Metal additive manufacturing flow path member and method for manufacturing same
A glass-coated metal additive manufacturing channel member with specific glass compositions addresses the high roughness and corrosion issues of metal additive manufacturing, achieving Ra ≤ 0.4 μm and improved corrosion resistance for semiconductor device manufacturing, ensuring precise gas flow and reduced particle adhesion.
Patent Information
- Application Number
- JP2023187640
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-08-11
- Filing Date
- 2023-11-01
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-11-12
AI Technical Summary
Metal additive manufacturing techniques produce flow path members with surface roughness exceeding the required Ra of 0.4 μm, which is necessary for semiconductor device manufacturing, and these members corrode when exposed to corrosive gases, leading to increased roughness and particle formation, reducing manufacturing yield.
A metal additive manufacturing channel member with a glass coating layer containing specific glass compositions (e.g., P2O5-ZnO-Al2O3-based glasses) is applied to fill surface irregularities, achieving an arithmetic mean roughness of Ra ≤ 0.4 μm and enhanced corrosion resistance against corrosive fluids like HF, HCl, and HBr.
The solution provides a channel member with both low surface roughness and improved corrosion resistance, ensuring precise gas flow control and reducing particle adhesion, thereby enhancing the manufacturing yield and productivity of semiconductor devices.
Smart Images

Figure 0007563553000008 
Figure 0007563553000009 
Figure 0007563553000010
Abstract
Description
[Technical field]
[0001] The present invention relates to a technique for a flow path member that allows the passage of a corrosive fluid (gas or liquid) used in a semiconductor device manufacturing process or the like, and in particular to a metal additive manufacturing flow path member manufactured using a metal additive manufacturing method. [Background technology]
[0002] As semiconductor device technology continues to advance, the wiring pitch of circuits is becoming smaller and smaller. To ensure a high manufacturing yield for such semiconductor devices, precise control of the amount of gas supplied during the manufacturing process and cleaning of the gas supply lines are essential technologies.
[0003] In precise control of the amount of gas supplied and in cleaning the gas supply line, the surface smoothness of the inner surface of the gas flow path (also called the gas contact surface) is one of the very important factors. The following are some examples of the reasons for this:
[0004] When the surface smoothness of the gas flow passage gas contact surface is poor (the surface roughness is large), (1) the gas flow is easily disturbed in the immediate vicinity of the gas contact surface, which reduces the accuracy of gas flow rate control; (2) the actual surface area of the gas contact surface becomes larger, which increases the amount of gas adsorbed, which lengthens the time it takes for the semiconductor device manufacturing equipment to reach a vacuum, which reduces productivity; and (3) once unwanted particles adhere to the gas contact surface (for example, if they are trapped in large valleys), it becomes difficult to completely remove the particles by gas line cleaning.
[0005] For the reasons mentioned above, in a flow path member used in a supply gas line of a semiconductor device manufacturing apparatus, the arithmetic mean roughness Ra of the gas-contacting surface is required to be 0.4 μm or less.
[0006] Meanwhile, in the manufacturing process of semiconductor devices, corrosive gases (e.g., HF (hydrogen fluoride), HCl (hydrogen chloride), Cl2 (chlorine), ClF3 (chlorine trifluoride), HBr (hydrogen bromide), etc.) are often used, and highly corrosion-resistant metal materials (e.g., stainless steel, Ni (nickel)-Cr (chromium)-Mo (molybdenum) alloys, etc.) have traditionally been used as flow path members for passing such corrosive gases.
[0007] However, even flow path members made of highly corrosion-resistant metal materials can corrode if exposed to corrosive gases for long periods of time, and the progress of corrosion can increase the surface roughness of the gas-contacting surface and the corrosion reaction products can become a source of particle generation. This reduces the manufacturing yield of semiconductor devices and has been a problem that requires measures to be taken.
[0008] To address such problems, for example, Patent Document 1 (JP Patent Publication 7-281759) discloses a mass flow controller having an inflow path for a fluid, a bypass path through which the fluid from the inflow path flows, a sensor path branching from the bypass path through which a fluid with a predetermined flow rate ratio flows, a flow sensor for measuring the flow rate of the fluid flowing through the sensor path, an outflow path through which the fluids from the bypass path and the sensor path join and flow, a flow control valve provided in the outflow path, and a comparison control section for comparing a detection signal detected by the flow sensor with a preset signal and controlling the flow control valve based on the result, wherein the bypass path and / or the sensor path are formed from one of the following metal materials: nickel, platinum, nickel-based alloy, copper, and copper alloy.
[0009] According to Patent Document 1, it is possible to provide a mass flow controller that improves the corrosion resistance of the sensor tube and bypass tube, which are susceptible to corrosion by halogen gases and the like, while suppressing reaction products and generating no particles.
[0010] Meanwhile, the fluid supply lines used in semiconductor device manufacturing processes often contain components and equipment that form flow paths with complex shapes (e.g., branch flow paths, merging flow paths, throttle flow paths, spiral flow paths, and combinations thereof.) Such components and equipment are often expensive due to the difficulty of processing them, which has been one of the factors that increase the cost of constructing fluid supply lines.
[0011] In response to these challenges, three-dimensional modeling technologies (so-called 3D printing) such as metal additive manufacturing (also known as metal additive manufacturing) have been attracting attention in recent years as a technology for manufacturing final products with complex shapes in near net shape / net shape.
[0012] For example, Patent Document 2 (JP 2018-170205 A) teaches a manufacturing method for a fluid heater comprising a flow path member having a flow path formed therein, a heater for heating the flow path member, a fixing member for fixing the flow path member to a fluid control device, and a connecting pipe connected to the flow path member for allowing a fluid to flow into the flow path member, wherein the flow path is spiral and has a polygonal cross-sectional shape along the longitudinal direction, the manufacturing method for a fluid heater comprising the steps of: creating the flow path member by a metal powder sintering molding method; and combining the heater, the fixing member, and the connecting pipe with the flow path member.
[0013] According to Patent Document 2, it is possible to provide a fluid heater, a fluid control device, and a method for manufacturing a fluid heater that can increase the heating efficiency of the fluid (thereby enabling miniaturization) in order to prevent the fluid heater and fluid control device from becoming larger. [Prior art documents] [Patent documents]
[0014] [Patent Document 1] Japanese Patent Application Publication No. 7-281759 [Patent Document 2] JP 2018-170205 A Summary of the Invention [Problem to be solved by the invention]
[0015] As mentioned above, metal additive manufacturing technology can produce final products in near net shape / net shape, so it is expected that even flow path components with complex shapes can be manufactured stably (i.e., at low cost) with high manufacturing yields.
