Packaging materials, packages and packaging articles

A polyethylene-based laminate with a crystallinity of 35% or more in the base layer addresses recyclability and strength issues in conventional packaging materials, offering enhanced heat resistance and expanded sealing temperature ranges for improved packaging performance.

JP7563636B2Active Publication Date: 2024-10-08TOPPAN HOLDINGS INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024000322
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-11-30
Filing Date
2024-01-04
Publication Date
2024-10-08
Estimated Expiration
2042-09-02

AI Technical Summary

Technical Problem

Conventional packaging materials composed of multiple resin types are difficult to recycle due to separation issues, leading to low recyclability and limitations in strength and heat resistance, which are essential for various packaging applications.

Method used

A laminate structure is designed with a base material layer and sealant layer containing polyethylene, where the base layer has a crystallinity of 35% or more, and optionally includes intermediate and protective layers, ensuring a high polyethylene content of 90% by mass, to enhance heat resistance and recyclability.

Benefits of technology

The laminate achieves excellent heat resistance, expanded heat sealing temperature range, improved productivity, and high recyclability, making it suitable for diverse packaging uses while maintaining strength and visibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563636000011
    Figure 0007563636000011
  • Figure 0007563636000012
    Figure 0007563636000012
  • Figure 0007563636000013
    Figure 0007563636000013
Patent Text Reader

Abstract

To provide a laminate that contains polyethylene and is suitable for recycling, the laminate having exceptional heat resistance and strength, and to provide a packaging body and a packaged article each including the laminate.SOLUTION: A laminate (10A1) comprises a base material layer (1), an adhesive layer (3), and a sealant layer (2) in the stated order. The base material layer (1) and the sealant layer (2) each contain polyethylene. The adhesive layer (3) contains a solvent-free adhesive. The degree of crystallization in the base material layer (1) is 40% or greater, the degree of crystallization being the ratio of the crystal peak area to the total peak area as measured within a diffraction angle range of 10-30° through a parallel beam technique in X-ray diffraction.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate, a package and a packaged article. [Background technology]

[0002] Packaging materials used for packaging bags and the like are required to have various properties depending on the application. Examples of required properties include heat resistance, transparency, heat sealability, strength, gas barrier properties, puncture resistance, visibility, suitability for bag making, suitability for printing, suitability for transportation, etc. In order to fully satisfy each of these various performance requirements, it has been common practice to use a combination of multiple types of synthetic resin films with different properties (see, for example, Patent Document 1).

[0003] In recent years, with the growing demand for the creation of a recycling-based society, packaging materials with high recyclability are in demand. In general, packaging materials are considered to have high recyclability when the ratio of the main resin contained therein is 90% by mass or more. However, as described above, conventional packaging materials are composed of different resin materials, and since it is difficult to separate the resin materials after use, they cannot be recycled as each material. Therefore, even if a package formed using conventional packaging materials is recovered, there is no other way than to burn it and recover and reuse it as heat, which is incompatible with the recent standpoint of global environmental protection.

[0004] From the viewpoint of recyclability, packaging materials with a high polyethylene content and technologies for making packaging films with as simple a layer structure as possible have been proposed (see, for example, Patent Documents 2 and 3). However, there are problems, such as the fact that they are limited to use in light packaging due to aspects such as strength and heat resistance, and there is room for improvement in order to satisfy various properties required according to the application as a packaging material. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 2009-241359 [Patent Document 2] Japanese Patent Publication No. 2020-196791 [Patent Document 3] Japanese Patent Application Publication No. 2020-55157 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a laminate containing polyethylene and having recyclability, which laminate has excellent heat resistance or strength, and a package and a packaged article containing the same. [Means for solving the problem]

[0007] According to one aspect of the present invention, there is provided a laminate comprising a base layer, an adhesive layer, and a sealant layer in this order, wherein the base layer and the sealant layer contain polyethylene, and the base layer has a crystallinity of 35% or more, which is the ratio of the crystalline peak area to the total peak area, measured by a parallel beam method of X-ray diffraction at a diffraction angle range of 10° to 30°.

[0008] According to another aspect of the present invention, there is provided a laminate according to the above aspect, further comprising an intermediate layer containing polyethylene and interposed between the base layer and the sealant layer.

[0009] According to yet another aspect of the present invention, there is provided a laminate according to the above aspect, wherein the intermediate layer has a crystallinity, which is the ratio of the crystalline peak area to the total peak area, of 35% or more, measured at a diffraction angle range of 10° to 30° by a parallel beam method of X-ray diffraction.

[0010] According to yet another aspect of the present invention, there is provided a laminate according to the above aspect, wherein the intermediate layer has a crystallinity, which is the ratio of the crystalline peak area to the total peak area, measured by a parallel beam method of X-ray diffraction in the diffraction angle range of 10° to 30°, of less than 35%.

[0011] According to yet another aspect of the present invention, there is provided a laminate according to any one of the above aspects, further comprising a protective layer as an outermost layer facing the sealant layer with the base layer sandwiched therebetween.

[0012] According to yet another aspect of the present invention, there is provided a laminate according to the above aspect, wherein the protective layer contains a thermosetting resin.

[0013] According to yet another aspect of the present invention, there is provided the laminate according to any one of the above aspects, wherein the base layer is a biaxially stretched film.

[0014] Alternatively, according to another aspect of the present invention, there is provided the laminate according to any one of the above aspects, wherein the base layer is a uniaxially stretched film.

[0015] According to yet another aspect of the present invention, there is provided a laminate according to any one of the above aspects, further comprising a gas barrier layer interposed between the base layer and the sealant layer.

[0016] According to yet another aspect of the present invention, there is provided the laminate according to any one of the above aspects, wherein the adhesive layer has gas barrier properties.

[0017] According to yet another aspect of the present invention, there is provided a laminate according to any of the above aspects, wherein the sealant layer is white.

[0018] According to yet another aspect of the present invention, there is provided a laminate according to any one of the above aspects, wherein the proportion of polyethylene in the laminate is 90 mass % or more.

[0019] According to yet another aspect of the present invention, there is provided a laminate relating to any of the above aspects, comprising a first adhesive layer and a second adhesive layer as the adhesive layer, the first adhesive layer being interposed between the base layer and the intermediate layer, and the second adhesive layer being interposed between the intermediate layer and the sealant layer.

[0020] According to yet another aspect of the present invention there is provided a package including a laminate according to any of the above aspects.

[0021] According to yet another aspect of the present invention, there is provided a package according to the above aspect which is a stand-up pouch.

[0022] According to yet another aspect of the present invention, there is provided a packaged article including a package according to any of the above aspects and contents contained therein. Effect of the Invention

[0023] According to the present invention, there is provided a laminate which contains polyethylene and has recyclability, and which has excellent heat resistance and strength, as well as a package and a packaged article which contain the same. [Brief description of the drawings]

[0024] [Figure 1] FIG. 1 is a cross-sectional view illustrating a laminate according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates a schematic diagram of a modified example of the laminate shown in FIG. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates a laminate according to a second embodiment of the present invention. [Figure 4] FIG. 4 is a cross-sectional view that illustrates a laminate according to a third embodiment of the present invention. [Diagram 5] FIG. 5 is a cross-sectional view that illustrates a laminate according to a fourth embodiment of the present invention. [Figure 6] FIG. 6 is a cross-sectional view that illustrates a laminate according to a fifth embodiment of the present invention. [Figure 7] FIG. 7 is a cross-sectional view that illustrates a laminate according to a sixth embodiment of the present invention. [Figure 8] FIG. 8 is a cross-sectional view that illustrates a laminate according to a seventh embodiment of the present invention. [Figure 9] FIG. 9 is a cross-sectional view that illustrates a laminate according to an eighth embodiment of the present invention. [Figure 10]FIG. 10 is a schematic diagram showing a packaging article according to a ninth embodiment of the present invention. [Figure 11] FIG. 11 is a schematic diagram showing a packaging article according to a tenth embodiment of the present invention. [Figure 12] FIG. 12 is a schematic diagram showing a packaging article according to an eleventh embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The embodiments described below are more specific embodiments of any of the above aspects. The following items can be incorporated into each of the above aspects alone or in combination.

[0026] The embodiments described below are merely examples of configurations for embodying the technical idea of ​​the present invention, and the technical idea of ​​the present invention is not limited by the materials, shapes, structures, etc. of the components described below. Various modifications can be made to the technical idea of ​​the present invention within the technical scope defined by the claims.

[0027] In addition, elements having the same or similar functions are given the same reference numerals in the drawings referred to below, and duplicated explanations are omitted. Therefore, matters mentioned in one embodiment can be applied to other embodiments unless otherwise specified. In addition, the drawings are schematic, and the relationship between dimensions in one direction and dimensions in another direction, the relationship between the dimensions of one member and the dimensions of another member, etc. may differ from the actual ones.

[0028] <1> First embodiment <1.1> Laminate FIG. 1 is a cross-sectional view illustrating a laminate according to a first embodiment of the present invention. The laminate 10A1 shown in FIG. 1 includes a base layer 1, a printed layer 4, an adhesive layer 3, and a sealant layer 2, in this order.

[0029] The base layer 1 and the sealant layer 2 contain polyethylene. The laminate 10A1 preferably has a polyethylene ratio of 90% by mass or more. Here, the ratio of polyethylene in the laminate means the ratio of the total amount of polyethylene to the total amount of resin material in each layer constituting the laminate. By making the ratio of polyethylene 90% by mass or more, high recyclability can be achieved.

[0030] <1.2> Base material layer The base layer 1 contains polyethylene. Preferably, the base layer 1 is made of polyethylene. The base layer 1 has a crystallinity of 35% or more, which is the ratio of the crystalline peak area to the total peak area, measured by a parallel beam method of X-ray diffraction in the diffraction angle range of 10° to 30°. Here, the crystallinity of the base layer 1 is a value obtained by the measurement method described below.

[0031] In the laminate 10A1 according to the present invention, the crystallinity of the base material layer 1 is 35% or more, which improves the heat resistance of the base material layer 1. As a result, even when the laminate 10A1 is used as a packaging material and processed into bags in a bag making machine, there is no need to reduce the bag making speed, and the laminate has excellent processability.

[0032] Furthermore, when the crystallinity of the base layer 1 is 35% or more, the base layer 1 is less prone to elongation, and the printability is improved.

[0033] The polyethylene contained in the base layer 1 may be a homopolymer of ethylene or a copolymer of ethylene and another monomer. When the polyethylene is a copolymer of ethylene and another monomer, the proportion of ethylene in the copolymer is, for example, 80 mol % or more.

[0034] The other monomer is, for example, an α-olefin. According to one example, the α-olefin has a carbon number in the range of 3 to 20. Such an α-olefin is, for example, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, 3-methyl-1-butene, 4-methyl-1-pentene, or 6-methyl-1-heptene.

[0035] The polyethylene may be a copolymer of ethylene and one of vinyl acetate and acrylic esters.

[0036] The substrate layer 1 is, for example, high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), or very low density polyethylene (VLDPE).

[0037] Here, high density polyethylene has a density of 0.942 g / cm 3 and medium density polyethylene has a density of 0.930 g / cm 3 More than 0.942g / cm 3 and low density polyethylene has a density of 0.910 g / cm 3 More than 0.930g / cm 3 Linear low density polyethylene has a density of 0.910 g / cm 3 More than 0.930cm 3 and ultra-low density polyethylene has a density of 0.910 g / cm 3 is less than. The density is a value obtained by a method in accordance with JIS K7112:1999.

[0038] The polyethylene contained in the base material layer 1 may be polyethylene derived from biomass. As the polyethylene derived from biomass, for example, Green Polyethylene (manufactured by Braskem) can be used.

[0039] Alternatively, the polyethylene contained in the base layer 1 may be polyethylene recycled by mechanical recycling. Here, mechanical recycling refers to decontaminating the polyethylene film by crushing collected polyethylene films and the like, cleaning the crushed films with an alkali to remove dirt and foreign matter on the film surface, and then drying the films at high temperature and reduced pressure to diffuse contaminants remaining inside the films. Alternatively, the polyethylene contained in the base layer 1 may be polyethylene recycled by chemical recycling.

[0040] The melting point of the base layer 1 is preferably within a range of 100° C. to 140° C., and more preferably within a range of 120° C. to 140° C. The melting point is a value obtained by a method in accordance with JIS K7121-1987.

[0041] The base layer 1 may be a non-stretched film or a stretched film. The base layer 1 is preferably a stretched film. When the base layer 1 is a stretched film in addition to having a crystallinity of 35% or more, the following effects are obtained. That is, the heat resistance and strength are particularly excellent. In addition, the elongation of the base layer 1 is reduced, improving the printability. In this specification, the term "film" does not include the concept of thickness.

[0042] When the base layer 1 is a stretched film, the base layer 1 may be a uniaxially stretched film or a biaxially stretched film. When a uniaxially stretched film is used as the base layer 1, the heat resistance during bag making, that is, the sealability described below, is further improved. When a biaxially stretched film is used as the base layer 1, the drop strength of a packaged article using the laminate 10A1 as a packaging material is improved.

[0043] Whether a stretched film is uniaxially or biaxially stretched can be determined by in-plane measurement using wide-angle X-ray diffraction, as described below. The X-ray diffraction pattern obtained by this measurement contains information about the degree of orientation of molecular chains present on the film surface.

[0044] When a polymer film is uniaxially stretched, a higher-order structure called a shish-kebab structure appears. The shish-kebab structure consists of a shish structure, which is an extended chain crystal, and a kebab structure, which is a lamellar crystal. In a uniaxially stretched film, this higher-order structure is arranged with a high degree of order, and therefore the X-ray diffraction pattern obtained by the above measurement of the uniaxially stretched film contains a sharp diffraction peak. That is, when the above measurement is performed on a uniaxially stretched film, a clear diffraction peak appears. Note that a "clear diffraction peak" means a diffraction peak with a half-width of less than 10°.

[0045] In contrast, in the manufacture of biaxially stretched films, the film is stretched in a specific direction, and then stretched in a direction perpendicular to the first direction. Therefore, although the first stretching creates the above-mentioned high-order structure, this high-order structure is disturbed by the second stretching. Therefore, when the above-mentioned measurements are performed on a biaxially stretched film, the diffraction peaks in the resulting X-ray diffraction pattern are broad. In other words, when the above-mentioned measurements are performed on a biaxially stretched film, no clear diffraction peaks appear.

[0046] As described above, the X-ray diffraction patterns obtained by the above-mentioned measurements are different between uniaxially stretched films and biaxially stretched films, and therefore it is possible to determine whether a stretched film is a uniaxially stretched film or a biaxially stretched film based on the X-ray diffraction patterns.

[0047] The film can be produced by a known production method such as a casting method or an inflation method. A multilayer polyethylene film obtained by co-extruding polyethylenes having different densities can also be used as the base layer 1. A stretched film can be obtained, for example, by stretching a film obtained by forming a polyethylene film by a T-die method or an inflation method. The base layer 1 may be a uniaxially stretched film or a biaxially stretched film.

[0048] The haze of the base layer 1 is preferably 20% or less, and more preferably 10% or less. The haze is a value obtained by a method in accordance with JIS K7136:2000.

[0049] The thickness of the base layer 1 is preferably in the range of 10 μm to 200 μm. The thickness of the base layer 1 is, for example, in the range of 10 μm to 50 μm, or in the range of 15 μm to 50 μm, or in the range of 12 μm to 35 μm. If the base layer 1 is too thin, the strength of the laminate 10A1 is likely to be reduced. Also, if the base layer 1 is too thick, the processability of the laminate 10A1 is likely to be reduced.

[0050] The substrate layer 1 is preferably surface-treated. This treatment can improve the adhesion between the substrate layer 1 and the layer adjacent to the substrate layer 1.

[0051] The method of the surface treatment is not particularly limited, and examples of the surface treatment include physical treatments such as corona discharge treatment, ozone treatment, low-temperature plasma treatment using oxygen gas and / or nitrogen gas, and glow discharge treatment, and chemical treatments such as oxidation treatment using chemicals.

[0052] The base layer 1 may further contain additives, such as crosslinking agents, antioxidants, antiblocking agents, slip agents, UV absorbers, light stabilizers, fillers, reinforcing agents, antistatic agents, pigments, and modifying resins.

[0053] The proportion of polyethylene in the base layer 1 is preferably 50% by mass or more, and more preferably 80% by mass or more. In one example, the base layer 1 is made of polyethylene. In another example, the base layer 1 is made of polyethylene and an additive.

[0054] The substrate layer 1 may be colored, for example, white.

[0055] As described above, the base layer 1 has a crystallinity of 35% or more. The printed layer 4 is disposed on the inner surface side of the base layer 1, and images such as patterns and characters displayed by the printed layer 4 can be seen with good visibility. From this viewpoint, the crystallinity of the base layer 1 is preferably 40% or more, and more preferably 50% or more. According to one example, the crystallinity is in the range of 50% to 75%. In addition, the polyethylene-containing layer having a crystallinity of 35% or more has excellent puncture strength, as described below. From this viewpoint, the crystallinity of the base layer 1 is preferably 40% or more, and more preferably 50% or more.

[0056] Polyethylene is a crystalline polymer, so it has both crystalline and amorphous parts. Polyethylene with a high degree of crystallinity has a high ratio of crystalline parts. This crystalline part controls the elastic part in the viscoelastic behavior of the resin, so a high degree of crystallinity improves the rigidity of the film.

