Method for separating joined members

Friction stir welding with a rotary tool and probe enables easy separation and rejoining of joined members by scraping out a joint portion using frictional heat, addressing the limitations of existing methods and enhancing work efficiency.

JP7562464B2Active Publication Date: 2024-10-07HONDA MOTOR CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021057225
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-30
Publication Date
2024-10-07
Estimated Expiration
2041-03-30

AI Technical Summary

Technical Problem

Existing methods for separating joined members, such as those described in Patent Documents 1 and 2, either do not account for easy separation after bonding or require external heating that can weaken the bond strength and potentially damage electronic components.

Method used

A method using friction stir welding with a rotary tool and probe to separate joined members by scraping out a portion of the joint through a through hole, utilizing frictional heat for separation without damaging the members, and rejoining them using the same tool configuration.

Benefits of technology

The method allows for easy separation and rejoining of members without additional material, reduces heat-induced damage, and improves work efficiency by using a common tool for both processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562464000001
    Figure 0007562464000001
  • Figure 0007562464000002
    Figure 0007562464000002
  • Figure 0007562464000003
    Figure 0007562464000003
Patent Text Reader

Abstract

To provide a separation method that can easily separate joined members so that the members can be rejoined to each other.SOLUTION: A separator 13 comprises a shoulder 14 having a through-hole 10 and a rotary tool 15 inserted through the through-hole 10. The rotary tool 15 includes a probe 17 at a tip part thereof. The shoulder 14 is pressed against a surface of a first member 1, and then the rotated probe 17 is plunged into a joining part 3 joining the first member 1 and a second member 2 to each other. A rotating direction of the probe 17 is a direction in which the joining part is scraped out by a screw groove. The joining part 3 is plastically flown to be scraped out by rotation of the probe 17, and therefore is guided by the shoulder 14 to change into a joining material part 20 connected to the first member 1 without nearly contributing to joining the first and second members 1 and 2 to each other.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for separating joined members. [Background technology]

[0002] Friction stir welding is a method of joining multiple overlapping members by pressing a rotating tool against them and stirring the area around the pressed portion by plastic flow caused by frictional heat. Friction stir line welding is a method in which the tool is pressed against the members and then moved along the surfaces of the members, while friction stir spot welding is a method in which the tool is not moved along the surfaces of the members after being pressed against them.

[0003] Patent Document 1 describes a method of friction stir welding in which a pin (probe) having a screw structure is used to push plastically flowed material to the tip of the pin by the screw structure. Patent Document 2 describes a method of heating a friction stir welded dissimilar metal joint to form a brittle intermetallic compound phase, and then applying an external load to destroy the brittle intermetallic compound phase, thereby separating the joined metal materials from each other. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-160318 A [Patent Document 2] JP 2007-54848 A Summary of the Invention [Problem to be solved by the invention]

[0005] There are cases where joined components are separated for inspection or repair, and rejoined after the inspection or repair. The method described in Patent Document 1 does not take into consideration separation after joining. The method described in Patent Document 2 requires an external input for separation, and since a fragile dissimilar intermetallic compound phase is generated by heating, measures are required to prevent a decrease in joint strength when attempting to rejoin. In addition, Patent Document 2 does not describe a specific heating method, and when attempting to release the joint in electronic or electrical components, there is a risk that the heating may have an adverse effect on these components, so the invention described in Patent Document 2 is not suitable for separating components that are to be rejoined for use.

[0006] In view of the above problems, an object of the present invention is to provide a separation method that allows joined members to be easily separated so that they can be rejoined. [Means for solving the problem]

[0007] According to one embodiment of the present invention, in a joining structure including a plate-shaped first member (1) and a second member (2) disposed so as to abut against an opposing surface of the first member (1) and joined to the first member (1) by a joining portion (3, 31), a method of separating the first member (1) from the second member (2) using friction stirring, the method comprising: a shoulder (14, 34) having a through hole (10, 36) extending along a central axis intersecting a surface of the first member (1) and an abutment surface (12, 38) capable of selectively abutting against the first member (1); and a probe (17, 35) having a thread groove on a side peripheral surface is provided at a tip thereof, and the through hole (10, 36) is joined to the second member (2) by a joining portion (3, 31). the step of preparing a rotating tool (15, 33) that is inserted into a threaded hole (14, 36) and extends along the central axis and is rotatable around the central axis; the step of pressing the abutment surface (12, 38) of the shoulder (14, 34) against the first member (1); the step of rotating the rotating tool (15, 33) in a direction in which the joint (3, 31) is scraped out by the thread groove so that at least a portion of the joint (3, 31) flows and is scraped out, and inserting the probe (17, 35) into the joint (3, 31); and the step of separating the first member (1) from the second member (2).

