DEPOSITION METHODS AND APPARATUS FOR PIEZOELECTRIC APPLICATIONS - Patent application
The deposition of seed and template layers with improved uniformity addresses the challenges of growing relaxer-PT piezoelectric materials, achieving superior piezoelectric properties and performance through enhanced crystallinity and XRD peak intensity.
Patent Information
- Application Number
- JP2023512357
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-24
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2040-08-24
AI Technical Summary
Conventional PVD processes struggle to grow relaxer-PT type piezoelectric materials with a uniform perovskite phase structure and crystal orientation due to a narrow growth window and sensitivity to stoichiometry and temperature changes, leading to phase transformations and suboptimal piezoelectric properties.
A method involving the deposition of seed and template film layers with improved thickness and crystal orientation uniformity, using X-ray diffraction techniques, to facilitate the growth of piezoelectric materials with superior properties, including an ultra-thin seed layer and a template layer that matches the crystal structure of the piezoelectric material.
The method achieves highly uniform piezoelectric films with enhanced crystallinity and piezoelectric properties, as evidenced by increased XRD peak intensity and suppressed parasitic phases, resulting in improved performance of piezoelectric devices.
Smart Images

Figure 0007561971000001 
Figure 0007561971000002 
Figure 0007561971000003
Abstract
Description
[Technical field]
[0001]
[0001] Embodiments of the present disclosure relate generally to piezoelectric devices. More specifically, embodiments disclosed herein relate to piezoelectric devices and methods of depositing films for piezoelectric devices. [Background technology]
[0002] In semiconductor processing, physical vapor deposition (PVD) (e.g., sputtering) is used to transfer material at the atomic level to deposit a thin film or coating on a substrate. In PVD, ions generated from a plasma in a process chamber are bombarded against a target having a source material. The impact with the target causes the source material to be sputtered (e.g., ejected) from the target toward the substrate being processed. In some examples, the sputtered source material may be accelerated toward the substrate by application of a voltage bias. Upon reaching the surface of the substrate, the source material may react with another material of the substrate to form a thin film or coating thereon.
[0003]
[0003] PVD processes can be used to form thin film piezoelectric materials, which are materials that accumulate an electric charge upon application of mechanical stress. Piezoelectric materials are frequently used in sensors and transducers for devices such as gyro sensors, inkjet printer heads, and other Microelectromechanical Systems (MEMS) devices, including acoustic resonators for mobile phones and other wireless electronics. Relaxor ferroelectrics, particularly relaxor-PT materials, are a class of piezoelectric materials that exhibit extremely high piezoelectric properties due to their unique free energy landscape. To achieve these outstanding piezoelectric properties, a perovskite phase structure and <001> There is a need to grow relaxor-PT films with uniform crystal orientation (e.g., (001) or (002) orientation). However, growing such relaxor-PT type materials by conventional PVD processes is difficult. <001> It is very complex because of the narrow growth window related to orientation and because the material undergoes various phase transformations with even small changes in stoichiometry and / or temperature.
[0004] Therefore, what is needed in the art is an improved piezoelectric stack and method of forming the piezoelectric stack via PVD. Summary of the Invention
[0005]
[0005] The present disclosure relates generally to piezoelectric devices. More specifically, embodiments disclosed herein relate to piezoelectric devices and methods of depositing films for piezoelectric devices.
[0006]
[0006] In order that the above-mentioned features of the present disclosure may be understood in detail, the present disclosure summarized above will now be more particularly described with reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings merely depict exemplary embodiments, and therefore should not be considered as limiting the scope of the present disclosure, which may admit of other equally effective embodiments. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 illustrates a plan view of a cluster tool adapted to deposit thin film layers on a substrate through the use of one or more processing chambers according to embodiments described herein. [Diagram 2] 2 is a cross-sectional side view of a processing chamber of the cluster tool shown in FIG. 1 adapted to deposit a thin film layer on a substrate according to embodiments described herein. [Diagram 3] FIG. 2A is a side view of an exemplary film stack fabricated in the cluster tool shown in FIG. 1 in accordance with an embodiment described herein; FIG. 2B is a side view of an exemplary film stack fabricated in the cluster tool shown in FIG. 1 in accordance with an embodiment described herein. [Figure 4] FIG. 4 is a flow diagram illustrating an exemplary method for fabricating the film stack shown in FIGS. 3A and 3B according to embodiments described herein. [Diagram 5] FIG. 4 is a plan view of a controller capable of sending instructions to any one of the processing chambers illustrated in FIGS. 1-3 according to embodiments described herein. [Figure 6] FIG. 5A is a diagram of X-ray diffraction (XRD) data for a piezoelectric film formed by the method illustrated in FIG. 4 according to an embodiment described herein; FIG. 5B is a diagram of X-ray diffraction (XRD) data for a piezoelectric film formed by the method illustrated in FIG. 4 according to an embodiment described herein.
