Thermally expandable polyvinyl chloride resin material, thermally expandable sheet, and window or door frame
The thermally expandable vinyl chloride resin material, enhanced with a dehydrochlorination inhibitor and specific compounds, addresses water resistance issues, ensuring effective flame and smoke blocking functions in outdoor environments.
Patent Information
- Application Number
- JP2021174494
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-10-26
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2036-12-28
AI Technical Summary
Conventional thermally expandable vinyl chloride resin materials exhibit poor water resistance when exposed to outdoor environments, leading to elution of components and impairment of flame and smoke blocking functions.
A thermally expandable vinyl chloride resin material is developed using a combination of vinyl chloride resin, thermally expandable graphite, a dehydrochlorination catalyst, and a dehydrochlorination inhibitor, with specific compounds containing amino or ammonium groups to suppress the catalytic function of the dehydrochlorination catalyst, enhancing cohesive strength and water resistance.
The material achieves higher cohesive strength, better shape retention, and improved mechanical strength while maintaining excellent water resistance, effectively blocking flames and smoke even in low-temperature ranges, suitable for outdoor applications.
Smart Images

Figure 0007562085000008 
Figure 0007562085000009 
Figure 0007562085000010
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermally expandable vinyl chloride resin material and a method for producing the thermally expandable vinyl chloride resin material. In particular, the present invention relates to a thermally expandable vinyl chloride resin material and a method for producing the thermally expandable vinyl chloride resin material, which can effectively exhibit a flame and smoke blocking function in a low temperature range, and when heated and expanded, the expanded body has excellent shape retention and mechanical strength, and in a preferred embodiment, can provide products such as thermally expandable sheets with excellent water resistance, and a method for producing the thermally expandable vinyl chloride resin material. The present invention relates to a technology for providing a thermally expandable vinyl chloride resin material that can provide products in the form of a thermally expandable vinyl chloride resin material such as a thermally expandable sheet, putty, or paint with excellent functionality in that the elution of components by rainwater, etc. is suppressed when the product is exposed to an outdoor environment, for example. [Background technology]
[0002] In the field of building materials, fire resistance is important, and various materials with fire resistance have been developed. Expandable graphite has the property of expanding rapidly when heated, and this property is used to manufacture sheets (hereinafter also called thermally expandable sheets) or amorphous objects (putty, paint, coatings) containing expandable graphite in resin, which are placed in spaces and used as fire prevention materials that expand when heated during a fire to slow the spread of fire. In this case, the resin components used in combination with expandable graphite are required to not only realize high fire resistance and flame retardancy of the resin material itself, but also to form an effective heat insulating layer during a fire, thereby blocking flames and smoke.
[0003] An example of a resin component having such a function is polyvinyl chloride resin, and for example, Patent Document 1 proposes a thermally expandable polyvinyl chloride resin material that utilizes the flame retardancy and moldability of polyvinyl chloride resin. This resin material is said to be easy to continuously manufacture by extrusion molding or the like while maintaining good expandability and shape retention after expansion, and the structure obtained by expanding the molded body is said to have the same fire resistance as conventional structures and the mechanical strength required to block fire and smoke.
[0004] Flame retardants are used in thermally expandable resin materials, including those described above, to improve flame retardancy. In particular, in the field of use as a fire prevention material that expands with heat in the event of a fire to slow the spread of fire, polyphosphate-based flame retardants are widely used because of their flame retardant effect and cost.
[0005] The inventors have already proposed a thermally expandable polyvinyl chloride resin material that can effectively exhibit a flame and smoke blocking function, particularly in a low temperature range, and that has an expanded body that has excellent shape retention and mechanical strength after expansion. The feature of this technology is that a dehydrochlorination catalyst that has the function of promoting the dehydrochlorination of polyvinyl chloride resin at the expansion start temperature of expandable graphite has been newly discovered, and as a result, this technology makes it possible to provide a product that has excellent shape retention and mechanical strength, with a high caking force of 0.8 kgf for the expanded body obtained by heating at 800°C, which was not possible with conventional thermally expandable resin materials. And, in this proposal, a polyphosphate-based flame retardant that is widely used in conventional technologies is used as the flame retardant. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 4250153 [Patent Document 2] Patent No. 5992589 Summary of the Invention [Problem to be solved by the invention]
[0007] In the course of further investigation of the above-mentioned conventional techniques already proposed, the present inventors recognized that although the thermally expandable polyvinyl chloride resin material provided by the above-mentioned techniques can realize products with excellent fire resistance, excellent shape retention and mechanical strength, and a high viscosity force of 0.8 kgf when heated to 800°C, the resin material has a problem to be considered in terms of water resistance, and that the water resistance needs to be improved. That is, for example, when the thermally expandable polyvinyl chloride resin material provided by the above-mentioned conventional techniques is used as a flame retardant at the boundary between the inside and outside of a window frame or a doorway that is exposed to rainwater or the like facing the outside, the water resistance is poor, and the components of the thermally expandable polyvinyl chloride resin material are eluted by rainwater or the like, which causes defects in appearance due to the precipitation of the eluted matter. Depending on the degree of the defect in appearance, there is a concern that the performance of the expandable body obtained by heating and expanding products such as thermally expandable sheets used as fire spread prevention materials during a fire may be reduced, and the high performance inherent to the expandable body may not be effectively demonstrated. Therefore, improving the water resistance of products made of thermally expandable polyvinyl chloride resin materials is an extremely important issue. At the same time, there is a need for technological development that can stably provide higher quality products by improving the binding force of the expandable body obtained by heating, improving the fire resistance performance with better shape retention and mechanical strength, and we recognized that further improvements are necessary for this purpose.
[0008] Therefore, the object of the present invention is to consistently provide a thermally expandable polyvinyl chloride resin material of higher quality and with better flame and smoke blocking properties, which can effectively exhibit flame and smoke blocking properties even in low temperature ranges, and which, when expanded by heating to 800°C, exhibits higher caking power and is of higher quality with excellent shape retention and mechanical strength, and which can be used outdoors and has excellent water resistance even when exposed to rainwater, etc., and which can be used as a product in a variety of environments, and which has better flame and smoke blocking properties, and products such as thermally expandable sheets using the same. [Means for solving the problem]
[0009] The above object is achieved by the present invention described below. That is, the present invention provides a thermally expandable vinyl chloride resin material comprising a vinyl chloride resin, a plasticizer for the resin, thermally expandable graphite having an expansion onset temperature of 180 to 240°C, a dehydrochlorination catalyst for the vinyl chloride resin, and a dehydrochlorination inhibiting compound, the thermally expandable graphite being contained in an amount ranging from 50 to 150 parts by mass per 100 parts by mass of the vinyl chloride resin, the dehydrochlorination catalyst being a substance that causes a weight loss of 25% or more when sample A having a blend of 52 parts by mass of a vinyl chloride resin having an average degree of polymerization of 400 to 3000, 42.8 parts by mass of dioctyl phthalate as a plasticizer for the resin, and 5.2 parts by mass of the dehydrochlorination catalyst is heated at 180°C for 15 minutes and then at 190°C for 15 minutes, and the amount of the dehydrochlorination catalyst per 100 parts by mass of the vinyl chloride resin is 25% or more. The present invention provides a thermally expandable polyvinyl chloride resin material, characterized in that sample B is prepared by adding 52 parts by mass of a polyvinyl chloride resin having an average degree of polymerization of 400 to 3000, 42.8 parts by mass of dioctyl phthalate as a plasticizer for said resin, and further adding a desired amount of a dehydrochlorination catalyst per 100 parts by mass of said polyvinyl chloride resin having an average degree of polymerization of 400 to 3000, and after heating at 180°C for 15 minutes and then at 190°C for 15 minutes, the weight loss of said sample B is within a range of 25% by mass or more, the dehydrochlorination inhibiting compound is a compound having an amino group and / or an ammonium group that has a function of inhibiting the catalytic function of the dehydrochlorination catalyst at an initial heated temperature of 160 to 240°C, and the caking strength of the expanded body obtained by heating at 800°C is 0.8 kgf or more.