[0008] According to this configuration, at least a part of the joint is scraped out and does not contribute to the joint, so that the first member can be easily separated from the second member. In addition, the heat generated during the separation operation is frictional heat caused by the rotation of the probe, so that the first member and the second member are not adversely affected, and the first member and the second member can be reused and rejoined.

[0009] One embodiment of the present invention is characterized in that, in the above configuration, the joining structure is a friction stir welding structure with the joining portion (3) formed by friction stir welding from the first member (1) side, the friction stir welding is friction stir spot welding, and in the penetrating step, the rotating tool (15) forms an annular gap (19) between the side surface of the probe (17) and the inner surface of the through hole (10) of the shoulder (14), and the annular gap (19) is configured to receive the scraped-out portion of the joining portion (3) in a state connected to the first member (1) to form a joining material portion (20).

[0010] According to this configuration, the scraped-out portion of the joint formed by friction stir spot welding is connected to the first component as the joining material portion, so that when the components are rejoined, little or no additional material is required to form the joint.

[0011] In one embodiment of the present invention, in the above configuration, in order to rejoin the separated first member (1) to the second member (2), a rejoining shoulder (22) having a through hole (10) extending along the central axis and an abutment surface (12) capable of selectively abutting against the first member (1), and a rejoining rotating tool (23) having a probe (8) at its tip, inserted into the through hole (10) of the rejoining shoulder (22), extending along the central axis, and rotatable about the central axis, are provided with a rejoining rotating tool (23); the step of placing the material (1) in the same position relative to the second member (2) as it was before separation; the step of pressing the abutment surface (12) of the rejoining shoulder (22) against the first member (1) so that the joining material part (20) is received in the through hole (10) of the rejoining shoulder (22); and the step of rotating the rejoining rotating tool (23) and inserting the probe (8) of the rejoining rotating tool (23) into the portion where the joining part (3) was formed so as to flow and push the joining material part (20).

[0012] According to this configuration, since the rejoining means is similar to the separating means, a common device for operating the tool can be used, improving operability.

[0013] One embodiment of the present invention is characterized in that, in the above-mentioned first configuration, the joining structure is a friction stir welding structure with the joining portion (31) formed by friction stir welding from the first member side, the friction stir welding is friction stir line welding, a groove (39) extending linearly in the radial direction from the through hole (36) to the outer peripheral surface of the shoulder (34) is formed on the abutment surface (38) of the shoulder (34), and the step of inserting the probe (35) into the joining portion (31) includes advancing the probe (35) in a direction opposite to the groove (39) while scraping out at least a part of the joining portion (31) toward inside the groove (39) and pulling away at least a part of the joining portion (31) toward a position facing the second member (2) with a gap therebetween, thereby forming a joining material portion (40) connected to the first member (1).

[0014] According to this configuration, the scraped-out portion of the joint formed by friction stir line welding is connected to the first member as the joining material portion, so that when the members are rejoined, little or no additional material is required to form the joint.

[0015] One embodiment of the present invention is characterized in that, in the above configuration, the method further includes the steps of: placing the first member (1) connected to the joining material portion (40) in the same position relative to the second member (2) as before separation, in order to rejoin the separated first member (1) to the second member (2); pressing the abutment surface (38) of the shoulder (34) against the first member (1) so that one end of the joining material portion (40) is received in the groove (39) of the shoulder (34); and penetrating the rotating tool (33) into the portion that formed the joint portion (31) while rotating the rotating tool (33) in the direction opposite to that at the time of separation, and moving the rotating tool (33) and the shoulder (34) along the joining material portion (40) so that the groove (39) is located at the front side.

[0016] According to this configuration, a common tool is used for separation and rejoining, which eliminates the need to change tools and improves workability.

[0017] In one embodiment of the present invention, in any of the above configurations, the strength of the material of the first member (1) is lower than the strength of the material of the second member (2).

[0018] According to this configuration, the probe enters from the side of the first member having low strength, so that the portion that has undergone plastic flow due to the rotation of the probe is easily stirred, making it easy to separate and rejoin the first member 1 to the second member 2.

[0019] In one embodiment of the present invention, in any of the above configurations, the first member (1) and the second member (2) constitute an electrical connection portion of an electronic component or an electric component.