[0008]
[0015] To facilitate understanding, wherever possible, the same reference numerals have been used to designate identical elements common to the figures. It is contemplated that elements and features of one embodiment may be beneficially incorporated in other embodiments without further recitation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009]
[0016] The present disclosure relates generally to piezoelectric devices. More specifically, embodiments disclosed herein relate to piezoelectric devices and methods of depositing films for piezoelectric devices.
[0010]
[0017] Traditionally, large-scale deposition of thin metal films has been difficult due to non-uniformity of the thin metal film from its center to its edge. During deposition processes, including sputtering (e.g., physical vapor deposition or "PVD"), differences in the arrangement of atoms in a film layer on a substrate can cause cone defects, stacking faults, and other surface defects to form in subsequently deposited film layers. In piezoelectric element stacks, such defects can weaken the piezoelectric bonds and result in suboptimal piezoelectric properties in the resulting elements.
[0011]
[0018] Improved deposited thin film properties can be achieved in various types of deposited films, such as piezoelectric materials, through the methods disclosed herein. The methods disclosed herein allow for the deposition of seed and template film layers with improved thickness and crystalline orientation uniformity, which can be examined using X-ray diffraction (XRD) techniques. In certain embodiments, an ultra-thin seed layer having a uniform thickness from its center to its edge is deposited on a substrate. In certain embodiments, a template layer is deposited on a substrate that closely matches the crystalline structure of the subsequently formed piezoelectric material layer. These layers have improved orientation and thickness uniformity, which facilitates the growth thereon of piezoelectric materials that exhibit improved crystallinity and, as a result, superior piezoelectric properties.
[0012]
[0019] 1 is a schematic plan view of a cluster tool 100. An example of a cluster tool 100 is the Endura® system from Applied Materials, Inc. of Santa Clara, Calif. It is understood that the cluster tool 100 described below is an exemplary cluster tool, and that other cluster tools, including those from other manufacturers, can be used with or modified to form the piezoelectric element stacks described herein.
[0013]
[0020] The cluster tool 100 includes a factory interface 104, a loading dock 140, a first transfer chamber 124, and a second transfer chamber 128. A plurality of cassettes 112, or front-opening unified pods ("FOUPs"), are disposed in the factory interface 104 and are configured to receive a plurality of substrates (shown as 201 in FIG. 2) for processing. The substrates 201 may have diameters ranging from about 100 mm to about 750 mm and may be formed from a variety of materials including silicon (Si), silicon carbide (SiC), or graphite coated with SiC. In one embodiment, the substrates 201 include a Si material and are approximately 1000 cm 2 In another embodiment, the surface area of the substrate 201 is about 2000 cm 2 Above 4000cm 2Prior to processing, the substrates 201 are removed from the cassettes 112 by the factory interface robot 120 and transferred to a loading dock 140 (i.e., load lock). After substrate processing in the cluster tool 100 is completed, the processed substrates 201 may be returned to their respective cassettes 112.
[0014]
[0021] The first transfer chamber 124 is part of the main frame 172 and houses a centrally located first transfer robot 132. The first transfer robot 132 is configured to move substrates 201 between the loading dock 140 and a plurality of first processing chambers 160 (160a-d shown in FIG. 1) and / or pass-through chambers 162. The first transfer chamber 124 can be selectively isolated from each of the first processing chambers 160 and pass-through chambers 162 by use of slit valves (not shown) disposed between each of the first processing chambers 160 and pass-through chambers 162 and the first transfer chamber 124.
[0015]
[0022] Each loading dock 140 is selectively isolated from the first transfer chamber 124 by a slit valve and from the interior region 116 of the factory interface 104 by a vacuum door (not shown). In this configuration, the factory interface robot 120 of the factory interface 104 is configured to move a substrate 201 from a cassette 112 to the loading dock 140, which can be sealed and pumped down to a desired pressure for transferring the substrate 201 to the first transfer chamber 124. Once the desired pressure is reached, the substrate 201 is then accessible by the first transfer robot 132 through a slit valve opening (not shown) formed between the first transfer chamber 124 and the loading dock 140.
[0016]
[0023] The first processing chambers 160 may include any suitable type of processing chamber for forming a thin film layer stack on the substrate 201. In certain embodiments, one or more of the first processing chambers 160 includes an orientation chamber that is disposed proximate the loading dock 140 and is used to align the substrate 201 to a desired rotational orientation within the cluster tool 100. In some embodiments, the orientation chamber may include a heat source, such as a lamp or an infrared generating radiant heater, adapted to heat the substrate 201 to a desired temperature. The orientation chamber may further be pressurized under vacuum conditions such that undesired water or other contamination is removed from the surface of the substrate 201 prior to processing in other downstream chambers.
