Laminate and sash
A laminate with a urethane resin primer layer and moisture-curable adhesive layer addresses the need for high adhesive strength in PVC-based sashes by enhancing bonding mobility and strength, using a water-based system for environmental friendliness.
Patent Information
- Application Number
- JP2023565930
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-04-26
- Filing Date
- 2022-10-13
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-10-13
AI Technical Summary
There is a strong demand for a water-based primer system with high adhesive strength for polyvinyl chloride (PVC)-based sashes, as current solvent-based primers used with moisture-curable polyurethane hot melt adhesives do not provide sufficient bonding strength.
A laminate structure comprising a base material, a primer layer made of a urethane resin with a glass transition temperature of 0°C or lower and water, and an adhesive layer formed from a moisture-curable polyurethane hot melt resin composition, which improves mobility and bonding strength.
The laminate achieves excellent adhesive strength, particularly when using polyvinyl chloride as the base material, making it suitable for PVC-based sashes.
Smart Images

Figure 0007563629000001 
Figure 0007563629000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate and a sash. [Background technology]
[0002] In the area of adhesives for building materials, the trend toward environmental friendliness is accelerating the shift from solvent-based materials to moisture-curing polyurethane hot melt adhesives (see, for example, Patent Document 1). In particular, for polyvinyl chloride (PVC) sashes, the decorative sheet wrapping process involves applying a current solvent-based primer to the PVC base material, and then laminating it with a moisture-curing polyurethane hot melt adhesive, but there is a strong demand for the primer to be water-based rather than solvent-based. However, the reality is that a system with high adhesive strength has yet to be found. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2005-232437 A Summary of the Invention [Problem to be solved by the invention]
[0004] The problem to be solved by the present invention is to provide a laminate having excellent adhesive strength. [Means for solving the problem]
[0005] The present invention provides a laminate having a substrate, a primer layer, and an adhesive layer, wherein the primer layer is formed from a resin composition containing a urethane resin (A) having a glass transition temperature of 0°C or less, and water, and the adhesive layer is formed from a moisture-curable polyurethane hot-melt resin composition.
[0006] The present invention also provides a sash comprising a decorative sheet on the adhesive layer of the laminate. Effect of the Invention
[0007] The laminate of the present invention has excellent adhesive strength. In particular, the laminate has excellent adhesive strength even when polyvinyl chloride (PVC) is used as the base material, and can be used particularly effectively as a PVC sash. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The laminate of the present invention has a substrate, a specific primer layer, and a specific adhesive layer.
[0009] Examples of the substrate that can be used include fiber substrates, glass substrates, wood substrates such as plywood, MDF (medium density fiberboard), and particle board, metal substrates, and resin substrates such as polyester, nylon, polystyrene, polycarbonate, polyvinyl chloride, ethylene-vinyl acetate copolymer, polyvinyl alcohol, polyethylene, and polypropylene. Note that the present invention has excellent adhesive strength even when polyvinyl chloride is used as the substrate.
[0010] The primer layer is formed from a resin composition containing a urethane resin (A) having a glass transition temperature of 0° C. or less and water. By using a urethane resin (A) having a glass transition temperature of 0° C. or less as the primer, the mobility of the primer layer is improved when it is bonded to a molten hot melt adhesive, and the substrate and the adhesive layer can be integrated, resulting in excellent adhesive strength. In addition, by using a resin composition containing water as the primer layer, it becomes an environmentally friendly material.
[0011] The glass transition temperature of the urethane resin (A) is preferably −50 to 0° C., more preferably −30 to 0° C., in terms of obtaining even better adhesive strength. The glass transition temperature of the urethane resin (A) is measured in accordance with JIS K7121-1987 using a DSC. Specifically, a resin composition (excluding a crosslinking agent) containing the urethane resin (A) is placed in a differential scanning calorimeter, heated to (Tmg+50° C.) at a heating rate of 10° C. / min, held for 3 minutes, and then rapidly cooled. The midpoint glass transition temperature (Tmg) is read from the differential thermal curve.
[0012] The urethane resin (A) is dispersible in water, and is, for example, a urethane resin having a hydrophilic group such as an anionic group, a cationic group, or a nonionic group. These urethane resins (A) may be used alone or in combination of two or more. Among these, from the viewpoints of production stability and water dispersion stability, urethane resins having an anionic group and / or a nonionic group are more preferred.
[0013] Examples of a method for obtaining a urethane resin having an anionic group include a method using, as a raw material, one or more compounds selected from the group consisting of glycol compounds having a carboxyl group and compounds having a sulfonyl group.
[0014] Examples of the glycol compound having a carboxyl group include 2,2-dimethylolpropionic acid, 2,2-dimethylolbutanoic acid, 2,2-dimethylolbutyric acid, 2,2-dimethylolpropionic acid, 2,2-valeric acid, etc. These compounds may be used alone or in combination of two or more.
