Water-based coating composition

The use of specific hydroxyl group-containing resins and alkyl etherified melamine resin in aqueous coating compositions improves film compatibility and resistance, enhancing repellency and water resistance in hydrophobic melamine resin-based paints.

JP7562536B2Active Publication Date: 2024-10-07KANSAI PAINT CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021537603
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-02
Filing Date
2020-06-08
Publication Date
2024-10-07
Estimated Expiration
2040-06-08

AI Technical Summary

Technical Problem

Water-based paints containing hydrophobic melamine resins suffer from compatibility issues with water, leading to cissing and insufficient repellency and water resistance in coating films.

Method used

Aqueous coating compositions comprising hydroxyl group-containing acrylic or polyester resins, an oligomer with a molecular weight of 200 to 800 and solubility parameter of 10.0 to 13.5, and alkyl etherified melamine resin with a molar ratio of methyl to butyl groups ranging from 50/50 to 0/100, which enhance film compatibility and resistance.

Benefits of technology

The solution results in coating films with excellent repellency and water resistance, addressing the compatibility and performance issues of hydrophobic melamine resin-based paints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562536000001
    Figure 0007562536000001
  • Figure 0007562536000002
    Figure 0007562536000002
  • Figure 0007562536000003
    Figure 0007562536000003
Patent Text Reader

Abstract

The present invention provides an aqueous coating composition which is capable of forming a coating film that has excellent cissing resistance and water resistance. An aqueous coating composition which contains (A) at least one hydroxyl group-containing resin that is selected from among (A1) hydroxyl group-containing acrylic resins and (A2) hydroxyl group-containing polyester resins, (B) an oligomer and (C) an alkyl etherified melamine resin, wherein: the oligomer (B) has a number average molecular weight within the range of from 200 to 800 and a solubility parameter within the range of from 10.0 to 13.5; and the molar ratio of methyl groups to butyl groups in the alkyl etherified melamine resin (C), namely (methyl group) / (butyl group) molar ratio is from 50 / 50 to 0 / 100.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aqueous coating composition. [Background technology]

[0002] Conventionally, water-based paints containing a base resin such as an acrylic resin or polyester resin having functional groups such as hydroxyl groups or carboxyl groups, and a melamine resin as a crosslinking agent, have been widely used as undercoat paints and topcoat paints for automobile exterior panels.

[0003] As the melamine resin, a water-soluble melamine resin having a relatively high content of methyl groups and excellent water dispersibility is often used, but recently, the use of a hydrophobic melamine resin having a relatively high content of butyl groups has also been considered. A water-based paint containing such a hydrophobic melamine resin has excellent coating film performance such as water resistance compared to a water-based paint containing the above-mentioned water-soluble melamine resin, but there is a problem that the use of the hydrophobic melamine resin may cause cissing because the compatibility of the hydrophobic melamine resin with water, which is a medium, is low.

[0004] Patent Document 1 describes an aqueous resin dispersion containing a reaction product obtained by heating 5-70% by weight of an acrylic resin (A), 10-90% by weight of a hydrophobic melamine resin (B), and 0-50% by weight of a polyester resin (C), characterized in that the thickening rate of the mixture of the components (A), (B), and (C) before and after the heating treatment is 20-200%. The document also describes that the aqueous resin dispersion has excellent water dispersibility, and that a coating film formed from the aqueous resin dispersion has excellent finish properties, water resistance, etc. However, the aqueous resin dispersion has a problem in that it may have insufficient cissing resistance.

[0005] Patent Document 2 describes an aqueous coating composition whose main film-forming component is a co-condensation composition of 100 parts by weight of an oil-free alkyd resin having a molecular weight of 500 to 10,000, an acid value of 20 to 100, and a hydroxyl value of 50 to 200, and 5 to 70 parts by weight of a water-insoluble amino resin compatible with the above resin, and describes that the use of the aqueous coating composition can provide an excellent coating film with good interlayer adhesion and no coating film defects such as repelling. However, there is a problem that the coating film formed by the aqueous coating composition may have insufficient water resistance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2002-308993 A [Patent Document 2] Japanese Patent Publication No. 52-107029 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in consideration of the above circumstances, and has as its object to provide an aqueous paint composition capable of forming a coating film having excellent cissing resistance and water resistance. [Means for solving the problem]

[0008] As a result of intensive research into achieving the above-mentioned object, the present inventors have found that the above-mentioned object can be achieved by an aqueous coating composition comprising (A) at least one hydroxyl-containing resin selected from (A1) a hydroxyl-containing acrylic resin and (A2) a hydroxyl-containing polyester resin, (B) an oligomer, and (C) an alkyl etherified melamine resin, wherein the oligomer (B) has a number average molecular weight in the range of 200 to 800, a solubility parameter value in the range of 10.0 to 13.5, and the alkyl etherified melamine resin (C) has a molar ratio of methyl groups to butyl groups, in terms of a (methyl group) / (butyl group) molar ratio, of 50 / 50 to 0 / 100.

[0009] The present invention relates to an aqueous coating composition and a method for forming a multilayer coating film, and includes the following embodiments. Item 1. An aqueous coating composition comprising (A) at least one hydroxyl-containing resin selected from (A1) a hydroxyl-containing acrylic resin and (A2) a hydroxyl-containing polyester resin, (B) an oligomer, and (C) an alkyl etherified melamine resin, wherein the oligomer (B) has a number average molecular weight in the range of 200 to 800, a solubility parameter value in the range of 10.0 to 13.5, and the alkyl etherified melamine resin (C) has a molar ratio of methyl groups to butyl groups of 50 / 50 to 0 / 100 in terms of a (methyl group) / (butyl group) molar ratio. Item 2. The aqueous coating composition according to Item 1, wherein the oligomer (B) has a number average molecular weight in the range of 200 to 500. Item 3. The aqueous coating composition according to Item 1 or 2, wherein the solubility parameter value of the oligomer (B) is within the range of 10.7 to 13.5. Item 4. The aqueous coating composition according to any one of Items 1 to 3, wherein the alkyl etherified melamine resin (C) has a molar ratio of methyl groups to butyl groups, expressed as a (methyl group) / (butyl group) molar ratio of 30 / 70 to 0 / 100. Item 5. A method for forming a multilayer coating film, comprising: applying the aqueous coating composition according to any one of items 1 to 4 onto a substrate to form a base coat film; and applying a clear coat coating composition (Z) onto the base coat film to form a clear coat film. Effect of the Invention

[0010] The aqueous coating composition of the present invention can form a coating film that is excellent in cissing resistance and water resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The aqueous coating composition of the present invention will now be described in further detail. The aqueous coating composition of the present invention (hereinafter sometimes abbreviated as "the coating") is an aqueous coating composition comprising (A) at least one hydroxyl-containing resin selected from (A1) a hydroxyl-containing acrylic resin and (A2) a hydroxyl-containing polyester resin, (B) an oligomer, and (C) an alkyl-etherified melamine resin, wherein the oligomer (B) has a number average molecular weight in the range of 200 to 800, a solubility parameter value in the range of 10.0 to 13.5, and the alkyl-etherified melamine resin (C) has a molar ratio of methyl groups to butyl groups of 50 / 50 to 0 / 100, in terms of the molar ratio of (methyl groups) / (butyl groups).

[0012] In this specification, the term "water-based paint" is a term that is contrasted with organic solvent-based paint, and generally means a paint in which a film-forming resin, pigment, etc. are dispersed and / or dissolved in water or a medium mainly composed of water (aqueous medium). The organic solvent-based paint is a paint that does not substantially contain water as a solvent, or a paint in which all or most of the solvent is an organic solvent.

[0013] Hydroxyl-containing resin (A) The hydroxyl-containing resin (A) according to the present invention is at least one hydroxyl-containing resin selected from the group consisting of a hydroxyl-containing acrylic resin (A1) and a hydroxyl-containing polyester resin (A2).

[0014] Hydroxyl-containing acrylic resin (A1) As the hydroxyl-containing acrylic resin (A1), any known water-soluble or water-dispersible acrylic resin that has been conventionally used in water-based paints can be used.

[0015] The hydroxyl-containing acrylic resin (A1) can be produced, for example, by copolymerizing a hydroxyl-containing polymerizable unsaturated monomer and another polymerizable unsaturated monomer copolymerizable with the hydroxyl-containing polymerizable unsaturated monomer by a method known per se, such as a solution polymerization method in an organic solvent or an emulsion polymerization method in water.