[0010] Preferred embodiments of the thermally expandable vinyl chloride resin material of the present invention include the following: The dehydrochlorination inhibitor is at least one selected from the group consisting of melamine polyphosphate, melamine-melam-melem polyphosphate, melamine phosphate, melamine metal polyphosphate, piperazine phosphate, ethylenediamine phosphate, melamine sulfate, melamine, melam, melem, melamine cyanurate, benzoguanamine, silane-coated ammonium polyphosphate, melamine-coated ammonium polyphosphate, urea, and ammonium chloride; The dehydrochlorination catalyst is at least one selected from the group consisting of benzoguanamine and silane-coated ammonium polyphosphate; the amount of the dehydrochlorination inhibitor used is within the range of 50 to 150 parts by mass relative to 100 parts by mass of the vinyl chloride resin; the dehydrochlorination catalyst is at least one selected from the group consisting of metallic zinc, zinc oxide, zinc carbonate, zinc chloride, copper, copper oxide and iron chloride; the amount of elution when immersed in hot water at 95°C for 24 hours is 2.5% or less by mass; a layer formed from a resin material having a thickness of 1.5 to 1.6 mm and an area of 20 × 20 mm has a density of 300 g / m 2 The adhesive strength of the expanded body obtained by heating a test piece laminated with a polyester nonwoven fabric of the above at 800°C is 1.0 kgf or more; the shape of the expanded body is sheet-like and has a thickness of 0.5 mm to 2.0 mm; the shape of the expanded body is paste or paint-like; and the expanded body is intended to be installed in a window frame or door frame.
[0011] As another embodiment, the present invention relates to a method for producing a thermally expandable vinyl chloride resin material, the method comprising the steps of: using 50 to 150 parts by mass of thermally expandable graphite having an expansion start temperature of 180 to 240°C relative to 100 parts by mass of the vinyl chloride resin; and further using a dehydrochlorination catalyst for promoting dehydrochlorination of the vinyl chloride resin at the expansion start temperature, a dehydrochlorination inhibiting compound for inhibiting dehydrochlorination, and a plasticizer for the vinyl chloride resin, the method comprising the steps of: producing a thermally expandable vinyl chloride resin material containing these compounds; heating a sample A having a blend of 52 parts by mass of a vinyl chloride resin having an average polymerization degree of 400 to 3000, 42.8 parts by mass of dioctyl phthalate as a plasticizer for the resin, and 5.2 parts by mass of the dehydrochlorination catalyst at 180°C for 15 minutes and then at 190°C for 15 minutes; and % by mass or more, and the amount of the dehydrochlorination catalyst to be added per 100 parts by mass of the vinyl chloride resin is determined so that a sample B prepared by adding 52 parts by mass of a vinyl chloride resin having an average degree of polymerization of 400 to 3000, 42.8 parts by mass of dioctyl phthalate as a plasticizer for the resin, and a desired amount of the dehydrochlorination catalyst per 100 parts by mass of the vinyl chloride resin having an average degree of polymerization of 400 to 3000 is subjected to heating at 180°C for 15 minutes and then at 190°C for 15 minutes, and further the dehydrochlorination inhibitor compound is a compound having an amino group and / or an ammonium group that has a function of inhibiting the catalytic function of the dehydrochlorination catalyst at an initial heating temperature of 160 to 240°C.
[0012] In a preferred embodiment of the method for producing a thermally expandable vinyl chloride resin material of the present invention, the compound having an amino group and / or an ammonium group is at least any one selected from the group consisting of melamine polyphosphate, melamine-melam-melem polyphosphate, melamine phosphate, melamine metal polyphosphate, piperazine phosphate, ethylenediamine phosphate, melamine sulfate, melamine, melam, melem, melamine cyanurate, benzoguanamine, silane-coated ammonium polyphosphate, melamine-coated ammonium polyphosphate, urea and ammonium chloride. Effect of the Invention
[0013] According to the present invention, a thermally expandable polyvinyl chloride resin material is provided, in which the expanded body obtained by heating and expanding at 800°C (hereinafter also referred to as "thermally expandable body") exhibits higher caking power, is more excellent in shape retention and mechanical strength, and can more effectively exhibit a flame and smoke blocking function from a low temperature range. Moreover, according to a preferred embodiment of the present invention, a thermally expandable polyvinyl chloride resin material is provided, which has excellent water resistance even when the formed product such as a thermally expandable sheet is used facing outdoors and exposed to rainwater, and has better flame and smoke blocking performance in all cases in which the product is used in various environments. The above-mentioned excellent thermally expandable polyvinyl chloride resin material provided by the present invention is not limited to a sheet form, but can be made into a paste form, for example, to be used as a putty that can be filled in an open space, or as a paint, which can be applied to metal or wooden pillars and walls, or applied to electric wires, etc., to become a useful thermally expandable body that exhibits higher caking power, is more excellent in shape retention and mechanical strength after expansion, and can form a thermally expandable covering, etc., making it possible to provide various useful products. [Brief description of the drawings]
[0014] [Figure 1] 1 is a graph showing the relationship between heating time and weight loss when a thermal expansion sheet according to an embodiment of the present invention and a thermal expansion sheet according to a comparative example are heated to 160° C. [Diagram 2] 1 is a graph showing the relationship between heating time and weight loss when a thermal expansion sheet according to an embodiment of the present invention and a thermal expansion sheet according to a comparative example are heated to 190° C. [Diagram 3] 1 is a graph showing the relationship between heating time and weight loss when a thermal expansion sheet according to an embodiment of the present invention and a thermal expansion sheet according to a comparative example are heated to 220° C. [Figure 4] 1 is a graph showing the relationship between heating time and weight loss when a thermal expansion sheet according to an embodiment of the present invention and a thermal expansion sheet according to a comparative example are heated to 240° C. [Diagram 5]FIG. 1 is a graph showing test results showing the expansion ratio when heated to 200° C. to 800° C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described in detail below with reference to preferred embodiments of the present invention. In the process of further studying the thermally expandable vinyl chloride resin material, which is based on vinyl chloride resin and is compounded with a plasticizer for the resin, thermally expandable graphite, and ammonium polyphosphate as a flame retardant, the inventors of the present invention have found the following problem to be solved by applying a product made of the resin material to window frames and the like and studying its use under various assumed actual use environments. That is, the inventors have found that a thermally expandable sheet formed from a conventional resin material loses weight in the sheet or covering due to rainwater in an outdoor environment, and in some cases, this can cause problems in preventing fire spread, and further study is required in order to stably supply higher quality products. The inventors recognized that the problem of water resistance of products used as fire spread prevention materials is important, and that it is urgent to improve this point in order to stably provide higher quality products.
[0016] The present inventors first conducted intensive research into the poor water resistance of products (hereinafter simply referred to as "products") made of conventional thermally expandable polyvinyl chloride resin materials, and found that the component causing the poor water resistance of the product was ammonium polyphosphate used as a flame retardant in the resin material. Ammonium polyphosphate is a highly stable compound that does not hydrolyze even when dissolved in water, exists in a molecular state, and is widely used as a flame retardant. In addition, when used as a flame retardant, the higher the polymerization degree of ammonium polyphosphate, the higher the flame retardant effect. The polymerization degree of commercially available products is 100 to 500, and in some cases, some have a polymerization degree of over 1000. On the other hand, it is said that the higher the polymerization degree, the lower the solubility, and when the polymerization degree exceeds 20, the solubility drops sharply, and when added as a flame retardant, it is generally considered that there is no problem with water resistance.
[0017] However, in the course of investigating the composition of a resin material that would become a thermally expandable body with a higher binding strength, the inventors discovered that when the thermally expandable polyvinyl chloride resin materials proposed thus far were used as products, they sometimes exhibited poor water resistance, and that the cause of this was the ammonium polyphosphate used as a flame retardant. They realized that in order to provide a stable, high-quality product, this point needed to be investigated.
[0018] Specifically, the inventors applied a product made of a thermally expandable polyvinyl chloride resin material, which is based on a polyvinyl chloride resin and is blended with a plasticizer for the resin, thermally expandable graphite, a dehydrochlorination catalyst, and ammonium polyphosphate as a flame retardant, to window frames and the like, and conducted research under various assumptions of actual usage environments. As a result, it was found that when placed in a harsh environment exposed to rainwater, etc., the appearance of sheets, coverings, etc. may change, which may impair the fire spread prevention function, and further research on thermally expandable polyvinyl chloride resin materials is required to enable stable supply of high-quality products in any of a variety of environments. That is, the present invention was made in consideration of the importance of developing a thermally expandable polyvinyl chloride resin material that is environmentally adaptable and that not only has a thermally expandable body that has a higher caking power and excellent shape retention and mechanical strength, but also allows the product to be water-resistant in harsh environments.