[0015] Examples of the compound having a sulfonyl group include 3,4-diaminobutanesulfonic acid, 3,6-diamino-2-toluenesulfonic acid, 2,6-diaminobenzenesulfonic acid, N-(2-aminoethyl)-2-aminosulfonic acid, N-(2-aminoethyl)-2-aminoethylsulfonic acid, N-2-aminoethane-2-aminosulfonic acid, and N-(2-aminoethyl)-β-alanine; salts thereof. These compounds may be used alone or in combination of two or more.
[0016] As a method for obtaining the urethane resin having a nonionic group, for example, a method using a compound having an oxyethylene structure as a raw material can be mentioned.
[0017] As the compound having an oxyethylene structure, for example, polyether polyols having an oxyethylene structure such as polyethylene glycol, polyoxyethylene polyoxypropylene glycol, polyoxyethylene polyoxytetramethylene glycol, and polyethylene glycol dimethyl ether can be used. These compounds may be used alone or in combination of two or more. Among these, it is preferable to use polyethylene glycol and / or polyethylene glycol dimethyl ether, since hydrophilicity can be controlled more easily.
[0018] The number average molecular weight of the raw material used to obtain the urethane resin having a nonionic group is preferably in the range of 200 to 10,000, more preferably in the range of 300 to 3,000, and even more preferably in the range of 300 to 2,000, from the viewpoint of obtaining even better emulsifiability and water dispersion stability. The number average molecular weight of the raw material used to obtain the urethane resin having a nonionic group is a value measured by gel permeation column chromatography (GPC).
[0019] The urethane resin having a cationic group can be obtained, for example, by using one or more compounds having an amino group as a raw material.
[0020] Examples of the compound having an amino group include compounds having primary and secondary amino groups such as triethylenetetramine and diethylenetriamine, compounds having a tertiary amino group such as N-alkyldialkanolamines such as N-methyldiethanolamine and N-ethyldiethanolamine, and N-alkyldiaminoalkylamines such as N-methyldiaminoethylamine and N-ethyldiaminoethylamine, etc. These compounds may be used alone or in combination of two or more.
[0021] Specific examples of the urethane resin (A) that can be used include a reaction product of a polyol (a1), a polyisocyanate (a2), and, if necessary, a compound (a3) having a hydrophilic group (raw materials used to obtain the urethane resin having an anionic group, the urethane resin having a cationic group, and the urethane resin having a nonionic group).
[0022] As the polyol (a1), for example, polyether polyol, polyester polyol, polyacrylic polyol, polycarbonate polyol, polybutadiene polyol, etc. can be used. These polyols may be used alone or in combination of two or more. When the urethane resin having a nonionic group is used as the urethane resin (A), the polyol (a1) is a material other than the raw material used to obtain the urethane resin having a nonionic group. As the polyol (a1), polyester polyol is preferable because it can obtain a better adhesive strength.
[0023] The number average molecular weight of the polyol (a1) is preferably 500 to 100,000, more preferably 800 to 10,000, from the viewpoint of the mechanical strength and adhesive strength of the resulting film. The number average molecular weight of the polyol (a1) is a value measured by gel permeation column chromatography (GPC).
[0024] The proportion of the polyol (a1) used is more preferably 40 to 90 mass %, particularly preferably 50 to 80 mass %, of the total mass of the raw materials constituting the urethane resin (A), in terms of obtaining even better mechanical strength and adhesive strength.
[0025] The polyol (a1) may be used in combination with a chain extender (a1-1) if necessary. The chain extender (a1-1) may have a molecular weight of less than 500 (preferably in the range of 50 to 450). Specifically, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, hexamethylene glycol, saccharose, methylene glycol, glycerin, sorbitol, bisphenol A, 4,4'-dihydroxydiphenyl, 4,4'-dihydroxydiphenyl ether, etc. Chain extenders having a hydroxyl group such as ethyl ether or trimethylolpropane; chain extenders having an amino group such as ethylenediamine, 1,2-propanediamine, 1,6-hexamethylenediamine, piperazine, 2,5-dimethylpiperazine, isophoronediamine, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 4,4'-dicyclohexylmethanediamine, 3,3'-dimethyl-4,4'-dicyclohexylmethanediamine, 1,4-cyclohexanediamine, and hydrazine can be used. These chain extenders may be used alone or in combination of two or more. The molecular weight of the chain extender (a1-1) is a value calculated from the chemical formula.
[0026] When the chain extender (a1-1) is used, the amount of the chain extender (a1-1) used is more preferably 0.1 to 30 mass %, particularly preferably 0.5 to 10 mass %, of the total mass of the raw materials constituting the urethane resin (A), in terms of obtaining even better mechanical strength and adhesive strength.
[0027] Examples of the polyisocyanate (a2) include aromatic polyisocyanates such as phenylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, naphthalene diisocyanate, polymethylene polyphenyl polyisocyanate, and carbodiimidized diphenylmethane polyisocyanate; and aliphatic or alicyclic polyisocyanates such as hexamethylene diisocyanate, lysine diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, dimer acid diisocyanate, and norbornene diisocyanate. These polyisocyanates may be used alone or in combination of two or more.