[0016] However, the problem with current metal additive manufacturing technologies is that the surface roughness of the products formed as is is relatively large (for example, Ra = 5 to 50 μm). This surface roughness is one to two orders of magnitude larger than the level (Ra ≦ 0.4 μm) required for flow path components used in the supply gas lines of semiconductor device manufacturing equipment. Therefore, it is conceivable to adjust the surface roughness by polishing the surface, but the more complex the shape, the more difficult the polishing process becomes.
[0017] Therefore, an object of the present invention is to provide a metal additive manufacturing flow path member and a manufacturing method thereof that combines surface roughness and corrosion resistance of the inner surface of the flow path at a level sufficient for use as a flow path member for use in a corrosive fluid supply line in a semiconductor device manufacturing apparatus. [Means for solving the problem]
[0018] (I) One aspect of the present invention is a metal additive manufacturing flow path member used in a supply gas line for circulating a corrosive fluid in a semiconductor device manufacturing apparatus, the corrosive fluid is HF, HCl or HBr; The metal substrate constituting the metal additive manufacturing flow path member has a surface unevenness, The inner surface of the flow path wall of the metal additive manufacturing flow path member has a glass coating layer formed thereon so as to fill at least the concave areas of the surface unevenness of the metal base, and the arithmetic mean roughness Ra of the inner surface is 0.4 μm or less; The glass coating layer includes at least one layer selected from the group consisting of a P2O5 (phosphorus oxide)-ZnO-Al2O3 (aluminum oxide)-(AM)2O (AM is an alkali metal) based glass layer containing 10 mol % or more of ZnO (zinc oxide) calculated as oxide, a P2O5-ZnO-Al2O3-(AEM)O (AEM is an alkaline earth metal) based glass layer containing 10 mol % or more of ZnO, a Bi2O3 (bismuth oxide)-ZnO-B2O3 (boron oxide) based glass layer, and a SiO2 (silicon oxide)-B2O3-Na2O (sodium oxide) based glass layer. The present invention provides a metal additive manufacturing flow path member characterized by the above-mentioned. In the present invention, the term "...-based" means that the components contained in the metal substrate are listed in order of their content (components with high content rates), and may contain components other than those listed. The surface irregularities of the metal substrate have an arithmetic mean roughness Ra of about 5 μm to 50 μm.
[0019] In the present invention, the above-mentioned metal additive manufacturing flow path member (I) can be improved or modified as follows. (i) when the corrosive fluid is HF, the glass coating layer includes at least one layer selected from the group consisting of a P2O5-ZnO-Al2O3-(AM)2O-based glass layer, a P2O5-ZnO-Al2O3-(AEM)O-based glass layer, and a Bi2O3-ZnO-B2O3-based glass layer, and when a corrosion resistance test is performed in which the glass is immersed in a 30 mass % HF aqueous solution at a temperature of 25°C for 25 hours, the amount of mass loss per unit area of the glass is smaller than that of SUS316L, When the corrosive fluid is the HCl or the HBr, the glass coating layer includes at least one layer of the P2O5-ZnO-Al2O3-(AM)2O-based glass layer, the P2O5-ZnO-Al2O3-(AEM)O-based glass layer, and the SiO2-B2O3-Na2O-based glass layer, and when a corrosion resistance test is conducted in which the glass is immersed in a 10 mass % aqueous HCl solution at a temperature of 60°C or a 10 mass % aqueous HBr solution at a temperature of 60°C for 25 hours, the mass loss per unit area of the glass is smaller than that of SUS316L. (ii) When a corrosion resistance test was performed in which the glass was immersed in a 30 mass % HF aqueous solution at a temperature of 25° C. for 25 hours, the mass loss of the glass was 0.68 mg / mm 2 is as follows: When a corrosion resistance test was performed in which the glass was immersed in a 10% by mass HCl aqueous solution at a temperature of 60° C. for 25 hours, the mass loss of the glass was 0.091 mg / mm 2 is as follows: When a corrosion resistance test was performed in which the glass was immersed in a 10% by mass HBr aqueous solution at a temperature of 60° C. for 25 hours, the mass loss of the glass was 0.024 mg / mm 2 The following is the result. (iii) The P2O5-ZnO-Al2O3-(AM)2O-based glass and the P2O5-ZnO-Al2O3-(AEM)O-based glass each have a chemical composition, calculated in terms of oxide, of 45 mol % or more and 65 mol % or less of P2O5, 10 mol % or more and 25 mol % or less of ZnO, 10 mol % or more and 25 mol % or less of Al2O3, and 2 mol % or more and 18 mol % or less of (AM)2O or (AEM)O. (iv) The P2O5-ZnO-Al2O3-(AM)2O-based glass has a chemical composition, calculated as oxides, of 51 mol % to 63 mol % P2O5, 16 mol % to 19 mol % ZnO, 10 mol % to 19 mol % Al2O3, and 6 mol % to 14 mol % (AM)2O. (v) the (AM)2O is at least one of Na2O and K2O, The (AEM)O is at least one of MgO, CaO, SrO, and BaO.
[0020] (II) Another aspect of the present invention is a method for producing the above-mentioned metal additive manufacturing flow path member, A metal additive manufacturing process for forming the metal base by a metal additive manufacturing method; and forming a glass coating layer on the inner surface of the flow path wall, The glass coating layer forming step includes: a glass paste preparation step of preparing a glass paste in which the glass powder, a resin binder, and an organic solvent are mixed; a glass paste application and baking process for applying the glass paste to the inner surface of the flow path wall and baking the glass coating layer by heat treating the metal substrate together; The glass paste has a resin binder content of 3% by mass or more and 13% by mass or less with respect to a total content of the organic solvent and the resin binder, and a glass powder content of the glass paste is 10% by mass or more and 90% by mass or less, The present invention provides a method for manufacturing a metal additive manufacturing flow path member, characterized in that the temperature of the heat treatment in the glass paste application and baking process is equal to or higher than the softening point temperature of the glass in the glass paste and equal to or lower than 700°C. Effect of the Invention
[0021] According to the present invention, it is possible to provide a metal additive manufacturing flow path member and a manufacturing method thereof that combine surface roughness and corrosion resistance of the inner surface of the flow path at a level sufficient for use as a flow path member for use in a corrosive fluid supply line in a semiconductor device manufacturing apparatus. [Brief description of the drawings]
[0022] [Figure 1] 1 is a cross-sectional schematic diagram showing an example of a metal additive manufacturing flow path member according to the present invention. FIG. [Diagram 2] 1A to 1C are process diagrams illustrating an example of a method for manufacturing a metal additive manufacturing flow path member according to the present invention. [Diagram 3] 1 is a photograph of the microstructure of the inner surface of a flow channel wall of a metal substrate on which a glass coating layer is not formed. [Figure 4] 13 is a photograph of the microstructure of the inner surface of a flow channel wall of an example of a metal additive manufacturing flow channel member having a glass coating layer formed thereon. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] (Basic concept of the present invention) As mentioned above, the problem with products formed by current metal additive manufacturing technology is that they have a large surface roughness unless polished. When the flow channel shape is complex, it is very difficult to install the counter electrode in the flow channel if the inner surface is electrolytically polished as in the case of conventional metal tubes. In addition, chemical polishing is also not suitable because highly corrosion-resistant metal materials are used as the flow channel components. In addition, when the flow channel has a complex shape, it is extremely difficult to physically polish the inner surface of the flow channel.