[0019] The present inventors first conducted intensive research into the fact that conventional thermally expandable vinyl chloride resin materials may have poor water resistance, and as a result, found that the occurrence of the phenomenon of poor water resistance is related to the type of flame retardant in the resin material, and recognized that in order to improve the quality of the product, it is necessary to thoroughly study the flame retardant used. Then, in the process of studying various components used as flame retardants, the present inventors found that, among the components having the function of a flame retardant, an amino group-containing compound having an amino group and / or an ammonium group-containing compound having an ammonium group in its structure is used in combination with the dehydrochlorination catalyst proposed by the present inventors in the technology disclosed above, the product can be made to have a higher caking power than that previously achieved by the thermally expandable body, and further, the range of the above-mentioned compounds that can be applied is wide, and if the compound is selected in consideration of water resistance, it is possible to provide a product with excellent water resistance. The present inventors believe that the reason for the above-mentioned effect is as follows. Below, the background to the invention will be explained, and the remarkable effect obtained by the configuration of the invention will be explained.
[0020] The present inventors have conducted research from an unprecedented perspective in developing a material in which the thermally expandable body can exhibit a better fire spread prevention function, and as a result, have found the existence of a dehydrochlorination catalyst that can effectively exhibit a flame and smoke blocking function in a low temperature range in a thermally expandable polyvinyl chloride resin material containing a polyvinyl chloride resin, a plasticizer for said resin, and thermally expandable graphite, and that makes the thermally expandable body exhibit high caking power, excellent shape retention, and excellent mechanical strength, and have proposed this technology. Details of this technology are described in Patent Document 2 cited above. That is, as specified in the present invention, this dehydrochlorination catalyst is a substance that exhibits a large weight loss in a low temperature range when sample A, which is a blend of 52 parts by mass of vinyl chloride resin having an average degree of polymerization of 400 to 3000, 42.8 parts by mass of dioctyl phthalate as a plasticizer for the resin, and 5.2 parts by mass of the dehydrochlorination catalyst, is heated at 180°C for 15 minutes and then at 190°C for 15 minutes, and the weight loss of the sample A is 25% by mass or more. Representative examples of the dehydrochlorination catalyst include, for example, metallic zinc, zinc oxide, zinc carbonate, zinc chloride, copper, copper oxide, and iron chloride. Note that the sample A is for evaluating the effect of the dehydrochlorination catalyst and does not contain a flame retardant.
[0021] By using these dehydrochlorination catalysts, the thermally expandable polyvinyl chloride resin material containing them undergoes a significant weight loss of the polyvinyl chloride resin in the low temperature range of 170 to 240°C, and dehydrochlorination (polyenation) and carbonization are promoted, so that the final thermally expandable body exhibits high caking power and is excellent in shape retention and mechanical strength. However, the proposal in Patent Document 2 does not conduct detailed studies on the flame retardant to be used, and ammonium polyphosphate is used as in the past.
[0022] In response to this, the present inventors found that the ammonium polyphosphate added as a flame retardant was the cause of the poor water resistance of the product, and in order to improve this point, they added various flame retardants to a resin material consisting of a base vinyl chloride resin (containing a plasticizer), thermally expandable graphite, and a dehydrochlorination catalyst exhibiting the above-mentioned function, and conducted tests. As a result, they surprisingly found that when a dehydrochlorination catalyst exhibiting the above-mentioned function is used, by combining a compound having a specific structural feature, the caking force of the thermally expandable body is further improved. In addition, there are many types of compounds having specific structural features that can achieve this surprising effect, as found by the present invention, and by selecting the type, it is possible to configure a thermally expandable vinyl chloride resin material that can improve the water resistance of the product in addition to the high caking force of the thermally expandable body, so that the thermally expandable vinyl chloride resin material of the present invention can provide a variety of products with higher performance and excellent applicability to harsh environments.
[0023] The present inventors believe that the reason why the thermally expandable vinyl chloride resin material of the present invention has a higher caking power and is more excellent is as follows. In vinyl chloride resin, dehydrochlorination is usually promoted at high temperatures of 240°C to 800°C, and it eventually becomes a carbonized material through a hard cured state. On the other hand, thermally expandable graphite expands according to temperature when it reaches the expansion start temperature, regardless of the composition. Here, when a dehydrochlorination catalyst that causes a significant weight loss of vinyl chloride resin in the low temperature range of 170 to 240°C is used, the progress of curing of vinyl chloride resin and the expansion of thermally expandable graphite, which has an expansion start temperature of 180 to 240°C, occur in the same temperature range, so that the vinyl chloride resin is entangled in the expanded part of the graphite and carbonized with dehydrochlorination, resulting in a thermally expandable material with a large caking power.
[0024] In contrast, when a dehydrochlorination catalyst is not used, the dehydrochlorination of the polyvinyl chloride resin is insufficient in the temperature range where the expansion of the thermally expandable graphite begins. In this way, when the expansion of the graphite is completed while the resin is in a softened state, it is considered that the binding force of the thermally expandable body cannot be supported because the resin is not sufficiently entangled. This is supported by the fact that, in conventional products that do not use a dehydrochlorination catalyst, the thermally expandable body is clearly inferior in binding force compared to when a dehydrochlorination catalyst is used, and it is not possible to make it excellent in shape retention and mechanical strength.
[0025] The present inventors have further studied the above-mentioned conventional techniques with the aim of realizing a higher quality product, as described above. First, if the curing of the resin proceeds quickly before the expansion of the thermally expandable graphite begins, the resin will naturally remain as a solid residue, but the thermally expandable body will not be sufficiently covered with the carbonized resin, and will not have a high caking force. This means that the presence of a dehydrochlorination catalyst that effectively promotes the dehydrochlorination of the vinyl chloride resin is absolutely necessary. Furthermore, the present inventors considered that in order to obtain a more optimal thermally expandable body that can effectively exhibit the flame and smoke blocking function, it is important to appropriately adjust the dehydrochlorination of the vinyl chloride resin promoted by the dehydrochlorination catalyst, the progress state in which the resin finally becomes a carbonized product via a hard cured state, and the expansion speed of the thermally expandable graphite. More specifically, they considered that it is necessary to adjust the progress speed in which the vinyl chloride resin finally becomes a carbonized product, promoted by the above-mentioned dehydrochlorination catalyst, and the expansion speed of the thermally expandable graphite. In contrast, since the dehydrochlorination of vinyl chloride resins is said to proceed in a zipper-like manner, the above idea can be rephrased as follows: at low temperatures up to the expansion starting temperature range of thermally expandable graphite, it is necessary to suppress the function of the dehydrochlorination catalyst added to promote the zipper-like progression, that is, to use in combination with a compound that suppresses the function.
[0026] Therefore, the inventors of the present invention conducted a study by changing the flame retardant, which is believed to be the causative component of the poor water resistance of the product that triggered the invention, in various ways, focusing on the behavior of suppressing the function of the dehydrochlorination catalyst used in combination at low temperatures up to the expansion start temperature range of thermally expandable graphite. As mentioned above, phosphorus-based flame retardants are generally used as flame retardants. It is also known that a highly effective flame retardant effect can be obtained by using phosphorus-based flame retardants in combination with nitrogen-based flame retardants. In the idea of intumescent flame retardants, that is, forming a foamed layer of carbonized (char) on the burning surface, the phosphorus-based flame retardant generates carbonized (char), and the nitrogen-based flame retardant generates nitrogen-based gas, which causes the carbonized layer to foam, thereby exerting a synergistic effect.
[0027] Based on the above, the inventors conducted a study test using a wide range of flame retardants consisting of compounds containing phosphorus and / or nitrogen in the presence of the dehydrochlorination catalyst specified in the present invention. As a result of the study, it was found that the combined use of a phosphorus-based flame retardant and a nitrogen-based flame retardant is not an essential factor for increasing the caking strength of the thermally expandable body. Then, it was found that the caking strength of the thermally expandable body can be further increased by the combined use of an amino group-containing compound and / or an ammonium group-containing compound, not by the intumescent effect, and this led to the present invention.
