Porous silicon microparticles and method for producing same
Patent Information
- Application Number
- JP2022510607
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-27
- Filing Date
- 2021-03-24
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2041-03-24
AI Technical Summary
【0015】 本発明の多孔質シリコン微粒子は、低酸素濃度であるとともに、塩素がシリコンの結晶格子内に存在することにより非晶質である。また、化学的に安定であるため、大気中に保持してもほとんど品質が変化することはない。これに加えて、高度な多孔質構造を有することにより膨張収縮によって破壊せず、しかも、圧密した際にも空隙を保持し、低い嵩密度を維持することができる。それ故、リチウムイオン電池の負極材として用いた際の体積変化を抑制する機能を有するため、シリコン特有の高い充放電容量を有しながら充電時の負極の膨張を効果的に抑制し、充放電の繰り返しに伴う電池性能の低下を効果的に抑制することが可能となる。
Smart Images

Figure 0007562640000003 
Figure 0007562640000001 
Figure 0007562640000002
Abstract
Description
[Technical field]
[0001] The present invention relates to novel porous silicon particles and a method for producing the same. [Background technology]
[0002] Silicon is known as a material for semiconductor substrates and solar cells, but in recent years, its use in a variety of applications, such as as an electrode material (negative electrode material) for lithium-ion secondary batteries, has been proposed.
[0003] Conventionally, carbon materials such as graphite and amorphous carbon have been commonly used as negative electrode materials for lithium-ion secondary batteries; however, their theoretical capacity is low at 372 mAh / g (when graphite is lithiated to LiC6), and a higher-capacity negative electrode material is desired. In addition, silicon has a larger lithium storage capacity per unit mass than carbon materials, with a theoretical capacity of 3,579 mAh / g (Li 15 Because it has an extremely high capacity (when lithiated to Si4), it is being considered as a next-generation anode material.
[0004] One problem with using silicon as a negative electrode material in lithium-ion secondary batteries is the large volume expansion that occurs when the battery is charged, i.e., when silicon and lithium form an alloy and absorb lithium. If the expansion and contraction of silicon due to charging and discharging is large, the following problems arise. First, repeated expansion and contraction causes accumulation of strain energy, which can lead to the silicon breaking into pieces, creating voids and causing a loss of electrical and ionic conductivity, resulting in a decrease in the charge capacity of the negative electrode. Secondly, the expansion and contraction of silicon leads to the expansion and contraction of the entire negative electrode, which causes the negative electrode to peel off from the current collector and electrolyte. Furthermore, the restraining load applied to the entire battery changes, which reduces the battery's charge capacity or makes it impossible to charge and discharge at all. This second problem is serious in conventional lithium-ion batteries that use organic electrolytes, but it is even more serious in next-generation lithium-ion batteries that use semi-solid electrolytes such as gels or solid electrolytes.
[0005] Regarding the first problem, it is known that by microparticulating silicon, the silicon microparticles become less likely to break during expansion and contraction, and durability can be increased (Non-Patent Document 1). However, when the particle size is reduced, the surface area per unit mass (specific surface area) increases, and the amount of oxygen impurities tends to increase due to the oxide film formed on the silicon surface. Since oxygen impurities in silicon irreversibly bind with lithium and cause irreversible capacity, reducing the charging capacity, silicon microparticles with as little oxygen impurity as possible are desired.
[0006] It is also known that the expansion rate of silicon when alloyed with lithium is greater for more crystalline silicon, and the smaller the crystal domains (crystallites) in the particles are and the closer they are to amorphous, the more likely they are to suppress the expansion that accompanies alloying with lithium, especially during the first charge. However, although there are known methods for amorphizing the surface of a silicon substrate to a limited extent, there are no known methods for industrially obtaining amorphous silicon microparticles. In particular, it is very difficult to industrially obtain amorphous silicon microparticles that have a low amount of oxygen impurities, which is desirable for battery materials.
[0007] Regarding the second problem of the large expansion and contraction of the negative electrode as a whole, if the silicon used in the negative electrode has a suitable amount of voids, the voids will mitigate the expansion of the silicon during charging, and the expansion and contraction of the negative electrode as a whole can be suppressed. As a method for making the silicon have voids, there is a method in which the fine particles themselves are made porous and voids are formed inside the fine particles. As a method for making the silicon itself porous, a method is known in which an alloy of silicon and a different metal is phase-separated, and the different metal is removed with an acid or alkali to obtain a porous body (Patent Document 1). However, in this method, silicon is mainly obtained as a crystalline substance, and there are problems such as metal contamination by the different metals and oxidation of silicon when the different metals are dissolved with an acid. In addition, the manufacturing method is complicated, and it is difficult to mass-produce silicon fine particles industrially and inexpensively. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Patent No. 3827642 [Non-patent literature]
[0009] [Non-Patent Document 1] XHLiu et al., “Size-Dependent Fracture of Silicon Nanoparticles During Lithiation”, ACSNANO Vol.6, No.2, pp.1522-1531(2012) Summary of the Invention [Problem to be solved by the invention]
[0010] Therefore, an object of the present invention is to provide porous silicon microparticles that are suitable for use as an electrode material for lithium ion batteries. Another object of the present invention is to provide a method for producing the above-mentioned porous silicon microparticles. [Means for solving the problem]
[0011] The inventors conducted many experiments and investigations into silicon suitable for use as an electrode material in lithium batteries, and as a result discovered that porous silicon microparticles suitable as an electrode material for lithium ion batteries can be obtained by heat-treating silicon microparticles obtained by thermal decomposition of chlorosilane within a certain temperature range, and then further treating them with hydrofluoric acid, thereby completing the present invention.