[0024] Therefore, the inventors of the present invention have investigated smoothing the surface of a metal additive manufacturing product by forming a coating layer so as to fill in the concave portions of the surface unevenness, rather than smoothing the convex portions of the surface unevenness by scraping them off. In particular, they have found that a glass coating layer is suitable from the viewpoints of application to the metal substrate surface, corrosion resistance to corrosive fluids, and heat resistance required for flow path members.
[0025] As a result of examining the suitability of the glass coating layer, it was found that by forming a coating layer made of P2O5-ZnO-Al2O3-based glass, Bi2O3-ZnO-B2O3-based glass, or SiO2-B2O3-Na2O-based glass, the surface can be smoothed to an arithmetic mean roughness of "Ra≦0.4 μm" and corrosion resistance against halogen-based corrosive gases (particularly HF, HCl, and / or HBr) and heat resistance can be ensured. Furthermore, it was found that as the P2O5-ZnO-Al2O3-based glass, P2O5-ZnO-Al2O3-(AM)2O glass and P2O5-ZnO-Al2O3-(AEM)O glass are preferable, and P2O5-ZnO-Al2O3-(AM)2O glass is particularly preferable. The present invention is based on this finding.
[0026] (Metal Additive Manufacturing Method) The additive manufacturing technology called 3D printing described above has made it possible to manufacture objects of complex shapes at low cost. By repeatedly supplying thermal energy to the raw powder to melt and solidify the raw powder (hereinafter referred to as melting and solidifying), it is possible to obtain an additively manufactured object of a three-dimensional shape with a near-net shape / net shape. Metal additive manufacturing methods for metal materials can be broadly divided into powder bed methods and powder deposition methods. The metal additive manufacturing flow path member of the present invention can be manufactured by either method.
[0027] The powder bed method is a method in which a powder bed is prepared by spreading metal powder, and then a laser beam or electron beam, which is used as heat energy, is irradiated to melt, solidify, or sinter only the part to be shaped. The method of melting and solidifying the part to be shaped in the powder bed using a laser beam as the heat source is called selective laser melting (SLM). The method of sintering the part to be shaped in the powder bed without melting it is called selective laser sintering (SLS). In the method using a laser beam as the heat source, an inert atmosphere such as nitrogen or argon is usually used. The powder bed method using an electron beam as the heat source is called selective electron beam melting (SEBM) or simply electron beam melting (EBM). In the method using an electron beam as the heat source, a high vacuum environment is used.
[0028] On the other hand, the powder deposition method uses a laser beam or electron beam as a heat source, continuously supplies metal powder into the beam or to the beam irradiation position, and melts and solidifies the metal powder along the beam irradiation trajectory to create a shape. The atmosphere and environment during modeling are the same as those of the powder bed method. The powder deposition method has the advantage that the amount of powder supply is easy to control and high-speed modeling is possible.
[0029] (Metal additive manufacturing flow channel components) Fig. 1 is a schematic cross-sectional view showing an example of a metal additive manufacturing flow path member according to the present invention. As shown in Fig. 1, a metal additive manufacturing flow path member 100 according to the present invention has a metal substrate 10 and a glass coating layer 20 formed on the inner surface of a flow path wall that constitutes a flow path.
[0030] Since the metal substrate 10 is manufactured using a metal additive manufacturing technique, the surface usually has irregularities with an arithmetic mean roughness Ra of about 5 to 50 μm, which are largely due to the particle size of the metal powder and the manufacturing conditions. The glass coating layer 20 is formed so as to fill in at least the concave areas of the surface irregularities. As a result, the arithmetic mean roughness Ra of the inner surface of the flow path wall is 0.4 μm or less. The arithmetic mean roughness Ra is more preferably 0.2 μm or less.
[0031] In other words, the smaller the arithmetic mean roughness Ra of the flow path wall inner surface, the better, but it is sufficient that the glass coating layer 20 is formed so that it is 0.4 μm or less. It is preferable that all of the apexes of the convex regions of the surface irregularities of the metal substrate 10 are covered with the glass coating layer 20. Note that, when the metal substrate 10 itself is made of a metal material (e.g., a supercorrosion-resistant alloy material) that has necessary and sufficient corrosion resistance against the corrosive fluid to be passed through, it is not necessary that all of the apexes are covered with the glass coating layer 20, provided that the flow path wall inner surface satisfies "Ra≦0.4 μm."
[0032] Furthermore, in the metal additive manufacturing flow path member 100 of the present invention, the formation of the glass coating layer 20 is not limited to the inner surface of the flow path wall, and the glass coating layer 20 may be formed on the outer surface of the flow path wall in addition to the inner surface of the flow path wall.
[0033] As the glass constituting the glass coating layer 20, P2O5-ZnO-Al2O3-based glass, Bi2O3-ZnO-B2O3-based glass, or SiO2-B2O3-Na2O-based glass is preferable. Specifically, P2O5-ZnO-Al2O3-based glass and Bi2O3-ZnO-B2O3-based glass are preferable for HF, and P2O5-ZnO-Al2O3-based glass and SiO2-B2O3-Na2O-based glass are preferable for HCl and HBr. As the P2O5-ZnO-Al2O3-based glass, P2O5-ZnO-Al2O3-(AM)2O glass and P2O5-ZnO-Al2O3-(AEM)O glass are preferable, and P2O5-ZnO-Al2O3-(AM)2O glass is particularly preferable.
