All-solid-state battery and method for producing same

A porous support with a conductive coating layer in the electrode structure addresses interfacial resistance and lithium dendrite issues in all-solid-state batteries, improving safety and lifespan by uniformly distributing pressure and lithium deposition.

JP7562208B2Active Publication Date: 2024-10-07LG ENERGY SOLUTION LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022566238
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-21
Filing Date
2021-07-06
Publication Date
2024-10-07
Estimated Expiration
2041-07-06

AI Technical Summary

Technical Problem

Conventional all-solid-state batteries face issues with high interfacial resistance, lithium dendrite growth leading to short circuits, and non-uniform lithium deposition causing stress and deformation, which affect battery safety and lifespan.

Method used

Incorporating a porous support with a conductive coating layer in the electrode structure to uniformly distribute pressure and reduce stress, using materials like polyolefin-based porous substrates and metal oxides to facilitate lithium deposition and stripping.

Benefits of technology

The solution reduces internal stress, prevents micro short circuits, and enhances battery safety and lifespan by maintaining a stable interface and uniform lithium distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562208000005
    Figure 0007562208000005
  • Figure 0007562208000006
    Figure 0007562208000006
  • Figure 0007562208000007
    Figure 0007562208000007
Patent Text Reader

Abstract

The present invention provides an electrode including a porous support and a conductive coating layer formed on at least one surface of the porous support. The electrode may be an anode or a cathode, preferably an anode. The electrode may be used in both all-solid-state batteries and lithium secondary batteries.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority to Korean Patent Application No. 2020-0083066 filed on July 6, 2020, Korean Patent Application No. 2020-0089135 filed on July 17, 2020, and Korean Patent Application No. 2020-0090272 filed on July 21, 2020, and all contents disclosed in the documents of those Korean patent applications are incorporated herein by reference.

[0002] The present invention relates to an all-solid-state battery and a manufacturing method thereof, more particularly to an electrode including a porous support and a conductive coating layer formed on the porous support, an all-solid-state battery including the electrode, and a manufacturing method thereof. [Background technology]

[0003] Lithium-ion secondary batteries have high energy density, low self-discharge rate, and long life, making them suitable for high-capacity batteries. The liquid electrolyte of lithium-ion secondary batteries has safety issues regarding leakage and overheating, and solid-state batteries have been proposed as a solution to these issues. Unlike existing lithium-ion secondary batteries, solid-state batteries can have a solid electrolyte layer containing a solid electrolyte. The solid electrolyte layer is disposed between the positive electrode and the negative electrode and also serves as a separator.

[0004] Since solid-state batteries use solid electrolytes instead of liquid electrolytes, there is no electrolyte evaporation due to temperature changes or leakage due to external impacts. Therefore, they have the advantage of being safe against explosions and fires. As solid-state batteries do not require parts to prevent leakage or explosion, they are also lighter and bulkier.

[0005] Since the solid electrolyte has a limited area where the positive electrode or negative electrode comes into contact, the contact surface is small, and it is difficult to form an interface between the positive electrode or negative electrode and the solid electrolyte layer. If it is difficult to form an interface between the solid electrolyte layer and the positive electrode or negative electrode, a problem occurs in that electrical resistance is high and output is reduced. To solve this problem, a unit cell including a solid electrolyte reduces interface resistance by stacking the positive electrode, the solid electrolyte layer, and the negative electrode and then pressing them together.

[0006] Even in the case of solid-state batteries with improved safety, the problem of lithium dendrites has not yet been solved. Lithium dendrites can grow during the compression and charging / discharging of solid-state batteries. The lithium dendrites can damage the solid electrolyte layer or increase the bulk of the battery.

[0007] Thus, the problem of lithium dendrites is a problem that must still be solved not only in conventional lithium ion secondary batteries but also in all-solid-state batteries.

[0008] FIG. 1 is a schematic diagram of an all-solid-state battery according to the prior art.

[0009] As shown in Fig. 1, a conventional all-solid-state battery includes a positive electrode 10 including a positive electrode current collector 11 and a positive electrode active material layer 12 coated on at least one surface of the positive electrode current collector 11, a solid electrolyte layer 20, and a negative electrode 30 including a negative electrode current collector 31 and a negative electrode active material layer 32 coated on at least one surface of the negative electrode current collector. Unlike Fig. 1, the negative electrode can be formed by a lithium plating and stripping technique using the current collector alone or lithium metal without a separate negative electrode active material layer 32 in order to increase the overall capacity of the all-solid-state battery.

[0010] In the conventional all-solid-state battery, the upper and lower parts of the battery are pressed with a pressing force F to reduce the interfacial resistance between the positive electrode 10, the solid electrolyte layer 20, and the negative electrode 30. When initial charging and discharging is performed while pressing, the active material expands as lithium is inserted into the negative electrode active material, or lithium is deposited on the negative electrode 30, increasing the thickness (z-axis) of the battery, and therefore the pressure inside the battery also increases. When the pressure inside the all-solid-state battery increases, the position and shape of the positive electrode 10, the solid electrolyte layer 20, and the negative electrode 30 inside the all-solid-state battery are deformed. In addition, if the lithium deposited on the negative electrode 30 is not uniform, the pressing force F is not applied uniformly, and the jig that presses from the outside may also be damaged.

[0011] Since the lithium metal used in solid-state batteries is soft, the capacity and performance of the unit cell vary depending on the degree and time of compression. The greater the compression force F, the greater the contact between the solid electrolyte and the lithium metal, and the greater the possibility that the lithium metal will flow into the battery through defects in the solid electrolyte layer, causing a short circuit.

[0012] To solve this, there is a need to evenly distribute or reduce the stress between the lithium metal and the solid electrolyte.

[0013] This problem may also occur in conventional lithium secondary batteries in which the solid electrolyte is replaced with a separator.

[0014] In Patent Document 1, a laminate consisting of a positive electrode, a solid electrolyte layer, and a negative electrode is pressed in order to improve electrical conductivity, electronic conductivity, and lithium ion conductivity, but the document does not recognize the prevention of a cell short phenomenon of a unit cell by reducing the stress applied to the all-solid-state battery.

[0015] Patent Document 2 also presses a laminate consisting of a positive electrode, a solid electrolyte layer, and a negative electrode in order to reduce the interface resistance, but does not recognize the point that the safety of the unit cell is improved by reducing the stress applied to the all-solid-state battery. [Prior art documents] [Patent documents]

[0016] [Patent Document 1] JP 2018-181451 A [Patent Document 2] JP 2019-200890 A Summary of the Invention [Problem to be solved by the invention]

[0017] The present invention aims to solve the above problems and to provide a structure for applying a constant pressure when pressing a lithium secondary battery or an all-solid-state battery to form an interface, and to distribute or reduce the internal stress of the lithium secondary battery or the all-solid-state battery evenly.

[0018] Another object of the present invention is to provide a lithium secondary battery or an all-solid-state battery that has improved safety, prevents cell shorts, and improves the life span.

[0019] Other objects and advantages of the present invention will become apparent from the following description. Meanwhile, it will be readily apparent that the objects and advantages of the present invention can be realized by the means or methods recited in the claims, and combinations thereof. [Means for solving the problem]

[0020] The present invention provides an electrode including a porous support and a conductive coating layer formed on at least one surface of the porous support. The electrode may be an anode or a cathode, preferably an anode. The electrode may be applicable to both an all-solid-state battery and a lithium secondary battery.

[0021] The porous support includes an elastic material, and the porous support is deformed when pressed, thereby reducing pressure. Here, the pressure may be an internal pressure of the porous support itself, or an external pressure that is reduced by the deformation of the porous support itself.