[0012] According to the present invention, there is provided porous silicon microparticles characterized by having the following properties: (A) average diameter is 80-500 nm; (B) BET specific surface area is 150m 2 / g, 500m 2 / g or less; (C) being amorphous (i.e., no peaks attributable to silicon crystals are detected in X-ray diffraction); (D) the chlorine concentration is in the range of 0.1 to 5.0 mass%; (E) Oxygen concentration in microparticles Co mass% and BET specific surface area Sm 2 / g Co / S is 0.030 or less;
[0013] In the porous silicon microparticles of the present invention, (1) the ratio Co / S of the oxygen concentration Co to the BET specific surface area S is less than 0.010; (2) 30 kN / cm 2 The bulk density when compressed is 0.8 to 1.0 g / cm 3 (Characteristic F), is preferred.
[0014] According to the present invention, there is also provided a method for producing a medicament for a medicament comprising the steps of: A pyrolysis step of pyrolyzing trichlorosilane to obtain silicon fine particle precursor; a dechlorination step of heating the silicon microparticle precursor obtained in the pyrolysis step at a temperature of 570 to 680°C under a supply of an inert gas or under reduced pressure to prepare a specific silicon microparticle precursor having a chlorine concentration adjusted to 20 to 55 mass%; and an etching step of treating the specific fine particle precursor obtained in the dechlorination step with hydrofluoric acid in the presence of an organic solvent compatible with water; The present invention provides a method for producing porous silicon microparticles, comprising the steps of: Effect of the Invention
[0015] The porous silicon microparticles of the present invention have a low oxygen concentration and are amorphous due to the presence of chlorine in the silicon crystal lattice. In addition, since they are chemically stable, their quality hardly changes even when they are kept in the air. In addition, since they have a highly porous structure, they do not break due to expansion and contraction, and they can maintain voids even when compacted, thereby maintaining a low bulk density. Therefore, since they have a function of suppressing volume change when used as a negative electrode material for a lithium ion battery, they can effectively suppress the expansion of the negative electrode during charging while having a high charge and discharge capacity specific to silicon, and can effectively suppress the deterioration of battery performance due to repeated charge and discharge.
[0016] Furthermore, the method for producing porous silicon microparticles of the present invention makes it possible to stably produce porous silicon microparticles having the above-mentioned properties. [Brief description of the drawings]
[0017] [Figure 1] 1 is a scanning electron microscope photograph showing the particle structure of porous silicon microparticles of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] <Porous silicon particles> The porous silicon microparticles of the present invention have the following characteristics (A) to (E).
[0019] (A) Average diameter; The porous silicon microparticles of the present invention have an average diameter in the range of 80 to 500 nm, preferably 100 to 250 nm. By having such a fine particle size, when used as a negative electrode material for a lithium ion battery, damage due to expansion and contraction can be extremely effectively suppressed.
[0020] (B) BET specific surface area; In addition, the porous silicon microparticles of the present invention have the above-mentioned average diameter and at the same time, have a particle size of 150 mm or less. 2 One of its characteristics is that it has an extremely high specific surface area exceeding 100 / g. For example, by observing it with an ultra-high magnification SEM (scanning electron microscope) of 300,000 times magnification, it was confirmed that the fine particles have a porous structure, which is presumed to have significantly increased the specific surface area. And, by adopting such a large specific surface area and porous structure, it is possible to exhibit the characteristic of being able to maintain a low bulk density and retain voids even when compacted, and for example, when used as a negative electrode material for lithium-ion batteries, the effect of suppressing destruction due to expansion and contraction can be further enhanced.
[0021] The specific surface area of the porous silicon particles is 200 m 2 The upper limit of the specific surface area is not particularly limited, but it is preferably 500 m 2 / g or less, especially 450m 2 It is preferable that the molecular weight is not more than 1 / g.
[0022] (C) amorphous; In the porous silicon microparticles of the present invention, no peaks derived from silicon crystals are detected in X-ray diffraction. In other words, because the porous silicon microparticles are amorphous, they have the property of suppressing volume change when used as a negative electrode material for lithium ion batteries.
[0023] (D) Chlorine concentration; The porous silicon microparticles of the present invention contain chlorine at a ratio of 0.1 to 5.0 mass%, preferably 0.5 to 4.5 mass%. That is, as can be understood from the presence of such a chlorine concentration, the porous silicon microparticles of the present invention have chlorine present in the crystal lattice of the silicon constituting the particles, are chemically stable, and the quality hardly changes even when kept in the air. In addition, this makes the porous silicon microparticles amorphous, and exhibits the function of suppressing volume change when used as a negative electrode material for lithium ion batteries.
[0024] (E) Oxygen concentration (Co: mass%) Generally, the oxygen concentration of silicon is mainly due to oxidation of the surface of silicon microparticles, so that as the particle size of the silicon microparticles decreases, the specific surface area increases and the oxygen concentration increases. For this reason, it is difficult to specify the specific surface area and oxygen concentration. However, as described below, the porous silicon microparticles of the present invention have silanol groups removed by hydrofluoric acid treatment and are further terminated with hydrogen to suppress oxidation, so that while they have a large BET specific surface area as described above, their oxygen concentration is low. For example, the oxygen concentration Co (mass%) and the BET specific surface area S (m 2 The ratio Co / S to the total carbon content (C / S) is less than or equal to 0.030 and can be less than 0.010.