[0057] Due to the influence of this viscoelastic behavior, in films with a high degree of crystallinity, the strain associated with the plastic deformation of the resin is also large. As a result, the effect of suppressing the deformation of the resin in response to the strain generated by the momentary impact applied to the film is obtained, making it difficult for breakage to occur. For this reason, the laminate 10A1 having the base material 1 containing polyethylene and having a crystallinity of 35% or more is excellent in resistance to momentary impact, and packaged articles using the laminate 10A1 as a packaging material are unlikely to be damaged (broken bag) by dropping. In other words, it has excellent resistance to breaking of the bag.

[0058] The crystallinity of the base layer 1 can be adjusted by controlling the degree of stretching of the polyethylene film used in the base layer 1, or the thermal history during or after the production of the film. For example, slow cooling after film formation increases the crystallinity, while rapid cooling decreases the crystallinity. It is also possible to improve the crystallinity by adding an additive such as a crystal nucleating agent.

[0059] <Method for measuring crystallinity> The crystallinity of the substrate layer 1 is measured by X-ray diffraction using a parallel beam method. An example of a method for measuring the crystallinity will be described below.

[0060] First, the X-ray diffraction pattern of the base layer 1 is obtained by out-of-plane measurement using a wide-angle X-ray diffractometer manufactured by Rigaku Corporation, scanning the diffraction angle range of 10° to 30° with 2θ / θ. The characteristic X-ray CuKα is used as the X-ray, and the X-ray is collimated by a multilayer mirror and made incident on the base layer 1. A scintillation detector equipped with a flat collimator is used as the light receiving unit.

[0061] From the obtained X-ray diffraction pattern, the peak area of ​​the crystalline component and the halo pattern area of ​​the amorphous component are determined, and the ratio of the peak area of ​​the crystalline component to the total area is calculated as the degree of crystallinity. When the base layer 1 has a plurality of layers, the crystallinity of one of the outermost surfaces of the base layer 1 is measured.

[0062] When the base layer 1 is a polyethylene film, scanning at a diffraction angle range of 10° to 30° reveals two sharp crystalline component peaks corresponding to the (110) and (200) planes, as well as a broad halo pattern of amorphous components. These are then analyzed separately to calculate the areas of the crystalline component peaks and the halo pattern of the amorphous components, and the degree of crystallinity can be calculated using the following formula (1).

[0063] Crystallinity = crystalline component peak area / (crystalline component peak area + amorphous component halo pattern area) ... (1) The focusing method is known as an X-ray diffraction method other than the parallel beam method, but in the case of samples with uneven surfaces such as resin films, the focusing method is prone to affecting the measurement results, such as peak broadening due to misalignment of the measurement surface. In contrast, in the case of parallel beam method, misalignment of the measurement surface has little effect on the measurement results, even in the case of samples with uneven surfaces.

[0064] On the other hand, the base layer 1 is preferably uniaxially or biaxially stretched, and as described above, the in-plane method using X-ray diffraction can be used to distinguish between them. In this in-plane method, the X-ray incidence angle θ and the angle 2θ at which the diffracted X-rays are detected by the detector are fixed to the angle θ and angle 2θ at which a diffraction peak corresponding to a specific crystal plane is detected in the out-of-plane method, for example, the diffraction peak corresponding to the (110) plane of a polyethylene film, respectively, and in this state, the film to be measured is scanned in the in-plane direction to obtain a diffraction pattern.

[0065] When in-plane measurements are performed on a uniaxially stretched film that has been uniaxially stretched in the machine direction (MD), a diffraction pattern can be obtained that has a sharp diffraction peak corresponding to the (110) plane at an angle 2θ of about ±90°, assuming that the MD direction is defined as 0°. On the other hand, in the case of a biaxially stretched film, the high-order structure obtained by uniaxial stretching is disturbed by the second stretching, and the anisotropy is reduced, so a diffraction pattern having a sharp diffraction peak corresponding to this (110) plane cannot be obtained. Therefore, in-plane measurements can be cited as one method for distinguishing uniaxially stretched films from biaxially stretched films.

[0066] <1.3> Sealant layer The sealant layer 2 faces the base layer 1. The sealant layer 2 contains polyethylene. Preferably, the sealant layer 2 is made of polyethylene. For example, the polyethylene contained in the base layer 1 may be any of those described above. The sealant layer 2 is preferably low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), or very high-density polyethylene (VLDPE), and more preferably linear low-density polyethylene.

[0067] From the viewpoint of environmental load, the polyethylene is preferably biomass-derived polyethylene or recycled polyethylene.

[0068] The sealant layer 2 may further contain the additives described above. The proportion of polyethylene in the sealant layer 2 is preferably 50% by mass or more, and more preferably 80% by mass or more. In one example, the sealant layer 2 is made of polyethylene. In another example, the sealant layer 2 is made of polyethylene and an additive.

[0069] The sealant layer 2 may be transparent or opaque. In the latter case, the sealant layer 2 is preferably white. When the laminate 10A1 having a transparent sealant layer 2 is used in a package, the contents are easily visible. When the laminate 10A1 having an opaque sealant layer 2 is used in a package, the contents do not interfere with the visibility of the image displayed by the printing layer 4. In particular, the white sealant layer 2 improves the visibility of the image displayed by the printing layer 4.

[0070] The thickness of the sealant layer 2 can be appropriately set in consideration of the shape of the packaging bag to be manufactured, the mass of the contents to be contained, and the like, and can be, for example, 30 to 150 μm.

[0071] The sealant layer 2 is, for example, an unstretched polyethylene resin film, or a layer formed by melt extrusion of polyethylene.

[0072] <1.4>Printing layer The printed layer 4 is provided on the surface of the base layer 1 facing the sealant layer 2, i.e., on the back surface of the base layer 1. The position at which the printed layer 4 is provided is not limited. That is, the printed layer 4 may be provided on the surface of the base layer 1, or may be provided at any position between the base layer 1 and the sealant layer 2. For example, when the laminate 10A1 further includes an intermediate layer described later, the printed layer 4 may be provided on any surface of the intermediate layer. The laminate 10A1 may also include multiple printed layers. The printed layer 4 may be omitted.

[0073] The printing ink used for the printing layer 4 is not particularly limited as long as it has adhesion to polyethylene. The printing layer 4 is composed of ink in which various additives such as pigments, extender pigments, plasticizers, drying agents, and stabilizers are added to ink binder resins that have been used conventionally, such as urethane-based, acrylic-based, nitrocellulose-based, rubber-based, and vinyl chloride-based inks. It is preferable to use ink derived from biomass as the printing ink. As the printing method, for example, well-known printing methods such as offset printing, gravure printing, flexographic printing, and silk screen printing, and well-known coating methods such as roll coating, knife edge coating, and gravure coating can be used. In addition, light-shielding inks can also be preferably used. For example, white, black, silver ink, sepia, etc. can be mentioned.

[0074] <1.5>Adhesive layer The adhesive layer 3 bonds the base material layer 1 provided with the print layer 4 to the sealant layer 2. The adhesive layer 3 includes at least one type of adhesive. The adhesive may be a one-component curing adhesive, a two-component curing adhesive, or a non-curing adhesive. The adhesive may be a solventless adhesive or a solvent-based adhesive.

[0075] Examples of the adhesive include epoxy adhesives such as polyether adhesives, polyester adhesives, silicone adhesives, and polyamine adhesives, urethane adhesives, rubber adhesives, vinyl adhesives, silicone adhesives, epoxy adhesives, phenol adhesives, and olefin adhesives. Adhesives containing biomass components can also be used. The adhesive is preferably a polyamine adhesive or a urethane adhesive having gas barrier properties. Specific examples of gas barrier adhesives include "Maxive" manufactured by Mitsubishi Gas Chemical Company, Inc. and "Paslim" manufactured by DIC Corporation.

[0076] The adhesive layer 3 may be a cured product of a resin composition containing a polyester polyol, an isocyanate compound, and a phosphoric acid-modified compound. Such an adhesive layer 3 can further improve the oxygen barrier property and water vapor barrier property of the laminate 10A1.

[0077] The thickness of the adhesive layer 3 is preferably in the range of 0.1 μm to 20 μm, more preferably in the range of 0.5 μm to 10 μm, and further preferably in the range of 1 to 5 μm.

[0078] The adhesive layer 3 can be formed by applying and drying on the sealant layer 2 using a conventional method such as a direct gravure roll coating method, a gravure roll coating method, a kiss coating method, a reverse roll coating method, a Fontaine method, or a transfer roll coating method.

[0079] <1.6> Effects The above-described laminate 10A1 has excellent heat resistance and recyclability, which will be described below.

[0080] The manufacture of packaging bags generally involves a process in which sealant layers of a laminate are brought into contact with each other, and the contacting portions are clamped with a jig and subjected to pressure and heat to thermally weld (heat seal) the contacting portions. The jig of the heat sealing machine is heated to a high temperature, and the surface of the base layer that directly contacts the jig is exposed to high temperatures. As a result, when polyethylene, which has poor heat resistance, is used for the base layer, problems such as the surface of the base layer being affected by heat and adhering to the jig may occur. For this reason, conventional laminates using polyethylene for the base layer have a narrow range of suitable bag-making temperatures, which has led to problems with poor productivity.

[0081] The present inventors measured the crystallinity of various polyethylenes and found that when the crystallinity of the base layer 1 is 35% or more, the base layer 1 exhibits excellent heat resistance, and therefore the laminate 10A1 also exhibits excellent heat resistance, and particularly, good heat sealability is achieved. The laminate 10A1 uses polyethylene, which is generally said to have poor heat resistance, as the base layer 1. However, by setting the crystallinity of the base layer 1 to 35% or more, the temperature range of heat sealing performed for bag making is expanded, and a package can be manufactured without causing a decrease in productivity or causing poor appearance due to shrinkage of the sealed portion.

[0082] The laminate 10A1, which has such excellent heat resistance, uses the crystallinity of the base layer 1 as an indicator, so the surface characteristics of the laminate 10A1 can be easily measured and understood, and its quality as a packaging material can be easily stabilized.

[0083] Furthermore, since the laminate 10A1 includes the base layer 1 and the seat heel layer, each of which is mainly composed of polyethylene, it is easy to make the proportion of polyethylene 90% by mass or more, and therefore the laminate 10A1 is also excellent in recyclability.

[0084] <1.7> Variations The laminate 10A1 can be modified in various ways. Fig. 2 is a cross-sectional view that shows a schematic diagram of a modified example of the laminate shown in Fig. 1. The laminate 10A2 shown in Fig. 2 is similar to the laminate 10A1, except that it further includes an inorganic compound layer 5 interposed between the base material layer 1 and the printed layer 4. The inorganic compound layer 5 is a thin film made of an inorganic compound, for example, an inorganic oxide such as aluminum oxide or silicon oxide, and functions as a gas barrier layer that suppresses the transmission of oxygen and water vapor.

[0085] <Inorganic compound layer> The inorganic compound layer 5 may be formed by coating, or may be formed by vapor deposition of an inorganic compound.

[0086] Examples of the inorganic compound contained in the inorganic compound layer 5 include metal oxides such as aluminum oxide, silicon oxide, magnesium oxide, and tin oxide. The inorganic compound layer 5 is preferably a vapor deposition film made of a metal oxide. From the viewpoint of transparency and barrier properties, the metal oxide may be selected from the group consisting of aluminum oxide, silicon oxide, and magnesium oxide. Furthermore, from the viewpoint of cost, the metal oxide is selected from aluminum oxide and silicon oxide. Furthermore, from the viewpoint of excellent tensile stretchability during processing, it is more preferable to use silicon oxide as the metal oxide. By making the inorganic compound layer 5 a vapor deposition film made of a metal oxide, high barrier properties can be obtained with a very thin layer within a range that does not affect the recyclability of the laminate 10A2.

[0087] A vapor-deposited film made of a metal oxide has the advantage of being transparent, and therefore less likely to cause a user holding a packaging material made of a laminate to mistakenly believe that a metal foil is used, compared to a vapor-deposited film made of a metal.

[0088] The thickness of the vapor-deposited film made of aluminum oxide is preferably 5 nm or more and 30 nm or less. When the thickness is 5 nm or more, sufficient gas barrier properties can be obtained. Furthermore, when the thickness is 30 nm or less, cracks caused by deformation due to internal stress of the thin film can be suppressed, and the deterioration of gas barrier properties can be suppressed. Note that, when the thickness exceeds 30 nm, the cost is likely to increase due to an increase in the amount of material used and a prolonged film formation time, and is therefore not preferable from an economical point of view. From the same viewpoint as above, the thickness of the vapor-deposited film made of aluminum oxide is more preferably 7 nm or more and 15 nm or less.

[0089] The thickness of the vapor-deposited film made of silicon oxide is preferably 10 nm or more and 50 nm or less. When the thickness is 10 nm or more, sufficient gas barrier properties can be obtained. Furthermore, when the thickness is 50 nm or less, the occurrence of cracks due to deformation caused by internal stress in the thin film can be suppressed, and the deterioration of gas barrier properties can be suppressed. Note that, when the thickness exceeds 50 nm, the cost is likely to increase due to an increase in the amount of material used and a prolonged film formation time, and is therefore not preferable from an economical point of view. From the same viewpoint as above, the thickness of the vapor-deposited film made of silicon oxide is more preferably 20 nm or more and 40 nm or less.

[0090] The inorganic compound layer 5 can be formed by, for example, vacuum film formation. In the vacuum film formation, physical vapor deposition or chemical vapor deposition can be used. Examples of physical vapor deposition include, but are not limited to, vacuum deposition, sputtering, and ion plating. Examples of chemical vapor deposition include, but are not limited to, thermal CVD (Chemical Vapor Deposition), plasma CVD, and photo CVD.

[0091] In the vacuum film formation, the resistance heating vacuum deposition method, the EB (Electron Beam) heating vacuum deposition method, the induction heating vacuum deposition method, the sputtering method, the reactive sputtering method, the dual magnetron sputtering method, the plasma enhanced chemical vapor deposition method (PECVD method), and the like are particularly preferably used. However, in terms of productivity, the vacuum deposition method is currently the most excellent. As the heating means for the vacuum deposition method, it is preferable to use any one of the electron beam heating method, the resistance heating method, and the induction heating method.

[0092] <Anchor coat layer> The laminate 10A2 may further include an anchor coat layer (not shown), as described in the second embodiment. The anchor coat layer can be formed on the surface of the base layer 1 on which the inorganic compound layer 5 is formed, using a known anchor coat agent. This can improve the adhesion of the inorganic compound layer 5 made of a metal oxide. Examples of the anchor coat agent include polyester polyurethane resin and polyether polyurethane resin. From the viewpoints of heat resistance and interlayer adhesive strength, the anchor coat agent is preferably a polyester polyurethane resin.

[0093] <Coating layer> Furthermore, as described in the second embodiment, the laminate 10A2 may further include a coating layer (not shown) between the inorganic compound layer 5 and the printing layer 4. The combination of the inorganic compound layer 5 and the coating layer may also function as a gas barrier layer. Hereinafter, the inorganic compound layer 5 may be referred to as a gas barrier layer, and the combination of the inorganic compound layer 5 and the coating layer may be referred to as a gas barrier layer.

[0094] The laminate 10A2 also has excellent heat resistance. In addition, since the inorganic compound layer 5 is substantially transparent, even if the inorganic compound layer 5 is provided between the base layer 1 and the printed layer 4, the image displayed by the printed layer 4 can be visually recognized from the front side. In addition, the laminate 10A2 also has excellent recyclability.

[0095] In order to impart light-shielding properties to the laminates 10A1 and 10A2, a metal vapor deposition layer may be provided between the base layer 1 and the sealant layer 2. When the laminate further includes an intermediate layer described below, a metal vapor deposition layer may be provided on either side of the intermediate layer. An example of the metal vapor deposition layer is an aluminum vapor deposition layer.

[0096] As already mentioned, the sealant layer 2 may be opaque, but the base layer 1 may also be opaque. For example, the base layer 1 may be white. When the laminate further includes an intermediate layer described later, the intermediate layer may be opaque. For example, the intermediate layer may be white.

[0097] <2> Second embodiment <2.1> Laminate FIG. 3 is a cross-sectional view that illustrates a laminate according to a second embodiment of the present invention. The laminate 10B shown in FIG. 3 includes a protective layer 6, a base material layer 1, a gas barrier layer 5, a printed layer 4, an adhesive layer 3, and a sealant layer 2, in this order. The gas barrier layer 5 included in the laminate 10B is composed of an inorganic compound layer, or an inorganic compound layer and a coating layer. The laminate 10B is similar to the laminate 10A1, except that it further includes a protective layer 6 provided on the surface of the base material layer 1, and a gas barrier layer 5 interposed between the base material layer 1 and the printed layer 4. The base material layer 1, the printed layer 4, the adhesive layer 3, and the sealant layer 2 included in the laminate 10B can be those described in the first embodiment.

[0098] <2.2>Protective layer The laminate 10B includes a protective layer 6 as the outermost layer. The protective layer 6 includes a thermosetting resin. The thermosetting resin is not particularly limited as long as it has heat resistance, and examples thereof include polyurethane resin, polyester resin, polyamide resin, polyamideimide resin, acrylic resin, epoxy resin, and water-soluble polymer. The protective layer 6 may include one type of thermosetting resin, or may include two or more types of thermosetting resin.