[0020] With this configuration, the loss of electrical energy during joining is smaller than when the electrical connections of these components are physically joined with bolts or the like, and the electrical connections can be easily separated and rejoined. Effect of the Invention

[0021] According to the present invention, members joined by friction stir welding can be easily separated so that they can be rejoined. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is an explanatory diagram of a joining method by friction stir spot joining according to a first embodiment; [Diagram 2] FIG. 1 is an explanatory diagram of a method for separating a joint formed by friction stir spot welding according to the first embodiment; [Diagram 3] FIG. 1 is an explanatory diagram of a rejoining method by friction stir spot welding according to a first embodiment. [Figure 4] FIG. 11 is a plan view showing joining by friction stir line joining according to the second embodiment; [Diagram 5] FIG. 5 is an explanatory diagram of a joining method by friction stir line joining according to the second embodiment (cross section AA in FIG. 4). [Figure 6]FIG. 5 is an explanatory diagram of a joining method by friction stir line joining according to the second embodiment (cross section BB of FIG. 4). [Figure 7] FIG. 5 is an explanatory diagram of a method for separating a welded joint by friction stir line welding according to a second embodiment (cross section taken along the line AA in FIG. 4). [Figure 8] FIG. 5 is an explanatory diagram of a method for separating a welded joint by friction stir line welding according to a second embodiment (cross section BB in FIG. 4). [Figure 9] FIG. 5 is an explanatory diagram of a rejoining method by friction stir line joining according to the second embodiment (cross section BB of FIG. 4). [Figure 10] 11 is a bottom view of the shoulder according to the second embodiment. [Figure 11] FIG. 11 is an explanatory diagram of a separation method according to a modified example of the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Figures 1 to 3 are vertical cross-sectional views showing a method for joining, separating and rejoining members using friction stir spot joining according to a first embodiment.

[0024] As shown in FIG. 1, a plate-shaped first member 1 and a plate-shaped second member 2 are joined to each other by a joint 3 formed by friction stir spot welding. The joint 3 is formed by applying a joining device 4 from the side of the first member 1. Another plate-shaped member may be included between the first member 1 and the second member 2. Preferably, the strength of the material of the first member 1 is lower than the strength of the material of the second member 2 in the portion to be joined. For example, the combination of the material of the first member 1 and the material of the second member 2 may be aluminum alloy-aluminum alloy, copper alloy-copper alloy, iron alloy-iron alloy, aluminum alloy-iron alloy, aluminum alloy-copper alloy, aluminum alloy-carbon fiber reinforced plastic, aluminum alloy-glass fiber reinforced plastic, magnesium alloy-iron alloy, magnesium alloy-copper alloy, magnesium alloy-carbon fiber reinforced plastic, or magnesium alloy-glass fiber reinforced plastic (the material of the first member 1 is described before the hyphen, and the material of the second member 2 is described after the hyphen).

[0025] The joining device 4 for joining the first member 1 to the second member 2 includes a joining rotating tool 5 that rotates around a central axis, and a joining shoulder 6. In the following description, the central axis extends in the vertical direction, and the side on which the joining device 4 is placed relative to the first member 1 is referred to as the top, and the side on which the second member 2 is placed is referred to as the bottom; however, the actual positional relationship between the first and second members 1, 2 and the joining device 4 may be upside down, or the central axis may extend horizontally or may be inclined. Furthermore, although the central axis is perpendicular to the surface of the first member 1, it may intersect at an angle other than 90°.

[0026] The joining rotation tool 5 is rotationally symmetric about the central axis. The joining rotation tool 5 includes a body 7 having a generally cylindrical shape centered on the central axis, and a probe 8 extending downward along the central axis from the lower end of the body 7. The probe 8 has a smaller diameter than the body 7, and the lower surface of the body 7 forms a shoulder surface 9 that is concave with respect to the first member 1. A thread groove is provided on the circumferential side surface of the probe 8.

[0027] The joining shoulder 6 is generally cylindrical in shape and has a through hole 10 extending along the central axis, a flange 11 extending radially outward (in a plane perpendicular to the central axis) at its upper portion, and a contact surface 12 on its lower surface that can selectively contact the first member 1.

[0028] A method of joining a first member 1 to a second member 2 by friction stir spot joining using a joining device 4 will be described. As shown in FIG. 1(A), an operator places the first member 1 on the second member 2 placed on a workbench (not shown), presses the abutment surface 12 of the joining shoulder 6 against the first member 1, and, as shown in FIG. 1(B), rotates the joining rotating tool 5 inserted into the through hole 10 of the joining shoulder 6 around the central axis while penetrating the probe 8 into the first and second members 1 and 2. At this time, the rotation direction of the joining rotating tool 5 is the direction in which the materials of the first and second members 1 and 2 that have been plastically flowed by frictional heat caused by the rotation of the probe 8 are pressed downward by the thread groove. The probe 8 is inserted into the first and second members 1 and 2 until its tip is positioned between the upper and lower surfaces of the second member 2. The materials of the first and second members 1 and 2 that have been plastically flowed by frictional heat caused by the rotation of the probe 8 are mixed with each other. When the probe 8 is inserted to the deepest depth into the first and second members 1, 2, the side surface and shoulder surface 9 of the probe 8, or the side surface, shoulder surface 9 and lower inner surface of the through hole 10 of the probe 8, cover the plastically flowed portions of the first and second members 1, 2. As shown in Fig. 1(C), when the worker pulls out the probe 8 while rotating it, the material of the first and second members 1, 2 that has plastically flowed and been stirred cools and hardens to become the welded portion 3.