[0017]
[0024] In some embodiments, the first processing chamber 160 further includes one or more pre-cleaning chambers adapted to clean the surface of the substrate 201. The pre-cleaning chambers may clean the surface of the substrate 201 by use of a cleaning process that includes exposing the surface of the substrate 201 to a radio frequency (RF) generated plasma and / or one or more pre-cleaning gas compositions that include a carrier gas (e.g., Ar, He, Kr) and / or a reactive gas (e.g., hydrogen). In some embodiments, the pre-cleaning chambers are adapted to perform a process that may include a non-selective sputter etching process.
[0018]
[0025] In certain embodiments, one or more of the first processing chambers 160 are configured to process the substrate 201 therein by cooling the substrate 201, heating the substrate 201, etching the substrate 201, and / or depositing one or more layers on a surface of the substrate 201. In certain embodiments, the deposition process may include a sputter deposition process (i.e., a PVD deposition process). In certain configurations, one or more of the processing chambers 160 are further configured to anneal the substrate 201.
[0019]
[0026] The first transfer chamber 124 and the second transfer chamber 128 are coupled to each other via a pass-through chamber 162. In some configurations, the first transfer chamber 124 can be vacuum pumped to a moderately low pressure, e.g., less than about 1 milliTorr (mTorr). The second transfer chamber 128 can be pumped to a lower pressure, e.g., 1 μTorr or less. In this manner, the first and second transfer chambers 124, 128 can be maintained at least at a moderate vacuum level to prevent the transfer of contamination between the transfer chambers 124, 128 and other modules of the cluster tool 100.
[0020]
[0027] Similar to the first transfer chamber 124, the second transfer chamber 128 is part of a main frame 172 and houses a centrally located second transfer robot 136. The second transfer robot 136 is configured to move substrates 201 between each of a plurality of second processing chambers 170 and / or pass-through chambers 162. The second transfer chamber 128 can be selectively isolated from each of the second processing chambers 170 and pass-through chambers 162 by use of slit valves (not shown) disposed between each of the second processing chambers 170 and pass-through chambers 162 and the second transfer chamber 128.
[0021]
[0028] In certain embodiments, one or more of the second processing chambers 170 are configured to process the substrate 201 therein by cooling the substrate 201, heating the substrate 201, etching the substrate 201, and / or depositing one or more layers on a surface of the substrate 201. In certain embodiments, the deposition process may include a sputter deposition process (i.e., a PVD deposition process). In certain configurations, one or more of the second processing chambers 170 are further configured to anneal the substrate 201.
[0022]
[0029] Figure 2 is a plan view of a processing chamber 200 that can be utilized as the first and / or second processing chambers 160, 170. Processing chamber 200 is a PVD chamber adapted to deposit a thin film layer on a substrate 201 in the cluster tool shown in Figure 1. It should be understood that processing chamber 200 described herein is an exemplary chamber and that other PVD chambers, including PVD chambers from other manufacturers, can be used with or modified to accomplish aspects of the present disclosure.
[0023]
[0030] 2, the processing chamber 200 includes a process region 202 defined by a chamber body 205. The process region 202 has a target 210 and a pedestal 204 operable to support a substrate 201. The pedestal 204 is movably disposed in the process region 202 by a stem 206 connected to a lift system (not shown) that moves the pedestal 204 between a raised processing position and a lowered position that facilitates transfer of the substrate 201 to and from the processing chamber 200 through an opening 208 in the chamber body 205.
[0024]
[0031] The target 210 is connected to a power source 212, such as a DC power source, an RF power source, an AC power source, a pulsed DC power source, or a pulsed RF power source, via a target switch 226. During the deposition process, the target 210 can be negatively biased via a pulsed DC power source that provides pulsed DC power. A sputter gas flow controller 218, such as a mass flow control (MFC) device, is disposed between the sputter gas source 214 and the process region 202 and controls the flow of sputter gas from the sputter gas source 214 to the process region 202. A reactive gas flow controller 220, such as an MFC device, is disposed between the reactive gas source 216 and the process region 202 and controls the flow of reactive gas from the reactive gas source 216 to the process region 202.
[0025]
[0032] The pedestal 204, when engaged, is connected to a pedestal switch 230 that connects the pedestal 204 to a power source 234, such as a DC power source, an RF power source, an AC power source, a pulsed DC power source, and a pulsed RF power source. During a deposition process, the pedestal 204 can be negatively biased via the power source 234 that provides RF power. In certain embodiments, the processing chamber 200 is operable to independently bias the target 210 and the pedestal 204. A controller 207 is coupled to the processing chamber 200 and configured to control aspects of the processing chamber 200 during processing, such as the connection of the target switch 226 and the connection of the pedestal switch 230.
[0026]
[0033] 3A is a side view of an exemplary film stack 300 fabricated in the cluster tool disclosed in FIG. The film stack 300 includes a substrate 201, a first seed layer 304, a bottom electrode layer 306, a second seed layer 308, a piezoelectric material layer 312, and a top electrode layer 314. Generally, the layers of the film stack 300 have high thickness uniformity. For example, the thickness of each layer has a delta (e.g., thickness non-uniformity) of about ±10% across the lateral length of the layer, such as a delta of about ±5%.