[0025] (F) Compacted bulk density; The silicon microparticles of the present invention are porous, and can maintain a low bulk density even when the microparticles are compressed. 2 The bulk density when compressed with a force of 0.8 to 1.0 g / cm 3 , preferably 0.9 to 1.0 g / cm 3In the manufacture of lithium-ion batteries, a process of pressing the negative electrode is generally included, so maintaining a low bulk density even after compaction is important for maintaining sufficient voids in the silicon-containing negative electrode after the battery is formed. These voids serve to mitigate the expansion of the negative electrode caused by the expansion of silicon when the battery is charged, improving the durability of the lithium-ion battery during repeated charging and discharging.
[0026] Incidentally, the above bulk density range is based on the true density of silicon being 2.33 g / cm 3 Converting this into a porosity of 57 to 66%, the preferred range is 61 to 66%.
[0027] As described above, the porous silicon microparticles of the present invention are chemically stable due to the presence of chlorine in the silicon crystal lattice, and are amorphous due to this, and have the function of suppressing volume change when used as a negative electrode material for a lithium ion battery. Furthermore, they are in the form of microparticles that are difficult to break due to expansion and contraction, and have a porous structure, so that they maintain a low bulk density and retain voids even when compacted, and have a high specific surface area but an extremely low concentration of oxygen impurities that cause irreversible capacity. Therefore, it is possible to configure a negative electrode that has a high charge and discharge capacity of silicon, while suppressing the expansion and contraction during charge and discharge, which is a drawback of a negative electrode using silicon, and has little decrease in charge and discharge capacity due to repeated charge and discharge.
[0028] The porous silicon microparticles can be crushed or granulated to a desired aggregate particle size as necessary, and further uniformly dispersed in a desired solvent as necessary, and can then be suitably used, particularly as a negative electrode material for lithium ion secondary batteries.
[0029] The porous silicon microparticles of the present invention can be mixed with various materials known per se, such as a negative electrode material, a conductive assistant, a binder, and other additives, as necessary, and the mixture can be compressed into a powder or dispersed in an arbitrary solvent, and then coated and dried on a current collector to obtain a negative electrode for a lithium battery. Examples of the negative electrode material include synthetic graphite, natural graphite, mesocarbon microbeads (MCMB), and amorphous carbon. Examples of the conductive assistant include acetylene black (AB), ketjen black (KB), fibrous carbon (VGCF), and carbon nanotubes (CNT). Furthermore, examples of the binder include polyvinylidene fluoride (PVDF), styrene-butadiene rubber (SBR), polyimide (PI), polyamide-imide (PAI), polyacrylic acid (PAA), and the like.
[0030] <Method of manufacturing porous silicon particles> The porous silicon particles of the present invention described above are produced using trichlorosilane as a raw material through a thermal decomposition step, a dechlorination step, and an etching step.
[0031] pyrolysis process; In the pyrolysis process, trichlorosilane is used as a silicon source, which is pyrolyzed to obtain silicon particles (silicon microparticle precursor). In this case, trichlorosilane may contain other silicon compounds such as dichlorosilane and silicon tetrachloride, but the amount thereof is desirably 30 mol % or less based on the total moles of the Si source.
[0032] In addition, an inert gas such as nitrogen, argon, or helium can be used as a carrier gas together with the Si source. That is, trichlorosilane has a high boiling point of about 32°C and is easily liquefied, but by mixing it with a carrier gas, it can be maintained in a gaseous state and easily supplied at a fixed amount. The amount of carrier gas is not particularly limited, and it is preferable to use it in the range of 5 to 80% by volume relative to trichlorosilane in order to stabilize the vaporization of trichlorosilane. Of course, by appropriately controlling the vaporization conditions and heating the gas piping, it is also possible to carry out the process industrially without using a carrier gas.
[0033] The reaction vessel is usually a tubular reaction vessel whose inner wall is made of a material such as quartz glass, carbon, etc., and is provided with a heating device capable of heating the inner wall to a predetermined temperature. The method of supplying the source gas to the reaction vessel is not particularly limited, but it is common to supply the source gas to a region heated to a predetermined temperature using a nozzle.
[0034] In this pyrolysis step, trichlorosilane, which is a Si source, is heated to a temperature of 600° C. or more and less than 700° C., preferably 650° C. or more and less than 700° C. As a result, trichlorosilane is pyrolyzed as shown in the following formula (1), for example, to obtain a silicon microparticle precursor containing an intermediate product SiClx (x is 1.0 or less). SiHCl3 →(1-n)SiCl4+nSiClx+(1 / 2)H2(1) In addition to silicon tetrachloride, the by-products also include dichlorosilane and polymeric silanes.
[0035] If the heating temperature is higher than the above range, the reactants do not form fine particles, but are fused to the inner wall of the reaction vessel, causing the reaction vessel to become clogged, and if the heating temperature is lower than the above range, the desired silicon fine particle precursor cannot be obtained in a sufficient yield.
[0036] The silicon fine particle precursor, which is a reaction product, is removed from the reaction vessel together with the exhaust gas and collected, and is separated from hydrogen, silicon tetrachloride, nitrogen, unreacted trichlorosilane, by-product dichlorosilane, polymeric silane, etc. The collection method is not particularly limited, and known methods such as a cyclone-type collection means, a bag filter, and an electric dust collector can be used.