[0022] The porous support has a large number of pores, and may be a porous polymer film or a porous polymer nonwoven fabric having a plurality of pores and capable of elastic deformation.

[0023] The porous support may include a polyolefin-based porous substrate, or a sheet or nonwoven fabric made from one or more materials selected from the group consisting of glass fiber and polyethylene.

[0024] The porous support may further include at least one of a ceramic, a metal, or a metal alloy in addition to the polymer having a porous structure.

[0025] The porous support may be formed by uniaxial or biaxial stretching.

[0026] The porosity of the porous support may be 10% to 90%, preferably 35% to 85%, where porosity is the ratio of voids to the total volume.

[0027] The porous support may have pores with a diameter of 0.01 μm to 10 μm.

[0028] The porous support has an elastic deformation rate due to compression of 30% or less. Here, the elastic deformation rate due to compression can be calculated by (thickness before compression - thickness under a pressure of 20 MPa) / thickness before compression x 100%.

[0029] The porous support may have a thickness retention rate due to pressing of 70% or more. Here, the thickness retention rate due to pressing may be calculated by (thickness after pressing / thickness before pressing)×100%. Here, the thickness after pressing may be the thickness under a pressing pressure of 20 MPa.

[0030] The thickness of the porous support before pressing may be 5 μm to 300 μm.

[0031] When pressed, the porous support may have a reduced thickness in the pressing direction and an increased area in a direction perpendicular to the pressing direction.

[0032] The electrode is preferably a negative electrode, and the negative electrode includes the conductive coating layer and a negative electrode active material layer. The negative electrode active material layer may be formed by plating on the conductive coating layer during a charging process of the battery, and may be stripped from the surface of the conductive coating layer during a discharging process of the battery.

[0033] The conductive coating layer may be a conductive material, preferably a metal or a metal oxide, coated on the surface of the porous support or on the surfaces of pores formed inside the porous support.

[0034] The conductive coating layer may include a metal having electrical conductivity, and more specifically, may be at least one of a metal powder and a metal oxide.

[0035] The conductive coating layer may include a lithium affinity material, and non-limiting examples of the lithium affinity material may be one or more selected from the group consisting of metals including Au, Ag, Fe, Mg, Al, Ti, Cr, Ni, Cu, Zn, In, Sn, Pt, Co, Mn, Li, Bi, and Si, and metal oxides including CuO, ZnO, MnO, and CoO.

[0036] The conductive coating layer may have a thickness of 100 nm to 5 μm.

[0037] The present invention also provides a lithium secondary battery including the electrode as a negative electrode.

[0038] The present invention also provides an all-solid-state battery including the electrode as a negative electrode.

[0039] The all-solid-state battery may be an all-solid-state battery including a positive electrode, a negative electrode, and a solid electrolyte layer interposed between the positive electrode and the negative electrode.

[0040] The conductive coating layer may be disposed on an opposite surface of the solid electrolyte layer.

[0041] The solid electrolyte layer includes a solid electrolyte, and the solid electrolyte is 10 -7 The electrolyte has an ion conductivity of at least S / cm, and may include a polymer-based solid electrolyte, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or a mixture of two or more of these.

[0042] The present invention also provides a method for manufacturing an all-solid-state battery, the method including: (S1) forming a laminate including a positive electrode, a solid electrolyte layer, and a negative electrode; (S2) pressing the laminate; and (S3) charging the pressed laminate while pressing the laminate, wherein at least one of the negative electrodes is a porous support having a conductive coating layer formed on one surface thereof.

[0043] The present invention also provides a method for producing a lithium secondary battery, in which the solid electrolyte layer in the method for producing an all-solid-state battery is replaced with a separator.

[0044] The steps (S2) and (S3) may be performed in reverse order or simultaneously, and the charging step (S3) may include providing a negative electrode active material layer on the conductive coating layer.

[0045] The conductive coating layer may be formed by depositing the conductive coating layer on one side of the porous support or by laminating the conductive coating layer on one side of the porous support.

[0046] The ratio of the thickness of the porous support before the laminate is pressed to the thickness of the porous support after the laminate is pressed may be 1:0.4 to 1:0.9, and the pressing force may be 20 MPa.

[0047] During or after step (S3), lithium may be deposited between the conductive coating layer used as the negative electrode and the solid electrolyte layer.

[0048] The positive electrode may include a positive electrode active material layer including a metal oxide containing lithium.

[0049] In steps S2) and S3), the porous support is deformed, thereby reducing the pressure applied thereto.

[0050] The positive electrode of the all-solid-state battery or lithium secondary battery may include a porous support on at least one surface.

[0051] The present invention can also provide various combinations of the above technical solutions. Effect of the Invention

[0052] According to an embodiment of the present invention, a battery, specifically a lithium secondary battery or an all-solid-state battery, and a manufacturing method thereof, in which an increase in thickness due to lithium deposition is reduced by using an anode including a porous support, can be provided. The porous support reduces internal stress generated by lithium deposition, thereby suppressing the occurrence of micro shorts, thereby improving the safety of the battery.

[0053] The stress caused by lithium deposition can be relieved by compressing the porous support, thereby suppressing physical changes in lithium in the battery that is not in a charging / discharging state. In addition, the problem of lithium deposited growing during charging / discharging and damaging the separator or solid electrolyte layer can be reduced, thereby improving the life characteristics of the battery.

[0054] According to one embodiment of the present invention, lithium released from the positive electrode during charging is plated on the conductive coating layer, and the deposited lithium itself can be used as the negative electrode active material layer without a separate negative electrode active material layer. In addition, the deposited lithium can be stripped during discharging. Therefore, the initial battery does not include a separate negative electrode active material layer.

[0055] In addition to charging and discharging, lithium, which has physically soft properties, grows as a positive electrode along the interfaces (grain boundaries) or voids between solid electrolyte particles in solid-state batteries, suppressing micro-short circuits that occur, thereby improving the life characteristics of solid-state batteries.

[0056] In addition, the lithium can be prevented from growing along the pores of the separator or penetrating the separator, thereby improving the life characteristics of the lithium secondary battery. [Brief description of the drawings]

[0057] [Figure 1] FIG. 1 is a schematic diagram of an all-solid-state battery according to the prior art. [Diagram 2] FIG. 2 is a schematic diagram illustrating a structure of a negative electrode according to an embodiment of the present invention. [Diagram 3] 1 is a schematic diagram illustrating a structure of a negative electrode including a negative electrode active material layer according to an embodiment of the present invention. [Figure 4] FIG. 1 is a schematic diagram of an all-solid-state battery according to an embodiment of the present invention. [Diagram 5] FIG. 2 is a schematic diagram of an all-solid-state battery according to an embodiment of the present invention after charging and pressing. [Figure 6]1 is a graph showing thickness retention rates of porous supports due to pressing in Examples 1-1, 1-2, 1-3, and Comparative Example 1-1. [Figure 7] 1 is a photograph taken before and after pressing of a porous support according to Example 1-1. [Figure 8] 1 is a photograph taken before and after pressing of a porous support according to Example 1-1. [Figure 9] 1 is a photograph taken before and after pressing the support according to Comparative Example 1-1. [Figure 10] 1 is a photograph taken before and after pressing the support according to Comparative Example 1-1. [Figure 11] 1 is a SEM photograph of the surface of a negative electrode current collector according to Example 2-3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0058] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings, which are provided to enable a person having ordinary skill in the art to which the present invention pertains to easily carry out the present invention. However, in describing the operation principle of the preferred embodiment of the present invention in detail, detailed description of related well-known functions or configurations will be omitted if it is determined that such detailed description may unnecessarily obscure the gist of the present invention.