[0029] The first and second members 1, 2 may be joined to each other without using the joining shoulder 6. Furthermore, the probe 8 used during joining does not need to have a thread groove on its circumferential side surface, and in this case, the rotation direction of the joining rotation tool 5 may be either clockwise or counterclockwise.

[0030] 2 shows a method for separating a first member 1 joined to a second member 2 by friction stir spot welding using a separating device 13. The separating device 13 includes a shoulder 14 and a rotating tool 15 that rotates about a central axis.

[0031] The separation shoulder 14, like the joining shoulder 6, includes a through hole 10 and an abutment surface 12. The diameter of the through hole 10 is equal to or greater than the diameter of the through hole 10 of the joining shoulder 6 (see FIG. 1). The joining shoulder 6 may be used as the separation shoulder 14.

[0032] The rotation tool 15 is different from the joining rotation tool 5. The rotation tool 15 is generally rotationally symmetric about the central axis. The rotation tool 15 includes a body 16 having a generally cylindrical shape centered on the central axis, and a probe 17 extending downward from the lower end of the body 16 along the central axis. The probe 17 has a smaller diameter than the body 16, and the lower surface of the body 16 forms a flat shoulder surface 18 facing the first member 1. A thread groove is provided on the side peripheral surface of the probe 17. The diameter of the probe 17 is equal to or larger than the diameter of the probe 8 (see FIG. 1) when joined. The protruding length of the probe 17 from the shoulder surface 18 is longer than the protruding length of the probe 8 from the shoulder surface 9 when joined.

[0033] A method of separating the first member 1 from the second member 2 using the separation device 13 will be described. As shown in FIG. 2(A), an operator places the first and second members 1, 2 joined together on a workbench (not shown) so that the first member 1 is placed on the second member 2, presses the abutment surface 12 of the shoulder 14 against the first member 1, and, as shown in FIG. 2(B), while rotating the rotating tool 15 inserted into the through hole 10 of the shoulder 14 about the central axis, inserts the probe 17 into the joint 3. At this time, the rotation direction of the rotating tool 15 is the direction in which the constituent material of the joint 3 that has plastically flowed due to frictional heat caused by the rotation of the probe 17 is scraped out upward. The probe 17 is inserted into the joint 3 until its tip is positioned between the upper and lower surfaces of the second member 2. At this time, the material constituting the joint 3 is plastically flowed by frictional heat caused by the rotation of the probe 17, scraped out by the thread groove, and received in the annular gap 19 formed between the side circumferential surface of the probe 17 and the inner circumferential surface of the through hole 10 of the shoulder 14. As shown in FIG. 2(C), when the worker pulls out the probe 17 while rotating it without changing the rotation direction, the plastically flowed part cools and solidifies to become the annular joint material part 20. Next, the worker separates the first member 1 from the second member 2. Since the lower part of the joint material part 20 is connected to the first member 1 and not to the second member 2, the first member 1 can be easily separated from the second member 2. Alternatively, the lower part of the joint material part 20 is connected to the first and second members 1 and 2, but the part connected to the second member 2 is small and thin, so it is easily peeled off from the second member 2 and easily broken. Therefore, when a force is applied in a direction pulling the first member 1 away from the second member 2, even a small force will cause the bonding material part 20 to peel off from the second member 2, or the bonding material part 20 will break near the boundary between the first member 1 and the second member 2, causing the first member 1 to separate from the second member 2 with all or most of the bonding material part 20 remaining connected.

[0034] 3 shows a method for rejoining a first member 1 to a second member 2 using a rejoining device 21. The rejoining device 21 includes a rejoining shoulder 22 and a rejoining rotating tool 23 that rotates about a central axis.

[0035] The rejoining shoulder 22, like the separation shoulder 14, includes a through hole 10 and an abutment surface 12, and the diameter of the through hole 10 of the rejoining shoulder 22 is equal to or greater than the diameter of the through hole 10 of the separation shoulder 14, and preferably equal to the diameter of the through hole 10 of the separation shoulder 14. The separation shoulder 14 may be used as the rejoining shoulder 22.