[0037] The collected silicon fine particle precursor is then sent to a dechlorination step. The means for transporting the silicon fine particle precursor is not particularly limited as long as it does not come into contact with oxygen and moisture and is free of contamination from the container.
[0038] For example, the silicon microparticle precursor may be filled in a container made of carbon, aluminum, nickel-coated SUS, or the like after replacing the atmosphere with nitrogen, and then transferred to the dechlorination process. Carbon containers are preferred because they are less susceptible to metal contamination, which is a problem particularly when used as a battery material, and do not denature even when filled with high-temperature particles. Alternatively, the silicon microparticle precursor captured by the known capture means may be accumulated in a hopper or the like, and then entrained in a gas that does not contain oxygen or water, such as nitrogen, and then air-transported through piping.
[0039] Dechlorination process; In the dechlorination step, the silicon microparticle precursor obtained above is introduced into a dechlorination reaction device and dechlorinated by heating at a temperature of 570 to 680° C., more preferably 580 to 650° C. By such dechlorination, the amount of chlorine is adjusted to obtain a specific silicon microparticle precursor.
[0040] Heating in the dechlorination apparatus is carried out under supply of an inert gas not containing oxygen atoms or under reduced pressure. The inert gas is not limited as long as it does not react with the silicon microparticle precursor and does not contain oxygen or water, and gases such as nitrogen, argon, helium, etc. are preferably used. In addition, it is preferable that such an inert gas has a dew point of -50°C or less and has moisture reduced as much as possible. When dechlorination is carried out by heating under reduced pressure, it is preferable to exhaust gas from the dechlorination reaction vessel so that the pressure becomes 1 kPa or less.
[0041] The above-mentioned dechlorination treatment causes the reaction of the following formula (2) to proceed, and a silicon fine particle precursor having an adjusted chlorine concentration is obtained. SiClx →((4-x) / (4-y))SiCly +((xy) / (4-y))SiCl4 (2) In the above formula, x and y are numbers that satisfy x>y>0.
[0042] In the heating of dechlorination, in order to heat the silicon microparticle precursor uniformly, it is preferable to heat the silicon microparticle precursor while stirring it. Stirring can be any known method, such as rolling or shaking the container itself in the reaction device, providing a stirring blade in the reaction device, stirring by air flow, further providing a baffle plate to improve stirring efficiency, or stirring and particle transport can be performed simultaneously, such as a rotary kiln-like device or a screw-type extruder-like device.
[0043] As mentioned above, the temperature of the dechlorination treatment is 570 to 680°C, particularly 580 to 650°C, and is very important for obtaining the desired porous silicon microparticles. That is, by heating at the above temperature for a predetermined time, specifically, for about 2 to 60 minutes, a specific silicon microparticle precursor is obtained in which the chlorine concentration is adjusted to 20 to 55 mass% (roughly calculated as 0.21>y>0.97), preferably 40 to 53 mass% (roughly calculated as 0.53>y>0.89). The specific silicon microparticle precursor having the chlorine concentration adjusted in this manner is efficiently made porous by the subsequent etching step, and becomes silicon microparticles that retain excellent voids even when compacted, i.e., maintain a low bulk density.
[0044] Etching process; The specific silicon fine particle precursor obtained in the above step is treated with hydrofluoric acid (aqueous solution of hydrogen fluoride) in the presence of an organic solvent compatible with water.
[0045] The chlorine groups remaining in the specific silicon fine particle precursor are converted to silanol groups by the moisture contained in hydrofluoric acid, as shown in the following formula (3). -Si-Cl+H2O→-Si-OH+HCl (3)
[0046] It is believed that the silanol groups generated here react with hydrogen fluoride as shown in the following formula to produce hexafluorosilicic acid (H2SiF6), and the silicon surface becomes terminated with hydrogen. [ka]
[0047] It is presumed that the above reaction etches silicon near the silanol groups, making the silicon particles porous.
[0048] In addition, since the silicon fine particle precursor has high water repellency and is difficult to mix directly with hydrofluoric acid, in the present invention, the treatment with hydrofluoric acid is carried out in the presence of an organic solvent that is compatible with water.
[0049] The above-mentioned hydrofluoric acid treatment can be carried out, for example, by the following first to third methods. First method: The silicon fine particle precursor is dispersed in an organic solvent, and then hydrofluoric acid is introduced into the dispersion. Second method: A solution in which hydrofluoric acid is dissolved in an organic solvent is prepared in advance, and then mixed with the specific silicon fine particle precursor. Third method: The silicon fine particle precursor and hydrofluoric acid are mixed, and then mixed with an organic solvent.
[0050] Of the above first to third methods, in order to efficiently mix the silicon fine particle precursor and hydrofluoric acid, the first method is most preferable, and the second method is next most preferable.
[0051] The hydrofluoric acid used in the above treatment is an aqueous solution of hydrogen fluoride. The hydrogen fluoride concentration in commercially available hydrofluoric acid is usually 47 to 48 mass%, but is not particularly limited to this concentration. Since hydrogen fluoride can be handled as a gas, the same effect can be expected by supplying water and hydrogen fluoride gas separately, but when hydrogen fluoride gas is contacted under dehydration conditions, the chlorine in the specific silicon fine particle precursor is not replaced with a silanol group, and the etching reaction that generates the above-mentioned hexafluorosilicic acid does not proceed, so the purpose of the present invention, which is to make the silicon fine particle precursor porous, is not achieved. For this reason, in the present invention, it is preferable to use hydrofluoric acid, which essentially means the coexistence of water and hydrogen fluoride.