[0059] In addition, the same reference numerals are used throughout the drawings for parts having similar functions and actions. Throughout the specification, when a part is said to be connected to another part, this includes not only the case where the part is directly connected to another part, but also the case where the part is indirectly connected via another element between the two parts. In addition, when a part includes a certain component, it does not mean that the other component is excluded, but that the part may further include the other component, unless otherwise specified.

[0060] Furthermore, descriptions that limit or add specific elements are applicable to all inventions and are not limited to a particular invention unless otherwise specified.

[0061] Furthermore, throughout the present specification, the singular includes the plural unless otherwise specified.

[0062] In addition, throughout the specification of the present invention, unless otherwise specified, "or" includes "and." Therefore, "including A or B" means three cases: including A, including B, or including both A and B.

[0063] Furthermore, all numerical ranges include the endpoints and all intermediate values ​​therebetween unless expressly stated to the contrary.

[0064] In addition, the terms "approximately," "substantially," and the like used throughout this specification are used to mean a numerical value or a value close to that value when manufacturing and material tolerances inherent in the referred meaning are presented, and are used to prevent unscrupulous infringers from unfairly using disclosure content that refers to exact or absolute numerical values ​​to aid in the understanding of the present invention.

[0065] Throughout this specification, the term "combinations thereof" in a Markush form expression means a mixture or combination of one or more selected from the group of elements set forth in the Markush form expression, and is meant to include one or more selected from the group of elements.

[0066] The present invention relates to an electrode, preferably a negative electrode, comprising a porous support and a conductive coating layer formed on at least one surface of the porous support, and a lithium secondary battery or an all-solid-state battery comprising the electrode.

[0067] For convenience, only the negative electrode will be described below as including a porous support and a conductive coating layer formed on at least one surface of the porous support, but this can also be applied to the positive electrode. The lithium secondary battery or all-solid-state battery according to the present invention can use at least one of the positive electrode and the negative electrode having the structure according to the present invention.

[0068] The all-solid-state battery according to the present invention will be specifically described below.

[0069] In the anode used in solid-state batteries, graphite-based materials can be used as the anode active material. When graphite-based materials are used as the anode active material, high interfacial resistance occurs between the graphite-based material and the solid electrolyte layer. The only way to reduce this interfacial resistance is to increase the number of interfaces, but in the process, the content of the anode active material decreases, which ultimately leads to a low energy density.

[0070] The use of Si, Sn, etc. as the negative electrode active material has the advantage of being able to increase the energy density compared to using graphite-based materials. However, Si, Sn, etc. have a large volume expansion rate, making it difficult to maintain contact with the solid electrolyte. As a result, the performance of the all-solid-state battery decreases.

[0071] 1, when lithium metal itself is used as the anode or a current collector is used alone to manufacture a battery with high energy density and high power output, lithium is deposited between the anode and the solid electrolyte layer during the charge and discharge process of the battery, which increases the internal stress of the electrode assembly and causes abnormal behavior.

[0072] In order to solve these problems, the present inventors aim to provide a new concept negative electrode for an all-solid-state battery.

[0073] Specifically, the all-solid-state battery according to an embodiment of the present invention includes a porous support and a conductive coating layer as a negative electrode current collector in a negative electrode, as shown in Fig. 2. Referring to Fig. 2, the negative electrode 300 according to an embodiment of the present invention includes a porous support 310 and a conductive coating layer 320 disposed on the porous support.

[0074] According to an embodiment of the present invention, the porous support can reduce the problem of expansion of the negative electrode due to lithium deposition. In addition, the volume of the initial porous support is reduced by lithium deposition, and as a result, it can function as a thin film current collector. Therefore, the energy density can be increased. The porous support can eliminate stress caused by lithium deposition, thereby suppressing physical changes in lithium in a battery that is not in a charge / discharge state. The problem of the deposited lithium growing and damaging the solid electrolyte layer during the charge / discharge process can be reduced. Therefore, the life characteristics of the battery are improved.

[0075] As described above, the negative electrode according to an embodiment of the present invention may use the porous support and the conductive coating layer formed on the porous support as a negative electrode current collector.

[0076] The negative electrode may include the negative electrode current collector and a negative electrode active material layer, as shown in Fig. 3. Referring to Fig. 3, a negative electrode 300 according to an embodiment of the present invention includes negative electrode current collectors 310 and 320 and a negative electrode active material layer 330.

[0077] Here, the negative electrode active material layer is formed by plating on the negative electrode current collector during a charging process of the battery, and is stripped from the surface of the negative electrode current collector during a discharging process of the battery.

[0078] That is, in the present invention, the evaporated lithium generated during the charge and discharge process of the battery can be used as the negative electrode active material layer.

[0079] (porous support) In a specific embodiment of the present invention, the porous support may be any material that does not interfere with the operation of the battery, has a plurality of pores, and is capable of elastic deformation. For example, the porous support may be a porous polymer film substrate, a porous polymer nonwoven fabric substrate, a mesh, or a porous foam, which has a plurality of pores and is capable of elastic deformation.

[0080] In order to more effectively perform the role of reducing pressure by being deformed when pressure is applied, the porous support may be made of a material that has approximately the same thickness after pressure is applied and that is largely deformed when pressure is applied, i.e., an elastic material.

[0081] The elastic material can be, for example, one or more selected from the group consisting of high density polyethylene, low density polyethylene, linear low density polyethylene, ultra-high molecular weight polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyether ether ketone, polyether sulfone, polyphenylene oxide, polyphenylene sulfide, polyethylene naphthalene, and combinations thereof.

[0082] In a specific embodiment of the present invention, the porous polymer nonwoven fabric substrate may be formed from a polymer selected from the group consisting of polyolefin, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, and polyethylene naphthalene, either alone or in combination.

[0083] A polymer nonwoven fabric substrate that has porosity but is not elastically deformable does not correspond to the porous substrate applicable to the present invention.

[0084] Since the porous support is made of an elastic material, the porous support can be deformed by the pressure applied to the battery, thereby dispersing or reducing the stress applied to the negative electrode.

[0085] The porous support may be made of a material similar to that used in the separator of the lithium secondary battery or the solid electrolyte layer of the all-solid-state battery. The porous support may include an olefin-based porous substrate including chemically resistant and hydrophobic polypropylene, or a sheet or nonwoven fabric made of at least one selected from the group consisting of glass and polyethylene. The olefin-based porous substrate used in the porous support is a polyolefin-based porous substrate used in the separator of a secondary battery, which does not have inorganic coating layers added to both sides, and may be, for example, polyethylene or polypropylene.

[0086] The porous support may have a nonwoven structure or a porous structure formed by uniaxial or biaxial stretching. The porous support may have pores with a diameter of 0.01 μm to 10 μm. The porosity of the porous support may be 10% to 90%, preferably 35% to 85%. For example, the porosity may be 35% or more, 40% or more, or 45% or more, and 85% or less, 80% or less, or 75% or less. Since the porous support has an appropriate elastic force within the above numerical range, it can eliminate stress generated during charging and discharging. The porous support has a minimum thickness deformation rate that can absorb stress within the above numerical range, and has an elastic force that can recover after lithium deposition and stripping within the above range.

[0087] Here, the porosity is the ratio of the void space to the total volume. As described above, when a porous support has many fine pores, the stress generated inside the battery can be reduced by reducing the size or number of the pores, even if the structure of the porous support does not change significantly.