[0036] The rejoining rotating tool 23 is different from the separation rotating tool 15 (see FIG. 2). The rejoining rotating tool 23 has a rotational symmetric shape around the central axis. Like the joining rotating tool 5, the rejoining rotating tool 23 includes a main body 7 and a probe 8, and a shoulder surface 9 is formed on the lower surface of the main body 7. The protruding length of the probe 8 from the shoulder surface 9 is shorter than the protruding length of the probe 17 from the shoulder surface 18 in the separation rotating tool 15 (see FIG. 2), and the diameter of the probe 8 is equal to or smaller than the diameter of the separation probe 17. The joining rotating tool 5 (see FIG. 1) may be used as the rejoining rotating tool 23.

[0037] A method of rejoining a first member 1 to a second member 2 using a rejoining device 21 will be described. As shown in FIG. 3(A), an operator places the first member 1 on the second member 2 placed on a workbench (not shown) in the same position as before separation, presses the abutment surface 12 of the rejoining shoulder 22 against the first member 1, and, as shown in FIG. 3(B), rotates the rejoining rotating tool 23 inserted into the through hole 10 of the rejoining shoulder 22 around the central axis while penetrating the probe 8 into the portion where the joint portion 3 was formed. At this time, the rotation direction of the rejoining rotating tool 23 is the direction in which the material of the joint material portion 20 that has plastically flowed due to frictional heat caused by the rotation of the probe 8 is pressed downward. Also, while the probe 8 is penetrating, the shoulder surface 9 hits the joint material portion 20 while rotating, and presses the plastically flowed material of the joint material portion 20 downward. The probe 8 is inserted into the portion where the joint 3 was formed until its tip is positioned between the upper and lower surfaces of the second member 2. When the probe 8 is inserted deepest into the portion where the joint 3 was formed, the side circumferential surface and shoulder surface 9 of the probe 8, or the side circumferential surface, shoulder surface 9 and the inner circumferential surface of the lower part of the through hole 10 of the probe 8 cover the material that constituted the joint material portion 20. As shown in FIG. 3(C), when the worker pulls out the probe 8 while rotating it without changing the rotation direction, the part that has plastically flowed solidifies and becomes the joint 3. The probe 8 used for rejoining does not need to have a thread groove on the side circumferential surface. In this case, the rotation direction of the rejoining rotating tool 23 may be either clockwise or counterclockwise. Before the probe 8 is inserted into the first and second members 1 and 2, the material to constitute the joint 3 may be added to the joint material portion 20.

[0038] The effects of the first embodiment will be described. When the joining portion 3 is transformed into the joining material portion 20 by the separation device 13, the lower portion of the joining material portion 20 is connected to the first and second members 1 and 2, but the portion connected to the second member 2 is small and thin, so the lower portion of the joining material portion 20 is easily peeled off from the second member 2 and easily broken. Therefore, with a slight force, the joining material portion 20 peels off from the second member 2 or breaks near the boundary between the first and second members 1 and 2, and the first member 1 can be easily separated from the second member 2.

[0039] The heat applied to the first and second members 1, 2 during separation is frictional heat generated by the probe 17, and therefore the range of influence is not significantly different from the frictional heat generated by the probe 8 during joining or rejoining. As a result, adverse effects on the first and second members 1, 2 are suppressed, and the first and second members 1, 2 can be reused and rejoined.

[0040] Since the constituent material of the joint portion 3 scraped out during separation is connected to the first member 1 as the joint material portion 20, the amount of newly added material for rejoining during rejoining is small or unnecessary.

[0041] Since the means for joining, separating, and rejoining are similar to each other, the devices for moving the joining rotation tool 5, the separating rotation tool 15, and the rejoining rotation tool 23, as well as the joining shoulder 6, the separating shoulder 14, and the rejoining shoulder 22, can be common, improving workability.

[0042] By applying the separation device 13 and the rejoining device 21 from the side of the first member 1, which has lower strength than the second member 2, the portion that has undergone plastic flow due to the rotation of the probe 17 is more easily stirred than in the case where the separation device 13 and the rejoining device 21 are applied from the side with higher strength, making it easier to separate and rejoin the first member 1 to the second member 2.

[0043] A second embodiment will be described with reference to Fig. 4 to Fig. 11. Fig. 4 is a plan view of joined members. A joint 31 extends linearly along the surface of the joined first member 1. Figs. 5 and 7 show cross sections corresponding to the AA section in Fig. 4, and Figs. 6, 8, and 9 show cross sections corresponding to the BB section in Fig. 4. Figs. 5 and 6 show a method of joining members using friction stir line welding, Figs. 7 and 8 show a separation method, and Fig. 9 shows a rejoining method.

