Manufacturing method of laminate

By discharging and curing two inkjet inks with specific properties to form a laminate, the method addresses the challenge of achieving adhesion and coating film fastness while improving productivity in laminate manufacturing.

JP7563159B2Active Publication Date: 2024-10-08RICOH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020211105
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-21
Publication Date
2024-10-08
Estimated Expiration
2040-12-21

AI Technical Summary

Technical Problem

Existing methods for manufacturing laminates using active energy ray-curable inks face challenges in achieving both adhesion and coating film fastness while maintaining productivity, as they often require separate processes like coating or laminating, which reduce efficiency.

Method used

A method involving the sequential discharge of two active energy ray-curable inkjet inks onto a substrate, where the first ink forms a lower layer with higher static surface tension and the second ink contains polyfunctional polymerizable compounds and inorganic particles, followed by simultaneous curing with active energy rays to form a laminate with improved adhesion and hardness.

Benefits of technology

This approach enables the production of laminates with both strong adhesion and coating film fastness while enhancing productivity by integrating the curing process, preventing ink mixing and ensuring robustness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563159000006
    Figure 0007563159000006
  • Figure 0007563159000001
    Figure 0007563159000001
  • Figure 0007563159000002
    Figure 0007563159000002
Patent Text Reader

Abstract

To provide a method for manufacturing a laminate which achieves both adhesion and coated film fastness and has good productivity.SOLUTION: There is provided a method for manufacturing a laminate that forms a first ink layer composed of first active energy ray-curable inkjet ink on a base material, forms a second ink layer composed of second active energy ray-curable inkjet ink on the first ink layer, then irradiates the first ink layer and the second ink layer with active energy rays, and forms a first curable layer and a second curable layer, in which static surface tension γ1 of the first active energy ray-curable inkjet ink is larger than static surface tension γ2 of the second active energy ray-curable inkjet ink, and the second active energy ray-curable inkjet ink contains 10 mass% or more and 40 mass% or less of a polyfunctional polymerizable compound having a weight average molecular weight (Mw) of 500 or more, and contains 1 mass% or more and 30 mass% or less of inorganic particles.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a laminate. [Background technology]

[0002] Traditionally, active energy ray curable inks, which are cured using active energy rays such as ultraviolet (UV) and electron beams (EB), have been supplied and used in offset, silk screen, topcoat agents, etc., but their usage has increased in recent years due to the advantages of cost reduction by simplifying the drying process and reducing the amount of solvent volatilization as an environmental measure. Recently, as an industrial application, their use in decorative printing and coating, especially using inkjet, has increased due to their on-demand nature. However, in terms of inkjet suitability, there is generally a trade-off between coating film robustness and adhesion, and inkjet ink coating alone often cannot meet market demands. Therefore, it becomes necessary to apply a separate coating or lamination, but adding a separate process reduces productivity.

[0003] Patent Document 1 proposes a method for improving adhesion to non-penetrating substrates by forming a multi-layer coating film using inks with different contact angles to the substrate. By using this method, it is possible to achieve both coating film fastness and adhesion. Patent Document 2 proposes a method of forming an image (layer) by discharging an ultraviolet curing material onto the liquid surface of an ultraviolet curing resin liquid by an inkjet method. Patent Document 3 proposes a method for forming a multilayer coating film in a wet-on-wet manner in an actinic radiation-curable inkjet ink containing a gelling agent and a white pigment. By using this method, it is possible to prevent the mixing of different inks by using a gelling agent. Summary of the Invention [Problem to be solved by the invention]

[0004] The method of Patent Document 1 employs a process of printing each layer of the multi-layer coating one by one, which reduces productivity. The method of Patent Document 2 forms a layer, but aims to spread the image pattern thinly on the surface, and it is difficult to impart a robust function because the film thickness of the upper layer is thin. An object of the present invention is to provide a method for producing a laminate which achieves both adhesion and coating fastness and has good productivity. [Means for solving the problem]

[0005] As a means for solving the above problems, the present invention relates to a method for producing a laminate as described below. A step of ejecting a first active energy ray-curable inkjet ink onto a substrate to form a first ink layer; a step of ejecting a second active energy ray curable inkjet ink onto the first ink layer to form a second ink layer; a step of irradiating the first ink layer and the second ink layer with active energy rays to cure the first ink layer to form a first cured layer and to cure the second ink layer to form a second cured layer; A method for producing a laminate having the first curable layer and the second curable layer, comprising: When the static surface tension of the first active energy ray curable inkjet ink is γ1 (mN / m) and the static surface tension of the second active energy ray curable inkjet ink is γ2 (mN / m), γ1 and γ2 satisfy the relationship of the following formula (1), γ1>γ2 (1) the second active energy ray curable inkjet ink contains 10% by mass or more and 40% by mass or less of a polyfunctional polymerizable compound having a weight average molecular weight (Mw) of 500 or more, and contains 1% by mass or more and 30% by mass or less of inorganic particles; A method for producing a laminate comprising the steps of: Effect of the Invention

[0006] According to the present invention, it is possible to provide a method for producing a laminate having both adhesion and coating fastness and good productivity. [Brief description of the drawings]

[0007] [Figure 1] 1 is a schematic diagram showing an example of an apparatus for carrying out the method for producing a laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The method for producing a laminate of the present invention will be described below with reference to the drawings. Note that the present invention is not limited to the following embodiments, and may be modified, added, modified, deleted, or otherwise altered within the scope of what a person skilled in the art can conceive, and any embodiment is within the scope of the present invention as long as it exhibits the functions and effects of the present invention.

