Processing method for iron-gallium alloy single crystal ingot

By growing prismatic iron-gallium alloy single crystals and cutting them along (100) planes, the method addresses inefficiencies in existing processing methods, reducing costs and material loss, and producing high-quality plate-shaped members.

JP7563058B2Active Publication Date: 2024-10-08SUMITOMO METAL MINING CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020150588
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-08
Publication Date
2024-10-08
Estimated Expiration
2040-09-08

AI Technical Summary

Technical Problem

The existing methods for processing iron-gallium alloy single crystals into rectangular plates are inefficient, leading to high processing costs and significant material loss due to the need for extensive manual cutting and the limitations of unidirectional solidification methods in producing smaller ingots.

Method used

A method involving the growth of prismatic iron-gallium alloy single crystals using a prismatic crucible and seed crystal, followed by cutting along the (100) planes with a wire saw, allowing for simultaneous processing of multiple ingots into plate-shaped members.

Benefits of technology

This approach reduces processing steps and costs while minimizing material loss, enabling the production of uniform, low-cost plate-shaped members with improved magnetostrictive properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563058000001
    Figure 0007563058000001
  • Figure 0007563058000002
    Figure 0007563058000002
  • Figure 0007563058000003
    Figure 0007563058000003
Patent Text Reader

Abstract

To provide a growing method and a processing method of a single crystal ingot of an iron gallium alloy, capable of greatly reducing processing cost, when cutting the single crystal ingot of the iron gallium alloy into a rectangular plate, and processing it into a plate-like member.SOLUTION: In a processing method of a single crystal ingot of an iron gallium alloy, the single crystal ingot of the iron gallium alloy has a prism shape, and side faces are all (100) planes, and after flattening pairing side two faces of the single crystal ingot of the iron gallium alloy to the (100) azimuth, the flattened side faces are stuck to form an aggregate of the single crystal ingot, and cut by using a wire saw in parallel with the side face flattened to the (100) azimuth.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for processing a single crystal ingot of an iron-gallium alloy (FeGa alloy), and more particularly to a method for processing a prismatic single crystal ingot of an iron-gallium alloy by a unidirectional solidification crystal growth method in which a melt is solidified in a crucible, such as the Vertical Bridgman method (hereinafter abbreviated as "VB method") or the Vertical Gradient Freeze method (hereinafter abbreviated as "VGF method"). [Background technology]

[0002] Iron-gallium alloys can be machined and exhibit large magnetostriction of about 100 to 350 ppm, making them suitable as materials for magnetostrictive vibration power generators, actuators, and the like, and have been attracting attention in recent years.

[0003] When using iron-gallium alloys in magnetostrictive vibration power generation devices, the magnetization direction is easy. <100> It is necessary to process the iron-gallium alloy into a rectangular plate-shaped magnetostrictive element with the direction of easy magnetization as the longitudinal direction. <100> It is necessary to increase the degree of orientation integration in the direction, and for this purpose it is advantageous to use a single crystal rather than a polycrystal.

[0004] As a method for producing a single crystal of an iron-gallium alloy, Patent Document 1 describes a method for growing a single crystal by a pulling method (Czochralski method, hereinafter also referred to as the "Cz method"). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-28831 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, because single crystals grown by the Cz method are cylindrical ingots, cutting them into rectangular plates poses the problem of increased labor and processing loss of the single crystal alloy.

[0007] In comparison, single crystals grown by unidirectional solidification crystal growth methods, such as the VB method and VGF method, in which the melt is solidified in a crucible, have the same shape as the crucible. When a prismatic crucible is used, it is possible to grow a prismatic single crystal. When this is cut and processed into a rectangular plate, the labor hours and processing loss can be significantly reduced.

[0008] Most of the cost of this processing occurs in the process of cutting the single crystal ingot into plates. By switching from discharge wire cutting to cutting using a wire saw, it is possible to reduce cutting time and processing loss. However, there is a problem in that the cost of materials increases when using a wire saw.

[0009] In addition, the Cz method makes it easier to produce larger single crystal ingots than the unidirectional solidification crystal growth method, but when the unidirectional solidification crystal growth method is used, the single crystal ingots are smaller than those grown by the Cz method, and there is a problem that the cost of wire saw parts per unit weight of the single crystal ingot increases.

[0010] In view of the above circumstances, the present invention aims to provide a method for processing a single crystal ingot of an iron-gallium alloy, which can significantly reduce processing costs when cutting a single crystal ingot of an iron-gallium alloy into a rectangular plate shape and processing it into a plate-shaped member. [Means for solving the problem]

[0011] One aspect of the present invention is a method for processing a single crystal ingot of an iron-gallium alloy, the single crystal ingot of the iron-gallium alloy being shaped into a rectangular column using a rectangular crucible and a seed crystal having a rectangular column shape, the seed crystal having a rectangular column shape being a single crystal of an iron-gallium alloy having all of its side surfaces in a (100) plane, the single crystal ingot of the iron-gallium alloy having a rectangular column shape and all of its side surfaces in a (100) plane, Opposing The method is characterized in that after two side faces are flattened in the (100) direction, the side faces of a plurality of the single crystal ingots that have been flattened in the (100) direction are attached to each other to form a collection of single crystal ingots, and the collection of single crystal ingots is cut using a wire saw parallel to the side faces that have been flattened in the (100) direction.

[0012] In this way, multiple rectangular columnar single crystal ingots of iron-gallium alloy can be cut at once with a wire saw, thereby reducing the number of processing steps required to process them into plate-shaped components, reducing processing losses, and significantly reducing processing costs.

[0013] In this case, in one aspect of the present invention, the iron-gallium alloy single crystal ingot may be shaped into a rectangular column by using any one of a vertical Bridgman method, a vertical temperature gradient solidification method, and a zone melting method.

[0014] In this way, a single crystal ingot of iron-gallium alloy can be grown to fit the shape of the crucible.

[0015] In this case, in one aspect of the present invention, the iron-gallium alloy may contain gallium in an amount of 17 at % or more and 20 at % or less.

[0016] In this way, the iron-gallium alloy can have high magnetostrictive properties, and since the iron-gallium alloy can have a body-centered cubic structure, it is possible to obtain a single crystal ingot whose top, bottom and side surfaces are all (100) faces.

[0017] In one embodiment of the present invention, in the above-mentioned processing method, multiple groups of single crystal ingots formed by bonding the same number of single crystal ingots together may be arranged in parallel in the wire direction, and cut using a wire saw parallel to the side surface that has been flattened in the (100) orientation.

[0018] In this way, more rectangular columnar iron-gallium alloy single crystal ingots can be cut at once with the wire saw, thereby reducing the number of processing steps required to process them into plate-shaped components, reducing processing losses, and significantly reducing processing costs.

