni / W / Co / Mo) (nickel 5% to 75% by weight, tungsten 5% to 35% by weight, cobalt 5% to 35% by weight, molybdenum 5% to 35% by weight, and unavoidable impurities) was plated on copper foil (thickness: 18 micrometers) by sputtering to form a first inorganic layer. Then, 100 grams of nickel tungsten cobalt molybdenum alloy (Ni / W / Co / Mo) (nickel 5% to 75% by weight, tungsten 5% to 35% by weight, cobalt 5% to 35% by weight, molybdenum 5% to 35% by weight, and unavoidable impurities) was plated on the first inorganic layer by electroplating to form a second inorganic layer. This resulted in the release film of Comparative Example 2.
[0035] Comparative Example 3 One gram of benzotriazole was dissolved in 1000 milliliters of water to form an organic substance-containing solution. Then, the organic substance-containing solution was used to form a first organic layer on a copper foil (thickness: 18 micrometers) by impregnation. Next, one gram of benzotriazole was dissolved in 1000 milliliters of water to form another organic substance-containing solution. Then, the other organic substance-containing solution was used to form a second organic layer on the first organic layer by impregnation. This resulted in the release film of Comparative Example 3.
[0036] Comparative Example 4 Five grams of 2-carboxybenzotriazole was dissolved in 1000 milliliters of water to form an organic substance-containing solution. Then, the organic substance-containing solution was used to form a first organic layer on a copper foil (thickness: 18 micrometers) by impregnation. Next, five grams of 2-carboxybenzotriazole was dissolved in 1000 milliliters of water to form another organic substance-containing solution. Then, the other organic substance-containing solution was used to form a second organic layer on the first organic layer by impregnation. This resulted in the release film of Comparative Example 4.
[0037] <Evaluation method> Examples 1 to 5 and Comparative Examples 2 to 4 An ultra-thin copper foil having a thickness of about 3 micrometers was formed on the top layer of the release film manufactured by Example 1 to Example 5 and Comparative Example 2 to Comparative Example 4 (for example, the first organic layer in Example 1 to Example 2, the second organic layer in Example 3 to Example 5 and Comparative Example 3 to Comparative Example 4, and the second inorganic layer in Comparative Example 2). Then, two steel plates were placed on the outermost surface of the release film on which the ultra-thin copper foil was formed. Then, the film was baked for 5 minutes at room temperature or at a temperature of 390°C in a high-temperature furnace (model number FB1300, manufactured by Thermo Fisher Scientific Inc.). Next, the heat-pressed release film was placed on a glass substrate, and after the ultra-thin copper foil and the glass substrate were bonded together, a sheet having a size of 15 cm was formed. TIFF0007561903000002.tif531.27 cm samples were cut. The samples were then measured for peel strength using a universal tensile tester (model number QC-528M1F, manufactured by Cometech Testing Machines Co., Ltd.), and the results are shown in Table 1. The smaller the peel strength, the more favorable the release film's peeling effect.
[0038] Comparative Example 1 An ultra-thin copper foil with a thickness of about 3 micrometers was formed on one side of the copper foil (thickness: 18 micrometers). Then, two steel plates were placed on the outermost surfaces of the copper foil on which the ultra-thin copper foil was formed (i.e., one steel plate was located on the side opposite to the side of the copper foil on which the ultra-thin copper foil was formed, and the other steel plate was located on the ultra-thin copper foil). Then, the copper foil on which the hot-pressed ultra-thin copper foil was formed was placed on a glass substrate, and after the ultra-thin copper foil and the glass substrate were bonded together, a sheet having a size of 15 cm was formed. TIFF0007561903000003.tif531.27 cm samples were cut. The peel strength of the samples was then measured using a universal tensile machine (model number QC-528M1F, Comtec Co., Ltd.), and the results are shown in Table 1.
[0039] [Table 1]
[0040] <Evaluation Results> As can be seen from Table 1, when the release film has at least one inorganic layer and at least one organic layer, and the material of the inorganic layer contains nickel, cobalt, tungsten, molybdenum or alloys thereof (Examples 1 to 5), the release film has a peel strength of 2.5 g / cm to 11 g / cm at room temperature, and a peel strength of 2 g / cm to 50 g / cm at a temperature of 390°C, that is, it has a favorable peeling effect, can be applied to the manufacture of electronic substrates, and can further recover the metal in the inorganic layer of the release film by electrochemical technology. In contrast, Comparative Example 1, which does not have a release film, cannot form an ultra-thin copper foil on the substrate at a temperature of 390°C.