[0034] More specifically, the chemical composition of the P2O5-ZnO-Al2O3-based glass is preferably, in terms of oxides, 45 mol% to 65 mol% P2O5, 10 mol% to 25 mol% ZnO, 10 mol% to 25 mol% Al2O3, and 2 mol% to 18 mol% (AM)2O or (AEM)O. Also, P2O5-ZnO-Al2O3-(AM)2O glass consisting of 51 mol% to 63 mol% P2O5, 16 mol% to 19 mol% ZnO, 10 mol% to 19 mol% Al2O3, and 6 mol% to 14 mol% (AM)2O is more preferable.
[0035] The glass coating layer 20 can be formed by combining (laminating) one or more of the above-mentioned glass layers. When laminating glass layers, it is preferable that the glass layer having the highest corrosion resistance be the gas-contacting surface.
[0036] There are no particular limitations on the flow path structure of the metal additive manufacturing flow path member of the present invention, but due to the significance of producing it using metal additive manufacturing technology, it can be said that the effective effect is greater in complex flow path structures (e.g., branching flow paths, merging flow paths, throttle flow paths, spiral flow paths, and combinations thereof).
[0037] There are no particular limitations on the material of the metal substrate 10, but highly corrosion-resistant alloy materials (e.g., stainless steels such as SUS316L) and super-corrosion-resistant alloy materials (e.g., Hastelloy (registered trademark), Ni-Cr-Mo alloys in which the top three components with the highest content are Ni, Cr, and Mo, and high-entropy alloys containing Co-Cr-Fe-Ni-Ti) can be suitably used.
[0038] There are no particular limitations on the equipment or devices that can use the metal additive manufacturing flow path member 100 of the present invention, but it can be suitably used in equipment and devices used in supply lines of corrosive fluids used in semiconductor device manufacturing processes (for example, mass flow controllers, mass flow meters, shut-off valves, switching valves, vaporizers, fluid heaters, piping units that combine these, etc. that circulate corrosive gases).
[0039] When the above-mentioned glass coating layer is applied to such equipment or devices, for example, a mass flow controller can accurately control the gas flow rate. Also, in a semiconductor device manufacturing device, the time required to reach a vacuum can be shortened. Furthermore, adhesion of particles to the inner surface of the flow path wall is suppressed, and even if particles do adhere, they can be easily removed by gas line cleaning.
[0040] (Metal additive manufacturing method for flow path member) Next, a method for producing the metal additive manufacturing flow path member 100 according to the present invention will be described.
[0041] Fig. 2 is a process diagram showing an example of a method for manufacturing a metal additive manufacturing flow path member according to the present invention. As shown in Fig. 2, the method is roughly divided into a metal additive manufacturing process S1 for forming a metal base 10 of the flow path member, and a glass coating layer forming process S2 for forming a glass coating layer 20 on the inner surface of the flow path wall of the metal base 10. The glass coating layer forming process S2 includes a glass paste preparing process S2a and a glass paste applying and baking process S2b.
[0042] There are no particular limitations to the metal additive manufacturing process S1, and the aforementioned metal additive manufacturing methods (e.g., selective laser melting (SLM), laser metal deposition (LMD), and electron beam melting (EBM)) can be suitably used as long as a metal substrate 10 having the desired flow path structure can be obtained.
[0043] The glass paste preparation step S2a is a step of preparing a glass paste by mixing a predetermined glass powder, an organic solvent, and a resin binder. There is no particular limitation on the mixing method, and a conventional mixing method (for example, mixing using a rotation-revolution mixer) may be used as appropriate. Note that this step S2a is not limited to being performed after step S1, and may be performed before step S1. Also, this step S2a is not an essential step in the manufacturing method according to the present invention, and glass paste mixed to a desired composition may be purchased to prepare the glass paste.
[0044] As described above, the glass is preferably a P2O5-ZnO-Al2O3-based glass, a Bi2O3-ZnO-B2O3-based glass, or a SiO2-B2O3-Na2O-based glass, and the P2O5-ZnO-Al2O3-based glass is preferably a P2O5-ZnO-Al2O3-(AM)2O glass or a P2O5-ZnO-Al2O3-(AEM)O glass. In addition, it is preferable that the glass has a softening point temperature higher than the maximum temperature (e.g., 300°C, more preferably 400°C) experienced by the metal additive manufacturing flow path member in the operating environment of the fluid supply line, and forms a coating layer at 700°C or less. Note that 700°C is the upper limit temperature in the subsequent glass paste application and baking process S2b, and is a guideline temperature at which the metal substrate 10 does not deteriorate.
[0045] The chemical composition of the glass will be briefly explained.
[0046] P2O5, Bi2O3, SiO2 and B2O3 are components that can form the skeleton of glass. In the P2O5-ZnO-Al2O3-(AM)2O glass and the P2O5-ZnO-Al2O3-(AEM)O glass, the P2O5 content is preferably 45 mol% or more and 65 mol% or less, more preferably 51 mol% or more and 63 mol% or less. By adjusting the P2O5 content within this range, excellent corrosion resistance against halogen-based corrosive substances is exhibited.
[0047] ZnO is a component that improves the chemical stability of glass and supports corrosion resistance. In the P2O5-ZnO-Al2O3-(AM)2O glass and the P2O5-ZnO-Al2O3-(AEM)O glass, the ZnO content is preferably 10 mol% or more and 25 mol% or less, more preferably 16 mol% or more and 19 mol% or less. By adjusting the ZnO content within this range, sufficient corrosion resistance against halogen-based corrosive substances is exhibited and the effect of suppressing crystallization of the glass is achieved.
[0048] Al2O3 is also a component that improves the chemical stability of glass and supports corrosion resistance. In P2O5-ZnO-Al2O3-(AM)2O glass and P2O5-ZnO-Al2O3-(AEM)O glass, the Al2O3 content is preferably 10 mol% or more and 25 mol% or less, more preferably 10 mol% or more and 19 mol% or less. By adjusting the Al2O3 content within this range, sufficient corrosion resistance against halogen-based corrosive substances is exhibited.
[0049] In the P2O5-ZnO-Al2O3-(AM)2O glass and the P2O5-ZnO-Al2O3-(AEM)O glass, (AM)2O and (AEM)O are components that contribute to improving corrosion resistance. Their contents are preferably 2 mol% or more and 18 mol% or less, and more preferably 6 mol% or more and 14 mol% or less. By adjusting the (AM)2O content and the (AEM)O content to within the corresponding ranges, sufficient corrosion resistance against halogen-based corrosive substances is exhibited.