[0009] In the method for producing a laminate of the present invention, a first active energy ray-curable ink-jet ink and a second active energy ray-curable ink-jet ink are used. The method for producing the laminate of the present invention includes the following steps. A step of ejecting a first active energy ray-curable inkjet ink onto a substrate to form a first ink layer. A step of ejecting a second active energy ray curable inkjet ink onto the first ink layer to form a second ink layer. a step of irradiating the first ink layer and the second ink layer with active energy rays to harden the first ink layer to form a first hardened layer and harden the second ink layer to form a second hardened layer. When the static surface tension of the first active energy ray curable inkjet ink is γ1 (mN / m) and the static surface tension of the second active energy ray curable inkjet ink is γ2 (mN / m), γ1 and γ2 satisfy the relationship of the following formula (1). γ1>γ2 (1) The second active energy ray curable inkjet ink contains 10% by mass or more and 40% by mass or less of a polyfunctional polymerizable compound having a weight average molecular weight (Mw) of 500 or more, and contains 1% by mass or more and 30% by mass or less of inorganic particles.

[0010] As described above, the method for producing a laminate of the present invention can improve productivity by forming a laminate structure consisting of a first ink layer and a second ink layer using a first ink-jet ink and a second ink-jet ink, and irradiating the first ink layer and the second ink layer with active energy rays to simultaneously cure the first ink layer and the second ink layer.

[0011] Furthermore, by making the static surface tension (γ1 [mN / m]) of the inkjet ink larger than the static surface tension (γ2 [mN / m]) of the second active energy ray-curable inkjet ink, it is possible to prevent the second inkjet ink from penetrating into the first inkjet ink layer.

[0012] In addition, the second active energy ray-curable inkjet ink contains, in its total amount, 10% by mass or more and 40% by mass or less of a polyfunctional polymerizable compound having a weight average molecular weight (Mw) of 500 or more, and thus can exhibit high hardness without impairing adhesion.

[0013] Furthermore, when the second inkjet ink contains inorganic particles in an amount of 1% by mass or more and 30% by mass or less in total, the inorganic particles are oriented at a high density on the coating film surface, thereby achieving both adhesion and robustness. This is because, when droplets of the second inkjet ink land on the liquid layer of the first inkjet ink, monofunctional monomers with low molecular weights contained in the second inkjet ink diffuse into the liquid layer of the first inkjet ink, increasing the density of inorganic particles in the droplets of the second inkjet ink, and increasing the density of inorganic particles in the layer of the second inkjet ink, thereby improving the hardness of the coating film and also improving adhesion due to the effect of suppressing surface peeling.

[0014] Inkjet ink The ink-jet ink of the present invention uses at least a first actinic energy ray-curable ink-jet ink and a second actinic energy ray-curable ink-jet ink in combination, each of which has different physical properties.

[0015] The material composition of the inkjet ink is not particularly limited. Since the monomer and surfactant have a large effect on the physical properties of the obtained cured product, it is preferable to select an appropriate one according to the physical properties of the target cured product. In addition to the monomer and surfactant, the inkjet ink further contains a polymerization initiator, a coloring material, a polymerization inhibitor, a diluting solvent, and other known components as necessary. Hereinafter, the first active energy ray-curable inkjet ink may be referred to as the "first inkjet ink", and the second active energy ray-curable inkjet ink may be referred to as the "second inkjet ink".

[0016] <Laminate> The laminate of the present invention comprises at least a first cured layer made of a cured product of a first ink-jet ink and a second cured layer made of a cured product of a second ink-jet ink. The first cured layer is located in the lower layer of the laminate and therefore preferably has a function of adhesion, and the second cured layer is located in the upper layer of the laminate and therefore preferably has a function of coating fastness.

[0017] <Monomer> The monomer is a compound that undergoes a polymerization reaction and hardens due to active energy rays (ultraviolet rays, electron beams, etc.) or active species generated by active energy rays, and includes polyfunctional monomers and monofunctional monomers depending on the number of functional groups. The monomer may be polymerizable, and may include a polymerizable oligomer or polymerizable polymer (macromonomer). There are no restrictions on the type of monomer for each inkjet ink, but since the first inkjet ink is located as the lower layer of the laminate, it is preferable for it to have adhesion functionality, and it is preferable for it to contain a large amount of monofunctional monomer, and it is preferable for it to contain 50% by mass or more of monofunctional monomer.