[0044] As shown in Figs. 4 to 6, a plate-shaped first member 1 and a plate-shaped second member 2 are joined to each other by a joint 31 formed by friction stir line welding. The joint 31 is formed by applying a joining and separating device 32 from the side of the first member 1. Another plate-shaped member may be included between the first member 1 and the second member 2. Preferably, the strength of the material of the first member 1 is lower than the strength of the material of the second member 2 in the portion to be joined. Examples of combinations of the material of the first member 1 and the material of the second member 2 are similar to those in the first embodiment.

[0045] In the second embodiment, the joining, separation and re-joining of the first member 1 to the second member 2 are performed by a common joining / separating apparatus 32. The joining / separating apparatus 32 includes a rotation tool 33 that rotates about a central axis, and a shoulder 34.

[0046] The rotary tool 33 is rotationally symmetric about its central axis. A probe 35 having a generally cylindrical shape centered on the central axis is provided at the lower end of the rotary tool 33. A thread groove is provided on the peripheral side surface of the probe 35.

[0047] The shoulder 34 has a generally cylindrical shape, is provided with a through hole 36 extending along the central axis, is provided at its upper part with a flange 37 extending radially outward, and is provided at its lower surface with an abutment surface 38 that can selectively abut against the first member 1. A probe 35 is inserted into the through hole 36, and the inner peripheral surface of the through hole 36 is in close contact with the inner peripheral surface of the through hole 36 to such an extent that the probe 35 can rotate about the central axis. As shown in Figs. 6 and 8 to 10, a groove 39 is formed in the abutment surface 38, extending linearly in the radial direction from the through hole 36 to the outer peripheral surface of the shoulder 34. The width of the groove 39 is approximately equal to the diameter of the through hole 36.

[0048] With reference to Figs. 5 and 6, a method for joining a first member 1 to a second member 2 by friction stir line joining using a joining and separating device 32 will be described. As shown in Fig. 5(A), an operator places the first member 1 on the second member 2 placed on a workbench (not shown), presses the abutment surface 38 of the shoulder 34 against the first member 1, and, as shown in Fig. 1(B), inserts the probe 35 into the through hole 36 of the shoulder 34, and while rotating the rotary tool 33 around the central axis, plunges the probe 35 into the first and second members 1 and 2. At this time, the rotation direction of the rotary tool 33 is the direction in which the parts of the first and second members 1 and 2 that have plastically flowed due to frictional heat caused by the rotation of the probe 35 are pressed downward by the thread groove. The probe 35 is plunged into the first and second members 1 and 2 until its tip is positioned between the upper and lower surfaces of the second member 2.

[0049] Next, as shown in FIG. 6, the worker moves the shoulder 34 and the probe 35 along the surface of the first member 1 in the direction in which the weld 31 should be formed, with the probe 35 inserted into the first and second members 1 and 2. At this time, the groove 39 of the shoulder 34 is disposed in the forward direction of the shoulder 34 and the probe 35 relative to the through hole 36. The parts of the first and second members 1 and 2 that have undergone plastic flow due to frictional heat caused by the rotation of the probe 35 move backward due to the thread groove of the probe 35. When the shoulder 34 and the probe 35 have moved to the end point of the weld 31, the worker pulls out the probe 35 while rotating it, as shown in FIG. 5(C). The parts of the first and second members 1 and 2 that have undergone plastic flow solidify when cooled, forming the weld 31.

[0050] 7 and 8, a method for separating a first member 1, which has been joined to a second member 2 by friction stir line welding, from the second member 2 using a joining and separating device 32 will be described. First, an operator places the first and second members 1, 2 on a workbench (not shown) at one end of a joining portion 31, as shown in FIG. 7(A), so that the first member 1 is placed on the second member 2, and presses the contact surface 38 of the shoulder 34 against the surface of the first member 1. At this time, the shoulder 34 is placed so that the groove 39 is located on the opposite side of the joining portion 31 with respect to the through hole 36. Next, an operator inserts a probe 35 into the through hole 36 of the shoulder 34, as shown in FIG. 7(B), and plunges the probe 35 into the joining portion 31 while rotating the rotating tool 33 around the central axis. At this time, the rotation direction of the rotating tool 33 is the opposite direction to that during joining, i.e., the direction in which the portion that has plastically flowed due to frictional heat caused by the rotation of the probe 35 in the joint 31 is scraped out upward. The probe 35 is inserted into the joint 31 until its tip is positioned between the upper and lower surfaces of the second member 2, preferably to the same depth as during joining.