[0050] When a plurality of AM oxides or AEM oxides are mixed as (AM)2O or (AEM)O, the total amount is 2 mol% or more and 18 mol% or less. As (AM)2O, Na2O and / or K2O are particularly preferred.
[0051] The average particle size of the glass powder is preferably 0.1 μm or more and 10 μm or less. If the average particle size is 0.1 μm or more, the glass powder is uniformly dispersed in the glass paste without agglomeration, making it easy to control the thickness of the glass coating layer. If the average particle size is 10 μm or less, the application property of the glass paste is good, and the surface smoothness of the glass coating layer can be appropriately ensured.
[0052] As the organic solvent, for example, diethylene glycol monobutyl ether acetate, terpineol, ethanol, acetone, or a mixture thereof can be preferably used.
[0053] The resin binder is preferably one that does not contain metal elements (no metal elements are present in the molecular structure) and can be removed by burning at 600° C. or less, and for example, ethyl cellulose or acrylic resin can be preferably used.
[0054] An example of the procedure of the glass paste preparation step S2a will be described. First, a resin binder is mixed with an organic solvent to prepare a mixed solvent. The resin binder concentration in the mixed solvent (hereinafter referred to as the resin binder concentration) is preferably 3% by mass or more and 13% by mass or less, and more preferably 5% by mass or more and 10% by mass or less. By adjusting the resin binder concentration to 3% by mass or more, the viscosity of the glass paste and the adhesive strength to the metal substrate can be ensured, and the glass paste is appropriately retained on the inner surface of the flow path wall of the metal substrate, so that a uniform glass coating layer can be formed in the next step S2b. On the other hand, by adjusting the resin binder concentration to 13% by mass or less, the viscosity can be adjusted to a level that allows excess glass paste to be discharged in the next step S2b.
[0055] Next, glass powder is added to the mixed solvent and mixed to prepare a glass paste. The mixing ratio (solid content concentration) of the glass powder in the glass paste is preferably 10% by mass or more and 90% by mass or less, and more preferably 20% by mass or more and 80% by mass or less. By adjusting the solid content concentration to 10% by mass or more, a sufficient amount of glass for forming a glass coating layer in the next step S2b can be secured. In addition, by adjusting the solid content concentration to 90% by mass or less, a uniform glass coating layer can be formed in the next step S2b without reducing the fluidity of the glass paste or the adhesive strength to the metal substrate.
[0056] The glass paste application and baking step S2b is a step in which the prepared glass paste is applied to the inner surface of the flow path wall of the metal base 10, and then the metal base 10 is heated to bake the glass coating layer 20. There is no particular limitation on the method of applying the glass paste, and for example, a method of spraying the glass paste onto the inner surface of the flow path wall using a spray gun, a method of pouring the glass paste into the flow path and then discharging the excess, a method of dip-coating the glass paste on the metal base 10 and then discharging the excess, or the like can be appropriately used.
[0057] The heat treatment temperature for baking the glass coating layer 20 is preferably equal to or higher than the softening point of the glass used and equal to or lower than 700°C. If the heat treatment temperature is lower than the softening point, the glass particles do not soften and flow, and a coating layer cannot be formed. If the heat treatment temperature exceeds 700°C, the metal substrate 10 may be altered.
[0058] In the present invention, the glass paste application and baking step S2b is not limited to one application and one baking, and the combination of application and baking may be repeated multiple times. From the viewpoint of controlling the thickness of the glass coating layer 20, it is preferable to repeat the combination of application and baking multiple times. In addition, it is also possible to prepare multiple types of glass pastes with different glass compositions and blending ratios, and repeat application and baking multiple times while changing the glass paste. EXAMPLES
[0059] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0060] [Experiment 1] (Testing and evaluation of corrosion resistance of materials) The corrosion resistance of glass materials that form the coating layer of glass and metal materials that form the metal substrate to hydrohalic acid was tested and evaluated.
[0061] The glass materials include P2O5-ZnO-Al2O3 glass (63 mol%P2O5-17 mol%ZnO-10 mol%Al2O3-10 mol%Na2O, softening point 550℃), Bi2O3-ZnO-B2O3 glass (70 mol%Bi2O3-11 mol%B2O3-8 mol%ZnO-5 mol%SiO2-4 mol%BaO-2 mol%CuO, softening point 510℃), SiO2-B2O3-Na2O glass (65 mol%SiO2-10 mol%B2O3-7 mol%Na2O-7 mol%Li2O-4 mol%Al2O3-4 mol%K2O, softening point 590℃), and V2O3-TeO2-Fe2O3 glass (40 mol%V2O3-30 mol%Na2O, softening point 590℃). The material used was SUS316L, which is often used as a piping material for gas supply lines.
[0062] As starting materials for the glass material, commercially available reagents of oxide powders of the above compositions (each with a purity of 99.9%) or commercially available reagents of carbonate powders of cations of the oxides of the above compositions (each with a purity of 99.9%) were used. The starting materials were mixed to obtain the desired glass composition and melted in a glass melting furnace, and the molten liquid was poured into a stainless steel mold or a graphite mold to produce bulks of glass material (about 200 g each). As can be estimated from the purity of the starting materials, the glass material in the present invention contains unavoidable impurities. A commercially available product of SUS316L was prepared as the metal material.
[0063] Test pieces (10 mm long x 5 mm wide x 5 mm thick) for corrosion resistance tests were taken from the bulk of each glass material and the SUS316L metal material. The SUS316L test pieces were used as the standard specimens for corrosion resistance.
[0064] As an accelerated corrosion resistance test, the test pieces were immersed in a given test liquid for a given time (5 hours, 25 hours). The test liquids prepared were 30% by mass hydrofluoric acid (temperature 25°C), 10% by mass hydrochloric acid (temperature 60°C), and 20% by mass hydrobromic acid (temperature 60°C). The mass loss per unit area (mg / mm2) was calculated by dividing the mass difference before and after immersion in the test liquid by the surface area of the test piece before immersion. 2 ) was investigated.
[0065] When the mass loss was smaller than that of the reference sample SUS316L, it was judged as “Good,” and when the mass loss was equal to or greater than that of the reference sample SUS316L, it was judged as “Not good.” The results are shown in Tables 1 to 3.
[0066] [Table 1]
[0067] [Table 2]
[0068] [Table 3]
[0069] As shown in Tables 1 to 3, P2O5-ZnO-Al2O3-based glass and Bi2O3-ZnO-B2O3-based glass are more corrosion resistant than SUS316L against hydrofluoric acid (30 mass% HF aqueous solution) and are judged to be "good". P2O5-ZnO-Al2O3-based glass and SiO2-B2O3-Na2O-based glass are more corrosion resistant than SUS316L against hydrochloric acid (10 mass% HCl aqueous solution) and are judged to be "good". P2O5-ZnO-Al2O3-based glass and SiO2-B2O3-Na2O-based glass are more corrosion resistant than SUS316L against hydrobromic acid (20 mass% HBr aqueous solution) and are judged to be "good".