[0052] As the organic solvent, one having high affinity with the specific silicon microparticle precursor and hydrofluoric acid is preferred, and specifically, at least one selected from methanol, ethanol, propanol, acetone, IPA (isopropyl alcohol), butanol, isobutanol, sec-butanol, tert-butanol, THF (tetrahydrofuran), and NMP (N-methylpyrrolidone) is preferred.
[0053] The mixing ratio of the specific silicon microparticle precursor and hydrofluoric acid is not particularly limited as long as sufficient water is introduced to sufficiently replace the chlorine in the precursor with silanol groups, and hydrogen fluoride is more than six times the amount of the silanol groups generated; however, it is usually preferable that the water in the hydrofluoric acid is 100 to 1000 mass%, preferably 400 to 500 mass%, relative to the mass of the precursor, and the hydrogen fluoride in the hydrofluoric acid is 100 to 500 mass%, preferably 200 to 300 mass%, relative to the mass of the precursor. The amount of organic solvent used is not particularly limited as long as it is an amount sufficient to uniformly mix the specific silicon microparticle precursor and hydrofluoric acid, but it is preferable that the amount is in the range of 100 to 1000 mass%, preferably 200 to 600 mass%, relative to the mass of the specific silicon microparticle precursor.
[0054] The specific silicon microparticle precursor is mixed with hydrofluoric acid and organic solvent, and can be usually adopted known means such as stirring, shaking, ultrasonic dispersion, etc. in a container.Note that, the mixing method using grinding medium such as ball mill or bead mill oxidizes the highly active surface of the broken silicon microparticle, or the organic solvent is chemically bonded to the silicon microparticle by mechanochemical reaction, so it is preferable to use the mixing means that does not use grinding medium.
[0055] When mixing specific silicon microparticle precursor with hydrofluoric acid and organic solvent, dispersant etc. may be used as appropriate.Dispersant is not particularly limited as long as it is easily volatilized, and anionic surfactants such as carboxylic acid, sulfonic acid, and sulfate ester, cationic surfactants such as amine salt and quaternary ammonium salt, nonionic surfactants such as polyether, ammonia, and bases such as triethanolamine are used, and the amount of use is preferably 5 mass% or less with respect to the mass of specific silicon microparticle precursor.
[0056] The temperature at which the specific silicon microparticle precursor is treated with hydrofluoric acid is not particularly limited as long as it is a temperature at which the organic solvent and hydrogen fluoride do not evaporate, and is usually, but not necessarily, performed at a temperature between room temperature and 80°C.
[0057] The treatment time is not particularly limited, and is about 1 to 120 minutes, so long as the entire mixture is fluidized and mixed.
[0058] In addition, in the hydrofluoric acid treatment, it is not preferable to add an oxidizing agent such as nitric acid or hydrogen peroxide, which is generally used as a method for etching the surface of a silicon wafer. If an oxidizing agent is added, the surface oxidation of the silicon particles and the removal of the oxide proceed vigorously, which causes the volume of the silicon particles to decrease, resulting in a significant drop in the yield, and in extreme cases, the entire silicon particles will dissolve and disappear.
[0059] The specific silicon microparticle dispersion liquid mixed with hydrofluoric acid is dried under heating and / or reduced pressure. This drying process removes the organic solvent, the remaining hydrofluoric acid, the generated hexafluorosilicic acid and water, as well as hydrogen chloride generated by the reaction of chlorine contained in the specific silicon microparticle precursor with water contained in hydrofluoric acid. The heating temperature is not particularly limited, and is carried out at a temperature equal to or higher than the temperature at which the above-mentioned components evaporate. Specifically, it is preferable to heat at atmospheric pressure and at a temperature of 80 to 300°C. The reduced pressure is also not particularly limited as long as the above-mentioned components can be removed, and it is sufficient to reduce the pressure below atmospheric pressure, for example, to a reduced pressure of 40 to 80 torr (about 5 to 10% of standard atmospheric pressure). The drying method is not particularly limited, and for example, static drying may be used, or spin drying, hot air drying, or spray drying may also be used. Furthermore, heating may be carried out during the reduced pressure.
[0060] In addition, it is also a preferred embodiment to subject the silicon microparticle dispersion to solid-liquid separation before drying. As a method for solid-liquid separation, known separation means such as centrifugation, suction filtration, ultrafiltration, and pressure filtration can be used.
[0061] The silicon microparticles obtained under the above-mentioned dechlorination and etching conditions are porous particles with a skeleton of silicon crystals, and can maintain excellent void retention, i.e., high bulk density, even when compacted. This property is important for maintaining sufficient voids in the silicon-containing anode when applied to silicon battery materials, particularly all-solid-state batteries that are constructed by applying high pressure (confining pressure). These voids play a role in mitigating the expansion of the anode caused by the expansion of silicon when the battery is charged, and are considered to be useful because they improve the durability of lithium-ion batteries during repeated charging and discharging, and allow high charging and discharging capabilities to be maintained for a long period of time. EXAMPLES
[0062] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way. Various physical properties and measurements of the silicon microparticles obtained in the following experiments were measured by the following methods.
[0063] (1) Reaction rate of trichlorosilane The reaction rate of trichlorosilane was calculated from the ratio of trichlorosilane, silicon tetrachloride, and dichlorosilane detected by analyzing the composition of the exhaust gas after the reaction by gas chromatography.