[0019] In this case, in one aspect of the present invention, in the above-mentioned processing method, Opposing The two faces of the group of single crystal ingots may be flattened so that the distance between the two faces is constant, and the group may be cut using a wire saw parallel to the side faces flattened in the (100) direction.

[0020] In this way, a plate member with a more uniform thickness can be obtained.

[0021] In this case, in one aspect of the present invention, the wire saw may be a multi-wire saw.

[0022] In this way, the iron-gallium alloy single crystal ingot can be cut into a plurality of plate-shaped parts at the same time, which can further reduce the number of processing steps. Effect of the Invention

[0023] According to the method for growing a single crystal ingot of an iron-gallium alloy of the present invention, the growth axis is <100> It is possible to grow a prismatic iron gallium alloy single crystal ingot in which not only the direction but also the side surface is the (100) plane. In addition, according to the processing method of the iron gallium alloy single crystal ingot of the present invention, it is possible to cut along the side surface of the prismatic iron gallium alloy single crystal ingot, and further to simultaneously cut a plurality of iron gallium alloy single crystal ingots with a wire saw, thereby reducing the processing man-hours when processing into a plate-shaped member, reducing processing loss, and significantly reducing the processing cost. In addition, it is possible to process the iron gallium alloy single crystal ingot into a plate-shaped member at low cost. [Brief description of the drawings]

[0024] [Figure 1] 1 is a schematic cross-sectional view of a growth apparatus for growing an iron-gallium alloy single crystal ingot according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a perspective view showing an example of the shape of a crucible and a seed crystal for growing a cylindrical single crystal ingot according to a comparative example. [Diagram 3] FIG. 2 is a perspective view showing examples of shapes of a crucible and a seed crystal for growing a prismatic single crystal ingot according to an embodiment of the present invention. [Figure 4] 4 is a schematic diagram of a method for processing a single crystal ingot of an iron-gallium alloy according to one embodiment of the present invention. FIG. 4(A) is a perspective view showing a single crystal ingot. FIG. 4(B) is an explanatory diagram of a process for obtaining a first (100) plane from a constant diameter portion. FIG. 4(C) is an explanatory diagram of a process for obtaining a second (100) plane from a constant diameter portion. FIG. 4(D) is a schematic diagram of a method for processing a single crystal ingot using a multi-wire saw. [Diagram 5] 1 is a perspective view showing an example of the shape of a collection of single crystal ingots of iron gallium alloy according to one embodiment of the present invention. FIG. [Figure 6] 6(A) and (B) are schematic diagrams of a method for processing a collection of single crystal ingots using a multi-wire saw. [Figure 7] FIG. 1 is a schematic diagram of a processing method for a plurality of single crystal ingots arranged side by side. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Hereinafter, a method for processing a single crystal ingot of an iron-gallium alloy according to one embodiment of the present invention will be described. Note that the present invention is not limited to the following examples, and can be arbitrarily modified without departing from the gist of the present invention.

[0026] Iron-gallium alloys have the property of producing large magnetostriction in a specific crystal orientation. When using this property in a magnetostrictive vibration power generation device, it is desirable to align the direction in which magnetostriction is required in the magnetostrictive member with the direction in which the crystal magnetostriction is at its maximum. Specifically, as mentioned above, the direction of easy magnetization <100> The iron-gallium alloy must be processed into a rectangular plate-shaped magnetostrictive element with the direction of the magnetostriction being the longitudinal direction. <100> In order to increase the degree of orientation integration in the direction and to improve the properties as a magnetostrictive material, it is advantageous to use a single crystal rather than a polycrystal.

[0027] In the above-mentioned method for growing a single crystal of an iron-gallium alloy (Patent Document 1), a seed crystal having a (100) plane is used, <100> The single crystal is grown by the Cz method with the direction as the growth axis. The single crystal grown by the Cz method is a cylindrical ingot. This ingot is processed into an iron-gallium alloy substrate to be used for a magnetostrictive vibration power generation device.

[0028] When cutting an ingot of an iron-gallium alloy into a plate shape, a discharge wire cutting method is generally used. However, this method requires a large amount of labor because it requires cutting one by one. For this reason, cutting with a multi-wire saw, which is used in processing wafers such as semiconductor devices and solar cells, is also being considered. However, when cutting with a multi-wire saw, the same tension must be applied to multiple wires in the crystal ingot. When applied to a cylindrical single crystal ingot grown by the Cz method, it is cut into a circular shape along a direction perpendicular to the growth axis. In this case, the size of the magnetostrictive vibration power generation device depends on the diameter of the single crystal ingot. If the magnetostrictive vibration power generation device has a relatively small shape, there is no problem, but if it has a long and thin rectangular plate shape, the size of the magnetostrictive vibration power generation device is restricted by the ingot diameter. In addition, in order to cut into a rectangular plate parallel to the growth axis, the ingot must be processed so that the upper and lower surfaces in the cutting direction are at the same height relative to each wire, which increases the labor. In addition, it is necessary to process the upper and lower surfaces parallel to the cutting direction, and the cutting range is limited to these parallel processed surfaces, resulting in significant processing loss.

[0029] The present inventors have conducted extensive research to solve the above-mentioned problems. They have noticed that iron-gallium alloys have a body-centered cubic structure and can be formed into a prismatic single crystal with each side being a (100) plane. They have also noticed that a prismatic single crystal ingot can be grown by a vertical Bridgman method, a vertical temperature gradient freezing method, or the like, using a rectangular crucible. Furthermore, because each side of the prismatic single crystal ingot is all a (100) plane, it can be cut in a direction parallel to the growth axis as well as in a direction perpendicular to the growth axis. <100> The inventors have noted that a single crystal having a rectangular column shape can be processed into a plate shape with the direction of the crystal in the longitudinal direction. Furthermore, the inventors have noted that a single crystal having a rectangular column shape grown by the vertical Bridgman method or the vertical temperature gradient freezing method using a rectangular crucible can be easily cut to the same dimensions because the shape is modeled after the rectangular crucible, and therefore a plurality of single crystals having a rectangular column shape can be lined up and cut simultaneously with a wire saw. Based on these findings, the inventors have completed the present invention. The details will be described below.

[0030] 1. Method for growing iron-gallium alloy single crystal ingots (Iron-gallium alloy single crystal) A method for growing a single crystal ingot of an iron-gallium alloy according to one embodiment of the present invention will be described. An iron-gallium alloy single crystal ingot having magnetostrictive properties can be grown, for example, by placing a seed crystal at the bottom of a crucible, melting a part of the seed crystal and raw material powders of iron and gallium, and gradually solidifying the melt in the crucible from above the seed crystal. Specifically, it can be grown by a unidirectional solidification crystal growth method, such as the VB method or the VGF method. Here, the iron-gallium alloy has a body-centered cubic lattice structure, and the first to third directional indices in the Miller indices are oriented in the direction of magnetostriction. <100> The basis is that the axes are equivalent, and the first to third {100} planes among the plane indices in the Miller indices are equivalent (i.e., (100), (010), and (001) are equivalent).