[0028] The proportion of the polyisocyanate (a2) used is more preferably 5 to 40 mass %, particularly preferably 10 to 35 mass %, of the total mass of the raw materials constituting the urethane resin (A), in terms of obtaining even better mechanical strength and adhesive strength.
[0029] The proportion of the compound (a3) having a hydrophilic group used is more preferably 0.25 to 2 mass%, particularly preferably 0.5 to 1.8 mass%, of the total mass of the raw materials constituting the urethane resin (A), in terms of obtaining even better emulsifiability, water dispersion stability, and film-forming properties.
[0030] The average particle diameter of the urethane resin (A) is preferably in the range of 0.01 to 1 μm, more preferably in the range of 0.05 to 0.9 μm, in order to obtain even better film-forming properties. The average particle diameter of the urethane resin (A) is measured by using a laser diffraction / scattering particle size distribution measuring device ("LA-910" manufactured by Horiba, Ltd.) to measure the average particle diameter of a resin composition containing the urethane resin (A) using water as a dispersion liquid, a relative refractive index of 1.10, and an area as the particle diameter standard.
[0031] The content of the urethane resin (A) in the resin composition forming the primer layer in the present invention is preferably from 10 to 90% by mass, more preferably from 20 to 70% by mass.
[0032] The water contained in the resin composition may be ion-exchanged water, distilled water, etc. These waters may be used alone or in combination of two or more kinds.
[0033] Next, a method for producing the resin composition containing the urethane resin (A) used in the present invention will be described.
[0034] The method for producing the resin composition used in the present invention comprises a step of reacting the polyol (a1), the polyisocyanate (a2), and the compound having a hydrophilic group (a3) in the absence of a solvent to obtain a urethane prepolymer (i) having an isocyanate group (hereinafter abbreviated as the "prepolymer step"); then, dispersing the urethane prepolymer (i) in water (hereinafter abbreviated as the "emulsification step"); and thereafter, reacting with the chain extender (a1-1) to obtain a urethane resin (X) (hereinafter abbreviated as the "chain extension step").
[0035] The prepolymer process can be carried out in an organic solvent such as methyl ethyl ketone or acetone; a reaction vessel equipped with an agitating blade; a kneading machine such as a kneader, continuous kneader, taper roll, single-screw extruder, twin-screw extruder, triple-screw extruder, universal mixer, Plastomill, or Bodeta-type kneader; a rotary dispersion mixer such as a TK Homomixer, Filmix, Ebara Milder, Clearmix, Ultra-Turrax, Cavitron, or Biomixer; an ultrasonic dispersion device; or a device such as an in-line mixer that has no moving parts and can mix by the flow of the fluid itself, in a solvent-free environment.
[0036] In the prepolymer step, the molar ratio [isocyanate group / (hydroxyl group and amino group)] of the sum of the hydroxyl group in the polyol (a1) and the hydroxyl group and amino group in the compound (a3) having a hydrophilic group to the isocyanate group in the polyisocyanate (a2) is preferably 1.1 to 3, and more preferably 1.2 to 2, in terms of obtaining even better adhesive strength and mechanical strength.
[0037] The reaction in the prepolymer step may be carried out, for example, at 50 to 120° C. for 1 to 10 hours.
[0038] The chain extension step is a step of obtaining a urethane resin (A) by increasing the molecular weight of the urethane prepolymer (i) through a reaction between the isocyanate group of the urethane prepolymer (i) and the chain extender (a1-1).
[0039] In the chain extension step, the molar ratio of the isocyanate groups in the urethane prepolymer (i) to the sum of the hydroxyl groups and amino groups in the chain extender (a1-1) [(hydroxyl groups and amino groups) / isocyanate groups] is preferably 0.8 to 1.1, and more preferably 0.9 to 1, in order to obtain even better adhesive strength and mechanical strength.
[0040] The chain extension step can be carried out using the same equipment as the prepolymer step.
[0041] The resin composition contains the urethane resin (A) and water as essential components, and may contain other additives as necessary.
[0042] Examples of the other additives that can be used include surfactants, crosslinking agents, emulsifiers, neutralizing agents, thickeners, urethane catalysts, fillers, pigments, dyes, flame retardants, leveling agents, antiblocking agents, etc. These additives may be used alone or in combination of two or more.
[0043] The adhesive layer is formed from a moisture-curable polyurethane hot-melt resin composition, which is solvent-free, environmentally friendly, and provides excellent adhesive strength.
[0044] The moisture-curable polyurethane hot-melt resin composition may, for example, be one containing a urethane prepolymer having an isocyanate group, which is a reaction product of a polyol (X) and a polyisocyanate (Y).
[0045] As the polyol (X), for example, polyester polyol, polycarbonate polyol, polyether polyol, etc. can be used. These polyols may be used alone or in combination of two or more. Among these, polyester polyols are preferable because they have a better adhesive strength with a polyvinyl chloride substrate. The content of the polyester polyol in the polyol (X) is preferably 50% by mass or more, more preferably 70% by mass or more.