[0064] (2) Average diameter of each particle The SEM images of the sample particles were analyzed, and the circle equivalent diameters of 100 particles were calculated, and the average was taken as the average diameter.
[0065] (3) Chlorine concentration in specific silicon particle precursor The specific silicon particle precursor was dispersed in ethanol mixed with 10% by mass of water to replace highly reactive chlorine groups with silanol groups, and the mixture was then evaporated to dryness to obtain a measurement sample. The molar concentrations of the measurement samples were calculated from the chlorine concentration (residual chlorine) measured by X-ray fluorescence analysis and the oxygen concentration (chlorine groups replaced with silanol groups) measured using an oxygen / nitrogen concentration analyzer (LECO TC-600), and the sum of these was calculated as the chlorine molar concentration of the specific silicon microparticle precursor, which was then converted to a mass % concentration.
[0066] (4) Chlorine concentration in porous silicon particles The samples were measured using X-ray fluorescence analysis.
[0067] (5) BET specific surface area of porous silicon particles The specific surface area of the sample was measured using a nitrogen gas BET adsorption method.
[0068] (6) Oxygen concentration in porous silicon particles The oxygen concentration Co (mass%) of the sample was measured using an oxygen / nitrogen concentration analyzer, and the BET specific surface area S (m 3 The values were normalized by dividing by the coefficient of friction (Co) / g and expressed as Co / S.
[0069] (7) Average crystallite size of porous silicon particles The diffraction profile obtained by X-ray diffraction of the sample was analyzed by the Halder-Wagner method. A material in which no peaks derived from silicon crystals could be detected by X-ray diffraction was defined as "amorphous."
[0070] (8) Bulk density of porous silicon microparticles and silicon microparticles when compressed The weighed sample was packed into a cylindrical powder compression die (made of ultra-steel) with a diameter of 10 mm, and pressure was applied to the specified load using a precision universal testing machine (Shimadzu Corporation, Autograph AG-X). The bulk density was calculated from the height and weight of the compressed sample at this time.
[0071] <Example 1> Synthesis of silicon particle precursor (pyrolysis); A graphite reaction tube with an inner diameter of 80 mm and a length of 2,500 mm was heated to 690°C, and trichlorosilane was supplied to it at a rate of 900 g / min and nitrogen gas at a rate of 37 NL (L is liters) / min to synthesize silicon microparticle precursors, which were then separated and collected from unreacted gases using a bag filter. The reaction rate of trichlorosilane was about 40%, and about 70% of the silicon microparticle precursor produced was captured by a bag filter. The captured silicon microparticle precursor was stored in a storage container whose atmosphere was replaced with nitrogen. A portion of the captured silicon microparticle precursor was sampled and observed with an SEM, and the average particle size (average diameter) of the microparticle precursor was found to be about 170 nm.
[0072] Dechlorination of silicon particulate precursors; The silicon fine particle precursor stored in the storage container was supplied to a nitrogen-substituted graphite heating crucible, while taking care not to expose it to the air. An appropriate amount of nitrogen was supplied to the inside of the graphite crucible, and while circulating, the crucible was heated to 580° C. After reaching 580° C., the crucible was held for 1 hour, and then heating was stopped and the crucible was allowed to cool naturally. After cooling, the crucible was opened to the atmosphere, and a specific silicon microparticle precursor having a chlorine concentration of 48.9% by mass was taken out.
[0073] Hydrofluoric acid treatment; 25 g of the specific silicon microparticle precursor obtained was collected in a fluororesin beaker and mixed with 170 g of ethanol, and then hydrofluoric acid prepared by mixing 125 g of 47 mass% hydrofluoric acid (Wako Pure Chemical Industries, special grade reagent) and 50 g of ion-exchanged water was added. The mixture was stirred at room temperature for 5 minutes using a fluororesin stirring rod, left to stand for 1 hour, and then heated and dried at 180°C. The obtained dry powder was transferred to a glass container and dried under reduced pressure at 120° C. for 12 hours in a vacuum dryer to obtain porous silicon microparticles.
[0074] The average diameter of the obtained porous silicon particles was 150 nm, and the BET specific surface area was 441 m 2 / g, was amorphous, and had a chlorine concentration of 1.05% by mass per microparticle mass. Oxygen concentration (Co: mass%) and BET specific surface area (S: m 2 The ratio (Co / S) to the total weight of the alloy was 0.003. The obtained porous silicon particles had a strength of 30 kN / cm 2 The bulk density when compacted is 0.93 g / cm 3 It was.
[0075] <Example 2> Synthesis of silicon particle precursor (pyrolysis); The same method as in Example 1 was used.
[0076] Dechlorination of silicon particulate precursors; The same method as in Example 1 was carried out except that the heating temperature was set to 600° C. The chlorine concentration of the obtained specific silicon fine particle precursor was 48.5 mass %.
[0077] Hydrofluoric acid treatment; 25 g of the specific silicon microparticle precursor obtained was collected in a fluororesin beaker and mixed with 152 g of ethanol, and then hydrofluoric acid prepared by mixing 125 g of 47 mass% hydrofluoric acid (Wako Pure Chemical Industries, special grade reagent) and 50 g of ion-exchanged water was added. The mixture was stirred at room temperature for 5 minutes using a fluororesin stirring rod, left to stand for 1 hour, and then heated and dried at 180°C. The obtained dry powder was transferred to a glass container and dried under reduced pressure at 120° C. for 12 hours in a vacuum dryer to obtain porous silicon microparticles.