[0099] In one embodiment, the protective layer 6 preferably contains a water-soluble polymer, and is preferably an organic-inorganic composite layer that further contains an organometallic compound.

[0100] Examples of the water-soluble polymer include polyvinyl alcohols, polysaccharides such as starch, methyl cellulose, carboxymethyl cellulose, and hydroxyl-containing polymers such as acrylic polyols. In one embodiment, the protective layer 6 preferably contains a polyvinyl alcohol-based hydroxyl-containing polymer that may be contained in a coating layer as the gas barrier layer 5 described later.

[0101] The protective layer 6 preferably contains at least one of a metal alkoxide, a hydrolysate of a metal alkoxide, and a reaction product of a metal alkoxide or the hydrolysate thereof as an organometallic compound. Examples of the metal alkoxide include compounds represented by the general formula M(OR), such as tetraethoxysilane [Si(OC2H5)4] and triisopropoxyaluminum [Al(OC3H7)3]. n Examples of the above-mentioned are represented by the following formula:

[0102] Moreover, the protective layer 6 preferably further contains, as the organometallic compound, at least one of a silane coupling agent, a hydrolysate of a silane coupling agent, and a reaction product of a silane coupling agent or a hydrolysate of a silane coupling agent.

[0103] In one embodiment, the protective layer 6 can be formed using a coating liquid for forming a coating layer as the gas barrier layer 5 described later. When the laminate 10B includes an inorganic compound layer and a coating layer as the gas barrier layer 5, the protective layer 6 may be a layer formed using the same coating liquid as the coating liquid used to form the coating layer.

[0104] The protective layer 6 reduces thermal damage to the surface of the laminate during heat sealing. The laminate 10B has the protective layer 6, which has excellent heat resistance, as the outermost layer, and therefore ensures heat sealability and productivity even though the laminate 10B uses polyethylene resin, which has poor heat resistance, as a base material.

[0105] The thickness of the protective layer 6 is preferably within the range of 0.3 μm to 3 μm. If the protective layer 6 is too thin, it tends to be difficult to achieve high heat resistance. If the protective layer 6 is too thick, it tends to be difficult to sufficiently dry the cured resin film in the manufacturing process of the laminate 10B.

[0106] <2.3> Gas barrier layer The gas barrier layer 5 improves, for example, the oxygen barrier property and water vapor barrier property of the layered product 10B. The gas barrier layer 5 is composed of an inorganic compound layer, or an inorganic compound layer and a coating layer. When the gas barrier layer 5 is composed of an inorganic compound layer and a coating layer, it is preferable that the inorganic compound layer and the coating layer are laminated in this order from the substrate layer 1 side. The gas barrier layer 5 may be formed by coating, or may be formed by depositing an inorganic compound. The inorganic compound layer is the same as the inorganic compound layer described in the modified example of the first embodiment.

[0107] The coating layer can be formed, for example, by coating. In this case, a coating liquid containing a resin such as polyvinyl alcohol (PVA), ethylene-vinyl alcohol copolymer, ethylene-vinyl acetate copolymer, polyvinylidene chloride, polyacrylonitrile, and epoxy resin can be used. Additives such as organic or inorganic particles, layered compounds, and curing agents may be added to the coating liquid.

[0108] The coating layer may be, for example, an organic-inorganic composite layer containing at least one of a metal alkoxide, a hydrolysate of a metal alkoxide, and a reaction product of a metal alkoxide or a hydrolysate of a metal alkoxide, and a water-soluble polymer. This organic-inorganic composite layer may further contain at least one of a silane coupling agent, a hydrolysate of a silane coupling agent, and a reaction product of a silane coupling agent or a hydrolysate of a silane coupling agent.

[0109] Examples of metal alkoxides and hydrolysates thereof contained in the organic-inorganic composite layer include compounds represented by the general formula M(OR), such as tetraethoxysilane [Si(OC2H5)4] and triisopropoxyaluminum [Al(OC3H7)3]. n and hydrolysates thereof. One of these may be contained alone, or two or more of them may be contained in combination.

[0110] The total content of the metal alkoxide, its hydrolysate or their reaction products in the coating liquid used to form the organic-inorganic composite layer may be, for example, 40% by mass or more, 50% by mass or more, or 65% by mass or more from the viewpoint of oxygen barrier property. The total content of the metal alkoxide, its hydrolysate or their reaction products in the coating liquid may be, for example, 70% by mass or less.

[0111] The water-soluble polymer contained in the organic-inorganic composite layer is not particularly limited, and examples thereof include polyvinyl alcohol-based polymers, polysaccharides such as starch, methyl cellulose, and carboxymethyl cellulose, and hydroxyl-containing polymers such as acrylic polyol-based polymers. From the viewpoint of further improving the oxygen gas barrier property, the water-soluble polymer preferably contains a water-soluble polymer of polyvinyl alcohol-based polymer. The number-average molecular weight of the water-soluble polymer is, for example, 40,000 to 180,000.

[0112] The polyvinyl alcohol-based water-soluble polymer contained in the organic-inorganic composite layer can be obtained, for example, by saponifying (including partial saponification) polyvinyl acetate. This water-soluble polymer may have several tens of percent of acetate groups remaining, or may have only a few percent of acetate groups remaining.

[0113] The content of the water-soluble polymer in the coating liquid used to form the organic-inorganic composite layer may be, for example, 15% by mass or more, or 20% by mass or more, from the viewpoint of oxygen barrier property. Also, the content of the water-soluble polymer in the coating liquid may be, for example, 50% by mass or less, or 45% by mass or less, from the viewpoint of oxygen barrier property.

[0114] The silane coupling agent used in the organic-inorganic composite layer may be a silane coupling agent having an organic functional group. Such silane coupling agents may be ethyltrimethoxysilane, vinyltrimethoxysilane, γ-chloropropylmethyldimethoxysilane, γ-chloropropyltrimethoxysilane, glycidoxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldimethoxysilane, etc. The silane coupling agent selected from these, its hydrolyzate, and their reaction product may be used alone or in combination of two or more.

[0115] It is preferable to use a silane coupling agent having an epoxy group as an organic functional group. Examples of silane coupling agents having an epoxy group include γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. Silane coupling agents having an epoxy group may have an organic functional group other than the epoxy group, such as a vinyl group, an amino group, a methacryl group, or a ureyl group. The silane coupling agents selected from these, their hydrolyzates, and their reaction products may be used alone or in combination of two or more.

[0116] A silane coupling agent having an organic functional group, its hydrolysate or reaction product thereof can further improve the oxygen barrier property of the coating layer and the adhesion to the adjacent layer by the interaction between the organic functional group and the hydroxyl group of the water-soluble polymer. In particular, when the silane coupling agent, its hydrolysate or reaction product thereof has an epoxy group and the water-soluble polymer is polyvinyl alcohol (PVA), the oxygen barrier property and the adhesion to the adjacent layer can be further improved by the interaction between the epoxy group and the hydroxyl group of the PVA.

[0117] The total content of the silane coupling agent, its hydrolysate and their reaction products in the coating liquid used for forming the organic-inorganic composite layer may be, for example, 1% by mass or more, or 2% by mass or more, from the viewpoint of oxygen barrier property. Also, the total content of the silane coupling agent, its hydrolysate and their reaction products in the coating liquid may be, for example, 15% by mass or less, or 12% by mass or less, from the viewpoint of oxygen barrier property.

[0118] The thickness of the coating layer is preferably 50 nm to 1000 nm, more preferably 100 nm to 500 nm. When the thickness of the gas barrier coating layer is 50 nm or more, more sufficient gas barrier properties tend to be obtained, and when the thickness is 1000 nm or less, sufficient flexibility tends to be maintained.

[0119] The gas barrier layer 5 is preferably subjected to the above-mentioned surface treatment, which can improve the adhesion between the gas barrier layer 5 and the adjacent layers. The material for the gas barrier layer 5 may be a nanocomposite.

[0120] In the laminate 10B, the printed layer 4 is interposed between the gas barrier layer 5 and the adhesive layer 3, but may be provided at any position between the protective layer 6 and the sealant layer 2. Since the base layer 1 is transparent, for example, no matter where the printed layer 4 is located between the base layer 1 and the sealant layer 2, when the laminate 10B is observed from the protective layer 6 side, the pattern displayed by the printed layer 4 can be clearly seen.

[0121] <Anchor coat layer> The laminate 10B may further include an anchor coat layer (not shown) on the main surface of the base layer 1 that faces the gas barrier layer 5. This can improve the adhesion of the gas barrier layer 5. Examples of the anchor coat agent include polyester-based polyurethane resins and polyether-based polyurethane resins. From the viewpoints of heat resistance and interlayer adhesive strength, the anchor coat agent is preferably a polyester-based polyurethane resin.

[0122] The ratio of polyethylene in the laminate 10B is, for example, 90% by mass or more, which results in the laminate 10B being a highly recyclable mono-material.

[0123] <2.4> Effects Like the laminate 10A1, the laminate 10B includes a base layer 1 that contains polyethylene and has a crystallinity within the above range. Therefore, like the laminate 10A1, the laminate 10B has excellent heat resistance.

[0124] Moreover, the laminate 10B includes a protective layer 6 on the outermost layer. As described above, the protective layer 6 reduces thermal damage to the surface of the laminate during heat sealing. Therefore, the laminate 10B can achieve even better heat resistance, and in particular, better heat sealing suitability. Therefore, when the above-described configuration is adopted for the laminate 10B, the temperature range of the heat sealing performed for bag making is expanded, and it becomes even more difficult to cause a decrease in productivity or a defective appearance due to shrinkage of the sealed portion.

[0125] Furthermore, since the above-mentioned gas barrier layer 5, i.e., the inorganic compound layer and the coating layer, are substantially transparent, even if the gas barrier layer 5 is provided between the base layer 1 and the printing layer 4, the image displayed by the printing layer 4 can be viewed from the surface side. That is, the laminate 10B has excellent heat resistance and recyclability.

[0126] <3> Third embodiment <3.1> Laminate FIG. 4 is a cross-sectional view that illustrates a laminate according to a third embodiment of the present invention. The laminate 10C shown in FIG. 4 includes a protective layer 6, a base layer 1, an inorganic compound layer 5, a coating layer 7, a printed layer 4, an adhesive layer 3, and a sealant layer 2 in this order. The laminate 10C has a polyethylene ratio of 90% by mass or more. The laminate 10C has a layer structure similar to that of the laminate 10B according to the second embodiment described above, including an inorganic compound layer and a coating layer from the side of the base layer 1 as a gas barrier layer 5. The protective layer 6, base layer 1, inorganic compound layer 5, coating layer 7, printed layer 4, adhesive layer 3, and sealant layer 2 included in the laminate 10C can be those described in the second embodiment. In the laminate 10C, the inorganic compound layer 5, coating layer 7, and printed layer 4 can be omitted.

[0127] <Anchor coat layer> The laminate 10C may further include an anchor coat layer (not shown) on the main surface of the base layer 1 that faces the inorganic compound layer 5, similarly to the laminate 10B according to the second embodiment. This can improve the adhesion of the inorganic compound layer 5. Examples of the anchor coat agent include polyester polyurethane resin and polyether polyurethane resin. From the viewpoints of heat resistance and interlayer adhesive strength, the anchor coat agent is preferably a polyester polyurethane resin.

[0128] <3.3> Effects Since the laminate 10C has a similar layer structure to the laminate 10B, it exhibits the same effects as the laminate 10B.

[0129] <4> Fourth embodiment <4.1> Laminate FIG. 5 is a cross-sectional view that illustrates a laminate according to a fourth embodiment of the present invention. The laminate 10D shown in FIG. 5 includes a base layer 1, a first adhesive layer 3A, a gas barrier layer 5, an intermediate layer 8, a printed layer 4, a second adhesive layer 3B, and a sealant layer 2, in this order. The laminate 10D is similar to the laminate 10B, except for the following points. That is, the laminate 10D further includes an intermediate layer 8. The laminate 10D also includes a first adhesive layer 3A and a second adhesive layer 3B instead of the adhesive layer 3. The base layer 1, the printed layer 4, and the sealant layer 2 included in the laminate 10D can be those described in the first embodiment.

[0130] <4.2> Gas barrier layer The gas barrier layer 5 improves, for example, the oxygen barrier property and water vapor barrier property of the laminate 10D. The gas barrier layer 5 is, for example, a metal layer, an inorganic oxide layer, a resin-containing layer, or a combination of two or more thereof. When microwave heating using a microwave oven is assumed, the gas barrier layer 5 is preferably an inorganic oxide layer, a resin-containing layer, or a combination thereof.

[0131] The gas barrier layer 5 may be formed by coating, by melt molding, or by vapor deposition of an inorganic oxide. Alternatively, the gas barrier layer 5 may be a metal foil such as an aluminum foil, or may be vapor deposited with a metal such as aluminum.

[0132] As the inorganic oxide, for example, silicon oxide, boron oxide, or metal oxides such as aluminum oxide, magnesium oxide, calcium oxide, potassium oxide, tin oxide, sodium oxide, titanium oxide, lead oxide, zirconium oxide, and yttrium oxide can be used.

[0133] The resin-containing layer can be formed, for example, by coating. In this case, a coating liquid containing a resin such as polyvinyl alcohol (PVA), ethylene-vinyl alcohol copolymer, ethylene-vinyl acetate copolymer, polyvinylidene chloride, polyacrylonitrile, and epoxy resin can be used. Additives such as organic or inorganic particles, layered compounds, and curing agents may be added to the coating liquid.

[0134] When the resin-containing layer is formed by melt molding, for example, extrusion molding techniques such as T-die and inflation can be used. In melt molding, for example, the above-mentioned resin or a mixture of the above-mentioned resin and additives is heated and melted, and a film or sheet to be used as the gas barrier layer 5 is obtained by T-die or inflation. Then, this film or sheet is bonded to the intermediate layer 8.

[0135] The thickness of the gas barrier layer 5 is preferably within the range of 1 nm to 200 nm, for example, in the case of an inorganic oxide layer. If the thickness is 1 nm or more, excellent oxygen barrier properties and water vapor barrier properties are obtained. If the thickness is 200 nm or less, the manufacturing cost can be kept low, and cracks due to external forces such as bending and pulling are unlikely to occur, and deterioration of the barrier properties can be suppressed. Also, for example, if the layer is a resin-containing layer, the thickness is preferably within the range of 0.1 μm to 10 μm, and more preferably within the range of 0.2 μm to 5 μm. If the thickness is 0.2 μm or more, excellent oxygen barrier properties and water vapor barrier properties can be obtained. If the thickness is 10 μm or less, the manufacturing cost can be kept low.

[0136] The gas barrier layer 5 is preferably subjected to the above-mentioned surface treatment, which can improve the adhesion between the gas barrier layer 5 and the adjacent layers. The material for the gas barrier layer 5 may be a nanocomposite.

[0137] <4.3> Middle class The intermediate layer 8 contains polyethylene. As the polyethylene, for example, the polyethylene contained in the base layer 1 described above can be used.

[0138] The polyethylene contained in the intermediate layer 8 may be the same as or different from the polyethylene contained in the base layer 1. In addition, the intermediate layer 8 may further contain the additives described above.

[0139] The proportion of polyethylene in the intermediate layer 8 is preferably 50% by mass or more, and more preferably 80% by mass or more. In one example, the intermediate layer 8 is made of polyethylene. In another example, the intermediate layer 8 is made of polyethylene and an additive.

[0140] The intermediate layer 8 has a crystallinity of 35% or more. The intermediate layer 8 preferably has a crystallinity of 40% or more, and more preferably has a crystallinity of 50% or more. In one example, the crystallinity of the intermediate layer 8 is in the range of 50% to 75%.

[0141] The intermediate layer 8 having a crystallinity of 35% or more increases the strength of the laminate 10D, particularly its puncture strength. Therefore, the laminate 10D has excellent strength, particularly its puncture strength. A laminate with a high proportion of polyethylene is weaker than other laminates, and therefore has many opportunities to be folded when used as a packaging material. When the laminate is folded more frequently, the possibility of pinholes occurring increases, but the laminate 10D having excellent puncture strength is less likely to have pinholes. From this perspective, the intermediate layer 8 having a crystallinity of 35% or more is preferably a stretched film, and it is more preferable that both the base layer 1 and the intermediate layer 8 are stretched films. In this case, the stretched film constituting the intermediate layer 8 may be the same as the stretched film constituting the base layer 1, or may be different.

[0142] The melting point of the intermediate layer 8 is preferably in the range of 100°C to 140°C, and more preferably in the range of 120°C to 140°C.

[0143] The thickness of the intermediate layer 8 is preferably in the range of 10 μm to 200 μm, and more preferably in the range of 15 μm to 50 μm.

[0144] The intermediate layer 8 may be colored, for example white.

[0145] The intermediate layer 8 can be produced by a known production method such as a casting method or an inflation method. A multilayer polyethylene film obtained by co-extruding polyethylenes having different densities can also be used as the intermediate layer 8. A stretched film can be obtained, for example, by stretching a film obtained by forming a polyethylene film by a T-die method or an inflation method.