[0046] As the polyester polyol, for example, a long-chain crystalline polyester polyol (x1), an aliphatic polyester polyol (x2) made from a glycol having a 2,2-dimethyl-1,3-propylene group other than the long-chain crystalline polyester polyol (x1), an aromatic polyester polyol (x3), an amorphous polyester polyol other than these, etc. can be used. These polyester polyols may be used alone or in combination of two or more. Among these, from the viewpoint of further excellent adhesive strength with a polyvinyl chloride substrate, one or more polyester polyols selected from the group consisting of the long-chain crystalline polyester polyol (x1), the aliphatic polyester polyol (x2), and the aromatic polyester polyol (x3) are preferred, and it is more preferable to use three components in combination.
[0047] The long-chain crystalline polyester polyol (x1) may be, for example, a reaction product of a compound having a hydroxyl group and a polybasic acid. In the present invention, "crystalline" refers to a material in which a peak of heat of crystallization or heat of fusion can be confirmed in a DSC (differential scanning calorimeter) measurement in accordance with JISK7121:2012, and "amorphous" refers to a material in which the peak cannot be confirmed.
[0048] Examples of the compound having a hydroxyl group include ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, decanediol, trimethylolpropane, trimethylolethane, and glycerin. These compounds may be used alone or in combination of two or more. Among these, it is preferable to use one or more selected from the group consisting of butanediol, hexanediol, octanediol, and decanediol, in order to increase crystallinity and obtain even better adhesive strength.
[0049] Examples of the polybasic acid that can be used include oxalic acid, malonic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, and dodecanedioic acid. These compounds may be used alone or in combination of two or more. Among these, it is preferable to use one or more selected from the group consisting of adipic acid, sebacic acid, and dodecanedioic acid, since this provides a higher adhesive strength.
[0050] The number average molecular weight of the long-chain crystalline polyester polyol (x1) is preferably 500 to 10,000, and more preferably 1,000 to 7,000, in terms of obtaining even better adhesive strength. The number average molecular weight of the crystalline polyester polyol (x1) is a value measured by gel permeation chromatography (GPC).
[0051] When the long-chain crystalline polyester polyol (x1) is used, the amount of use is preferably 32 to 40 mass%, and more preferably 33 to 37 mass%, based on the total amount of the polyol (X) and the polyisocyanate (Y), in terms of obtaining even better adhesive strength.
[0052] The aliphatic polyester polyol (x2) is other than the long-chain crystalline polyester polyol (x1) and is made from a glycol having a 2,2-dimethyl-1,3-propylene group as a raw material.
[0053] In order to achieve excellent adhesive strength, the aliphatic polyester polyol (a2) is more preferably a combination of an aliphatic polyester polyol (x2-1) having a number average molecular weight of 1,000 to 3,000 and an aliphatic polyester polyol (x2-2) having a number average molecular weight of 5,000 to 9,000, and the mass ratio [(x2-1) / (x2-2)] in the combined use is preferably 1 to 3. In the above-mentioned configuration, the glass transition temperature and viscosity of the aliphatic polyester polyol as a whole are increased, so that very excellent adhesive strength, particularly to polyvinyl chloride, can be obtained.
[0054] The aliphatic polyester polyol (x2-1) and the aliphatic polyester polyol (x2-2) can both be a reaction product of a compound having a hydroxyl group, which contains as an essential component a glycol having a 2,2-dimethyl-1,3-propylene group, and a polybasic acid.
[0055] Examples of the glycol having a 2,2-dimethyl-1,3-propylene group include neopentyl glycol, its dimer, and its trimer. These compounds may be used alone or in combination of two or more. Among these, neopentyl glycol is preferred because it provides a higher adhesive strength.
[0056] The amount of the glycol having a 2,2-dimethyl-1,3-propylene group used is preferably 10% by mass or more, and more preferably 10 to 20% by mass, based on the total amount of the compound having a hydroxyl group.
[0057] Examples of the compound having a hydroxyl group that can be used other than the glycol having a 2,2-dimethyl-1,3-propylene group include ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, decanediol, cyclohexanedimethanol, bisphenol A, bisphenol F, alkylene oxide adducts thereof, triethylene glycol, trimethylolpropane, trimethylolethane, and glycerin.
[0058] Examples of the polybasic acid that can be used include oxalic acid, malonic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, dodecanedioic acid, etc. These compounds may be used alone or in combination of two or more kinds.
[0059] The number average molecular weight of the aliphatic polyester polyol (x2-1) is preferably 1,500 to 2,500 in terms of obtaining even better adhesive strength, and the number average molecular weight of the aliphatic polyester polyol (x2-2) is preferably 6,000 to 8,000. The number average molecular weights of the aliphatic polyester polyol (x2-1) and the aliphatic polyester polyol (x2-2) are values measured by gel permeation chromatography (GPC).
[0060] The mass ratio of the aliphatic polyester polyol (x2-1) to the aliphatic polyester polyol (x2-2) [(x2-1) / (x2-2)] is more preferably from 1 to 2.5, since even better adhesive strength can be obtained.