[0016] The hydroxyl-containing polymerizable unsaturated monomer is a compound having one or more hydroxyl groups and one or more polymerizable unsaturated bonds in one molecule. Examples of the hydroxyl-containing polymerizable unsaturated monomer include monoesters of (meth)acrylic acid and dihydric alcohols having 2 to 8 carbon atoms, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; ε-caprolactone-modified monoesters of (meth)acrylic acid and dihydric alcohols having 2 to 8 carbon atoms; N-hydroxymethyl (meth)acrylamide; allyl alcohol; and (meth)acrylates having polyoxyethylene chains whose molecular terminals are hydroxyl groups. However, in the present invention, a monomer corresponding to "(xvii) polymerizable unsaturated monomer having an ultraviolet absorbing functional group" described later should be defined as "another polymerizable unsaturated monomer copolymerizable with the above hydroxyl group-containing polymerizable unsaturated monomer" and is excluded from "hydroxyl group-containing polymerizable unsaturated monomer". These can be used alone or in combination of two or more kinds.

[0017] As other polymerizable unsaturated monomers copolymerizable with the above-mentioned hydroxyl group-containing polymerizable unsaturated monomers, for example, the following monomers (i) to (xx) can be used. These polymerizable unsaturated monomers can be used alone or in combination of two or more kinds.

[0018] (i) Alkyl or cycloalkyl (meth)acrylates: for example, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, tridecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, cyclododecyl (meth)acrylate, tricyclodecanyl (meth)acrylate, and the like. (ii) Polymerizable unsaturated monomers having an isobornyl group: isobornyl (meth)acrylate, etc. (iii) Polymerizable unsaturated monomers having an adamantyl group: adamantyl (meth)acrylate, etc. (iv) Polymerizable unsaturated monomers having a tricyclodecenyl group: tricyclodecenyl (meth)acrylate, etc. (v) Aromatic ring-containing polymerizable unsaturated monomers: benzyl (meth)acrylate, styrene, α-methylstyrene, vinyltoluene, and the like.

[0019] (vi) Polymerizable unsaturated monomers having an alkoxysilyl group: vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, γ-(meth)acryloyloxypropyltrimethoxysilane, γ-(meth)acryloyloxypropyltriethoxysilane, and the like. (vii) Polymerizable unsaturated monomers having a fluorinated alkyl group: perfluoroalkyl (meth)acrylates such as perfluorobutylethyl (meth)acrylate and perfluorooctylethyl (meth)acrylate; fluoroolefins, and the like. (viii) Polymerizable unsaturated monomers having a photopolymerizable functional group such as a maleimide group. (ix) Vinyl compounds: N-vinylpyrrolidone, ethylene, butadiene, chloroprene, vinyl propionate, vinyl acetate, etc. (x) Carboxyl group-containing polymerizable unsaturated monomers: (meth)acrylic acid, maleic acid, crotonic acid, β-carboxyethyl (meth)acrylate, etc.

[0020] (xi) Nitrogen-containing polymerizable unsaturated monomers: (meth)acrylonitrile, (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylamide, methylene bis(meth)acrylamide, ethylene bis(meth)acrylamide, adducts of glycidyl (meth)acrylate and amine compounds, and the like. (xii) Polymerizable unsaturated monomers having two or more polymerizable unsaturated groups in one molecule: allyl (meth)acrylate, ethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, etc. (xiii) Epoxy group-containing polymerizable unsaturated monomers: glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 3,4-epoxycyclohexylethyl (meth)acrylate, 3,4-epoxycyclohexylpropyl (meth)acrylate, allyl glycidyl ether, and the like. (xiv) (meth)acrylates having a polyoxyethylene chain whose molecular terminal is an alkoxy group. (xv) Polymerizable unsaturated monomers having a sulfonic acid group: 2-acrylamido-2-methylpropanesulfonic acid, 2-sulfoethyl (meth)acrylate, allylsulfonic acid, 4-styrenesulfonic acid, and the like; sodium salts and ammonium salts of these sulfonic acids.

[0021] (xvi) Polymerizable unsaturated monomers having a phosphoric acid group: acid phosphooxyethyl (meth)acrylate, acid phosphooxypropyl (meth)acrylate, acid phosphooxypoly(oxyethylene)glycol (meth)acrylate, acid phosphooxypoly(oxypropylene)glycol (meth)acrylate, and the like. (xvii) Polymerizable unsaturated monomers having an ultraviolet absorbing functional group: 2-hydroxy-4-(3-methacryloyloxy-2-hydroxypropoxy)benzophenone, 2-hydroxy-4-(3-acryloyloxy-2-hydroxypropoxy)benzophenone, 2,2'-dihydroxy-4-(3-methacryloyloxy-2-hydroxypropoxy)benzophenone, 2,2'-dihydroxy-4-(3-acryloyloxy-2-hydroxypropoxy)benzophenone, 2-[2-hydroxy-5-[2-(methacryloyloxy)ethyl]phenyl]-2H-benzotriazole, and the like. (xviii) Light-stable polymerizable unsaturated monomers: 4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine, 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-crotonoyloxy-2,2,6,6-tetramethylpiperidine, 4-crotonoylamino-2,2,6,6-tetramethylpiperidine, 1-crotonoyl-4-crotonoyloxy-2,2,6,6-tetramethylpiperidine, etc. (xix) Polymerizable unsaturated monomers having a carbonyl group: acrolein, diacetone acrylamide, diacetone methacrylamide, acetoacetoxyethyl methacrylate, formylstyrol, vinyl alkyl ketones having 4 to 7 carbon atoms (for example, vinyl methyl ketone, vinyl ethyl ketone, vinyl butyl ketone), and the like. (xx) Polymerizable unsaturated monomers having an acid anhydride group: maleic anhydride, itaconic anhydride, citraconic anhydride, etc.

[0022] In this specification, the polymerizable unsaturated group refers to an unsaturated group capable of undergoing radical polymerization. Examples of such polymerizable unsaturated groups include vinyl groups and (meth)acryloyl groups.

[0023] In addition, in this specification, "(meth)acrylate" means acrylate or methacrylate. "(meth)acrylic acid" means acrylic acid or methacrylic acid. "(meth)acryloyl" means acryloyl or methacryloyl. "(meth)acrylamide" means acrylamide or methacrylamide.

[0024] The proportion of the hydroxyl-containing polymerizable unsaturated monomer used in producing the hydroxyl-containing acrylic resin (A1) is preferably 1 to 50 mass %, more preferably 1 to 40 mass %, and even more preferably 1 to 30 mass %, based on the total amount of the monomer components.

[0025] From the viewpoints of the curability, chipping resistance, adhesion, finished appearance, etc. of the resulting coating film, the hydroxyl value of the hydroxyl-containing acrylic resin (A1) is preferably from 1 to 200 mgKOH / g, more preferably from 2 to 180 mgKOH / g, and even more preferably from 5 to 150 mgKOH / g.

[0026] From the viewpoints of storage stability of the coating material and water resistance of the resulting coating film, the hydroxyl-containing acrylic resin (A1) preferably has an acid value of 1 to 150 mgKOH / g, more preferably 5 to 100 mgKOH / g, and even more preferably 5 to 80 mgKOH / g.

[0027] When the aqueous coating composition contains the above-mentioned hydroxyl-containing acrylic resin (A1), the content of the hydroxyl-containing acrylic resin (A1) is preferably 2 to 70 mass%, more preferably 5 to 50 mass%, and even more preferably 10 to 40 mass%, based on the resin solid content in the aqueous coating composition.

[0028] Hydroxyl-containing polyester resin (A2) As the hydroxyl-containing polyester resin (A2), any known water-soluble or water-dispersible polyester resin that has been conventionally used in water-based paints can be used.

[0029] The hydroxyl-containing polyester resin (A2) can usually be produced by an esterification reaction or transesterification reaction between an acid component and an alcohol component.

[0030] The acid component may be any compound that is commonly used as an acid component in the production of polyester resins, such as an aliphatic polybasic acid, an alicyclic polybasic acid, or an aromatic polybasic acid.

[0031] The above-mentioned aliphatic polybasic acid is generally an aliphatic compound having two or more carboxyl groups in one molecule, an acid anhydride of the aliphatic compound, and an esterification product of the aliphatic compound. Examples of the aliphatic polybasic acid include aliphatic polybasic carboxylic acids such as succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecane diacid, dodecane diacid, brassylic acid, octadecanedioic acid, citric acid, and butanetetracarboxylic acid; anhydrides of the aliphatic polybasic carboxylic acids; and esterification products of the aliphatic polybasic carboxylic acids with lower alkyls having about 1 to 4 carbon atoms. The above-mentioned aliphatic polybasic acids can be used alone or in combination of two or more kinds.

[0032] As the aliphatic polybasic acid, it is preferable to use adipic acid and / or adipic anhydride from the viewpoint of smoothness of the resulting coating film.