[0146] In this embodiment, an intermediate layer having a crystallinity of less than 35% may be used. By using an intermediate layer having a crystallinity of less than 35%, the strength of the laminate 10D, particularly the drop strength, can be improved. The intermediate layer having a crystallinity of less than 35% is preferably a non-stretched film.

[0147] <4.4>Adhesive layer The adhesives for forming the first adhesive layer 3A and the second adhesive layer 3B may be the same or different. The adhesives for forming the first adhesive layer 3A and the second adhesive layer 3B include at least one type of adhesive.

[0148] The adhesive may be a one-component curing adhesive, a two-component curing adhesive, or a non-curing adhesive. In addition, the adhesive may be a solventless adhesive or a solvent-based adhesive.

[0149] Examples of the adhesive include epoxy adhesives such as polyether adhesives, polyester adhesives, silicone adhesives, and polyamine adhesives, urethane adhesives, rubber adhesives, vinyl adhesives, silicone adhesives, epoxy adhesives, phenol adhesives, and olefin adhesives. Adhesives containing biomass components can also be used. The adhesive is preferably a polyamine adhesive or a urethane adhesive having gas barrier properties.

[0150] The first adhesive layer 3A and the second adhesive layer 3B may be a cured product of a resin composition containing a polyester polyol, an isocyanate compound, and a phosphoric acid-modified compound. Such a first adhesive layer 3A and a second adhesive layer 3B provide the laminate 10D with excellent oxygen barrier properties and water vapor barrier properties.

[0151] The thickness of the first adhesive layer 3A and the second adhesive layer 3B is preferably in the range of 0.1 μm to 20 μm, more preferably in the range of 0.5 μm to 10 μm, and even more preferably in the range of 1 to 5 μm.

[0152] The first adhesive layer 3A and the second adhesive layer 3B can be formed by applying and drying on the base material layer 1 using a conventionally known method such as, for example, a direct gravure roll coating method, a gravure roll coating method, a kiss coating method, a reverse roll coating method, a Fontaine method, or a transfer roll coating method.

[0153] In addition, in FIG. 5, the laminate 10D includes a gas barrier layer 5 between the first adhesive layer 3A and the intermediate layer 8, but the laminate 10D may also include a gas barrier layer 5 between the intermediate layer 8 and the second adhesive layer 3B.

[0154] 5, the printed layer 4 is provided between the intermediate layer 8 and the second adhesive layer 3B, but the printed layer 4 may be provided anywhere between the base layer 1 and the sealant layer 2. The printed layer 4 is preferably provided between the first adhesive layer 3A and the base layer 1. In this case, when the laminate 10B is observed from the base layer 1 side, the pattern displayed by the printed layer 4 is easily and clearly seen.

[0155] Furthermore, an anchor coat layer may be formed on the surface facing the first adhesive layer 3A, among the main surfaces of the base layer 1. Furthermore, the gas barrier layer 5 and the printed layer 4 may be omitted.

[0156] The ratio of polyethylene in the laminate 10D is, for example, 90% by mass or more, which makes the laminate 10D a highly recyclable mono-material.

[0157] <4.5> Effects The laminate 10D described above, like the laminate 10A1, includes a base layer 1 that contains polyethylene and has a crystallinity within the above range. Therefore, like the laminate 10A1, the laminate 10D has excellent heat resistance.

[0158] Moreover, the laminate 10D includes an intermediate layer 8 having a crystallinity within the above range. The intermediate layer 8 increases the strength, particularly the puncture strength, of the laminate 10D. Therefore, the laminate 10D is excellent in strength, particularly the puncture strength.

[0159] Moreover, in the laminate 10D, the base layer 1, the intermediate layer 8, and the sealant layer 2 all contain polyethylene, so that this laminate has excellent recyclability.

[0160] As described above, a laminate with a high proportion of polyethylene is weaker than other laminates, and therefore is frequently folded when used as a packaging material. Frequent folding increases the likelihood of pinholes occurring, but laminate 10D, which has excellent puncture strength, is less likely to develop pinholes.

[0161] Here, the "piercing strength" of the laminate 10D is a value obtained by piercing the laminate 10D from the base layer 1 side in a method specified in JIS Z1707:2019 "General Rules for Food Packaging Plastic Films". Specifically, a needle having a diameter of 1 mm and a semicircular tip is pierced from the base layer 1 side of the laminate 10D at a speed of 50 mm / min, and the maximum force until the needle penetrates is measured. This measurement is performed multiple times, and the arithmetic average of the maximum forces is obtained as the piercing strength.

[0162] <5> Fifth embodiment <5.1> Laminate FIG. 6 is a cross-sectional view that illustrates a laminate according to a fifth embodiment of the present invention. The laminate 10E shown in FIG. 6 includes a protective layer 6, a base material layer 1, a printed layer 4, a first adhesive layer 3A, an intermediate layer 8, a gas barrier layer 5, a second adhesive layer 3B, and a sealant layer 2 in this order. The laminate 10E is similar to the laminate 10D except for the following points. That is, the laminate 10E further includes a protective layer 6. In the laminate 10E, the inorganic compound layer 5 is interposed between the second adhesive layer 3B and the intermediate layer 8. In the laminate 10E, the printed layer 4 is interposed between the base material layer 1 and the first adhesive layer 3A. As the base material layer 1, the printed layer 4, the first adhesive layer 3A, the intermediate layer 8, the second adhesive layer 3B, and the sealant layer 2 included in the laminate 10E, those described in the fourth embodiment can be used.

[0163] <5.2>Protective layer The protective layer 6 includes a thermosetting resin. The thermosetting resin is not particularly limited as long as it has heat resistance, and examples thereof include polyurethane resin, polyester resin, polyamide resin, polyamideimide resin, acrylic resin, epoxy resin, and water-soluble polymer. The protective layer 6 may include one type of thermosetting resin, or may include two or more types of thermosetting resin.

[0164] In one embodiment, the protective layer 6 is preferably an organic-inorganic composite layer containing a water-soluble polymer and an organometallic compound.

[0165] Examples of the water-soluble polymer include polyvinyl alcohols, polysaccharides such as starch, methyl cellulose, carboxymethyl cellulose, and hydroxyl-containing polymers such as acrylic polyols. In one embodiment, the protective layer 6 preferably contains a polyvinyl alcohol-based hydroxyl-containing polymer that may be contained in a coating layer as the gas barrier layer 5 described later.

[0166] The protective layer 6 preferably contains at least one of a metal alkoxide, a hydrolysate of a metal alkoxide, and a reaction product of a metal alkoxide or the hydrolysate thereof as an organometallic compound. Examples of the metal alkoxide include compounds represented by the general formula M(OR), such as tetraethoxysilane [Si(OC2H5)4] and triisopropoxyaluminum [Al(OC3H7)3]. n Examples of the above-mentioned are represented by the following formula:

[0167] Moreover, the protective layer 6 preferably further contains, as the organometallic compound, at least one of a silane coupling agent, a hydrolysate of a silane coupling agent, and a reaction product of a silane coupling agent or a hydrolysate of a silane coupling agent.

[0168] In one embodiment, the protective layer 6 can be formed using a coating liquid for forming a coating layer as the gas barrier layer 5 described later. When the laminate 10E includes an inorganic compound layer and a coating layer as the gas barrier layer 5, the protective layer 6 may be a layer formed using the same coating liquid as the coating liquid used to form the coating layer.

[0169] The laminate 10E has the protective layer 6, which has excellent heat resistance, as the outermost layer, and therefore ensures heat sealability and productivity even though the laminate 10E uses polyethylene resin, which has poor heat resistance, as the base material.

[0170] The thickness of the protective layer 6 is preferably within the range of 0.3 μm to 3 μm. If the protective layer 6 is too thin, it tends to be difficult to achieve high heat resistance. If the protective layer 6 is too thick, it tends to be difficult to sufficiently dry the cured resin film in the manufacturing process of the laminate 10E.

[0171] <5.3> Gas barrier layer The gas barrier layer 5 improves, for example, the oxygen barrier property and water vapor barrier property of the layered product 10E. The gas barrier layer 5 is made of an inorganic compound layer or an inorganic compound layer and a coating layer. When the gas barrier layer 5 is made of an inorganic compound layer and a coating layer, the inorganic compound layer and the coating layer are preferably laminated in this order from the intermediate layer 8 side.

[0172] The gas barrier layer 5 may be formed by coating, or by vapor deposition of an inorganic compound.

[0173] Examples of the inorganic compound contained in the inorganic compound layer include metal oxides such as aluminum oxide, silicon oxide, magnesium oxide, and tin oxide. The inorganic compound layer is preferably, for example, a vapor deposition film made of a metal oxide. From the viewpoint of transparency and barrier properties, the metal oxide may be selected from the group consisting of aluminum oxide, silicon oxide, and magnesium oxide. Furthermore, from the viewpoint of cost, the metal oxide is selected from aluminum oxide and silicon oxide. Furthermore, from the viewpoint of excellent tensile stretchability during processing, it is more preferable to use silicon oxide as the metal oxide. By making the inorganic compound layer contained in the gas barrier layer 5 a vapor deposition film made of a metal oxide, high barrier properties can be obtained with a very thin layer within a range that does not affect the recyclability of the laminate 10E.

[0174] A vapor-deposited film made of a metal oxide has the advantage of being transparent, and therefore less likely to cause a user holding a packaging material made of a laminate to mistakenly believe that a metal foil is used, compared to a vapor-deposited film made of a metal.

[0175] The thickness of the vapor-deposited film made of aluminum oxide is preferably 5 nm or more and 30 nm or less. When the thickness is 5 nm or more, sufficient gas barrier properties can be obtained. Furthermore, when the thickness is 30 nm or less, cracks caused by deformation due to internal stress of the thin film can be suppressed, and the deterioration of gas barrier properties can be suppressed. Note that, when the thickness exceeds 30 nm, the cost is likely to increase due to an increase in the amount of material used and a prolonged film formation time, and is therefore not preferable from an economical point of view. From the same viewpoint as above, the thickness of the vapor-deposited film made of aluminum oxide is more preferably 7 nm or more and 15 nm or less.

[0176] The thickness of the vapor-deposited film made of silicon oxide is preferably 10 nm or more and 50 nm or less. When the thickness is 10 nm or more, sufficient gas barrier properties can be obtained. Furthermore, when the thickness is 50 nm or less, the occurrence of cracks due to deformation caused by internal stress in the thin film can be suppressed, and the deterioration of gas barrier properties can be suppressed. Note that, when the thickness exceeds 50 nm, the cost is likely to increase due to an increase in the amount of material used and a prolonged film formation time, and is therefore not preferable from an economical point of view. From the same viewpoint as above, the thickness of the vapor-deposited film made of silicon oxide is more preferably 20 nm or more and 40 nm or less.

[0177] The inorganic compound layer can be formed, for example, by vacuum film formation. In the vacuum film formation, physical vapor deposition or chemical vapor deposition can be used. Examples of physical vapor deposition include, but are not limited to, vacuum deposition, sputtering, and ion plating. Examples of chemical vapor deposition include, but are not limited to, thermal CVD (Chemical Vapor Deposition), plasma CVD, and photo CVD.

[0178] In the vacuum film formation, the resistance heating vacuum deposition method, the EB (Electron Beam) heating vacuum deposition method, the induction heating vacuum deposition method, the sputtering method, the reactive sputtering method, the dual magnetron sputtering method, the plasma enhanced chemical vapor deposition method (PECVD method), and the like are particularly preferably used. However, in terms of productivity, the vacuum deposition method is currently the most excellent. As the heating means for the vacuum deposition method, it is preferable to use any one of the electron beam heating method, the resistance heating method, and the induction heating method.

[0179] The coating layer can be formed, for example, by coating. In this case, a coating liquid containing a resin such as polyvinyl alcohol (PVA), ethylene-vinyl alcohol copolymer, ethylene-vinyl acetate copolymer, polyvinylidene chloride, polyacrylonitrile, and epoxy resin can be used. Additives such as organic or inorganic particles, layered compounds, and curing agents may be added to the coating liquid.

[0180] The coating layer may be, for example, an organic-inorganic composite layer containing at least one of a metal alkoxide, a hydrolysate of a metal alkoxide, and a reaction product of a metal alkoxide or a hydrolysate of a metal alkoxide, and a water-soluble polymer. This organic-inorganic composite layer may further contain at least one of a silane coupling agent, a hydrolysate of a silane coupling agent, and a reaction product of a silane coupling agent or a hydrolysate of a silane coupling agent.

[0181] Examples of metal alkoxides and hydrolysates thereof contained in the organic-inorganic composite layer include compounds represented by the general formula M(OR), such as tetraethoxysilane [Si(OC2H5)4] and triisopropoxyaluminum [Al(OC3H7)3]. n and hydrolysates thereof. One of these may be contained alone, or two or more of them may be contained in combination.

[0182] The total content of the metal alkoxide, its hydrolysate or their reaction products in the coating liquid used to form the organic-inorganic composite layer may be, for example, 40% by mass or more, 50% by mass or more, or 65% by mass or more from the viewpoint of oxygen barrier property. The total content of the metal alkoxide, its hydrolysate or their reaction products in the coating liquid may be, for example, 70% by mass or less.

[0183] The water-soluble polymer contained in the organic-inorganic composite layer is not particularly limited, and examples thereof include polyvinyl alcohol-based polymers, polysaccharides such as starch, methyl cellulose, and carboxymethyl cellulose, and hydroxyl-containing polymers such as acrylic polyol-based polymers. From the viewpoint of further improving the oxygen gas barrier property, the water-soluble polymer preferably contains a water-soluble polymer of polyvinyl alcohol-based polymer. The number-average molecular weight of the water-soluble polymer is, for example, 40,000 to 180,000.

[0184] The polyvinyl alcohol-based water-soluble polymer contained in the organic-inorganic composite layer can be obtained, for example, by saponifying (including partial saponification) polyvinyl acetate. This water-soluble polymer may have several tens of percent of acetate groups remaining, or may have only a few percent of acetate groups remaining.

[0185] The content of the water-soluble polymer in the coating liquid used to form the organic-inorganic composite layer may be, for example, 15% by mass or more, or 20% by mass or more, from the viewpoint of oxygen barrier property. Also, the content of the water-soluble polymer in the coating liquid may be, for example, 50% by mass or less, or 45% by mass or less, from the viewpoint of oxygen barrier property.

[0186] The silane coupling agent used in the organic-inorganic composite layer may be a silane coupling agent having an organic functional group. Such silane coupling agents may be ethyltrimethoxysilane, vinyltrimethoxysilane, γ-chloropropylmethyldimethoxysilane, γ-chloropropyltrimethoxysilane, glycidoxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldimethoxysilane, etc. The silane coupling agent selected from these, its hydrolyzate, and their reaction product may be used alone or in combination of two or more.

[0187] It is preferable to use a silane coupling agent having an epoxy group as an organic functional group. Examples of silane coupling agents having an epoxy group include γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. Silane coupling agents having an epoxy group may have an organic functional group other than the epoxy group, such as a vinyl group, an amino group, a methacryl group, or a ureyl group. The silane coupling agents selected from these, their hydrolyzates, and their reaction products may be used alone or in combination of two or more.

[0188] A silane coupling agent having an organic functional group, its hydrolysate or reaction product thereof can further improve the oxygen barrier property of the organic-inorganic composite layer and the adhesion to adjacent layers by the interaction between the organic functional group and the hydroxyl group of the water-soluble polymer. In particular, when the silane coupling agent, its hydrolysate or reaction product thereof has an epoxy group and the water-soluble polymer is polyvinyl alcohol (PVA), the oxygen barrier property and the adhesion to adjacent layers can be further improved by the interaction between the epoxy group and the hydroxyl group of the PVA.

[0189] The total content of the silane coupling agent, its hydrolysate and their reaction products in the coating liquid used for forming the organic-inorganic composite layer may be, for example, 1% by mass or more, or 2% by mass or more, from the viewpoint of oxygen barrier property. Also, the total content of the silane coupling agent, its hydrolysate and their reaction products in the coating liquid may be, for example, 15% by mass or less, or 12% by mass or less, from the viewpoint of oxygen barrier property.

[0190] The gas barrier layer 5 is preferably subjected to the above-mentioned surface treatment, which can improve the adhesion between the gas barrier layer 5 and the adjacent layers. The material for the gas barrier layer 5 may be a nanocomposite.

[0191] The thickness of the coating layer is preferably 50 nm to 1000 nm, more preferably 100 nm to 500 nm. When the thickness of the gas barrier coating layer is 50 nm or more, more sufficient gas barrier properties tend to be obtained, and when the thickness is 1000 nm or less, sufficient flexibility tends to be maintained.

[0192] <Anchor coat layer> The laminate 10E may further include an anchor coat layer (not shown) on the surface of the intermediate layer 8 on which the gas barrier layer 5 is formed. Alternatively, the laminate 10E may further include an anchor coat layer (not shown) on the main surface of the base layer 1 that faces the first adhesive layer 3A. The anchor coat layer can be formed using a known anchor coat agent. This can improve the adhesion of the inorganic compound layer made of metal oxide. Examples of the anchor coat agent include polyester polyurethane resin and polyether polyurethane resin. From the viewpoint of heat resistance and interlayer adhesive strength, the anchor coat agent is preferably a polyester polyurethane resin.