[0061] When the aliphatic polyester polyol (x2) is used, the total amount used is preferably 15 to 38 mass%, more preferably 20 to 37 mass%, based on the total amount of the polyol (X) and the polyisocyanate (Y), in terms of obtaining even better adhesive strength.
[0062] The aromatic polyester polyol (x3) may be, for example, a reaction product of a compound having a hydroxyl group with a polybasic acid including an aromatic polybasic acid; a reaction product of an aromatic compound having two or more hydroxyl groups with a polybasic acid; a reaction product of an aromatic compound having two or more hydroxyl groups with a polybasic acid including an aromatic polybasic acid; or the like.
[0063] Examples of the compound having a hydroxyl group include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, diethylene glycol, triethylene glycol, triethylene glycol, tetraethylene glycol, neopentyl glycol, 1,2-butanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, and 2-methyl-1,3-propanediol. Examples of the compounds that can be used include aliphatic compounds such as propanediol, 2,2-diethyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2-ethyl-2-butyl-1,3-propanediol, 2-methyl-1,8-octanediol, 2,4-diethyl-1,5-pentanediol, trimethylolethane, trimethylolpropane, and pentaerythritol; and alicyclic compounds such as cyclopentanediol, cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, and alkylene oxide adducts thereof. These compounds may be used alone or in combination of two or more.
[0064] Examples of the aromatic compound having two or more hydroxyl groups include bisphenol A, bisphenol F, and their alkylene oxide (ethylene oxide, propylene oxide, butylene oxide, etc.) adducts. These compounds may be used alone or in combination of two or more.
[0065] As the aromatic polybasic acid, for example, phthalic acid, isophthalic acid, terephthalic acid, phthalic anhydride, etc. can be used. As other polybasic acids, for example, oxalic acid, malonic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, 1,12-dodecanedicarboxylic acid, etc. can be used. These polybasic acids may be used alone or in combination of two or more. As the aromatic polybasic acid, from the viewpoint of obtaining even more excellent adhesive strength,
[0066] Other polybasic acids that can be used include, for example, succinic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, decanedioic acid, dodecanedioic acid, eicosadioic acid, citraconic acid, itaconic acid, citraconic anhydride, and itaconic anhydride.
[0067] As the aromatic polyester polyol (x3), one made from one or more phthalic acid compounds selected from the group consisting of phthalic acid, isophthalic acid, terephthalic acid, and phthalic anhydride is preferable, since even better adhesive strength can be obtained.
[0068] The number average molecular weight of the aromatic polyester polyol (x3) is preferably from 500 to 10,000, and more preferably from 1,000 to 5,000, in terms of obtaining even better adhesion. The number average molecular weight of the aromatic polyester polyol (x3) is a value measured by gel permeation chromatography (GPC).
[0069] The amount of the aromatic polyester polyol (x3) used is preferably 15 to 35 mass%, and more preferably 18 to 32 mass%, based on the total amount of the polyol (X) and the polyisocyanate (Y), in terms of obtaining even better adhesive strength.
[0070] As the polyisocyanate (Y), for example, aromatic polyisocyanates such as polymethylene polyphenyl polyisocyanate, diphenylmethane diisocyanate, carbodiimide-modified diphenylmethane diisocyanate, xylylene diisocyanate, phenylene diisocyanate, tolylene diisocyanate, and naphthalene diisocyanate; aliphatic or alicyclic polyisocyanates such as hexamethylene diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and tetramethylxylylene diisocyanate can be used. These polyisocyanates may be used alone or in combination of two or more. Among these, aromatic polyisocyanates are preferred, and diphenylmethane diisocyanate is more preferred, from the viewpoint of obtaining even better adhesive strength.
[0071] The urethane prepolymer is obtained by reacting the polyol (X) with the polyisocyanate (Y), and has an isocyanate group capable of reacting with moisture present in the air or in the substrate to which the moisture-curable polyurethane hot-melt resin composition is applied to form a crosslinked structure.
[0072] The urethane prepolymer can be produced, for example, by adding the polyisocyanate (Y) to a reaction vessel containing the polyol (X) and reacting them under conditions in which the isocyanate groups of the polyisocyanate (Y) are in excess of the hydroxyl groups of the polyol (X).
[0073] In producing the urethane prepolymer, the equivalent ratio [NCO / OH] of the isocyanate groups in the polyisocyanate (Y) to the hydroxyl groups in the polyol (X) is preferably 1.5 to 4, and more preferably 1.8 to 3.0, in terms of obtaining even better adhesive strength.
[0074] The isocyanate group content (hereinafter abbreviated as "NCO%") of the urethane prepolymer obtained by the above method is preferably 1 to 6 mass%, more preferably 2 to 4 mass%, in order to obtain even better adhesive strength. The NCO% of the hot-melt urethane prepolymer is a value measured by potentiometric titration in accordance with JIS K1603-1:2007.