[0033] The alicyclic polybasic acid is generally a compound having one or more alicyclic structures and two or more carboxyl groups in one molecule, an acid anhydride of the compound, and an esterification product of the compound. The alicyclic structure is mainly a 4- to 6-membered ring structure. Examples of the alicyclic polybasic acid include alicyclic polycarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 4-cyclohexene-1,2-dicarboxylic acid, 3-methyl-1,2-cyclohexanedicarboxylic acid, 4-methyl-1,2-cyclohexanedicarboxylic acid, 1,2,4-cyclohexanetricarboxylic acid, and 1,3,5-cyclohexanetricarboxylic acid; anhydrides of the alicyclic polybasic acid; and esterification products of the alicyclic polybasic carboxylic acid with lower alkyl having about 1 to 4 carbon atoms. The alicyclic polybasic acids can be used alone or in combination of two or more kinds.

[0034] From the viewpoint of smoothness of the resulting coating film, it is preferable to use 1,2-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic anhydride, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 4-cyclohexene-1,2-dicarboxylic acid, or 4-cyclohexene-1,2-dicarboxylic anhydride as the alicyclic polybasic acid, and among these, it is more preferable to use 1,2-cyclohexanedicarboxylic acid and / or 1,2-cyclohexanedicarboxylic anhydride.

[0035] The aromatic polybasic acid is generally an aromatic compound having two or more carboxyl groups in one molecule, an acid anhydride of the aromatic compound, and an esterification product of the aromatic compound, and examples thereof include aromatic polybasic carboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, trimellitic acid, and pyromellitic acid; anhydrides of the aromatic polybasic carboxylic acids; and esterification products of the aromatic polybasic carboxylic acids with lower alkyls having about 1 to 4 carbon atoms. The aromatic polybasic acids can be used alone or in combination of two or more kinds.

[0036] As the aromatic polybasic acid, it is preferable to use phthalic acid, phthalic anhydride, isophthalic acid, trimellitic acid, or trimellitic anhydride.

[0037] In addition, acid components other than the above-mentioned aliphatic polybasic acids, alicyclic polybasic acids, and aromatic polybasic acids can also be used. Such acid components are not particularly limited, and examples thereof include fatty acids such as coconut oil fatty acid, cottonseed oil fatty acid, hempseed oil fatty acid, rice bran oil fatty acid, fish oil fatty acid, tall oil fatty acid, soybean oil fatty acid, linseed oil fatty acid, tung oil fatty acid, rapeseed oil fatty acid, castor oil fatty acid, dehydrated castor oil fatty acid, and safflower oil fatty acid; monocarboxylic acids such as lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, benzoic acid, p-tert-butylbenzoic acid, cyclohexanoic acid, and 10-phenyloctadecanoic acid; and hydroxycarboxylic acids such as lactic acid, 3-hydroxybutanoic acid, and 3-hydroxy-4-ethoxybenzoic acid. These acid components can be used alone or in combination of two or more.

[0038] As the alcohol component, a polyhydric alcohol having two or more hydroxyl groups in one molecule can be suitably used. Examples of the polyhydric alcohol include ethylene glycol, propylene glycol, diethylene glycol, trimethylene glycol, tetraethylene glycol, triethylene glycol, dipropylene glycol, 1,4-butanediol, 1,3-butanediol, 2,3-butanediol, 1,2-butanediol, 2-methyl-1,3-propanediol, 3-methyl-1,2-butanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,2-pentanediol, 1,5-pentanediol, 1,4-pentanediol, 2,4-pentanediol, 2,3-dimethyltrimethylene glycol, tetramethylene glycol, 3-methyl-4,3-pentanediol, 3-methyl-1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 1,6-hexanediol, 1,5-hexanediol, 1,4-hexanediol, 2,5-hexanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, tricyclohexane Examples of the polylactone diols include dihydric alcohols such as rodecanedimethanol, hydroxypivalic acid neopentyl glycol ester, hydrogenated bisphenol A, hydrogenated bisphenol F, and dimethylolpropionic acid; polylactone diols obtained by adding lactone compounds such as ε-caprolactone to these dihydric alcohols; ester diol compounds such as bis(hydroxyethyl)terephthalate; polyether diol compounds such as alkylene oxide adducts of bisphenol A, polyethylene glycol, polypropylene glycol, and polybutylene glycol; trihydric or higher alcohols such as glycerin, trimethylolethane, trimethylolpropane, diglycerin, triglycerin, 1,2,6-hexanetriol, pentaerythritol, dipentaerythritol, tris(2-hydroxyethyl)isocyanuric acid, sorbitol, and mannitol; polylactone polyol compounds obtained by adding lactone compounds such as ε-caprolactone to these trihydric or higher alcohols; and fatty acid esters of glycerin.

[0039] In addition, alcohol components other than the above polyhydric alcohols can also be used. Examples of such alcohol components include, but are not limited to, monoalcohols such as methanol, ethanol, propyl alcohol, butyl alcohol, stearyl alcohol, and 2-phenoxyethanol; and alcohol compounds obtained by reacting monoepoxy compounds such as propylene oxide, butylene oxide, and "Cardura E10P" (trade name, manufactured by HEXION, glycidyl ester of synthetic highly branched saturated fatty acid) with acids.

[0040] The method for producing the hydroxyl-containing polyester resin is not particularly limited and can be carried out according to a conventional method. For example, the hydroxyl-containing polyester resin can be produced by heating the acid component and the alcohol component in a nitrogen stream at about 150 to 250°C for about 5 to 10 hours to carry out an esterification reaction or an ester exchange reaction between the acid component and the alcohol component.

[0041] When the acid component and the alcohol component are subjected to an esterification reaction or an ester exchange reaction, they may be added to a reaction vessel at once, or one or both may be added in several portions. Alternatively, a hydroxyl-containing polyester resin may be first synthesized, and then the obtained hydroxyl-containing polyester resin may be reacted with an acid anhydride to be half-esterified to obtain a carboxyl- and hydroxyl-containing polyester resin. Alternatively, a carboxyl-containing polyester resin may be first synthesized, and then the alcohol component may be added to obtain a hydroxyl-containing polyester resin.

[0042] In the esterification or transesterification reaction, a catalyst known per se, such as dibutyltin oxide, antimony trioxide, zinc acetate, manganese acetate, cobalt acetate, calcium acetate, lead acetate, tetrabutyl titanate, or tetraisopropyl titanate, can be used as a catalyst for promoting the reaction.

[0043] The hydroxyl-containing polyester resin may be modified with a fatty acid, a monoepoxy compound, a polyisocyanate compound, an acrylic resin, or the like during or after the preparation of the resin.

[0044] Examples of the fatty acids include coconut oil fatty acids, cottonseed oil fatty acids, hempseed oil fatty acids, rice bran oil fatty acids, fish oil fatty acids, tall oil fatty acids, soybean oil fatty acids, linseed oil fatty acids, tung oil fatty acids, rapeseed oil fatty acids, castor oil fatty acids, dehydrated castor oil fatty acids, safflower oil fatty acids, and the like. An example of the monoepoxy compound that can be suitably used is "Cardura E10P" (trade name, manufactured by HEXION, glycidyl ester of synthetic highly branched saturated fatty acid).

[0045] Examples of the polyisocyanate compound include aliphatic diisocyanate compounds such as lysine diisocyanate, hexamethylene diisocyanate, and trimethylhexane diisocyanate; and aliphatic diisocyanate compounds such as hydrogenated xylylene diisocyanate, isophorone diisocyanate, methylcyclohexane-2,4-diisocyanate, methylcyclohexane-2,6-diisocyanate, 4,4'-methylenebis(cyclohexylisocyanate), and 1,3-(isocyanatomethyl)cyclohexane. Examples of the polyisocyanate include cyclic diisocyanate compounds, aromatic diisocyanate compounds such as tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, etc., organic polyisocyanates themselves such as trivalent or higher polyisocyanates such as lysine triisocyanate, etc., adducts of these organic polyisocyanates with polyhydric alcohols, low molecular weight polyester resins, water, etc., cyclic polymers of these organic polyisocyanates (for example, isocyanurates), biuret-type adducts, etc. These polyisocyanate compounds can be used alone or in combination of two or more.

[0046] The method for modifying the hydroxyl group-containing polyester resin with an acrylic resin can be a known method, for example, a method of polymerizing a mixture of a polymerizable unsaturated group-containing polyester resin and a polymerizable unsaturated monomer, a method of reacting a hydroxyl group-containing polyester resin with an acrylic resin, and the like.

[0047] The hydroxyl value of the hydroxyl-containing polyester resin (A2) is preferably from 1 to 250 mgKOH / g, more preferably from 2 to 200 mgKOH / g, and even more preferably from 5 to 200 mgKOH / g.

[0048] When the hydroxyl-containing polyester resin (A2) further contains a carboxyl group, the acid value is preferably from 1 to 150 mgKOH / g, more preferably from 2 to 100 mgKOH / g, and even more preferably from 3 to 80 mgKOH / g.