[0018] Since the second inkjet ink is located in the upper layer of the laminate, it is preferable to provide a coating fastness function, and it is preferable to include 45% by mass or more of a monofunctional monomer and 10% to 40% by mass or less of a polyfunctional monomer having Mw of 500 or more, and more preferably 15% to 30% by mass or less. When a layer is formed in a liquid state using the first inkjet ink and the second inkjet ink, the components contained in the second inkjet ink may diffuse into the layer made of the first inkjet ink, thereby reducing the substrate adhesion. By including 45% by mass or more of a monofunctional monomer and 10% to 40% by mass or less of a polyfunctional monomer having Mw of 500 or more in the second inkjet ink, high substrate adhesion can be maintained even if the monofunctional monomer diffuses into the layer made of the first inkjet ink, and the polyfunctional monomer has a certain molecular weight, making it difficult to diffuse, and remaining in the layer made of the second inkjet ink, it is possible to achieve both high adhesion and coating fastness. If the polyfunctional monomer is included in an amount of more than 40% by mass, it becomes impossible to maintain substrate adhesion. The content of the polyfunctional monomer in the inkjet inks preferably satisfies the relationship: [content of the polyfunctional monomer in the first inkjet ink < content of the polyfunctional monomer in the second inkjet ink]. If the first inkjet ink contains an excessive amount of polyfunctional monomer, adhesion decreases due to the effect of cure shrinkage, and if the second inkjet ink contains a small amount of polyfunctional monomer, sufficient hardness is not achieved.

[0019] As the polyfunctional monomer, it is preferable to use a difunctional monomer, a trifunctional monomer, or a (meth)acrylate monomer having a higher number of functional groups. The polyfunctional monomer is not particularly limited as long as it has a weight average molecular weight (Mw) of 500 or more, and can be appropriately selected depending on the purpose. The weight average molecular weight (Mw) can be measured using a gel permeation chromatography device manufactured by Shimadzu Corporation. Examples of polyfunctional monomers include neopentyl glycol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, (poly)tetramethylene glycol di(meth)acrylate, propylene oxide of bisphenol A ( PO) adduct di(meth)acrylate, ethoxylated neopentyl glycol di(meth)acrylate, propoxylated neopentyl glycol di(meth)acrylate, ethylene oxide (EO) adduct di(meth)acrylate of bisphenol A, EO modified pentaerythritol tri(meth)acrylate, PO modified pentaerythritol tri(meth)acrylate, EO modified pentaerythritol tetra(meth)acrylate, PO modified pentaerythritol tetra(meth)acrylate, EO modified dipenta Erythritol tetra(meth)acrylate, PO modified dipentaerythritol tetra(meth)acrylate, EO modified trimethylolpropane tri(meth)acrylate, PO modified trimethylolpropane tri(meth)acrylate, EO modified tetramethylolmethane tetra(meth)acrylate, PO modified tetramethylolmethane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate Acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, trimethylolethane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, bis(4-(meth)acryloxypolyethoxyphenyl)propane, diallyl phthalate, triallyl trimellitate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,10-Decanediol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, tetramethylolmethane tri(meth)acrylate, dimethyloltricyclodecane di(meth)acrylate, modified glycerin tri(meth)acrylate, bisphenol A diglycidyl ether (meth)acrylic acid adduct, modified bisphenol A di(meth)acrylate, caprolactone modified dipentaerythritol hexa(meth)acrylate, dipentaerythritol hexa(meth)acrylate, pentaerythritol Examples of the urethane prepolymer include tri(meth)acrylate tolylene diisocyanate urethane prepolymer, pentaerythritol tri(meth)acrylate hexamethylene diisocyanate urethane prepolymer, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate hexamethylene diisocyanate urethane prepolymer, urethane acrylate oligomer, epoxy acrylate oligomer, polyester acrylate oligomer, polyether acrylate oligomer, and silicone acrylate oligomer. These may be used alone or in combination of two or more.

[0020] The monofunctional monomer is a monomer having one functional group. The monofunctional monomer is not particularly limited and can be appropriately selected depending on the purpose. For example, hydroxyethyl (meth)acrylamide, (meth)acryloylmorpholine, dimethylaminopropylacrylamide, isobornyl (meth)acrylate, adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, 3,3,5-trimethylcyclohexane (meth)acrylate, Examples of the acrylate include tert-butyl methacrylate, tetrahydrofurfuryl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl acrylate, isobutyl acrylate, tert-butyl acrylate, phenoxyethyl acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl acrylate, and cyclic trimethylolpropane formal acrylate. These may be used alone or in combination of two or more.

[0021] <Surfactant> The surfactant has the effect of preventing the compositions of the first ink-jet ink and the second ink-jet ink from mixing with each other when the ink-jet ink and the second ink-jet ink are in liquid form to form layers. It is preferable that each inkjet ink contains a small amount of a surfactant as necessary, and it is preferable that at least the second inkjet ink contains a surfactant, and it is preferable that the surfactant is contained in an amount of 0.01% by mass to 1% by mass. This is because if an excessive amount of surfactant is added, the antifouling properties and ejection stability in inkjet printing are impaired. In addition, if the amount of surfactant added is small or no surfactant is included, when the first inkjet ink and the second inkjet ink are liquid and form a layer, the inks mix with each other, which causes a failure to achieve both adhesion and coating fastness. As the surfactant, one type may be used alone, or two or more types may be used in combination.

[0022] <Inorganic particles> By adding the inorganic particles to the second inkjet ink, the inorganic particles are oriented at a high density on the coating surface, and both robustness and adhesion can be achieved. This is because, when droplets of the second inkjet ink land on the liquid layer of the first inkjet ink, monofunctional monomers with low molecular weights diffuse into the liquid layer of the first inkjet ink, increasing the density of the inorganic particles in the droplets of the second inkjet ink. Increasing the density of inorganic particles in the layer of the second inkjet ink improves the hardness of the coating, and also improves adhesion due to the effect of suppressing surface peeling.