[0051] Next, as shown in FIG. 8, the worker moves the shoulder 34 and the rotating tool 33 along the joint 31 toward the other end of the joint 31 with the probe 35 inserted into the joint 31. Therefore, the shoulder 34 and the rotating tool 33 advance in the opposite direction to the groove 39. At this time, at least a part of the joint 31 plastically flows due to frictional heat caused by the rotation of the probe 35, is scraped upward and backward by the thread groove, and is received in the groove 39 so as to face the second member 2 with a gap therebetween. The material constituting the joint 31 received in the groove 39 cools and hardens to become a joint material part 40 that is connected to the first member 1 and not connected to the second member 2. When the shoulder 34 and the probe 35 move to the other end of the joint 31, the worker pulls out the probe 35 while rotating it without changing the rotation direction, as shown in FIG. 7(C). Since the bonding material 40 does not contribute to the bonding between the first and second members 1, 2, a worker can easily pull the first member 1 away from the second member 2.

[0052] With reference to FIG. 9, a method of rejoining a first member 1 to a second member 2 using a joining and separating device 32 will be described. The worker places the first member 1 on the second member 2 placed on a workbench (not shown) in the same position as before separation, and presses the abutting surface 38 of the shoulder 34 against the first member 1. At this time, the shoulder 34 is positioned so that the groove 39 receives one end of the joining material portion 40. Next, the worker rotates the rotating tool 33 with the probe 35 inserted into the through hole 36 of the shoulder 34 around the central axis, and plunges the probe 35 into the portion where the joining portion 31 was provided via the joining material portion 40. At this time, the rotation direction of the rotating tool 33 is the opposite direction to that at the time of separation, that is, the direction in which the portion that has plastically flowed due to frictional heat caused by the rotation of the probe 35 is pressed downward. The probe 35 is plunged into the portion where the joining portion 31 was formed up to the same vertical position as at the time of separation.

[0053] Next, the worker moves the shoulder 34 and the probe 35 along the joining material part 40 toward the other end of the joining material part 40 with the probe 35 entering the part where the joint 31 was formed. Therefore, the shoulder 34 and the probe 35 advance in the direction of the groove 39 as viewed from the through hole 36. At this time, the material constituting the joining material part 40 plastically flows due to frictional heat caused by the rotation of the probe 35 and is pushed downward and backward by the thread groove, and the upward movement is restricted by the abutting part, so that it is pushed in to fill the gap between the joining material part 40 and the second member 2. The material constituting the moved joining material part 40 cools and hardens, forming the joint 31 and joining the first and second members 1 and 2 to each other. When the shoulder 34 and the rotating tool 33 move to the other end of the joining material part 40, the worker pulls out the probe 35 from the first and second members 1 and 2 while rotating it without changing the rotation direction.

[0054] The effects of the second embodiment will be described. In the joining, separation, and rejoining, a common rotating tool 33 and shoulder 34 can be used, so that the attachment and detachment of these tools from the joining and separation device 32 is not necessary. By forming the joining portion 31 as the joining material portion 40 connected to the first member 1 facing the second member 2 with a gap in the joining and separation device 32, the first and second members 1, 2 are released from each other, so that the first member 1 can be easily separated from the second member 2. In addition, since the material constituting the joining portion 31 is connected to the first member 1 as the joining material portion 40, it is not necessary to add a new material for rejoining when rejoining. The adverse effects of heat generated during the separation operation are suppressed, and the first member 1 has a lower strength than the second member 2, so that separation and rejoining are easy, as in the first embodiment.

[0055] Fig. 11 shows a modified example of the second embodiment. This modified example differs from the second embodiment in that the first member 1 to the second member 2 is initially joined by known friction stir line joining, rather than by a joining and separating device 32. Therefore, as shown in Fig. 11(A), the shape of the joint 31 does not match the shape of the probe 35 (see Fig. 7, etc.). This modified example also differs from the second embodiment in that the second member 2 is not plate-shaped.

[0056] The first member 1 is a terminal of a conductor of an electronic or electrical component 41, and the second member 2 is a terminal of a battery 42 electrically connected to the electronic or electrical component 41. Compared to when both terminals are physically joined to each other with a bolt or the like, the loss of electrical energy during joining is smaller, and both terminals can be easily separated from each other and rejoined.

[0057] The diameter of the probe 35 and the diameter of the through hole 36 are equal to or greater than the width of the joint 31 on the lower surface of the first member 1. The width of the groove 39 is preferably approximately equal to the width of the joint 31 on the upper surface of the first member 1. By setting the diameter of the probe 35, the diameter of the through hole 36, and the width of the groove 39 in this manner, the first and second members 1, 2 can be separated from each other and rejoined by the separating method and rejoining method of the second embodiment described above.