[0049] The weight average molecular weight of the hydroxyl group-containing polyester resin (A2) is preferably from 3,000 to 100,000, more preferably from 4,000 to 50,000, and even more preferably from 5,000 to 30,000.

[0050] In this specification, the average molecular weight is a value calculated from a chromatogram measured by gel permeation chromatography based on the molecular weight of standard polystyrene. The gel permeation chromatograph used was "HLC8120GPC" (manufactured by Tosoh Corporation). Four columns, "TSKgel G-4000HXL", "TSKgel G-3000HXL", "TSKgel G-2500HXL", and "TSKgel G-2000HXL" (all of which are product names manufactured by Tosoh Corporation), were used, and the measurement was performed under the following conditions: mobile phase: tetrahydrofuran, measurement temperature: 40°C, flow rate: 1 mL / min, and detector: RI.

[0051] When the aqueous coating composition contains the above-mentioned hydroxyl-containing polyester resin (A2), the content of the hydroxyl-containing polyester resin (A2) is preferably 2 to 70 mass%, more preferably 5 to 50 mass%, and even more preferably 10 to 40 mass%, based on the resin solid content in the aqueous coating composition.

[0052] Oligomer (B) The oligomer (B) has a number average molecular weight in the range of 200 to 800 and a solubility parameter value in the range of 10.0 to 13.5.

[0053] When the number average molecular weight of the oligomer (B) is 200 or more, a coating film having excellent water resistance can be obtained, and when it is 800 or less, a coating film having excellent cissing resistance can be obtained. In particular, the number average molecular weight of the oligomer (B) is preferably 200 to 500, more preferably 200 to 300, and even more preferably 200 to 280, from the viewpoints of water resistance and cissing resistance.

[0054] When the solubility parameter value of the oligomer (B) is 10.0 or more, a coating film excellent in cissing resistance can be obtained, and when it is 13.5 or less, a coating film excellent in water resistance can be obtained. In particular, the solubility parameter value of the oligomer (B) is preferably 10.7 to 13.5, more preferably 11.0 to 13.5, from the viewpoints of cissing resistance and water resistance.

[0055] Specific examples of the oligomer (B) include polyoxyalkylene glycols such as polyoxyethylene glycol, polyoxypropylene glycol, and polyoxytetramethylene glycol, and etherified products thereof, etc. Among these, polyoxypropylene glycol and polyoxytetramethylene glycol are preferred, and polyoxytetramethylene glycol is more preferred.

[0056] As the oligomer (B), a commercially available product can be used. Examples of commercially available products include "Sannix GP250" (number average molecular weight 250, solubility parameter value 13.2), "Sannix GP400" (number average molecular weight 400, solubility parameter value 11.5), "Sannix GP600" (number average molecular weight 600, solubility parameter value 10.6) (all manufactured by Sanyo Chemical Industries, polyoxypropylene glyceryl ether), "Sannix PP200" (number average molecular weight 200, solubility parameter value 11.7), "Sannix PP400" (number average molecular weight 400, solubility parameter value 10.4) (all manufactured by Sanyo Chemical Industries, polyoxypropylene glycol), "PTMG250" (number average molecular weight 250, solubility parameter value 11.4), "PTMG650" (number average molecular weight 650, solubility parameter value 10.0) (all manufactured by Mitsubishi Chemical Corporation, polyoxytetramethylene glycol). The oligomer (B) can be used alone or in combination of two or more kinds.

[0057] The solubility parameter value can be calculated by the Fedors method, which is described in Polymer Engineering and Science, 14, (2), 147 (1974).

[0058] The content of the oligomer (B) in the aqueous coating composition of the present invention is preferably 1 to 20 mass %, more preferably 2 to 15 mass %, and even more preferably 3 to 10 mass %, based on the resin solid content in the aqueous coating composition.

[0059] Alkyl etherified melamine resin (C) The alkyl-etherified melamine resin (C) is a melamine resin in which the molar ratio of methyl groups to butyl groups, in terms of the (methyl group) / (butyl group) molar ratio, is 50 / 50 to 0 / 100.

[0060] The water resistance of the resulting coating film is good when the molar ratio of butyl groups in the above (methyl group) / (butyl group) is at least 50. In particular, the molar ratio of methyl groups to butyl groups in the alkyl-etherified melamine resin (C) is preferably 30 / 70 to 0 / 100, more preferably 10 / 90 to 0 / 100, and even more preferably 0 / 100, and is preferably a butyl-etherified melamine resin.

[0061] The alkyl-etherified melamine resin (C) can be synthesized by subjecting melamine to an addition reaction or addition-condensation reaction with an aldehyde such as formaldehyde, paraformaldehyde, acetaldehyde, or benzaldehyde to produce a methylol-melamine resin, and then methyl-etherifying and / or butyl-etherifying the methylol group portion of this resin with an alcohol.

[0062] The alcohol used in the methyl etherification can be methyl alcohol, and the alcohol used in the butyl etherification can be n-butyl alcohol or isobutyl alcohol.

[0063] By adjusting the types and amounts of the methyl alcohol, n-butyl alcohol and isobutyl alcohol used, the molar ratio of methyl groups to butyl groups in the alkyl-etherified melamine resin (C) can be adjusted.

[0064] The alkyl-etherified melamine resin (C) may be a condensate of an alkyl-etherified melamine resin (a polymerized alkyl-etherified melamine resin obtained by a condensation reaction).

[0065] The alkyl etherified melamine resin (C) generally has a weight average molecular weight within the range of 400 to 6,000, preferably 500 to 4,000, and more preferably 600 to 3,000.

[0066] The alkyl etherified melamine resin (C) may be a commercially available product, such as "Cymel 203", "Cymel 204", "Cymel 250", "Cymel 251", "Cymel 1156", "Cymel 1158" (all manufactured by Allnex Japan Co., Ltd.), "U-Van 20SE60", "U-Van 28-60" (all manufactured by Mitsui Chemicals, Inc.), etc.

[0067] The alkyl etherified melamine resins (C) can be used alone or in combination of two or more kinds.

[0068] A catalyst can be used in the curing reaction of the hydroxyl-containing resin and the alkyl-etherified melamine resin (C). Examples of the catalyst include sulfonic acids such as paratoluenesulfonic acid, dodecylbenzenesulfonic acid, and dinonylnaphthalenesulfonic acid; alkyl phosphates such as monobutyl phosphate, dibutyl phosphate, mono-2-ethylhexyl phosphate, and di-2-ethylhexyl phosphate; and salts of these acids with amines.

[0069] The content of the alkyl etherified melamine resin (C) in the aqueous coating composition of the present invention is preferably 1 to 60 mass%, more preferably 5 to 50 mass%, and even more preferably 10 to 40 mass%, based on the resin solid content in the aqueous coating composition.

[0070] The reason why the aqueous coating composition of the present invention can obtain a coating film having excellent water resistance and cissing resistance is not clear, but it is presumed that the molar ratio of butyl groups in the alkyl etherified melamine resin (C) in the aqueous coating composition is relatively high, so that the coating film formed has high hydrophobicity and excellent water resistance. In addition, the number average molecular weight of the oligomer (B) in the aqueous coating composition is relatively small and the solubility parameter is relatively high, so that the oligomer (B) can dissolve in both the water layer and the oil layer. Therefore, it is presumed that the oligomer (B) acts as a compatibilizer that prevents the alkyl etherified melamine resin (C) from being localized in the aqueous coating composition, and a coating film having excellent cissing resistance is provided.

[0071] Other Ingredients The aqueous coating composition of the present invention may further contain, as necessary, at least one hydroxyl-containing resin (A) selected from the hydroxyl-containing acrylic resin (A1) and the hydroxyl-containing polyester resin (A2), an oligomer (B), and a component other than the alkyl-etherified melamine resin (C). Examples of such components include resin components other than the at least one hydroxyl-containing resin (A) selected from the hydroxyl-containing acrylic resin (A1) and the hydroxyl-containing polyester resin (A2), crosslinkable components other than the alkyl-etherified melamine resin (C), pigments, organic solvents, dispersants, anti-settling agents, defoamers, thickeners, ultraviolet absorbers, light stabilizers, surface conditioners, and the like.

[0072] Examples of the resin component other than the at least one hydroxyl-containing resin (A) selected from the hydroxyl-containing acrylic resin (A1) and the hydroxyl-containing polyester resin (A2) include hydroxyl-free acrylic resins, hydroxyl-free polyester resins, polyurethane resins which may contain hydroxyl groups, olefin resins which may contain hydroxyl groups, and epoxy resins which may contain hydroxyl groups.

[0073] Of these, from the viewpoint of the water resistance of the resulting coating film, it is preferable to use a polyurethane resin which may contain hydroxyl groups, and in particular, it is preferable to use a hydroxyl group-containing polyurethane resin.