[0078] The average diameter of the obtained porous silicon particles was 150 nm, and the specific surface area was 396 m 2 / g, amorphous, and the chlorine concentration was 1.58 mass% per microparticle mass. The oxygen concentration (Co: mass%) and BET specific surface area (S: m 2 The ratio (Co / S) to the total weight of the alloy was 0.009.
[0079] The obtained porous silicon particles had a strength of 30 kN / cm 2 The bulk density when compacted is 0.95g / cm 3 It was.
[0080] <Example 3> Synthesis of silicon particle precursor (pyrolysis); The same method as in Example 1 was used.
[0081] Dechlorination of silicon particulate precursors; The same procedure as in Example 1 was carried out except that the heating temperature was set to 620° C. The chlorine concentration of the obtained specific silicon fine particle precursor was 42.0 mass %.
[0082] Hydrofluoric acid treatment; 25 g of the specific silicon microparticle precursor obtained was collected in a fluororesin beaker and mixed with 175 g of ethanol, and then hydrofluoric acid prepared by mixing 125 g of 47 mass% hydrofluoric acid (Wako Pure Chemical Industries, special grade reagent) and 50 g of ion-exchanged water was added. The mixture was stirred at room temperature for 5 minutes using a fluororesin stirring rod, left to stand for 1 hour, and then heated and dried at 180°C. The obtained dry powder was transferred to a glass container and dried under reduced pressure at 120° C. for 12 hours in a vacuum dryer to obtain porous silicon microparticles.
[0083] The average diameter of the obtained porous silicon particles was 170 nm, and the BET specific surface area was 224 m 2 / g, was amorphous, and had a chlorine concentration of 4.34% by mass based on the mass of the fine particles. Oxygen concentration (Co: mass%) and BET specific surface area (S: m 2 The ratio (Co / S) to the total weight of the alloy was 0.005.
[0084] The obtained porous silicon particles had a strength of 30 kN / cm 2 The bulk density when compacted is 1.00 g / cm 3 It was.
[0085] <Example 4> Synthesis of silicon particle precursor (pyrolysis); The same method as in Example 1 was used.
[0086] Dechlorination of silicon particulate precursors; Except for changing the heating temperature to 640° C. and the holding time to 0.5 hours, the same method as in Example 1 was carried out. The chlorine concentration of the obtained specific silicon fine particle precursor was 51.3 mass %.
[0087] Hydrofluoric acid treatment; 25 g of the specific silicon microparticle precursor obtained was collected in a fluororesin beaker and mixed with 175 g of ethanol, and then hydrofluoric acid prepared by mixing 125 g of 47 mass% hydrofluoric acid (Wako Pure Chemical Industries, special grade reagent) and 50 g of ion-exchanged water was added. The mixture was stirred at room temperature for 5 minutes using a fluororesin stirring rod, left to stand for 1 hour, and then heated and dried at 180°C. The obtained dry powder was transferred to a glass container and dried under reduced pressure at 120° C. for 12 hours in a vacuum dryer to obtain porous silicon microparticles.
[0088] The average diameter of the obtained porous silicon particles was 160 nm, and the BET specific surface area was 200 m 2 / g, was amorphous, and had a chlorine concentration of 1.25% by mass per microparticle mass. Oxygen concentration (Co: mass%) and BET specific surface area (S: m 2 The ratio (Co / S) to the total weight of the alloy was 0.022. The obtained porous silicon particles had a strength of 30 kN / cm 2 The bulk density when compacted is 1.00 g / cm 3 It was.
[0089] <Example 5> Synthesis of silicon particle precursor (pyrolysis); The same method as in Example 1 was used.
[0090] Dechlorination of silicon particulate precursors; The same method as in Example 1 was carried out except that the heating temperature was set to 640° C. The chlorine concentration of the obtained specific silicon fine particle precursor was 20.9 mass %.
[0091] Hydrofluoric acid treatment; 25 g of the specific silicon microparticle precursor obtained was collected in a fluororesin beaker and mixed with 75 g of ethanol, and then hydrofluoric acid prepared by mixing 50 g of 47% by mass hydrofluoric acid (Wako Pure Chemical Industries, special grade reagent) and 50 g of ion-exchanged water was added. The mixture was stirred at room temperature for 5 minutes using a fluororesin stirring rod, left to stand for 1 hour, and then heated and dried at 180°C. The obtained dry powder was transferred to a glass container and dried under reduced pressure at 120° C. for 12 hours in a vacuum dryer to obtain porous silicon microparticles.
[0092] The average diameter of the obtained porous silicon particles was 170 nm, and the BET specific surface area was 225 m 2 / g, was amorphous, and had a chlorine concentration of 1.21% by mass per microparticle mass. Oxygen concentration (Co: mass%) and BET specific surface area (S: m 2 The ratio (Co / S) to the total weight of the alloy was 0.014. The obtained porous silicon particles had a strength of 30 kN / cm 2 The bulk density when compacted is 0.95g / cm 3 It was.
[0093] <Comparative Example 1> Synthesis of silicon particle precursor (pyrolysis); The same method as in Example 1 was used.
[0094] Dechlorination of silicon particulate precursors; The same method as in Example 1 was used.
[0095] Hydrofluoric acid treatment; Not implemented.