[0070] [Experiment 2] (Investigation of changes in roughness of the inner surface of the gas flow passage wall in gas flow passage components) In this experiment, a simple gas flow passage member was fabricated, and hydrogen halide gas was passed through it to investigate the change in roughness of the inner surface of the flow passage wall.
[0071] A metal substrate made of SUS316L (channel inner diameter 10 mm, channel length 250 mm) was fabricated by metal additive manufacturing (metal additive manufacturing step S1). As a comparison sample, a commercially available SUS316L pipe for gas supply lines (channel inner diameter 10 mm, channel length 250 mm) was prepared. In addition, a SUS316L substrate made by metal additive manufacturing and a commercially available SUS316L pipe were also prepared separately for microstructure investigation.
[0072] The various conditions in the metal additive manufacturing process S1 were as follows: (1) SUS316L powder: particle size 10~60μm, median diameter 40μm (2) Additive manufacturing equipment: M290, manufactured by Electro Optical Systems, Germany (3) Additive manufacturing conditions: laser power 300 W, scanning speed 800 mm / s, scanning pitch 0.1 mm, powder bed thickness 0.04 mm, Ar atmosphere Energy density = laser power / (scan speed x scan pitch x powder bed thickness) = 94 J / mm 3 .
[0073] The SUS316L substrate and SUS316L pipe for microstructure investigation were cut, and the inner surface roughness of the flow channel was measured using a contact type surface roughness measuring instrument (Mitutoyo Corporation, Surftest SV-3000). In the surface roughness measurement, the measurement length (evaluation length) was set to 4 to 40 mm and the reference length was set to 0.8 to 8 mm in accordance with the ISO / JIS standard (ISO 4288:1996 / JIS B 0633:2001). As a result, the arithmetic mean roughness Ra of the SUS316L substrate and SUS316L pipe, respectively, was 20 μm and 0.4 μm.
[0074] A glass paste was prepared to form a glass coating layer on the inner surface of the flow channel wall of the additively manufactured SUS316L substrate. The remaining part from the specimens taken for the corrosion resistance test in Experiment 1 was pulverized using a stamp mill and a jet mill to prepare glass powder (average particle size 3 μm). The glass paste was produced by mixing P2O5-ZnO-Al2O3-based glass powder with diethylene glycol monobutyl ether acetate (BCA) as an organic solvent and ethyl cellulose (EC) as a resin binder (glass paste preparation process S2a).
[0075] Next, glass paste was applied to the inner surface of the flow channel wall of the SUS316L substrate using a spray gun and baked at 600°C to form a glass coating layer (glass paste application and baking process S2b). At this time, the number of times the glass paste was applied and baked was controlled to produce samples of multiple types of metal additive manufacturing flow channel components with different average thicknesses of the glass coating layer. Samples for microstructure investigation were also produced.
[0076] The relationship between the surface roughness of the inner surface of the flow channel wall and the microstructure of the samples for microstructure investigation was investigated. The surface roughness of the inner surface of the flow channel wall with the glass coating layer was measured in the same manner as above, and the microstructure was observed using a scanning electron microscope (SEM).
[0077] It was confirmed that metal additive manufacturing flow channel components with arithmetic mean roughness Ra of 2.5 μm, 1.2 μm, 0.5 μm, 0.4 μm, and 0.2 μm were obtained. As a result of microstructural observation, in samples with an arithmetic mean roughness Ra of 0.5 μm or more, the bare surface of the SUS316L substrate was confirmed on the inner surface of the flow channel wall. In other words, it was found that in samples with an arithmetic mean roughness Ra of 0.5 μm or more, there remained areas in the convex parts of the surface unevenness of the metal substrate that were not covered by the glass coating layer (areas in which the concave parts of the surface unevenness of the metal substrate were not completely filled with the glass coating layer). On the other hand, in samples with an arithmetic mean roughness Ra of 0.4 μm or less, the bare surface of the SUS316L substrate was not confirmed on the inner surface of the flow channel wall (the concave parts of the surface unevenness of the metal substrate were considered to be completely filled with the glass coating layer).
[0078] A test was conducted on the prepared metal additive manufacturing flow path component and a commercially available SUS316L pipe, in which HCl gas (at 100°C) was passed for 100 hours, and then N2 (nitrogen) gas was passed for 5 minutes to purge the HCl gas from inside the flow path. After the test, each sample was cut and the arithmetic mean roughness Ra of the inner surface of the flow path wall was measured in the same manner as above. If there was no change in the arithmetic mean roughness Ra before and after the test, it was judged as "passed", and if there was a change in the arithmetic mean roughness Ra, it was judged as "failed". The results are shown in Table 4.
[0079] [Table 4]
[0080] As shown in Table 4, the surface roughness of the gas-contacting surface of the commercially available SUS316L pipe increased after the HCl gas flow test. This is believed to be due to corrosion caused by the flow of HCl gas. On the other hand, the surface roughness of the gas-contacting surface of the additive manufacturing flow path component samples with an initial arithmetic mean roughness Ra of 0.5 μm or more decreased after the HCl gas flow test. This is believed to be because only the bare surface of the SUS316L substrate, which had become convex on the gas-contacting surface due to the flow of HCl gas, was corroded, resulting in an apparent decrease in the surface roughness of the gas-contacting surface. In both cases, there was a change in surface roughness before and after the HCl gas flow test, so the commercially available SUS316L pipe and the additive manufacturing flow path component samples with an initial arithmetic mean roughness Ra of 0.5 μm or more were judged to be "failed."
[0081] In contrast, samples of additively manufactured flow path components with an initial arithmetic mean roughness Ra of 0.4 μm or less were judged to be "passed" because there was no change in surface roughness before and after the HCl gas flow test. These results are thought to be due to whether or not the bare surface of the metal substrate, which has insufficient corrosion resistance, is exposed on the inner surface of the flow path wall (whether or not the concave parts of the metal substrate's surface irregularities are completely filled with a glass coating layer). It was also separately confirmed that the additively manufactured flow path components that passed the test had a high cleaning effect on gas lines. It is also thought to be effective in shortening the time it takes to reach a vacuum in semiconductor manufacturing equipment.