[0075] The moisture-curable polyurethane hot-melt resin composition used in the present invention preferably contains the urethane prepolymer, and may further contain other additives, if necessary.
[0076] Examples of the other additives that can be used include light resistance stabilizers, curing catalysts, plasticizers, stabilizers, fillers, dyes, pigments, carbon black, vehicles, fluorescent brighteners, silane coupling agents, waxes, thermoplastic resins, etc. These additives may be used alone or in combination of two or more.
[0077] As described above, the laminate of the present invention has excellent adhesive strength. In particular, the laminate has excellent adhesive strength even when polyvinyl chloride (PVC) is used as the base material, and can be used particularly effectively as a PVC sash.
[0078] The PVC-based sash may be configured, for example, with polyvinyl chloride as the base material, the primer layer, the adhesive layer, and a decorative sheet such as wood grain decorative paper on the adhesive layer.
[0079] As a method for producing the PVC-based sash, for example, a method can be mentioned in which a resin composition for forming the primer layer is applied onto a PVC base material, dried, and then the moisture-curable polyurethane hot melt resin composition is applied onto a decorative sheet, and the two are laminated together and allowed to mature.
[0080] The resin composition and the moisture-curable polyurethane hot-melt resin composition can be applied using, for example, a roll coater, a spray coater, a T-tie coater, a knife coater, a comma coater, or the like.
[0081] The thickness of the primer layer is, for example, 0.5 to 20 μm, and the thickness of the adhesive layer is, for example, 20 to 150 μm.
[0082] The aging conditions after lamination can be appropriately determined, for example, at a temperature of 20 to 50° C., at a relative humidity of 40 to 90% RH, and for a period of 0.5 to 5 days. EXAMPLES
[0083] The present invention will now be described in more detail with reference to examples.
[0084] [Synthesis Example 1] Resin composition for forming primer layer <p1>Manufacturing method In a nitrogen-substituted vessel equipped with a thermometer, nitrogen gas, an inlet tube, and a stirrer, 155 parts by mass of 1,6-hexanediol (hereinafter abbreviated as "HG"), 137 parts by mass of neopentyl glycol, and 424 parts by mass of adipic acid were added and melted at 120 ° C. Then, the mixture was heated to 220 ° C. over 3 to 4 hours with stirring and held for 5 hours, then cooled to 150 ° C., and 88 parts by mass of 2,2-dimethylolpropionic acid (hereinafter abbreviated as "DMPA") was added, and the mixture was held at 150 ° C. for 5 to 10 hours with stirring, and then 300 parts by mass of methyl ethyl ketone was added to prepare a methyl ethyl ketone solution (P1-A) of polyester polyol having a carboxyl group with a non-volatile content of 70% by mass. In a nitrogen-substituted vessel equipped with a thermometer, nitrogen gas, an inlet tube, and a stirrer, 198 parts by mass of a methyl ethyl ketone solution of the above-mentioned polyester polyol (P1-A) having a carboxyl group, 160 parts by mass of a polyester polyol ("Crisbon CMA-654" manufactured by DIC Corporation, number average molecular weight: 1,500), 19 parts by mass of HG, 75 parts by mass of tolylene diisocyanate, and 152 parts by mass of methyl ethyl ketone were reacted at 70°C until the specified NCO% of the reactants was reached, thereby obtaining a methyl ethyl ketone solution of a urethane prepolymer having an isocyanate group at its end. Next, 17.2 parts by mass of triethylamine was added as a neutralizing agent to the organic solvent solution of the urethane prepolymer and stirred, and then 653 parts by mass of water and 7.7 parts by mass of piperazine were added and mixed to cause a chain extension reaction, thereby obtaining an aqueous dispersion of the urethane resin. Next, the solvent was removed from this aqueous dispersion to obtain a primer layer forming resin composition (P1) with a non-volatile content of 40% by mass. The glass transition temperature of the obtained urethane resin was -30°C.
[0085] [Synthesis Example 2] Resin composition for forming primer layer <p2>Manufacturing method 2 parts by mass of a silane coupling agent (KBM-403 manufactured by Shin-Etsu Silicones Co., Ltd.) and 5 parts by mass of water were added to 100 parts by mass of the above-mentioned resin composition for forming a primer layer (P1) to obtain a 40% by mass resin composition for forming a primer layer (P2).