[0027]
[0034] The substrate 201 may, in some embodiments, be <001> The substrate 201 is a 200 mm silicon (Si) substrate having a crystal orientation (e.g., (001) or (002)). The substrate 201 may be formed of polycrystalline molybdenum (Mo), strontium ruthenium oxide (SrRuO3, SRO), lanthanum nickel oxide (LaNiO3, LNO), lanthanum strontium manganite (LaSrMnO3, LSMO), and calcium ruthenate (CaRuO3) with suitable lattice structures. In a particular embodiment, a thermal oxide layer 302 is grown on the surface of the substrate 201, such as a Si or silicon oxide (SiOx) layer. For example, the thermal oxide layer 302 may be formed of silicon dioxide (SiO2). The thermal oxide layer 302 may have a thickness of about 10 nm to about 1000 nm, such as about 15 nm to about 750 nm, such as about 20 nm to about 500 nm. In certain embodiments, the thermal oxide layer 302 has a thickness of about 25 nm to about 200 nm, such as about 50 nm to about 150 nm. For example, the thermal oxide layer 302 may have a thickness of about 75 nm to about 125 nm, such as about 100 nm.
[0028]
[0035] The first seed layer 304 may be formed directly on the surface of the substrate 201 or on the surface of the thermal oxide layer 302. The first seed layer 304 supports the growth of a bottom electrode layer 306 that may be deposited on the surface of the first seed layer 304 and function as a bottom electrode of the device. Examples of suitable materials for the bottom electrode layer 306 include platinum (Pt), SrRuO3, LaNiO3, CaRuO3, LaSrMnO3, etc. In a specific embodiment, the first seed layer 304 is made of a metal such as titanium dioxide (TiO2). <001> The bottom electrode layer 306 is formed of titanium oxide (TiOx) having an orientation (e.g., (001) or (002)). <111> It is made of highly oriented Pt. <111> The layer is essential for forming a uniform second seed layer 308, which in turn aids in the formation of a piezoelectric material layer 312 with high orientation control. <111> It is possible to support the growth of the Pt bottom electrode layer 306 with only orientation.
[0029]
[0036] It should be noted that, similar to the seed layers 304, 308, the orientation of the bottom electrode layer 306 can be detected and confirmed by X-ray diffraction (XRD) analysis, such as 2 theta-omega scanning, as well as cross-sectional high resolution transmission electron microscopy (HRTEM). <111> It was found that only peaks corresponding to orientation could be detected in 2 theta-omega scans, and these peaks exhibited high intensities of over 10,000 counts per second (cps), indicating that the bottom electrode layer 306, like the first seed layer 304, is also highly oriented.
[0030]
[0037] In certain embodiments, the first seed layer 304 has a thickness of about 10 nm to about 50 nm, such as about 20 nm to about 30 nm, e.g., about 25 nm. In certain embodiments, the bottom electrode layer 306 has a thickness of about 50 nm to about 200 nm, such as about 75 nm to about 175 nm, e.g., about 100 nm to about 150 nm, e.g., about 125 nm.
[0031]
[0038] The second seed layer 308 is deposited on the bottom electrode layer 306 and may be formed of any suitable ultra-thin metal film. In certain embodiments, the second seed layer 308 is formed of Pt or titanium (Ti). In certain embodiments, the second seed layer 308 is formed of the same material or a different material than the first seed layer 304. The second seed layer 308 has a uniform thickness of about 0.5 nm to about 5 nm, such as about 1 nm to about 3 nm, as confirmed by cross-sectional HRTEM. For example, the second seed layer 308 has a uniform thickness of about 1.5 nm to about 2.5 nm, such as about 2 nm. As discussed above, a thin, highly uniform seed layer provides uniformity for subsequent device layers and allows for improved process integration.
[0032]
[0039] A piezoelectric material layer 312 is deposited over the second seed layer 308 and is formed of any suitable piezoelectric material. In certain embodiments, the piezoelectric material layer 312 is formed from one or more layers including scandium doped aluminum nitride (ScAlN) or AlN. In certain embodiments, the piezoelectric material layer 312 is formed from one or more layers including titanium nitride (TiN), hafnium nitride (HfN), or silicon nitride (SiN). x N y ), or a combination thereof. In some embodiments, the piezoelectric material layer 312 is formed of relaxor-lead titanate (PT) type materials, such as lead magnesium niobate-lead titanate (PMN-PT) and lead indium niobate-lead magnesium niobate-lead titanate (PIN-PMN-PT). The piezoelectric material layer 312 may have a thickness of about 500 nm to about 2000 nm, such as about 750 nm to about 1500 nm, such as about 1000 nm.