[0028] Specifically, the thermally expandable vinyl chloride resin material of the present invention is characterized in that it is made of a vinyl chloride resin as a base resin, a plasticizer for the resin, thermally expandable graphite having an expansion start temperature of 180 to 240 ° C, and a dehydrochlorination catalyst for the vinyl chloride resin as specified in the present invention, and further comprises an amino group-containing compound and / or an ammonium group-containing compound having a function of suppressing the catalytic function of the dehydrochlorination catalyst. By being configured in this way, the thermally expandable vinyl chloride resin material of the present invention suppresses the progress of dehydrochlorination of the vinyl chloride resin in the low temperature range of 180 to 240 ° C, which is the expansion start temperature of the thermally expandable graphite, despite the use of a dehydrochlorination catalyst that promotes dehydrochlorination. On the other hand, at high temperatures, it becomes possible to effectively proceed with dehydrochlorination, so that a product with better performance can be provided. The thermally expandable vinyl chloride resin material of the present invention, which utilizes the combination of the above-mentioned substances, can more effectively exhibit a flame and smoke blocking function even in the low temperature range, and the thermally expandable body thereof exhibits a higher caking force and has better shape retention and mechanical strength. In addition, by selecting and using an amino group-containing compound and / or an ammonium group-containing compound that are particularly poorly soluble in water as the dehydrochlorination inhibitor compound in the above-mentioned combination of substances, a new effect is obtained in that products such as thermally expandable sheets made of the obtained resin material have excellent water resistance. Specifically, it is possible to realize a product with excellent water resistance in which the amount of elution when the product is immersed in hot water at 95°C for 24 hours is 2.5% or less by mass.
[0029] The effect of the dehydrochlorination inhibiting compound constituting the present invention, an amino group-containing compound and / or an ammonium group-containing compound having the function of inhibiting the catalytic function of a dehydrochlorination catalyst (hereinafter, sometimes simply referred to as a dehydrochlorination inhibiting compound), on the caking strength of the thermally expandable material will be described in detail later, but the inventors believe that the compound reacts with hydrochloric acid generated during dehydrochlorination promoted by the dehydrochlorination catalyst used in combination, thereby inhibiting rapid polyenization.
[0030] In the present invention, as the dehydrochlorination catalyst specified in the present invention, a dehydrochlorination catalyst was appropriately selected based on the difference in the effect on dehydrochlorination between metal powder and metal compounds described in the above-mentioned Patent Document 2, and a combustion test was performed at high temperature (800°C) in a system in which thermally expandable graphite having an expansion start temperature of 180 to 240°C and a dehydrochlorination inhibiting compound were blended with a polyvinyl chloride resin. The caking force of the thermally expandable body after the combustion test was measured to investigate the effect of using the dehydrochlorination inhibiting compound in combination.
[0031] First, in the course of the study, a test was carried out on the use and non-use of ammonium polyphosphate, which was used as a flame retardant in the technology described in Patent Document 2. As a result, it was surprisingly found that even if a metal compound or the like exhibiting the effect of the dehydrochlorination catalyst defined in the present invention is present, the caking force of the thermally expandable body is not good when ammonium polyphosphate is not added. On the other hand, even if ammonium polyphosphate is present, the caking force of the thermally expandable body is insufficient when a metal compound exhibiting the effect of the dehydrochlorination catalyst is not added. As a result, it was found that in order to improve the caking force of the thermally expandable body, it is clearly necessary for the metal compound or the like exhibiting the effect of the dehydrochlorination catalyst and ammonium polyphosphate to coexist.
[0032] As a result of further investigation, the inventors discovered that it is important to use a dehydrochlorination catalyst in combination with not only ammonium polyphosphate but also an amino group-containing compound and / or an ammonium group-containing compound so that these components coexist during heating, and thus arrived at the present invention. Specifically, as a result of the following investigation, it was found in the above-mentioned test that the contribution of the use of ammonium polyphosphate to the improvement of the caking power of the thermally expandable body is due to the ammonium group in its structure, and further investigation was conducted based on this knowledge, leading to the achievement of the present invention.
[0033] Instead of ammonium polyphosphate, which was used as the flame retardant in the above-mentioned study, various flame retardants that are generally used as similar flame retardants were used and the following results were obtained. In the test using metal polyphosphate compounds, the effect was small, while in the test using melamine-coated polyphosphate and melamine-melam-melem polyphosphate, good effects were shown, similar to those of ammonium polyphosphate. In addition, melamine sulfate, benzoguanamine, and melamine cyanurate, which do not contain phosphorus, also showed good effects. Furthermore, surprisingly, ammonium chloride, an inorganic salt, also showed good effects. On the other hand, phosphazene, phosphate ester, and methylol melamine, which does not contain amino groups, and methylol melamine, which has methylolated amino groups, did not show good results in improving the caking power. Details of these study results will be described later.
[0034] In order to clarify the reason why the above-mentioned phenomenon occurs, the present inventors added the above-mentioned various phosphorus-based flame retardants and nitrogen-based flame retardants in the presence of zinc oxide, which exhibits catalytic effect as a dehydrochlorination catalyst, and measured the weight loss at each of the temperatures of 160°C, 190°C, 220°C, and 240°C, which are the expansion start temperature ranges of thermally expandable graphite. The results are shown in Figures 1 to 4.
[0035] As a result, when the compounds having amino groups, melamine-coated polyphosphate, melamine-melam-melem polyphosphate, melamine sulfate, benzoguanamine, and melamine cyanurate, which have an amino group and show an effect of improving the caking power of the thermally expandable body, were present, the weight loss curves over time were gentle at each temperature, as shown in Figures 1 to 4. This was the opposite result to the weight loss value after dehydrochlorination when ammonium polyphosphate was not present, as mentioned above. On the other hand, the compounds having no amino groups, such as phosphazene, phosphoric acid ester, and methylol melamine having amino groups, which do not show a significant effect on improving the caking power of the thermally expandable body, showed large weight loss curves at 160°C and 190°C. At the higher temperatures of 220°C and 240°C, most of the compounds showed simple weight loss curves.
[0036] As mentioned above, the dehydrochlorination of vinyl chloride resins is said to have a strong zipper effect, and there are many references on this, as listed below. For example, "Sakura Yamada, PVC and Polymers, 20, (12), (1980)" and "Mitsuo Onozuka, Polymers, 13, (8), (1964)" are included. Dehydrochlorination is promoted by electrophilic compounds such as zinc chloride and tin chloride, and the generated hydrochloric acid further acts as a catalyst. Various stabilizers are known to stop this zipper effect. P. Simon et al. have reported a dynamic study based on metal stearates, and have described the effects of Mg and Pb. References include "P. Simon et al., PVC and Polymers, 31, (9), (1991)" and "P. Simon et al., PVC and Polymers, 31, (10), (1991)". Since stabilizers react with dehydrochlorination, they are thought to inevitably inhibit dehydrochlorination while the added stabilizers are reacting and consumed. For example, there is a report on the use of dibutyltin maleate as a stabilizer (see, for example, Kagawa et al., Tosoh Research Report, 12, (1998)).
[0037] The above results of the investigation have revealed that in order to produce a better thermally expandable polyvinyl chloride resin material with a thermally expandable body having a stronger caking power, it is essential that the composition of the material includes, in addition to the presence of a dehydrochlorination catalyst having a strong dehydrochlorination effect, an amino group-containing compound and / or an ammonium group-containing compound which, when added, inhibits dehydrochlorination in the temperature range where the thermally expandable graphite begins to expand and has the effect of promoting weight loss at temperatures above this temperature range, in other words, which functions as a dehydrochlorination inhibiting compound.
[0038] Furthermore, in order to make the thermal expansion sheet or other products excellent in water resistance, this can be easily achieved by selecting a compound that is poorly soluble in water, which has a very low solubility in water, from among the amino group-containing compounds and / or ammonium group-containing compounds. The components constituting the present invention are described below.
[0039] <Dehydrochlorination inhibiting compounds (amino group-containing compounds and ammonium group-containing compounds)> The thermally expandable vinyl chloride resin material of the present invention can form a thermally expandable sheet having a certain thickness by utilizing the comma coat molding method. In addition, the thermally expandable sheet obtained is foamed (expanded) by heat to form a thermally expandable body that is more resistant to collapse, is not easily blown away by the pressure of a flame, and has excellent shape retention. According to the study by the present inventors, these effects are clearly different from those when other flame retardants are used, and are superior in terms of effectiveness. According to the study by the present inventors, it has been confirmed that the superiority of the effect of using an amino group-containing compound and / or an ammonium group-containing compound as a constituent component in the thermally expandable vinyl chloride resin material of the present invention is brought about by the fact that a useful synergistic effect is obtained by using the compound in combination with a component that functions as a dehydrochlorination catalyst as specified in the present invention. In other words, in the thermally expandable vinyl chloride resin material of the present invention, the amino group-containing compound and the ammonium group-containing compound are used not simply as flame retardants, but as dehydrochlorination inhibitor compounds for the dehydrochlorination catalyst used in combination.