[0086] [Comparative synthesis example 1] Resin composition for forming primer layer <rp1>Manufacturing method In a reaction vessel equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, 33.3 parts by mass of isophthalic acid, 16.7 parts by mass of sebacic acid, 7.3 parts by mass of adipic acid, 6 parts by mass of ethylene glycol, 11.0 parts by mass of 1,6-hexanediol, and 22.5 parts by mass of neopentyl glycol were charged while introducing nitrogen gas, and a polycondensation reaction was carried out at 230°C for 24 hours at 180 to 230°C until the acid value became 1 or less, and the mixture was cooled to 90°C or less, and 20.4 parts by mass of methyl ethyl ketone was added and mixed to obtain an aromatic polyester polyol (RP1-A). 207 parts by mass of aromatic polyester polyol (RP1-A), 7.4 parts by mass of 1,4 butanediol, and 17.0 parts by mass of methyl ethyl ketone were added to a reaction vessel, and the mixture was stirred and mixed uniformly. Next, 14.7 parts by mass of DMPA was added, followed by 46.8 parts by mass of tolylene diisocyanate, and the mixture was reacted at 70°C for 12 hours to carry out a urethane-forming process. After confirming that the isocyanate value was 0.1% or less, 97 parts by mass of methyl ethyl ketone and 0.7 parts by mass of 1,3 butanediol were added to obtain an organic solvent solution of urethane prepolymer. Next, 11.6 parts by mass of triethylamine was added as a neutralizing agent to the organic solvent solution of urethane prepolymer, and the mixture was stirred, and 1000 parts by mass of water was added and mixed to obtain an aqueous dispersion of urethane resin. Next, the aqueous dispersion was desolvated to obtain a primer layer forming resin composition (RP1) with a non-volatile content of 23% by mass. The glass transition temperature of the obtained urethane resin was 5°C.
[0087] [Comparative Synthesis Example 2] Resin composition for forming primer layer <rp2>Manufacturing method In a reaction vessel equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, 29.3 parts by mass of isophthalic acid, 29.3 parts by mass of terephthalic acid, 13 parts by mass of ethylene glycol, and 22.3 parts by mass of diethylene glycol were charged while introducing nitrogen gas, and a polycondensation reaction was carried out at 230°C for 24 hours at 180 to 230°C until the acid value became 1 or less. The mixture was then cooled to 90°C or less, and 26.3 parts by mass of methyl ethyl ketone was added and mixed to obtain an aromatic polyester polyol (RP2-A). 226 parts by mass of aromatic polyester polyol (RP2-A) and 40.0 parts by mass of methyl ethyl ketone were added to a reaction vessel, and the mixture was stirred and mixed uniformly. Next, 13 parts by mass of 2,2-dimethylolpropionic acid was added, followed by 44.3 parts by mass of isophorone diisocyanate and 0.2 parts by mass of stannous octylate, and the mixture was reacted at 70°C for 12 hours to carry out a urethane-forming process. After confirming that the isocyanate value was 0.1% or less, 25 parts by mass of methyl ethyl ketone and 0.4 parts by mass of methanol were added to obtain an organic solvent solution of a urethane prepolymer. Next, 7.1 parts by mass of aqueous ammonia was added as a neutralizing agent to the organic solvent solution of the urethane prepolymer and stirred, and 877 parts by mass of water was further added and mixed to obtain an aqueous dispersion of the urethane resin. Next, the solvent was removed from this aqueous dispersion to obtain a resin composition for forming a primer layer (RP-2) with a non-volatile content of 22% by mass. The glass transition temperature of the obtained urethane resin was 50°C.
[0088] [Synthesis Example 3] Moisture-curable polyurethane hot melt resin composition for forming adhesive layer <pur1> Into a four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet, and a reflux condenser, 34 parts by mass of long-chain crystalline polyester polyol (a reaction product of 1,6-hexanediol and dodecanedioic acid, number average molecular weight: 3,500, hereinafter abbreviated as "crystalline PEs (1)"), 10 parts by mass of aliphatic polyester polyol (a reaction product of diethylene glycol, neopentyl glycol, 1,6-hexanediol, and adipic acid, number average molecular weight: 2,000, the amount of neopentyl glycol used in the total amount of all glycols: 14 mass%, hereinafter abbreviated as "aliphatic PEs (1)"), 10 parts by mass of an aliphatic polyester polyol (a reaction product of diethylene glycol, neopentyl glycol, 1,6-hexanediol, and adipic acid; number average molecular weight: 7,000; the amount of neopentyl glycol used in the total amount of all glycols: 14 mass%; hereinafter abbreviated as "aliphatic PEs (2)") and 30 parts by mass of an aromatic polyester polyol (a reaction product of neopentyl glycol and orthophthalic acid; number average molecular weight: 2,000; hereinafter abbreviated as "aromatic PEs (1)") were charged and heated at 100°C under reduced pressure to dehydrate until the moisture in the flask was 0.05 mass%. After cooling the flask to 90°C, 16 parts by mass of 4,4'-diphenylmethane diisocyanate (hereinafter abbreviated as "MDI") melted at 70°C is added, and the mixture is reacted at 110°C for about 2 hours under a nitrogen atmosphere until the NCO% becomes constant, thereby obtaining a moisture-curable polyurethane hot melt resin composition for forming an adhesive layer containing a urethane prepolymer. <pur1>obtained.