[0074] The hydroxyl group-containing polyurethane resin may be, for example, a hydroxyl group-containing polyurethane resin obtained by reacting a polyol with a polyisocyanate.

[0075] Examples of the polyols include low molecular weight dihydric alcohols such as ethylene glycol, diethylene glycol, propylene glycol, butylene glycol, and hexamethylene glycol, and trihydric alcohols such as trimethylolpropane, glycerin, and pentaerythritol. Examples of the polyols with high molecular weight include polyether polyols, polyester polyols, acrylic polyols, and epoxy polyols. Examples of the polyether polyols include polyethylene glycol, polypropylene glycol, and polytetramethylene glycol. Examples of the polyester polyols include polycondensates of alcohols such as the dihydric alcohols and dibasic acids such as adipic acid, azelaic acid, and sebacic acid, lactone-based ring-opening polymer polyols such as polycaprolactone, and polycarbonate diols. In addition, carboxyl group-containing polyols such as 2,2-dimethylolpropionic acid and 2,2-dimethylolbutanoic acid can also be used.

[0076] Examples of the polyisocyanate to be reacted with the polyol include aliphatic polyisocyanates such as hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, dimer acid diisocyanate, and lysine diisocyanate; and biuret type adducts and isocyanurate ring adducts of these polyisocyanates; isophorone diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), methylcyclohexane-2,4-(or -2,6-)diisocyanate, Alicyclic diisocyanates such as 1,3-(or 1,4-)di(isocyanatomethyl)cyclohexane, 1,4-cyclohexane diisocyanate, 1,3-cyclopentane diisocyanate, and 1,2-cyclohexane diisocyanate; and biuret-type adducts and isocyanurate ring adducts of these polyisocyanates; xylylene diisocyanate, metaxylylene diisocyanate, tetramethylxylylene diisocyanate, tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate. aromatic diisocyanate compounds such as bis(4-isocyanatophenyl)sulfone, bis(4-phenylisocyanate), ... Examples of such polyisocyanates include biuret type adducts and isocyanurate ring adducts of isocyanates; polyisocyanates having three or more isocyanate groups in one molecule, such as triphenylmethane-4,4',4''-triisocyanate, 1,3,5-triisocyanatobenzene, 2,4,6-triisocyanatotoluene, and 4,4'-dimethyldiphenylmethane-2,2',5,5'-tetraisocyanate; and biuret type adducts and isocyanurate ring adducts of these polyisocyanates.

[0077] When the aqueous coating composition of the present invention contains a hydroxyl group-containing polyurethane resin, the content of the hydroxyl group-containing polyurethane resin is preferably 1 to 40 mass%, more preferably 3 to 30 mass%, and even more preferably 5 to 25 mass%, based on the resin solid content in the aqueous coating composition.

[0078] As the crosslinkable component other than the alkyl etherified melamine resin (C), a compound reactive with a hydroxyl group can be suitably used since the hydroxyl-containing resin (A) has a hydroxyl group. Examples of the compound reactive with a hydroxyl group include a polyisocyanate compound, a blocked polyisocyanate compound, and an amino resin other than the alkyl etherified melamine resin (C).

[0079] Also, for example, when the hydroxyl-containing resin (A) has a crosslinkable functional group other than a hydroxyl group, a compound having reactivity with the crosslinkable functional group other than a hydroxyl group can be used as the crosslinkable component.Specifically, for example, when the hydroxyl-containing resin (A) has a carboxyl group, a carbodiimide group-containing compound can be used as the crosslinkable component.

[0080] Examples of the pigment include color pigments, extender pigments, luster pigments, etc. The pigments may be used alone or in combination of two or more kinds.

[0081] When the aqueous coating composition of the present invention contains the above-mentioned pigment, the blending amount of the pigment can be 1 to 100 parts by mass, preferably 2 to 60 parts by mass, and more preferably 3 to 40 parts by mass, based on 100 parts by mass of the resin solids in the aqueous coating composition.

[0082] Examples of the color pigment include titanium oxide, zinc oxide, carbon black, molybdenum red, Prussian blue, cobalt blue, azo pigments, phthalocyanine pigments, quinacridone pigments, isoindoline pigments, threne pigments, perylene pigments, dioxazine pigments, and diketopyrrolopyrrole pigments.

[0083] When the aqueous coating composition of the present invention contains the above-mentioned coloring pigment, the blending amount of the coloring pigment can be 1 to 80 parts by mass, preferably 5 to 50 parts by mass, and more preferably within the range of 10 to 30 parts by mass, based on 100 parts by mass of the resin solids in the aqueous coating composition.

[0084] Examples of the extender pigment include barium sulfate, talc, clay, kaolin, barium carbonate, calcium carbonate, silica, alumina white, etc. As the extender pigment, barium sulfate can be preferably used from the viewpoint of improving design properties, etc.

[0085] When the aqueous coating composition of the present invention contains the above-mentioned body pigment, the blending amount of the body pigment can be 50 parts by mass or less, preferably 3 to 50 parts by mass, and more preferably within the range of 5 to 30 parts by mass, based on 100 parts by mass of the resin solids in the aqueous coating composition of the present invention.

[0086] Examples of the luster pigment include aluminum (including vapor-deposited aluminum), copper, zinc, brass, nickel, glass flake, aluminum oxide, mica, aluminum oxide coated with titanium oxide and / or iron oxide, and mica coated with titanium oxide and / or iron oxide.

[0087] When the aqueous coating composition of the present invention contains the above-mentioned luster pigment, the amount of the luster pigment can be 1 to 80 parts by mass, preferably 5 to 50 parts by mass, and more preferably 10 to 30 parts by mass, based on 100 parts by mass of the resin solids in the aqueous coating composition of the present invention.

[0088] Examples of the organic solvent include ketone-based solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; ester-based solvents such as ethyl acetate, butyl acetate, methyl benzoate, ethyl ethoxypropionate, ethyl propionate, and methyl propionate; alcohol-based solvents such as isopropanol, n-butanol, isobutanol, and 2-ethylhexanol; ether-based solvents such as tetrahydrofuran, dioxane, and dimethoxyethane; glycol ether-based solvents such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and 3-methoxybutyl acetate; aromatic hydrocarbon-based solvents, and aliphatic hydrocarbon-based solvents.

[0089] When used, the aqueous coating composition of the present invention can be diluted by adding water and / or an organic solvent, etc., as necessary, and adjusted to an appropriate viscosity before use in coating.

[0090] The appropriate viscosity varies depending on the coating composition, but for example, when adjusted using a Ford cup viscometer No. 4, the viscosity can usually be adjusted to about 20 to 60 seconds, preferably about 25 to 50 seconds, at 20° C. In addition, in the above, it is suitable that the solids concentration of the aqueous coating composition of the present invention at the time of coating is usually about 5 to 50 mass %, preferably about 10 to 40 mass %.

[0091] The aqueous coating composition of the present invention may be either a one-component coating or a multi-component coating, but is preferably a one-component coating from the viewpoints of excellent productivity since there is no need for a coating mixing process and simplification of maintenance of coating machines.

[0092] The aqueous coating composition of the present invention can be applied to a substrate by a method known per se, such as air spray coating, airless spray coating, rotary atomization coating, curtain coat coating, etc., and electrostatic application may be performed during coating. Among these, air spray coating, rotary atomization coating, etc. are preferred. Furthermore, such coating methods can be performed once or several times until a desired film thickness is obtained.

[0093] The amount of the aqueous coating composition of the present invention to be applied is usually an amount that results in a cured film thickness of 3 to 30 μm, preferably 5 to 25 μm, and more preferably 10 to 20 μm.

[0094] Multi-layer coating method The present invention includes a method for forming a multilayer coating film, in which the aqueous coating composition of the present invention is applied onto a substrate to form a base coat film, and then a clear coat paint is applied onto the base coat film to form a clear coat film.

[0095] As preferred embodiments of the method for forming a multilayer coating film of the present invention, the following methods 1 and 2 can be mentioned.

[0096] <Method 1> (1) A step of applying the aqueous coating composition of the present invention onto a substrate to form an uncured base coat film; (2) applying a clear coat paint composition (Z) onto the uncured base coat film to form an uncured clear coat film; and (3) heating the uncured base coat film and the uncured clear coat film to simultaneously cure them; A method for forming a multilayer coating film comprising the steps of:

[0097] <Method 2> (1) A step of applying an intermediate coating composition onto a substrate to form an uncured intermediate coating film; (2) applying the aqueous coating composition of the present invention onto the uncured intermediate coating film to form an uncured base coat coating film; (3) applying a clear coat paint composition (Z) onto the uncured base coat film to form an uncured clear coat film; and (4) a step of heating the uncured undercoat coating film, the basecoat coating film, and the uncured clearcoat coating film to simultaneously cure them; A method for forming a multilayer coating film comprising the steps of:

[0098] The above-mentioned substrate is not particularly limited, and examples thereof include outer panels of automobile bodies such as passenger cars, trucks, motorcycles, and buses, automobile parts, and outer panels of household electrical appliances such as mobile phones and audio equipment. Of these, the outer panels of automobile bodies and automobile parts are preferred.