[0040] Specific examples of the dehydrochlorination inhibiting compound constituting the present invention include ammonium polyphosphate, melamine polyphosphate, melamine-melam-melem polyphosphate, melamine phosphate, melamine polyphosphate metal salts, piperazine phosphate, ethylenediamine phosphate, melamine sulfate, melamine, melam, melem, melamine cyanurate, benzoguanamine, silane-coated ammonium polyphosphate, melamine-coated ammonium polyphosphate, urea, and ammonium chloride.
[0041] The amount of the dehydrochlorination inhibiting compound added is preferably 50 to 150 parts by mass, more preferably 70 to 100 parts by mass, per 100 parts by mass of the vinyl chloride resin. If the amount is too small, the flame retardant effect and the shape retention effect during expansion are not achieved, whereas if the amount is too large, molding of the resin material tends to become difficult and the expansion coefficient decreases, which is undesirable.
[0042] <Dehydrochlorination catalyst> As mentioned above, the dehydrochlorination catalyst constituting the present invention is described in detail in the above-mentioned Patent Document 2. Specific examples include metallic zinc, zinc oxide, zinc carbonate, zinc chloride, copper, copper oxide, and iron chloride, and any of these can be suitably used. However, the catalyst is not limited to these, and any substance can be used as long as it causes a weight loss of 25% by mass or more when sample A specified in the present invention is heated at 180°C for 15 minutes and then at 190°C for 15 minutes. In addition, if the blending ratio is too low, the effect of improving flame retardancy cannot be expected, and if it is too high, the viscosity of the resin material increases, making it difficult to blend, which is not preferable. From these points of view, , Books Regarding sample B specified in the invention As will be described later, The temperature may be appropriately determined within a range in which the weight loss of sample B is 25% by mass or more after heating at 180° C. for 15 minutes and then at 190° C. for 15 minutes.
[0043] <Vinyl chloride resin> The vinyl chloride resin constituting the thermally expandable vinyl chloride resin material of the present invention may be (1) a vinyl chloride homopolymer, or (2) a vinyl chloride copolymer which is a copolymer of vinyl chloride and a monomer having an unsaturated bond copolymerizable with vinyl chloride and contains 50 mass% or more of vinyl chloride.
[0044] Examples of monomers having an unsaturated bond copolymerizable with vinyl chloride include vinyl esters such as vinyl acetate and vinyl propionate; acrylic acid, methacrylic acid; acrylic acid esters such as methyl acrylate and ethyl acrylate; methacrylic acid esters such as methyl methacrylate and ethyl methacrylate; olefins such as ethylene and propylene; acrylonitrile; aromatic vinyls such as styrene; and vinylidene chloride.
[0045] The average degree of polymerization of the vinyl chloride resin used in the present invention is not particularly limited, but is preferably 400 to 3,000, and more preferably 1,000 to 2,000. If the average degree of polymerization is less than 400, the mechanical properties of the resulting molded product may be poor. If the average degree of polymerization is more than 3,000, the melt viscosity of the vinyl chloride resin during molding may increase, making molding difficult. If the molding temperature is increased to reduce the melt viscosity, the vinyl chloride resin may decompose, making it difficult to obtain a good molded product. The thermally expandable vinyl chloride resin material of the present invention preferably has a viscosity of 5000 to 20000 mPa·sec at 25° C., depending on the molding method. The vinyl chloride resin may be used alone or in combination of two or more types.
[0046] <Plasticizer> The thermally expandable vinyl chloride resin material of the present invention contains a plasticizer for the resin. Examples of the plasticizer include phthalic acid derivatives (particularly phthalic acid esters) such as bis(2-ethylhexyl)phthalate, diisononyl phthalate, diisodecyl phthalate, ditridecyl phthalate, and mixed phthalic acid esters of higher alcohols; trimellitic acid derivatives (particularly trimellitic acid esters) such as tris(2-ethylhexyl)trimellitate, tri(n-octyl)trimellitate, and triisooctyl trimellitate; adipic acid derivatives (particularly adipic acid esters) such as bis(2-ethylhexyl)adipate, diisononyl adipate, diisodecyl adipate, and mixed adipic acid esters of higher alcohols; bis(2-ethylhexyl)azelate, diisooctyl adipate, and mixed adipic acid esters of higher alcohols; Azelaic acid derivatives (particularly azelaic acid esters) such as ethyl azelate and di-(n-hexyl) azelate; sebacic acid derivatives (particularly sebacic acid esters) such as bis(2-ethylhexyl) sebacate and diisooctyl sebacate; sulfonic acid derivatives (particularly sulfonic acid esters) such as phenol-based alkylsulfonic acid esters; epoxy derivatives (particularly epoxidized esters) such as epoxidized soybean oil and epoxidized linseed oil; polyester-based plasticizers which are polymerized esters of dicarboxylic acids such as adipic acid, azelaic acid, sebacic acid, and phthalic acid with dihydric alcohols such as ethylene glycol, propylene glycol, and butylene glycol, etc., can be used. Among these plasticizers, high molecular weight plasticizers are preferred in terms of migration, extractability, bleeding, etc. Note that the plasticizers may be used alone or in combination of two or more.
[0047] The amount of the plasticizer is about 10 to 100 parts by mass, preferably about 20 to 80 parts by mass, based on 100 parts by mass of the vinyl chloride resin. If the amount is less than 10 parts by mass, the melt viscosity is high, the moldability when forming a sheet-like product is poor, and the molded body is brittle and easily broken, which is not preferable. On the other hand, if the amount is more than 100 parts by mass, the flame retardancy of the molded body is reduced and the amount of smoke generated during combustion is increased, which is not preferable.
[0048] <Thermal expandable graphite> The thermally expandable graphite constituting the thermally expandable vinyl chloride resin material of the present invention is, for example, when placed in a space such as a window frame as a thermally expandable sheet, a foaming component that causes the sheet to expand due to a rise in temperature during a fire, etc. Thermally expandable graphite is obtained by inserting a compound between the layers of naturally occurring flake graphite to neutralize it, and the compound contained therein generates a gas when exposed to heat, which results in the expansion of the flake graphite.
[0049] According to the study by the inventors, the ratio of thermally expandable graphite to the vinyl chloride resin is not an important factor, but if it is too much, the density of the expanded body after thermal expansion becomes low, and if it is too much, the expansion ratio is small and it does not play a role in preventing the spread of fire. The expansion ratio is calculated as the ratio of the vertical height of the expanded body after heating at 800°C to the thickness before the test, and is preferably 10 times or more to 40 times or less. In order to obtain this range, in the present invention, the blending amount of thermally expandable graphite is set to 50 to 150 parts by mass per 100 parts by mass of the vinyl chloride resin.
[0050] It is preferable that the powder of naturally occurring flake graphite is treated with an inorganic acid such as concentrated sulfuric acid, nitric acid, selenic acid, etc., or an organic acid such as acetic acid, formic acid, etc., or a strong oxidizing agent such as concentrated nitric acid, perchloric acid, perchlorates, permanganates, dichromates, hydrogen peroxide, etc. The graphite treated as described above is preferably neutralized with, for example, ammonia, aliphatic lower amines, alkali metal compounds, alkaline earth metal compounds, etc.
[0051] In order to prevent the spread of fire in the early stages of a fire, it is necessary for the thermally expandable graphite to start expanding at a low temperature. Therefore, when a low-temperature expandable graphite with an expansion start temperature of 180 to 240°C is used, it is considered that the vinyl chloride resin becomes entangled in the expanding thermally expandable graphite like a reinforcing material, and it is possible to obtain a thermally expandable vinyl chloride resin material having a performance that can effectively exhibit a flame and smoke blocking function from a low temperature range. Therefore, the thermally expandable sheet provided by the present invention exhibits a fire spread prevention effect at an early stage of the initial stage of a fire.
[0052] The thermally expandable graphite used in the present invention preferably has an average particle size in the range of 100 to 600 μm, more preferably in the range of 120 to 500 μm. When the average particle size falls within this range, the graphite has good expandability, workability, and shape retention.
[0053] As described above, the amount of thermally expandable graphite added is about 50 to 150 parts by mass, and more preferably 70 to 100 parts by mass, relative to 100 parts by mass of the vinyl chloride resin. If the amount is too small, the flame retardant effect due to expansion is not sufficiently obtained, and if the amount is too large, molding of the resin material becomes difficult and shape retention during foaming (expansion) becomes poor.
[0054] <Other optional ingredients> (Heat stabilizer) When molding the vinyl chloride resin material of the present invention, it is preferable to add a heat stabilizer to suppress thermal decomposition. As the heat stabilizer, for example, Pb-based or Sn-based, Ba / Zn composite, Ca / Zn composite, or other heat stabilizers generally used for rigid vinyl chloride resins can be used. These heat stabilizers may be used alone or in combination of two or more. In addition, the amount of the heat stabilizer added is about 0.1 to 10 parts by mass, more preferably about 0.5 to 5 parts by mass, relative to 100 parts by mass of the vinyl chloride resin.