[0023] The inorganic particles are not particularly limited and can be appropriately selected depending on the purpose. The inorganic particles are preferably silica. This is because silica is particularly likely to be oriented on the coating surface and to exhibit hardness. The average primary particle size of the inorganic particles is preferably 30 nm or more and 1 μm or less, and more preferably 100 nm or more. This is because the larger the average primary particle size of the inorganic particles, the higher the hardness of the coating film. By making the average primary particle size of the inorganic particles 1 μm or less, it is possible to suppress the decrease in ejection stability.

[0024] The blending ratio of inorganic particles is preferably 1% by mass or more and 30% by mass or less, more preferably 5% by mass or more and 20% by mass or less. This is because if the blending amount of inorganic particles is small, the above-mentioned effect of inorganic particles cannot be obtained sufficiently, and if the blending amount of inorganic particles is excessive, the inorganic particles tend to settle in the inkjet head, and the ejection stability is impaired. As the inorganic particles, one type may be used alone, or two or more types may be used in combination.

[0025] <Curing means> The curable ink-jet ink of the present invention can be cured by heat curing or by curing with active energy rays, and among these, curing with active energy rays is preferred. The active energy rays used to cure the active energy ray-curable inkjet ink of the present invention are not particularly limited, and may be any rays capable of imparting energy necessary for promoting the polymerization reaction of the polymerizable component in the composition, such as ultraviolet rays, electron beams, α rays, β rays, γ rays, and X-rays. In particular, when a high-energy light source is used, the polymerization reaction can be promoted without using a polymerization initiator. In addition, in the case of ultraviolet irradiation, mercury-free devices are strongly desired from the viewpoint of environmental protection, and replacement with GaN-based semiconductor ultraviolet light-emitting devices is very useful industrially and environmentally. Furthermore, ultraviolet light-emitting diodes (UV-LEDs) and ultraviolet laser diodes (UV-LDs) are small, have a long life, are highly efficient, and are low cost, making them preferable as ultraviolet light sources.

[0026] <Polymerization initiator> The active energy ray curable inkjet ink of the present invention may contain a polymerization initiator. The polymerization initiator may be any one that can generate active species such as radicals or cations by the energy of active energy rays and initiate polymerization of a polymerizable compound (monomer or oligomer). As such a polymerization initiator, known radical polymerization initiators, cationic polymerization initiators, base generators, etc. may be used alone or in combination of two or more kinds, and among them, it is preferable to use a radical polymerization initiator. In addition, in order to obtain a sufficient curing speed, the polymerization initiator is preferably contained in an amount of 5 to 20% by mass with respect to the total mass (100% by mass) of the inkjet ink. Examples of the radical polymerization initiator include aromatic ketones, acylphosphine oxide compounds, aromatic onium salt compounds, organic peroxides, thio compounds (thioxanthone compounds, thiophenyl group-containing compounds, etc.), hexaarylbiimidazole compounds, ketoxime ester compounds, borate compounds, azinium compounds, metallocene compounds, active ester compounds, compounds having a carbon-halogen bond, and alkylamine compounds. In addition to the polymerization initiator, a polymerization accelerator (sensitizer) can also be used in combination. The polymerization accelerator is not particularly limited, but for example, amine compounds such as trimethylamine, methyldimethanolamine, triethanolamine, p-diethylaminoacetophenone, ethyl p-dimethylaminobenzoate, 2-ethylhexyl p-dimethylaminobenzoate, N,N-dimethylbenzylamine, and 4,4'-bis(diethylamino)benzophenone are preferred, and the content thereof may be appropriately set according to the polymerization initiator used and its amount.

[0027] <Coloring material> The active energy ray curable inkjet ink of the present invention may contain a coloring material. As the coloring material, various pigments or dyes that impart glossy colors such as black, white, magenta, cyan, yellow, green, orange, gold, and silver can be used depending on the purpose and required characteristics of the inkjet ink of the present invention. The content of the coloring material may be appropriately determined in consideration of the desired color density and dispersibility in the inkjet ink, and is not particularly limited, but is preferably 0.1 to 20% by mass with respect to the total mass (100% by mass) of the composition. The active energy ray curable inkjet ink of the present invention may be colorless and transparent without containing a coloring material, and in that case, it is suitable as an overcoat layer for protecting an image, for example. Although the addition of coloring materials to the inkjet ink combination of the present invention is optional, it is particularly preferable that the second inkjet ink that lands last is a color ink for drawing that contains coloring materials or a clear ink that does not contain coloring materials, which makes it easy to arrange droplet dots with high precision. The first inkjet ink that serves as a base is preferably a white ink or a clear ink. As the pigment, an inorganic pigment or an organic pigment can be used, and one type may be used alone, or two or more types may be used in combination. Examples of inorganic pigments that can be used include carbon blacks (CI Pigment Black 7) such as furnace black, lamp black, acetylene black, and channel black, iron oxide, and titanium oxide. Examples of organic pigments include azo pigments such as insoluble azo pigments, condensed azo pigments, azo lakes, and chelate azo pigments; polycyclic pigments such as phthalocyanine pigments, perylene and perinone pigments, anthraquinone pigments, quinacridone pigments, dioxane pigments, thioindigo pigments, isoindolinone pigments, and quinophthalone pigments; dye chelates (e.g., basic dye chelates, acid dye chelates, etc.); dye lakes (basic dye lakes, acid dye lakes), nitro pigments, nitroso pigments, aniline black, and daylight fluorescent pigments. In order to improve the dispersibility of the pigment, a dispersant may be further included. The dispersant is not particularly limited, but examples thereof include dispersants commonly used in preparing pigment dispersions, such as polymer dispersants. As the dye, for example, acid dyes, direct dyes, reactive dyes, and basic dyes can be used, and one type may be used alone, or two or more types may be used in combination.