[0088] In addition, the porous support according to the present invention may have a thickness before pressing of 5 μm to 300 μm, preferably 5 μm to 100 μm, in order to efficiently reduce the stress generated inside the battery. More specifically, the thickness of the porous polymer support may be 5 μm or more, 10 μm or more, or 20 μm or more, and 100 μm or less, 80 μm or less, or 50 μm or less. This numerical range is advantageous in terms of minimizing the reduction in energy density and obtaining the effect of relieving stress. If the thickness of the porous support is too small, the internal stress of the battery cannot be reduced, and if the thickness is too large, it is not preferable because the performance relative to the size of the battery is reduced.

[0089] When the porous support has a large number of pores and is made of an elastic material, the pores are smaller or the number of pores is reduced compared to when only an elastic material is used, and thus the change in the position or shape of the porous support is reduced, so that stress reduction within the battery can be more effectively achieved. In addition, the pores can easily return to their original state when pressure is removed due to the elastic force.

[0090] Furthermore, when the porous support is made of the same or similar material as the separator of a lithium secondary battery or the solid electrolyte layer of an all-solid-state battery, it has an advantage that the unit cells can be stacked without a separate separator or insulating material.

[0091] The porous polymer of the porous support may further include at least one of ceramic, metal, or metal alloy. Therefore, by including ceramic, metal, or metal alloy in the porous support, the porous support may function as an anode together with the anode current collector layer. In this case, a separate conductive coating layer according to the present invention may not be necessary. However, in this case, when stacking unit cells, a separate separator or insulating material may be necessary.

[0092] In one embodiment of the present invention, lithium ions released from the positive electrode may be deposited on the negative electrode current collector. To this end, the negative electrode current collector has porosity. In addition, since the porous support is elastically deformable, when the deposited lithium forms a negative electrode active material layer between the conductive coating layer and the solid electrolyte layer, the thickness may be reduced. That is, the porous support may be compressed. Thus, the stress generated by the deposited lithium may be reduced.

[0093] For example, the thickness of the porous support can be controlled to reduce stress caused by some or all of the amount of lithium deposited. For example, if the amount of lithium deposited by charging the battery is less than 1 mAh / cm2 for the positive electrode, the thickness of the porous support can be controlled to reduce stress caused by some or all of the amount of lithium deposited by the positive electrode. 2 When loaded at 10 ...

[0094] For this reason, in a specific embodiment of the present invention, the porous support may have an elastic deformation rate due to compression of 30% or less, where the elastic deformation rate due to compression can be calculated by (thickness before compression - thickness under a pressure of 20 MPa) / thickness before compression x 100%.

[0095] In a specific embodiment of the present invention, the porous support may have a thickness retention rate due to pressing of 70% or more. Here, the thickness retention rate due to pressing may be calculated by (thickness after pressing / thickness before pressing)×100%. Here, the thickness after pressing may be a thickness under a pressing pressure of 20 MPa.

[0096] Since the porous support has elasticity, even if lithium is plated between the negative electrode and the solid electrolyte layer during charging of the battery, the volume of the substrate can be reduced by the volume of the plated lithium, thereby reducing the expansion of the negative electrode due to lithium deposition.

[0097] When the porous support is deformed, it can be deformed in the thickness direction, in width, or both simultaneously.

[0098] In addition, the porous support may have fine irregularities on its surface to strengthen the bonding force with the separator or solid electrolyte layer.

[0099] (Conductive coating layer) The conductive coating layer is formed by coating a metal on the surface of the porous support or on the surfaces of pores formed inside the porous support. The conductive coating layer allows the porous support to function as a current collector. From the perspective of battery operation, it is preferable to form a layer by coating only the surface of the porous support. However, during the metal coating process, the metal may also be coated on some of the surfaces of the pores formed inside the porous support. As another embodiment, the conductive material of the conductive coating layer may be uniformly distributed within the porous support.

[0100] The conductive coating layer may be coated on the porous support by any method, including, but not limited to, immersion, spin coating, dip coating, spray coating, doctor blade, solution casting, drop coating, physical vapor deposition (PVD), or chemical vapor deposition (CVD).

[0101] That is, the conductive coating layer has electrical conductivity. To this end, the conductive coating layer includes a metal having electrical conductivity. Here, electrical conductivity refers to the property of having electrical conductivity. Specifically, the degree to which a substance or solution can carry an electric charge can be calculated as the reciprocal of resistance, which is a physical quantity.

[0102] The conductive coating layer may include a metal having electrical conductivity, and more specifically, may be at least one of a metal powder and a metal oxide.

[0103] The conductive coating layer may include a lithium affinity material, and non-limiting examples of the lithium affinity material may be at least one selected from the group consisting of metals including Au, Ag, Fe, Mg, Al, Ti, Cr, Ni, Cu, Zn, In, Sn, Pt, Co, Mn, Li, Bi, and Si, and metal oxides including CuO, ZnO, MnO, and CoO.

[0104] In one embodiment of the present invention, the conductive coating layer may have a thickness of 100 nm to 5 μm. More specifically, the conductive coating layer may have a thickness of 100 nm or more, 500 nm or more, or 1 μm or less, and may have a thickness of 5 μm or less, 3 μm or less, or 2 μm or less. This numerical range is advantageous in that it can minimize a decrease in energy density.

[0105] (solid electrolyte layer) In the present invention, the solid electrolyte layer includes a solid electrolyte. In a specific embodiment of the present invention, the solid electrolyte is 10 -7 S / cm or more, preferably 10 -5 The electrolyte has an ion conductivity of S / cm or more, and may include a polymer-based solid electrolyte, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or a mixture of two or more of these.

[0106] In a specific embodiment of the present invention, the solid electrolyte plays a role in transmitting lithium ions in the electrode, so the solid electrolyte is a material having high ionic conductivity, for example, an ionic conductivity of 10 -5 S / cm or more or 10 -4 It can be made of S / cm material.

[0107] In a specific embodiment of the present invention, the polymer-based solid electrolyte may include a solid polymer electrolyte and a lithium salt.

[0108] For example, the solid polymer electrolyte may be one in which a lithium salt is added to a polymer containing a hetero element such as oxygen, nitrogen, or sulfur, so that ions of the dissociated salt can move within the polymer.

[0109] In a specific embodiment of the present invention, the polymer-based solid electrolyte may include a solid polymer electrolyte formed by adding a polymer resin to a solvated lithium salt.

[0110] In a specific embodiment of the present invention, the polymer resin may include a polyether-based polymer, a polycarbonate-based polymer, an acrylate-based polymer, a polysiloxane-based polymer, a phosphazene-based polymer, a polyethylene derivative, an alkylene oxide derivative such as polyethylene oxide, a phosphate polymer, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, a polymer containing an ionically dissociable group, or a mixture of two or more of these.

[0111] In addition, in a specific embodiment of the present invention, the solid polymer electrolyte may include a polymer resin, such as a branched copolymer in which a polyethylene oxide main chain is copolymerized with an amorphous polymer copolymer such as PMMA, polycarbonate, polysiloxane (pdms) and / or phosphazene, a comb-like polymer resin, and a crosslinked polymer resin, or may be a mixture of the above polymers.

[0112] In one embodiment of the present invention, the lithium salt has Li as a cation. + Contains F as an anion - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , AlO4 - , AlCl4 - , PF6 - , SbF6 - , AsF6 - , F2C2O4 - , BC4O8 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , C4F9SO3 -, CF3CF2SO3 - , (CF3SO2)2N - , (F2SO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , and (CF3CF2SO2)2N - It may contain at least one selected from the group consisting of:

[0113] In a specific embodiment of the present invention, the sulfide-based solid electrolyte contains sulfur (S) and may contain a metal belonging to Group 1 or Group 2 of the periodic table, and thus preferably has the ionic conductivity of the metal and electronic insulation.