[0099] The material of these substrates is not particularly limited. For example, metal materials such as iron, aluminum, brass, copper, tinplate, stainless steel, zinc-plated steel, zinc alloy (Zn-Al, Zn-Ni, Zn-Fe, etc.)-plated steel, polyethylene resin, polypropylene resin, acrylonitrile-butadiene-styrene (ABS) resin, polyamide resin, acrylic resin, vinylidene chloride resin, polycarbonate resin, polyurethane resin, epoxy resin, and other resins, plastic materials such as various FRP, inorganic materials such as glass, cement, concrete, wood, and fiber materials such as paper and cloth. Among these, metal materials and plastic materials are preferred.

[0100] The surfaces of the objects to which the multilayer coating film is applied may be metal surfaces such as the outer panels of automobile bodies, automobile parts, household electrical appliances, and the metal substrates such as the steel plates that make up these products, which have been subjected to surface treatments such as phosphate treatment, chromate treatment, and composite oxide treatment.

[0101] A coating film may be further formed on the object, which may or may not have been surface-treated. For example, the substrate to be coated may be surface-treated as necessary, and an undercoat coating film and / or an intermediate coating film may be formed thereon. For example, when the substrate to be coated is an automobile body, the undercoat coating film and / or intermediate coating film may be formed using a coating composition for undercoat and / or intermediate coating that is known per se and that is usually used in the painting of automobile bodies.

[0102] As the undercoat paint composition for forming the undercoat paint film, for example, an electrodeposition paint, preferably a cationic electrodeposition paint, can be used. Also, as the intermediate coat paint composition for forming the intermediate coat paint film, a paint made of a base resin such as an acrylic resin, a polyester resin, an alkyd resin, a urethane resin, an epoxy resin, etc., having a crosslinkable functional group such as a carboxyl group or a hydroxyl group, an amino resin such as a melamine resin or a urea resin, or a crosslinking agent such as a polyisocyanate compound which may be blocked, together with a pigment, a thickener, and other optional components can be used.

[0103] As the clear coat paint composition (Z), any known thermosetting clear coat paint composition for painting automobile bodies, etc. Examples of the thermosetting clear coat paint composition include an organic solvent-based thermosetting paint composition containing a base resin having a crosslinkable functional group and a curing agent, an aqueous thermosetting paint composition, a powder thermosetting paint composition, etc.

[0104] Examples of the crosslinkable functional group of the base resin include a carboxyl group, a hydroxyl group, an epoxy group, a silanol group, etc. Examples of the type of base resin include an acrylic resin, a polyester resin, an alkyd resin, a urethane resin, an epoxy resin, a fluororesin, etc. Examples of the curing agent include a polyisocyanate compound, a blocked polyisocyanate compound, a melamine resin, a urea resin, a carboxyl group-containing compound, a carboxyl group-containing resin, an epoxy group-containing resin, an epoxy group-containing compound, etc.

[0105] Preferred combinations of base resin / curing agent for the clear coat paint composition (Z) include carboxyl group-containing resin / epoxy group-containing resin, hydroxyl group-containing resin / polyisocyanate compound, hydroxyl group-containing resin / blocked polyisocyanate compound, hydroxyl group-containing resin / melamine resin, etc.

[0106] The clear coat paint composition (Z) may be a one-liquid paint or a multi-liquid paint such as a two-liquid urethane resin paint.

[0107] Furthermore, the above-mentioned clear coat paint composition (Z) may contain color pigments, luster pigments, dyes, etc., as necessary, to the extent that transparency is not impaired. Furthermore, extender pigments, ultraviolet absorbers, light stabilizers, defoamers, thickeners, rust inhibitors, surface conditioners, etc. may be appropriately contained.

[0108] The application method of the clear coat paint composition (Z) is not particularly limited, but examples thereof include air spray coating, airless spray coating, rotary atomization coating, curtain coating, etc., and a wet coating film can be formed by these coating methods. In these coating methods, electrostatic application may be performed as necessary. Among these, air spray coating or rotary atomization coating is particularly preferred. The application amount of the clear coat paint composition (Z) is usually set to an amount that results in a cured film thickness of 10 to 50 μm, preferably 20 to 40 μm.

[0109] In addition, when air spray coating, airless spray coating, or rotary atomization coating is performed, it is preferable to appropriately adjust the viscosity of the clear coat paint composition (Z) using a solvent such as an organic solvent so that the viscosity is within a viscosity range suitable for the coating, usually within a viscosity range of about 15 to 60 seconds, particularly about 20 to 50 seconds, at 20°C using a Ford Cup No. 4 viscometer.

[0110] The heating can be carried out by known means, for example, a drying oven such as a hot air oven, an electric oven, or an infrared induction heating oven. The heating temperature is preferably within a range of 70 to 160° C., more preferably 90 to 150° C. The heating time is not particularly limited, but is preferably within a range of 10 to 60 minutes, more preferably 20 to 40 minutes. EXAMPLES

[0111] The present invention will be described in more detail below with reference to Production Examples, Examples, and Comparative Examples. Note that these Production Examples, Examples, and Comparative Examples are merely illustrative and are not intended to limit the scope of the present invention. In the Production Examples, Examples, and Comparative Examples, "parts" and "%" are based on mass unless otherwise specified. Furthermore, the film thickness of the coating film is based on the cured coating film.

[0112] Preparation of hydroxyl-containing acrylic resin (A1) Manufacturing Example 1 In a reaction vessel equipped with a thermometer, thermostat, stirrer, reflux condenser, nitrogen inlet tube, and dropping device, 130 parts of deionized water and 0.52 parts of "Aqualon KH-10" (trade name, Daiichi Kogyo Seiyaku Co., Ltd., emulsifier, active ingredient 97%) were charged, mixed by stirring in a nitrogen stream, and heated to 80°C. Next, 1% of the total amount of the monomer emulsion (1) described below and 5.3 parts of a 6% aqueous solution of ammonium persulfate were introduced into the reaction vessel and maintained at 80°C for 15 minutes. Thereafter, the remaining monomer emulsion (1) was dropped into the reaction vessel maintained at the same temperature over a period of 3 hours, and after completion of the dropping, the reaction vessel was aged for 1 hour. Then, the following monomer emulsion (2) was added dropwise over 1 hour, and after aging for 1 hour, 40 parts of a 5% dimethylethanolamine aqueous solution was gradually added to the reaction vessel while cooling to 30°C, and the mixture was discharged while filtering through a 100-mesh nylon cloth to obtain a hydroxyl-containing acrylic resin emulsion (A1-1) with a solids concentration of 30%. The obtained hydroxyl-containing acrylic resin emulsion (A1-1) had an acid value of 33 mgKOH / g and a hydroxyl value of 25 mgKOH / g.

[0113] Monomer emulsion (1): 42 parts of deionized water, 0.72 parts of "Aqualon KH-10", 2.1 parts of methylenebisacrylamide, 2.8 parts of styrene, 16.1 parts of methyl methacrylate, 28 parts of ethyl acrylate and 21 parts of n-butyl acrylate were mixed and stirred to obtain a monomer emulsion (1).

[0114] Monomer emulsion (2): 18 parts of deionized water, 0.31 parts of "Aqualon KH-10", 0.03 parts of ammonium persulfate, 5.1 parts of methacrylic acid, 5.1 parts of 2-hydroxyethyl acrylate, 3 parts of styrene, 6 parts of methyl methacrylate, 1.8 parts of ethyl acrylate, and 9 parts of n-butyl acrylate were mixed and stirred to obtain a monomer emulsion (2).

[0115] Manufacturing Example 2 A mixed solvent of 27.5 parts of methoxypropanol and 27.5 parts of isobutanol was placed in a reaction vessel equipped with a thermometer, a thermostat, a stirrer, a reflux condenser and a dropping device, and heated to 110 ° C., and 25 parts of styrene, 27.5 parts of n-butyl methacrylate, 20 parts of "isostearyl acrylate" (trade name, manufactured by Osaka Organic Chemical Industry Co., Ltd., branched higher alkyl acrylate), 7.5 parts of 4-hydroxybutyl acrylate, 15 parts of the following phosphoric acid group-containing polymerizable monomer, 12.5 parts of 2-methacryloyloxyethyl acid phosphate, 10 parts of isobutanol and 4 parts of t-butyl peroxy octanoate were added to the mixed solvent over 4 hours, and a mixture of 0.5 parts of t-butyl peroxy octanoate and 20 parts of isopropanol was added dropwise for 1 hour. After that, the mixture was stirred and aged for 1 hour to obtain a hydroxyl group-containing acrylic resin solution (A1-2) with a solid content concentration of 50%. The resin had a hydroxyl value of 29 mgKOH / g, an acid value due to phosphate groups of 83 mgKOH / g, and a weight average molecular weight of 10,000.