[0041] Furthermore, compared to the case where no release layer for the organic layer (Comparative Example 2) is provided, the release layers having both an organic layer and an inorganic layer (Examples 1 to 5) have a smaller release force at room temperature, that is, a more favorable release effect.
[0042] Furthermore, compared to the case where a release layer for an inorganic layer is not provided (Comparative Examples 3 to 4), the release layers for an organic layer and an inorganic layer simultaneously provided (Examples 1 to 5) have a smaller release force at room temperature, i.e., a more preferable release effect, and at the same time have a preferable release effect at a temperature of 390°C.
[0043] Furthermore, compared with the release films having one inorganic layer and one organic layer (Examples 1-2), the release films having at least two inorganic layers and at least two organic layers (Examples 3-5) have a smaller peel force at room temperature, i.e., a more favorable peel effect, and at the same time have a favorable peel effect at a temperature of 390°C.
[0044] In addition, compared with the release films in which the organic layer material does not contain 2-carboxybenzotriazole (CBTA) (Examples 1 and 3), the release films in which the organic layer material contains 2-carboxybenzotriazole (CBTA) (Examples 2, 4 to 5) have a smaller peel force at a temperature of 390°C, that is, a more favorable peel effect, and at the same time have a favorable peel effect at room temperature.
[0045] In summary, the release film of the present invention and the release film produced by the method for producing the same comprise at least one inorganic layer and at least one organic layer, and the material of the inorganic layer comprises nickel, cobalt, tungsten, molybdenum or alloy thereof, the release film has a good release effect at room temperature and high temperature, and can be used for the production of electronic substrates, and can further recover the metal in the inorganic layer of the release film by electrochemical technology.In particular, the release film has a good release effect at high temperature, and can be used for the production of substrates for electronic products used in the 5th generation mobile communication technology.
[0046] The present invention has been disclosed above in the form of examples, but is not intended to limit the present invention. A person skilled in the art may make some changes and modifications without departing from the spirit and scope of the present invention, so the scope of protection of the present invention should be based on the appended claims.
Claims
1. At least two inorganic layers; At least two organic layers; Equipped with the material of the inorganic layer comprises nickel, cobalt, tungsten, molybdenum or an alloy thereof; The release film comprises the organic layers and the inorganic layers laminated alternately.
2. The release film according to claim 1 , wherein the material of the organic layer comprises a nitrogen-containing heterocyclic compound or a derivative thereof.
3. The release film of claim 1 , wherein the material of the organic layer comprises benzotriazole or a derivative thereof.
4. The release film of claim 1 , wherein the inorganic layer has a thickness of from 10 nanometers to 100 nanometers.
5. 10. The release film of claim 1 having a thickness of from 80 nanometers to 150 nanometers.
6. 2. The release film of claim 1, which has a release force of 0 to 20 grams / centimeter at room temperature and a release force of 0 to 50 grams / centimeter at a temperature of 390°C.
7. forming at least two inorganic layers on a substrate; forming at least two organic layers on the inorganic layer to form a release film comprising the inorganic layer and the organic layers; Including, the material of the inorganic layer comprises nickel, cobalt, tungsten, molybdenum or an alloy thereof; The method for producing a release film, in which the organic layers and the inorganic layers are laminated alternately.
8. The method for producing a release film according to claim 7 , wherein the inorganic layer is formed by a sputtering method or an electroplating method.
9. The method for producing a release film according to claim 7 , wherein the organic layer is formed by an impregnation method.
10. The method for producing a release film according to claim 7 , wherein the material of the organic layer comprises a nitrogen-containing heterocyclic compound or a derivative thereof.
11. The method for producing a release film according to claim 7 , wherein the material of the organic layer comprises benzotriazole or a derivative thereof.
12. The method for producing a release film according to claim 7, wherein the inorganic layer has a thickness of 10 nanometers to 100 nanometers.
13. The method for producing a release film according to claim 7, wherein the release film has a thickness of 80 nanometers to 150 nanometers.
14. The method for producing a release film according to claim 7, wherein the release strength of the release film at room temperature is 0 to 20 grams / centimeter and the release strength at a temperature of 390°C is 0 to 50 grams / centimeter.
Citation Information
Patent Citations
Composite metal foil, flexible foil-clad plate and preparation method of flexible foil-clad plate
CN113022048A
Composite metal foil and printed circuit board
CN211968681U
Metal powder
JP1989230701A
Carrier-provided copper foil, printed wiring board, laminate sheet, electronic equipment, laminate and method of producing printed wiring board
JP2015200025A
Copper foil with carrier, laminate, method for manufacturing copper foil with carrier, method for manufacturing printed wiring board, and method for manufacturing electric equipment