[0114] In a specific embodiment of the present invention, the sulfide-based solid electrolyte may be a lithium ion conductive solid electrolyte including a compound represented by the following Formula 1: [Formula 1] L a1 M b1 P c1 S d1 A e1 In the formula 1, L represents an element selected from Li, Na, and K, and Li is preferred. M represents an element selected from B, Zn, Sn, Si, Cu, Ga, Sb, Al, and Ge. Among them, B, Sn, Si, Al, and Ge are preferred, and Sn, Al, and Ge are more preferred. A represents I, Br, Cl, and F, and I and Br are preferred, and I is particularly preferred. a1 to e1 represent the composition ratio of each element, and a1:b1:c1:d1:e1 satisfies 1-12:0-1:1:2-12:0-5. Also, a1 is preferably 1-9, and more preferably 1.5-4. b1 is preferably 0-0.5. d1 is preferably 3-7, and more preferably 3.25-4.5. e1 is preferably 0-3, and more preferably 0-1.

[0115] In a specific embodiment of the present invention, the sulfide-based solid electrolyte includes Li, X, and S, and X may include one or more selected from the group consisting of P, Ge, B, Si, Sn, As, Cl, F, and I.

[0116] In a specific embodiment of the present invention, the oxide-based solid electrolyte contains oxygen (O) and may contain a metal belonging to Group 1 or Group 2 of the periodic table, and thus preferably has the ionic conductivity of the metal and electronic insulation.

[0117] In a specific embodiment of the present invention, the oxide-based solid electrolyte includes Li, A, and O, and A may include at least one selected from the group consisting of La, Zr, Ti, AlP, and I.

[0118] In a specific embodiment of the present invention, the average particle size of the sulfide-based or oxide-based solid electrolyte is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.1 μm or more. The upper limit is preferably 100 μm or less, more preferably 50 μm or less. The average particle size of the sulfide-based or oxide-based solid electrolyte particles can be measured by the following method.

[0119] First, prepare a dispersion liquid in which the solid electrolyte particles are dispersed at 1% by mass in water (heptane in the case of substances unstable in water) in a 20 ml sample bottle. After that, irradiate the dispersion liquid with 1 kHz ultrasonic waves for 10 minutes, and use it for testing immediately after that. For the dispersion liquid, use a laser diffraction / scattering type particle size distribution measuring device LA-920 (manufactured by HORIBA) to read data 50 times at a temperature of 25°C using a measurement quartz cell, and obtain the volume average particle size, which is the average particle size. For other detailed conditions, refer to the description in JIS Z8828:2013 "Particle Size Interpretation - Dynamic Light Scattering Method" as necessary.

[0120] The oxide-based solid electrolyte is, for example, Li 6.25 La3Zr2A l0 . 25 O 12, Li3PO4, Li3+xPO4-xN x Sulfides, nitrides, and halides of Li can be used, such as (LiPON), Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, or Li4SiO4-LiI-LiOH.

[0121] The sulfide is not particularly limited in the present invention, and may be any sulfide-based material known in the art for use in lithium batteries. The sulfide-based material may be a commercially available product, or may be prepared by a crystallization process from an amorphous sulfide-based material. For example, the sulfide-based solid electrolyte may be a crystalline sulfide-based solid electrolyte, an amorphous sulfide-based solid electrolyte, or any one or combination of these. Examples of usable composite compounds include sulfur-halogen compounds, sulfur-germanium compounds, and sulfur-silicon sulfides, and may include sulfides such as SiS2, GeS2, and B2S3, and Li3PO4, halogens, halogen compounds, and the like may be added. Preferably, 10 -4 A sulfide-based electrolyte capable of realizing lithium ion conductivity of 100 S / cm or more can be used.

[0122] Representative examples include Li6PS5Cl (LPSCl), Thio-LISICON (Li 3.25 Ge 0.25 P 0.75 S4), Li2S-P2S5-LiCl, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-P2S5, Li3PS4, Li7P3S 11 , LiI-Li2S-B2S3, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiPO4-Li2S-SiS, Li 10 GeP2S 12 , Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 , and Li7P3S11 Includes.

[0123] (positive electrode) The positive electrode to be applied to the present invention is not particularly limited, and may be prepared by a conventional method known in the art in the form of an electrode active material layer attached to an electrode current collector.

[0124] In a specific embodiment of the present invention, the positive electrode may include a current collector and a positive electrode active material layer formed on at least one surface of the current collector, and the positive electrode active material layer may further include a positive electrode active material, a binder, and a conductive material. The positive electrode may include a solid electrolyte. The solid electrolyte may be the same as that described above.

[0125] The positive electrode current collector generally has a thickness of 3 μm to 500 μm. Such a positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can have fine irregularities on its surface to increase the adhesive force of the positive electrode active material, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0126] The positive electrode active material is not particularly limited as long as it is a positive electrode active material that can be used for the positive electrode of an electrochemical element. For example, the positive electrode active material can be LiCoO2, LiNiO2, LiMn2O4, LiCoPO4, LiFePO4, LiNiMnCoO2, and LiNi 1-x-y-z Co x M1 y M2 zO2 (M1 and M2 are each independently any one selected from the group consisting of Al, Ni, Co, Fe, Mn, V, Cr, Ti, W, Ta, Mg, and Mo, and x, y, and z are each independently atomic fractions of oxide composition elements, and 0≦x<0.5, 0≦y<0.5, 0≦z<0.5, x+y+z≦1).

[0127] The solid electrolyte contained in the positive electrode may be a polymer-based solid electrolyte, an oxide-based solid electrolyte, or a sulfide-based solid electrolyte.

[0128] In a specific embodiment of the present invention, the positive electrode active material layer may further include a lithium salt.

[0129] In a specific embodiment of the present invention, the lithium salt has Li as a cation. + Contains F as an anion - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , AlO4 - , AlCl4 - , PF6 - , SbF6 - , AsF6 - , F2C2O4 - , BC4O8 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , C4F9SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (F2SO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH -, CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , and (CF3CF2SO2)2N - It may contain at least one selected from the group consisting of:

[0130] The conductive material is usually added in an amount of 0.1 to 30% by weight based on the total weight of the mixture including the positive electrode active material. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of such conductive materials include graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and summer black; conductive fibers such as carbon fiber and metal fiber; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0131] The binder contained in the positive electrode is a component that helps to bind the active material and conductive material and to bind to the current collector, and is usually added in an amount of 0.1 to 30% by weight based on the total weight of the mixture including the positive electrode active material. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, various copolymers, etc.

[0132] The present invention also provides an all-solid-state battery or a lithium secondary battery including the electrode as a negative electrode.The present invention also provides an all-solid-state battery including the electrode as a negative electrode.The all-solid-state battery may be an all-solid-state battery including a positive electrode, the negative electrode, and a solid electrolyte layer interposed between the positive electrode and the negative electrode.The conductive coating layer may be disposed on the opposite side of the solid electrolyte layer.

[0133] (Manufacturing method of all-solid-state batteries) Another aspect of the present invention relates to a method for producing an all-solid-state battery.

[0134] The present invention also provides a method for manufacturing an all-solid-state battery, the method including: (S1) forming a laminate including a positive electrode, a solid electrolyte layer, and a negative electrode; (S2) pressing the laminate; and (S3) charging the pressed laminate while pressing the laminate, wherein at least one of the negative electrodes is a porous support having a conductive coating layer formed on one surface thereof.