[0116] Phosphate-containing polymerizable monomer: 57.5 parts of monobutyl phosphate and 41 parts of isobutanol were placed in a reaction vessel equipped with a thermometer, a thermostat, a stirrer, a reflux condenser and a dropping device, and the temperature was raised to 90°C. After that, 42.5 parts of glycidyl methacrylate were dropped over 2 hours, and the mixture was further stirred and aged for 1 hour. Then, 59 parts of isopropanol were added to obtain a phosphate-containing polymerizable monomer solution with a solid content concentration of 50%. The acid value of the resulting monomer due to the phosphate group was 285 mgKOH / g.

[0117] Preparation of Hydroxyl-Containing Polyester Resin (A2) Production Example 3 In a reaction vessel equipped with a thermometer, a thermostat, a stirrer, a reflux condenser and a water separator, 109 parts of trimethylolpropane, 141 parts of 1,6-hexanediol, 126 parts of hexahydrophthalic anhydride and 120 parts of adipic acid were charged, and the temperature was raised between 160°C and 230°C over 3 hours, and then condensation reaction was carried out at 230°C for 4 hours. Next, in order to add a carboxyl group to the obtained condensation reaction product, 38.3 parts of trimellitic anhydride were further added, and the reaction was carried out at 170°C for 30 minutes, and then diluted with 2-ethyl-1-hexanol to obtain a hydroxyl group-containing polyester resin solution (A2-1) with a solid content concentration of 70%. The obtained hydroxyl group-containing polyester resin had an acid value of 46 mgKOH / g, a hydroxyl value of 150 mgKOH / g, a solid content concentration of 70%, and a weight average molecular weight of 6,400.

[0118] Production Example 4 In a reactor equipped with a thermometer, agitator, a heater, and a distillation column, 118 parts of 1,6-hexanediol and 102 parts of adipic acid were mixed, and a small amount of xylene for reflux was added. The mixture was gradually heated to 250°C and held at the same temperature for 5 hours to carry out an esterification reaction while dehydrating, to obtain a polyester resin. 102.5 parts of ethylene glycol monobutyl ether and 2.5 parts of orthophosphoric acid were added per 100 parts of the polyester resin, and the mixture was held at 100°C for 3 hours to obtain a hydroxyl group-containing polyester resin solution (A2-2) with a solid content of 50%. The number average molecular weight of the resin was 4,000.

[0119] Pigment dispersion manufacturing Production Example 5 In a stirring and mixing vessel, 19 parts (solid content 14 parts) of aluminum pigment paste “GX-180A” (product name, manufactured by Asahi Kasei Metals Corporation, metal content 74%), 35 parts of 2-ethyl-1-hexanol, 8 parts of the hydroxyl group-containing acrylic resin solution (A1-2) obtained in Production Example 2, and 0.2 parts of 2-(dimethylamino)ethanol were uniformly mixed to obtain a pigment dispersion (P-1).

[0120] Production Example 6 In a stirring and mixing vessel, 19 parts (solid content 14 parts) of aluminum pigment paste “GX-180A” (product name, manufactured by Asahi Kasei Metals Corporation, metal content 74%), 35 parts of 2-ethyl-1-hexanol, 8 parts of the hydroxyl group-containing polyester resin solution (A2-2) obtained in Production Example 4, and 0.2 parts of 2-(dimethylamino)ethanol were uniformly mixed to obtain a pigment dispersion (P-2).

[0121] Preparation of water-based coating composition Example 1 62 parts of pigment dispersion (P-1) obtained in Production Example 5, 100 parts (30 parts solids) of hydroxyl-containing acrylic resin emulsion (A1-1) obtained in Production Example 1, 28.6 parts (20 parts solids) of hydroxyl-containing polyester resin solution (A2-1) obtained in Production Example 3, 5 parts (5 parts solids) of "Sannix PP-200" (trade name, manufactured by Sanyo Chemical Industries, Ltd., polyoxypropylene glycol, 100% solids, number average molecular weight 200, solubility parameter value 11.7), 5 parts (5 parts solids), melamine resin (C-1) (alkyl etherified melamine resin, (methyl group) / ( 51.7 parts (31 parts solids) of "Eukoat UX-8100" (trade name, manufactured by Sanyo Chemical Industries, urethane emulsion, 35% solids) were uniformly mixed, and then 28.6 parts (10 parts solids) of "Eukoat UX-8100" (trade name, manufactured by Rohm and Haas, thickener), 2-(dimethylamino)ethanol and deionized water were added to obtain Water-based Coating Composition No. 1 having a pH of 8.0, a coating solids content of 25%, and a viscosity of 40 seconds according to Ford Cup No. 4 at 20°C.

[0122] Examples 2 to 10, Comparative Examples 1 to 6 Water-based coating compositions Nos. 2 to 16 each having a Ford Cup No. 4 viscosity at 20° C. of 40 seconds were obtained in the same manner as in Example 1, except that the blending compositions were as shown in Table 1 below.

[0123] [Table 1-1]

[0124] [Table 1-2]

[0125] In addition, (*1) to (*13) in the table have the following meanings. (*1) "Sannyx GP250": Product name, manufactured by Sanyo Chemical Industries, polyoxypropylene glyceryl ether, solid content 100%, number average molecular weight 250, solubility parameter value 13.2, (*2) "PTMG250": Product name, manufactured by Mitsubishi Chemical Corporation, polyoxytetramethylene glycol, solid content 100%, number average molecular weight 250, solubility parameter value 11.7, (*3) "Sannyx PP400": Product name, manufactured by Sanyo Chemical Industries, polyoxypropylene glycol, solid content 100%, number average molecular weight 400, solubility parameter value 10.4, (*4) "Sannyx GP400": Product name, manufactured by Sanyo Chemical Industries, Ltd., polyoxypropylene glyceryl ether, solid content 100%, number average molecular weight 400, solubility parameter value 11.5, (*5) "Sannyx GP600": Product name, manufactured by Sanyo Chemical Industries, Ltd., polyoxypropylene glyceryl ether, solid content 100%, number average molecular weight 600, solubility parameter value 10.6, (*6) "PTMG650": Trade name, manufactured by Mitsubishi Chemical Corporation, polyoxytetramethylene glycol, solid content 100%, number average molecular weight 650, solubility parameter value 10.0, (*7) "Sannyx PP600": Product name, manufactured by Sanyo Chemical Industries, polyoxypropylene glycol, solid content 100%, number average molecular weight 600, solubility parameter value 9.8, (*8) "Sannyx PP1000": Product name, manufactured by Sanyo Chemical Industries, polyoxypropylene glycol, solid content 100%, number average molecular weight 1000, solubility parameter value 9.4, (*9) "Sannyx GP1000": Product name, manufactured by Sanyo Chemical Industries, polyoxypropylene glyceryl ether, solid content 100%, number average molecular weight 1000, solubility parameter value 9.9, (*10) "PTMG1000": Product name, manufactured by Mitsubishi Chemical Corporation, polyoxytetramethylene glycol, solid content 100%, number average molecular weight 1000, solubility parameter value 9.7, (*11) Melamine resin (C-2): Alkyl etherified melamine resin, (methyl group) / (butyl group) molar ratio is 30 / 70, solid content is 75%, (*12) Melamine resin (C-3): Alkyl etherified melamine resin, (methyl group) / (butyl group) molar ratio is 70 / 30, solid content is 70%, (*13) Melamine resin (C-4): Alkyl etherified melamine resin, (methyl group) / (butyl group) molar ratio is 100 / 0, solid content is 97%.

[0126] Preparation of intermediate coating composition (V) Intermediate coating composition (V-1) "TP-65-2" (product name, manufactured by Kansai Paint Co., Ltd., polyester resin / amino resin organic solvent-based paint composition) was used as the undercoat paint composition (V-1).

[0127] Intermediate coating composition (V-2) "WP-523H" (product name, manufactured by Kansai Paint Co., Ltd., an acrylic melamine resin-based water-based intermediate coating composition) was used as the intermediate coating composition (V-2).

[0128] Preparation of clear coat paint composition (Z) Clearcoat paint composition (Z-1) "Magicron KINO-1210" (product name, manufactured by Kansai Paint Co., Ltd., acrylic resin-based organic solvent-based topcoat clear coat paint composition, base resin / crosslinker is a combination of carboxyl group-containing resin / epoxy group-containing resin) was used as the clear coat paint composition (Z-1).