[0193] 6 includes the printed layer 4 between the base layer 1 and the first adhesive layer 3A, but the printed layer 4 may be included at any position between the protective layer 6 and the sealant layer 2. Since the base layer 1 and intermediate layer 8 included in the laminate 10E are transparent, the pattern displayed by the printed layer 4 can be clearly seen when the laminate 10E is observed from the protective layer 6 side, regardless of the position at which the printed layer 4 is included. According to one example, it is preferable that the printed layer 4 is included between the intermediate layer 8 and the protective layer 6, because the pattern displayed by the printed layer 4 can be more clearly seen.

[0194] In addition, in FIG. 6, the laminate 10E includes a gas barrier layer 5 on the side of the intermediate layer 8 facing the sealant layer 2, but the laminate 10E may also include a gas barrier layer 5 on the side of the intermediate layer 8 facing the base layer 1.

[0195] The ratio of polyethylene in the laminate 10E is, for example, 90% by mass or more, which makes the laminate 10E a highly recyclable mono-material.

[0196] <5.4> Effects Like the laminate 10A1, the laminate 10E described above includes a polyethylene-containing layer having a crystallinity within the above range as the base layer 1. Therefore, like the laminate 10A1, the laminate 10E has excellent heat resistance.

[0197] The laminate 10E also includes a protective layer 6. As described above, the protective layer 6 reduces thermal damage to the surface of the laminate during heat sealing. Therefore, the laminate 10E can achieve even better heat resistance, and in particular, better heat sealability. Therefore, when the above-described configuration is adopted for the laminate 10E, the temperature range of heat sealing performed for bag making is expanded, and a decrease in productivity is further prevented.

[0198] Moreover, the laminate 10E includes an intermediate layer 8 having a crystallinity within the above range. The intermediate layer 8 increases the strength, particularly the puncture strength, of the laminate 10E. Therefore, the laminate 10E is excellent in strength, particularly the puncture strength.

[0199] Moreover, since the base layer 1, the intermediate layer 8, and the sealant layer 2 of the laminate 10E all contain polyethylene, this laminate has excellent recyclability.

[0200] Furthermore, laminates with a high proportion of polyethylene are weaker than other laminates, and therefore are frequently folded when used as packaging materials. Frequent folding increases the likelihood of pinholes occurring, but laminate 10E, which has excellent puncture strength, is less likely to develop pinholes.

[0201] Furthermore, in the laminate 10E, since the base material layer 1 and the intermediate layer 8 are transparent, for example, no matter where the printed layer 4 is located between the base material layer 1 and the sealant layer 2, the pattern displayed by the printed layer 4 can be clearly seen when the printed layer 4 is observed from the protective layer 6 side. Furthermore, in a packaged article including the above-mentioned laminate 10E, the visibility of the contents is high.

[0202] <6> Sixth embodiment <6.1> Laminate FIG. 7 is a cross-sectional view that illustrates a laminate according to a sixth embodiment of the present invention. 7 includes a protective layer 6, a base layer 1, a printed layer 4, a first adhesive layer 3A, an intermediate layer 8, a gas barrier layer 5, a second adhesive layer 3B, and a sealant layer 2, in this order. The laminate 10F is similar to the laminate 10E, except that the crystallinity of the intermediate layer 8 is less than 35%. Among the layers included in the laminate 10F, the layers other than the intermediate layer 8, i.e., the protective layer 6, the base layer 1, the printed layer 4, the first adhesive layer 3A, the gas barrier layer 5, the second adhesive layer 3B, and the sealant layer 2, can be those described in the fifth embodiment.

[0203] <6.2> Middle class The intermediate layer 8 contains polyethylene. As the polyethylene, for example, the above-mentioned polyethylene contained in the base layer 1 can be used. The intermediate layer 8 is, for example, high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), or very low density polyethylene (VLDPE).

[0204] The polyethylene contained in the intermediate layer 8 may be the same as or different from the polyethylene contained in the base layer 1. In addition, the intermediate layer 8 may further contain the additives described above.

[0205] The proportion of polyethylene in the intermediate layer 8 is preferably 50% by mass or more, and more preferably 80% by mass or more. In one example, the intermediate layer 8 is made of polyethylene. In another example, the intermediate layer 8 is made of polyethylene and an additive.

[0206] The degree of crystallinity of the intermediate layer 8 is less than 35%. The degree of crystallinity of the intermediate layer 8 is preferably 30% or less. The degree of crystallinity of the intermediate layer 8 is preferably 15% or more.

[0207] The intermediate layer 8 having a crystallinity of less than 35% can increase the strength, particularly the drop strength, of the laminate 10F. A non-stretched film is preferable for such an intermediate layer 8. From the viewpoint of drop strength, it is preferable that the intermediate layer 8 is a non-stretched film having a crystallinity of less than 35%, and the base layer 1 is a stretched film having a crystallinity of 35% or more.

[0208] In this embodiment, an intermediate layer having a crystallinity of 35% or more may be used. When an intermediate layer having a crystallinity of 35% or more is used, the strength, particularly the puncture strength, of the laminate 10 can be improved. The intermediate layer having a crystallinity of 35% or more is preferably a stretched film.

[0209] The thickness of the intermediate layer 8 is preferably in the range of 10 μm to 200 μm, and more preferably in the range of 15 μm to 50 μm.

[0210] The intermediate layer 8 can be manufactured by known methods such as the casting method and inflation method described above, and it is also possible to use a multilayer polyethylene film as the base layer 1, in which polyethylenes of different densities are extruded by a coextrusion method.

[0211] <Anchor coat layer> The laminate 10F may further include an anchor coat layer (not shown) on the surface of the intermediate layer 8 on which the gas barrier layer 5 is formed. Alternatively, the laminate 10F may further include an anchor coat layer (not shown) on the surface facing the first adhesive layer 3A among the main surfaces of the base layer 1. As the anchor coat layer, the one described in the fifth embodiment can be used.

[0212] In addition, in FIG. 7, the laminate 10F includes a gas barrier layer 5 between the intermediate layer 8 and the second adhesive layer 3B, but the laminate 10F may also include a gas barrier layer 5 between the first adhesive layer 3A and the intermediate layer 8.

[0213] 7, the printed layer 4 is provided between the base layer 1 and the first adhesive layer 3A, but it is preferable that the printed layer 4 is provided between the protective layer 6 and the first adhesive layer 3A. In this case, when the laminate 10F is observed from the protective layer 6 side, the pattern displayed by the printed layer 4 is easily and clearly seen.

[0214] In addition, in the laminate 10F, the printed layer 4 and the gas barrier layer 5 may be omitted.

[0215] The ratio of polyethylene in the laminate 10F is, for example, 90% by mass or more, which makes the laminate 10F a highly recyclable mono-material.

[0216] <6.3> Effects In the above-described laminate 10F, the crystallinity of the base layer 1 is within the above range. Therefore, the laminate 10F has excellent heat resistance, similar to the laminate 10A1.

[0217] The laminate 10F also includes a protective layer 6. As described above, the protective layer 6 reduces thermal damage to the surface of the laminate during heat sealing. Therefore, the laminate 10F can achieve even better heat resistance, and in particular, better heat sealability. Therefore, when the above-described configuration is adopted for the laminate 10F, the temperature range of heat sealing performed for bag making is expanded, and a decrease in productivity is further prevented.

[0218] Moreover, the laminate 10F includes an intermediate layer 8 having a crystallinity within the above range. This intermediate layer 8 increases the strength, particularly the drop strength, of the laminate 10F. That is, in the laminate 10F, when used in a package, the intermediate layer 8 located on the inner side of the base layer 1 is softer than the base layer 1. This structure is suitable for absorbing the impact that occurs when a packaged article using the laminate 10F as a packaging material is dropped. Therefore, a packaged article using the laminate 10F as a packaging material is unlikely to be damaged (broken bag) by being dropped. Therefore, the laminate 10F has excellent strength, particularly the drop strength.

[0219] Moreover, the laminate 10F has excellent recyclability because the base layer 1, the intermediate layer 8, and the sealant layer 2 all contain polyethylene.

[0220] <7> Seventh embodiment <7.1> Laminate FIG. 8 is a cross-sectional view that illustrates a laminate according to a seventh embodiment of the present invention. The laminate 10G shown in FIG. 8 includes a protective layer 6, a base layer 1, a printed layer 4, a first adhesive layer 3A, an intermediate layer 8, an inorganic compound layer 5, a coating layer 7, a second adhesive layer 3B, and a sealant layer 2 in this order. The laminate 10G has a polyethylene ratio of 90% by mass or more. The laminate 10G is similar to the laminate 10E according to the fifth embodiment in which the gas barrier layer 5 includes an inorganic compound layer and a coating layer. The protective layer 6, the base layer 1, the printed layer 4, the first adhesive layer 3A, the intermediate layer 8, the inorganic compound layer 5, the coating layer 7, the second adhesive layer 3B, and the sealant layer 2 included in the laminate 10G can be those described in the fifth embodiment.

[0221] <7.2> Effects Like laminate 10A1, laminate 10G includes a polyethylene-containing layer having a crystallinity within the above range as base layer 1. Therefore, like laminate 10A1, laminate 10G has excellent heat resistance.

[0222] The laminate 10G also includes a protective layer 6. As described above, the protective layer 6 reduces thermal damage to the surface of the laminate during heat sealing. Therefore, the laminate 10G can achieve even better heat resistance, and in particular, better heat sealability. Therefore, when the above-described configuration is adopted for the laminate 10G, the temperature range of heat sealing performed for bag making is expanded, and a decrease in productivity is further prevented.

[0223] Moreover, the laminate 10G includes an intermediate layer 8 having a crystallinity within the above range. The intermediate layer 8 increases the strength, particularly the puncture strength, of the laminate 10G. Therefore, the laminate 10G is excellent in strength, particularly the puncture strength.

[0224] In the laminate 10G, the base layer 1, the intermediate layer 8, and the sealant layer 2 all contain polyethylene, and the proportion of polyethylene is 90% by mass or more.This laminate has excellent recyclability.

[0225] Furthermore, laminates with a high proportion of polyethylene are weaker than other laminates, and therefore are often folded when used as packaging materials. The more often the laminate is folded, the higher the possibility of pinholes occurring. However, laminate 10G, which has excellent puncture strength, is less likely to develop pinholes.

[0226] Furthermore, in the laminate 10G, since the base material layer 1 and the intermediate layer 8 are transparent, for example, no matter where the printed layer 4 is located between the base material layer 1 and the sealant layer 2, the pattern displayed by the printed layer 4 can be clearly seen when the printed layer 4 is observed from the protective layer 6 side. Furthermore, in a packaged article including the above-mentioned laminate 10G, the visibility of the contents is high.

[0227] <8> Eighth embodiment <8.1> Laminate FIG. 9 is a cross-sectional view that illustrates a laminate according to an eighth embodiment of the present invention. The laminate 10H shown in FIG. 9 includes a protective layer 6, a base layer 1, a printed layer 4, a first adhesive layer 3A, an intermediate layer 8, an inorganic compound layer 5, a coating layer 7, a second adhesive layer 3B, and a sealant layer 2 in this order. The laminate 10H has a polyethylene ratio of 90% by mass or more. The laminate 10H is similar to the laminate 10F according to the sixth embodiment in which the gas barrier layer 5 includes an inorganic compound layer and a coating layer. The protective layer 6, the base layer 1, the printed layer 4, the first adhesive layer 3A, the intermediate layer 8, the inorganic compound layer 5, the coating layer 7, the second adhesive layer 3B, and the sealant layer 2 included in the laminate 10H can be those described in the sixth embodiment.

[0228] <8.2> Effects In the laminate 10H, the crystallinity of the base layer 1 is within the above range. Therefore, the laminate 10H has excellent heat resistance, similar to the laminate 10A1.

[0229] Furthermore, the laminate 10H includes a protective layer 6. As described above, the protective layer 6 reduces thermal damage to the surface of the laminate during heat sealing. Therefore, the laminate 10H can achieve even better heat resistance, and in particular, better heat sealability. Thus, when the above-described configuration is adopted for the laminate 10H, the temperature range of heat sealing performed for bag making is expanded, and a decrease in productivity is further prevented.

[0230] Moreover, the laminate 10H includes an intermediate layer 8 having a crystallinity within the above range. This intermediate layer 8 increases the strength, particularly the drop strength, of the laminate 10H. That is, in the laminate 10H, when used in a package, the intermediate layer 8 located on the inner side of the base layer 1 is softer than the base layer 1. This structure is suitable for absorbing the impact that occurs when a packaged article using the laminate 10H as a packaging material is dropped. Therefore, a packaged article using the laminate 10H as a packaging material is unlikely to be damaged (broken bag) by being dropped. Therefore, the laminate 10H has excellent strength, particularly drop strength.

[0231] The laminate 10H has a polyethylene content of 90% by mass or more, and therefore has excellent recyclability.

[0232] The printing layer 4 may be provided on the surface of the base layer 1, on the surface of the intermediate layer 8, or on the back surface of the intermediate layer 8. In any case, the images such as patterns and characters displayed by the printing layer 4 can be viewed with good visibility. The printing layer 4 may be omitted.

[0233] <9> Ninth embodiment FIG. 10 is a schematic diagram showing a packaging article according to a ninth embodiment of the present invention.

[0234] Packaged article 100A shown in FIG. 10 includes package 110A and contents contained therein.

[0235] The package 110A is a flat pouch. The package 110A includes a pair of main films. Each of the main films is one of the laminates described in the first to eighth embodiments, or is cut out from the laminate. The main films are overlapped with their sealant layers facing each other, and the peripheral portions are heat-sealed to each other. The package 110A has a notch in the heat-sealed portion as an easy-open structure.

[0236] The contents may be any of liquids, solids, and mixtures thereof, and may be, for example, food or medicine.

[0237] <10> Tenth embodiment FIG. 11 is a schematic diagram showing a packaging article according to a tenth embodiment of the present invention.

[0238] The packaged article 100B shown in Fig. 11 includes a package 110B and contents contained therein. The contents are, for example, similar to those described for the packaged article 100A.

[0239] The package 110B is a standing pouch. The package 110B includes a pair of body and bottom films. Each of these films is one of the laminates described in the first to eighth embodiments or is cut from the laminate.

[0240] The pair of main films are overlapped with their sealant layers facing each other, and the peripheral portions are heat-sealed to each other except for one end and the area nearby. The bottom film is folded in half to form a mountain fold when viewed from the sealant layer side, and is sandwiched between the pair of main films at the position of the one end so that the mountain fold faces the other end of the main film. The bottom film is heat-sealed to the pair of main films except for its central portion. The outer surfaces of the bottom films are bonded to each other at both sides of the bottom of the package 110B.

[0241] The package 110B has a notch as an easy-open structure at a portion where the main film is heat-sealed. The easy-open structure may be provided so that an upper corner of the packaged article 100B can be used as a mouth when the packaged article 100B is opened. Alternatively, the packaged article 100B may further include a mouth member and a lid body described in the eleventh embodiment.

[0242] <11> Eleventh embodiment FIG. 12 is a schematic diagram showing a packaging article according to an eleventh embodiment of the present invention.

[0243] The packaged article 100C shown in Fig. 12 includes a package 110C and contents contained therein. The contents are, for example, similar to those described for the packaged article 100A.

[0244] The packaging body 110C is a gusset-type pouch and includes a container body 110C1, a mouth member 110C2, and a lid body 110C3.

[0245] The container body 110C1 includes a pair of body films and a pair of side films.

[0246] The pair of main body films are overlapped with their sealant layers facing each other and sandwiching a part of the mouth member 110C2 at one end. The peripheral portions of the main body films are heat-sealed to the mouth member 110C2 at the one end and are heat-sealed to each other in the vicinity of the one end. The peripheral portions of the main body films are also heat-sealed to each other at the opposite end except for the regions on both sides.

[0247] Each of the side films is folded in half so as to form a mountain fold when viewed from the sealant layer side. These side films are sandwiched between a pair of main films on both sides of the main films so that the mountain folds face each other. Each of the side films has a part of its peripheral edge heat-sealed to one of the main films, and the remaining part of the peripheral edge heat-sealed to the other main film. In addition, the outer surfaces of each of the side films are bonded to each other at the upper and lower positions of the package 110C. The container body 110C1 may further include a bottom film.

[0248] As described above, the mouth member 110C2 is sandwiched between the body films and includes a portion where they are heat sealed. The mouth member 110C2 further includes a mouth portion protruding outward from the container body 110C1. The mouth portion has a substantially cylindrical shape and is provided with a male screw on the outer surface of the side wall. The lid body 110C3 has a cylindrical shape with a bottom. The lid body 110C3 has a female screw on the inner surface of the side wall and is screwed into the mouth portion of the mouth member 110C2. EXAMPLES

[0249] The results of tests carried out in relation to the present invention are described below. (1) Test A (1.1) Manufacturing of Laminate (1.1.1) Example 1A The laminate 10A2 shown in FIG. 2 was produced by the following method. First, a polyethylene film having a thickness of 25 μm and a crystallinity of 58.5% was prepared as a base layer. The crystallinity shown in this example and the examples and comparative examples described below was measured by the above-mentioned measurement method.

[0250] Next, a silicon oxide (SiO x ) A vapor deposition film was formed. Then, a printing layer was formed on the inorganic compound layer.