[0135] The present invention also provides a method for producing a lithium secondary battery, in which the solid electrolyte layer in the method for producing an all-solid-state battery is replaced with a separator.

[0136] The steps (S2) and (S3) may be performed in reverse order or simultaneously, and the charging step (S3) may include providing a negative electrode active material layer on the conductive coating layer.

[0137] The conductive coating layer may be formed by depositing the conductive coating layer on one side of the porous support or by laminating the conductive coating layer on one side of the porous support.

[0138] The ratio of the thickness of the porous support before pressing the laminate to the thickness of the porous support after pressing the laminate may be 1:0.4 to 1:0.9, and the pressing force may be 20 MPa.

[0139] After step S3), lithium may be deposited between the conductive coating layer used as the negative electrode and the solid electrolyte layer.

[0140] The positive electrode may include a positive electrode active material layer including a metal oxide containing lithium.

[0141] In steps S2) and S3), the porous support is deformed, so that the pressure applied thereto can be reduced.

[0142] The (S1) may include the following steps.

[0143] (S1-1) preparing a negative electrode including a negative electrode current collector having a conductive coating layer disposed on one surface of a porous support having a large number of pores; (S1-2) preparing a positive electrode including a positive electrode current collector and a positive electrode active material formed on the positive electrode current collector; (S1-3) preparing a battery cell including an electrode assembly having a positive electrode, a negative electrode, and a solid electrolyte layer interposed between the positive electrode and the negative electrode.

[0144] Here, the steps (S1-1) and (S1-2) are steps of preparing a positive electrode and a negative electrode, and the order of the steps is not limited. That is, the positive electrode may be prepared first, or the negative electrode may be prepared first. Alternatively, the positive electrode and the negative electrode may be prepared simultaneously.

[0145] Here, in the step (S1-1), the conductive coating layer may be disposed by depositing a conductive coating layer on one side of the porous support or laminating a conductive coating layer on one side of the porous support.

[0146] Here, the ratio of the thickness of the porous support before pressing the laminate to the thickness of the porous support after pressing the laminate may be 1:0.4 to 1:0.9, and the pressing force may be 20 MPa.

[0147] By performing step (S3), lithium may be deposited between the negative electrode current collector and the solid electrolyte layer. The deposited lithium may serve as a negative electrode active material layer. In addition, stress generated by the lithium deposition may be reduced by compressing the porous support.

[0148] The steps (S1-2) and (S1-3) are not particularly limited as long as they are methods commonly used in the art.

[0149] In the step (S3), the charging step is not particularly limited as long as it is a method commonly used in the art. In the step (S3), lithium released from the positive electrode during the charging process is plated on the negative electrode current collector, and the deposited lithium itself can be used as the negative electrode active material layer.

[0150] In addition, in steps S2) and / or S3), the porous support is deformed to reduce the pressure F applied from the outside, and the pressure F is uniformly applied to the entire battery, thereby reducing the pressure applied to the entire battery. As a result, the positions of the positive electrode, separator / solid electrolyte layer, and negative electrode inside the battery do not change, and when they are pressed, they receive a constant pressure, ultimately preventing internal cell shorts and improving the safety of the battery.

[0151] Here, the porous support is deformed such that its length decreases in the pressing direction and its length increases in the direction perpendicular to the pressing direction, thereby reducing the pressure applied to the entire battery.

[0152] FIG. 4 is a schematic diagram of an all-solid-state battery according to an embodiment of the present invention, and FIG. 5 is a schematic diagram of the all-solid-state battery according to an embodiment of the present invention after charging and pressing.

[0153] As shown in FIG. 4, the all-solid-state battery according to the present invention includes a positive electrode 100 including a positive electrode current collector 110 and a positive electrode active material layer 120 coated on at least one surface thereof, a separator / solid electrolyte layer 200, a porous support 310, and a negative electrode 300 including a conductive coating layer 320 coated on at least one surface of the porous support 310.

[0154] 5 is a schematic diagram of an all-solid-state battery according to the present invention after charging and pressing. As shown in FIG. 5, after charging, lithium is deposited on the battery according to the present invention to form a lithium layer 330. The lithium layer 330 is charged under a constant current / constant voltage (CC / CV) condition. At this time, the pressure F applied to the entire all-solid-state battery may vary depending on the amount of lithium formed in the battery, the charge / discharge rate and time, etc. The lithium layer 330 corresponds to the negative electrode active material layer in the present specification.

[0155] When the porous support 310 receives a certain force due to the pressure F, the size and amount of pores in the porous support 310 first decrease, thereby relieving the stress due to the pressure F. When the pressure F is further applied, the length of the porous support 310 increases due to the pressure F in the direction perpendicular to the pressing direction, i.e., the horizontal (f1, x) and vertical (f2, y) directions of the porous support 310, and the thickness (f3, z) of the porous support 310 decreases in the pressing direction, thereby reducing the pressure F applied to the lithium secondary battery, thereby reducing the force applied to the lithium layer 330 and the entire lithium secondary battery.

[0156] The deformation in the horizontal, vertical, and thickness directions may be performed as shown in FIG. 5, and three types of deformation may be performed: deformation in the horizontal and vertical directions, deformation in the thickness direction, and deformation in the horizontal, vertical, and thickness directions.

[0157] Here, the porous support 310 may be present on one side of the positive electrode 100. The porous support 310 has the same shape as that used in the negative electrode 300 of the present invention, so a form in which the porous support is present in the positive electrode 100 instead of the negative electrode 300 may be used, or a form in which the porous support is present in the positive electrode 100 while the negative electrode 300 is being used may be used.

[0158] 4 and 5 according to the present invention can be directly applied to a lithium secondary battery when the solid electrolyte layer is changed to a separator.

[0159] Hereinafter, the present invention will be described in detail based on examples in order to specifically explain the present invention. However, the examples according to the present invention can be modified into many different forms, and the scope of the present invention should not be construed as being limited to the following examples. The examples of the present invention are provided to more completely explain the present invention to those having average knowledge in the art.

[0160] (Experiment 1) Elastic force experiment on porous support A polyethylene (hereinafter referred to as PE) porous support having a porosity of 45% (Example 1-1), a PE porous support having a porosity of 47% (Example 1-2), a PET (polyethylene terephthalate) nonwoven fabric having a porosity of 49% (Example 1-3), and a nickel foam having a porosity of 89% (Comparative Example 1-1) were each cut to 26.8 cm x 26.8 cm, and pressed at 5 MPa, 10 MPa, 15 MPa, and 20 MPa, respectively. The thicknesses of Examples 1-1 to 1-3 and Comparative Example 1-1 before and after pressing were measured and are shown in Table 1 below. The thickness after pressing is the thickness measured after the pressing force is removed.

[0161] [Table 1]

[0162] As shown in Table 1, in the case of Examples 1-1, 1-2, and 1-3, the thickness does not change significantly even in various pressing ranges. FIG. 6 is a graph showing the thickness retention rate of the porous supports by pressing in Examples 1-1, 1-2, 1-3, and Comparative Example 1-1. It can be seen that the porous supports according to all the examples of the present invention have a thickness retention rate by pressing of 70% or more even when pressed at 20 MPa. Here, the thickness retention rate by pressing can be calculated by (thickness after pressing / thickness before pressing)×100%.

[0163] This can also be seen in Figures 7 and 8, which are photographs taken before and after pressing of the porous support according to Example 1-1. From Figures 7 and 8, it can be seen that there is almost no difference in thickness and surface morphology of the porous support according to Example 1-1 before and after pressing.