[0082] [Experiment 3] (Detailed investigation of P2O5-ZnO-Al2O3 glass system) In experiment 1, the P2O5-ZnO-Al2O3 glass system showed good corrosion resistance against all three types of hydrohalic acid (HF aq., HCl aq., HBr aq.) (see Tables 1 to 3). Therefore, in this experiment, a more detailed investigation was conducted on the P2O5-ZnO-Al2O3 glass system.
[0083] The glass materials prepared were P2O5-ZnO-Al2O3-(AM)2O glass and P2O5-ZnO-Al2O3-(AEM)O glass (AEM is an alkaline earth metal). In the same manner as in Experiment 1, glass materials G-01 to G-42 (approximately 200 g each) having the chemical compositions shown in Tables 5 and 6 described below were prepared, and test pieces (length 10 mm × width 5 mm × thickness 5 mm) for corrosion resistance tests were taken from them.
[0084] Next, to evaluate the corrosion resistance of each glass material, an accelerated test was performed in which test pieces were immersed in test solutions of 30 mass% HF aq. (temperature 25°C), 10 mass% HCl aq. (temperature 60°C), and 20 mass% HBr aq. (temperature 60°C) for a specified time (25 hours), as in Experiment 1, and the mass loss per unit area of the test pieces (mg / mm 2 ) was sought.
[0085] When the mass loss of the glass material in any of the three test solutions (HF aq., HCl aq., HBr aq.) was smaller than that of the reference material, it was evaluated as "Good," and when the mass loss was smaller than that of the reference material in all three test solutions, it was evaluated as "Excellent." The corrosion resistance results are shown in Tables 5 and 6.
[0086] [Table 5]
[0087] [Table 6]
[0088] As shown in Tables 5 and 6, the P2O5-ZnO-Al2O3-(AM)2O glass materials G-01 to G-02, G-06 to G-08, G-11 to G-13, G-16 to G-19, G-23 to G-26, G-30 to G-33, G-37 to G-38, and the P2O5-ZnO-Al2O3-(AEM)O glass materials G-39 to G-42 have mass loss in the HCl aq. test solution that is 1 / 4 or less of that of the reference material, and are evaluated as "good."
[0089] In addition, the P2O5-ZnO-Al2O3-(AM)2O glass materials G-03 to G-05, G-09 to G-10, G-14 to G-15, G-20 to G-22, G-27 to G-29, and G-34 to G-36 had smaller mass losses than the reference material in all three test solutions, and were evaluated as "excellent." The glass materials evaluated as excellent have a chemical composition consisting of 51 mol% to 63 mol% P2O5, 16 mol% to 19 mol% ZnO, 10 mol% to 19 mol% Al2O3, and 6 mol% to 14 mol% (AM)2O, calculated as oxides.
[0090] [Experiment 4] (Investigation of glass paste conditions and roughness of the inner surface of the channel wall) In this experiment, simple gas flow path members were fabricated by changing the glass paste conditions, and hydrogen halide gas was passed through them to investigate the change in roughness of the inner surface of the flow path wall.
[0091] In the same manner as in Experiment 2, a metal substrate (U-shaped flow path pipe, flow path inner diameter 4.35 mm, U-shaped part curvature radius 22.5 mm, straight part length 50 mm, total flow path length 150 mm) made of SUS316L was fabricated by metal additive manufacturing (metal additive manufacturing process S1). In addition, a metal substrate for microstructure investigation was also prepared separately.
[0092] A glass paste was prepared in order to form a glass coating layer on the inner surface of the flow path wall of the additively manufactured metal substrate.
[0093] First, the remaining part of G-09 from which the test pieces for the corrosion resistance test were taken in Experiment 3 was pulverized using a stamp mill and a jet mill to prepare glass powder (average particle size 5 μm). After adding the resin binder EC to 50 g of the organic solvent BCA, they were mixed using a planetary centrifugal mixer (ARE-310, manufactured by Thinky Corporation) to prepare mixed solvents with different resin binder concentrations (resin binder concentration = 1 to 15 mass%).
[0094] The glass material G-10 powder in Table 1 was added to these mixed solvents so that the mixing ratio of the glass powder in the glass paste (solid content concentration) was 60 mass %, and then the mixture was mixed using the rotation-revolution mixer described above to prepare a glass paste (glass paste preparation step S2a).
[0095] Next, after pouring glass paste into the flow path of the metal substrate, excess glass paste was removed using a squeegee separately made to match the shape of the flow path of the metal substrate. After applying glass paste to the inner surface of the flow path wall, it was baked at 600°C to form a glass coating layer (glass paste application and baking process S2b), and a sample of a metal additive manufacturing flow path member was produced.
[0096] The fabricated metal additive manufacturing flow channel member and the metal substrate alone were cut to measure the roughness of the flow channel wall inner surface and observe the microstructure. The surface roughness was measured using a contact type surface roughness measuring instrument (Mitutoyo Corporation, Surftest SV-3000). In the surface roughness measurement, the measurement length (evaluation length) was set to 4 to 40 mm and the reference length was set to 0.8 to 8 mm in accordance with the ISO / JIS standard (ISO 4288:1996 / JIS B 0633:2001). The results of the roughness measurement of the flow channel wall inner surface are shown in Table 7.
[0097] The microstructure observation was performed using a digital microscope (VHX-1000, manufactured by Keyence Corporation). Figure 3 is a photograph of the microstructure of the inner surface of the flow channel wall of a metal substrate on which no glass coating layer is formed, and Figure 4 is a photograph of the microstructure of the inner surface of the flow channel wall of an example of a metal additive manufacturing flow channel member on which a glass coating layer is formed.
[0098] [Table 7]
[0099] As shown in Table 7, the arithmetic mean roughness Ra of the inner surface of the flow channel wall of the metal substrate on which no glass coating layer is formed is 8.9 μm. Also, as shown in Figure 3, it is confirmed that the inner surface of the flow channel wall of the metal substrate has large irregularities.
[0100] In contrast, it was confirmed that the Ra of the inner surface of the flow channel wall of the metal additive manufacturing flow channel member on which the glass coating layer was formed was 1 / 10 or less. Also, from Figure 4, it was confirmed that the surface smoothness of the inner surface of the flow channel wall of the metal additive manufacturing flow channel member was significantly improved by the formation of the glass coating layer. The sample shown in Figure 4 is a sample with a resin binder concentration of 7 mass% in the mixed solvent.