[0251] Next, a dry lamination adhesive (urethane adhesive) was applied to the surface of the base layer on which the print layer was formed, and a linear low-density polyethylene resin (LLDPE) film (thickness 60 μm) was attached to the base layer as a sealant layer via this adhesive layer. In this manner, a laminate was produced.

[0252] (1.1.2) Example 2A A laminate 10A2 shown in FIG. 2 was produced in the same manner as in Example 1A, except that no inorganic compound layer was provided.

[0253] (1.1.3) Example 3A Laminate 10A2 shown in FIG. 2 was produced in the same manner as in Example 1A, except that a polyamine-based gas barrier adhesive was used as the adhesive instead of the dry lamination adhesive (urethane-based adhesive).

[0254] (1.1.4) Example 4A The laminate 10A2 shown in FIG. 2 was produced in the same manner as in Example 1A, except that a polyethylene film having a thickness of 25 μm and a crystallinity of 71.8% was used as the base layer instead of a polyethylene film having a thickness of 25 μm and a crystallinity of 58.5%.

[0255] (1.1.5) Example 5A The laminate 10A2 shown in FIG. 2 was produced in the same manner as in Example 1A, except that a polyethylene film having a thickness of 25 μm and a crystallinity of 55.9% was used as the base layer instead of a polyethylene film having a thickness of 25 μm and a crystallinity of 58.5%.

[0256] (1.1.6) Example 6A The laminate 10A2 shown in FIG. 2 was produced in the same manner as in Example 1A, except that a polyethylene film having a thickness of 20 μm and a crystallinity of 54.1% was used as the base layer instead of a polyethylene film having a thickness of 25 μm and a crystallinity of 58.5%.

[0257] (1.1.7) Example 7A The laminate 10A2 shown in FIG. 2 was produced in the same manner as in Example 1A, except that a polyethylene film having a thickness of 30 μm and a crystallinity of 55.9% was used as the base layer instead of a polyethylene film having a thickness of 25 μm and a crystallinity of 58.5%.

[0258] (1.1.8) Example 8A The laminate 10A2 shown in FIG. 2 was produced in the same manner as in Example 1A, except that a linear low-density polyethylene resin (LLDPE) film having a thickness of 40 μm was used as the sealant layer instead of the linear low-density polyethylene resin (LLDPE) film having a thickness of 60 μm.

[0259] (1.1.9) Example 9A The laminate 10A2 shown in FIG. 2 was produced in the same manner as in Example 1A, except that a linear low-density polyethylene resin (LLDPE) film having a thickness of 120 μm was used as the sealant layer instead of a linear low-density polyethylene resin (LLDPE) film having a thickness of 60 μm.

[0260] (1.1.10) Example 10A The laminate 10A2 shown in FIG. 2 was produced in the same manner as in Example 1A, except that no inorganic compound layer was provided, and a polyamine-based gas barrier adhesive was used as the adhesive instead of a dry lamination adhesive (urethane-based adhesive).

[0261] (1.1.11) Example 11A The laminate 10A2 shown in FIG. 2 was produced in the same manner as in Example 1A, except that no inorganic compound layer was provided, and a urethane-based gas barrier adhesive was used as the adhesive instead of a dry lamination adhesive (urethane-based adhesive).

[0262] (1.1.12) Comparative Example 1A A laminate was produced in the same manner as in Example 1A, except that a polyethylene film having a thickness of 32 μm and a crystallinity of 14.8% was used as the base layer instead of a polyethylene film having a thickness of 25 μm and a crystallinity of 58.5%.

[0263] (1.1.13) Comparative example 2A A laminate was produced in the same manner as in Example 1A, except that a polyethylene film having a thickness of 25 μm and a crystallinity of 20.6% was used as the base layer instead of a polyethylene film having a thickness of 25 μm and a crystallinity of 58.5%.

[0264] (1.2) Measurement and evaluation methods The substrate layer used in the production of the laminate was subjected to in-plane measurement by the wide-angle X-ray diffraction method described above, and it was examined whether the diffraction pattern obtained by this measurement had a sharp diffraction peak corresponding to the (110) plane.

[0265] Furthermore, the laminate was evaluated for sealing property, heat resistance, visibility, and gas barrier property. The evaluation methods for sealing property, heat resistance, visibility, and gas barrier property are described below.

[0266] (1.2.1) Sealing performance evaluation method A sample cut into a 10 cm square of the laminate was folded in half so that the sealant layer was on the inside, and heat-sealed using a heat seal tester. Specifically, first, the bottom seal temperature was set to 100°C, the top seal temperature was set to 120°C, and a pressure of 0.1 MPa was applied for 1 second. Then, the presence or absence of melting of the seal surface was confirmed, and the area of ​​the top surface of the folded sample where the heat seal bar was applied was observed. If the seal surface was not melted and the top surface of the sample was not melted, the bottom seal temperature was fixed at 100°C, and the top seal temperature was increased by 10°C at a time, and the same pressure and observation were performed as above, until at least one of the seal surface and the top surface of the sample was melted. Then, the sealability was evaluated according to the following criteria. A: There was no melting on the top surface of the sample, and there were no problems with the appearance. B: The upper surface of the sample was melted, and there was a problem with the appearance.

[0267] (1.2.2) Heat resistance evaluation method A sample cut into a 10 cm square of the laminate was folded in half so that the sealant layer was on the inside. Next, the lower seal temperature of the heat seal tester was set to 30°C, and the upper seal temperature was set to 170°C, and a pressure of 0.2 MPa was applied to the folded sample for 1 second. Then, the presence or absence of melting of the seal surface was confirmed, and the area of ​​the upper surface of the folded sample that was touched with the heat seal bar was observed to see if it was attached to the heat seal bar, and the heat resistance was evaluated according to the following criteria. A: The upper surface of the sample did not adhere to the heat seal bar. B: The top surface of the sample adhered to the heat seal bar.

[0268] (1.2.3) Visibility evaluation method The pattern displayed by the print layer was visually observed from the substrate layer side, and the visibility was evaluated according to the following criteria. A: The pattern displayed by the printing layer was clearly visible. B: The pattern displayed by the printing layer was blurred and unclear.

[0269] (1.2.4) Gas barrier property evaluation method The laminate was subjected to a boiling treatment, and then the oxygen transmission rate (OTR) was measured at 30°C and a relative humidity of 70%. This measurement was performed in accordance with JIS K-7126, Method B. The oxygen transmission rate was then evaluated for gas barrier properties with reference to the following criteria. A: OTR is 10cc / m 2 ·day·atm. B: OTR is 10cc / m 2 ·day·atm or more.

[0270] (1.3) Results The results of the above measurements and evaluations are summarized in Tables 1-1 and 1-2 below.

[0271] [Table 1-1]

[0272] [Table 1-2]

[0273] As shown in Tables 1-1 and 1-2, all of the laminates having a crystallinity of 35% or more in the base layer had good sealing properties, heat resistance, and visibility. In contrast, all of the laminates having a crystallinity of less than 35% in the base layer had insufficient sealing properties, heat resistance, and visibility.

[0274] (2) Test B (2.1) Manufacturing of Laminate (2.1.1) Example 1B The laminate 10B shown in Fig. 3 was produced by the following method. In this example, an anchor coat layer was further provided between the base layer 1 and the gas barrier layer 5, and an inorganic compound layer and a coating layer were provided as the gas barrier layer 5.

[0275] First, coating solutions for forming an anchor coating agent, a protective layer, and a covering layer were prepared by the following method: In this example, the protective layer and the covering layer were formed using the same coating solution.

[0276] (Preparation of anchor coating agent) Acrylic polyol and tolylene diisocyanate were mixed so that the number of NCO groups in tolylene diisocyanate was equal to the number of OH groups in the acrylic polyol, and diluted with ethyl acetate so that the total solid content (total amount of acrylic polyol and tolylene diisocyanate) was 5 mass%. β-(3,4-epoxycyclohexyl)trimethoxysilane was further added to the diluted mixture so that the amount was 5 mass parts per 100 mass parts of the total amount of acrylic polyol and tolylene diisocyanate, and these were mixed to prepare an anchor coating agent.

[0277] (Preparation of Coating Solution for Forming Protective Layer and Covering Layer) A coating liquid for forming a protective layer and a covering layer containing an organic / inorganic mixture (hereinafter, simply referred to as a "coating liquid") was prepared by mixing the following liquids A, B, and C in a mass ratio of 70 / 20 / 10, respectively. Liquid A: A hydrolysis solution with a solid content of 5 mass% (SiO2 equivalent) obtained by adding 72.1 g of 0.1N hydrochloric acid to 17.9 g of tetraethoxysilane (Si(OC2H5)4) and 10 g of methanol and stirring for 30 minutes. Liquid B: 5% by mass solution of polyvinyl alcohol in water / methanol (mass ratio of water:methanol is 95:5). Liquid C: A hydrolysis solution in which 1,3,5-tris(3-trialkoxysilylpropyl)isocyanurate was diluted with a mixture of water and isopropyl alcohol (water:isopropyl alcohol mass ratio 1:1) to a solid content of 5 mass%.

[0278] The substrate layer has a thickness of 25 μm, a crystallinity of 58.5%, a haze of 1.6%, and a density of 0.94 g / cm 3 The crystallinity shown in this example and the following examples and comparative examples was measured by the above-mentioned measuring method.

[0279] Next, one surface of the base layer was subjected to a corona treatment, and then the coating solution prepared above was applied to the corona-treated surface of the base layer by a gravure coating method and dried to form a protective layer made of an organic / inorganic mixture and having a thickness of 0.5 μm (in a dry state).

[0280] Next, the other surface of the base layer was subjected to a corona treatment. Subsequently, the above-mentioned anchor coating agent was applied to the corona-treated surface of the base layer by a gravure coating method to form an anchor coating layer having a thickness of 0.1 μm (in a dry state).

[0281] Next, an electron beam heating vacuum deposition apparatus was used to deposit silicon oxide (SiO x) A vapor-deposited film having a thickness of 40 nm was formed. Next, the coating solution prepared above was applied to the inorganic compound layer to form a coating layer consisting of an organic-inorganic mixture having a thickness of 0.3 μm (in a dry state).

[0282] Thereafter, a water-based flexographic ink was pattern-printed on the coating layer to form a print layer.

[0283] Next, a dry lamination adhesive (urethane adhesive) was applied to the surface of the base layer on which the print layer was formed, and a linear low-density polyethylene resin (LLDPE) film (thickness 60 μm) was attached to the base layer as a sealant layer via this adhesive layer. In this manner, a laminate was produced.

[0284] (2.1.2) Example 2B The laminate 10B shown in FIG. 3 was fabricated by using a polyethylene film having a crystallinity of 58.5% as a base layer, instead of the polyethylene film having a crystallinity of 55.9%, a haze of 5.9%, and a density of 0.95 g / cm. 3 The polyethylene film was biaxially stretched and was corona-treated on one side.

[0285] (2.1.3) Example 3B Laminate 10B shown in FIG. 3 was produced in the same manner as in Example 2B, except that no protective layer was provided.

[0286] (2.1.4) Example 4B Laminate 10B shown in FIG. 3 was produced in the same manner as in Example 1B, except that a protective layer having a thickness of 0.5 μm was formed from a urethane resin instead of forming a protective layer having a thickness of 0.5 μm by applying a polyamideimide resin.

[0287] (2.1.5) Example 5B Laminate 10B shown in FIG. 3 was produced in the same manner as in Example 1B, except that a protective layer having a thickness of 1 μm and made of a urethane resin was formed instead of forming a protective layer having a thickness of 0.5 μm by applying a polyamideimide resin.

[0288] (2.1.6) Example 6B Laminate 10B shown in FIG. 3 was produced in the same manner as in Example 1B, except that a protective layer having a thickness of 1 μm was formed from an ethylene-vinyl alcohol copolymer (EVOH) instead of forming a protective layer having a thickness of 0.5 μm by applying a polyamideimide resin.

[0289] (2.1.7) Example 7B Laminate 10B shown in FIG. 3 was produced in the same manner as in Example 1B, except that a protective layer made of acrylic resin and having a thickness of 1 μm was formed instead of forming a protective layer having a thickness of 0.5 μm by applying a polyamideimide resin.

[0290] (2.1.8) Comparative example 1B The laminate 10B shown in FIG. 3 was produced in the same manner as in Example 1B, except for the following: no protective layer was provided. Furthermore, instead of using the above-mentioned polyethylene film with a crystallinity of 58.5%, a laminate with a thickness of 25 μm, a crystallinity of 27.5%, a haze of 21.5%, and a density of 0.950 g / cm was used as the base layer. 3 The polyethylene film was corona-treated on one side.

[0291] (2.2) Measurement and Evaluation Methods The substrate layer used in the production of the laminate was subjected to in-plane measurement by the wide-angle X-ray diffraction method described above, and it was examined whether the diffraction pattern obtained by this measurement had a sharp diffraction peak corresponding to the (110) plane.

[0292] The laminate was also evaluated for sealing property, heat resistance, visibility and recyclability. The evaluation methods for sealing property, heat resistance, visibility and recyclability are described below.

[0293] (2.2.1) Sealing performance evaluation method A sample of the laminate cut into a 10 cm square was folded in half with the sealant layer on the inside, and heat-sealed using a heat seal tester. Specifically, a temperature of 140°C and a pressure of 0.1 MPa were applied to the folded sample for 1 second. The area of ​​the sample surface where the heat seal bar was applied was observed, and the sealability was evaluated according to the following criteria. A: There was no melting on the surface of the sample, and there were no problems with the appearance. B: The surface of the sample was melted, and there was a problem with the appearance.

[0294] (2.2.2) Heat resistance evaluation method A sample cut into a 10 cm square of the laminate was folded in half so that the sealant layer was on the inside. Next, the lower seal temperature of the heat seal tester was set to 30°C, and the upper seal temperature was set to 170°C, and a pressure of 0.2 MPa was applied to the folded sample for 1 second. Then, the presence or absence of melting of the seal surface was confirmed, and the area of ​​the upper surface of the folded sample that was touched with the heat seal bar was observed to see if it was attached to the heat seal bar, and the heat resistance was evaluated according to the following criteria. A: The upper surface of the sample did not adhere to the heat seal bar. B: The top surface of the sample adhered to the heat seal bar. For the laminates having a protective layer, the heat resistance was further evaluated in the same manner as above, except that the top seal temperature was set to 190°C.

[0295] (2.2.3) Visibility evaluation method Visibility was evaluated using the method described in (1.2.3).

[0296] (2.2.4) Recyclability assessment method The percentage of polyethylene in the total mass of the laminate was calculated. This percentage was used to evaluate the recyclability with reference to the following criteria. Here, evaluation A means that the recyclability is excellent as a monomaterial. A: The proportion of polyethylene was 90 mass % or more. B: The proportion of polyethylene was less than 90% by mass.

[0297] (2.3) Results The results of the above measurements and evaluations are summarized in Table 2 below.

[0298] [Table 2]

[0299] As shown in Table 2, all of the laminates in which the crystallinity of the base layer was 35% or more had good heat resistance and visibility while being suitable for recycling. The laminates in which the crystallinity of the base layer was 35% or more and had a protective layer also had excellent sealability. In contrast, the laminates in which the crystallinity of the base layer was less than 35% and did not have a protective layer had insufficient sealability, heat resistance, and visibility.

[0300] (3) Test C (3.1) Manufacturing of Laminate (3.1.1) Example 1C 4 was produced by the following method. In this example, an anchor coat layer was further provided between the base layer 1 and the inorganic compound layer 5.

[0301] First, an anchor coating agent and a coating liquid for forming a covering layer were prepared in the same manner as in Example 1 B. In addition, an organic solvent solution of a polyamideimide resin (non-volatile component concentration 5% by mass) was prepared as a coating liquid for forming a protective layer.

[0302] The substrate layer has a thickness of 25 μm, a crystallinity of 58.5%, a haze of 1.6%, and a density of 0.950 g / cm 3 A polyethylene film having the following properties was prepared. This polyethylene film was subjected to corona treatment on both sides. The crystallinity shown in this example and the following examples and comparative examples was measured by the above-mentioned measuring method.

[0303] Next, the coating solution containing the polyamideimide prepared above was applied by gravure coating onto one of the corona-treated surfaces of the base layer, and then dried to form a protective layer having a thickness of 0.5 μm.

[0304] Next, the above-mentioned anchor coating agent was applied to the other corona-treated surface of the base layer by gravure coating to form an anchor coating layer having a thickness of 0.1 μm (in a dry state).

[0305] Next, an electron beam heating vacuum deposition apparatus was used to deposit silicon oxide (SiO x ) was deposited to a thickness of 40 nm. The coating solution for forming a coating layer prepared above was then applied to the inorganic compound layer to form a coating layer of an organic-inorganic mixture having a thickness of 0.3 μm (in a dry state).

[0306] Thereafter, an image was formed on the coating layer by a flexographic printing method using a water-based flexographic ink, thereby forming a print layer.

[0307] Next, a dry lamination adhesive (urethane adhesive) was applied to the surface of the base layer on which the print layer was formed, and a linear low-density polyethylene resin (LLDPE) film (thickness 60 μm) was attached to the base layer as a sealant layer via this adhesive layer. In this manner, a laminate was produced.

[0308] (3.1.2) Example 2C Laminate 10C shown in FIG. 4 was produced in the same manner as in Example 1C, except that the thickness of the protective layer was changed from 0.5 μm to 1 μm, and further, no covering layer was provided.