[0028] <Organic solvent> The active energy ray curable inkjet ink of the present invention may contain an organic solvent, but preferably does not contain an organic solvent if possible. If the composition does not contain an organic solvent, particularly a volatile organic solvent (VOC (Volatile Organic Compounds)-free), the safety of the place where the composition is handled is improved and it is also possible to prevent environmental pollution. Note that the term "organic solvent" refers to a general non-reactive organic solvent such as ether, ketone, xylene, ethyl acetate, cyclohexanone, toluene, etc., and should be distinguished from a reactive monomer. In addition, "not containing" an organic solvent means that the organic solvent is substantially not contained, and it is preferably less than 0.1% by mass.

[0029] <Other ingredients> The active energy ray-curable inkjet ink of the present invention may contain other known components as necessary. The other components are not particularly limited, and examples thereof include conventionally known polymerization inhibitors, leveling agents, defoamers, fluorescent brighteners, penetration promoters, wetting agents (moisturizing agents), fixing agents, viscosity stabilizers, antifungal agents, preservatives, antioxidants, ultraviolet absorbers, chelating agents, pH adjusters, and thickeners.

[0030] <Preparation of active energy ray-curable composition> The actinic ray-curable inkjet ink of the present invention can be prepared using the various components described above. The preparation means and conditions are not particularly limited. For example, the inkjet ink can be prepared by feeding a polymerizable monomer, a pigment, a dispersant, etc. into a dispersing machine such as a ball mill, a Kitty mill, a disk mill, a pin mill, or a Dyno mill, dispersing the ingredients to prepare a pigment dispersion, and then mixing a polymerizable monomer, an initiator, a polymerization inhibitor, a surfactant, etc. into the pigment dispersion.

[0031] <Viscosity> The viscosity of the active energy ray curable inkjet ink of the present invention may be appropriately adjusted depending on the application and application means, and is not particularly limited. For example, when an ejection means is used that ejects the composition from a nozzle, the viscosity in the range of 20°C to 65°C, desirably the viscosity at 25°C is preferably 3 to 40 mPa·s, more preferably 5 to 15 mPa·s, and particularly preferably 6 to 12 mPa·s. It is particularly preferable that the viscosity range is satisfied without containing the organic solvent. The viscosity can be measured by a cone-plate type rotational viscometer VISCOMETER TVE-22L manufactured by Toki Sangyo Co., Ltd., using a cone rotor (1°34'×R24), with a rotation speed of 50 rpm and a temperature of the constant temperature circulating water appropriately set in the range of 20°C to 65°C. A VISCOMATE VM-150III can be used to adjust the temperature of the circulating water.

[0032] <Application>

[0043] The use of the active energy ray-curable inkjet ink of the present invention is not particularly limited as long as it is in a field in which active energy ray-curable materials are generally used, and can be appropriately selected depending on the purpose. Examples of the use include molding resins, paints, adhesives, insulating materials, release agents, coating materials, sealing materials, various resists, and various optical materials. The present invention also includes a molded article obtained by processing a cured product obtained by curing the active energy ray-curable ink-jet ink or a structure on a substrate on which the cured product is formed. The molded article is, for example, a product obtained by subjecting a cured product or structure formed into a sheet or film shape to a molding process such as heat stretching or punching, and is suitably used for applications requiring molding after surface decoration, such as meters and operation panels for automobiles, office automation equipment, electric and electronic devices, and cameras. The substrate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the substrate include paper, thread, fiber, cloth, leather, metal, plastic, glass, wood, ceramics, and composite materials thereof. From the viewpoint of processability, a plastic substrate is preferred.

[0033] <Composition storage container> The inkjet ink storage container of the present invention means a container in which an active energy ray-curable inkjet ink is stored, and is suitable for use in the above-mentioned applications. For example, when the active energy ray-curable composition of the present invention is used for ink, the container in which the ink is stored can be used as an ink cartridge or ink bottle, which eliminates the need to directly touch the ink during ink transport, ink replacement, and other operations, and can prevent the staining of hands, fingers, and clothing. In addition, it is possible to prevent the inclusion of foreign matter such as dust in the ink. The shape, size, material, and the like of the container itself may be any suitable one for the application and usage, and are not particularly limited, but it is preferable that the material is a light-shielding material that does not transmit light, or that the container is covered with a light-shielding sheet or the like.