[0031] The iron-gallium alloy according to one embodiment of the present invention preferably has a gallium content of 17 at% or more and 20 at% or less. With the gallium content in this range, the iron-gallium alloy can obtain high magnetostriction characteristics. Since the iron-gallium alloy can have a body-centered cubic structure, a single crystal ingot can be obtained in which the upper, lower and side surfaces are all (100) faces. When the gallium content is less than 17 at% or exceeds 20 at%, it is difficult for the iron-gallium alloy to obtain high magnetostriction characteristics.

[0032] (Single crystal growth equipment) To more specifically explain the method for growing an iron-gallium alloy single crystal ingot according to one embodiment of the present invention, a single crystal growth apparatus shown in FIG. 1 will first be described as an example of a growth apparatus used in the method.

[0033] Fig. 1 is a schematic cross-sectional view of a single crystal growth apparatus for growing an iron-gallium alloy single crystal ingot according to one embodiment of the present invention. Fig. 1 shows a schematic positional relationship between a single crystal growth crucible (hereinafter also referred to as "crucible") 10, an iron-gallium alloy seed crystal (hereinafter also referred to as "seed crystal") 16, and a mixture of iron and gallium 17 as raw materials in the single crystal growth apparatus 100.

[0034] The single crystal growth apparatus 100 includes a heat insulating material 11, a resistance heater 12 consisting of an upper heater 12a, a middle heater 12b, and a lower heater 12c, a movable rod 13, a crucible receiver 14, a thermocouple 15, a vacuum pump 18, and a chamber 19. The configuration is capable of realizing a temperature distribution in the chamber 19 with a high temperature at the top and a low temperature at the bottom, and a single crystal ingot of an iron-gallium alloy can be grown by gradually solidifying a molten mixture 17 of iron and gallium in the crucible 10 from the top of a seed crystal 16 by a unidirectional solidification crystal growth method such as the VB method or the VGF method.

[0035] As shown in FIG. 1, in a single crystal growth apparatus 100, a carbon resistance heater 12 is disposed inside a heat insulating material 11. When growing a single crystal ingot of an iron-gallium alloy, a hot zone is formed by the resistance heater 12. The resistance heater 12 is composed of an upper heater 12a, a middle heater 12b, and a lower heater 12c, and it is possible to control the temperature gradient in the hot zone by adjusting the power input to these heaters 12a to 12c. There is no particular limitation on the heating method of the single crystal growth apparatus 100 as long as a temperature gradient can be created in the hot zone.

[0036] A single crystal growth crucible 10 is placed inside the resistance heater 12 and placed on a crucible receiver 14 (support) provided with a movable rod 13 that can move up and down. An iron-gallium alloy seed crystal 16 is filled in the lower part of the single crystal growth crucible 10, and a mixture 17 of iron and gallium in the form of particles, flakes, etc. is filled on top of the iron-gallium alloy seed crystal 16 as a raw material.

[0037] The single crystal growth apparatus 100 is equipped with a chamber 19 and a vacuum pump 18, and the inside of the chamber 19 can be adjusted to a vacuum atmosphere to grow a single crystal ingot of an iron-gallium alloy. Furthermore, an inert gas such as argon or nitrogen can be introduced into the chamber 19, and the inside of the chamber 19 can also be adjusted to an inert atmosphere.

[0038] The material of the single crystal growth crucible 10 is preferably alumina, which has low chemical reactivity with the iron-gallium alloy and a high melting point, or may be magnesia or pyrolitic boron nitride.

[0039] As described above, the single crystal growth crucible 10 is placed on the crucible receiver 14 provided with the movable rod 13 in the single crystal growth apparatus 100, and the single crystal growth crucible 10 can be moved up and down in the growth furnace by moving the movable rod 13 up and down. In addition, the single crystal growth crucible 10 is equipped with a thermocouple 15 that can monitor the temperature of the crucible.

[0040] (Method of growing single crystal ingots of iron-gallium alloy) Next, a method for growing a single crystal ingot of an iron-gallium alloy by the VB method using a single crystal growth apparatus will be described with reference to FIG. <100> An iron-gallium alloy seed crystal 16 having a desired orientation is placed on the iron-gallium alloy seed crystal 16. A required amount of a mixture 17 of iron and gallium, which are raw materials, is placed on the iron-gallium alloy seed crystal 16.

[0041] (Melting process) Next, an inert gas such as argon or nitrogen is flowed into the chamber 19 to adjust the inside of the chamber 19 to an inert atmosphere. As the inert gas, it is preferable to introduce argon gas, which is unlikely to generate gallium nitride or the like. After the inside of the chamber 19 becomes an inert atmosphere, the upper heater 12a, the middle heater 12b, and the lower heater 12c arranged to surround the single crystal growth crucible 10 are operated to raise the temperature and start melting the mixture 17 of iron and gallium.

[0042] (nurturing process) Next, a single crystal ingot of iron gallium alloy is grown inside the single crystal growth crucible 10. Specifically, the single crystal growth crucible 10 containing the iron gallium alloy seed crystal 16 and the melt (iron and gallium mixture 17) is heated using the resistance heater 12 so as to have a temperature distribution in which the temperature is high at the top in the height direction and low at the bottom. In this state, the temperature inside the chamber 19 is raised until the iron gallium alloy seed crystal 16 melts to about the upper half in the height direction, and seeding is performed.

[0043] Seeding for growing a single crystal ingot of an iron-gallium alloy is performed by melting the upper part of the iron-gallium alloy seed crystal 16 and the mixture of iron and gallium 17 to form a stable solid-liquid interface. Here, the temperature of the solid-liquid interface and the holding time at that temperature are appropriately set.

[0044] For example, the crucible 10 for single crystal growth is set at a position where the temperature of the interface between the iron-gallium alloy seed crystal 16 and the melt is within the range from the melting point of the iron-gallium alloy to a temperature 20° C. higher than the melting point. These temperatures are maintained for a predetermined time, preferably one hour or more, and the upper part of the iron-gallium alloy seed crystal 16 and the mixture of iron and gallium 17 are melted to perform seeding. The iron-gallium alloy seed crystal 16 is partially melted to be integrated with the mixture of iron and gallium 17, but the entire iron-gallium alloy seed crystal 16 must not be melted.

[0045] After the seeding is completed, the single crystal growth crucible 10 is gradually lowered to pass through the temperature gradient region in the hot zone. In this manner, the melt is cooled and solidified to grow a single crystal ingot of iron-gallium alloy according to the crystal orientation of the iron-gallium alloy seed crystal 16.

[0046] After the entire melt has solidified, it is cooled at a predetermined rate to obtain a single crystal ingot of iron gallium alloy.