[0033]
[0040] A top electrode layer 314 may be deposited on the piezoelectric material layer 312 and function as a top electrode in the completed device. In certain embodiments, the top electrode layer 314 may be formed of the same or a different material than the bottom electrode layer 306. For example, the top electrode layer 314 may be <111> In a specific embodiment, the top electrode layer 314 has a thickness of about 30 nm to about 200 nm, such as about 50 nm to about 150, for example about 100 nm.
[0034]
[0041] 3B is a side view of another exemplary film stack 301 fabricated in the cluster tool disclosed in FIG. 1. As described with reference to film stack 300, the layers of film stack 301 are highly uniform in thickness. For example, the thickness of each layer has a delta (e.g., variance) of about ±10% across the lateral length of the layer, such as a delta of about ±5%. Film stack 301 includes the layers described above with reference to FIG. 3A and further includes a template layer 310. Template layer 310 may be deposited directly on a surface of bottom electrode layer 306 or second seed layer 308 and below piezoelectric material layer 312.
[0035]
[0042] Formation of template layer 310 is beneficial when piezoelectric material layer 312 is formed of relaxor-PT type piezoelectric material, a class of complex oxide materials that exhibit very high piezoelectric properties due to a unique free energy landscape. <001> Thus, in an example where the piezoelectric material layer 312 is formed of a relaxor-PT type piezoelectric material, such as PMN-PT, the template layer 310 may be <001> PZT has a crystal structure that closely matches the crystal structure of the relaxor PT type piezoelectric material, and therefore the PZT template layer 310 may be formed of a perovskite PZT film having a crystalline orientation of <001> The nucleation energy for growing the oriented relaxor-PT type piezoelectric material layer 312 can be lowered, resulting in heteroepitaxial, cube-on-cube crystal growth. This type of growth, when analyzed by XRD, such as 2 theta-omega scan, <001> The improved crystallinity shows a five-fold (e.g., 5x) increase in peak intensity. High XRD intensity is important to dramatically improve the piezoelectric properties. Furthermore, since PZT itself is a piezoelectric material, increasing the thickness of the PZT template layer 310 does not adversely affect the electromechanical properties or response of the relaxor-PT type piezoelectric material layer 312. In some embodiments, the template layer 310 has a thickness of about 10 nm to about 200 nm, e.g., about 25 nm to about 175 nm, about 50 nm to about 150, about 75 nm to about 125, e.g., about 100 nm.
[0036]
[0043] Figure 4 is a flow diagram illustrating a method 400 for fabricating film stacks 300 and 301. For ease of explanation, Figure 4 will be described with reference to the cluster tool 100 of Figure 1. However, it should be noted that cluster tools other than the cluster tool 100 of Figure 1 can be utilized in conjunction with method 400.
[0037]
[0044] In block 402, the substrate 201 is loaded into the cluster tool 100 and pre-processed. The substrate 201 may or may not already have a thermal oxide layer formed thereon, such as the thermal oxide layer 302, before being loaded into the cluster tool 100. In a particular embodiment, the substrate is loaded into the loading dock 140 by one of the factory interface robots 120 and then transferred by the first transfer robot 132 through the first transfer chamber 124 to the orientation chamber, pre-clean chamber, and / or other first processing chambers 160. As mentioned above, the pressure (P) of the first transfer chamber 124 may be about 1 microTorr. Thus, the pressure of the cluster tool 100 is maintained at a vacuum state.
[0038]
[0045] During pre-treatment, the substrate 201 may be exposed to a degassing process performed in one of the first processing chambers 160. Optionally, the surface of the substrate 201 may be exposed to plasma to pre-clean the surface of the substrate 201, which may be performed before or after performing the degassing process. For example, the surface of the substrate 201 may be pre-cleaned (e.g., bombarded (e.g., etched) with reactive gas (e.g., H2) or non-reactive gas (e.g., Ar, Ne, He) ions and / or gas radicals) in a pre-cleaning chamber before being transferred to another first or second processing chamber 160, 170 for deposition of the first seed layer 304. Pre-cleaning the surface of the substrate 201 before depositing the first seed layer 304 may reduce surface defects of the first seed layer 304 when it is deposited on the substrate 201. Other processes that may be performed during block 402 may also include heating, maintaining the inlet temperature of the substrate 201, or cooling the substrate 201. After pre-processing in block 402, the substrate 201 may be transferred to one or more processing chambers 160, 170, which may include the components shown in processing chamber 200, for forming individual layers of the film stack 300 or 301 thereon.
[0039]
[0046] In block 404, a first seed layer 304 is formed on the substrate 201. In certain embodiments, the first seed layer 304 is formed on the substrate 201 by PVD and / or an annealing and oxidation process. For example, a thin crystalline Ti film can be deposited by PVD at room temperature, and then the Ti film can be exposed to an annealing and oxidation process to form a TiO2 layer.