[0034] <Image forming method and apparatus> The image forming method of the present invention may use active energy rays or heating. In order to cure the curable inkjet ink of the present invention with active energy rays, an irradiation step of irradiating active energy rays is included, and the image forming apparatus of the present invention includes an irradiation means for irradiating active energy rays and a storage section for storing the active energy ray curable inkjet ink of the present invention, and the storage section may store the container. Furthermore, the apparatus may include a discharge step and a discharge means for discharging the active energy ray curable inkjet ink. The discharge method is not particularly limited, and examples thereof include a continuous jet type and an on-demand type. Examples of the on-demand type include a piezo type, a thermal type, and an electrostatic type. FIG. 1 is a schematic diagram showing an example of an image forming apparatus equipped with an inkjet ejection means according to the present invention. Using a head unit (movable in the AB direction) in which inkjet heads are arranged, a first inkjet ink 22 is ejected from a head unit 25, and a second inkjet ink 23 having a composition different from that of the first inkjet ink is ejected from a head unit 26, and these inkjet inks are laminated while being cured by an adjacent active energy ray irradiation device 27. The head units 25 and 26 may be provided with a heating mechanism so that the ink is liquefied in the ink ejection section. If necessary, a mechanism for cooling the substrate 21 to about room temperature by contact or non-contact may be provided. In addition, as the inkjet recording method, any of a serial method in which the head is moved to eject ink onto the recording medium that moves intermittently according to the ejection head width, and a line method in which the recording medium is moved continuously and ink is ejected onto the recording medium from a head held at a fixed position. The substrate 21 is not particularly limited, but may be paper, film, ceramics, glass, metal, a composite material thereof, or the like, and may be in the form of a sheet. The substrate may be configured to allow only one-sided printing, or may be configured to allow both-sided printing. The substrate is not limited to those used as general recording media, and may be cardboard, building materials such as wallpaper and flooring, concrete, cloth for clothing such as T-shirts, textiles, leather, or the like, as appropriate. Recorded matters recorded with the ink of the present invention include not only those printed on smooth surfaces such as ordinary paper or resin film, but also those printed on uneven printing surfaces and those printed on printing surfaces made of various materials such as metals and ceramics. In addition, by laminating two-dimensional images, it is also possible to form an image with a partially three-dimensional effect (an image consisting of two and three dimensions) or a three-dimensional object. EXAMPLES

[0035] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way. In the following examples, "parts" means "parts by mass" and "%" means "% by mass".

[0036] <Preparation of Inorganic Particle Dispersion> (Preparation of Inorganic Particle Dispersion A) 56 parts of AEROSIL 50 (manufactured by Nippon Aerosil Co., Ltd.), 40 parts of monofunctional monomer TMCHA (manufactured by Osaka Organic Chemical Industry Ltd.), and 4 parts of SOLSPERSE32000 (manufactured by Lubrizol) were added and stirred for 24 hours in a bead mill to prepare [inorganic particle dispersion A].

[0037] (Preparation of Inorganic Particle Dispersion B) 56 parts of X-24-9600A (Shin-Etsu Chemical Co., Ltd.), 40 parts of monofunctional monomer TMCHA (Osaka Organic Chemical Industry Ltd.), and 4 parts of SOLSPERSE32000 (Lubrizol) were added and stirred for 24 hours in a bead mill to prepare [Inorganic Particle Dispersion B].

[0038] (Preparation of Inorganic Particle Dispersion C) 56 parts of Sicastar (manufactured by Corefront Co., Ltd.), 40 parts of monofunctional monomer TMCHA (manufactured by Osaka Organic Chemical Industry Co., Ltd.), and 4 parts of SOLSPERSE32000 (manufactured by Lubrizol) were added and stirred for 24 hours in a bead mill to prepare [inorganic particle dispersion C].

[0039] (Preparation of Inorganic Particle Dispersion D) 56 parts of titanium oxide (white ink colorant) (manufactured by Dai Nippon Printing Co., Ltd.), 40 parts of monofunctional monomer TMCHA (manufactured by Osaka Organic Chemical Industry Ltd.), and 4 parts of SOLSPERSE32000 (manufactured by Lubrizol) were added and stirred for 24 hours in a bead mill to prepare [Inorganic Particle Dispersion D].

[0040] <Preparation of active energy ray curable inkjet ink> (Preparation of First Inkjet Ink) Based on the materials and contents (parts by mass) shown in Table 1-1, actinic ray curable inkjet inks 1 to 3, which are the first inkjet inks, were prepared by a conventional method.

[0041] (Preparation of second inkjet ink) Based on the materials and contents (parts by mass) shown in Tables 1-1 and 1-2, actinic ray-curable inkjet inks, inks 4 to 19, which are the second inkjet inks, were prepared by a conventional method.

[0042] The compositions and physical properties of Inks 1 to 19 are shown in Tables 1-1 and 1-2. Furthermore, while "inorganic particles" are shown as a blending component in Tables 1-1 and 1-2, the compositions and physical properties of inks 4 to 19 when "inorganic particle dispersion" is shown as a blending component are shown in Table 2. In Table 2, the inorganic particle dispersion contains the monofunctional monomer TMCHA, so the values ​​shown in the column for monofunctional monomer TMCHA in Tables 1-1 and 1-2 are different from the values ​​shown in the column for monofunctional monomer TMCHA in Table 2.