[0047] Next, after confirming that the temperature inside the chamber 19 has reached approximately room temperature, the single crystal growth crucible 10 containing the grown single crystal ingot is removed from the crucible receiver 14, and the grown single crystal ingot is then taken out from the single crystal growth crucible 10.

[0048] The above describes a method for growing a single crystal ingot of an iron-gallium alloy by the VB method using a single crystal growth apparatus. However, the same single crystal growth apparatus can also be used to grow a single crystal ingot of an iron-gallium alloy by the VGF method, in which the temperature is controlled by adjusting a resistance heater instead of moving the single crystal growth crucible up and down during the growth of the single crystal ingot.

[0049] In addition, the growth of the single crystal ingot of the iron-gallium alloy in the method of growing the single crystal ingot is not limited to the VB method and the VGF method, and a crystal growth method in which the ingot is solidified in the shape of a crucible can be adopted. For example, a growth method such as a zone melting method can be adopted. In addition, when using the zone melting method, it is necessary to place an iron-gallium raw material with a uniform composition in the crucible, and raw material melting and rapid solidification are required as a pre-growth process.

[0050] (Crucible and seed crystal for growing cylindrical single crystal ingots) Here, as a conventional technique, a crucible and a seed crystal for growing a cylindrical single crystal ingot will be described with reference to FIG. 2. FIG. 2 is a perspective view showing an example of the shape of a crucible and a seed crystal for growing a cylindrical single crystal ingot according to a comparative example. By using a cylindrical crucible and a cylindrical seed crystal as shown in FIG. 2, a cylindrical single crystal ingot is grown according to the shape of the crucible in the above-mentioned single crystal growing apparatus. Note that, as far as a cylindrical single crystal ingot is concerned, a pulling method such as a Cz method can be adopted in addition to the VB method and VGF method. The seed crystal used has (100) faces only on the top and bottom surfaces. Note that the shape of the seed crystal is not limited to a cylindrical shape, and may be a prismatic shape. In this growing method, the single crystal ingot is grown on the top surface of the <100> It is developed with the direction as the growth axis.

[0051] (Crucible and seed crystal for growing prismatic single crystal ingots) A crucible and seed crystal for growing a single crystal ingot according to one embodiment of the present invention will be described with reference to Fig. 3. Fig. 3 is a perspective view showing an example of the shape of a crucible 10 and a seed crystal 16 for growing a prismatic single crystal ingot according to one embodiment of the present invention. By using the rectangular crucible 10 and the prismatic seed crystal 16 as shown in Fig. 3, a prismatic single crystal ingot is grown in accordance with the crucible shape in the above-mentioned single crystal growth apparatus. At this time, the prismatic single crystal has a surface in the growth axis direction that is <100> and the prismatic single crystal is grown so that all of its side faces are (100) faces.

[0052] The seed crystal 16 is a single crystal in a prismatic shape, with the top, bottom, and side surfaces all being (100) planes. Since the iron-gallium alloy according to one embodiment of the present invention is composed of a single phase having a body-centered cubic structure, a single crystal ingot in a prismatic shape, with the top, bottom, and side surfaces all being (100) planes, can be obtained. <100> A single crystal grows in the direction.

[0053] The growth axis direction is <100> Even when a seed crystal 16 having only a crystal growth surface with a (100) plane is used, the longitudinal direction is the growth axis direction. <100> If the seed crystal 16 is processed into a rectangular plate shape so that all side surfaces are (100) planes, it can be used for a vibration power generation device. However, by using a seed crystal 16 with all side surfaces being (100) planes, all side surfaces of the prismatic single crystal ingot can be (100) planes. This makes it easy to cut parallel to the (100) plane, which is also the cleavage plane, and improves surface precision such as thickness and parallelism.

[0054] The crucible 10 has a well-shaped narrow diameter section 10a in which a seed crystal 16 is placed, a tubular increased diameter section 10b in the shape of an inverted pyramid whose diameter increases upward from the narrow diameter section, and a square cylindrical constant diameter section 10c that continues upward from the increased diameter section as a crystal growth section. The inner wall of the increased diameter section 10b has an angle of 30 to 60 degrees with respect to the horizontal direction. This angle is preferably 40 to 50 degrees. If this angle is less than 40 degrees, the increased diameter section becomes unnecessarily long and the cost increases. If it is more than 50 degrees, the grown crystal is likely to become polycrystalline. The angle is preferably around 45 degrees. The cross sections of the narrow diameter section 10a, the increased diameter section 10b, and the constant diameter section 10c each have a square shape. The crucible 10 has a shape in which the center points of each square are the same and the sides of each square are parallel to each other. The size and height of the narrow diameter portion 10a and the constant diameter portion 10c are appropriately determined depending on the size and height of the seed crystal 16 and the single crystal to be grown. The size and height of the larger diameter portion 10b are appropriately determined so as to satisfy the above angle.

[0055] The seed crystal 16 is placed in the narrow diameter portion 10a so that the side surface of the seed crystal 16 is parallel to the inner wall of the narrow diameter portion 10a. <100> In the narrow diameter portion 10a and the increased diameter portion 10b, the single crystal grows in the direction perpendicular to the surface of the seed crystal 16, i.e., vertically upward in the narrow diameter portion 10a, the increased diameter portion 10b, and the constant diameter portion 10c. <100> Here, since the side surface of the seed crystal 16 and the inner wall of the constant diameter portion 10c are parallel, the side surface of the single crystal ingot in contact with the inner wall of the constant diameter portion 10c is a (100) plane.

[0056] As described above, in a method for growing a single crystal ingot according to one embodiment of the present invention, by using a rectangular crucible 10 as shown in FIG. 3 and a rectangular columnar seed crystal 16 having all side surfaces formed as (100) planes, a rectangular columnar single crystal ingot having all side surfaces formed as (100) planes can be grown in a crystal growth apparatus.

[0057] 2. Processing method of iron gallium alloy single crystal ingot Next, a method for processing a single crystal ingot of an iron gallium alloy according to an embodiment of the present invention will be described. In this processing method, a single crystal ingot of an iron gallium alloy is cut in a direction parallel to the growth axis using a single wire saw or a multi-wire saw, and processed into a plate shape. This will be described in detail below.

[0058] (Method of processing cylindrical single crystal ingots) As a conventional technique, an example of cutting the above-mentioned cylindrical single crystal ingot with a multi-wire saw will be described. The cylindrical single crystal ingot is grown by the VB method, the VGF method, the Cz method, or the like, with the top and bottom surfaces being (100) planes.

[0059] First, the seed crystal portion and the diameter-increasing portion of the single crystal ingot are cut to obtain a constant diameter portion. The top and bottom surfaces of the constant diameter portion are then machined so that the first (100) plane perpendicular to the growth axis becomes the top and bottom surfaces of the constant diameter portion. In the case of growth by the VB method, the final solidification surface is almost flat, so no machining is necessary, but in the case of growth by the Cz method, if the final solidification surface has large irregularities, the final solidification surface is also machined to a flat surface.