[0164] Meanwhile, in the case of metals that are conventionally used as current collectors (Comparative Example 1-1), the thickness change due to pressure is very large. When a battery is manufactured using Comparative Example 1-1 as an anode current collector, the thickness of the nickel foam decreases due to the increase in the thickness of the deposited lithium when the battery is charged, but it cannot be restored during discharge, making it difficult to maintain the internal pressure of the battery. Figures 9 and 10 are photographs taken before and after pressing the support according to Comparative Example 1-1. Referring to Figures 6, 9, and 10, it can be seen that the thickness of the support according to Comparative Example 1-1 decreased when pressure was applied, and the surface of the support became smooth.

[0165] 6, in the case of Comparative Example 1-1, the thickness retention rate is less than 40% at 20 MPa, and is less than 70% even at a relatively weak pressure of 5 MPa, while in the cases of Examples 1-1, 1-2, and 1-3, a high thickness retention rate of 70% or more is shown even at a high pressure of 20 MPa. From this, it can be seen that the support according to Comparative Example 1-1 is unable to maintain porosity, and therefore is difficult to reduce the stress generated by the deposition of lithium.

[0166] (Experiment 2) Comparison of recovery force of porous support before and after compression To compare the recovery force before and after pressing with a polymer film, a PET release film (Example 1-4), a PE zipper bag (Example 1-5), and a Parafilm (Comparative Example 1-2) were each cut to 26.8 cm x 26.8 cm and pressed with a weight of 0.5 tons and 6 tons. The thickness before pressing, the thickness during pressing, the thickness in a recovered state after pressing, and the area after pressing of Examples 1-4, 1-5, and Comparative Example 1-2 were each measured and shown in Table 2 below.

[0167] Here, PET release film is a thin coating of silicone release agent on one or both sides of PET film using the microgravure method and then hardened, which can release adhesive materials, prevent contamination, and protect the adhesive layer. PE zipper bag is a product made using PE among products used as regular zipper bags. Parafilm is a translucent flexible film made of a mixture of wax and polyolefin, and the name Parafilm is a registered trademark of Bemis Company, Inc., headquartered in Neenah, Wisconsin.

[0168] [Table 2]

[0169] As shown in Table 2, the area and thickness of the PET release film (Examples 1-4) before pressing are the same as those after pressing, and the PE zipper bag also shows the same level of elasticity, but the Parafilm shows a decrease in elasticity. Thus, even films using polymers show very different physical properties.

[0170] (Experiment 3) Measurement of electrical conductivity of conductive coating layer As shown in Table 3, samples of Examples 2-1 to 2-6 and Comparative Examples 2-1 to 2-3 were prepared in a size of 5 cm x 5 cm. To measure electrical conductivity, measurements were performed in 25 areas using a 4-point probe device. The average Rs of the measured values ​​was obtained and the electrical conductivity was calculated. The electrical conductivities are compared in Table 3 below.

[0171] [Table 3]

[0172] In Table 3, Rs is the resistivity measured by the equipment, ρcal is the resistivity calculated by applying the thickness, and ρbulk is the resistivity of a commonly known material.

[0173] When silver (Ag) is deposited on a porous support to form a thin negative electrode current collector as in Examples 2-1 to 2-3, 2-5, and 2-6 in Table 3, the current collector has a resistance value equivalent to that of a typical nickel current collector. This is believed to be because silver has an affinity for lithium. Even when the deposited silver coating layer is extremely thin, at 1 μm, as in Examples 2-3 and 2-5, the current collector shows significantly improved electrical conductivity compared to the stainless steel SUS304 current collector commonly used in the art.

[0174] As can be seen from Table 3, when a metal was deposited on a porous support and used as a negative electrode current collector, the ρcal value and ρbulk value were the same or equivalent, indicating that the metal was uniformly deposited. FIG. 11 is an SEM image of the surface of the negative electrode current collector according to Example 2-3, and it was confirmed that the deposited silver (Ag) particles were in close contact with each other and had conductivity. In addition, as shown in Table 3, it was confirmed that metals having electrical conductivity such as silver (Ag) and gold (Au) can be used as a negative electrode current collector together with a porous support.

[0175] On the other hand, in the case of Comparative Example 2-2 where there was no metal layer, the resistance value of the porous support was high and Rs itself could not be measured. In other words, it was confirmed that when only the porous support exists without the metal layer, it cannot be used as a negative electrode current collector.

[0176] (Experiment 4) Battery performance evaluation The battery performances of the negative electrode current collectors obtained in Experiments 1 to 3 were compared.

[0177] In experiment 4, a negative electrode formed with the following composition was used, and the initial capacity, efficiency, and cell short occurrence rate were measured after the first charge and discharge (charge conditions: CC (constant current) / CV (constant voltage), (4.25 V, 0.05 C, 0.01 C current cut-off), discharge conditions: CC (constant current) conditions 3 V, 0.05 C, 60°C evaluation).

[0178] The initial capacity was measured by performing charging and discharging at 60° C., and the efficiency was calculated by dividing the discharge capacity by the charge capacity, and is shown in Table 4 below.

[0179] (Example 3-1) As the negative electrode, the negative electrode of Example 2-3 was used.

[0180] The positive electrode was manufactured as follows. Specifically, the positive electrode active material was NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 A positive electrode slurry was prepared by dispersing and stirring the following materials: Li6PS5Cl, argyrodite solid electrolyte (Li6PS5Cl), conductive carbon black, and binder polymer polytetrafluoroethylene (PTFE) in anisole at a weight ratio of 77.5:19.5:1.5:1.5. This was applied to a 15μm-thick aluminum current collector with a doctor blade and vacuum dried at 100℃ for 12 hours.

[0181] The solid electrolyte layer was manufactured as follows. Specifically, argyrodite solid electrolyte (Li6PS5Cl) and polytetrafluoroethylene (PTFE) as a binder polymer were dispersed and stirred in anisole at a weight ratio of 95:5 to manufacture a slurry. This was applied to an aluminum current collector with a thickness of 15 μm using a doctor blade and vacuum dried at 100°C for 12 hours.

[0182] The prepared positive electrode, the prepared solid electrolyte layer, and the negative electrode were sequentially interposed to fabricate an electrode assembly, which was then placed between jigs and subjected to a pressure of 5 MPa.

[0183] (Example 3-2) This is the same as Example 3-1, except that the negative electrode was a nickel foil having a thickness of 11 μm, and the porous support of Example 1-1 was used instead.

[0184] (Example 3-3) This is the same as Example 3-2, except that the porous support of Example 1-3 was used instead of the porous support of Example 1-1.

[0185] (Examples 3-4) This is the same as Example 3-2, except that the specimen was fastened to the jig so as to apply a pressure of 10 MPa instead of 5 MPa.

[0186] (Examples 3-5) This is the same as Example 3-1, except that the negative electrode was a nickel foil having a thickness of 11 μm and the porous support of Example 1-4 was used instead.

[0187] (Examples 3 to 6) This is the same as Example 3-1, except that the negative electrode was a nickel foil having a thickness of 11 μm and the porous support of Example 1-5 was used instead.

[0188] (Comparative Example 3-1) It is the same as Example 3-2, except that the negative electrode does not have the porous support of Example 1-1.

[0189] (Comparative Example 3-2) An experiment was carried out in the same manner as in Example 3-2, except that a PET nonwoven fabric with a porosity of 47% was used instead of the porous support of Example 1-1. The PET nonwoven fabric with a porosity of 47% is a nonwoven fabric with small elastic deformation and very little change in thickness due to pressure.

[0190] Table 4 shows the experimental results for Examples 3-1 to 3-6 and Comparative Examples 3-1 and 3-2.