[0058] As shown in FIG. 11(B), a joint remnant 43 that was part of the joint 31 (see FIG. 11(A)) may remain on the second material. However, if the probe 35 is inserted below the top surface of the second member 2, the joint remnant 43 is not connected to the first member 1 and does not contribute to the joining. For this reason, as shown in FIG. 11(C), even if the joint remnant 43 remains, the first member 1 can be easily separated from the second member 2.

[0059] Although the description of the specific embodiment is finished above, the present invention is not limited to the above embodiment and can be widely modified. For example, in the embodiment of the present invention, the joining structure to which the separation method is applied is a friction stir welding structure, but the separation method can also be applied to a welded structure such as laser welding or a joining structure using an adhesive. The separation method according to the present invention can be used not only for repairing or inspecting joined equipment, but also for separating different materials for recycling. [Explanation of symbols]

[0060] 1: First member 2: Second member 3,31:Joint part 8,17,35: Probe 9,18: Shoulder surface 10,36:Through hole 12,38: Contact surface 13: Separation device 14,34: Shoulder 15,33: Rotation tool 19: Annular gap 20,40:Joining material part 21: Rejoining device 22: Reconnecting shoulder 23: Rotation tool for rejoining 32: Junction separation device 39: Groove

Claims

1. A method for separating a plate-like first member from a second member in a joining structure including a plate-like first member and a second member arranged to abut on an opposing surface of the first member and joined to the first member by a joining portion, comprising the steps of: preparing a rotary tool having a through hole extending along a central axis intersecting a surface of the first member, a shoulder having an abutment surface capable of selectively abutting against the first member, and a probe having a thread groove on a side peripheral surface at a tip end thereof, the rotary tool being inserted into the through hole, extending along the central axis, and rotatable about the central axis; pressing the abutment surface of the shoulder against the first member; Rotating the rotation tool in a direction in which the joint is scraped out by the thread groove so that at least a portion of the joint flows and is scraped out, and inserting the probe into the joint; pulling the first member away from the second member; 23. A method comprising:

2. The joining structure is a friction stir welding structure formed by the joining portion formed by friction stir welding from the first member side, The friction stir welding is friction stir spot welding, 2. The method of claim 1, wherein in the penetrating step, the rotating tool forms an annular gap between the side surface of the probe and an inner surface of the through hole of the shoulder, the annular gap being configured to receive the scraped-out portion of the joint in a connected state with the first member to form a joint material portion.

3. rejoining the separated first member to the second member; preparing a rejoining shoulder having a through hole extending along the central axis and an abutment surface selectively abuttable against the first member, and a rejoining rotating tool having a probe at a tip end, being inserted into the through hole of the rejoining shoulder, extending along the central axis, and rotatable about the central axis; placing the first member connected by the bonding material portion at the same position relative to the second member as before separation; pressing the abutment surface of the rejoining shoulder against the first member such that the joining material is received in the through hole of the rejoining shoulder; rotating the rejoining rotation tool and inserting the probe of the rejoining rotation tool into the portion where the joint was formed so as to flow and push the joining material portion; 3. The method of claim 2 further comprising:

4. The joining structure is a friction stir welding structure formed by the joining portion formed by friction stir welding from the first member side, The friction stir welding is friction stir line welding, a groove is formed on the abutment surface of the shoulder, the groove extending linearly in a radial direction from the through hole to an outer circumferential surface of the shoulder, 2. The method of claim 1, wherein the step of inserting the probe into the joint includes advancing the probe in a direction away from the groove while scraping at least a portion of the joint into the groove and pulling at least a portion of the joint away from the second member to a position opposite the second member with a gap therebetween to form a joint material portion connected to the first member.

5. rejoining the separated first member to the second member; placing the first member connected by the bonding material portion at the same position relative to the second member as before separation; pressing the abutment surface of the shoulder against the first member such that one end of the joining material is received in the groove of the shoulder; a step of inserting the rotating tool into the portion that formed the joint while rotating the rotating tool in a direction opposite to that of separation, and moving the rotating tool and the shoulder along the joint material portion so that the groove is located on the front side; 5. The method of claim 4, further comprising:

6. 6. The method according to claim 1, wherein the strength of the material of the first member is lower than the strength of the material of the second member.

7. The method according to any one of claims 1 to 6, characterized in that the first member and the second member constitute an electrical connection of an electronic or electrical component.

Citation Information

Patent Citations

  • Manufacture of plate type heat pipe

    JP1999047961A

  • Separation of dissimilar metal material joined body produced by friction stirring method

    JP2007054848A

  • Hollow structure forming method, and hollow structure

    JP2012135789A

  • Copper adhering terminal

    JP2012160318A

  • Device and method for friction stir welding

    JP2014208358A