[0309] (3.1.3) Example 3C A laminate 10C shown in FIG. 4 was produced in the same manner as in Example 1C, except that the thickness of the protective layer was changed from 0.5 μm to 3 μm.

[0310] (3.1.4) Example 4C A laminate 10C shown in FIG. 4 was produced in the same manner as in Example 1C, except that no protective layer was provided.

[0311] (3.1.5) Comparative example 1C Laminate 10C shown in FIG. 4 was produced in the same manner as in Example 1C, except for the following: no protective layer was provided. Furthermore, instead of using the above-mentioned polyethylene film with a crystallinity of 58.5%, a polyethylene film with a thickness of 25 μm, a crystallinity of 27.6%, and a haze of 21.5% was used as the base layer.

[0312] (3.2) Measurement and Evaluation Methods The substrate layer used in the production of the laminate was subjected to in-plane measurement by the wide-angle X-ray diffraction method described above, and it was examined whether the diffraction pattern obtained by this measurement had a sharp diffraction peak corresponding to the (110) plane.

[0313] The laminate was also evaluated for sealing property, heat resistance, visibility and recyclability. The evaluation methods for sealing property, heat resistance, visibility and recyclability are described below.

[0314] (3.2.1) Sealing performance evaluation method The sealing performance was evaluated by the method described in (1.2.1).

[0315] (3.2.2) Heat resistance evaluation method Heat resistance was evaluated by the method described in (2.2.2).

[0316] (3.2.3) Visibility Evaluation Method Visibility was evaluated using the method described in (1.2.3).

[0317] (3.2.3) Recyclability assessment method Recyclability was evaluated using the method described in (2.2.4).

[0318] (3.3) Results The results of the above measurements and evaluations are summarized in Table 3 below.

[0319] [Table 3]

[0320] As shown in Table 3, all of the laminates in which the crystallinity of the base layer was 35% or more had good heat resistance and visibility while being suitable for recycling. The laminates in which the crystallinity of the base layer was 35% or more and had a protective layer also had excellent sealability. In contrast, the laminates in which the crystallinity of the base layer was less than 35% and did not have a protective layer had insufficient sealability, heat resistance, and visibility.

[0321] (4) Test D (4.1) Manufacturing of Laminate (4.1.1) Example 1D The laminate 10D shown in FIG. 5 was produced by the following method. First, the substrate layer and the intermediate layer had a thickness of 25 μm, a crystallinity of 58.5%, a haze of 1.6%, and a density of 0.94 g / cm 3 The crystallinity shown in this example and the following examples and comparative examples was measured by the above-mentioned measuring method.

[0322] Next, on the intermediate layer, silicon oxide (SiO x ) A vapor-deposited film was formed to a thickness of 50 nm.

[0323] A dry lamination adhesive (urethane adhesive) was applied onto the base layer to form a first adhesive layer. The base layer and the intermediate layer were bonded together so that the base layer and the inorganic compound layer faced each other with the first adhesive layer sandwiched therebetween. Next, a print layer was formed on the reverse side of the surface of the intermediate layer on which the inorganic compound layer was formed.

[0324] Next, a linear low-density polyethylene resin (LLDPE) film (thickness 60 μm) was prepared as a sealant layer, and a dry lamination adhesive (urethane adhesive) was applied onto the sealant layer to form a second adhesive layer. The base layer and the sealant layer were bonded together with the second adhesive layer sandwiched between them so that the sealant layer and the print layer faced each other. In this manner, a laminate was produced. (4.1.2) Example 2D Laminate 10D shown in FIG. 5 was produced in the same manner as in Example 1D, except that a gas-barrier polyamine-based adhesive was used instead of a urethane-based adhesive as the adhesive for the first adhesive layer and the second adhesive layer.

[0325] (4.1.3) Example 3D The laminate 10D shown in FIG. 5 was fabricated by using a polyethylene film having a crystallinity of 71.8%, a haze of 4.1%, and a density of 0.95 g / cm3 as a base layer instead of the polyethylene film having a crystallinity of 58.5%. 3 The polyethylene film was produced in the same manner as in Example 1D, except that the polyethylene film was a longitudinal uniaxially stretched film, and one side of the film was subjected to a corona treatment.

[0326] (4.1.4) Example 4D Laminate 10D shown in FIG. 5 was produced in the same manner as in Example 1D, except for the following: instead of using the above-mentioned polyethylene film with a crystallinity of 58.5% as the substrate layer, a laminate with a thickness of 25 μm, a crystallinity of 55.9%, a haze of 5.9, and a density of 0.95 g / cm was used. 3 The polyethylene film was a biaxially stretched film, and was corona-treated on one side. Furthermore, instead of using the above-mentioned polyethylene film with a crystallinity of 58.5%, a polyethylene film with a thickness of 25 μm, a crystallinity of 71.8%, a haze of 4.1, and a density of 0.95 g / cm was used as the intermediate layer. 3The polyethylene film was a uniaxially oriented film, and one side of the film was subjected to a corona treatment.

[0327] (4.1.5) Example 5D The laminate 10D shown in FIG. 5 was fabricated using a polyethylene film having a thickness of 25 μm, a crystallinity of 14.8%, a haze of 21.5%, and a density of 0.950 g / cm 3 instead of the above-mentioned polyethylene film having a crystallinity of 58.5% as the intermediate layer. 3 The method of Example 1D was repeated, except that a polyethylene film having a thickness of 100 nm and a thickness of 100 nm was used. The polyethylene film was corona-treated on one side.

[0328] (4.1.6) Example 6D A laminate 10D shown in FIG. 5 was produced in the same manner as in Example 1D, except that no gas barrier layer was provided.

[0329] (4.1.7) Comparative Example 1D The laminate 10D shown in FIG. 5 was fabricated by using a polyethylene film having a crystallinity of 58.5% as a base layer, instead of the polyethylene film having a thickness of 25 μm, a crystallinity of 14.8%, a haze of 21.5%, and a density of 0.950 g / cm. 3 The method of Example 1D was repeated, except that a polyethylene film having a thickness of 100 nm and a thickness of 100 nm was used. The polyethylene film was corona-treated on one side.

[0330] (4.1.8) Comparative example 2D The laminate 10D shown in FIG. 5 was fabricated using a polyethylene film having a thickness of 25 μm, a crystallinity of 14.8%, a haze of 21.5%, and a density of 0.950 g / cm instead of the above-mentioned polyethylene film having a crystallinity of 58.5% as the base layer and intermediate layer. 3 The method of Example 1D was repeated, except that a polyethylene film having a thickness of 100 nm and a thickness of 100 nm was used. The polyethylene film was corona-treated on one side.

[0331] (4.1.9) Comparative example 3D Laminate 10D shown in FIG. 5 was produced in the same manner as in Example 1D, except for the following: instead of using the above-mentioned polyethylene film with a crystallinity of 58.5% as the substrate layer, a laminate with a thickness of 25 μm, a crystallinity of 14.8%, a haze of 21.5%, and a density of 0.950 g / cm was used. 3 The polyethylene film was subjected to a corona treatment on one side, and no gas barrier layer was provided.

[0332] (4.2) Measurement and Evaluation Methods The substrate layer and intermediate layer used in the production of the laminate were subjected to in-plane measurement by the wide-angle X-ray diffraction method described above. Then, it was examined whether the diffraction pattern obtained by this measurement had a sharp diffraction peak corresponding to the (110) plane.

[0333] The laminate was also evaluated for sealing property, heat resistance, visibility, puncture strength and gas barrier property. The evaluation methods for sealing property, heat resistance, visibility, puncture strength and gas barrier property are described below.

[0334] (4.2.1) Sealing performance evaluation method The sealing performance was evaluated by the method described in (2.2.1).

[0335] (4.2.2) Heat resistance evaluation method Heat resistance was evaluated by the method explained in (1.2.2).

[0336] (4.2.3) Visibility Evaluation Method Visibility was evaluated using the method described in (1.2.3).

[0337] (4.2.4) Evaluation method for puncture strength A needle with a radius of 0.5 mm and a hemispherical tip is pressed against the laminate from the base layer side at a speed of 50 mm / min, and the maximum force until the needle penetrates is measured. This measurement was performed multiple times, and the arithmetic average of the maximum forces was obtained as the penetration strength.

[0338] (4.2.5) Gas barrier property evaluation method The gas barrier properties were evaluated by the method explained in (1.2.4).

[0339] (4.3) Results The results of the above measurements and evaluations are summarized in Tables 4-1 and 4-2 below.

[0340] [Table 4-1]

[0341] [Table 4-2]

[0342] As shown in Tables 4-1 and 4-2, all of the laminates in which the crystallinity of the base layer was 35% or more had good sealing properties and heat resistance. In addition, the laminates in which the crystallinity of the base layer and intermediate layer was 35% or more also had excellent visibility and puncture strength. In contrast, the laminates in which the crystallinity of the base layer was less than 35% had insufficient sealing properties, heat resistance, and visibility.

[0343] (5) Test E (5.1) Manufacturing of Laminate (5.1.1) Example 1E 6 was produced by the following method. In this example, an anchor coat layer was further provided between the intermediate layer 8 and the gas barrier layer 5, and an inorganic compound layer and a coating layer were provided as the gas barrier layer 5.

[0344] First, an anchor coating agent, a coating liquid for forming a covering layer, and a coating liquid for forming a protective layer were prepared in the same manner as in Example 1B. In this example, the protective layer and the covering layer were formed using the same coating liquid as in Example 1B.

[0345] The substrate layer and the intermediate layer have a thickness of 25 μm, a crystallinity of 58.5%, a haze of 1.6%, and a density of 0.94 g / cm3 The crystallinity shown in this example and the following examples and comparative examples was measured by the above-mentioned measuring method.

[0346] Next, one surface of the base layer was subjected to a corona treatment, and then the above-prepared protective layer forming coating solution was applied to the corona-treated surface of the base layer by a gravure coating method and dried to form a protective layer of an organic / inorganic mixture having a thickness of 0.5 μm.

[0347] Next, the other surface of the base layer was subjected to a corona treatment. Next, a water-based flexographic ink was pattern-printed on the corona-treated surface of the base layer to form a print layer.

[0348] One surface of the intermediate layer was subjected to a corona treatment. Then, the above-mentioned anchor coating agent was applied to the corona-treated surface of the intermediate layer by gravure coating to form an anchor coating layer having a thickness of 0.1 μm (in a dry state).

[0349] Next, an electron beam heating vacuum deposition apparatus was used to deposit silicon oxide (SiO x ) was formed on the anchor coat layer to a thickness of 40 nm. Next, the coating solution for forming a coating layer prepared above was applied to the inorganic compound layer to form a coating layer of an organic-inorganic mixture having a thickness of 0.3 μm (in a dry state).

[0350] Next, a dry lamination adhesive (urethane adhesive) was applied to the surface of the intermediate layer opposite to the surface on which the inorganic compound layer was formed to form a first adhesive layer. The base layer and the intermediate layer were bonded together so that the printed layer and the intermediate layer faced each other with the first adhesive layer sandwiched therebetween.

[0351] Next, a linear low-density polyethylene resin (LLDPE) film (thickness 60 μm) was prepared as a sealant layer. A dry lamination adhesive (urethane adhesive) was applied onto the sealant layer to form a second adhesive layer. The base layer and the sealant layer were bonded together with the second adhesive layer sandwiched between them so that the sealant layer and the coating layer faced each other. In this manner, a laminate was produced.

[0352] (5.1.2) Example 2E Laminate 10E shown in Fig. 6 was produced in the same manner as in Example 1E, except for the following: instead of using the above-mentioned polyethylene film with a crystallinity of 58.5% as the base layer and intermediate layer, a laminate with a thickness of 25 µm, a crystallinity of 55.9%, a haze of 5.9%, and a density of 0.95 g / cm3 was used. 3 The polyethylene film used was one side of which was corona-treated.

[0353] (5.1.3) Example 3E A laminate 10E shown in FIG. 6 was produced in the same manner as in Example 2E, except for the following: no protective layer was provided. Furthermore, instead of using the above-mentioned polyethylene film with a crystallinity of 55.9% as the intermediate layer, a laminate having a thickness of 25 μm, a crystallinity of 27.5%, a haze of 21.5%, and a density of 0.950 g / cm3 was used. 3 The polyethylene film used was one side of which was corona-treated.

[0354] (5.1.4) Comparative Example 1E A laminate 10E shown in FIG. 6 was produced in the same manner as in Example 1E, except for the following: no protective layer was provided. Furthermore, instead of using the above-mentioned polyethylene film with a crystallinity of 58.5% as the base layer and intermediate layer, a laminate 10E having a thickness of 25 μm, a crystallinity of 27.5%, a haze of 21.5%, and a density of 0.950 g / cm3 was used. 3 The polyethylene film used was one side of which was corona-treated.

[0355] (5.2) Measurement and Evaluation Methods The substrate layer and intermediate layer used in the production of the laminate were subjected to in-plane measurement by the wide-angle X-ray diffraction method described above. Then, it was examined whether the diffraction pattern obtained by this measurement had a sharp diffraction peak corresponding to the (110) plane.

[0356] The laminate was also evaluated for sealing property, heat resistance, visibility, puncture strength, and recyclability. The evaluation methods for sealing property, heat resistance, visibility, puncture strength, and recyclability are described below.

[0357] (5.2.1) Sealing performance evaluation method The sealing property (heat resistance) was evaluated by the method explained in (2.2.1).

[0358] (5.2.2) Heat resistance evaluation method Heat resistance was evaluated by the method described in (2.2.2).

[0359] (5.2.3) Visibility Evaluation Method Visibility was evaluated using the method described in (1.2.3).

[0360] (5.2.4) Evaluation method for puncture strength The puncture strength was evaluated by the method described in (4.2.4).

[0361] (5.2.5) Recyclability assessment method Recyclability was evaluated using the method described in (2.2.4).

[0362] (5.3) Results The results of the above measurements and evaluations are summarized in Table 5 below.

[0363] [Table 5]

[0364] As shown in Table 5, all of the laminates in which the crystallinity of the base layer was 35% or more were good in heat resistance, visibility, and puncture strength. Furthermore, the laminates in which the crystallinity of the base layer and intermediate layer was 35% or more and which were provided with a protective layer also had excellent sealing properties and further improved puncture strength. In contrast, the laminates in which the crystallinity of the base layer was less than 35% and which were not provided with a protective layer were insufficient in sealing properties, heat resistance, visibility, and puncture strength.

[0365] (6) Test F (6.1) Manufacturing of Laminates (6.1.1) Example 1F 7 was produced by the following method. In this example, an anchor coat layer was further provided between the intermediate layer 8 and the gas barrier layer 5, and an inorganic compound layer and a coating layer were provided as the gas barrier layer 5.

[0366] First, an anchor coating agent, a coating liquid for forming a covering layer, and a coating liquid for forming a protective layer were prepared in the same manner as in Example 1B. In this example, the protective layer and the covering layer were formed using the same coating liquid as in Example 1B.

[0367] The substrate layer has a thickness of 25 μm, a crystallinity of 58.5%, and a density of 0.950 g / cm 3 A polyethylene film having the following composition was prepared. One side of the polyethylene film was subjected to a corona treatment. The crystallinity shown in this example and the following examples and comparative examples was measured by the above-mentioned measuring method.

[0368] Next, one surface of the base layer was subjected to a corona treatment, and then the above-prepared protective layer forming coating solution was applied to the corona-treated surface of the base layer by a gravure coating method and dried to form a protective layer of an organic / inorganic mixture having a thickness of 0.5 μm.

[0369] Next, the other surface of the base layer was subjected to a corona treatment. Next, a water-based flexographic ink was pattern-printed on the corona-treated surface of the base layer to form a print layer.

[0370] Next, as the intermediate layer, a thickness of 25 μm, a crystallinity of 27.5%, and a density of 0.950 g / cm 3 A polyethylene film having the following characteristics was prepared. One side of this polyethylene film was subjected to a corona treatment.

[0371] The above-mentioned anchor coating agent was applied by gravure coating to form an anchor coating layer having a thickness of 0.1 μm (in a dry state).

[0372] Next, as an inorganic compound layer, silicon oxide (SiO x ) was formed on the anchor coat layer to a thickness of 40 nm. Next, the coating solution for forming a coating layer prepared above was applied to the inorganic compound layer to form a coating layer of an organic-inorganic mixture having a thickness of 0.3 μm (in a dry state).

[0373] Next, a dry lamination adhesive (urethane adhesive) was applied to the surface of the intermediate layer opposite to the surface on which the inorganic compound layer was formed to form a first adhesive layer. The base layer and the intermediate layer were bonded together so that the printed layer and the intermediate layer faced each other with the first adhesive layer sandwiched therebetween.

[0374] Next, a linear low-density polyethylene resin (LLDPE) film (thickness 60 μm) was prepared as a sealant layer. A dry lamination adhesive (urethane adhesive) was applied onto the sealant layer to form a second adhesive layer. The base layer and the sealant layer were bonded together with the second adhesive layer sandwiched between them so that the sealant layer and the coating layer faced each other. In this manner, a laminate was produced.