[0129] Clearcoat paint composition (Z-2) The amount of surface conditioner in "Magicron KINO-1210" (product name, manufactured by Kansai Paint Co., Ltd., an acrylic resin-based organic solvent-based topcoat clear coat paint composition, with a base resin / crosslinker combination of a carboxyl group-containing resin / epoxy group-containing resin) was reduced by half and used as clear coat paint composition (Z-2).

[0130] Preparation of test plates Example 11 Preparation of test panel A for evaluating water-resistant adhesion A zinc phosphate-treated cold-rolled steel plate of 10 cm x 15 cm was electrocoated with "Elecron GT-10" (trade name, Kansai Paint Co., Ltd., cationic electrocoating paint) to a dry film thickness of 20 μm, and heated at 170 ° C for 30 minutes to cure. Next, on this cured electrocoated coating film, an intermediate coating composition (V-1) was applied to a film thickness of 35 μm, and heated at 140 ° C for 30 minutes to cure. Next, on this cured intermediate coating film, the aqueous coating composition No. 1 obtained in Example 1 was electrostatically coated using a rotary atomizing electrostatic coating machine to a dry film thickness of 15 μm to form an uncured base coat coating film. After leaving it for 3 minutes, it was preheated at 80 ° C for 3 minutes, and then, on the uncured base coat coating film, a clear coat coating composition (Z-1) was electrostatically coated using a rotary atomizing electrostatic coating machine to a cured film thickness of 35 μm to form a clear coat coating film. After leaving it for 7 minutes, it was heated at 140° C. for 30 minutes to simultaneously cure the uncured base coat film and the uncured clear coat film, thereby producing test panel A for evaluating water-resistant adhesion.

[0131] Preparation of test panel B for evaluating cissing resistance Test plate B for evaluating cissing resistance was prepared in the same manner as in the preparation of test plate A, except that in the preparation method of test plate A, the 10 cm x 15 cm zinc phosphate-treated cold-rolled steel plate was replaced with a 30 cm x 45 cm zinc phosphate-treated cold-rolled steel plate, and the clear coat paint composition (Z-1) was replaced with the clear coat paint composition (Z-2).

[0132] Examples 12 to 20, Comparative Examples 7 to 12 Test panel A for evaluating water-resistant adhesion and test panel B for evaluating cissing resistance were prepared in the same manner as in Example 11, except that the aqueous coating composition No. 1 was changed to the aqueous coating composition shown in Table 2.

[0133] Example 21 Preparation of test panel A for evaluating water-resistant adhesion A zinc phosphate-treated cold-rolled steel plate of 10 cm x 15 cm was electrocoated with "Elecron GT-10" (trade name, Kansai Paint Co., Ltd., cationic electrocoating paint) to a dry film thickness of 20 μm, and then heated at 170 ° C for 30 minutes to cure. Next, on this cured electrocoated coating film, an intermediate coating composition (V-2) was applied to a dry film thickness of 20 μm to form an uncured intermediate coating film. After leaving it for 7 minutes, the aqueous coating composition No. 1 obtained in Example 1 was electrostatically coated on the uncured intermediate coating film using a rotary atomizing type electrostatic coating machine to a dry film thickness of 15 μm to form an uncured base coat coating film. After leaving it for 3 minutes, it was preheated at 80 ° C for 3 minutes, and then the clear coat coating composition (Z-1) was electrostatically coated on the uncured base coat coating film using a rotary atomizing type electrostatic coating machine to a cured film thickness of 35 μm to form a clear coat coating film. After leaving it for 7 minutes, it was heated at 140°C for 30 minutes to simultaneously cure the uncured undercoat coating film, the uncured basecoat coating film, and the uncured clearcoat coating film, thereby producing test panel A for evaluating water resistance adhesion.

[0134] Preparation of test panel B for evaluating cissing resistance Test plate B for evaluating cissing resistance was prepared in the same manner as in the preparation of test plate A, except that in the preparation method of test plate A, the 10 cm x 15 cm zinc phosphate-treated cold-rolled steel plate was replaced with a 30 cm x 45 cm zinc phosphate-treated cold-rolled steel plate, and the clear coat paint composition (Z-1) was replaced with the clear coat paint composition (Z-2).

[0135] Examples 22 to 30, Comparative Examples 13 to 18 Test panel A for evaluating water-resistant adhesion and test panel B for evaluating cissing resistance were prepared in the same manner as in Example 21, except that the aqueous coating composition No. 1 was changed to the aqueous coating composition shown in Table 3.

[0136] The test panels obtained above were evaluated by the following test methods. The evaluation results are shown in Tables 2 and 3.

[0137] (Test Method) Water-resistant adhesion: Each test panel A obtained was immersed in 40°C warm water for 240 hours, removed, and dried at 20°C for 12 hours. Then, 100 2mm x 2mm cross-hatch patterns were made on the coating film in accordance with JIS K 5600-5-6 (1990), adhesive tape was applied to the surface, and the tape was quickly peeled off, after which the number of cross-hatch patterns remaining on the coating film was evaluated. ◎ and ○ indicate pass. ◎: Remaining number / total number = 100 / 100 with no chipped edges ○: Remaining number / total number = 100 / 100 with chipped edges △: Remaining number / Total number=99~90 / 100 ×: Remaining number / total number = 89 or less / 100.

[0138] Crack resistance: The obtained test panels B were visually observed and evaluated according to the following criteria: Excellent and Good are acceptable. ◎: No dents or cratering on the painted surface ◯: Small dents are observed on the coating surface, but are not a problem for practical use. △: Several large dents were observed on the coating surface, which was problematic for practical use. ×: Cracks reaching the substrate were observed over the entire coating surface.

[0139] [Table 2]

[0140] [Table 3]

[0141] Although the embodiments and examples of the present invention have been specifically described above, the present invention is not limited to the above-mentioned embodiments, and various modifications based on the technical ideas of the present invention are possible. For example, the configurations, methods, steps, shapes, materials, and values ​​given in the above-mentioned embodiments and examples are merely examples, and configurations, methods, steps, shapes, materials, and values ​​different from these may be used as necessary. In addition, the configurations, methods, steps, shapes, materials, and values ​​of the above-mentioned embodiments can be combined with each other as long as they do not deviate from the gist of the present invention.

Claims

1. (A) an aqueous coating composition for base coat comprising at least one hydroxyl-containing resin selected from (A1) a hydroxyl-containing acrylic resin and (A2) a hydroxyl-containing polyester resin, (B) an oligomer, and (C) an alkyl-etherified melamine resin, The oligomer (B) has a number average molecular weight in the range of 200 to 800 and a solubility parameter value in the range of 10.0 to 13.5; The alkyl-etherified melamine resin (C) has a molar ratio of methyl groups to butyl groups, in terms of a (methyl group) / (butyl group) molar ratio, of 50 / 50 to 0 / 100; The aqueous base coat coating composition is applied to a substrate by anionic electrodeposition coating, except that A water-based paint composition for base coat.

2. (A) an aqueous coating composition for base coat comprising at least one hydroxyl-containing resin selected from (A1) a hydroxyl-containing acrylic resin and (A2) a hydroxyl-containing polyester resin, (B) an oligomer, and (C) an alkyl-etherified melamine resin, The oligomer (B) has a number average molecular weight in the range of 200 to 800 and a solubility parameter value in the range of 10.0 to 13.5; The alkyl-etherified melamine resin (C) has a molar ratio of methyl groups to butyl groups, in terms of a (methyl group) / (butyl group) molar ratio, of 50 / 50 to 0 / 100; The aqueous base coat coating composition is applied to a substrate by air spray coating, airless spray coating, rotary atomization coating, curtain coat coating, or a combination thereof. A water-based paint composition for base coat.

3. 3. The aqueous base coat paint composition according to claim 1, wherein the number average molecular weight of the oligomer (B) is within the range of 200 to 500.

4. 4. The aqueous base coat coating composition according to claim 1, wherein the solubility parameter value of the oligomer (B) is within the range of 10.7 to 13.

5.

5. The aqueous base coat coating composition according to any one of claims 1 to 4, wherein the molar ratio of methyl groups to butyl groups in the alkyl etherified melamine resin (C) is 30 / 70 to 0 / 100 in terms of the molar ratio (methyl groups) / (butyl groups).

6. A method for forming a multilayer coating film, comprising: applying the aqueous base coat coating composition according to any one of claims 1 to 5 onto a substrate to form a base coat coating film; and applying a clear coat coating composition (Z) onto the base coat coating film to form a clear coat coating film.

Citation Information

Patent Citations

  • Waterrbase coating composition

    JP1977107029A

  • Aqueous resin dispersion and water-based coating material composition containing the same

    JP2002308993A

  • Anionic electrodeposition coating and method for forming coating film

    JP2007009059A

  • Emulsion and method of manufacturing the same, and aqueous coating composition using the same

    JP2008274045A

  • Metallic coating composition

    JP2014009288A