[0043] The trade names and manufacturer names of the compounds shown in Tables 1-1, 1-2 and 2 are as follows:

[0044] <Monomer> (Monofunctional Monomer) ·ACMO: Acryloylmorpholine - KJ Chemicals Co., Ltd. NVC: N-vinylcaprolactam - Tokyo Chemical Industry Co., Ltd. PEA: Phenoxyethyl acrylate (Osaka Organic Chemical Industry Ltd.) TMCHA: 3,5,5, trimethylcyclohexyl acrylate (Osaka Organic Chemical Industry Ltd.) (Polyfunctional Monomer) DPGDA: Dipropylene glycol diacrylate (Osaka Organic Chemical Industry Ltd.) Molecular weight 242 DPHA: Dipentaerythritol hexaacrylate (manufactured by Nippon Kayaku Co., Ltd.) molecular weight 524 CN963: Aliphatic urethane acrylate (manufactured by Sartomer) Viscoat #1000: Tripentaerythritol acrylate (Osaka Organic Chemical Industry Co., Ltd.) molecular weight 2000

[0045] <Polymerization initiator> TPO: 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (BASF)

[0046] <Surfactant> TEGO GRIDE432 (EVONIK) TEGO WET500 (EVONIK) Megafac RS-76NS (DIC)

[0047] <Inorganic particles> AEROSIL 50 (manufactured by Nippon Aerosil Co., Ltd.) X-24-9600A (Shin-Etsu Chemical Co., Ltd.) · Sicastar (manufactured by Corefront Co., Ltd.) · TiO2: Titanium oxide (coloring material for white ink) (manufactured by Dai Nippon Printing Co., Ltd.)

[0048] <Inorganic particle dispersant> SOLSPERSE32000 (Lubrizol)

[0049] <Coloring material> · TiO2: Titanium oxide (coloring material for white ink) (manufactured by Dai Nippon Printing Co., Ltd.) Magenta pigment: PR122 (magenta ink colorant) (manufactured by Dai Nippon Printing Co., Ltd.)

[0050] The methods for measuring the physical properties of each ink are shown below. <Static surface tension> The measurement was performed at 25° C. using an automatic surface tensiometer (DY-300, manufactured by Kyowa Interface Science Co., Ltd.) by the plate method using a platinum plate.

[0051] <Viscosity at 25℃> Measurements were performed using a cone-plate type rotational viscometer VISCOMETER TVE-22L manufactured by Toki Sangyo Co., Ltd., using a cone rotor (1°34' x R24), setting the rotation speed to 50 rpm and the temperature of the constant temperature circulating water to 25°C.

[0052] <Average primary particle size of inorganic particles> The primary particle size of the inorganic particles in the inorganic particle dispersion was measured using Microtrac UPA150 manufactured by Nikkiso Co., Ltd., by diluting the dispersion 100 times with PEA (manufactured by Osaka Organic Chemical Industry Ltd.).

[0053] [Examples 1 to 12, Comparative Examples 1 to 6] An inkjet ejection device having multiple inkjet heads and a UV light source mounted on a series of carriages as shown in Figure 1 was equipped with an MH5421 (manufactured by Ricoh Co., Ltd.) as an inkjet head and a UV-LED light source with a wavelength of 395 nm as an active energy ray irradiation device, and the inkjet inks were set in the combinations shown in Table 3. Using this inkjet ejection device, a laminate was produced by ejecting an ink set consisting of the first and second inkjet inks onto a polycarbonate substrate (manufactured by Mitsubishi Gas Chemical Company, Iupilon NF-2000, thickness 0.5 mm, length 100 mm, width 100 mm) and irradiating it with UV light. The output of the UV-LED light source with a wavelength of 395 nm was 4.5 W / cm2. 2 The carriage movement speed was set to 840 mm / sec, the distance from the head to the UV irradiator was set to 30 cm, the drop amount per drop was set to 12 μg, and the dot density was set to 600 dpi × 600 dpi.

[0054] -Evaluation method- For each of the laminates of the Examples and Comparative Examples, the pencil hardness, adhesion, and ejection stability of the second ink-jet ink were measured by the following evaluation methods. The measurement results are shown in Table 3. <Pencil hardness> In accordance with JIS K 5600 5-4, a scratch hardness test (pencil method) was carried out using a Cortec model KT-VF2391 with a load of 750 g.

[0055] <Adhesion> The laminate was cut using a cutter guide with 11 cuts at 1 mm intervals in a row and column to create 100 grids. Cellotape (registered trademark) No. 405 manufactured by Nichiban was firmly pressed onto the grids, and the frequency of exposed substrate when it was peeled off in one go was confirmed. (Evaluation Criteria) ○: Less than 5% of the substrate is exposed △: Exposure of substrate is 5% or more and less than 35% ×: 35% or more of the substrate is exposed

[0056] <Discharge stability> The second inkjet ink was ejected continuously for 5 minutes from 320 nozzles in one row using an inkjet ejection device equipped with MH5421 (manufactured by Ricoh Co., Ltd.), the number of nozzles that had missing nozzles was counted, and the ejection stability was evaluated based on the following evaluation criteria. The inkjet ejection device was set to a drive frequency of 10 kHz and the amount of ink ejected per ejection was set to 12 μg. (Evaluation Criteria) 〇: 2 nozzles or less △: 3 to 5 nozzles ×: 6 nozzles or more

[0057] [Table 1-1]

[0058] [Table 1-2]