[0040]
[0047] In block 406, a bottom electrode layer 306 is formed on the first seed layer 304 in one of the processing chambers 160, 170. For example, the bottom electrode layer 306 may be deposited on the first seed layer 304 via a PVD process performed in a PVD chamber, such as the processing chamber 200. In a particular embodiment, the PVD process is performed at about 37° C. to about 600° C., such as about 400° C. to about 600° C., such as about 500° C. In a particular embodiment, the target of the PVD chamber is negatively biased during the PVD process by a pulsed or continuous power supply providing DC power having a power level of about 400 W to about 1000 W, such as about 600 W to about 800 W. In certain embodiments, which can be combined with other embodiments described herein, the flow rate of Ar during the PVD process is from about 20 sccm to about 60 sccm, e.g., from about 30 sccm to about 50 sccm, and the pressure in the PVD chamber is from about 4 mTorr to about 25 mTorr, e.g., from about 10 mTorr to about 20 mTorr.
[0041]
[0048] As mentioned above, in certain embodiments, the bottom electrode layer 306 is <111> oriented Pt, thus aiding in the subsequent formation of the highly oriented piezoelectric material layer 312. In a further embodiment, a Pt bottom electrode layer 306 is deposited on the TiO2 first seed layer 304.
[0042]
[0049] At block 408, a second seed layer 308 is formed on the bottom electrode layer 306. Similar to the first seed layer 304, the second seed layer 308 may be formed by depositing a thin Ti layer via PVD at room temperature and then annealing the Ti layer to form a TiO2 layer. In other embodiments, the second seed layer 308 is formed of a different material and / or by a different process. The second seed layer 308 has a uniform thickness of about 0.5 nm to about 5 nm, e.g., about 1 nm to about 3 nm, e.g., about 2 nm, and a uniform surface area of about 0.5 nm to about 5 nm. <001> A thin, highly uniform seed layer with conformal crystalline orientation enables uniformity in subsequent device layers and facilitates the formation of piezoelectric material layers with excellent piezoelectric properties.
[0043]
[0050] Optionally, a template layer 310 may then be deposited on the second seed layer 308 in block 410 as shown in the film stack 301 . <001> The template layer, which may be formed of a perovskite PZT film having an orientation of is deposited via a PVD process at a temperature of about 500° C. to about 750° C., e.g., about 650° C., and a pressure of about 5 mTorr to about 25 mTorr, e.g., about 18 mTorr to about 20 mTorr. In a particular embodiment, the target of the PVD chamber is negatively biased during the PVD process by a pulsed or continuous power source providing RF power having a power level of about 1000 W to about 2500 W, e.g., about 1200 W to about 2000 W. In a particular embodiment that can be combined with other embodiments described herein, the flow rate of Ar during the PVD process is about 20 sccm to about 60 sccm, e.g., about 30 sccm to about 50 sccm, and the flow rate of O2 is about 0 sccm to about 20 sccm, e.g., about 5 sccm to about 15 sccm.
[0044]
[0051] As a result of the above-described deposition process, template layer 310 has a uniform thickness ranging from about 10 nm to about 200 nm, such as from about 50 nm to about 150 nm, and such as about 100 nm. As previously described, template layer 310 may be formed of a piezoelectric material having similar properties as piezoelectric material layer 312, and thus forming a thicker template layer 310 does not adversely affect the piezoelectric properties of the film stack.
[0045]
[0052] In block 412, a piezoelectric material layer 312 is formed, for example, by a PVD process substantially similar to the process for forming the template layer 310. In a particular embodiment, the target of the PVD chamber is negatively biased by a pulsed or continuous power source providing RF power having a power level of about 1000 W to about 2500 W, for example, about 1200 W to about 2000 W. In a particular embodiment, which can be combined with other embodiments described herein, the flow rate of Ar during the PVD process is about 20 sccm to about 60 sccm, for example, about 30 sccm to about 50 sccm, and the flow rate of O2 is about 0 sccm to about 20 sccm, for example, about 5 sccm to about 15 sccm.
[0046]
[0053] In certain embodiments, the piezoelectric material layer 312 is formed directly on the second seed layer 308 as illustrated in film stack 300. In certain other embodiments, the piezoelectric material layer 312 is deposited on the template layer 310 as illustrated in film stack 301. Forming the piezoelectric material layer 312 on the template layer 310 is particularly beneficial when the piezoelectric material layer 312 is formed of a relaxor-PT type material, such as lead PMN-PT or PIN-PMN-PT. In such instances, the template layer 310 may be formed with a crystal structure that closely matches the crystal structure of the relaxor-PT type material, and thus <001> This facilitates uniform heteroepitaxial growth of the piezoelectric material layer 312 with good orientation and excellent piezoelectric properties.