[0055] (Modifier) In addition, in order to improve moldability and physical properties when forming a thermally expandable sheet using the thermally expandable vinyl chloride resin material of the present invention, modifiers such as acrylic processing aids, acrylonitrile-butadiene-styrene copolymers (ABS resins), methyl methacrylate-butadiene-styrene copolymers (MBS resins), acrylic polymers, and chlorinated polyethylene may be added to the resin material within a range that does not impair the effects of the present invention.
[0056] (foaming agent) Furthermore, in order to increase the foaming property (expansion property), an auxiliary foaming agent may be added, for example, an azo compound such as azodicarbonamide, a hydrazine compound such as 4,4'-oxybis(benzenesulfonylhydrazide), a nitroso compound such as N,N'-dinitrosopentamethylenetetramine, or a bicarbonate such as sodium hydrogen carbonate.
[0057] In the present invention, it is possible to use a filler made of an inorganic compound other than those specified in the present invention in combination, if necessary, within the scope of not impairing the effects of the present invention. In such a case, however, it is preferable to keep the amount added small.
[0058] Examples of other inorganic fillers that can be added as necessary include conventionally known fillers such as those listed below. For example, metal oxides such as alumina, titanium oxide, calcium oxide, magnesium oxide, iron oxide, tin oxide, antimony oxide, and ferrites; hydrated inorganic substances such as calcium hydroxide, magnesium hydroxide, aluminum hydroxide, and hydrotalcite; metal carbonates such as basic magnesium carbonate, calcium carbonate, magnesium carbonate, zinc carbonate, strontium carbonate, and barium carbonate; calcium salts such as calcium sulfate, gypsum fiber, and calcium silicate; silica, diatomaceous earth, dawnnite, barium sulfate, talc, clay, malic acid, and the like. Examples of suitable materials include squid, montmorillonite, bentonite, activated clay, sepiolite, imogolite, sericite, glass fibers, glass beads, silica-based balloons, aluminum nitride, boron nitride, silicon nitride, carbon black, graphite, carbon fibers, carbon balloons, charcoal powder, various metal powders, potassium titanate, magnesium sulfate, lead zirconate titanate, aluminum borate, molybdenum sulfide, silicon carbide, stainless steel fibers, zinc borate, various magnetic powders, slag fibers, fly ash, and dewatered sludge.
[0059] <Method of manufacturing thermally expandable polyvinyl chloride resin material> The method for producing a thermally expandable vinyl chloride resin material of the present invention uses 50 to 150 parts by mass of thermally expandable graphite having an expansion start temperature of 180 to 240°C relative to 100 parts by mass of vinyl chloride resin, and further uses a dehydrochlorination catalyst for promoting dehydrochlorination of the vinyl chloride resin at the expansion start temperature, a dehydrochlorination inhibitor compound for inhibiting dehydrochlorination, and a plasticizer for the vinyl chloride resin to produce a thermally expandable vinyl chloride resin material. As described above, the type of substance to be the dehydrochlorination catalyst and the amount of addition thereof are selected as specified in the present invention, and a compound having an amino group and / or an ammonium group that has the function of inhibiting the catalytic function of the dehydrochlorination catalyst at an initial heating temperature of 160 to 240°C is used as the dehydrochlorination inhibitor compound to be used in combination with the dehydrochlorination catalyst.
[0060] (Method of preparing resin material) The thermally expandable vinyl chloride resin material of the present invention can be obtained by kneading the above-mentioned essential components of the present invention and optional components added as necessary, using a kneading device such as a dissolver mixer or a kneader mixer. Kneading is preferably performed so that the temperature of the resin material in the kneading device is 20 to 50°C. Depending on the method for molding the thermally expandable sheet thereafter, for example, when molding the thermally expandable sheet by the comma coat molding method, it is necessary to make the thermally expandable vinyl chloride resin material into a suitable paste state, so it is preferable to adjust the viscosity at 25°C to about 5000 to 20000 mPa·sec. This resin material can be used as a putty by adding a solvent to make it into a paste state. In addition, it can be used as a paint (coating agent) by using an appropriate amount of a solvent that has affinity for vinyl chloride resin. Examples of solvents that have affinity for vinyl chloride resin include tetrahydrofuran and toluene.
[0061] <Method of molding thermal expansion sheet> The thermally expandable vinyl chloride resin material of the present invention can be easily molded into a thermally expandable sheet, for example, by utilizing a simple comma coat molding method. A sheet of an appropriate thickness can be easily obtained by coating a paste-like thermally expandable vinyl chloride resin material on a substrate (base paper) having mold releasability. The thermally expandable sheet of the present invention is preferably about 0.5 mm to 2.0 mm, and can be easily obtained by using the thermally expandable vinyl chloride resin material of the present invention and applying the comma coat molding method. At this time, unlike the case of producing a thermally expandable sheet by extrusion molding or calendar molding, there is no need to melt the resin material with heat and pressure, so the problem of shrinkage when the sheet is cooled, which occurs in these methods, is suppressed, and a uniform sheet in good condition can be obtained.
[0062] (Thermal expansion sheet) The thermally expandable sheet obtained by the thermally expandable vinyl chloride resin material of the present invention can be easily obtained by comma coat molding of the thermally expandable vinyl chloride resin material described above. The thermally expandable sheet of the present invention expands by heating to an expansion temperature (usually 180°C) or higher, for example, by flame from a gas burner or hot air. The expanded body expanded by heat can not only retain its shape by itself, but also has sufficient mechanical strength to block flames and smoke. Therefore, by using the thermally expandable sheet of the present invention in the window frame (for example, between the sash and the wall) of a building such as a house or a building, the molded body can hold the window glass without burning even in the event of a fire, and can prevent the flame from spreading to the back side. The thermally expandable sheet of the present invention can also be used in applications requiring fire resistance such as gaps in fire doors or other places where fire prevention is required.
[0063] The measurement of the adhesive strength of the expanded body after the high-temperature combustion test at 800°C used to evaluate the function of the thermally expandable polyvinyl chloride resin material of the present invention was performed by our own method, without any official method. Specifically, a sample with a thickness of 1.5 to 1.6 mm and a surface area of 20 mm x 20 mm was prepared from the thermally expandable polyvinyl chloride resin material, and this was heated at 800°C. A smooth plate was pressed down on the top of the expanded body obtained using a compression tester or the like, and the maximum resistance measured from the bottom to a height of 8 mm was expressed in kgf. EXAMPLES
[0064] Next, the present invention will be described in more detail with reference to the following examples, examples, and comparative examples. The present invention is not limited to these examples. In the text, "parts" and "%" are based on mass unless otherwise specified.
[0065] The main components used in the study examples, examples, and comparative examples are as follows. The zinc oxide and iron chloride used in the dehydrochlorination catalyst are both commercially available as reagents. The substances used to determine whether they are dehydrochlorination inhibitors will be described later. ·Vinyl chloride resin The vinyl chloride resin used was Ryuron Paste 772A (product name) manufactured by Tosoh Corporation, which has an average degree of polymerization of 1,650. Hereinafter, this may be abbreviated as PVC. Plasticizers Dioctyl phthalate (Sanso Cizer DOP (product name), manufactured by New Japan Chemical Co., Ltd.), a plasticizer for vinyl chloride resin, was used. Hereinafter, it may be abbreviated as DOP. Thermally expandable graphite The thermally expandable graphite used was SYZR802 (product name) manufactured by Sanyo Trading Co., Ltd., which has an expansion start temperature of 180° C. and an average particle size of 180 μm. Heat stabilizer The heat stabilizer used was a Zn / Ca composite, specifically LX-550 manufactured by Daikyo Kasei Co., Ltd.
[0066] [Study Example 1] - Example of how to select a dehydrochlorination catalyst As shown in Table 1, thermally expandable polyvinyl chloride resin materials were prepared by using thermally expandable graphite and ammonium polyphosphate, a typical flame retardant, and blending this with zinc oxide or calcium carbonate. Figure 5 shows a graph of the expansion ratio when the two types of blends prepared above were heated to 800°C. From Figure 5, it can be seen that in both compositions, expansion begins at 200°C, the expansion start temperature of the thermally expandable graphite, and foaming progresses rapidly, and the foaming speed decreases from temperatures of about 500 to 600°C.