[0191] [Table 4]

[0192] As can be seen from Table 4, it was confirmed that the rate of short circuit occurrence in a battery was significantly low when a porous support according to one aspect of the present invention was used. When only a metal layer was present without a separate porous support as in Comparative Example 3-1, the rate of short circuit occurrence was high, making it difficult to use it as a negative electrode current collector.

[0193] It can be seen that when a porous support having good elasticity is used as in Examples 3-1 to 3-3, 3-5, and 3-6 of the present invention, the rate of short circuit occurrence in the battery is significantly lower than when it is not used. Comparing Examples 3-5 and 3-6, it can be seen that even in the case of a porous support, the higher the rate of recovery to the original shape after compression, the lower the rate of short circuit occurrence.

[0194] In the case of Example 3-4, even though the pressing force was increased to 10 MPa, an excellent value was still shown in the ratio of short circuit occurrences.

[0195] The support of Comparative Example 3-2 is in the form of a nonwoven fabric with a very low change in thickness due to pressure, so the fibers in the nonwoven fabric do not shrink, and pressure is concentrated at the junctions between the fibers. As a result, lithium is deposited non-uniformly on the surface of the current collector during charging and discharging, and the rate of short circuiting in the secondary battery is higher than in the Examples.

[0196] As described above, it can be seen from Table 4 that the use of the negative electrode according to the present invention improves the safety of the battery, and the efficiency of the battery is equal or higher. [Industrial Applicability]

[0197] INDUSTRIAL APPLICABILITY The present invention relates to an electrode including a porous support and a conductive coating layer formed on at least one surface of the porous support, and therefore has industrial applicability. [Explanation of symbols]

[0198] 10, 100 positive electrode 11, 110 Positive electrode current collector 12, 120 Cathode active material layer 20, 200 solid electrolyte layer 30, 300 negative electrode 31 Negative electrode current collector 310 Porous support 320 Conductive coating layer 330 Negative electrode active material layer, lithium layer F Pressure f1 horizontal f2 vertical f3 Thickness

Claims

1. A porous support; A conductive coating layer formed on at least one surface of the porous support, The porous support includes an elastic material; The porous support is a porous polymer film or a porous polymer nonwoven fabric having a plurality of pores and capable of elastic deformation; The porous support has a thickness retention rate of 70% or more due to pressing, The porous support has an elastic deformation rate of 30% or less due to pressure. Electrode: Here, the thickness maintenance rate due to the pressing can be calculated by (thickness after pressing / thickness before pressing)×100%, Here, the elastic deformation rate due to the pressing can be calculated by (thickness before pressing-thickness under a pressing force of 20 MPa) / thickness before pressing×100%.

2. The electrode of claim 1 , wherein the electrode is a negative electrode or a positive electrode.

3. 3. The electrode of claim 1 or 2, wherein the porous support has a large number of pores.

4. 4. The electrode according to claim 1, wherein the porous support comprises a sheet or nonwoven fabric made from one or more selected from the group consisting of polyolefin-based porous substrates and polyethylene.

5. The electrode according to claim 1 , wherein the porous support further comprises a ceramic in addition to the polymer having a porous structure.

6. 6. The electrode of claim 1, wherein the porous support is formed by uniaxial or biaxial stretching.

7. 7. The electrode according to claim 1, wherein the porosity of the porous support is between 10% and 90%.

8. 8. The electrode according to claim 1, wherein the porous support has pores with a diameter of 0.01 μm to 10 μm.

9. 9. The electrode according to claim 1, wherein the porous support has a thickness of from 5 μm to 300 μm.

10. The electrode according to claim 1 , wherein the porous support decreases in thickness in a pressing direction and increases in area in a direction perpendicular to the pressing direction.

11. The electrode is a negative electrode, the negative electrode includes the conductive coating layer and a negative electrode active material layer, 2. The electrode according to claim 1, wherein the negative electrode active material layer is formed by deposition on the conductive coating layer during a charging process of the battery, and is stripped from the surface of the conductive coating layer during a discharging process of the battery.

12. 12. The electrode according to claim 1, wherein the conductive coating layer is a metal or metal oxide coated on the surface of the porous support or on the surfaces of pores formed inside the porous support.

13. 13. The electrode of claim 1, wherein the conductive coating layer comprises a metal having electrical conductivity.

14. the conductive coating layer comprises a lithium affinity material; 14. The electrode according to claim 1, wherein the lithium affinity material is at least one selected from the group consisting of metals including Au, Ag, Fe, Mg, Al, Ti, Cr, Ni, Cu, Zn, In, Sn, Pt, Co, Mn, Li, Bi, and Si, and metal oxides including CuO, ZnO, MnO, and CoO.

15. 15. The electrode according to any one of claims 1 to 14, wherein the conductive coating layer has a thickness of from 100 nm to 5 μm.

16. 16. A lithium secondary battery comprising the electrode according to claim 1 as a negative electrode.

17. 16. An all-solid-state battery comprising the electrode according to claim 1 as a negative electrode.

18. 18. The all-solid-state battery of claim 17, comprising a positive electrode, the negative electrode, and a solid electrolyte layer interposed between the positive electrode and the negative electrode.

19. 20. The all-solid-state battery of claim 18, wherein the conductive coating layer is disposed on a surface of the porous support facing the solid electrolyte layer.

20. the solid electrolyte layer includes a solid electrolyte, The solid electrolyte is 10 -7 20. The all-solid-state battery according to claim 18 or 19, having an ion conductivity of at least 100 S / cm, comprising a polymer-based solid electrolyte, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or a mixture of two or more of these.

21. (S1) forming a laminate including a positive electrode, a solid electrolyte layer, and a negative electrode; (S2) pressing the laminate; (S3) charging the pressed stack while pressing it; A method for producing an all-solid-state battery comprising: At least one of the negative electrodes is a porous support having a conductive coating layer formed on one surface thereof, The porous support includes an elastic material; The porous support is a porous polymer film or a porous polymer nonwoven fabric having a plurality of pores and capable of elastic deformation; The porous support has a thickness retention rate of 70% or more due to pressing, The porous support has an elastic deformation rate of 30% or less due to pressing. Here, the thickness maintenance rate due to the pressing can be calculated by (thickness after pressing / thickness before pressing)×100%, Here, the elastic deformation rate due to the pressing can be calculated by (thickness before pressing-thickness under a pressing force of 20 MPa) / thickness before pressing×100%.

22. The method for manufacturing an all-solid-state battery according to claim 21 , wherein (S2) and (S3) are performed in reverse order or simultaneously.

23. The method for manufacturing an all-solid-state battery according to claim 21 or 22, wherein the charging in step (S3) comprises providing a negative electrode active material layer on the conductive coating layer.

24. 24. The method for manufacturing an all-solid-state battery according to claim 21, wherein the conductive coating layer is formed by depositing the conductive coating layer on one surface of the porous support or laminating the conductive coating layer on one surface of the porous support.

25. The method for producing an all-solid-state battery according to any one of claims 21 to 24, wherein a ratio of a thickness of the porous support after the laminate is pressed to a thickness of the porous support before the laminate is pressed is 1:0.7 to 1:0.9.

Citation Information

Patent Citations

  • Current collecting material for lithium battery, its manufacturing method, and lithium battery

    JP2005243588A

  • Charge / discharge method of secondary battery and battery device

    JP2010009989A

  • All-solid-state lithium secondary battery

    JP2015092433A

  • Laminate type all-solid battery and manufacturing method thereof

    JP2018181451A

  • Solid electrolyte for all-solid secondary battery, all-solid secondary battery, and method for manufacturing solid electrolyte

    JP2019091599A