[0059] [Table 2]

[0060] [Table 3-1]

[0061] [Table 3-2]

[0062] The present invention relates to the following method for producing a laminate (1), but also includes the following (2) to (7) as embodiments. (1) ejecting a first actinic ray-curable inkjet ink onto a substrate to form a first ink layer; a step of ejecting a second active energy ray curable inkjet ink onto the first ink layer to form a second ink layer; a step of irradiating the first ink layer and the second ink layer with active energy rays to cure the first ink layer to form a first cured layer and to cure the second ink layer to form a second cured layer; A method for producing a laminate having the first curable layer and the second curable layer, comprising: When the static surface tension of the first active energy ray curable inkjet ink is γ1 (mN / m) and the static surface tension of the second active energy ray curable inkjet ink is γ2 (mN / m), γ1 and γ2 satisfy the relationship of the following formula (1), γ1>γ2 (1) the second active energy ray curable inkjet ink contains 10% by mass or more and 40% by mass or less of a polyfunctional polymerizable compound having a weight average molecular weight (Mw) of 500 or more, and contains 1% by mass or more and 30% by mass or less of inorganic particles; A method for producing a laminate comprising the steps of: (2) The method for producing a laminate according to (1) above, wherein the second active energy ray-curable ink-jet ink contains inorganic particles in an amount of 5% by mass to 20% by mass. (3) The method for producing a laminate according to (1) or (2) above, wherein the primary particle diameter of the inorganic particles contained in the second active energy ray-curable ink-jet ink is 100 nm or more and 1 μm or less. (4) The method for producing a laminate according to any one of (1) to (3) above, wherein the inorganic particles contained in the second active energy ray-curable ink-jet ink are silica particles. (5) The method for producing a laminate according to any one of (1) to (4) above, wherein the content of the polyfunctional monomer contained in the second active energy ray-curable inkjet ink is 15% by mass or more and 30% by mass or less. (6) The method for producing a laminate according to any one of (1) to (5) above, wherein the content of the monofunctional monomer contained in the first active energy ray-curable inkjet ink is 50% by mass or more. (7) The method for producing a laminate according to any one of the above (1) to (6), wherein the first active energy ray-curable inkjet ink is a clear ink and the second active energy ray-curable inkjet ink is a color ink, or the first active energy ray-curable inkjet ink is a white ink and the second active energy ray-curable inkjet ink is a clear ink. [Explanation of symbols]

[0063] 21 Base material 22 The first inkjet ink 23 Second Inkjet Ink 25, 26 Head unit 27 Active energy ray irradiation equipment 30 Active energy rays [Prior art documents] [Patent documents]

[0064] [Patent Document 1] Patent No. 5568857 [Patent Document 2] Patent No. 5990868 [Patent Document 3] International Publication No. 2016 / 098678

Claims

1. A step of ejecting a first active energy ray-curable inkjet ink onto a substrate to form a first ink layer; forming a second ink layer by ejecting a second active energy ray-curable inkjet ink onto the first ink layer; a step of irradiating the first ink layer and the second ink layer with active energy rays to cure the first ink layer to form a first cured layer and to cure the second ink layer to form a second cured layer; A method for producing a laminate having the first cured layer and the second cured layer, comprising: When the static surface tension of the first active energy ray curable inkjet ink is γ1 (mN / m) and the static surface tension of the second active energy ray curable inkjet ink is γ2 (mN / m), γ1 and γ2 satisfy the relationship of the following formula (1), γ1>γ2 (1) the second active energy ray-curable inkjet ink contains 10% by mass or more and 40% by mass or less of a polyfunctional polymerizable compound having a weight average molecular weight (Mw) of 500 or more, and contains 1% by mass or more and 30% by mass or less of inorganic particles; A method for producing a laminate comprising the steps of:

2. The method for producing a laminate according to claim 1 , wherein the second active energy ray-curable ink-jet ink contains inorganic particles in an amount of 5% by mass to 20% by mass.

3. The method for producing a laminate according to claim 1 or 2, wherein a primary particle diameter of the inorganic particles contained in the second active energy ray-curable ink-jet ink is 100 nm or more and 1 μm or less.

4. The method for producing a laminate according to claim 1 , wherein the inorganic particles contained in the second active energy ray-curable ink-jet ink are silica particles.

5. The method for producing a laminate according to claim 1 , wherein the content of the polyfunctional monomer contained in the second active energy ray-curable ink-jet ink is 15% by mass or more and 30% by mass or less.

6. The method for producing a laminate according to claim 1 , wherein the content of the monofunctional monomer contained in the first active energy ray-curable ink-jet ink is 50% by mass or more.

7. 7. The method for producing a laminate according to claim 1, wherein the first active energy ray curable inkjet ink is a clear ink and the second active energy ray curable inkjet ink is a color ink, or the first active energy ray curable inkjet ink is a white ink and the second active energy ray curable inkjet ink is a clear ink.

Citation Information

Patent Citations

  • Smalllsized motor

    JP1980068857A

  • Both side recording apparatus

    JP1984090868A

  • Production method for membrane by inkjet method and membrane

    JP2011230501A

  • Single-pass inkjet printing method

    JP2013514904A

  • Photocurable inkjet ink set and inkjet recording method using the same

    JP2017061686A