[0067] TIFF0007562085000001.tif60170
[0068] On the other hand, the two types of thermally expandable polyvinyl chloride resin materials prepared were used to measure the binding strength by the following method, and the binding strength was high at 1.22 kgf when zinc oxide was added, while it was low at 0.38 kgf when calcium carbonate was added. Here, zinc oxide is a substance that causes a weight loss of 45% by mass (residual amount % is 55%) of sample A, which is a blend of 52 parts by mass of polyvinyl chloride resin, 42.8 parts by mass of plasticizer, and 5.2 parts by mass of zinc oxide as a dehydrochlorination catalyst, as specified in the present invention, when the sample A is heated at 180°C for 15 minutes and then at 190°C for 15 minutes. On the other hand, calcium carbonate is a substance that hardly loses weight in the low temperature range, which is the expansion initiation temperature of thermally expandable graphite, when sample A having a composition defined in the present invention, in which 5.2 parts by mass of calcium carbonate is added to 52 parts by mass of polyvinyl chloride resin and 42.8 parts by mass of plasticizer, is heated at 180°C for 15 minutes and then at 190°C for 15 minutes, the weight loss of sample A is 3% by mass (residual content is 97%).
[0069] These facts show that the caking force of the thermally expandable body can be increased by using a compound that causes a large weight loss of sample A, such as zinc oxide. In the present invention, such a substance is called a dehydrochlorination catalyst. Details on this point are described in the above-mentioned Patent Document 2. As described in the Patent Document 2, the caking force of the thermally expandable body can be increased by using a compound that causes a large weight loss of sample A, such as the above-mentioned zinc oxide, as a dehydrochlorination catalyst. Other substances include, for example, metallic zinc, zinc carbonate, zinc chloride, and iron chloride, but the present invention is not limited to these substances, and any substance can be used as long as it is a substance that corresponds to the weight loss of sample A specified in the present invention.
[0070] The above-mentioned caking force was measured by preparing a sheet-like sample with a thickness of 1.5 to 1.6 mm and a surface area of 20 x 20 mm from the thermally expandable polyvinyl chloride resin material obtained above, heating this at 800°C to expand it, placing a smooth plate on the top of the resulting thermally expandable body, and pressing down on the plate with a compression testing machine until the plate was 8 mm high from the bottom. The maximum resistance force was measured in kgf.
[0071] [Study Example 2] - Study to find dehydrochlorination inhibitor compounds For the thermally expandable polyvinyl chloride resin material of basic formulation C shown in Table 2, which was prepared by using zinc oxide as a dehydrochlorination catalyst and adding various amino group-containing compounds and ammonium group-containing compounds shown in Table 4 as dehydrochlorination inhibitor compounds, the caking strength of the thermally expandable body of each resin material was measured to confirm the effect of adding these compounds on the caking strength of the thermally expandable body. Zinc oxide and iron chloride were used as representative examples of dehydrochlorination catalysts. Table 2 shows the formulation when zinc oxide is used, and the following explanation will be given taking the case of zinc oxide as an example.
[0072] TIFF0007562085000002.tif61170
[0073] The reason why zinc oxide was used as the dehydrochlorination catalyst in the above blend C and why the amount of zinc oxide was 11.1 parts per 100 parts of the base polyvinyl chloride resin is that zinc oxide is a substance that causes a weight loss of 45% by mass (residual amount % is 55%) of sample A specified in the present invention when heated at 180°C for 15 minutes and then at 190°C for 15 minutes, and is a substance that causes a high caking force of the thermal expandable body. The amount of zinc oxide added was determined based on the value obtained by heating sample B, which is made of 52 parts by mass of vinyl chloride resin and 42.8 parts by mass of plasticizer, and further contains a desired amount of dehydrochlorination catalyst per 100 parts by mass of vinyl chloride resin, at 180°C for 15 minutes and then at 190°C for 15 minutes, within the range where the weight loss of sample B is 25% by mass or more. Table 3 shows the relationship between the amount of zinc oxide added and the weight loss in sample B.
[0074] TIFF0007562085000003.tif55170
[0075] Using the basic formulation C shown in Table 2, solutions were prepared by varying the type of compound to be examined in order to find the dehydrochlorination inhibitor compound specified in the present invention, and each of the solutions obtained was coated on a release paper to a thickness of 1.5 to 1.6 mm. Furthermore, a 450 g / m2 density film was applied to the surface of the coating solution. 2 Next, the laminates were prepared by heating the laminates in a hot air drying oven at 190 to 195°C for 3 to 5 minutes, and the release paper was peeled off to prepare test samples.
[0076] The laminate samples obtained above were each cut into a size of 20 x 20 mm to be used as samples to be heated. The thickness of the laminate sample was measured before heating. The laminate sample was heated at 800°C, and the expansion ratio and caking strength of the thermally expanded body obtained after heating and expansion were measured by the following method.
[0077] The expansion ratio of each resin material was calculated by measuring the vertical height of the thermally expanded body obtained above, and calculating the vertical height of the expanded body after the test / thickness before the test. The binding strength of the thermally expanded body was measured by heating and expanding each laminate sample obtained above at 800°C, placing a smooth plate on the top of the thermally expanded body, and pressing down the plate with a compression tester. The maximum resistance force measured from the bottom to a height of 8 mm was expressed in kgf. The results are shown in Table 4.
[0078] Each laminate sample obtained above was cut into a size of 5×10 mm to prepare a sample for the elution test, and the weight of each sample was measured. Five samples were then immersed in 100 g of purified water and left at 95° C. for 24 hours to conduct the elution test. After the test, the samples were removed from the hot water and dried at 95° C. for 3 hours, and the weight after drying was measured. The amount of elution due to hot water was calculated from the weight before immersion in hot water and the weight after drying, and the weight loss ratio compared to before immersion was expressed in % to be the water resistance. The results are shown in Table 4.
[0079] The overall evaluation results are shown in Table 4, and the criteria are as follows: ⊚: The caking force of the thermally expandable body is 1.0 kgf or more, and the weight loss rate, which indicates water resistance, is 2.5% or less. ◯: The caking force of the thermally expandable body is 1.0 kgf or more, and the weight loss rate indicating water resistance is more than 2.5% and 7.5% or less. △: The caking force of the thermally expandable body is 1.0 kgf or more, and the weight loss rate indicating water resistance is more than 7.5%. ×: The caking force of the thermally expanded body is less than 1.0 kgf.
[0080] TIFF0007562085000004.tif190170
[0081] As shown in Table 4, it was confirmed that the caking power of the thermally expandable body is clearly higher when a compound containing an amino group or an ammonium group in its structure is added than when a compound without these groups is used. Also, as shown in Table 4, when melamine is used, the expansion ratio is very high, and it was found that when a compound with an amino group structure is used, a high caking power can be achieved despite the very high expansion ratio of the thermally expandable body. From this, the inventors expect that the caking power of the thermally expandable body when melamine having an amino group in its structure is used in combination with a dehydrochlorination catalyst such as zinc oxide will be even higher if the expansion ratio can be kept at the same level as other compounds.
[0082] In the case of methylol melamine, which is a melamine that does not have an amino group in its structure, a high caking strength cannot be achieved in the thermally expandable body. This shows the remarkable effect of using a dehydrochlorination catalyst such as zinc oxide in combination with the "compound having an amino group and / or an ammonium group" defined in the present invention. As shown in Table 2, the compounds that were judged to have excellent water resistance in the resin material and high caking strength in the thermally expandable body in the overall judgment were melamine polyphosphate, melam, melem, melamine cyanurate, and melamine polyphosphate. The compounds that, when used in combination with a dehydrochlorination catalyst such as zinc oxide, showed high caking strength in the thermally expandable body but slightly inferior water resistance in the resin material were ammonium polyphosphate, melamine sulfate, benzoguanamine, melamine, and silane-coated ammonium polyphosphate. It was confirmed that the caking strength of the thermally expandable body can be increased compared to the conventional case by using a dehydrochlorination catalyst in combination with the "compound having an amino group and / or an ammonium group" defined in the present invention, although the resin material had inferior water resistance. This means that although there are restrictions on where it can be used, such as it must not be exposed to rainwater, etc., if this point is kept in mind, it can be used as a fire prevention material that expands with heat in the event of a fire, slowing the spread of the fire.