[0101] However, as shown in Table 7, when the resin binder concentration in the mixed solvent used in the glass paste preparation process is less than 3 mass% or more than 13 mass%, the Ra of the flow path wall inner surface exceeds 0.4 μm, which is considered to be desirable for a flow path member. In other words, it is confirmed that the resin binder concentration in the mixed solvent when preparing the glass paste is preferably 3 mass% or more and 13 mass% or less.
[0102] The above-mentioned embodiments and experimental examples have been described to aid in understanding the present invention, and the present invention is not limited to the specific configurations described. For example, it is possible to replace a part of the configuration of the embodiments with a configuration according to the technical common sense of a person skilled in the art, and it is also possible to add a configuration according to the technical common sense of a person skilled in the art to the configuration of the embodiments. In other words, it is possible to delete, replace, or add a part of the configuration of the embodiments and experimental examples in this specification without departing from the technical idea of the invention. [Explanation of symbols]
[0103] 100...metal additive manufacturing flow path member, 10...metal substrate, 20...glass coating layer.
Claims
1. A metal additive manufacturing flow path member for use in a supply gas line for circulating a corrosive fluid in a semiconductor device manufacturing apparatus, the corrosive fluid is HF, HCl or HBr; The metal substrate constituting the metal additive manufacturing flow path member has a surface unevenness, The inner surface of the flow path wall of the metal additive manufacturing flow path member has a glass coating layer formed thereon so as to fill at least the concave areas of the surface unevenness of the metal base, and the arithmetic mean roughness Ra of the inner surface is 0.4 μm or less; The glass coating layer is a P containing 10 mol % or more of ZnO in terms of oxide. 2 O 5 -ZnO-Al 2 O 3 -(AM) 2 O (AM is an alkali metal) glass layer, P containing 10 mol% or more ZnO 2 O 5 -ZnO-Al 2 O 3 -(AEM)O (AEM is an alkaline earth metal) glass layer, Bi 2 O 3 -ZnO-B 2 O 3 A layer of SiO 2 -B 2 O 3 -Na 2 At least one layer of O-based glass, A metal additive manufacturing flow path member.
2. The metal additive manufacturing flow path member according to claim 1, When the corrosive fluid is the HF, the coating layer of the glass is 2 O 5 -ZnO-Al 2 O 3 -(AM) 2 O-based glass layer, 2 O 5 -ZnO-Al 2 O 3 -(AEM)O-based glass layer, and the Bi 2 O 3 -ZnO-B 2 O 3 The glass has at least one layer of a SUS316L glass, and when subjected to a corrosion resistance test in which the glass is immersed in a 30% by mass HF aqueous solution at a temperature of 25°C for 25 hours, the amount of mass loss per unit area is smaller than that of SUS316L, When the corrosive fluid is the HCl or the HBr, the coating layer of the glass is 2 O 5 -ZnO-Al 2 O 3 -(AM) 2 O-based glass layer, 2 O 5 -ZnO-Al 2 O 3 -(AEM)O-based glass layer, and the SiO 2 -B 2 O 3 -Na 2 It includes at least one layer of an O-based glass layer, and when a corrosion resistance test is performed in which the glass is immersed in a 10 mass% HCl aqueous solution at a temperature of 60°C or a 10 mass% HBr aqueous solution at a temperature of 60°C for 25 hours, the mass loss per unit area of the glass is smaller than that of SUS316L. A metal additive manufacturing flow path member.
3. The metal additive manufacturing flow path member according to claim 2, When a corrosion resistance test was performed in which the glass was immersed in a 30 mass % HF aqueous solution at a temperature of 25° C. for 25 hours, the mass loss of the glass was 0.68 mg / mm 2 is as follows: When a corrosion resistance test was performed in which the glass was immersed in a 10% by mass HCl aqueous solution at a temperature of 60° C. for 25 hours, the mass loss of the glass was 0.091 mg / mm 2 is as follows: When a corrosion resistance test was performed in which the glass was immersed in a 10% by mass HBr aqueous solution at a temperature of 60° C. for 25 hours, the mass loss of the glass was 0.024 mg / mm 2 Below is the A metal additive manufacturing flow path member.
4. The metal additive manufacturing flow path member according to any one of claims 1 to 3, P 2 O 5 -ZnO-Al 2 O 3 -(AM) 2 O-based glass and the above P 2 O 5 -ZnO-Al 2 O 3 -(AEM)O-based glasses contain 45 mol % to 65 mol % P, calculated as oxide. 2 O 5 10 mol % or more and 25 mol % or less of ZnO; and 10 mol % or more and 25 mol % or less of Al. 2 O 3 and 2 mol% or more and 18 mol% or less (AM) 2 A metal additive manufacturing flow path member having a chemical composition consisting of O or (AEM)O.
5. The metal additive manufacturing flow path member according to claim 4, P 2 O 5 -ZnO-Al 2 O 3 -(AM) 2 O-based glass is a glass containing 51 mol % to 63 mol % of P in terms of oxide. 2 O 5 16 mol% to 19 mol% ZnO, and 10 mol% to 19 mol% Al 2 O 3 and 6 mol% to 14 mol% (AM) 2 A metal additive manufacturing flow path member having a chemical composition consisting of O.
6. The metal additive manufacturing flow path member according to any one of claims 1 to 5, Said (AM) 2 O is Na 2 O and K 2 O or more. The (AEM)O is at least one of MgO, CaO, SrO and BaO; A metal additive manufacturing flow path member.
7. A method for producing a metal additive manufacturing flow path member according to any one of claims 1 to 6, comprising the steps of: A metal additive manufacturing process for forming the metal base by a metal additive manufacturing method; and forming a glass coating layer on the inner surface of the flow path wall, The glass coating layer forming step includes: a glass paste preparation step of preparing a glass paste in which the glass powder, a resin binder, and an organic solvent are mixed; a glass paste application and baking process for applying the glass paste to the inner surface of the flow path wall and baking the glass coating layer by heat treating the metal substrate together; the glass paste has a resin binder content of 3% by mass or more and 13% by mass or less with respect to a total content of the organic solvent and the resin binder, and a glass powder content of the glass paste is 10% by mass or more and 90% by mass or less; The temperature of the heat treatment in the glass paste coating and baking step is equal to or higher than the softening point temperature of the glass and equal to or lower than 700° C. A method for manufacturing a metal additive manufacturing flow path member, comprising:
Citation Information
Patent Citations
Conduit made of metal
JP1986059087A
Chemical vapor growing apparatus
JP1994314653A
Mass flow controller
JP1995281759A
Glass composition for film formation
JP2011219325A
Glass paste
JP2013256437A