[0060] Next, in order to cut along the (100) plane parallel to the growth axis, one second (100) plane is processed perpendicular to the first (100) plane. At this time, it is necessary to confirm the orientation by X-ray diffraction. Then, two third (100) planes are processed so that they are perpendicular to the first (100) plane and the second (100) plane so that they can contact each wire in parallel. If the two third (100) planes are not processed here, the surface that contacts the wire when cutting into a plate will be a curved surface. For this reason, the wire will come into contact with an inclined surface, causing problems such as misalignment of the cutting position and the wire coming off the groove of the work roll that supports the wire, making it difficult to process the constant diameter part into a plate.

[0061] After adjusting the number of wire turns so that the wire fits within the third (100) plane processed into a flat surface, the single crystal ingot is processed into a plate shape using a multi-wire saw so that the wire is parallel to the second (100) plane. If the wire does not fit within the third (100) plane, the wire will come into contact with the curved surface between the third (100) plane and the second (100) plane, causing problems such as misalignment of the cutting position and wire coming off the groove of the work roll that supports the wire, making it difficult to process the constant diameter part into a plate shape. For this reason, when the single crystal is cylindrical, it is necessary to rewind the multi-wire saw and adjust the width of the multi-wire saw each time according to the size of the single crystal ingot (the size of the third (100) plane processed into a flat surface), which increases the number of processing steps.

[0062] In this way, when cutting a cylindrical single crystal ingot along the crystal growth axis direction, it is necessary to process the top and bottom surfaces parallel to the cutting direction, and the cutting range is limited to the parallel processed surfaces, resulting in a large amount of processing labor and processing loss. When cutting a cylindrical single crystal ingot along a surface perpendicular to the crystal growth axis direction, the cut single crystal becomes circular, which limits the ingot diameter. It is also possible to cut a cylindrical single crystal ingot from the bottom side (or top side), but the cut crystals will vary in size, which will be an obstacle when processing them into rectangular plates later.

[0063] (Method of processing a rectangular prism-shaped single crystal ingot) A method for processing a prismatic single crystal ingot according to one embodiment of the present invention will be described with reference to Fig. 4(A) to Fig. 4(D). Fig. 4(A) to Fig. 4(D) are schematic diagrams of a method for processing a single crystal ingot of an iron-gallium alloy according to one embodiment of the present invention. A prismatic single crystal ingot is grown by the VB method, VGF method, or the like, with the top, bottom, and side surfaces all being (100) planes. Note that in the Cz method, a single crystal is grown by pulling it up while rotating, so that a prismatic single crystal ingot cannot be grown.

[0064] (single crystal ingot) The single crystal ingot obtained by the above-mentioned growing method will be described with reference to the drawings. FIG. 4(A) is a perspective view showing a single crystal ingot. As shown in FIG. 4(A), a prismatic single crystal ingot 20 has a seed crystal portion 20a, an increased diameter portion 20b, and a constant diameter portion 20c. The seed crystal portion 20a, the increased diameter portion 20b, and the constant diameter portion 20c correspond to the single crystal ingot grown in the narrow diameter portion, the increased diameter portion, and the constant diameter portion of the above-mentioned single crystal growing crucible. The seed crystal portion 20a and the increased diameter portion 20b are cut from the single crystal ingot 20 to obtain the constant diameter portion 20c. The method of cutting the seed crystal portion 20a and the increased diameter portion 20b is not particularly limited.

[0065] (First (100) face) The process of obtaining the first (100) plane from the single crystal ingot 20 will be described with reference to the drawings. FIG. 4(B) is an explanatory diagram of the process of obtaining the first (100) plane from the constant diameter portion. First, the (100) plane perpendicular to the growth axis is identified for the obtained constant diameter portion 20c. There are no particular limitations on the identification method as long as the (100) plane can be identified, but it is preferable to use an X-ray diffraction device from the viewpoint of ease of identification. Then, the upper and lower surfaces of the constant diameter portion 20c are processed by surface grinding so that the (100) plane is perpendicular to the growth axis, and the first (100) plane is obtained.

[0066] In addition, the single crystal ingot is processed into a plate shape using a multi-wire saw so as to be parallel to the second (100) plane, which is the side surface of the single crystal ingot, as a reference, but in the case of a prismatic single crystal ingot, it is possible to process the first (100) plane from the side surface of the constant diameter portion 20c. The second (100) plane, which is the side surface parallel to the growth axis, is specified, and the increasing diameter portion 20b and the constant diameter portion 20c are cut using this second (100) plane as a reference, and the upper and lower surfaces of the constant diameter portion 20c are processed by surface grinding so as to be perpendicular to the second (100) plane, thereby obtaining the first (100) plane.

[0067] (The second (100) face) The process of obtaining the second (100) plane will be described with reference to the drawings. FIG. 4(C) is an explanatory diagram of the process of obtaining the second (100) plane from the constant diameter portion. In the case of a prismatic single crystal ingot, the side surface of the constant diameter portion 20c is almost the (100) plane. The (100) plane parallel to the growth axis of the constant diameter portion 20c is identified based on the side surface. As long as the (100) plane can be identified, the method of identification is not particularly limited, but from the viewpoint of ease of identification, it is preferable to use an X-ray diffraction device. Then, the side surface of the constant diameter portion 20c is processed by surface grinding so that it is parallel to the growth axis, and the second (100) plane is obtained.

[0068] (Single crystal ingot processing) The method of processing a single crystal ingot using a wire saw will be explained with reference to the drawings. FIG. 4(D) is a schematic diagram of the method of processing a single crystal ingot using a multi-wire saw. After obtaining the first (100) and second (100) faces of the constant diameter portion 20c, the constant diameter portion 20c is cut with a multi-wire saw along the growth axis so that the cut surface is parallel to the second (100) plane, and processed into a plate shape. In this case, since the constant diameter portion 20c is in a prismatic state, the surface where the wire contacts the constant diameter portion 20c may be the first (100) face, or may be a third plane perpendicular to the first (100) and second (100) faces.

[0069] Since the contact surface between the multiple wires and the first (100) plane or the third plane is flat, the constant diameter portion 20c can be cut stably. When the single crystal ingot is a cylindrical crystal, as described above, in order to process the constant diameter portion into a plate shape, it is necessary to process the surface that contacts the wire from a curved surface to a flat surface, but this process can be omitted with a single crystal ingot that is prismatic.

[0070] In addition, the number of turns of the multi-wire saw is not particularly limited, and the width of the multi-wire saw is not particularly limited. Depending on the number of turns of the multi-wire saw, the width of the multi-wire saw becomes wider than the width of the constant diameter portion 20c (the minor axis of the third plane). However, the constant diameter portion 20c has a prismatic shape, and when cutting the constant diameter portion 20c, the multi-wire saw outside the constant diameter portion 20c does not come into contact with the constant diameter portion 20c. When the single crystal has a prismatic shape, there is no need to adjust the width of the multi-wire saw, so the processing step when processing into a plate-shaped member can be simplified and the number of steps can be reduced. In addition, by cutting the constant diameter portion 20c along the growth axis, a plate-shaped member longer than the size of the constant diameter portion 20c can be obtained.