[0375] (6.1.2) Example 2F Laminate 10F shown in Fig. 7 was produced in the same manner as in Example 1F, except for the following: instead of using the above-mentioned polyethylene film with a crystallinity of 58.5% as the base layer, a laminate having a thickness of 25 µm, a crystallinity of 55.9%, a haze of 21.5%, and a density of 0.95 g / cm3 was used. 3The polyethylene film used was one side of which was corona-treated.

[0376] (6.1.3) Example 3F Laminate 10F shown in FIG. 7 was produced in the same manner as in Example 1F, except for the following: no protective layer was provided. Furthermore, instead of using the above-mentioned polyethylene film having a crystallinity of 58.5% as the base layer and the above-mentioned polyethylene film having a crystallinity of 27.5% as the intermediate layer, a laminate having a thickness of 25 μm, a crystallinity of 55.9%, and a density of 0.95 g / cm3 was used. 3 The polyethylene film used was one side of which was corona-treated.

[0377] (6.1.4) Comparative Example 1F Laminate 10F shown in FIG. 7 was produced in the same manner as in Example 1F, except for the following: no protective layer was provided. Furthermore, instead of using the above-mentioned polyethylene film with a crystallinity of 58.5%, a laminate with a thickness of 25 μm, a crystallinity of 27.5%, and a density of 0.950 g / cm was used as the base layer. 3 A polyethylene film having a thickness of 25 μm, a crystallinity of 55.9%, and a density of 0.95 g / cm was used as the intermediate layer instead of the above polyethylene film having a crystallinity of 27.5%. 3 The polyethylene film used was one side of which was corona-treated.

[0378] (6.2) Measurement and Evaluation Methods The substrate layer and intermediate layer used in the production of the laminate were subjected to in-plane measurement by the wide-angle X-ray diffraction method described above. Then, it was examined whether the diffraction pattern obtained by this measurement had a sharp diffraction peak corresponding to the (110) plane.

[0379] The laminate was also evaluated for sealing property, heat resistance, drop strength, and recyclability. The evaluation methods for sealing property, heat resistance, drop strength, and recyclability are described below.

[0380] (6.2.1) Sealing performance evaluation method The sealing performance was evaluated by the method described in (2.2.1).

[0381] (6.2.2) Heat resistance evaluation method Heat resistance was evaluated by the method described in (2.2.2).

[0382] (6.2.3) Drop Strength Evaluation Method The laminate was cut to a predetermined size, and the periphery was heat-sealed to prepare 10 bags. An opening was provided in each bag to insert the contents. The dimensions of the bags were 100 mm x 150 mm. Next, 200 mL of tap water was filled into each bag, and the opening was heat-sealed to obtain a packaged article. Next, each packaged article was stored at 5°C for one day, and then dropped 50 times from a height of 1.5 m. The ratio of the number of packaged articles whose bags were broken within 50 times to the total number of packaged articles (10) was calculated as the drop strength.

[0383] (6.2.4) Recyclability assessment method Recyclability was evaluated using the method described in (2.2.4).

[0384] (6.3) Results The results of the above measurements and evaluations are summarized in Table 6 below.

[0385] [Table 6]

[0386] As shown in Table 6, all of the laminates in which the crystallinity of the base layer was 35% or more had good heat resistance while being suitable for recycling. In addition, the laminates in which the crystallinity of the base layer was 35% or more, the crystallinity of the intermediate layer was less than 35%, and the protective layer was also excellent in sealability and drop strength. In contrast, the laminates in which the crystallinity of the base layer was less than 35% and the protective layer was not provided had insufficient sealability, heat resistance, and drop strength.

[0387] (7) Test G (7.1) Manufacturing of Laminates (7.1.1) Example 1G 8 was produced by the following method. In this example, an anchor coat layer was further provided between the intermediate layer 8 and the inorganic compound layer 5.

[0388] First, a coating liquid for forming an anchor coat layer and a coating liquid for forming a cover layer were prepared in the same manner as in Example 1B. In addition, a solution of polyamideimide resin in an organic solvent (non-volatile component concentration: 5% by mass) was prepared as a coating liquid for forming a protective layer.

[0389] The substrate layer and the intermediate layer have a thickness of 25 μm, a crystallinity of 58.5%, a haze of 1.6%, and a density of 0.950 g / cm 3 A polyethylene film having the following composition was prepared. This polyethylene film has a three-layer structure (HDPE / MDPE / HDPE) and is subjected to corona treatment on both sides. The crystallinity shown in this example and the examples and comparative examples described below was measured by the above-mentioned measurement method.

[0390] Next, the protective layer forming coating solution prepared above was applied by gravure coating to one side of the base layer that had been subjected to the corona treatment, and dried to form a protective layer having a thickness of 0.5 μm. Subsequently, a water-based flexographic ink was pattern-printed on the other side of the base layer that had been subjected to the corona treatment to form a printing layer.

[0391] Next, the above-mentioned anchor coating agent was applied by gravure coating to one of the corona-treated surfaces of the intermediate layer to form an anchor coating layer having a thickness of 0.1 μm (in a dry state).

[0392] Next, as an inorganic compound layer, a transparent silicon oxide (SiO x A vapor-deposited film having a thickness of 40 nm was formed on the anchor coat layer. The O / Si ratio of the vapor-deposited film was set to 1.8 by adjusting the type of material used for vapor deposition.

[0393] Next, the coating solution for forming a coating layer prepared above was applied to the inorganic compound layer to form a coating layer consisting of an organic / inorganic mixture and having a thickness of 0.3 μm (in a dry state).

[0394] Next, a dry lamination adhesive (urethane adhesive) was applied to the surface of the intermediate layer opposite to the surface on which the inorganic compound layer was formed to form a first adhesive layer. The base layer and the intermediate layer were bonded together so that the printed layer and the intermediate layer faced each other with the first adhesive layer sandwiched therebetween.

[0395] Next, a linear low-density polyethylene resin (LLDPE) film (thickness 60 μm) was prepared as a sealant layer. A dry lamination adhesive (urethane adhesive) was applied onto the sealant layer to form a second adhesive layer. The base layer and the sealant layer were bonded together with the second adhesive layer sandwiched between them so that the sealant layer and the coating layer faced each other. In this manner, a laminate was produced.

[0396] (7.1.2) Example 2G A laminate 10G shown in FIG. 8 was produced in the same manner as in Example 1G, except that the thickness of the protective layer was changed from 0.5 μm to 1 μm. (7.1.3) Example 3G A laminate 10G shown in FIG. 8 was produced in the same manner as in Example 1G, except that the thickness of the protective layer was changed from 0.5 μm to 3 μm. (7.1.4) Example 4G Laminate 10G shown in Fig. 8 was produced in the same manner as in Example 1G, except for the following: no protective layer was provided, and instead of using the polyethylene film with a crystallinity of 58.5% as the intermediate layer, a polyethylene film with a thickness of 25 µm, a crystallinity of 27.6%, and a haze of 21.5% was used. (7.1.5) Comparative Example 1G Laminate 10G shown in Fig. 8 was produced in the same manner as in Example 1G, except for the following: no protective layer was provided, and instead of using the polyethylene film with a crystallinity of 58.5% as the substrate layer and intermediate layer, a polyethylene film with a thickness of 25 µm and a crystallinity of 27.6% was used.

[0397] (7.2) Measurement and Evaluation Methods The substrate layer and intermediate layer used in the production of the laminate were subjected to in-plane measurement by the wide-angle X-ray diffraction method described above. Then, it was examined whether the diffraction pattern obtained by this measurement had a sharp diffraction peak corresponding to the (110) plane.

[0398] The laminate was also evaluated for sealing property, heat resistance, visibility, puncture strength, and recyclability. The evaluation methods for sealing property, heat resistance, visibility, puncture strength, and recyclability are described below.

[0399] (7.2.1) Sealing performance evaluation method The sealing performance was evaluated by the method described in (1.2.1).

[0400] (7.2.2) Heat resistance evaluation method Heat resistance was evaluated by the method described in (2.2.2).

[0401] (7.2.3) Visibility Evaluation Method Visibility was evaluated using the method described in (1.2.3).

[0402] (7.2.4) Evaluation method for puncture strength The puncture strength was evaluated by the method described in (4.2.4).

[0403] (7.2.5) Recyclability assessment method Recyclability was evaluated using the method described in (2.2.4). (7.3) Results The results of the above measurements and evaluations are summarized in Table 7 below.

[0404] [Table 7]

[0405] As shown in Table 7, all of the laminates in which the crystallinity of the base layer was 35% or more had good heat resistance and visibility while being suitable for recycling. In addition, the laminates in which the crystallinity of the base layer and intermediate layer was 35% or more and which had a protective layer also had excellent sealing properties and puncture strength. In contrast, the laminates in which the crystallinity of the base layer was less than 35% and which did not have a protective layer had insufficient sealing properties, heat resistance, visibility, and puncture strength.

[0406] (8) Test G (8.1) Manufacturing of Laminates (8.1.1) Example 1H 9 was produced by the following method. In this example, an anchor coat layer was further provided between the intermediate layer 8 and the inorganic compound layer 5.

[0407] First, a coating liquid for forming an anchor coat layer and a coating liquid for forming a cover layer were prepared in the same manner as in Example 1B. In addition, a solution of polyamideimide resin in an organic solvent (non-volatile component concentration: 5% by mass) was prepared as a coating liquid for forming a protective layer.

[0408] A polyethylene film having a thickness of 25 μm, a crystallinity of 58.5%, and a haze of 1.6% was prepared as the substrate layer. This polyethylene film was subjected to corona treatment on both sides. The crystallinity shown in this example and the examples and comparative examples described below was measured by the above-mentioned measurement method.

[0409] Next, the protective layer forming coating solution prepared above was applied by gravure coating to one side of the base layer that had been subjected to the corona treatment, and dried to form a protective layer having a thickness of 0.5 μm. Subsequently, a water-based flexographic ink was pattern-printed on the other side of the base layer that had been subjected to the corona treatment to form a printing layer.

[0410] As the intermediate layer, a polyethylene film having a thickness of 25 μm, a crystallinity of 27.6%, and a haze of 21.5% was prepared. This polyethylene film was subjected to corona treatment on both sides. Next, the above-mentioned anchor coating agent was applied by gravure coating to one of the corona-treated sides of the intermediate layer to form an anchor coating layer having a thickness of 0.1 μm (in a dry state).

[0411] Next, as an inorganic compound layer, a transparent silicon oxide (SiO x A vapor-deposited film having a thickness of 40 nm was formed on the anchor coat layer. The O / Si ratio of the vapor-deposited film was set to 1.8 by adjusting the type of material used for vapor deposition.

[0412] Next, the coating solution for forming a coating layer prepared above was applied to the inorganic compound layer to form a coating layer consisting of an organic / inorganic mixture and having a thickness of 0.3 μm (in a dry state).

[0413] Next, a dry lamination adhesive (urethane adhesive) was applied to the surface of the intermediate layer opposite to the surface on which the inorganic compound layer was formed to form a first adhesive layer. The base layer and the intermediate layer were bonded together so that the printed layer and the intermediate layer faced each other with the first adhesive layer sandwiched therebetween.

[0414] Next, a linear low-density polyethylene resin (LLDPE) film (thickness 60 μm) was prepared as a sealant layer. A dry lamination adhesive (urethane adhesive) was applied onto the sealant layer to form a second adhesive layer. The base layer and the sealant layer were bonded together with the second adhesive layer sandwiched between them so that the sealant layer and the coating layer faced each other. In this manner, a laminate was produced.

[0415] (8.1.2) Example 2H A laminate 10H shown in FIG. 9 was produced in the same manner as in Example 1H, except that the thickness of the protective layer was changed from 0.5 μm to 1 μm, and further, no covering layer was provided.

[0416] (8.1.3) Example 3H A laminate 10H shown in FIG. 9 was produced in the same manner as in Example 1H, except that the thickness of the protective layer was changed from 0.5 μm to 3 μm.

[0417] (8.1.4) Example 4H Laminate 10H shown in FIG. 9 was produced in the same manner as in Example 1H, except for the following: no protective layer was provided. Furthermore, instead of using the polyethylene film with a crystallinity of 27.6% as the intermediate layer, a polyethylene film with a thickness of 25 μm, a crystallinity of 58.5%, and a haze of 1.6% was used. This polyethylene film was subjected to corona treatment on both sides.

[0418] (8.1.5) Comparative Example 1H The laminate 10H shown in FIG. 9 was produced in the same manner as in Example 1H, except for the following. That is, no protective layer was provided. Furthermore, instead of using the above-mentioned polyethylene film having a crystallinity of 58.5%, a polyethylene film having a thickness of 25 μm, a crystallinity of 27.6%, and a haze of 21.5% was used as the base layer. This polyethylene film was subjected to corona treatment on both sides. Furthermore, instead of using the above-mentioned polyethylene film having a crystallinity of 27.6%, a polyethylene film having a thickness of 25 μm, a crystallinity of 58.5%, and a haze of 1.6% was used as the intermediate layer. This polyethylene film was subjected to corona treatment on both sides.

[0419] (8.2) Measurement and Evaluation Methods The substrate layer and intermediate layer used in the production of the laminate were subjected to in-plane measurement by the wide-angle X-ray diffraction method described above. Then, it was examined whether the diffraction pattern obtained by this measurement had a sharp diffraction peak corresponding to the (110) plane.

[0420] The laminate was also evaluated for sealing property, heat resistance, visibility, drop strength, and recyclability. The evaluation methods for sealing property, heat resistance, visibility, drop strength, and recyclability are described below.

[0421] (8.2.1) Sealing performance evaluation method The sealing performance was evaluated by the method described in (1.2.1).

[0422] (8.2.2) Visibility Evaluation Method Visibility was evaluated using the method described in (1.2.2).

[0423] (8.2.3) Drop Strength Evaluation Method The drop strength was evaluated by the method described in (6.2.3).

[0424] (8.2.4) Recyclability assessment method Recyclability was evaluated using the method described in (2.2.4). (8.3) Results The results of the above measurements and evaluations are summarized in Table 8 below.

[0425] [Table 8]

[0426] As shown in Table 8, all of the laminates in which the crystallinity of the base layer was 35% or more had good heat resistance and visibility while being suitable for recycling. In addition, the laminates in which the crystallinity of the base layer was 35% or more, the crystallinity of the intermediate layer was less than 35%, and the protective layer was provided with excellent sealing properties and drop strength. In contrast, the laminates in which the crystallinity of the base layer was less than 35% and the protective layer was not provided with sufficient sealing properties, heat resistance, and visibility. [Explanation of symbols]

[0427] Reference Signs List 1...base material layer, 2...sealant layer, 3...adhesive layer, 3A...first adhesive layer, 3B...second adhesive layer, 4...printed layer, 5...gas barrier layer (inorganic compound layer), 6...protective layer, 7...coating layer, 8...intermediate layer, 10A1...laminate, 10A2...laminate, 10B...laminate, 10C...laminate, 10D...laminate, 10E...laminate, 10F...laminate, 10G...laminate, 10H...laminate, 100A...packaged article, 100B...packaged article, 100C...packaged article, 110A...packaged body, 110B...packaged body, 110C...packaged body, 110C1...container body, 110C2...mouth member, 110C3...lid body. [Note] The invention as described in the claims of the present application as originally filed is set forth below. [1] A substrate layer, an adhesive layer, and a sealant layer are provided in this order; the substrate layer and the sealant layer comprise polyethylene; The adhesive layer comprises a solventless adhesive, The substrate layer is a laminate having a crystallinity of 40% or more, which is the ratio of the crystalline peak area to the total peak area, measured by a parallel beam method of X-ray diffraction in the diffraction angle range of 10° to 30°. [2] The laminate described in Appendix [1], wherein the adhesive layer has a thickness in the range of 0.1 μm to 20 μm. [3] The laminate according to claim [1], wherein the adhesive layer is a cured product of a resin composition containing a polyester polyol, an isocyanate compound, and a phosphoric acid-modified compound. [4] A package comprising a laminate according to any one of claims [1] to [3]. [5] The packaging body described in appendix [4] which is a stand-up pouch. [6] A packaged article comprising the package described in appendix [4] and contents contained therein.

Claims

1. A substrate layer, an adhesive layer, and a sealant layer are provided in this order; the substrate layer and the sealant layer comprise polyethylene; The adhesive layer comprises a solventless adhesive, The substrate layer has a crystallinity of 40% or more, which is the ratio of the crystalline peak area to the total peak area, measured by a parallel beam method of X-ray diffraction in the diffraction angle range of 10° to 30°.

2. 2. The packaging material of claim 1, wherein the adhesive layer has a thickness in the range of 0.1 μm to 20 μm.

3. 2. The packaging material according to claim 1, wherein the adhesive layer is a cured product of a resin composition containing a polyester polyol, an isocyanate compound, and a phosphoric acid-modified compound.

4. A package comprising the packaging material according to any one of claims 1 to 3.

5. 5. The package according to claim 4, which is a stand-up pouch.

6. A packaged article comprising the package according to claim 4 and contents contained therein.

Citation Information

Patent Citations

  • Vacuum heat insulating material

    JP2007056922A

  • Multilayer film and packaging bag using this film

    JP2009241359A

  • Laminate film having excellent lubricity and blocking resistance, and packaging material and package prepared therewith

    JP2018062173A

  • Multi-layer structure, laminate including the multi-layer structure, and article including the laminate

    JP2018500206A

  • Laminate, packaging material, packaging bag and stand pouch

    JP2020055157A