[0089] [Synthesis Example 4] Moisture-curable polyurethane hot melt resin composition for forming adhesive layer <pur2> A four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet, and a reflux condenser was charged with 34 parts by mass of crystalline PEs (1), 20 parts by mass of aliphatic PEs (1), 10 parts by mass of aliphatic PEs (2), and 20 parts by mass of aromatic PEs (1), and heated to 100°C under reduced pressure to dehydrate the water content in the flask to 0.05% by mass. After cooling the flask to 90°C, 16 parts by mass of MDI melted at 70°C was added, and the mixture was reacted at 110°C for about 2 hours under a nitrogen atmosphere until the NCO% became constant, to obtain a moisture-curable polyurethane hot melt resin composition for forming an adhesive layer, which contains urethane prepolymer (i-2). <pur2>obtained.
[0090] [Example 1] On a polyvinyl chloride substrate, the primer layer-forming resin composition obtained in Synthesis Example 1 was <p1>The composition was applied with a roller so that the thickness after drying was 3 μm, and dried in a dryer at 60° C. for 10 minutes. Next, the moisture-curable polyurethane hot melt resin composition for forming an adhesive layer obtained in Synthesis Example 3, which was melted at 120° C. for 1 hour, was applied onto a decorative sheet. <pur1>was applied to a thickness of 50 μm and laminated to the above-mentioned primer layer. This laminate was aged for 48 hours in an environment of 23° C. and 50% humidity to obtain a PVC-based laminate.
[0091] [Examples 2 to 3, Comparative Examples 1 to 3] A PVC laminate was obtained in the same manner as in Example 1, except that the type of the resin composition for forming a primer layer used was changed as shown in Tables 1 and 2.
[0092] [Method of measuring number average molecular weight and weight average molecular weight] The number average molecular weights of the polyols used in the Synthesis Examples and Comparative Synthesis Examples are values measured by gel permeation column chromatography (GPC) under the following conditions.
[0093] Measurement equipment: High-speed GPC equipment (Tosoh Corporation "HLC-8220GPC") Column: The following columns manufactured by Tosoh Corporation were used, connected in series. "TSKgel G5000" (7.8mm I.D. x 30cm) x 1 "TSKgel G4000" (7.8mm I.D. x 30cm) x 1 "TSKgel G3000" (7.8mm I.D. x 30cm) x 1 "TSKgel G2000" (7.8mmI.D. x 30cm) x 1 Detector: RI (differential refractometer) Column temperature: 40℃ Eluent: tetrahydrofuran (THF) Flow rate: 1.0mL / min Injection volume: 100 μL (sample concentration 0.4% by mass in tetrahydrofuran solution) Standard sample: A calibration curve was prepared using the following standard polystyrene.
[0094] (Standard polystyrene) "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-5000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation
[0095] [Method for evaluating adhesive strength] (1) 180 degree peeling test The PVC laminates obtained in the examples and comparative examples were cut into 1 inch widths to prepare test pieces, which were peeled off in a 180 degree direction and their strength was measured using an autograph ("AG-1" manufactured by Shimadzu Corporation) and evaluated as follows. "〇";40N / inch or more "×": Other than the above
[0096] (2) Heat creep test The PVC laminates obtained in the Examples and Comparative Examples were cut into 1 inch widths to prepare test pieces, which were then placed in a 60°C dryer with a load of 500 g / inch applied, and the travel distance after 24 hours or the time it took for the specimen to fall after a 40 mm movement was measured. "〇"; 5mm or less "×": Other than the above
[0097] [Table 1]
[0098] [Table 2]
[0099] It was found that Examples 1 to 3, which are the laminates of the present invention, were excellent in adhesive strength.
[0100] On the other hand, in Comparative Examples 1 and 2, the glass transition temperature of the urethane resin used in the primer layer exceeded the range specified in the present invention, but the adhesive strength was poor.
[0101] Comparative Example 3 was an embodiment without a primer layer, but the adhesive strength was poor.
Claims
1. A laminate having a substrate, a primer layer, and an adhesive layer, the primer layer is formed from a resin composition containing a urethane resin (A) having a glass transition temperature of 0° C. or lower and water, The urethane resin (A) is made from at least a polyol (a1) including a polyester polyol and a polyisocyanate (a2) as raw materials, The adhesive layer is formed from a moisture-curable polyurethane hot-melt resin composition, The moisture-curable polyurethane hot-melt resin composition is a reaction product of a polyol (X) including a polyester polyol and a polyisocyanate (Y), The polyester polyol contained in the polyol (X) includes a long-chain crystalline polyester polyol (x1), an aliphatic polyester polyol (x2) other than the long-chain crystalline polyester polyol (x1) that is derived from a glycol having a 2,2-dimethyl-1,3-propylene group, and an aromatic polyester polyol (x3).
2. 2. The laminate according to claim 1, wherein the substrate is polyvinyl chloride.
3. 3. A sash comprising a decorative sheet on said adhesive layer of the laminate according to claim 1 or 2.
Citation Information
Patent Citations
Moisture curable polyurethane adhesive composition
CN112601792A
Manufacture of decorative sheet coating material
JP1999320805A
Moisture-curing polyurethane hot melt resin composition
JP2005206828A
Moisture hardenable hot melt adhesive
JP2005232437A
Moisture-curing type polyurethane hot melt adhesive
JP2007091996A