[0071] 3. Methods for processing multiple iron-gallium alloy single crystal ingots Next, a plurality of single crystal ingots of the iron gallium alloy according to one embodiment of the present invention are cut in parallel to the growth axis using one wire saw or a multi-wire saw, and processed into a plate shape. This will be described in detail below.

[0072] (Method of processing cylindrical single crystal ingots) A method for simultaneously cutting a plurality of single crystal ingots in a direction perpendicular to the growth axis is known in which two (100) planes perpendicular to the growth axis are machined to be parallel to each other.

[0073] However, in order to simultaneously cut multiple single crystal ingots in a direction parallel to the growth axis, it is possible to first process the first (100) plane perpendicular to the growth axis to beveled, then process two second (100) planes perpendicular to the first (100) plane to beveled, and then attach the second (100) planes in parallel to each other. However, this method gives rise to the same problems as when processing a single cylindrical single crystal ingot.

[0074] (Method of processing a rectangular prism-shaped single crystal ingot) In the case of a prismatic single crystal ingot, two opposing side faces are processed to be (100) planes to form second (100) planes, and the second (100) planes are attached in parallel to each other, so that multiple iron-gallium alloy single crystal ingots can be easily cut with wire at the same time. Figure 5 shows a single crystal ingot formed by attaching three single crystal ingots together.

[0075] The collection of single crystal ingots is processed into a plate shape by cutting the constant diameter portion 20c with a multi-wire saw along the growth axis so that the cut surface is parallel to the second (100) plane. In this case, the surface where the wire contacts the constant diameter portion 20c may be the first (100) plane, or a third plane perpendicular to the first (100) plane and the second (100) plane. Figures 6(A) and 6(B) show a method for processing a collection of single crystal ingots using a multi-wire saw. Here, Figure 6(A) shows a processing method in an embodiment where the wire contacts the third plane perpendicular to the first (100) plane and the second (100) plane. Also, Figure 6(B) shows a processing method in an embodiment where the wire contacts the first (100) plane. The third plane perpendicular to the first (100) plane and the second (100) plane with which the wire contacts includes a parallel plane that pairs with the third plane, and the first (100) plane with which the wire contacts includes a parallel plane that pairs with the first (100) plane.

[0076] In the case of a prismatic single crystal ingot, the dimensions of the faced (100) face can be made uniform by standardizing the growth conditions. Therefore, even after multiple single crystal ingots are bonded together, they will still have a prismatic shape, and can be wire cut in the same way as when there is a single single crystal ingot.

[0077] The method of attachment is not particularly limited, and an appropriate adhesive or the like can be used. For example, an epoxy adhesive can be used.

[0078] The attachment direction is such that the two side faces, which are the second (100) planes, are attached to the second (100) planes. Also, by attaching the faces parallel to the pressing direction of the wire of the multi-wire saw (the direction in which the wire is moved to the single crystal), the plate material having the attachment portion can be easily removed. Also, it is possible to prevent the attachment portion from being included in the magnetostrictive member.

[0079] The number of single crystal ingots to be attached is not particularly limited and can be changed as appropriate. As described above, the number of turns of the multi-wire saw is not particularly limited, and the width of the multi-wire saw is not particularly limited. The number of turns and width of the multi-wire saw can be changed as appropriate depending on the number of single crystal ingots to be attached.

[0080] Before cutting with a wire saw, the surfaces of the collection of single crystal ingots in the direction perpendicular to the crystal growth axis can be appropriately flattened. At this time, all or some of the single crystal ingots in the collection of single crystal ingots can be flattened so that the distance between the two pairs of surfaces in the direction perpendicular to the crystal growth axis is constant. According to the processing method of the single crystal ingot of the present invention, a plate-like member with a uniform thickness can be obtained even if only some of the single crystal ingots have the same length in the crystal growth axis direction. In addition, by making the lengths of all the single crystal ingots in the direction of the crystal growth axis uniform, a plate-like member with a more uniform thickness can be obtained when cutting with a wire saw.

[0081] The single crystal ingot groups may be arranged in two in parallel in the wire direction, or more than two. In this case, the surface where the wire contacts the constant diameter section 20c may be the first (100) surface, or a third plane perpendicular to the first (100) surface and the second (100) surface. FIG. 7 shows a processing method in which two single crystal ingot groups are arranged in parallel in the wire direction so that the first (100) surface contacts the wire. The number of single crystal ingots arranged can be changed as appropriate depending on the width of the wire saw and the orientation of the single crystal ingot groups.

[0082] In this way, the iron gallium alloy single crystal ingot according to one embodiment of the present invention can simplify the processing steps when processing into a plate-shaped member by using a prismatic single crystal ingot, and can reduce the number of steps. In addition, since a prismatic single crystal ingot can be obtained without cutting a cylindrical single crystal ingot, the loss of single crystal due to such cutting is significantly reduced. In addition, the iron gallium alloy single crystal ingot can be processed into a plate-shaped member at low cost. In addition, depending on the cutting direction, a plate-shaped member of an iron gallium alloy single crystal longer than the size of the ingot constant diameter part can be obtained.

[0083] Furthermore, since a plurality of rectangular columnar single crystal ingots can be cut simultaneously, the cost required for cutting can be significantly reduced. EXAMPLES

[0084] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples in any way.

[0085] [Example 1] (Growth of single crystals) First, in an air environment at room temperature of 20°C, the iron raw material and the gallium raw material were weighed out so that the stoichiometric ratio of iron to gallium was 80:20, i.e., the gallium content was 20% by atomic weight. The iron raw material was poured into the gallium raw material that had been melted in a water bath, and after stirring in a container, it was cooled to room temperature to produce a mixture of the raw materials iron and gallium.

[0086] A dense alumina crucible was prepared for growing single crystals. The crucible had a thickness of 4 mm, a narrower diameter section having an inner cylindrical shape with inner dimensions of 5 mm × 5 mm square and a height of 30 mm, a larger diameter section having an inverted square pyramid seed trapezoid shape with a half apex angle of 45°, a constant diameter section having an inner cylindrical shape with inner dimensions of 50 mm × 50 mm, and an overall height of 200 mm.

[0087] The iron-gallium alloy seed crystal was a rectangular parallelepiped with a length of 5 mm, a width of 5 mm, and a height of 30 mm, and was processed with all sides facing (100). The edges were then ground to be chamfered so that the crystal could fit into the crucible. The length and width were then adjusted by machining two of the side faces with a surface grinder, leaving the two side faces uncut to prevent misorientation.