[0096] The average diameter of the obtained silicon particles was 170 nm, and the BET specific surface area was 36 m 2 / g, was amorphous, and had a chlorine concentration of 6.24% by mass based on the mass of the fine particles. Oxygen concentration (Co: mass%) and specific surface area (S: m 2 The ratio (Co / S) to the total weight of the alloy was 0.100. The obtained porous silicon particles had a strength of 30 kN / cm 2 The bulk density when compacted is 1.17 g / cm 3 It was.
[0097] <Comparative Example 2> Synthesis of silicon particle precursor (pyrolysis); The same method as in Example 1 was used.
[0098] Dechlorination of silicon particulate precursors; The same method as in Example 1 was carried out except that the heating temperature was set to 720° C. The chlorine concentration of the obtained specific silicon fine particle precursor was 24.2 mass %.
[0099] Hydrofluoric acid treatment; 25 g of the specific silicon microparticle precursor obtained was collected in a fluororesin beaker and mixed with 175 g of ethanol, and then hydrofluoric acid prepared by mixing 125 g of 47 mass% hydrofluoric acid (Wako Pure Chemical Industries, special grade reagent) and 50 g of ion-exchanged water was added. The mixture was stirred at room temperature for 5 minutes using a fluororesin stirring rod, left to stand for 1 hour, and then heated and dried at 180°C. The obtained dry powder was transferred to a glass container and dried under reduced pressure at 120° C. for 12 hours in a vacuum dryer to obtain porous silicon microparticles.
[0100] The average diameter of the obtained porous silicon particles was 170 nm, and the BET specific surface area was 56 m 2 / g, was amorphous, and the chlorine concentration was 6.60 mass% based on the mass of the fine particles. Oxygen concentration (Co: mass%) and BET specific surface area (S: m 2 The ratio (Co / S) to the total weight of the alloy was 0.050. The obtained porous silicon particles had a strength of 30 kN / cm 2 The bulk density when compacted is 1.06 g / cm 3 It was.
[0101] <Comparative Example 3> Synthesis of silicon particle precursor (pyrolysis); The same method as in Example 1 was used.
[0102] Dechlorination of silicon particulate precursors; The same method as in Example 1 was carried out except that the heating temperature was set to 550° C. The chlorine concentration of the obtained specific silicon fine particle precursor was 55.8 mass %.
[0103] Hydrofluoric acid treatment; 25 g of the obtained specific silicon microparticle precursor was placed in a fluororesin beaker and mixed with 126 g of ethanol, and then a mixture of 150 g of 47 mass % hydrofluoric acid (Wako Pure Chemicals Special Grade Reagent) and 50 g of ion-exchanged water was added. The mixture was stirred at room temperature for 5 minutes using a fluororesin stirring rod, then left to stand for 1 hour and then heated and dried at 180°C. As a result, the entire amount of the precursor had dissolved and no porous silicon particles were obtained.
[0104] <Comparative Example 4> Crushed polycrystalline silicon powder (average diameter 5 μm) was dispersed in ethanol and wet-crushed using a bead mill (zirconia beads, diameter 0.05 mm) to obtain plate-shaped microparticles with an average diameter of 200 nm. The BET specific surface area of the obtained silicon particles is 85m 2 / g, the average crystallite diameter was 6 nm, the chlorine concentration was below the detection limit (0.1 mass%), and the oxygen concentration (Co: mass%) and BET specific surface area (S: m 2 The ratio (Co / S) to the total weight of the alloy was 0.129. The obtained porous silicon particles had a strength of 30 kN / cm 2The bulk density when compacted is 1.58g / cm 3 It was.
[0105] The above results are summarized in Table 1.
[0106] [Table 1]
Claims
1. Porous silicon microparticles characterized by having the following properties: A: average diameter is 80 to 500 nm; B: BET specific surface area is 150 m 2 / g, 500m 2 / g or less; C: being amorphous; D: The chlorine concentration is in the range of 0.1 to 5.0 mass%; E: Oxygen concentration Co mass% and BET specific surface area Sm in the fine particles 2 / g, the ratio Co / S is 0.030 or less.
2. 2. The porous silicon particles according to claim 1, wherein the ratio Co / S of the oxygen concentration Co to the BET specific surface area S is less than 0.
010.
3. The porous silicon microparticles according to claim 1, further comprising the following characteristics: F: 30 kN / cm 2 The bulk density when compressed is 0.8 to 1.0 g / cm 3 be within the range.
4. A pyrolysis step of pyrolyzing trichlorosilane to obtain a silicon microparticle precursor; a dechlorination step of heating the silicon microparticle precursor obtained in the pyrolysis step at a temperature of 570 to 680° C. under a supply of an inert gas or under reduced pressure to prepare a specific silicon microparticle precursor having a chlorine concentration adjusted to 20 to 55 mass %; and an etching step of treating the specific fine particle precursor obtained in the dechlorination step with hydrofluoric acid in the presence of an organic solvent compatible with water; 2. A method for producing porous silicon microparticles, comprising:
Citation Information
Patent Citations
Aggregate and method for producing the same
JP2011256057A
Porous silicone
JP2013514252A
Silicon-based particle, lithium ion secondary battery negative electrode active material including the same, and manufacturing methods thereof
JP2017112057A
Negative electrode active material for lithium secondary batteries and method for manufacturing the same, and lithium secondary battery
JP3827642B2
Silicon fine particles and method for producing same
WO2019221157A1