[0083] [Study Example 3] - Confirmation of the effect of using a dehydrochlorination catalyst in combination with a "compound having an amino group and / or an ammonium group" In the basic blend C used in Study Example 2, 3.0 parts of zinc oxide or 3.0 parts of iron chloride were used as a dehydrochlorination catalyst for 27.0 parts of PVC, and 20 parts of ammonium polyphosphate, melamine, etc. were used as a "compound having an amino group and / or an ammonium group" to prepare a thermally expandable polyvinyl chloride resin material. In this example, thermally expandable polyvinyl chloride resin materials were prepared without these compounds or with only one of them, and evaluated. The evaluation was performed by measuring the expansion ratio of the resin material and the binding force of the thermally expandable body in the same manner as described above. Table 5 shows the differences in the blends and the measurement results.
[0084] TIFF0007562085000005.tif59170
[0085] [Study Example 4] - Verification test of the effect of combined use with dehydrochlorination inhibitor compound The test samples obtained by peeling off the release paper prepared in Study Example 2 were cut to a predetermined size of 20 x 20 mm to prepare test pieces, and the weights of the test pieces obtained were measured. Then, each test piece was placed in a hot air dryer to measure the heat loss. Specifically, the temperature in the hot air dryer was set to 160°C, 190°C, 220°C, and 240°C, which are temperatures that are assumed to be the rising part of the expansion start temperature range of thermally expandable graphite, and weight measurements were performed every 10 minutes for 60 minutes to determine the remaining amount rate (%), and the results were graphed in Figures 1 to 4. Surprisingly, in the results shown in Figures 1 and 2, especially in the results of heating at low temperatures of 160°C and 190°C, it was confirmed that the thermally expandable polyvinyl chloride resin material containing "amino group-containing compounds and / or ammonium group-containing compounds" that showed a large value for the caking strength of the thermally expandable body in the results shown in Table 2 above showed a high residual amount, while additives that did not have either amino or ammonium groups in their structure, which showed a low caking strength of the thermally expandable body, showed a rapid decrease in residual amount over heating time. In contrast to the above, as shown in Figures 3 and 4, when the temperature reached 220°C and 240°C, a monotonous weight loss curve was shown in both cases.
[0086] These results appear to contradict the results of the method for selecting a dehydrochlorination catalyst in Study Example 1, which stated that a substance that loses weight significantly when heated at low temperatures has the effect of increasing the caking power of the thermally expandable body. However, considering the results shown in Figures 1 to 4 and the effect of adding a dehydrochlorination catalyst obtained in Study Example 3, the inventors of the present invention make the following inference.
[0087] In order to increase the caking power of the thermally expanded body, it is necessary for the vinyl chloride resin components to sufficiently cling to the thick fibrous graphite expansion body that appears in accordance with the expansion of the graphite. If the weight loss is too rapid in the expansion start temperature range, that is, if the dehydrochlorination proceeds too rapidly, it is considered that the clinging effect of the resin components will be difficult to occur. In contrast, as shown in Figures 1 and 2, it is inferred that the presence of "amino group-containing compounds and / or ammonium group-containing compounds" that have the function of suppressing the catalytic function of the dehydrochlorination catalyst captures the hydrochloric acid that is generated when the dehydrochlorination proceeds too rapidly, thereby preventing the zipper effect.
[0088] From the results of Figures 3 and 4, it is believed that as the temperature rises thereafter, once the rapid rise in expansion has passed, the catalytic effect of dehydrochlorination becomes more dominant than the effect of inhibiting dehydrochlorination. Alternatively, it is believed that the amino and ammonium groups absorb all the hydrochloric acid generated and lose their zipper inhibition effect. Then, at temperatures beyond this point, the dehydrochlorination catalyst works sufficiently to advance the carbonization of the polyvinyl chloride resin. At this stage, the resin components are already attached to the expanded fiber, so the carbonization proceeds while binding together, which is believed to have created good caking power. The above is an inference from the phenomenon obtained, and has not yet been fully elucidated.
[0089] [Study Example 5] - Confirmation of the effect on the caking strength of the thermally expandable body when changing the amount of amino group-containing compound added to Blend C TIFF0007562085000006.tif47170
[0090] From the results in Table 6, it was confirmed that the more parts of the amino group-containing compound added, the greater the caking power of the thermally expandable body. It was also found that the amount added was nearly saturated at 15 to 20 parts. If the amount was more than 20 parts, the processing characteristics deteriorated, so the amount is preferably about 20 parts.
[0091] If the contribution of amino group-containing compounds to the caking strength is due to the removal of hydrochloric acid generated by dehydrochlorination catalysts such as zinc oxide from the system, it will be affected by the number of amino groups contained in the compound. Although it is not clear from Table 6, the effect on the caking strength of the thermally expandable body, which is probably caused by the number of parts added, is based on this, and it is presumed that when the hydrochloric acid absorption of amino groups is saturated, the self-catalysis of hydrochloric acid also begins to work and adds to the effect of the dehydrochlorination catalyst.
[0092] [Study Example 6] - Confirmation of the effect on the viscosity of the thermally expandable body when the amount of the amino group-containing compound added in Blend C is kept constant and the amount of zinc oxide added is changed TIFF0007562085000007.tif46170
[0093] From the results in Table 7, it was confirmed that the caking power increases as the amount of zinc oxide added increases. In the case of this composition, it was confirmed that it saturates at about 75% of the standard. This phenomenon shows the same tendency as Table 3, which shows the relationship between the amount of zinc oxide added and the residual amount after heating (%), and indicates the existence of a saturation amount.
Claims
1. a vinyl chloride resin, a plasticizer for the resin, and 50 to 150 parts by mass of thermally expandable graphite having an expansion starting temperature of 180 to 240°C per 100 parts by mass of the vinyl chloride resin; a thermally expandable vinyl chloride resin material that does not use ammonium polyphosphate, the thermally expandable vinyl chloride resin material comprising at least one component selected from the group consisting of metallic zinc, zinc oxide, zinc carbonate, zinc chloride, and iron chloride in an amount such that a weight loss of the sample is 25% by mass or more after heating a sample obtained by adding a desired amount of the component to 52 parts by mass of a vinyl chloride resin having an average degree of polymerization of 400 to 3000, 42.8 parts by mass of dioctyl phthalate as a plasticizer for said resin, and 100 parts by mass of the vinyl chloride resin having an average degree of polymerization of 400 to 3000 at 180°C for 15 minutes and then at 190°C for 15 minutes; The thermally expandable vinyl chloride resin material further comprises at least one selected from the group consisting of melamine polyphosphate, melamine melam melem polyphosphate, and melamine cyanurate in an amount of 50 to 150 parts by mass per 100 parts by mass of the vinyl chloride resin.
2. a vinyl chloride resin, a plasticizer for the resin, and 50 to 150 parts by mass of thermally expandable graphite having an expansion starting temperature of 180 to 240°C per 100 parts by mass of the vinyl chloride resin; the composition contains at least one component selected from the group consisting of metallic zinc, zinc oxide, zinc carbonate, zinc chloride, and iron chloride in an amount such that a weight loss of the sample is 25% by mass or more after heating a sample obtained by adding a desired amount of the component to 52 parts by mass of a vinyl chloride resin having an average degree of polymerization of 400 to 3000, 42.8 parts by mass of dioctyl phthalate as a plasticizer for said resin, and 100 parts by mass of the vinyl chloride resin having an average degree of polymerization of 400 to 3000 at 180°C for 15 minutes and then at 190°C for 15 minutes, Furthermore, a thermally expandable vinyl chloride resin material containing no ammonium polyphosphate contains at least one compound having an amino group selected from the group consisting of melamine polyphosphate, melamine melam melem polyphosphate, melamine cyanurate, melamine sulfate, and melamine in an amount of 50 to 150 parts by mass relative to 100 parts by mass of the vinyl chloride resin, A thermally expandable vinyl chloride resin material characterized in that a sample formed from the resin material, having a thickness of 1.5 to 1.6 mm and an area of 20 x 20 mm, is heated at 800°C, and the resulting expanded body has a cohesive strength of 1.0 kgf or more.
3. 3. The thermally expandable vinyl chloride resin material according to claim 1, which is in the form of a sheet, a paste, or a paint.
4. A thermally expandable sheet, characterized in that the thermally expandable vinyl chloride resin material according to claim 1 or 2 is formed into a sheet.
5. The thermally expandable sheet according to claim 4, which is to be installed in a window frame or a door frame.
6. A window frame or door frame comprising the thermally expandable sheet according to claim 4 or 5.
Citation Information
Patent Citations
Semiconductor laser device
JP1984092589A
Thermally expandable vinyl chloride resin composition and molded article thereof
JP4250153B2
Fire-resistant resin composition
WO2016182059A1