[0047]
[0054] Following the formation of the piezoelectric material layer 312, a top electrode layer 314 is formed on the film stack 300 or 301 in block 414. Similar to the bottom electrode layer 306, the top electrode layer 314 may be formed of Pt deposited on the piezoelectric material layer 312 via a PVD process carried out at a temperature of about 300° C. to about 600° C., for example, about 500° C. In a particular embodiment, the target of the PVD chamber is negatively biased during the PVD process by a pulsed or continuous power source providing DC power having a power level of about 400 W to about 1000 W, for example, about 600 W to about 800 W. In a particular embodiment, which can be combined with other embodiments described herein, the flow rate of Ar during the PVD process is about 20 sccm to about 60 sccm, for example, about 30 sccm to about 50 sccm, and the pressure in the PVD chamber is about 4 mTorr to about 25 mTorr, for example, about 10 mTorr to about 20 mTorr.
[0048]
[0055] After blocks 402-414 are completed and the film stack 300 or 301 is formed, the substrate 201 may be returned to the factory interface 104 via one of the first and / or second transfer robots 132, 136 and the factory interface robot 120.
[0049]
[0056] FIG. 5 is a schematic plan view of a controller 500 that may provide instructions to any one of the processing chambers shown in FIGS.
[0050]
[0057] An optional display unit 501 may be coupled to the controller 500. The controller 500 includes a processor 504, a memory 508, and support circuits 512 coupled together. The controller 500 may be on-board the cluster tool 100, or in the alternative, the controller 500 may be on-board the processing chamber of FIG. 2 or a remote device (not shown).
[0051]
[0058] The display unit 501 includes input control units, such as power supplies, clocks, cache, input / output (I / O) circuits, etc., coupled to various components of the display unit 501 to facilitate its control. The processor 504 may be one of any form of general purpose microprocessor, or a general purpose central processing unit (CPU), each of which may be used in an industrial environment, such as a programmable logic controller (PLC).
[0052]
[0059] The memory 508 includes at least one non-transitory computer readable medium and may be one or more of a random access memory (RAM), a read only memory (ROM), or any other form of readily available memory such as local or remote digital storage. The memory 508 includes instructions that, when executed by the processor 504 (e.g., a central processing unit (CPU), a digital signal processor (DSP), an application specific integrated circuit (ASIC)), facilitate steps and processes within any of the process chambers shown in FIGS. 1-2. The instructions in the memory 508 are in the form of a program product, such as a program that implements the methods of the present disclosure. The program code of the program product may conform to any one of a number of different programming languages. Exemplary computer-readable storage media include, but are not limited to, (i) non-writable storage media in which information is permanently stored (e.g., a read-only memory device in a computer, such as a CD-ROM disk readable by a CD-ROM drive, a flash memory, a ROM chip, or any type of solid-state non-volatile semiconductor memory); and (ii) writable storage media in which changeable information is stored (e.g., a floppy disk in a diskette drive or hard disk drive, or any type of solid-state random access semiconductor memory). Such computer-readable storage media are examples of the present disclosure when they carry computer-readable instructions that direct the functions of the methods described herein. The program code in the memory 508 can be executed by the processor 504 to perform various processing methods in the apparatus, for example, to perform one or more of the method steps described in connection with FIG. 4 to fabricate the film stack 300 or 301 using the various process chambers and supporting components included in the cluster tool 100 illustrated in FIG. 1.
[0053]
[0060] In one embodiment, the controller 500 may be implemented as a program product stored on a computer-readable storage medium (e.g., 508) for use with a computer system (not shown). The program(s) of the program product define the functions of the present disclosure as described herein.
[0054]
[0061] FIG. 6A shows a comparison of X-ray diffraction (XRD) readouts of a PMN-PT piezoelectric material layer 602 formed on a TiOx seed layer and a PMN-PT piezoelectric material layer 604 formed on a PZT template layer, according to an embodiment of the present invention. Piezoelectric material layers 602, 604 are an example of piezoelectric material layer 312 described above. The vertical axis of FIG. 6A represents relative intensity in arbitrary units (au) and the horizontal axis represents the 2-theta scale in degrees (°). Both XRD readouts show strong (001) and (002) peaks and a highly uniform <001> 6 shows that the piezoelectric layers have a crystalline orientation. Furthermore, pyrochlore, lead oxide (PbO), and (111) are suppressed to different degrees in each of the piezoelectric layers 602, 604. Suppression of pyrochlore and Pbo is desirable because they are parasitic phases that degrade piezoelectric performance.
[0055]
[0062] Figure 6B illustrates the XRD intensity values of Figure 6A as a ratio of desired to undesired peaks. In particular, bar 610 represents the ratio of the (002) peak intensity to the (111) peak intensity, and bar 620 represents the ratio of the (002) peak intensity to the maximum of the PbO or pyrochlore peak intensity. As shown, piezoelectric material layer 602 exhibited a higher ratio of (002) / maximum (PbO, pyrochlore) intensity, and piezoelectric material layer 604 exhibited a significantly larger ratio of (002) / (111) intensity.