[0088] Then, an iron-gallium alloy seed crystal was filled in the lower part of the single crystal growth crucible, and a mixture of iron and gallium was filled on top of the iron-gallium alloy seed crystal.

[0089] Next, the iron-gallium alloy seed crystal and the crucible for single crystal growth filled with the mixture of iron and gallium were placed on a crucible holder made of porous alumina, and the tip of the thermocouple was brought into contact with the side of the crucible for single crystal growth.

[0090] Next, the movable rod was driven to set the crucible receiver at the lowest position in the chamber. After that, argon gas was introduced into the chamber to adjust the inside of the chamber to an inert atmosphere at atmospheric pressure. The upper, middle and lower heaters, which were made of carbon resistance heaters, were independently controllable and had a height of 200 mm.

[0091] The temperature of the upper heater was set to 1450°C, the temperature of the middle heater to 1400°C, and the temperature of the lower heater to 1300°C, and the temperature inside the chamber was raised. After the temperature inside the chamber was stabilized after the temperature increase, the movable rod was driven to raise the crucible holder, and the crucible for single crystal growth was raised at a gentle speed. Since a temperature gradient was created inside the chamber, with a high temperature at the top and a low temperature at the bottom, the temperature inside the crucible for single crystal growth rose as it moved to the top of the chamber, and the mixture of iron and gallium melted to form a molten material.

[0092] The crucible for single crystal growth was raised so that the temperature of the thermocouple was stable in the range of 1350 to 1400 ° C. near the location of the crucible for single crystal growth where the melt was formed. After the position for holding the crucible for single crystal growth was determined, it was held for 3 hours and seeded, and then the movable rod was driven to lower the crucible for single crystal growth at a speed of 5 mm / h, and the growth of the single crystal of the iron gallium alloy was started. After the lowering distance of the crucible for single crystal growth reached 150 mm, the growth was completed.

[0093] After the above single crystal growth was completed, the grown iron-gallium alloy single crystal ingot was removed from the single crystal growth crucible, yielding an iron-gallium alloy single crystal ingot with a constant diameter portion in the shape of a rectangular column, 50 mm in length, 50 mm in width and 100 mm in length.

[0094] (Crystal processing process) The seed crystal portion and the increased diameter portion of the obtained single crystal ingot were cut by an outer circumferential blade cutter, and one first (100) plane was machined near the cut surfaces of the constant diameter portion and the increased diameter portion.

[0095] Next, the {100} plane of the side surface was identified using an X-ray diffraction device, and a second (100) plane was ground by surface grinding.

[0096] Next, the side surface opposite the second (100) plane was ground so as to be parallel to the second (100) plane.

[0097] Next, one surface of the first (100) plane was subjected to surface grinding so that it was perpendicular to the second (100) plane.

[0098] (Crystal attachment process) Three single crystal ingots were processed using the above procedure, and the second (100) planes of each single crystal ingot were attached to each other with epoxy adhesive so that the first (100) plane was aligned with a third plane perpendicular to the first (100) plane and the second (100) plane.

[0099] With the three single crystal ingots attached, the opposite surface was ground to be parallel to the first (100) plane, and the lengths were made uniform.

[0100] (cutting process) Next, a wire saw with 70 or more turns of 0.16 mm piano wire was prepared using No. 1000 SiC abrasive grains and a 0.7 mm pitch work roller, and the three attached crystals were fixed to the wire saw base on the third plane side so that they were parallel to the second, unattached (100) plane, and cut into plates.

[0101] As a result, 210 iron-gallium alloy single crystal plate members of 100 mm×50 mm×0.5 mm thickness were obtained, and the thickness of the plate members was within 0.5±0.01 mm.

[0102] [Example 2] In the cutting process, the fixing direction to the wire saw pedestal was changed by 90° so that the first (100) plane was on the side, but the iron and gallium single crystals were grown and processed in the same manner as in Example 1, and then cut into plates.

[0103] As a result, 210 iron-gallium alloy single crystal plate members of 100 mm×50 mm×0.5 mm thickness were obtained, and the thickness of the plate members was within 0.5±0.01 mm.

[0104] [Example 3] The crystal attachment process was repeated twice to prepare two sets of single crystal ingots each having three single crystal ingots attached to each other.

[0105] Next, a wire saw was prepared using 1000-number SiC abrasive grains and a 0.7 mm pitch work roller, with 70 or more turns of 0.16 mm piano wire, and the set of three single crystal ingots attached to the left side of the pedestal was fixed to the wire saw pedestal with the first (100) plane side so that they were parallel to the second (100) plane that was not attached. The position of the second (100) plane was aligned so that the wire was in the same position as the first set, and the set of three single crystal ingots attached to the right side of the pedestal was fixed to the wire saw pedestal with the first (100) plane side so that they were parallel to the second (100) plane that was not attached, and cut into plates.

[0106] As a result, 420 iron-gallium alloy single crystal plate members of 100 mm×50 mm×0.5 mm thickness were obtained, and the thickness of the plate members was within 0.5±0.02 mm.

[0107] Furthermore, when the wire saw was fixed to the wire saw base facing the third plane, the width of the wire saw we had was insufficient to allow two sets to be fixed to the base.

[0108] [Example 4] In the same manner as in Example 2, a rectangular columnar iron-gallium alloy single crystal was grown.

[0109] The crystal processing process was carried out in the same manner as in Example 1, except that two of the three single crystal ingots were cut with a peripheral blade so that the width of the plane opposite the first (100) plane was 90 mm, and then the plane was ground.

[0110] The three single crystal ingots were arranged with a width of 90 mm at both ends and 100 mm in the center, and the second (100) planes of each single crystal ingot were attached to each other with epoxy adhesive so that the first (100) plane and the third plane perpendicular to the first (100) plane and the second (100) plane were aligned. Only the central ingot was cut for 10 mm from the start of wire cutting.

[0111] The plates were cut in the same manner as in Example 2. Then, 70 iron-gallium alloy single crystal plate members measuring 100 mm×50 mm×0.5 mm in thickness and 140 iron-gallium alloy single crystal plate members measuring 90 mm×50 mm×0.5 mm in thickness were obtained.

[0112] The thickness of the 140 90 mm x 50 mm plate-like members was within 0.5 ± 0.01 mm.

[0113] The thickness of the 70 100mm x 50mm plate-shaped components was within 0.5±0.02mm, and was thinner at the starting side of the cut.

[0114] [Comparative Example 1] Iron and gallium single crystals were grown and processed in the same manner as in Example 1, and then cut into plates, except that instead of attaching a single single crystal ingot, the crystal was fixed to the wire saw base on the third plane side so that it was parallel to the second (100) plane.

[0115] Then, 70 iron-gallium alloy single crystal plate members of 100 mm×50 mm×0.5 mm thickness were obtained, and the thickness of the plate members was within 0.5±0.01 mm.