[0056]
[0063] In summary, through the methods disclosed herein, thin piezoelectric films having highly uniform thickness and crystalline orientation can be formed. In certain embodiments, highly uniform piezoelectric films are promoted by the deposition of an ultra-thin TiOx seed layer having uniform thickness from center to edge. In certain embodiments, highly uniform piezoelectric films are promoted by the deposition of a PZT template layer that closely matches the crystalline structure of the subsequently formed piezoelectric film. The increased uniformity of the piezoelectric film can result in superior piezoelectric properties and therefore improved piezoelectric performance of the resulting device.
[0057]
[0064] While the foregoing is directed to embodiments of the present disclosure, other and further embodiments of the present disclosure may be devised without departing from the basic scope thereof, as determined by the following claims.
Claims
1. 1. A piezoelectric element stack comprising: a substrate including a thermal oxide layer; a first seed layer formed on the thermal oxide layer, the first seed layer comprising titanium (Ti); a bottom electrode layer formed on the first seed layer; a second seed layer comprising titanium (Ti) and having a thickness of 0.5 nm to 5 nm and a thickness non-uniformity of ±10%; a piezoelectric material layer formed on the second seed layer, the piezoelectric material layer including a piezoelectric material; A piezoelectric element stack comprising:
2. 2. The piezoelectric stack of claim 1, wherein the piezoelectric material is a relaxor-lead titanate (PT) type material.
3. The piezoelectric stack of claim 2 , wherein the relaxor-PT type material comprises lead magnesium niobate-PT (PMN-PT) or lead indium niobate-lead magnesium niobate-PT (PIN-PMN-PT).
4. a template layer formed over the second seed layer and below the piezoelectric material layer, the template layer having a crystal structure substantially identical to a crystal structure of the piezoelectric material layer; The piezoelectric stack of claim 3 further comprising:
5. The piezoelectric stack of claim 4 , wherein the template layer comprises perovskite lead zirconate titanate (PZT).
6. The piezoelectric stack of claim 4 , wherein the template layer has a thickness of 10 nm to 200 nm.
7. The piezoelectric stack of claim 4 , wherein the template layer and the piezoelectric material layer have an orientation of <001>.
8. The piezoelectric stack of claim 1 , wherein the first seed layer comprises titanium dioxide.
9. The piezoelectric stack of claim 1 , wherein the second seed layer comprises titanium dioxide having a <001> orientation.
10. The piezoelectric stack of claim 1 , wherein the bottom electrode is formed of platinum (Pt) having a <111> orientation.
11. 1. A piezoelectric element stack comprising: a substrate including a thermal oxide layer; a first titanium oxide (TiOx) seed layer disposed on the thermal oxide layer; a first platinum (Pt) electrode layer disposed on the first TiOx seed layer; a second TiOx seed layer disposed on the first Pt electrode layer and having a thickness of 0.5 nm to 5 nm and a thickness non-uniformity of ±10%; a perovskite lead zirconate titanate (PZT) template layer disposed on the second TiOx seed layer; a relaxor-lead titanate (PT) type piezoelectric material layer disposed on the PZT template layer; A piezoelectric element stack comprising:
12. 12. The piezoelectric element stack of claim 11, wherein the relaxor-PT type piezoelectric material layer comprises lead magnesium niobate-PT (PMN-PT) or lead indium niobate-lead magnesium niobate-PT (PIN-PMN-PT).
13. 1. A method of forming a piezoelectric element stack, comprising: forming a seed layer over a substrate, depositing a titanium (Ti) film onto the substrate via physical vapor deposition (PVD); exposing the titanium film to an annealing process to form titanium dioxide (TiO2), the seed layer having a thickness of 0.5 nm to 5 nm and a thickness non-uniformity of ±10%; forming a seed layer over the substrate; forming a piezoelectric material layer over the seed layer, the piezoelectric material being deposited via PVD; The method includes:
14. The method of claim 13 , wherein the seed layer has a thickness of 2 nm.
15. The method of claim 13 , wherein the piezoelectric material layer is deposited directly on the seed layer.
16. The method of claim 13 , wherein the piezoelectric material layer is deposited on a template layer formed over the seed layer.
17. The method of claim 16 , wherein the template layer has a crystal structure substantially identical to a crystal structure of the piezoelectric material layer.
18. 20. The method of claim 17, wherein the template layer comprises perovskite lead zirconate titanate (PZT).
19. The method of claim 16, wherein the piezoelectric material is a relaxor-lead titanate (PT) type material.
20. 20. The method of claim 19, wherein the relaxor-PT type material comprises lead magnesium niobate-PT (PMN-PT) or lead indium niobate-lead magnesium niobate-PT (PIN-PMN-PT).
Citation Information
Patent Citations
Piezoelectric element and its fabrication process, liquid ejection head and its manufacturing process, and liquid ejector
JP2006245247A
Piezoelectric element, its manufacturing method, and liquid jetting head
JP2008060259A
Actuator, method of manufacturing actuator, liquid droplet ejecting head, liquid cartridge, ink jet recording apparatus, and micropump
JP2015027789A
Piezoelectric element, liquid discharge head and liquid discharge device
JP2021183379A