[0116] However, the labor and costs required for cutting with a wire saw were the same as in Example 1, and the cost per ingot increased.

[0117] [Comparative Example 2] (Growth of single crystals) As a crucible for growing single crystals, a dense alumina crucible was prepared with a thickness of 4 mm, a narrow diameter part with an inner diameter of 5 mm and a height of 30 mm, a cone-shaped part with a half apex angle of 45°, a constant diameter part with an inner diameter of 52 mm, and an overall height of 200 mm. The iron-gallium alloy seed crystal was processed into a cylindrical shape with a diameter of 5 mm and a height of 30 mm, with the circular parts that were the upper and lower surfaces being the (100) planes. A single crystal ingot was grown in the same manner as in Example 1 except for the above.

[0118] After the single crystal growth was completed, the grown iron-gallium alloy single crystal ingot was removed from the single crystal growth crucible, yielding an iron-gallium alloy single crystal ingot with a cylindrical constant diameter portion having a diameter of 52 mm and a length of 100 mm.

[0119] The seed crystal portion and the increased diameter portion of the obtained single crystal ingot were cut with a peripheral blade. Then, the {100} plane perpendicular to the growth axis was identified using an X-ray diffraction device, and a first (100) plane was machined near the cut surfaces of the constant diameter portion and the increased diameter portion by surface grinding.

[0120] Next, an X-ray diffraction apparatus was used to identify the {100} plane on the side of the cylinder, and a second (100) plane was ground by surface grinding.

[0121] Next, two third planes with a width of 37 mm were machined so as to be perpendicular to the first (100) plane and the second (100) plane, with the distance between these parallel third planes being 36 mm.

[0122] Next, a wire saw was prepared using 1000-number SiC abrasive grains and a 0.7 mm pitch work roller, with 50 turns of 0.16 mm piano wire, and the crystal was fixed so that it was parallel to the second (100) plane, and cut into plates from the third plane. Then, 50 plate-shaped members of the iron-gallium alloy single crystal measuring 100 mm x 37 mm x 0.5 mm were obtained. The thickness of the plate-shaped members was within 0.5 ± 0.01 mm.

[0123] Considering the volume and total number of the plate-shaped iron gallium alloy single crystals, the yield of the plate-shaped members obtained in Comparative Example 2 was about 53% of the yield of the plate-shaped members in Comparative Example 1. In Comparative Example 1, the ratio of the volume of the entire plate-shaped members to the volume of the entire constant diameter portion of the iron gallium alloy single crystal was 70%, while the ratio in Comparative Example 2 was about 44%. From this, it can be seen that Comparative Example 1 has less loss of iron gallium alloy single crystals in processing into plate-shaped members than Comparative Example 2, that is, the loss of iron gallium alloy single crystals in processing into plate-shaped members is less than that in ...

[0124] From the results of the above examples, the growth axis <100> It is understood that when a vibration power generation device is manufactured using the direction, a plate-shaped member of an iron gallium alloy single crystal can be manufactured at low cost compared to the conventional method of Comparative Example 2. Furthermore, it is understood that a plate-shaped member of an iron gallium alloy single crystal can be manufactured at low cost compared to the case of processing ingots one by one of Comparative Example 1.

[0125] Although one embodiment of the present invention and each example have been described in detail above, it will be readily apparent to those skilled in the art that many modifications are possible without substantially departing from the novel features and effects of the present invention. Therefore, all such modifications are intended to be included within the scope of the present invention.

[0126] For example, a term described at least once in the specification or drawings together with a different term having a broader meaning or the same meaning may be replaced with that different term anywhere in the specification or drawings. In addition, the configuration of the method for processing a single crystal ingot of an iron-gallium alloy is not limited to the embodiment of the present invention and each example described above, and various modifications are possible. [Explanation of symbols]

[0127] 10 Single crystal growth crucible, 10a narrow diameter section, 10b increasing diameter section, 10c fixed diameter section, 11 heat insulating material, 12 resistance heater, 12a upper heater, 12b middle heater, 12c lower heater, 13 movable rod, 14 crucible receiver, 15 thermocouple, 16 iron gallium alloy seed crystal, 17 mixture of iron and gallium, 18 vacuum pump, 19 chamber, 20 single crystal ingot, 20a seed crystal section, 20b increasing diameter section, 20c fixed diameter section, 30 wire saw, 100 single crystal growth device

Claims

1. A method for processing a single crystal ingot of an iron-gallium alloy, comprising the steps of: The single crystal ingot of the iron-gallium alloy is shaped into a rectangular column using a rectangular crucible and a seed crystal having a rectangular column shape, The prismatic seed crystal is an iron-gallium alloy single crystal whose side faces are all (100) faces, The iron-gallium alloy single crystal ingot has a rectangular column shape, and all of the side surfaces are (100) faces; A method for processing a single crystal ingot of an iron gallium alloy, comprising the steps of: flattening two opposing side surfaces of the single crystal ingot of the iron gallium alloy in a (100) direction; attaching the side surfaces of a plurality of the single crystal ingots that have been flattened in the (100) direction to each other to form a collection of single crystal ingots; and cutting the collection of single crystal ingots using a wire saw parallel to the side surfaces that have been flattened in the (100) direction.

2. The method for processing a single crystal ingot of an iron-gallium alloy according to claim 1, characterized in that the single crystal ingot of the iron-gallium alloy is shaped into a rectangular column shape by using any one of a vertical Bridgman method, a vertical temperature gradient solidification method, and a zone melting method.

3. 3. The method for processing a single crystal ingot of an iron-gallium alloy according to claim 1, wherein the iron-gallium alloy contains 17 at % or more and 20 at % or less of gallium.

4. The processing method according to claim 1, A method for processing a single crystal ingot of an iron gallium alloy, comprising arranging a plurality of the single crystal ingots formed by bonding the same number of the single crystal ingots together in parallel in the wire direction, and cutting the single crystal ingots using a wire saw parallel to the side surface that has been flattened in the (100) orientation.

5. In the processing method according to claim 1 or 4, A method for processing a single crystal ingot of an iron gallium alloy, comprising: planarizing two surfaces of the group of single crystal ingots so that the distance between the two surfaces facing each other in the direction of the crystal growth axis and the direction perpendicular thereto is constant; and cutting the group of single crystal ingots using a wire saw parallel to the side surfaces planarized in the (100) orientation.

6. 6. The method for processing a single crystal ingot of an iron-gallium alloy according to claim 1, 4 or 5, characterized in that the wire saw is a multi-wire saw.

Citation Information

Patent Citations

  • Method for producing nitride semiconductor substrate

    JP2013060349A

  • METHOD AND APPARATUS FOR GROWING Fe-Ga-BASED ALLOY SINGLE CRYSTAL

    JP2016028831A

  • Rearing method for single crystal ingot of iron gallium alloy and processing method therefor, and single crystal ingot of iron gallium alloy

    JP2020158346A